Adhesive composition and adhesive sheet

The adhesive composition with specific structural units and a crosslinking agent ensures high adhesive strength at high temperatures and easy removal at room temperature, addressing the challenges of adhesive residue in electronic device manufacturing.

JP7553387B2Active Publication Date: 2024-09-18NIPPON CARBIDE KOGYO KK
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021044090
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-17
Publication Date
2024-09-18
Estimated Expiration
2041-03-17

AI Technical Summary

Technical Problem

Adhesives used for temporary fixing in electronic device manufacturing face challenges in maintaining high adhesive strength at high temperatures without leaving residue and peeling off easily at room temperature after exposure to high temperatures.

Method used

An adhesive composition comprising 30% to 70% structural units derived from (meth)acrylic acid alkyl ester monomers with branched alkyl groups, 10% to 50% structural units from (meth)acrylic acid alkyl ester monomers with linear alkyl groups having 16 or more carbon atoms, and 10% to 50% structural units from monomers with carboxy groups, along with a crosslinking agent, forms an adhesive layer that maintains high adhesive strength at high temperatures and allows easy removal at room temperature.

Benefits of technology

The adhesive composition achieves high adhesive strength in high-temperature environments and excellent removability at room temperature, preventing residue on adherends after peeling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007553387000001
    Figure 0007553387000001
  • Figure 0007553387000002
    Figure 0007553387000002
  • Figure 0007553387000003
    Figure 0007553387000003
Patent Text Reader

Abstract

To provide an adhesive composition capable of forming an adhesive layer which exhibits a high adhesive force in a high-temperature environment and exhibits excellent re-releasability under an ordinary temperature environment after exposed to the high temperature environment and to provide an adhesive sheet.SOLUTION: There are provided: an adhesive composition which comprises a (meth)acrylic copolymer containing 30 to 70 mass% of a constitutional unit derived from a (meth)acrylic acid alkyl ester monomer having a branched-chain alkyl group based on the total constitutional units, 10 to 50 mass% of a constitutional unit derived from a (meth)acrylic acid alkyl ester monomer having a linear alkyl group having 16 or more carbon atoms based on the total constitutional units and 10 mass% or more of a constitutional unit derived from a monomer having a carboxy group based on the total constitutional units and a crosslinking agent; and an adhesive sheet.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a pressure-sensitive adhesive composition and a pressure-sensitive adhesive sheet. [Background technology]

[0002] Conventionally, adhesives have been used to temporarily fix various members in the manufacturing process of electronic devices. Various reports have been made on adhesives used for temporary fixing (for example, see Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2016-196544 A [Patent Document 2] JP 2008-179744 A Summary of the Invention [Problem to be solved by the invention]

[0004] In the manufacturing process of electronic devices, a member temporarily fixed to an adherend may be exposed to a high temperature environment, and in some processes, the atmospheric temperature may reach around 150°C. For this reason, the adhesive used for temporary fixing is required to be able to form an adhesive layer that exhibits such high adhesive strength that the member does not peel off from the adherend or shift from the initial position where the member was temporarily fixed, even when exposed to a high temperature environment of, for example, 150°C. In addition, the member temporarily fixed to the adherend is removed from the adherend when the fixation is no longer necessary. However, the adhesive layer exposed to a high temperature environment may have an increased adhesive strength over time, making it difficult to peel off from the adherend after cooling. In addition, the adhesive layer exposed to a high temperature environment may transfer to the surface of the adherend when peeled off from the adherend after cooling, thereby contaminating the adherend. For this reason, the adhesive used for temporary fixation is required to be capable of forming an adhesive layer that can be easily peeled from the adherend even when exposed to a high-temperature environment of, for example, 150°C, and that is unlikely to leave adhesive residue on the surface of the adherend when subsequently peeled off in a room-temperature environment of, for example, 25°C, and that has excellent removability.

[0005] An object of one embodiment of the present disclosure is to provide a pressure-sensitive adhesive composition capable of forming a pressure-sensitive adhesive layer that exhibits high adhesive strength in a high-temperature (e.g., 150°C; the same applies below) environment and that exhibits excellent removability in a room temperature (e.g., 25°C; the same applies below) environment after exposure to the high-temperature environment. The problem that another embodiment of the present disclosure aims to solve is to provide an adhesive sheet having an adhesive layer that exhibits high adhesive strength in a high-temperature environment and also exhibits excellent removability in a room temperature environment after being exposed to a high-temperature environment. [Means for solving the problem]

[0006] Specific means for solving the problems include the following aspects. <1> a (meth)acrylic copolymer containing 30% by mass to 70% by mass of structural units derived from a (meth)acrylic acid alkyl ester monomer having a branched alkyl group, based on all structural units, 10% by mass to 50% by mass of structural units derived from a (meth)acrylic acid alkyl ester monomer having a linear alkyl group having 16 or more carbon atoms, based on all structural units, and 10% by mass or more of structural units derived from a monomer having a carboxy group, based on all structural units; A cross-linking agent; A pressure-sensitive adhesive composition comprising: <2> The crosslinking agent is an epoxy crosslinking agent. <1> The pressure-sensitive adhesive composition according to claim 1. <3> The weight average molecular weight of the (meth)acrylic copolymer is 100,000 to 300,000. <1> or <2> The pressure-sensitive adhesive composition according to claim 1. <4> The (meth)acrylic copolymer has a glass transition temperature of 40° C. to 70° C. <1> ~ <3> 13. The pressure-sensitive adhesive composition according to claim 12 . <5> The (meth)acrylic acid alkyl ester monomer having a linear alkyl group having 16 or more carbon atoms is stearyl methacrylate. <1> ~ <4> 13. The pressure-sensitive adhesive composition according to claim 12 . <6> <1> ~ <5> 13. A pressure-sensitive adhesive sheet comprising a pressure-sensitive adhesive layer formed from the pressure-sensitive adhesive composition according to any one of claims 1 to 22. Effect of the Invention

[0007] According to one embodiment of the present disclosure, there is provided a pressure-sensitive adhesive composition capable of forming a pressure-sensitive adhesive layer that exhibits high adhesive strength in a high-temperature environment and excellent removability in a room temperature environment after exposure to a high-temperature environment. According to another embodiment of the present disclosure, there is provided an adhesive sheet including an adhesive layer that exhibits high adhesive strength in a high-temperature environment and exhibits excellent removability in a room temperature environment after being exposed to the high-temperature environment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The pressure-sensitive adhesive composition and pressure-sensitive adhesive sheet of the present disclosure will be described in detail below. The following description of the requirements may be based on a representative embodiment of the present disclosure, but the present disclosure is not limited to such an embodiment, and can be modified as appropriate within the scope of the purpose of the present disclosure.

[0009] In the present disclosure, a numerical range indicated using "to" means a range that includes the numerical values ​​before and after "to" as the lower limit and upper limit, respectively. In the numerical ranges described in the present disclosure, the upper or lower limit value described in a certain numerical range may be replaced with the upper or lower limit value of another numerical range described in the present disclosure. In addition, in the numerical ranges described in the present disclosure, the upper or lower limit value described in a certain numerical range may be replaced with a value shown in the examples.

[0010] In the present disclosure, combinations of two or more preferred embodiments are more preferred embodiments. In the present disclosure, when the adhesive composition contains multiple substances corresponding to each component, the amount of each component in the adhesive composition means the total amount of the multiple substances present in the adhesive composition, unless otherwise specified.

[0011] In the present disclosure, "(meth)acrylic copolymer" means a copolymer in which the content of structural units derived from monomers having a (meth)acryloyl group is 50 mass% or more of all structural units (i.e., all structural units of the (meth)acrylic copolymer). In the present disclosure, "(meth)acrylic monomer" means a monomer having a (meth)acryloyl group.

[0012] In this disclosure, "(meth)acrylic" is a term that encompasses both "acrylic" and "methacrylic", "(meth)acrylate" is a term that encompasses both "acrylate" and "methacrylate", and "(meth)acryloyl" is a term that encompasses both "acryloyl" and "methacryloyl".

[0013] In this disclosure, "n-" means normal, "i-" means iso, "s-" means secondary, and "t-" means tertiary.

[0014] In the present disclosure, the terms "adhesive" and "adhesive composition" have the same meaning.

[0015] [Adhesive composition] The pressure-sensitive adhesive composition of the present disclosure is a pressure-sensitive adhesive composition comprising a (meth)acrylic copolymer (hereinafter also referred to as a "specific (meth)acrylic copolymer") containing 30% by mass to 70% by mass of structural units derived from a (meth)acrylic acid alkyl ester monomer having a branched alkyl group, relative to all structural units, 10% by mass to 50% by mass of structural units derived from a (meth)acrylic acid alkyl ester monomer having a linear alkyl group having 16 or more carbon atoms, relative to all structural units, and 10% by mass or more of structural units derived from a monomer having a carboxy group, relative to all structural units, and a crosslinking agent. The pressure-sensitive adhesive composition of the present disclosure can form a pressure-sensitive adhesive layer that exhibits high adhesive strength in a high-temperature environment and also exhibits excellent removability in a room temperature environment after exposure to a high-temperature environment. The reason why the pressure-sensitive adhesive composition of the present disclosure can exhibit such an effect is unclear, but the present inventors speculate as follows, however, the following speculation is not intended to limit the pressure-sensitive adhesive composition of the present disclosure, but is merely an example.

