Synthetic gas production apparatus and method for producing synthetic gas

The synthesis gas production apparatus with a non-noble metal catalyst in a porous zeolite carrier and controlled reducing gas use addresses catalyst deactivation issues, ensuring stable production of carbon monoxide and hydrogen.

JP7553048B2Active Publication Date: 2024-09-18FURUKAWA ELECTRIC CO LTD +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020147387
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-02
Publication Date
2024-09-18
Estimated Expiration
2040-09-02

AI Technical Summary

Technical Problem

Existing catalysts for methane and carbon dioxide dry reforming suffer from catalyst deactivation due to coking and oxidation, leading to reduced activity and stability, especially when using non-noble metal catalysts.

Method used

A synthesis gas production apparatus and method utilizing a catalyst structure with non-noble metal fine particles embedded in a porous zeolite-type compound carrier, where the catalyst is heated with a controlled ratio of reducing gas to raw materials, and a refresh section regenerates catalyst activity by reducing oxidation.

Benefits of technology

The method stabilizes catalyst activity over a long period by suppressing coking and oxidation, enabling efficient production of synthesis gas containing carbon monoxide and hydrogen.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007553048000008
    Figure 0007553048000008
  • Figure 0007553048000007
    Figure 0007553048000007
  • Figure 0007553048000006
    Figure 0007553048000006
Patent Text Reader

Abstract

To provide an apparatus and a method for producing a synthetic gas capable of stably producing a synthetic gas containing CO and H2 by suppressing the deterioration of catalytic activity for a long period of time even when dry reforming is performed on a catalyst structure having a non-noble metal catalyst substance.SOLUTION: An apparatus for producing a synthetic gas comprises: a raw material gas supply part for producing a synthetic gas containing CO and H2 and supplying a raw material gas containing CH4 and CO2; a reducing gas supply part for supplying a reducing gas; and a synthetic gas generation part for generating a synthetic gas from the raw material gas by heating the catalyst structure while supplying the raw material gas and the reducing gas and circulating the raw material gas and the reducing gas in the catalyst structure. The catalyst structure comprises a support having a porous structure composed of a zeolite type compound, and a catalyst substance inherent in the support. The support has passages communicating with each other inside. The catalyst substance is non-noble metal fine particles and exists at least in the passages of the support.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to an apparatus for producing syngas and a method for producing syngas. [Background technology]

[0002] In recent years, dry reforming, a technology that converts methane (CH4) and carbon dioxide (CO2), which are substances that cause global warming, into synthetic gas containing carbon monoxide (CO) and hydrogen (H2), has been attracting attention as a measure against global warming.

[0003] As a catalyst for use in producing such a synthesis gas, for example, Patent Document 1 describes a catalyst that uses an oxygen-deficient perovskite-type composite oxide containing manganese, a specific alkaline earth metal, and the like as a support and nickel as the support metal.

[0004] However, the reaction of converting methane and carbon dioxide into a synthesis gas containing carbon monoxide and hydrogen takes place at high temperatures of 800° C. or higher. In the catalyst described in Patent Document 1, nickel, which is a catalytic substance, is supported on the outer surface of the carrier. At high temperatures, nickel particles tend to aggregate and carbon deposits (coking) on ​​the nickel surface, which tends to reduce catalytic activity.

[0005] As a method for suppressing adhesion between catalyst particles and increasing the specific surface area of ​​the catalyst particles, for example, Patent Document 2 describes a method in which catalyst particles are fixed to the surface of a substrate and then oxidation and reduction treatments are carried out under specified conditions.

[0006] However, even in the catalyst structure having catalyst particles fixed to the surface of a substrate described in Patent Document 2, the catalyst activity decreases when the catalyst structure is placed in a high-temperature reaction field. Also, in order to refresh the catalytic function that has decreased due to the decrease in the specific surface area of ​​the catalyst particles, it is necessary to carry out oxidation treatment and reduction treatment again to increase the specific surface area of ​​the catalyst particles, which is a very complicated process.

[0007] Patent Document 3 describes a catalyst for dry reforming in which nickel is supported on a composite oxide. As in the above, in dry reforming, coking is likely to occur on the catalyst surface, which tends to lead to a decrease in catalytic activity.

[0008] The decrease in catalytic activity in dry reforming is due to the higher carbon content in the raw material in dry reforming compared to steam reforming, which reacts methane with steam. Also, problems occur when the catalyst layer in the reaction tube is blocked by coking. In particular, the nickel-supported catalyst described in the above patent document has high catalytic activity among non-precious metal catalysts, but is more susceptible to coking than precious metal catalysts, making it difficult to maintain catalytic activity.

[0009] In Patent Document 4, the present inventors have disclosed a catalyst structure having excellent catalytic activity by incorporating a metal catalyst substance in a porous structure such as zeolite. Even when used in dry reforming, the catalyst structure described in Patent Document 4 suppresses coking by incorporating the metal catalyst substance in the carrier, thereby preventing the rapid deactivation of the catalyst due to coking as in Patent Document 3. On the other hand, by realizing the maintenance of catalytic activity for a long period of time by suppressing coking, a new catalyst deterioration mode has been observed. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] JP 2013-255911 A [Patent Document 2] JP 2016-2527 A [Patent Document 3] JP 2014-200705 A [Patent Document 4] International Publication No. 2018 / 221697 Summary of the Invention [Problem to be solved by the invention]

[0011] An object of the present disclosure is to provide a synthesis gas production apparatus and a synthesis gas production method that can suppress a decrease in catalytic activity over a long period of time even when dry reforming is performed using a catalyst structure including a non-precious metal catalytic substance, and can stably produce a synthesis gas containing carbon monoxide and hydrogen. [Means for solving the problem]

[0012] [1] A synthesis gas production apparatus for producing a synthesis gas containing carbon monoxide and hydrogen, the synthesis gas production apparatus comprising: a raw material gas supplying unit for supplying a raw material gas containing methane and carbon dioxide; a reducing gas supplying unit for supplying a reducing gas; and a synthesis gas generating unit to which the raw material gas is supplied from the raw material gas supplying unit and the reducing gas is supplied from the reducing gas supplying unit, and which heats the catalyst structure while circulating the raw material gas and the reducing gas through the catalyst structure, thereby producing a synthesis gas containing carbon monoxide and hydrogen from the methane and carbon dioxide contained in the raw material gas. The synthesis gas production apparatus comprises: a carrier having a porous structure composed of a zeolite-type compound; and at least one catalytic substance present in the carrier, the carrier having passages therein that communicate with each other; and the catalytic substance is a non-precious metal fine particle that is present in at least the passages of the carrier. [2] The synthesis gas producing apparatus according to the above [1], wherein a content ratio (B×100 / (A+B)) of the supply amount of the reducing gas (B) supplied to the synthesis gas production unit relative to a total amount (A+B) of the supply amount of the raw material gas (A) and the supply amount of the reducing gas (B) supplied to the synthesis gas production unit is 0.01 vol% or more. [3] The synthesis gas production apparatus according to the above [1] or [2], wherein the heating temperature of the catalyst structure in the synthesis gas production section is 500°C or higher and 1150°C or lower. [4] The synthesis gas production apparatus according to any one of the above [1] to [3], further comprising a refresh unit which refreshes catalytic activity of the catalyst structure, wherein the refresh unit stops the supply of the raw material gas from the raw material gas supply unit to the synthesis gas production unit, and heats the catalyst structure while circulating the reducing gas through the catalyst structure. [5] The synthesis gas production apparatus according to the above [4], wherein the heating temperature of the catalyst structure in the synthesis gas production section is 600°C or higher and 1000°C or lower. [6] The synthesis gas production apparatus according to any one of the above [1] to [5], wherein the metal microparticles contain at least one non-precious metal selected from the group consisting of iron (Fe), cobalt (Co) and nickel (Ni). [7] The synthesis gas production apparatus according to any one of [1] to [6] above, wherein the passage has any one of one-dimensional pores, two-dimensional pores and three-dimensional pores in the skeletal structure of the zeolite-type compound and an expanded diameter portion different from any of the one-dimensional pores, the two-dimensional pores and the three-dimensional pores, and the catalytic substance is present at least in the expanded diameter portion. [8] The synthesis gas production apparatus described in [7] above, wherein the expansion section connects a plurality of holes constituting any one of the one-dimensional holes, the two-dimensional holes, and the three-dimensional holes. [9] The synthesis gas production apparatus according to [7] or [8] above, wherein the average particle size of the metal microparticles is larger than the average inner diameter of the passage and is equal to or smaller than the inner diameter of the expanded portion.

[10] The synthesis gas production apparatus according to any one of the above [1] to [9], further comprising a separation section which separates the synthesis gas, methane and carbon dioxide from the synthesis gas discharged from the synthesis gas production section.

[11] The synthesis gas production apparatus according to

[10] above, further comprising a first supply unit that supplies the methane and carbon dioxide separated in the separation unit to the synthesis gas production unit.

[12] The synthesis gas production apparatus according to any one of the above [1] to

[11] , further comprising a second supply unit that separates hydrogen from the synthesis gas discharged from the synthesis gas production unit and supplies the hydrogen to the synthesis gas production unit.

[13] The synthesis gas production apparatus according to any one of the above [1] to

[12] , further comprising a detection unit for detecting carbon monoxide and hydrogen in the synthesis gas discharged from the synthesis gas production unit.

