How paper is made

By using a combination of two light calcium carbonates with different particle sizes and an amphoteric polymer in the paper manufacturing process, the method enhances paper strength and reduces machine stains, addressing the limitations of single-type filler methods.

JP7552084B2Active Publication Date: 2024-09-18OJI HLDG CORP
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2020102985
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-06-15
Publication Date
2024-09-18
Estimated Expiration
2040-06-15

AI Technical Summary

Technical Problem

Existing paper manufacturing methods using composite fillers face issues of reduced paper strength and machine contamination due to the use of single-type calcium carbonate fillers.

Method used

A method involving a pulp slurry containing two types of light calcium carbonates with different particle sizes and an amphoteric polymer, where a first mixture of smaller particle size calcium carbonate and the polymer is added to a pulp and water dispersion, followed by a second larger particle size calcium carbonate, enhancing paper strength and reducing machine stains.

Benefits of technology

The method maintains paper strength while significantly reducing machine stains during the manufacturing process, achieving high ash content and improved paper properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007552084000001
    Figure 0007552084000001
Patent Text Reader

Abstract

To provide a method of producing paper, the method producing high strength paper, in which soiling in a paper-making system is reduced.SOLUTION: A method of producing paper of this invention includes the steps of: obtaining pulp slurry; and making paper from the pulp slurry, the paper containing 10-35 mass% of ash. The pulp slurry includes first light calcium carbonate, second light calcium carbonate, and amphoteric polymer. A primary average particle diameter of the first light calcium carbonate is smaller than a primary average particle diameter of the second light calcium carbonate. The step of obtaining the pulp slurry includes a step of adding a mixture of the first light calcium carbonate and the amphoteric polymer to a dispersion liquid containing pulp and water.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for making paper. [Background technology]

[0002] Generally, paper is made from a pulp slurry in which pulp fibers are suspended in water, and various chemicals are added to the pulp slurry in addition to the pulp fibers as necessary. The main chemicals used are retention aids, paper strength agents, fillers, sizing agents, and viscosity agents.

[0003] In recent years, efforts to reduce the weight of paper have been underway to reduce logistics costs, etc. One approach to reducing the weight of paper is to increase the content of inorganic particles (fillers) to increase the ash content in order to improve the whiteness, opacity, strength, etc. of the paper.

[0004] For example, Patent Document 1 discloses a method for making paper from a stock containing pulp fibers, a filler, and aluminum sulfate, characterized in that the filler is mixed with sodium polyacrylate to form a filler slurry during the stock preparation step, and then the filler slurry is added. Patent Document 2 discloses a papermaking method for improving the surface strength of paper by pre-treating the filler, characterized in that a water-soluble or water-dispersible cationic polymer is added to the filler in advance in the papermaking step at 1.0 to 10.0% (by weight) based on the filler, and this is added as a paper strength agent to a pulp slurry containing an anionic polymer at 0.1 to 0.7% (by weight) based on the pulp.

[0005] Patent Document 3 discloses a method for producing a composite filler for papermaking, in which calcium carbonate and an acrylamide copolymer are mixed to obtain excellent paper strength. In this method, the composite filler is added to a pulp slurry and paper is made to produce a filled paper. In both documents, only one type of calcium carbonate is used. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2014-19995 A [Patent Document 2] Japanese Patent Application Publication No. 55-163298 [Patent Document 3] JP 2016-102265 A Summary of the Invention [Problem to be solved by the invention]

[0007] As mentioned above, it has been considered to improve the whiteness, opacity and strength of paper by using a composite filler in which calcium carbonate is treated with a polymer. However, in the conventional technology, the strength of paper may decrease when a composite filler is used, which is a problem. In addition, in the conventional technology, when trying to produce high ash content paper, machine staining may occur frequently, so improvement was required.

[0008] Therefore, in order to solve such problems of the conventional technology, the present inventors have carried out studies aimed at reducing stains in the papermaking system in the paper manufacturing process in a method for producing high strength paper. [Means for solving the problem]

[0009] As a result of intensive research to solve the above problems, the present inventors have found that, in a step of obtaining a pulp slurry containing a first light calcium carbonate, a second light calcium carbonate, and an amphoteric polymer, by adding a mixture of the first light calcium carbonate and the amphoteric polymer to a dispersion containing pulp and water, and then adding the second light calcium carbonate, it is possible to increase the strength of paper and reduce staining in a papermaking system in a paper manufacturing process. Specifically, the present invention has the following configuration.

