Battery pack
The laminated battery design with controlled thickness and gap limits and a step filler addresses stress concentration and cracking issues in high-pressure environments, ensuring battery reliability.
Patent Information
- Application Number
- JP2020011852
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-01-28
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2040-01-28
AI Technical Summary
Lithium ion batteries face issues with stress concentration and cracking in high-pressure environments due to gaps and thickness differences between components, which are not adequately addressed by existing configurations.
A laminated battery design with controlled thickness differences and gaps between frame members and laminated units, using a step filler to minimize stress concentration, ensuring components are within specific thickness and gap limits.
The design prevents stress concentration and cracking in high-pressure environments, maintaining battery integrity and performance.
Smart Images

Figure 0007553243000004 
Figure 0007553243000002 
Figure 0007553243000014
Abstract
Description
[Technical field]
[0001] The present invention relates to a battery pack. [Background technology]
[0002] In recent years, there has been an increasing demand for deeper diving depths and longer diving times for deep-sea equipment, submersible research vessels, submersible work robots, etc., and this has resulted in an increasing demand for larger capacity batteries to power these devices as their main drive power sources or to power the instruments and communication equipment installed on them.
[0003] Furthermore, batteries used in the deep sea are required to be configured for use in a high-pressure environment, and Patent Document 1 discloses a battery for use in the deep sea that is equipped with a pressure equalizing device having an expandable bellows.
[0004] Furthermore, Patent Document 2 discloses a single cell made of a lithium ion battery, and describes that a plurality of such cells are stacked in series for use as a stacked battery module. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2007-18573 A [Patent Document 2] JP 2018-125213 A Summary of the Invention [Problem to be solved by the invention]
[0006] The present inventors have investigated whether a lithium ion battery such as that described in Patent Document 2 can be used in a high-pressure environment. The lithium-ion battery described in Patent Document 2 has a single cell including an electrolyte, in which a positive electrode current collector, a positive electrode active material layer, a separator, a negative electrode active material layer, and a negative electrode current collector are laminated in this order, and is provided with a fixing part that is disposed between the positive electrode current collector and the negative electrode current collector to fix the peripheral portion of the separator between the positive electrode current collector and the negative electrode current collector, and that seals the positive electrode active material layer, the separator, and the negative electrode active material layer.
[0007] When a lithium-ion battery formed by stacking the unit cells described in Patent Document 2 was used in a high-pressure environment, the gaps between the positive electrode active material layer and the negative electrode active material layer and the surrounding fixing parts could become significantly recessed. When such a recess occurs, there is a concern that stress concentration occurs in the recess, causing cracks in the positive electrode current collector and / or the negative electrode current collector.
[0008] From the above investigations, it was thought that some improvement was necessary to make the lithium ion battery described in Patent Document 2 into a battery that could be used in a high-pressure environment. The battery described in Patent Document 1 is intended for use in a high-pressure environment, but since this battery has a different basic battery configuration, it would be difficult to improve the battery described in Patent Document 2 by referring to the configuration described in Patent Document 1.
[0009] The present invention has been made in consideration of the above problems, and has an object to provide a battery pack suitable for use in a high-voltage environment. [Means for solving the problem]
[0010] The present invention relates to an assembled battery having two or more unit cells each having a laminate unit consisting of a set of a positive electrode current collector, a positive electrode active material layer, a separator, a negative electrode active material layer, and a negative electrode current collector which are laminated in order, and an annular frame member which is arranged around the positive electrode active material layer, the separator, and the negative electrode active material layer between the positive electrode current collector and the negative electrode current collector, wherein the difference in thickness between a portion where the frame member is present and a portion where the laminate unit is present is 0.3 mm or less for each unit cell which constitutes the assembled battery, and the gap between the frame member and the laminate unit is 0.5 mm or less for each unit cell which constitutes the assembled battery; and the stacked unit is a negative electrode current collector, and an annular frame member is disposed around the positive electrode active material layer, the separator, and the negative electrode active material layer between the positive electrode current collector and the negative electrode current collector, wherein a step filler is provided on the frame member and on the positive electrode current collector and / or the negative electrode current collector in a gap between the frame member and the stacked unit, and the step filler is provided such that a difference between a thickness at a portion where the frame member is present, a thickness at a portion between the portion where the frame member is present and the portion where the stacked unit is present, and a thickness at a portion where the stacked unit is present is 0.3 mm or less. Effect of the Invention
[0011] According to the present invention, it is possible to provide a battery pack suitable for use in a high-voltage environment. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a cross-sectional view that illustrates an example of a unit cell that constitutes the battery pack of the present invention. [Diagram 2] FIG. 2 is a top view for explaining how to determine the gap between the frame member and the stack unit. [Diagram 3] FIG. 3 is a cross-sectional view that shows a schematic example of a cell in which there is a large difference in thickness between a portion where a frame member is present and a portion where a laminate unit is present, and there is a large gap between the frame member and the laminate unit. [Figure 4]FIG. 4 is a cross-sectional view that illustrates an example of a battery pack in which the unit cells shown in FIG. 3 are stacked. [Diagram 5] FIG. 5 is a cross-sectional view that illustrates an example of a battery pack in which the unit cells shown in FIG. 1 are stacked. [Figure 6] FIG. 6 is a cross-sectional view that illustrates a schematic diagram of another example of a unit cell that constitutes the battery pack of the present invention. [Figure 7] FIG. 7 is a cross-sectional view that illustrates an example of a battery pack in which a step filler is provided on the outside of the battery pack. [Figure 8] FIG. 8 is a photograph showing an enlarged view of a part of the upper surface of the laminate cell of Example 1. As shown in FIG. [Figure 9] FIG. 9 is a photograph showing an enlarged view of a part of the upper surface of the laminate cell of Example 2. As shown in FIG. [Figure 10] FIG. 10 is a photograph showing an enlarged view of a part of the upper surface of the laminate cell of Comparative Example 1. As shown in FIG. [Figure 11] FIG. 11 is a photograph showing an enlarged view of a part of the upper surface of the laminate cell of Comparative Example 2. As shown in FIG. [Figure 12] FIG. 12 is a photograph showing an enlarged view of a part of the upper surface of the laminate cell of Comparative Example 3. As shown in FIG. [Figure 13] FIG. 13 is a photograph showing an enlarged view of a part of the upper surface of the laminate cell of Example 5. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The present invention will be described in detail below. In this specification, the term "lithium ion battery" is intended to include the concept of a lithium ion secondary battery.