[14] A method for producing a synthesis gas containing carbon monoxide and hydrogen, comprising the steps of: a step S1 of supplying a raw material gas containing methane and carbon dioxide and a reducing gas to a catalyst structure; and a step S2 of heating the catalyst structure while passing the raw material gas and the reducing gas through the catalyst structure to produce a synthesis gas containing carbon monoxide and hydrogen from the methane and carbon dioxide contained in the raw material gas, wherein the catalyst structure comprises a porous support made of a zeolite-type compound and at least one catalytic substance present in the support, the support having passages therein that communicate with each other, and the catalytic substance is fine metal particles of a non-precious metal that are present in at least the passages of the support. Effect of the Invention

[0013] According to the present disclosure, it is possible to provide a synthesis gas production apparatus and a synthesis gas production method that can suppress a decrease in catalytic activity over a long period of time even when dry reforming is performed using a catalyst structure including a non-precious metal catalytic substance, and can stably produce a synthesis gas containing carbon monoxide and hydrogen. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is a block diagram showing a synthesis gas production apparatus and a synthesis gas production method according to an embodiment. [Diagram 2] FIG. 2 is a perspective view (part of which is shown in cross section) that shows a schematic internal structure of an example of a catalyst structure used in the synthesis gas production apparatus and production method of the embodiment. [Diagram 3] FIG. 3 is a schematic cross-sectional view showing an enlarged portion of a catalyst structure used in the synthesis gas production apparatus and production method of the embodiment. [Figure 4]FIG. 4 is a perspective view that illustrates another example of a catalyst structure used in the synthesis gas production apparatus and production method of the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, the embodiments will be described in detail with reference to the drawings.

[0016] As described above, the present inventors have already disclosed a catalyst structure having excellent catalytic activity by having a metal catalyst substance present in a porous structure such as zeolite in Patent Document 4. Even when used in dry reforming, the catalyst structure described in Patent Document 4 suppresses coking by having the metal catalyst substance present in the carrier, thereby preventing rapid catalyst deactivation due to coking as in Patent Document 3.

[0017] On the other hand, by suppressing coking and realizing long-term catalytic activity maintenance, a new catalyst deterioration mode has been observed. This new deterioration mode gradually reduces the activity of the catalyst, and shows a different tendency from the previously known rapid catalyst deactivation caused by coking. The inventors have found that this different tendency is due to the oxidation of the metal catalyst by water (H2O) molecules generated as a by-product by the reverse shift reaction, which is a side reaction during dry reforming. Based on this knowledge, the inventors have completed the present disclosure.

[0018] A synthesis gas production apparatus according to an embodiment is an apparatus for producing a synthesis gas containing carbon monoxide and hydrogen, and includes a raw material gas supplying unit which supplies a raw material gas containing methane and carbon dioxide, a reducing gas supplying unit which supplies a reducing gas, and a synthesis gas generating unit which receives the raw material gas from the raw material gas supplying unit and the reducing gas from the reducing gas supplying unit, heats the catalyst structure while circulating the raw material gas and the reducing gas through the catalyst structure, and generates a synthesis gas containing carbon monoxide and hydrogen from the methane and carbon dioxide contained in the raw material gas, and the catalyst structure includes a porous support made of a zeolite-type compound and at least one catalytic substance present in the support, the support having passages therein which communicate with each other, and the catalytic substance is metal fine particles of a non-precious metal and is present in at least the passages of the support.

[0019] A synthesis gas production method according to an embodiment is a synthesis gas production method for producing a synthesis gas containing carbon monoxide and hydrogen, and includes the steps of: step S1 of supplying a raw material gas containing methane and carbon dioxide and a reducing gas to a catalyst structure; and step S2 of heating the catalyst structure while passing the raw material gas and the reducing gas through the catalyst structure to produce a synthesis gas containing carbon monoxide and hydrogen from the methane and carbon dioxide contained in the raw material gas. The catalyst structure includes a carrier having a porous structure composed of a zeolite-type compound and at least one catalytic substance present in the carrier, the carrier having passages therein that communicate with each other, and the catalytic substance is metal fine particles of a non-precious metal that are present in at least the passages of the carrier.

[0020] [Configuration of synthetic gas production equipment] Fig. 1 is a block diagram showing a synthesis gas production apparatus and a synthesis gas production method according to an embodiment. Fig. 2 is a perspective view (partially shown in cross section) showing a schematic internal structure of an example of a catalyst structure used in the synthesis gas production apparatus and the synthesis gas production method. Fig. 3 is a schematic cross-sectional view showing an enlarged portion of the catalyst structure used in the synthesis gas production apparatus and the synthesis gas production method.

[0021] The synthesis gas production apparatus 1 (hereinafter also simply referred to as the production apparatus) shown in FIG. 1 is an apparatus for producing synthesis gas containing carbon monoxide and hydrogen, and includes a raw material gas supply unit 2, a reducing gas supply unit 3, and a synthesis gas production unit 4.

[0022] The raw material gas supplying unit 2 includes a methane supplying unit 2a and a carbon dioxide supplying unit 2b, and supplies raw material gas containing methane and carbon dioxide to the synthesis gas generating unit 4. The methane supplying unit 2a is composed of, for example, a methane gas cylinder or a methane gas generator, and can control the amount of methane gas supplied to the synthesis gas generating unit 4. The carbon dioxide supplying unit 2b is composed of, for example, a carbon dioxide gas cylinder or a carbon dioxide gas generator, and can control the amount of carbon dioxide supplied to the synthesis gas generating unit 4.

[0023] The reducing gas supply unit 3 supplies the reducing gas to the synthesis gas generation unit 4. The reducing gas supply unit 3 is composed of, for example, a reducing gas cylinder or a reducing gas generator, and can control the amount of reducing gas supplied to the synthesis gas generation unit 4. The reducing gas can suppress the oxidation of the catalyst structure 40 accommodated in the catalyst structure accommodation unit 4a of the synthesis gas generation unit 4 to suppress the decrease in the catalytic activity of the catalyst structure 40, and can reduce the oxidized catalyst structure 40 to refresh the catalytic activity of the catalyst structure 40. When the catalytic activity of the catalyst structure 40 is refreshed, the catalytic activity of the catalyst structure 40 that is equal to or higher than a predetermined activity but lower than the maximum activity can be restored, and the catalytic activity of the catalyst structure 40 that has decreased to or below a predetermined activity can be regenerated. The reducing gas only needs to contain hydrogen, and hydrogen may be supplied in a state diluted with an inert gas (nitrogen or argon) as a supply form. Hydrogen may also be introduced so that only hydrogen is desorbed from the predetermined raw material gas during the dry reforming process.

[0024] The synthesis gas generation unit 4 includes a catalyst structure housing unit 4a that houses the catalyst structure 40 and a heating unit (not shown) such as a heating furnace, and the catalyst structure 40 in the catalyst structure housing unit 4a is heated to a predetermined temperature by the heating unit. A raw material gas containing methane and carbon dioxide is supplied to the synthesis gas generation unit 4 from a raw material gas supply unit 2, and a reducing gas is supplied from a reducing gas supply unit 3. The synthesis gas generation unit 4 heats the catalyst structure 40 while circulating the raw material gas and reducing gas through the catalyst structure 40 in the catalyst structure housing unit 4a, and generates a synthesis gas containing carbon monoxide and hydrogen from the methane and carbon dioxide contained in the raw material gas.

[0025] Specifically, a raw material gas containing methane and carbon dioxide is supplied from the raw material gas supply unit 2 to the synthesis gas production unit 4, and at the same time, a catalyst structure 40 provided inside the synthesis gas production unit 4 is heated, whereby the supplied methane and carbon dioxide react with each other through the catalyst structure 40, thereby producing a synthesis gas containing carbon monoxide and hydrogen. In the synthesis gas production unit 4, such a synthesis gas production reaction, i.e., a dry reforming reaction, takes place.

[0026] The heating temperature of the catalyst structure 40 in the synthesis gas generation section 4 is preferably within a temperature range of 500° C. to 1150° C. Since the reforming efficiency of the raw material gas to synthesis gas and the reforming characteristics of the catalyst structure 40 may be reduced by heat, the heating temperature of the catalyst structure 40 in the synthesis gas generation section 4 is more preferably 500° C. to 1000° C., and further preferably 500° C. to 900° C.

[0027] Furthermore, during the dry reforming, in addition to the supply of the raw material gas to the synthesis gas generating section 4, the reducing gas is supplied from the reducing gas supplying section 3 to the synthesis gas generating section 4. The reducing gas is supplied to the heated catalyst structure 40 in addition to the raw material gas. Regarding the catalytic activity of the catalyst material 45, which is reduced by the oxidation of the catalyst material 45 by water molecules as a by-product generated in the reverse shift reaction during the dry reforming, the reducing gas is supplied to the catalyst structure 40 during the dry reforming, thereby suppressing the oxidation of the catalyst material 45 present in the support 41 of the catalyst structure 40 in the reduction treatment of the reducing gas to the catalyst structure 40, and the decrease in the catalytic activity of the catalyst material 45 due to the dry reforming can be suppressed. In this way, the synthesis gas production apparatus 1 can suppress the decrease in the catalytic activity of the catalyst structure 40 due to the dry reforming for a long period of time by supplying the raw material gas and the reducing gas to the synthesis gas generating section 4, and can stably produce synthesis gas for a long period of time.

