Resin film, manufacturing method of resin film, resin film / adhesive layer laminate, manufacturing method of resin film / adhesive layer laminate, electric circuit body, health care sensor, wearable sensor, manufacturing method of resin film processed product
A resin film with tailored mechanical properties and a particle layer enhances flexibility and restorability, addressing the limitations of conventional films in wearable devices and electrical circuits by improving printability and adhesion.
Patent Information
- Application Number
- JP2020125080
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-01-27
- Filing Date
- 2020-07-22
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2040-07-22
AI Technical Summary
Conventional resin films used in wearable devices and electrical circuits lack sufficient flexibility, restorability, printability, and adhesion, making them unsuitable for stretchable wiring and post-processing applications.
A resin film with specific mechanical properties, including a storage modulus of 0.5 MPa to 50 MPa, a loss tangent of 0.5 or less, and surface roughness of 150 nm to 5,000 nm, combined with a particle layer and adhesive layer, to enhance flexibility, restorability, and printability.
The resin film achieves high flexibility and resilience, enabling effective post-processing such as screen printing without blurring, maintaining adhesion to metal wiring, and reducing electrical resistance.
Smart Images

Figure 0007552116000026 
Figure 0007552116000033 
Figure 0007552116000034
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin film that is suitable for post-processing while maintaining high flexibility and recovery properties, a method for manufacturing a resin film, a resin film / adhesive layer laminate, a method for manufacturing a resin film / adhesive layer laminate, an electric circuit, a healthcare sensor, a wearable sensor, and a method for manufacturing a resin film processed product. [Background technology]
[0002] A wide variety of sensors that detect distortion, minute displacement, pressure, and temperature are used in a wide range of fields, from industrial to consumer. Furthermore, as they have become smaller and lighter, they can now be attached to various objects in daily life, including mobile devices, helping to improve convenience and avoid danger in daily life. Furthermore, in recent years, these sensors have been attached to the human body in the form of health care sensors and wearable sensors, and are expected to fundamentally change our lives by collecting huge amounts of data and using them to provide alarms and advice.
[0003] In the field of such sensors and devices, various resin films have been used as substrates for their electrical circuits to reduce their weight and size. However, conventional materials are films with rigid chemical bonds and strong crystallinity, such as polyimide, which can be bent freely but cannot be stretched. Therefore, in such health care sensors and wearable devices such as wearable sensors, there is a demand for resin films that are easily stretchable for use in the electrical circuits.
[0004] As an example of an existing resin film that is easily stretchable, Patent Document 1 proposes "a polyurethane produced by reacting a polyether polyol (a) having a carbonate bond with an isocyanate compound (b), wherein the hydroxyl value of the polyether polyol (a) is 55 or less."
[0005] Furthermore, Patent Document 2 proposes "an active energy ray-curable resin composition comprising at least (a-1) a polyisocyanate, (a-2) a low molecular weight polyol having an alicyclic structure and a number average molecular weight of 500 or less, and (a-3) a urethane (meth)acrylate oligomer (A) which is a reaction product of a hydroxyalkyl (meth)acrylate, wherein the calculated network crosslinking molecular weight of the composition is 1,000 or more and 6,000 or less."
[0006] Furthermore, as a material having excellent elasticity and being easy to handle as a resin film, Patent Document 3 proposes "a composition for forming a flexible resin, which contains (A) an elastomer containing monomer units derived from styrene, (B) a polymerizable compound, and (C) a polymerization initiator, wherein the mass ratio of the monomer units derived from styrene to the total amount of the elastomer (A) is 27 mass% or more," while Patent Document 4 proposes "a curable resin composition for forming a flexible resin, which contains (A) a styrene-based elastomer, (B) a polymerizable monomer, and (C) a polymerization initiator, wherein the polymerizable monomer contains a silicone compound having a (meth)acryloyloxy group." [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2015-189886 A [Patent Document 2] JP 2010-222568 A [Patent Document 3] JP 2018-172460 A [Patent Document 4] JP 2018-203827 A Summary of the Invention [Problem to be solved by the invention]
[0008] It is important that wearable devices such as the aforementioned healthcare sensors and wearable sensors do not cause any strain on the human body when attached to them. To achieve this, they need to be able to bend and stretch without strain and then return to their original shape. For this reason, the resin film used as the base material for the electrical circuit body needs to have high "flexibility" and "restorability," and also needs to be suitable for post-processing so that stretchable wiring can be formed on the resin film.
[0009] One method of making stretchable wiring is to laminate copper foil onto the surface of a stretchable resin film, etch the copper foil to form a specific pattern, and then deform the copper foil to impart stretchability; however, this limits the stretchability to around 120%, and to achieve even greater stretchability, a specific metal paste that can create stretchable wiring is often used, and the wiring is formed by screen printing or other methods.
[0010] In this case, the resin film needs to have the following post-processing suitability: "printability" so that the wiring does not bleed or fade when the metal paste is screen-printed, "heat resistance" so that the printed wiring can withstand drying, and "adhesion" to the formed wiring.
[0011] In order to impart the above-mentioned "printability" and "adhesion", one side of the resin film may have a particle layer. In this case, the resin film is required to have adhesion between the particle layer and the resin film serving as a substrate, i.e., so-called "particle layer adhesion", as a processing suitability in a post-processing step.
[0012] In response to the above demands, the present inventors have confirmed the above-mentioned conventional techniques, and found that the resin film made of the resin described in Patent Document 1 had good flexibility and adhesion, but had problems with restoration, printability, and heat resistance. The resin film made of the resin composition described in Patent Document 2 had good heat resistance, but was insufficient in flexibility, restoration, printability, and adhesion. The resin film made of the resin composition described in Patent Document 3 had good printability, heat resistance, and adhesion, but was insufficient in flexibility and restoration. The resin film made of the resin composition described in Patent Document 4 had good flexibility, printability, and heat resistance, but was insufficient in restoration and adhesion.
[0013] In view of the above, an object of the present invention is to provide a resin film that is suitable for subsequent processing while maintaining high flexibility and resilience, a method for manufacturing a resin film, a resin film / adhesive layer laminate, a method for manufacturing a resin film / adhesive layer laminate, an electrical circuit, a health care sensor, a wearable sensor, and a method for manufacturing a resin film processed product. [Means for solving the problem]
[0014] In order to solve the above problems, the present inventors have conducted extensive research and have completed the following invention. 1) A resin film that meets the following conditions: Condition 1. The storage modulus at a temperature of 25°C and a frequency of 1 Hz is 0.5 MPa or more and 50 MPa or less. Condition 2. Loss tangent at a temperature of 25°C and a frequency of 1 Hz is 0.5 or less. Condition 3. The surface roughness Sa of at least one surface is 150 nm or more and 5,000 nm or less. 2) The resin film according to 1), wherein at least one surface of the resin film has a surface free energy of 25 mN / m or more. 3) The resin film according to 1) or 2), which has a resin layer containing segments of Chemical Formula 1 and Chemical Formula 2.
[0015] [ka]
[0016] [ka]
[0017] R 1 refers to a hydrogen or a methyl group. R 2 refers to any of the following: A substituted or unsubstituted alkylene group. A substituted or unsubstituted arylene group. An alkylene group having an internal ether group, ester group, or amide group. An arylene group having an internal ether group, ester group, or amide group. An unsubstituted alkylene group having an ether group, an ester group, or an amide group inside. An unsubstituted arylene group having an ether group, an ester group, or an amide group therein. R 3 refers to any of the following: A substituted or unsubstituted alkylene group. A substituted or unsubstituted arylene group. 4) The resin film according to any one of 1) to 3), wherein the resin film has a particle layer containing resin particles. 5) The resin film according to 4) above, wherein the number average particle diameter of the resin particles contained in the particle layer is 2 μm or more and 20 μm or less. 6) The resin film according to 4) or 5), which has a resin layer and a particle layer on at least one surface thereof, the particle layer containing a segment of Chemical Formula 3.
[0018] [ka]
[0019] 7) The resin film according to any one of 1) to 6), wherein the skewness Ssk of at least one surface of the resin film is −0.2 or more and 1.0 or less. 8) A resin film / adhesive layer laminate in which the resin film of 7) is in contact with an adhesive layer. 9) A method for producing a resin film / adhesive layer laminate, comprising laminating the resin film and adhesive layer of 7). 10) A method for producing a resin film according to any one of 1) to 7), comprising a step of applying a coating composition for a particle layer containing resin particles to form a particle layer. 11) An electrical circuit body comprising a resin film according to any one of 1) to 7) or a resin film / adhesive layer laminate according to 8), and a conductor circuit formed on the resin film. 12) A healthcare sensor comprising a resin film according to any one of 1) to 7) or a resin film / adhesive layer laminate according to 8), and a conductor circuit formed on the resin film. 13) A wearable sensor comprising a resin film according to any one of 1) to 7) or a resin film / adhesive layer laminate according to 8), and a conductor circuit formed on the resin film. 14) A method for producing a resin film processed product, comprising a step of processing a resin film described in any one of 1) to 7) or a resin film / adhesive layer laminate described in 8) by screen printing. Effect of the Invention
[0020] The present invention is able to provide resin films that are suitable for post-processing while maintaining high flexibility and resilience, methods for manufacturing resin films, resin film / adhesive layer laminates, methods for manufacturing resin film / adhesive layer laminates, electrical circuits, healthcare sensors, wearable sensors, and methods for manufacturing resin film processed products. [Brief description of the drawings]
[0021] [Figure 1] FIG. 1 is a cross-sectional view showing an example of a resin film in the present invention. [Diagram 2] FIG. 1 is a schematic diagram showing an example of a method for producing a resin film in the present invention, in which a particle layer is formed in a laminate state. [Diagram 3]FIG. 1 is a cross-sectional view showing an example of a laminate according to the present invention. [Figure 4] FIG. 1 is a cross-sectional view showing an example of a laminate according to the present invention. [Diagram 5] FIG. 1 is a schematic diagram showing an example of a method for producing a resin film in the present invention, which is an example in which a supporting substrate having an uneven surface is used. [Figure 6] FIG. 1 is a schematic diagram showing an example of a method for producing a resin film in the present invention, in which a release layer having an uneven surface is used. [Figure 7] FIG. 1 is a cross-sectional view showing an example of a laminate according to the present invention. [Figure 8] FIG. 1 is a cross-sectional view showing an example of a laminate according to the present invention. [Figure 9] FIG. 1 is a cross-sectional view showing an example of a laminate according to the present invention. [Figure 10] FIG. 1 is a cross-sectional view showing an example of a laminate according to the present invention. [Figure 11] FIG. 2 is a plan view showing an example of an electric circuit body according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] Before describing the mode for carrying out the present invention, the inventors will explain why it is difficult to achieve the objectives of the present invention, particularly printability, with the conventional techniques, by citing Patent Document 3 and Patent Document 4, which provide good printability, as examples.
[0023] The reason why the technology described in Patent Document 3 has good printability is believed to be that the styrene content of the styrene-based elastomer is set to a certain value or more to increase the elastic modulus, and the surface free energy is lowered to reduce tack and suppress the adhesion of the printing plate. However, an increase in the elastic modulus reduces flexibility, and an increase in the styrene content increases physical crosslinking, which is thought to reduce recovery. For this reason, there is a trade-off between printability, flexibility, and recovery, making it difficult to achieve both.
[0024] The technology described in Patent Document 4 has good printability because it reduces tack by lowering the surface free energy, suppressing the adhesion of the printing plate. However, there is a problem that the low surface free energy causes poor adhesion of metal wiring, and there is a trade-off between printability and adhesion, making it difficult to achieve both.
[0025] In contrast to these conventional techniques, the present inventors have succeeded in achieving both flexibility, restorability, and suitability for subsequent processing by focusing on the surface shape of a resin film as a method for solving the above-mentioned problems, and have arrived at the present invention. The present invention will be specifically described below.
[0026] First, in order to solve the above-mentioned problems, it is important that the resin film of the present invention has specific mechanical properties and, in addition, has a specific surface shape, and the specific details are as follows. Condition 1. The storage modulus at a temperature of 25°C and a frequency of 1 Hz is 0.5 MPa or more and 50 MPa or less. Condition 2. Loss tangent at a temperature of 25°C and a frequency of 1 Hz is 0.5 or less. Condition 3. The surface roughness Sa of at least one surface is 150 nm or more and 5,000 nm or less.
[0027] From the viewpoints of printability, improved film handling, and improved flexibility, the storage modulus of the resin film under condition 1 at a temperature of 25° C. and a frequency of 1 Hz is preferably 0.5 MPa or more and 50 MPa or less, and more preferably 2.0 MPa or more and 25 MPa or less. The storage modulus refers to a value measured by a DMA (dynamic viscoelasticity measurement) method, and the measurement method will be described later. By having the storage modulus of the resin film be 0.5 MPa or more, it is possible to prevent problems in handling the film in subsequent processes, and from the same viewpoint, it is more preferable that the storage modulus be 2.0 MPa or more.
