Lithium ion battery PET protective film and preparation method thereof

By using a combined structure of polyester film reinforcement surface and modified PMMA adhesive, aluminum film layer and plastic film layer in the lithium-ion battery aluminum-plastic film, combined with the hot rolling technology of hollowing out and epoxy resin adhesive, the problem is solved It solves the problems of poor impact resistance and short service life at high temperatures of the aluminum-plastic film of lithium-ion batteries, and significantly improves the high-temperature resistance and mechanical properties of lithium-ion batteries.

CN118789900AInactive Publication Date: 2024-10-18DONGGUAN XINGGUANG NEW MATERIAL TECHNOLOGY CO LTD

Patent Information

Application Number
CN202410788735.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-10-18
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The aluminum-plastic film of lithium-ion batteries has poor impact resistance and is prone to deformation and damage when impacted by external forces. Its service life is not long in high-temperature environments, posing safety risks.

Method used

It adopts a structure of transparent protective layer, aluminum film layer and plastic film layer. The transparent protective layer is composed of polyester film reinforced surface and modified PMMA adhesive. The aluminum film layer is made of aluminum material. The plastic film layer is cast polyester. Propylene film, through the hot rolling technology of hollow structure and epoxy resin adhesive, enhances the high temperature resistance and impact resistance of the film layer.

Benefits of technology

Significantly improves the high temperature resistance and mechanical properties of lithium-ion batteries, reduces the risk of damage to external forces, and extends the service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118789900A_ABST
    Figure CN118789900A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of PET protective films, in particular to a lithium ion battery PET protective film and a preparation method thereof. The composite film comprises a transparent protective layer, an aluminum film layer and a plastic film layer, the transparent protective layer adopts a polyester film as a substrate, and a single surface is coated with acrylic acid glue and cured to form a reinforced surface; the surface of the polyester film is provided with a plurality of hollows distributed at equal intervals, and the hollows are of circular structures; the acrylic glue adopts acrylic resin, specifically a modified PMMA (Polymethyl Methacrylate) adhesive; according to the lithium ion battery PET protective film and the preparation method thereof, when the transparent protective layer is combined with the aluminum film layer, due to the special hollowed-out arrangement of the polyester film, the first cementing layer can be fully combined with the reinforced surface at the hollowed-out part of the polyester film in a hot rolling manner, and the effects of bubble removal and smooth appearance are achieved during fitting; when the composite material is applied to the lithium ion battery, the high temperature resistance and the mechanical property of the lithium ion battery can be greatly improved, and the situation that the lithium ion battery is easily damaged by external force is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of PET protective films, in particular to a lithium ion battery PET protective film and a preparation method thereof. Background Art

[0002] As a green, efficient and portable energy source, lithium-ion batteries are widely used in the fields of 3C consumer electronics, electric vehicles, energy storage power stations, etc. The soft packaging shell of lithium-ion is also called aluminum-plastic shell (or aluminum-plastic film). From the perspective of the battery, in order from the outside to the inside, its structure consists of a nylon layer (polyamide fiber layer), an aluminum foil layer and a polypropylene layer.

[0003] At present, the aluminum-plastic film of lithium-ion batteries has poor impact resistance on the surface. When the film layer is impacted by external force, it is very easy to deform, which can easily cause damage to the outer layer (nylon layer) of the aluminum-plastic film, resulting in electrolyte leakage and unnecessary safety hazards. In addition, the high temperature resistance of the nylon layer is generally not high. When used in a working environment under high temperature for a long time, the service life of the aluminum-plastic film is not high. In view of this, there is an urgent need for a lithium-ion battery aluminum-plastic film with better mechanical properties to improve the shortcomings of the existing technology. Summary of the invention

[0004] The object of the present invention is to provide a lithium-ion battery PET protective film and a preparation method thereof, so as to solve the problems raised in the above background technology.

[0005] To achieve the above object, on the one hand, the present invention provides a lithium-ion battery PET protective film, comprising a transparent protective layer, an aluminum film layer and a plastic film layer, wherein: the transparent protective layer uses a polyester film as a substrate, and a single-side coating of acrylic glue is cured to form a reinforced surface, and the overall thickness is 48-52um;

[0006] The polyester film surface is provided with a number of equally spaced hollows, the hollows are circular in structure, 6-10 are provided for every 20 cm in length, and the radius of each hollow is 1 cm. Through the hollow setting, when the modified PMMA adhesive is attached to the polyester film surface, it can enter the hollow position, so that the modified PMMA adhesive can be fully combined with the polyester film, thereby enhancing the overall strength of the transparent protective layer;

[0007] The acrylic glue is made of acrylic resin, specifically modified PMMA adhesive.

