Steel plate for hot stamping and its manufacturing method, and hot stamped member and its manufacturing method

A steel plate with a bainite-based microstructure and controlled composition addresses the limitations of conventional hot stamping by enhancing hardenability and collision resistance, ensuring high strength and deformability even at low cooling rates.

JP7553837B2Active Publication Date: 2024-09-19NIPPON STEEL CORPORATION
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2022557488
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-10-16
Filing Date
2021-10-15
Publication Date
2024-09-19
Estimated Expiration
2041-10-15

AI Technical Summary

Technical Problem

Conventional hot stamping methods do not adequately harden thick steel plates, leading to insufficient strength and difficulty in managing mold clearance during hot stamping, especially when joining steel plates of different thicknesses, and fail to provide adequate collision resistance and crack suppression during large deformations.

Method used

A steel plate with a microstructure predominantly composed of upper bainite and specific iron-based carbides, along with controlled chemical composition, allowing for high strength and excellent collision resistance, even at low cooling rates during hot stamping.

Benefits of technology

The steel plate achieves high strength and excellent collision resistance, with improved hardenability and ability to suppress cracking during large deformations, maintaining workability and ensuring sufficient strength post-hot stamping.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007553837000006
    Figure 0007553837000006
  • Figure 0007553837000005
    Figure 0007553837000005
  • Figure 0007553837000001
    Figure 0007553837000001
Patent Text Reader

Abstract

This steel plate for hot stamping has a chemical composition containing, in terms of mass%, 0.060-0.120% of C, 0-0.70% of Si, 1.60-3.00% of Mn, 0.100% or less of P, 0.0100% or less of S, 0.0100% or less of N, 0.001-0.100% of Al, 0.005-0.050% of Ti, and 0.0005-0.0100% of B, and furthermore containing, as necessary, one or more substances from among Nb, V, W, Ni, Cu, C, Mo, Sn, Ca, Mg, and REM, the balance being Fe and unavoidable impurities. In the steel plate for hot stamping, the microstructure includes at least 70% of upper bainite by area ratio, and the number density of iron-based carbides having a long diameter of 0.1 μm or greater contained in the upper bainite is 4 per μm2 or greater.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a steel sheet for hot stamping and a manufacturing method thereof, and a hot stamped member and a manufacturing method thereof. This application claims priority based on Japanese Patent Application No. 2020-174457, filed on October 16, 2020, the contents of which are incorporated herein by reference. [Background technology]

[0002] In recent years, further improvement in fuel efficiency of automobiles is required from the viewpoint of greenhouse gas emission regulations associated with global warming countermeasures. Since many automobile structures are formed of iron, particularly steel plates, by reducing the weight of these steel plates by making them thinner, the vehicle body becomes lighter and fuel efficiency improves. However, there is a concern that simply reducing the thickness of the steel plate to reduce its weight will reduce the strength of the structure and reduce collision safety. Therefore, in order to reduce the thickness of the steel plate, it is required to increase the mechanical strength of the steel plate used so as not to reduce the strength of the structure. Therefore, in recent years, the application of high-strength steel plates in automobile parts is becoming more and more widespread in order to reduce the weight of the vehicle body and ensure collision safety.

[0003] Similarly, in the area of ​​automobiles, the shift to electric vehicles (EVs) is underway as a measure to combat global warming. EVs generally have a significantly heavier vehicle weight than gasoline-powered vehicles. This creates a high demand for the use of high-strength steel plates. Furthermore, collision regulations have been strengthened in recent years. For this reason, the use of ultra-high tensile steel (steel with a tensile strength of 980 MPa or more) for collision deformation components in EVs is being considered.

[0004] For example, Patent Document 1 discloses a method for producing a high-strength steel sheet having excellent balance between strength and ductility and strength and hole expandability, and excellent stretch flangeability. Patent Document 1 also discloses that the tensile strength is 980 MPa or more.

[0005] However, in the case of EVs, some vehicle models are heavy, so even if ultra-high tensile steel is used, a plate thickness of 3 mm or more may be required from the perspective of rigidity, etc. Ultra-high tensile steel of this thickness cannot be cold press formed.

[0006] Therefore, as a method for reducing the load during press forming, hot stamping, which performs hot forming and die hardening, has attracted attention. In hot stamping, the material to be formed is once heated to a high temperature, and the material softened by heating is pressed to form it, and then cooled after, or at the same time as, forming. In other words, the material is once heated to a high temperature to soften it, and then pressed in the softened state, so that the material can be easily press-formed. However, the cold-rolled steel sheet of Patent Document 1 does not take into consideration subsequent hot stamping.

[0007] For example, Patent Document 2 describes that a member having a tensile strength of 1400 MPa or more can be obtained by hot stamping a steel plate having a thickness of 1.0 to 1.8 mm and a tensile strength of 500 to 600 MPa.

[0008] However, when forming a thick steel sheet by hot stamping as described above, the steel sheet is not sufficiently hardened and sufficient strength cannot be obtained in the steel sheet (hot stamped member) after hot stamping in the conventional hot stamping such as that in Patent Document 2. Even if the sheet is thin, when it is joined to a steel sheet of a different thickness as a TWB (tailor welded blank), it is difficult to manage the clearance of the die in the part where the sheet thickness changes, and the sheet may not be sufficiently hardened. For this reason, a steel sheet to be subjected to hot stamping is required to have sufficient strength after hot stamping even when the cooling rate during hot stamping is slow. However, such a study has not been conducted in the past, including in Patent Document 2.

[0009] In addition, conventional hot stamped members are primarily used for non-deformation parts (parts that ensure the safety of passengers by suppressing deformation), and are not designed for use in deformed parts. That is, as described above, when considering application to collision-deformed parts, properties that can suppress cracking during large deformation are required, but in conventional hot stamped members, ensuring such properties has been hardly considered. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] Japanese Patent No. 5407168 [Patent Document 2] Japanese Patent Publication No. 2002-102980 Summary of the Invention [Problem to be solved by the invention]

[0011] The present invention has been made in view of the above problems. An object of the present invention is to provide a steel sheet for hot stamping, which has excellent hardenability during hot stamping (high strength can be obtained after hot stamping even when the cooling rate during hot stamping is relatively low) and excellent impact resistance properties after hot stamping (characteristics that can suppress cracking during large deformation can be obtained), and a manufacturing method thereof. Another object of the present invention is to provide a hot stamped member obtained using the above steel sheet for hot stamping as a raw material, and a manufacturing method of the hot stamped member using the above steel sheet for hot stamping. [Means for solving the problem]

[0012] The present inventors have conducted extensive research to obtain a steel sheet (steel sheet for hot stamping) that has high strength and excellent impact resistance after hot stamping. As a result, they have found that by making the microstructure of the steel sheet mainly of upper bainite and by having carbides of a predetermined size present, the hardenability of the steel sheet is improved, and by hot stamping this steel sheet, a hot stamped member that has high strength and excellent impact resistance (has excellent deformability and is unlikely to break during impact) can be obtained.