[0014] (First embodiment) A first embodiment of a battery pack of the present invention is an assembled battery including two or more single cells each having a lamination unit including a set of a positive electrode current collector, a positive electrode active material layer, a separator, a negative electrode active material layer, and a negative electrode current collector, which are laminated in order, and an annular frame member disposed around the positive electrode active material layer, the separator, and the negative electrode active material layer between the positive electrode current collector and the negative electrode current collector, With respect to the unit cells constituting the assembled battery, the difference in thickness between a portion where the frame member is present and a portion where the laminated unit is present is 0.3 mm or less; The battery pack is characterized in that the gap between the frame member and the stacking unit is 0.5 mm or less for each cell constituting the battery pack.
[0015] First, a case where the unit cells constituting the battery pack are the unit cells of the first embodiment will be described. FIG. 1 is a cross-sectional view that illustrates an example of a unit cell that constitutes the battery pack of the present invention. The single battery 100 shown in FIG. 1 has a positive electrode current collector 11, a positive electrode active material layer 13, a separator 30, a negative electrode active material layer 23, and a negative electrode current collector 21 laminated in this order, with the positive electrode current collector 11 and the negative electrode current collector 21 as the outermost layers. The positive electrode current collector 11 , the positive electrode active material layer 13 , the separator 30 , the negative electrode active material layer 23 and the negative electrode current collector 21 constitute a laminate unit 50 .
[0016] The stacking unit 50 is a position where all of the elements, i.e., the positive electrode collector 11, the positive electrode active material layer 13, the separator 30, the negative electrode active material layer 23, and the negative electrode collector 21, are present in the vertical direction in the cross section shown in FIG. 1, and is the region indicated by the double-headed arrow (reference symbol 50) in FIG. 1. The region of the positive electrode current collector 11 that is not in contact with the positive electrode active material layer 13 and the region of the negative electrode current collector 21 that is not in contact with the negative electrode active material layer 23 are not included in the laminate unit.
[0017] Between the positive electrode current collector 11 and the negative electrode current collector 21, an annular frame member 40 is disposed around the positive electrode active material layer 13, the separator 30, and the negative electrode active material layer . The unit cell is sealed by a frame member 40, a positive electrode current collector 11, and a negative electrode current collector 21, and an electrolyte is enclosed. The annular frame member means a structure that is annular when the unit cell is viewed from above, and is a structure in which stack units can be disposed within the ring of the frame member. The frame member may be one annular frame member formed by joining a frame member arranged around the positive electrode active material and a frame member arranged around the negative electrode active material. In FIG. 1, there is no distinction between a member that has been joined together to form a single annular frame member and a member that was originally a single annular frame member, and they are shown as a single annular frame member 40.
[0018] In the unit cell, the difference in thickness between the portion where the frame member is present and the portion where the laminate unit is present is 0.3 mm or less. The thicknesses of the portion where the frame member is present and the portion where the laminate unit is present include the thicknesses of the positive electrode current collector and the negative electrode current collector, respectively. The thickness of the portion where the frame member exists is indicated by a double-headed arrow T1 in FIG. 1, and the thickness of the portion where the laminate unit exists is indicated by a double-headed arrow T2 in FIG.
[0019] The difference in thickness between the portion where the frame member exists and the portion where the laminate unit exists is determined as follows. The thickness is measured at five or more points in the area where the frame member is present, and the average thickness is defined as the thickness of the area where the frame member is present (frame member thickness).Similarly, the thickness is measured at five or more points in the area where the laminate unit is present, and the average thickness is defined as the thickness of the area where the laminate unit is present (lamination unit thickness). The absolute value of the difference between the thickness of the frame member and the thickness of the laminate unit is defined as the difference in thickness between the portion where the frame member is present and the portion where the laminate unit is present.
[0020] It is also preferable that the difference between the total thickness of the positive electrode active material layer, the separator and the negative electrode active material layer and the thickness of the frame member is 0.3 mm or less. The total thickness of the positive electrode active material layer, the separator, and the negative electrode active material layer is indicated by a double-headed arrow T4 in FIG. 1, and the thickness of the frame member is indicated by a double-headed arrow T3 in FIG. The cell shown in FIG. 1 has a configuration in which the difference in thickness between the portion where the frame member is present and the portion where the laminate unit is present is reduced by matching the thickness of the frame member with the total thickness of the positive electrode active material layer, the separator, and the negative electrode active material layer.
[0021] By reducing the difference in thickness between the portion where the frame member is present and the portion where the laminate unit is present, the step between the portion where the frame member is present and the portion where the laminate unit is present when the unit cells are stacked is reduced, thereby preventing stress concentration between the frame member and the laminate unit when pressure is applied to the battery pack.
[0022] In addition, for each cell constituting the battery pack, the gap between the frame member and the stacking unit is 0.5 mm or less. The method of determining the gap between the frame member and the stacking unit in the unit cell will be described with reference to the drawings. FIG. 2 is a top view for explaining how to determine the gap between the frame member and the stack unit. The cell is viewed from above, and the gap (distance) between the frame member and the stacking unit is measured at four or more measurement points, and the average value is taken as the gap between the frame member and the stacking unit. When the shape of the laminate unit in top view is polygonal, the center of each side constituting the polygon is set as the measurement site. 2, the gaps between the frame member 40 and the laminate unit 50 are indicated by double-headed arrows W1, W2, W3, and W4 at the center of each side of a rectangle. The average value of W1, W2, W3, and W4 is defined as the gap between the frame member and the laminate unit.