[0028] In addition, by setting the storage modulus of the resin film at 25° C. and 1 Hz, the film can have a certain degree of flexibility and can reduce discomfort when wearing the device. From the same viewpoint, it is more preferable that the storage modulus is 25 MPa or less.
[0029] The loss tangent of the resin film under condition 2 at a temperature of 25° C. and a frequency of 1 Hz is preferably 0.5 or less. The loss tangent refers to a value measured by a DMA method, and the measurement method will be described later. By making the loss tangent of the resin film 0.5 or less, sufficient restorability can be obtained when used as a resin film. From the same viewpoint, the loss tangent of the resin film at a temperature of 25° C. and a frequency of 1 Hz is more preferably 0.2 or less.
[0030] The surface roughness Sa of the resin film in condition 3 is preferably 150 nm or more and 5,000 nm or less. The method for measuring the surface roughness of the resin film will be described later. By having the surface roughness Sa of 150 nm or more, it is possible to suppress the deterioration of printability due to adhesion to the screen plate during printing, and to reduce the deterioration of handleability in the subsequent process due to the film sticking to the roll during transport. From the same viewpoint, the surface roughness Sa of the resin film is more preferably 200 nm or more, and particularly preferably 400 nm or more. In addition, in order to suppress the resin film satisfying conditions 1 and 2 from being torn when stretched, the surface roughness Sa of the resin film is preferably 5,000 nm or less.
[0031] In addition to the above viewpoint, from the viewpoint of reducing the electrical resistance of the electric circuit when the circuit is printed, the surface roughness Sa of the resin film is more preferably 1,000 nm or less.
[0032] That is, from the viewpoints of improving printability, suppressing breakage when stretched, and reducing electrical resistance when used as an electrical circuit, the surface roughness Sa of the resin film is preferably 150 nm or more and 5,000 nm or less, more preferably 200 nm or more and 1,000 nm or less, and particularly preferably 400 nm or more and 1,000 nm or less.
[0033] The storage modulus and loss tangent can be within the above ranges by adjusting the material and configuration of the resin film as described below. The surface roughness can be adjusted by including a particle layer as described below or by devising the manufacturing process as described below. A shape formation method using an imprint method with a micro mold can also be preferably used.
[0034] (Method of measuring storage modulus and loss tangent) The resin film was cut into a 10 mm wide rectangle to be used as the test piece. The storage modulus and loss tangent of the resin film were determined using a Seiko Instruments Inc. dynamic viscoelasticity measuring device DMS6100 based on the tensile vibration-non-resonance method (dynamic viscoelasticity method) of JIS K7244 (1998). Measurement mode: Tensile. -Chuck distance: 20mm. -Specimen width: 10mm. Frequency: 1Hz ·Distortion amplitude: 10μm. ·Minimum tension: 20mN. Initial force amplitude: 40mN. Measurement temperature: -100℃ to 200℃. Heating rate: 5℃ / min.
[0035] (Method of measuring surface roughness Sa) The surface roughness Sa of the resin film was measured under the following conditions using a non-contact surface shape measurement system "VertScan" (registered trademark) R550H-M100 manufactured by Ryoka Systems Co., Ltd. The arithmetic average value of five measurements was used as the surface roughness Sa. -Measurement mode: WAVE mode. -Objective lens: 50x. 0.5×Tube lens. ·Measurement area 187×139μm.
[0036] There is a preferred range for the surface properties of the resin film of the present invention. Specifically, the surface free energy of at least one surface of the resin film is preferably 25 mN / m or more, and more preferably 30 mN / m or more.
[0037] Here, the surface free energy of a resin film refers to a value obtained by determining the static contact angles of water, ethylene glycol, and diiodomethane at 25°C on the surface of the resin film, and introducing the static contact angles with each liquid and the dispersion term, polarity term, and hydrogen bond term of the surface free energy of each liquid described in Non-Patent Document 1 below into the "Extended Hawks Equation of Hata and Kitazaki" described in Non-Patent Document 2 below, and solving the simultaneous equations. The details of the measurement method will be described later. Non-Patent Document 1: J. Panzer: J. Colloid Interface Sci., 44, 142 (1973). Non-patent literature 2: Kitazaki, Y. and Hata, T.: Japan Adhesion Association Journal, 8, (3) 131 (1972).
[0038] By having a surface free energy of 25 mN / m or more on at least one surface of the resin film, the metal paste forming the circuit can have sufficient adhesion to the resin film surface, and when a circuit pattern is formed on the resin film and the resin film is repeatedly stretched, the decrease in the S / N ratio of the signal obtained from the sensor can be reduced, and further, the occurrence of poor conduction due to breakage of the circuit pattern can be suppressed. From the same viewpoint, it is more preferable that the surface free energy of at least one surface of the resin film is 30 mN / m or more.
[0039] The surface free energy can be adjusted to fall within the above range by appropriately selecting the material contained in the resin film and the surface treatment method, which will be described later.
[0040] (Method for measuring static contact angle) The static contact angle is measured after leaving the sample in an environment of 25°C for 12 hours. A Drop Master DM-501 manufactured by Kyowa Interface Science Co., Ltd. is used to create droplets, and conditions are selected to create droplets as small as possible without the droplets creeping up the needle. The static contact angle is calculated using an image taken 5 seconds after the droplets land on the resin film surface, using the θ / 2 method.
[0041] (Resin layer / particle layer) Moreover, the resin film of the present invention preferably has a resin layer containing segments of Chemical Formula 1 and Chemical Formula 2. By adopting this embodiment, the mechanical properties of the resin film can satisfy the above conditions 1 and 2.
[0042] [ka]
[0043] [ka]
[0044] Here, the segment of Chemical Formula 1 is a segment in which a (meth)acryloyl group is radically polymerized, that is, the resin film has a crosslink caused by polymerization of the (meth)acryloyl group, that is, a chemical crosslink. By having a chemical crosslink, it is possible to impart heat resistance to the resin film while maintaining its high flexibility and restorability. 1 R in Chemical Formula 1 represents a hydrogen or methyl group. 2 refers to one of the following: Substituted or unsubstituted alkylene groups. Substituted or unsubstituted arylene groups. An alkylene group having an internal ether, ester, or amide group. Arylene groups containing an internal ether, ester, or amide group. An unsubstituted alkylene group having an internal ether group, ester group, or amide group. An unsubstituted arylene group having an internal ether group, ester group, or amide group.
[0045] The segment of Chemical Formula 2 means a segment formed by a urethane bond. By having a urethane bond, a strong crosslinking reaction can be promoted in the resin film manufacturing method described later, even if the resin precursor has few crosslinking sites. 3 refers to one of the following: - a substituted or unsubstituted alkylene group, Substituted or unsubstituted arylene groups.
[0046] Whether the resin film has a resin layer containing the segment of Chemical Formula 1 or Chemical Formula 2 can be determined by various analytical methods, but a method using pyrolysis GC-MS is convenient. It can also be determined from the raw materials that form the resin film.
[0047] The resin film of the present invention preferably has a particle layer containing resin particles. Here, the particle layer is a layer consisting of particles and a resin component. By using resin particles as the particles, particles with a large particle size can be dispersed in the particle layer, and as a result, a preferable surface shape can be formed. In addition, since the resin particles can follow the elasticity of the resin film, by including resin particles in the particle layer, defects due to particle detachment during expansion and contraction can be suppressed, so that the resin film can have high elasticity that is comparable to that of a resin film without particles.
[0048] Here, the particle layer may also serve as the resin layer, but it is preferable that the particle layer and the resin layer are different layers from the viewpoint of improving the stretching characteristics. In particular, it is more preferable that the particle layer is provided on at least one surface of the resin film from the viewpoint of forming appropriate unevenness. In addition, from the viewpoint of satisfying the above-mentioned condition 1 and condition 2 regarding the mechanical properties of the resin film, it is preferable that the resin layer has a storage modulus of 0.5 MPa or more and 50 MPa or less at a temperature of 25° C. and a frequency of 1 Hz, and a loss tangent of 0.5 or less at a temperature of 25° C. and a frequency of 1 Hz, and more preferably contains segments of chemical formula 1 and chemical formula 2.
[0049] The method for setting the storage modulus and loss tangent of the resin layer within the above ranges is to combine one or more polymer polyols selected from polyester polyols, polyether polyols, and polycarbonate polyols with TDI (tolylene diisocyanate), MDI (4,4'-diphenylmethane diisocyanate), NDI (1,5-naphthalene diisocyanate), TODI (tolidine diisocyanate), XDI (xylylene diisocyanate), PPDI (paraphenylene diisocyanate), TMXDI (tetramethylxylylene diisocyanate), HMDI (hexamethylene diisocyanate), IPDI (isophorone diisocyanate), H6XDI (hydrogenated xylylene diisocyanate), H 12A method of reacting one or more bifunctional isocyanates selected from MDI (dicyclohexylmethane diisocyanate) with one or more acrylic raw materials selected from HEA (hydroxyethyl acrylate) and 4HBA (4-hydroxybutyl acrylate) at a molar ratio of 1: (1-2): (0.4-1.0) and polymerizing with heat or active energy rays can be preferably used. Here, when the amount of high molecular weight polyol is set to 1 in terms of the molar ratio of the feed, the amount of low molecular weight polyol having a molecular weight of 500 g / mol or less, such as 1,6-hexanediol, triethylene glycol, and 3-methyl-1,5-pentanediol, is preferably 0.1 or less. In addition, when the amount of bifunctional isocyanate is set to 1 in terms of the molar ratio of the feed, the amount of trifunctional or higher isocyanate is preferably 0.1 or less. In addition, the content of ash contained in 100% by mass of the resin layer is preferably 1% by mass or less. Here, ash content refers to the components when heated at 500°C for 1 hour under nitrogen.
[0050] In order to obtain a desired storage modulus and loss tangent for the resin layer, when the content of the monomer unit derived from the polymer polyol is taken as 1 mole, the content of the monomer unit derived from the bifunctional isocyanate is preferably 1 to 2 moles, the content of the monomer unit derived from the acrylic raw material is preferably 0.4 to 1.0 moles, the content of the monomer unit derived from the low molecular weight polyol is preferably 0.1 or less, and the content of the monomer unit derived from the trifunctional or higher isocyanate is preferably 0.2 moles or less. The qualitative and quantitative analysis of each monomer unit can be carried out by combining nuclear magnetic resonance spectroscopy, GC-MS, size exclusion chromatography, and time-of-flight mass spectrometry after alkaline hydrolysis of the resin layer.
[0051] The number average particle size of the resin particles contained in the particle layer is preferably 2 μm or more and 20 μm or less.
[0052] Here, the resin particles refer to particles entirely made of resin or particles whose surfaces are coated with resin. Details of the particles and resin particles will be described later.
[0053] The size of the resin particles contained in the particle layer is preferably a number average particle diameter of 2 μm or more and 20 μm or less, and more preferably a number average particle diameter of 4 μm or more and 10 μm or less, from the viewpoint of suppressing tackiness and suppressing the falling off of the resin particles. By having the size of the resin particles contained in the particle layer be 2 μm or more, the effect of suppressing surface tackiness can be sufficiently obtained. From the same viewpoint, the size of the resin particles contained in the particle layer is more preferably a number average particle diameter of 4 μm or more.
[0054] Furthermore, by making the size of the resin particles contained in the particle layer to be a number average particle diameter of 20 μm or less, it is possible to prevent the resin particles from falling off from the particle layer.
[0055] The size of the resin particles can be adjusted to the above range by appropriately selecting the material and particle size of the resin particles used, and the method for forming the particle layer.
[0056] The ratio of the resin and resin particles in the particle layer is preferably 10% by mass or more and 50% by mass or less with respect to 100% by mass of the entire particle layer. By having the ratio of the resin particles be 10% by mass or more, a preferable surface shape can be formed, and the effect of suppressing surface tackiness can be sufficiently obtained.
[0057] On the other hand, by making the proportion of resin particles in the particle layer 50% by mass or less, sufficient stretchability can be obtained when used in a resin film.
[0058] (Method for measuring number average particle size) The number average particle diameter of the resin particles contained in the particle layer is measured by observing the cross section of the resin film with a scanning electron microscope (SEM). The number average particle diameter is measured by observing at a magnification where the number of primary particles as an aggregate is 10 to 50 per visual field, calculating the diameter of the circumscribed circle of the primary particles from the obtained image, and using this as the equivalent particle diameter. The number of observations is increased and the number average particle diameter is calculated from the value measured for 100 primary particles.
[0059] The thickness of the particle layer is not particularly limited as long as the above-mentioned surface shape can be achieved, but is preferably 1 μm or more and 20 μm or less. In the case where a resin layer and a particle layer are provided from the viewpoint of improving the elasticity characteristics, the thickness of the resin layer is preferably 10 μm or more and 500 μm or less, and the thickness of the particle layer is preferably 1 μm or more and 25 μm or less. From the same viewpoint, the value of the thickness of the resin layer (μm) / the thickness of the particle layer (μm) is preferably 2 or more and 50 or less.