[0028] The catalyst structure accommodation unit 4a may be disposed in the synthesis gas production unit 4 in any manner as long as the heated catalyst structure 40 accommodated in the catalyst structure accommodation unit 4a can come into contact with the raw material gas and reducing gas flowing through the catalyst structure accommodation unit 4a. For example, as shown in Fig. 1, the catalyst structure accommodation unit 4a is disposed so as to connect a connection between the synthesis gas production unit 4 and a pipe for supplying the raw material gas and reducing gas, and the synthesis gas production unit 4, with a connection between the synthesis gas production unit 4 and a pipe for discharging the produced gas.

[0029] The synthesis gas discharged from the synthesis gas production unit 4 contains synthesis gas containing at least carbon monoxide and hydrogen. In this manner, the production apparatus 1 can produce synthesis gas by reacting the raw material gas.

[0030] The content of synthesis gas in the generated gas can be appropriately adjusted by adjusting the dry reforming conditions such as the heating temperature of the catalyst structure 40 and the supply amount of the raw material gas.

[0031] As will be described in detail below, in the catalyst structure 40 used in the production apparatus 1, the catalyst material 45 is present inside the support 41. On the other hand, in the past, the catalyst material was supported on the outer surface of a substrate or a support. It is believed that such differences in the supported state of the catalyst material reduce the catalytic activity of the catalyst material through different mechanisms.

[0032] Conventionally, in order to suppress the decrease in catalytic activity of the catalytic substance, attention has been focused on the coking that occurs on the surface of the catalytic substance, and the occurrence of coking has been suppressed and the generated coking has been decomposed. On the other hand, in this embodiment, attention is focused on the oxidation of the catalytic substance, which is a newly discovered deterioration mode of the catalytic substance, as a result of realizing the maintenance of the catalytic activity of the catalytic substance over a long period of time by suppressing coking, and the oxidation of the catalytic substance is suppressed and the oxidized catalytic substance is reduced.

[0033] In this manner, in the synthesis gas production apparatus 1 of the embodiment, a reducing gas is supplied to the catalyst structure 40 containing the catalyst material 45 together with the raw material gas. By heating the catalyst structure 40 while circulating the raw material gas and the reducing gas through the catalyst structure 40, the catalyst structure 40 reacts the carbon monoxide and hydrogen contained in the raw material gas to produce a raw material gas containing methane and carbon dioxide. Furthermore, since the reducing gas is supplied to the catalyst structure 40 during the production of the synthesis gas, the reduction process of the reducing gas on the catalyst structure 40 can suppress the oxidation of the catalyst structure 40 accompanying the production of the synthesis gas, and suppress the decrease in the catalytic activity of the catalyst structure 40. As a result, the production apparatus 1 can stably produce the synthesis gas for a long period of time.

[0034] Furthermore, the content ratio (B×100 / (A+B)) of the supply amount (B) of the reducing gas supplied to the synthesis gas generating unit 4 relative to the total amount (A+B) of the supply amount (A) of the raw material gas and the supply amount (B) of the reducing gas supplied to the synthesis gas generating unit 4 is preferably 0.01 vol% or more, more preferably 0.25 vol% or more, and further preferably 4.50 vol% or more. When the content ratio (B×100 / (A+B)) of the reducing gas supplied to the synthesis gas generating unit 4 is 0.01 vol% or more, the oxidation of the catalyst structure 40 accompanying the production of synthesis gas can be efficiently suppressed by the reduction treatment of the reducing gas, and therefore the decrease in the catalytic activity of the catalyst structure 40 can be further suppressed.

[0035] Moreover, the manufacturing apparatus 1 preferably further includes a refresh section 5 that selectively refreshes the catalytic activity of the catalyst structure 40. The refresh section 5 stops the supply of raw material gas from the raw material gas supply section 2 to the synthesis gas production section 4, and heats the catalyst structure 40 while circulating a reducing gas through the catalyst structure 40.

[0036] The refresh unit 5 stops the supply of raw material gas from the raw material gas supply unit 2 to the synthesis gas generation unit 4, and stops the dry reforming in the synthesis gas generation unit 4. The refresh unit 5 also supplies a reducing gas to the synthesis gas generation unit 4 while stopping the supply of raw material gas to the synthesis gas generation unit 4. That is, the refresh unit 5 selectively performs a reduction process of the reducing gas on the catalyst structure 40 in the synthesis gas generation unit 4 while stopping the dry reforming in the synthesis gas generation unit 4.

[0037] In this way, the refresh unit 5 selectively circulates only the reducing gas out of the raw material gas and the reducing gas through the catalyst structure 40. Therefore, the dry reforming is stopped to avoid a decrease in the catalytic activity of the catalytic material 45 due to the dry reforming, and the catalytic activity of the catalytic material 45, the catalytic activity of which has been decreased by oxidation, is actively refreshed by reducing the catalytic activity of the catalytic material 45 with the reducing gas.

[0038] When the synthesis gas production efficiency by the catalyst structure 40 falls below a desired value, or when it is desired to actively increase the reduced synthesis gas production efficiency, the refresh unit 5 performs a reduction process on the oxidized catalyst structure 40. For example, when the methane conversion rate calculated from the amount of methane in the raw material gas and the amount of methane in the generated gas (amount of methane in generated gas×100 / amount of methane in raw material gas) falls below a predetermined value, the refresh unit 5 performs a reduction process on the catalyst structure 40.

[0039] In addition, when the raw material gas is not supplied to the synthesis gas generating section 4 by the refresh section 5 and the reducing gas is supplied, the lower limit of the heating temperature of the catalyst structure 40 in the synthesis gas generating section 4 is preferably 600°C or more, more preferably 700°C or more, and even more preferably 800°C or more, and the upper limit is preferably 1000°C or less, and more preferably 900°C or less. When the heating temperature of the catalyst structure 40 in which the raw material gas is not circulated but the reducing gas is circulated is 600°C or more, the oxidized catalyst structure 40 can be efficiently reduced, and the catalytic activity of the catalyst structure 40 can be further refreshed. When the heating temperature of the catalyst structure 40 is 1000°C or less, synthesis gas can be efficiently produced.

[0040] The production apparatus 1 may further include a separation section 6 that separates the synthesis gas, methane, and carbon dioxide from the synthesis gas discharged from the synthesis gas generation section 4. The separation section 6 is, for example, a cryogenic separation type separation section, and separates the discharged synthesis gas into a raw material gas containing unreacted methane and carbon dioxide by dry reforming in the synthesis gas generation section 4, and a synthesis gas containing carbon monoxide and hydrogen. By separating the unreacted raw material gas contained in the discharged synthesis gas, it is possible to obtain a high percentage of synthesis gas.

[0041] The production apparatus 1 may further include a first supply unit 7 that supplies the methane and carbon dioxide separated in the separation unit 6 to the synthesis gas production unit 4. The first supply unit 7 can control the supply amount of the raw material gas containing unreacted methane and carbon dioxide to be supplied to the synthesis gas production unit 4. The raw material gas supplied from the first supply unit 7 to the synthesis gas production unit 4 can be reused for dry reforming, so that the amount of raw material gas used can be reduced.

[0042] Moreover, the production apparatus 1 may further include a second supply unit 8 which separates hydrogen from the synthesis gas discharged from the synthesis gas production unit 4 and supplies the hydrogen to the synthesis gas production unit 4. The second supply unit 8 separates at least a portion of the hydrogen produced by dry reforming in the synthesis gas production unit 4 from the synthesis gas, and supplies the hydrogen to the synthesis gas production unit 4. The second supply unit 8 can control the amount of hydrogen supplied to the synthesis gas production unit 4. The hydrogen supplied from the second supply unit 8 to the synthesis gas production unit 4 can be used as a reducing gas in the reduction treatment of the catalyst structure 40, and therefore the amount of reducing gas used can be reduced.

[0043] The manufacturing apparatus 1 may further include a detection unit 9 that detects carbon monoxide and hydrogen in the generated gas discharged from the synthesis gas generation unit 4. When the detection unit 9 can detect carbon monoxide and hydrogen in the generated gas, it can be determined that the manufacturing apparatus 1 is operating normally. On the other hand, when the detection unit 9 cannot detect carbon monoxide and hydrogen in the generated gas, it can be determined that the manufacturing apparatus 1 is abnormal. This makes it possible to shut down, inspect, and repair parts related to rapid dry reforming.

[0044] Although FIG. 1 shows an example in which methane and carbon dioxide are individually supplied to the synthesis gas generation unit 4 by the methane supply unit 2a and the carbon dioxide supply unit 2b, a mixed gas of methane and carbon dioxide may be supplied to the synthesis gas generation unit 4.

[0045] In addition, the concentration of methane supplied from the methane supply unit 2a and the concentration of carbon dioxide supplied from the carbon dioxide supply unit 2b are not particularly limited. For example, these concentrations may be 100%, or may be mixed with an inert gas such as nitrogen or argon to adjust to a predetermined value. When an inert gas is used, the inert gas is supplied to the manufacturing apparatus 1 from an inert gas supply unit (not shown).

[0046] 1 illustrates an example in which the catalyst structure 40 is accommodated in the catalyst structure accommodation section 4a, but the arrangement is not particularly limited as long as the catalyst structure 40 in a heated state can contact the raw material gas and the reducing gas. For example, the catalyst structure 40 may be accommodated in a part or the whole of the synthesis gas production section 4. Dry reforming using the catalyst structure 40 can be performed in, for example, a fixed bed, a supercritical fixed bed, a slurry bed, a fluidized bed, or the like. Among these, a fixed bed, a supercritical fixed bed, and a slurry bed are preferable.

