Nitride semiconductor photocatalytic thin film
The nitride semiconductor photocatalytic thin film with a structured catalyst layer and protective coating addresses the efficiency decline in conventional devices by reducing etching, thereby enhancing the longevity and performance of water splitting reactions.
Patent Information
- Application Number
- JP2022527272
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-05-25
- Publication Date
- 2024-09-19
- Estimated Expiration
- 2040-05-25
AI Technical Summary
Conventional water decomposition devices with nitride semiconductor photocatalysts face issues of complexity, size, and a decrease in light energy conversion efficiency due to side reactions like etching, which degrade the photocatalytic thin film over time.
A nitride semiconductor photocatalytic thin film with a conductive substrate, a first catalyst layer forming an ohmic junction, a second catalyst layer forming a Schottky junction, and a protective layer to cover the substrate and side surfaces, all made of materials with the same crystal structure, reducing dislocation density and suppressing etching reactions.
The solution extends the lifespan of solar energy conversion efficiency by minimizing etching and maintaining high hydrogen and oxygen production rates over extended light irradiation periods.
Smart Images

Figure 0007553836000004 
Figure 0007553836000005 
Figure 0007553836000008
Abstract
Description
[Technical field]
[0001] The present invention relates to a nitride semiconductor photocatalytic thin film and a method for producing the nitride semiconductor photocatalytic thin film. [Background technology]
[0002] The water splitting reaction using a photocatalyst consists of a water oxidation reaction and a proton reduction reaction.
[0003] Oxidation reaction: 2H2O+4h + →O2+4H + Reduction reaction: 4H + +4e - →2H2
[0004] When light is irradiated onto an n-type photocatalytic material, electrons and holes are generated and separated within the photocatalyst. The holes move to the surface of the photocatalytic material and contribute to the reduction reaction of protons. Meanwhile, the electrons move to the reduction electrode and contribute to the reduction reaction of protons. Ideally, this type of oxidation-reduction reaction proceeds, resulting in a water splitting reaction.
[0005] A conventional water decomposition device has an oxidation tank and a reduction tank connected via a proton exchange membrane, and an aqueous solution and an oxidation electrode are placed in the oxidation tank, and an aqueous solution and a reduction electrode are placed in the reduction tank. The oxidation electrode and the reduction electrode are electrically connected by a conductor. The oxidation electrode is, for example, a nitride semiconductor, titanium oxide, or amorphous silicon. The reduction electrode is a metal or a metal compound, for example, nickel, iron, gold, platinum, silver, copper, indium, or titanium. The water decomposition reaction is caused by irradiating light from a light source with a wavelength that can be absorbed by the material that constitutes the oxidation electrode. For example, when the oxidation electrode is made of gallium nitride, the absorbable wavelength is a wavelength of 365 nm or less. The light source is, for example, a xenon lamp, a mercury lamp, a halogen lamp, a pseudo-sun light source, or sunlight, or a combination of these. [Prior art documents] [Non-patent literature]
[0006] [Non-Patent Document 1] S. Yotsuhashi, et al., “CO2 Conversion with Light and Water by GaN Photoelectrode”, Japanese Journal of Applied Physics 51 (2012) 02BP07 [Non-Patent Document 2] SY Reece, et al., “Wireless Solar Water Splitting Using Silicon-Based Semiconductors and Earth-Abundant Catalysts”, Science, 2011, Volume 334, pp. 645-648 Summary of the Invention [Problem to be solved by the invention]
[0007] The water splitting device as described above has many components and a complex reaction system, so that it is desirable to realize a simpler reaction system and to make the reaction system smaller. For example, a device configured with a photocatalytic thin film and an aqueous solution placed in a photocatalytic tank is used, and the photocatalytic thin film in the aqueous solution is irradiated with light from a light source to cause a water splitting reaction. The photocatalytic thin film is a nitride semiconductor, titanium oxide, or amorphous silicon, like the oxidation electrode. A metal promoter that promotes the water splitting reaction is supported on the surface of the photocatalytic thin film. The reaction system of this device is simple, and it is expected that the system can be reduced in cost and size.
