Resin composition, resin-coated metal foil, prepreg, laminate, multilayer printed wiring board, and semiconductor package
A resin composition with polyphenylene ether derivative, fluororesin filler, and titanate coupling agent addresses copper foil peel strength and resin powder adhesion issues, enhancing dielectric properties and performance in high-frequency applications.
Patent Information
- Application Number
- JP2020169851
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-07
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2040-10-07
AI Technical Summary
Existing resin compositions used in high-frequency applications suffer from reduced copper foil peel strength and resin powder adhesion during cutting, leading to contamination and poor dielectric properties.
A resin composition containing a polyphenylene ether derivative, fluororesin filler, and titanate coupling agent is formulated to enhance high-frequency properties and prevent resin powder fall-off during cutting, while maintaining strong copper foil adhesion.
The composition exhibits excellent dielectric properties above 10 GHz, suppresses resin powder fall-off, and improves copper foil peel strength, resulting in improved performance of resin-coated metal foils, prepregs, laminates, and multilayer printed wiring boards.
Smart Images

Figure 0007552218000031 
Figure 0007552218000032 
Figure 0007552218000033
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition, a resin-coated metal foil, a prepreg, a laminate, a multilayer printed wiring board, and a semiconductor package. [Background technology]
[0002] In mobile communication devices such as mobile phones, their base station equipment, network infrastructure devices such as servers and routers, and large computers, the speed and capacity of signals used are increasing year by year. Accordingly, the printed wiring boards mounted on these electronic devices must be compatible with higher frequencies, and there is a demand for board materials with excellent dielectric properties in high frequency bands that enable reduction in transmission loss. In recent years, in addition to the electronic devices mentioned above, new systems that handle high frequency wireless signals are being planned and put into practical use in the ITS field (related to automobiles and traffic systems) and in the field of indoor short-range communications, as applications that handle such high frequency signals. Therefore, it is expected that in the future, low transmission loss board materials will also be required for the printed wiring boards mounted on these devices.
[0003] Polyphenylene ether (PPE) resins have been used as thermoplastic polymers with excellent high-frequency characteristics. For example, a resin composition containing polyphenylene ether and an epoxy resin (see, for example, Patent Document 1) and a resin composition containing polyphenylene ether and a cyanate resin (see, for example, Patent Document 2) are known. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 58-069046 [Patent Document 2] Special Publication No. 61-018937 Summary of the Invention [Problem to be solved by the invention]
[0005] In recent years, there has been a strong demand for the development of a resin composition with improved dielectric properties (low dielectric constant and low dielectric loss tangent; hereinafter, sometimes referred to as high frequency properties) in the 10 GHz band or higher that can be used for fifth generation mobile communication system (5G) antennas that use radio waves in a frequency band exceeding 6 GHz and millimeter wave radars that use radio waves in a frequency band of 30 to 300 GHz. In other words, there is a demand for resin compositions that have even better high frequency properties than conventional ones. Furthermore, a resin-coated metal foil having a layer of a resin composition on the metal foil may be used in the manufacture of a metal-clad laminate, and this resin-coated metal foil is usually cut by a cutter to adjust the size. In this case, resin powder may adhere to the blade of the cutter (hereinafter also referred to as the slit blade) due to powder falling off the end of the resin-coated metal foil. Such contamination of the slit blade may cause waviness and resin cracks on the cut surface, or the resin adhering to the slit blade may fall onto the resin-coated metal foil, thereby contaminating the product. In order to solve the above problems, the present inventors investigated the blending of components having excellent high-frequency characteristics and found that although the high-frequency characteristics of the resin composition were improved, the copper foil peel strength was reduced.
[0006] In view of the current situation, the present invention aims to provide a resin composition that exhibits excellent dielectric properties in the high frequency band of 10 GHz or more, suppresses powder falling off at the ends when the resin-coated metal foil is cut, and has excellent copper foil peel strength, as well as a resin-coated metal foil, a prepreg, a laminate, a multilayer printed wiring board, and a semiconductor package that use the resin composition. [Means for solving the problem]
[0007] As a result of extensive research to achieve the above-mentioned object, the inventors have discovered that a resin composition containing a polyphenylene ether derivative, a fluororesin filler and a titanate coupling agent exhibits excellent high-frequency characteristics, suppresses powder falling off at the edges when the resin-coated metal foil is cut, and has excellent copper foil peel strength, thereby completing the present invention.
[0008] That is, one embodiment of the present invention relates to the following [1] to
[20] . [1] A resin composition comprising a polyphenylene ether derivative (A), a fluororesin filler (B), and a titanate coupling agent (X). [2] The resin composition according to the above [1], wherein the component (A) has an ethylenically unsaturated bond-containing group at a molecular terminal. [3] The resin composition according to the above [1] or [2], wherein the ethylenically unsaturated bond-containing group of the component (A) is a (meth)acrylic group. [4] The resin composition according to any one of the above [1] to [3], wherein the weight average molecular weight (Mw) of the component (A) is 500 to 7,000. [5] The resin composition according to any one of the above [1] to [4], wherein the component (B) is at least one selected from the group consisting of polytetrafluoroethylene (PTFE) filler, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA) filler, tetrafluoroethylene-hexafluoropropylene copolymer (FEP) filler, tetrafluoroethylene-ethylene copolymer (ETFE) filler, and polychlorotrifluoroethylene (PCTFE) filler. [6] The resin composition according to any one of the above [1] to [5], wherein the average particle size of the component (B) is 0.1 to 10 μm. [7] The resin composition according to any one of the above [1] to [6], wherein the content of the component (B) is 1% by mass or more and less than 50% by mass based on the solid content of the resin composition. [8] The resin composition according to any one of the above [1] to [7], wherein the content of the component (B) is 1 to 40 mass % based on the solid content of the resin composition. [9] The resin composition according to any one of the above [1] to [8], wherein the component (X) has a hydroxy group and a hydrocarbon group.
[10] The resin composition according to the above [9], wherein the hydrocarbon group contains a hydrocarbon group having 1 to 4 carbon atoms and a hydrocarbon group having 5 to 30 carbon atoms.
[11] The resin composition according to any one of the above [1] to
[10] , further comprising one or more thermosetting resins (C) selected from the group consisting of epoxy resins, cyanate resins and maleimide compounds.
[12] The resin composition according to the above
[11] , which contains the maleimide compound as the component (C), and which is a modified maleimide compound having a structural unit derived from a maleimide compound (c1) having at least two N-substituted maleimide groups and a structural unit derived from an amine compound (c2) having a primary amino group.
[13] The resin composition according to the above
[12] , wherein the modified maleimide compound is a compound represented by the following general formula (C-1): [ka] (In the formula, X c1 and X c2 are each independently a divalent organic group.
[14] The resin composition according to any one of the above
[11] to
[13] , wherein a content ratio of the component (A) to the component (C) [(A) / (C)], in terms of mass ratio, is 5 / 95 to 80 / 20.
[15] The resin composition according to any one of the above [1] to
[14] , further comprising one or more members selected from the group consisting of a thermoplastic elastomer (D), a curing accelerator (E) and an inorganic filler (F).
[16] A resin-coated metal foil having a layer of the resin composition according to any one of the above [1] to
[15] on the metal foil.
[17] A prepreg comprising the resin composition according to any one of the above [1] to
[15] and a sheet-like fiber reinforcing substrate.
[18] A laminate comprising (i) the resin-coated metal foil according to
[16] above or (ii) the prepreg and metal foil according to
[17] above.
[19] A multilayer printed wiring board comprising: (i) the resin-coated metal foil according to
[16] above; (ii) the prepreg according to
[17] above; or (iii) the laminate according to
[18] above.
[20] A semiconductor package comprising the multilayer printed wiring board according to
[19] above and a semiconductor element mounted thereon. Effect of the Invention
[0009] The present invention can provide a resin composition that exhibits excellent dielectric properties in high frequency bands of 10 GHz or more, suppresses powder falling off at the ends when the resin-coated metal foil is cut, and has excellent copper foil peel strength, as well as a resin-coated metal foil, a prepreg, a laminate, a multilayer printed wiring board, and a semiconductor package that use the resin composition. [Brief description of the drawings]
[0010] [Figure 1] 1 is a photograph of a slit blade of a cutter used in evaluating edge powder fall when cutting resin-coated copper foil in Examples and Comparative Examples. [Diagram 2] FIG. 2 is a schematic diagram showing the state of a slit blade when edge powder fall during cutting of a resin-coated copper foil is evaluated as "A" in Examples and Comparative Examples. [Diagram 3] FIG. 2 is a schematic diagram showing the state of a slit blade when edge powder fall during cutting of a resin-coated copper foil is evaluated as “C” in Examples and Comparative Examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] In the numerical ranges described in this specification, the upper or lower limit of the numerical range may be replaced with the values shown in the examples. In addition, the lower and upper limits of a numerical range may be arbitrarily combined with the lower or upper limit of another numerical range. In the expression of a numerical range "AA to BB", the numerical values AA and BB at both ends are included in the numerical range as the lower and upper limits, respectively. In addition, each component and material exemplified in this specification may be used alone or in combination of two or more types, unless otherwise specified. In this specification, the content of each component in the composition means the total amount of the multiple substances present in the composition when multiple substances corresponding to each component are present in the composition, unless otherwise specified. Any combination of the descriptions in this specification is also included in the present invention and this embodiment. In this embodiment, the term "resin component" is defined as all components among the solid contents constituting the resin composition, excluding inorganic compounds such as inorganic fillers, which will be described later, and flame retardants and flame retardant assistants. In addition, the solid content in the present embodiment refers to components in the resin composition other than volatile substances such as water, the solvent described below, etc. In other words, the solid content includes those that are liquid, syrup-like, or wax-like at room temperature around 25° C., and does not necessarily mean that they are solid.
[0012] [Resin composition] The resin composition of this embodiment is a resin composition containing a polyphenylene ether derivative (A) [hereinafter sometimes abbreviated as "(A) component"], a fluororesin filler (B) [hereinafter sometimes abbreviated as "(B) component"], and a titanate coupling agent (X) [hereinafter sometimes abbreviated as "(X) component"]. The resin composition of this embodiment is preferably a thermosetting resin composition. In the resin composition of this embodiment, the total content of the (A) component, the (B) component, and the (X) component is preferably 15% by mass or more, more preferably 20% by mass or more, and even more preferably 30% by mass, based on the solid content of the resin composition. There is no particular upper limit to the total content of the (A) component, the (B) component, and the (X) component, and the total content may be 100% by mass, 80% by mass or less, 60% by mass or less, 50% by mass or less, or 45% by mass or less, based on the solid content of the resin composition. Hereinafter, each component contained in the resin composition of the present embodiment will be described.
[0013] <Polyphenylene ether derivative (A)> The polyphenylene ether derivative (A) is not particularly limited, and may be a known polyphenylene ether derivative, such as one having a structural unit represented by general formula (A-2) described later. In particular, from the viewpoint of high frequency characteristics and compatibility with the thermosetting resin (C) and thermoplastic elastomer (D) used as necessary, the polyphenylene ether derivative (A) is preferably a polyphenylene ether derivative having an ethylenically unsaturated bond-containing group at the molecular terminal, and more preferably a polyphenylene ether derivative having an ethylenically unsaturated bond-containing group at both molecular terminals. In this specification, the term "ethylenically unsaturated bond-containing group" refers to a substituent containing a carbon-carbon double bond capable of undergoing an addition reaction, and does not include a double bond in an aromatic ring. The polyphenylene ether derivative (A) may be used alone or in combination of two or more kinds.