[0060] (Segments of chemical formulas 3 and 4) Furthermore, the particle layer preferably contains a segment of Chemical Formula 3, and more preferably contains a segment of Chemical Formula 3 and a segment of Chemical Formula 4.
[0061] [ka]
[0062] [ka]
[0063] Here, the segment of Chemical Formula 3 is preferably a polyolefin modified with maleic anhydride and / or a maleic anhydride-copolymerized polyolefin. R Y1 indicates one or more groups selected from a (meth)acrylic group, an epoxy group, a vinyl group, a phenyl group, and an amino group. R Y2 indicates one or more alkyl groups selected from alkyl groups having 1 to 4 carbon atoms.
[0064] The segment of Chemical Formula 4 is a polyalkoxysilane segment, that is, a hydrolysis condensation product of an alkoxysilane described in Compound Group 1 below.
[0065] (Compound Group 1) At least one alkoxysilane selected from the group consisting of (meth)acryloxyalkoxysilane, epoxyalkoxysilane, vinylalkoxysilane, phenylalkoxysilane, and aminoalkoxysilane.
[0066] An example of a hydrolysis condensation product is shown in chemical formula 4. Y1 R is a (meth)acrylic group, an epoxy group, a vinyl group, a phenyl group, an amino group, etc. Y2 is preferably one or more selected from alkyl groups having 1 to 4 carbon atoms. Y2 ) is partially hydrolyzed to form silanol groups (Si-OH), which then undergo silanol condensation to form siloxane bonds (Si-O-Si).
[0067] When the polyalkoxysilane is a hydrolysis condensate of an alkoxysilane described in the above-mentioned compound group 1, the affinity between the particle layer and the resin layer described below is increased, and the adhesion between the particle layer and the resin layer can be improved, and the adhesion when an electric circuit body is formed on the surface of the resin film can also be improved.
[0068] From the above viewpoint, the alkoxysilane is more preferably an aminoalkoxysilane among the above-mentioned compound group 1. Among them, as the amino group, a secondary amine is more preferable than a primary amine, and a phenylamine is particularly preferable.
[0069] Specific examples of alkoxysilanes include vinyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-acryloxypropyltrimethoxysilane, γ-aminopropyltriethoxysilane, 5-hexenyltrimethoxysilane, trifluoropropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, γ-glycidoxypropylmethyldiisopropenoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, phenyltrimethoxysilane, and phenyldimethoxysilane.
[0070] By including a segment of Chemical Formula 3 in the particle layer, the affinity between the particle layer and the resin layer is increased, and the adhesion between the particle layer and the resin layer can be improved, and the adhesion can also be improved when an electric circuit body is formed on the surface of the resin film. In addition, since those containing a segment of Chemical Formula 3 have excellent elasticity and excellent adhesion to resin particles, by including a segment of Chemical Formula 3 in the particle layer, problems caused by particle detachment during expansion and contraction can be suppressed, and the high expansion and contraction followability can improve the elasticity of the resin film. In particular, when the resin film has a resin layer and a particle layer on at least one surface, and the resin layer has a storage modulus of 0.5 MPa or more and 50 MPa or less at a temperature of 25°C and a frequency of 1 Hz, and a loss tangent of 0.5 or less at a temperature of 25°C and a frequency of 1 Hz, or when the resin layer contains segments of chemical formula 1 and chemical formula 2, it is difficult to obtain appropriate unevenness while following the expansion and contraction characteristics, and by using a particle layer containing a segment of chemical formula 3, it is possible to closely follow the expansion and contraction characteristics of the resin layer, and to suppress peeling of the resin layer and the particle layer during expansion and contraction, and to suppress detachment of the resin particles during expansion and contraction, and further to form appropriate surface unevenness. In addition, from the viewpoint of further improving adhesion, it is more preferable that the particle layer contains a segment of chemical formula 3 and a segment of chemical formula 4.
[0071] Whether the particle layer contains the segment of Chemical Formula 3 or the segment of Chemical Formula 4 can be determined by various analytical methods, but a method using pyrolysis GC-MS is convenient. It can also be determined from the raw materials that form the resin film.
[0072] From the above, a preferred embodiment of the resin film of the present invention is a resin film having a resin layer and a particle layer on at least one surface, the particle layer containing resin particles and a segment of chemical formula 3, the resin layer having a storage modulus of 0.5 MPa or more and 50 MPa or less at a temperature of 25 ° C and a frequency of 1 Hz, and a loss tangent of 0.5 or less at a temperature of 25 ° C and a frequency of 1 Hz. When the resin layer has the above mechanical properties, it was difficult to provide a particle layer that can follow the mechanical properties and elastic properties. Therefore, by adopting this embodiment, it is possible to suppress peeling between the resin layer and the particle layer and detachment of the resin particles from the particle layer when stretching, and further to form surface unevenness suitable for screen printing on the surface, and further to improve the elastic properties of the resin film. The resin layer, particle layer, resin particles, and surface state in this embodiment can be the same as the preferred embodiments described above, and the resin film in this embodiment can be preferably obtained by the method described later.
[0073] (Skewness Ssk) In addition, it is preferable that the skewness Ssk of at least one surface of the resin film of the present invention is -0.2 or more and 1.0 or less. When an adhesive layer is further provided on the resin film, it has been difficult to ensure adhesion to the adhesive layer while taking advantage of its elasticity. By setting the skewness Ssk within the above range, the anchoring property with the adhesive layer is improved and the adhesiveness can be increased. The surface having a skewness Ssk of -0.2 or more and 1.0 or less may be the same as the particle layer, but it is preferable that it is different from the viewpoint of functional separation.
[0074] Skewness Ssk represents the deviation of the height distribution from the average plane and indicates the symmetry of the peaks and valleys, Ssk=0 indicates that the height distribution is symmetrical from top to bottom and that there are equal amounts of peaks and valleys, Ssk>0 indicates that there are many fine peaks, and Ssk<0 indicates that there are many fine valleys. The following method can be preferably used to measure the skewness SsK of a resin film.
[0075] (Method of measuring skewness Ssk) The skewness Ssk is measured using a surface roughness meter (SURFCORDER ET4000A, manufactured by Kosaka Laboratory Co., Ltd.) under the following conditions. The arithmetic average value of five measurements is used as the skewness Ssk. Analysis equipment: 3D surface roughness analysis system (model TDA-31) Stylus: Tip radius 0.5μmR, diameter 2μm, made of diamond Needle pressure: 100μN X measurement length: 1.0mm X-feed speed: 0.1 mm / s (measurement speed) Y feed pitch: 5 μm (measurement interval) Number of Y lines: 81 (measured number) Z magnification: 2000x (vertical magnification) Low-frequency cutoff: 0.20 mm (swell cutoff value) High Cutoff: None Filter type: Gaussian spatial type Leveling: Yes (tilt correction) The method of making the skewness Ssk -0.2 or more and 1.0 or less can be preferably obtained by using the same segments and resin particles as the particle layer and appropriately adjusting the compounding ratio and particle shape. Specifically, a method of coating a coating composition for a particle layer, which is prepared by dispersing a solid content concentration of 20 mass% using an organic solvent at a compounding ratio such that one or more particles selected from melamine resin, (meth)acrylic resin, nylon resin, copolymerized nylon resin, styrene resin, polyolefin resin, olefin copolymer resin, (meth)acrylic resin-styrene resin copolymer, and urethane resin are contained in 15 mass% to 35 mass% of the entire particle layer 100 mass%, is preferably adopted. Here, the number average particle diameter of the particles is preferably 2 μm or more and 9 μm or less. In addition, a shape forming method by imprinting using a minute mold or shape transfer using a mold release film can also be preferably used. In addition, from the same viewpoint as above, the surface roughness Ra on a surface with a skewness Ssk of -0.2 or more and 1.0 or less is preferably 200 nm or more and 700 nm or less.
[0076] (Resin film / adhesive layer laminate) In addition, in the resin film-adhesive layer laminate of the present invention, the resin film and the adhesive layer are preferably in contact with each other. In particular, the resin film-adhesive layer laminate obtained by laminating a resin film having a skewness Ssk of -0.2 or more and 1.0 or less with an adhesive layer has high anchoring properties between the resin film and the adhesive layer, and can suppress peeling during expansion and contraction or during processing. Here, the adhesive layer refers to a layer having an adhesive strength of 3N / 20mm or more to a SUS304 plate at 23°C, a peeling speed of 300mm / min, and a peeling angle of 180°. From the viewpoint of suppressing peeling during expansion and contraction or during processing, the adhesive layer is preferably at least one selected from acrylic adhesives, urethane adhesives, rubber adhesives, and silicone adhesives, and more preferably at least one selected from acrylic adhesives and urethane adhesives.
[0077] [Mode of the present invention] Hereinafter, the embodiment of the present invention will be described in detail.
[0078] [Resin film] The resin film of the present invention is not particularly limited in the number of layers, as long as it has a film-like structure by itself, and may be formed from one layer or two or more layers. Here, the layer refers to a part that has a boundary surface that can be distinguished from adjacent parts in the thickness direction and has a finite thickness. More specifically, when the cross section of the resin film is observed with an electron microscope (transmission type, scanning type) or an optical microscope, it refers to a part that can be distinguished by the presence or absence of a discontinuous boundary surface. Even if the composition changes in the thickness direction of the resin film, if there is no boundary surface between them, it is treated as one layer.
[0079] The resin film of the present invention may have other functions such as fingerprint resistance, moldability, designability, scratch resistance, antifouling, antireflection, antistatic, electrical conductivity, heat reflection, near infrared absorption, electromagnetic wave shielding, etc., in addition to the flexibility, recovery property, printability, heat resistance, and adhesion, and in this case, one or more layers may be further formed. For example, a functional layer having the above-mentioned functions, an adhesive layer, an electronic circuit layer, a printing layer, an optical adjustment layer, or other functional layers may be provided.
[0080] The thickness of the resin film of the present invention is not particularly limited and is appropriately selected depending on the application. The lower limit of the thickness of the resin film is not generally determined because it is affected by the elastic modulus, breaking elongation, peeling force and peeling angle from the laminate, etc. of the resin film itself, but when the same physical properties as those of a general flexible material are realized using the resin film manufacturing method described later, the lower limit is about 10 μm.
[0081] [Particle layer] In the resin film of the present invention, it is important to give a specific surface shape. The method is not particularly limited, but it is preferable to have a particle layer on one side. As an example of the configuration of a resin film having a particle layer, as shown in FIG. 1, a particle layer 2 containing resin particles 3 is laminated on one side of a resin layer 7.
[0082] The surface layer is not particularly limited as long as it can obtain a specific shape. Although the particle layer may be formed directly on the resin layer, it is preferable to form the particle layer 2 in the state of the laminate 4 as shown in FIG. 2, and then peel off the support substrate 6 having the release layer 5 to obtain a resin film.
[0083] The particle layer is a layer containing particles and a resin component, and its thickness is not particularly limited as long as the above-mentioned surface shape can be achieved, but it is preferably 1 μm or more and 20 μm or less. The particles contained in the particle layer are preferably resin particles.
[0084] The resin particles are preferably resin particles containing at least one resin selected from the group consisting of melamine resin, (meth)acrylic resin, nylon resin, copolymer nylon resin, styrene resin, polyolefin resin, olefin copolymer resin, (meth)acrylic resin-styrene resin copolymer, and urethane resin, and from the viewpoint of maintaining sufficient restorability, particles made of urethane resin are particularly preferable. When a resin film has a resin layer and a particle layer on at least one surface, and the resin layer has a storage modulus of 0.5 MPa or more and 50 MPa or less at a temperature of 25°C and a frequency of 1 Hz, and a loss tangent of 0.5 or less at a temperature of 25°C and a frequency of 1 Hz, or the resin layer contains segments of chemical formula 1 and chemical formula 2, it is difficult to obtain appropriate unevenness while following the expansion and contraction characteristics, and by using a particle layer containing resin particles made of urethane resin, it is possible to closely follow the expansion and contraction characteristics of the resin layer, and to suppress peeling between the resin layer and the particle layer during expansion and contraction, and to suppress detachment of the resin particles during expansion and contraction, and further to form appropriate surface unevenness. Particles made of urethane resin correspond to the above-mentioned particles and have a segment of chemical formula 2.
[0085] As a method for achieving the above-mentioned state, the particle layer preferably contains 60% by mass or more and 90% by mass or less of maleic anhydride-modified polyolefin, 10% by mass or more and 40% by mass or less of urethane particles, and has a Si / C ratio of 0.01% by mass or more and 2% by mass or less as analyzed by X-ray photoelectron spectroscopy (XPS). The amount of acid modification of the maleic anhydride polyolefin is preferably 0.1% by mass or more and 3% by mass or less.
