Soldering elastomer

A single-component elastic body for soldering, utilizing a Sn film-coated filler in insulating rubber, addresses the high cost and complexity of existing conductive contact members and rubber parts by offering cost-effective solderability and conductivity.

JP7553755B2Active Publication Date: 2024-09-19KITAGAWA INDS
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020060264
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-03-30
Publication Date
2024-09-19
Estimated Expiration
2040-03-30

AI Technical Summary

Technical Problem

Conductive contact members and conductive rubber parts for soldering require multiple components, leading to high manufacturing costs and complex processes.

Method used

An elastic body for soldering is developed with a Sn film-coated filler integrated into an insulating rubber, allowing for a single-component configuration with solderability and conductivity.

Benefits of technology

The elastic body provides a cost-effective and simplified manufacturing process while ensuring excellent solderability and electrical conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007553755000004
    Figure 0007553755000004
  • Figure 0007553755000005
    Figure 0007553755000005
  • Figure 0007553755000003
    Figure 0007553755000003
Patent Text Reader

Abstract

To provide an elastic body for soldering, which can be constituted as one component and which has at least solderability.SOLUTION: An elastic body 1 for soldering according to the present invention comprises: an insulating elastic body 5 including an insulating rubber; and a filler 6 with an Sn film, in which a core material 61 is coated with the Sn film 62 made of Sn or an Sn alloy and which is contained in the insulating elastic body 5. The elastic body for soldering has a soldering surface 3 that comprises a surface 50 of the insulating elastic body 5 and the filler 6 with the Sn film exposed from the surface 50 and that can be soldered to the other side.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an elastomer for soldering. [Background technology]

[0002] As shown in Patent Document 1, a conductive contact member is known that is mounted on a wiring board and provides electrical continuity between the wiring board and a case or the like. This conductive contact member is made by combining a base portion made of a thin metal plate and a contact portion formed by filling an elastomer such as silicone with a conductive filler. The metallic base portion of the conductive contact member is soldered to a circuit pattern on the wiring board by reflow soldering.

[0003] Also, as shown in Patent Document 2, a conductive rubber part that can be mounted by soldering based on surface mounting technology is known. This conductive rubber part includes a conductive rubber unit made of radical reaction curing silicone rubber mixed with a conductive filler made of silver-coated glass powder. A metal coating that can be electrically connected to a wiring board by soldering is formed on a part of the surface (compressed surface) of the conductive rubber unit. The metal coating is two or more layers, and the outermost layer is made of gold. Such a metal coating is formed on the conductive rubber unit by a sputtering method. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2003-168507 A [Patent Document 2] Patent No. 5340485 Summary of the Invention [Problem to be solved by the invention]

[0005] Although the conductive contact member has excellent conductivity and solderability, it is composed of two parts, a base part and a contact part, and therefore there is room for improvement in terms of reducing the number of parts and manufacturing costs.

[0006] Furthermore, since the conductive rubber part uses a metal coating that is prepared separately from the conductive rubber alone in order to ensure solderability to the wiring board, the manufacturing costs are high and the manufacturing process is complicated.

[0007] An object of the present invention is to provide an elastomer for soldering that can be constructed as one component and has at least solderability. Another object of the present invention is to provide an elastomer for soldering that further has electrical conductivity. [Means for solving the problem]

[0008] As a result of intensive research into achieving the above-mentioned object, the inventors discovered that a Sn-filmed filler, which is a core material coated with a Sn film made of Sn or a Sn alloy, can be exposed from the surface of an insulating elastomer including insulating rubber, and that the surface including the exposed Sn-filmed filler can be soldered to a counterpart. This led to the completion of the present invention.

[0009] The means for solving the above problems are as follows. <1> A soldering elastomer comprising an insulating elastomer containing insulating rubber, a core material coated with a Sn film made of Sn or a Sn alloy, and a filler with a Sn film contained in the insulating elastomer, the filler having a Sn film being comprised of a surface of the insulating elastomer and the filler with a Sn film exposed from the surface, and the soldering surface being capable of being soldered to a counterpart.