[0014] Examples of the ethylenically unsaturated bond-containing group include unsaturated aliphatic hydrocarbon groups such as vinyl, allyl, 1-methylallyl, isopropenyl, 2-butenyl, 3-butenyl, and styryl groups; maleimide groups, and groups containing a heteroatom and an ethylenically unsaturated bond such as a group represented by the following general formula (A-1). Among these, the group represented by the following general formula (A-1) is preferred from the viewpoints of high-frequency characteristics and adhesion to a conductor.
[0015] [ka] (In the formula, R a1 represents a hydrogen atom or an alkyl group having 1 to 20 carbon atoms. * represents the bonding position.)
[0016] R a1 The alkyl group having 1 to 20 carbon atoms represented by may be any of a linear alkyl group, a branched alkyl group, or a cyclic alkyl group, and is preferably a linear alkyl group. The alkyl group preferably has 1 to 10 carbon atoms, more preferably 1 to 5 carbon atoms, further preferably 1 to 3 carbon atoms, and particularly preferably 1 carbon atom. Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a decyl group, a pentadecyl group, a hexadecyl group, and a heptadecyl group. Of these, a methyl group is preferable. The group represented by the above general formula (A-1) is preferably a (meth)acrylic group [i.e., R a1 is a hydrogen atom or a methyl group, and is more preferably a methacryl group. In the present embodiment, the term "(meth)acryl group" refers to an acryl group or a methacryl group.
[0017] In this specification, groups which contain an unsaturated aliphatic hydrocarbon group in a portion thereof, such as a maleimide group or a group represented by the above general formula (A-1), but which cannot be considered an unsaturated aliphatic hydrocarbon group when viewed as a whole, are not included in the above "unsaturated aliphatic hydrocarbon group".
[0018] The number of ethylenically unsaturated bond-containing groups in one molecule of the polyphenylene ether derivative (A) is not particularly limited, but is preferably 2 to 5, more preferably 2 to 3, and even more preferably 2. When the number of ethylenically unsaturated bond-containing groups is equal to or greater than the above lower limit, excellent high-frequency characteristics and good compatibility with the thermosetting resin (C) and thermoplastic elastomer (D) described below tend to be obtained. On the other hand, when the number of ethylenically unsaturated bond-containing groups is equal to or less than the above upper limit, excellent flowability and moldability tend to be obtained. As described above, the polyphenylene ether derivative (A) preferably has an ethylenically unsaturated bond-containing group at the molecular end, and may further have an ethylenically unsaturated bond-containing group at other than the molecular end, but more preferably has an ethylenically unsaturated bond-containing group only at the molecular end. The polyphenylene ether derivative (A) is preferably a polyphenylene ether having a methacryl group at the molecular end, and more preferably a polyphenylene ether having methacryl groups at both molecular ends. The methacryl group may be bonded to an oxygen atom, that is, may be a methacryloyl group.
[0019] The polyphenylene ether derivative (A) has a phenylene ether bond, and preferably has a structural unit represented by the following general formula (A-2).
[0020] [ka] (In the formula, R a2 represents an aliphatic hydrocarbon group having 1 to 5 carbon atoms or a halogen atom. a1 represents an integer from 0 to 4.
[0021] R in the above general formula (A-2) a2 Examples of the aliphatic hydrocarbon group having 1 to 5 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a t-butyl group, an n-pentyl group, etc. As the aliphatic hydrocarbon group, an aliphatic hydrocarbon group having 1 to 3 carbon atoms is preferable, an alkyl group having 1 to 3 carbon atoms is more preferable, and a methyl group is further preferable. n a1 represents an integer of 0 to 4, preferably 1 or 2, and more preferably 2. a1 If is 1 or 2, R a2 is preferably substituted at the ortho position on the benzene ring (based on the substitution position of the oxygen atom). a1 If is an integer equal to or greater than 2, multiple R a2They may be the same or different. The structural unit represented by the above general formula (A-2) is preferably a structural unit represented by the following general formula (A-2').
[0022] [ka]
[0023] From the viewpoints of high-frequency characteristics and adhesion to a conductor, the polyphenylene ether derivative (A) is preferably a compound represented by the following general formula (A-3).
[0024] [ka] (In the formula, R a2 and n a1 is as described above in relation to the general formula (A-2). a3 and R a4 Each of n independently represents an aliphatic hydrocarbon group having 1 to 5 carbon atoms or a halogen atom. a2 and n a3 Each independently represents an integer of 0 to 4. a4 and n a5 Each independently represents an integer of 0 to 20, a4 and n a5 The sum of is an integer between 1 and 30. a1 represents an alkylene group having 1 to 5 carbon atoms, an alkylidene group having 2 to 5 carbon atoms, an ether group, a sulfide group, a sulfonyl group, a carbonyloxy group, a keto group, or a single bond. a1 and Y a2 each independently represents the above ethylenically unsaturated bond-containing group.
[0025] R in the above general formula (A-3) a3 and R a4 The aliphatic hydrocarbon group having 1 to 5 carbon atoms represented by R in the above general formula (A-2) is explained below. a2 This is the same as the explanation for the aliphatic hydrocarbon group having 1 to 5 carbon atoms represented by the formula (1). n a2and n a3 represents an integer of 0 to 4, preferably an integer of 0 to 3, and more preferably 2 or 3. a2 If is an integer equal to or greater than 2, multiple R a3 may be the same or different. a3 If is an integer equal to or greater than 2, multiple R a4 They may be the same or different from each other. n a4 and n a5 represents an integer of 0 to 20, preferably an integer of 1 to 20, more preferably an integer of 2 to 15, and further preferably an integer of 3 to 10. a4 or n a5 If is an integer equal to or greater than 2, multiple n a1 They may be the same or different. n a4 and n a5 The sum of these is an integer of 1 to 30, preferably an integer of 2 to 25, more preferably an integer of 5 to 20, and even more preferably an integer of 7 to 15.
[0026] X in the above general formula (A-3) a1 Examples of the alkylene group having 1 to 5 carbon atoms include a methylene group, a 1,2-dimethylene group, a 1,3-trimethylene group, a 1,4-tetramethylene group, and a 1,5-pentamethylene group. X a1 Examples of the alkylidene group having 2 to 5 carbon atoms include an ethylidene group, a propylidene group, an isopropylidene group, a butylidene group, an isobutylidene group, a pentylidene group, and an isopentylidene group. X a1 Among the groups represented by the formula (I), an isopropylidene group is preferred from the viewpoints of high frequency characteristics and adhesion to a conductor. Y a1 and Y a2 The preferred embodiments of the ethylenically unsaturated bond-containing group represented by are as described above. From the viewpoints of high-frequency characteristics and adhesion to a conductor, the compound represented by the above general formula (A-3) is preferably a compound represented by the following general formula (A-4).
[0027] [ka] (In the formula, n a4 and n a5 is as described above in relation to the general formula (A-3). a5 and R a6 Each of X independently represents a hydrogen atom or a methyl group. a2 represents a methylene group or an isopropylidene group.
[0028] [Weight average molecular weight (Mw) of polyphenylene ether derivative (A)] The weight average molecular weight (Mw) of the polyphenylene ether derivative (A) is not particularly limited, but is preferably 500 to 7,000, more preferably 800 to 5,000, even more preferably 1,000 to 3,000, and particularly preferably 1,200 to 2,500. When the weight average molecular weight (Mw) of the (A) component is equal to or greater than the lower limit, a cured product having excellent dielectric properties of polyphenylene ether and excellent heat resistance tends to be obtained. When the weight average molecular weight (Mw) of the (A) component is equal to or less than the upper limit, excellent moldability tends to be obtained. In this specification, the weight average molecular weight is a value calculated from a calibration curve using standard polystyrene by gel permeation chromatography (GPC), and more specifically, a value determined by the measurement method described in the examples.
[0029] The method for synthesizing the polyphenylene ether derivative (A) is not particularly limited, and known methods for synthesizing and modifying polyphenylene ether can be applied.
[0030] (Content of component (A)) The content of the polyphenylene ether derivative (A) in the resin composition of this embodiment is not particularly limited, but is preferably 1 to 80 parts by mass, more preferably 1 to 45 parts by mass, even more preferably 1 to 20 parts by mass, and particularly preferably 2 to 10 parts by mass, relative to 100 parts by mass of the total of the resin components. When the content of the (A) component is equal to or greater than the above lower limit, better high frequency characteristics and low moisture absorption tend to be obtained. When the content of the (A) component is equal to or less than the above upper limit, better heat resistance, moldability, and processability tend to be obtained.
[0031] <Fluororesin filler (B)> The resin composition of this embodiment contains the fluororesin filler (B), which provides excellent high-frequency characteristics and effectively prevents powder falling off at the ends when the resin-coated metal foil is cut. This effect is more pronounced when the components (A) and (B) are combined. The inclusion of the fluororesin filler (B) in the resin composition improves the high-frequency characteristics and prevents powder falling off at the ends when the resin-coated metal foil is cut, more effectively than the inclusion of the fluororesin itself in the resin composition. The shape of the fluororesin filler (B) may be, for example, particulate, powdery, needle-like, columnar, plate-like, scaly, etc. Of these, particulate is preferred. The fluororesin filler (B) may be used in the form of a slurry mixed with an organic solvent, such as ketone compounds such as acetone, methyl ethyl ketone, methyl isobutyl ketone (MIBK), and cyclohexanone. The fluororesin filler (B) may be used alone or in combination of two or more kinds.
[0032] Examples of the fluororesin filler (B) include polytetrafluoroethylene (PTFE) filler, tetrafluoroethylene-perfluoroalkylvinylether copolymer (PFA) filler, tetrafluoroethylene-hexafluoropropylene copolymer (FEP) filler, tetrafluoroethylene-ethylene copolymer (ETFE) filler, polychlorotrifluoroethylene (PCTFE) filler, etc. Among these, PTFE filler is preferred as the fluororesin filler (B) from the viewpoint of high frequency characteristics and suppression of powder falling off at the end when cutting the resin-coated metal foil. In addition, the surface of the fluororesin filler (B) may be coated with an inorganic filler. The average particle size of the fluororesin filler (B) is preferably 0.1 to 10 μm, more preferably 0.2 to 5 μm, further preferably 0.5 to 4.0 μm, and particularly preferably 1.5 to 4.0 μm. Here, the average particle size can be calculated, for example, by laser diffraction particle size distribution measurement, and the same applies hereinafter.
[0033] (B) Component Content The content of the fluororesin filler (B) is preferably 1% by mass or more and less than 50% by mass, more preferably 1 to 45% by mass, further preferably 1 to 40% by mass, particularly preferably 5 to 40% by mass, and may be 15 to 40% by mass or may be 25 to 40% by mass, based on the solid content of the resin composition. If the content of the fluororesin filler (B) is equal to or more than the lower limit, sufficient high-frequency characteristics tend to be obtained. On the other hand, if the content of the fluororesin filler (B) is less than 50% by mass based on the solid content of the resin composition, the decrease in adhesion between the metal foil and the organic components in the resin composition can be suppressed, and the decrease in heat resistance and copper foil peel strength tends to be avoided.
[0034] <Titanate coupling agent (X)> The resin composition of this embodiment contains a titanate coupling agent (X) in addition to the polyphenylene ether derivative (A) and the fluororesin filler (B), which allows the resin composition of this embodiment to exhibit excellent high-frequency characteristics, suppress powder falling off at the ends when the resin-coated metal foil is cut, and also provide excellent copper foil peel strength. The titanate coupling agent (X) may be used alone or in combination of two or more kinds, and may also be used in combination with a silane coupling agent.