[0086] [Manufacturing method of resin film] The method for producing the resin film of the present invention is not particularly limited, but it is preferable to carry out the following steps in this order: applying a coating composition for a resin layer, which contains a resin precursor containing a segment of chemical formula 5 or 6, onto a support substrate having a release layer to form a coating layer (step 1); removing the solvent from the coating layer (step 2); irradiating with active energy rays to crosslink the resin precursor and form a laminate having a resin layer on the support substrate (step 3); and peeling the support substrate from the laminate to obtain a resin film (step 4).
[0087] [ka]
[0088] Here, R of the segment of formula 5 7 refers to hydrogen or a methyl group, and R 8 refers to one of the following: Substituted or unsubstituted alkylene groups. Substituted or unsubstituted arylene groups. An alkylene group having an internal ether, ester, or amide group. Arylene groups containing an internal ether, ester, or amide group. An unsubstituted alkylene group having an internal ether group, ester group, or amide group. An unsubstituted arylene group having an internal ether group, ester group, or amide group.
[0089] Further, R of the segment of formula 5 9refers to any of the following: Substituted or unsubstituted alkylene groups. Substituted or unsubstituted arylene groups.
[0090] [ka]
[0091] Here, R of the segment of formula 6 10 refers to hydrogen or a methyl group, and R 11 , R 13 refers to one of the following, where n is an integer of 3 or greater: Substituted or unsubstituted alkylene groups. Substituted or unsubstituted arylene groups. An alkylene group having an internal ether, ester, or amide group. Arylene groups containing an internal ether, ester, or amide group. An unsubstituted alkylene group having an internal ether group, ester group, or amide group. An unsubstituted arylene group having an internal ether group, ester group, or amide group.
[0092] Further, R of the segment of formula 6 12 refers to any of the following: Substituted or unsubstituted alkylene groups. Substituted or unsubstituted arylene groups.
[0093] The method of applying the resin layer coating composition onto the supporting substrate in step 1 is not particularly limited as long as the coating composition can be applied onto the supporting substrate to form a uniform coating layer in the plane. The coating method onto the film can be appropriately selected from dip coating, roller coating, wire bar coating, gravure coating, die coating (US Pat. No. 2,681,294), etc. Here, the coating layer refers to a "liquid layer" formed by the coating step.
[0094] The method for removing the solvent in step 2, i.e., the drying method, is not particularly limited as long as it can remove the solvent from the coating layer formed on the support substrate. Drying methods include heat transfer drying (contact with a high-heat object), convection heat transfer (hot air), radiation heat transfer (infrared rays), and others (microwaves, induction heating), and among these, in the manufacturing method of the present invention, a method using convection heat transfer or radiation heat transfer is preferred because it is necessary to precisely make the drying speed uniform even in the width direction.
[0095] In the crosslinking method of step 3, the coating layer from which the solvent has been removed after drying is irradiated with active energy rays to cause a reaction and crosslink the coating film. Crosslinking by active energy rays is preferably performed using electron beams (EB) and / or ultraviolet rays (UV) from the viewpoint of versatility. Examples of the types of ultraviolet lamps used for irradiating ultraviolet rays include discharge lamp type, flash type, laser type, and electrodeless lamp type. When ultraviolet curing is performed using a high-pressure mercury lamp that is a discharge lamp type, the illuminance of the ultraviolet rays is preferably 100 mW / cm. 2 More than 3,000mW / cm 2 Preferably less than 200 mW / cm 2 More than 2,000mW / cm 2 Less than 300mW / cm, more preferably 300mW / cm 2 More than 1,500mW / cm 2 It is recommended to irradiate ultraviolet rays under the following conditions: the integrated amount of ultraviolet rays is 100 mJ / cm 2 More than 3,000mJ / cm 2 Less than or equal to 200 mJ / cm is preferred, and more preferably 200 mJ / cm 2 More than 2,000mJ / cm 2 Less than 300 mJ / cm, more preferably 300 mJ / cm 2 More than 1,500mJ / cm 2It is recommended to perform ultraviolet irradiation under the following conditions. Here, ultraviolet illuminance is the irradiation intensity received per unit area, and varies depending on the lamp output, light emission spectral efficiency, diameter of the light emitting bulb, design of the reflector, and the distance between the irradiated object and the light source. However, illuminance does not vary depending on the transport speed. Also, the integrated ultraviolet light amount is the irradiation energy received per unit area, and is the total amount of photons that reach the surface. The integrated light amount is inversely proportional to the irradiation speed passing under the light source, and proportional to the number of irradiations and the number of lamps.
[0096] As described above, the resin film is preferably prepared by forming a laminate having a resin layer on one side of a supporting substrate, and then peeling off the supporting substrate to prepare the resin film. The structure of this laminate will be described with reference to the drawings.
[0097] As shown in Fig. 3, the laminate is preferably a laminate 9 having a resin layer 7 on a supporting substrate 8. Here, the supporting substrate is an article that is flat in the in-plane direction and on whose surface a coating composition for a resin layer can be spread, as described above, when a resin layer is provided on one surface of the supporting substrate in forming the laminate of the present invention.
[0098] The reason why it is preferable to first produce a laminate as a method for producing the resin film of the present invention is that using a production method in which a liquid coating composition is applied and crosslinked is preferable in terms of mechanical properties such as flexibility and resilience of the resin film, and when the resin film is subjected to post-processing such as printing or lamination, it is easier to handle if the processing is applied to the surface of the resin film while it is still in the form of a laminate with a supporting substrate attached.
[0099] Therefore, there is a preferred range for the peeling force when peeling the support substrate from the laminate, and in the laminate of the present invention, the peeling force between the support substrate and the resin layer is preferably 1N / 50mm or less, more preferably 800mN / 50mm or less. There is no particular lower limit for the peeling force between the support substrate and the resin layer, but if it is less than 10mN / 50mm, the support substrate and the resin layer may peel off or float during the manufacturing process, so the peeling force between the support substrate and the resin layer is preferably 10mN / 50mm or more. From the viewpoint of controlling the peeling force within the above range, it is preferable that the laminate 4 has a support substrate 6 including a release layer 5 between the resin layer 7 as shown in FIG. 4.
[0100] In order to give the surface of the resin film a specific shape, as shown in FIG. 2, a method of forming a particle layer 2 in the state of a laminate 4, and then peeling off a support substrate 6 having a release layer 5 to obtain a resin film can be suitably used. A specific method of producing a resin film is not particularly limited, but preferably, after the above-mentioned "step 3", a step of applying a coating composition for a particle layer containing particles and a resin component to form a coating layer (step A1), and a step of removing a solvent from the coating layer (step B1) are performed in this order, or after "step 3", a step of applying a coating composition for a particle layer containing particles and a resin precursor to form a coating layer (step A2), a step of removing a solvent from the coating layer (step B2), and a step of irradiating active energy rays to crosslink the resin precursor and form a laminate having a resin film on a support substrate (step C2) may be performed.
[0101] The method for producing the resin film of the present invention preferably includes a step of forming a particle layer by applying a coating composition for a particle layer containing resin particles having a number average particle diameter of 2 μm or more and 20 μm or less, from the viewpoint of forming a specific shape while suppressing variation.
[0102] In the method for producing a resin film of the present invention, the number average particle diameter of the resin particles is a value obtained by observation and measurement using a scanning electron microscope (SEM). The observed sample is prepared by diluting the coating composition for particle layer with a dispersion medium to a solid content concentration of 0.5% by mass, dispersing the mixture with ultrasonic waves, dropping the mixture onto a conductive tape, and drying the mixture. The number average particle diameter is measured by observing the particle layer at a magnification where the number of primary particle aggregates per field of view is 10 to 50, and the diameter of the circumscribed circle of the primary particles is calculated from the obtained image and used as the equivalent particle diameter. The number of observations is increased and the number average particle diameter is calculated from the value measured for 100 primary particles.
[0103] In addition, in order to give the surface of a resin film a specific shape, in addition to forming the above-mentioned particle layer on one side of the resin film as shown in Figure 2, it is also possible to use a method in which a laminate 11 is made using a supporting substrate 10 having an uneven surface and the supporting substrate 10 is peeled off from it as shown in Figure 5, or a method in which a laminate 15 is made using a supporting substrate 14 having a release layer 13 having an uneven surface and a resin layer 7 and the supporting substrate 14 is peeled off from it as shown in Figure 6.
[0104] The supporting substrate used in the above-mentioned laminate may be made of either a thermoplastic resin or a thermosetting resin, and may be a homoresin, a copolymer, or a blend of two or more types.
[0105] The support substrate may further contain various additives such as antioxidants, antistatic agents, crystal nucleating agents, inorganic particles, organic particles, viscosity reducing agents, heat stabilizers, lubricants, infrared absorbing agents, ultraviolet absorbing agents, doping agents for adjusting the refractive index, etc. The support substrate may be configured as a single layer or a multilayer, and there is no restriction on the total number of layers.
[0106] In addition, functional layers such as an easy-adhesion layer, an antistatic layer, an undercoat layer, an ultraviolet absorbing layer, and a release layer can be provided on the surface of the support substrate in advance, in addition to the resin film of the present invention. These functional layers may be formed before or after the surface treatment of the support substrate described below. The resin film of the present invention preferably has a release layer in order to control the peeling force between the support substrate and the resin film. Details of the release layer will be described later.
[0107] The surface of the supporting substrate may be subjected to various surface treatments before the resin film is formed. Examples of the surface treatments include chemical treatments, mechanical treatments such as sand matting and hairline, corona discharge treatment, flame treatment, ultraviolet irradiation treatment, high frequency treatment, glow discharge treatment, active plasma treatment, laser treatment, mixed acid treatment, and ozone oxidation treatment.
[0108] Among these, glow discharge treatment, ultraviolet irradiation treatment, corona discharge treatment, active plasma treatment and flame treatment are preferred from the viewpoint of ensuring adhesion of the functional layer to the supporting substrate, and sand matte, hairline and active plasma treatments are preferred from the viewpoint of imparting an uneven shape to the surface of the supporting substrate.
[0109] The support substrate used in the laminate is preferably one having a release layer, and the support substrate having a release layer is also called a release film. The release layer may be composed of a plurality of layers from the viewpoint of imparting adhesion of the release layer, antistatic property of the film, solvent resistance, etc., and may be present on both sides of the support substrate.
[0110] The composition and thickness of the release layer are not particularly limited as long as the peel strength from the resin film can be within the above-mentioned preferred range, but from the viewpoints of the in-plane uniformity, quality, and peel strength of the release layer, it is preferably 10 nm or more and 500 nm or less, and more preferably 20 nm or more and 300 nm or less. From the viewpoint of imparting an uneven shape to the surface of the supporting substrate, various particles may be added to the release layer.
[0111] Commercially available supporting substrates having a release layer include "Therapeel" (registered trademark) manufactured by Toray Film Processing Co., Ltd., "Unipeel" (registered trademark) manufactured by Unitika Ltd., "Panapeel" (registered trademark) manufactured by Panac Corporation, "Toyobo Ester" (registered trademark) manufactured by Toyobo Co., Ltd., and "Purex" (registered trademark) manufactured by Teijin Limited, and these products can also be used.
[0112] The laminate may have a protective material 18 on the surface opposite to the support substrate 8 of the resin layer, as shown in FIG. 7, to improve transportability in the resin layer process and prevent scratches. The protective material and the support substrate are distinguished by the fact that in the manufacturing method of the resin film, the one to which the resin layer coating composition is applied is the support substrate, and the one to which the resin layer is laminated after the resin layer is formed is the protective material. The protective material may be the same as or different from the support substrate described above, but it is preferable that the protective material has a difference in peel strength from the support substrate described above in the use of the subsequent process. The magnitude relationship between the peel strength of the protective material and the support substrate from the resin film is appropriately selected depending on the method of use in the subsequent process. Therefore, the protective material may have a release layer 21 as shown in FIG. 8, may have an adhesive layer 24 as shown in FIG. 9, or may not have a functional layer as shown in FIG. 10.
[0113] [Resin precursor] The resin precursor is not particularly limited as long as it is a compound having a site that can be crosslinked. A resin precursor containing a segment of Chemical Formula 5 is preferred, and a resin precursor containing a segment of Chemical Formula 6 is more preferred.
[0114] [ka]
[0115] Here, R of the segment of formula 5 7 refers to hydrogen or a methyl group, and R 8 refers to one of the following: Substituted or unsubstituted alkylene groups. Substituted or unsubstituted arylene groups. An alkylene group having an internal ether, ester, or amide group. Arylene groups containing an internal ether, ester, or amide group. An unsubstituted alkylene group having an internal ether group, ester group, or amide group. An unsubstituted arylene group having an internal ether group, ester group, or amide group.
[0116] Further, R of the segment of formula 5 9 refers to any of the following: Substituted or unsubstituted alkylene groups. Substituted or unsubstituted arylene groups.
[0117] [ka]
[0118] Here, R of the segment of formula 6 10 refers to hydrogen or a methyl group, and R 11 , R 13 refers to one of the following, where n is an integer of 3 or greater: Substituted or unsubstituted alkylene groups. Substituted or unsubstituted arylene groups. An alkylene group having an internal ether, ester, or amide group. Arylene groups containing an internal ether, ester, or amide group. An unsubstituted alkylene group having an internal ether group, ester group, or amide group. An unsubstituted arylene group having an internal ether group, ester group, or amide group.
