Silica sol, polishing composition, method for polishing silicon wafer, method for manufacturing silicon wafer, chemical mechanical polishing composition, and method for manufacturing semiconductor device

Optimized colloidal silica with specific particle sizes and low metal impurities addresses the issues of insufficient polishing rates and contamination, enhancing silicon wafer polishing efficiency and productivity.

JP7552669B2Active Publication Date: 2024-09-18MITSUBISHI CHEM CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2022171489
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2017-11-10
Filing Date
2022-10-26
Publication Date
2024-09-18
Estimated Expiration
2038-08-27

AI Technical Summary

Technical Problem

Existing colloidal silica used in polishing silicon wafers and semiconductor manufacturing suffers from insufficient polishing rates and contamination from metal impurities, affecting semiconductor characteristics and productivity.

Method used

Optimizing colloidal silica with a surface silanol group density of 4/nm², average primary particle diameter of 15-100 nm, and average secondary particle diameter of 40-200 nm, produced from tetraalkoxysilane, with a metal impurity content of 1 ppm or less, and incorporating it into a silica sol and polishing composition with water-soluble polymers.

Benefits of technology

The optimized colloidal silica and polishing composition achieve enhanced polishing rates and improved silicon wafer productivity by reducing metal impurities and surface roughness, ensuring high precision and cleanliness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007552669000001
    Figure 0007552669000001
Patent Text Reader

Abstract

The present invention provides colloidal silica, silica sol, and polishing composition having a low content of metal impurities and an excellent polishing rate, as well as a method for polishing silicon wafers and a method for manufacturing silicon wafers that are excellent in productivity. The silica sol for polishing silicon wafers, excluding silicon wafers with a TEOS film, contains colloidal silica and water, has a metal impurity content of 1 ppm or less, and has a surface silanol group density of 5 / nm2 as measured by the Sears method. 2 ~14 pieces / nm 2 A polishing composition comprising the silica sol and a water-soluble polymer.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to colloidal silica. Also, the present invention relates to a silica sol. Also, the present invention relates to a polishing composition. Also, the present invention relates to a method for polishing a silicon wafer. Also, the present invention relates to a method for producing a silicon wafer. Also, the present invention relates to a chemical mechanical polishing composition. Furthermore, the present invention relates to a method for producing a semiconductor device. [Background technology]

[0002] Polishing methods using polishing liquids are known as methods for polishing the surfaces of materials such as metals and inorganic compounds. In particular, in the final polishing of prime silicon wafers for semiconductors and reclaimed silicon wafers, and in chemical mechanical polishing (CMP) for planarizing interlayer insulating films during semiconductor device manufacturing, forming metal plugs, forming buried wiring, and the like, the surface condition has a significant effect on the semiconductor characteristics, so the surfaces and end faces of these components are required to be polished with extremely high precision. In such precision polishing, a polishing composition containing silica sol is adopted, and colloidal silica is widely used as the abrasive grains, which are the main component. Depending on the manufacturing method, colloidal silica is known to be produced by pyrolysis of silicon tetrachloride (fumed silica, etc.), by deionization of alkali silicate such as water glass, by hydrolysis reaction of alkoxysilane (generally called the "sol-gel method"), etc.

[0003] It is known that the physical properties of colloidal silica affect its performance as a polishing liquid, and many studies have been conducted on it. In particular, the effect of silanol groups on the surface of colloidal silica particles on polishing performance has been extensively studied not only in the polishing of silicon wafers, but also in the chemical mechanical polishing used in the manufacture of semiconductor devices.

[0004] For example, Patent Document 1 discloses colloidal silica for use in polishing silicon wafers. Patent Document 2 discloses colloidal silica for use in polishing insulating films of semiconductor wafers. Patent Document 3 discloses colloidal silica for use in polishing metal films, barrier metal films, and insulating films. Patent Document 4 discloses colloidal silica for use in selective polishing of multilayer wiring sections. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 02-158684 [Patent Document 2] JP 2006-231436 A [Patent Document 3] JP 2009-224767 A [Patent Document 4] International Publication No. 2014 / 007063 Brochure Summary of the Invention [Problem to be solved by the invention]

[0006] However, it is unclear whether the colloidal silica disclosed in Patent Document 1 is made mainly from tetraalkoxysilane, and it is also unclear whether the metal impurity content is low. Therefore, even if silicon wafers are polished using the colloidal silica disclosed in Patent Document 1, it is highly likely that a sufficient polishing rate will not be achieved. In addition, since the colloidal silicas disclosed in Patent Documents 2 to 4 are not intended to polish silicon wafers, even if silicon wafers are polished using the colloidal silicas disclosed in Patent Documents 2 to 4, there is a high possibility that they will not have a sufficient polishing rate.

[0007] However, in the polishing of silicon wafers for semiconductors and in the chemical mechanical polishing in the manufacture of semiconductor devices, there is a problem that transition metals, alkali metals, alkaline earth metals, etc. adhere to the surface of the object to be polished as impurities, contaminating the surface and adversely affecting the semiconductor characteristics. Therefore, in these polishing processes, there is a demand for high-purity colloidal silica in which the inclusion of metal impurities is minimized, that is, colloidal silica produced by hydrolysis reaction using tetraalkoxysilane as the main raw material. Furthermore, in polishing silicon wafers using such high purity colloidal silica, there is a demand for improving the polishability of silicon wafers, i.e., improving the polishing rate, in order to improve the productivity of silicon wafers.