[0008] As a further improvement of the present technical solution, the aluminum film layer is a film layer made of aluminum as a base material, and the overall thickness is 45um.

[0009] As a further improvement of the technical solution, the plastic film layer is made of cast polypropylene film with an overall thickness of 45 um.

[0010] As a further improvement of the present technical solution, the modified PMMA adhesive comprises at least: 60-80 parts by weight of MMA monomer, 11-17 parts by weight of nanofiller, 1-5 parts by weight of dispersant and 0.1-3 parts by weight of initiator. The modified method can further improve the high temperature resistance, impact strength and adhesion of the polyester film.

[0011] As a further improvement of the technical solution, the nano filler is selected from one or more of mica powder, silicon dioxide, alumina powder and glass fiber.

[0012] As a further improvement of the technical solution, a first adhesive layer is provided between the transparent protective layer and the aluminum film layer, and a second adhesive layer is provided between the aluminum film layer and the plastic film layer. Both the first adhesive layer and the second adhesive layer are formed by curing an epoxy resin adhesive.

[0013] As a further improvement of the technical solution, the thickness of the first adhesive layer and the second adhesive layer are both 3-5 um.

[0014] On the other hand, the present invention provides a method for preparing a lithium-ion battery PET protective film as described in any one of the above, comprising the following steps:

[0015] S1. Add MMA monomer to a reactor, add a dispersant and stir thoroughly, then add a nanofiller and stir evenly, then add an initiator and heat up and continue stirring to react, so as to obtain a modified PMMA adhesive; lay a polyester film flat, then spray the modified PMMA adhesive, and after curing, form a reinforced surface to obtain a transparent protective layer;

[0016] S2. Flatten the aluminum film layer, apply epoxy resin adhesive on one side, and then attach the side of the transparent protective layer without the reinforcement surface to the surface of the aluminum film layer. Combine the film layers by hot rolling, and cure the epoxy resin adhesive between the transparent protective layer and the aluminum film layer by heating to form a first bonding layer. During the thermal curing process of the epoxy resin adhesive, the hot pressing temperature can melt the reinforcement surface of the hollow part of the polyester film, so that the PMMA component in the hollow part can be blended and combined with the epoxy resin adhesive by extrusion, so that the mechanical properties of the connection between the two are further improved, and the adhesion between the film layers can be improved;

[0017] S3. Turn over the aluminum film layer, apply epoxy resin adhesive on the surface, and then attach the plastic film layer to the surface of the aluminum film layer. Use hot roller pressing to combine the film layers at a temperature of 90-110°C. The epoxy resin adhesive is cured by heating to form a second bonding layer between the aluminum film layer and the plastic film layer, and a lithium-ion battery PET protective film can be obtained.

[0018] Preferably, in S2, the hot pressing temperature between the transparent protective layer and the aluminum film layer is 130-150°C.

[0019] Preferably, in S3, the hot pressing temperature between the plastic film layer and the aluminum film layer is 90-110°C.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] In the lithium-ion battery PET protective film and the preparation method thereof, a modified PMMA adhesive is used to form a reinforced surface on the surface of a polyester film to prepare a transparent protective layer with good high temperature resistance and impact resistance. When the transparent protective layer is combined with the aluminum film layer, due to the special hollowing arrangement of the polyester film, the first adhesive layer and the reinforced surface of the hollowed-out part of the polyester film can be fully combined through hot rolling, and the effects of air bubble removal and smooth appearance can be achieved during lamination, so that the mechanical properties of the connection between the two are further improved, and the adhesion effect between the transparent protective layer and the aluminum film layer can be enhanced. When applied to lithium-ion batteries, the high temperature resistance and mechanical properties of the lithium-ion batteries can be greatly improved, and the situation in which the lithium-ion batteries are easily damaged by external forces can be reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a schematic diagram of the overall structure of the present invention.

[0023] The meaning of each number in the figure is:

[0024] 1. Aluminum film layer; 2. Transparent protective layer; 21. Strengthening surface; 22. Hollowing; 3. Plastic film layer; 4. First bonding layer; 5. Second bonding layer. DETAILED DESCRIPTION

[0025] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention.

