Steel plate and its manufacturing method
A phenolic resin film with specific wax and surface roughness enhances steel plate formability and removability, addressing press formability and weldability issues in complex molding.
Patent Information
- Application Number
- JP2021206704
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-06-04
- Filing Date
- 2021-12-21
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2041-12-21
AI Technical Summary
Existing steel plates face challenges in achieving sufficient press formability for complex molding, die galling, and require effective film removability in alkaline degreasing processes, while maintaining weldability.
A steel plate coated with a phenolic resin film containing a specific amount of wax with a melting point between 100°C and 145°C, along with a base resin, to enhance lubricity and film removability, and a surface roughness of 1.5 μm or less for improved sliding properties.
The solution provides excellent press formability, reduced friction with molds, stable film removability, and maintained weldability, ensuring effective processing without interference in post-processes like welding and painting.
Smart Images

Figure 0007552576000006 
Figure 0007552576000007 
Figure 0007552576000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a steel sheet having excellent sliding properties in press forming, and a method for producing the same, and in particular to a steel sheet having excellent formability even in severe drawing and a lubricating coating which can be removed by alkali, and a method for producing the same. [Background technology]
[0002] Cold-rolled steel sheets and hot-rolled steel sheets are widely used in a wide range of fields, mainly for automobile body applications, and in such applications, they are subjected to press forming before use. In recent years, there has been a demand for the integration of parts to reduce processes and for improved design, making it necessary to enable more complex forming. If more complex press forming is attempted, there is a possibility that the steel sheet will not be able to withstand the forming and break, or that die galling will occur during continuous press forming, which could have a serious adverse effect on automobile productivity. Therefore, it is necessary to improve the press formability of steel sheets.
[0003] One method for improving the press formability of cold-rolled steel sheets and hot-rolled steel sheets is to perform surface treatment on the die. This method is widely used, but the die cannot be adjusted after the surface treatment. In addition, this method has problems such as high costs. Therefore, there is a strong demand for improving the press formability of the steel sheet itself.
[0004] One method to improve press formability without surface treatment of the die is to use a high viscosity lubricant, but this can lead to poor degreasing after press forming, which can lead to poor paintability.
[0005] In response to this, various types of lubricant surface-treated steel sheets have been investigated as a technology that enables press forming without the need for surface treatment of dies or high-viscosity lubricants.
[0006] Patent Document 1 describes a technique for forming a lubricating film, which is an acrylic resin film containing synthetic resin powder, on a zinc-plated steel sheet.
[0007] Patent Document 2 describes a technique in which lithium silicate is used as a coating component, to which wax and metal soap are added as lubricants, to form a coating on a steel sheet.
[0008] Patent Document 3 describes a lubricating surface-treated metal product having excellent press formability, which is coated with a 0.5 to 5 μm thick film made of polyurethane resin containing a lubricant.
[0009] Patent Document 4 describes a technique for forming an alkali-soluble organic film, which is an epoxy resin containing a lubricant added thereto, on a steel sheet. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] Japanese Patent Application Publication No. 9-170059 [Patent Document 2] JP 2002-307613 A [Patent Document 3] JP 2000-309747 A [Patent Document 4] JP 2000-167981 A Summary of the Invention [Problem to be solved by the invention]
[0011] However, in Patent Documents 1 to 4, although lubricity is achieved by the lubricating effect of the lubricant contained therein, press formability is not necessarily sufficient in complex forming.
[0012] The present invention has been made in consideration of the above circumstances, and aims to provide a steel sheet that is subjected to complex forming that is difficult to press form, and that has low sliding resistance in areas at risk of cracking during press forming, and excellent press formability in areas where the surface pressure is high and mold galling is expected to occur, and a manufacturing method thereof.
[0013] In addition, when the steel sheet is used as an automobile steel sheet, it is required to have sufficient removability in the alkaline degreasing step in the painting process, and further, excellent weldability. In such applications, it is a further object to have both good removability and weldability. [Means for solving the problem]
[0014] The present inventors have conducted extensive research to solve the above problems, and as a result, have found that the above problems can be dramatically improved by forming, on the surface of a steel sheet, a phenolic resin coating containing a specific amount of wax having a melting point of 100°C or more and 145°C or less, or a base resin coating consisting of a phenolic resin and a resin other than the phenolic resin, in a specific range of adhesion amount.