[0013] The present invention has been made based on the above findings and has the following gist. [1] A steel sheet for hot stamping according to one embodiment of the present invention has, by mass%, C: 0.060 to 0.120%, Si: 0 to 0.70%, Mn: 1.60 to 3.00%, P: 0.100% or less, S: 0.0100% or less, N: 0.0100% or less, Al: 0.001 to 0.100%, Ti: 0.005 to 0.050%, B: 0.0005 to 0.0100%, Nb: 0 to 0.100%, V: 0 to 0.100%, W: 0 to 0.100%, Ni: 0. The chemical composition of the steel sheet is: Cu: 0-2.00%, Cr: 0-2.00%, Mo: 0-2.00%, Sn: 0-0.200%, Ca: 0-0.0500%, Mg: 0-0.0500%, and REM: 0-0.0500%, with the balance being Fe and impurities. The microstructure contains upper bainite at an area ratio of 70% or more, and the number density of iron-based carbides having a major axis of 0.1 μm or more contained in the upper bainite is 4 / μm 2 That's all. [2] The steel sheet for hot stamping described in [1] may have a chemical composition, in mass%, of one or more selected from Nb: 0.005 to 0.100%, V: 0.005 to 0.100%, W: 0.005 to 0.100%, Ni: 0.01 to 2.00%, Cu: 0.01 to 2.00%, Cr: 0.01 to 2.00%, Mo: 0.01 to 2.00%, Sn: 0.0003 to 0.0500%, Ca: 0.0003 to 0.0500%, Mg: 0.0003 to 0.0500%, and REM: 0.0003 to 0.0500%. [3] The steel sheet for hot stamping according to [1] or [2] may have a tensile strength of less than 980 MPa. [4] The steel sheet for hot stamping according to any one of [1] to [3] may have a plating layer on the surface. [5] In the steel sheet for hot stamping described in [4], the plating layer may be a hot-dip galvanized layer, a galvannealed layer, an electrolytic galvanized layer, or an Al plating layer. [6] A method for producing a steel sheet for hot stamping according to another aspect of the present invention comprises the steps of: A method for producing a steel sheet for hot stamping according to [1], The method includes a heating step of heating a steel ingot or slab having the chemical composition described in [1] to 1150 to 1300°C, either directly or after cooling once; a hot rolling step of hot rolling the steel ingot or slab after the heating step to a finishing temperature of 850°C or higher to obtain a hot rolled steel sheet; a coiling step of coiling the hot rolled steel sheet after the hot rolling step at 640 to 450°C; a holding step of holding the hot rolled steel sheet after the coiling step in a temperature range of 500 to 450°C for 1.0 hour or more; and a cooling step of cooling the hot rolled steel sheet after the holding step to room temperature. [7] The method for producing a steel sheet for hot stamping described in [6] may further include a cold rolling step of cold rolling the hot-rolled steel sheet after the holding step at a cumulative rolling reduction of 30 to 70% to obtain a cold-rolled steel sheet. [8] A method for producing a steel sheet for hot stamping according to another aspect of the present invention comprises the steps of: A method for producing a steel sheet for hot stamping according to [1], A heating step of heating a steel ingot or slab having the chemical composition described in [1] to 1150 to 1300°C, either directly or after cooling once; a hot rolling step of hot rolling the steel ingot or slab after the heating step to a finishing temperature of 850°C or higher to obtain a hot rolled steel sheet; a coiling step of coiling the hot rolled steel sheet after the hot rolling step at 700 to 500°C; a cooling step of cooling the hot rolled steel sheet after the coiling step to room temperature; a cold rolling process in which the hot-rolled steel sheet after the pickling process is cold-rolled at a cumulative reduction rate of 30 to 70% to obtain a cold-rolled steel sheet; an annealing process in which the cold-rolled steel sheet is heated to an annealing temperature range of 840 to 900°C and held in the annealing temperature range for 10 to 2000 seconds; and a heat treatment process in which the cold-rolled steel sheet after the annealing process is cooled to a temperature range of 400 to 600°C, held in the temperature range for 100 to 1000 seconds, and then cooled to room temperature. [9] [8] The method for producing a steel sheet for hot stamping may further include a plating step of immersing the cold-rolled steel sheet after the heat treatment step in a plating bath to form a plating layer on the surface.

[10] The method for producing a steel sheet for hot stamping described in [9] may further include an alloying step of holding the cold-rolled steel sheet after the plating step in an alloying temperature range of 450 to 600°C to alloy the plating layer.

[11] The method for producing a steel sheet for hot stamping according to [8] teeth, Furthermore, the method may include a plating step of immersing the cold-rolled steel sheet after the annealing step and before the heat treatment step in a plating bath to form a plating layer on the surface.

[12] The method for producing a steel sheet for hot stamping described in

[11] may further include an alloying step of holding the cold-rolled steel sheet after the plating step and before the heat treatment step in an alloying temperature range of 450 to 600°C to alloy the plating layer.

[13] A hot stamped member according to another embodiment of the present invention has, in mass%, C: 0.060 to 0.120%, Si: 0 to 0.70%, Mn: 1.60 to 3.00%, P: 0.100% or less, S: 0.0100% or less, N: 0.0100% or less, Al: 0.001 to 0.100%, Ti: 0.005 to 0.050%, B: 0.0005 to 0.0100%, Nb: 0 to 0.100%, and V: 0 to 0. The chemical composition of this steel sheet is 100%, W: 0-0.100%, Ni: 0-2.00%, Cu: 0-2.00%, Cr: 0-2.00%, Mo: 0-2.00%, Sn: 0-0.200%, Ca: 0-0.0500%, Mg: 0-0.0500%, and REM: 0-0.0500%, with the balance being Fe and impurities, and the microstructure contains 90% or more tempered martensite by area ratio.

[14] The hot stamped member described in

[13] may have a chemical composition, in mass%, of one or more selected from Nb: 0.005 to 0.100%, V: 0.005 to 0.100%, W: 0.005 to 0.100%, Ni: 0.01 to 2.00%, Cu: 0.01 to 2.00%, Cr: 0.01 to 2.00%, Mo: 0.01 to 2.00%, Sn: 0.0003 to 0.0500%, Ca: 0.0003 to 0.0500%, Mg: 0.0003 to 0.0500%, and REM: 0.0003 to 0.0500%.

[15] A method for producing a hot stamped member according to another aspect of the present invention includes the steps of: A method for producing a hot-stamped member according to

[13] , The method includes a hot stamping process in which the steel sheet for hot stamping according to any one of [1] to [5] is heated in a heating furnace at an atmospheric temperature of 850 to 950°C for 3 minutes or more, and then cooled at a cooling rate of 10°C / sec or more to a martensitic transformation start temperature or lower.

[16] In the method for producing a hot-stamped member according to

[15] , the cooling rate in the hot stamping step may be 10 to 20° C. / sec. Effect of the Invention

[0014] Effects of the Invention According to the present invention, it is possible to provide a steel sheet for hot stamping which has excellent hardenability during hot stamping and excellent impact resistance after hot stamping, a manufacturing method thereof, and a hot stamped member using the steel sheet for hot stamping and a manufacturing method thereof. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] A hot stamping steel sheet according to one embodiment of the present invention (hereinafter referred to as the steel sheet according to the present embodiment) and a manufacturing method thereof, a hot stamped member obtained by hot stamping the steel sheet according to the present embodiment (the hot stamped member according to the present embodiment), and a method for manufacturing the hot stamped member using the steel sheet according to the present embodiment will be described.

[0016] First, the steel sheet according to the present embodiment will be described. The steel sheet according to the present embodiment has a predetermined chemical composition, and the microstructure contains upper bainite at an area ratio of 70% or more, and the number density of iron-based carbides having a major axis of 0.1 μm or more contained in the upper bainite is 4 particles / μm 2 That's all.

[0017] <Microstructure> [The microstructure contains upper bainite at an area ratio of 70% or more] [The number density of iron-based carbides with a major axis of 0.1 μm or more in the upper bainite is 4 / μm 2 That's all.] Generally, hot stamping steel sheets are designed to be easy to process during cutting and other processes, and to have high strength after hot stamping. Therefore, the microstructure of hot stamping steel sheets (before hot stamping) is often a structure containing a lot of soft ferrite (e.g., ferrite-pearlite structure). On the other hand, if a large amount of alloying elements is added to improve the hardenability during hot stamping heat treatment, the strength of the hot stamping steel sheet also increases, resulting in problems such as poor cuttability and difficulty in straightening with a leveler. In addition, the addition of a large amount of alloying elements increases the hardenability of the steel sheet and lowers the Ms point. Therefore, the microstructure of the formed body after hot stamping is mainly fresh martensite (martensite without carbides). In this case, the deformability during collision is poor. In response to this, the present inventors have set the area ratio of upper bainite in the microstructure of a steel sheet for hot stamping to 70% or more, and set the number density of iron-based carbides with a major axis of 0.1 μm or more contained in the upper bainite to 4 particles / μm 2 By doing so, it has been found that it is possible to suppress the hardness of the steel sheet for hot stamping in order to ensure workability, including cutting, even when the steel sheet contains a large amount of alloying elements, while simultaneously achieving both hardenability that provides sufficient strength after hot stamping and impact resistance after hot stamping.