[0035] From the viewpoint of copper foil peel strength, the titanate coupling agent (X) preferably has a hydroxy group and a hydrocarbon group. It is considered that the hydroxy group has affinity with the fluororesin filler (B), and therefore the titanate coupling agent (X) has a hydroxy group, so that the hydroxy group is oriented toward the fluororesin filler (B). Therefore, it is considered that the hydrocarbon group tends to be oriented in the opposite direction to the fluororesin filler (B). And, since the hydrocarbon group has a high affinity with the hydrocarbon group of the polyphenylene ether derivative (A) and the thermosetting resin (C) and thermoplastic elastomer (D) that are blended as necessary, it is presumed that the titanate coupling agent (X) plays a role as a binder between the polyphenylene ether derivative (A) and the thermosetting resin (C) and thermoplastic elastomer (D) that are blended as necessary and the fluororesin filler (B). As a result, it is presumed that the site with high affinity with copper foil in the resin composition is oriented toward the outside of the resin composition, and the copper foil peel strength tends to increase. In addition, when the titanate coupling agent (X) has a hydroxy group and a hydrocarbon group, the effect of suppressing aggregation of the fluororesin filler (B) in the resin composition tends to be enhanced.
[0036] The titanate coupling agent (X) may have a phosphorus atom or a phosphate group. The hydroxy group contained in the titanate coupling agent (X) may be a hydroxy group derived from a phosphate group. The hydrocarbon group contained in the titanate coupling agent (X) may include a hydrocarbon group having 1 to 4 carbon atoms and a hydrocarbon group having 5 to 30 carbon atoms. In particular, when the hydrocarbon group contained in the titanate coupling agent (X) includes a hydrocarbon group having 5 to 30 carbon atoms, the copper foil peel strength tends to be increased and the aggregation suppression effect of the fluororesin filler (B) in the resin composition tends to be enhanced. The number of carbon atoms in the hydrocarbon group having 1 to 4 carbon atoms may be 2 to 4 or 3. The number of carbon atoms in the hydrocarbon group having 5 to 30 carbon atoms may be 5 to 20, 6 to 18, 6 to 15, 6 to 12, or 6 to 10.
[0037] From the viewpoint of copper foil peel strength, the titanate coupling agent (X) is preferably a titanate coupling agent represented by the following general formula (X-1) or the following general formula (X-2), and more preferably a titanate coupling agent represented by the following general formula (X-1). [ka] (In the formula, R x1 R represents an organic group. x2 represents an organic group having a hydroxyl group and a hydrocarbon group. x2 may be the same or different.) [ka] (In the formula, R x3 represents an organic group. x3 may be bonded to each other. x4 represents an organic group having a hydroxyl group and a hydrocarbon group. x3 may be the same or different. x4 may be the same or different.)
[0038] (Explanation of each group in general formula (X-1)) R x1 The organic group represented by is not particularly limited, but is preferably an organic group having an alkyl group having 1 to 10 carbon atoms, more preferably an alkyl group having 1 to 10 carbon atoms, may be an alkyl group having 1 to 5 carbon atoms, may be an alkyl group having 2 to 4 carbon atoms, or may be an alkyl group having 3 carbon atoms. x1 may be an isopropyl group. R x1 The organic group represented by may or may not have a keto group, an ether group, or the like. R x2 In the "organic group having a hydroxy group and a hydrocarbon group" represented by the formula (1), the number of carbon atoms in the hydrocarbon group is not particularly limited, but is preferably 5 to 30, and may be 5 to 20, 6 to 18, 6 to 15, 6 to 12, or 6 to 10. The hydrocarbon group may be an octyl group. The Three R's x2 may be the same or different, but is preferably the same. R x2 The "organic group having a hydroxy group and a hydrocarbon group" represented by the formula (X-3) below may have a phosphate group, but is not particularly limited thereto.
[0039] [ka] (In the formula, R x5 and R x6 Each independently represents a hydrocarbon group. * indicates the bonding position.
[0040] In the general formula (X-3), R x5 and R x6 The number of carbon atoms in the hydrocarbon group represented by is not particularly limited, but is preferably 5 to 30, and may be 5 to 20, 6 to 18, 6 to 15, 6 to 12, or 6 to 10. The hydrocarbon group may be an octyl group. R x5 and R x6 may be the same or different, but is preferably the same.
[0041] (Explanation of each group in general formula (X-2)) R x3 The organic group represented by is not particularly limited, but is preferably an organic group having an alkyl group having 1 to 10 carbon atoms, more preferably an alkyl group having 1 to 10 carbon atoms, may be an alkyl group having 1 to 5 carbon atoms, may be an alkyl group having 2 to 4 carbon atoms, or may be an alkyl group having 3 carbon atoms. The Two R's x3 may be bonded to each other. Specifically, two R x3 may be bonded to each other to form, for example, a substituted or unsubstituted alkylene group. The number of carbon atoms in the alkylene group may be 1 to 5, 1 to 3, or 2. Examples of the substituent that the alkylene group may have include an oxy group (═O). R x4 In the "organic group having a hydroxy group and a hydrocarbon group" represented by the formula (1), the number of carbon atoms in the hydrocarbon group is not particularly limited, but is preferably 5 to 30, and may be 5 to 20, 6 to 18, 6 to 15, 6 to 12, or 6 to 10. The hydrocarbon group may be an octyl group. The Two R's x3 may be the same or different. x4 may be the same or different, but is preferably the same.
[0042] (Method of adding titanate coupling agent (X)) The method of adding the titanate coupling agent (X) to the resin composition may be a so-called integral blending method in which the titanate coupling agent (X) is added to a resin composition containing a fluororesin filler (B). Alternatively, the titanate coupling agent (X) may be added to a slurry in which the fluororesin filler (B) is dispersed in an organic solvent, and then the mixture is preferably stirred, and the resulting slurry is added to a resin composition containing the (A) component and other components as required. By adopting the method of adding the titanate coupling agent (X) to a slurry in which the fluororesin filler (B) is dispersed in an organic solvent, it is possible to obtain an effect of suppressing the settling of the fluororesin filler (B) in the slurry.
[0043] (Content of component (X)) The content of the titanate coupling agent (X) is not particularly limited, but is preferably 0.1 to 10 mass%, more preferably 0.1 to 5 mass%, further preferably 0.3 to 2.5 mass%, and particularly preferably 0.5 to 2.0 mass% relative to the fluororesin filler (B). When the content of the titanate coupling agent (X) is equal to or greater than the lower limit, the copper foil peel strength tends to be high. When the content of the titanate coupling agent (X) is equal to or less than the upper limit, the decrease in heat resistance caused by the decomposition of the group of the titanate coupling agent (X), such as a phosphate group, tends to be suppressed.
[0044] <Thermosetting resin (C)> The resin composition of the present embodiment preferably further contains one or more thermosetting resins (C) selected from the group consisting of epoxy resins, cyanate resins, and maleimide compounds. Among these, from the viewpoints of high-frequency characteristics, insulation reliability, adhesion to conductors, and flame retardancy, it is preferable that the thermosetting resin (C) contains a maleimide compound. The thermosetting resin (C) may be used alone or in combination of two or more kinds.
[0045] (Epoxy resin) The epoxy resin is preferably an epoxy resin having two or more epoxy groups in one molecule. Here, the epoxy resin is classified into glycidyl ether type epoxy resin, glycidyl amine type epoxy resin, glycidyl ester type epoxy resin, etc. Among these, glycidyl ether type epoxy resin is preferable. Epoxy resins are also classified into various epoxy resins depending on the difference in the main skeleton, and each of the above types of epoxy resins is further classified into bisphenol type epoxy resins such as bisphenol A type epoxy resins, bisphenol F type epoxy resins, and bisphenol S type epoxy resins; alicyclic epoxy resins such as dicyclopentadiene type epoxy resins; aliphatic linear epoxy resins; novolac type epoxy resins such as phenol novolac type epoxy resins, cresol novolac type epoxy resins, bisphenol A novolac type epoxy resins, bisphenol F novolac type epoxy resins, phenol aralkyl novolac type epoxy resins, and biphenyl aralkyl novolac type epoxy resins; stilbene type epoxy resins; naphthalene skeleton-containing epoxy resins such as naphthol novolac type epoxy resins and naphthol aralkyl type epoxy resins; biphenyl type epoxy resins; xylylene type epoxy resins; and dihydroanthracene type epoxy resins. When an epoxy resin is used, a curing agent, a curing assistant, etc. for the epoxy resin may be used in combination, if necessary.
[0046] (cyanate resin) Examples of cyanate resins include 2,2-bis(4-cyanatophenyl)propane, bis(4-cyanatophenyl)ethane, bis(3,5-dimethyl-4-cyanatophenyl)methane, 2,2-bis(4-cyanatophenyl)-1,1,1,3,3,3-hexafluoropropane, α,α'-bis(4-cyanatophenyl)-m-diisopropylbenzene, cyanate ester compounds of phenol-added dicyclopentadiene polymers, phenol novolac-type cyanate ester compounds, and cresol novolac-type cyanate ester compounds. When a cyanate resin is used, a curing agent, a curing assistant, etc. for the cyanate resin may be used in combination, if necessary.
[0047] (Maleimide compounds) The maleimide compound is preferably at least one selected from the group consisting of maleimide compounds (c1) having two or more N-substituted maleimide groups [hereinafter, sometimes simply referred to as "maleimide compound (c1)" or "(c1) component)] and derivatives thereof. In addition, examples of the "derivative" include an addition reaction product between a maleimide compound having two or more N-substituted maleimide groups and an amine compound such as a diamine compound described later.
[0048] The maleimide compound (c1) is not particularly limited as long as it is a maleimide compound having two or more N-substituted maleimide groups. Specific examples of the maleimide compound (c1) include aromatic maleimide compounds such as bis(4-maleimidophenyl)methane, polyphenylmethane maleimide, bis(4-maleimidophenyl)ether, bis(4-maleimidophenyl)sulfone, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide, 4-methyl-1,3-phenylene bismaleimide, m-phenylene bismaleimide, and 2,2-bis[4-(4-maleimidophenoxy)phenyl]propane; and aliphatic maleimide compounds such as 1,6-bismaleimido-(2,2,4-trimethyl)hexane and pyrrolidine acid binder type long chain alkyl bismaleimide. Among these, from the viewpoints of adhesion to the conductor and mechanical properties, the maleimide compound (c1) is preferably an aromatic maleimide compound, more preferably an aromatic bismaleimide compound, and even more preferably 2,2-bis[4-(4-maleimidophenoxy)phenyl]propane or 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide.
[0049] The maleimide compound (c1) is preferably a compound represented by the following general formula (C1-1).
[0050] [ka] (In the formula, X c1 represents a divalent organic group.
[0051] X in the above general formula (C1-1) c1 Examples of the divalent organic group represented by the formula (C1-2), (C1-3), (C1-4) or (C1-5) below can be mentioned.
[0052] [ka] (In the formula, R c1 represents an aliphatic hydrocarbon group having 1 to 5 carbon atoms or a halogen atom. c1 represents an integer of 0 to 4. * represents a bonding position.)
[0053] R c1 Examples of the aliphatic hydrocarbon group having 1 to 5 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a t-butyl group, an n-pentyl group, etc. As the aliphatic hydrocarbon group, an aliphatic hydrocarbon group having 1 to 3 carbon atoms is preferable, and a methyl group is more preferable. n c1 represents an integer of 0 to 4, and from the viewpoint of availability, an integer of 0 to 2 is preferable, and 0 is more preferable. c1 If is an integer equal to or greater than 2, multiple R c1 They may be the same or different.