[0016] The pressure-sensitive adhesive composition of the present disclosure comprises a specific (meth)acrylic copolymer containing specific amounts of a structural unit derived from a (meth)acrylic acid alkyl ester monomer, a structural unit derived from a (meth)acrylic acid alkyl ester monomer having a linear alkyl group having 16 or more carbon atoms, and a structural unit derived from a monomer having a carboxy group, and a crosslinking agent. In the pressure-sensitive adhesive composition of the present disclosure, the specific (meth)acrylic copolymer contains a relatively large amount of structural units derived from a monomer having a carboxy group, and therefore the pressure-sensitive adhesive layer formed has high cohesive strength. For this reason, it is believed that the pressure-sensitive adhesive layer formed by the pressure-sensitive adhesive composition of the present disclosure exhibits high adhesive strength even in a high-temperature environment. However, the adhesive layer exposed to a high-temperature environment may have increased adhesive strength over time, and may be difficult to peel off from the adherend after cooling. The (meth)acrylic acid alkyl ester monomer having a linear alkyl group with 16 or more carbon atoms, which is a structural unit of a specific (meth)acrylic copolymer, is a monomer called a crystalline monomer. The crystalline monomer crystallizes when the temperature is lower than the melting point. Since the adhesive composition of the present disclosure contains a structural unit derived from the (meth)acrylic acid alkyl ester monomer having a linear alkyl group with 16 or more carbon atoms, which is a crystalline monomer, at a specific ratio or more, it is presumed that the adhesive strength of the formed adhesive layer decreases due to crystallization of the crystalline monomer when cooled to room temperature after being exposed to a high-temperature environment. For this reason, it is considered that the adhesive layer formed by the adhesive composition of the present disclosure can be easily peeled off when peeled off from the adherend in a room temperature environment after being exposed to a high-temperature environment. In addition, the pressure-sensitive adhesive layer exposed to a high-temperature environment may transfer to the surface of the adherend and contaminate the adherend when peeled off from the adherend after cooling. The pressure-sensitive adhesive composition of the present disclosure contains a specific range of structural units derived from a (meth)acrylic acid alkyl ester monomer having a branched alkyl group in the (meth)acrylic copolymer, and therefore the formed pressure-sensitive adhesive layer is considered to have high cohesive strength due to strong entanglement between molecular chains. Furthermore, the pressure-sensitive adhesive composition of the present disclosure contains a specific ratio or less of structural units derived from a (meth)acrylic acid alkyl ester monomer having a linear alkyl group having 16 or more carbon atoms, which is a crystalline monomer, and therefore the formed pressure-sensitive adhesive layer is considered not to be excessively wetted by the adherend when exposed to a high-temperature environment. Therefore, the pressure-sensitive adhesive layer formed by the pressure-sensitive adhesive composition of the present disclosure is considered to be less likely to leave adhesive residue on the surface of the adherend when peeled off from the adherend in a normal temperature environment after being exposed to a high-temperature environment. From the above, it is presumed that the pressure-sensitive adhesive composition of the present disclosure can form a pressure-sensitive adhesive layer that exhibits excellent removability in a room temperature environment after being exposed to a high-temperature environment.

[0017] In contrast to the adhesive composition of the present disclosure, the adhesive described in Patent Document 1 (JP 2016-196544 A; hereinafter the same) and the adhesive described in Patent Document 2 (JP 2008-179744 A; hereinafter the same) do not pay any attention to adhesive residue that may occur when the adhesive layer is peeled off from the adherend in a room temperature environment after being exposed to a high temperature environment. In addition, the adhesive described in Patent Document 1 and the adhesive described in Patent Document 2 contain structural units derived from an acrylic acid alkyl ester monomer having a linear alkyl group having 16 or more carbon atoms, but do not contain structural units derived from a (meth)acrylic acid alkyl ester monomer having a branched alkyl group, so that the adhesive layer formed is likely to cause adhesive residue on the surface of the adherend when peeled off from the adherend in a room temperature environment after being exposed to a high temperature environment.

[0018] [Specific (meth)acrylic copolymer] The pressure-sensitive adhesive composition of the present disclosure comprises a (meth)acrylic copolymer [i.e., a specific (meth)acrylic copolymer] including 30% by mass to 70% by mass of structural units derived from a (meth)acrylic acid alkyl ester monomer having a branched alkyl group, relative to all structural units, 10% by mass to 50% by mass of structural units derived from a (meth)acrylic acid alkyl ester monomer having a linear alkyl group having 16 or more carbon atoms, relative to all structural units, and 10% by mass or more of structural units derived from a monomer having a carboxy group, relative to all structural units.

[0019] <Structural Unit Derived from (Meth)acrylic Acid Alkyl Ester Monomer Having a Branched Alkyl Group> The specific (meth)acrylic copolymer contains 30% by mass to 70% by mass of structural units derived from a (meth)acrylic acid alkyl ester monomer having a branched alkyl group, based on the total structural units.

[0020] In the present disclosure, a "structural unit derived from a (meth)acrylic acid alkyl ester monomer having a branched alkyl group" means a structural unit formed by addition polymerization of a (meth)acrylic acid alkyl ester monomer having a branched alkyl group. The "(meth)acrylic acid alkyl ester monomer having a branched alkyl group" in the present disclosure does not include a monomer that corresponds to a monomer having a carboxy group, which will be described later.

[0021] The type of the (meth)acrylic acid alkyl ester monomer having a branched alkyl group is not particularly limited. The (meth)acrylic acid alkyl ester monomer having a branched alkyl group is preferably unsubstituted. The number of carbon atoms in the branched alkyl group is not particularly limited. The branched alkyl group preferably has 4 or more carbon atoms, more preferably 6 or more carbon atoms, and further preferably 8 or more carbon atoms. Moreover, the number of carbon atoms in the branched alkyl group is preferably 26 or less, for example, from the viewpoint of production suitability.

[0022] Specific examples of (meth)acrylic acid alkyl ester monomers having a branched alkyl group include i-butyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, i-pentyl (meth)acrylate (also known as isoamyl (meth)acrylate), 2-ethylhexyl (meth)acrylate, i-decyl (meth)acrylate, i-octyl (meth)acrylate, i-nonyl (meth)acrylate, i-octadecyl (meth)acrylate, and 2-decyltetradecanyl (meth)acrylate. The (meth)acrylic acid alkyl ester monomer having a branched alkyl group is preferably at least one selected from the group consisting of i-pentyl (meth)acrylate [i.e., isoamyl (meth)acrylate], 2-ethylhexyl (meth)acrylate, and i-decyl (meth)acrylate, more preferably at least one selected from the group consisting of i-pentyl acrylate (i.e., isoamyl acrylate), 2-ethylhexyl methacrylate, and i-decyl methacrylate, and further preferably 2-ethylhexyl methacrylate.

[0023] The specific (meth)acrylic copolymer may contain only one type of structural unit derived from a (meth)acrylic acid alkyl ester monomer having a branched alkyl group, or may contain two or more types.

[0024] The content of the structural units derived from the (meth)acrylic acid alkyl ester monomer having a branched alkyl group in the specific (meth)acrylic copolymer is 30% by mass to 70% by mass based on the total structural units of the specific (meth)acrylic copolymer. When the content of the structural unit derived from the (meth)acrylic acid alkyl ester monomer having a branched alkyl group in the specific (meth)acrylic copolymer is 30% by mass or more relative to the total structural units of the specific (meth)acrylic copolymer, the pressure-sensitive adhesive layer formed tends to be less likely to leave adhesive residue on the surface of the adherend when peeled off from the adherend in a room temperature environment after being exposed to a high temperature environment. From this viewpoint, the content of the structural unit derived from the (meth)acrylic acid alkyl ester monomer having a branched alkyl group in the specific (meth)acrylic copolymer is 30% by mass or more, preferably 35% by mass or more, more preferably 40% by mass or more, and even more preferably 45% by mass or more relative to the total structural units of the specific (meth)acrylic copolymer. When the content of the structural unit derived from the (meth)acrylic acid alkyl ester monomer having a branched alkyl group in the specific (meth)acrylic copolymer is 70% by mass or less based on the total structural units of the specific (meth)acrylic copolymer, the pressure-sensitive adhesive layer formed tends to show high adhesive strength in a high-temperature environment. From this viewpoint, the content of the structural unit derived from the (meth)acrylic acid alkyl ester monomer having a branched alkyl group in the specific (meth)acrylic copolymer is 70% by mass or less based on the total structural units of the specific (meth)acrylic copolymer, preferably 65% ​​by mass or less, more preferably 60% by mass or less, and even more preferably 55% by mass or less.

[0025] The content of constituent units derived from (meth)acrylic acid alkyl ester monomers having a branched alkyl group in the specific (meth)acrylic copolymer is preferably higher than the content of constituent units derived from (meth)acrylic acid alkyl ester monomers having a linear alkyl group having 16 or more carbon atoms in the specific (meth)acrylic copolymer. According to such an embodiment, the pressure-sensitive adhesive layer formed tends to be less likely to leave adhesive residue on the surface of the adherend when peeled from the adherend in a normal temperature environment after being exposed to a high temperature environment.

[0026] <Structural Unit Derived from a (Meth)acrylic Acid Alkyl Ester Monomer Having a Linear Alkyl Group Having 16 or More Carbon Atoms> The specific (meth)acrylic copolymer contains 10% by mass to 50% by mass of structural units derived from (meth)acrylic acid alkyl ester monomers having a linear alkyl group having 16 or more carbon atoms, based on the total structural units.