[0026] The embodiment of the present invention provides a lithium-ion battery PET protective film, comprising a transparent protective layer 2, an aluminum film layer 1 and a plastic film layer 3, wherein: the transparent protective layer 2 uses a polyester film as a substrate, and is coated with acrylic glue on one side and then cured to form a reinforced surface, with an overall thickness of 48-52um. The transparent protective layer 2 has good high temperature resistance, a small high temperature shrinkage rate, and easy discharge of bubbles during use; the aluminum film layer 1 uses a film layer made of aluminum as a base material, with an overall thickness of 45um; the plastic film layer 3 uses a cast polypropylene film, with an overall thickness of 45um.

[0027] On the basis of the above, the acrylic glue adopts acrylic resin, specifically modified PMMA adhesive, which has high transparency, good bearing capacity, high impact strength and good weather resistance; the modified PMMA adhesive at least includes: 60-80 parts by weight of MMA monomer, 11-17 parts by weight of nano filler, 1-5 parts by weight of dispersant and 0.1-3 parts by weight of initiator; specifically: the nano filler is selected from one or more of mica powder, silica, alumina powder and glass fiber, and the modification method can further improve the high temperature resistance, impact strength and adhesion of the polyester film.

[0028] The polyester film surface is provided with a number of equally spaced hollows 22, the hollows 22 are circular in structure, 6-10 are provided for every 20 cm in length, and the radius of each hollow 22 is 1 cm. Through the hollow 22, when the modified PMMA adhesive is attached to the polyester film surface, it can enter the hollow 22 position, so that the modified PMMA adhesive can be fully combined with the polyester film, thereby enhancing the overall strength of the transparent protective layer 2;

[0029] A first adhesive layer 4 is provided between the transparent protective layer 2 and the aluminum film layer 1, and a second adhesive layer 5 is provided between the aluminum film layer 1 and the plastic film layer 3. Both the first adhesive layer 4 and the second adhesive layer 5 are formed by curing epoxy resin adhesive and are used to connect the film layers. The thickness of the two adhesive layers is 3-5um.

[0030] according to Figure 1 As shown, the embodiment of the present invention also provides a method for preparing the above-mentioned lithium-ion battery PET protective film, and the specific steps are as follows:

[0031] S1, adding MMA monomer to a reactor, adding a dispersant and stirring thoroughly, then adding a nanofiller and stirring evenly, adding an initiator and heating and continuing to stir and react to obtain a modified PMMA adhesive; laying a polyester film flat, then spraying the modified PMMA adhesive, and forming a strengthening surface 21 after curing to obtain a transparent protective layer 2;

[0032] S2, flatten the aluminum film layer 1, apply epoxy resin adhesive on one side, then attach the side of the transparent protective layer 2 without the strengthening surface 21 to the surface of the aluminum film layer 1, and combine the film layers by hot rolling at a temperature of 130-150°C, and cure the epoxy resin adhesive between the transparent protective layer 2 and the aluminum film layer 1 by heating to form a first bonding layer 4. During the heat curing process of the epoxy resin adhesive, the hot pressing temperature can make the strengthening surface 21 at the hollow 22 of the polyester film melt, so that the PMMA component at the hollow 22 can be mixed and combined with the epoxy resin adhesive by extrusion, so that the mechanical properties of the connection between the two are further improved, and the adhesion between the film layers can be improved;

[0033] S3. Turn over the aluminum film layer 1, apply epoxy resin adhesive on the surface, and then attach the plastic film layer 3 to the surface of the aluminum film layer 1. Use hot rolling to combine the film layers at a temperature of 90-110°C. The epoxy resin adhesive is cured by heating to form a second bonding layer 5 between the aluminum film layer 1 and the plastic film layer 3, and the lithium-ion battery PET protective film can be obtained.

[0034] In the present invention, a modified PMMA adhesive is used to form a reinforced surface on the surface of a polyester film to prepare a transparent protective layer 2 with good high temperature resistance and impact resistance. When the transparent protective layer 2 is combined with the aluminum film layer 1, due to the special hollow 22 setting of the polyester film, the first bonding layer 4 and the reinforced surface at the hollow 22 of the polyester film can be fully combined through hot rolling, so that the mechanical properties of the connection between the two are further improved, and the adhesion effect between the transparent protective layer 2 and the aluminum film layer 1 can be enhanced. When applied to lithium-ion batteries, the high temperature resistance and mechanical properties of the lithium-ion batteries can be greatly improved, and the situation where the lithium-ion batteries are easily damaged by external forces can be reduced.

