Surface-treated steel sheet

The surface-treated steel sheet with a Zn-Al-Mg plated steel sheet and a specifically formulated coating film addresses the challenge of achieving both corrosion resistance and weldability, particularly at joints, by controlling the adhesion of Al and Mg during welding, resulting in enhanced performance in corrosion resistance and weldability tests.

WO2024204822A1PCT designated stage expired Publication Date: 2024-10-03NIPPON STEEL CORPORATION

Patent Information

Application Number
PCT/JP2024/013330
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-29
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Surface-treated steel sheets used in applications like automobile parts face challenges in achieving both excellent corrosion resistance and weldability, particularly at joints where chemical conversion and electrodeposition coatings may not fully cover, exposing these areas to corrosive environments and affecting weld quality.

Method used

A surface-treated steel sheet with a Zn-Al-Mg plated steel sheet coated with a film containing a binder resin, doped zinc oxide particles, and a rust inhibitor, along with an optional intermediate coating film, is developed. The coating film has specific composition and thickness ranges to enhance corrosion resistance and weldability by controlling the adhesion of Al and Mg during welding and ensuring effective contact with the welding electrode.

Benefits of technology

The solution provides improved corrosion resistance and weldability by reducing Al and Mg adhesion to the welding electrode, preventing welding defects, and maintaining the performance of the coating film, as demonstrated through corrosion resistance and spot weldability tests.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024013330_03102024_PF_FP_ABST
    Figure JP2024013330_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a surface-treated steel sheet comprising a Zn-Al-Mg plated steel sheet having a plating amount of 20-60 g / m2 per one surface and a coating film disposed on at least one main surface of the Zn-Al-Mg plated steel sheet, wherein the coating film comprises a binder resin, doped zinc oxide particles, and a rust preventive, the coating film has an average film thickness of 0.5-3 μm, the doped zinc oxide particles have an average particle diameter of 0.1-2 μm, the content of the doped zinc oxide particles is 20-40 mass% with respect to the coating film, and the content of inorganic substances other than any Zn-containing compounds in the coating film is 0-1 mass% with respect to the coating film.
Need to check novelty before this filing date? Find Prior Art

Description

Surface-treated steel sheet

[0001] The present disclosure relates to a surface-treated steel sheet.

[0002] Surface-treated steel sheets are assembled into the desired shape by, for example, press forming, spot welding, or the like, followed by electroplating. If electroplating is omitted, they are then coated with an undercoat and used as automotive components. The corrosion resistance of automotive components is often ensured by a chemical conversion coating applied in a chemical conversion treatment process and an electroplating coating applied in a subsequent electroplating process. However, at the joints (sheet joints) of formed materials of surface-treated steel sheets, particularly at the joints on the inner surface of bag-shaped components and at folded hems, there may be areas where the chemical conversion coating and electroplating coating do not extend. In such cases, the joints of formed materials are likely to be exposed to a corrosive environment in their bare state. For this reason, there is a demand for surface-treated steel sheets that can ensure corrosion resistance.

[0003] Thus, surface-treated steel sheets must have an electrically conductive coating film to improve weldability so that resistance welding is possible, and must also be provided with corrosion resistance.

[0004] For example, Patent Document 1 describes a surface-treated steel sheet having a coating film on at least one side of a plated steel sheet, the coating film containing a binder resin, V-containing non-oxide ceramic particles (excluding VC particles), and doped zinc oxide particles, the content of the V-containing non-oxide ceramic particles and the doped zinc oxide particles relative to the coating film satisfying the following formula: C Zn ≧10.0 ... (1) CV ≦0.5・C Zn ...(2) CV ≦70-C Zn ...(3) CV ≧0.125・C Zn ... (4) CV ≧ 2.0 ... (5) where CV means the content (mass%) of the V-containing non-oxide ceramic particles, and CZn means the content (mass%) of the doped zinc oxide particles." has been proposed." has been proposed." Patent Document 1 states that "a surface-treated steel sheet having excellent corrosion resistance and weldability before electrodeposition coating can be provided."

[0005] Patent Document 1: International Publication No. 2018 / 092244

[0006] Surface-treated steel sheets are widely used for applications such as automobile components, machine components, home appliance components, and building materials, and are required to have improved corrosion resistance and weldability. However, although various research and development efforts have been conducted in the past, including the above-mentioned Patent Document 1, recent demands currently demand further improvements in the corrosion resistance and weldability of surface-treated steel sheets.

[0007] Therefore, an object of the present disclosure is to provide a surface-treated steel sheet that is excellent in both corrosion resistance and weldability.

[0008] The means for solving the above problems include the following aspects: <1> A plating coating weight per side is 20 to 60 g / m 2 and a coating film disposed on at least one main surface of the Zn-Al-Mg plated steel sheet, wherein the coating film contains a binder resin, doped zinc oxide particles, and a rust inhibitor, the coating film having an average thickness of 0.5 to 3 μm, the doped zinc oxide particles having an average particle size of 0.1 to 2 μm, the doped zinc oxide particles having a content of 20 to 40 mass% of the coating film, and a content of inorganic substances other than Zn-containing compounds in the coating film being 0 to 1 mass% or less of the coating film. <2> The surface-treated steel sheet according to <1>, wherein the rust inhibitor is an organic acid, and the content of the rust inhibitor is 1 to 20 mass% of the coating film. <3> The surface-treated steel sheet according to <1> or <2>, further comprising an intermediate coating film between the Zn-Al-Mg-plated steel sheet and the coating film, the intermediate coating film containing a binder resin, a silane coupling agent, silica fine particles, a phosphate compound, and a fluorine compound, and the intermediate coating film has an average thickness of 0.1 to 0.5 μm. <4> The surface-treated steel sheet according to any one of <1> to <3>, wherein the Zn-Al-Mg-plated layer of the Zn-Al-Mg-plated steel sheet has a chemical composition containing, on average, 4 to 22 mass% Al and 1.0 to 10 mass% Mg, with the balance containing Zn and impurities.