[0047] Furthermore, with regard to the arrangement of the separation section 6 and the second supply section 8, FIG. 1 shows an example in which the generated gas discharged from the separation section 6 is supplied to the second supply section 8, but the arrangement order of the separation section 6 and the second supply section 8 may be changed so that the generated gas discharged from the second supply section 8 is supplied to the separation section 6.

[0048] [Method of producing synthetic gas] The synthesis gas production method of the embodiment (hereinafter also simply referred to as the production method) is a method for producing synthesis gas containing carbon monoxide and hydrogen, and is carried out using a production apparatus 1 shown in FIG. 1, for example.

[0049] The method for producing a synthesis gas according to the embodiment includes a step S1 (a first supply step S1) and a step S2 (a production step S2).

[0050] In the first supply step S1, a raw material gas containing methane and carbon dioxide and a reducing gas are supplied to the catalyst structure. In the production apparatus 1 shown in Fig. 1, the raw material gas is supplied from the raw material gas supply unit 2 to the catalyst structure 40 in the catalyst structure housing unit 4a provided inside the synthesis gas generation unit 4, and the reducing gas is supplied from the reducing gas supply unit 3 to the catalyst structure 40.

[0051] In the generating step S2, the catalyst structure is heated while the raw material gas and reducing gas supplied in the first supply step S1 are circulated through the catalyst structure, and a synthesis gas containing carbon monoxide and hydrogen is generated from the methane and carbon dioxide contained in the raw material gas. In the manufacturing apparatus 1, the catalyst structure 40 heated to a predetermined temperature in the synthesis gas generating section 4 generates a synthesis gas containing carbon monoxide and hydrogen from the methane and carbon dioxide in the raw material gas. Furthermore, in the manufacturing apparatus 1, by supplying a reducing gas from the reducing gas supplying section 3 to the catalyst structure 40 during dry reforming, a decrease in the catalytic activity of the catalyst structure 40 due to water molecules generated during dry reforming can be suppressed for a long period of time.

[0052] The synthesis gas production method may further include a step S11 (refresh step S11) of stopping the supply of the raw material gas containing methane and carbon dioxide to the catalyst structure and supplying a reducing gas to the catalyst structure. In the production apparatus 1, the refresh unit 5 stops the supply of the raw material gas from the raw material gas supply unit 2 to the synthesis gas production unit 4. Then, the refresh unit 5 continues the supply of the reducing gas from the reducing gas supply unit 3 to the synthesis gas production unit 4 without stopping it. The catalyst structure 40 is heated while the reducing gas is circulated through the catalyst structure 40. In this way, the dry reforming is selectively stopped, and the catalyst structure 40, whose catalytic activity has been reduced by oxidation, is reduced with the reducing gas to refresh the catalytic activity of the catalyst structure 40.

[0053] The synthesis gas production method may further include a step S12 (separation step S12) of separating the synthesis gas from methane and carbon dioxide from the synthesis gas generated in the generation step S2. In the production apparatus 1, the separation section 6 separates the synthesis gas generated in the generation step S2 into a raw material gas containing unreacted methane and carbon dioxide, and a synthesis gas containing carbon monoxide and oxygen. Therefore, the synthesis gas can be obtained at a high rate.

[0054] The synthesis gas production method may further include a step S13 (second supply step S13) of supplying the methane and carbon dioxide separated in the separation step S12 to the production step S2. In the production apparatus 1, the first supply unit 7 supplies unreacted methane and carbon dioxide to the production step S2 carried out in the synthesis gas production unit 4. Therefore, the methane and carbon dioxide are reused in the dry reforming carried out in the production step S2, and the amount of raw material gas used can be reduced.

[0055] The synthesis gas production method may further include a step S14 (third supply step S14) of separating hydrogen from the synthesis gas generated in the production step S2 and supplying it to the production step S2. In the production apparatus 1, the second supply unit 8 separates at least a portion of hydrogen from the synthesis gas generated in the production step S2, and supplies the separated hydrogen to the production step S2. In the production step S2 and the refreshing step S11, hydrogen is reused as a reducing gas in the reduction treatment of the catalyst structure, so that the amount of reducing gas used can be reduced.

[0056] The method for producing a synthesis gas may further include a step S15 of detecting carbon monoxide and hydrogen in the synthesis gas produced in the production step S2 (detection step S15). In the production apparatus 1, the detection unit 9 detects the carbon monoxide and hydrogen produced in the production step S2.

[0057] [Catalyst structure] In the synthesis gas production apparatus and production method of the embodiment, the catalyst structure 40 accommodated in the synthesis gas generation unit 4 includes a carrier 41 having a porous structure composed of a zeolite-type compound, and at least one catalyst substance 45 present in the carrier 41, as shown in Figures 2 and 3.

[0058] In the catalyst structure 40, a plurality of catalyst substances 45, 45, ... are enclosed within the porous structure of the support 41. The catalyst substance 45 is a substance having catalytic ability (catalytic activity), and specifically is metal fine particles of a non-precious metal.

[0059] The support 41 has a porous structure, and preferably has a plurality of holes 42a, 42a, ... formed therein to form passages 42 that communicate with each other. The passages 42 inside the support 41 also communicate with the outside of the support 41. The catalytic material 45 is present in at least the passages 42 of the support 41, and is preferably held in at least the passages 42 of the support 41.

[0060] With this configuration, the movement of the catalytic material 45 within the carrier 41 is restricted, and the agglomeration of the catalytic materials 45, 45 is effectively prevented. As a result, the reduction in the effective surface area of ​​the catalytic material 45 can be effectively suppressed, and the catalytic activity of the catalytic material 45 is maintained for a long period of time. That is, according to the catalytic structure 40, the decrease in catalytic activity due to the agglomeration of the catalytic material 45 can be suppressed, and the life of the catalytic structure 40 can be extended. Furthermore, the extended life of the catalytic structure 40 can reduce the frequency of replacement of the catalytic structure 40, and the amount of waste of used catalytic structure 40 can be significantly reduced, thereby saving resources.

[0061] In addition, it is preferable that the passage 42 has any one-dimensional pore, two-dimensional pore, or three-dimensional pore defined by the skeletal structure of the zeolite-type compound, and an expanded diameter portion 43 different from any of the one-dimensional pore, the two-dimensional pore, or the three-dimensional pore. In this case, it is preferable that the catalyst material 45 is present at least in the expanded diameter portion 43, and it is more preferable that the catalyst material 45 is encapsulated in at least the expanded diameter portion 43.

[0062] This further restricts the movement of the catalytic substance 45 within the carrier 41, and makes it possible to more effectively prevent the catalytic substance 45 from being separated or the catalytic substances 45, 45 from agglomerating together. The term "enclosed" refers to a state in which the catalytic substance 45 is enclosed within the carrier 41, and means that the catalytic substance 45 is not in contact with the outside of the zeolite except through the regular paths formed by the synthesis of the zeolite. In this case, the catalytic substance 45 and the carrier 41 do not necessarily need to be in direct contact with each other, and the catalytic substance 45 may be indirectly held by the carrier 41 with another substance (e.g., a surfactant) intervening between the catalytic substance 45 and the carrier 41.

[0063] The one-dimensional pores referred to here refer to tunnel- or cage-type pores forming a one-dimensional channel, or multiple tunnel- or cage-type pores (multiple one-dimensional channels) forming multiple one-dimensional channels. In addition, the two-dimensional pores refer to two-dimensional channels in which multiple one-dimensional channels are connected two-dimensionally, and the three-dimensional pores refer to three-dimensional channels in which multiple one-dimensional channels are connected three-dimensionally. Therefore, the expanded diameter section does not include those in which the pores expand as a regular structure of zeolite, such as a supercage.

[0064] 3 shows an example in which catalytic material 45 is enclosed in enlarged diameter portion 43, but the present invention is not limited to this configuration, and catalytic material 45 may be present in passage 42 with a part of it protruding outside enlarged diameter portion 43. In addition, catalytic material 45 may be partially embedded in a portion of passage 42 other than enlarged diameter portion 43 (for example, an inner wall portion of passage 42) or may be held by adhesion or the like.

[0065] In addition, it is preferable that the expanded diameter portion 43 communicates with the plurality of holes 42a, 42a constituting any one of the one-dimensional holes, the two-dimensional holes, and the three-dimensional holes, thereby providing a passage having a different configuration from the one-dimensional holes, the two-dimensional holes, or the three-dimensional holes inside the carrier 41, thereby enabling the catalyst material 45 to exhibit its function more effectively.

[0066] Moreover, the passage 42 is formed three-dimensionally inside the carrier 41, including a branching portion or a junction portion, and the expanded diameter portion 43 is preferably provided at the branching portion or the junction portion of the passage 42.

[0067] The average inner diameter D of the passages 42 formed in the carrier 41 F is calculated from the average value of the minor axis and major axis of the pores 42a constituting any one of the one-dimensional pores, the two-dimensional pores, and the three-dimensional pores, and is, for example, preferably 0.1 nm or more and 1.5 nm or less, and more preferably 0.5 nm or more and 0.8 nm or less. E The inner diameter D of the expanded diameter portion 43 is, for example, preferably 0.5 nm or more and 50 nm or less, more preferably 1.1 nm or more and 40 nm or less, and further preferably 1.1 nm or more and 3.3 nm or less. E is, for example, the pore size of the precursor material (A) described later and the average particle size D of the catalytic substance 45 to be enclosed. C The inner diameter D of the expanded portion 43 depends on E is a size capable of encapsulating the catalyst material 45 .

