Manufacturing method of molded body

The method of mixing cellulose fibers with a finely powdered binding material and controlled humidification and molding addresses the environmental impact of paper manufacturing, achieving strong and eco-friendly molded articles with minimal water and energy use.

JP7552201B2Active Publication Date: 2024-09-18SEIKO EPSON CORP
View PDF 16 Cites 0 Cited by

Patent Information

Application Number
JP2020163404
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-29
Publication Date
2024-09-18
Estimated Expiration
2040-09-29

AI Technical Summary

Technical Problem

Existing paper manufacturing methods that replace synthetic resins with natural materials like starch require significant water addition for binding, increasing environmental impact and energy consumption.

Method used

A method involving mixing cellulose fibers with a binding material having an average particle diameter of 20.0 μm or less, applying water to form a web, and heating/pressurizing to create a molded body, utilizing a manufacturing apparatus with controlled humidification and molding processes.

Benefits of technology

Produces molded articles with excellent mechanical strength, biodegradability, and reduced environmental footprint by minimizing water usage and energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007552201000002
    Figure 0007552201000002
  • Figure 0007552201000001
    Figure 0007552201000001
Patent Text Reader

Abstract

To provide a molded article that can achieve excellent mechanical strength of a molded article such as a paper molded using the molded article while having good biodegradability.SOLUTION: A molded article manufacturing method includes a mixing step to obtain a mixture by mixing fibers and powder of binding material, an accumulation step to form a web by accumulating the mixture, a humidification step to apply water to the web, and a molding step to obtain a molded article by heating and pressurizing the web applied with water. The binding material binds the fibers to each other when being applied with water. An average particle diameter (D50) of the powder is 20.0 μm or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a molded article. [Background technology]

[0002] As a method for producing molded products such as paper, a method that uses almost no or little water, called a dry method, is expected. For example, Patent Document 1 discloses a method for producing paper by piling up a mixture of dried fibers and resin and applying pressure / heat, as a sheet production method that can reduce energy in the drying process because it does not use a large amount of water as in the papermaking method. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2012-144826 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, in the paper manufacturing method described in Patent Document 1, a resin is used as a binding material between fibers. If such a resin is to be replaced with a natural material such as starch in order to reduce the environmental impact, it is necessary to add a relatively large amount of moisture to exhibit binding properties between the fibers. [Means for solving the problem]

[0005] One aspect of the method for producing a molded body according to the present invention is to A mixing step of mixing the fibers and the powder of the binder material to obtain a mixture; depositing the mixture to form a web; a moistening step of applying water to the web; a molding step of heating and pressing the web to which water has been applied to obtain a molded body; A method for producing a molded body comprising the steps of: The binding material binds the fibers together when water is applied thereto, The powder has an average particle size (D50) of 20.0 μm or less. [Brief description of the drawings]

[0006] [Figure 1] FIG. 2 is a diagram showing a molded body manufacturing apparatus according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] Several embodiments of the present invention will be described below. The embodiments described below are merely examples of the present invention. The present invention is not limited to the following embodiments, and includes various modified forms that are implemented within the scope of the present invention. Note that not all of the configurations described below are necessarily essential configurations of the present invention.

[0008] 1. Manufacturing method of molded body The method for producing a molded body according to this embodiment includes a mixing step of mixing fibers and powder of a binding material to obtain a mixture, a deposition step of depositing the mixture to form a web, a humidifying step of applying water to the web, and a molding step of heating and pressurizing the web to which water has been applied to obtain a molded body. The binding material bonds the fibers together when water is applied, and the average particle size (D50) of the powder is 20.0 μm or less.

[0009] 1.1.Mixing process The method for producing a molded body according to the present embodiment includes a mixing step in which fibers and a powder of a binder material are mixed to obtain a mixture.

[0010] Fibers The fibers are the main component of the molded article produced using the mixture, and they contribute greatly to maintaining the shape of the molded article, and are one of the components that impart properties such as strength to the molded article.

[0011] The fibers are preferably made of a material containing at least one of the chemical structures of a hydroxyl group, a carbonyl group, and an amino group, which facilitates the formation of hydrogen bonds between the fibers and the binding material described below, and improves the bonding strength between the fibers and the binding material, the overall strength of the molded product produced using the mixture, for example, the tensile strength of a sheet-like molded product, and the like.

[0012] The fibers may be synthetic fibers made of synthetic resins such as polypropylene, polyester, and polyurethane, but are preferably naturally derived fibers, i.e., biomass-derived fibers, and are more preferably cellulose fibers. This allows for more appropriate responses to environmental issues and the saving of buried resources. In particular, when the fibers are cellulose fibers, the following effects can be obtained.

[0013] That is, cellulose is a natural material derived from plants and is abundant, and the use of cellulose as a fiber constituting the mixture can more appropriately address environmental issues and save buried resources, and is also preferable from the viewpoints of stable supply of the mixture and molded articles produced using the same, cost reduction, etc. Furthermore, among various fibers, cellulose fibers have particularly high theoretical strength, and are advantageous from the viewpoint of further improving the strength of molded articles. Furthermore, cellulose fibers have good biodegradability.

[0014] The fibers may contain components other than cellulose, such as hemicellulose, lignin, etc. The cellulose fibers may be subjected to a process such as bleaching.

[0015] The fibers may also be treated with ultraviolet light, ozone, plasma, or other such treatments. This can increase the hydrophilicity of the fibers and enhance their affinity with the binding material. More specifically, these treatments can introduce functional groups such as hydroxyl groups onto the fiber surface, allowing the fibers to form hydrogen bonds more efficiently with the binding material.

[0016] The mixture obtained in this step includes fibers and a binder material. In the mixture, the binder material may be attached to the fibers, or there may be fibers to which the binder material is not attached. In addition, in the mixture, the binder material may be attached to the fibers, or there may be binder material that is not attached to the fibers.

[0017] The average length of the fibers is not particularly limited, but is preferably from 0.1 mm to 50 mm, more preferably from 0.2 mm to 5.0 mm, and even more preferably from 0.3 mm to 3.0 mm.

[0018] This makes it possible to improve the stability of shape, strength, etc. of the molded article produced using the mixture.

[0019] The average thickness of the fibers is not particularly limited, but is preferably 0.005 mm or more and 0.5 mm or less, and more preferably 0.010 mm or more and 0.05 mm or less.

[0020] This makes it possible to improve the stability of shape, strength, etc. of the molded article produced using the mixture. In addition, it is possible to prevent unintended irregularities from occurring on the surface of the molded article produced using the mixture.