[0009] According to the present disclosure, it is possible to provide a surface-treated steel sheet that is excellent in both corrosion resistance and weldability.

[0010] Fig. 1 is a schematic cross-sectional view showing an example of a surface-treated steel sheet according to the present embodiment. Fig. 2 is a cross-sectional view showing an example of a coated member according to the present embodiment. Fig. 3 is a schematic plan view showing a bonded test piece prepared in a corrosion resistance test of an example. Fig. 4 is a schematic side view showing a bonded test piece prepared in a corrosion resistance test of an example.

[0011] An embodiment serving as an example of the present disclosure will be described below. In this specification, when the lower limit of the content of each element in a chemical composition is expressed as "0," this means that the element is an optional component and may not be present. In a numerical range expressed using "to", when the numerical values ​​before and after "to" are not followed by "greater than" or "less than," this means a range that includes these numerical values ​​as the lower and upper limits. Furthermore, when the numerical values ​​before and after "to" are followed by "greater than" or "less than," this means a range that does not include these numerical values ​​as the lower or upper limits. In numerical ranges expressed in stages, the upper limit of a certain numerical range may be replaced by the upper limit of another numerical range described in stages, or may be replaced by a value shown in an example. Furthermore, the lower limit of a certain numerical range may be replaced by the lower limit of another numerical range described in stages, or may be replaced by a value shown in an example. The term "process" does not only refer to an independent process, but also includes processes that cannot be clearly distinguished from other processes, as long as the intended purpose of the process is achieved.

[0012] <Surface-treated steel sheet> The surface-treated steel sheet according to this embodiment has a coating weight of 20 to 60 g / m 2and a coating film disposed on at least one main surface of the Zn-Al-Mg-plated steel sheet (see FIG. 1 ), wherein the coating film contains a binder resin, doped zinc oxide particles, and a rust inhibitor, wherein the coating film has an average thickness of 0.5 to 3 μm, the doped zinc oxide particles have an average particle size of 0.1 to 2 μm, the doped zinc oxide particles are contained in an amount of 20 to 40 mass % of the coating film, and the coating film contains inorganic substances other than Zn-containing compounds in an amount of 0 to 1 mass % of the coating film. In FIG. 1 , 10 denotes a surface-treated steel sheet, 11 denotes a base steel sheet (a steel sheet on which the Zn-Al-Mg-plated layer is to be formed) in the Zn-Al-Mg-plated steel sheet, 12 denotes the Zn-Al-Mg-plated layer of the Zn-Al-Mg-plated steel sheet, and 13 denotes the coating film. The term "main surfaces" used herein refers to two surfaces of the Zn-Al-Mg-plated steel sheet that face each other in the thickness direction of the Zn-Al-Mg-plated steel sheet, and the term "one surface of the Zn-Al-Mg-plated steel sheet" used herein refers to one of a pair of surfaces of the Zn-Al-Mg-plated steel sheet that face each other in the thickness direction of the Zn-Al-Mg-plated steel sheet.

[0013] The surface-treated steel sheet according to this embodiment has the above-described configuration, and is excellent in both corrosion resistance and weldability. The surface-treated steel sheet according to this embodiment was discovered based on the following findings.

[0014] The inventors have studied the corrosion resistance and weldability of surface-treated steel sheets. As a result, they have obtained the following findings. To date, zinc-plated steel sheets, in which zinc is plated on the steel sheet, have been mainly used for surface-treated steel sheets used in applications such as automotive parts to ensure corrosion resistance and weldability. To further improve corrosion resistance while maintaining weldability, painted steel sheets have been studied, in which a coating film containing a binder resin, an anti-rust pigment, and an anti-rust agent is provided on the zinc-plated steel sheet. Meanwhile, at joints (sheet joints) between formed materials of surface-treated steel sheets, there are areas where the chemical conversion coating and the electrodeposition coating film do not extend. This leaves the joints of the formed materials exposed to a corrosive environment in a bare state, which can lead to corrosion progression. Therefore, by using Zn-Al-Mg-plated steel sheets as the zinc-plated steel sheets, the surface-treated steel sheets can exhibit excellent corrosion resistance.

[0015] However, when Zn-Al-Mg-plated steel sheets with excellent corrosion resistance are used, Al and Mg, which are components of the plating, adhere to the welding electrode during welding, deteriorating weldability (particularly the ability to weld continuously in spot welding). Therefore, the plating weight per side of the Zn-Al-Mg-plated steel sheets is set to 20 to 60 g / m 2 By reducing the concentration to 0.1 μm, adhesion of Al and Mg to the welding electrode during welding is suppressed. In addition, doped zinc oxide particles with a large average particle size of 0.1 to 2 μm are used as the rust-preventive pigment contained in the coating film, and the content of the doped zinc oxide particles is increased to 20 to 40 mass %. This makes it easier for the welding electrode to come into contact with the doped zinc oxide particles during welding, and makes it less likely for the welding electrode to come into contact with the Zn-Al-Mg-based plating layer of the Zn-Al-Mg-plated steel sheet. Furthermore, Zn-containing compounds such as doped zinc oxide particles come into contact with the welding electrode during welding, and even if the Zn-containing compounds adhere, welding defects are less likely to occur. This is because, among inorganic substances, Zn-containing compounds adhere to the welding electrode mainly as zinc oxide and have low reactivity with metal components (e.g., Cu) of the welding electrode, so even if they adhere to the welding electrode, they are less likely to interfere with welding. Therefore, the coating film must not contain any inorganic substances other than the Zn-containing compound, or even if it does contain inorganic substances other than the Zn-containing compound, the content of inorganic substances other than the Zn-containing compound must be controlled to 1 mass% or less of the coating film.