[0068] The carrier 41 is composed of a zeolite type compound. Examples of the zeolite type compound include silicate compounds such as zeolite (aluminosilicate), cation-exchanged zeolite, and silicalite, zeolite-related compounds such as aluminoborates, aluminoarsenates, and germanates, and phosphate-based zeolite-like substances such as molybdenum phosphate. Among them, the zeolite type compound is preferably a silicate compound.

[0069] The framework structure of the zeolite compound is selected from MTW type, MFI type (ZSM-5), FER type (ferrierite), LTA type (A type), MOR type (mordenite), LTL type (L type), etc., preferably MFI type, and more preferably Silicalite-1. In the zeolite compound, a plurality of pores having a pore size according to each framework structure are formed, for example, the maximum pore size of the MFI type is 0.636 nm (6.36 Å) and the average pore size is 0.560 nm (5.60 Å).

[0070] The catalytic material 45 will be described in detail below. The catalytic material 45 is a metal fine particle of a non-precious metal. The metal fine particles may be present in the passage 42 in the form of primary particles, or may be present in the passage 42 in the form of secondary particles formed by agglomeration of the primary particles. In either case, the average particle diameter D C is preferably the average inner diameter D of the passage 42 F and the inner diameter D of the expanded diameter portion 43 is larger than E The following is true: F <D C ≦D E ). In the passages 42, the catalyst material 45 is preferably enclosed in the enlarged diameter portions 43, and the movement of the catalyst material 45 in the carrier 41 is restricted. Therefore, even if the catalyst material 45 is subjected to an external force from the fluid, the movement of the catalyst material 45 in the carrier 41 is restricted, and the catalyst materials 45, 45, ... enclosed in the enlarged diameter portions 43, 43, ... dispersedly arranged in the passages 42 of the carrier 41 can be effectively prevented from contacting each other.

[0071] Average particle size of metal particles D C The average particle diameter D of the metal particles is preferably 1 nm or more and 13.0 nm or less. C When the average particle diameter D is within the range, the catalytic activity is sufficiently increased. C As the average particle diameter D of the metal particles decreases, the catalytic activity improves. C is preferably 9.0 nm or less, and more preferably 4.5 nm or less. In addition, when the metal fine particles are fine particles containing at least one non-precious metal selected from the group consisting of iron (Fe), cobalt (Co) and nickel (Ni) as described later, the average particle diameter D of the metal fine particles is C When the amount of the catalyst falls within the range, both the catalytic activity and the coking resistance are sufficiently improved.

[0072] The metal element (M) of the metal fine particles is preferably contained in the catalyst structure 40 at 0.5 mass% or more and 7.6 mass% or less, more preferably at 0.5 mass% or more and 6.9 mass% or less, even more preferably at 0.5 mass% or more and 2.5 mass% or less, and most preferably at 0.5 mass% or more and 1.5 mass% or less. The metal element (M) is a non-precious metal element. For example, when the metal element (M) is Ni, the content (mass%) of the Ni element is expressed by {(mass of Ni element) / (mass of all elements of the catalyst structure 40)}×100.

[0073] Metal microparticles may be composed of a non-oxidized metal, and may be composed of, for example, a single metal or a mixture of two or more metals. In this specification, the term "metal" (as a material) constituting the metal microparticles means a simple metal containing one metal element (M) and a metal alloy containing two or more metal elements (M), and is a general term for metals containing one or more metal elements. In addition, when a metal oxide having the same metal element as the metal microparticles is reduced in the usage environment and results in the composition of the metal microparticles, the metal oxide can be considered to be substantially the metal microparticles.

[0074] From the viewpoint of catalytic activity, such non-precious metal fine particles are preferably composed of at least one non-precious metal selected from the group consisting of iron (Fe), cobalt (Co) and nickel (Ni). In particular, from the viewpoint of both cost and performance, it is particularly preferable that the metal fine particles are composed of nickel (Ni).

[0075] Furthermore, the ratio of silicon (Si) constituting the carrier 41 to the metal element (M) constituting the metal microparticles (atomic ratio Si / M) is preferably 10 or more and 1000 or less, and more preferably 50 or more and 200 or less. If the ratio is more than 1000, the catalytic activity is low and the action as a catalytic substance may not be sufficiently obtained. On the other hand, if the ratio is less than 10, the proportion of the metal microparticles becomes too large, and the mechanical strength of the carrier 41 tends to decrease. Note that the metal microparticles referred to here refer to microparticles present or held inside the carrier 41, and do not include metal microparticles supported on or attached to the outer surface 41a of the carrier 41.

[0076] [Functions of the catalyst structure] As described above, the catalyst structure 40 includes a carrier 41 having a porous structure and at least one catalyst material 45 present in the carrier 41. The catalyst structure 40 exerts catalytic activity according to the function of the catalyst material 45 by contacting the catalyst material 45 present in the carrier 41 with a fluid. Specifically, the fluid that has come into contact with the outer surface 41a of the catalyst structure 40 flows into the inside of the carrier 41 through holes 42a formed in the outer surface 41a by diffusion, is guided into the passage 42, moves through the passage 42, and exits the catalyst structure 40 through other holes 42a. In the path along which the fluid moves through the passage 42, the fluid comes into contact with the catalyst material 45 present in the passage 42, causing a catalytic reaction according to the catalyst material 45. In addition, the catalyst structure 40 has a molecular sieve function because the carrier 41 has a porous structure.

[0077] First, the molecular sieving ability of the catalyst structure 40 will be described using an example in which the fluid is a methane-containing gas and carbon dioxide. The methane-containing gas refers to a mixed gas containing methane and a gas other than methane. The catalyst structure 40 may be contacted with the methane-containing gas and carbon dioxide in sequence or simultaneously.

[0078] Compounds (e.g., methane, carbon dioxide) composed of molecules having a size equal to or smaller than the pore size of the hole 42a, in other words, equal to or smaller than the inner diameter of the passage 42, can diffuse into the carrier 41. On the other hand, gas components composed of molecules having a size larger than the pore size of the hole 42a cannot diffuse into the carrier 41. In this way, when the fluid contains multiple types of compounds, the reaction of the substances that cannot diffuse into the carrier 41 is restricted, and the substances that can diffuse into the carrier 41 can react. In this embodiment, the reaction of methane and carbon dioxide and the reaction of the reducing gas and the catalytic substance 45 proceed.

[0079] Of the substances produced in the carrier 41 by the reaction, only those having a size equal to or smaller than the diameter of the holes 42a can escape to the outside of the carrier 41 through the holes 42a and are obtained as reaction products. On the other hand, substances that cannot escape to the outside of the carrier 41 through the holes 42a can escape to the outside of the carrier 41 if they are converted into substances having a size that allows them to escape to the outside of the carrier 41. In this way, by using the catalyst structure 40, a specific reaction product can be selectively obtained. In this embodiment, methane and carbon dioxide react with each other to obtain a synthesis gas containing carbon monoxide and hydrogen as a reaction product.

[0080] In the catalyst structure 40, the catalyst material 45 is enclosed in the enlarged diameter portion 43 of the passage 42. The average particle diameter D of the catalyst material 45 (metallic fine particles) C is the average inner diameter D of the passage 42 F The inner diameter D of the expanded portion 43 is larger than E If it is smaller than (D F1 <D C1 <D E1 ), small passages 44 are formed between the enlarged diameter portion 43 and the catalyst material 45. The fluid that has flowed into the small passages 44 by diffusion comes into efficient contact with the catalyst material 45. Since each catalyst material 45 is enclosed in the enlarged diameter portion 43, movement within the carrier 41 is restricted. This prevents the catalyst materials 45 from coagulating within the carrier 41. Furthermore, a large contact area between the catalyst material 45 and the fluid can be stably maintained.

[0081] In this embodiment, a synthesis gas containing carbon monoxide and hydrogen can be produced from methane and carbon dioxide as raw materials by using the catalyst structure 40. Even if this catalytic reaction is carried out at a high temperature, preferably 500° C. or higher and 1150° C. or lower, for example, 800° C. or higher, the catalyst material 45 is present inside the support 41 and is therefore unlikely to be affected by heating.

[0082] During the dry reforming, the catalytic material 45 present in the carrier 41 is oxidized, and the catalytic activity of the catalytic material 45 gradually decreases. When the reducing gas that has flowed into the carrier 41 from the holes 42a by diffusion comes into contact with the oxidized catalytic material 45, the oxidized catalytic material 45 is reduced, refreshing the catalytic activity of the catalytic material 45. As a result, synthesis gas can be stably produced for a long period of time.

[0083] [Method of manufacturing catalyst structure] An example of a method for producing the catalyst structure will be described below.

[0084] (Step S1-1: Preparation process) First, a precursor material (A) for obtaining a porous support composed of a zeolite-type compound is prepared. The precursor material (A) is preferably an ordered mesoporous substance, and can be appropriately selected depending on the type (composition) of the zeolite-type compound constituting the support of the catalyst structure.

[0085] Here, when the zeolite-type compound constituting the carrier of the catalyst structure is a silicate compound, the ordered mesoporous material is preferably a compound consisting of a Si-O skeleton in which pores having a pore diameter of 1 nm or more and 50 nm or less are uniform in size and regularly developed in one, two or three dimensions. Such ordered mesoporous materials can be obtained as various synthetic products depending on the synthesis conditions. Specific examples of synthetic products include SBA-1, SBA-15, SBA-16, KIT-6, FSM-16, MCM-41, etc., and among them, MCM-41 is preferred. The pore diameter of SBA-1 is 10 nm or more and 30 nm or less, the pore diameter of SBA-15 is 6 nm or more and 10 nm or less, the pore diameter of SBA-16 is 6 nm, the pore diameter of KIT-6 is 9 nm, the pore diameter of FSM-16 is 3 nm or more and 5 nm or less, and the pore diameter of MCM-41 is 1 nm or more and 10 nm or less. Examples of such regular mesoporous substances include mesoporous silica, mesoporous aluminosilicate, and mesoporous metallosilicate.