[0119] Further, R of the segment of formula 6 12 refers to any of the following: Substituted or unsubstituted alkylene groups. Substituted or unsubstituted arylene groups.
[0120] As described above, the segment of Chemical Formula 5 has a (meth)acrylic group represented by X in the formula at its terminal, and this (meth)acrylic group (X) at the terminal corresponds to a site that can be crosslinked. Furthermore, the (meth)acrylic group (X) is adjacent to the urethane bond represented by Y via a linker. Furthermore, the segment of Chemical Formula 6 means that the other end of the urethane bond of the polyisocyanate residue represented by Y is adjacent to the polyol residue (Z) represented by Z in Chemical Formula 6.
[0121] The urethane bond (Y) in Chemical Formula 5 and Chemical Formula 6 is preferably selected from the group consisting of TDI (tolylene diisocyanate), MDI (4,4'-diphenylmethane diisocyanate), NDI (1,5-naphthalene diisocyanate), TODI (tolidine diisocyanate), XDI (xylylene diisocyanate), PPDI (paraphenylene diisocyanate), TMXDI (tetramethylxylylene diisocyanate), HMDI (hexamethylene diisocyanate), IPDI (isophorone diisocyanate), H6XDI (hydrogenated xylylene diisocyanate), H 12 It is a residue of a polyisocyanate such as MDI (dicyclohexylmethane diisocyanate). The polyol residue represented by Z in Chemical Formula 6 preferably includes polyester polyol, polyether polyol, and polycarbonate polyol.
[0122] [Paint composition] The coating composition for the resin layer and the coating composition for the particle layer used in the above-mentioned resin film manufacturing method are not particularly limited as long as they can be uniformly applied on the support substrate or on the resin layer and can form a resin film exhibiting the characteristics of the present invention, but it is preferable that they are coating compositions suitable for the above-mentioned resin film manufacturing method. Specifically, it is preferable to add the above-mentioned resin precursor or resin component to the solvent and other components described later to prepare a coating composition.
[0123] [Method for forming a particle layer including particles made of urethane resin and including a segment of Chemical Formula 3] A particle layer containing particles made of urethane resin and containing a segment of Chemical Formula 3 can be formed by applying a coating composition obtained by mixing maleic anhydride modified polyolefin, a solvent, and particles made of urethane resin as a coating composition for the particle layer. In addition, by adding an alkoxysilane described in the above compound group 1 to the coating composition for the particle layer, a particle layer containing a segment of Chemical Formula 4 can be formed.
[0124] [solvent] The coating composition used in the above-mentioned resin film manufacturing method may contain a solvent, and it is preferable to contain a solvent in order to form a coating layer uniformly in the plane. The number of types of solvents is preferably 1 to 20, more preferably 1 to 10, even more preferably 1 to 6, and particularly preferably 1 to 4. Here, the term "solvent" refers to a substance that is liquid at room temperature and normal pressure and can be evaporated almost entirely in the above-mentioned drying process.
[0125] Here, the type of solvent is determined by the molecular structure that constitutes the solvent. In other words, solvents that have the same elemental composition and the same type and number of functional groups but different bond relationships (structural isomers), and solvents that are not structural isomers but do not overlap exactly in any conformation in three-dimensional space (stereoisomers) are treated as different types of solvents. For example, 2-propanol and n-propanol are treated as different solvents.
[0126] [Other components in the coating composition] The coating composition used in the above-mentioned method for producing a resin film preferably contains an antioxidant, a polymerization initiator, a curing agent, and a catalyst. The polymerization initiator and catalyst are used to promote crosslinking of the resin film. The polymerization initiator is preferably one that can initiate or promote polymerization, condensation, or crosslinking reaction of the components contained in the coating composition by anionic, cationic, or radical polymerization reaction, etc.
[0127] Antioxidants are broadly classified into radical chain initiation inhibitors, radical scavengers, and peroxide decomposers based on their mechanism of action. Any of these can achieve the effect of the present invention in terms of inhibiting deterioration under high temperature conditions, which is the subject of the present invention. However, radical scavengers or peroxide decomposers are more preferred, and hindered phenol-based and semi-hindered phenol-based radical scavengers, and phosphite-based and thioether-based peroxide decomposers are particularly preferred.
[0128] Various polymerization initiators, curing agents, and catalysts can be used. The polymerization initiators, curing agents, and catalysts may be used alone, or a plurality of polymerization initiators, curing agents, and catalysts may be used simultaneously. Furthermore, an acid catalyst or a thermal polymerization initiator may be used in combination. Examples of the acid catalyst include an aqueous hydrochloric acid solution, formic acid, and acetic acid. Examples of the thermal polymerization initiator include peroxides and azo compounds. Examples of the photopolymerization initiator include alkylphenone compounds, sulfur-containing compounds, acylphosphine oxide compounds, and amine compounds. Examples of the crosslinking catalyst that promotes the reaction of forming a urethane bond include dibutyltin dilaurate and dibutyltin diethylhexoate.
[0129] As the photopolymerization initiator, an alkylphenone compound is preferable from the viewpoint of curability. Specific examples of the alkylphenone compound include 1-hydroxy-cyclohexyl-phenyl-ketone, 2,2-dimethoxy-1,2-diphenylethane-1-one, 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-phenyl)-1-butane, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-(4-phenyl)-1-butane, 2-benzyl-2-dimethylamino-1-(4- morpholinophenyl)-1-butane, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butane, 1-cyclohexyl-phenyl ketone, 2-methyl-1-phenylpropan-1-one, 1-[4-(2-ethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, bis(2-phenyl-2-oxoacetate)oxybisethylene, and polymerized versions of these materials.
[0130] In addition, a leveling agent, a lubricant, an antistatic agent, etc. may be added to the coating composition used to form the resin film as long as the effects of the present invention are not impaired. As a result, the resin film can contain a leveling agent, a lubricant, an antistatic agent, etc.
[0131] Examples of the leveling agent include acrylic copolymers, silicone-based, and fluorine-based leveling agents. Examples of the antistatic agent include metal salts such as lithium salts, sodium salts, potassium salts, rubidium salts, cesium salts, magnesium salts, and calcium salts.
[0132] [Application] The resin film or resin film / adhesive layer of the present invention has high flexibility and recovery, and can be suitably used in applications requiring various post-processing processes. For example, the resin film or resin film / adhesive layer of the present invention is used in an electric circuit, a health care sensor, or a wearable sensor. As another example, the resin film or resin film / adhesive layer of the present invention can be suitably used in a wearable device, a stretchable sensor for a health care device, or a stretchable actuator.
[0133] In addition, from the viewpoint of high flexibility and resilience, the composition can be suitably used as a surface material, internal material, constituent material, or manufacturing process material for a variety of products that require resilience, such as a substrate for an adhesive tape, an impact absorbing material for a display, a substrate for a medical film, a substrate for a surface protection film for an automobile, and a core material for a pressure sensor.
[0134] [Electrical circuit body] The electric circuit body of the present invention is not particularly limited as long as it is a body in which a conductor circuit is formed on at least one surface of the resin film of the above-mentioned resin film or resin film-adhesive layer laminate. An example of the configuration of the electric circuit body will be described with reference to FIG. 11. In the electric circuit body 27, an electric circuit 29 is formed on a resin film 28. There is no particular limitation on the method for forming the electric circuit, and a general method for forming a flexible printed circuit board (FPC) or a screen printing method may be used.
[0135] [Healthcare sensor] The healthcare sensor of the present invention is not particularly limited as long as a conductor circuit is formed on at least one surface of the resin film of the aforementioned resin film or resin film-adhesive layer laminate. The healthcare sensor of the present invention refers to a sensor that is directly attached to a living body to continuously record biological information such as respiratory rate, heart rate, body temperature, blood pressure, electrocardiogram, and brain wave, for the purpose of maintaining health and improving the quality of medical care, and a device using the sensor.
[0136] An example of a method for manufacturing a health care sensor will be described. After printing a paste (LS-453-6B, manufactured by Asahi Chemical Laboratory Co., Ltd.) on a resin film to form electrodes, an overcoat agent (CR-120T, manufactured by Asahi Chemical Laboratory Co., Ltd.) for protecting the electrodes was printed, leaving two exposed electrode parts. Next, one exposed electrode part was connected to an electrocardiogram recorder (EV-301, manufactured by Parama Tech Co., Ltd.), the other exposed electrode part was brought into contact with the chest, and the sensor was attached to a living body using adhesive tape (9917, manufactured by 3M Japan Co., Ltd.), thereby manufacturing a health care sensor for measuring electrocardiograms.
[0137] [Wearable sensors] The wearable sensor of the present invention is not particularly limited as long as a conductor circuit is formed on at least one surface of the resin film of the aforementioned resin film or resin film-adhesive layer laminate. The wearable sensor of the present invention refers to medical and health devices such as the aforementioned health care sensor, as well as devices such as atmospheric pressure sensors, temperature sensors, acceleration sensors, and strain sensors, sensors that continuously record various data in the fields of fitness and sports, and devices using them.
[0138] An example of a manufacturing method for a wearable sensor will be described. A paste (LS-453-6B, manufactured by Asahi Chemical Laboratory Co., Ltd.) and an overcoat agent (CR-120T, manufactured by Asahi Chemical Laboratory Co., Ltd.) were printed on both sides of a resin film in that order to form electrodes, and then the electrodes were connected to a data logger (NR-500, manufactured by Keyence Corporation). Next, a wearable sensor can be manufactured by attaching an adhesive tape (1504XL, manufactured by 3M Japan Co., Ltd.) to one side of the resin film on which the electrodes were printed, and by attaching it to the elbow, it can be used as a wearable sensor for a strain sensor.
[0139] [Manufacturing method for resin film processed products] A preferred embodiment of the method for producing a resin film product of the present invention includes a step of processing the resin film side of the resin film of the present invention or the resin film-adhesive layer laminate of the present invention by screen printing. Since the resin film of the present invention does not easily stick to the screen printing plate, a resin film product having excellent stretchability can be efficiently obtained. EXAMPLES
[0140] Next, the present invention will be described based on examples, but the present invention is not necessarily limited to these.
[0141] [Examples 1 to 35, Comparative Examples 1 to 6] "Synthesis of resin precursors" In the synthesis of the resin precursor, the raw materials used are as follows: ·IPDI: Isophorone diisocyanate. ·MDI: 4,4'-diphenylmethane diisocyanate. · MPDAA: Poly(3-methylpentanediol adipate) Kuraray Polyol P-2010 (weight average molecular weight 2,000) manufactured by Kuraray Co., Ltd. · PBAA-1: Polybutylene adipate "Nippolan" (registered trademark) 3027 (weight average molecular weight 2,500) manufactured by Tosoh Corporation. · PTMG: Polytetramethylene glycol PTMG2000 (weight average molecular weight 2,000) manufactured by Mitsubishi Chemical Corporation. · PEAA: Polyethylene glycol adipate "Nippolan" (registered trademark) 4040 (weight average molecular weight 2,000) manufactured by Tosoh Corporation. ·HEA: Hydroxyethyl acrylate. ·4HBA: 4-Hydroxybutyl acrylate.
[0142] [Resin precursor 1] In a four-neck flask equipped with a thermometer, a stirrer, a water-cooled condenser, and a nitrogen gas inlet, IPDI as a diisocyanate, MPDAA as a polyol, and toluene were placed. At this time, the molar ratio of diisocyanate to polyol was set to 0.43:0.29, and the solid content concentration was set to 60 mass%. The reaction was performed at 90°C, and when the remaining isocyanate group in the unreacted state was set to 100 mass%, the temperature was lowered to 70°C when the remaining isocyanate group became 1.4 mass% by reaction, and HEA was added as a hydroxyacrylate. At this time, the molar ratio of diisocyanate to polyol to hydroxyacrylate in the unreacted state was set to 0.43:0.29:0.29. When the amount of remaining isocyanate groups before reaction was taken as 100% by mass, the reaction was terminated by stopping heating when the amount of remaining isocyanate groups reached 0.3% by mass. Toluene was then added to adjust the solids concentration to 60% by mass, thereby obtaining a toluene solution of resin precursor 1.
[0143] [Resin precursors 2-8] Toluene solutions of resin precursors 2 to 8 were synthesized in the same manner as in the synthesis of resin precursor 1, except that the combination of diisocyanate, polyol, and hydroxyacrylate and the molar ratio of each component when unreacted were changed to the combination and molar ratio shown in Table 1.
[0144] [Resin A] 0.22 mol% PTMG, 0.50 mol% MDI, 0.25 mol% BD, and 0.03 mol% 3-methyl-1,5-pentanediol were continuously fed in a liquid state under heating all at once using a metering pump to a twin-screw extruder (L / D=34; φ=30 mm) and polymerized at 260°C to obtain resin A.