[0027] In the present disclosure, "a structural unit derived from a (meth)acrylic acid alkyl ester monomer having a linear alkyl group having 16 or more carbon atoms" means a structural unit formed by addition polymerization of a (meth)acrylic acid alkyl ester monomer having a linear alkyl group having 16 or more carbon atoms. In the present disclosure, the "(meth)acrylic acid alkyl ester monomer having a linear alkyl group having 16 or more carbon atoms" does not include a monomer that corresponds to a monomer having a carboxy group, which will be described later.

[0028] The type of (meth)acrylic acid alkyl ester monomer having a linear alkyl group having 16 or more carbon atoms is not particularly limited. The (meth)acrylic acid alkyl ester monomer having a linear alkyl group having 16 or more carbon atoms is preferably unsubstituted. The linear alkyl group has 16 or more carbon atoms, and preferably 18 or more carbon atoms. The upper limit of the number of carbon atoms in the linear alkyl group is not particularly limited, but from the viewpoint of production suitability, for example, it is preferably 22 or less.

[0029] Specific examples of (meth)acrylic acid alkyl ester monomers having a linear alkyl group having 16 or more carbon atoms include hexadecyl (meth)acrylate, octadecyl (meth)acrylate (also known as stearyl (meth)acrylate), eicosyl (meth)acrylate, and docosyl (meth)acrylate (also known as behenyl (meth)acrylate). As the (meth)acrylic acid alkyl ester monomer having a linear alkyl group having 16 or more carbon atoms, at least one selected from the group consisting of octadecyl (meth)acrylate [i.e., stearyl (meth)acrylate] and docosyl (meth)acrylate [i.e., behenyl (meth)acrylate] is preferred, and octadecyl methacrylate (i.e., stearyl methacrylate) is more preferred.

[0030] The specific (meth)acrylic copolymer may contain only one type of structural unit derived from a (meth)acrylic acid alkyl ester monomer having a linear alkyl group having 16 or more carbon atoms, or may contain two or more types of structural units derived from a (meth)acrylic acid alkyl ester monomer having 16 or more carbon atoms.

[0031] The content of the structural units derived from the (meth)acrylic acid alkyl ester monomer having a linear alkyl group having 16 or more carbon atoms in the specific (meth)acrylic copolymer is 10% by mass to 50% by mass based on the total structural units of the specific (meth)acrylic copolymer. When the content of the structural unit derived from the (meth)acrylic acid alkyl ester monomer having a linear alkyl group having 16 or more carbon atoms in the specific (meth)acrylic copolymer is 10% by mass or more relative to the total structural units of the specific (meth)acrylic copolymer, the pressure-sensitive adhesive layer formed tends to be easily peeled off when peeled off from the adherend in a room temperature environment after being exposed to a high temperature environment. From this viewpoint, the content of the structural unit derived from the (meth)acrylic acid alkyl ester monomer having a linear alkyl group having 16 or more carbon atoms in the specific (meth)acrylic copolymer is 10% by mass or more, preferably 15% by mass or more, more preferably 20% by mass or more, and even more preferably 25% by mass or more relative to the total structural units of the specific (meth)acrylic copolymer. When the content of the structural unit derived from the (meth)acrylic acid alkyl ester monomer having a linear alkyl group having 16 or more carbon atoms in the specific (meth)acrylic copolymer is 50% by mass or less relative to the total structural units of the specific (meth)acrylic copolymer, the pressure-sensitive adhesive layer formed tends to be less likely to leave adhesive residue on the surface of the adherend when peeled off from the adherend in a room temperature environment after being exposed to a high temperature environment. From this viewpoint, the content of the structural unit derived from the (meth)acrylic acid alkyl ester monomer having a linear alkyl group having 16 or more carbon atoms in the specific (meth)acrylic copolymer is 50% by mass or less, preferably 45% by mass or less, more preferably 40% by mass or less, and even more preferably 35% by mass or less relative to the total structural units of the specific (meth)acrylic copolymer.

[0032] <Structural Unit Derived from Monomer Having a Carboxy Group> The specific (meth)acrylic copolymer contains 10% by mass or more of structural units derived from a monomer having a carboxy group based on the total structural units. The carboxy group of the structural unit derived from a monomer having a carboxy group can contribute to crosslinking with a crosslinking agent described below.

[0033] In the present disclosure, a "structural unit derived from a monomer having a carboxy group" refers to a structural unit formed by addition polymerization of a monomer having a carboxy group.

[0034] The type of the monomer having a carboxy group is not particularly limited. An example of a monomer having a carboxy group is a monomer having at least one carboxy group and an ethylenically unsaturated group in one molecule. The ethylenically unsaturated group is not particularly limited. Specific examples of the ethylenically unsaturated group include a vinyl group, an allyl group, a vinylphenyl group, a (meth)acrylamide group, and a (meth)acryloyl group. The ethylenically unsaturated group is preferably a (meth)acryloyl group.

[0035] Specific examples of monomers having a carboxy group include acrylic acid, methacrylic acid, crotonic acid, maleic anhydride, fumaric acid, itaconic acid, glutaconic acid, citraconic acid, ω-carboxy-polycaprolactone mono(meth)acrylate [e.g., ω-carboxy-polycaprolactone (n≒2) monoacrylate], succinic acid esters (e.g., 2-acryloyloxyethyl-succinic acid), vinyl formate, vinyl acetate, vinyl propionate, and vinyl neodecanoate. A preferred example of the monomer having a carboxy group is acrylic acid.

[0036] The specific (meth)acrylic copolymer may contain only one type of structural unit derived from a monomer having a carboxy group, or may contain two or more types.

[0037] The content of the structural units derived from the monomer having a carboxy group in the specific (meth)acrylic copolymer is 10% by mass or more based on the total structural units of the specific (meth)acrylic copolymer. When the content of the structural unit derived from the monomer having a carboxyl group in the specific (meth)acrylic copolymer is 10% by mass or more based on the total structural units of the specific (meth)acrylic copolymer, the pressure-sensitive adhesive layer formed tends to show high adhesive strength in a high-temperature environment. From this viewpoint, the content of the structural unit derived from the monomer having a carboxyl group in the specific (meth)acrylic copolymer is 10% by mass or more based on the total structural units of the specific (meth)acrylic copolymer, preferably 15% by mass or more, more preferably 20% by mass or more. The upper limit of the content of the structural units derived from monomers having a carboxy group in the specific (meth)acrylic copolymer is not particularly limited, but from the viewpoint of pot life, for example, it is preferably 40 mass% or less with respect to the total structural units of the specific (meth)acrylic copolymer.

[0038] <Other structural units derived from (meth)acrylic acid alkyl ester monomers> The specific (meth)acrylic copolymer may contain a constituent unit derived from a (meth)acrylic acid alkyl ester monomer other than a (meth)acrylic acid alkyl ester monomer having a branched alkyl group and a (meth)acrylic acid alkyl ester monomer having a linear alkyl group having 16 or more carbon atoms (so-called other (meth)acrylic acid alkyl ester monomer). The other structural units derived from alkyl (meth)acrylate monomers can contribute to adjusting the adhesive strength of the pressure-sensitive adhesive layer.

[0039] In the present disclosure, the term "structural units derived from other (meth)acrylic acid alkyl ester monomers" refers to structural units formed by addition polymerization of other (meth)acrylic acid alkyl ester monomers. The "other (meth)acrylic acid alkyl ester monomers" in the present disclosure do not include monomers that fall under the above-mentioned monomers having a carboxy group.

[0040] The type of the other (meth)acrylic acid alkyl ester monomer is not particularly limited. Specific examples of other (meth)acrylic acid alkyl ester monomers include methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, n-octyl (meth)acrylate, n-nonyl (meth)acrylate, n-decyl (meth)acrylate, n-dodecyl (meth)acrylate, cyclohexyl (meth)acrylate, and isobornyl (meth)acrylate. As the other (meth)acrylic acid alkyl ester monomer, for example, methyl acrylate is preferable.

[0041] When the specific (meth)acrylic copolymer contains a structural unit derived from another (meth)acrylic acid alkyl ester monomer, the specific (meth)acrylic copolymer may contain only one type of structural unit derived from the other (meth)acrylic acid alkyl ester monomer, or may contain two or more types of structural units derived from the other (meth)acrylic acid alkyl ester monomer.

[0042] When the specific (meth)acrylic copolymer contains a constituent unit derived from another (meth)acrylic acid alkyl ester monomer, the content of the constituent unit derived from the other (meth)acrylic acid alkyl ester monomer in the specific (meth)acrylic copolymer is not particularly limited, and can be appropriately set depending on the purpose within a range that does not impair the effects of the pressure-sensitive adhesive composition of the present disclosure.

[0043] <Other building blocks> The specific (meth)acrylic copolymer may contain structural units (so-called other structural units) other than the structural units already described, i.e., the essential structural units, i.e., structural units derived from a (meth)acrylic acid alkyl ester monomer having a branched alkyl group, structural units derived from a (meth)acrylic acid alkyl ester monomer having a linear alkyl group having 16 or more carbon atoms, and structural units derived from a monomer having a carboxy group, as well as optional structural units derived from other (meth)acrylic acid alkyl ester monomers, within the scope of not impairing the effects of the pressure-sensitive adhesive composition of the present disclosure.