[0023] If the gap between the frame member and the stacking unit defined in this manner is small, there is little room for a dent to form in the gap between the frame member and the stacking unit when pressure is applied to a battery pack formed by stacking single cells, and the problem of stress concentration in the dent is less likely to occur. The gap between the frame member and the laminate unit is preferably 0.3 mm or less, more preferably 0.1 mm or less. The lower limit of the gap between the frame member and the laminate unit is preferably 0 mm, and the lower limit of the gap between the frame member and the laminate unit is preferably 0.05 mm.
[0024] For comparison with the battery pack of the present invention, a problem that occurs when there is a large difference in thickness between the portion where the frame member is present and the portion where the laminate unit is present, and there is a large gap between the frame member and the laminate unit, will be described. FIG. 3 is a cross-sectional view that shows a schematic example of a cell in which there is a large difference in thickness between a portion where a frame member is present and a portion where a laminate unit is present, and there is a large gap between the frame member and the laminate unit.
[0025] The single battery 500 shown in FIG. 3 has a positive electrode current collector 11, a positive electrode active material layer 13, a separator 30, a negative electrode active material layer 23, and a negative electrode current collector 21 laminated in this order, with the positive electrode current collector 11 and the negative electrode current collector 21 as the outermost layers. The positive electrode current collector 11 , the positive electrode active material layer 13 , the separator 30 , the negative electrode active material layer 23 and the negative electrode current collector 21 constitute a laminate unit 50 . Between the positive electrode current collector 11 and the negative electrode current collector 21, an annular frame member 40 is disposed around the positive electrode active material layer 13, the separator 30, and the negative electrode active material layer .
[0026] In this unit cell 500, the thickness of the frame member (thickness indicated by double arrow t3) is thin, so that the thickness t1 of the portion where the frame member exists is thinner than the thickness t2 of the portion where the laminate unit exists. Moreover, the gap (the width indicated by the double-headed arrow w) between the frame member and the stack unit becomes larger.
[0027] FIG. 4 is a cross-sectional view that illustrates an example of a battery pack in which the unit cells shown in FIG. 3 are stacked. The battery pack 600 shown in FIG. 4 is formed by stacking five of the unit cells 500 shown in FIG. 4 is a schematic diagram showing a state in which pressure is applied to the battery pack 600 under a high-pressure environment. It can be seen that when pressure is applied to the battery pack 600, the gap between the frame member and the stacking unit is significantly depressed. When such a depression occurs, stress is concentrated in the depression, which may cause cracks in the positive electrode current collector and / or the negative electrode current collector.
[0028] On the other hand, a battery pack having two or more unit cells as shown in FIG. 1 is one example of the battery pack of the present invention. FIG. 5 is a cross-sectional view that illustrates an example of a battery pack in which the unit cells shown in FIG. 1 are stacked. The battery pack 300 shown in FIG. 5 is formed by stacking five of the cells 100 shown in FIG. FIG. 5 shows a schematic diagram of a state in which pressure is applied to the battery pack 300 in a high-pressure environment. In the cells 100 constituting the battery pack 300, the difference in thickness between the portion where the frame member is present and the portion where the stack unit is present is small, so that when the cells are stacked, the step between the portion where the frame member is present and the portion where the stack unit is present is small, which prevents stress concentration between the frame member and the stack unit when pressure is applied to the battery pack. In addition, since the gap between the frame member and the stacking unit of the single cells 100 constituting the battery pack 300 is small, when pressure is applied to a battery pack made up of stacked single cells, there is little room for a dent to form in the gap between the frame member and the stacking unit, making it less likely that the problem of stress concentration in the dent will occur.
[0029] A preferred embodiment of each of the components constituting the unit cell will be described below. The positive electrode active material layer contains a positive electrode active material. The positive electrode active material may be a composite oxide of lithium and a transition metal {composite oxides containing one type of transition metal (e.g., LiCoO2, LiNiO2, LiAlMnO4, LiMnO2, and LiMn2O4), composite oxides containing two types of transition metal elements (e.g., LiFeMnO4, LiNi 1-x Co x O2, LiMn 1-y Co y O2, LiNi 1 / 3 Co 1 / 3 Al 1 / 3 O2 and LiNi 0.8 Co 0.15 Al 0.05 O2) and composite oxides containing three or more metal elements [e.g. LiM a M' b M'' c O2(M, M' and M'' are different transition metal elements and satisfy a+b+c=1. For example, LiNi 1 / 3 Mn 1 / 3 Co 1 / 3Examples of the conductive polymer include lithium-containing transition metal phosphates (e.g., LiFePO4, LiCoPO4, LiMnPO4, and LiNiPO4), transition metal oxides (e.g., MnO2 and V2O5), transition metal sulfides (e.g., MoS2 and TiS2), and conductive polymers (e.g., polyaniline, polypyrrole, polythiophene, polyacetylene, poly-p-phenylene, and polyvinylcarbazole), and two or more of these may be used in combination. The lithium-containing transition metal phosphate may have some of the transition metal sites substituted with other transition metals.
[0030] The positive electrode active material is preferably a coated positive electrode active material coated with a conductive assistant and a coating resin. When the positive electrode active material is coated with a coating resin, the volume change of the electrode is mitigated, and the expansion of the electrode can be suppressed.
[0031] Examples of the conductive additive include metal-based conductive additives [aluminum, stainless steel (SUS), silver, gold, copper, titanium, etc.], carbon-based conductive additives [graphite and carbon black (acetylene black, ketjen black, furnace black, channel black, thermal lamp black, etc.)], and mixtures thereof. These conductive assistants may be used alone or in combination of two or more, and may also be used as alloys or metal oxides thereof. Among these, from the viewpoint of electrical stability, aluminum, stainless steel, silver, gold, copper, titanium, carbon-based conductive assistants, and mixtures thereof are more preferable, silver, gold, aluminum, stainless steel, and carbon-based conductive assistants are even more preferable, and carbon-based conductive assistants are particularly preferable. Furthermore, these conductive assistants may be formed by coating a particulate ceramic material or a resin material with a conductive material (preferably a metal one of the conductive assistants described above) by plating or the like.
[0032] The shape (form) of the conductive additive is not limited to a particulate form, and may be a form other than a particulate form, and may be a form that is in practical use as a so-called filler-based conductive additive, such as carbon nanofibers or carbon nanotubes.