[0010] [1] A method for producing paper containing 10 to 35% by mass of ash, comprising the steps of obtaining a pulp slurry and making paper from the pulp slurry, The pulp slurry includes a first light calcium carbonate, a second light calcium carbonate, and an amphoteric polymer, and the first light calcium carbonate has a primary average particle size smaller than the primary average particle size of the second light calcium carbonate. The method for producing paper, wherein the step of obtaining a pulp slurry includes a step of adding a mixture of a first precipitated calcium carbonate and an amphoteric polymer to a dispersion containing pulp and water. [2] The method for producing paper described in [1], wherein the ash content of the paper is 22% by mass or more. [3] The method for producing paper according to [1] or [2], wherein the first precipitated calcium carbonate has an average primary particle diameter of 0.5 μm or more and less than 3.0 μm, and a zeta potential of the first precipitated calcium carbonate of -80 to -15 mV. [4] The method for producing paper according to any one of [1] to [3], wherein the second precipitated calcium carbonate has an average primary particle diameter of 3.0 to 8.0 μm and a zeta potential of greater than −15 mV. [5] The method for producing paper according to any one of [1] to [4], wherein the amount of the amphoteric polymer added is 0.1 to 2.0 parts by mass per 100 parts by mass of the first precipitated calcium carbonate. [6] The method for producing paper according to any one of [1] to [5], wherein the amphoteric polymer is polyacrylamide. [7] The method for producing paper according to any one of [1] to [6], wherein the ash contains light calcium carbonate, and the content of the light calcium carbonate is 80 mass% or more based on the total mass of the ash. [8] The method for producing paper according to any one of [1] to [7], wherein the paper has a tensile strength index in the longitudinal direction of 40 to 60 Nm / g and a tensile strength index in the transverse direction of 35 to 55 Nm / g. [9] A method for producing paper according to any one of [1] to [8], in which a composition image of a distribution image of precipitated calcium carbonate on a paper surface is obtained using a scanning electron microscope (SEM) and converted to black and white using image analysis software IOMate 2007, resulting in a white area ratio of 5 to 30%. Effect of the Invention

[0011] According to the manufacturing method of the present invention, it is possible to increase the strength of paper while reducing stains in the papermaking system during the paper manufacturing process. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present invention will be described in detail below. The following description of the constituent elements may be based on representative embodiments or specific examples, but the present invention is not limited to such embodiments. In this specification, a numerical range expressed using "~" means a range including the numerical values ​​before and after "~" as the lower and upper limits.

[0013] (Paper manufacturing method) The present invention relates to a method for producing paper containing 10 to 35% by mass of ash, comprising a step of obtaining a pulp slurry and a step of making paper from the pulp slurry. Here, the pulp slurry contains a first light calcium carbonate, a second light calcium carbonate, and an amphoteric polymer, and the primary average particle size of the first light calcium carbonate is smaller than the primary average particle size of the second light calcium carbonate. The step of obtaining the pulp slurry includes a step of adding a mixture of the first light calcium carbonate and the amphoteric polymer to a dispersion containing pulp and water. In the present invention, by adding a mixture of the first light calcium carbonate and the amphoteric polymer having a small particle size in the step of obtaining the pulp slurry, it is possible to maintain the strength of the paper and further suppress the occurrence of stains (machine stains, etc.) in the papermaking system.

[0014] Conventionally, in the process of obtaining a pulp slurry, light calcium carbonate is added to improve the whiteness and opacity of paper. However, when light calcium carbonate is added, the strength of the paper is reduced, and the light calcium carbonate precipitates on the surface of the paper, which may cause machine staining, which is problematic. Therefore, in order to solve the above problem, the present inventors have conducted extensive research into a method for producing paper containing light calcium carbonate. As a result, the present inventors have found a method of using two types of light calcium carbonate with different primary average particle sizes in combination, and further, of the two types of light calcium carbonate, the light calcium carbonate with the smaller particle size is mixed with an amphoteric polymer in advance and then added to the pulp slurry. Surprisingly, they have discovered that the strength of paper produced by such a method is maintained and machine staining is reduced.

[0015] In the process for producing paper of the present invention, the step of obtaining a pulp slurry preferably includes a step of adding a mixture of a first light calcium carbonate and an amphoteric polymer to a dispersion containing pulp and water, and further includes a step of adding a second light calcium carbonate thereafter. That is, the step of obtaining a pulp slurry preferably includes a step (A) of adding a mixture of a first light calcium carbonate and an amphoteric polymer to a dispersion containing pulp and water, and a step (B) of adding the second light calcium carbonate after the step (A). In addition, the step of obtaining a pulp slurry may further include a step of mixing optional components as described below, and the order of addition of these optional components is not particularly limited.

[0016] In the step of obtaining a mixture of the first light calcium carbonate and the amphoteric polymer, the amphoteric polymer is added to an aqueous solution containing the first light calcium carbonate to obtain a mixed solution. In this case, the content of the first light calcium carbonate in the aqueous solution containing the first light calcium carbonate is preferably 1% by mass or more, more preferably 5% by mass or more, and even more preferably 10% by mass or more. In addition, the content of the first light calcium carbonate in the aqueous solution containing the first light calcium carbonate is preferably 50% by mass or less. By setting the content of the first light calcium carbonate within the above range, the polymer treatment of the first light calcium carbonate can be efficiently performed. The polymer-treated first light calcium carbonate is also called a composite filler.