[0008] However, even in devices with a simple configuration, there was a problem in that the light energy conversion efficiency of the photocatalytic thin film decreased with increasing light irradiation time.
[0009] For example, a gallium nitride thin film grown on a sapphire substrate is used as the photocatalytic thin film. When the gallium nitride thin film is irradiated with light in an aqueous solution, a GaN etching reaction takes place as a side reaction on the gallium nitride surface in addition to the intended water oxidation reaction.
[0010] Etching reaction: 2GaN+3H2O+6h + →N2+Ga2O3+6H +
[0011] As the etching reaction progresses, the reaction sites in which the target reaction can proceed decrease, causing a problem in that the solar energy conversion efficiency decreases within a few hours.
[0012] The present invention has been made in view of the above, and has an object to realize a long life of the solar energy conversion efficiency of a semiconductor photocatalytic thin film. [Means for solving the problem]
[0013] The nitride semiconductor photocatalytic thin film according to one embodiment of the present invention is a nitride semiconductor photocatalytic thin film that exhibits catalytic function by irradiation with light to cause an oxidation-reduction reaction, and has an electrically conductive n-GaN A substrate and a substrate disposed on a surface of the substrate. Nitride A semiconductor thin film and the Nitrides An ohmic junction is formed on a part of the surface of the semiconductor thin film, and a first catalyst layer which is a promoter for a reduction reaction; Nitride A Schottky junction is formed on a part of the surface of the semiconductor thin film, and a second catalyst layer which is a promoter for an oxidation reaction is formed on the back surface of the substrate and on the substrate and the Nitride A protective layer is disposed so as to cover the side surface of the semiconductor thin film, Nitride Semiconductor thin films contain the same elements and have the same crystal structure. R . Effect of the Invention
[0015] According to the present invention, it is possible to realize an extension of the life span of the solar energy conversion efficiency of a semiconductor photocatalytic thin film. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a cross-sectional view showing the configuration of the nitride semiconductor photocatalytic thin film of this embodiment. [Diagram 2]FIG. 2 is a diagram for explaining a first catalytic layer and a second catalytic layer dispersed on the surface of the nitride semiconductor photocatalytic thin film. [Diagram 3] FIG. 3 is a cross-sectional view showing the configuration of another nitride semiconductor photocatalytic thin film of the present embodiment. [Figure 4] FIG. 4 is a flowchart showing a method for manufacturing the nitride semiconductor photocatalytic thin film of FIG. [Diagram 5] FIG. 5 is a flowchart showing a method for manufacturing the nitride semiconductor photocatalytic thin film of FIG. [Figure 6] FIG. 6 is a diagram showing an outline of an apparatus for carrying out an oxidation-reduction reaction test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. Note that the present invention is not limited to the embodiment described below, and modifications may be made without departing from the spirit of the present invention.
[0018] [Composition of nitride semiconductor photocatalytic thin film] Fig. 1 is a cross-sectional view showing an example of the configuration of the nitride semiconductor photocatalytic thin film of this embodiment. The nitride semiconductor photocatalytic thin film of Fig. 1 is a nitride semiconductor photocatalytic thin film that exerts a catalytic function and causes an oxidation-reduction reaction when irradiated with light in an aqueous solution.
[0019] The nitride semiconductor photocatalytic thin film 1 shown in Figure 1 comprises a conductive substrate 11, a semiconductor thin film 12 arranged on the surface of the substrate 11, a first catalytic layer 13 that forms an ohmic junction on part of the surface of the semiconductor thin film 12, a second catalytic layer 14 that forms a Schottky junction on part of the surface of the semiconductor thin film 12, and a protective layer 15 formed to cover the back surface of the substrate 11 and the side surfaces of the substrate 11 and the semiconductor thin film 12.
[0020] The substrate 11 and the semiconductor thin film 12 contain the same elements and have the same crystal structure. For example, the substrate 11 and the semiconductor thin film 12 are III-V compound semiconductors such as gallium nitride (GaN), aluminum gallium nitride (AlGaN), or indium gallium nitride (InGaN). The semiconductor thin film 12 has a photocatalytic function that causes a reaction of a target substance when irradiated with light.