[0018] In the microstructure, ferrite, pearlite, martensite, etc. may be contained in addition to upper bainite. However, if the area ratio of upper bainite is less than 70% and the total area ratio of ferrite and pearlite is more than 30%, excellent impact resistance properties cannot be obtained after hot stamping (the VDA bendability described later decreases), and it is difficult to suppress fracture during impact. On the other hand, if the area ratio of upper bainite is less than 70% and the area ratio of martensite is more than 30%, the strength of the steel plate for hot stamping becomes too high and the workability is poor. Therefore, the area ratio of upper bainite is set to 70% or more.

[0019] The number density of iron-based carbides with a major axis of 0.1 μm or more is 2 The reason for specifying four or more per side is that the carbides are uniformly dispersed to promote dissolution of the carbides during hot stamping, improve hardenability, and improve bendability during collision. The carbides contained in the upper bainite have a needle-like shape, exist between the laths of the upper bainite, and have a shape elongated in one direction. In this embodiment, the major axis is defined as the size of the iron-based carbides. Iron-based carbides of 0.1 μm or more are 1 μm 2 If there are less than four particles per square meter, assuming the chemical composition and microstructure of the steel plate according to this embodiment (area percentage of upper bainite is 70% or more), this means that many iron-based carbides smaller than 0.1 μm have precipitated, or that the iron-based carbides have become excessively coarsened. If many iron-based carbides with a major axis of less than 0.1 μm have precipitated, the strength of the steel plate increases excessively due to precipitation strengthening, and workability decreases. In addition, excessively large carbides do not melt during hot stamping, reducing hardenability, and become the starting point for crack formation during collision deformation. For this reason, it is preferable to reduce the number density of iron-based carbides of 0.1 μm or more to 1 μm. 2 The number of carbides is set to 4 or more per unit area. The size of the carbides is preferably 0.1 to 0.5 μm. In addition, by setting the size of the carbides to 0.1 to 0.5 μm, the strength of the hot stamping steel sheet is also contributed to being 980 MPa or less. Furthermore, although the detailed mechanism is unknown, by setting the carbides in the above range, it is also contributed to increasing the area ratio of tempered martensite in the hot stamped body (hot stamped member).

[0020] The area ratio of the microstructure and the number density of iron-based carbides in the upper bainite can be determined by the following method. First, the steel plate is cut parallel to the rolling direction, polished so that the plate thickness direction becomes the observation surface, and etched with Nital reagent. Then, using an SEM, observation is made at a magnification of 1000 to 30000 times in the plate thickness direction from the surface to a position of 1 / 4 of the plate thickness (a range of 1 / 8 to 3 / 8 of the plate thickness from the surface is acceptable) to identify ferrite, upper bainite, lower bainite, pearlite, and martensite. When identifying, it is possible to judge from the structure morphology that ferrite is an equiaxed grain that does not contain iron-based carbides, pearlite is a layered structure of ferrite and cementite, upper bainite is a structure with a lath-like shape that contains cementite and retained austenite between the laths, lower bainite contains carbides within the laths, etc. The area ratio of each identified structure is calculated from the SEM observation image. Martensite exists in both tempered martensite, which contains carbides in the laths, and as-quenched martensite (fresh martensite), which does not contain carbides, and these can be identified by observing with a SEM or TEM to confirm the presence or absence of carbides. For example, 10 fields of view of 30 μm × 25 μm are observed at a magnification of 3000 times, and the average value is taken as the area ratio. Carbides in upper bainite can also be quantified by the above observation. However, since the carbides in upper bainite are fine, on the order of 0.1 μm, it is desirable to observe them with a high-resolution FE (Field Emission)-SEM. For example, observe 20 fields of view of 10 μm × 8 μm at 10,000x magnification, and take the average value as the number density.

[0021] The reason for measuring the position at 1 / 4 of the plate thickness from the surface in the plate thickness direction is that the structure at this position generally shows the most representative structure of the steel plate, but since the steel plate according to this embodiment has a structure that is generally uniform in the plate thickness direction, similar structures can be obtained even if measurements are made at other positions.

[0022] In the steel sheet according to the present embodiment, the microstructure is controlled as described above, and the chemical composition is controlled as described below, so that the microstructure of the member (hot stamped member) after hot stamping can contain 90% or more of tempered martensite in a wide range of cooling rates during hot stamping of 10°C / s or more, and sufficient strength can be obtained. In particular, the hardenability at a cooling rate range of 10 to 30°C / s, which was a problem with conventional hot stamping steel sheets, is significantly improved. Therefore, not only when the thickness of the hot stamping steel sheet is thin, but also when the thickness is relatively thick (for example, about 3 to 6 mm), high strength can be obtained after hot stamping.

[0023] <Chemical composition> Next, the chemical composition of the steel sheet according to this embodiment will be described. In the following, % regarding the chemical composition means % by mass.

[0024] C: 0.060~0.120% C is an element that increases the strength of the steel sheet and contributes to improving the VDA bendability by controlling the martensite transformation start temperature during cooling in the hot stamping process. If the C content is less than 0.060%, it is not possible to ensure a tensile strength (maximum tensile strength) of 980 MPa or more after hot stamping. Therefore, the C content is set to 0.060% or more. The C content is preferably 0.070% or more. On the other hand, if the C content exceeds 0.120%, the martensite transformation start temperature becomes too high, and sufficient area ratio of tempered martensite cannot be obtained in the hot stamping process. In this case, the steel plate (hot stamped member) after hot stamping has insufficient fracture suppression during collision. Therefore, the C content is set to 0.120% or less. The C content is preferably 0.110% or less.

[0025] Silicon: 0 to 0.70% Silicon is an element that increases the Ae3 point, and increases the heating temperature required to make tempered martensite the main phase after hot stamping. Therefore, if the silicon content is excessive, productivity and economic efficiency will decrease. For this reason, the silicon content is set to 0.70% or less. On the other hand, the Si content may be 0%, but Si is an element that increases the strength of the steel sheet. In addition, for non-plated steel sheets, Si is an element that improves scale adhesion. Therefore, Si may be contained. To obtain this effect, the Si content is preferably 0.05% or more.

[0026] Mn: 1.60-3.00% Mn is an element that enhances the hardenability of steel sheets. It delays the ferrite transformation during the cooling process during hot stamping, and allows the microstructure of the hot stamped body to become tempered martensite as the main phase at a cooling rate of 10°C / sec or more. To this end, the Mn content is set to 1.60% or more. On the other hand, if the Mn content exceeds 3.00%, not only does the effect saturate, but the steel sheet becomes embrittled and cracks occur during casting, cold rolling, or hot rolling. Therefore, the Mn content is set to 3.00% or less.

[0027] P:0.100% or less P is an element that segregates in the center of the steel plate thickness and also embrittles the welded portion. If the P content exceeds 0.100%, the embrittlement of the welded portion becomes significant, so the P content is set to 0.100% or less. The P content is preferably 0.050% or less. There is no particular lower limit for the P content, and it may be 0%, but reducing the P content to less than 0.001% is economically disadvantageous, so the P content may be set to 0.001% or more.

[0028] S: 0.0100% or less S exists as inclusions such as MnS and is an element that deteriorates crashworthiness. Therefore, it is desirable to reduce the S content. If the S content exceeds 0.0100%, the deterioration of crashworthiness becomes significant, so the S content is set to 0.0100% or less. There is no particular lower limit for the S content, and it may be 0%, but since reducing the S content to less than 0.0001% is economically disadvantageous, the S content may be set to 0.0001% or more.

[0029] N: 0.0100% or less N is an element that forms coarse nitrides, which become the starting point of cracks during a collision and deteriorate the impact resistance properties. If the N content exceeds 0.0100%, the impact resistance properties deteriorate significantly. Therefore, the N content is set to 0.0100% or less. There is no particular need to set a lower limit for the N content, and it may be 0%, but if the N content is reduced to less than 0.0001%, the manufacturing costs will increase significantly. Therefore, the N content may be set to 0.0001% or more, or 0.0005% or more.

[0030] Al: 0.001 to 0.100% Al is an element that acts as a deoxidizer. If the Al content is less than 0.001%, a sufficient deoxidizing effect cannot be obtained, and a large amount of inclusions (oxides) will be present in the steel sheet. These inclusions are not preferable because they can become the starting point of cracks during a collision and cause breakage. Therefore, the Al content is set to 0.001% or more. On the other hand, if the Al content exceeds 0.100%, the Ae3 point increases, and it becomes necessary to increase the heating temperature during hot stamping, which is undesirable, so the Al content is set to 0.100% or less.