[0033] The ratio of the coating resin to the conductive assistant is not particularly limited, but from the viewpoint of the internal resistance of the battery, etc., the weight ratio of the coating resin (resin solid content weight):conductive assistant is preferably 1:0.01 to 1:50, and more preferably 1:0.2 to 1:3.0.
[0034] As the coating resin, those described in JP2017-054703A as a resin for coating a non-aqueous secondary battery active material can be suitably used.
[0035] The positive electrode active material layer may contain a conductive assistant other than the conductive assistant contained in the coated positive electrode active material. As the conductive assistant, the same conductive assistant as that contained in the coated positive electrode active material described above can be suitably used.
[0036] The positive electrode active material layer preferably contains a positive electrode active material and is a non-binding material that does not contain a binder that binds the positive electrode active material together. Here, non-bound material means that the positive electrode active material is not fixed in position by a binding material (also called a binder), and the positive electrode active materials are not irreversibly fixed to each other or to the current collector.
[0037] The positive electrode active material layer may contain an adhesive resin. As the adhesive resin, for example, a resin for coating a non-aqueous secondary battery active material described in JP 2017-054703 A in which a small amount of an organic solvent is mixed to adjust the glass transition temperature to room temperature or lower, and a resin described as an adhesive in JP 10-255805 A can be suitably used. The adhesive resin means a resin that does not solidify even when the solvent component is evaporated and dried, and has adhesiveness (the property of adhering by applying slight pressure without using water, solvent, heat, etc.). On the other hand, the solution-drying type electrode binder used as a binding material means a material that dries and solidifies by evaporating the solvent component, and firmly adheres and fixes active materials together. Therefore, the solution drying type electrode binder (binding material) and the adhesive resin are different materials.
[0038] The thickness of the positive electrode active material layer is not particularly limited, but from the viewpoint of battery performance, it is preferably 150 to 600 μm, and more preferably 200 to 450 μm.
[0039] The negative electrode active material layer contains a negative electrode active material. As the negative electrode active material, known negative electrode active materials for lithium ion batteries can be used, and examples of the negative electrode active material include carbon-based materials [graphite, non-graphitizable carbon, amorphous carbon, resin baked bodies (e.g., phenolic resins and furan resins baked and carbonized, etc.), cokes (e.g., pitch coke, needle coke, petroleum coke, etc.), and carbon fibers, etc.], silicon-based materials [silicon, silicon oxide (SiOx), silicon-carbon composites (carbon particles whose surfaces are coated with silicon and / or silicon carbide, silicon particles or silicon oxide particles whose surfaces are coated with carbon and / or silicon carbide, silicon carbide, etc.)], and silicon-based materials [silicon, silicon oxide (SiOx), silicon-carbon composites (carbon particles whose surfaces are coated with silicon and / or silicon carbide, silicon particles or silicon oxide particles whose surfaces are coated with carbon and / or silicon carbide, silicon carbide, etc.], and silicon-based materials [silicon, silicon oxide (SiOx), silicon-carbon composites (carbon particles whose surfaces are coated with silicon and / or silicon carbide, silicon carbide, etc.)] ... oxide (SiOx), silicon oxide (SiOx), silicon oxide Examples of the conductive material include silicon alloys (silicon-aluminum alloy, silicon-lithium alloy, silicon-nickel alloy, silicon-iron alloy, silicon-titanium alloy, silicon-manganese alloy, silicon-copper alloy, silicon-tin alloy, etc.), conductive polymers (for example, polyacetylene and polypyrrole), metals (tin, aluminum, zirconium, titanium, etc.), metal oxides (titanium oxide and lithium-titanium oxide, etc.) and metal alloys (for example, lithium-tin alloy, lithium-aluminum alloy, lithium-aluminum-manganese alloy, etc.), and mixtures of these with carbon-based materials.
[0040] The negative electrode active material may be a coated negative electrode active material coated with a conductive assistant and a coating resin similar to the coated positive electrode active material described above. As the conductive assistant and the coating resin, the same conductive assistant and coating resin as those in the coated positive electrode active material described above can be suitably used.
[0041] The negative electrode active material layer may contain a conductive assistant other than the conductive assistant contained in the coated negative electrode active material. As the conductive assistant, the same conductive assistant as the conductive assistant contained in the coated positive electrode active material described above can be suitably used.
[0042] The negative electrode active material layer is preferably a non-binding material that does not contain a binder that binds the negative electrode active materials together, similar to the positive electrode active material layer, and may contain an adhesive resin, similar to the positive electrode active material layer.
[0043] The thickness of the negative electrode active material layer is not particularly limited, but from the viewpoint of battery performance, it is preferably 150 to 600 μm, and more preferably 200 to 450 μm.
[0044] Examples of materials constituting the positive electrode current collector and the negative electrode current collector (hereinafter collectively referred to simply as current collectors) include metal materials such as copper, aluminum, titanium, stainless steel, nickel, and alloys thereof, as well as baked carbon, conductive polymer materials, conductive glass, and the like. Of these materials, from the viewpoints of weight reduction, corrosion resistance, and high electrical conductivity, aluminum is preferred for the positive electrode current collector, and copper is preferred for the negative electrode current collector.
[0045] The current collector is preferably a resin current collector made of a conductive polymer material. The shape of the current collector is not particularly limited, and may be a sheet-like current collector made of the above-mentioned material, or a deposition layer made of fine particles made of the above-mentioned material. The thickness of the current collector is not particularly limited, but is preferably 50 to 500 μm.
[0046] The conductive polymer material constituting the resin collector may be, for example, a conductive polymer or a resin to which a conductive agent has been added as necessary. As the conductive agent constituting the conductive polymer material, the same conductive assistant as that contained in the coated positive electrode active material described above can be suitably used.