[0010] <2> The content (mass%) of the Sn-filmed filler is 55 mass% or more. <1> 2. The soldering elastomer according to claim 1 .

[0011] <3> The insulating rubber is made of heat-resistant rubber having a heat-resistant temperature of 200° C. or higher. <1> or <2> 2. The soldering elastomer according to claim 1 . Effect of the Invention

[0012] According to the present invention, it is possible to provide an elastomer for soldering that can be configured as one component and has at least solderability. According to another aspect of the present invention, it is possible to provide an elastomer for soldering that further has electrical conductivity. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a perspective view showing a schematic configuration of an elastomer for soldering according to a first embodiment; [Diagram 2] An explanatory diagram showing a schematic diagram of the bottom surface of the soldering elastomer [Diagram 3] Schematic cross-sectional view of a filler with Sn film [Figure 4] An explanatory diagram showing a schematic view of a part of a cross section of a soldering elastomer [Diagram 5] FIG. 1 is an explanatory diagram showing a state in which a soldering elastic body is fixed by soldering onto a wiring layer provided on the surface of a wiring board. [Figure 6] 13A and 13B are perspective views each showing a schematic configuration of a cubic and a sheet-shaped soldering elastic body according to another embodiment; [Figure 7] 1 is a side view of an elastomer for soldering according to another embodiment; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] [Elastic body for soldering] Hereinafter, the soldering elastic body 1 according to the first embodiment of the present invention will be described. Fig. 1 is a perspective view showing a schematic configuration of the soldering elastic body 1 according to the first embodiment, and Fig. 2 is an explanatory view showing a schematic bottom surface 3 of the soldering elastic body 1.

[0015] The soldering elastomer 1 of the present embodiment 1 is generally cylindrical, and has a top surface 2, a bottom surface 3, and a peripheral surface 4. Such a soldering elastomer 1 is made of a cylindrical insulating elastomer 5 containing insulating rubber, and contains a predetermined amount of Sn-filmed filler 6.

[0016] The insulating elastomer 5 is a base material containing the Sn-coated filler 6, and contains insulating rubber as a main component. The insulating rubber is contained in an amount of 90 mass % or more, preferably 95 mass % or more, and more preferably 98 mass % or more, based on the total mass (100 mass %) of the insulating elastomer 5. In this specification, the "insulating" of the insulating elastomer 5 and insulating rubber refers to, for example, a material having a volume resistivity of 1×10 in the state of a composition and / or a cured product. 10 In this specification, the volume resistivity is determined by a measurement method in accordance with JIS K 7194.

[0017] In particular, the insulating rubber is preferably a heat-resistant rubber having a heat resistance of 200° C. or higher so that it can be used in a reflow soldering process. Examples of such insulating rubber include silicone rubber and fluorine-based rubber.

[0018] The silicone rubber is not particularly limited as long as it does not impair the object of the present invention, but millable silicone rubber is preferred from the viewpoint of ease of mixing with the Sn film-coated filler 6. Millable silicone rubber is a silicone rubber compound whose pre-cured state is similar to unvulcanized compounded rubber such as natural rubber or ordinary synthetic rubber, and which can be plasticized and mixed with a kneading roll machine or an internal mixer.

[0019] Examples of the millable silicone rubber that can be used include KE-571-U, KE-1571-U, KE-951-U, KE-541-U, KE-551-U, KE-561-U, KE-961T-U, KE-1541-U, KE-1551-U, KE-941-U, and KE-971T-U manufactured by Shin-Etsu Chemical Co., Ltd. These silicone rubbers may be used alone or in combination of two or more kinds.

[0020] The fluororubber is not particularly limited as long as it does not impair the object of the present invention, and examples of the fluororubber that can be used include fluorosilicone rubber, tetrafluoroethylene-propylene rubber, vinylidene fluoride-hexafluoropropylene rubber, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene rubber, fluorinated polyether, etc. These may be used alone or in combination of two or more kinds.