[0021] The average aspect ratio of the fibers, that is, the average length to the average thickness, is not particularly limited, but is preferably 10 or more and 1,000 or less, and more preferably 15 or more and 500 or less.

[0022] This makes it possible to improve the stability of shape, strength, etc. of the molded article produced using the mixture. In addition, it is possible to prevent unintended irregularities from occurring on the surface of the molded article produced using the mixture.

[0023] The fiber content in the mixture is not particularly limited, but is preferably 60.0% by mass or more and 99.0% by mass or less, more preferably 85.0% by mass or more and 98.0% by mass or less, and even more preferably 88.0% by mass or more and 97.0% by mass or less.

[0024] This makes it possible to improve the properties such as shape stability and strength of a molded body produced using the mixture. In addition, the moldability during production of the molded body can be improved, which is also advantageous in terms of improving the productivity of the molded body.

[0025] 1.1.2. Bonding material The binding material is a component that functions as a binder that binds fibers together in a molded product produced using the mixture. In particular, the binding material can be derived from biomass, which can be used to suitably address environmental issues and the conservation of buried resources. In addition, the binding material can exhibit adhesion at a relatively low temperature with a small amount of moisture relative to the amount of binding material, and excellent binding properties can be obtained.

[0026] Examples of binding materials that can be used include starch, dextrin, glycogen, amylose, hyaluronic acid, kudzu, konjac, potato starch, etherified starch, esterified starch, natural gum paste (etherified tamarind gum, etherified locust bean gum, etherified guar gum, acacia arabic gum), fiber-derived paste (etherified carboxymethylcellulose, hydroxyethylcellulose), seaweed (sodium alginate, agar), animal protein (collagen, gelatin, hydrolyzed collagen, sericin), and any mixture of these may be used.

[0027] Among these, the binding material is more preferably at least one of starch and dextrin, and even more preferably dextrin or a mixture of dextrin and starch with a high dextrin ratio. On the other hand, in terms of the powder being relatively insoluble in water and making the binding material easy to handle, it is more preferable to use starch or a mixture of dextrin and starch with a high starch ratio. Using at least one of starch and dextrin as the binding material is preferable in terms of less coloring, easier adjustment of the average particle size of the powder, and relatively easy availability.

[0028] Starch and dextrin are polymeric materials formed by the polymerization of multiple α-glucose molecules through glycosidic bonds. Starch and dextrin may be linear or branched.

[0029] Starch and dextrin can be derived from various plants. Examples of the raw materials for starch and dextrin include cereals such as corn, wheat, and rice, beans such as broad beans, mung beans, and red beans, tubers such as potato, sweet potato, and tapioca, wild plants such as dogtooth violets, bracken, and kudzu, and palms such as sago palm.

[0030] In addition, processed starch or modified starch may be used as the starch. Examples of processed starch include acetylated adipic acid crosslinked starch, acetylated starch, oxidized starch, sodium octenyl succinate starch, hydroxypropyl starch, hydroxypropylated phosphate crosslinked starch, phosphorylated starch, phosphate esterified phosphate crosslinked starch, urea phosphate esterified starch, sodium starch glycolate, and high amylose corn starch. Examples of modified starch include alpha-starch, modified dextrin, lauryl polyglucose, cationic starch, thermoplastic starch, and carbamic acid starch.

[0031] As the dextrin, commercially available products may be used, and for example, products sold under names such as dextrol, yellow dextrin, A-sol, enzyme-modified dextrin, British gum, etc. may be appropriately used.

[0032] The binder is mixed in the form of powder. By using the binder in powder form, it can be mixed uniformly with the fibers in the mixing process. The particle size of the binder powder is 20.0 μm or less as the volume-based average particle diameter D50. The average particle diameter (D50) of the binder powder is more preferably 18.0 μm or less, more preferably 15.0 μm or less, and even more preferably 10.0 μm or less. If the average particle diameter (D50) of the powder is in this range, the binder powder can be mixed with the fibers better. On the other hand, the lower limit of the average particle diameter (D50) of the binder powder is not particularly limited, but is 0.5 μm or more, preferably 1.0 μm or more, and more preferably 1.5 μm or more. If the lower limit of the average particle diameter (D50) is in this range, the binder powder can be handled more easily as a powder, and can also be manufactured more easily by crushing or the like.

[0033] If the average particle size of the powder of the binding material is within the above range, when the binding material capable of binding fibers together by adding moisture is supplied as a powder to the web, the powder particles are small, so that the added moisture easily penetrates into the powder, and dry molding can be easily carried out even with a small amount of moisture. This also makes it possible to reduce the burden on the environment by using a natural binding material, and to reduce the amount of energy consumed for drying the moisture.

[0034] 1.1.3.Mixture Through this process, at least the fibers and the powder of the binder material are mixed to obtain a mixture. The content of the binder material in the total amount of the mixture is preferably 1.0% by mass or more and 30.0% by mass or less, more preferably 2.0% by mass or more and 28.0% by mass or less, and even more preferably 3.0% by mass or more and 25.0% by mass or less.

[0035] The web formed in the deposition step described below is made of the mixture, and therefore the content of the binding material relative to the total amount of the web is preferably 1.0% by mass or more and 30.0% by mass or less, more preferably 2.0% by mass or more and 28.0% by mass or less, and even more preferably 3.0% by mass or more and 25.0% by mass or less, similar to the mixture.

[0036] When the content of the binder material in the mixture or web is within the above range, the web contains a sufficient amount of binder material, and the web can be stably transported, for example, during the manufacturing process.

[0037] The content of the binding material can be measured by component analysis such as thermogravimetric analysis or NMR, and can be measured using a pretreatment method such as enzymatic decomposition as necessary.

[0038] The mixture may contain components other than the fibers and binding materials described above. Examples of such components include sizing agents, impurities derived from fibers, and impurities derived from binding materials. The mixture may also contain components for imparting desired performance to a molded product to be described later. Examples of such components include fillers such as calcium carbonate, talc, titanium oxide, silica, and diatomaceous earth; coloring materials such as pigments, dyes, and toners; and paper strength agents such as polyvinyl alcohol (PVA).

[0039] However, the content of components other than the fibers and the binder material in the mixture is preferably 10% by mass or less, more preferably 5.0% by mass or less, and even more preferably 2.0% by mass or less.