[0145] [Table 1]
[0146] "Formulation of coating composition for resin layer" [Coating composition 1 for resin layer] Using the following materials and methyl ethyl ketone, a resin layer coating composition 1 having a solid content concentration of 40 mass % was obtained. Resin precursor 1 toluene solution (solid content concentration 60% by mass): 100 parts by mass. Photopolymerization initiator “IRGACURE” (registered trademark) 184 (manufactured by BASF Japan Ltd.): 1.5 parts by mass. Fluorine-based leveling agent “Ftergent” (registered trademark) 650AC (manufactured by NEOS Corporation): 0.03 parts by mass.
[0147] [Coating composition for resin layer 2-4, 8, 9, 11, 12] Resin layer coating compositions 2 to 4, 8, 9, 11, and 12 were prepared in the same manner as in the preparation of the resin layer coating composition 1, except that resin precursor 1 was replaced with the combination of resin precursors shown in Table 2.
[0148] [Table 2]
[0149] [Coating composition 5 for resin layer] Using the following materials and toluene, a resin layer coating composition 5 having a solid content concentration of 40 mass % was obtained. Styrene-ethylene / butylene-styrene block polymer “Kraton” (registered trademark) G1643 (manufactured by Kraton Polymer Japan Co., Ltd.): 80 parts by mass. Tricyclodecane dimethanol diacrylate A-DCP (manufactured by Shin-Nakamura Chemical Co., Ltd.): 20 parts by mass. Photopolymerization initiator “IRGACURE” (registered trademark) 184 (manufactured by BASF Japan Ltd.): 1.5 parts by mass. Fluorine-based leveling agent “Ftergent” (registered trademark) 650AC (manufactured by NEOS Corporation): 0.03 parts by mass.
[0150] [Coating composition 6 for resin layer] A 500 ml flask equipped with a stirrer, thermometer, condenser, and nitrogen gas inlet tube was charged with 106 parts by mass of ethanol, 270 parts by mass of methyltrimethoxysilane, 23 parts by mass of γ-methacryloxypropylmethyldimethoxysilane, 100 parts by mass of deionized water, 1 part by mass of 1% by mass hydrochloric acid, and 0.1 parts by mass of hydroquinone monomethyl ether, and reacted at 80° C. for 3 hours to synthesize polysiloxane a. This was adjusted to a solids concentration of 50% by mass with methyl isobutyl ketone.
[0151] Next, using the same apparatus as in the synthesis of polysiloxane a, 50 parts by mass of toluene, 50 parts by mass of methyl isobutyl ketone, 20 parts by mass of a polydimethylsiloxane-based polymer polymerization initiator (Wako Pure Chemical Industries, Ltd., VPS-0501), 18 parts by mass of methyl methacrylate, 38 parts by mass of butyl methacrylate, 23 parts by mass of 2-hydroxyethyl methacrylate, 1 part by mass of methacrylic acid, and 0.5 parts by mass of 1-thioglycerin were charged and reacted at 180°C for 8 hours to obtain a polydimethylsiloxane-based block copolymer a. The obtained block copolymer was adjusted to a solid content concentration of 50% by mass with methyl isobutyl ketone.
[0152] Using the following materials and methyl ethyl ketone, a resin layer coating composition 6 having a solid content concentration of 40 mass % was obtained. Polydimethylsiloxane block copolymer a: 75 parts by mass. Polysiloxane a: 10 parts by mass. Hydroxyl group-containing polycaprolactone triol "Placel" (registered trademark) 308 (manufactured by Daicel Chemical Industries, Ltd., weight average molecular weight 850): 15 parts by mass. Isocyanurate of hexamethylene diisocyanate “Takenate” (registered trademark) D-170N (manufactured by Takeda Pharmaceutical Co., Ltd.): 25 parts by mass.
[0153] [Coating composition for resin layer 7] Into a 300 mL separable flask equipped with a cooling tube and a stirring blade and purged with argon gas, 74.7 g (252 mmol) of octamethylcyclotetrasiloxane and 0.1 g of potassium siliconate were placed, and the temperature was raised to 120° C. and stirred for 30 minutes. The temperature was then raised to 155° C. and stirring was continued for 3 hours. After 3 hours, 0.1 g (0.6 mmol) of 1,3-divinyltetramethyldisiloxane was added, and the mixture was further stirred at 155° C. for 4 hours.
[0154] After 4 hours, the mixture was diluted with 250 mL of toluene and washed three times with water. The washed organic layer was washed several times with 1.5 L of methanol for reprecipitation purification, and the oligomer and polymer were separated. The resulting polymer was dried overnight at 60°C under reduced pressure to obtain vinyl group-containing linear organopolysiloxane A1.
[0155] Vinyl-containing linear organopolysiloxane A2 was synthesized in the same manner as in the synthesis process of vinyl-containing linear organopolysiloxane A1, except that in addition to 74.7 g (252 mmol) of octamethylcyclotetrasiloxane, 0.86 g (2.5 mmol) of 2,4,6,8-tetramethyl-2,4,6,8-tetravinylcyclotetrasiloxane was used.
[0156] The following materials were mixed together to obtain silicone rubber compound 1. Vinyl-containing organopolysiloxane A1: 72 parts by mass. Vinyl-containing organopolysiloxane A2: 18 parts by mass. Hexamethyldisilazane SIH6110.1 (Gelest): 10 parts by mass. Divinyltetramethyldisilazane SID4612.0 (manufactured by Gelest): 0.5 parts by mass. Deionized water: 5.25 parts by weight.
[0157] Then, 25 parts by mass of silica particles "AEROSIL" (registered trademark) 300 (manufactured by Nippon Aerosil Co., Ltd.) were added to 100 parts by mass of silicone rubber compound 1, and the mixture was kneaded for 1 hour at 60 to 90°C in a nitrogen atmosphere in the first step for a coupling reaction, and for 2 hours at 160 to 180°C in a reduced pressure atmosphere in the second step for removing the by-product (ammonia). The mixture was then cooled, and 8 parts by mass of vinyl group-containing organopolysiloxane A1 and 2 parts by mass of vinyl group-containing organopolysiloxane were added and kneaded for 20 minutes to obtain silicone rubber compound 2.
[0158] Subsequently, the mixture was diluted with the following materials and toluene to obtain a resin layer coating composition 7 having a solid content concentration of 30 mass %. Silicone rubber compound 2: 100 parts by mass. Organohydrogenpolysiloxane 88466 (manufactured by Momentive Corporation: 0.35 parts by mass. Platinum catalyst SIP6831.2 (Gelest): 0.05 parts by mass. Reaction inhibitor (1-ethynyl-1-cyclohexanol): 0.1 parts by mass.
[0159] [Coating composition 10 for resin layer] While stirring the cooled toluene, pellet-shaped resin A was added so that the solids concentration was 20% by mass. After confirming that the solution had become transparent, the temperature was raised to 70°C to completely dissolve the resin, and coating composition 18 was obtained.
[0160] "Formulation of coating composition for particle layer" In formulating the particle coating composition, the raw materials used are as follows: Resin precursor 1 Resin B: Acid-modified SEBS-B: “Tuftec” (registered trademark) M1911 (manufactured by Asahi Kasei Corporation), maleic anhydride-modified SEBS, hydrogenation rate 100%, styrene monomer content of hydrogenated product (hydrogenated) before acid modification 30 mass%, Mw of hydrogenated product (Z) 100,000, acid modification amount 0.2 mass%. Resin C: acid-modified ethylene-α-olefin copolymer "AMPLIFIE" (registered trademark) GR216 (manufactured by Dow Chemical), maleic anhydride-modified ethylene-α-olefin copolymer, acid modification amount 0.5 mass %. Photoinitiator: “OMNIRAD” (registered trademark) 184 (manufactured by IGM RESINS BV). Additive 1: Fluorine-based leveling agent "Futergent" (registered trademark) 650AC (manufactured by Neos Corporation, active ingredient 30% by mass). Additive 2: Fluorine-based leveling agent "Futergent" (registered trademark) 610FM (manufactured by Neos Corporation, active ingredient 50% by mass). Additive 3: Fluorine-based leveling agent "Futergent" (registered trademark) 710FM (manufactured by Neos Corporation, active ingredient 50% by mass). Additive 4: Fluorine-based leveling agent "Futergent" (registered trademark) 212M (manufactured by Neos Corporation, 100% active ingredient by mass). Resin particle 1: Urethane particle “Art Pearl” (registered trademark) C-800 transparent (manufactured by Negami Chemical Industrial Co., Ltd., active ingredient 100% by mass). Resin particle 2: Urethane particle “Art Pearl” (registered trademark) C-1000 transparent (manufactured by Negami Chemical Industrial Co., Ltd., active ingredient 100% by mass). Resin particle 4: Acrylic particle “Art Pearl” (registered trademark) G-800 transparent (manufactured by Negami Chemical Industrial Co., Ltd., active ingredient 100% by mass). · Alkoxysilane 1: 3-methacryloxypropyltrimethoxysilane KBM-503 (Shin-Etsu Chemical Co., Ltd.). · Alkoxysilane 2:3-glycidopropyltrimethoxysilane KBM-403 (Shin-Etsu Chemical Co., Ltd.). · Alkoxysilane 3: Vinyltrimethoxysilane KBM-1003 (manufactured by Shin-Etsu Chemical Co., Ltd.). · Alkoxysilane 4: Phenyltrimethoxysilane KBM-103 (Shin-Etsu Chemical Co., Ltd.). · Alkoxysilane 5: 3-aminopropyltrimethoxysilane KBM-903 (Shin-Etsu Chemical Co., Ltd.). · Alkoxysilane 6: Bis(3-trimethoxysilylpropyl)amine “Dynasylan” (registered trademark) 1124 (manufactured by Evonik Japan Co., Ltd.). · Alkoxysilane 7: N-phenyl-3-aminopropyltrimethoxysilane KBM-573 (Shin-Etsu Chemical Co., Ltd.).
[0161] [Coating composition 1 for particle layer] Using the following materials and methyl ethyl ketone, a coating composition 1 for a particle layer having a solid content concentration of 20 mass % was obtained. Resin precursor 1: 80 parts by mass. ·Resin particles 1: 20 parts by mass. Additive 1: 0.03 parts by mass. Photopolymerization initiator: 0.02 parts by mass.
[0162] [Coating composition 2-6 for particle layer] Coating compositions 2 to 6 for particle layer were prepared in the same manner as in the preparation of coating composition 1 for resin layer, except that the combinations of the types and amounts of particles and additives shown in Table 3 were changed.
[0163] [Coating composition for particle layer 7] The following materials were diluted with toluene to obtain coating composition 7 for particle layer having a solid content concentration of 20 mass %. ·Resin A: 80 parts by mass. ·Resin particles 1: 20 parts by mass. Additive 1: 0.03 parts by mass.
[0164] [Coating composition for particle layer 8] The following materials were diluted with toluene to obtain coating composition 8 for particle layer having a solid content concentration of 20 mass %. ·Resin B: 80 parts by mass. ·Resin particles 1: 20 parts by mass. Additive 1: 0.03 parts by mass.
[0165] [Coating composition for particle layer 9] The following materials were diluted with toluene to obtain coating composition 9 for particle layer having a solid content concentration of 20 mass %. ·Resin B: 80 parts by mass. ·Resin particles 1: 20 parts by mass. Additive 1: 0.03 parts by mass. · Alkoxysilane 1: 1 part by mass.
[0166] [Coating composition for particle layer 10-20] Coating compositions 10 to 20 for particle layer were prepared in the same manner as in the preparation of coating composition 9 for resin layer, except that the combinations of the types and amounts of particles, additives, and alkoxysilane were changed to those shown in Table 3.
[0167] [Table 3]
[0168] "Formulation of coating composition for release layer" In preparing the coating composition for the release layer, the raw materials used are as follows: · Alkyd compound 1: Acrylic modified alkyd resin Hariftal KV-905 (manufactured by Harima Chemicals Co., Ltd., solid content concentration 53% by mass). Melamine compound 1: isobutyl alcohol modified melamine resin “Melan” (registered trademark) 2650L (manufactured by Hitachi Chemical Co., Ltd., solid content concentration 60% by mass). Silicone compound 1: Side-chain modified reaction type silicone oil KF-6123 (Shin-Etsu Chemical Co., Ltd., active ingredient 100% by mass). Resin particles 3: Acrylic particles “Art Pearl” (registered trademark) J-5P (manufactured by Negami Chemical Industrial Co., Ltd., active ingredient 100% by mass).
[0169] [Release layer coating composition 1] The following materials were mixed and diluted with a mixed solvent of methyl ethyl ketone / isopropyl alcohol (mixture ratio by mass: 50 / 50) to obtain coating composition 1 for a release layer having a solid content concentration of 5 mass %. ·Alkyd compound 1: 100 parts by mass. Melamine compound 1: 20 parts by weight. Paratoluenesulfonic acid: 5 parts by mass. Silicone compound 1: 5 parts by weight.