[0008] The present invention has been made in view of the above problems, and an object of the present invention is to provide a colloidal silica, a silica sol, and a polishing composition having a low content of metal impurities and an excellent polishing rate. Another object of the present invention is to provide a method for polishing silicon wafers and a method for manufacturing silicon wafers, which are excellent in productivity of silicon wafers. [Means for solving the problem]

[0009] When silicon wafers are polished using conventional high-purity colloidal silica, the polishing rate is not necessarily sufficient. However, the present inventors have conducted extensive research and found that optimizing the surface silanol group density of high-purity colloidal silica improves the polishing rate in polishing silicon wafers using high-purity colloidal silica, thereby completing the present invention.

[0010] That is, the gist of the present invention is as follows. [1] A colloidal silica made primarily from tetraalkoxysilane, with a surface silanol group density of 4 / nm2 as measured by the Sears method. 2 That's it, colloidal silica. [2] The colloidal silica according to [1], having an average primary particle diameter measured by a BET method of 15 nm to 100 nm. [3] The colloidal silica according to [1] or [2], having an average secondary particle diameter of 40 nm to 200 nm as measured by a DLS method. [4] The colloidal silica according to any one of [1] to [3], wherein the tetraalkoxysilane is tetramethoxysilane. [5] A silica sol comprising the colloidal silica according to any one of [1] to [4] and water. [6] The silica sol according to [5], wherein the content of colloidal silica is 3% by mass to 50% by mass with respect to 100% by mass of the total amount of the silica sol. [7] The silica sol according to [5] or [6], having a metal impurity content of 1 ppm or less. [8] A polishing composition comprising the silica sol according to any one of [5] to [7] and a water-soluble polymer. [9] A method for polishing a silicon wafer, comprising polishing a silicon wafer with the polishing composition according to [8].

[10] A method for producing a silicon wafer, comprising the method for polishing a silicon wafer according to [9].

[11] A chemical mechanical polishing composition comprising the silica sol according to any one of [5] to [7].

[12] A method for manufacturing a semiconductor device, comprising a step of performing chemical mechanical polishing using the chemical mechanical polishing composition described in

[11] . Effect of the Invention

[0011] The colloidal silica of the present invention has an excellent polishing rate. The silica sol of the present invention has an excellent polishing rate. The polishing composition of the present invention has an excellent polishing rate. The method for polishing silicon wafers of the present invention has excellent silicon wafer productivity. Furthermore, the method for producing silicon wafers of the present invention has excellent silicon wafer productivity. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present invention will be described in detail below, but the present invention is not limited to the following embodiments and can be modified and practiced in various ways within the scope of the gist. In addition, when the expression "~" is used in this specification, it is used as an expression including the numerical value or physical property value before and after it.

[0013] (Colloidal Silica) The colloidal silica of the present invention has a surface silanol group density of 4 / nm2 as measured by the Sears method. 2 The surface silanol group density of colloidal silica is set to 4 / nm 2 By satisfying the above, the polishing rate is excellent and the productivity of silicon wafers is excellent because the polishing agent has excellent adhesion to silicon wafers and excellent affinity with water-soluble polymers.

[0014] (Surface silanol group density) In this specification, the surface silanol group density of colloidal silica is measured by the Sears method, and specifically, is measured and calculated under the conditions shown below. Take a silica sol equivalent to 1.5 g of silica, add pure water to make the liquid volume 90 mL, add 0.1 mol / L hydrochloric acid aqueous solution until the pH becomes 3.6 in an environment of 25°C, add 30 g of sodium chloride, gradually add pure water to completely dissolve the sodium chloride, and finally add pure water until the total volume of the test liquid is 150 mL to obtain the test liquid. The obtained test liquid is placed in an automatic titrator, and 0.1 mol / L aqueous sodium hydroxide solution is added dropwise to measure the titer A (mL) of 0.1 mol / L aqueous sodium hydroxide solution required to change the pH from 4.0 to 9.0. The amount of 0.1 mol / L sodium hydroxide solution consumed per 1.5 g of colloidal silica to change the pH from 4.0 to 9.0, V (mL), was calculated using the following formula (1), and the surface silanol group density ρ (particles / nm 2 ) is calculated. V=(A×f×100×1.5) / (W×C) ··· (1) A: The amount (mL) of 0.1 mol / L sodium hydroxide solution required to change the pH of 1.5 g of colloidal silica from 4.0 to 9.0 f: Potency of the 0.1 mol / L sodium hydroxide solution used C: Silica concentration in silica sol (mass%) W: Amount of silica sol collected (g) ρ = (B × NA) / (10 18 ×M×S BET ) ··· (2) B: The amount of sodium hydroxide (mol) required to change the pH from 4.0 to 9.0 per 1.5 g of silica calculated from V N A : Avogadro's number (pieces / mol) M: Silica content (1.5g) S BET : Specific surface area (m2) of colloidal silica measured when calculating the average primary particle size 2 / g)

[0015] The method for measuring and calculating the surface silanol group density of the colloidal silica was based on "GW Ears, Jr., Analytical Chemistry, Vol. 28, No. 12, pp. 1981-1983 (1956)," "Haba Shinichi, Development of Abrasives for Semiconductor Integrated Circuit Processes, Doctoral Dissertation, Kochi University of Technology, pp. 39-45, March 2004," "Patent No. 5967118," and "Patent No. 6047395."