[0086] The precursor material (A) may be either a commercially available product or a synthetic product. When synthesizing the precursor material (A), a known method for synthesizing an ordered mesoporous material can be adopted. For example, a mixed solution containing raw materials containing the constituent elements of the precursor material (A) and a template agent for defining the structure of the precursor material (A) is prepared, and the pH is adjusted as necessary, followed by hydrothermal treatment (hydrothermal synthesis). Thereafter, the precipitate (product) obtained by the hydrothermal treatment is collected (for example, filtered), washed and dried as necessary, and further calcined to obtain the precursor material (A), which is a powdered ordered mesoporous material. Here, as the solvent for the mixed solution, for example, water, an organic solvent such as alcohol, or a mixed solvent thereof can be used. In addition, the raw material is selected according to the type of carrier, and examples thereof include silica agents such as tetraethoxysilane (TEOS), fumed silica, and quartz sand. In addition, as the template agent, various surfactants, block copolymers, etc. can be used, and it is preferable to select according to the type of the synthetic ordered mesoporous material. For example, when preparing MCM-41, a surfactant such as hexadecyltrimethylammonium bromide is suitable. The hydrothermal treatment can be carried out, for example, in a closed vessel under the conditions of 80°C to 800°C, 5 hours to 240 hours, and more than 0 kPa to 2000 kPa. The calcination treatment can be carried out, for example, in air under the conditions of 350°C to 850°C, 2 hours to 30 hours.

[0087] (Step S1-2: Impregnation process) Next, the prepared precursor material (A) is impregnated with a metal-containing solution of a non-precious metal to obtain a precursor material (B).

[0088] The metal-containing solution may be any solution containing a metal component (e.g., metal ion) corresponding to the metal element (M) constituting the metal microparticles, and may be prepared, for example, by dissolving a metal salt containing the metal element (M) in a solvent. Examples of such metal salts include chlorides, hydroxides, oxides, sulfates, and nitrates, and among these, nitrates are preferred. Examples of the solvent that can be used include water, organic solvents such as alcohol, and mixtures thereof.

[0089] The method of impregnating the precursor material (A) with the metal-containing solution is not particularly limited, but for example, it is preferable to add the metal-containing solution in small amounts in multiple batches while stirring the powdered precursor material (A) before the firing step S1-3 described later. In addition, from the viewpoint of making it easier for the metal-containing solution to penetrate into the pores of the precursor material (A), it is preferable to add a surfactant as an additive to the precursor material (A) before adding the metal-containing solution to the precursor material (A). Such an additive has the function of coating the outer surface of the precursor material (A), and is thought to suppress the adhesion of the metal-containing solution added thereafter to the outer surface of the precursor material (A), making it easier for the metal-containing solution to penetrate into the pores of the precursor material (A).

[0090] Examples of such additives include nonionic surfactants such as polyoxyethylene alkyl ethers, such as polyoxyethylene oleyl ether, and polyoxyethylene alkyl phenyl ethers. These surfactants have a large molecular size and cannot penetrate into the pores of the precursor material (A), so they do not adhere to the pores and are considered not to hinder the metal-containing solution from penetrating into the pores. As a method for adding the nonionic surfactant, for example, it is preferable to add 50% by mass or more and 500% by mass or less of the nonionic surfactant to the precursor material (A) before the firing step S1-3 described later. If the amount of the nonionic surfactant added to the precursor material (A) is less than 50% by mass, the above-mentioned suppressing effect is difficult to manifest, and if the nonionic surfactant is added in an amount of more than 500% by mass to the precursor material (A), the viscosity of the solution increases too much.

[0091] In addition, the amount of the metal-containing solution added to the precursor material (A) is preferably adjusted appropriately in consideration of the amount of the metal element (M) contained in the metal-containing solution impregnated into the precursor material (A) (i.e., the amount of the metal element (M) to be contained in the precursor material (B)). For example, the amount of the metal-containing solution added to the precursor material (A) before the firing step S1-3 described later is preferably adjusted so that the ratio of silicon (Si) constituting the precursor material (A) to the metal element (M) in the metal-containing solution added to the precursor material (A) (atomic ratio Si / M) is 10 or more and 1000 or less, more preferably 50 or more and 200 or less. For example, when a surfactant is added as an additive to the precursor material (A) before adding the metal-containing solution to the precursor material (A), the amount of the metal-containing solution added to the precursor material (A) is 50 to 200 in terms of the atomic ratio Si / M, so that the metal element (M) of the metal fine particles can be contained at 0.5% by mass to 7.6% by mass relative to the catalyst structure. The amount of the metal element (M) present inside the pores of the precursor material (B) is roughly proportional to the amount of the metal-containing solution added to the precursor material (A) if the metal concentration of the metal-containing solution, the presence or absence of the additive, and other conditions such as temperature and pressure are the same. The amount of the metal element (M) present in the precursor material (B) is also proportional to the amount of the metal element constituting the metal fine particles present in the carrier of the catalyst structure. Therefore, by controlling the amount of the metal-containing solution added to the precursor material (A) within the above range, the metal-containing solution can be sufficiently impregnated into the pores of the precursor material (A), and further, the amount of metal fine particles present in the support of the catalyst structure can be adjusted.

[0092] After the precursor material (A) is impregnated with the metal-containing solution, a washing process may be performed as necessary. As the washing solution, water, an organic solvent such as alcohol, or a mixture of these solvents may be used. In addition, after the precursor material (A) is impregnated with the metal-containing solution and washed as necessary, it is preferable to further perform a drying process. Examples of the drying process include natural drying for about one night, and high-temperature drying at 150°C or less. Note that if the calcination process S1-3 described below is performed in a state where a large amount of moisture contained in the metal-containing solution and moisture from the washing solution remain in the precursor material (A), the skeleton structure of the precursor material (A) as a regular mesoporous material may be destroyed, so it is preferable to dry it thoroughly.

[0093] (Step S1-3: Firing process) Next, in order to obtain a support having a porous structure composed of a zeolite-type compound, precursor material (B) in which precursor material (A) is impregnated with a metal-containing solution is calcined to obtain precursor material (C).

[0094] The calcination is preferably carried out in air at a temperature of 350° C. to 850° C. for 2 hours to 30 hours, for example. Such a calcination causes crystal growth of the metal components impregnated in the pores of the ordered mesoporous material, forming fine particles of non-precious metals or fine particles of a metal oxide of non-precious metals in the pores.

[0095] (Step S1-4: Hydrothermal treatment process) Next, a mixed solution is prepared by mixing the precursor material (C) and the structure directing agent, and the precursor material (B) is calcined to obtain the precursor material (C), which is then subjected to a hydrothermal treatment to obtain a catalyst structure.

[0096] The structure-directing agent is a template agent for defining the skeletal structure of the support of the catalyst structure, and for example, a surfactant can be used. The structure-directing agent is preferably selected according to the skeletal structure of the support of the catalyst structure, and for example, surfactants such as tetramethylammonium bromide (TMABr), tetraethylammonium bromide (TEABr), and tetrapropylammonium bromide (TPABr) are suitable.

[0097] The precursor material (C) and the structure directing agent may be mixed during the hydrothermal treatment process or before the hydrothermal treatment process. The method for preparing the mixed solution is not particularly limited, and the precursor material (C), the structure directing agent, and the solvent may be mixed at the same time, or the precursor material (C) and the structure directing agent may be dispersed in a solvent, and then the respective dispersion solutions may be mixed. As the solvent, for example, water, an organic solvent such as alcohol, or a mixture of these may be used. In addition, it is preferable to adjust the pH of the mixed solution using an acid or a base before performing the hydrothermal treatment.

[0098] The hydrothermal treatment can be carried out by a known method, and is preferably carried out in a sealed container under the treatment conditions of 80° C. to 260° C., 5 hours to 240 hours, and a pressure of more than 0 kPa and less than 2000 kPa. The hydrothermal treatment is preferably carried out in a basic atmosphere.

[0099] The reaction mechanism here is not entirely clear, but is believed to be as follows: By carrying out hydrothermal treatment using precursor material (C) as a raw material, the skeletal structure of precursor material (C) as an ordered mesoporous substance gradually collapses, but the positions of the metal particles inside the pores of precursor material (C) are roughly maintained, and a new skeletal structure (porous structure) is formed as a support for the catalyst structure due to the action of the structure-directing agent. The catalyst structure thus obtained comprises a support with a porous structure and metal particles present in the support, and the support further has paths in which a plurality of pores are interconnected due to the porous structure, and at least a portion of the metal particles supported on the catalyst structure are present in the paths of the support.

[0100] In the above-mentioned hydrothermal treatment step, a mixed solution is prepared by mixing the precursor material (C) and the structure-directing agent, and the precursor material (C) is hydrothermally treated. However, this is not limited thereto, and the precursor material (C) may be hydrothermally treated without mixing the precursor material (C) and the structure-directing agent.