[0035] According to different raw material dosages, the lithium ion battery PET protective film provided by the present invention is further described through the following specific examples.

[0036] Example 1

[0037] S1, adding 60 parts by weight of MMA monomer to a reactor, adding 1 part by weight of a dispersant and stirring thoroughly, then adding 11 parts by weight of a nanofiller and stirring evenly, adding 0.1 parts by weight of an initiator and heating and continuing to stir and react to obtain a modified PMMA adhesive; laying a polyester film flat, then spraying the modified PMMA adhesive, and forming a strengthening surface 21 after curing to obtain a transparent protective layer 2 with a thickness of 52 um, and setting 10 hollows 22 for every 20 cm of the polyester film;

[0038] S2, flatten the aluminum film layer 1, apply epoxy resin adhesive on one side, and then attach the side of the transparent protective layer 2 without the strengthening surface 21 to the surface of the aluminum film layer 1, and combine the film layers by hot rolling at a temperature of 130° C. The epoxy resin adhesive is cured by heating between the transparent protective layer 2 and the aluminum film layer 1 to form a first bonding layer 4 with a thickness of 3 μm;

[0039] S3. Turn over the aluminum film layer 1, apply epoxy resin adhesive on the surface, and then attach the plastic film layer 3 to the surface of the aluminum film layer 1. Use hot rolling to combine the film layers at a temperature of 90°C. The epoxy resin adhesive is cured by heating to form a second bonding layer 5 with a thickness of 3um between the aluminum film layer 1 and the plastic film layer 3, and the lithium-ion battery PET protective film can be obtained.

[0040] Example 2

[0041] S1, adding 70 parts by weight of MMA monomer to a reactor, adding 3 parts by weight of a dispersant and stirring well, then adding 14 parts by weight of a nanofiller and stirring evenly, adding 2 parts by weight of an initiator and heating and continuing to stir and react to obtain a modified PMMA adhesive; laying a polyester film flat, then spraying the modified PMMA adhesive, and forming a strengthening surface 21 after curing to obtain a transparent protective layer 2 with a thickness of 50 um, and setting 8 hollows 22 for every 20 cm of the polyester film;

[0042] S2, flatten the aluminum film layer 1, apply epoxy resin adhesive on one side, and then attach the side of the transparent protective layer 2 without the strengthening surface 21 to the surface of the aluminum film layer 1, and combine the film layers by hot rolling at a temperature of 140° C. The epoxy resin adhesive is cured by heating between the transparent protective layer 2 and the aluminum film layer 1 to form a first bonding layer 4 with a thickness of 4 μm;

[0043] S3. Turn over the aluminum film layer 1, apply epoxy resin adhesive on the surface, and then attach the plastic film layer 3 to the surface of the aluminum film layer 1. Use hot rolling to combine the film layers at a temperature of 100°C. Heat to cure the epoxy resin adhesive to form a second bonding layer 5 with a thickness of 4um between the aluminum film layer 1 and the plastic film layer 3, and the lithium-ion battery PET protective film can be obtained.

[0044] Example 3

[0045] S1, adding 80 parts by weight of MMA monomer to a reactor, adding 5 parts by weight of a dispersant and stirring thoroughly, then adding 17 parts by weight of a nanofiller and stirring evenly, adding 3 parts by weight of an initiator and heating and continuing to stir and react to obtain a modified PMMA adhesive; laying a polyester film flat, then spraying the modified PMMA adhesive, and forming a strengthening surface 21 after curing to obtain a transparent protective layer 2 with a thickness of 48 um, and setting 6 hollows 22 for every 20 cm of the polyester film;

[0046] S2, flatten the aluminum film layer 1, apply epoxy resin adhesive on one side, and then attach the side of the transparent protective layer 2 without the strengthening surface 21 to the surface of the aluminum film layer 1, and combine the film layers by hot rolling at a temperature of 150° C. The epoxy resin adhesive is cured by heating between the transparent protective layer 2 and the aluminum film layer 1 to form a first bonding layer 4 with a thickness of 5 μm;

[0047] S3. Turn over the aluminum film layer 1, apply epoxy resin adhesive on the surface, and then attach the plastic film layer 3 to the surface of the aluminum film layer 1. Use hot rolling to combine the film layers at a temperature of 110°C. The epoxy resin adhesive is cured by heating to form a second bonding layer 5 with a thickness of 5um between the aluminum film layer 1 and the plastic film layer 3, and the lithium-ion battery PET protective film can be obtained.