[0040] 1.2. Deposition process The method for producing a molded body of this embodiment includes a deposition step in which the mixture is deposited to form a web. The deposition step is a step in which the mixture is dropped onto an appropriate object and deposited. In the deposition step, for example, the mixture is dropped onto a mesh that allows air to pass through, which makes it easier to form a web. Furthermore, the deposition step can be performed, for example, using a mesh belt of a production device described later, to form a continuous web.

[0041] 1.3. Humidification process The method for producing a molded article according to the present embodiment includes a humidifying step of applying water to the web. By applying water to the web in the humidifying step, a part or all of the surface of the binding material becomes adhesive to fibers, and can adhere to the fibers.

[0042] In addition, when the web is humidified by the humidifying step, the bonding strength between the fibers and the bonding material and the bonding strength between the fibers via the bonding material can be excellent in the molding step described below, and the strength of the finally obtained molded body can be sufficiently excellent. In addition, when the web is humidified by the humidifying step, molding in the molding step can be suitably performed at a relatively low temperature.

[0043] The method of humidifying the web is not particularly limited, but is preferably performed without contact with the web, and examples of the method include a method of placing the web in a high humidity atmosphere, a method of passing the web through a high humidity space, a method of spraying a mist of a liquid containing water onto the web, a method of passing the web through a space in which a mist of a liquid containing water is suspended, etc. One or more methods selected from these may be combined. Note that the liquid containing water may contain, for example, a preservative, a fungicide, an insecticide, etc.

[0044] The humidification of the web may be carried out at multiple stages, for example, in the process of producing a molded article. More specifically, for example, moisture may be imparted to the web by at least one of humidifying the raw materials of the mixture, humidifying the mixture, and humidifying the web, and these methods may be carried out multiple times in combination.

[0045] As described above, by humidifying the web or its raw material at multiple stages in the process of producing a molded product, for example, it is not necessary to increase the amount of humidification more than necessary at each stage. As a result, for example, the conveying speed of the mixture or web in the molded product production apparatus can be increased, and the productivity of the molded product can be improved.

[0046] The amount of moisture to be added to the raw material, mixture, and web in the moistening step is not particularly limited, but the moisture content of the web at the end of the moistening step, i.e., the moisture content of the web relative to the total mass of the web at the end of the moistening step, is preferably 5.0% by mass or more and 60.0% by mass or less, more preferably 7.0% by mass or more and 50.0% by mass or less, and even more preferably 10.0% by mass or more and 40.0% by mass or less. The method for producing a molded body of this embodiment can produce a dry molded body with such a small amount of moisture. This also makes it possible to further reduce the amount of energy consumed to dry the moisture.

[0047] The moisture content can be determined by measurement using a heat-dry type moisture meter manufactured by A&D Co., Ltd.

[0048] 1.4. Molding process The method for producing a molded body of this embodiment includes a molding step in which a web to which water has been added is heated and pressurized to obtain a molded body. In the molding step, the humidified web is heated and pressurized to form a sheet, board, or plate. This results in a molded body in which the fibers are bonded together by the binding material. The humidification step and the molding step may be performed simultaneously.

[0049] The heating temperature in the molding step is not particularly limited, but is preferably 50°C to 100°C, more preferably 55°C to 95°C, and even more preferably 60°C to 90°C. Here, the heating temperature is the surface temperature of the molded body. Heating in the molding step is performed, for example, by a heating roller, in which case the temperature immediately after the web leaves the roller corresponds to the heating temperature, and the temperature of the heating roller is set so that the surface temperature of the molded body becomes the above temperature. When heating is performed by a heating roller, the surface temperature of the molded body is adjusted taking into consideration the set temperature of the heating roller and the transport speed of the web.

[0050] By going through the molding process, the adhesive strength of the binding material that has been through the humidification process can be sufficiently obtained. In addition, since the humidification process does not give excessive moisture to the web, the temperature of the molding process can be set low, and deterioration of the constituent materials of the molded body can be suppressed. This is also preferable from the viewpoint of energy saving, since it reduces the amount of moisture that evaporates. In addition, by going through the molding process, a molded body with excellent mechanical strength can be obtained. Note that the above temperature is sufficiently lower than when synthetic resin such as polyester is used as the binding material.

[0051] The pressure in the molding step is preferably 0.1 MPa or more and 100 MPa or less, more preferably 0.3 MPa or more and 20 MPa or less. This step can be carried out, for example, using a heat press, a heat roller, or the like. The order of pressurization and heating in the molding step is not particularly limited. In addition, pressurization and heating in the molding step may be carried out multiple times independently, as necessary.

[0052] 1.5. Molded body The molded article produced by the manufacturing method of the present embodiment is a molded article having a desired shape while suppressing the use of petroleum-derived materials. In addition, such a molded article is also excellent in biodegradability. In addition, such a molded article is also excellent in recyclability, strength, etc.

[0053] The shape of the molded product is not particularly limited and may be any shape, such as a sheet, a block, a sphere, or a three-dimensional shape. However, since the molded product is molded by heating and pressing the web, it is preferably in the form of a sheet, a board, or a plate. The sheet shape referred to here is a shape having a thickness of 30 μm to 30 mm and a density of 0.05 g / cm. 3 More than 1.5g / cm 3 This refers to a molded article molded so as to have the following properties. This allows the molded article to be suitably used as a recording medium, for example. In addition, by using a manufacturing device as described below, the molded article can be manufactured more efficiently.

[0054] The molded body may have at least a part composed of the above-mentioned mixture, and may have a part not composed of the mixture. The use of the molded body is not particularly limited, and examples thereof include a recording medium, a liquid absorbent, a buffer material, and a sound absorbing material. In addition, the molded body may be used after being subjected to mechanical processing such as cutting or various chemical treatments after the molding process.

[0055] When the molded body is a liquid absorbent, it is preferable that the thickness is 0.3 mm or more and 30 mm or less. Furthermore, the density is 0.05 g / m 3 More than 0.4g / m 3 It is preferable that the above-mentioned condition is satisfied. This allows the molded article to be more suitably used as a liquid absorbent. In addition, by using a manufacturing apparatus as described later, the molded article can be manufactured more efficiently.

[0056] 1.6.Other processes The method for producing a molded body according to the present embodiment may include a preparation step, a processing step, and the like in addition to the above-mentioned mixing step, depositing step, humidifying step, and molding step.

[0057] The preparation step is a step of preparing materials to be mixed before the mixing step. Examples of the preparation step include a fiberization step for preparing fibers and a pulverization step for obtaining a powdered binding material.