[0044] Examples of monomers constituting other structural units include aromatic ring-containing (meth)acrylates such as benzyl (meth)acrylate and phenoxyethyl (meth)acrylate, alkoxyalkyl (meth)acrylates such as methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate, aromatic monovinyls such as styrene, α-methylstyrene, t-butylstyrene, p-chlorostyrene, chloromethylstyrene, and vinyltoluene, vinyl cyanides such as acrylonitrile and methacrylonitrile, and vinyl esters such as vinyl formate, vinyl acetate, vinyl propionate, and vinyl versatate. Also included are various derivatives of these monomers.

[0045] When the specific (meth)acrylic copolymer contains other structural units, it may contain only one type of other structural unit, or may contain two or more types of other structural units.

[0046] When the specific (meth)acrylic copolymer contains other structural units, the content of the other structural units in the specific (meth)acrylic copolymer is not particularly limited and can be appropriately set depending on the purpose within a range that does not impair the effects of the pressure-sensitive adhesive composition of the present disclosure.

[0047] <<Glass transition temperature of specific (meth)acrylic copolymer>> The glass transition temperature (also referred to as "Tg") of the specific (meth)acrylic copolymer is not particularly limited, but is, for example, preferably 25°C to 100°C, more preferably 30°C to 90°C, even more preferably 35°C to 80°C, and particularly preferably 40°C to 70°C. When the glass transition temperature of the specific (meth)acrylic copolymer is 25° C. or higher, the pressure-sensitive adhesive layer formed tends to exhibit higher adhesive strength in a high-temperature environment. When the glass transition temperature of the specific (meth)acrylic copolymer is 100°C or lower, the pressure-sensitive adhesive layer formed tends to be less likely to leave adhesive residue on the surface of the adherend when it is peeled off from the adherend in a room temperature environment after being exposed to a high-temperature environment.

[0048] The glass transition temperature of the specific (meth)acrylic copolymer is a value obtained by converting the absolute temperature (unit: K; the same applies below) calculated from the following formula 1 into Celsius temperature (unit: °C; the same applies below). 1 / Tg=m1 / Tg1+m2 / Tg2+ +m(k-1) / Tg(k-1)+mk / Tgk (Formula 1)

[0049] In formula 1, Tg1, Tg2, . . . , Tg(k-1), and Tgk each represent a glass transition temperature, expressed as an absolute temperature, when each monomer constituting the specific (meth)acrylic copolymer is made into a homopolymer. In formula 1, m1, m2, , m(k-1), and mk represent the molar fractions of the monomers constituting the specific (meth)acrylic copolymer, respectively, and m1 + m2 + ⋅ ⋅ + m(k-1) + mk = 1. Note that absolute temperatures can be converted to Celsius temperatures by subtracting 273 from the absolute temperature, and Celsius temperatures can be converted to absolute temperatures by adding 273 to the Celsius temperature.

[0050] In the present disclosure, the "glass transition temperature expressed as absolute temperature when made into a homopolymer" refers to the glass transition temperature expressed as absolute temperature of a homopolymer produced by polymerizing the monomer alone. The glass transition temperature of the homopolymer was measured using a differential scanning calorimeter (DSC) [model: EXSTAR6000, manufactured by Seiko Instruments Inc.] under conditions of a nitrogen gas flow, a measurement sample of 10 mg, and a heating rate of 10°C / min, and the inflection point of the obtained DSC curve was taken as the glass transition temperature of the homopolymer.

[0051] The glass transition temperatures of representative monomers, expressed in Celsius degrees when made into homopolymers, are -76°C for 2-ethylhexyl acrylate (2EHA), -10°C for 2-ethylhexyl methacrylate (2EHMA), -57°C for n-butyl acrylate (n-BA), 21°C for n-butyl methacrylate (n-BMA), 41°C for t-butyl acrylate (t-BA), and 42°C for t-butyl methacrylate (t-BMA). MA) at 107°C, i-butyl methacrylate (i-BMA) at 48°C, methyl acrylate (MA) at 5°C, methyl methacrylate (MMA) at 103°C, isobornyl methacrylate (IBXMA) at 155°C, isobornyl acrylate (IBXA) at 96°C, ethyl acrylate (EA) at -27°C, methacrylic acid (MAA) at 185°C, 4-hydroxybutyl acrylate (4HBA) at -39°C, 2 -Hydroxyethyl acrylate (2HEA) at -15°C, 2-hydroxyethyl methacrylate (2HEMA) at 55°C, 2-hydroxypropyl acrylate (2HPA) at -7°C, acrylic acid (AA) at 163°C, n-octyl acrylate (n-OA) at -65°C, i-octyl acrylate (i-OA) at -75°C, i-decyl acrylate at -62°C, and i-decyl methacrylate (IDMA) at -75°C. The temperatures are −41°C, i-amyl acrylate (IAA) at −45°C, stearyl acrylate (STA) at 30°C, stearyl methacrylate (STMA) at 38°C, behenyl methacrylate (VMA) at 47°C, dimethylaminoethyl methacrylate (DM) at 18°C, ω-carboxy-polycaprolactone (n≈2) monoacrylate at −30°C, and 2-acryloyloxyethyl-succinic acid at −40°C.

[0052] The glass transition temperature of the specific (meth)acrylic copolymer can be appropriately adjusted, for example, by using two or more kinds of monomers having different glass transition temperatures when made into homopolymers.

[0053] <<Weight average molecular weight of specific (meth)acrylic copolymer>> The weight average molecular weight (also referred to as "Mw") of the specific (meth)acrylic copolymer is not particularly limited, but is, for example, preferably from 30,000 to 1,000,000, more preferably from 50,000 to 500,000, even more preferably from 100,000 to 400,000, and particularly preferably from 100,000 to 300,000. When the weight-average molecular weight of the specific (meth)acrylic copolymer is 30,000 or more, the pressure-sensitive adhesive layer formed tends to be less likely to leave adhesive residue on the surface of the adherend when it is peeled off from the adherend in a room temperature environment after being exposed to a high-temperature environment. When the weight average molecular weight of the specific (meth)acrylic copolymer is 1,000,000 or less, the pressure-sensitive adhesive layer formed tends to exhibit higher adhesive strength in a high-temperature environment.

[0054] The weight average molecular weight of the specific (meth)acrylic copolymer is a value measured by the following method, specifically, according to the following (1) to (3). (1) A solution of the specific (meth)acrylic copolymer is applied to a release paper and dried at 100° C. for 1 minute to obtain a film of the specific (meth)acrylic copolymer. (2) Using the film-like specific (meth)acrylic copolymer obtained in (1) above and tetrahydrofuran, a sample solution having a solid content concentration of 0.2% by mass is obtained. Note that the "solid content concentration" here means the mass ratio of the specific (meth)acrylic copolymer in the sample solution. (3) Using gel permeation chromatography (GPC), the weight average molecular weight of the specific (meth)acrylic copolymer is measured in terms of standard polystyrene under the following conditions.

[0055] ~Conditions~ Measurement equipment: High-speed GPC [Model: HLC-8220 GPC, manufactured by Tosoh Corporation] Detector: Differential refractometer (RI) [installed in HLC-8220, manufactured by Tosoh Corporation] Column: TSKgel GMH XL Four Tosoh Corporation-made Column temperature: 40℃ Eluent: Tetrahydrofuran Sample solution injection volume: 100 μL Flow rate: 0.8mL / min

[0056] The weight average molecular weight of the specific (meth)acrylic copolymer can be adjusted to a desired value by adjusting the polymerization temperature, polymerization time, amount of organic solvent used, type of polymerization initiator, amount of polymerization initiator used, and the like.

[0057] <<Content of specific (meth)acrylic copolymer>> The content of the specific (meth)acrylic copolymer in the pressure-sensitive adhesive composition of the present disclosure is not particularly limited, but for example, it is preferably 75% by mass to 99.99% by mass, more preferably 80% by mass to 99.95% by mass, even more preferably 85% by mass to 99.9% by mass, and particularly preferably 90% by mass to 99.9% by mass, relative to the total solid content in the pressure-sensitive adhesive composition. In the present disclosure, the "total solid content in the PSA composition" means the total mass of the PSA composition when the PSA composition does not contain a solvent, and means the mass of the residue remaining after removing the solvent from the PSA composition when the PSA composition contains a solvent. In this disclosure, "solvent" means water and organic solvents.

[0058] [Method for producing specific (meth)acrylic copolymer] The method for producing the specific (meth)acrylic copolymer is not particularly limited. The specific (meth)acrylic copolymer can be produced by polymerizing the above-mentioned monomers by a known polymerization method typified by, for example, a solution polymerization method, an emulsion polymerization method, a suspension polymerization method, or a bulk polymerization method. As a polymerization method, a solution polymerization method is preferred in that the processing steps are relatively simple and can be carried out in a short time when preparing the pressure-sensitive adhesive composition of the present disclosure after production.

[0059] In the solution polymerization method, a predetermined organic solvent, a monomer, a polymerization initiator, and a chain transfer agent used as required are generally charged into a polymerization tank, and the mixture is heated and reacted for several hours with stirring at the reflux temperature of the organic solvent. In this case, at least a part of the organic solvent, the monomer, the polymerization initiator, and the chain transfer agent used as required may be added successively. The reaction may also be carried out in a nitrogen gas flow.