[0017] In the step of obtaining a mixture of the first light calcium carbonate and the amphoteric polymer, when the amphoteric polymer is added to the aqueous solution containing the first light calcium carbonate, the first light calcium carbonate is polymer-treated, and the particle size of the first light calcium carbonate increases. The average particle size of the polymer-treated first light calcium carbonate is preferably 3 to 20 μm.

[0018] In the process of making paper from the pulp slurry (hereinafter also referred to as the papermaking process), any papermaking method such as an acidic papermaking method, a neutral papermaking method, or an alkaline papermaking method can be used. Among them, in the process of making paper from the pulp slurry, it is preferable to use a neutral papermaking method or an alkaline papermaking method. As the papermaking machine, a twin-wire papermaking machine, a gap former papermaking machine, a Fourdrinier papermaking machine, a cylinder papermaking machine, an on-top papermaking machine, a Yankee papermaking machine, or the like can be used. Among them, in the papermaking process, it is preferable to use a twin-wire papermaking machine or a gap former papermaking machine, and it is particularly preferable to use a gap former papermaking machine. The twin-wire papermaking machine and the gap former papermaking machine are papermaking machines of a type in which the raw material is sandwiched between two wires and traveled to dehydrate both above and below. Therefore, the raw material is dehydrated almost evenly on both sides, and the dehydration speed is increased. That is, the twin-wire type papermaking machine and the gap former type papermaking machine have the advantage that high-speed papermaking is possible and the difference in texture between the front and back of the resulting paper is small.

[0019] In the paper manufacturing process of the present invention, the surface of the paper may be subjected to a smoothing treatment in order to improve the surface strength of the paper or to increase the adhesiveness with the adhesive. Such smoothing treatment can be carried out, for example, by pressurizing the paper between reels capable of applying pressure. In addition, when performing the smoothing treatment, it is preferable that the roll that comes into contact with the surface of the paper has a smooth surface and is a heatable metal roll.

[0020] The smoothing treatment can also be carried out during the paper making process, for example, by calendaring with a calendar roll having one or more pairs of metal rolls (calendering with a machine calendar), calendaring with a calendar roll having one or more pairs of a metal roll and a resin roll (calendering with a soft calendar), or drying with a Yankee dryer, etc. By using such a manufacturing method, the smoothness of the paper surface is improved, enabling printing with higher accuracy.

[0021] (paper) The present invention may relate to paper produced by the above-mentioned production method. The paper obtained by the production method of the present invention has high strength. Specifically, the specific tensile strength in the longitudinal direction of the paper is preferably 40 Nm / g or more, more preferably 42 Nm / g or more, and even more preferably 44 Nm / g or more. The specific tensile strength in the longitudinal direction of the paper is preferably 60 Nm / g or less. The specific tensile strength in the transverse direction of the paper is preferably 35 Nm / g or more, more preferably 37 Nm / g or more, even more preferably 40 Nm / g or more, and particularly preferably 42 Nm / g or more. The specific tensile strength in the transverse direction of the paper is preferably 55 Nm / g or less. The specific tensile strength of the paper is a value obtained by measuring in accordance with JIS P 8113:2006.

[0022] The ash content of the paper may be 10% by mass or more, preferably 15% by mass or more, more preferably 20% by mass or more, and particularly preferably 22% by mass or more. The ash content of the paper is preferably 35% by mass or less, more preferably 33% by mass or less, and even more preferably 30% by mass or less. Thus, the paper obtained by the manufacturing method of the present invention is preferably a high-ash paper. The ash content is a value measured by the ash content test method (525°C combustion method) described in JIS P 8251.

[0023] Here, the ash content includes light calcium carbonate. In this case, the content of light calcium carbonate is preferably 80% by mass or more, more preferably 85% by mass or more, and even more preferably 90% by mass or more, based on the total mass of the ash content. By setting the content of light calcium carbonate within the above range, it becomes possible to inexpensively produce paper with excellent printability.

[0024] The basis weight of the paper is not particularly limited, but is preferably 20 g / m 2 It is preferable that the thickness is 25 g / m or more. 2 More preferably, the basis weight of the paper is 200 g / m or more. 2 It is preferable that the thickness is less than 170 g / m 2More preferably, it is 150 g / m or less. 2 It is even more preferable that:

[0025] The thickness of the paper is not particularly limited, but is preferably 25 μm or more, more preferably 30 μm or more, and even more preferably 35 μm or more. The thickness of the paper is preferably 250 μm or less, more preferably 225 μm or less, and even more preferably 200 μm or less.

[0026] The paper obtained by the manufacturing method of the present invention contains light calcium carbonate. Here, when a composition image of the distribution image of light calcium carbonate on the surface of the paper is obtained using a scanning electron microscope (SEM) and binarized into black and white using image analysis software IOMate 2007, the white area ratio is preferably 5% or more, more preferably 10% or more, and even more preferably 12% or more. Moreover, the white area ratio is preferably 30% or less. By setting the white area ratio of the paper surface within the above range, it is possible to more effectively reduce machine stains.