[0015] They also discovered that there are suitable ranges for the type and average particle size of the wax, and that the surface roughness of the steel sheet to which the resin film is to be attached has an effect.
[0016] The present invention has been completed based on the above findings, and the gist of the present invention is as follows. [1] A lubricating coating containing a phenolic resin and a wax, the melting point of which is 100°C or more and 145°C or less, and containing 10% by mass or more and 50% by mass or less of wax relative to 100% by mass of the phenolic resin, is applied to at least one side of the coating in an amount of 0.2 g / m per side after drying. 2 More than 2.0g / m 2 Steel plate having the following properties: [2] A lubricating coating containing a base resin composed of a phenolic resin and a resin other than a phenolic resin, and a wax, the solid content of the phenolic resin being 30% by mass or more and less than 100% by mass of the total solid content of the base resin, the wax having a melting point of 100°C or more and 145°C or less, and containing 10% by mass or more and 50% by mass or less of wax relative to 100% by mass of the total solid content of the base resin, is formed on at least one side in an amount of 0.2 g / m per side after drying. 2 More than 2.0g / m 2 Steel plate having the following properties: [3] The steel sheet according to [1] or [2], wherein the wax is a hydrocarbon-based wax. [4] The steel sheet according to any one of [1] to [3], wherein the wax has an average particle size of 0.01 μm or more and 4 μm or less. [5] The steel sheet according to any one of [1] to [4], characterized in that the surface roughness of the steel sheet before the application of a lubricating coating thereto is 1.5 μm or less in terms of arithmetic mean roughness Ra. [6] A method for producing a steel sheet according to any one of [1] to [5], comprising applying a coating material obtained by mixing a base resin, which is made of a phenolic resin or a resin other than a phenolic resin, and wax, to a steel sheet using an aqueous solvent, and then drying the coating material by heating to obtain a coating weight of 0.2 g / m per side after drying. 2 More than 2.0g / m 2 A method for manufacturing a steel sheet, comprising forming the following lubricating film on the steel sheet.
[0017] In the present invention, the steel sheet refers to a hot-rolled steel sheet and a cold-rolled steel sheet.
[0018] The surface roughness of a steel sheet before a lubricating coating is applied is the roughness of the base steel sheet before the lubricating coating is applied, but after the lubricating coating is applied, the lubricating coating can be removed with an organic solvent or the like to expose the base steel sheet surface, and the surface roughness can be measured. Effect of the Invention
[0019] According to the present invention, a steel sheet having excellent press formability can be obtained. The coefficient of friction between the steel sheet and a die or the like is significantly reduced. Therefore, it is possible to impart stable and excellent press formability to a steel sheet having a relatively low strength that is subjected to complex forming. Furthermore, even in a high-strength steel sheet in which the surface pressure during press forming increases, a steel sheet having low sliding resistance in areas at risk of cracking during press forming and excellent press formability in areas where the surface pressure is high and die galling is expected to occur can be obtained. Furthermore, there is no impediment to subsequent processes such as welding, degreasing, chemical conversion treatment, and painting.
[0020] In the above, "high strength" refers to a tensile strength (TS) of 440 MPa or more, and "relatively low strength" refers to a TS of less than 440 MPa. [Brief description of the drawings]
[0021] [Figure 1] FIG. 2 is a schematic front view showing a friction coefficient measuring device. [Diagram 2] FIG. 2 is a schematic perspective view showing the shape and dimensions of the bead in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] Hereinafter, an embodiment of the present invention will be described.
[0023] The present invention is characterized in that the steel sheet surface has a phenolic resin film and a lubricating film containing 10% by mass or more and 50% by mass or less of wax having a melting point of 100°C or more and 145°C or less, relative to 100% by mass of the phenolic resin, or a base resin film consisting of a phenolic resin and a resin other than phenolic resin, and a lubricating film containing 10% by mass or more and 50% by mass or less of wax having a melting point of 100°C or more and 145°C or less, relative to 100% by mass of the total solids content of the base resin. The reason for using a phenol-based resin is that it has better sliding properties than other resins.