[0016] The surface silanol group density of colloidal silica is 4 / nm 2 ~15 pieces / nm 2 is preferable, and 5 particles / nm 2 ~14 pieces / nm 2 More preferably, 5.5 particles / nm 2 ~13 pieces / nm 2 It is more preferable that the surface silanol group density of the colloidal silica is 4 / nm 2When the surface silanol group density of the colloidal silica is 15 / nm or more, the surface silanol group density is 15 / nm and the surface silanol group density is 15 / nm. 2 When the colloidal silica is less than this value, the strength of the colloidal silica is excellent when used on a workpiece such as a silicon wafer, resulting in an excellent polishing rate and excellent removal of particles and the like during cleaning after polishing.

[0017] The surface silanol group density of colloidal silica can be set within a desired range by adjusting the conditions of the hydrolysis and condensation reactions of tetraalkoxysilane. Specifically, the following method can be used. The so-called sol-gel method, which uses tetraalkoxysilane as the main raw material, is a method of obtaining colloidal silica by hydrolyzing tetraalkoxysilane in the presence of a catalyst such as an acid or a base, dehydrating and condensing the resulting silanol groups, and growing particles while forming siloxane bonds. In this process, the silanol groups disappear as the condensation reaction progresses, but the silanol group density inside and on the surface of colloidal silica can be increased by setting conditions such as the composition of tetraalkoxysilane, solvent, dispersion medium, catalyst during the hydrolysis reaction and condensation reaction, reaction temperature, and reaction time. In addition, the surface silanol group density can also be increased by subjecting colloidal silica to hot water treatment to hydrate the siloxane bonds. On the other hand, the silanol group density inside and on the surface can also be reduced by subjecting colloidal silica to treatment such as firing in a dry gas atmosphere at 600°C to 1250°C.

[0018] (Average primary particle size) The colloidal silica of the present invention preferably has an average primary particle diameter of 30 nm to 70 nm as measured by the BET method.

[0019] In this specification, the average primary particle size of colloidal silica is measured by the BET method. Specifically, the specific surface area of ​​colloidal silica is measured using an automatic specific surface area measuring device, and the density is calculated as 2.2 g / cm using the following formula (3). 3 and calculate the average primary particle size. Average primary particle diameter (nm) = 6000 / (specific surface area (m 2 / g) x density (g / cm 3 )) ··· (3)

[0020] The average primary particle size of colloidal silica is preferably 15 nm to 100 nm, more preferably 20 nm to 90 nm, and even more preferably 30 nm to 70 nm. When the average primary particle size of colloidal silica is 15 nm or more, the polishing rate for a workpiece such as a silicon wafer is excellent, and the storage stability of the silica sol is excellent. In addition, when the average primary particle size of colloidal silica is 100 nm or less, the surface roughness and scratches of a workpiece such as a silicon wafer during polishing can be reduced, and the dispersion stability of the silica sol is excellent.

[0021] The average primary particle size of the colloidal silica can be set within a desired range by known conditions and methods.

[0022] (Average secondary particle size) The colloidal silica of the present invention preferably has an average secondary particle diameter of 60 nm to 120 nm as measured by a DLS method.

[0023] In this specification, the average secondary particle size of colloidal silica is measured by a DLS method, specifically, using a dynamic light scattering particle size measurement device.

[0024] The average secondary particle diameter of colloidal silica is preferably 40 nm to 200 nm, more preferably 50 nm to 160 nm, and even more preferably 60 nm to 120 nm. When the average secondary particle diameter of colloidal silica is 40 nm or more, the polishing rate for a workpiece such as a silicon wafer is excellent, the removal of particles and the like during cleaning after polishing is excellent, and the storage stability of the silica sol is excellent. When the average secondary particle diameter of colloidal silica is 200 nm or less, the surface roughness and scratches of a workpiece such as a silicon wafer during polishing can be reduced, the removal of particles and the like during cleaning after polishing is excellent, and the dispersion stability of the silica sol is excellent.

[0025] The average secondary particle size of the colloidal silica can be set within a desired range according to known conditions and methods.

[0026] The cv value of the colloidal silica is preferably 15 to 50, more preferably 20 to 40. When the cv value of the colloidal silica is 15 or more, the polishing rate for a workpiece such as a silicon wafer is excellent, and the productivity of the silicon wafer is excellent. When the cv value of the colloidal silica is 50 or less, the surface roughness and scratches of a workpiece such as a silicon wafer during polishing can be reduced, and the removal of particles and the like during cleaning after polishing is excellent.

[0027] In this specification, the cv value of colloidal silica is calculated by measuring the average secondary particle size of colloidal silica using a dynamic light scattering particle size measurement device and using the following formula (4). cv value = (standard deviation (nm) / average secondary particle size (nm)) × 100 (4)

[0028] The association ratio of colloidal silica is preferably 1.2 to 2.5, more preferably 1.5 to 2.2. When the association ratio of colloidal silica is 1.2 or more, the polishing rate for a polished object such as a silicon wafer is excellent, and the productivity of silicon wafers is excellent. When the association ratio of colloidal silica is 2.5 or less, the surface roughness and scratches of a polished object such as a silicon wafer during polishing can be reduced, and the aggregation of colloidal silica in the silica sol or polishing composition can be suppressed, and the storage stability of the silica sol or polishing composition is excellent.