[0047] Examples of resins that constitute the conductive polymer material include polyethylene (PE), polypropylene (PP), polymethylpentene (PMP), polycycloolefin (PCO), polyethylene terephthalate (PET), polyethernitrile (PEN), polytetrafluoroethylene (PTFE), styrene butadiene rubber (SBR), polyacrylonitrile (PAN), polymethyl acrylate (PMA), polymethyl methacrylate (PMMA), polyvinylidene fluoride (PVdF), epoxy resin, silicone resin, and mixtures thereof. From the viewpoint of electrical stability, polyethylene (PE), polypropylene (PP), polymethylpentene (PMP) and polycycloolefin (PCO) are preferred, and polyethylene (PE), polypropylene (PP) and polymethylpentene (PMP) are more preferred.
[0048] The current collector may be a resin current collector having a metal layer on one or both sides thereof. Examples of the metal include copper, aluminum, titanium, stainless steel, nickel, and alloys thereof, which are listed as examples of the metal constituting the current collector itself. Methods for providing the metal layer include metal deposition and sputtering.
[0049] Examples of the separator include known separators for lithium ion batteries, such as porous films made of polyethylene or polypropylene, laminated films of porous polyethylene film and porous polypropylene, nonwoven fabrics made of synthetic fibers (polyester fibers, aramid fibers, etc.) or glass fibers, and those having ceramic particles such as silica, alumina, titania, etc. attached to their surfaces.
[0050] The positive electrode active material layer and the negative electrode active material layer contain an electrolyte. As the electrolytic solution, a known electrolytic solution containing an electrolyte and a non-aqueous solvent, which is used in the production of known lithium ion batteries, can be used.
[0051] As the electrolyte, those used in known electrolytic solutions can be used, for example, lithium salts of inorganic acids such as LiN(FSO2)2, LiPF6, LiBF4, LiSbF6, LiAsF6, and LiClO4, and lithium salts of organic acids such as LiN(CF3SO2)2, LiN(C2F5SO2)2, and LiC(CF3SO2)3, etc. Among these, imide-based electrolytes [LiN(FSO2)2, LiN(CF3SO2)2, LiN(C2F5SO2)2, etc.] and LiPF6 are preferred from the viewpoint of battery output and charge / discharge cycle characteristics.
[0052] As the non-aqueous solvent, those used in known electrolytic solutions can be used, such as lactone compounds, cyclic or chain carbonates, chain carboxylates, cyclic or chain ethers, phosphates, nitrile compounds, amide compounds, sulfones, sulfolane, and mixtures thereof.
[0053] The electrolyte concentration of the electrolytic solution is preferably 1 to 5 mol / L, more preferably 1.5 to 4 mol / L, and further preferably 2 to 3 mol / L. If the electrolyte concentration of the electrolytic solution is less than 1 mol / L, the battery may not exhibit sufficient input / output characteristics, whereas if it exceeds 5 mol / L, the electrolyte may precipitate. The electrolyte concentration of the electrolyte solution can be confirmed by extracting the electrolyte solution constituting the lithium ion battery electrode or the lithium ion battery without using a solvent or the like and measuring the concentration.
[0054] The material for the frame member is not particularly limited as long as it is durable against the electrolyte, but a polymer material is preferable, and a thermosetting polymer material is more preferable. Specific examples include epoxy resins, polyolefin resins, polyurethane resins, and polyvinylidene fluoride resins, with epoxy resins being preferred because of their high durability and ease of handling.
[0055] Second embodiment A second embodiment of the battery pack of the present invention is an assembled battery including two or more single cells each having a lamination unit including a set of a positive electrode current collector, a positive electrode active material layer, a separator, a negative electrode active material layer, and a negative electrode current collector, which are laminated in order, and an annular frame member disposed around the positive electrode active material layer, the separator, and the negative electrode active material layer between the positive electrode current collector and the negative electrode current collector, a step filler is provided on the frame member, and on the positive electrode current collector and / or the negative electrode current collector in a gap between the frame member and the stacking unit; The above-mentioned step filling material is a thickness at a portion where the frame member is present; and a thickness at a portion between a portion where the frame member is present and a portion where the laminate unit is present; The thickness difference between the portion where the laminate unit is present is set to be 0.3 mm or less.
[0056] The following describes a case where the unit cells constituting the battery pack are the unit cells of the second embodiment. In the unit cell of the second embodiment, step fillers are provided on the frame member, and on the gaps between the frame member and the stack units, and on the positive electrode current collector and / or the negative electrode current collector. The step filler is provided so that the difference between the thickness at the location where the frame member is present, the thickness at the location between the location where the frame member is present and the location where the laminate unit is present, and the thickness at the location where the laminate unit is present is 0.3 mm or less.
[0057] FIG. 6 is a cross-sectional view that illustrates a schematic diagram of another example of a unit cell that constitutes the battery pack of the present invention. In the single battery 200 shown in FIG. 6, a positive electrode current collector 11, a positive electrode active material layer 13, a separator 30, a negative electrode active material layer 23, and a negative electrode current collector 21 are laminated in this order, with the positive electrode current collector 11 and the negative electrode current collector 21 being the outermost layers. The positive electrode current collector 11 , the positive electrode active material layer 13 , the separator 30 , the negative electrode active material layer 23 and the negative electrode current collector 21 constitute a laminate unit 50 . Between the positive electrode current collector 11 and the negative electrode current collector 21, an annular frame member 40 is disposed around the positive electrode active material layer 13, the separator 30, and the negative electrode active material layer .
[0058] Furthermore, step fillers 60 are provided on the positive electrode current collector 11 on the frame member 40, on the positive electrode current collector 11 in the gap between the frame member 40 and the stacking unit 50, on the negative electrode current collector 21 on the frame member 40, and on the negative electrode current collector 21 in the gap between the frame member 40 and the stacking unit 50. The step filler 60 is not provided on the positive electrode current collector 11 in contact with the positive electrode active material layer 13 , and is not provided on the negative electrode current collector 21 in contact with the negative electrode active material layer 23 .