[0021] The first catalyst layer 13 and the second catalyst layer 14 are made of a material having a promoter function for the semiconductor thin film 12, and are distributed on the semiconductor thin film 12. Specifically, as shown in FIG. 2, the first catalyst layer 13 is disk-shaped with a diameter of 10 μm, and is distributed at intervals of 210 μm. The second catalyst layer 14 is disk-shaped with a diameter of 10 μm, and is distributed with an interval of 100 μm between the first catalyst layer 13. The first catalyst layer 13 is a promoter for reduction reaction. The second catalyst layer 14 is a promoter for oxidation reaction, and may be one or more metals or oxides of metals selected from Ni, Co, Cu, W, Ta, Pd, Ru, Fe, Zn, and Nb. The thickness of the second catalyst layer 14 is preferably 1 nm to 10 nm, and particularly 1 nm to 3 nm, which allows sufficient light transmission. The second catalyst layer 14 may cover the entire exposed surface of the semiconductor thin film 12.
[0022] The protective layer 15 is intended to prevent deterioration of the substrate 11 and the semiconductor thin film 12 due to contact with the aqueous solution. The protective layer 15 is made of an insulating material, such as an epoxy resin, that does not react with the aqueous solution, the substrate 11, and the semiconductor thin film 12.
[0023] Fig. 3 is a cross-sectional view showing an example of another configuration of the nitride semiconductor photocatalytic thin film of this embodiment. The nitride semiconductor photocatalytic thin film of Fig. 3 is a nitride semiconductor photocatalytic thin film that exerts a catalytic function and causes an oxidation-reduction reaction when irradiated with light in an aqueous solution.
[0024] The nitride semiconductor photocatalytic thin film 1 shown in Figure 3 comprises an insulating substrate 16, an n-type semiconductor thin film 17 arranged on the surface of the substrate 16, a semiconductor thin film 12 arranged on the surface of the semiconductor thin film 17, a first catalytic layer 13 that forms an ohmic junction on part of the surface of the semiconductor thin film 12, a second catalytic layer 14 that forms a Schottky junction on part of the surface of the semiconductor thin film 12, and a protective layer 15 formed to cover the back surface of the substrate 11 and the side surfaces of the substrate 11 and the semiconductor thin films 12 and 17.
[0025] The substrate 16, the semiconductor thin film 17, and the semiconductor thin film 12 contain the same elements and have the same crystal structure. For example, the substrate 16, the semiconductor thin film 17, and the semiconductor thin film 12 are III-V compound semiconductors such as gallium nitride (GaN), aluminum gallium nitride (AlGaN), or indium gallium nitride (InGaN). The semiconductor thin film 12 has a photocatalytic function that causes a reaction of a target substance when irradiated with light.
[0026] The first catalytic layer 13, the second catalytic layer 14, and the protective layer 15 are the same as the nitride semiconductor photocatalytic thin film in FIG.
[0027] [Method of manufacturing nitride semiconductor photocatalytic thin film] A method for producing the nitride semiconductor photocatalytic thin film of FIG. 1 will be described with reference to FIG.
[0028] In step S11, a semiconductor thin film 12 made of a III-V group compound semiconductor is formed on a conductive substrate 11 made of a III-V group compound semiconductor.
[0029] In step S12, a first catalyst layer 13 is formed on a portion of the upper surface of the semiconductor thin film 12.
[0030] In step S13, in order to form an ohmic junction at the interface between the semiconductor thin film 12 and the first catalyst layer 13, the nitride semiconductor having the first catalyst layer 13 formed thereon is subjected to a heat treatment.
[0031] In step S14, a second catalyst layer 14 is formed on a portion of the upper surface of the semiconductor thin film 12.
[0032] In step S15, the nitride semiconductor having the second catalyst layer 14 formed thereon is heat-treated. This heat treatment step may be performed on a hot plate or in an electric furnace.
[0033] In step S16, protective layer 15 is formed so as to cover the surfaces of semiconductor thin film 12 other than the upper surface on which first catalyst layer 13 and second catalyst layer 14 are formed.
[0034] Next, a method for producing the nitride semiconductor photocatalytic thin film of FIG. 3 will be described with reference to FIG.