[0060] Examples of the organic solvent used in the polymerization reaction include aromatic hydrocarbon compounds, aliphatic hydrocarbon compounds, alicyclic hydrocarbon compounds, ester compounds, ketone compounds, glycol ether compounds, and alcohol compounds. More specifically, examples of the organic solvent used in the polymerization reaction include aromatic hydrocarbon compounds such as benzene, toluene, ethylbenzene, n-propylbenzene, t-butylbenzene, o-xylene, m-xylene, p-xylene, tetralin, decalin, and aromatic naphtha; aliphatic or alicyclic hydrocarbon compounds such as n-hexane, n-heptane, n-octane, i-octane, n-decane, dipentene, petroleum spirit, petroleum naphtha, and turpentine oil; ester compounds such as ethyl acetate, n-butyl acetate, n-amyl acetate, 2-hydroxyethyl acetate, 2-butoxyethyl acetate, 3-methoxybutyl acetate, and methyl benzoate; acetone, methyl ethyl acetate, and the like. Examples of the alcohol compounds include ketones, ketone compounds represented by methyl-i-butyl ketone, isophorone, cyclohexanone, and methylcyclohexanone, glycol ether compounds represented by ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, and diethylene glycol monobutyl ether, and alcohol compounds represented by methyl alcohol, ethyl alcohol, n-propyl alcohol, i-propyl alcohol, n-butyl alcohol, i-butyl alcohol, s-butyl alcohol, and t-butyl alcohol.

[0061] In producing the specific (meth)acrylic copolymer, it is preferable to use an organic solvent that is unlikely to cause chain transfer during the polymerization reaction, such as an aromatic hydrocarbon compound, an ester compound, or a ketone compound. In particular, it is preferable to use ethyl acetate from the viewpoints of the solubility of the specific (meth)acrylic copolymer, the ease of the polymerization reaction, and the like.

[0062] During the polymerization reaction, only one type of organic solvent may be used, or two or more types may be used.

[0063] Examples of the polymerization initiator include organic peroxides and azo compounds that are used in ordinary solution polymerization methods. Specific examples of organic peroxides include t-butyl hydroperoxide, cumene hydroperoxide, dicumyl peroxide, benzoyl peroxide, lauroyl peroxide, caproyl peroxide, di-i-propyl peroxydicarbonate, di-2-ethylhexyl peroxydicarbonate, t-butyl peroxypivalate, 2,2-bis(4,4-di-t-butylperoxycyclohexyl)propane, 2,2-bis(4,4-di-t-amylperoxycyclohexyl)propane, 2,2-bis(4,4-di-t-octylperoxycyclohexyl)propane, 2,2-bis(4,4-di-α-cumylperoxycyclohexyl)propane, 2,2-bis(4,4-di-t-butylperoxycyclohexyl)butane, and 2,2-bis(4,4-di-t-octylperoxycyclohexyl)butane. Specific examples of azo compounds include 2,2'-azobisisobutyronitrile (AIBN), 2,2'-azobis(2,4-dimethylvaleronitrile) (ABVN), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 1,1'-azobis(cyclohexane-1-carbonitrile), and 2,2'-azobis(isobutyrate) dimethyl. In producing the specific (meth)acrylic copolymer, it is preferable to use a polymerization initiator that does not cause a graft reaction during the polymerization reaction, and it is particularly preferable to use an azo compound.

[0064] In the polymerization reaction, only one type of polymerization initiator may be used, or two or more types may be used.

[0065] The amount of the polymerization initiator used is not particularly limited, and can be appropriately set depending on, for example, the molecular weight of the target specific (meth)acrylic copolymer.

[0066] In producing the specific (meth)acrylic copolymer, a chain transfer agent may be used, if necessary. Examples of the chain transfer agent include cyanoacetic acid, alkyl ester compounds of cyanoacetic acid having 1 to 8 carbon atoms, bromoacetic acid, alkyl ester compounds of bromoacetic acid having 1 to 8 carbon atoms, aromatic compounds such as α-methylstyrene, anthracene, phenanthrene, fluorene, and 9-phenylfluorene, aromatic nitro compounds such as p-nitroaniline, nitrobenzene, dinitrobenzene, p-nitrobenzoic acid, p-nitrophenol, and p-nitrotoluene, benzoquinone derivatives such as benzoquinone and 2,3,5,6-tetramethyl-p-benzoquinone, borane derivatives such as tributylborane, carbon tetrabromide, ... Examples of the halogenated hydrocarbon compounds include carbon chloride, 1,1,2,2-tetrabromoethane, tribromoethylene, trichloroethylene, bromotrichloromethane, tribromomethane, and 3-chloro-1-propene, aldehyde compounds such as chloral and furaldehyde, alkyl mercaptan compounds having 1 to 18 carbon atoms, aromatic mercaptan compounds such as thiophenol and toluene mercaptan, mercaptoacetic acid, alkyl ester compounds of mercaptoacetic acid having 1 to 10 carbon atoms, hydroxyalkyl mercaptan compounds having 1 to 12 carbon atoms, and terpene compounds such as pinene and terpinolene.

[0067] When a chain transfer agent is used in producing the specific (meth)acrylic copolymer, the amount of the chain transfer agent used is not particularly limited and can be appropriately set depending on, for example, the molecular weight of the target specific (meth)acrylic copolymer.

[0068] The polymerization temperature is not particularly limited, and can be appropriately set depending on, for example, the molecular weight of the target specific (meth)acrylic copolymer.

[0069] [Crosslinking Agent] The pressure-sensitive adhesive composition of the present disclosure contains a crosslinking agent. The type of crosslinking agent is not particularly limited. Examples of the crosslinking agent include an epoxy-based crosslinking agent, an isocyanate-based crosslinking agent, a metal chelate-based crosslinking agent, and an aziridine-based crosslinking agent. The crosslinking agent is preferably at least one type of crosslinking agent selected from the group consisting of, for example, epoxy-based crosslinking agents, isocyanate-based crosslinking agents, and metal chelate-based crosslinking agents, and more preferably an epoxy-based crosslinking agent.

[0070] In this disclosure, the term "epoxy-based crosslinking agent" refers to a compound having two or more epoxy groups in one molecule (so-called bifunctional or higher epoxy compound). The term "isocyanate-based crosslinking agent" refers to a compound having two or more isocyanate groups in one molecule (so-called polyisocyanate compound). The term "metal chelate-based crosslinking agent" refers to a metal chelate compound that functions as a crosslinking agent. The term "aziridine-based crosslinking agent" refers to a compound having two or more aziridine groups in one molecule (so-called bifunctional or higher aziridine compound).

[0071] The type of the epoxy crosslinking agent is not particularly limited. Specific examples of epoxy crosslinking agents include ethylene glycol diglycidyl ether, diethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, tripropylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, neopentyl glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, polytetramethylene glycol diglycidyl ether, glycerol diglycidyl ether, glycerol triglycidyl ether, diglycerol polyglycidyl ether, polyglycerol di ... Examples of such glycidyl ethers include glycerol polyglycidyl ether, resorcinol diglycidyl ether, 2,2-dibromoneopentyl glycol diglycidyl ether, trimethylolpropane triglycidyl ether, pentaerythritol polyglycidyl ether, sorbitol polyglycidyl ether, adipic acid diglycidyl ester, phthalic acid diglycidyl ester, tris(glycidyl)isocyanurate, tris(glycidoxyethyl)isocyanurate, 1,3-bis(N,N-glycidylaminomethyl)cyclohexane, and N,N,N',N'-tetraglycidyl-1,3-benzenedi(methanamine).

[0072] As the epoxy-based crosslinking agent, a commercially available product can be used. Examples of commercially available epoxy crosslinking agents include "TETRAD (registered trademark)-X" and "TETRAD (registered trademark)-C" (both manufactured by Mitsubishi Gas Chemical Company, Inc.).

[0073] The type of the isocyanate-based crosslinking agent is not particularly limited. Examples of the isocyanate crosslinking agent include aromatic polyisocyanate compounds such as xylylene diisocyanate (XDI), diphenylmethane diisocyanate, triphenylmethane triisocyanate, and tolylene diisocyanate (TDI), and aliphatic polyisocyanate compounds or alicyclic polyisocyanate compounds such as hexamethylene diisocyanate (HMDI), pentamethylene diisocyanate (PDI), isophorone diisocyanate, and hydrogenated aromatic polyisocyanate compounds. Further, examples of the isocyanate-based crosslinking agent include dimers, trimers, and pentamers of the above polyisocyanate compounds, adducts of the above polyisocyanate compounds with polyol compounds such as trimethylolpropane, and biuret forms of the above polyisocyanate compounds.

[0074] As the isocyanate-based crosslinking agent, a commercially available product can be used. Examples of commercially available isocyanate crosslinking agents include "Coronate (registered trademark) HX", "Coronate (registered trademark) HL-S", "Coronate (registered trademark) L", "Coronate (registered trademark) L-45E", "Coronate (registered trademark) 2031", "Coronate (registered trademark) 2037", "Coronate (registered trademark) 2234", "Coronate (registered trademark) 2785", "Aquanate (registered trademark) 200", and "Aquanate (registered trademark) 210" (all manufactured by Tosoh Corporation), "Sumidur (registered trademark) N3300", "Desmodur (registered trademark) N3400", and "Sumidur (registered trademark) N75" (all manufactured by Sumika Covestro Urethane Co., Ltd.), "Duranate (registered trademark) E-405-80T", "Duranate (registered trademark) AE700-100", "Duranate (registered trademark) Examples of such polyurethane foams include "Duranate (registered trademark) 24A-100" and "Duranate (registered trademark) TSE-100" (all manufactured by Asahi Kasei Corporation), as well as "Takenate (registered trademark) D-110N", "Takenate (registered trademark) D-120N", "Takenate (registered trademark) M-631N", "MT-Olestar (registered trademark) NP1200", and "STABIO (registered trademark) XD-340N" (all manufactured by Mitsui Chemicals, Inc.).