[0031] Ti: 0.005 to 0.050% Ti is an element that combines with N to form TiN, thereby suppressing the formation of nitrides by B, and improving hardenability. To obtain this effect, the Ti content is set to 0.005% or more. The Ti content is preferably 0.007% or more. On the other hand, if the Ti content exceeds 0.050%, the amount of C that contributes to strengthening martensite is reduced due to the formation of Ti carbides, and the strength of the steel sheet (hot stamped member) after hot stamping is not sufficient. Therefore, the Ti content is set to 0.050% or less. The Ti content is preferably 0.040% or less.

[0032] B: 0.0005~0.0100% B is an element effective for improving the hardenability of a steel sheet and turning the main phase of the microstructure of the steel sheet (hot stamped member) after hot stamping into tempered martensite. This effect is remarkable when the B content is 0.0005% or more, so the B content is set to 0.0005% or more. On the other hand, if the B content exceeds 0.0100%, not only does the effect saturate, but iron-based borides precipitate, and the effect of B in improving hardenability decreases. Therefore, the B content is set to 0.0100% or less. The B content is preferably 0.0080% or less, and more preferably 0.0050% or less.

[0033] In the steel sheet according to the present embodiment, the balance of the above elements may be Fe and impurities. The impurities refer to elements that may be mixed in during the manufacturing process of the steel sheet, etc., and are permissible within a range that does not clearly affect the steel sheet according to the present embodiment. Examples of impurities include the above-mentioned P, S, O, etc. When O is contained, it often forms an oxide and exists as an inclusion. On the other hand, the steel sheet according to this embodiment may further contain the following elements as necessary.

[0034] Ni: 0 to 2.00% Cu: 0-2.00% Cr: 0~2.00% Mo: 0 to 2.00% Ni, Cu, Cr, and Mo are elements that contribute to high strength by improving the hardenability of the steel sheet and turning the main phase of the microstructure of the steel sheet after hot stamping into tempered martensite. This effect becomes significant when one or more of Ni, Cu, Cr, and Mo are contained in an amount of 0.01% or more. Therefore, in order to obtain the above effect, it is preferable that the total content or each content of these elements is 0.01% or more. On the other hand, if the amount of each element is excessive, the weldability and hot workability deteriorate, or the strength of the steel sheet for hot stamping becomes too high, leading to manufacturing problems. Therefore, if these elements are contained, the content of Ni, Cu, Cr, and Mo is set to 2.00% or less.

[0035] Nb: 0 to 0.100% V: 0~0.100% W: 0~0.100% Nb, V, and W are elements that suppress the growth of austenite during hot stamping and contribute to increasing the strength and toughness of hot stamped components by strengthening fine grains. This effect is remarkable when one or more of Nb, V, and W are contained in an amount of 0.005% or more. Therefore, to obtain the above effect, it is preferable that the total content or each content of these elements is 0.005% or more. On the other hand, if the content of each element exceeds 0.100%, the amount of C that contributes to strengthening martensite is reduced due to the formation of carbides of Nb, V, and W, resulting in a decrease in strength. Therefore, when these elements are contained, the content of each of Nb, V, and W is set to 0.100% or less, and preferably 0.090% or less.

[0036] REM: 0~0.0500% Ca: 0 to 0.0500% Magnesium: 0 to 0.0500% REM, Ca, and Mg are elements that contribute to improving the strength and material properties of steel sheets. If the total content of one or more of REM and Ca is less than 0.0003%, sufficient effects cannot be obtained. Therefore, in order to obtain the above effects, it is preferable that the total content of REM, Ca, and Mg is 0.0003% or more. On the other hand, if the total content of one or more of REM, Ca, and Mg exceeds 0.0500%, castability and hot workability deteriorate, so if these elements are contained, the content of these elements is set to 0.0500% or less. REM is an abbreviation for Rare Earth Metal, and refers to Sc, Y, and elements belonging to the lanthanoid series. La and Ce are often included as REMs, and are often added as misch metals, but the effect can also be achieved by including elements of the lanthanoid series in combination with La and Ce, or by adding metals.

[0037] Sn: 0 to 0.200% Sn is an element that improves corrosion resistance. This effect is significant when the Sn content is 0.005% or more. Therefore, in order to obtain this effect, the Sn content is preferably 0.005% or more. On the other hand, if the Sn content exceeds 0.200%, the slab becomes embrittled, causing cracks during casting and cracks on the surface of the hot-rolled steel sheet, so if Sn is contained, the Sn content is set to 0.200% or less.

[0038] The above-mentioned chemical compositions may be measured by a general analytical method. For example, they may be measured using ICP-AES (Inductively Coupled Plasma-Atomic Emission Spectrometry). C and S may be measured using a combustion-infrared absorption method, and N may be measured using an inert gas fusion-thermal conductivity method.

[0039] The steel sheet according to the present embodiment may have a plating layer on the surface thereof. The plating layer is preferable because it prevents the formation of scale during hot stamping and improves corrosion resistance. The plating layer is not limited, but may be, for example, a hot-dip galvanized layer, a galvannealed hot-dip galvanized layer, an electrolytic galvanized layer, or an Al plating layer, which may be formed according to the application.

[0040] <Mechanical properties, plate thickness> Tensile strength (TS): preferably less than 980 MPa It is preferable that the steel sheet for hot stamping is easy to process during processing such as cutting, and has high strength after hot stamping. Therefore, if the tensile strength is, for example, 980 MPa or more, the wear of the shear blade becomes severe and correction of the sheet shape becomes difficult, so that the advantages of ease of cutting and ease of shape correction, which are one of the purposes of applying hot stamping, are lost, which is not preferable. Therefore, the tensile strength of the steel sheet according to this embodiment is preferably less than 980 MPa.

[0041] The tensile strength of a steel plate is determined by taking a tensile test piece having a JIS No. 5 shape from the steel plate so that the direction perpendicular to the rolling direction is the tensile direction, and conducting a tensile test in accordance with JIS Z 2241:2011.

[0042] The thickness of the steel plate according to the present embodiment is not limited. For example, it is 1.0 to 6.0 mm, but the thickness at which the effect of the steel plate according to the present embodiment becomes significant is 3.0 mm or more. However, even a thin steel plate of 1.0 to 3.0 mm can obtain a stable hardness even under conditions where the clearance with the die is large and the cooling rate is slow, so that the effect can be obtained even when used in applications where the plate thickness is small.

[0043] The steel sheet according to the present embodiment has excellent hardenability during hot stamping and excellent impact resistance after hot stamping. Therefore, for example, when the steel sheet is heated for 3 minutes or more in a heating furnace with an atmospheric temperature of 850 to 950°C, and then is hot stamped by cooling to a martensitic transformation start temperature or lower at a wide range of cooling rates of 10°C / sec or more, including a cooling rate as slow as 20°C / sec or less, the steel sheet has a tensile strength of 980 MPa or more and excellent impact resistance such that the maximum VDA bending angle is 80° or more when a VDA bending test described later is performed.

[0044] <Manufacturing method> The steel plate according to the present embodiment has the following properties. <1> or <2> It can be produced by the production method described in . <1> A heating process in which a steel ingot or slab having a predetermined chemical composition is heated to 1150 to 1300 °C, either directly or after cooling once; a hot rolling step of hot rolling the steel ingot or the slab after the heating step at a finishing temperature of 850°C or higher to obtain a hot rolled steel sheet; A coiling process in which the hot-rolled steel sheet after the hot rolling process is coiled at 640 to 450 ° C.; A holding step of holding the hot-rolled steel sheet after the coiling step in a temperature range of 500 to 450 ° C. for 1.0 hour or more; A cooling process of cooling the hot-rolled steel sheet after the holding process to room temperature; A manufacturing method comprising: <2> A heating process in which a steel ingot or slab having a predetermined chemical composition is heated to 1150 to 1300 °C, either directly or after cooling once; a hot rolling step of hot rolling the steel ingot or the slab after the heating step at a finishing temperature of 850°C or higher to obtain a hot rolled steel sheet; a coiling process in which the hot-rolled steel sheet after the hot rolling process is coiled at 700 to 500 ° C.; A cooling process of cooling the hot-rolled steel sheet after the coiling process to room temperature; A pickling process of pickling the hot-rolled steel sheet after the cooling process; A cold rolling process in which the hot-rolled steel sheet after the pickling process is cold-rolled at a cumulative reduction rate of 30 to 70% to obtain a cold-rolled steel sheet; An annealing process in which the cold-rolled steel sheet is heated to an annealing temperature range of 840 to 900 ° C. and held in the annealing temperature range for 10 to 2000 seconds; A heat treatment process in which the cold-rolled steel sheet after the annealing process is cooled to a temperature range of 400 to 600 ° C., held at the temperature range for 100 to 1000 seconds, and then cooled to room temperature; A manufacturing method comprising: The preferred conditions for each step are described below. The preferred conditions up to the hot rolling step are as follows: <1> , <2> Since the manufacturing method is the same for both of the above, they will be explained together. On the other hand, the transition to the winding process has different preferable condition ranges, <1> , <2> Each of the above will be described below. For conditions that are not described below, known conditions can be used.