[0054] [ka] (In the formula, R c2 and R c3 Each of X independently represents an aliphatic hydrocarbon group having 1 to 5 carbon atoms or a halogen atom. c2represents an alkylene group having 1 to 5 carbon atoms, an alkylidene group having 2 to 5 carbon atoms, an ether group, a sulfide group, a sulfonyl group, a carbonyloxy group, a keto group, a single bond, or a divalent group represented by the following general formula (C1-3-1): c2 and n c3 Each independently represents an integer of 0 to 4. * indicates a bonding position.)
[0055] R c2 and R c3 The aliphatic hydrocarbon group having 1 to 5 carbon atoms represented by R in the above general formula (C1-2) is explained below. c1 This is the same as the explanation for the aliphatic hydrocarbon group having 1 to 5 carbon atoms represented by the formula (1). X c2 Examples of the alkylene group having 1 to 5 carbon atoms include a methylene group, a 1,2-dimethylene group, a 1,3-trimethylene group, a 1,4-tetramethylene group, a 1,5-pentamethylene group, etc. As the alkylene group, an alkylene group having 1 to 3 carbon atoms is preferable, and a methylene group is more preferable. X c2 Examples of the alkylidene group having 2 to 5 carbon atoms include an ethylidene group, a propylidene group, an isopropylidene group, a butylidene group, an isobutylidene group, a pentylidene group, an isopentylidene group, etc. As the alkylidene group, an isopropylidene group is preferable. n c2 and n c3 represents an integer of 0 to 4, and from the viewpoint of availability, an integer of 0 to 2 is preferable, and 0 or 2 is more preferable. c2 If is an integer equal to or greater than 2, multiple R c2 may be the same or different. c3 If is an integer equal to or greater than 2, multiple R c3 They may be the same or different from each other. X c2 The divalent group represented by the general formula (C1-3-1) is as follows.
[0056] [ka] (In the formula, R c4 and R c5 Each of X independently represents an aliphatic hydrocarbon group having 1 to 5 carbon atoms or a halogen atom. c3 represents an alkylene group having 1 to 5 carbon atoms, an alkylidene group having 2 to 5 carbon atoms, an ether group, a sulfide group, a sulfonyl group, a carbonyloxy group, a keto group, or a single bond. c4 and n c5 Each independently represents an integer of 0 to 4. * indicates a bonding position.)
[0057] R c4 and R c5 The aliphatic hydrocarbon group having 1 to 5 carbon atoms represented by R in the above general formula (C1-2) is explained below. c1 This is the same as the explanation for the aliphatic hydrocarbon group having 1 to 5 carbon atoms represented by the formula (1). X c3 The alkylene group having 1 to 5 carbon atoms and the alkylidene group having 2 to 5 carbon atoms represented by the formula (C1-3) above are preferably represented by the formula (C1-4) c2 and the alkylene group having 1 to 5 carbon atoms and the alkylidene group having 2 to 5 carbon atoms represented by the formula (1) above. Among these, an isopropylidene group is preferred from the viewpoints of high frequency characteristics, adhesion to a conductor, heat resistance, glass transition temperature and thermal expansion coefficient. X c3 Among the groups represented by the formula (I), an alkylidene group having 2 to 5 carbon atoms is preferred, and an isopropylidene group is more preferred. n c4 and n c5 represents an integer of 0 to 4, and from the viewpoint of availability, an integer of 0 to 2 is preferable, and 0 is more preferable. c4 If is an integer equal to or greater than 2, multiple R c4 may be the same or different. c5 If is an integer equal to or greater than 2, multiple R c5 They may be the same or different from each other.
[0058] [ka] (In the formula, n c6 represents an integer from 1 to 10. * represents a bonding position.)
[0059] n c6 From the viewpoint of availability, an integer of 1 to 5 is preferable, and an integer of 1 to 3 is more preferable.
[0060] [ka] (In the formula, R c6 and R c7 Each of n independently represents a hydrogen atom or an aliphatic hydrocarbon group having 1 to 5 carbon atoms. c7 represents an integer of 1 to 8. * represents a bonding position.)
[0061] R c6 and R c7 The aliphatic hydrocarbon group having 1 to 5 carbon atoms represented by R in the above general formula (C1-2) is explained below. c1 This is the same as the explanation for the aliphatic hydrocarbon group having 1 to 5 carbon atoms represented by the formula (1). n c7 represents an integer of 1 to 8, preferably an integer of 1 to 3, and more preferably 1. n c7 If is an integer equal to or greater than 2, multiple R c6 may be the same or different, and multiple R c7 They may be the same or different from each other.
[0062] X in the above general formula (C1-1) c1 From the viewpoint of high frequency characteristics, the following formula (X c1 -1)~(X c1 -3), and is preferably a divalent group represented by the following formula (X c1 -3) is more preferable.
[0063] [ka] (In the formula, * indicates the bonding position with the nitrogen atom in the maleimide group.)
[0064] As the maleimide compound, from the viewpoints of solubility in organic solvents, compatibility, adhesion to conductors, and high-frequency characteristics, a derivative of the maleimide compound (c1) is preferred. The derivative of the maleimide compound (c1) is preferably a modified maleimide compound (Z) [hereinafter, sometimes abbreviated as "modified maleimide compound (Z)" or "(Z) component)] having a structural unit derived from the maleimide compound (c1) and a structural unit derived from an amine compound (c2) having a primary amino group [hereinafter, sometimes abbreviated as "amine compound (c2)" or "(c2) component)]. In other words, the resin composition of the present embodiment preferably contains the maleimide compound as component (C), and the maleimide compound is a modified maleimide compound having a structural unit derived from a maleimide compound (c1) having at least two N-substituted maleimide groups and a structural unit derived from an amine compound (c2) having a primary amino group. The structural unit derived from the component (c1) and the structural unit derived from the component (c2) contained in the modified maleimide compound (Z) may each be one type or a combination of two or more types.
[0065] The modified maleimide compound (Z) is preferably a compound having a structure represented by the following formula (C-1), which is formed by an addition reaction between a maleimide group in the component (c1) and a primary amino group in the component (c2). [ka] (* indicates the bond position to other structures.)
[0066] Examples of the structural unit derived from the component (c1) include one or more types selected from the group consisting of groups represented by the following general formula (C1-6) and groups represented by the following general formula (C1-7).
[0067] [ka] (In the formula, X c1 represents X in the above general formula (C1-1). c1 where * indicates the position of attachment to other structures.)
[0068] The content of the structural unit derived from the (c1) component in the modified maleimide compound (Z) is not particularly limited, but is preferably 50 to 95 mass%, more preferably 70 to 92 mass%, and even more preferably 85 to 90 mass%. When the content of the structural unit derived from the (c1) component is within the above range, the high frequency characteristics become better and good film handling properties tend to be obtained.
[0069] The amine compound (c2) is preferably a compound having two or more amino groups, and more preferably a diamine compound having two amino groups. Examples of the amine compound (c2) include 4,4'-diaminodiphenylmethane, 4,4'-diamino-3,3'-dimethyldiphenylmethane, 3,3'-diethyl-4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl ketone, 4,4'-diaminobiphenyl, 3,3'-dimethyl-4,4 '-Diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dihydroxybenzidine, 2,2-bis(3-amino-4-hydroxyphenyl)propane, 3,3'-dimethyl-5,5'-diethyl-4,4'-diaminodiphenylmethane, 2,2-bis(4-aminophenyl)propane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 1,3-bis(3-aminophenoxy)benzene , 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, 1,3-bis[1-[4-(4-aminophenoxy)phenyl]-1-methylethyl]benzene, 1,4-bis[1-[4-(4-aminophenoxy)phenyl]-1-methylethyl]benzene, 4,4'-[1,3-phenylenebis(1-methylethylidene)]bisaniline aromatic diamine compounds such as 4,4'-[1,4-phenylenebis(1-methylethylidene)]bisaniline, 3,3'-[1,3-phenylenebis(1-methylethylidene)]bisaniline, bis[4-(4-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)phenyl]sulfone, and 9,9-bis(4-aminophenyl)fluorene; and amine-modified siloxane compounds having a primary amino group.
[0070] Among these, 4,4'-diaminodiphenylmethane, 4,4'-diamino-3,3'-dimethyldiphenylmethane, 3,3'-diethyl-4,4'-diaminodiphenylmethane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 4,4'-[1,3-phenylenebis(1-methylethylidene)]bisaniline, and 4,4'-[1,4-phenylenebis(1-methylethylidene)]bisaniline are preferred as the (c2) component from the viewpoints of excellent solubility in organic solvents, reactivity with the (c1) component, and heat resistance. Also, 3,3'-dimethyl-5,5'-diethyl-4,4'-diaminodiphenylmethane is preferred as the (c2) component from the viewpoints of excellent high-frequency characteristics and low water absorption. From the viewpoint of excellent mechanical properties such as adhesion to the conductor, elongation, and breaking strength, 2,2-bis[4-(4-aminophenoxy)phenyl]propane is preferred as component (c2). Furthermore, from the viewpoint of excellent solubility in organic solvents, reactivity during synthesis, heat resistance, adhesion to the conductor, high frequency properties, and low moisture absorption, 4,4'-[1,3-phenylenebis(1-methylethylidene)]bisaniline and 4,4'-[1,4-phenylenebis(1-methylethylidene)]bisaniline are preferred as component (c2).
[0071] The amine compound (c2) is preferably a compound represented by the following general formula (C2-1).
[0072] [ka] (In the formula, X c4 represents a divalent organic group.
[0073] The component (c2) is X in the above general formula (C2-1). c4 It is preferable that the aromatic diamine compound (C2-2) contains an aromatic diamine compound which is a divalent group represented by the following general formula (C2-2) [hereinafter, sometimes abbreviated as "aromatic diamine compound (C2-2)."].
[0074] [ka] (In the formula, R c11 and R c12 each independently represents an aliphatic hydrocarbon group having 1 to 5 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, a hydroxyl group, or a halogen atom. c5 represents an alkylene group having 1 to 5 carbon atoms, an alkylidene group having 2 to 5 carbon atoms, an ether group, a sulfide group, a sulfonyl group, a carbonyloxy group, a keto group, a fluorenylene group, a single bond, or a divalent group represented by the following general formula (C2-2-1) or (C2-2-2). c8 and n c9 Each independently represents an integer of 0 to 4. * indicates a bonding position.)
[0075] R in the above general formula (C2-2) c11 and R c12 Examples of the aliphatic hydrocarbon group having 1 to 5 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a t-butyl group, and an n-pentyl group. X c5 Examples of the alkylene group having 1 to 5 carbon atoms include a methylene group, a 1,2-dimethylene group, a 1,3-trimethylene group, a 1,4-tetramethylene group, and a 1,5-pentamethylene group. X c5 Examples of the alkylidene group having 2 to 5 carbon atoms include an ethylidene group, a propylidene group, an isopropylidene group, a butylidene group, an isobutylidene group, a pentylidene group, and an isopentylidene group. n c8 and n c9 represents an integer of 0 to 4, and is preferably 0 or 1 from the viewpoint of availability. c8 or n c9 If is an integer equal to or greater than 2, multiple R c11 R c12 They may be the same or different from each other. X in the above general formula (C2-2) c5 The divalent group represented by the general formula (C2-2-1) is as follows.