[0059] The gap filling material is provided so as to fill gaps in the area where the frame member is present, the area between the area where the frame member is present and the area where the laminate unit is present, and the area where the laminate unit is present. When the step filling material is not taken into consideration, the thickness t1 of the portion where the frame member exists is much thinner than the thickness t2 of the portion where the laminate unit exists. By providing the step filler on the current collector on the frame member, the thickness T1 of the portion where the frame member is present becomes thicker, and the difference between the thickness T1 of the portion where the frame member is present and the thickness t2 of the portion where the laminate unit is present becomes smaller. In addition, by providing the step filler on the current collector above the gap between the frame member and the laminate unit, the thickness T5 at the portion between the portion where the frame member is present and the portion where the laminate unit is present becomes thicker, and the difference between the thickness T5, the thickness T1 at the portion where the frame member is present, and the thickness t2 at the portion where the laminate unit is present becomes smaller. Specifically, the step filler is provided so that the difference between the thickness T1 of the portion where the frame member is present, the thickness T5 of the portion between the portion where the frame member is present and the portion where the laminate unit is present, and the thickness t2 of the portion where the laminate unit is present is 0.3 mm or less.
[0060] When a step filler is provided, the difference between the thickness at the portion where the frame member is present, the thickness between the portion where the frame member is present and the portion where the laminate unit is present, and the thickness at the portion where the laminate unit is present is calculated by measuring the thickness at five or more points at each portion, calculating the average, and then calculating the difference between the maximum and minimum values of the average values.
[0061] In addition, in Figure 6, on the positive electrode side, a step filler 60 is provided on the underside of the positive electrode current collector 11 outside the frame member 40, but when a step filler is provided on the outside of the current collector regardless of the top or bottom in the figure, it is considered that "a step filler is provided on the current collector."
[0062] In the cell of the second embodiment as well, the gap between the frame member and the stack unit is preferably 0.5 mm or less. Furthermore, by using the unit cell of the second embodiment, the same effects as those obtained by using the unit cell of the first embodiment can be obtained. That is, when pressure is applied to the battery pack, stress concentration between the frame member and the laminated units is prevented. Furthermore, since there are small gaps within the cells when pressure is applied to a battery pack formed by stacking the cells, there is little room for dents to form in the cells, making it less likely that the problem of stress concentration in the dents will occur.
[0063] Each component constituting the unit cell of the second embodiment can be similar to each component constituting the unit cell of the first embodiment, and therefore detailed description thereof will be omitted. In the battery of the second embodiment, the material of the step filler is not particularly limited, but is preferably a resin material, which may be applied to the current collector and cured, such as epoxy resin, polyolefin resin, polyurethane resin, and polyvinylidene fluoride resin.
[0064] Next, a method for manufacturing the unit cell and the battery pack will be described. The cell 100 can be manufactured as follows. The positive electrode current collector 11 is joined to one frame surface of an annular frame member, and one end of the frame member is sealed. Next, the frame member is filled with a positive electrode active material that will become the positive electrode active material layer 13. At this time, it is preferable to fill the frame member with as much positive electrode active material as possible so that no gap occurs between the frame member and the positive electrode active material layer. Next, a separator is placed on the other frame surface of the frame member. Similarly, the negative electrode current collector 21 is joined to one frame surface of the annular frame member, and one end of the frame member is sealed. Next, the frame member is filled with a negative electrode active material that will become the negative electrode active material layer 23. At this time, it is preferable to fill the frame member with as much negative electrode active material as possible so that no gap occurs between the frame member and the negative electrode active material layer. Next, a separator is placed on the other frame surface of the frame member. The frame members are then bonded together and sealed to obtain the unit cell 100. The two bonded frame members are joined together to form frame member 40. In the above example, separators are placed in both the frame member filled with the positive electrode active material and the frame member filled with the negative electrode active material, and the two separators are stacked to form separator 30, but the separator may be placed in only one of the frame members. It is preferable to adjust the thickness of the frame member so that the difference between the total thickness of the positive electrode active material layer, the separator, and the negative electrode active material layer and the thickness of the frame member is 0.3 mm or less. The unit cell manufactured in this manner is the unit cell of the first embodiment.
[0065] In addition, after producing a single battery without adjusting the thickness of the frame member, a step filler is provided to fill in the steps at the location where the frame member is present, the location between the location where the frame member is present and the location where the stack unit is present, and the location where the stack unit is present, thereby making it possible to manufacture the single battery of the second embodiment. The step filling material can be provided on the current collector by applying a resin material constituting the step filling material and curing it.
[0066] A plurality of the thus manufactured single cells can be stacked to manufacture a battery pack. When stacking the single cells, the single cells are stacked in the same orientation so that the positive electrode current collector of one cell is in contact with the negative electrode current collector of an adjacent cell, thereby obtaining a battery pack in which multiple single cells are connected in series.
[0067] Furthermore, even if a battery pack is manufactured in which a step filler is provided on the outside of the battery pack, a battery pack suitable for use in a high-pressure environment can be provided. FIG. 7 is a cross-sectional view that illustrates an example of a battery pack in which a step filler is provided on the outside of the battery pack. The battery pack 400 shown in Fig. 7 is based on a battery pack formed by stacking unit cells, such as the battery pack 600 shown in Fig. 4, in which there is a large difference in thickness between the portion where the frame member is present and the portion where the stacking unit is present. In the battery pack 400, the battery pack 600 shown in Fig. 4 is surrounded by an outer frame member 410, an upper frame member 420, and a lower frame member 430. Step fillers 60 are provided in the gaps between the battery pack 600 and each frame member. As the step filling material 60, the step filling material constituting the unit cell of the second embodiment can be used. 7, the step between the outer frame member 410 and the battery assembly 600 is small, which prevents stress concentration between the outer frame member 410 and the battery assembly 600 when pressure is applied to the battery assembly 400. This makes it possible to provide a battery assembly suitable for use in high-pressure environments. EXAMPLES
[0068] The present invention will now be described in detail with reference to examples, but the present invention is not limited to these examples as long as they do not deviate from the gist of the present invention. In addition, unless otherwise specified, parts means parts by weight and % means % by weight.