[0029] In this specification, the association ratio of colloidal silica is calculated using the following formula (5) from the average primary particle size measured by the above-mentioned measurement method and the average secondary particle size measured by the above-mentioned measurement method. Association ratio = average secondary particle diameter / average primary particle diameter (5)

[0030] The particle shape of colloidal silica is such that the surface silanol group density is 4 / nm 2There are no particular limitations on the above shapes, and examples of the shapes include spherical, chain-like, cocoon-like (also called lump-like or peanut-like), irregular shapes (for example, wart-like, bent, branched, etc.) Among these particle shapes of colloidal silica, spherical shapes are preferred when it is desired to reduce the surface roughness and scratches on a polished object, such as a silicon wafer, during polishing, and irregular shapes are preferred when it is desired to further increase the polishing rate for a polished object, such as a silicon wafer.

[0031] The colloidal silica of the present invention is made mainly from tetraalkoxysilane. In this specification, the term "main raw material" refers to a material that accounts for 50 mass % or more of the raw materials constituting the colloidal silica.

[0032] (Method of manufacturing colloidal silica) The colloidal silica of the present invention can be obtained by subjecting the main raw material tetraalkoxysilane to a hydrolysis reaction and a condensation reaction. The colloidal silica of the present invention can be produced by a known production method.

[0033] Examples of tetraalkoxysilane include tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, and tetraisopropoxysilane. These tetraalkoxysilanes may be used alone or in combination of two or more. Among these tetraalkoxysilanes, tetramethoxysilane and tetraethoxysilane are preferred, and tetramethoxysilane is more preferred, because they undergo rapid hydrolysis reaction, are less likely to leave unreacted material, are highly productive, and can easily produce a stable silica sol.

[0034] As the raw material for forming colloidal silica, in addition to tetraalkoxysilane, a low condensate obtained by partially hydrolyzing tetraalkoxysilane may be used.

[0035] Examples of the solvent or dispersion medium used in the hydrolysis reaction or condensation reaction include water, methanol, ethanol, propanol, isopropanol, and ethylene glycol. These solvents or dispersion media may be used alone or in combination of two or more. Among these solvents or dispersion media, water and alcohol are preferred, and water and methanol are more preferred, because the solvents used in the hydrolysis reaction or condensation reaction and the by-products are the same, and therefore are convenient for production.

[0036] The hydrolysis reaction and the condensation reaction may be carried out in the presence or absence of a catalyst, but are preferably carried out in the presence of a catalyst, since this can accelerate the hydrolysis reaction and the condensation reaction. Examples of the catalyst include acid catalysts such as hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, acetic acid, formic acid, and citric acid, and alkali catalysts such as ethylenediamine, diethylenetriamine, triethylenetetraamine, ammonia, urea, ethanolamine, and tetramethylammonium hydroxide. Among these catalysts, alkali catalysts are preferred because they have excellent catalytic action and are easy to control the particle shape, and alkali catalysts are preferred because they can suppress the inclusion of metal impurities, are highly volatile, and are easy to remove after the condensation reaction, with ammonia being more preferred.

[0037] (Silica sol) The silica sol of the present invention contains the colloidal silica of the present invention and water.

[0038] The content of colloidal silica is preferably 3% by mass to 50% by mass, more preferably 4% by mass to 40% by mass, and even more preferably 5% by mass to 30% by mass, based on the total amount of silica sol (100% by mass). When the content of colloidal silica is 3% by mass or more, the polishing rate for a polished object such as a silicon wafer is excellent. When the content of colloidal silica is 50% by mass or less, the aggregation of colloidal silica in the silica sol or polishing composition can be suppressed, and the storage stability of the silica sol or polishing composition is excellent.

[0039] The water content is preferably 50% by mass to 97% by mass, more preferably 60% by mass to 96% by mass, and even more preferably 70% by mass to 95% by mass, based on the total amount of silica sol (100% by mass). When the water content is 50% by mass or more, aggregation of colloidal silica in the silica sol or polishing composition can be suppressed, and the storage stability of the silica sol or polishing composition is excellent. Furthermore, when the water content is 97% by mass or less, the polishing rate for a workpiece such as a silicon wafer is excellent.

[0040] Examples of water include ion-exchanged water, distilled water, pure water, and ultrapure water.

[0041] In addition to colloidal silica and water, the silica sol of the present invention may contain other components, such as an oxidizing agent, an antiseptic, an antifungal agent, a pH adjuster, a pH buffer, a surfactant, a chelating agent, an antibacterial agent, or a biocide, as necessary, within the range that does not impair the performance of the silica sol. In particular, it is preferable to incorporate an antibacterial / biocide in the silica sol, since the storage stability of the silica sol is excellent.

[0042] Examples of antibacterial and biocide agents include hydrogen peroxide, ammonia, quaternary ammonium hydroxide, quaternary ammonium salt, ethylenediamine, glutaraldehyde, hydrogen peroxide, methyl p-hydroxybenzoate, sodium chlorite, etc. These antibacterial and biocide agents may be used alone or in combination of two or more. Among these antibacterial and biocide agents, hydrogen peroxide is preferred because of its excellent affinity with silica sol. Biocides also include those commonly referred to as bactericides.

[0043] The content of the antibacterial / biocide is preferably 0.0001% by mass to 10% by mass, and more preferably 0.001% by mass to 1% by mass, based on the total amount of the silica sol (100% by mass). When the content of the antibacterial / biocide is 0.0001% by mass or more, the storage stability of the silica sol is excellent. When the content of the antibacterial / biocide is 10% by mass or less, the original performance of the silica sol is not impaired.