[0016] From the above findings, it has been found that the surface-treated steel sheet according to this embodiment is a surface-treated steel sheet that is excellent in both corrosion resistance and weldability.

[0017] Hereinafter, the surface-treated steel sheet according to this embodiment will be described in detail.

[0018] (Zn-Al-Mg-plated steel sheet) The Zn-Al-Mg-plated steel sheet is a steel sheet in which a Zn-Al-Mg-plated layer containing at least Zn, Al, and Mg is formed on a base steel sheet. The Zn-Al-Mg-plated layer containing at least Zn, Al, and Mg contains Zn as a main component (e.g., 40 mass% or more of Zn as the maximum component) and is a plating layer with excellent corrosion resistance. In addition to Zn, Al, and Mg, the Zn-Al-Mg-plated layer may contain elements such as Si, Ni, Ti, Zr, Sr, Fe, Sb, Pb, Sn, Ca, Co, Mn, P, B, Bi, Cr, Sc, Y, REM, Hf, and C. A specific example of the chemical composition of the Zn-Al-Mg-based plating layer is a chemical composition containing, on average, 4 to 22 mass% Al, 1 to 10 mass% Mg, and the balance including Zn and impurities. A more specific example of the chemical composition of the Zn-Al-Mg-based plating layer is a chemical composition containing, on average, 4 to 22 mass% Al, 1 to 10 mass% Mg, and 0.0001 to 2 mass% Si, and the balance including Zn and impurities. In the Zn-Al-Mg-based plating layer, impurities refer to components contained in raw materials or components mixed in during the manufacturing process, but not intentionally added. For example, trace amounts of components other than Fe may be mixed into the Zn-Al-Mg-based plating layer due to mutual atomic diffusion between the base steel sheet and the Zn-Al-Mg-based plating layer.

[0019] Here, the base steel sheet for the Zn-Al-Mg-plated steel sheet (the steel sheet on which the Zn-Al-Mg-plated layer is formed) is not particularly limited. The base steel sheet may be a hot-rolled steel sheet obtained by hot-rolling a slab having an appropriate chemical composition for steel, or a cold-rolled steel sheet obtained by cold-rolling such a hot-rolled steel sheet. The strength of the base steel sheet may be, for example, 270 to 1470 MPa in tensile strength class. The thickness of the base steel sheet is not particularly limited, but is preferably 0.4 to 3.2 mm, and more preferably 0.5 to 2.4 mm. The thickness of the Zn-Al-Mg-plated steel sheet is measured using a microgauge (CPM-MX, manufactured by Mitutoyo Corporation).

[0020] Zn-Al-Mg coated steel sheet with a coating weight of 20 to 60 g / m per side2 If the coating weight is too low, the corrosion resistance will decrease. On the other hand, if the coating weight is too high, Al and Mg will easily adhere to the welding electrode during welding, resulting in a decrease in weldability. Therefore, the coating weight is set to the above range. The coating weight is 25 to 50 g / m 2 is preferred, and 30 to 40 g / m 2 is more preferable. Here, the coating weight is measured as follows. The coating weight of the coating layer can be measured by dissolving the coating layer in an acid solution to which an inhibitor that suppresses corrosion of the base steel sheet has been added (pickling), and measuring the change in weight before and after pickling. If a coating film is present, it can be measured by removing the coating film with a chemical (remover, etc.) or resin shot before performing the above-mentioned pickling.

[0021] The method for forming the Zn—Al—Mg-based coating layer of the Zn—Al—Mg-based coated steel sheet is not particularly limited. For example, the Zn—Al—Mg-based coating layer can be formed by hot-dip galvanization or the like. The Zn—Al—Mg-based coating layer can be formed by either a continuous process or a batch process. Furthermore, after the Zn—Al—Mg-based coating layer is formed, it may be subjected to treatments such as zero spangle treatment for uniform appearance, annealing treatment for modifying the Zn—Al—Mg-based coating layer, and temper rolling for adjusting the surface condition or material properties.

[0022] (Coating Film) The coating film contains a binder resin, doped zinc oxide particles, and a rust inhibitor. If necessary, the coating film may contain other components.

[0023] - Binder Resin - The binder resin may be either a water-soluble or water-dispersible aqueous resin that dissolves or disperses in water, or a solvent-based resin that dissolves or disperses in an organic solvent. However, from the viewpoints of production cost and environmental friendliness, an aqueous resin is preferred.

[0024] Examples of aqueous resins include water-soluble or water-dispersible resins such as polyester resin, urethane resin, polyolefin resin, acrylic resin, epoxy resin, phenolic resin, and a mixture of two or more of these resins. When using polyester resin, the molecular weight is preferably 10,000 to 30,000. A molecular weight of 10,000 or more ensures sufficient processability. On the other hand, a molecular weight of 30,000 or less increases the number of bonding sites in the resin itself, ensuring excellent adhesion to the electrodeposition coating film. Furthermore, when crosslinking is performed using a curing agent such as melamine, the crosslinking reaction is sufficiently carried out, ensuring the performance of the coating film. Here, the molecular weight of the polyester resin is the weight-average molecular weight. When using urethane resin, the urethane resin is preferably in the form of an emulsion with an emulsion particle size of 10 to 100 nm (preferably 20 to 60 nm). An emulsion particle size of 10 nm or more reduces costs. On the other hand, an emulsion particle size of 100 nm or less minimizes the gaps between emulsion particles when formed into a coating film, ensuring the barrier properties of the coating film. The types of urethane resin include ether-based, polycarbonate-based, ester-based, acrylic graphite-based, etc. These may be used alone or in combination.

