Converter lining structure and converter repair method

By employing magnesia carbon bricks with controlled particle sizes and graphite content, and optimizing slag coating conditions, the peeling and wear issues in thermal spray and slag coating methods are mitigated, improving the durability and thermal shock resistance of converter linings.

JP7553801B2Active Publication Date: 2024-09-19NIPPON STEEL CORPORATION
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2020197098
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-13
Filing Date
2020-11-27
Publication Date
2024-09-19
Estimated Expiration
2040-11-27

AI Technical Summary

Technical Problem

Existing thermal spray repair methods for magnesia carbon bricks in converters face issues with peeling and wear due to thermal shock, while slag coatings at lower temperatures create voids leading to peeling, compromising the protective effect.

Method used

Using magnesia carbon bricks without clinker particles smaller than 0.075 mm, combined with a specific graphite content and porosity, and applying slag coating under controlled temperature conditions to suppress void formation and improve adhesion.

Benefits of technology

The solution effectively prevents peeling and wear of the slag coating, enhancing the durability and thermal shock resistance of the refractory lining, allowing more frequent repairs and reducing exposure to thermal stress.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007553801000012
    Figure 0007553801000012
  • Figure 0007553801000011
    Figure 0007553801000011
  • Figure 0007553801000001
    Figure 0007553801000001
Patent Text Reader

Abstract

To prevent a slag-coating layer from peeling off when a lining refractory of a revolving furnace, consisting of magnesia-carbon bricks, is protected by a slag coating.SOLUTION: A lining structure for a revolving furnace has: magnesia-carbon bricks that constitute a lining refractory, wherein a content of a magnesia clinker having a grain diameter of less than 0.075 mm is 3 mass% or less (including 0); and a slag coating that is formed on an operation surface side of the lining refractory. A repairing method for the revolving furnace includes a step of forming the slag coating on the operation surface side of the lining refractory consisting of the magnesia-carbon bricks in which the content of the magnesia clinker having the grain diameter of less than 0.075 mm is 3 mass% or less (including 0).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a lining structure of a converter and a method for repairing a converter, and more particularly to a lining structure of a converter using magnesia carbon bricks as a refractory lining and a method for repairing a converter. [Background technology]

[0002] Methods for repairing magnesia carbon bricks damaged during converter blowing include thermal spray repair, in which a thermal sprayed body is sprayed from a thermal spraying device onto the working surface of the refractory, and slag coating, in which slag, a by-product of converter blowing, is applied to the working surface of the refractory to act as a protective layer.

[0003] For example, Patent Document 1 discloses a spray repair method for magnesia carbon bricks, which describes a spray repair method in which the content of magnesia clinker with a particle size of less than 0.075 mm in magnesia carbon bricks with a graphite content of 13 mass% or less is set to less than 10 mass% (including 0), thereby suppressing gas generation at the interface between the refractory material and the body to which the spray is applied, and preventing peeling of the body to which the spray is applied.

[0004] Furthermore, Patent Document 2 discloses a method for coating magnesia carbon bricks with slag, which adjusts the amount of FeO in the slag remaining in the converter by spraying gas from above, thereby controlling the viscosity of the slag and enabling the refractory material to be protected by the slag coating up to the upper part of the furnace. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2008-151425 A [Patent Document 2] JP 2011-184737 A Summary of the Invention [Problem to be solved by the invention]

[0006] In the thermal spray repair described in Patent Document 1, the temperature of the working surface of the refractory reaches nearly 2000°C during repair, which may cause the refractory to peel off and wear away due to thermal shock, or the refractory structure to deteriorate (loosening of the structure or the occurrence of cracks) due to thermal shock. On the other hand, the slag coating described in Patent Document 2 is performed at a lower temperature of about 300°C to 400°C compared to thermal spray repair, so the thermal shock during repair is smaller, and it is possible to suppress the refractory's peeling and wear away and the deterioration of the refractory structure. However, in magnesia-carbon bricks, voids are generated directly below the slag-coated working surface during operation due to the magnesia-carbon reaction shown in the following formula (1). The slag coating layer peels off from these voids, and there are cases in which the refractory cannot be sufficiently protected. MgO(s)+C(s)=Mg(g)+CO(g) ···(1)

[0007] Therefore, an object of the present invention is to provide a lining structure for a converter and a repair method for a converter that can suppress peeling of the slag coating layer when protecting the lining refractory material of the converter, which is made of magnesia carbon bricks, with a slag coating. [Means for solving the problem]