[0045] [Heating process] <1> <2> common In the heating step, a steel ingot or slab produced by casting and having the same chemical composition as the steel plate according to the present embodiment described above is heated prior to hot rolling. As the slab to be subjected to hot rolling, a continuous cast slab or one produced by a thin slab caster or the like can be used. After casting, the slab may be heated once its temperature is lowered to near room temperature, or it may be reheated during the temperature drop. The heating temperature of the steel ingot or slab is 1150 to 1300°C. If the heating temperature is less than 1150°C, the finish rolling temperature will be lowered in the next hot rolling process, which will cause an increase in the load on the rolling machine. In this case, rolling will become difficult and the shape of the steel sheet after rolling will be defective. On the other hand, if the heating temperature exceeds 1300°C, not only will the cost increase, but it will also cause surface cracks. In this case, the impact resistance of the steel sheet after hot stamping (hot stamped member) will deteriorate.

[0046] [Hot rolling process] <1> <2> common In the hot rolling process, the heated steel ingot or slab is rolled so that the finish rolling temperature (the temperature at the exit of the final pass of finish rolling) is 850°C or higher to produce a hot-rolled steel sheet. If the finish rolling temperature is less than 850°C, the rolling load increases, making rolling difficult and causing defects in the shape of the steel sheet after rolling. There is no need to set an upper limit for the finish rolling temperature, but if the finish rolling temperature is made too high, the heating temperature in the heating process must be made too high to ensure that temperature. Therefore, it is preferable to set the finish rolling temperature to 1000°C or lower.

[0047] below, <1> The manufacturing method of the present invention will be described below from the winding step onward.

[0048] [Winding process] <1> In the coiling process, the hot-rolled steel sheet after the hot rolling process is coiled at 640 to 450°C. If the coiling temperature exceeds 640°C, structures such as ferrite and pearlite are formed, and the area ratio of upper bainite cannot be 70% or more in the microstructure of the hot-rolled steel sheet. In addition, the carbides present in the upper bainite become coarse, and the number density of iron-based carbides cannot be sufficiently obtained. Coarse carbides are difficult to melt even when heated during hot stamping, which causes a decrease in hardenability, and the unmelted coarse carbides become crack initiation points, which causes a decrease in impact resistance after hot stamping. For this reason, the coiling temperature is set to 640°C or less. On the other hand, if the coiling temperature is less than 450°C, the structure of the steel sheet will be mainly martensite, resulting in excessively high strength and reduced formability.

[0049] [Holding process] <1> In the holding step, the hot-rolled steel sheet after the coiling step is held in a temperature range of 500 to 450° C. for 1.0 hour or more. By this holding, the area ratio of upper bainite in the microstructure is set to 70% or more, and iron-based carbides with a major axis of 0.1 μm or more are formed in the upper bainite to a ratio of 1 μm or more. 2 Precipitate 4 or more particles per side. When the temperature is maintained at more than 500°C, the carbides in the upper bainite become coarse, and the number density of iron-based carbides with a major axis of 0.1 μm or more becomes 1 μm. 2 There cannot be more than four per side. On the other hand, when the temperature is maintained below 450°C, many carbides with major axes less than 0.1 μm are precipitated, and the strength of the steel sheet increases excessively due to strengthening. 2 There cannot be more than four per side. In addition, even if the holding time in the temperature range of 500 to 450 °C is less than 1.0 hour, the number density of iron-based carbides with a major axis of 0.1 μm or more is 1 μm 2 There cannot be more than four per side. The temperature does not need to be kept constant, and may vary as long as it is within the temperature range of 500 to 450° C. In addition, when the material is left to stand after normal winding, it is difficult to hold the material at 500 to 450° C. for 1.0 hour or more, so the material may be held at this temperature for 1.0 hour or more by insuring or heating. <1> When the manufacturing method described above is used as a premise, it is difficult to substitute the holding step with a BAF (box annealing furnace). Since the steel sheet according to the present embodiment has high hardenability, if it is cooled without holding, it is likely to have a structure mainly composed of martensite. Therefore, even if a heat treatment is performed in a post-process using BAF or the like after cooling, it will have a structure mainly composed of tempered martensite, and it is difficult to make the area ratio of upper bainite 70% or more. In addition, coarse carbides may precipitate due to the BAF, resulting in poor hardenability during hot stamping.

[0050] [Cooling process] <1> In the cooling step, the hot-rolled steel sheet after the holding step is cooled to room temperature. The cooling conditions are not particularly limited.

[0051] [Pickling process] <1> After the cooling step, pickling may be performed to remove scale formed on the surface of the steel sheet. Pickling may be performed by any method capable of removing scale, and may be performed using hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, or a mixture of these. An inhibitor may be added to suppress dissolution of the base steel. Pickling may be performed in one step or in multiple steps.

[0052] [Cold rolling process] <1> The hot-rolled steel sheet after the pickling process may be further subjected to cold rolling to obtain a cold-rolled steel sheet. When cold rolling is performed, if the cumulative reduction is less than 30%, it becomes difficult to keep the shape of the steel sheet flat, and the ductility of the final product deteriorates. On the other hand, if the cumulative reduction exceeds 70%, the rolling load becomes too large, making cold rolling difficult. Therefore, the cumulative reduction is preferably set to 30 to 70%. The cumulative reduction is more preferably 40 to 70%. The number of rolling passes and the reduction rate per pass are not particularly limited.

[0053] below, <2> The manufacturing method of the present invention will be described below from the winding step onward.

[0054] [Winding process] <2> In the coiling process, the hot-rolled steel sheet after the hot rolling process is coiled at 700 to 500°C. If the coiling temperature exceeds 700°C, the structure of the steel sheet will become a ferrite and pearlite structure, so the coiling temperature is set to 700°C or less. On the other hand, if the coiling temperature is less than 500°C, the structure of the steel sheet will be mainly martensite, resulting in excessively high strength and reduced formability.

[0055] [Cooling process] <2> In the cooling step, the hot-rolled steel sheet after the coiling step is cooled to room temperature. The cooling conditions are not particularly limited.

[0056] [Pickling process] <2> In the pickling process, scale formed on the surface of the steel sheet after the cooling process is removed. Pickling may be performed by any method capable of removing scale, and may be performed using hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, or a mixture of these. An inhibitor may be added to suppress dissolution of the base steel. Pickling may be performed in one step or in multiple steps.

[0057] [Cold rolling process] <2> The hot-rolled steel sheet after the pickling process is cold-rolled to obtain a cold-rolled steel sheet. When cold-rolling is performed, if the cumulative reduction is less than 30%, it becomes difficult to keep the shape of the steel sheet flat, and the ductility of the final product deteriorates. On the other hand, if the cumulative reduction exceeds 70%, the rolling load becomes too large, making cold rolling difficult. Therefore, the cumulative reduction is set to 30 to 70%. The cumulative reduction is preferably 40 to 70%. The number of rolling passes and the reduction per pass do not need to be particularly specified.