[0101] The precipitate (catalyst structure) obtained after the hydrothermal treatment is preferably subjected to washing, drying and calcination as necessary after recovery (for example, filtration). As the washing solution, water, an organic solvent such as alcohol, a mixed solvent thereof, etc. can be used. As the drying treatment, natural drying for about one night, or high-temperature drying at 150°C or less can be used. If the calcination treatment is performed in a state where a large amount of moisture remains in the precipitate, the skeletal structure as a support of the catalyst structure may be broken, so it is preferable to dry it thoroughly. In addition, the calcination treatment can be performed, for example, in air under treatment conditions of 350°C to 850°C and 2 hours to 30 hours. The structure-directing agent attached to the catalyst structure is burned off by such a calcination treatment. In addition, the catalyst structure can be used as it is without performing a calcination treatment on the precipitate after recovery depending on the purpose of use. For example, when the environment in which the catalyst structure is used is a high-temperature environment with an oxidizing atmosphere, the structure-directing agent is burned off by exposing it to the use environment for a certain period of time. In this case, the catalyst structure is obtained similar to that obtained when the calcination treatment is performed, so there is no need to perform the calcination treatment.

[0102] When the metal element (M) in the metal-containing solution to be impregnated into the precursor material (A) contains metal components such as Fe, Co, and Ni that are relatively easily oxidized, it is preferable to perform a reduction treatment on the precipitate obtained after the hydrothermal treatment step. In this case, the metal components are oxidized by the heat treatment in the steps (steps S1-3 to S1-4) following the impregnation treatment (step S1-2). Therefore, the support formed in the hydrothermal treatment step (step S1-4) contains metal oxide fine particles of non-precious metals. Therefore, in order to obtain a catalyst structure in which metal fine particles of non-precious metals are contained in the support, it is preferable to perform a calcination treatment on the recovered precipitate after the hydrothermal treatment, and further a reduction treatment under a reducing gas atmosphere such as hydrogen gas. By performing the reduction treatment, the metal oxide fine particles contained in the support are reduced, and metal fine particles corresponding to the metal element (M) constituting the metal oxide fine particles are formed. As a result, a catalyst structure in which metal fine particles are contained in the support is obtained. For example, when the catalyst structure is used in a reducing atmosphere, the metal oxide fine particles are reduced by exposing the catalyst structure to the use environment for a certain period of time. In this case, the catalyst structure is obtained in the same manner as when the reduction treatment is performed, and therefore there is no need to perform the reduction treatment.

[0103] [Modification of catalyst structure] FIG. 4 is a perspective view that illustrates another example of a catalyst structure used in the synthesis gas production apparatus and production method of the embodiment.

[0104] 2 includes a carrier 41 and a catalytic material 45 present in the carrier 41, but the catalytic structure used in the synthesis gas production apparatus and production method of the embodiment is not limited to this configuration. For example, as shown in FIG. 4, a catalytic structure 40a may further include at least one other catalytic material 45a held on an outer surface 41a of the carrier 41 in addition to the catalytic material 45 present in the carrier 41.

[0105] The catalytic substance 45a is a substance that exhibits one or more catalytic activities. The catalytic activity of the catalytic substance 45a may be the same as or different from that of the catalytic substance 45. In addition, when both the catalytic substance 45 and the catalytic substance 45a are substances having the same catalytic activity, the material of the catalytic substance 45a may be the same as or different from that of the catalytic substance 45. According to this configuration, the content of the catalytic substance held in the catalytic structure 40a can be increased, and the catalytic activity of the catalytic structure can be further promoted.

[0106] In this case, the content of the catalytic material 45 present in the carrier 41 is preferably greater than the content of the catalytic material 45a held on the outer surface 41a of the carrier 41. This makes the catalytic activity of the catalytic material 45 held inside the carrier 41 predominant, and the catalytic activity of the catalytic material 45 is stably exhibited.

[0107] As described above, according to the synthesis gas production apparatus and production method of the embodiment, it has been discovered that the cause of the decrease in catalytic activity of a catalyst structure having a catalyst substance present in a carrier is the oxidation of the catalyst substance present in the carrier, and further, by supplying a reducing gas to the catalyst structure, even when dry reforming is performed, it is possible to suppress the decrease in catalytic activity of the catalyst structure for a long period of time, and it is possible to stably produce a synthesis gas containing carbon monoxide and hydrogen for a long period of time.

[0108] Although the embodiments have been described above, the present invention is not limited to the above embodiments, but includes all aspects included in the concept and scope of the claims of the present disclosure, and can be modified in various ways within the scope of the present disclosure. EXAMPLES

[0109] Next, examples and comparative examples will be described, but the present invention is not limited to these examples.

[0110] (Example 1-1) First, a catalyst structure 1 was produced as follows.

[0111] A mixed solution was prepared by mixing tetraethoxysilane (TEOS) (manufactured by Wako Pure Chemical Industries, Ltd.) as a silica agent and a surfactant (hexadecyltrimethylammonium bromide (CTAB) (manufactured by Wako Pure Chemical Industries, Ltd.)) as a template agent, and the pH was appropriately adjusted. The solution was subjected to hydrothermal treatment at 80°C to 350°C for 100 hours in a sealed container. The precipitate formed by the hydrothermal treatment was then filtered, washed with water and ethanol, and further calcined in air at 600°C for 24 hours to obtain MCM-41 as precursor material (A).

[0112] Next, nickel (II) nitrate hexahydrate (manufactured by Wako Pure Chemical Industries, Ltd.) was dissolved in water to prepare a metal-containing solution of a non-precious metal. The metal-containing solution was then added in small amounts in multiple batches to the powdered precursor material (A), and the mixture was dried at room temperature (20°C ± 10°C) for 12 hours or more to obtain precursor material (B).

[0113] Before the addition of the metal-containing solution, the precursor material (A) was pretreated by adding an aqueous solution of polyoxyethylene (15) oleyl ether (NIKKOL BO-15V, manufactured by Nikko Chemicals Co., Ltd.) as an additive, and then the metal-containing solution was added as described above.

[0114] In addition, the amount of the metal-containing solution added to the precursor material (A) was adjusted so that the ratio of silicon (Si) constituting the precursor material (A) to the metal element (M) contained in the metal-containing solution (atomic number ratio Si / M) was 100.

[0115] Next, the precursor material (B) impregnated with the metal-containing solution obtained as above was calcined in air at 600° C. for 24 hours to obtain a precursor material (C).

[0116] Next, the precursor material (C) obtained as described above and tetrapropylammonium bromide (TPABr) as a structure directing agent were mixed to prepare a mixed solution, which was then subjected to hydrothermal treatment in a sealed container. The resulting precipitate was then filtered off, washed with water, dried at 100°C for 12 hours or more, and then calcined in air at 550°C for 24 hours to obtain catalyst structure 1. When catalyst structure 1 was observed, it was found that the catalytic substance Ni (metallic fine particles) was present within the support and supported on the outer surface of the support. The amount of Ni present within the support was greater than the amount of Ni supported on the outer surface of the support.

[0117] Next, the catalyst structure 1 was placed inside the synthesis gas generation section of the synthesis gas production apparatus shown in FIG. 1. As a pretreatment, the catalyst structure 1 was reduced under a hydrogen atmosphere at 700°C for 1.5 hours. Next, while the catalyst structure 1 was heated to 700°C, the raw material gas (methane and carbon dioxide) and the reducing gas (hydrogen) were added to the synthesis gas generation section in the ratio shown in Table 1 for 20 hours, GHSV=2400h. -1 was supplied.

[0118] After measuring the flow rate of the generated gas discharged from the synthesis gas generation section, the components in the generated gas were analyzed using a flame ionization detector (FID) and a thermal conductivity detector (TCD). The amount of methane in the generated gas was then derived from the measured flow rate of the generated gas and the analysis results of the FID / TCD, and the methane conversion rate was calculated from the following formula (1). Furthermore, the mass of carbon on the catalyst structure 1 after 3 hours and 20 hours was measured using a CHN elemental analyzer (CE-440, manufactured by EXETER ANALYTICAL, INC.), and the carbon amount (coke amount) was calculated from the following formula (2). These results are also shown in Table 1. The higher the methane conversion rate, the higher the synthesis gas production rate.

[0119] Methane conversion rate (%) = methane content in generated gas (cm 3 / h) × 100 / methane content in feed gas (cm 3 / h)...Formula (1)

[0120] Carbon content (mass%) = measured mass of carbon x 100 / (mass of catalyst structure + measured mass of carbon)

[0121] (Examples 1-2 to 1-4) The methane conversion rate and the carbon amount were measured in the same manner as in Example 1-1, except that the raw material gas (methane and carbon dioxide) and the reducing gas (hydrogen) supplied to the synthesis gas production section were changed to the values ​​shown in Table 1.

[0122] (Comparative Example 1-1) The methane conversion rate and carbon amount were measured in the same manner as in Example 1-1, except that no reducing gas was supplied to the synthesis gas production section and the raw material gas (methane and carbon dioxide) supplied to the synthesis gas production section was changed to the values ​​shown in Table 1.

[0123] (Comparative Example 1-2) The catalyst structure 1 was replaced with a commercially available nickel-based catalyst (product code: 31276, product name: Nickel on silica-alumina, catalyst, manufactured by Alfa Aesar), and the raw material gas was not supplied to the synthesis gas generation section, and the raw material gas (methane and carbon dioxide) supplied to the synthesis gas generation section was changed to the values ​​shown in Table 1. The methane conversion rate and carbon amount were measured in the same manner as in Example 1-1. In the nickel-based catalyst used in Comparative Example 1-2, Ni (metal fine particles) was not present in the support, but was supported only on the outer surface of the support. In Comparative Example 1-2, the internal pressure of the synthesis gas generation section rose significantly and became dangerous within 3 hours, so the production of synthesis gas was stopped midway. The carbon amount was measured based on the Ni particles supported on the outer surface of the support at the time of stopping.