[0048] Example 4

[0049] S1, adding 80 parts by weight of MMA monomer into a reactor, adding 2 parts by weight of a dispersant and stirring thoroughly, then adding 11 parts by weight of a nanofiller and stirring evenly, adding 1.5 parts by weight of an initiator and heating and continuing to stir and react to obtain a modified PMMA adhesive; laying a polyester film flat, then spraying the modified PMMA adhesive, and forming a strengthening surface 21 after curing to obtain a transparent protective layer 2 with a thickness of 51 um, and setting 9 hollows 22 for every 20 cm of the polyester film;

[0050] S2, flatten the aluminum film layer 1, apply epoxy resin adhesive on one side, and then attach the side of the transparent protective layer 2 without the strengthening surface 21 to the surface of the aluminum film layer 1, and combine the film layers by hot rolling at a temperature of 140° C. The epoxy resin adhesive is cured by heating between the transparent protective layer 2 and the aluminum film layer 1 to form a first bonding layer 4 with a thickness of 4 μm;

[0051] S3. Turn over the aluminum film layer 1, apply epoxy resin adhesive on the surface, and then attach the plastic film layer 3 to the surface of the aluminum film layer 1. Use hot rolling to combine the film layers at a temperature of 100°C. Heat to cure the epoxy resin adhesive to form a second bonding layer 5 with a thickness of 4um between the aluminum film layer 1 and the plastic film layer 3, and the lithium-ion battery PET protective film can be obtained.

[0052] Example 5

[0053] S1, adding 70 parts by weight of MMA monomer to a reactor, adding 3.5 parts by weight of a dispersant and stirring well, then adding 17 parts by weight of a nanofiller and stirring evenly, adding 2.5 parts by weight of an initiator and heating and continuing to stir and react to obtain a modified PMMA adhesive; laying a polyester film flat, then spraying the modified PMMA adhesive, and forming a strengthening surface 21 after curing to obtain a transparent protective layer 2 with a thickness of 49 um, and setting 7 hollows 22 for every 20 cm of the polyester film;

[0054] S2, flatten the aluminum film layer 1, apply epoxy resin adhesive on one side, and then attach the side of the transparent protective layer 2 without the strengthening surface 21 to the surface of the aluminum film layer 1, and combine the film layers by hot rolling at a temperature of 140° C. The epoxy resin adhesive is cured by heating between the transparent protective layer 2 and the aluminum film layer 1 to form a first bonding layer 4 with a thickness of 4 μm;

[0055] S3. Turn over the aluminum film layer 1, apply epoxy resin adhesive on the surface, and then attach the plastic film layer 3 to the surface of the aluminum film layer 1. Use hot rolling to combine the film layers at a temperature of 100°C. Heat to cure the epoxy resin adhesive to form a second bonding layer 5 with a thickness of 4um between the aluminum film layer 1 and the plastic film layer 3, and the lithium-ion battery PET protective film can be obtained.

[0056] Table 1 Formulas of modified PMMA adhesives in Examples 1-5 (parts)

[0057] Example 1 Example 2 Example 3 Example 4 Example 5 MMA monomer 60 70 80 80 70 Nanofillers 11 14 17 11 17 Dispersants 1 3 5 2 3.5 Initiator 0.1 2 3 1.5 2.5

[0058] Table 2 Transparent protective layers of Examples 1-5

[0059]

[0060] In order to verify that the PET protective film prepared in the embodiment of the present invention has good mechanical properties, the lithium-ion battery PET protective film provided in the embodiment of the present invention is compared and described through the following comparative examples.

[0061] Comparative Example 1

[0062] This comparative example adopts the preparation method of Example 1, directly replacing the transparent protective layer 2 with a polyester film, and canceling the setting of the hollow 22 on the polyester film. The other raw materials and methods remain unchanged. The specific steps are as follows:

[0063] S1, flatten the aluminum film layer 1, apply epoxy resin adhesive on one side, then attach one side of the polyester film to the surface of the aluminum film layer 1, and combine the film layers by hot rolling at a temperature of 130°C. The epoxy resin adhesive is cured between the polyester film and the aluminum film layer 1 by heating to form a first bonding layer 4 with a thickness of 3um;

[0064] S2. Turn over the aluminum film layer 1, apply epoxy resin adhesive on the surface, and then attach the plastic film layer 3 to the surface of the aluminum film layer 1. Use hot rolling to combine the film layers at a temperature of 90°C. The epoxy resin adhesive is cured by heating to form a second bonding layer 5 with a thickness of 3um between the aluminum film layer 1 and the plastic film layer 3, and the lithium-ion battery PET protective film can be obtained.