[0058] The fiberization step includes, for example, obtaining fibers by defibrating the cellulose raw material in a dry state, or obtaining fibers by disintegrating the cellulose raw material in water. In the fiberization step, it is more preferable to obtain fibers by defibrating in a dry state, since the mixing step is performed in a dry state. Defibration can be performed, for example, by a defibrating unit of a manufacturing device described later.

[0059] The pulverization step can be carried out by a known method, for example, by using a known device such as an FM mixer, a Henschel mixer, a super mixer, or a nanojetmizer. The device may be one that uses high-speed rotating blades to pulverize, or one that utilizes the rotation of a container such as a V-type mixer. Furthermore, the device may be a batch type device or a continuous type device.

[0060] 2. Molded body manufacturing equipment Next, a molded body manufacturing apparatus that can be suitably applied to the molded body manufacturing method will be described. Fig. 1 is a schematic side view showing a suitable example of the molded body manufacturing apparatus.

[0061] In the following, the upper side of FIG. 1 may be referred to as "upper" or "upper side", and the lower side may be referred to as "lower" or "lower side". FIG. 1 is a schematic diagram, and the positional relationship of each part of the molded body manufacturing apparatus 100 may differ from the actual positional relationship. In each figure, the direction in which the fiber raw material M1, the coarsely crushed pieces M2, the defibrated material M3, the first sorted material M4-1, the second sorted material M4-2, the first web M5, the finely divided body M6, the mixture M7, the second web M8, and the sheet S are transported, that is, the direction indicated by the arrow, is also referred to as the transport direction. The tip side of the arrow is also referred to as the downstream side of the transport direction, and the base end side of the arrow is also referred to as the upstream side of the transport direction.

[0062] The molded body manufacturing apparatus 100 shown in FIG. 1 is an apparatus that roughly crushes and defibrates a fiber raw material M1 to obtain fibers (defibrated material M3), mixes the fibers with a binding material in a mixing section 17, deposits the mixture, and molds the deposited second web M8 in a molding section 20 to obtain a sheet S as a molded body.

[0063] The fiber raw material M1 may be, for example, waste paper that has been used or is no longer needed. Alternatively, the fiber raw material M1 may be, for example, a sheet material containing fibers and a binding material attached to the fibers. The sheet material may be, for example, recycled paper that has been processed so that waste paper can be reused, or may be non-recycled paper.

[0064] 1 includes a sheet supplying device 11, a crushing section 12, a defibrating section 13, a sorting section 14, a first web forming section 15, a fragmenting section 16, a mixing section 17, a dispersion section 18, a second web forming section 19, a forming section 20, a cutting section 21, a stocking section 22, a recovery section 27, and a control section 28 that controls the operation of these sections. Each of the crushing section 12, the defibrating section 13, the sorting section 14, the first web forming section 15, the fragmenting section 16, the mixing section 17, the dispersion section 18, the second web forming section 19, the forming section 20, the cutting section 21, and the stocking section 22 is a processing section that processes a sheet.

[0065] The sheet supplying device 11 and the crushing section 12 or the defibrating section 13 form a sheet processing device 10A. The sheet processing device 10A and the second web forming section 19 form a fibrous material depositing device 10B.

[0066] The molded body manufacturing apparatus 100 also includes a humidifier section 231, a humidifier section 232, a humidifier section 233, a humidifier section 234, a humidifier section 235, and a humidifier section 236. In addition, the molded body manufacturing apparatus 100 also includes a blower 261, a blower 262, and a blower 263.

[0067] Moreover, the humidifiers 231 to 236 and the blowers 261 to 263 are electrically connected to the control unit 28, and their operation is controlled by the control unit 28. That is, in this embodiment, the operation of each part of the molded body manufacturing apparatus 100 is controlled by one control unit 28. However, without being limited thereto, for example, the molded body manufacturing apparatus 100 may be configured to have a control unit that controls the operation of each part of the sheet supplying device 11 and a control unit that controls the operation of parts other than the sheet supplying device 11.

[0068] In addition, the molded body manufacturing apparatus 100 executes a raw material supplying process, a coarse crushing process, a defibrating process, a sorting process, a first web forming process, a dividing process, a mixing process, a releasing process, a stacking process, a sheet forming process, and a cutting process. The sheet forming process corresponds to the molding process in the molded body manufacturing method. In addition, the process of humidifying in each humidifying section described in detail later corresponds to the humidifying process.

[0069] The configuration of each part will be described below. The sheet supplying device 11 is a part that performs a raw material supplying process of supplying the fiber raw material M1 to the crushing part 12. As the fiber raw material M1, a material containing cellulose fiber as the fiber is used, but for example, a molded body manufactured by the manufacturing method of this embodiment may also be used.

[0070] The crushing unit 12 is a section that performs a crushing step of crushing the fiber raw material M1 supplied from the sheet supplying device 11 in air or the like. The crushing unit 12 has a pair of crushing blades 121 and a chute 122.

[0071] The pair of crushing blades 121 rotate in opposite directions to each other, and can crush the fiber raw material M1 between them, i.e., cut it into crushed pieces M2. The shape and size of the crushed pieces M2 are preferably suitable for the defibration process in the defibration unit 13, and are preferably small pieces with a side length of 100 mm or less, and more preferably 10 mm or more and 70 mm or less.

[0072] The chute 122 is disposed below the pair of crushing blades 121 and has, for example, a funnel shape. This allows the chute 122 to receive the coarsely crushed pieces M2 that have been crushed by the crushing blades 121 and dropped.

[0073] In addition, above the chute 122, a humidifying section 231 is disposed adjacent to the pair of coarse crushing blades 121. The humidifying section 231 humidifies the coarsely crushed pieces M2 in the chute 122. The humidifying section 231 is configured as an evaporation type humidifier that has a moisture-containing filter and supplies humidified air with increased humidity to the coarsely crushed pieces M2 by passing air through the filter. By supplying humidified air to the coarsely crushed pieces M2, the humidifying process described above can be performed, and the effects described above can be obtained. In addition, the coarsely crushed pieces M2 can be prevented from adhering to the chute 122, etc. due to static electricity.

[0074] The chute 122 is connected to the defibrating unit 13 via a pipe 241. The coarse crushed pieces M2 collected in the chute 122 pass through the pipe 241 and are transported to the defibrating unit 13.