[0008] As a result of intensive research aimed at solving the above problems, the inventors have discovered that by applying a slag coating to a refractory lining made of magnesia carbon bricks that do not contain magnesia clinker having a particle size of less than 0.075 mm, it is possible to suppress the formation of voids and the spalling wear that originates from these voids, and have thus completed the present invention. (1) A magnesia carbon brick constituting a lining refractory material, the content of magnesia clinker having a particle size of less than 0.075 mm being 3% by mass or less (including 0%); A slag coating formed on the working surface of the refractory lining The lining structure of a converter having the above structure. (2) The lining structure of a converter according to (1), wherein the magnesia carbon brick contains 15% by mass or more and 17% by mass or less of graphite. (3) A lining structure for a converter according to (1) or (2), wherein the magnesia carbon brick has an apparent porosity of 6.5% or more and less than 8.7% after reduction firing at 1400°C for 10 hours. (4) A method for repairing a converter, comprising a step of forming a slag coating on the working surface side of a lining refractory material composed of magnesia carbon bricks having a magnesia clinker content of 3 mass% or less (including 0) having a particle size of less than 0.075 mm. (5) The method for repairing a converter according to (4), wherein the magnesia carbon brick contains 15% by mass or more and 17% by mass or less of graphite. (6) A method for repairing a converter according to (4) or (5), wherein the magnesia carbon brick has an apparent porosity of 6.5% or more and less than 8.7% after reduction firing at 1400°C for 10 hours. (7) A method for repairing a converter according to any one of (4) to (6), in which the temperature of the slag in the converter is reduced by 100°C or more and less than 150°C from the time when the step of forming a slag coating is carried out after the steel is tapped. Effect of the Invention

[0009] According to the present invention, peeling of the slag coating layer can be suppressed, and the durability of the refractory lining made of magnesia carbon bricks can be improved. [Brief description of the drawings]

[0010] [Figure 1] 1 is a cross-sectional view of a converter to which a repair method according to an embodiment of the present invention is applied. [Diagram 2] FIG. 1 is a schematic diagram of a microstructure observation piece cut out from the working surface side toward the back surface side of the lining refractory and the slag coating layer after an actual machine test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Fig. 1 is a cross-sectional view of a converter to which a repair method according to an embodiment of the present invention is applied. As shown in Fig. 1, the lining refractory 2 of the converter 1 is a magnesia carbon brick mainly composed of magnesia clinker and graphite. More specifically, the lining refractory 2 is a magnesia carbon brick obtained by mixing magnesia clinker and graphite having a particle size of 0.075 mm or more as a refractory raw material mixture, adding an appropriate amount of organic binder, kneading the mixture, and then molding and heat treating the mixture. A slag coating layer 3 is formed on the working surface of the lining refractory 2.

[0012] Here, magnesia clinker with a particle size of less than 0.075 mm contributes to the densification of the structure of the magnesia carbon brick and improves the corrosion resistance, while its large specific surface area accelerates the magnesia carbon reaction shown in formula (1) above. When the magnesia carbon reaction is accelerated, the magnesia clinker and graphite in the magnesia carbon brick are gasified, and the slag coating layer 3 is peeled off from the voids generated by the gasification at the interface between the lining refractory 2 and the slag coating layer 3. The present inventors, who found out this phenomenon from the observation of refractories used in actual machines, came up with the idea of ​​using magnesia carbon bricks that do not contain magnesia clinker with a particle size of less than 0.075 mm as the lining refractory 2, thereby suppressing the peeling and wear of the slag coating layer 3 attached to the working surface and continuously protecting the refractory. Incidentally, magnesia clinker smaller than 0.075 mm, which is inevitably contained in magnesia clinker of 0.075 mm or more, does not pose a problem, and even if it contains up to 3 mass %, it does not affect the effect of the present invention.

[0013] In addition, repair by slag coating can be performed frequently because the time required for repair is shorter than that for thermal spray repair. If repair by slag coating is performed frequently and the peeling wear of the slag coating layer 3 can be suppressed as described above, it is possible to operate the furnace with reduced frequency of exposure of the graphite contained in the lining refractory 2. In this case, it is not necessary to consider the liquid phase oxidation of graphite by FeO, and the graphite content of the magnesia carbon brick used in the lining refractory 2 can be increased. As an example, the graphite content of the magnesia carbon brick may be increased to 15% by mass or more and 17% by mass or less. Since graphite has high thermal conductivity, the thermal shock resistance of the lining refractory 2 is improved as the graphite content increases, enabling further peeling suppression effect.