[0076] [ka] (In the formula, R c13 and R c14 Each of X independently represents an aliphatic hydrocarbon group having 1 to 5 carbon atoms or a halogen atom. c6 represents an alkylene group having 1 to 5 carbon atoms, an alkylidene group having 2 to 5 carbon atoms, an m-phenylenediisopropylidene group, a p-phenylenediisopropylidene group, an ether group, a sulfide group, a sulfonyl group, a carbonyloxy group, a keto group, or a single bond. c10 and n c11 Each independently represents an integer of 0 to 4. * indicates a bonding position.)
[0077] R in the above general formula (C2-2-1) c13 and R c14 The aliphatic hydrocarbon group having 1 to 5 carbon atoms represented by R in the above general formula (C2-2) is explained below. c11 and R c12 This is the same as the explanation for the aliphatic hydrocarbon group having 1 to 5 carbon atoms represented by the formula (1). X c6 The alkylene group having 1 to 5 carbon atoms and the alkylidene group having 2 to 5 carbon atoms represented by X in the above general formula (C2-2) are explained below. c5 This is the same as the explanation for the alkylene group having 1 to 5 carbon atoms and the alkylidene group having 2 to 5 carbon atoms represented by the formula (I). n c10 and n c11 represents an integer of 0 to 4, and from the viewpoint of availability, an integer of 0 to 2 is preferable, and 0 is more preferable. c10 If is an integer equal to or greater than 2, multiple R c13 may be the same or different. c11 If is an integer equal to or greater than 2, multiple R c14 They may be the same or different from each other. X in the above general formula (C2-2) c5 The divalent group represented by the general formula (C2-2-2) is as follows.
[0078] [ka] (In the formula, R c15 represents an aliphatic hydrocarbon group having 1 to 5 carbon atoms or a halogen atom. c7 and X c8 each independently represents an alkylene group having 1 to 5 carbon atoms, an alkylidene group having 2 to 5 carbon atoms, an ether group, a sulfide group, a sulfonyl group, a carbonyloxy group, a keto group, or a single bond. c12 represents an integer of 0 to 4. * represents a bonding position.)
[0079] R in the above general formula (C2-2-2) c15 The aliphatic hydrocarbon group having 1 to 5 carbon atoms represented by R in the above general formula (C2-2) is explained below. c11 and R c12 This is the same as the explanation for the aliphatic hydrocarbon group having 1 to 5 carbon atoms represented by the formula (1). X c7 and X c8 The alkylene group having 1 to 5 carbon atoms and the alkylidene group having 2 to 5 carbon atoms represented by the formula (C2-2) are c5 Examples of the alkylene group having 1 to 5 carbon atoms and the alkylidene group having 2 to 5 carbon atoms are the same as those shown by X c7 and X c8 is preferably an alkylidene group having 2 to 5 carbon atoms, and more preferably an isopropylidene group. n c12 represents an integer of 0 to 4, and from the viewpoint of availability, an integer of 0 to 2 is preferable, and 0 is more preferable. c12 If is an integer equal to or greater than 2, multiple R c15 They may be the same or different.
[0080] The component (c2) is X in the above general formula (C2-1). c4 may contain an amine-modified siloxane compound which is a divalent group containing a structural unit represented by the following general formula (C2-3), and X in the above general formula (C2-1) c4may contain a terminal amine-modified siloxane compound which is a divalent group represented by the following general formula (C2-4) [hereinafter, may be abbreviated as "terminal amine-modified siloxane compound (C2-4)"].
[0081] [ka] (In the formula, R c16 and R c17 each independently represents an alkyl group having 1 to 5 carbon atoms, a phenyl group, or a substituted phenyl group. * indicates the bonding position.)
[0082] [ka] (In the formula, R c16 and R c17 is the same as in the above general formula (C2-3), and R c18 and R c19 each independently represents an alkyl group having 1 to 5 carbon atoms, a phenyl group, or a substituted phenyl group. c9 and X c10 each independently represents a divalent organic group; c13 represents an integer from 2 to 100. * represents a bonding position.)
[0083] R in the above general formulas (C2-3) and (C2-4) c16 ~R c19 Examples of the alkyl group having 1 to 5 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a t-butyl group, an n-pentyl group, etc. As the alkyl group, an alkyl group having 1 to 3 carbon atoms is preferable, and a methyl group is more preferable. R c16 ~R c19Examples of the substituent that the phenyl group has in the substituted phenyl group represented by the formula (I) include an alkyl group having 1 to 5 carbon atoms, an alkenyl group having 2 to 5 carbon atoms, and an alkynyl group having 2 to 5 carbon atoms. Examples of the alkyl group having 1 to 5 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a t-butyl group, and an n-pentyl group. Examples of the alkenyl group having 2 to 5 carbon atoms include a vinyl group and an allyl group. Examples of the alkynyl group having 2 to 5 carbon atoms include an ethynyl group and a propargyl group. X c9 and X c10 Examples of the divalent organic group represented by include an alkylene group, an alkenylene group, an alkynylene group, an arylene group, -O-, or a divalent linking group formed by combining these groups. Examples of the alkylene group include alkylene groups having 1 to 10 carbon atoms, such as a methylene group, an ethylene group, or a propylene group. Examples of the alkenylene group include alkenylene groups having 2 to 10 carbon atoms. Examples of the alkynylene group include alkynylene groups having 2 to 10 carbon atoms. Examples of the arylene group include arylene groups having 6 to 20 carbon atoms, such as a phenylene group or a naphthylene group. Among these, X c9 and X c10 As the alkyl group, an alkylene group or an arylene group is preferable, and an alkylene group is more preferable. n c13 represents an integer of 2 to 100, preferably an integer of 2 to 50, more preferably an integer of 3 to 40, and further preferably an integer of 5 to 30. c13 If is an integer equal to or greater than 2, multiple R c16 R c17 They may be the same or different from each other.
[0084] Examples of the structural unit derived from the component (c2) include one or more types selected from the group consisting of groups represented by the following general formula (C2-5) and groups represented by the following general formula (C2-6). [ka] (In the formula, X c4 represents X in the above general formula (C2-1). c4 where * indicates the position of attachment to other structures.)
[0085] The content of the structural unit derived from the (c2) component in the modified maleimide compound (Z) is not particularly limited, but is preferably 5 to 50 mass%, more preferably 8 to 30 mass%, and even more preferably 10 to 15 mass%. When the content of the structural unit derived from the (c2) component is within the above range, excellent high-frequency characteristics, and better heat resistance, flame retardancy, and glass transition temperature tend to be obtained.
[0086] The total content of the structural units derived from the component (c1) and the structural units derived from the component (c2) in the modified maleimide compound (Z) is not particularly limited, but is preferably 80 mass% or more, more preferably 90 mass% or more, even more preferably 95 mass% or more, and particularly preferably 100 mass% (i.e., consisting only of structural units derived from the component (c1) and structural units derived from the component (c2)).
[0087] The content ratio of the structural unit derived from the component (c1) and the structural unit derived from the component (c2) in the modified maleimide compound (Z) is not particularly limited. 2 Group derived from (-NH 2 The content ratio is such that the equivalent ratio (Ta1 / Ta2) of the total equivalent (Ta1) of groups (including maleimide groups) derived from component (c1) to the total equivalent (Ta2) of groups (including maleimide groups) derived from component (c1) is preferably 0.05 to 10, and more preferably 1 to 5. When the equivalent ratio (Ta1 / Ta2) is within the above range, excellent high-frequency characteristics, and better heat resistance, flame retardancy, and glass transition temperature tend to be obtained.
[0088] From the viewpoints of high frequency characteristics, insulation reliability, solubility in organic solvents, adhesion to conductors, moldability, and the like, the maleimide compound preferably contains a compound represented by the following general formula (C-2).
[0089] [ka] (In the formula, X c1 and X c4 is as explained in the above general formulas (c1-1) and (c2-1).
[0090] (Method for producing modified maleimide compound (Z)) The component (Z) can be produced, for example, by reacting the components (c1) and (c2) in an organic solvent. Specifically, a reactor is charged with predetermined amounts of component (c1), component (c2), and other components as necessary, and component (c1) and component (c2) are subjected to a Michael addition reaction (hereinafter sometimes referred to as a "pre-reaction") to obtain a modified maleimide compound (Z). The reaction conditions are not particularly limited, but from the viewpoint of obtaining good reactivity and workability while suppressing gelation, the reaction temperature is preferably 50 to 160° C. and the reaction time is preferably 1 to 10 hours.
[0091] In the pre-reaction, a reaction catalyst may be used as necessary. Examples of the reaction catalyst include acid catalysts such as p-toluenesulfonic acid; amines such as triethylamine, pyridine, and tributylamine; imidazoles such as methylimidazole and phenylimidazole; and phosphorus-based catalysts such as triphenylphosphine. These may be used alone or in combination of two or more. There is no particular restriction on the amount of the reaction catalyst to be added, but it is, for example, 0.01 to 5 parts by mass with respect to 100 parts by mass of the total amount of the (c1) component and the (c2) component.
[0092] In the pre-reaction, the organic solvent may be added or concentrated as necessary to adjust the solid content concentration of the reaction raw materials and the viscosity of the reaction liquid. The solid content concentration of the reaction raw materials is not particularly limited, but is preferably 10 to 90 mass%, more preferably 20 to 80 mass%. When the solid content concentration of the reaction raw materials is equal to or higher than the lower limit, a sufficient reaction rate is obtained, which tends to be advantageous in terms of production costs, and when the solid content concentration is equal to or lower than the upper limit, better solubility is obtained, stirring efficiency is improved, and gelation tends to be less likely to occur.
[0093] The weight average molecular weight (Mw) of the modified maleimide compound (Z) is not particularly limited, but is preferably from 400 to 10,000, more preferably from 1,000 to 5,000, further preferably from 1,500 to 4,000, and particularly preferably from 2,000 to 3,000.
[0094] ((C) Component Content) When the resin composition of the present embodiment contains the thermosetting resin (C), its content is not particularly limited, but from the viewpoints of high-frequency characteristics, heat resistance, and moldability, it is preferably 5 to 80 parts by mass, more preferably 5 to 60 parts by mass, even more preferably 10 to 50 parts by mass, and particularly preferably 25 to 45 parts by mass, per 100 parts by mass of the total of the resin components.
[0095] When the resin composition of the present embodiment contains a thermosetting resin (C), the content ratio [(A) / (C)] of the polyphenylene ether derivative (A) to the thermosetting resin (C) is not particularly limited, but is preferably 5 / 95 to 80 / 20, more preferably 6 / 94 to 60 / 40, even more preferably 8 / 92 to 40 / 60, and particularly preferably 10 / 90 to 20 / 80, in terms of mass ratio. When the content ratio [(A) / (C)] is 5 / 95 or more, better high frequency characteristics and low moisture absorption tend to be obtained. When the content ratio [(A) / (C)] is 80 / 20 or less, better heat resistance, moldability and processability tend to be obtained.
[0096] The resin composition of the present embodiment preferably further contains one or more selected from the group consisting of a thermoplastic elastomer (D), a curing accelerator (E) and an inorganic filler (F). Next, each of these components will be described.
[0097] <Thermoplastic elastomer (D)> By containing the thermoplastic elastomer (D), the resin composition of this embodiment tends to have a good balance of high-frequency characteristics, moldability, adhesion to a conductor, solder heat resistance, glass transition temperature, and thermal expansion coefficient. The thermoplastic elastomer (D) may be used alone or in combination of two or more kinds.
[0098] The thermoplastic elastomer (D) may be a thermoplastic elastomer having a structural unit represented by the following general formula (D-1), and the structural unit derived from styrene (i.e., R d1 is a hydrogen atom, and n d1 It is preferable that the thermoplastic elastomer has a structural unit in which Mn is 0 (hereinafter, sometimes referred to as a styrene-based thermoplastic elastomer).