[0075] The type of the metal chelate crosslinking agent is not particularly limited. Examples of metal chelate crosslinking agents include aluminum chelate compounds, titanium chelate compounds, zirconium chelate compounds, and cobalt chelate compounds. As the metal chelate crosslinking agent, an aluminum chelate compound is preferred. Specific examples of aluminum chelate compounds include aluminum monoacetylacetonate bis(ethylacetoacetate), aluminum tris(ethylacetoacetate), and aluminum tris(acetylacetonate).

[0076] As the metal chelate crosslinking agent, commercially available products can be used. Examples of commercially available metal chelate crosslinking agents include Aluminum Chelate A (trade name: aluminum tris(acetylacetonate), manufactured by Kawaken Fine Chemicals Co., Ltd.), Aluminum Chelate D (trade name: aluminum monoacetylacetonate bis(ethylacetoacetate), manufactured by Kawaken Fine Chemicals Co., Ltd.), and ALCH-TR (trade name: aluminum tris(ethylacetoacetate), manufactured by Kawaken Fine Chemicals Co., Ltd.).

[0077] The type of the aziridine-based crosslinking agent is not particularly limited. Examples of the aziridine crosslinking agent include trimethylolpropane-tri-β-aziridinylpropionate, tetramethylolmethane-tri-β-aziridinylpropionate, trimethylolpropane-tri-β-(2-methylaziridine)propionate, N,N'-diphenylmethane-4,4'-bis(1-aziridinecarboxamide), N,N'-hexamethylene-1,6-bis(1-aziridinecarboxamide), and N,N'-toluene-2,4-bis(1-aziridinecarboxamide).

[0078] As the aziridine-based crosslinking agent, a commercially available product can be used. An example of a commercially available aziridine-based crosslinking agent is "ChemiTite (registered trademark) PZ-33" (manufactured by Nippon Shokubai Co., Ltd.).

[0079] The pressure-sensitive adhesive composition of the present disclosure may contain only one type of crosslinking agent, or may contain two or more types.

[0080] The content of the crosslinking agent in the pressure-sensitive adhesive composition of the present disclosure is not particularly limited, but for example, it is preferably 0.01 parts by mass to 5 parts by mass, more preferably 0.03 parts by mass to 3 parts by mass, even more preferably 0.05 parts by mass to 2 parts by mass, and particularly preferably 0.1 parts by mass to 1 part by mass, relative to 100 parts by mass of the specific (meth)acrylic copolymer. When the content of the crosslinking agent in the pressure-sensitive adhesive composition of the present disclosure is 0.01 parts by mass or more relative to 100 parts by mass of the specific (meth)acrylic copolymer, the pressure-sensitive adhesive layer formed tends to show higher adhesive strength in a high-temperature environment. Also, when the content of the crosslinking agent in the pressure-sensitive adhesive composition of the present disclosure is 0.01 parts by mass or more relative to 100 parts by mass of the specific (meth)acrylic copolymer, the pressure-sensitive adhesive layer formed tends to be less likely to leave adhesive residue on the surface of the adherend when peeled off from the adherend in a normal temperature environment after being exposed to a high-temperature environment. When the content of the crosslinking agent in the pressure-sensitive adhesive composition of the present disclosure is 5 parts by mass or less relative to 100 parts by mass of the specific (meth)acrylic copolymer, the pressure-sensitive adhesive layer formed tends to exhibit higher adhesive strength in a high-temperature environment.

[0081] [Organic Solvent] The pressure-sensitive adhesive composition of the present disclosure may contain an organic solvent. When the pressure-sensitive adhesive composition of the present disclosure contains an organic solvent, the coatability can be improved. As the organic solvent, for example, the same organic solvent as that used in the polymerization reaction of the specific (meth)acrylic copolymer can be used.

[0082] When the pressure-sensitive adhesive composition of the present disclosure contains an organic solvent, it may contain only one type of organic solvent, or may contain two or more types of organic solvent.

[0083] When the pressure-sensitive adhesive composition of the present disclosure contains an organic solvent, the content of the organic solvent is not particularly limited and can be appropriately set depending on the purpose.

[0084] [Other ingredients] The pressure-sensitive adhesive composition of the present disclosure may contain components other than the components described above (so-called other components) as necessary, provided that the effects of the composition are not impaired. Examples of other components include various additives such as polymers other than the specific (meth)acrylic copolymer, crosslinking catalysts, tackifiers, antioxidants, colorants (e.g., dyes and pigments), light stabilizers (e.g., ultraviolet absorbers), and antistatic agents.

[0085] When the pressure-sensitive adhesive composition of the present disclosure contains other components, the contents of the other components can be appropriately set within a range that does not impair the effects of the pressure-sensitive adhesive composition of the present disclosure.

[0086] <Application> The application of the pressure-sensitive adhesive composition of the present disclosure is not particularly limited. The pressure-sensitive adhesive composition of the present disclosure is capable of forming a pressure-sensitive adhesive layer that exhibits high adhesive strength in a high-temperature environment and also exhibits excellent removability in a room temperature environment after exposure to a high-temperature environment. Therefore, the pressure-sensitive adhesive composition of the present disclosure is suitable as a pressure-sensitive adhesive composition for temporary fixation used in situations where the device is exposed to a high-temperature environment, for example, in the manufacturing process of electronic devices.

[0087] [Adhesive sheet] The pressure-sensitive adhesive sheet of the present disclosure includes a pressure-sensitive adhesive layer formed from the pressure-sensitive adhesive composition of the present disclosure. The adhesive layer of the adhesive sheet of the present disclosure exhibits high adhesive strength in a high-temperature environment and exhibits excellent removability in a room-temperature environment after exposure to a high-temperature environment. Therefore, the adhesive sheet of the present disclosure does not peel off from the adherend or shift from its initial position on the adherend even in a high-temperature environment, and can be easily peeled off when peeled off from the adherend in a room-temperature environment after cooling, and is unlikely to leave adhesive residue on the surface of the adherend.

[0088] The thickness of the pressure-sensitive adhesive layer provided in the pressure-sensitive adhesive sheet of the present disclosure is not particularly limited. The thickness of the pressure-sensitive adhesive layer is generally 1 μm to 100 μm, preferably 3 μm to 50 μm, and more preferably 5 μm to 30 μm.

[0089] In the present disclosure, the "thickness of the pressure-sensitive adhesive layer" means the average thickness of the pressure-sensitive adhesive layer. The average thickness of the pressure-sensitive adhesive layer is a value measured by the following method. The arithmetic mean value of the thicknesses of the adhesive layer measured at 10 randomly selected points in the thickness direction of the adhesive layer is calculated, and the obtained value is regarded as the average thickness of the adhesive layer. The thickness of the adhesive layer is measured using a film thickness meter.

[0090] The pressure-sensitive adhesive sheet of the present disclosure may be a substrate-free pressure-sensitive adhesive sheet that does not have a substrate, or a substrate-containing pressure-sensitive adhesive sheet that has a pressure-sensitive adhesive layer on one or both sides of a substrate. When the adhesive sheet of the present disclosure is a substrate-free adhesive sheet that does not have a substrate, or when it is a substrate-containing adhesive sheet that has an adhesive layer on one side of a substrate, the exposed surface of the adhesive layer in the adhesive sheet of the present disclosure may be protected by a release film.

[0091] The release film is not particularly limited as long as it can be easily peeled off from the pressure-sensitive adhesive layer. For example, the release film may be a resin film having one or both sides surface-treated with a release agent (so-called easy-release treatment). An example of the resin film is a polyester film, typically a polyethylene terephthalate (PET) film. Examples of the release agent include silicone-based release agents (eg, silicone), wax-based release agents (eg, paraffin wax), and fluorine-based release agents (eg, fluorine-based resins). The release film protects the surface of the pressure-sensitive adhesive layer until the pressure-sensitive adhesive sheet is put to practical use, and is peeled off at the time of use.

[0092] When the pressure-sensitive adhesive sheet of the present disclosure includes a substrate, the substrate is not particularly limited as long as a pressure-sensitive adhesive layer can be formed on the substrate. Examples of the substrate include films containing resins such as polyolefin resins (e.g., polyethylene (PE) and polypropylene (PP)), polyester resins (e.g., polyethylene terephthalate (PET)), acetate resins (e.g., triacetyl cellulose resin), polyethersulfone resins, polycarbonate resins, polyamide resins, polyimide resins, acrylic resins, vinyl chloride resins, ABS (Acrylonitrile Butadiene Styrene) resins, and fluorine-based resins.

[0093] The surface of the substrate on which the adhesive layer is provided may be subjected to a surface treatment such as corona discharge treatment or plasma discharge treatment (so-called adhesion enhancing treatment) in order to improve adhesion between the substrate and the adhesive layer.

[0094] The substrate may contain various additives, such as plasticizers, colorants (eg, dyes and pigments), heat stabilizers, light stabilizers, antistatic agents, flame retardants, antioxidants, and the like. The substrate may be partially or entirely patterned.

[0095] The thickness of the substrate is not particularly limited, but is generally 10 μm to 500 μm, preferably 10 μm to 300 μm, more preferably 10 μm to 200 μm, and further preferably 10 μm to 100 μm.