[0021] In addition, the insulating elastomer 5 may contain a base material rubber component or a resin component other than the insulating rubber, as long as the object of the present invention is not impaired. In addition, the insulating elastomer 5 may contain a vulcanizing agent, a hardening agent, a plasticizer, a foaming agent, etc., as necessary.

[0022] 2, on the bottom surface 3 of the soldering elastomer 1, a large number of Sn-coated fillers 6 are exposed from the surface 50 of the insulating elastomer 5 so as to be dotted on the surface. Such a bottom surface 3 is composed of the surface 50 of the insulating elastomer 5 and a large number of Sn-coated fillers 6 exposed from the surface 50, and constitutes a soldering surface 3 that can be soldered to a counterpart, as described below. In this embodiment, similarly to the bottom surface 3, a large number of Sn-coated fillers 6 are exposed from the surface 50 of the insulating elastomer 5 on the top surface 2 and the peripheral surface 4 of the soldering elastomer 1. In particular, similarly to the bottom surface 3, the top surface 2 can be a soldering surface that can be soldered.

[0023] 3 is a cross-sectional view that shows a schematic representation of the Sn-filmed filler 6. The Sn-filmed filler 6 is formed by coating a core material 61 with a Sn film 62 made of Sn or a Sn alloy.

[0024] The core material 61 is a conductive or non-conductive material in the shape of a general filler. The shape of the core material 61 is not particularly limited as long as it does not impair the object of the present invention, and examples thereof include needle-like, spherical, flat, block-like, disk-like, and dendrite-like shapes. In addition, the conductive core material 61 is not particularly limited as long as it does not impair the object of the present invention, and examples thereof include metal / alloy powders such as copper powder, copper alloy powder, silver powder, and silver alloy powder. These may be used alone or in combination of two or more kinds.

[0025] The shape of the core material 61 is preferably flat, for example, from the viewpoint of easily and reliably bringing the Sn-filmed fillers 6 into contact with each other within the insulating elastomer body 5. As a method for producing the flat core material 61, for example, a spherical metal powder (e.g., copper powder) can be mechanically processed into a flat shape to obtain the flat metal powder.

[0026] The non-conductive core material 61 is not particularly limited as long as it does not impair the object of the present invention, and examples thereof include plastic powder, glass powder, etc. These may be used alone or in combination of two or more. A conductive Sn film 62 made of Sn (tin) or a Sn (tin) alloy is formed so as to cover the surface of such core material 61.

[0027] There are no particular limitations on the method for forming the Sn film 62 on the surface of the core material 61 as long as it does not impair the object of the present invention, but for example, when coating the surface of copper powder that is the core material with Sn, an electroless Sn plating method may be used. Examples of electroless Sn plating include substitution type Sn plating in which Sn ions in a plating solution are reduced and precipitated as the underlying copper powder (core material) dissolves, reduction type Sn plating in which Sn coating is performed by reducing Sn ions in a plating solution with a reducing agent, and disproportionation reaction type Sn plating in which Sn coating is performed by utilizing the disproportionation reaction of Sn ions to become metallic Sn.

[0028] In addition, when coating a Sn alloy by Sn alloy plating, a Sn alloy coating can be formed by adding soluble salts of alloy-constituting silver, bismuth, zinc, etc. to a substitution type Sn plating solution, a reduction type Sn plating solution, or a disproportionation reaction type Sn plating solution, and precipitating these metals simultaneously with Sn.

[0029] When the Sn-coated filler 6 is spherical, lumpy, or the like, its particle size (average particle size) is not particularly limited as long as it does not impair the object of the present invention, and may be, for example, 10 μm to 20 μm. The particle size (average particle size) is the volume-based average particle size (D50) determined by a laser diffraction scattering type particle size distribution measurement method.

[0030] Furthermore, when the Sn-coated filler 6 is needle-like, flat, or the like, its particle size (average particle size) is expressed by an average major axis diameter and an average minor axis diameter. The average major axis diameter of the Sn-coated filler 6 is not particularly limited as long as it does not impair the object of the present invention, and may be, for example, 5 μm to 50 μm. The average major axis diameter of the Sn-coated filler 6 may be 4 to 30 times its average minor axis diameter. The average minor axis diameter of the Sn-coated filler 6 is not particularly limited as long as it does not impair the object of the present invention, and may be, for example, 0.2 μm to 1.1 μm.