[0024] The phenolic resin used in the present invention is not particularly limited. From the viewpoint of the coating environment, a resol-based phenolic resin that can be dissolved or dispersed in an aqueous solvent is preferably used. Although there are many unknowns regarding the mechanism by which the use of a phenolic resin exhibits excellent sliding properties, it is considered possible that the three-dimensional network structure obtained after thermal curing contributes to protecting the steel sheet surface during sliding and reducing sliding resistance.
[0025] In the present invention, not only an embodiment using only a phenolic resin as a resin, but also an embodiment using a base resin consisting of a phenolic resin and a resin other than a phenolic resin can be used. In such an embodiment, the solid content of the phenolic resin must be 30% by mass or more and less than 100% by mass of the total solid content of the base resin. If the solid content of the phenolic resin is less than 30% by mass of the total solid content of the base resin, the desired sliding properties cannot be obtained. In addition, examples of resins other than phenolic resins include acrylic resins, urethane resins, epoxy resins, polyester resins, vinyl resins, etc., but are not limited thereto.
[0026] The wax used in the present invention must have a melting point of 100°C or higher and 145°C or lower. From the viewpoint of cost and performance, a hydrocarbon wax is preferable. A hydrocarbon wax is a lubricant consisting of carbon and hydrogen, and includes natural waxes such as paraffin and microcrystalline wax, and synthetic waxes such as polyethylene and polypropylene. If the wax has a melting point of less than 100°C, it will melt due to frictional heat caused by sliding during press molding, and sufficient lubricating effect will not be obtained. If the melting point exceeds 145°C, the lubricating effect will not be exerted during sliding.
[0027] Here, the melting point of the wax is the melting temperature measured based on JIS K 7121:1987 "Method of measuring transition temperature of plastics". The particle size of the wax is preferably 0.01 μm or more and 4 μm or less. If the particle size is 0.01 μm or less, the effect of improving sliding properties may not be exhibited and the paint stability is also low. If the particle size exceeds 4 μm, the wax may not be mixed well into the film when applied and may easily fall off from the coating when handling the steel sheet after application, resulting in a loss of sliding properties.
[0028] Here, the particle size of the wax is the median diameter of the volume average diameter, and can be determined by a laser diffraction / scattering method, for example, by measuring a sample diluted with pure water using a laser diffraction / scattering type particle size distribution measuring device Partica (registered trademark) LA-960V2 (manufactured by Horiba, Ltd.).
[0029] The wax content in the coating is 10% by mass or more and 50% by mass or less based on 100% by mass of the phenolic resin. If it is less than 10% by mass, sufficient lubrication effect cannot be obtained. If it exceeds 50% by mass, the wax is likely to fall off due to a lack of resin components, and the coating may not be stable.
[0030] When a base resin composed of a phenolic resin and a resin other than a phenolic resin is used as the resin, the wax content in the coating is 10% by mass or more and 50% by mass or less relative to 100% by mass of the total solid content of the base resin, for the reasons explained above.
[0031] Here, the mass ratio of the wax in the coating is the mass ratio of the solid content of the wax in the coating to the total mass of the solid content of the organic resin in the coating and the solid content of the wax in the coating. As a specific measurement method, a test piece with a known amount of the organic resin and wax attached to the steel plate is prepared, infrared absorption spectrum is measured by an FT-IR measurement device, and a calibration curve of the amount of the organic resin and the wax attached is created from the peak intensity derived from each of the organic resin and the wax. Next, the infrared absorption spectrum of the lubricating coating coated steel plate to be measured is measured, and the amount of the resin and the wax attached is calculated from the calibration curve, so that the mass ratio of the wax in the coating can be calculated.
[0032] In the present invention, a surface conditioner for adjusting the surface tension, a defoamer, a dispersant, etc. may be included as components other than the phenolic resin and the wax. Also, a rust inhibitor for improving rust prevention may be added.
[0033] The surface roughness of the steel plate used in the present invention is preferably 1.5 μm or less in terms of arithmetic mean roughness Ra. If Ra is 1.5 μm or less, the lubricating effect of the film can be stably obtained. If Ra exceeds 1.5 μm, the unevenness of the steel plate becomes large, so that the film in the recessed parts does not work effectively during sliding, and the lubricating effect of the film may be reduced. The arithmetic mean roughness Ra (μm) of the steel plate can be measured according to JIS B 0633:2001 (ISO 4288:1996). For example, when Ra is greater than 0.1 and less than 2, the cutoff value and the reference length are set to 0.8 mm, and the evaluation length is set to 4 mm, and the roughness is determined from the roughness curve measured. When Ra is greater than 2 and less than 10, the cutoff value and the reference length are set to 2.5 mm, and the evaluation length is set to 12.5 mm, and the roughness is determined from the roughness curve measured.