[0075] The defibrating unit 13 is a section that performs a defibrating process in which the coarsely crushed pieces M2 are defibrated in the air, i.e., in a dry manner. The defibrating process in this defibrating unit 13 makes it possible to generate a defibrated material M3 from the coarsely crushed pieces M2. Here, "defibrating" refers to untangling the coarsely crushed pieces M2, which are made up of multiple fibers bound together, into individual fibers. This untangled material becomes the defibrated material M3. The shape of the defibrated material M3 is linear or band-like. The defibrated material M3 may also be present in a state where it is entangled with other pieces to form a mass, that is, in a state where it forms so-called "lumps."

[0076] In this embodiment, for example, the defibrating unit 13 is configured with an impeller mill having a rotary blade that rotates at high speed and a liner located on the outer periphery of the rotary blade. The coarse fragments M2 that flow into the defibrating unit 13 are sandwiched between the rotary blade and the liner and defibrated.

[0077] Furthermore, the defibrating unit 13 can generate an air flow from the crushing unit 12 toward the sorting unit 14, i.e., an airflow, by the rotation of the rotary blades. This allows the coarsely crushed pieces M2 to be sucked into the defibrating unit 13 from the pipe 241. Furthermore, after the defibrating process, the defibrated material M3 can be sent to the sorting unit 14 via the pipe 242.

[0078] A blower 261 is installed in the middle of the pipe 242. The blower 261 is an airflow generating device that generates an airflow toward the screening unit 14. This promotes the sending out of the defibrated material M3 to the screening unit 14.

[0079] The sorting unit 14 is a section that performs a sorting process in which the defibrated material M3 is sorted according to the length of the fibers. In the sorting unit 14, the defibrated material M3 is sorted into a first sorted material M4-1 and a second sorted material M4-2 that is larger than the first sorted material M4-1. The first sorted material M4-1 has a size suitable for the subsequent production of the sheet S. It is preferable that the average length is 1 μm or more and 30 μm or less. On the other hand, the second sorted material M4-2 includes, for example, insufficiently defibrated material and material in which defibrated fibers are excessively aggregated.

[0080] The sorting unit 14 has a drum unit 141 and a housing unit 142 that houses the drum unit 141.

[0081] The drum part 141 is a sieve composed of a cylindrical mesh body and rotates around its central axis. The defibrated material M3 flows into this drum part 141. Then, as the drum part 141 rotates, the defibrated material M3 smaller than the mesh opening is sorted as the first sorted material M4-1, and the defibrated material M3 larger than the mesh opening is sorted as the second sorted material M4-2. The first sorted material M4-1 falls from the drum part 141.

[0082] Meanwhile, the second sorted material M4-2 is sent to a pipe 243 connected to the drum section 141. The pipe 243 is connected to the pipe 241 on the side opposite the drum section 141, i.e., the upstream side. The second sorted material M4-2 that passes through this pipe 243 merges with the coarsely crushed pieces M2 in the pipe 241 and flows into the defibrating section 13 together with the coarsely crushed pieces M2. As a result, the second sorted material M4-2 is returned to the defibrating section 13 and is defibrated together with the coarsely crushed pieces M2.

[0083] The first selected object M4-1 that has fallen from the drum unit 141 falls while being dispersed in the air, and heads toward the first web forming unit 15 located below the drum unit 141. The first web forming unit 15 is a section that carries out a first web forming step of forming a first web M5 from the first selected object M4-1. The first web forming unit 15 has a mesh belt 151, three tension rollers 152, and a suction unit 153.

[0084] The mesh belt 151 is an endless belt on which the first sorted material M4-1 is accumulated. The mesh belt 151 is wound around three tension rollers 152. As the tension rollers 152 rotate, the first sorted material M4-1 on the mesh belt 151 is transported downstream.

[0085] The size of the first sorted material M4-1 is equal to or larger than the mesh size of the mesh belt 151. This restricts the passage of the first sorted material M4-1 through the mesh belt 151, and therefore the first sorted material M4-1 can be piled up on the mesh belt 151. Furthermore, the first sorted material M4-1 is transported downstream together with the mesh belt 151 while being piled up on the mesh belt 151, and is thus formed as a layered first web M5.

[0086] In addition, the first sorted material M4-1 may contain, for example, dust or dirt. Dust or dirt may be generated, for example, by crushing or defibrating. Such dust or dirt will be collected in the collection section 27.

[0087] The suction unit 153 is a suction mechanism that sucks air from below the mesh belt 151. This makes it possible to suck in dust and dirt that has passed through the mesh belt 151 together with the air.

[0088] In addition, the suction unit 153 is connected to the collection unit 27 via a pipe 244. The dust and dirt sucked by the suction unit 153 is collected in the collection unit 27.

[0089] A pipe 245 is further connected to the collection unit 27. A blower 262 is installed in the middle of the pipe 245. By operating the blower 262, a suction force can be generated in the suction unit 153. This promotes the formation of the first web M5 on the mesh belt 151. Dust and dirt are removed from this first web M5. By operating the blower 262, the dust and dirt pass through the pipe 244 and reach the collection unit 27.

[0090] The housing part 142 is connected to the humidifying part 232. The humidifying part 232 is configured as an evaporative humidifier. This allows humidified air to be supplied into the housing part 142. The above-mentioned humidifying process can be performed by this humidified air, and the above-mentioned effects can be obtained. In addition, the first sorted object M4-1 can be humidified, and therefore, the first sorted object M4-1 can be prevented from adhering to the inner wall of the housing part 142 due to electrostatic force.

[0091] The humidifying section 235 is disposed downstream of the sorting section 14. The humidifying section 235 is configured with an ultrasonic humidifier that sprays water. This allows moisture to be supplied to the first web M5, and the above-mentioned humidifying process can be performed, thereby obtaining the above-mentioned effects. In addition, adhesion of the first web M5 to the mesh belt 151 due to electrostatic force can be suppressed. This allows the first web M5 to be easily peeled off from the mesh belt 151 at the position where the mesh belt 151 is folded back by the tension roller 152.

[0092] The segmentation unit 16 is disposed downstream of the humidification unit 235. The segmentation unit 16 is a section that performs a segmentation step of segmenting the first web M5 peeled off from the mesh belt 151. The segmentation unit 16 has a rotatably supported propeller 161 and a housing portion 162 that houses the propeller 161. The rotating propeller 161 can segment the first web M5. The segmented first web M5 becomes segmented bodies M6. The segmented bodies M6 move down inside the housing portion 162.