[0027] The white area ratio is a value calculated by observing the light calcium carbonate part in the composition of the surface of the paper as white and the pulp part in gray, and performing binarization processing. Specifically, first, the surface of the paper is observed using an electron microscope to obtain a composition image (four or more images per sheet). Here, the composition image reflects the composition of the surface of the paper, and in this specification, the light calcium carbonate part is observed as white and the pulp part is observed as gray. Then, the obtained composition image is binarized using image analysis software IOMate2007 (manufactured by i-Spec Co., Ltd.). In the conditions of the binarization processing, the threshold value is the median of the distribution derived from calcium carbonate + the standard deviation of the distribution derived from calcium carbonate. From the image after the binarization processing, the number of pixels in the white part and the number of pixels in the entire image are measured, and the white area ratio is calculated by the following formula. White area ratio (%) = number of white pixels / total number of pixels in the image x 100

[0028] (Light calcium carbonate) The paper obtained by the manufacturing method of the present invention contains two kinds of light calcium carbonate. Specifically, it contains a first light calcium carbonate and a second light calcium carbonate having different primary average particle diameters. Here, the primary average particle diameter of the first light calcium carbonate is smaller than the primary average particle diameter of the second light calcium carbonate. In addition, the zeta potential of the first light calcium carbonate is -80 to -15 mV, and the zeta potential of the second light calcium carbonate is larger than -15 mV.

[0029] The primary average particle diameter of the first light calcium carbonate is preferably 0.5 μm or more, more preferably 0.7 μm or more, and even more preferably 1.0 μm or more. The primary average particle diameter of the first light calcium carbonate is preferably less than 3.0 μm, more preferably 2.8 μm or less, and even more preferably 2.5 μm or less. Here, the particle diameter of the first light calcium carbonate is measured by measuring the particle size distribution of a 30 mass% slurry of the first light calcium carbonate using a laser diffraction particle size distribution measuring device (MT 3300II, manufactured by Microtrack Bell). The median diameter (particle diameter at which the cumulative frequency is 50%) is taken as the primary average particle diameter.

[0030] The zeta potential of the first light calcium carbonate is preferably -80 mV or more, more preferably -70 mV or more, and even more preferably -60 mV or more. The zeta potential of the first light calcium carbonate is preferably -15 mV or less. By setting the zeta potential of the first light calcium carbonate within the above range, the efficiency of the polymer treatment can be improved in the step of obtaining a mixture of the first light calcium carbonate and the amphoteric polymer. The zeta potential of the first light calcium carbonate is a value measured in accordance with JIS Z 8836:2017 electrophoretic light scattering (ELS) method.

[0031] The content of the first light calcium carbonate is preferably 5 parts by mass or more, more preferably 7 parts by mass or more, and even more preferably 10 parts by mass or more, based on 100 parts by mass of pulp contained in the paper. The content of the first light calcium carbonate is preferably 45 parts by mass or less, more preferably 42 parts by mass or less, and even more preferably 40 parts by mass or less, based on 100 parts by mass of pulp contained in the paper. By setting the content of the first light calcium carbonate within the above range, the effect of maintaining paper strength by the polymer treatment can be more effectively enhanced.

[0032] The primary average particle diameter of the second light calcium carbonate is preferably 3.0 μm or more, more preferably 3.5 μm or more, and even more preferably 4.0 μm or more. The primary average particle diameter of the second light calcium carbonate is preferably 8.0 μm or less, more preferably 7.5 μm or less, and even more preferably 7.0 μm or less. Here, the particle diameter of the second light calcium carbonate is measured by measuring the particle size distribution of a 30 mass% slurry of the second light calcium carbonate using a laser diffraction particle size distribution measuring device (MT 3300II, manufactured by Microtrack Bell). The median diameter (particle diameter at which the cumulative frequency is 50%) is taken as the primary average particle diameter.

[0033] The zeta potential of the second precipitated calcium carbonate is preferably greater than −15 mV. The zeta potential of the second precipitated calcium carbonate is a value measured in accordance with JIS Z 8836:2017 electrophoretic light scattering (ELS) method.

[0034] The content of the second light calcium carbonate is preferably 5 parts by mass or more, more preferably 7 parts by mass or more, and even more preferably 10 parts by mass or more, per 100 parts by mass of pulp contained in the paper. The content of the second light calcium carbonate is preferably 45 parts by mass or less, more preferably 42 parts by mass or less, and even more preferably 40 parts by mass or less, per 100 parts by mass of pulp contained in the paper. By setting the content of the second light calcium carbonate within the above range, the effect of maintaining paper strength by the polymer treatment can be more effectively enhanced.