[0034] Next, a method for producing a steel sheet according to the present invention will be described.
[0035] The method for producing a steel sheet of the present invention is a method for producing a steel sheet having a phenolic resin coating containing wax having a melting point of 100°C to 145°C on the surface of the steel sheet. A paint prepared by adding wax to a phenolic resin solution or emulsion in which a phenolic resin is dissolved or dispersed in a solvent is applied to the surface of the steel sheet and then dried. The application method is not particularly limited, and examples include a method using a roll coater or a bar coater, and a method of application by spraying, immersion, or brushing. The method for drying the steel sheet after application can be a general method. For example, drying by hot air, drying by an IH heater, or infrared heating can be used. The maximum temperature reached by the steel sheet during drying is preferably 60°C to 150°C. If the temperature is less than 60°C, it will take a long time to dry and the rust prevention properties may be poor. If the temperature is 150°C or higher, the film removal properties may be deteriorated. The adhesion amount after drying is 0.2 g / m 2 More than 2.0g / m 2 Not more than 0.2g / m 2 If the density is less than 2.0 g / m, sufficient press formability cannot be obtained. 2The coating weight can be determined by a method in which the difference in weight of the steel sheet before and after coating is divided by the area, or by a method in which the coating of the steel sheet after coating is completely removed with an alkaline aqueous solution or an organic solvent, and then the difference in weight of the steel sheet before and after coating removal is divided by the area. EXAMPLES
[0036] The present invention will be described below with reference to examples, but the present invention is not limited to the following examples.
[0037] Cold-rolled steel sheets (TS: 270 MPa) with a thickness of 0.8 mm and cold-rolled steel sheets (TS: 590 MPa class) with different surface roughness (arithmetic mean roughness Ra) shown in Table 1, A to D, and cold-rolled steel sheets (TS: 590 MPa class) with a thickness of 1.0 mm shown in E were degreased using Fine Cleaner (registered trademark) E6403 (manufactured by Nihon Parkerizing Co., Ltd.) as a pretreatment to remove oil and dirt from the surface. After rinsing with tap water to confirm that the test material was 100% wetted with water, the test material was heated in an electric oven with the heating temperature set to 100°C to form a substrate on which a lubricating film was formed.
[0038] [Table 1]
[0039] The types of resins used as test materials, the types of waxes, their mass percentages relative to the resin, melting points, and particle sizes are shown in Table 2. Phenol resin, acrylic resin, and urethane resin were used as test materials.
[0040] The waxes used as test materials were polyethylene wax, polypropylene wax, and microcrystalline wax.
[0041] Paint containing the resin and wax shown in Table 2 was applied with a bar coater so that the specified amount of paint would adhere to the steel plate after drying, and the steel plate was heated and dried using an electric oven set at 100°C so that the surface temperature of the steel plate reached 80°C, forming a coating.
[0042] [Table 2]
[0043] (1) Method for evaluating press formability (sliding characteristics) In order to evaluate the press formability, the friction coefficient of each test material was measured as follows.
[0044] FIG. 1 is a schematic front view showing a friction coefficient measuring device. As shown in the figure, a friction coefficient measuring sample 1 taken from a test material is fixed to a sample stage 2, and the sample stage 2 is fixed to the upper surface of a horizontally movable slide table 3. A slide table support base 5 having a roller 4 in contact with the slide table 3 and movable up and down is provided on the lower surface of the slide table 3, and a first load cell 7 is attached to the slide table support base 5 for measuring the pressing load N of the bead 6 on the friction coefficient measuring sample 1 by pushing it up. A second load cell 8 is attached to one end of the slide table 3 for measuring the sliding resistance force F for moving the slide table 3 in the horizontal direction while the pressing force is applied. The test was performed by applying press cleaning oil Pleton (registered trademark) R352L manufactured by Sugimura Chemical Industry Co., Ltd. as a lubricant to the surface of the sample 1.