[0035] In step S20, a semiconductor thin film 17 made of a III-V group compound semiconductor is formed on an insulating substrate 16 made of a III-V group compound semiconductor.
[0036] In step S21, the semiconductor thin film 12 made of a III-V compound semiconductor is formed on the semiconductor thin film 17.
[0037] Thereafter, the first catalyst layer 13, the second catalyst layer 14, and the protective layer 15 are formed in the same manner as in steps S12 to S16 of FIG.
[0038] [Example of nitride semiconductor photocatalytic thin film] Examples 1 to 3 in which the semiconductor thin film 12 of the nitride semiconductor photocatalytic thin film in FIG. 1 was changed, and Examples 4 and 5 in which the semiconductor thin film 12 of the nitride semiconductor photocatalytic thin film in FIG. 2 was changed were produced, and a redox reaction test described below was carried out.
[0039] <Example 1> Example 1 is a nitride semiconductor photocatalytic thin film having the configuration shown in FIG.
[0040] In step S11, a GaN semiconductor thin film was epitaxially grown on an n-GaN substrate by metalorganic chemical vapor deposition (MOCVD) to form a semiconductor thin film 12 as a light absorbing layer (a layer that absorbs light and generates electrons and holes) on the substrate 11. Ammonia gas and trimethylgallium were used as growth materials. Hydrogen was used as the carrier gas sent into the growth furnace. The thickness of the semiconductor thin film 12 was set to 100 nm, which is sufficient to absorb light. After that, this nitride semiconductor was cleaved into a size of 1 cm x 1 cm for testing.
[0041] 2, disk-shaped metals (Ti / Al / Ti / Pt) with a diameter of 10 μm were vacuum-deposited on the surface of the semiconductor thin film 12 with an interval of 210 μm to form the first catalyst layer 13. Here, Ti with a thickness of 25 nm, Al with a thickness of 50 nm, Ti with a thickness of 25 nm, and Pt with a thickness of 100 nm were laminated in this order from the semiconductor thin film 12 side.
[0042] In step S13, the nitride semiconductor on which the first catalytic layer 13 was formed was subjected to a heat treatment at 800° C. for 30 seconds in a nitrogen atmosphere. A pseudo-ohmic junction was formed at the interface between the semiconductor thin film 12 and the first catalytic layer 13 by the heat treatment.
[0043] In step S14, as shown in FIG. 2, a disk-shaped Ni having a diameter of 10 μm was vacuum-deposited on the surface of the semiconductor thin film 12 with a gap of 100 μm between it and the first catalyst layer 13, thereby forming a Schottky junction between the semiconductor thin film 12 and the Ni.
[0044] In step S15, the nitride semiconductor on which Ni was vacuum-deposited was heat-treated in air at 300° C. for 1 hour to form NiO, thereby obtaining a second catalyst layer 14. When the cross section of the sample was observed with a transmission electron microscope (TEM), the thickness of the NiO film was found to be 2 nm.
[0045] In step S16, a protective layer 15 was formed using epoxy resin so as to cover the rear surface of the substrate 11 (the surface on which the semiconductor thin film 12 is not formed) and the side surfaces of the substrate 11 and the semiconductor thin film 12.
[0046] By the above steps, the nitride semiconductor photocatalytic thin film of Example 1 was obtained.
[0047] <Example 2> Example 2 is a nitride semiconductor photocatalytic thin film having the configuration shown in FIG.
[0048] In step S11, an InGaN semiconductor thin film with an indium composition ratio of 1% was epitaxially grown on an n-GaN substrate by MOCVD to form a semiconductor thin film 12 on the substrate 11. Ammonia gas, trimethylgallium, and trimethylindium were used as growth materials. Hydrogen was used as the carrier gas sent into the growth furnace. The thickness of the semiconductor thin film 12 was set to 100 nm, which is sufficient for absorbing light.
[0049] Thereafter, the steps from step S12 onwards in Example 1 were carried out to form the first catalytic layer 13, the second catalytic layer 14 and the protective layer 15, thereby obtaining the nitride semiconductor photocatalytic thin film of Example 2.
[0050] <Example 3> Example 3 is a nitride semiconductor photocatalytic thin film having the configuration shown in FIG.