[0035] The mass ratio of the first light calcium carbonate to the second light calcium carbonate is preferably 3:7 to 7:3, and more preferably 4:6 to 6:4. By setting the mass ratio of the first light calcium carbonate to the second light calcium carbonate within the above range, the effect of maintaining paper strength by the polymer treatment can be more effectively enhanced.

[0036] (Amphoteric polymer) The paper obtained by the production method of the present invention contains an amphoteric polymer. In this specification, an amphoteric polymer is a polymer having both an anionic group and a cationic group in one molecule. The amphoteric polymer has a function of agglomerating a part of the light calcium carbonate by covering the light calcium carbonate in the pulp slurry. This allows the strength of the paper to be maintained even if the paper contains a certain amount or more of light calcium carbonate.

[0037] The weight average molecular weight of the amphoteric polymer is preferably 1 million or more, more preferably 1.5 million or more, and even more preferably 2 million or more. The weight average molecular weight of the amphoteric polymer is preferably 10 million or less, more preferably 8 million or less, and even more preferably 7 million or less. The weight average molecular weight of the amphoteric polymer is a value measured by gel permeation chromatography (GPC) and calculated using a calibration curve prepared using standard polystyrene with a known molecular weight.

[0038] The amphoteric polymer is preferably polyacrylamide. Polyacrylamide is a polymer obtained by polymerizing a monomer and acrylamide. The polyacrylamide is preferably one obtained by polymerizing an ionic monomer and a nonionic monomer, and more preferably one having a branched structure.

[0039] The amount of amphoteric polymer added is preferably 0.1 parts by mass or more, more preferably 0.3 parts by mass or more, and even more preferably 0.5 parts by mass or more, relative to 100 parts by mass of the first light calcium carbonate. The amount of amphoteric polymer added is preferably 2.0 parts by mass or less, more preferably 1.8 parts by mass or less, and even more preferably 1.5 parts by mass or less, relative to 100 parts by mass of the first light calcium carbonate. By setting the amount of amphoteric polymer added within the above range, the strength of the paper can be more effectively increased. Furthermore, by setting the amount of amphoteric polymer added within the above range, machine staining can be more effectively suppressed.

[0040] (Pulp raw material) In the step of obtaining a pulp slurry, first, a dispersion liquid containing pulp and water is obtained. Pulps that can be used in the present invention include, for example, pulp derived from hardwood, pulp derived from softwood, and pulp derived from non-wood. Hardwood kraft pulp includes, for example, unbleached hardwood kraft pulp (LUKP), bleached hardwood kraft pulp (LBKP), semi-bleached hardwood kraft pulp (LSBKP), and sulfite hardwood pulp. Softwood kraft pulp includes, for example, unbleached softwood kraft pulp (NUKP), bleached softwood kraft pulp (NBKP), semi-bleached softwood kraft pulp (NSBKP), and sulfite softwood pulp.

[0041] In addition, the pulp contained in the paper of the present invention preferably contains acacia-derived hardwood pulp. The content of acacia-derived hardwood pulp is preferably 30% by mass or more based on the total mass of the raw materials for the pulp. The content of acacia-derived hardwood pulp may be 30-100% by mass based on the total mass of the raw materials for the pulp, preferably 50-100% by mass, and more preferably 70-100% by mass. By setting the content of acacia-derived pulp within the above range, paper with a small static friction coefficient can be produced. Furthermore, by setting the content of acacia-derived hardwood pulp within the above range, the drying time of the paper in the production process can be shortened.

[0042] Examples of acacia-derived pulp that can be used include pulp obtained from Acacia mangium, A. auriculiformis, A. catechu, A. decurrens, A. holosericea, A. leptocarpa, A. maidenii, A. mearnsii, A. melanoxylon, A. neriifolia, A. silvestris, A. peregrinalis, and hybrids thereof.

[0043] In the present invention, in addition to softwood kraft pulp and hardwood kraft pulp, various known pulps can be used, such as mechanical pulps such as stone ground pulp (SGP), pressed stone ground pulp (PGW), refiner ground pulp (RGP), thermo ground pulp (TGP), chemi-ground pulp (CGP), groundwood pulp (GP) and thermo mechanical pulp (TMP); disintegrated waste paper pulp, disintegrated and deinked waste paper pulp, or disintegrated, deinked and bleached waste paper pulp produced from brown paper, kraft envelope paper, magazine paper, newspaper paper, flyer paper, office paper, corrugated cardboard, white paper, Kent paper, imitation waste paper, and land certificate paper; and pulp produced chemically or mechanically from non-wood fibers such as kenaf, hemp, and reed. The content of recycled paper pulp relative to the total mass of the paper is preferably less than 30% by mass, more preferably less than 20% by mass, and even more preferably less than 10% by mass.