[0099] [ka] (In the formula, R d1 represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms; R d2 represents an alkyl group having 1 to 5 carbon atoms. d1 represents an integer from 0 to 5.)
[0100] R d1 Examples of the alkyl group having 1 to 5 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a t-butyl group, and an n-pentyl group. R d1 Among the groups represented by the formula (I), a hydrogen atom is preferred. R d2 Examples of the alkyl group having 1 to 5 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a t-butyl group, an n-pentyl group, etc. The alkyl group is preferably an alkyl group having 1 to 3 carbon atoms, and more preferably a methyl group. n d1 represents an integer of 0 to 5, preferably an integer of 0 to 2, and more preferably 0. n d1 If is an integer equal to or greater than 2, multiple R d1 They may be the same or different.
[0101] Examples of structural units other than those derived from compounds contained in the thermoplastic elastomer (D) include structural units derived from butadiene, structural units derived from isoprene, structural units derived from maleic acid, and structural units derived from maleic anhydride. The butadiene-derived structural unit and the isoprene-derived structural unit are preferably hydrogenated. When hydrogenated, the butadiene-derived structural unit is a mixed structural unit of ethylene units and butylene units, and the isoprene-derived structural unit is a mixed structural unit of ethylene units and propylene units.
[0102] Examples of the thermoplastic elastomer (D) include hydrogenated styrene-based thermoplastic elastomers such as hydrogenated styrene-butadiene-styrene block copolymer (SBS) and hydrogenated styrene-isoprene-styrene block copolymer (SIS). Among these, hydrogenated styrene-butadiene-styrene block copolymer (SBS) is preferred from the viewpoints of high frequency characteristics, adhesion to conductors, heat resistance, glass transition temperature and thermal expansion coefficient.
[0103] Examples of hydrogenated styrene-butadiene-styrene block copolymers (SBS) include styrene-ethylene-butylene-styrene copolymers (SEBS) obtained by completely hydrogenating the carbon-carbon double bonds in the butadiene block, and styrene-butadiene-butylene-styrene (SBBS) obtained by partially hydrogenating the carbon-carbon double bonds at the 1,2-bond sites in the butadiene block. Note that the completely hydrogenated ratio in SEBS is usually 90% or more, 95% or more, 99% or more, or substantially 100% of the total carbon-carbon double bonds. The partial hydrogenation ratio in SBBS is, for example, 60 to 85% of the total carbon-carbon double bonds.
[0104] In SEBS, the content of structural units derived from styrene [hereinafter sometimes abbreviated as "styrene content"] is not particularly limited, but from the viewpoints of high-frequency characteristics, adhesion to a conductor, heat resistance, glass transition temperature, and thermal expansion coefficient, it is preferably 5 to 80 mass%, more preferably 10 to 70 mass%, further preferably 15 to 60 mass%, and particularly preferably 20 to 50 mass%. The melt flow rate (MFR) of SEBS is not particularly limited, but is preferably 0.1 to 20 g / 10 min, more preferably 1 to 15 g / 10 min, further preferably 2 to 10 g / 10 min, and particularly preferably 3 to 7 g / 10 min, measured under conditions of 230° C. and a load of 2.16 kgf (21.2 N).
[0105] In SBBS, the styrene content is not particularly limited, but from the viewpoints of high-frequency characteristics, adhesion to a conductor, heat resistance, glass transition temperature, and thermal expansion coefficient, it is preferably 40 to 80 mass%, more preferably 50 to 75 mass%, and even more preferably 55 to 75 mass%. The MFR of SBBS is not particularly limited, but is preferably 0.1 to 10 g / 10 min, more preferably 0.5 to 8 g / 10 min, and even more preferably 1 to 6 g / 10 min, measured under conditions of 190° C. and a load of 2.16 kgf (21.2 N).
[0106] The thermoplastic elastomer (D) may be acid-modified with maleic anhydride or the like. The acid value of the acid-modified thermoplastic elastomer (D) is not particularly limited, but is preferably 2 to 20 mgCH 3 ONa / g is preferred, 5-15mgCH 3 ONa / g is more preferable, 7 to 13 mg CH 3 ONa / g is more preferred.
[0107] ((D) Component Content) When the resin composition of the present embodiment contains the thermoplastic elastomer (D), its content is not particularly limited, but is preferably 2 to 40 parts by mass, more preferably 5 to 30 parts by mass, further preferably 8 to 25 parts by mass, and particularly preferably 10 to 20 parts by mass, relative to 100 parts by mass of the total of the resin components. When the content of the thermoplastic elastomer (D) is equal to or more than the above lower limit, better high frequency characteristics and moisture absorption resistance tend to be obtained. When the content of the thermoplastic elastomer (D) is equal to or less than the above upper limit, good heat resistance, moldability, and processability tend to be obtained.
[0108] <Curing accelerator (E)> By containing the curing accelerator (E), the resin composition of the present embodiment tends to have improved curability and to have better high frequency characteristics, heat resistance, adhesion to a conductor, elastic modulus, and glass transition temperature. When the resin composition of the present embodiment contains a curing accelerator (E), a suitable curing accelerator (E) may be appropriately selected depending on the type of the thermosetting resin (C) component used. The curing accelerator (E) may be used alone or in combination of two or more kinds.
[0109] Examples of the component (E) include amine-based curing accelerators, imidazole-based curing accelerators, phosphorus-based curing accelerators, organometallic salts, acid catalysts, organic peroxides, etc. In the present embodiment, imidazole-based curing accelerators are not classified as amine-based curing accelerators. Examples of the amine-based curing accelerator include amine compounds having primary to tertiary amines, such as triethylamine, pyridine, tributylamine, and dicyandiamide; and quaternary ammonium compounds. Examples of the imidazole-based curing accelerator include imidazole compounds such as methylimidazole, phenylimidazole, 2-undecylimidazole, and isocyanate-masked imidazole (eg, an addition reaction product of hexamethylene diisocyanate resin and 2-ethyl-4-methylimidazole). Examples of the phosphorus-based curing accelerator include tertiary phosphines such as triphenylphosphine; and quaternary phosphonium compounds such as an addition product of p-benzoquinone and tri-n-butylphosphine. Examples of the organic metal salt include carboxylates of manganese, cobalt, zinc, and the like. An example of the acid catalyst is p-toluenesulfonic acid. Examples of organic peroxides include dicumyl peroxide, 2,5-dimethyl-2,5-bis(t-butylperoxy)hexyne-3,2,5-dimethyl-2,5-bis(t-butylperoxy)hexane, t-butylperoxyisopropyl monocarbonate, and α,α'-di(t-butylperoxy)diisopropylbenzene. Among these, from the viewpoint of obtaining better high frequency characteristics, heat resistance, adhesion to conductor, elastic modulus and glass transition temperature, amine-based curing accelerators, imidazole-based curing accelerators and phosphorus-based curing accelerators are preferred, dicyandiamide, imidazole-based curing accelerators and quaternary phosphonium compounds are more preferred, and it is even more preferred to use these in combination. At this time, organic peroxides may also be used in combination, but from the viewpoint of the physical properties of the cured product, it is preferable not to contain organic peroxides.
[0110] ((E) Component Content) When the resin composition of the present embodiment contains the curing accelerator (E), its content is not particularly limited, but is preferably 0.01 to 10 parts by mass, more preferably 0.05 to 5 parts by mass, further preferably 0.1 to 5 parts by mass, and particularly preferably 0.5 to 4 parts by mass, relative to 100 parts by mass of the thermosetting resin (C). When the content of the curing accelerator (E) is within the above range, better high-frequency characteristics, heat resistance, storage stability, and moldability tend to be obtained.
[0111] <Inorganic filler (F)> By containing the inorganic filler (F), the resin composition of the present embodiment tends to have better low thermal expansion properties, high elastic modulus, heat resistance, and flame retardancy. The inorganic filler (F) may be used alone or in combination of two or more kinds.
[0112] Examples of the inorganic filler (F) include silica, alumina, titanium oxide, mica, beryllia, barium titanate, potassium titanate, strontium titanate, calcium titanate, aluminum carbonate, magnesium hydroxide, aluminum hydroxide, aluminum silicate, calcium carbonate, calcium silicate, magnesium silicate, silicon nitride, boron nitride, clay (calcined clay, etc.), talc, aluminum borate, and silicon carbide. Among these, from the viewpoints of thermal expansion coefficient, elastic modulus, heat resistance, and flame retardancy, the inorganic filler (F) is preferably silica, alumina, mica, and talc, more preferably silica and alumina, and even more preferably silica. Examples of silica include precipitated silica produced by a wet method and having a high water content, and dry method silica produced by a dry method and containing almost no bound water. Examples of dry method silica include crushed silica, fumed silica, and fused silica (fused spherical silica), depending on the production method. Among these, fused spherical silica is preferable as the inorganic filler (F).
[0113] The average particle size of the inorganic filler (F) is not particularly limited, but is preferably from 0.01 to 20 μm, more preferably from 0.1 to 10 μm, further preferably from 0.2 to 1 μm, and particularly preferably from 0.3 to 0.8 μm.
[0114] When the resin composition of the present embodiment contains an inorganic filler (F), the content thereof is not particularly limited, but from the viewpoints of thermal expansion coefficient, elastic modulus, heat resistance, and flame retardancy, it is preferably 1 to 40 mass% relative to the solid content, more preferably 5 to 35 mass%, even more preferably 10 to 35 mass%, and even more preferably 15 to 35 mass%.
[0115] When the inorganic filler (F) is used, a coupling agent may be used in combination as necessary to improve the dispersibility of the inorganic filler (F) and the adhesion between the inorganic filler (F) and the organic component in the resin composition. The coupling agent may be the titanate coupling agent (X) or another coupling agent such as a silane coupling agent. When the titanate coupling agent (X) is used as the coupling agent, it is preferable to set the content within the range of the titanate coupling agent (X). The coupling agents may be used alone or in combination of two or more. When a coupling agent is used, the treatment method may be a so-called integral blend treatment method in which the inorganic filler (F) is blended in the resin composition and then the coupling agent is added, but it is preferable to use an inorganic filler that has been surface-treated in advance with a coupling agent in a dry or wet manner. By adopting this method, the characteristics of the inorganic filler (F) can be more effectively expressed. If necessary, the inorganic filler (F) may be used in the form of a slurry in which it is dispersed in an organic solvent in advance.
[0116] <Flame retardants, flame retardant assistants, adhesion improvers> The resin composition of the present embodiment may contain one or more selected from the group consisting of a flame retardant, a flame retardant assistant, and an adhesion improver, as necessary, within a range that does not impair the effects of the present embodiment. Each of these components may be used alone or in combination of two or more. The resin composition of the present embodiment may not contain these components.
[0117] (Flame retardant) Examples of flame retardants include inorganic phosphorus-based flame retardants, organic phosphorus-based flame retardants, and metal hydrates such as aluminum hydroxide hydrate and magnesium hydroxide hydrate. Although metal hydroxides may also be considered inorganic fillers, they are classified as flame retardants when they are materials capable of imparting flame retardancy. Examples of inorganic phosphorus-based flame retardants include red phosphorus; ammonium phosphates such as monoammonium phosphate, diammonium phosphate, triammonium phosphate, and ammonium polyphosphate; inorganic nitrogen-containing phosphorus compounds such as phosphoric acid amide; phosphoric acid; and phosphine oxide. Examples of organic phosphorus-based flame retardants include aromatic phosphate esters, phosphonic acid diesters, and phosphinic acid esters; metal salts of phosphinic acid, organic nitrogen-containing phosphorus compounds, cyclic organic phosphorus compounds, etc. Here, examples of the "metal salts" include lithium salts, sodium salts, potassium salts, calcium salts, magnesium salts, aluminum salts, titanium salts, zinc salts, etc.