[0170] [Release layer coating composition 2] The following materials were mixed and diluted with a mixed solvent of methyl ethyl ketone / isopropyl alcohol (mixture ratio by mass: 50 / 50) to obtain coating composition 2 for a release layer having a solids concentration of 5 mass %. ·Alkyd compound 1: 100 parts by mass. Melamine compound 1: 20 parts by weight. Paratoluenesulfonic acid: 5 parts by mass. Silicone compound 1: 5 parts by weight. ·Resin particles 3: 10 parts by mass.
[0171] [Release layer coating composition 3] The following materials were mixed and diluted with a mixed solvent of methyl ethyl ketone / isopropyl alcohol (mixture ratio by mass: 50 / 50) to obtain coating composition 3 for a release layer having a solids concentration of 5% by mass. ·Alkyd compound 1: 100 parts by mass. Melamine compound 1: 20 parts by weight. Paratoluenesulfonic acid: 5 parts by mass. Silicone compound 1: 5 parts by weight. ·Resin particles 3: 20 parts by mass.
[0172] [Support base material] The supporting substrate used in the production of the resin film is as follows. Support substrate 1: Toray Industries, Inc.'s "Lumirror" (registered trademark) U48 50 μm. Support substrate 2: Toray Industries, Inc.'s "Lumirror" (registered trademark) X42 50 μm. Support substrate 3: Toray Industries, Inc.'s "Lumirror" (registered trademark) T60 50 μm, which was sandblasted.
[0173] [Formation of release layer] Using a coating device with a small diameter gravure coater, a combination of the support substrate and the coating composition for the release layer shown in Tables 4 and 5 was used, and the gravure roll line count, the gravure roll peripheral speed, and the solids concentration of the coating composition for the release layer were adjusted so that the release layer had a thickness of 200 nm. The coating was then dried and crosslinked by holding the substrate at a hot air temperature of 140°C for 30 seconds, thereby forming a release layer.
[0174] [Formation of resin layer] A resin layer was formed on the release layer prepared on the support substrate in the previous section by using the above-mentioned resin layer coating composition in combination with the resin layer formation method described below in the combinations shown in Tables 4 and 5.
[0175] [Method 1 for forming resin layer] In step 1, the above-mentioned resin layer coating composition was applied to the release layer side of the support substrate using a continuous coating device such as a slot die coater, with the discharge flow rate adjusted so that the thickness of the resin layer after crosslinking would be the specified film thickness, thereby forming a coating layer.
[0176] In step 2, the coating layer formed in step 1 was dried under the following conditions to remove the solvent. ·Blow temperature: Temperature: 80℃. ·Wind speed: Application side: 5m / sec, non-application side: 5m / sec. Air direction: coated side: parallel to the surface of the substrate, non-coated side: perpendicular to the surface of the substrate. Residence time: 2 minutes.
[0177] In step 3, the coating layer (uncrosslinked resin layer) obtained by removing the solvent was irradiated with active energy rays under the following conditions to crosslink the layer, thereby obtaining a resin layer and a laminate. · Light source: High pressure mercury lamp. Radiation output: 400W / cm 2 . Accumulated light output: 120mJ / cm 2 . Oxygen concentration: 0.1% by volume.
[0178] [Method 2 for forming resin layer] In step 1, the above-mentioned resin layer coating composition was applied to the release layer side of the support substrate using a continuous coating device such as a slot die coater, with the discharge flow rate adjusted so that the thickness of the resin layer after crosslinking would be the specified film thickness, thereby forming a coating layer.
[0179] In step 2, the coating layer formed in step 1 was dried under the following conditions to remove the solvent. ·Blow temperature: Temperature: 120℃. ·Wind speed: Application side: 5m / sec, non-application side: 5m / sec. Air direction: coated side: parallel to the surface of the substrate, non-coated side: perpendicular to the surface of the substrate. Residence time: 2 minutes.
[0180] In step 3, the coating layer obtained by removing the solvent in step 2 was heated at 40° C. for 2 days to be crosslinked to form a resin layer, thereby obtaining a laminate.
[0181] [Method 3 for forming resin layer] In step 1, the above-mentioned resin layer coating composition was applied to the release layer side of the support substrate using a continuous coating device such as a slot die coater, with the discharge flow rate adjusted so that the thickness of the resin layer after crosslinking would be the specified film thickness, thereby forming a coating layer.
[0182] In step 2, the coating layer formed in step 1 was dried under the following conditions to remove the solvent. ·Blow temperature: Temperature: 80℃. ·Wind speed: Application side: 5m / sec, non-application side: 5m / sec. Air direction: coated side: parallel to the surface of the substrate, non-coated side: perpendicular to the surface of the substrate. Residence time: 2 minutes.
[0183] In step 3, the coating layer (uncrosslinked resin layer) obtained by removing the solvent was irradiated with active energy rays under the following conditions to crosslink the layer, thereby obtaining a resin layer and a laminate. · Light source: High pressure mercury lamp. Radiation output: 400W / cm 2 . Accumulated light output: 120mJ / cm 2 . Oxygen concentration: 0.1% by volume.
[0184] In step 4, the adhesive layer side of "PANAPROTECT" (registered trademark) HUCB Type 2 manufactured by PANAC Corporation was bonded to the resin layer side of the laminate obtained in step 3, and then the support substrate of "PANAPROTECT" (registered trademark) was peeled off to obtain a laminate.
[0185] [Method 4 for forming resin layer] In step 1, the above-mentioned resin layer coating composition was applied to the release layer side of the support substrate using a continuous coating device such as a slot die coater, with the discharge flow rate adjusted so that the thickness of the resin layer after crosslinking would be the specified film thickness, thereby forming a coating layer.
[0186] In step 2, the coating layer formed in step 1 was dried under the following conditions to remove the solvent. ·Blow temperature: Temperature: 140℃. ·Wind speed: Application side: 5m / sec, non-application side: 5m / sec. Air direction: coated side: parallel to the surface of the substrate, non-coated side: perpendicular to the surface of the substrate. Residence time: 2 minutes.
[0187] In step 3, the coating layer obtained by removing the solvent in step 2 was heated at 60° C. for 2 days to be crosslinked to form a resin layer, thereby obtaining a laminate.
[0188] [Formation of particle layer] A resin layer was formed on the resin layer prepared in the previous section by using the above-mentioned coating composition for the particle layer in combination with the method for forming the particle layer described below in the combinations shown in Tables 4 and 5.
[0189] [Method 1 for forming particle layer] In step 1, the above-mentioned coating composition for the particle layer was applied to the resin layer side of the laminate using a continuous coating device with a slot die coater, while adjusting the discharge flow rate so that the thickness of the particle layer after crosslinking would be the specified film thickness, to form a particle layer.
[0190] In step 2, the particle layer formed in step 1 was dried under the following conditions to remove the solvent. ·Blow temperature: Temperature: 80℃. ·Wind speed: Application side: 5m / sec, non-application side: 5m / sec. Air direction: coated side: parallel to the surface of the substrate, non-coated side: perpendicular to the surface of the substrate. Residence time: 2 minutes.
[0191] In step 3, the particle layer (uncrosslinked particle layer) obtained by removing the solvent was irradiated with active energy rays under the following conditions to be crosslinked, thereby obtaining a particle layer and a laminate. · Light source: High pressure mercury lamp. Radiation output: 400W / cm 2 . Accumulated light output: 120mJ / cm 2 . Oxygen concentration: 0.1% by volume.
[0192] [Method 2 for forming particle layer] In step 1, the above-mentioned coating composition for the particle layer was applied to the resin layer side of the laminate using a continuous coating device with a slot die coater, while adjusting the discharge flow rate so that the thickness of the particle layer after crosslinking would be the specified film thickness, to form a particle layer.
[0193] In step 2, the particle layer formed in step 1 was dried under the following conditions to remove the solvent. ·Blow temperature: Temperature: 80℃. ·Wind speed: Application side: 5m / sec, non-application side: 5m / sec. Air direction: coated side: parallel to the surface of the substrate, non-coated side: perpendicular to the surface of the substrate. Residence time: 2 minutes.
[0194] [How to make resin film] The supporting substrate was peeled off from the laminate produced by the above method, thereby producing the resin films of Examples 1 to 35 and Comparative Examples 1 to 6.
[0195] [Table 4]
[0196] [Table 5]
[0197] [Evaluation of resin film] The resin films were subjected to the following performance evaluations, and the results are shown in Tables 6 to 9. Unless otherwise specified, measurements were performed three times for one sample in each Example and Comparative Example at different locations, and the arithmetic average value was used.
[0198] [Measurement of storage modulus and loss tangent of resin film] The resin film was cut into a rectangular specimen measuring 10 mm wide x 150 mm long. The storage modulus and loss tangent of the resin film were determined using a dynamic viscoelasticity measuring device DMS6100 manufactured by Seiko Instruments Inc. based on the tensile vibration-non-resonance method of JIS K7244 (1998) (this is called the dynamic viscoelasticity method). Measurement mode: Tensile. -Chuck distance: 20mm. -Specimen width: 10mm. Frequency: 1Hz ·Distortion amplitude: 10μm. ·Minimum tension: 20mN. Initial force amplitude: 40mN. Measurement temperature: -100℃ to 200℃. Heating rate: 5℃ / min.
[0199] [Measurement of surface roughness of resin film] The surface roughness Sa of the resin film was measured under the following conditions using a non-contact surface shape measuring system "VertScan" (registered trademark) R550H-M100 manufactured by Ryoka Systems Co., Ltd. The arithmetic average value of five measurements was used as the surface roughness Sa. Note that for Examples 9 to 12, the surface of the resin film that was in contact with the supporting substrate (the surface on the supporting substrate side) was measured, and for Examples 1 to 8, 13 to 35 and Comparative Examples 1 to 7, the surface of the resin film on the non-supporting substrate side was measured.
[0200] (Measurement conditions) -Measurement mode: WAVE mode. -Objective lens: 50x. 0.5×Tube lens. ·Measurement area 187×139μm.
[0201] [Measurement of surface free energy of resin film] The surface free energy γ of the resin film was determined by measuring the static contact angles of water, ethylene glycol, and diiodomethane at 25°C on the surface of the resin film, and then introducing the static contact angles with each liquid and the dispersion term, polarity term, and hydrogen bond term of the surface free energy of each liquid described in Non-Patent Document 1 into the "extended Hawkes' equation of Hata and Kitazaki" described in Non-Patent Document 2 to solve the simultaneous equations.
[0202] The static contact angle was measured after the sample was left in an environment of 25°C for 12 hours. Drop Master DM-501 manufactured by Kyowa Interface Science Co., Ltd. was used, and the conditions for creating droplets were selected so that droplets could be created as small as possible without creeping up the needle. The static contact angle was calculated using an image taken 5 seconds after the droplets landed on the resin film surface and the θ / 2 method. In Examples 9 to 12, the surface of the resin film on the supporting substrate side was measured, and in Examples 1 to 8, 13 to 35 and Comparative Examples 1 to 7, the surface of the resin film on the non-supporting substrate side was measured.
[0203] [Evaluation of resin film flexibility] The resin film was cut into a rectangular specimen measuring 10 mm wide and 150 mm long. The direction of the 150 mm length was aligned with the longitudinal direction of the resin film. The initial tensile chuck distance was 50 mm, the tensile speed was set to 300 mm / min, and the tensile test was performed at a measurement temperature of 23°C.
[0204] Read the load b (N) applied to the sample when the chuck distance is a (mm), and use the following formula to calculate the strain x (%) and stress y (N / mm 2 ) was calculated, where the sample thickness before the test was k (mm). Strain amount: x = ((a-50) / 50) x 100 Stress: y=b / (k×10).
[0205] Of the data obtained above, the stress at a strain of 5% was defined as the 5% strain stress.
[0206] [Evaluation of Resin Film Restoration] The resin film was cut into a rectangle of 10 mm width x 150 mm length to prepare a test piece. The direction of the 150 mm length was aligned with the longitudinal direction of the resin film. Using a tensile tester "Tensilon" (registered trademark) UCT-100 manufactured by Orientec Co., Ltd., evaluation was performed under two conditions of different deformation speed and strain amount at a measurement temperature of 23°C to determine the superiority or inferiority of the restoring property.
[0207] Condition A: The sample was stretched to a strain of 20% with an initial chuck distance of 50 mm and a tensile speed of 50 mm / min. The tensile load on the sample was then released, and the distance that had been marked as the initial test length before the measurement was measured and recorded as L1 (mm). The elastic recovery rate z1 (%) was calculated using the following formula. Elastic recovery rate z1 = (1-(L1-50) / 10) x 100 (%) Condition B: The sample was stretched to a strain of 100% with an initial chuck distance of 20 mm and a tensile speed of 300 mm / min. The tensile load on the sample was then released, and the distance that had been marked as the initial test length before the measurement was measured and recorded as L2 mm. The elastic recovery rate z2% was calculated using the following formula. Elastic recovery rate z2 = (1-(L2-20) / 20) x 100 (%).