[0044] The freeness of the pulp raw material used in the present invention is preferably 350 to 650 ml CSF. Before the step of obtaining the pulp slurry, a beating step may be performed as necessary to obtain the above freeness. The freeness is the freeness value measured by a Canadian standard freeness tester in accordance with JIS-P8121 after a sample is disintegrated in a standard disintegrator in accordance with JIS-P8220.

[0045] (optional ingredient) In the present invention, in addition to the above-mentioned precipitated calcium carbonate and amphoteric polymer, other internal additives, fillers, etc., may be added. Examples of internal additives include various known agents such as paper strength enhancers such as starch, freeness retention improvers such as polyamides, antifoaming agents, basic dyes, acid dyes, anionic direct dyes, and cationic direct dyes.

[0046] In addition, a water-soluble aluminum compound may be added to the pulp slurry as an internal additive. The water-soluble aluminum compound functions as a fixing agent for fixing the paper strength agent, sizing agent, etc. in the paper. Examples of the water-soluble aluminum compound include polyaluminum chloride (PAC) and aluminum sulfate.

[0047] Furthermore, an internal sizing agent may be added to the pulp slurry as an internal chemical. Examples of the internal sizing agent include rosin-based sizing agents, alkyl ketene dimers, and alkenyl succinic anhydrides. By adding the internal sizing agent, the water resistance of the paper can be improved, and the printability can be improved.

[0048] The filler may contain talc in addition to the above-mentioned light calcium carbonate. Talc is mainly composed of hydrated magnesium silicate (3MgO·4SiO2·H2O). The filler may contain fillers other than talc. Examples of inorganic fillers other than talc include inorganic pigments such as heavy calcium carbonate, calcium sulfite, gypsum, kaolin, delaminated kaolin, hydrated silicate, diatomaceous earth, magnesium carbonate, barium carbonate, zinc oxide, titanium dioxide, aluminum hydroxide, calcium hydroxide, magnesium hydroxide, or zinc hydroxide, and organic pigments such as urea-formaldehyde resin fine particles or hollow fine particles. In addition, when waste paper or broke paper is used as a pulp raw material, the filler contained therein may also be contained. Note that two or more types of inorganic fillers may be mixed and used. EXAMPLES

[0049] The features of the present invention will be described in more detail below with reference to examples and comparative examples. The materials, amounts used, ratios, processing contents, processing procedures, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the specific examples shown below.

[0050] <Example 1> As the raw pulp, 400 mL of hardwood bleached kraft pulp (LBKP) was used. 0.5 parts by mass of aluminum sulfate (aluminum sulfate 18-hydrate) and 1.2 parts by mass of cationic starch (P-3Y, manufactured by Pillar Starch Co., Ltd.) were added to 100 parts by mass (bone dry mass) of pulp, and the mixture was diluted to a pulp concentration of 0.5% by mass. 0.14 parts by mass of alkenyl succinic anhydride (manufactured by Arakawa Chemical Co., Ltd.) was added to the diluted pulp slurry to 100 parts by mass (bone dry mass) of pulp. In another container, 16 parts by mass of light calcium carbonate (a) (Tama Pearl TP-121, primary average particle size 1.7 μm, manufactured by Okutama Kogyo Co., Ltd.) was prepared relative to 100 parts by mass (bone dry mass) of pulp, and diluted with water to 30% by mass. 0.5 parts by mass of amphoteric polymer (compound A, amphoteric polyacrylamide manufactured by Seiko PMC Co., Ltd.) was added relative to 100 parts by mass (bone dry mass) of light calcium carbonate (a) contained in this diluted solution, and stirred for 3 minutes. The light calcium carbonate (a) thus polymer-treated was added to a pulp slurry with a pulp concentration of 0.5% by mass. Next, 12 parts by mass of light calcium carbonate (b) (Tama Pearl TP-NPF, primary average particle size 5.0 μm, manufactured by Okutama Kogyo Co., Ltd.) relative to 100 parts by mass (bone dry mass) of pulp was added to a pulp slurry with a pulp concentration of 0.5% by mass. Next, 0.02 parts by mass of a retention aid (ND-300, manufactured by HYMO Co., Ltd.) was added to the pulp slurry per 100 parts by mass of pulp (bone dry mass), and paper was made using a square hand-made papermaking machine in accordance with the Japanese Industrial Standard JIS P8222 to produce a paper with a basis weight of 60 g / m. 2 As a result, handmade paper of

[0051] <Example 2> Handmade paper was obtained in the same manner as in Example 1, except that the amount of amphoteric polymer (compound A) added in the mixed solution was changed to 1.0 part by mass per 100 parts by mass (bone dry mass) of precipitated calcium carbonate (a).

[0052] <Example 3> Handmade paper was obtained in the same manner as in Example 1, except that the amount of amphoteric polymer (compound A) added in the mixed solution was changed to 0.1 parts by mass per 100 parts by mass (bone dry mass) of precipitated calcium carbonate (a).