[0025] Examples of solvent-based resins include polyester resins, urethane resins, epoxy resins, acrylic resins, and mixed resins of two or more of these resins.

[0026] Here, the binder resin may be a crosslinked resin having a crosslinked structure or a non-crosslinked resin not having a crosslinked structure, but a non-crosslinked resin is preferable from the viewpoint of low-temperature film formation of the coating film. As a crosslinking agent (curing agent) that imparts a crosslinked structure to the binder resin, a water-soluble crosslinking agent is preferable. Specific examples of the crosslinking agent include melamine, isocyanate, silane compounds, zirconium compounds, and titanium compounds.

[0027] The amount of crosslinking agent added is preferably 5 to 30 parts by mass per 100 parts by mass of resin solids. When the amount of crosslinking agent added is 5 parts by mass or more, the crosslinking reaction with the binder resin is ensured, resulting in sufficient performance as a coating film. On the other hand, when the amount of crosslinking agent added is 30 parts by mass or less, the crosslinking reaction proceeds moderately, preventing the coating film from becoming excessively hard. This ensures processability. In addition, the paint stability of silane compounds, zirconium compounds, and titanium compounds can be ensured.

[0028] The binder resin content is preferably 10.0 to 90.0% by mass relative to the coating film (total solids content of the coating film). When the binder resin content is 10.0% by mass or more, the binder function is easily exhibited and the cohesive strength of the coating film is improved. As a result, internal failure of the coating film (cohesive failure of the coating film) is less likely to occur during adhesion tests and molding processes. On the other hand, when the binder resin content is 90.0% by mass or less, the proportion of pigment components contained in the coating film is reduced, making it easier to achieve both weldability, corrosion resistance, and adhesion to the electrodeposition coating film. The binder resin content is more preferably 15.0 to 80.0% by mass relative to the coating film (total solids content of the coating film) in order to exhibit the binder function and achieve both weldability, corrosion resistance, and adhesion to the electrodeposition coating film.

[0029] - Doped zinc oxide particles - Doped zinc oxide particles are conductive zinc oxide particles. When the coating film contains conductive doped zinc oxide particles, the weldability is improved.

[0030] Examples of doped zinc oxide particles include zinc oxide particles that have been doped with at least one element selected from the group consisting of elements in Group 13 of the periodic table and elements in Group 15 of the periodic table (hereinafter also referred to as "dope element") to exhibit electrical conductivity.

[0031] Examples of Group 13 elements of the periodic table include B, Al, Ga, and In. Examples of Group 15 elements of the periodic table include P and As. Among these, from the viewpoint of improving electrical conductivity, the doping element is preferably Al or Ga. Furthermore, from the viewpoint of cost, the doping element is more preferably Al.

[0032] From the viewpoint of improving electrical conductivity, the content of the doping element is preferably 0.05 to 5 atom %, more preferably 0.1 to 5 atom %, based on the undoped zinc oxide particles.

[0033] The doped zinc oxide particles have an average particle size of 0.1 to 2 μm. If the average particle size is too small, the welding electrode will likely come into contact with the Zn—Al—Mg-based plating layer of the Zn—Al—Mg-plated steel sheet during welding, resulting in reduced weldability. On the other hand, if the average particle size is too large, the doped zinc oxide particles will be less likely to come into uniform contact with the welding electrode (e.g., a Cu electrode) during welding, resulting in the welding electrode likely coming into contact with the Zn—Al—Mg-based plating layer of the Zn—Al—Mg-plated steel sheet and reduced weldability. Therefore, the average particle size of the doped zinc oxide particles is set to the above range. The average particle size of the doped zinc oxide particles is preferably 0.2 to 1.5 μm, and more preferably 0.4 to 1.0 μm.

[0034] The "average particle size" of the doped zinc oxide particles refers to the average primary particle size when the doped zinc oxide particles are present alone in the coating film, and refers to the average secondary particle size representing the particle size of the oxide particles in the aggregated state when the doped zinc oxide particles are present in the coating film.

[0035] The average particle size of doped zinc oxide particles is determined by the following measurement method. First, a surface-treated substrate on which a coating film has been formed is cut along the thickness direction to expose the cross section. After embedding with resin, the exposed cross section is polished using a polishing machine. After polishing, Au is vapor-deposited on the cross section to prepare a sample for cross-sectional observation. The cross section thus obtained is observed using a scanning electron microscope to obtain an observation image of the cross section in the coating film. 25 doped zinc oxide particles present in the field of view of the observation image are randomly selected, and the long and short side lengths of each doped zinc oxide particle are measured. Finally, the average long side length and the arithmetic mean of the short side length are calculated, and the average particle size is calculated by arithmetically averaging the arithmetic mean long side length and the arithmetic mean of the arithmetic mean short side length. Note that doped zinc oxide particles present in the field of view of the observation image were identified as particles located in a region where Al was detected within a region where Zn was detected in EPMA analysis of the field of view. The observation conditions for the scanning electron microscope are as follows: Measurement device: JSM-7200F manufactured by JEOL Ltd. Magnification: 5000 times Acceleration voltage: 10 keV Image analysis software: Image J Ver. 1.54f

[0036] The content of the doped zinc oxide particles is 20 to 40 mass% of the coating film (total solid content of the coating film). If the content of the doped zinc oxide particles is low, the welding electrode is more likely to come into contact with the Zn-Al-Mg-based plating layer of the Zn-Al-Mg-plated steel sheet during welding, resulting in reduced weldability. On the other hand, if the content of the doped zinc oxide particles is high, the proportion of conductive pigment in the coating film decreases, resulting in insufficient performance such as weldability and corrosion resistance. Therefore, the content of the doped zinc oxide particles is set to the above range. The content of the doped zinc oxide particles is preferably 25 to 35 mass%, more preferably 27 to 33 mass%.