[0044] The silica sol of the present invention preferably has a metal impurity content of 1 ppm or less for the reasons described below. When polishing silicon wafers for semiconductor devices, metallic impurities adhere to and contaminate the surface of the workpiece being polished, adversely affecting the characteristics of the wafer and diffusing into the wafer, degrading its quality, resulting in a significant decrease in the performance of semiconductor devices manufactured from such wafers. In addition, the silica sol of the present invention can achieve an excellent polishing rate for a polished object such as a silicon wafer by optimizing the surface silanol group density of the colloidal silica. If metal impurities are present in the silica sol, a coordination interaction occurs between the acidic surface silanol group and the metal impurity, which changes the chemical properties (acidity, etc.) of the surface silanol group and the three-dimensional environment of the colloidal silica surface (ease of aggregation of colloidal silica, etc.), thereby affecting the polishing rate.

[0045] In this specification, the metal impurity content of silica sol is measured by inductively coupled plasma mass spectrometry (ICP-MS). Specifically, 2 g of silica sol is accurately weighed, sulfuric acid and hydrofluoric acid are added, and the mixture is heated, dissolved, and evaporated. Pure water is added to the remaining sulfuric acid droplets so that the total amount is exactly 10 g to create a test solution, which is then measured using an inductively coupled plasma mass spectrometry device. The target metals are sodium, potassium, iron, aluminum, calcium, magnesium, zinc, cobalt, chromium, copper, manganese, lead, titanium, and silver.

[0046] The metal impurity content of silica sol can be reduced to 1 ppm or less by carrying out hydrolysis and condensation reactions (sol-gel method) using tetraalkoxysilane as the main raw material. In the method of deionizing alkali silicate such as water glass, sodium and other impurities derived from the raw material remain, making it difficult to reduce the metal impurity content of the silica sol to 1 ppm or less.

[0047] (Method of producing silica sol) The silica sol of the present invention can be obtained by removing unnecessary components from the reaction solution immediately after the production of colloidal silica and adding necessary components. The method for producing the silica sol of the present invention may be a known production method.

[0048] The silica sol of the present invention may contain components other than the colloidal silica and water in the reaction solution immediately after the production of the colloidal silica, as long as the components do not impair the performance of the silica sol, such as a solvent or dispersion medium such as alcohol, and a catalyst such as ammonia.

[0049] The colloidal silica content and water content in the silica sol can be adjusted by removing unnecessary components in the reaction liquid immediately after the production of colloidal silica, and then adding water.

[0050] The production of the silica sol may include a filtration step in order to remove coarse particles and to avoid aggregation of fine particles. Examples of the filtration method include natural filtration under normal pressure, reduced pressure filtration, pressure filtration, centrifugal filtration, and the like. Filtration may be carried out at any time and any number of times during the production of the silica sol, but is preferably carried out immediately before the preparation of the polishing composition, as this provides excellent storage stability and polishing performance of the polishing composition.

[0051] The pH of the silica sol is preferably 6.0 to 9.0, more preferably 7.0 to 8.0. When the pH of the silica sol is 6.0 or more, the silica sol has excellent long-term storage stability. When the pH of the silica sol is 9.0 or less, the aggregation of colloidal silica can be suppressed, and the silica sol has excellent dispersion stability.

[0052] (polishing composition) The polishing composition of the present invention comprises the silica sol of the present invention and a water-soluble polymer. The water-soluble polymer enhances the wettability of the polishing composition to the object to be polished, such as a silicon wafer. The water-soluble polymer is preferably a polymer having a functional group with high water affinity, and this functional group with high water affinity has a high affinity with the surface silanol group of the colloidal silica, so that the colloidal silica and the water-soluble polymer are stably dispersed in the polishing composition in a closer vicinity. Therefore, when polishing an object to be polished, such as a silicon wafer, the effects of the colloidal silica and the water-soluble polymer function synergistically.

[0053] Examples of the water-soluble polymer include cellulose derivatives, polyvinyl alcohol, polyvinylpyrrolidone, copolymers having a polyvinylpyrrolidone skeleton, and polymers having a polyoxyalkylene structure. Examples of cellulose derivatives include hydroxyethyl cellulose, hydrolyzed hydroxyethyl cellulose, hydroxypropyl cellulose, hydroxyethyl methyl cellulose, hydroxypropyl methyl cellulose, methyl cellulose, ethyl cellulose, ethyl hydroxyethyl cellulose, and carboxymethyl cellulose. An example of the copolymer having a polyvinylpyrrolidone skeleton is a graft copolymer of polyvinyl alcohol and polyvinylpyrrolidone. Examples of polymers having a polyoxyalkylene structure include polyoxyethylene, polyoxypropylene, and copolymers of ethylene oxide and propylene oxide. These water-soluble polymers may be used alone or in combination of two or more. Among these water-soluble polymers, cellulose derivatives are preferred, and hydroxyethyl cellulose is more preferred, because they have high affinity with the surface silanol groups of colloidal silica and act synergistically to impart good hydrophilicity to the surface of the polished object.