[0053] <Example 4> Handmade paper was obtained in the same manner as in Example 1, except that the light calcium carbonate (a) (Tamapearl TP-121, average primary particle size 1.7 μm, manufactured by Okutama Kogyo Co., Ltd.) in Example 1 was changed to light calcium carbonate (a) (Tamapearl TP-221BM, average primary particle size 2.8 μm, manufactured by Okutama Kogyo Co., Ltd.).

[0054] <Example 5> Handmade paper was obtained in the same manner as in Example 1, except that the light calcium carbonate (a) (Tamapearl TP-121, average primary particle size 1.7 μm, manufactured by Okutama Kogyo Co., Ltd.) in Example 1 was changed to light calcium carbonate (a) (Tamapearl TP-121SA, average primary particle size 1.1 μm, manufactured by Okutama Kogyo Co., Ltd.).

[0055] <Comparative Example 1> Handsheets were obtained in the same manner as in Example 1, except that the amphoteric polymer (compound A) was not added.

[0056] <Comparative Example 2> Handmade paper was obtained in the same manner as in Example 1, except that a cationic polymer (compound B, cationic polyacrylamide, manufactured by Seiko PMC Corporation) was used instead of the amphoteric polymer (compound A).

[0057] <Comparative Example 3> Handmade paper was obtained in the same manner as in Example 1, except that an anionic polymer (compound C, anionic polyacrylamide, manufactured by Seiko PCM Co., Ltd.) was used instead of the amphoteric polymer (compound A).

[0058] <Comparative Example 4> Handmade paper was obtained in the same manner as in Example 1, except that the amount of light calcium carbonate (a) added was 22 parts by mass per 100 parts by mass (bone dry mass) of pulp, and the amount of light calcium carbonate (b) added was 18 parts by mass per 100 parts by mass (bone dry mass) of pulp.

[0059] <Comparative Example 5> To the diluted pulp slurry in Example 1, 0.14 parts by mass of alkenyl succinic anhydride (Fibran, manufactured by Arakawa Chemical Industries, Ltd.) was added relative to 100 parts by mass (bone dry mass) of pulp. In another container, 12 parts by mass of light calcium carbonate (b) (Tama Pearl TP-NPF, primary average particle size 5.0 μm, manufactured by Okutama Kogyo Co., Ltd.) was prepared for 100 parts by mass (bone dry mass) of pulp, and diluted with water to 30% by mass. 0.5 parts by mass of amphoteric polymer (compound A, amphoteric polyacrylamide, manufactured by Seiko PMC Co., Ltd.) was added for 100 parts by mass (bone dry mass) of light calcium carbonate (b) contained in this diluted solution, and stirred for 3 minutes. The light calcium carbonate (b) thus polymer-treated was added to a pulp slurry with a pulp concentration of 0.5% by mass. Next, 16 parts by mass of light calcium carbonate (a) (Tama Pearl TP-121, primary average particle size 1.7 μm, manufactured by Okutama Kogyo Co., Ltd.) was added to a pulp slurry with a pulp concentration of 0.5% by mass for 100 parts by mass (bone dry mass) of pulp. Next, 0.02 parts by mass of a retention aid (ND-300, manufactured by HYMO Co., Ltd.) was added to the pulp slurry per 100 parts by mass of pulp (bone dry mass), and paper was made using a square hand-made papermaking machine in accordance with the Japanese Industrial Standard JIS P8222 to produce a paper with a basis weight of 60 g / m. 2 As a result, handmade paper of

[0060] (evaluation) <Particle size> The particle size distribution of a 30% by mass slurry of precipitated calcium carbonate was measured using a laser diffraction particle size distribution analyzer (MT 3300II, manufactured by Microtrac-Bell), and the median diameter (particle diameter at which the cumulative frequency is 50%) was taken as the primary average particle diameter.

[0061] <Zeta potential measurement> The zeta potential of a 30 mass% slurry of precipitated calcium carbonate was measured in accordance with JIS Z 8836:2017 electrophoretic light scattering (ELS) method.

[0062] <Measurement of ash content in paper> The ash content of the papers obtained in the Examples and Comparative Examples was measured in accordance with JIS P 8251.

[0063] <Ratio of light calcium carbonate in ash of paper In accordance with JIS P 8251, after the papers obtained in the examples and comparative examples were ashed, the particle size distribution of the ash was measured using a laser diffraction particle size distribution measuring device (MT3000II, manufactured by Microtrac Bell Co., Ltd.). The ratio of light calcium carbonate was calculated with particles having a particle diameter of 1 μm or more and less than 11 μm being light calcium carbonate and those having a particle diameter of 11 μm or more and less than 16 μm being talc

[0064] <Method for measuring specific tensile strength The specific tensile strength of the papers obtained in the examples and comparative examples was measured in accordance with JIS P 8113:2006