[0051] In step S11, an AlGaN semiconductor thin film with an aluminum composition ratio of 5% was epitaxially grown on an n-GaN substrate by MOCVD to form a semiconductor thin film 12 on the substrate 11. Ammonia gas, trimethylgallium, and trimethylaluminum were used as growth materials. Hydrogen was used as the carrier gas sent into the growth furnace. The thickness of the semiconductor thin film 12 was set to 100 nm, which is sufficient for absorbing light.
[0052] Thereafter, the steps from step S12 onwards in Example 1 were carried out to form the first catalytic layer 13, the second catalytic layer 14 and the protective layer 15, thereby obtaining the nitride semiconductor photocatalytic thin film of Example 3.
[0053] <Example 4> Example 4 is a nitride semiconductor photocatalytic thin film having the configuration shown in FIG.
[0054] In step S20, a silicon-doped n-GaN semiconductor thin film was epitaxially grown on the GaN substrate by MOCVD to form an electronically conductive semiconductor thin film 17 on the substrate 16. Ammonia gas and trimethylgallium were used as growth materials. Silane gas was used as the n-type impurity source. Hydrogen was used as the carrier gas sent into the growth furnace. The thickness of the n-GaN semiconductor thin film was 2 μm. The carrier density was 3×10 18 cm -3 It was.
[0055] In step S21, an InGaN semiconductor thin film with an indium composition ratio of 1% was epitaxially grown on the n-GaN semiconductor thin film by MOCVD to form a semiconductor thin film 12 as a light absorbing layer on the semiconductor thin film 17. Ammonia gas, trimethylgallium, and trimethylindium were used as growth materials. Hydrogen was used as the carrier gas sent into the growth furnace. The thickness of the semiconductor thin film 12 was set to 100 nm, which is sufficient for absorbing light.
[0056] Thereafter, the steps from step S12 onwards in Example 1 were carried out to form the first catalytic layer 13, the second catalytic layer 14 and the protective layer 15, thereby obtaining the nitride semiconductor photocatalytic thin film of Example 4.
[0057] <Example 5> Example 5 is a nitride semiconductor photocatalytic thin film having the configuration shown in FIG.
[0058] In step S20, a silicon-doped n-GaN semiconductor thin film was epitaxially grown on the GaN substrate by MOCVD to form an electronically conductive semiconductor thin film 17 on the substrate 16. Ammonia gas and trimethylgallium were used as growth materials. Silane gas was used as the n-type impurity source. Hydrogen was used as the carrier gas sent into the growth furnace. The thickness of the n-GaN semiconductor thin film was 2 μm. The carrier density was 3×10 18 cm -3 It was.
[0059] In step S21, an AlGaN semiconductor thin film with an aluminum composition ratio of 5% was epitaxially grown on the n-GaN semiconductor thin film by MOCVD to form a semiconductor thin film 12 as a light absorbing layer on the semiconductor thin film 17. Ammonia gas, trimethylgallium, and trimethylaluminum were used as growth materials. Hydrogen was used as the carrier gas sent into the growth furnace. The film thickness of the semiconductor thin film 12 was set to 100 nm, which is sufficient for absorbing light.
[0060] Thereafter, the steps from step S12 onwards in Example 1 were carried out to form the first catalytic layer 13, the second catalytic layer 14 and the protective layer 15, thereby obtaining the nitride semiconductor photocatalytic thin film of Example 5.
[0061] [Comparison example] Comparative Examples 1 to 10 were prepared by changing the material of the substrate 11 from Examples 1 to 5, and Comparative Examples 11 and 12 were prepared by not forming the protective layer 15 from Examples 1 and 4, and were subjected to the oxidation-reduction reaction test described below.
[0062] <Comparative Example 1> Comparative Example 1 differs from Example 1 in that an n-Si substrate is used as the substrate 11. In other respects, Comparative Example 1 is similar to Example 1.
[0063] <Comparative Example 2> Comparative Example 2 differs from Example 2 in that an n-Si substrate is used as the substrate 11. In other respects, Comparative Example 2 is similar to Example 2.