[0031] The average major axis diameter and the average minor axis diameter of the Sn-coated filler 6 are determined by measuring the major axis diameter (maximum diameter) and minor axis diameter of 100 Sn-coated fillers 6 based on images obtained by a scanning electron microscope or a transmission electron microscope, and averaging them. The minor axis diameter of the Sn-coated filler 6 is defined as the length of the axis perpendicular to the major axis diameter.

[0032] The Sn film-coated filler 6 is blended into the insulating elastomer 5 at a predetermined ratio that takes into consideration ensuring at least the solderability of the soldering elastomer 1. In the soldering elastomer 1 (100 mass%), the content (mass%) of the Sn film-coated filler is preferably 55 mass% or more. When the content of the Sn film-coated filler is within this range, the solderability of the soldering elastomer 1 is easily ensured.

[0033] In addition to ensuring solderability, the content (mass %) of the Sn-filmed filler may be set in consideration of ensuring electrical conductivity. The content (mass %) of the Sn-filmed filler is more preferably 60 mass % or more, and even more preferably 65 mass % or more. There is no particular upper limit to the content (mass %) of the Sn-filmed filler as long as it does not impair the object of the present invention, but from the viewpoint of ease of molding the soldering elastic body 1, it is preferably 75 mass % or less, and more preferably 70 mass % or less.

[0034] FIG. 4 is an explanatory diagram showing a schematic representation of a part of a cross section of the soldering elastomer 1. FIG. 4 shows a part of a cross section of the soldering elastomer 1 cut along the vertical direction. As shown in FIG. 4, inside the insulating elastomer 5, a conductive path 7 is formed in which the Sn-filmed fillers 6 are connected to each other. If many such conductive paths 7 are formed inside the insulating elastomer 5, the conductivity of the soldering elastomer 1 is ensured. The conductive paths 7 are formed in various directions, and the conductivity of the soldering elastomer 1 is isotropic. The soldering elastomer 1 is used to ensure conductivity between the top surface 2 and the bottom surface 3, for example. The conductive paths 7 may be formed on the surfaces (top surface 2, bottom surface 3, and peripheral surface 4) of the soldering elastomer 1.

[0035] The elastomer for soldering 1 may contain other components such as antioxidants, ultraviolet absorbers, colorants, fillers, and flame retardants in addition to the Sn film-covered filler 6, as long as the object of the present invention is not impaired.

[0036] The soldering elastomer 1 can be produced, for example, by the following method. An insulating rubber (for example, silicone rubber) having fluidity is mixed with the Sn-filmed filler 6 to fill the insulating rubber with the Sn-filmed filler 6. Examples of a method for mixing the insulating rubber and the Sn-filmed filler 6 include a method of kneading using a machine such as a vacuum degassing mixer, and a method of kneading using an extrusion, two-roll, kneader, Banbury mixer, etc. If necessary, a hardening retarder, an antioxidant, a flame retardant, a plasticizer, etc. may be added to the insulating rubber having fluidity. In another embodiment, a semi-solid material such as a pellet may be used as the insulating rubber to be mixed with the Sn-filmed filler 6.

[0037] Next, the mixture composition obtained by mixing the insulating rubber having fluidity and the Sn-coated filler 6 is molded. Examples of the molding method include known molding methods such as press molding, injection molding, extrusion molding, coater, and calendar roll. The soldering elastic body 1 shown in FIG. 1 is manufactured, for example, by press molding using a predetermined mold.