[0065] <Binarization of SEM image The surfaces of the papers obtained in the examples and comparative examples were observed under the following conditions using an electron microscope to obtain a composite image (4 or more images per sheet). The composite image reflects the composition of the sample. In this example, the light calcium carbonate portion was observed as white and the pulp portion was observed as gray <Electron microscope observation conditions · Analytical apparatus Scanning electron microscope (S-3600N, manufactured by Hitachi High-Technologies Corporation) · Observed image Secondary electron image (composite image) · Magnification 100 - 150 times · Acceleration voltage 15.0 kV The obtained composite image was subjected to binarization processing using image analysis software IOMate2007 (manufactured by Eye Spec Co., Ltd.). The conditions for the binarization processing were as follows <Binarization processing conditions · Threshold value Median value of the distribution derived from calcium carbonate + Standard deviation of the distribution derived from calcium carbonate From the image after binarization processing, the number of pixels in the white portion and the number of pixels in the entire image were measured, and the white area ratio was calculated White area ratio (%) = Number of pixels in white portion / Number of pixels in entire image × 100

[0066] <Evaluation of machine dirt The papers obtained in the examples and comparative examples were cut into 240 mm squares, and an adhesive film (CPETT75 / AC / T2(-R3) manufactured by Shin-Tack Chemical Co., Ltd.) of 6 cm x 12 cm was attached to the center of the paper, and calendaring was performed using an induction heating test calendar (35F-FC-200C manufactured by Kumagai Riki Kogyo Co., Ltd.). <Calendar conditions> ·Temperature: 30℃ Roll speed: 60m / min Number of pressurizations: 1 round trip ·Line pressure: 65kgf / cm Next, the adhesive film was peeled off from the paper, and the amount of calcium (X-ray intensity of calcium atoms) attached to the central 6cm x 6cm of the adhesive film, excluding 3cm on both ends, was measured with an X-ray fluorescence analyzer and used as an index of machine soiling. A smaller value indicates less light calcium carbonate peeled off from the paper surface, which means less machine soiling. <X-ray fluorescence analysis measurement conditions> Analytical equipment: Rigaku scanning X-ray fluorescence analyzer ZSX Primus IV Measurement sample: diameter 27mm X-ray tube: Rh target 4kW Excitation light energy: 40kV-75mA Measurement line: Ca-KA 2θ angle peak: 113.130deg ·Measurement time: 0.1sec(110-116deg)

[0067] [Table 1]

[0068] The papers obtained in the examples did not show a significant decrease in strength, and machine staining during the manufacturing process was reduced.

Claims

1. A method for producing paper containing 10 to 35% by mass of ash, comprising the steps of obtaining a pulp slurry and making paper from the pulp slurry, the pulp slurry includes a first light calcium carbonate, a second light calcium carbonate, and an amphoteric polymer, the first light calcium carbonate having a primary average particle size smaller than the primary average particle size of the second light calcium carbonate, The first precipitated calcium carbonate has a primary average particle size of 0.5 μm or more and less than 3.0 μm, and a zeta potential of −80 to −15 mV. The second precipitated calcium carbonate has a primary average particle size of 4.0 to 8.0 μm and a zeta potential of greater than −15 mV; The amount of the first precipitated calcium carbonate added is 5 parts by mass or more and 45 parts by mass or less relative to 100 parts by mass of pulp contained in the paper, The amount of the second precipitated calcium carbonate added is 5 parts by mass or more and 45 parts by mass or less relative to 100 parts by mass of pulp contained in the paper, the amphoteric polymer is polyacrylamide; The amount of the amphoteric polymer added is 0.1 parts by mass or more and 2.0 parts by mass or less with respect to 100 parts by mass of the first precipitated calcium carbonate, The method for producing paper, wherein the step of obtaining a pulp slurry includes a step of adding a mixture of the first precipitated calcium carbonate and the amphoteric polymer to a dispersion containing pulp and water.

2. The method for producing paper according to claim 1 , wherein the ash content of the paper is 22% by mass or more.

3. 3. The method for producing paper according to claim 1, wherein the ash contains light calcium carbonate, and the content of the light calcium carbonate is 80 mass% or more based on the total mass of the ash.

4. The method for producing paper according to any one of claims 1 to 3, wherein the paper has a longitudinal tensile specific strength of 40 to 60 Nm / g and a transverse tensile specific strength of 35 to 55 Nm / g.

5. The method for producing paper according to any one of claims 1 to 4, wherein when a composition image of a distribution image of the precipitated calcium carbonate on the surface of the paper is obtained using a scanning electron microscope (SEM) and binarized into black and white using image analysis software IOMate 2007, the white area ratio is 5 to 30%.

Citation Information

Patent Citations

  • Filler containing paper product and production

    JP1979116405A

  • Paper making method for enhancing surface strength of paper by filler pretreatment

    JP1980163298A

  • Internal sized paper

    JP1984026595A

  • Cigarette having controlled frequency of smoking and rolled paper

    JP1993187000A

  • Regulation of gas permeability of wrapping paper for smoking product and system therefor

    JP1999036194A