[0096] "Substrate thickness" in this disclosure means the average thickness of the substrate. The average thickness of the substrate is a value measured by a method conforming to the above-mentioned method for measuring the average thickness of the pressure-sensitive adhesive layer.

[0097] [How to make adhesive sheets] The method for producing the pressure-sensitive adhesive sheet of the present disclosure is not particularly limited. The pressure-sensitive adhesive sheet of the present disclosure can be produced by known methods. The pressure-sensitive adhesive sheet of the present disclosure can be produced, for example, by the following method. In the case of a substrate-free type adhesive sheet, first, the adhesive composition of the present disclosure is applied to the easy-release treated surface of a release film to form a coating film on the release film.Then, the formed coating film is dried to form an adhesive film on the release film.Then, the exposed surface of the formed adhesive film is laminated and attached to the easy-release treated surface of a separately prepared release film, and then cured to produce a substrate-free type adhesive sheet having a laminated structure of release film / adhesive layer / release film.

[0098] In the case of a substrate-type adhesive sheet, first, the adhesive composition of the present disclosure is applied to the easy-adhesion treated surface of the substrate to form a coating film on the substrate. Then, the formed coating film is dried to form an adhesive film on the substrate. Then, the exposed surface of the formed adhesive film is laminated on the easy-release treated surface of the release film, and then cured to produce a substrate-type adhesive sheet having a laminated structure of release film / adhesive layer / substrate.

[0099] As another method, for example, the following method can be mentioned. The adhesive composition of the present disclosure is applied to the easy-release treated surface of a release film to form a coating film on the release film. The formed coating film is then dried to form an adhesive film on the release film. The exposed surface of the formed adhesive film is then laminated to the easy-adhesion treated surface of a substrate, and then cured to produce a substrate-type adhesive sheet having a laminated structure of substrate / adhesive layer / release film.

[0100] The method for applying the pressure-sensitive adhesive composition is not particularly limited. Examples of methods for applying the pressure-sensitive adhesive composition include known methods using a gravure roll coater, reverse roll coater, kiss roll coater, dip roll coater, knife coater, spray coater, bar coater, applicator, and the like. The amount of the adhesive composition to be applied is not particularly limited, and is appropriately set depending on, for example, the thickness of the adhesive layer to be formed.

[0101] The method for drying the coating film is not particularly limited. Examples of methods for drying the coating film include natural drying, heat drying, hot air drying, and vacuum drying. The drying temperature and drying time of the coating film are not particularly limited, and are appropriately set depending on the thickness of the coating film, the amount of the organic solvent in the coating film, and the like. An example of the drying conditions is drying using a hot air dryer at 70° C. to 120° C. for 30 to 180 seconds.

[0102] The curing is carried out, for example, for 4 to 7 days in an environment with an atmospheric temperature of 20° C. to 35° C. and a relative humidity of 45% to 55% (ie, 45% RH to 55% RH). EXAMPLES

[0103] The pressure-sensitive adhesive composition and the like of the present disclosure will be described in more detail below with reference to examples. The present disclosure is not limited to the following examples as long as it does not deviate from the gist of the disclosure.

[0104] [Production of (meth)acrylic copolymer] [Manufacturing example A-1] In a reaction vessel equipped with a stirrer and a thermometer, 130 parts by mass of ethyl acetate (organic solvent for polymerization), 50 parts by mass of 2-ethylhexyl methacrylate [2EHMA; (meth)acrylic acid alkyl ester monomer having a branched alkyl group], 30 parts by mass of stearyl methacrylate [STMA; (meth)acrylic acid alkyl ester monomer having a linear alkyl group having 16 or more carbon atoms], 20 parts by mass of acrylic acid [AA; monomer having a carboxy group], and 0.125 parts by mass of 2,2'-azobisisobutyronitrile [AIBN; polymerization initiator] were put and mixed to obtain a mixture. Next, the temperature of the mixture in the reaction vessel was raised to the reflux temperature, and then the mixture was stirred while maintaining the temperature and polymerized for 6 hours to obtain a polymerization reaction product. The obtained polymerization reaction product was diluted with ethyl acetate so that the solid content concentration was 40% by mass, and a solution of (meth)acrylic copolymer A-1 was obtained.

[0105] The term "solid content concentration" used herein means the mass proportion of the (meth)acrylic copolymer A-1 in the solution of the (meth)acrylic copolymer A-1. The same applies to each of the solutions of the following (meth)acrylic copolymers A-2 to A-22.

[0106] [Production Examples A-2 to A-12 and A-16 to A-22] In Production Examples A-2 to A-12 and A-16 to A-22, the monomer composition of the (meth)acrylic copolymer was changed to the monomer composition shown in Table 1, but the same operation as in Production Example A-1 was performed to obtain solutions of (meth)acrylic copolymers A-2 to A-12 and A-16 to A-22 each having a solid content concentration of 40 mass%.

[0107] [Manufacturing examples A-13 to A-15] In Production Examples A-13 to A-15, the same operations as in Production Example A-1 were carried out except that the weight average molecular weight of the (meth)acrylic copolymer was adjusted to the weight average molecular weight shown in Table 1 by adjusting at least one of the amount of the organic solvent used and the amount of the polymerization initiator used, thereby obtaining solutions of (meth)acrylic copolymers A-13 to A-15 each having a solid content concentration of 40 mass%.

[0108] The monomer composition (unit: mass%) of (meth)acrylic copolymers A-1 to A-22, the glass transition temperature (Tg) of (meth)acrylic copolymers A-1 to A-22 (unit: °C), and the weight average molecular weight (Mw) of (meth)acrylic copolymers A-1 to A-22 (unit: 10,000 (in the table, "×10 4 " are shown in Table 1.

[0109] The glass transition temperatures of the (meth)acrylic copolymers A-1 to A-22 were calculated by the same method as the above-mentioned method for calculating the glass transition temperature of a specific (meth)acrylic copolymer. The weight average molecular weights of the (meth)acrylic copolymers A-1 to A-22 were measured by the same method as the above-mentioned method for measuring the weight average molecular weight of the specific (meth)acrylic copolymer.

[0110] Of the (meth)acrylic copolymers A-1 to A-22 obtained above, the (meth)acrylic copolymers A-1 to A-15 correspond to the specific (meth)acrylic copolymer in the present disclosure.

[0111] [Table 1]

[0112] Details of each monomer listed in Table 1 are as follows. <(Meth)acrylic acid alkyl ester monomer having branched alkyl group> 2EHMA: 2-Ethylhexyl methacrylate (number of carbon atoms in the alkyl group: 8) "IDMA"; Isodecyl methacrylate [Number of carbon atoms in alkyl group: 10] "IAA"; Isoamyl acrylate [alkyl group carbon number: 5]

[0113] <(Meth)acrylic acid alkyl ester monomer having a linear alkyl group with 16 or more carbon atoms> "STMA": Stearyl methacrylate [Number of carbon atoms in alkyl group: 18] "VMA"; behenyl methacrylate [alkyl group carbon number: 22] "STA": Stearyl acrylate [number of carbon atoms in alkyl group: 18]

[0114] <Monomers having a carboxy group> "AA": acrylic acid <Other (meth)acrylic acid alkyl ester monomers> "MA": Methyl acrylate

[0115] In Table 1, "-" in the monomer composition column means that the monomer in that column was not used.

[0116] [Preparation of Adhesive Composition] Example 1 100 parts by mass (solid content equivalent) of the solution of (meth)acrylic copolymer A-1 and 0.1 parts by mass (solid content equivalent) of a crosslinking agent [product name: TETRAD (registered trademark)-X, solid content concentration: 100 mass%, epoxy crosslinking agent, manufactured by Mitsubishi Gas Chemical Company, Inc.] were thoroughly mixed to obtain a pressure-sensitive adhesive composition of Example 1.

[0117] [Examples 2 to 20] The same procedure as in Example 1 was carried out except that the composition of the adhesive composition in Example 1 was changed to the composition shown in Table 2, to obtain each of the adhesive compositions of Examples 2 to 20.

[0118] [Comparative Examples 1 to 7] The same procedure as in Example 1 was carried out except that the composition of the adhesive composition in Example 1 was changed to the composition shown in Table 3, to obtain each of the adhesive compositions of Comparative Examples 1 to 7.

[0119] [Preparation of adhesive sheets for evaluation] The adhesive composition prepared above was applied to one side of a polyimide film (trade name: Kapton (registered trademark) 100H, manufactured by Toray DuPont Co., Ltd.) as a substrate so that the thickness after drying was 10 μm, forming a coating film. The formed coating film was then dried using a hot air circulation dryer under drying conditions of a drying temperature of 100° C. and a drying time of 1 minute, forming an adhesive film on the polyimide film. Next, the surface on which the adhesive film was exposed was laminated on the easy-release treated surface of a release film (trade name: Film Vina (registered trademark) 100E-0010 No. 23, thickness: 100 μm, manufactured by Fujimori Kogyo Co., Ltd.) that had been treated for easy peeling with a silicone-based release treatment agent, and then aged for 168 hours in an environment with an atmospheric temperature of 25° C. and 50% RH to promote the crosslinking reaction, thereby preparing an adhesive sheet for evaluation. The prepared adhesive sheet for evaluation has a laminated structure of a substrate (polyimide film) / adhesive layer / release film.