[0058] [Annealing process] <2> In the annealing step, the cold-rolled steel sheet obtained by cold rolling is heated to an annealing temperature of 840 to 900° C., and is held at this annealing temperature for 10 to 2000 seconds. If the annealing temperature is less than 840°C, it is not possible to obtain a single austenite phase during annealing, and it is not possible to obtain an upper bainite area ratio of 70% or more by subsequent heat treatment.On the other hand, if the annealing temperature exceeds 950°C, the effect is saturated, and not only is it inferior in economic efficiency, but also the bainite transformation is delayed due to the coarsening of the austenite grain size, so that it is not possible to obtain an upper bainite ratio of 70% or more by subsequent holding at a temperature range of 400 to 600°C for 100 to 1000 seconds. Furthermore, if the annealing time (holding time) is less than 10 seconds, the carbides formed by hot rolling cannot be dissolved, making it impossible to form a single austenite phase during annealing, and the area ratio of upper bainite cannot be increased to 70% or more by subsequent heat treatment. On the other hand, if the annealing time exceeds 2000 seconds, the austenite becomes coarse and the bainite transformation is delayed, making it impossible to ensure 70% or more of upper bainite by subsequent holding in the temperature range of 400 to 600°C for 100 to 1000 seconds.

[0059] [Heat treatment process] <2> In the heat treatment step, the cold-rolled steel sheet after the annealing step (after holding for a predetermined time) is cooled to a temperature range of 400 to 600° C., held in this temperature range for 100 to 1000 seconds, and then cooled to room temperature. This heat treatment increases the area ratio of upper bainite in the microstructure to 70% or more, and also increases the number of iron-based carbides with a major axis of 0.1 μm or more to 1 μm in the upper bainite. 2 Precipitate 4 or more particles per side. If the holding temperature exceeds 600°C, ferrite and pearlite are generated, and the area ratio of upper bainite cannot be set to 70% or more. On the other hand, if the holding temperature is less than 400°C, the structure will be mainly martensite. In addition, if the holding time is less than 100 seconds, the area ratio of upper bainite cannot be sufficiently obtained, and martensite is formed during the subsequent cooling, so that the area ratio of upper bainite in the steel sheet after cooling cannot be 70% or more. On the other hand, if the holding time exceeds 1000 seconds, the number density of iron-based carbides of 0.1 μm or more decreases to 1 μm or less due to the coarsening of the carbides. 2 There will be less than four per side. After the temperature is maintained, the material is cooled to room temperature. The cooling conditions are not particularly limited as long as the time for which the material is maintained at 400 to 600° C. does not exceed 1000 seconds.

[0060] [Plating process] <2> When forming a plating layer on the surface of the steel sheet, the cold-rolled steel sheet may be immersed in a plating bath after the annealing step and before the heat treatment step, or after the heat treatment step. The bath temperature of the plating bath is usually 400 to 600°C, even in the case of zinc plating or plating containing other elements, and immersion in the plating bath forms a plating layer on the surface and upper bainite in the steel sheet. However, since the immersion time does not exceed 100 seconds in a normal plating device, the heat treatment step cannot be omitted even if the plating step is performed. When a plating step is performed, the upper limit of the holding time in the heat treatment step is preferably set to 1000 seconds minus the immersion time in the plating bath.

[0061] [Alloying process] <2> After the plating process (or, if the plating process is performed before the heat treatment process, after the plating process and before the heat treatment process), the cold-rolled steel sheet having a plating layer formed on its surface may be held in a temperature range of 450 to 600°C (alloying temperature range) to alloy the plating layer. When the plating step and the alloying step are performed, the upper limit of the holding time in the heat treatment step is preferably set to 1000 seconds minus the time for immersion in the plating bath and the time for holding at 450 to 600° C. for alloying.

[0062] Next, the hot stamped member according to this embodiment will be described.

[0063] <Chemical composition> The hot stamped member according to this embodiment is obtained by hot stamping the steel sheet according to the embodiment described above (steel sheet for hot stamping). Since the chemical composition does not substantially change due to hot stamping, the range of the chemical composition of the hot stamped member according to this embodiment is the same as that of the steel sheet according to the embodiment described above. Therefore, the description will be omitted here.

[0064] <Microstructure> [Tempered martensite: 90% or more by area] The reason why the tempered martensite content is set at 90% or more is to achieve both tensile strength and bendability. If the area ratio of ferrite and upper bainite exceeds 10%, a strength of 980 MPa or more cannot be secured, and if the fresh martensite content exceeds 10%, the angle at the time of crack initiation in the VDA test falls below 80°, resulting in poor impact resistance. For this reason, the tempered martensite content is set at 90% or more. Tempered martensite is martensite that contains carbides. In this embodiment, the tempered martensite is ensured in the hot stamping process by controlling the chemical composition of the steel sheet for hot stamping and the microstructure of the steel sheet for hot stamping, rather than by performing a special heat treatment. That is, the martensite transformation start temperature is increased by limiting the C content to 0.060 to 0.120%, and the microstructure of the steel sheet for hot stamping is mainly upper bainite, so that martensite is formed during cooling in the hot stamping process, and carbides are precipitated in the martensite to obtain tempered martensite. As the microstructure other than tempered martensite, ferrite, pearlite, upper bainite, lower bainite, and fresh martensite (martensite not containing carbides) may be included as long as their area ratio is less than 10%.

[0065] The area ratio of each phase in the microstructure can be determined by the following method. First, the hot stamped part (compact) is cut in a direction parallel to the rolling direction, polished, and etched with Nital reagent. Then, using an SEM, the part is imaged at 8000 μm at a magnification of 1000 to 30000 times. 2 In the above range, by observing a position of 1 / 4 of the sheet thickness from the surface in the sheet thickness direction, it is possible to identify ferrite, upper bainite, lower bainite, pearlite, tempered martensite, and fresh martensite. The microstructure of the hot stamped member according to this embodiment has the same microstructure whether observed from a direction parallel to or perpendicular to the rolling direction of the steel sheet, so long as it is at a position of 1 / 4 of the sheet thickness from the surface in the sheet thickness direction. As with steel sheets for hot stamping, identification can be made from the structure morphology, such as that ferrite is equiaxed grains that do not contain iron carbides, pearlite is a layered structure of ferrite and cementite, upper bainite is a structure with a lath-like shape that contains cementite and retained austenite between the laths, and lower bainite contains carbides within the laths. The area ratio of each identified structure is obtained from the SEM observation image. Martensite exists in both tempered martensite, which contains carbides in the laths, and as-quenched martensite (fresh martensite), which does not contain carbides, and these can be identified by observing with a SEM or TEM to confirm the presence or absence of carbides. For example, 10 fields of view of 30 μm × 25 μm are observed at a magnification of 3000 times, and the average value is taken as the area ratio.

[0066] <Characteristics> The hot stamped member according to the present embodiment has high strength and excellent impact resistance. In the present embodiment, excellent impact resistance means that the member is unlikely to break even if it is deformed during impact, and means that the VDA maximum bending angle is 80° or more in the method described in VDA238-100. Also, high strength means that the tensile strength is 980 MPa or more.

[0067] The VDA maximum bend angle (bendability) is measured in accordance with the method described in VDA 238-100. Specifically, the thickness of the steel sheet is reduced to 1.2 mm from one side, and then the VDA bend test is performed so that the hot stamped surface that has not been subjected to thickness reduction is on the outside of the bend. In VDA238-100, the test piece size is 60 mm wide x 60 mm long, but depending on the material, the flat surface is limited and it is difficult to take test pieces of this size. For this reason, in order to measure the bending property of a molded body, the test piece size may be changed to, for example, 30 mm wide x 60 mm long, and the bending property may be evaluated by changing the width.

[0068] <Method of manufacturing components> Next, a method for producing a hot-stamped member according to this embodiment will be described.