[0069] <Preparation of coating resin solution> Into a four-neck flask equipped with a stirrer, a thermometer, a reflux condenser, a dropping funnel, and a nitrogen gas inlet tube, 83 parts of ethyl acetate and 17 parts of methanol were placed and heated to 68°C. Next, a monomer blend solution containing 242.8 parts of methacrylic acid, 97.1 parts of methyl methacrylate, 242.8 parts of 2-ethylhexyl methacrylate, 52.1 parts of ethyl acetate, and 10.7 parts of methanol, and an initiator solution containing 0.263 parts of 2,2'-azobis(2,4-dimethylvaleronitrile) dissolved in 34.2 parts of ethyl acetate were continuously dropped into a four-neck flask with nitrogen for 4 hours under stirring to carry out radical polymerization. After the dropwise addition was completed, an initiator solution containing 0.583 parts of 2,2'-azobis(2,4-dimethylvaleronitrile) dissolved in 26 parts of ethyl acetate was continuously added using a dropping funnel for 2 hours. Furthermore, polymerization was continued at the boiling point for 4 hours. After removing the solvent to obtain 582 parts of resin, 1,360 parts of isopropanol were added to obtain a coating resin solution consisting of a vinyl resin with a resin concentration of 30% by weight.
[0070] <Preparation of Positive Electrode Composition> LiNi 0.8 Co 0.15 Al 0.05 94 parts of O2 powder was placed in a universal mixer and stirred at room temperature (25°C) at 150 rpm. The above-mentioned coating resin solution (resin solids concentration: 30% by mass) was added dropwise over 60 minutes to 3 parts of resin solids, and the solution was then stirred for an additional 30 minutes. Next, while stirring, 3 parts of acetylene black (Denka Black (registered trademark) manufactured by Denka Co., Ltd.) (average particle diameter (primary particle diameter): 0.036 μm) was added in three separate batches, and the mixture was heated to 70° C. with stirring for 30 minutes, reduced pressure to 100 mmHg, and held for 30 minutes to obtain coated positive electrode active material particles. 100 parts of the coated positive electrode active material particles and 6 parts of carbon fiber (DonaCarbo Milled S-243, manufactured by Osaka Gas Chemicals Co., Ltd.: average fiber length 500 μm, average fiber diameter 13 μm: electrical conductivity 200 mS / cm) were dry blended to obtain a positive electrode material mixture. Then, 11 parts of an electrolyte were added to the positive electrode material mixture and mixed in a mixer to obtain a positive electrode composition.
[0071] <Preparation of negative electrode composition> 88 parts of non-graphitizable carbon [Carbotron (registered trademark) PS(F) manufactured by Kureha Battery Materials Japan Co., Ltd.] was placed in a universal mixer and stirred at room temperature (25°C) and 150 rpm. A coating resin solution (resin solids concentration: 30% by weight) was added dropwise over 60 minutes to the mixture so that the resin solids amounted to 6 parts, and the mixture was further stirred for 30 minutes. Next, while stirring, 6 parts of acetylene black [Denka Black (registered trademark) manufactured by Denka Co., Ltd.] (average particle diameter (primary particle diameter): 0.036 μm) was mixed in three batches, and the mixture was heated to 70° C. with stirring for 30 minutes, reduced pressure to 0.01 MPa, and held for 30 minutes to obtain coated negative electrode active material particles. 100 parts of the coated negative electrode active material particles and 1 part of carbon fiber (DonaCarbo Milled S-243, manufactured by Osaka Gas Chemicals Co., Ltd.: average fiber length 500 μm, average fiber diameter 13 μm: electrical conductivity 200 mS / cm) were dry-blended to obtain a negative electrode material mixture. Then, 0.11 parts of an electrolyte was added to the negative electrode material mixture and mixed in a mixer to obtain a negative electrode composition.
[0072] <Preparation of electrolyte> An electrolyte solution was obtained by dissolving LiPF6 at a ratio of 1 mol / L in a mixed solvent of ethylene carbonate (EC) and propylene carbonate (PC) (volume ratio 1:1).
[0073] <Manufacturing of positive electrode current collector> In a twin-screw extruder, 69.7 parts of polypropylene (PP) [trade name "Sunallomer PC630S", manufactured by Sunallomer Co., Ltd.], 25.0 parts of acetylene black [Denka Black (registered trademark), manufactured by Denka Co., Ltd.], and 5.0 parts of a dispersant [trade name "UMEX 1001 (acid-modified polypropylene)", manufactured by Sanyo Chemical Industries, Ltd.] were melt-kneaded under conditions of 180 ° C., 100 rpm, and a residence time of 5 minutes to obtain a positive electrode resin current collector material. The obtained positive electrode resin current collector material was passed through a T-die extrusion film molding machine and then rolled multiple times with a hot press machine to obtain a positive electrode current collector with a film thickness of 42 μm.
[0074] <Manufacturing of negative electrode current collector> A negative electrode resin current collector material was obtained by melt-kneading 70 parts of polypropylene [trade name "Sunallomer PL500A", manufactured by Sunallomer Co., Ltd.], 25 parts of nickel particles [manufactured by Vale], and 5 parts of a dispersant [trade name "UMEX 1001", manufactured by Sanyo Chemical Industries, Ltd.] in a twin-screw extruder at 200°C and 200 rpm. The obtained negative electrode resin current collector material was passed through a T-die extrusion film molding machine and then rolled multiple times with a hot press machine to obtain a negative electrode resin current collector roll having a thickness of 45 μm. A copper metal layer was formed to a thickness of 5 nm on one side of this negative electrode resin current collector raw sheet by vacuum deposition to obtain a negative electrode current collector having a metal layer on one side.
[0075] Example 1 An annular frame member made of epoxy resin and having a rectangular shape when viewed from above was prepared. One end of the positive electrode current collector was joined to one of the frame surfaces of the frame member. The frame member was filled with a positive electrode composition, and a separator was placed on the other frame surface of the frame member. A frame member different from the frame member filled with the positive electrode composition was prepared, and one end of the negative electrode current collector was joined to one frame surface of the frame member in the same manner as above, with the metal layer in a direction in which it contacted the negative electrode composition. The negative electrode composition was filled in the frame member, and a separator was placed on the other frame surface of the frame member. The frame member filled with the positive electrode composition and the frame member filled with the negative electrode composition were attached to each other with the separators facing each other, and sealed to obtain a single cell. The dimensions of this single cell were adjusted so that the difference between the total thickness of the positive electrode active material layer, the separator and the negative electrode active material layer and the thickness of the frame member was 0 mm. In addition, the electrode composition was filled so that the gap between the frame member and the laminate unit was 0 mm. In this unit cell, the difference in thickness between the portion where the frame member is present and the portion where the laminate unit is present is 0 mm.