[0120] [Measurement and Evaluation] 1. Adhesion strength in high temperature environments The adhesive sheet for evaluation prepared above was cut into a size of 25 mm × 150 mm to prepare an adhesive sheet piece for evaluation. In addition, a glass plate [product name: soda lime glass (ordinary glass), thickness: 1.8 mm, manufactured by Kawamura Kyuzo Shoten Co., Ltd.] was prepared as an adherend. The release film was peeled off from the adhesive sheet piece for evaluation, and the surface of the adhesive layer exposed by peeling was laminated on one side of a glass plate, and then a 2 kg roller was moved back and forth once to press and bond the two pieces together to prepare a test piece. The prepared test piece has a laminated structure of adherend (glass plate) / adhesive sheet piece for evaluation [adhesive layer / substrate (polyimide film)]. Next, the prepared test piece was left to stand for 30 minutes in an environment with an atmospheric temperature of 150°C. For the test piece after standing, the adhesive sheet piece for evaluation (configuration: adhesive layer / polyimide film) was peeled off 180° in the long side (150 mm) direction from the glass plate in an environment with an atmospheric temperature of 150°C, and the adhesive strength (unit: N / 25 mm) was measured using a Tensilon universal material testing machine (model number: RTF-1350) manufactured by A&D Co., Ltd. as a measuring device, at a peeling speed of 300 mm / min. Evaluation was then performed according to the following evaluation criteria. The results are shown in Tables 2 and 3. In the following evaluation criteria, "A", "B", and "C" are levels that are acceptable for practical use, with "A" being the most preferable.

[0121] -Evaluation criteria- A: The adhesive strength is 8.0N / 25mm or more. B: The adhesive strength is 5.0N / 25mm or more and less than 8.0N / 25mm. C: The adhesive strength is 2.0 N / 25 mm or more and less than 5.0 N / 25 mm. D: The adhesive strength is less than 2.0N / 25mm.

[0122] 2. Removability at room temperature after exposure to high temperature (1) Adhesive strength The adhesive sheet for evaluation prepared above was cut into a size of 25 mm × 150 mm to prepare an adhesive sheet piece for evaluation. In addition, a glass plate [product name: soda lime glass (ordinary glass), thickness: 1.8 mm, manufactured by Kawamura Kyuzo Shoten Co., Ltd.] was prepared as an adherend. The release film was peeled off from the adhesive sheet piece for evaluation, and the surface of the adhesive layer exposed by peeling was laminated on one side of a glass plate, and then a 2 kg roller was moved back and forth once to press the adhesive sheet piece for evaluation [adhesive layer / substrate (polyimide film)] to prepare a test piece. The prepared test piece has a laminated structure of adherend (glass plate) / adhesive sheet piece for evaluation [adhesive layer / substrate (polyimide film)]. Next, the prepared test piece was left to stand for 30 minutes in an environment with an atmospheric temperature of 150°C, and then left to stand for 30 minutes in an environment with an atmospheric temperature of 25°C and 50% RH. For the test piece after this standing, the adhesive force (unit: N / 25 mm) when the adhesive sheet piece for evaluation (configuration: adhesive layer / polyimide film) was peeled off 180° in the long side (150 mm) direction from the glass plate was measured using a Tensilon universal material testing machine (model number: RTF-1350) manufactured by A&D Co., Ltd. as a measuring device, at a peeling speed of 300 mm / min. The results are shown in Tables 2 and 3. In the following evaluation criteria, "A", "B", and "C" are levels that are not problematic in practical use, with "A" being the most preferable.

[0123] -Evaluation criteria- A: The adhesive strength is less than 1.0N / 25mm. B: The adhesive strength is 1.0N / 25mm or more and less than 3.0N / 25mm. C: The adhesive strength is 3.0N / 25mm or more and less than 5.0N / 25mm. D: The adhesive strength is 5.0N / 25mm or more.

[0124] (2) Glue residue In the evaluation test of "(1) Adhesive strength" above, the surface of the glass plate after peeling off the evaluation adhesive sheet piece (structure: adhesive layer / polyimide film) was visually observed. Evaluation was then performed according to the following evaluation criteria. The results are shown in Tables 2 and 3. In the following evaluation criteria, "A", "B", and "C" are levels that are not problematic in practical use, with "A" being the most preferable.

[0125] -Evaluation criteria- A: No adhesive residue was observed at all. B: A small amount of glue residue is observed. C: Adhesive residue was observed, but at a level that did not cause any practical problems. D: Adhesive residue is clearly visible.

[0126] [Table 2]

[0127] [Table 3]

[0128] Details of the crosslinking agents listed in Table 2 and / or Table 3 are as follows. <Epoxy-based crosslinking agent> "TETRAD-X" [product name, solid content: 100% by mass, manufactured by Mitsubishi Gas Chemical Co., Ltd.] <Isocyanate-based crosslinking agent> "Coronate L-45E" [product name, tolylene diisocyanate compound (adduct of tolylene diisocyanate (TDI) and trimethylolpropane (TMP)), solid content concentration: 45% by mass, manufactured by Tosoh Corporation] <Metal chelate crosslinking agent> "Aluminum Chelate A" [Product name, chemical name: aluminum tris(acetylacetonate), manufactured by Kawaken Fine Chemicals Co., Ltd.] <Aziridine-based crosslinking agent> "ChemiTite PZ-33" (product name, manufactured by Nippon Shokubai Co., Ltd.) The above "TETRAD", "Coronate", and "ChemiTite" are all registered trademarks.

[0129] As shown in Table 2, it was confirmed that the adhesive layers formed using the adhesive compositions of Examples 1 to 20 exhibited high adhesive strength in a high-temperature environment and also exhibited excellent removability in a room temperature environment after exposure to a high-temperature environment.

[0130] On the other hand, as shown in Table 3, it was confirmed that the adhesive layer formed from the adhesive composition of Comparative Example 1, in which the (meth)acrylic copolymer does not contain a structural unit derived from a (meth)acrylic acid alkyl ester monomer having a branched alkyl group, is likely to leave adhesive residue on the surface of the adherend when exposed to a high-temperature environment and then peeled from the adherend in a room temperature environment. It was confirmed that the adhesive layers formed from the adhesive compositions of Comparative Example 2 and Comparative Example 3, in which the content of structural units derived from monomers having a carboxy group in the (meth)acrylic copolymer is less than 10 mass% relative to the total structural units, do not exhibit high adhesive strength in a high-temperature environment. It was confirmed that the adhesive layer formed from the adhesive composition of Comparative Example 4, in which the (meth)acrylic copolymer does not contain a structural unit derived from a (meth)acrylic acid alkyl ester monomer having a linear alkyl group having 16 or more carbon atoms, cannot be easily peeled off when exposed to a high-temperature environment and then peeled off from an adherend in a room temperature environment. It was confirmed that the adhesive layer formed from the adhesive composition of Comparative Example 5, in which the content of structural units derived from (meth)acrylic acid alkyl ester monomers having a linear alkyl group having 16 or more carbon atoms in the (meth)acrylic copolymer is less than 10 mass% relative to all structural units, cannot be easily peeled off when exposed to a high-temperature environment and then peeled off from an adherend in a room temperature environment. It was confirmed that the adhesive layer formed from the adhesive composition of Comparative Example 6, in which the content of structural units derived from (meth)acrylic acid alkyl ester monomers having a linear alkyl group having 16 or more carbon atoms in the (meth)acrylic copolymer exceeds 50 mass% relative to all structural units, is prone to leaving adhesive residue on the surface of the adherend when exposed to a high-temperature environment and then peeled from the adherend in a room temperature environment. It was confirmed that the adhesive layer formed from the adhesive composition of Comparative Example 7, in which the content of structural units derived from (meth)acrylic acid alkyl ester monomers having branched alkyl groups in the (meth)acrylic copolymer exceeds 70 mass% relative to all structural units, does not exhibit high adhesive strength in a high temperature environment.

Claims

1. a (meth)acrylic copolymer containing 30% by mass to 70% by mass of structural units derived from a (meth)acrylic acid alkyl ester monomer having a branched alkyl group, based on all structural units, 10% by mass to 50% by mass of structural units derived from a (meth)acrylic acid alkyl ester monomer having a linear alkyl group having 16 or more carbon atoms, based on all structural units, and 10% by mass or more of structural units derived from a monomer having a carboxy group, based on all structural units; A cross-linking agent; A pressure-sensitive adhesive composition comprising:

2. The pressure-sensitive adhesive composition according to claim 1 , wherein the crosslinking agent is an epoxy-based crosslinking agent.

3. 3. The pressure-sensitive adhesive composition according to claim 1, wherein the (meth)acrylic copolymer has a weight average molecular weight of 100,000 to 300,000.

4. The pressure-sensitive adhesive composition according to any one of claims 1 to 3, wherein the (meth)acrylic copolymer has a glass transition temperature of 40°C to 70°C.

5. The pressure-sensitive adhesive composition according to any one of claims 1 to 4, wherein the (meth)acrylic acid alkyl ester monomer having a linear alkyl group having 16 or more carbon atoms is stearyl methacrylate.

6. A pressure-sensitive adhesive sheet comprising a pressure-sensitive adhesive layer formed from the pressure-sensitive adhesive composition according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Film for window and its pasting method, and scattering-preventing film and crime-preventing film

    JP2007031658A

  • Adhesive agent

    JP2008179744A

  • Temperature sensitive adhesive

    JP2016196544A

  • Adhesive composition for decorative film, decorative film and decorative molded product

    JP2019073641A

  • Adhesive sheet for oil surface

    JP2020045418A