[0045] Figure 2 is a schematic perspective view showing the shape and dimensions of the bead used. The bead 6 slides while its underside is pressed against the surface of the sample 1. The shape of the bead 6 shown in Figure 2 is 10 mm wide, 59 mm long in the sliding direction of the sample, and the lower parts of both ends in the sliding direction are curved surfaces with a curvature of 4.5 mmR, and the underside of the bead against which the sample is pressed has a flat surface with a width of 10 mm and a length of 50 mm in the sliding direction.
[0046] The friction coefficient measurement test was performed using the bead shown in Figure 2, with a pressing load N of 400 kgf and a sample pull-out speed (horizontal movement speed of the slide table 3) of 20 cm / min. The friction coefficient μ between the test material and the bead was calculated by the formula μ = F / N. A friction coefficient of 0.110 or less was evaluated as being particularly excellent slidability, with a rating of ◎, a coefficient of friction between more than 0.110 and 0.130 or less was evaluated as being good slidability, a coefficient of friction between more than 0.130 and 0.150 or less was evaluated as being slightly poor, with a rating of ×, and a coefficient of friction exceeding 0.150 being evaluated as being insufficient.
[0047] (2) Evaluation method for film removal To determine the removability of the coating of the steel sheet, first, each test piece was degreased with an alkaline degreaser Fine Cleaner (registered trademark) E6403 (manufactured by Nippon Parkerizing Co., Ltd.). In this treatment, the test piece was immersed in a degreasing solution with a degreaser concentration of 20 g / L and a temperature of 40° C. for a predetermined period of time, and then washed with tap water. After this treatment, the surface carbon intensity of the test piece was measured using an X-ray fluorescence analyzer, and the coating peeling rate was calculated according to the following formula using this measured value, the previously measured surface carbon intensity before degreasing, and the measured value of the surface carbon intensity of the untreated steel sheet.
[0048] The removability of the coating of the steel sheet was evaluated according to the following criteria, based on the immersion time in the alkaline degreasing solution at which the coating peeling rate reached 98% or more. <Coating peeling rate> Film peeling rate (%) = [(carbon strength before degreasing - carbon strength after degreasing) / (carbon strength before degreasing - carbon strength of untreated steel plate)] x 100 <Evaluation criteria> Good ○: Within 60 seconds Bad ×: Over 60 seconds
[0049] (3) Weldability evaluation method For each test piece, a continuous welding test was performed under the following conditions: electrode used: DR type Cr-Cu electrode, pressure: 150 kgf, current application time: 10 cycles / 60 Hz, welding current: 7.5 kA, and the welding performance was evaluated based on the number of continuous welding points. The evaluation criteria were as follows: <Evaluation criteria> Good ○: 5000 points or more Defective ×: Less than 5000 points Table 3 shows the amount of the lubricating film on the test materials and the performance evaluation results.
[0050] The test material for paint No. 1 did not have good sliding properties because the mass % of wax to phenolic resin was less than 10 mass %. The test materials for paint Nos. 11, 12, and 13 did not have good sliding properties because the melting point of the wax was outside the range of 110 to 145°C. The test materials for paint Nos. 15, 16, 17, and 18 did not have good sliding properties because the resin was not a phenolic resin. Furthermore, the test materials for paint Nos. 17 and 18 had poor film removal properties because the resin was a urethane resin. The lubricating film thickness of specimens No. 4 and No. 31 was 0.2 g / m 2 The lubricating film adhesion amount of the test pieces No. 7 and No. 34 was less than 2 g / m. 2 Therefore, the weldability was not good.
[0051] In comparison, all of the examples of the present invention were excellent in terms of sliding properties, film removal properties, and weldability.
[0052] [Table 3] EXAMPLES
[0053] A cold-rolled steel sheet (TS: 270 MPa) with a thickness of 0.8 mm and a surface roughness (arithmetic mean roughness Ra) shown in B of Table 1 was degreased using Fine Cleaner (registered trademark) E6403 (manufactured by Nihon Parkerizing Co., Ltd.) as a pretreatment to remove oil and dirt from the surface. The test material was then rinsed with tap water to confirm that it was 100% wetted with water, and then heated in an electric oven with the heating temperature set to 100°C to form a substrate on which a lubricating film was formed.