[0124] [Table 1]

[0125] From Table 1, in the production apparatuses of Examples 1-1 to 1-4, the methane conversion rate was good for a long period of time. The reason for this is that by mixing a trace amount of hydrogen, which is a reducing gas, with the raw material gas (methane and carbon dioxide) and supplying it to the catalyst structure, the decrease in the catalytic activity of the catalyst structure could be suppressed for a long period of time. In addition, the deposition of carbon on the catalyst structure was below the detection limit. From the above, it became clear that synthesis gas can be stably produced for a long period of time.

[0126] (Examples 2-1 to 2-4) First, the raw material gas (methane and carbon dioxide) and reducing gas (hydrogen) supplied to the synthesis gas generating section were changed to the values ​​shown in Table 2, and the methane conversion rate (before refresh) was measured in the same manner as in Example 1-1, except that these gases were supplied for 48 hours. Next, a refresh process of the catalyst structure was performed under the refresh conditions shown in Table 2, and the methane conversion rate after the refresh (after refresh) was measured. Then, the value obtained by subtracting the methane conversion rate before the refresh from the methane conversion rate after the refresh was calculated as the reactivation rate.

[0127] [Table 2]

[0128] From Examples 2-1 to 2-4, the reactivation rate was improved by mixing reducing gas with methane and carbon dioxide during synthesis. Furthermore, the effect was more pronounced as the amount of reducing gas mixed increased. For example, the methane conversion rate before and after refreshing was the best in Example 2-1.

[0129] (Examples 3-1 to 3-3) First, in order to intentionally oxidize the catalyst structure and reduce the catalytic activity, the reducing gas was not supplied to the synthesis gas generating section, and the raw material gas (methane and carbon dioxide) supplied to the synthesis gas generating section was changed to the values ​​shown in Table 3, and these gases were supplied for 48 hours. Except for this, the methane conversion rate (before refresh) was measured in the same manner as in Example 1-1. Next, the catalyst structure was refreshed under the refresh conditions shown in Table 3, and the methane conversion rate (after refresh) after refreshing was measured. Then, the reactivation rate was calculated.

[0130] [Table 3]

[0131] It was found from Examples 3-1 to 3-3 that the reactivation rate of the catalyst structure improved when the temperature during the refresh treatment increased.

[0132] (Example 4-1) First, in order to intentionally oxidize the catalyst structure and reduce the catalytic activity, the reducing gas was not supplied to the synthesis gas generation section, and the raw material gases (methane and carbon dioxide) supplied to the synthesis gas generation section were changed to the values ​​shown in Table 4. These gases were supplied for 48 hours. Except for this, the methane conversion rate (before refreshing) was measured in the same manner as in Example 1-1.

[0133] Next, a decoking treatment was carried out under the decoking conditions shown in Table 4 to remove the coke from the catalyst structure using oxygen in the air.

[0134] Next, the catalyst structure was refreshed under the refresh conditions shown in Table 4, and the methane conversion rate after refreshing was measured. The reactivation rate was approximately the same as that of Example 3-1. Example 3-1 is shown in Table 4 for reference.

[0135] [Table 4]

[0136] Even if the conventional catalysts such as those shown in Comparative Example 1-2 are subjected to the refresh treatment of the present invention, the catalytic activity does not recover. In order to recover the catalytic activity, it is effective to perform a decoking treatment in which oxygen is supplied at high temperatures to gasify the coke. On the other hand, as shown in Examples 3-1 and 4-1, in the catalyst structure of the present disclosure, the catalytic activity can be refreshed only by a reduction treatment using a reducing gas. This is because a new deterioration mode different from that of conventional catalysts exists in the catalyst structure, and this new deterioration mode is thought to be caused by the oxidation of the catalytic material contained in the catalyst structure. [Explanation of symbols]

[0137] 1. Syngas production equipment 2. Raw gas supply section 2a Methane supply section 2b Carbon dioxide supply unit 3. Reducing gas supply section 4. Syngas Generation Section 4a Catalyst structure housing 5. Refreshment Section 6 Separation section 7 1st supply section 8 Second supply section 9. Detection Unit 40, 40a Catalyst structure 41 Carrier 41a Outer surface of carrier 42 Passage 42a hole 43 Expanded diameter part 44 Small passage 45, 45a Catalyst material

Claims

1. A synthesis gas production apparatus for producing a synthesis gas containing carbon monoxide and hydrogen, a raw material gas supply unit for supplying a raw material gas containing methane and carbon dioxide; A reducing gas supply unit that supplies a reducing gas; a synthesis gas generating section including a heating section for heating the catalyst structure, the raw material gas being supplied from the raw material gas supplying section and the reducing gas being supplied from the reducing gas supplying section, the catalyst structure being heated by the heating section while the raw material gas and the reducing gas are circulated through the catalyst structure, and a synthesis gas generating section generating a synthesis gas containing carbon monoxide and hydrogen from methane and carbon dioxide contained in the raw material gas; Equipped with The catalyst structure comprises a carrier having a porous structure composed of a zeolite type compound and at least one catalyst substance present in the carrier; The carrier has passages therein that communicate with each other, 2. A synthesis gas production apparatus, comprising: a catalyst material comprising fine particles of a non-noble metal, the fine particles being present in at least the passages of the support;

2. 2. The synthesis gas producing apparatus according to claim 1, wherein a content ratio (B×100 / (A+B)) of the supply amount (B) of the reducing gas supplied to the synthesis gas production unit with respect to a total amount (A+B) of the supply amount (A) of the raw material gas supplied to the synthesis gas production unit and the supply amount (B) of the reducing gas supplied to the synthesis gas production unit is 0.01 vol % or more.

3. 3. The synthesis gas production apparatus according to claim 1, wherein the heating temperature of the catalyst structure in the synthesis gas production section is 500° C. or higher and 1150° C. or lower.

4. Further comprising a refresh section for refreshing the catalytic activity of the catalyst structure, 4. The synthesis gas production apparatus according to claim 1, wherein the refresh unit continues to supply the reducing gas to the catalyst structure in a heated state while stopping the supply of the raw material gas from the raw material gas supply unit to the synthesis gas generation unit.

5. 5. The synthesis gas production apparatus according to claim 4, wherein the heating temperature of the catalyst structure in the synthesis gas production section is 600° C. or higher and 1000° C. or lower.

6. The synthesis gas production apparatus according to any one of claims 1 to 5, wherein the metal fine particles contain at least one non-precious metal selected from the group consisting of iron (Fe), cobalt (Co) and nickel (Ni).

7. the passage has one of one-dimensional pores, two-dimensional pores and three-dimensional pores in the framework structure of the zeolite-type compound, and an expanded portion different from any of the one-dimensional pores, the two-dimensional pores and the three-dimensional pores; the average particle diameter of the metal microparticles is larger than the average inner diameter of the passage and is equal to or smaller than the inner diameter of the expanded portion; the average inner diameter of the passage is calculated from an average value of the minor axis and the major axis of the pores constituting any one of the one-dimensional pores, the two-dimensional pores, and the three-dimensional pores; 7. The synthesis gas production apparatus according to claim 1, wherein the catalytic substance is present as being included in at least the expanded diameter portion.

8. The synthesis gas production apparatus according to claim 7 , wherein the expanded diameter section connects a plurality of holes constituting any one of the one-dimensional hole, the two-dimensional hole, and the three-dimensional hole to each other.

9. 9. The synthesis gas production apparatus according to claim 1, further comprising a separation section that separates the synthesis gas from methane and carbon dioxide from the synthesis gas discharged from the synthesis gas production section.

10. The synthesis gas producing apparatus according to claim 9 , further comprising a first supply unit that supplies the methane and carbon dioxide separated in the separation unit to the synthesis gas production unit.

11. The synthesis gas production apparatus according to any one of claims 1 to 10, further comprising a second supply unit that separates hydrogen from the synthesis gas discharged from the synthesis gas production unit and supplies the hydrogen to the synthesis gas production unit.

12. 12. The synthesis gas production apparatus according to claim 1, further comprising a detection unit for detecting carbon monoxide and hydrogen in the synthesis gas discharged from the synthesis gas production unit.

13. A method for producing a synthesis gas comprising the steps of: A step S1 of supplying a raw material gas containing methane and carbon dioxide and a reducing gas to a catalyst structure; a step S2 of heating the catalyst structure while flowing the raw material gas and the reducing gas through the catalyst structure to generate a synthesis gas containing carbon monoxide and hydrogen from methane and carbon dioxide contained in the raw material gas; having The catalyst structure comprises a carrier having a porous structure composed of a zeolite type compound and at least one catalyst substance present in the carrier; The carrier has passages therein that communicate with each other, The method for producing synthesis gas, wherein the catalytic material is fine metal particles of a non-noble metal and is present in at least the passages of the support.

Citation Information

Patent Citations

  • Method and apparatus for catalytically reacting lower hydrocarbon into aromatic compound, and method for producing aromatic compound and hydrogen

    JP2004269398A

  • Catalyst for producing synthesis gas and production method of synthesis gas

    JP2013255911A

  • Catalyst and method for producing syngas

    JP2014200705A

  • Catalyst for synthesis gas production, regeneration process of the catalyst, and process for producing synthesis gas

    JP2014217793A

  • Method for producing catalyst

    JP2016002527A