[0118] (Flame retardant content) When the resin composition of the present embodiment contains a flame retardant, the content is not particularly limited, but may be, for example, 0.1 parts by mass or more, 1 part by mass or more, 5 parts by mass or more, 10 parts by mass or more, and 40 parts by mass or less, 30 parts by mass or less, 25 parts by mass or less, or 20 parts by mass or less, relative to 100 parts by mass of the total of the resin components. The resin composition of the present embodiment may not contain a flame retardant.
[0119] (Flame retardant assistant) Examples of the flame retardant assistant include inorganic flame retardant assistants such as antimony trioxide and zinc molybdate. When the resin composition of the present embodiment contains a flame retardant auxiliary, the content is not particularly limited, but is preferably 0.1 to 20 parts by mass, more preferably 0.1 to 10 parts by mass, per 100 parts by mass of the total of the resin components. When the content of the flame retardant auxiliary is within the above range, better chemical resistance tends to be obtained. In addition, the resin composition of the present embodiment does not need to contain a flame retardant auxiliary.
[0120] (Adhesion improver) Examples of the adhesion improver include nitrogen-containing compounds such as triazine derivatives and carbodiimides. When the resin composition of the present embodiment contains an adhesion improver, its content is not particularly limited, but is preferably 0.1 to 20 parts by mass, more preferably 0.1 to 10 parts by mass, relative to 100 parts by mass of the total of the resin components. When the content of the adhesion improver is within the above range, better copper foil peel strength tends to be obtained. In addition, the resin composition of the present embodiment does not need to contain an adhesion improver.
[0121] <Organic solvent> The resin composition of the present embodiment may be a varnish-like resin composition containing an organic solvent, from the viewpoint of facilitating handling and facilitating production of a prepreg, which will be described later. Examples of the organic solvent include alcohol-based solvents such as ethanol, propanol, butanol, methyl cellosolve, butyl cellosolve, and propylene glycol monomethyl ether; ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ether-based solvents such as tetrahydrofuran; aromatic solvents such as toluene, xylene, and mesitylene; nitrogen-containing solvents such as dimethylformamide, dimethylacetamide, and N-methylpyrrolidone; sulfur-containing solvents such as dimethylsulfoxide; and ester-based solvents such as γ-butyrolactone. These organic solvents may be used alone or in combination of two or more.
[0122] When the resin composition of the present embodiment contains an organic solvent, its content is not particularly limited, but is preferably such that the solid content concentration of the resin composition of the present embodiment is 30 to 90 mass%, more preferably 40 to 80 mass%, and even more preferably 40 to 60 mass%. When the content of the organic solvent is within the above range, the resin composition is easy to handle, and the impregnation into the substrate and the appearance of the prepreg produced are good. Furthermore, it becomes easy to adjust the solid content concentration of the resin in the prepreg described later, and there is a tendency that the production of a prepreg having a desired thickness becomes easier.
[0123] <Other ingredients> Furthermore, the resin composition of the present embodiment may contain, as necessary, one or more selected from the group consisting of resin materials, coupling agents, antioxidants, heat stabilizers, antistatic agents, ultraviolet absorbers, pigments, colorants, and lubricants other than the above-mentioned components [hereinafter, sometimes abbreviated as "other components". ] within the range that does not impair the effects of the present embodiment. For each of these components, one type may be used alone, or two or more types may be used in combination. In addition, the resin composition of the present embodiment may not contain these components. When the resin composition of the present embodiment contains the above-mentioned other components, the content of each of them is not particularly limited, but may be, for example, 0.01 parts by mass or more, and may be 10 parts by mass or less, 5 parts by mass or less, or 1 part by mass or less, per 100 parts by mass of the total of the resin components. Furthermore, the total content of the (A), (B), (C), (D) and (E) components in the resin components contained in the resin composition of this embodiment is not particularly limited, but is preferably 80 parts by mass or more, more preferably 90 parts by mass or more, and even more preferably 95 parts by mass or more, per 100 parts by mass of the total of the resin components (however, all of these amounts include 100 parts by mass).
[0124] <Dielectric properties (high frequency properties)> The dielectric constant (Dk) at 10 GHz when the resin composition of this embodiment is made into a test piece by the method described in the Examples below is not particularly limited, but is preferably 3.0 or less, more preferably 2.7 or less, and even more preferably 2.5 or less. The smaller the dielectric constant (Dk), the more preferable it is, and there is no particular limit to the lower limit, but in consideration of the balance with other physical properties, it may be, for example, 2.0 or more, or 2.3 or more. The dielectric loss tangent (Df) at 10 GHz when the resin composition of this embodiment is made into a test piece by the method described in the examples below is not particularly limited, but is preferably 0.0045 or less, more preferably 0.0040 or less, and even more preferably 0.0035 or less. The dielectric loss tangent (Df) is preferably as small as possible, and there is no particular limit to the lower limit, but in consideration of the balance with other physical properties, it may be, for example, 0.0020 or more, or 0.0025 or more. The dielectric constant (Dk) and the dielectric loss tangent (Df) are values based on the cavity resonator perturbation method, more specifically, values measured by the method described in the Examples. In this specification, the term "dielectric constant" refers to the relative dielectric constant.
[0125] The resin composition of the present embodiment can be produced by mixing the (A) component, the (B) component, and any optional components used in combination as necessary by a known method. At this time, each component may be dissolved or dispersed in the above-mentioned organic solvent while stirring. The mixing order, temperature, time, and other conditions are not particularly limited and can be set arbitrarily.
[0126] [Metal foil with resin] The resin-coated metal foil of this embodiment has a layer of the resin composition of this embodiment on a metal foil. Specifically, the resin-attached metal foil can be produced by applying the resin composition of the present embodiment onto a metal foil and semi-curing (B-stage) the resin composition in a drying oven. The drying conditions are not particularly limited, but the drying temperature is preferably 80 to 180° C., more preferably 110 to 160° C. The coating method is not particularly limited, and for example, a known coater such as a die coater, comma coater, bar coater, kiss coater, or roll coater can be used. Examples of the metal foil of the resin-coated metal foil include copper foil and aluminum foil, but other metal foils can also be used. Among these, copper foil is preferred.
[0127] [Prepreg] The prepreg of the present embodiment contains the resin composition of the present embodiment and a sheet-like fiber reinforcing substrate. The prepreg can be formed using the resin composition of this embodiment and a sheet-like fiber-reinforced substrate, and can be produced, for example, by impregnating or coating the resin composition of this embodiment into a sheet-like fiber-reinforced substrate, and heating and drying the substrate at a temperature of 80 to 200°C for 1 to 30 minutes in a drying furnace to semi-cure (B-stage) the resin composition. The solid content derived from the resin composition in the prepreg of this embodiment is not particularly limited, but is preferably 30 to 90 mass%, more preferably 35 to 80 mass%, further preferably 40 to 70 mass%, and particularly preferably 45 to 60 mass%. When the solid content derived from the resin composition in the prepreg is within the above range, better moldability tends to be obtained when the prepreg is made into a laminate.
[0128] As the sheet-like fiber reinforcement substrate of the prepreg, a known one used in various laminates for electrical insulating materials is used. Examples of the material of the sheet-like fiber reinforcement substrate include inorganic fibers such as E glass, D glass, S glass, and Q glass; organic fibers such as polyimide, polyester, and tetrafluoroethylene; and mixtures thereof. These sheet-like fiber reinforcement substrates have shapes such as woven fabric, nonwoven fabric, roving, chopped strand mat, and surfacing mat. In addition, the thickness of the sheet-like fiber reinforcement substrate is not particularly limited, and for example, a substrate having a thickness of 0.02 to 0.5 mm can be used. In addition, from the viewpoints of impregnation of the resin composition, heat resistance, moisture absorption resistance, and processability when made into a laminate, a substrate that has been surface-treated with a coupling agent or the like, a substrate that has been mechanically opened, and the like can be used.
[0129] The resin composition can be impregnated or coated on a sheet-like fiber-reinforced substrate by the following hot melt method or solvent method. The hot melt method is a method in which the resin composition does not contain an organic solvent, and (1) the resin composition is first coated onto a coated paper that has good peelability from the resin composition, and then the coated paper is laminated onto a sheet-like fiber-reinforced substrate, or (2) the resin composition is directly coated onto a sheet-like fiber-reinforced substrate using a die coater. On the other hand, the solvent method is a method in which an organic solvent is added to a resin composition, a sheet-shaped fiber-reinforced substrate is immersed in the obtained resin composition to impregnate the sheet-shaped fiber-reinforced substrate with the resin composition, and then the substrate is dried.
[0130] [Laminate] The laminate of the present embodiment is a laminate containing (i) the resin-coated metal foil of the present embodiment or (ii) the prepreg and metal foil of the present embodiment. The laminate of this embodiment can be obtained by hot pressing one sheet of the resin-coated metal foil of this embodiment, or by arranging two sheets of resin-coated metal foil so that the metal foil is the outer layer, and then hot pressing. Alternatively, the laminate can be obtained by arranging metal foil on one or both sides of one prepreg of this embodiment, or by arranging metal foil on one or both sides of two or more stacked prepregs of this embodiment, and then hot pressing. A laminate having metal foil is sometimes called a metal-clad laminate. The metal of the metal foil is not particularly limited as long as it is used in electrical insulating material applications. From the viewpoint of electrical conductivity, the metal may be copper, gold, silver, nickel, platinum, molybdenum, ruthenium, aluminum, tungsten, iron, titanium, chromium, or an alloy containing one or more of these metal elements, with copper and aluminum being preferred, and copper being more preferred.
[0131] [Multilayer printed wiring board] The multilayer printed wiring board of the present embodiment contains (i) the resin-coated metal foil of the present embodiment, (ii) the prepreg of the present embodiment, or (iii) the laminate of the present embodiment. The multilayer printed wiring board of the present embodiment can be manufactured by performing a circuit formation process and a multilayer adhesive process using the resin-coated metal foil, prepreg, or laminate of the present embodiment by a known method, such as drilling, metal plating, and etching of the metal foil.
[0132] [Semiconductor package] The semiconductor package of this embodiment is formed by mounting a semiconductor element on the multilayer printed wiring board of this embodiment. The semiconductor package of this embodiment can be manufactured, for example, by mounting semiconductor elements such as semiconductor chips and memories at predetermined positions on the multilayer printed wiring board of this embodiment by a known method and sealing the semiconductor elements with sealing resin or the like.
[0133] Although the preferred embodiments of the present invention have been described above, these are merely examples for the purpose of explaining the present invention, and the scope of the present invention is not limited to these embodiments. The present invention can be embodied in various forms different from the above-described embodiments without departing from the gist of the present invention. EXAMPLES
[0134] The present embodiment will be specifically described below with reference to examples, although the present embodiment is not limited to the following examples.