[0208] [Evaluation of heat resistance of resin film] The resin film was cut into a rectangular shape measuring 10 mm wide x 150 mm long to prepare a test piece.
[0209] Based on the tensile vibration-non-resonance method of JIS K7244 (1998), the storage modulus and loss modulus of the resin film were determined using a dynamic viscoelasticity measuring device DMS6100 manufactured by Seiko Instruments Inc. Measurement mode: Tensile. Chuck distance: 20mm. Specimen width: 10mm. Frequency: 1Hz Strain amplitude: 10μm. Minimum tension: 20mN. Initial force amplitude: 40 mN. Measurement temperature: -100℃ to 200℃. Heating rate: 5°C / min.
[0210] At this time, the dL value (output value of the LVDT (Linear Variable Differential Transformer)) is obtained at the same time as the measurement of the storage modulus and loss modulus, and this value represents the value corresponding to the dimension of the test piece at the time of measurement. The dL value at 30°C was set to a30 (μm) and the dL value at 150°C was set to a150 (μm), and the dimensional change rate was calculated using the following formula. Dimensional change rate = ((a150-a30) / 20,000) x 100 (%) Furthermore, the absolute value of the dimensional change rate at 150°C was calculated based on the dimension at 30°C obtained by the above formula.
[0211] [Evaluation of printability of resin film using metal paste] Using a resin film, a printing plate, and a conductive ink, an electric circuit body with a circuit pattern as shown in FIG. 11 was printed by screen printing. In detail, a printing plate with a screen mesh #200 woven from synthetic fibers such as polyester was prepared, and the conductive ink was pressed against the stretchable sheet with a squeegee to print the conductive ink on the stretchable sheet (printing speed: 100 mm / sec, printing angle 60 degrees). At this time, the presence or absence of adhesion of the resin film to the printing plate (adhesion during printing), the presence or absence of peeling between the separator and the resin film (floating during printing), and the state of bleeding or fading of the wiring of the printed matter were visually observed and evaluated on the following four levels. Note that for Examples 9 to 12, the surface of the resin film on the supporting substrate side was evaluated, and for Examples 1 to 8, 13 to 35, and Comparative Examples 1 to 7, the surface of the resin film on the non-supporting substrate side was evaluated.
[0212] A: There is no sticking or lifting during printing, and there is no bleeding or fading of wiring.
[0213] B: There is no lifting during printing, but there is some sticking and some bleeding and fading of the wiring can be seen in some places.
[0214] C: There is no lifting during printing, but the print is strongly adhered to the surface, and bleeding and fading of the wiring can be seen in most areas.
[0215] D: There is strong adhesion during printing, causing lifting during printing.
[0216] [Evaluation of metal paste adhesion to resin film] A resin film was fixed on a glass plate, a paste (LS-453-6B, manufactured by Asahi Chemical Laboratory Co., Ltd.) was applied thereon using an applicator so that the coating thickness after drying would be 5 μm, and after drying for 30 minutes at 80° C., adhesion evaluation was performed according to the adhesion (cross-cut method) described in JIS K5600-5-6 (1999). Note that for Examples 9 to 12, the surface of the resin film facing the supporting substrate was evaluated, and for Examples 1 to 8, 13 to 35, and Comparative Examples 1 to 7, the surface of the resin film facing the non-supporting substrate was evaluated.
[0217] [Evaluation of metal paste adhesion to resin film under humid conditions] A resin film was fixed on a glass plate, and a paste (LS-453-6B, manufactured by Asahi Chemical Laboratory Co., Ltd.) was applied thereon using an applicator so that the coating thickness after drying would be 5 μm. After drying at 80° C. for 30 minutes, the film was left to stand for 24 hours in an environment with a temperature of 85° C. and a relative humidity of 85%. Adhesion evaluation was performed according to the adhesion (cross-cut method) described in JIS K5600-5-6 (1999), and an approximate residual rate of the metal paste layer was obtained as observed visually. For Examples 9 to 12, the surface of the resin film facing the supporting substrate was evaluated, and for Examples 1 to 8, 13 to 35, and Comparative Examples 1 to 7, the surface of the resin film facing the non-supporting substrate was evaluated.
[0218] [Evaluation of particle layer adhesion of resin film] A Haize Gauze NT-4 (manufactured by Ozu Sangyo) was placed vertically on the particle layer side of the resin film with two different load conditions, and the approximate remaining rate of the particle layer as seen with the naked eye after it was moved back and forth 10 times over a length of 5 cm was determined.
[0219] Condition C: Load 50g / cm 2 .
[0220] Condition D: Load 250g / cm 2 .
[0221] [Evaluation of extension stability] The resin film was cut into a rectangle of 10 mm width x 150 mm length to prepare a test piece. The direction of the 150 mm length was aligned with the longitudinal direction of the resin film. A creep test was performed using a tensile tester "Tensilon" (registered trademark) UCT-100 manufactured by Orientec Co., Ltd., with an initial tensile chuck distance of 50 mm, a creep rate of 300 mm / min, a load of 10 MPa, and a measurement temperature of 23°C. In the above evaluation, the retention time until breakage was recorded, up to a maximum of 300 seconds.
[0222] [Skewness Ssk] The skewness Ssk was measured using a surface roughness meter (SURFCORDER ET4000A, manufactured by Kosaka Laboratory Co., Ltd.) under the following conditions. The arithmetic average of five measurements was used as the skewness Ssk. In Examples 9 to 12, the surface of the resin film facing the supporting substrate was measured, and in Examples 1 to 8, 13 to 35 and Comparative Examples 1 to 7, the surface of the resin film facing the non-supporting substrate was measured. Analysis equipment: 3D surface roughness analysis system (model TDA-31) Stylus: Tip radius 0.5μmR, diameter 2μm, made of diamond Needle pressure: 100μN X measurement length: 1.0mm X-feed speed: 0.1 mm / s (measurement speed) Y feed pitch: 5 μm (measurement interval) Number of Y lines: 81 (measured number) Z magnification: 2000x (vertical magnification) Low-frequency cutoff: 0.20 mm (swell cutoff value) High Cutoff: None Filter type: Gaussian spatial type Leveling: Yes (tilt correction) [Adhesion to adhesive layer] The adhesion with the adhesive layer was evaluated by the load (N) when the adhesive layer was peeled off from the resin film at 180 degrees using a tensile tester "Tensilon" (registered trademark) UCT-100 manufactured by Orientec Co., Ltd. The resin film was cut into a rectangle of 25 mm width x 120 mm length to prepare a test piece. The direction of the 120 mm length was aligned with the longitudinal direction of the resin film. One of the support substrates of an acrylic adhesive film (product number: MCS70) manufactured by Mitate Imaging Co., Ltd. was peeled off, and the adhesive layer was attached to a PET film "Lumirror" (registered trademark) S10 25 μm manufactured by Toray Industries, Inc., to prepare a PET film with an adhesive layer. Next, the PET film with the adhesive layer was attached to the surface of the resin film to be evaluated. Furthermore, a double-sided tape (product number: No. 5000NS) manufactured by Nitto Denko Corporation was attached to the other surface of the resin film, the support substrate of the double-sided tape was peeled off, and the tape was attached to a SUS304 plate to prepare an evaluation structure. Finally, the evaluation structure was attached to UCT-100, a part of the adhesive layer / resin film interface was peeled off, one end of the adhesive layer-attached PET film was fixed to a load cell with tape, and measurements were performed under the following conditions: For Examples 9 to 12, the surface of the resin film facing the supporting substrate was evaluated, and for Examples 1 to 8, 13 to 35, and Comparative Examples 1 to 7, the surface of the resin film facing the non-supporting substrate was evaluated. Measurement distance: 50mm Test piece width: 20mm Peel speed: 300mm / min (Pulling speed: 600mm / min) Peel angle: 180 degrees Tables 6 to 9 summarize the presence / absence of the segments of Chemical Formula 1 and Chemical Formula 2 in the resin films and the results of each evaluation.
[0223] [Table 6]
[0224] [Table 7]
[0225] [Table 8]
[0226] [Table 9]
[0227] In Tables 6 and 7, "including" in the column for Chemical Formula 1 means that each Example contains a segment of Chemical Formula 1, and "not including" means that each Example does not contain a segment of Chemical Formula 1. The same applies to Chemical Formulas 2 to 4.
[0228] [Comparative Example 7] The resin film of Example 1 was rubbed with a brass brush so that the surface roughness Sa was 5,500 nm. When the restorability of the resin film of Comparative Example 5 was evaluated under condition A, it broke and could not be measured. [Industrial Applicability]
[0229] The resin film of the present invention has high flexibility and recovery, and can be suitably used in applications requiring various processing in a post-process. For example, the resin film of the present invention is used in an electric circuit body, a health care sensor, or a wearable sensor. As another example, the resin film of the present invention can be suitably used for wearable devices, stretchability for health care devices, stretchable sensors, and stretchable actuators.
[0230] In addition, from the viewpoint of high flexibility and resilience, the composition can be suitably used as a surface material, internal material, constituent material, or manufacturing process material for a variety of products that require resilience, such as a substrate for an adhesive tape, an impact absorbing material for a display, a substrate for a medical film, a substrate for a surface protection film for an automobile, and a core material for a pressure sensor. [Explanation of symbols]
[0231] 1, 12, 16, 28: Resin film 2: Particle layer 3: Resin particles 4, 9, 11, 15, 17, 19, 22, 25: Laminate 5, 21: Release layer 6, 8, 14: Supporting base material 7: Resin layer 10: Support substrate having an uneven surface 13: Release layer having an uneven surface 18, 20, 23, 26: Protective material 24: Adhesive layer 27: Electrical circuit body 29: Electrical Circuits
Claims
1. A resin film that satisfies the following conditions, the resin film having a resin layer containing a segment of Chemical Formula 1 or Chemical Formula 2. Condition 1. The storage modulus at a temperature of 25° C. and a frequency of 1 Hz is 0.5 MPa or more and 50 MPa or less. Condition 2. The loss tangent at a temperature of 25°C and a frequency of 1 Hz is 0.5 or less. Condition 3. The surface roughness Sa of at least one surface is 150 nm or more and 5,000 nm or less. 【Chemistry 1】 【Chemistry 2】 R 1 represents hydrogen or a methyl group. R 2 represents any of the following: A substituted or unsubstituted alkylene group. A substituted or unsubstituted arylene group. An alkylene group having an internal ether group, ester group, or amide group. An arylene group having an internal ether group, ester group, or amide group. An unsubstituted alkylene group having an ether group, an ester group, or an amide group inside. An unsubstituted arylene group having an ether group, an ester group, or an amide group therein. R 3 represents any of the following: A substituted or unsubstituted alkylene group. A substituted or unsubstituted arylene group.
2. The resin film according to claim 1 , wherein at least one surface of the resin film has a surface free energy of 25 mN / m or more.
3. The resin film according to claim 1 or 2, which has a resin layer containing segments of Chemical Formula 1 and Chemical Formula 2.
4. The resin film according to claim 1 , further comprising a particle layer containing resin particles.
5. The resin film according to claim 4 , wherein the number average particle diameter of the resin particles contained in the particle layer is 2 μm or more and 20 μm or less.
6. The resin film according to claim 4 or 5, comprising a resin layer and a particle layer on at least one surface thereof, the particle layer containing a segment of Chemical Formula 3. 【Chemistry 3】
7. The resin film according to any one of claims 1 to 6, wherein the skewness Ssk of at least one surface of the resin film is -0.2 or more and 1.0 or less.
8. A resin film / adhesive layer laminate in which the resin film according to claim 7 is in contact with an adhesive layer.
9. A method for producing a resin film / adhesive layer laminate, comprising laminating the resin film of claim 7 and an adhesive layer.
10. 8. A method for producing a resin film according to claim 1, comprising a step of applying a coating composition for a particle layer, the coating composition including resin particles, to form a particle layer.
11. 9. An electric circuit body comprising: the resin film according to claim 1; or the resin film / adhesive layer laminate according to claim 8; and a conductor circuit formed on the resin film.
12. A healthcare sensor comprising: the resin film according to any one of claims 1 to 7; or the resin film / adhesive layer laminate according to claim 8; and a conductor circuit formed on the resin film.
13. A wearable sensor comprising: the resin film according to any one of claims 1 to 7; or the resin film / adhesive layer laminate according to claim 8; and a conductor circuit formed on the resin film.
14. A method for producing a resin film processed product, comprising a step of processing the resin film according to any one of claims 1 to 7 or the resin film / adhesive layer laminate according to claim 8 by screen printing.
Citation Information
Patent Citations
Photo-setting resin composition and optical member
JP2000344845A
Photosensitive resin composition, laminate, wiring board, and flexible wiring board
JP2004318047A
Image formation device and image formation method
JP2005001201A
Active energy ray-curing resin composition, cured film and laminated body
JP2010222568A
Method for manufacturing composite film, and composite film
JP2013060546A