[0054] The mass average molecular weight of the water-soluble polymer is preferably 1,000 to 3,000,000, more preferably 5,000 to 2,000,000, and even more preferably 10,000 to 1,000,000. When the mass average molecular weight of the water-soluble polymer is 1,000 or more, the hydrophilicity of the polishing composition is improved. When the mass average molecular weight of the water-soluble polymer is 3,000,000 or less, the affinity with silica sol is excellent, and the polishing rate for the object to be polished, such as a silicon wafer, is excellent.

[0055] In this specification, the mass average molecular weight of a water-soluble polymer is measured by size exclusion chromatography using a 0.1 mol / L NaCl solution as the mobile phase, in terms of polyethylene oxide.

[0056] The content of the water-soluble polymer is preferably 0.02% by mass to 10% by mass, more preferably 0.05% by mass to 5% by mass, based on the total amount of the polishing composition (100% by mass). When the content of the water-soluble polymer is 0.02% by mass or more, the hydrophilicity of the polishing composition is improved. Furthermore, when the content of the water-soluble polymer is 10% by mass or less, aggregation of colloidal silica during preparation of the polishing composition can be suppressed.

[0057] The pH of the polishing composition is preferably 8.0 to 12.0, more preferably 9.0 to 11.0. When the pH of the polishing composition is 8.0 or more, the aggregation of colloidal silica in the polishing composition can be suppressed, and the dispersion stability of the polishing composition is excellent. When the pH of the polishing composition is 12.0 or less, the dissolution of colloidal silica can be suppressed, and the stability of the polishing composition is excellent. The pH of the polishing composition can be adjusted to a desired range by adding a pH adjuster described below.

[0058] In addition to the silica sol and the water-soluble polymer, the polishing composition of the present invention may contain other components, such as a basic compound, a polishing accelerator, a surfactant, a hydrophilic compound, a preservative, an antifungal agent, a pH adjuster, a pH buffer, a surfactant, a chelating agent, an antibacterial agent or a biocide, as necessary, within the range that does not impair the performance of the composition. In particular, it is preferable to include a basic compound in the polishing composition because it is possible to apply a chemical action to the surface of an object to be polished, such as a silicon wafer, to perform chemical polishing (chemical etching), and because of the synergistic effect with the surface silanol groups of the colloidal silica, it is possible to improve the polishing rate of an object to be polished, such as a silicon wafer.

[0059] Examples of the basic compound include organic basic compounds, alkali metal hydroxides, alkali metal hydrogen carbonates, alkali metal carbonates, and ammonia. These basic compounds may be used alone or in combination of two or more. Among these basic compounds, ammonia, tetramethylammonium hydroxide, tetraethylammonium hydroxide, ammonium hydrogen carbonate, and ammonium carbonate are preferred because they are highly soluble in water and have excellent affinity with colloidal silica and water-soluble polymers, and ammonia, tetramethylammonium hydroxide, and tetraethylammonium hydroxide are more preferred, with ammonia being even more preferred.

[0060] The content of the basic compound is preferably 0.001% by mass to 5% by mass, more preferably 0.01% by mass to 3% by mass, based on the total amount of the polishing composition (100% by mass). When the content of the basic compound is 0.001% by mass or more, the polishing speed of the object to be polished, such as a silicon wafer, can be improved. When the content of the basic compound is 5% by mass or less, the stability of the polishing composition is excellent.

[0061] The polishing composition of the present invention can be obtained by mixing the silica sol of the present invention, the water-soluble polymer, and, if necessary, other components. However, in consideration of storage and transportation, the composition may be prepared at a high concentration and then diluted with water or the like immediately before polishing.

[0062] (Application) The colloidal silica, silica sol, and polishing composition of the present invention can be suitably used for polishing purposes, for example, polishing semiconductor materials such as silicon wafers, polishing electronic materials such as hard disk substrates, polishing (chemical mechanical polishing) in the planarization step in manufacturing integrated circuits, polishing synthetic quartz glass substrates used for photomasks and liquid crystals, polishing magnetic disk substrates, and the like. Because of their excellent affinity for silicon surfaces, they can be particularly suitably used for polishing silicon wafers.

[0063] By polishing silicon wafers with the colloidal silica, silica sol, and polishing composition of the present invention, adhesion and contamination of silicon wafers due to metal impurities can be suppressed and the manufacturing time can be shortened, resulting in excellent productivity of high-purity silicon wafers. EXAMPLES

[0064] The present invention will be described in more detail below using examples. However, the present invention is not limited to the description of the following examples as long as it does not deviate from the gist of the present invention.

[0065] (Measurement of average primary particle size) The silica sol obtained in the examples and comparative examples was freeze-dried, and the specific surface area of ​​the colloidal silica was measured using an automatic specific surface area measuring device "Flowsorb II" (model name, manufactured by Shimadzu Corporation). The density was calculated to be 2.2 g / cm using the following formula (3). 3 The average primary particle size was calculated based on the above. Average primary particle diameter (nm) = 6000 / (specific surface area (m 2 / g) x density (g / cm 3 )) ··· (3)

[0066] (Measurement of average secondary particle size and cv value) The average secondary particle size of colloidal silica of the silica sol obtained in the examples and comparative examples was measured using a dynamic light scattering particle size measurement device "Zetersizer Nano ZS" (model name, manufactured by Malvern Instruments), and the cv value was calculated using the following formula (4). cv value = (standard deviation (nm) / average secondary particle size (nm)) × 100 (4)

[0067] (Calculation of association ratio) The association ratio was calculated from the measured average primary particle size and average secondary particle size using the following formula (5). Association ratio = average secondary particle diameter / average primary particle diameter (5)