[0014] In particular, when the operating rate of the converter 1 is low (for example, less than 20 times a day), the temperature inside the furnace repeatedly rises and falls between about 1600°C to 1800°C during operation and about 800°C to 1000°C during standby, frequently causing large thermal shocks. In such cases, by increasing the graphite content of the magnesia carbon bricks to, for example, 15% by mass or more and 17% by mass or less, it is possible to effectively suppress the spalling and wear of the refractory lining 2 caused by thermal shock.

[0015] In this embodiment, the magnesia carbon brick used for the lining refractory 2 preferably has an apparent porosity of 6.5% or more and less than 8.7% after reduction firing at 1400°C for 10 hours. By increasing the apparent porosity, the magnesia carbon brick has a low elasticity and improves the thermal shock resistance of the entire structure. As a result, even if a void is generated directly under the slag coating layer, crack growth starting from the void driven by thermal shock can be suppressed, and peeling wear can be more effectively suppressed. By suppressing peeling of the coating layer, it is possible to prevent the infiltration of molten slag into the magnesia carbon brick, and the corrosion resistance is not reduced due to the high apparent porosity. The effect of improving the thermal shock resistance by increasing the apparent porosity is more remarkable when the operating rate of the converter is low (for example, the number of operations per day is less than 15). The apparent porosity of the magnesia carbon brick used in this embodiment can be adjusted by reducing the molding pressure during production (up to 50% at most).

[0016] In this embodiment, the magnesia clinker to be mixed with the magnesia carbon bricks used in the lining refractory material 2 may be either fused magnesia or sintered magnesia. However, since sintered magnesia has a small crystal grain size and a large specific surface area, it is considered that the progress of the magnesia carbon reaction is accelerated, so it is more preferable to mix fused magnesia when repair by slag coating is assumed. As for the graphite to be mixed with the magnesia carbon bricks, since thermal shock resistance is required as described above, it is preferable to select a graphite type with high thermal conductivity, such as, but not limited to, flaky graphite.

[0017] The alloys added to the magnesia carbon bricks can be Al, Si, Mg, B4C or a combination of these. The main effects of adding alloys are oxidation prevention and densification, such as preventing the oxidation of graphite to suppress the generation of voids and densifying the structure through a spinel reaction. Adding such alloys can reduce the voids in the structure of the refractory lining 2 and enhance the effect of suppressing the peeling and wear of the slag coating layer 3.

[0018] In this embodiment, for example, slag splash coating (SSC) or furnace swinging is used as the slag coating method. SSC is a technique in which slag 4 remaining in the converter 1 is splashed onto the furnace wall (including the trunnion) using an inert gas such as nitrogen or argon sprayed from a top blowing lance after tapping, thereby forming a slag coating layer 3 on the working surface of the refractory lining 2. The furnace swinging is a technique in which the converter 1 is tilted multiple times with the slag 4 remaining in the furnace after tapping, thereby causing the slag 4 to adhere to the furnace wall (excluding the trunnion) and forming a slag coating layer 3 on the working surface of the refractory lining 2.

[0019] In the above-mentioned slag coating method, when conventional magnesia carbon bricks containing magnesia clinker of less than 0.075 mm are used as the lining refractory 2, the lining refractory 2 is exposed in many parts of the working surface due to peeling and wear of the slag coating layer 3. Since the wettability between the graphite contained in the lining refractory 2 and the slag 4 is low, in order to improve the slag adhesion, the temperature drop of the slag in the furnace from after the steel is tapped until the step of forming the slag coating (hereinafter also simply referred to as the temperature drop) needs to be relatively large, specifically 150°C or more.

[0020] In contrast, in the present embodiment, magnesia carbon bricks that do not contain magnesia clinker less than 0.075 mm are used for the lining refractory 2, thereby suppressing the peeling and wear of the slag coating layer 3, and therefore the lining refractory 2 is not exposed in many parts of the working surface. Compared to the case where the lining refractory 2 containing graphite is exposed, the wettability between the slag coating layer 3 already formed on the working surface and the slag 4 is high, so the temperature drop is relatively small, specifically, it may be 100°C or more and less than 150°C.

[0021] The temperature drop of the slag in the furnace can be measured using a thermoviewer when the converter 1 is tilted. Taking into account the viscosity of the slag, it is desirable that the temperature drop be 100°C or more and 250°C or less. If the temperature drop exceeds 250°C, the slag has a low temperature and a large solid phase, which increases the viscosity and reduces the slag's scattering ability, thereby limiting the range of the working surface on which the slag coating layer 3 is formed. On the other hand, if the temperature drop is less than 100°C, the slag's temperature is high and the viscosity is too low, reducing the adhesion of the slag to the working surface.