[0064] <Comparative Example 3> Comparative Example 3 differs from Example 3 in that an n-Si substrate is used as the substrate 11. In other respects, Comparative Example 3 is similar to Example 3.
[0065] <Comparative Example 4> Comparative Example 1 differs from Example 1 in that a SiC substrate is used as the substrate 11. In other respects, Comparative Example 1 is similar to Example 1.
[0066] <Comparative Example 5> Comparative Example 5 differs from Example 2 in that a SiC substrate is used as the substrate 11. In other respects, it is similar to Example 2.
[0067] <Comparative Example 6> Comparative Example 6 differs from Example 3 in that a SiC substrate is used as the substrate 11. In other respects, Comparative Example 6 is similar to Example 3.
[0068] <Comparative Example 7> Comparative Example 7 differs from Example 4 in that a sapphire substrate is used as the substrate 11. Other points are the same as Example 4.
[0069] <Comparative Example 8> Comparative Example 8 differs from Example 5 in that a sapphire substrate is used as the substrate 11. In other respects, it is similar to Example 5.
[0070] <Comparative Example 9> Comparative Example 9 differs from Example 4 in that a Si substrate is used as the substrate 11. In other respects, Comparative Example 9 is similar to Example 4.
[0071] <Comparative Example 10> Comparative Example 10 differs from Example 5 in that a Si substrate is used as the substrate 11. In other respects, Comparative Example 10 is similar to Example 5.
[0072] <Comparative Example 11> Comparative Example 11 differs from Example 1 in that it uses a nitride semiconductor photocatalytic thin film without forming a protective layer 15. In other respects, it is similar to Example 1.
[0073] <Comparative Example 12> Comparative Example 11 differs from Example 4 in that it uses a nitride semiconductor photocatalytic thin film without forming a protective layer 15. In other respects, it is similar to Example 4.
[0074] [Oxidation-reduction reaction test] For Examples 1 to 5 and Comparative Examples 1 to 12, an oxidation-reduction reaction test was carried out using the device shown in FIG.
[0075] A reaction cell with a quartz window and a capacity of 150 ml was used as the photocatalyst tank 110, and a stirrer 120 and an aqueous solution 130 were placed in the photocatalyst tank 110. As the aqueous solution 130, 125 ml of a 1 mol / l aqueous potassium hydroxide solution was used.
[0076] The semiconductor photocatalytic thin films of Examples 1 to 5 and Comparative Examples 1 to 12 were immersed in an aqueous solution 130 and fixed so that the surface of the semiconductor thin film 12 on which the first catalyst layer 13 and the second catalyst layer 14 were formed faced the light source 140.
[0077] Nitrogen gas was bubbled at 200 ml / min for 30 minutes to remove bubbles and replace with air, and then the photocatalyst tank 110 was sealed with a silicon Teflon septum. The pressure inside the photocatalyst tank 110 was set to atmospheric pressure (1 atm).
[0078] The light source 140 is a 300W high-pressure xenon lamp (cuts out wavelengths of 400nm or more, illuminance 5mW / cm 2 The light from the light source 140 was uniformly irradiated onto the semiconductor photocatalytic thin film from the outside of the quartz window of the photocatalytic vessel 110.
[0079] The light irradiation area of the sample is 1 cm 2 The aqueous solution 130 was stirred at a rotation speed of 250 rpm at the center position of the bottom of the photocatalyst tank 110 using the stirring bar 120 and the stirrer.
[0080] At any time after the light irradiation, the gas in the photocatalyst tank 110 was sampled from the septum with a syringe, and the reaction products were analyzed with a gas chromatograph mass spectrometer. As a result, it was confirmed that hydrogen and oxygen were produced.
[0081] [Test Results] Table 1 shows the amounts of oxygen and hydrogen gas produced versus light irradiation time in Examples 1 to 5 and Comparative Examples 1 to 12. The amounts of each gas produced were normalized by the surface area of the semiconductor photoelectrode.
[0082] [Table 1]
[0083] It was found that in all cases oxygen and hydrogen were produced upon irradiation with light.