[0093] The housing part 162 is connected to the humidifying part 233. The humidifying part 233 is configured as an evaporation type humidifier. This allows humidified air to be supplied into the housing part 162. The humidifying process can be performed by this humidified air, and the above-mentioned effects can be obtained. In addition, it is also possible to prevent the fragmented bodies M6 from adhering to the propeller 161 and the inner wall of the housing part 162 due to electrostatic force.

[0094] A mixing section 17 is disposed downstream of the subdivision section 16. The mixing section 17 is a section in which a mixing step is performed to mix the subdivision bodies M6 and the binding material P1. The mixing section 17 has an additive supply section 171, a pipe 172, and a blower 173.

[0095] The pipe 172 connects the housing portion 162 of the subdivision portion 16 and the housing 182 of the dispersion portion 18, and is a flow path through which the mixture M7 of the subdivision bodies M6 and the binding material P1 passes.

[0096] An additive supply unit 171 is connected to the middle of the pipe 172. The additive supply unit 171 has a housing portion 170 in which a binding material is accommodated, and a screw feeder 174 provided in the housing portion 170. By the rotation of the screw feeder 174, the binding material in the housing portion 170 is pushed out from the housing portion 170 and supplied into the pipe 172. The binding material P1 supplied into the pipe 172 is mixed with the fragmented bodies M6 to become a mixture M7.

[0097] Here, the binding material P1 supplied from the additive supply unit 171 may contain, for example, a colorant for coloring the fibers, an aggregation inhibitor for inhibiting aggregation of the fibers, a flame retardant for making the fibers etc. less flammable, a paper strength enhancer for enhancing the paper strength of the sheet S, defibrated material, etc., and one or a combination of multiple types of these may be used.

[0098] By supplying the binding material P1 from the additive supply unit 171, the binding material P1 can be adhered with high uniformity to the fibers constituting the sheet S. That is, since the average particle size of the powder of the binding material P1 is small, it is possible to suppress unevenness in the composition in the mixture and variation in the composition of the sheet S as the final molded body, and the like, and the reliability of the sheet S can be improved.

[0099] In addition, a blower 173 is installed in the middle of the pipe 172 downstream of the additive supply section 171. The action of a rotating section such as a blade of the blower 173 promotes mixing of the fragmented bodies M6 and the binding material P1. In addition, the blower 173 can generate an airflow toward the dispersion section 18. This airflow can agitate the fragmented bodies M6 and the binding material P1 in the pipe 172. As a result, the mixture M7 is transported to the dispersion section 18 in a state in which the fragmented bodies M6 and the binding material P1 are uniformly dispersed. In addition, the fragmented bodies M6 in the mixture M7 are loosened in the process of passing through the pipe 172, becoming finer fibrous.

[0100] 1, blower 173 is electrically connected to control unit 28, and the operation thereof is controlled by blower 173. By adjusting the airflow rate of blower 173, the amount of air sent into drum 181 can be adjusted.

[0101] Although not shown in the figure, the end of pipe 172 on the drum 181 side is branched into two, and the branched ends are each connected to an inlet port (not shown) formed on the end face of drum 181.

[0102] 1 is a section that performs a discharging step of loosening and discharging entangled fibers in the mixture M7. The dispersing section 18 has a drum 181 that introduces and discharges the defibrated mixture M7, a housing 182 that contains the drum 181, and a drive source 183 that drives the drum 181 to rotate.

[0103] The drum 181 is a sieve that is composed of a cylindrical mesh body and rotates around its central axis. As the drum 181 rotates, fibers and the like of the mixture M7 that are smaller than the mesh openings can pass through the drum 181. At that time, the mixture M7 is loosened and discharged together with air. That is, the drum 181 functions as a discharge section that discharges the material including fibers.

[0104] Although not shown, the driving source 183 has a motor, a reducer, and a belt. The motor is electrically connected to the control unit 28 via a motor driver. Furthermore, the rotational force output from the motor is reduced by the reducer. The belt is, for example, an endless belt, and is wound around the output shaft of the reducer and the outer periphery of the drum. As a result, the rotational force of the output shaft of the reducer is transmitted to the drum 181 via the belt.

[0105] The housing 182 is also connected to the humidifying section 234. The humidifying section 234 is configured as an evaporative humidifier. This allows humidified air to be supplied into the housing 182. The inside of the housing 182 can be humidified by this humidified air, and the humidifying process can be performed, thereby obtaining the above-mentioned effects. In addition, it is also possible to prevent the mixture M7 from adhering to the inner wall of the housing 182 due to electrostatic force.

[0106] Furthermore, the mixture M7 discharged from the drum 181 falls while being dispersed in the air, and heads toward the second web forming unit 19 located below the drum 181. The second web forming unit 19 is a section where a deposition step is carried out in which the mixture M7 is deposited to form a second web M8, which is a deposit. The second web forming unit 19 has a mesh belt 191, a tension roller 192, and a suction unit 193.

[0107] The mesh belt 191 is a mesh member, and in the illustrated configuration, is configured as an endless belt. The mixture M7 dispersed and discharged by the dispersion unit 18 is accumulated on the mesh belt 191. The mesh belt 191 is wound around four tension rollers 192. The mixture M7 on the mesh belt 191 is transported downstream by the rotational drive of the tension rollers 192.

[0108] In the illustrated configuration, the mesh belt 191 is used as an example of the mesh member, but the present invention is not limited to this, and the mesh member may be, for example, a flat plate-like member.

[0109] Moreover, most of the mixture M7 on the mesh belt 191 has a size equal to or larger than the mesh openings of the mesh belt 191. This prevents the mixture M7 from passing through the mesh belt 191, and therefore the mixture M7 can be accumulated on the mesh belt 191. Moreover, the mixture M7 is transported downstream together with the mesh belt 191 while being accumulated on the mesh belt 191, and is thus formed as a layered second web M8.

[0110] The suction unit 193 is a suction mechanism that sucks air from below the mesh belt 191. This allows the mixture M7 to be sucked onto the mesh belt 191, thereby facilitating the accumulation of the mixture M7 on the mesh belt 191.

[0111] A pipe 246 is connected to the suction unit 193. A blower 263 is provided midway through the pipe 246. By operating the blower 263, the suction unit 193 can generate a suction force.

[0112] The humidifying section 236 is disposed downstream of the dispersion section 18. The humidifying section 236 is configured with an ultrasonic humidifier similar to the humidifying section 235. This allows moisture to be supplied to the second web M8. This allows the humidifying process to be performed, and the above-mentioned effects to be obtained. In addition, the adhesion of the second web M8 to the mesh belt 191 due to electrostatic force can be suppressed. This allows the second web M8 to be easily peeled off from the mesh belt 191 at the position where the mesh belt 191 is folded back by the tension roller 192.