[0022] If the temperature drop of the slag 4 is not sufficient, the temperature is lowered by adding auxiliary materials to the slag remaining in the converter 1 after the steel tapping. As such auxiliary materials, raw dolomite or magnesia can be used, for example. Here, as described above, when the conventional magnesia carbon bricks containing magnesia clinker of less than 0.075 mm are used for the lining refractory 2, the temperature drop needs to be 150°C or more, and therefore, the addition of auxiliary materials is required. On the other hand, when the magnesia carbon bricks not containing magnesia clinker of less than 0.075 mm are used for the lining refractory 2 in this embodiment, the temperature drop only needs to be 100°C or more, so that the addition of auxiliary materials becomes unnecessary or the amount of auxiliary materials added can be reduced compared to the conventional case.

[0023] In addition, the amount of FeO in the slag 4 during slag coating is controlled by oxygen blowing using a top blowing lance or the like, but if the amount or time of oxygen blowing is too long, the magnesia carbon bricks of the lining refractory 2 may be damaged. In addition, if the amount of FeO in the slag 4 is too large, the melting point of the slag 4 becomes too low, and the adhesiveness of the slag decreases. Therefore, it is preferable that the amount of FeO in the slag 4 is 30 mass% or less. This reduces the effect of oxygen blowing on the lining refractory 2 and increases the adhesiveness of the slag, thereby enhancing the protective effect of the slag coating layer 3 on the lining refractory 2. EXAMPLES

[0024] Hereinafter, the embodiment of the present invention will be described with reference to examples.

[0025] Figure 2 is a schematic diagram of a 15 mm square microstructure observation piece cut from the working surface side of the refractory lining 2 and the slag coating layer 3 of a converter 1 after the actual machine test toward the back surface side. As shown in the figure, after the actual machine test, a void 5 was generated at the interface between the slag coating layer 3 formed on the working surface side and the refractory lining 2 of the magnesia-carbon brick. The void 5 was mainly generated by the magnesia-carbon reaction, and as mentioned above, the void 5 was the starting point for the peeling of the slag coating layer 3.

[0026] Tables 1 to 3 show the results of an investigation carried out in an actual machine into the effect of the presence or absence of magnesia clinker with a particle size of less than 0.075 mm (hereinafter also referred to as fine magnesia clinker) mixed into the magnesia carbon brick of the lining refractory on the wear rate of the lining refractory. Examples 1-1 to 3 are examples of magnesia carbon bricks that do not contain fine magnesia clinker. In these examples, the void index was smaller and the wear rate index was also smaller than those of Comparative Examples 1 to 3, which are magnesia carbon bricks that contain fine magnesia clinker. The void index and wear rate index will be described later. The converter operating rate is the number of times the converter is operated per day.

[0027] [Table 1]

[0028] [Table 2]

[0029] [Table 3]

[0030] In the results of the above examples, the void index is an index of the size of the void 5 at the interface between the refractory lining 2 and the slag coating layer 3. The void index in each example is shown with the void index in the corresponding comparative example taken as 100. It is considered that the higher the void index, the more likely the slag coating layer 3 is to peel off. To calculate the void index, a structural observation piece as shown in FIG. 2 is used. The cut-out structural observation piece is vacuum-impregnated with epoxy resin, mirror-polished, and observed under an optical microscope, and the void index is calculated by the following formula (2). Here, the specified range is a range of 6 mm from the uppermost end 5a of the void 5 (the part of the void closest to the working surface) toward the back surface, as shown by reference symbol 6 in FIG. 2. Void index = (void area) × (specified area) (2)

[0031] On the other hand, the wear rate index is an index of the wear rate of the refractory lining 2, and a smaller value indicates a slower wear rate. The wear rate index in each example is shown with the wear rate index in the corresponding comparative example set at 100. Since the refractory lining 2 itself is repaired in addition to slag coating in an actual converter, the wear rate was calculated for the operating period of the converter 1 excluding the end of the furnace period (after 2000 operations). This makes it possible to calculate the wear rate excluding the effects of repairs other than slag coating.

[0032] From the above results, it is seen that the use of magnesia carbon bricks that do not contain magnesia clinker with a particle size of less than 0.075 mm as the lining refractory suppresses the generation of voids and the spalling wear of the lining refractory starting from the voids. In particular, in the magnesia carbon brick examples 1-1, 1-2 and 2-1, 2-2 in which the graphite content is 15 mass% or more and 17 mass% or less, the void index and wear rate index are smaller than those of Example 3 in which the graphite content is 13 mass%, and it is seen that the thermal shock resistance is improved by increasing the graphite content, and the generation of voids and the spalling wear of the lining refractory starting from the voids are more effectively suppressed.