[0069] The method for producing a hot stamped member according to the present embodiment includes a hot stamping step in which the steel sheet (steel sheet for hot stamping) according to the present embodiment obtained by the above-mentioned method is heated for 3 minutes or more in a heating furnace with an atmospheric temperature of 850 to 950°C, and then cooled to a martensitic transformation start temperature or lower at a cooling rate of 10°C / sec or higher. Here, the cooling rate is a value obtained by dividing the difference between the temperature at which the steel sheet is removed from the furnace and the temperature at which the die cooling is completed by the time from removal from the furnace to the completion of die cooling. The effect of the present invention can be obtained without particularly setting the die removal temperature (die cooling completion temperature), but since a die removal temperature exceeding 200°C causes safety issues such as burns, it is preferable to set the die removal temperature to 200°C or lower. According to this manufacturing method, a hot stamped member having an area ratio of tempered martensite of 90% or more, a tensile strength of 980 MPa or more, and excellent impact resistance properties can be obtained. If the atmospheric temperature is less than 850°C or the heating time is less than 3 minutes, austenite transformation does not occur sufficiently, the area ratio of tempered martensite in the hot stamped component does not reach 90% or more, and sufficient strength is not obtained. Moreover, if the atmospheric temperature exceeds 950°C, not only will the effect saturate, but the austenite grains will become excessively coarse, resulting in a decrease in TS, which is undesirable. EXAMPLES

[0070] Example 1 A slab having the chemical composition shown in Table 1 was cast, heated to 1150 to 1300°C, and then hot-rolled to the finish rolling temperature shown in Table 2A to obtain a hot-rolled steel sheet (HR) having a thickness of 4.0 mm. Thereafter, the film was wound at the winding temperature shown in Table 2A, and held at 500 to 450° C. for the time shown in Table 2A. Thereafter, the mixture was cooled to room temperature by air cooling. Some of the steel sheets were then pickled to remove scale formed on the surface, and cold rolled at a cumulative reduction rate of 50% to produce cold-rolled steel sheets (FH) with a thickness of 2.0 mm.

[0071] The microstructure of the obtained steel plate (hot-rolled steel plate or cold-rolled steel plate) was observed at a position from the surface to 1 / 4 of the plate thickness using the method described above, and the upper bainite area fraction and the number density of iron-based carbides with a major axis of 0.1 μm or more were determined. The results are shown in Tables 2A and 2B. In Tables 2A and 2B, the first letters A to N and a to m of the steel numbers indicate that steels having chemical compositions A to N and a to m in Table 1 were used, respectively.

[0072] The tensile strength of the resulting steel sheets was determined by the method described above.

[0073] In addition, a 350 mm x 650 mm sample was taken from the obtained steel sheet, and this sample was heated in a furnace at a temperature of 910°C for 6 minutes to simulate hot stamping using a hat-shaped die, and then immediately cooled in the die at the cooling rate shown in Table 2B. The cooling rate was determined by dividing the difference between the temperature at removal from the furnace and the temperature at removal from the die by the time from removal from the furnace to the end of die cooling.

[0074] After the die had been cooled, the microstructure of the sample (hot stamped part) was observed at a position 1 / 4 of the plate thickness from the surface using the method described above.

[0075] In addition, a tensile test piece having a JIS No. 5 shape was taken from the sample (hot stamped part (formed body)) after the die cooling was completed, and a tensile test was performed according to JIS Z 2241: 2011 to determine the tensile strength. If the tensile strength (TS) was 980 MPa or more, it was determined that the hardenability of the steel plate was sufficient. The results are shown in Table 2B.

[0076] In addition, a bending test piece measuring 50 x 50 mm was taken from the sample (molded body) after the die had finished cooling. At that time, it was ground from one side until the plate thickness was 1.2 mm. After that, a VDA bending test was carried out in accordance with VDA238-100, with the polished surface facing the punch side. If the VDA maximum bending angle was 80° or more, it was determined that the impact resistance characteristics were excellent (cracks could be suppressed during large deformation). The results are shown in Table 2B.

[0077] [Table 1]

[0078] [Table 2A]

[0079] [Table 2B]

[0080] As can be seen from Table 1 and Tables 2A to 2B, the examples of the present invention had a tensile strength (TS) of 980 MPa or more and a VDA maximum bending angle of 80° or more after hot stamping. In contrast, the comparative examples were inferior in at least either the tensile strength (TS) after hot stamping or the maximum VDA bending angle.

[0081] Example 2 A slab having the chemical composition shown in Table 1 was heated to 1180 to 1250°C, and then hot-rolled to a finishing temperature of 880 to 960°C to obtain a hot-rolled steel sheet having a thickness of 4.0 mm. The hot-rolled steel sheet was then coiled at a coiling temperature of 700 to 500°C, cooled to room temperature by air-cooling, and pickled to remove scale formed on the surface. The hot-rolled steel sheet was then cold-rolled at a cumulative reduction rate of 50% to obtain a cold-rolled steel sheet having a thickness of 2.0 mm. Furthermore, this cold-rolled steel sheet was annealed and heat treated under the conditions shown in Table 3A to obtain a cold-rolled steel sheet (CR).

[0082] For the obtained steel plate, the microstructure was observed to determine the area fraction of upper bainite and the number density of iron-based carbides having a major axis of 0.1 μm or more in the same manner as in Example 1. In addition, a tensile test was performed to determine the tensile strength. The results are shown in Tables 3A and 3B.

[0083] In addition, a 350 x 650 mm sample was taken from the obtained steel sheet, and this sample was heated in a furnace at a temperature of 910°C for 4 minutes to simulate hot stamping using a hat-shaped die, and then immediately cooled in the die. The cooling rate was as shown in Table 3C. The cooling rate was determined by dividing the difference between the temperature at removal from the furnace and the temperature at removal from the die by the time from removal from the furnace to the end of die cooling.

[0084] After the die cooling was completed, the sample (formed body) was subjected to microstructural observation in the same manner as in Example 1. In addition, a tensile test was performed to determine the tensile strength in the same manner as in Example 1. If the tensile strength (TS) was 980 MPa or more, it was determined that the hardenability of the steel sheet was sufficient. The results are shown in Table 3B.

[0085] In addition, a VDA bending test was performed on the sample (molded body) after the die cooling was completed in the same manner as in Example 1. If the VDA maximum bending angle was 80° or more, it was determined that the impact resistance characteristics were excellent (cracking could be suppressed during large deformation). The results are shown in Table 3B. In Tables 3A and 3B, the first letters A to N and a to m of the steel numbers indicate that steels having chemical compositions A to N and a to m in Table 1 were used, respectively.

[0086] [Table 3A]

[0087] [Table 3B]

[0088] As can be seen from Table 1 and Tables 3A to 3B, the examples of the present invention had a tensile strength (TS) of 980 MPa or more and a VDA maximum bending angle of 80° or more after hot stamping. In contrast, the comparative examples were inferior in at least either the tensile strength (TS) after hot stamping or the maximum VDA bending angle.

[0089] Example 3 A slab having the chemical composition shown in Table 1 was heated to 1180 to 1250°C, and then hot-rolled to a finishing temperature of 880 to 960°C to obtain a hot-rolled steel sheet having a thickness of 4.0 mm. The hot-rolled steel sheet was then coiled at a coiling temperature of 680 to 500°C, cooled to room temperature by air-cooling, and then pickled to remove scale formed on the surface. The hot-rolled steel sheet was then cold-rolled at a cumulative reduction rate of 50% to obtain a cold-rolled steel sheet having a thickness of 2.0 mm. Furthermore, this cold-rolled steel sheet was annealed and heat treated under the conditions shown in Table 4A to obtain a cold-rolled steel sheet (CR). Thereafter, an annealing step, a heat treatment step, a plating step, and, if necessary, an alloying step were performed using a hot-dip galvanizing facility. The plating step and the alloying step were performed either after the annealing step and before the heat treatment step, or after the heat treatment step. As a result, a hot-dip galvanized steel sheet (GI) or a galvannealed steel sheet (GA) was obtained.

[0090] For the obtained steel plate, the microstructure was observed to determine the area fraction of upper bainite and the number density of iron-based carbides having a major axis of 0.1 μm or more in the same manner as in Example 1. In addition, a tensile test was performed to determine the tensile strength. The results are shown in Tables 4B and 4C.

[0091] In addition, a 350 x 650 mm sample was taken from the obtained steel sheet, and this sample was heated for 4 minutes in a furnace at a temperature of 910°C to simulate hot stamping, and then immediately cooled in a die. The cooling rate was as shown in Table 4C. The cooling rate was determined by dividing the difference between the temperature at removal from the furnace and the temperature at removal from the die by the time from removal from the furnace to the end of die cooling.

[0092] After the die cooling was completed, the sample (formed body) was subjected to microstructural observation in the same manner as in Example 1. In addition, a tensile test was performed to determine the tensile strength in the same manner as in Example 1. If the tensile strength (TS) was 980 MPa or more, it was determined that the hardenability of the steel sheet was sufficient. The results are shown in Table 4C.