[0113] The total amount of moisture added from humidifier 231 to humidifier 236 is not particularly limited, but it is preferable that the moisture content of the web at the end of the humidification process, i.e., the ratio of the mass of moisture contained in second web M8 to the mass of second web M8 in a state humidified by humidifier 236, be 1.0 mass% or more and 30.0 mass% or less.

[0114] At least one moistening step is performed before the second web M8 is formed, and at least a part of the binding material P1 adheres to the fibers of the second web M8. If the moistening step is not performed before the second web M8 is formed, the moistening step is performed on the second web M8 by the moistening section 236, and moisture is added to the second web M8.

[0115] A forming section 20 is disposed downstream of the second web forming section 19. The forming section 20 is a section in which a sheet forming step is performed to form a sheet S from the second web M8, which is a mixture. The forming section 20 has a pressurizing section 201 and a heating section 202.

[0116] The pressurizing unit 201 has a pair of calender rollers 203, and can pressurize the second web M8 between the calender rollers 203 without heating it. This increases the density of the second web M8. The second web M8 is transported toward the heating unit 202. Note that one of the pair of calender rollers 203 is a driven roller driven by the operation of a motor (not shown), and the other is a driven roller.

[0117] The heating section 202 has a pair of heating rollers 204, and can apply pressure to the second web M8 while heating it between the heating rollers 204. By this heating and pressurization, the binding material that has absorbed water due to humidification adheres to the fibers in the second web M8, and by pressurizing and heating the second web M8 together with the binding material, the fibers are bonded together via the binding material. In this way, a sheet S is formed. Then, this sheet S is transported toward the cutting section 21. One of the pair of heating rollers 204 is a driven roller driven by the operation of a motor (not shown), and the other is a driven roller.

[0118] The cutting unit 21 is disposed downstream of the forming unit 20. The cutting unit 21 is a portion that performs a cutting step of cutting the sheet S. The cutting unit 21 has a first cutter 211 and a second cutter 212.

[0119] The first cutter 211 cuts the sheet S in a direction intersecting the conveying direction of the sheet S, particularly in a direction perpendicular to the conveying direction.

[0120] The second cutter 212 is located downstream of the first cutter 211 and cuts the sheet S in a direction parallel to the conveying direction of the sheet S. This cutting is performed to remove unnecessary portions on both side edges of the sheet S in the width direction to adjust the width of the sheet S, and the cut and removed portions are so-called "selvages."

[0121] A sheet S having a desired shape and size is obtained by such cutting by the first cutter 211 and the second cutter 212. Then, this sheet S is conveyed further downstream and accumulated in the stock unit 22.

[0122] Each unit included in the molded body manufacturing apparatus 100 is electrically connected to a control unit 28, which will be described later. The operation of each unit is controlled by the control unit 28.

[0123] Although the preferred embodiments of the present invention have been described above, the present invention is not limited to these.

[0124] For example, each part constituting the molded body manufacturing apparatus used for manufacturing the molded body can be replaced with any other part capable of exerting the same function. Any other components may be added. The molded body manufacturing method of the present invention may include the above-mentioned mixing step, humidifying step, and molding step, and may use any other device, not limited to the above-mentioned molded body manufacturing apparatus.

[0125] 3. Examples and Comparative Examples The present invention will be further described below with reference to examples and comparative examples, but the present invention is not limited to the following examples in any way.

[0126] 3.1. Preparation of evaluation samples For each example, a sheet S was produced as a molded body using a molded body production apparatus 100 as shown in FIG. 1 in the following manner.

[0127] First, a number of sheets of G80 (manufactured by Mitsubishi Paper Mills) made of cellulose fiber were prepared as the fiber raw material M1, and these were stored in the storage section of the sheet supplying device 11, while the starch or dextrin of each example was stored in the housing section 170 of the additive supplying section 171. Thereafter, the molded body manufacturing apparatus 100 was operated as described above.

[0128] As a result, in the mixing section 17, the fibers and the binder material were mixed at 6.0 mass % with respect to the total mass of the mixture, and a mixture M7 was obtained.

[0129] The mixture M7 obtained in the mixing section 17 passed through the dispersing section 18 and was made into a second web M8 containing fibers and a binder material in the second web forming section 19.

[0130] Humidification was performed in humidifying section 231, humidifying section 232, humidifying section 233, humidifying section 234, humidifying section 235, and humidifying section 236, respectively, so that the ratio of the mass of moisture contained in second web M8 to the mass of second web M8 in a humidified state in humidifying section 236 became the moisture content (mass %) (water / web; mass basis) in Table 1. The moisture content was measured using a heat-drying moisture meter MS-70 manufactured by A&D Corporation.

[0131] The second web M8 was heated and pressurized in the forming section 20 to become a sheet S, which was a long formed body. The heating temperature in the forming section 20 was 80° C., the heating time was 15 seconds, and the pressure in the forming section 20 was 70 MPa.

[0132] The sheet S, which is a long molded product thus obtained, was cut at the cutting section 21 into sheets S of A4 size.

[0133] The starch used in each example was soybean-derived acid-treated starch (NSP-EA, manufactured by Nippon Starch Chemical Co., Ltd.), and the volume average particle size (D50) was adjusted by pulverizing the starch with a nanojetmizer. The dextrin used in each example was tapioca-derived yellow dextrin (ND-S, manufactured by Nippon Starch Chemical Co., Ltd.), and the volume average particle size (D50) was adjusted by pulverizing the dextrin with a nanojetmizer.

[0134] [Table 1]

[0135] Evaluation The molded articles (sheets) of each of the Examples and Comparative Examples were subjected to the following tensile strength index evaluation. For each example sheet, measurements were carried out in accordance with JIS P8113 using an AUTOGRAP AGC-X 500N (Shimadzu Corporation) to determine the specific tensile strength (N m / g), which was then evaluated as paper strength according to the following criteria, with the results shown in Table 1. Note that for the recycled compacts, the following evaluation was carried out using the rate of decrease in the specific tensile strength of the recycled compact relative to the tensile strength of the raw material compact before recycling.