[0068] (Surface silanol group density) Of the silica sols obtained in the Examples and Comparative Examples, an amount equivalent to 1.5 g of silica was placed in a 200 mL tall beaker, and purified water was added to make the liquid volume 90 mL. In an environment of 25°C, a pH electrode was inserted into the tall beaker, and the test liquid was stirred for 5 minutes with a magnetic stirrer. With stirring continued with the magnetic stirrer, 0.1 mol / L aqueous hydrochloric acid solution was added until the pH reached 3.6. The pH electrode was removed from the tall beaker, and with stirring continued with the magnetic stirrer, 30 g of sodium chloride was added, and pure water was gradually added until the sodium chloride was completely dissolved, and finally pure water was added until the total volume of the test liquid was 150 mL, and the test liquid was stirred for 5 minutes with a magnetic stirrer to obtain a test liquid.

[0069] The tall beaker containing the obtained test solution was placed in an automatic titration device "COM-1600" (manufactured by Hiranuma Sangyo Co., Ltd.), and the pH electrode and burette included with the device were inserted into the tall beaker. While stirring the test solution with a magnetic stirrer, 0.1 mol / L aqueous sodium hydroxide solution was dropped through the burette, and the titration amount A (mL) of 0.1 mol / L aqueous sodium hydroxide solution required to change the pH from 4.0 to 9.0 was measured. The amount of 0.1 mol / L sodium hydroxide solution consumed per 1.5 g of colloidal silica to change the pH from 4.0 to 9.0, V (mL), was calculated using the following formula (1), and the surface silanol group density ρ (particles / nm 2 ) was calculated. V=(A×f×100×1.5) / (W×C) ··· (1) A: The amount (mL) of 0.1 mol / L sodium hydroxide solution required to change the pH of 1.5 g of colloidal silica from 4.0 to 9.0 f: Potency of the 0.1 mol / L sodium hydroxide solution used C: Colloidal silica concentration in silica sol (mass%) W: Amount of silica sol collected (g) ρ = (B × NA) / (10 18 ×M×S BET ) ··· (2) B: The amount of sodium hydroxide (mol) required to change the pH from 4.0 to 9.0 per 1.5 g of silica calculated from V N A : Avogadro's number (pieces / mol) M: Silica content (1.5g) S BET : Specific surface area (m2) of colloidal silica measured when calculating the average primary particle size 2 / g)

[0070] (polishing rate) 97.5 g of the silica sol obtained in the examples and comparative examples was mixed with 3 g of 29 mass % ammonia water to obtain a silica sol with a pH of 10.7. 40 g of a 1.4 mass % hydroxyethyl cellulose aqueous solution ("SE550" (trade name), manufactured by Daicel Corporation, mass average molecular weight approximately 800,000) was added and mixed with the obtained silica sol with a pH of 10.7, and further 62.5 g of pure water was added and mixed, and the mixture was filtered through a 1 μm membrane filter to obtain a polishing composition with a pH of 10.5.

[0071] The obtained polishing composition was diluted 30 times with pure water and applied to a silicon chip (p-type, crystal orientation 100-150 mm) cut into a 3 cm square. <100> ) was polished under the following polishing conditions. Polishing device: Doctor wrap "ML-180" (model name, manufactured by Maruto Co., Ltd.) and simple drive arm "MLK-250" (model name, manufactured by Maruto Co., Ltd.) Load: 200g / cm 2 Plate rotation speed: 150 rpm Wafer holder rotation speed: 150 rpm Polishing pad: suede type Polishing composition supply rate: 30 mL / min Polishing time: 1hr The relative polishing rate of the silica sol obtained in the examples was calculated using the following formula (6). Relative polishing rate=(Mass difference (g) before and after polishing of silicon chip of Example / polishing time (hours)) / (Mass difference (g) before and after polishing of silicon chip of Comparative Example 1 / polishing time (hours)) (6)

[0072] (Metal impurity content) 2 g of the silica sol obtained in Example 2 was accurately weighed out, sulfuric acid and hydrofluoric acid were added, and the mixture was heated, dissolved, and evaporated. Pure water was added to the remaining sulfuric acid droplets so that the total amount became exactly 10 g to prepare a test solution, and the metal impurity content was measured using a high-frequency inductively coupled plasma mass spectrometer "ELEMENT2" (model name, manufactured by Thermo Fisher Scientific). The metal impurity contents were 0.290 ppm for sodium, 0.020 ppm for potassium, 0.002 ppm for iron, 0.013 ppm for aluminum, 0.024 ppm for calcium, 0.001 ppm for magnesium, 0.026 ppm for zinc, and less than 0.001 ppm for cobalt, chromium, copper, manganese, lead, titanium, and silver.

[0073] [Example 1] Tetramethoxysilane and methanol were mixed at a volume ratio of 3:1 to prepare a raw material solution. A reaction solvent, which was a mixture of methanol, pure water, and ammonia, was charged in advance into a reaction tank equipped with a thermometer, a stirrer, a supply pipe, and a distillation line. The concentration of water in the reaction solvent was 32% by mass, and the concentration of ammonia in the reaction solvent was 2% by mass. While maintaining the temperature of the reaction solvent at 30°C, the reaction solvent and the raw material solution were adjusted to 2.3:1 (volume ratio), and the raw material solution was dropped into the reaction tank at a uniform rate for 180 minutes to obtain a silica sol. The temperature of the obtained silica sol was raised to remove methanol and ammonia while adjusting the liquid volume by adding pure water so that the colloidal silica content was about 20 mass%, and a silica sol with a colloidal silica content of about 20 mass% was obtained. The evaluation results of the obtained silica sol are shown in Table 1.