[0093] In addition, a VDA bending test was performed on the sample (molded body) after the die cooling was completed in the same manner as in Example 1. If the VDA maximum bending angle was 80° or more, it was determined that the impact resistance characteristics were excellent (cracking could be suppressed during large deformation). The results are shown in Table 4C. In Tables 4A to 4C, the first letters A to N and a to m of the steel numbers indicate that steels having chemical compositions A to N and a to m in Table 1 were used, respectively.

[0094] [Table 4A]

[0095] [Table 4B]

[0096] [Table 4C]

[0097] As can be seen from Table 1 and Tables 4A to 4C, the examples of the present invention had a tensile strength (TS) of 980 MPa or more and a VDA maximum bending angle of 80° or more after hot stamping. In contrast, the comparative examples were inferior in at least either the tensile strength (TS) after hot stamping or the maximum VDA bending angle.

Claims

1. In mass percent, C: 0.060-0.120%, Si: 0 to 0.70%, Mn: 1.60-3.00%, P: 0.100% or less, S: 0.0100% or less, N: 0.0100% or less, Al: 0.001-0.100%, Ti: 0.005-0.050%, B: 0.0005-0.0100%, Nb: 0 to 0.100%, V: 0-0.100%, W: 0-0.100%, Ni: 0-2.00%, Cu: 0-2.00%, Cr: 0-2.00%, Mo: 0-2.00%, Sn: 0-0.200%, Ca: 0-0.0500%, Mg: 0 to 0.0500%, and REM: 0 to 0.0500% The balance has a chemical composition consisting of Fe and impurities, The microstructure contains upper bainite of 70% or more by area ratio, The number density of iron-based carbides having a major axis of 0.1 μm or more contained in the upper bainite is 4 / μm 2 That's all. Steel plate for hot stamping.

2. The chemical composition, in mass%, Nb: 0.005-0.100%, V: 0.005-0.100%, W: 0.005-0.100%, Ni: 0.01-2.00%, Cu: 0.01-2.00%, Cr: 0.01-2.00%, Mo: 0.01-2.00%, Sn: 0.005-0.200%, Ca: 0.0003-0.0500%, Mg: 0.0003 to 0.0500%, and REM: 0.0003-0.0500%, Contains one or more selected from The steel sheet for hot stamping according to claim 1.

3. The steel sheet for hot stamping according to claim 1 or 2, having a tensile strength of less than 980 MPa.

4. The steel sheet for hot stamping according to any one of claims 1 to 3, having a plating layer on a surface thereof.

5. The steel sheet for hot stamping according to claim 4, wherein the plating layer is a hot-dip galvanized layer, a galvannealed layer, an electrolytic galvanized layer, or an Al plating layer.

6. A method for producing a steel sheet for hot stamping according to claim 1, comprising: A heating step of heating a steel ingot or slab having the chemical composition according to claim 1 to 1150 to 1300°C, either directly or after cooling once; a hot rolling step of hot rolling the steel ingot or the slab after the heating step at a finishing temperature of 850° C. or higher to obtain a hot-rolled steel sheet; A winding process in which the hot-rolled steel sheet after the hot rolling process is wound at 640 to 450 ° C.; A holding step of holding the hot-rolled steel sheet after the coiling step in a temperature range of 500 to 450 ° C. for 1.0 hour or more; A cooling process of cooling the hot-rolled steel sheet after the holding process to room temperature; Equipped with A manufacturing method of steel sheet for hot stamping.

7. The manufacturing method of a steel sheet for hot stamping according to claim 6, further comprising a cold rolling step of cold rolling the hot-rolled steel sheet after the holding step at a cumulative rolling reduction rate of 30 to 70% to obtain a cold-rolled steel sheet.

8. A method for producing a steel sheet for hot stamping according to claim 1, comprising: A heating step of heating a steel ingot or slab having the chemical composition according to claim 1 to 1150 to 1300°C, either directly or after cooling once; a hot rolling step of hot rolling the steel ingot or the slab after the heating step at a finishing temperature of 850° C. or higher to obtain a hot-rolled steel sheet; A winding process in which the hot-rolled steel sheet after the hot rolling process is wound at 700 to 500 ° C.; A cooling process of cooling the hot-rolled steel sheet after the coiling process to room temperature; A pickling process of pickling the hot-rolled steel sheet after the cooling process; A cold rolling process in which the hot-rolled steel sheet after the pickling process is cold-rolled at a cumulative reduction rate of 30 to 70% to obtain a cold-rolled steel sheet; An annealing step of heating the cold-rolled steel sheet to an annealing temperature range of 840 to 900 ° C. and holding the cold-rolled steel sheet in the annealing temperature range for 10 to 2000 seconds; A heat treatment process in which the cold-rolled steel sheet after the annealing process is cooled to a temperature range of 400 to 600 ° C., held at the temperature range for 100 to 1000 seconds, and then cooled to room temperature; Equipped with A manufacturing method of steel sheet for hot stamping.

9. The method for producing a steel sheet for hot stamping according to claim 8, further comprising a plating step of immersing the cold-rolled steel sheet after the heat treatment step in a plating bath to form a plating layer on a surface thereof.

10. The method for producing a steel sheet for hot stamping according to claim 9, further comprising an alloying step of holding the cold-rolled steel sheet after the plating step in an alloying temperature range of 450 to 600 ° C. to alloy the plating layer.

11. The method for producing a steel sheet for hot stamping according to claim 8, further comprising a plating step of immersing the cold-rolled steel sheet after the annealing step and before the heat treatment step in a plating bath to form a plating layer on a surface thereof.

12. The method for producing a steel sheet for hot stamping according to claim 11, further comprising an alloying step of holding the cold-rolled steel sheet after the plating step and before the heat treatment step in an alloying temperature range of 450 to 600 ° C. to alloy the plating layer.

13. In mass percent, C: 0.060-0.120%, Si: 0 to 0.70%, Mn: 1.60-3.00%, P: 0.100% or less, S: 0.0100% or less, N: 0.0100% or less, Al: 0.001-0.100%, Ti: 0.005-0.050%, B: 0.0005-0.0100%, Nb: 0 to 0.100%, V: 0-0.100%, W: 0-0.100%, Ni: 0-2.00%, Cu: 0-2.00%, Cr: 0-2.00%, Mo: 0-2.00%, Sn: 0-0.200%, Ca: 0-0.0500%, Mg: 0 to 0.0500%, and REM: 0 to 0.0500% The balance has a chemical composition consisting of Fe and impurities, The microstructure contains tempered martensite at an area ratio of 90% or more. A hot stamped member characterized by:

14. The chemical composition, in mass%, Nb: 0.005-0.100%, V: 0.005-0.100%, W: 0.005-0.100%, Ni: 0.01-2.00%, Cu: 0.01-2.00%, Cr: 0.01-2.00%, Mo: 0.01-2.00%, Sn: 0.005-0.200%, Ca: 0.0003-0.0500%, Mg: 0.0003 to 0.0500%, and REM: 0.0003-0.0500%, Contains one or more selected from The hot stamped component of claim 13.

15. A method for producing a hot stamped component according to claim 13, comprising the steps of: A method for producing a hot stamped member, comprising: heating the hot stamping steel sheet according to any one of claims 1 to 5 for 3 minutes or more using a heating furnace at an atmospheric temperature of 850 to 950 ° C., and then cooling the hot stamping steel sheet at a cooling rate of 10 ° C. / sec or more to a martensitic transformation start temperature or lower.

16. The method for producing a hot-stamped member according to claim 15, wherein the cooling rate in the hot stamping step is 10 to 20 ° C. / sec.

Citation Information

Patent Citations

  • Soldering method and device

    JP1979007168A

  • Manufacturing method for collision reinforcing material for vehicle and collision reinforcing material

    JP2002102980A

  • High strength hot rolled steel sheet for hot forming with reduced cracking in cooling and coiling and manufacturing method thereof

    KR1020090071177A

  • Method for producing a component by hot forming a pre-product made of steel

    US20160130675A1

  • Steel sheet for hot pressing use, method for producing same, and hot press steel sheet member

    WO2014027682A1