[0038] FIG. 5 is an explanatory diagram showing a state in which the soldering elastic body 1 is fixed by soldering on the wiring layer E provided on the surface of the wiring board. FIG. 5 shows a schematic cross section of the soldering elastic body 1. The bottom surface 3 of the soldering elastic body 1 is a solderable soldering surface 3, and the soldering surface 3 is joined to the wiring layer E via a solder layer 8. During such soldering, the Sn film 62 of the Sn film-attached filler 6 exposed from the soldering surface 3 melts and is joined to the solder layer 8. The wiring layer (copper foil) E is joined while forming an alloy layer between the Sn film and the solder layer 8. Note that the Sn film 62 of the Sn film-attached filler 6 exposed from the soldering surface 3 may be partially melted and directly joined to the wiring layer (copper foil) E. A fillet 9 made of solder is formed around the soldering surface (bottom surface) 3 of the soldering elastic body 1. In this manner, the elastic body for soldering 1 is soldered to the mating wiring layer E. For ease of explanation, only the Sn-filmed filler 6 present near the bottom surface 3 is shown in FIG.

[0039] Such an elastomer for soldering 1 can be mounted by soldering using surface mount technology (SMT), and is mounted, for example, on a wiring board (printed wiring board, etc.) of an electronic device, etc. The process for soldering the elastomer for soldering 1 may be a flow soldering process or a reflow soldering process.

[0040] The soldering elastomer 1 may be used in a state where it is sandwiched so as to be compressed in the vertical direction. For example, the bottom surface (soldering surface) 3 of the soldering elastomer 1 may be mounted on a wiring board, and the top surface 2 may be brought into contact with a housing (ground) that houses the wiring board.

[0041] As described above, the soldering elastomer 1 of this embodiment can be configured as one component, and can be soldered to a mating part such as a wiring board (has solderability). Furthermore, the soldering elastomer 1 of this embodiment also has electrical conductivity as described above.

[0042] In addition, when the soldering elastic body 1 has electrical conductivity, the volume resistivity is, for example, 1×10 10 It is preferably less than Ω·cm. EXAMPLES

[0043] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to these examples in any way.

[0044] Example 1 Silicone rubber (product name "KE-941-U", manufactured by Shin-Etsu Chemical Co., Ltd.) was prepared as insulating rubber (heat-resistant rubber). In addition, Sn-plated copper powder was prepared by plating the surface of flat copper powder with Sn as a filler with Sn film. The Sn-plated copper powder was flat, with an average major axis diameter of 7 μm and an average minor axis diameter of 1 μm. The Sn plating content in the Sn-plated copper powder was 26.03 mass%. 100 mass parts of this silicone rubber were mixed with 129.6 mass parts of flat Sn-plated copper powder and 1 mass part of a vulcanizing agent, and the resulting mixed composition was press-molded to obtain an elastic body for soldering (diameter 9 mm x height 10 mm, cylindrical shape) of Example 1.

[0045] Example 2 An elastic body for soldering of Example 2 was produced in the same manner as in Example 1, except that the amount of Sn-plated copper powder was changed to 194.4 parts by mass.

[0046] Comparative Example 1 An elastic body for soldering of Example 2 was produced in the same manner as in Example 1, except that the amount of Sn-plated copper powder was changed to 116.6 parts by mass.

[0047] [Implementation test] For each of the elastomer bodies for soldering in Examples 1 and 2 and Comparative Example 1, a mounting test was carried out in the following manner.

[0048] A substrate (polyimide substrate) with a copper foil wiring pattern formed on its surface was prepared. A solder paste was applied onto the wiring pattern of the substrate, and a soldering elastomer was placed on the solder paste with its bottom surface in contact with the solder paste. The substrate with the soldering elastomer placed thereon was placed in a specified heating furnace, and heated for 30 to 60 seconds (5 to 10 seconds at 250°C) while increasing the temperature from 220°C to 250°C. The substrate was then removed from the heating furnace and air-cooled to obtain a substrate with a soldering elastomer mounted thereon (hereinafter referred to as a "mounted product").

[0049] (Implementation Experiment A) The mounted product obtained as described above was first placed so that the soldering elastic body faced downward and was maintained in this state for 300 seconds. Then, while maintained in this state, it was confirmed whether the soldering elastic body of the mounted product peeled off from the board and fell due to its own weight.

[0050] (Implementation Experiment B) Next, the mounted product was placed so that the soldering elastic body faced sideways and the board surface (mounting surface) was aligned vertically (i.e., the soldering elastic body was laid on its side), and this state was maintained for 300 seconds. Then, while this state was maintained, it was confirmed whether the soldering elastic body of the mounted product peeled off from the board and fell due to its own weight.