[0084] The dislocation density of each sample is shown in Table 2. For each sample, an X-ray diffractometer was used to measure the rocking curve (XRC) corresponding to the (002) plane perpendicular to the crystal growth direction at the center position of the substrate. The screw dislocation density was calculated from the obtained half-width using the following formula. Here, β is the half-width and b is 0.5185 nm.
[0085] Screw dislocation density = β 2 / 4.35b 2
[0086] [Table 2]
[0087] It was found that dislocation density changes by changing the type of substrate. The dislocation density of the semiconductor thin films 12, 17 is affected by the difference between the crystal structure and lattice constant of the semiconductor thin films 12, 17 and the crystal structure and lattice constant of the substrate. If those of the semiconductor thin films 12, 17 are significantly different from those of the substrate, many dislocations occur in the semiconductor thin films 12, 17. On the other hand, if those of the semiconductor thin films 12, 17 are close to those of the substrate, the number of dislocations occurring in the semiconductor thin films 12, 17 decreases.
[0088] When comparing the amounts of oxygen and hydrogen generated in Example 1 and Comparative Examples 1 and 4, there was no significant difference in the amounts generated immediately after light irradiation, but as time passed from the start of light irradiation, differences in the amounts generated were observed. In Comparative Examples 1 and 4, the amount of hydrogen generated was reduced by about 50% 50 hours after light irradiation, while in Example 1, the amount of hydrogen generated was maintained at about 10% after 50 hours after light irradiation. In addition, 100 hours after light irradiation, the amount of hydrogen generated in Example 1 was reduced by 20%, while the amount of hydrogen generated in Comparative Examples 1 and 4 was reduced by 90% and the amount of oxygen generated was reduced by 95%. In the case of the Comparative Examples, in addition to the large reduction in the amount generated, the ratio of oxygen and hydrogen generated was no longer 1:2, which is considered to have caused hydrogen generation due to a side reaction (etching reaction) on the semiconductor electrode surface to become prominent. These phenomena were similar when comparing Example 2 with Comparative Examples 2 and 5, and when comparing Example 3 with Comparative Examples 3 and 6. This is believed to be because growing a semiconductor photocatalyst on a substrate made of the same elements and crystal structure reduced the dislocation density, thereby suppressing the etching reaction at the dislocation origin and extending the life of the water splitting reaction.
[0089] When comparing the amounts of oxygen and hydrogen generated in Example 4 and Comparative Examples 7 and 9, there was no significant difference in the amounts generated immediately after light irradiation, but as time passed from the start of light irradiation, differences were observed in the amounts generated. In Comparative Examples 7 and 9, the amount of hydrogen generated was reduced by about 30% and about 50%, respectively, 50 hours after light irradiation, while in Example 4, the amount of hydrogen generated was maintained at about 15% after 50 hours after light irradiation. In addition, 100 hours after light irradiation, the amount of hydrogen generated in Example 4 was reduced by 20%, while in Comparative Examples 7 and 9, the amount of hydrogen generated was reduced by about 90% and about 90%, respectively, and the amount of oxygen generated was reduced by about 70% and about 95%, respectively. In the case of the Comparative Examples, in addition to the large decrease in the amount generated, the ratio of oxygen and hydrogen generated was no longer 1:2, which is considered to have significantly affected the hydrogen generation due to a side reaction (etching reaction) on the semiconductor electrode surface. These phenomena were also observed when comparing Example 5 with Comparative Examples 8 and 10. This is believed to be because growing a semiconductor photocatalyst on a substrate made of the same elements reduced the dislocation density, suppressing the etching reaction at the dislocation origin and extending the life of the water splitting reaction.
[0090] Moreover, a larger amount of gas was detected in Examples 2, 4, 3, and 5 than in Example 1. This is because the InGaN used in Examples 2 and 4 has a narrower band gap than GaN, widening the wavelength range that can be absorbed and improving the light absorption rate. Also, the AlGaN used in Examples 3 and 5 has a smaller lattice constant than GaN, and the large electric field generated in AlGaN by the piezoelectric effect promotes the separation of electrons and holes, improving the quantum yield.