[0074] [Example 2] A silica sol was obtained by the same operation as in Example 1, except that the water concentration in the reaction solvent was 26 mass%, the ammonia concentration in the reaction solvent was 1.9 mass%, and the reaction solvent and raw material solution ratio was 2.5:1 (volume ratio). The evaluation results of the obtained silica sol are shown in Table 1.

[0075] [Example 3] The same operation as in Example 1 was carried out, except that the water concentration in the reaction solvent was 26 mass%, the ammonia concentration in the reaction solvent was 1.7 mass%, the reaction solvent temperature was kept at 28°C, and the reaction solvent and raw material solution were in a volume ratio of 2.5:1, to obtain a silica sol. The evaluation results of the obtained silica sol are shown in Table 1.

[0076] [Example 4] A silica sol was obtained by the same operation as in Example 1, except that the water concentration in the reaction solvent was 26 mass%, the ammonia concentration in the reaction solvent was 1.7 mass%, and the reaction solvent and raw material solution ratio was 2.5:1 (volume ratio). The evaluation results of the obtained silica sol are shown in Table 1.

[0077] [Example 5] A silica sol was obtained by the same operation as in Example 1, except that the water concentration in the reaction solvent was 32 mass%, the ammonia concentration in the reaction solvent was 1.5 mass%, the reaction solvent temperature was kept at 33°C, and the reaction solvent and raw material solution were in a volume ratio of 2.3:1. The evaluation results of the obtained silica sol are shown in Table 1.

[0078] [Example 6] A silica sol was obtained by the same operation as in Example 1, except that the water concentration in the reaction solvent was 35 mass%, the ammonia concentration in the reaction solvent was 1.9 mass%, and the reaction solvent and raw material solution ratio was 2.4:1 (volume ratio). The evaluation results of the obtained silica sol are shown in Table 1.

[0079] [Example 7] A silica sol was obtained by the same operation as in Example 1, except that the water concentration in the reaction solvent was 26 mass%, the ammonia concentration in the reaction solvent was 1.8 mass%, and the reaction solvent and raw material solution ratio was 2.5:1 (volume ratio). The evaluation results of the obtained silica sol are shown in Table 1.

[0080] [Comparative Example 1] As the silica sol, ultra-high purity colloidal silica "PL-7" (product name, manufactured by Fuso Chemical Co., Ltd.) was used. The evaluation results of the obtained silica sol are shown in Table 1.

[0081] [Table 1]

[0082] As can be seen from Table 1, the silica sols obtained in Examples 1 to 7, which had a high surface silanol group density, were superior in polishing rate compared to the silica sol obtained in Comparative Example 1, which had a low surface silanol group density. [Industrial Applicability]

[0083] The colloidal silica, silica sol, and polishing composition of the present invention can be suitably used for polishing purposes, for example, polishing semiconductor materials such as silicon wafers, polishing electronic materials such as hard disk substrates, polishing (chemical mechanical polishing) in the planarization step in manufacturing integrated circuits, polishing synthetic quartz glass substrates used for photomasks and liquid crystals, polishing magnetic disk substrates, and the like. Because of their excellent affinity for silicon surfaces, they can be particularly suitably used for polishing silicon wafers.

Claims

1. A silica sol for polishing silicon wafers, excluding silicon wafers with a TEOS film, comprising: Colloidal silica and water are included, The metal impurity content is 1 ppm or less, The surface silanol group density of the colloidal silica measured by the Sears method is 5 / nm 2 ∼14 particles / nm2, silica sol.

2. 2. The silica sol according to claim 1, wherein the colloidal silica has an average primary particle diameter of 15 nm to 100 nm as measured by a BET method.

3. 3. The silica sol according to claim 1, wherein the colloidal silica has an average secondary particle diameter of 40 nm to 200 nm as measured by a DLS method.

4. A silica sol described in any one of claims 1 to 3, wherein the cv value of the colloidal silica is 15 to 50.

5. A silica sol described in any one of claims 1 to 4, wherein the content of the colloidal silica is 3 mass% to 50 mass% out of a total amount of the silica sol of 100 mass%.

6. A polishing composition comprising the silica sol according to any one of claims 1 to 5 and a water-soluble polymer.

7. A method for polishing a silicon wafer, comprising polishing a silicon wafer with the polishing composition according to claim 6.

8. A method for producing a silicon wafer, comprising the method for polishing a silicon wafer according to claim 7.

9. A chemical mechanical polishing composition comprising the silica sol according to any one of claims 1 to 5.

10. A method for manufacturing a semiconductor device, comprising the step of performing chemical mechanical polishing using the chemical mechanical polishing composition of claim 9.

Citation Information

Patent Citations

  • Fine-polishing composition for wafer

    JP1990158684A

  • Concentrated composition for fine abrasion of wafer

    JP1992063428A

  • Polishing slurry and polishing method

    JP2006231436A

  • "konpeito" (pointed sugar candy ball)-like composite silica sol

    JP2009078935A

  • Aqueous dispersion for chemical mechanical polishing and method of manufacturing the same, and chemical mechanical polishing method

    JP2009224767A