[0051] In either case of the above mounting experiment A or B, if the soldering elastomer did not peel off from the board, the result of the mounting experiment was good, and is indicated as "O" in Table 1. Also, in either case of the above mounting experiment A or B, if the soldering elastomer peeled off from the board, the result of the mounting experiment was not good, and is indicated as "X" in Table 1. The results are shown in Table 1.

[0052] [Table 1]

[0053] As shown in Table 1, it was confirmed that the soldering elastomers of Examples 1 and 2 had excellent solderability. In contrast, it was confirmed that the soldering elastomer of Comparative Example 1, which has a lower content of Sn-plated copper powder than Examples 1 and 2, did not have sufficient solderability. Specifically, during the above mounting experiment B, the soldering elastomer peeled off from the board.

[0054] <Other embodiments> The present invention is not limited to the embodiments described above and illustrated in the drawings, and the following embodiments, for example, are also included within the technical scope of the present invention.

[0055] (1) In the above embodiment, the soldering elastomer is shaped like a cylinder, but the present invention is not limited thereto. The soldering elastomer may have various shapes depending on the application. For example, as shown in FIG. 6, the soldering elastomer may be a cube-shaped soldering elastomer 1A or a sheet-shaped soldering elastomer 1B. In still another embodiment, the soldering elastomer may be a cylinder-shaped soldering elastomer 1C with a narrowed peripheral surface, as shown in FIG. 7. When compressed in the vertical direction, the soldering elastomer 1C is prevented from protruding outward beyond the top or bottom surface, even if the narrowed portion is deformed so as to spread outward.

[0056] (2) The solder used when soldering the elastomer for soldering is not particularly limited as long as it does not impair the object of the present invention. For example, common solder containing tin or lead, lead-free solder, etc. can be used.

[0057] (3) In the elastomer for soldering, the Sn-filmed filler may be uniformly dispersed in the insulating elastomer or may be partially unevenly distributed therein, as long as the object of the present invention is not impaired. For example, the Sn-filmed filler may be unevenly distributed only near the surface of the insulating elastomer, or may be gathered in a specific direction in the insulating elastomer.

[0058] (4) In the above embodiment 1, the Sn-filmed filler was exposed in a dotted pattern on the soldering surface of the soldering elastomer, but the present invention is not limited to this. For example, a large number of Sn-filmed fillers may be exposed in a regular or irregular pattern (concentric circles, mosaic pattern) overall. [Explanation of symbols]

[0059] 1...elastic body for soldering, 2...upper surface, 3...bottom surface (soldering surface), 4...periphery, 5...insulating elastic body, 6...filler with Sn film, 61...core material, 62...Sn film, 7...conductive path, 8...solder layer, 9...fillet, E...wiring layer

Claims

1. an insulating elastomer including an insulating rubber made of a heat-resistant rubber having a heat-resistant temperature of 200° C. or higher; The insulating elastomer comprises a flat core material covered with a Sn film made of Sn or a Sn alloy, and a filler with a Sn film is contained in the insulating elastomer; a soldering surface including a surface of the insulating elastomer and the Sn-film-attached filler exposed from the surface, the soldering surface being capable of being soldered to a counterpart; The content (mass%) of the Sn-filmed filler is 55 mass% or more and 75 mass% or less, The elastic body for soldering, wherein the average major axis diameter of the Sn film-attached filler is 5 μm to 50 μm, and the average minor axis diameter of the Sn film-attached filler is 0.2 μm to 1.1 μm.

2. 2. The elastomer for soldering according to claim 1, wherein said insulating rubber is silicone rubber.

Citation Information

Patent Citations

  • Method of conveying blank to press machines and and table used for same

    JP1978040485A

  • Conductive auxiliary member and connector empoying the conductive auxiliary member

    JP1996190950A

  • Conductive contact member

    JP2003168507A

  • Space transforming land grid array interposers

    US20070232090A1