[0037] -Rust Inhibitor- As the rust inhibitor, organic rust inhibitors such as organic acids, organic acid salts, amine salts, and esters are used to impart high weldability. When used as an organic rust inhibitor, they burn and carbonize due to the heat of welding, making them less likely to adhere to the welding electrode. Among these, organic acids are preferred because they can impart high corrosion resistance. Examples of organic acids include carboxylic acids (tartaric acid, tannic acid, oleic acid, dimer acid, naphthalene acid, etc.). Examples of organic acid salts include carboxylic acid metal soaps (lanolin calcium, naphthenate zinc, oxidized wax calcium, barium salts, etc.), sulfonates (sodium sulfonate, calcium sulfonate, barium sulfonate), etc. Examples of esters include glycerin esters of higher fatty acids, sorbitan monoisostearate, and sorbitan norate. The content of the rust inhibitor is preferably 1 to 20% by mass based on the coating film (total solids content of the coating film). When the content of the rust inhibitor is 1% by mass or more, corrosion resistance is sufficiently improved. On the other hand, when the content of the rust inhibitor is 20% by mass or less, a decrease in the liquid stability of the paint is suppressed. From the viewpoints of corrosion resistance and paint stability, the content of the rust inhibitor is more preferably 1 to 3% by mass based on the coating film (total solids content of the coating film).

[0038] (Other Components) Examples of other components include well-known additives such as lubricants, silane coupling agents, and leveling agents. However, if inorganic substances other than the Zn-containing compound adhere to the welding electrode during welding, they will reduce weldability. Therefore, the content of inorganic substances other than the Zn-containing compound in the coating film is set to 0 to 1 mass% or less relative to the coating film. In other words, the coating film does not contain any inorganic substances other than the Zn-containing compound, or if it does contain any inorganic substances other than the Zn-containing compound, the content of inorganic substances other than the Zn-containing compound is controlled to 1 mass% or less relative to the coating film. Here, the Zn-containing compound includes the doped zinc oxide particles described above. Examples of Zn-containing compounds containing doped zinc oxide particles include Al-doped zinc oxide, Sn-doped zinc oxide, zinc oxide, zinc hydroxide, and inorganic zinc salts. Examples of inorganic zinc include zinc sulfate, zinc nitrate, and zinc phosphide. Note that the inorganic substances other than the Zn-containing compound containing the doped zinc oxide particles do not include metal salts of organic substances (such as metal salts of organic acids).

[0039] The solid lubricant can impart excellent lubricity to the coating film and improve the powdering resistance of the coating film. Examples of the solid lubricant include the solid lubricants (1) and (2) below.

[0040] (1) Polyolefin wax, paraffin wax: for example, polyethylene wax, synthetic paraffin, natural paraffin, microwax, chlorinated hydrocarbon, etc. (2) Fluorine resin wax: for example, polyfluoroethylene resin (polytetrafluoroethylene resin, etc.), polyvinyl fluoride resin, polyvinylidene fluoride resin, etc.

[0041] When polyethylene wax is used as the solid lubricant, the average particle size is preferably 0.5 to 10 μm. When the average particle size of the polyethylene wax is 0.5 μm or more, surface thickening of the polyethylene wax is suppressed, and a decrease in adhesion between the coating film and the electrodeposition coating film can be suppressed. On the other hand, when the average particle size of the solid lubricant is 10 μm or less, peeling of the polyethylene wax from the coating film is suppressed, and lubricity and corrosion resistance can be ensured. The average particle size of the solid lubricant is more preferably 1 to 5 μm in order to obtain excellent adhesion between the coating film and the electrodeposition coating film, corrosion resistance, lubricity, and powdering resistance.

[0042] The softening point of the solid lubricant is preferably 100° C. to 135° C., more preferably 110 to 130° C. When the softening point of the solid lubricant is 100° C. to 135° C., the lubricity and powdering resistance of the coating film are further improved.

[0043] The content of the solid lubricant is preferably 0.1 to 10 mass% relative to the coating film (total solid content of the coating film). When the content of the solid lubricant is 0.1 mass% or more, sufficient lubricity is obtained. On the other hand, when the content of the solid lubricant is 10 mass% or less, a decrease in adhesion between the coating film and the electrodeposition coating film and in corrosion resistance can be suppressed. From the viewpoints of adhesion between the coating film and the electrodeposition coating film, lubricity, and corrosion resistance, the content of the solid lubricant is more preferably 0.5 to 5 mass%, and even more preferably 0.5 to 2.5 mass% relative to the coating film (total solid content of the coating film).

[0044] (Average Film Thickness of Coating Film) The average film thickness of the coating film is 0.5 to 3 μm. If the average film thickness of the coating film is too thin, sufficient corrosion resistance cannot be obtained. In addition, sufficient adhesion between the coating film and the electrodeposition coating film cannot be obtained. On the other hand, if the average film thickness of the coating film is too thick, the cohesive force of the coating film decreases, and sufficient weldability cannot be obtained. Therefore, the average film thickness of the coating film is set to the above range. The average film thickness of the coating film is preferably 0.8 to 2.2 μm, and more preferably 1.2 to 1.8 μm.