[0065] Comparative Examples 2-5

[0066] The preparation method of Example 2-5 is adopted, the polyester film is directly used to replace the transparent protective layer 2, and the setting of the hollow 22 on the polyester film is cancelled. The other raw materials and methods remain unchanged. The specific steps are similar to those of Comparative Example 1, and Comparative Examples 2-5 are not repeated.

[0067] Comparative Example 6

[0068] This comparative example adopts the preparation method of Example 1, and directly replaces the transparent protective layer 2 with a nylon layer and adheres it to the surface of the aluminum film layer 1. The other raw materials and methods remain unchanged to form a lithium-ion battery PET protective film of nylon layer / aluminum film layer 1 / plastic film layer 3. The specific steps are as follows:

[0069] S1, flatten the aluminum film layer 1, apply epoxy resin adhesive on one side, then attach one side of the nylon layer to the surface of the aluminum film layer 1, and combine the film layers by hot rolling at a temperature of 130°C. The epoxy resin adhesive is cured between the nylon layer and the aluminum film layer 1 by heating to form a first bonding layer 4 with a thickness of 3 um;

[0070] S2. Turn over the aluminum film layer 1, apply epoxy resin adhesive on the surface, and then attach the plastic film layer 3 to the surface of the aluminum film layer 1. Use hot rolling to combine the film layers at a temperature of 90°C. The epoxy resin adhesive is cured by heating to form a second bonding layer 5 with a thickness of 3um between the aluminum film layer 1 and the plastic film layer 3, and the lithium-ion battery PET protective film can be obtained.

[0071] Comparative Examples 7-10

[0072] The preparation method of Example 2-5 is adopted, and the nylon layer directly replaces the transparent protective layer 2 and is bonded to the surface of the aluminum film layer 1. The other raw materials and methods remain unchanged to form a lithium-ion battery PET protective film of nylon layer / aluminum film layer 1 / plastic film layer 3. The specific steps are similar to those of Comparative Example 6, and Comparative Examples 2-5 are not repeated here.

[0073] Test example

[0074] In this test example, the mechanical properties of the lithium-ion battery PET protective films provided in the above-mentioned examples 1-5 and comparative examples 1-10 were tested. The peeling force test was carried out in accordance with the inspection standard GB / T2792. Examples 1-5 tested the peeling force between the transparent protective layer 2 and the aluminum film layer 1, comparative examples 1-5 tested the peeling force between the polyester film and the aluminum film layer 1, and comparative examples 6-10 tested the peeling force between the nylon layer and the aluminum film layer 1;

[0075] The tensile strength is in accordance with the inspection standard GB / T30776; the elongation at break is in accordance with the inspection standard GB / T30776; the specific inspection indicators are shown in Table 3-Table 5.

[0076] Table 3 Detection indexes of samples in Examples 1-5

[0077]

[0078] Table 4 Test indicators of samples in comparative examples 1-5

[0079]

[0080]

[0081] Table 5 Test indicators of samples in comparative examples 6-10

[0082]

[0083] As shown in Tables 3 to 5, the lithium-ion battery PET protective films provided by Examples 1-5 of the present invention all have good mechanical properties, and all test indicators are better than the lithium-ion battery aluminum plastic provided by Comparative Examples 1-10; as shown in Table 4, after the modified PMMA adhesive is removed from Comparative Examples 1-5, the peel force, tensile strength, elongation at break and high temperature resistance all decrease to varying degrees, and after the transparent protective layer 2 is replaced by the nylon layer in Comparative Examples 1-5, all indicators decrease significantly; at the same time, the aluminum film layer of Comparative Examples 1-10 has a small amount of bubbles and protrusions compared to that of Examples 1-5, so it can be explained that the use of the transparent protective layer 2 provided by the present invention is an important factor affecting the mechanical properties and appearance of the lithium-ion battery PET protective film.