[0033] Table 4 shows the results of an investigation using an actual furnace into the effect of the temperature drop in the slag inside the furnace after tapping until slag coating is performed on the adhesion of slag to the lining refractory. The adhesion of slag was evaluated based on the thickness of the slag coating layer on the working surface of the refractory after slag coating. In the examples of magnesia carbon bricks not containing fine magnesia clinker shown in Examples 4 to 6, it has been confirmed that a sufficient thickness of the slag coating layer is obtained compared to the comparative examples, even when the temperature drop is low (100°C≦temperature drop<150°C).

[0034] [Table 4]

[0035] Tables 5 to 7 show the results of investigating the wear rate of magnesia carbon bricks with reduced molding pressure and increased apparent porosity in an actual converter (operated about 13 times per day). Examples 7-1, 7-2, 7-3, 8-1, 8-2, 8-3, 9-1, 9-2 and 9-3 (hereinafter also referred to as the first group of examples) are examples of magnesia carbon bricks with reduced molding pressure and increased apparent porosity. On the other hand, Examples 7-4, 8-4 and 9-4 (hereinafter also referred to as the second group of examples) are examples of magnesia carbon bricks manufactured with normal molding pressure that is not reduced. In the first group of examples, the thermal shock resistance was improved and the wear rate index was smaller than in the second group of examples. In particular, the wear rate index is smaller in Examples 7-3, 8-3 and 9-3 than in Examples 7-4, 8-4 and 9-4. These results show that increasing the apparent porosity of magnesia carbon bricks improves their thermal shock resistance and enables a further reduction in the wear rate index.

[0036] [Table 5]

[0037] [Table 6]

[0038] [Table 7]

[0039] Tables 8 to 10 show the results of investigating the effect of the temperature drop of the slag in the furnace until the slag coating is performed after tapping on the adhesion of the slag to the lining refractory, using magnesia carbon bricks with reduced molding pressure and increased apparent porosity, in an actual converter (operated about 13 times per day). Examples 10-1, 10-2, 10-3, 11-1, 11-2, 11-3, 12-1, 12-2 and 12-3 (hereinafter also referred to as the third group of examples) are examples of magnesia carbon bricks with reduced molding pressure and increased apparent porosity. On the other hand, Examples 10-4, 11-4 and 12-4 (hereinafter also referred to as the fourth group of examples) are examples of magnesia carbon bricks manufactured with normal molding pressure that is not reduced. The third example group, in which the apparent porosity of the magnesia carbon brick was increased, also had a sufficient slag coating layer thickness equivalent to that of the fourth example group, in which the apparent porosity was normal. Furthermore, in examples 10-3, 11-3, and 12-3 of the third example group, the slag coating layer had a sufficient thickness equivalent to that of the magnesia carbon brick, in spite of the small temperature drop of 100°C. This shows that a sufficient slag coating layer thickness can be obtained even when a magnesia carbon brick with increased apparent porosity due to reduced molding pressure is used.

[0040] [Table 8]

[0041] [Table 9]

[0042] [Table 10] [Explanation of symbols]

[0043] 1...converter, 2...refractory lining, 3...slag coating layer, 4...slag, 5...gap, 5a...top end, 6...specified area.

Claims

1. a magnesia carbon brick which constitutes a lining refractory material, does not contain magnesia clinker having a particle size of less than 0.075 mm, contains 15% by mass or more and 17% by mass or less of graphite, and has an apparent porosity of 6.5% or more and less than 8.7% after reduction firing at 1400°C for 10 hours; a slag coating formed on the working surface of the refractory lining; The lining structure of a converter having the above structure.

2. A method for repairing a converter, comprising a step of forming a slag coating on a working surface side of a lining refractory material made of magnesia carbon bricks, which does not contain magnesia clinker with a particle size of less than 0.075 mm, contains 15 mass % or more and 17 mass % or less of graphite, and has an apparent porosity of 6.5% or more and less than 8.7% after reduction firing at 1,400°C for 10 hours.

3. 3. The method for repairing a converter according to claim 2, wherein the temperature of the slag in the converter is reduced by 100° C. or more and less than 150° C. from the time of tapping until the step of forming the slag coating is carried out.

4. A method for repairing a converter as described in claim 2 or claim 3, wherein the converter is operated less than 20 times per day.

Citation Information

Patent Citations

  • Graphite-containing refractory having high strength

    JP1992260655A

  • Magnesia-carbon brick for inner lining of vessel for molten metal

    JP1995017758A

  • Method for coating slag on inner wall surface of converter

    JP1997209022A

  • Magnesia-carbon type refractory

    JP2007297246A

  • Repair method of magnesia carbon brick

    JP2008151425A