[0045] The average film thickness of the coating film is measured as follows. First, a surface-treated substrate having a coating film is cut along the thickness direction to expose the cross section, and after embedding with resin, the exposed cross section is polished using a polishing machine. After polishing, Au is vapor-deposited on the cross section to prepare a sample for cross-sectional observation. The cross section thus obtained is observed with a scanning electron microscope to obtain an observation image of the cross section in the coating film. In the observation image, the film thickness of the coating film is measured at 10 points, spaced 40 μm apart, in the direction in which the coating film extends on the observation image. Here, the observation conditions for the scanning electron microscope are as follows: Measuring device: JSM-7200F manufactured by JEOL Ltd. Magnification: 3000x Acceleration voltage: 10 keV

[0046] (Coating Film Formation) The method for forming the coating film is not particularly limited, and well-known methods can be used. For example, a coating film-forming composition (paint) is obtained by mixing a binder resin, doped zinc oxide particles, a rust inhibitor, and, if necessary, other components in a solvent. The solvent may be water or an organic solvent, but water is preferred from the standpoints of production cost and environmental friendliness. In other words, the coating film-forming composition is preferably an aqueous composition. The coating film is formed by applying the coating film-forming composition to at least one surface of a Zn—Al—Mg-plated steel sheet and drying, or by drying and heating. Note that the surface of the Zn—Al—Mg-plated steel sheet is preferably degreased and washed with water before applying the coating film-forming composition. Here, the coating film-forming composition can be applied using a coating method such as bar coating, roll coating, blade coating, or curtain coating. The drying temperature of the coating film, in terms of the maximum temperature reached on the surface of the Zn—Al—Mg-plated steel sheet, is preferably 50 to 120° C., more preferably 60 to 100° C. The heating temperature of the coating film, in terms of the maximum temperature reached on the surface of the Zn—Al—Mg-plated steel sheet, is preferably 100 to 240° C., more preferably 120 to 210° C.

[0047] <Other Aspects of the Surface-Treated Steel Sheet> The surface-treated steel sheet according to this embodiment may have an intermediate coating film (a functional coating film such as a chemical conversion coating film) between the Zn-Al-Mg-plated steel sheet and the coating film. The intermediate coating film preferably contains a binder resin, a silane coupling agent, silica fine particles, a phosphate compound, and a fluorine compound and has an average film thickness of 0.1 to 0.5 μm. Having an intermediate coating film with the above composition and average film thickness makes it possible to improve corrosion resistance without compromising weldability. This is because a relatively thin intermediate coating film has little effect on weldability and improves adhesion between the plated steel sheet and the coating film, thereby improving corrosion resistance. Therefore, the surface-treated steel sheet according to this embodiment preferably has an intermediate coating film (functional coating film) with the above composition and average film thickness between the Zn-Al-Mg-plated steel sheet and the coating film.

[0048] The average thickness of the intermediate coating is measured in the same manner as the average thickness of the coating.

[0049] <Coated Member> The coated member according to this embodiment includes a formed material obtained by forming the surface-treated steel sheet according to this embodiment and an electrodeposition coating film formed on the formed material (i.e., the coating film of the surface-treated steel sheet) (see FIG. 2). In FIG. 2, 100 denotes the coated member, 10A denotes the formed material, 11A denotes the base steel sheet in the formed material (the steel sheet on which the Zn—Al—Mg-based plating layer is to be formed), 12A denotes the Zn—Al—Mg-based plating layer of the formed material, 13A denotes the coating film of the formed material, and 14 denotes the electrodeposition coating film. While FIG. 2 shows an example of a coated member having a hat-shaped cross section, the overall shape and cross-sectional shape of the coated member are not particularly limited and may have any shape.

[0050] The coated member according to this embodiment is manufactured, for example, as follows: First, a surface-treated steel sheet is formed into a formed product having a desired shape using, for example, well-known forming techniques such as cutting and press forming. If necessary, the formed product may be assembled into a desired shape by welding (such as spot welding).

[0051] Next, the coating film of the molding material is subjected to an electrodeposition coating treatment. As a result, an electrodeposition coating film is formed on the coating film. The electrodeposition coating treatment may be either anionic electrodeposition coating or cationic electrodeposition coating, but cationic electrodeposition coating is preferred from the viewpoint of corrosion resistance.

[0052] In particular, when an electrodeposition coating film is formed by cationic electrodeposition coating using an aqueous paint containing a resin [for example, an aqueous resin (such as an acrylic resin, polyester resin, alkyd resin, epoxy resin, or polyurethane resin) having a hydrophilic group such as a carboxyl group, a hydroxyl group, a methylol group, an amino group, a sulfonic acid group, or a polyoxyethylene bond, and a functional group such as a hydroxyl group that reacts with a curing agent], a curing agent (such as a melamine resin or a blocked polyisocyanate), and other additives (such as a coloring pigment, a light interference pigment, an extender pigment, a dispersant, an anti-settling agent, a reaction accelerator, an antifoaming agent, a thickener, an anti-corrosion agent, an ultraviolet absorber, or a surface conditioner), the adhesion between the coating film and the electrodeposition coating film is likely to be improved.

[0053] Thereafter, other coating films such as an intermediate coating film and a top coating film may be formed on the electrodeposition coating film of the molding material, if necessary.

[0054] Through these steps, the coated member according to this embodiment is manufactured.

[0055] Before electrodeposition coating, the molded material on which the coating film has been formed may be degreased, the surface adjusted, and then chemically treated (for example, phosphate treatment, Zr treatment, etc.). By performing chemical conversion treatment, it is difficult for a chemical conversion treatment film to form on the coating film, but a chemical conversion treatment film is formed in required areas other than the coating film. Therefore, the adhesion of the electrodeposition coating film to the entire molded material (coated member) can be improved.