[0084] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited by the above embodiments. The above embodiments and descriptions are only preferred examples of the present invention and are not intended to limit the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A lithium-ion battery PET protective film, It is characterized in that It comprises a transparent protective layer (2), an aluminum film layer (1) and a plastic film layer (3), wherein: the transparent protective layer (2) uses a polyester film as a base, and acrylic glue is coated on one side and then cured to form a reinforced surface, and the overall thickness is 48-52um; The polyester film surface is provided with a plurality of equally spaced hollows (22), the hollows (22) are circular in structure, 6 to 10 are arranged for every 20 cm in length, and the radius of each hollow (22) is 1 cm; The acrylic glue is made of acrylic resin, specifically modified PMMA adhesive.

2. The lithium-ion battery PET protective film according to claim 1, Features: The aluminum film layer (1) is a film layer made of aluminum as a base material, and has an overall thickness of 45 um.

3. The lithium-ion battery PET protective film according to claim 1, Features: The plastic film layer (3) is made of cast polypropylene film with an overall thickness of 45 um.

4. The lithium-ion battery PET protective film according to claim 1, It is characterized in that The modified PMMA adhesive at least comprises: 60-80 parts by weight of MMA monomer, 11-17 parts by weight of nano filler, 1-5 parts by weight of dispersant and 0.1-3 parts by weight of initiator.

5. The lithium-ion battery PET protective film according to claim 4, Features: The nano filler is selected from one or more of mica powder, silicon dioxide, alumina powder and glass fiber.

6. The lithium-ion battery PET protective film according to claim 1, Features: A first adhesive layer (4) is provided between the transparent protective layer (2) and the aluminum film layer (1), and a second adhesive layer (5) is provided between the aluminum film layer (1) and the plastic film layer (3). Both the first adhesive layer (4) and the second adhesive layer (5) are formed by curing an epoxy resin adhesive.

7. The lithium-ion battery PET protective film according to claim 1, Features: The thickness of the first adhesive layer (4) and the second adhesive layer (5) are both 3-5 um.

8. A method for preparing a lithium-ion battery PET protective film according to any one of claims 1 to 7, It is characterized in that The following steps are involved: S1, adding MMA monomer to a reaction kettle, adding a dispersant and stirring thoroughly, then adding a nanofiller and stirring evenly, adding an initiator and heating and continuing to stir and react to obtain a modified PMMA adhesive; laying a polyester film flat, then spraying the modified PMMA adhesive, and forming a reinforcement surface (21) after curing to obtain a transparent protective layer (2); S2, flattening the aluminum film layer (1), coating one side of the aluminum film layer (1) with epoxy resin adhesive, and then attaching the side of the transparent protective layer (2) not provided with the strengthening surface (21) to the surface of the aluminum film layer (1), combining the film layers by hot rolling, and curing the epoxy resin adhesive between the transparent protective layer (2) and the aluminum film layer (1) by heating to form a first bonding layer (4); S3. Turn over the aluminum film layer (1), apply epoxy resin adhesive on the surface, and then attach the plastic film layer (3) to the surface of the aluminum film layer (1). Use hot rolling to combine the film layers at a temperature of 90-110°C. Heat is used to cure the epoxy resin adhesive to form a second adhesive layer (5) between the aluminum film layer (1) and the plastic film layer (3), thereby obtaining a lithium-ion battery PET protective film.

9. The method for preparing the lithium-ion battery PET protective film according to claim 8, Features: In the above-mentioned S2, the hot pressing temperature between the transparent protective layer (2) and the aluminum film layer (1) is 130-150°C.

10. The method for preparing the lithium-ion battery PET protective film according to claim 8, Features: In S3, the hot pressing temperature between the plastic film layer (3) and the aluminum film layer (1) is 90-110°C.

Citation Information

Patent Citations

  • Aluminum-plastic membrane used for packaging lithium battery

    CN101992570A

  • Acrylic protective film with high temperature resistance and excellent exhaust property and preparation method of acrylic protective film

    CN112920727A

  • Four-side antistatic PU adhesive protective film

    CN211367452U

Cited By

  • PET (Polyethylene Terephthalate) composite film material for glucometer switch and preparation method of PET composite film material

    CN118978870A

  • Lithium battery composite protective film and preparation method thereof

    CN121642332A

  • Composite film, battery cell and manufacturing method therefor, battery apparatus, and electric apparatus

    WO2026108363A1