[0136] A: Tensile strength is 20.0 (N·m / g) or more B: Specific tensile strength is 10.0 (N·m / g) or more and less than 20.0 (N·m / g) C: Specific tensile strength is 10.0 (N·m / g) or more but less

[0137] As is clear from Table 1, excellent results were obtained in each of the Examples in which the average particle size (D50) of the binder powder was 20.0 μm or less. In other words, the molded bodies obtained in each Example were able to obtain excellent mechanical strength while ensuring biodegradability. It was also found that the molded bodies in each Example could be molded with a low moisture content and achieved sufficient mechanical strength. Furthermore, looking at Examples 6, 7, 10, and 11, it was found that the use of dextrin provided a superior tensile strength index compared to the use of starch.

[0138] On the other hand, Reference Example 1 shows that even if the average particle size of starch is large, the tensile strength index is good if the moisture content is high, but the energy required to evaporate the moisture is large, which is not preferable. Also, in each of the comparative examples in which the average particle size exceeds 20.0 μm, the biodegradability is considered to be good, but the mechanical strength is insufficient.

[0139] The present invention includes configurations that are substantially the same as the configurations described in the embodiments, for example, configurations with the same functions, methods, and results, or configurations with the same purpose and effects. The present invention also includes configurations in which non-essential parts of the configurations described in the embodiments are replaced. The present invention also includes configurations that achieve the same effects as the configurations described in the embodiments, or configurations that can achieve the same purpose. The present invention also includes configurations in which publicly known technology is added to the configurations described in the embodiments.

[0140] The following can be derived from the above-described embodiment and modified examples.

[0141] The method for producing the molded body includes the steps of: A mixing step of mixing the fibers and the powder of the binder material to obtain a mixture; depositing the mixture to form a web; a moistening step of applying water to the web; a molding step of heating and pressing the web to which water has been applied to obtain a molded body; A method for producing a molded body comprising the steps of: The binding material binds the fibers together when water is applied thereto, The powder has an average particle size (D50) of 20.0 μm or less.

[0142] In the method for producing the molded body, The powder may have an average particle size (D50) of 1.0 μm or more.

[0143] According to this manufacturing method of molded products, when a binding material capable of binding fibers together by adding moisture is supplied to a web as a powder, the particles of the powder are small, so the added moisture easily penetrates into the powder, and therefore a dry molded product can be manufactured with a small amount of moisture. This also makes it possible to use a natural binding material and reduce the amount of energy consumed for drying the moisture.

[0144] In the method for producing the molded body, The binding material may be selected from starch and dextrin.

[0145] According to this method for producing a molded body, it is easy to obtain the binding material and adjust the average particle size of the powder.

[0146] In the method for producing the molded body, In the moistening step, the web may be moistened so that the moisture content of the web is 7.0% by mass or more and 50.0% by mass or less with respect to the total mass of the web.

[0147] According to this method for producing a molded body, a dry molded body can be produced with a small amount of water, which further reduces the amount of energy consumed for drying the water.

[0148] In the method for producing the molded body, The content of the binding material in the web may be 1.0% by mass or more and 30.0% by mass or less with respect to the total mass of the web.

[0149] According to this method for producing a molded article, since a sufficient amount of binding material is contained in the web, for example, the web can be stably transported during the production process.

[0150] In the method for producing the molded body, The heating temperature may be 50.0°C or higher and 100.0°C or lower.

[0151] According to this method for producing a molded body, a molded body can be produced by heating at a relatively low temperature, as compared with the conventional method using a resin as a binder. [Explanation of symbols]

[0152] 100... Molded body manufacturing apparatus, 10A... Sheet processing apparatus, 10B... Fiber body depositing apparatus, 11... Sheet supplying apparatus, 12... Crushing section, 13... Defibration section, 14... Screening section, 15... First web forming section, 16... Dividing section, 17... Mixing section, 18... Dispersion section, 19... Second web forming section, 20... Molding section, 21... Cutting section, 22... Stock section, 27... Recovery section, 28... Control section, 121... Crushing blade, 122... Chute, 141... Drum section, 142... Housing section, 151... Mesh belt, 152... Tension roller, 153... Suction section, 161... Propeller, 162... Housing section, 170... Housing section, 171... Additive supply section, 172... Pipe, 173... Blower, 174... Screw feeder, 181... Drum, 182... Housing, 183... Drive Power source, 191... mesh belt, 192... tension roller, 193... suction section, 201... pressure section, 202... heating section, 203... calendar roller, 204... heating roller, 211... first cutter, 212... second cutter, 231... humidification section, 232... humidification section, 233... humidification section, 234... humidification section, 235... humidification section, 236... humidification section, 241... tube, 242... tube , 243... pipe, 244... pipe, 245... pipe, 246... pipe, 261... blower, 262... blower, 263... blower, 281... CPU, 282... memory unit, M1... fiber raw material, M2... coarsely crushed pieces, M3... defibrated material, M4-1... first sorted material, M4-2... second sorted material, M5... first web, M6... finely divided body, M7... mixture, M8... second web, S... sheet, P1... bonding material

Claims

1. A mixing step of mixing the fibers and the powder of the binder material to obtain a mixture; depositing the mixture to form a web; a moistening step of applying water to the web; a molding step of heating and pressing the web to which water has been applied to obtain a molded body; A method for producing a molded body comprising the steps of: The binding material binds the fibers together when water is applied thereto, The method for producing a molded body, wherein the powder has an average particle size (D50) of 20.0 μm or less.

2. In claim 1, The method for producing a molded body, wherein the powder has an average particle size (D50) of 1.0 μm or more.

3. In claim 1 or 2, The method for producing a molded body, wherein the binding material is selected from starch and dextrin.

4. In any one of claims 1 to 3, The method for producing a shaped body, wherein in the humidifying step, the web is humidified so that the moisture content of the web is 7.0 mass % or more and 50.0 mass % or less with respect to the total mass of the web.

5. In any one of claims 1 to 4, A method for producing a molded body, wherein the content of the bonding material in the web is 1.0 mass % or more and 30.0 mass % or less with respect to the total mass of the web.

6. In any one of claims 1 to 5, The method for producing a molded body, wherein the heating temperature is 50.0°C or higher and 100.0°C or lower.

Citation Information

Patent Citations

  • Degradable nonwoven fabric

    JP1991027165A

  • Cellulose products using bulky cellulose fibers

    JP1997511029A

  • Paper recycling apparatus and paper recycling method

    JP2012144826A

  • Sheet production apparatus and sheet production method

    JP2015137437A

  • Fiber board and method for producing the same

    JP2016055620A