[0056] The coated member according to this embodiment is widely used in applications such as automobile members (automobile bodies, undercarriage members, etc.), machine members (casings, etc.), home appliance members (casings, etc.), and building materials (roofs, walls, etc.).

[0057] The present disclosure will be further described below with reference to examples, but the present disclosure is not limited to the following examples. The present disclosure allows various conditions to be adopted as long as they do not deviate from the gist of the disclosure and the object of the disclosure is achieved.

[0058] Examples 1. Production of Surface-Treated Steel Sheets 1.1 Preparation of Zinc-Based Plated Steel Sheets The following five types of zinc-based plated steel sheets were prepared and immersed in an aqueous solution (2.5 mass %, 40°C) of an aqueous alkaline degreasing agent (FC-301 manufactured by Nippon Parkerizing Co., Ltd.) for 2 minutes to degrease the surface, followed by rinsing with water and drying to obtain zinc-based plated steel sheets for surface treatment. However, cold-rolled steel sheets were also prepared as steel sheets for surface treatment.

[0059] ZA: Zn-Al-Mg ternary hot-dip galvanized steel sheet (Zn-11%Al-3%Mg-0.2%Si) (sheet thickness 0.8mm) ZB: Zn-Al-Mg ternary hot-dip galvanized steel sheet (Zn-2%Al-2%Mg) (sheet thickness 0.8mm) ZC: Hot-dip galvanized steel sheet (sheet thickness 0.8mm) ZD: Galvannealed hot-dip galvanized steel sheet (sheet thickness 0.8mm, 10% Fe by mass) C: Cold-rolled steel sheet (sheet thickness 0.8mm, uncoated)

[0060] The coating weights of the plating are shown in Table 2. The coating weights were controlled by adjusting the plating pull-up speed and wiping amount during plating preparation.

[0061] 1.2 Formation of intermediate coating film (chemical conversion coating) Next, the following chemical conversion treatment solution S was prepared and applied to the above-mentioned zinc-based plated steel sheet or cold-rolled steel sheet while changing the bar coat count so as to obtain the average film thickness of the intermediate coating film shown in Table 2. Thereafter, the zinc-based plated steel sheet or cold-rolled steel sheet was heated and dried in a hot air furnace so that the temperature reached on the surface of the zinc-based plated steel sheet or cold-rolled steel sheet was 70°C, and then air-dried, thereby forming an intermediate coating film on the surface of the zinc-based plated steel sheet or cold-rolled steel sheet. However, in some examples, the formation of the intermediate coating film was not carried out.

[0062] S1: A chemical conversion treatment solution having a solids concentration of 10% and consisting of a silane coupling agent, silica fine particles, a urethane resin, a phosphate compound, and a fluorine compound. S2: A chemical conversion treatment solution having a solids concentration of 10% and consisting of a Zr compound, a silane coupling agent, a phosphate compound, and a vanadium compound.

[0063] 1.3 Formation of Coating Film Next, in order to form a coating film having the composition ratio (mass %) shown in Table 1, the components were mixed to a solids concentration of 20 mass % to prepare a paint for forming a coating film. The paint was applied to a zinc-based plated steel sheet or cold-rolled steel sheet or a chemical conversion coating using a bar coater, while changing the bar coat count and dilution ratio so as to obtain the average film thickness shown in Table 2, and then dried in an oven under conditions resulting in the maximum temperature reached (PMT) shown in Table 2, or by drying and heating, to form a coating film. The components contained in the paint are shown below.

[0064] (Binder resins, etc.) J1: Epoxy resin (ADEKA ADEKA RESIN EM-0461N) J2: Polyester resin (Vylon MD1480) J3: Urethane resin (Dai-ichi Kogyo Seiyaku Co., Ltd. Superflex 150) J4: Epoxy resin (ADEKA ADEKA RESIN EP-4100) J5: Polyester resin (Vylon 200) J6: Melamine resin (Allnex Cymel 325) J7: Water-soluble isocyanate (Dai-ichi Kogyo Seiyaku Co., Ltd. Elastron BN-77)

[0065] (Doped zinc oxide particles) Z1: Doped zinc oxide particles (23-Kt manufactured by Hakusui Tech Co., Ltd., average particle size 0.5 μm) Z2: Doped zinc oxide particles (23-K manufactured by Hakusui Tech Co., Ltd., average particle size 0.2 μm) Z3: Doped zinc oxide particles (Pazet CK manufactured by Hakusui Tech Co., Ltd., average particle size 0.03 μm) Z4: Zinc oxide particles (general reagent, average particle size 0.5 μm) Z5: Titanium nitride particles (general reagent, average particle size 2.0 μm)

[0066] (Rust inhibitors) B1: A mixture of tannic acid (general reagent) and zinc naphthenate (general reagent) in a 1:1 mass ratio. B2: A mixture of tartaric acid (general reagent) and zinc naphthenate (general reagent) in a 1:1 mass ratio. B3: A mixture of tannic acid (general reagent) and trizinc phosphate (general reagent) in a 1:1 mass ratio. B4: A mixture of tartaric acid (general reagent) and trizinc phosphate (general reagent) in a 1:1 mass ratio. B5: Colloidal silica (particle size 20 nm) B6: Aluminum dihydrogen tripolyphosphate (particle size 2 μm) B7: Calcium ion-exchanged silica (Ca exchange rate 9%) (particle size 2 μm) B8: Silica (particle size 2 μm)

[0067] (Solid lubricant) W1: Polyethylene wax (S-394 MG manufactured by CHEMBASE) W2: Polytetrafluoroethylene (PTFE) particles (SST-1MG-RC manufactured by CHEMBASE)

[0068] 2. Performance Evaluation Tests The surface-treated steel sheets of each example were subjected to the following performance evaluation tests.