[0135] In each example, the weight average molecular weight (Mw) was measured by the following method. The values were calculated from a calibration curve using standard polystyrene by gel permeation chromatography (GPC). The calibration curve was approximated by a third-order equation using standard polystyrene: TSKstandard POLYSTYRENE (Type; A-2500, A-5000, F-1, F-2, F-4, F-10, F-20, F-40) [manufactured by Tosoh Corporation, product name]. The measurement conditions for GPC are shown below. Device: Pump: L-6200 type [manufactured by Hitachi High-Technologies Corporation] Detector: L-3300 type RI [Hitachi High-Technologies Corporation] Column oven: L-655A-52 [Hitachi High-Technologies Corporation] Column: Guard column; "TSK Guardcolumn HHR-L" + column; "TSKgel G4000HHR" + "TSKgel G2000HHR" (all product names manufactured by Tosoh Corporation) Column size: 6.0 x 40 mm (guard column), 7.8 x 300 mm (column) Eluent: Tetrahydrofuran Sample concentration: 30mg / 5mL Injection volume: 20μL Flow rate: 1.00mL / min Measurement temperature: 40℃
[0136] [Production Example 1: Production of modified maleimide compound (Z1)] In a 5-liter reaction vessel equipped with a thermometer, a stirrer, and a water content meter with a reflux condenser, capable of heating and cooling, 100 parts by mass of 2,2-bis[4-(4-maleimidophenoxy)phenyl]propane, 13.5 parts by mass of 3,3'-diethyl-4,4'-diaminodiphenylmethane (manufactured by Nippon Kayaku Co., Ltd., trade name: KAYAHARD (registered trademark) AA), and 171 parts by mass of propylene glycol monomethyl ether were added and reacted for 2 hours under reflux. This was concentrated at the reflux temperature for 3 hours to produce a modified maleimide compound (Z1)-containing liquid with a solid content concentration of 65% by mass. The weight average molecular weight (Mw) of the obtained modified maleimide resin (Z1) was about 2,700.
[0137] [Examples 1-2, Comparative Examples 1-3] (Preparation of Resin Composition) Each component shown in Table 1 was stirred and mixed at room temperature together with 58 parts by mass of toluene and 10 parts by mass of methyl isobutyl ketone according to the formulation shown in Table 1 to prepare a resin composition having a solid content concentration of 45 to 55% by mass. However, X-1 and Y-1 had been previously mixed and stirred with B-1 in methyl isobutyl ketone (MIBK) at 25°C. In order to standardize the filler contents in each of the Examples and Comparative Examples, the total content of the fluororesin filler (B) and the inorganic filler (F) was adjusted to be equal. (Preparation of resin-coated copper foil) The resin composition obtained in each example was applied to a copper foil (MT18FL1.5, manufactured by Mitsui Mining & Smelting Co., Ltd.) having a thickness of 0.0195 mm using a coater, and then heated and dried at 120°C for 3 minutes to produce a resin-coated copper foil having a coating thickness of 25 µm. (Preparation of laminated plates and resin plates) The resin composition was applied to a PET film having a thickness of 0.050 mm by a coating machine, and the film was dried by heating at 120°C for 3 minutes to produce a PET film with a resin coating thickness of 25 μm. The resin surfaces of the PET film with resin were laminated together by vacuum pressure lamination (temperature 110°C, pressure 0.5 MPa). Furthermore, the PET film on one side was peeled off, and the peeled surfaces were laminated together until the resin thickness reached 325 μm. The PET on both sides of the PET film with resin having a resin thickness of 325 μm was peeled off, and low-profile copper foil (BF-ANP18, Rz of M side: 1.5 μm, manufactured by CIRCUIT FOIL) having a thickness of 18 μm was laminated on the top and bottom of the resin so that the M side was in contact with the resin, and this laminate was placed in a mold with a thickness of 300 μm. Next, the laminate was heated and pressurized at a temperature of 230°C, a pressure of 3.0 MPa, and a time of 90 minutes to produce a double-sided copper-clad laminate. The outer copper foil of this double-sided copper-clad laminate was removed by immersion in a copper etching solution (a 10 mass % solution of ammonium persulfate, manufactured by Mitsubishi Gas Chemical Company, Inc.) to produce a resin plate with a thickness of 300 μm.
[0138] [Evaluation method] The measurements and evaluations were carried out according to the following methods, and the results are shown in Table 1.
[0139] (1. Measurement of dielectric properties (high frequency properties)) The resin plates produced in each example were cut into test pieces of 60 mm in length and 2 mm in width, and the dielectric constant and dielectric loss tangent were measured by the cavity resonator perturbation method. The measuring device used was Agilent Technologies' vector network analyzer "N5227A," the cavity resonator was Kanto Electronics Application Development Co., Ltd.'s "CP129" (10 GHz band resonator), and the measurement program was "CPMA-V2." The measurements were performed at a frequency of 10 GHz and at a temperature of 25°C.
[0140] (2. Evaluation of powder fall at the edge when cutting resin-coated copper foil) When the resin-coated copper foil produced in each example was cut with a cutter "Refined Slitter W-650" (slit blade size: 98mm x 66mm, thickness: 2mm, see Figure 1, manufactured by Soltec Industrial Co., Ltd.), the amount of resin powder adhering to the slit blade was visually observed. When there was almost no resin powder adhering to the slit blade (see Figure 2), it was judged as "A," and when there was a large amount of resin powder adhering to the slit blade (see Figure 3), it was judged as "C."
[0141] (3. Measurement of copper foil peel strength) The copper foil of the double-sided copper-clad laminate prepared in each example was partially etched to form a 3 mm wide copper foil line. Next, using a thermostatic chamber-mounted peel tester (manufactured by Shimadzu Corporation), the temperature was set to 25°C and the load was measured when the copper foil line was peeled off at a speed of 50 mm / min in a 90° direction relative to the adhesive surface.
[0142] [Table 1]
[0143] The abbreviations for each material in Table 1 are as follows. [Component (A): Polyphenylene ether derivative] A-1: Polyphenylene ether having methacryl groups at the molecular terminals (both terminals) (weight average molecular weight (Mw): 1,700). Corresponding to the compound represented by the general formula (A-4) above. [Component (B): Fluorine resin filler] B-1: PTFE filler; manufactured by Admatechs Co., Ltd., particulate, average particle size: 3 μm [Component (X): Titanate coupling agent] X-1: PLENACT (registered trademark) 38S; manufactured by Ajinomoto Fine-Techno Co., Ltd., see the structural formula below [ka] [Coupling agent other than component (X): silane coupling agent] Y-1: KBM-903; 3-aminopropyltrimethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd. [(C) Component: Thermosetting resin] C-1: Modified maleimide compound (Z1) prepared in Production Example 1 [Component (D): Thermoplastic elastomer] D-1: Tuftec (registered trademark) M1913; Asahi Kasei Corporation, maleic anhydride modified hydrogenated styrene-based thermoplastic elastomer (SEBS), acid value 10 mgCH 3 ONa / g, styrene content 30%, MFR 5.0g / 10min (MFR measurement conditions: measured in accordance with ISO1133 at 230°C and a load of 2.16kg.) [Component (E): Curing accelerator] E-1: p-Benzoquinone and tri-n-butylphosphine adduct E-2: 2-Undecylimidazole E-3: Dicyandiamide [(F) Component: Inorganic filler] F-1: Spherical fused silica: average particle size 0.5 μm, methyl isobutyl ketone 70% by mass slurry
[0144] As is clear from the results shown in Table 1, the resin-coated copper foils and laminates of Examples 1 and 2 produced using the resin composition of this embodiment have superior high-frequency characteristics, suppressed powder fall at the edges when the resin-coated metal foil is cut, and have superior copper foil peel strength compared to the resin-coated copper foils and laminates of Comparative Examples 1 to 3. In particular, in contrast to Comparative Example 2 in which no titanate coupling agent (X) was used, Comparative Example 3 used a silane coupling agent, but there was no change in the copper foil peel strength. [Industrial Applicability]
[0145] The resin composition of the present embodiment exhibits excellent dielectric properties in the high frequency band of 10 GHz or more, suppresses powder falling off at the ends when the resin-coated metal foil is cut, and has excellent copper foil peel strength. Therefore, resin-coated metal foils, prepregs, laminates, multilayer printed wiring boards, semiconductor packages, and the like obtained using the resin composition are suitable for use in electronic components that handle high frequency signals.
Claims
1. A resin composition comprising a polyphenylene ether derivative (A), a fluororesin filler (B), and a titanate coupling agent (X), The resin composition, wherein the component (A) has an ethylenically unsaturated bond-containing group at a molecular terminal.
2. The resin composition according to claim 1 , wherein the component (A) has an ethylenically unsaturated bond-containing group at both terminals of the molecule.
3. The resin composition according to claim 1 or 2, wherein the ethylenically unsaturated bond-containing group contained in the component (A) is a (meth)acrylic group.
4. The resin composition according to any one of claims 1 to 3, wherein the weight average molecular weight (Mw) of the component (A) is 500 to 7,000.
5. The resin composition according to any one of claims 1 to 4, wherein the component (B) is at least one selected from the group consisting of polytetrafluoroethylene (PTFE) filler, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA) filler, tetrafluoroethylene-hexafluoropropylene copolymer (FEP) filler, tetrafluoroethylene-ethylene copolymer (ETFE) filler and polychlorotrifluoroethylene (PCTFE) filler.
6. The resin composition according to any one of claims 1 to 5, wherein the average particle size of the component (B) is 0.1 to 10 µm.
7. The resin composition according to any one of claims 1 to 6, wherein the content of the component (B) is 1 mass% or more and less than 50 mass% based on the solid content of the resin composition.
8. The resin composition according to any one of claims 1 to 7, wherein the content of the component (B) is 1 to 40 mass% based on the solid content of the resin composition.
9. The resin composition according to any one of claims 1 to 8, wherein the component (X) has a hydroxy group and a hydrocarbon group.
10. The resin composition according to claim 9, wherein the hydrocarbon group includes a hydrocarbon group having 1 to 4 carbon atoms and a hydrocarbon group having 5 to 30 carbon atoms.
11. The resin composition according to any one of claims 1 to 10, further comprising one or more thermosetting resins (C) selected from the group consisting of epoxy resins, cyanate resins, and maleimide compounds.
12. The resin composition according to claim 11, comprising the maleimide compound as the component (C), the maleimide compound being a modified maleimide compound having a structural unit derived from a maleimide compound (c1) having at least two N-substituted maleimide groups and a structural unit derived from an amine compound (c2) having a primary amino group.
13. The resin composition according to claim 12, wherein the modified maleimide compound is a compound represented by the following general formula (C-1): 【Chemistry 1】 (In the formula, X c1 and X c2 are each independently a divalent organic group.
14. The resin composition according to any one of claims 11 to 13, wherein the content ratio of the (A) component to the (C) component [(A) / (C)] is 5 / 95 to 80 / 20 in terms of mass ratio.
15. The resin composition according to any one of claims 1 to 14, further comprising one or more selected from the group consisting of a thermoplastic elastomer (D), a curing accelerator (E), and an inorganic filler (F).
16. A resin-coated metal foil having a layer of the resin composition according to any one of claims 1 to 15 on the metal foil.
17. A prepreg comprising the resin composition according to any one of claims 1 to 15 and a sheet-like fiber reinforcing substrate.
18. A laminate comprising (i) the resin-coated metal foil according to claim 16 or (ii) the prepreg according to claim 17 and a metal foil.
19. A multilayer printed wiring board comprising: (i) the resin-coated metal foil according to claim 16; (ii) the prepreg according to claim 17; or (iii) the laminate according to claim 18.
20. A semiconductor package comprising the multilayer printed wiring board according to claim 19 and a semiconductor element mounted thereon.
Citation Information
Patent Citations
Laminated board and its molding method
JP1983069046A
Lighting device of industrial telecamera
JP1986018937A
Curable resin composition
JP2002129006A
Resin composition, insulating film using the same, and semiconductor device