[0076] (Examples 2 to 4, Comparative Examples 1 to 3) A single cell was fabricated by changing the thickness of the frame member or by changing the gap between the frame member and the stacking unit. Table 1 shows the difference in thickness between the portion where the frame member is present and the portion where the laminate unit is present in each unit cell.
[0077] (Production of assembled batteries and pressure testing) Eight cells obtained in each of the Examples and Comparative Examples were stacked to obtain a battery pack. The entire battery pack was then covered with an aluminum laminate film and evacuated (vacuum packed) to simulate a high-pressure environment.
[0078] (External Observation) After the pressure test, the aluminum laminate cells were observed to see whether there were any dents in the gaps between the frame members and the laminate units. The observation results are shown in Table 1.
[0079] (Observation of the current collector) After the pressure test, the aluminum laminate cell was opened and the state of the current collector of the single cell was observed. The current collector was observed for the presence or absence of cracks, and the observation results are shown in Table 1.
[0080] [Table 1]
[0081] The drawings show photographs showing the presence or absence of dents in Examples 1 and 2 and Comparative Examples 1, 2, and 3. Each drawing shows an enlarged photograph of the vicinity of a vertex of a laminate unit having a rectangular shape when viewed from above. FIG. 8 is a photograph showing an enlarged view of a part of the upper surface of the laminate cell of Example 1, and FIG. 9 is a photograph showing an enlarged view of a part of the upper surface of the laminate cell of Example 2. The black lines in Figures 8 and 9 are marks (indicating the vertices of the rectangular stacked units) for observation under a microscope. FIG. 10 is a photograph showing an enlarged portion of the upper surface of the laminate cell of Comparative Example 1, FIG. 11 is a photograph showing an enlarged portion of the upper surface of the laminate cell of Comparative Example 2, and FIG. 12 is a photograph showing an enlarged portion of the upper surface of the laminate cell of Comparative Example 3.
[0082] As shown in Figures 8 and 9, no dents were observed in the gaps between the frame member and the laminated member in Examples 1 and 2. On the other hand, as shown in Figures 10, 11, and 12, dents were observed in the gaps between the frame member and the laminated member in all of Comparative Examples 1 to 3.
[0083] These results show that in the assembled batteries of Examples 1 to 4, stress concentration between the frame member and the laminate unit was prevented when pressure was applied, and cracks were prevented from occurring in the current collectors.
[0084] Example 5 After producing the single battery of Comparative Example 3, an epoxy resin was applied as a gap filler and cured so as to fill in the gaps in the area where the frame member was present, the area between the area where the frame member was present and the area where the laminate unit was present, and the area where the laminate unit was present. In this cell, the difference in thickness between the portion where the frame member is present, the portion between the portion where the frame member is present and the portion where the laminate unit is present, and the portion where the laminate unit is present is 0 mm. A battery pack was fabricated in the same manner as in Example 1, and a pressure test was carried out. As a result, no dents were found in the gaps between the frame members and the laminate units, and no cracks were found in the current collectors. FIG. 13 is a photograph showing an enlarged view of a part of the upper surface of the laminate cell of Example 5. As shown in FIG. 13, in Example 5 as well, no depressions were observed in the gaps between the frame members and the laminated members. [Industrial Applicability]
[0085] The battery pack of the present invention is particularly useful as a battery for use in a high-pressure environment. [Explanation of symbols]
[0086] 11 Positive electrode current collector 13 Cathode active material layer 21 Negative electrode current collector 23 Negative electrode active material layer 30 Separator 40 Frame members 50 stacking units 60 Step filling material 100, 200, 500 Cells 300, 400, 600 battery packs 410 Outer frame members 420 Upper frame member 430 Lower frame member
Claims
1. A battery pack including two or more unit cells each having a stacking unit including a set of a positive electrode current collector, a positive electrode active material layer, a separator, a negative electrode active material layer, and a negative electrode current collector, which are stacked in order, and an annular frame member disposed around the positive electrode active material layer, the separator, and the negative electrode active material layer between the positive electrode current collector and the negative electrode current collector, With respect to the unit cells constituting the assembled battery, the difference in thickness between a portion where the frame member is present and a portion where the laminated unit is present is 0.3 mm or less; The battery pack is characterized in that, for each cell constituting the battery pack, a gap between the frame member and the stacking unit is 0.05 mm or more and 0.5 mm or less.
2. 2. The battery pack according to claim 1, wherein a difference between a total thickness of the positive electrode active material layer, the separator and the negative electrode active material layer and a thickness of the frame member is 0.3 mm or less.
3. A battery pack including two or more unit cells each having a stacking unit including a set of a positive electrode current collector, a positive electrode active material layer, a separator, a negative electrode active material layer, and a negative electrode current collector, which are stacked in order, and an annular frame member disposed around the positive electrode active material layer, the separator, and the negative electrode active material layer between the positive electrode current collector and the negative electrode current collector, a step filler is provided on the frame member, and on a positive electrode current collector and / or a negative electrode current collector in a gap between the frame member and the stacking unit; The step filling material is a thickness at a portion where the frame member is present; and a thickness at a portion between the portion where the frame member is present and the portion where the laminate unit is present; a difference in thickness between the laminated unit and a portion where the laminated unit is present is set to be 0.3 mm or less.
Citation Information
Patent Citations
Activated carbon / polyacene material composite, its production, electrical double-layer capacitor and its composite part
JP1992288361A
Electrochemical cell laminate
JP2005100926A
Objective driving device
JP2007018573A
Bipolar type battery, battery module, and battery pack
JP2007194090A
Battery module, battery pack, and vehicle with such batteries mounted thereon
JP2007242593A