[0054] The types of base resins used in the test materials, the mass% of each base resin solid content relative to the total solid content of the resin, the type of wax, its mass% relative to the resin, melting point, and particle size are shown in Table 4. The base resin used in the test materials was a mixture of phenolic resin and acrylic resin. The wax used in the test materials was polyethylene wax.
[0055] A paint containing the base resin and wax shown in Table 4 was applied with a bar coater so that the specified amount of paint would adhere to the steel plate after drying, and the steel plate was heated and dried in an electric oven set at 100°C so that the surface temperature of the steel plate reached 80°C, forming a coating.
[0056] [Table 4]
[0057] The press formability (sliding characteristics), film removal property, and weldability were evaluated in the same manner as in Example 1 described above.
[0058] Table 5 shows the amount of the lubricating film adhered to the test materials and the performance evaluation results.
[0059] The test material for paint No. 23 did not have good sliding properties because it did not contain a phenolic resin in the film. In contrast, all of the inventive examples of the present invention had good sliding properties, film removal properties, and weldability. Furthermore, when the solid content of the phenolic resin relative to the total solid content of the resin was 30 mass% or more, the sliding properties were good, and when the solid content of the phenolic resin was 50 mass% or more, the sliding properties were particularly good.
[0060] [Table 5] [Industrial Applicability]
[0061] The steel sheet of the present invention is excellent in press formability, coating removal property, and weldability, and therefore can be used in a wide range of fields, primarily in automobile body applications. [Explanation of symbols]
[0062] 1. Sample for measuring friction coefficient 2 Sample stage 3 Slide table 4. Lola 5 Slide table support 6 Beads 7 First load cell 8 Second Load Cell 9. Rail
Claims
1. A lubricating coating containing a resin consisting of only a phenolic resin and a wax, the wax having a melting point of 100° C. or more and 145° C. or less, and containing 10% by mass or more and 50% by mass or less of wax relative to 100% by mass of the resin consisting of only the phenolic resin, is applied to at least one surface in an amount of 0.2 g / m per surface after drying. 2 2.0g / m or more 2 Steel plate having the following properties:
2. A lubricating coating containing a base resin composed of a phenolic resin and a resin other than a phenolic resin and wax, the solid content of the phenolic resin being 50% by mass or more and less than 100% by mass of the total solid content of the base resin, the wax having a melting point of 100°C or more and 145°C or less, and containing 10% by mass or more and 50% by mass or less of wax relative to 100% by mass of the total solid content of the base resin, is formed on at least one surface in an amount of 0.2 g / m per surface after drying. 2 More than 2.0g / m 2 Steel plate having the following properties:
3. The steel sheet according to claim 1 or 2, wherein the wax is a hydrocarbon wax.
4. The steel sheet according to any one of claims 1 to 3, wherein the wax has an average particle size of 0.01 µm or more and 4 µm or less.
5. 5. The steel sheet according to claim 1, wherein the surface roughness of the steel sheet before the lubricating coating is applied is 1.5 μm or less in terms of arithmetic mean roughness Ra.
6. 6. The steel sheet according to claim 5, wherein the surface roughness of the steel sheet before the lubricating coating is applied is 0.5 μm or more in terms of arithmetic mean roughness Ra.
7. A method for producing a steel sheet according to any one of claims 1 to 6, comprising applying a coating material, which is a mixture of wax and a base resin consisting of only a phenolic resin or a phenolic resin and a resin other than a phenolic resin, to a steel sheet using an aqueous solvent, and then drying by heating to obtain a coating amount of 0.2 g / m per side after drying. 2 2.0g / m or more 2 A method for manufacturing a steel sheet, comprising forming the following lubricating film on the steel sheet.
Citation Information
Patent Citations
Steel plate having high clear reflection excellent in workability
JP1988132728A
Precoat steel plate for di can
JP1990303633A
High tensile strength thin steel sheet having excellent press-formability
JP1995032056A
Galvanized steel sheet covered with alkali-soluble resin coating film having excellent adhesiveness by adhesive
JP1997170059A
Alkali-soluble type organic film-coated steel sheet having excellent adhesiveness and anti-mold galling property