[0091] Comparing the amount of oxygen and hydrogen generated in Example 1 and Comparative Examples 11 and 12, there was no significant difference in the amount generated immediately after light irradiation, but as time passed from the start of light irradiation, differences in the amount generated were observed. When a protective layer was not formed as in the Comparative Examples, it is believed that a side reaction (etching reaction) occurred on the back surface of the substrate that came into contact with the aqueous solution and on the side surface of the semiconductor.
[0092] From the above, it was possible to extend the life of the hydrogen and oxygen production (solar energy conversion efficiency) through the water splitting reaction by using a semiconductor photocatalytic thin film with reduced dislocation density using an n-GaN substrate or a GaN substrate.
[0093] As described above, the nitride semiconductor photocatalytic thin film 1 of this embodiment is a nitride semiconductor photocatalytic thin film 1 that exhibits catalytic function when irradiated with light to cause an oxidation-reduction reaction, and has a conductive substrate 11, a semiconductor thin film 12 arranged on the surface of the substrate 11, a first catalytic layer 13 that forms an ohmic junction on part of the surface of the semiconductor thin film 12, a second catalytic layer 14 that forms a Schottky junction on part of the surface of the semiconductor thin film 12, and a protective layer 15 arranged to cover the back surface of the substrate 11 and the side surfaces of the substrate 11 and the semiconductor thin film 12, and the substrate 11 and the semiconductor thin film 12 contain the same elements and have the same crystal structure.
[0094] When the gallium nitride thin film is irradiated with light in an aqueous solution, a GaN etching reaction proceeds as a side reaction on the gallium nitride surface in addition to the intended water oxidation reaction. This etching reaction is likely to proceed at the dislocation lines (lattice defects) exposed on the gallium nitride surface. These dislocation lines are generated during the manufacturing stage of the gallium nitride thin film, and the higher the dislocation density in the material, the more dislocation lines are exposed, and the easier the etching reaction proceeds. In the nitride semiconductor photocatalytic thin film 1 of this embodiment, the crystal structure and lattice constant of the substrate 11 and the semiconductor thin film 12 are close to each other, so that the dislocation density in the semiconductor thin film 12 after film formation can be suppressed. Therefore, the deterioration reaction (etching) of the semiconductor thin film 12 that proceeds from the dislocation lines (lattice defects) is suppressed, and the solar energy conversion efficiency of the nitride semiconductor photocatalytic thin film can be extended.
[0095] Furthermore, by changing the metal on the surface of the first catalytic layer 13 to, for example, Ni, Fe, Au, Pt, Ag, Cu, In, Ti, Co, or Ru, or by changing the atmosphere inside the cell, it is also possible to produce carbon compounds through the reduction reaction of carbon dioxide and ammonia through the reduction reaction of nitrogen. [Explanation of symbols]
[0096] 1. Nitride semiconductor photocatalytic thin film 11,16…Substrate 12,17...Semiconductor thin film 13...First catalyst layer 14…Second catalyst layer 15...Protective layer
Claims
1. A nitride semiconductor photocatalytic thin film that exhibits a catalytic function by light irradiation to cause an oxidation-reduction reaction, a conductive n-GaN substrate; a nitride semiconductor thin film disposed on a surface of the substrate; a first catalyst layer that forms an ohmic junction on a part of the surface of the nitride semiconductor thin film and serves as a reduction reaction promoter; a second catalyst layer that forms a Schottky junction on a portion of the surface of the nitride semiconductor thin film and is an oxidation reaction promoter; a protective layer disposed so as to cover a rear surface of the substrate and side surfaces of the substrate and the nitride semiconductor thin film; The substrate and the nitride semiconductor thin film contain the same elements and have the same crystal structure. Nitride semiconductor photocatalytic thin film.
2. The nitride semiconductor photocatalytic thin film according to claim 1, The second catalyst layer covers the entire exposed surface portion of the nitride semiconductor thin film. Nitride semiconductor photocatalytic thin film.
Citation Information
Patent Citations
Photo-reactive membrane like catalyst
JP1985044053A
Light energy conversion apparatus and semiconductor photoelectrode
JP2007239048A
Photocatalyst unit and gas generation apparatus
JP2010247109A
Nitride semiconductor photocatalyst and nitride semiconductor electrode
JP2014208324A
Photocatalyst device
JP2016043304A