[0069] 2.1 Corrosion Resistance Test (Preparation 1) Test specimen A was cut to a size of 70 mm × 150 mm, and test specimen B was cut to a size of 50 mm × 100 mm. Next, as shown in Figures 3 and 4 , test specimen A and test specimen B were overlapped with each other so that their centers overlapped and their longitudinal directions were parallel in a plan view. Then, test specimen A and test specimen B were spot-welded at their respective centers to prepare a joined test specimen C. The spot welding was performed at a single location in the center of test specimen A and test specimen B. The spot welding conditions were as follows: electrode used: R40 CF-type Cr—Cu electrode with a tip diameter of 5 mm; welding pressure: 1.96 kN; welding current: 8 kA; and welding time: 12 cycles / 50 Hz. In addition, during spot welding, a 0.1 mm gauge was sandwiched between test piece A and test piece B, and spot welding was performed to provide a gap (clearance) between test piece A and test piece B.

[0070] (Preparation 2) The bonded test specimens C prepared from the surface-treated steel sheets of each example were subjected to surface conditioning at room temperature for 20 seconds using a surface conditioning treatment agent, Preparen X (trade name), manufactured by Nihon Parkerizing Co., Ltd. Furthermore, a chemical conversion treatment (phosphate treatment) was performed using a chemical conversion treatment solution (zinc phosphate treatment solution), "Palbond 3020 (trade name)" manufactured by Nihon Parkerizing Co., Ltd. The temperature of the chemical conversion treatment solution was set to 43°C, and the bonded test specimens C were immersed in the chemical conversion treatment solution for 120 seconds, then rinsed with water and dried. After the chemical conversion treatment (phosphate treatment), the bonded test specimens C were electrodeposited with a cationic electrodeposition paint manufactured by Nippon Paint Co., Ltd. using a ramp current of 160V, and further baked at a baking temperature of 170°C for 20 minutes. The average thickness of the electrodeposition coating film was 10 μm for all bonded test specimens C.

[0071] (Corrosion Resistance Test of Laminated Plates) After the electrodeposition coating, the end face of test piece A of the bonded test piece C was sealed, and a corrosion cycle test was performed on the bonded test piece C in a state where salt water was sprayed on the side of test piece B of the bonded test piece C. The corrosion cycle consisted of 2 hours of salt spray (SST: Salt Spray Test, 5% NaCl, 35°C atmosphere) for 2 hours, 2 hours of dry (60°C) for 2 hours, and 4 hours of wet (50°C, 98% RH) for 360 cycles. The corrosion cycle test was performed in accordance with JASO M609-91. After the corrosion test, the spot weld of the bonded test piece C was drilled out with a drill or the like, and test piece A and test piece B were separated. The corrosion condition of the overlapping surface of test piece A with test piece B was observed and assigned the following rating. Furthermore, test piece A was immersed in an ammonium citrate aqueous solution to remove corrosion products, and the corrosion depth of test piece A was measured. Specifically, after removing the corrosion products, test piece A was cut into eight equal parts (in FIG. 3, two parts were cut horizontally and four parts were cut vertically, for a total of eight equal parts), and the corrosion depth (mm) of each small piece was measured. The largest corrosion depth (mm) of the eight small pieces was taken as the maximum corrosion depth (mm) and evaluated as the result of the corrosion resistance test of the plate joint of the example. In the corrosion resistance test, a rating of "3", "4", or "5" was determined to be excellent in corrosion resistance. The results are shown in Table 2. The corrosion depth was measured using a micrometer (CPM-MX, manufactured by Mitutoyo Corporation). 1: Red rust occurs on the entire mating surface of test piece A with test piece B, or the maximum corrosion depth is 0.4 mm or more. 2: Red rust occurs on 20% or more of the mating surface of test piece A with test piece B, or the maximum corrosion depth is 0.2 mm or more and less than 0.4 mm. 3: Red rust occurs on 5% or more and less than 20% of the mating surface of test piece A with test piece B, or the maximum corrosion depth is 0.1 mm or more and less than 0.2 mm. 4: Red rust occurs on less than 5% of the mating surface of test piece A with test piece B, or the maximum corrosion depth is more than 0 mm and less than 0.1 mm. 5: No red rust occurs on the mating surface of test piece A with test piece B, and the maximum corrosion depth is 0 mm (none).

[0072] 2.2 Spot Weldability Five hundred spot welds were performed on each surface-treated steel sheet using a 5 mm tip diameter, R40 CF-type Cr-Cu electrode. The welding current was varied to achieve a nugget diameter of 4√t (t = thickness of the surface-treated steel sheet) at a pressure of 1.96 kN and a welding time of 12 cycles / 50 Hz. The nugget diameter and electrode condition after 500 welds were observed and assigned the following rating. Spot welds where no current was applied were judged as having no nugget. The presence or absence of nugget formation and nugget diameter were measured by observing the cross section of the sheet thickness including the center of the weld. A rating of "3," "4," or "5" in this weldability test was considered to have excellent weldability. The results are shown in Table 2. 1: 500 dots cannot be performed. 2: 500 dots can be performed, but there is no current flow at 10 dots (including no current flow), and the diameter of the electrode contact surface when using pressure-sensitive paper at the end of 500 dots is 1.7 times or more the diameter of the electrode contact surface at the first dot. 3: 500 dots are performed, no current flow, and the diameter of the electrode contact surface when using pressure-sensitive paper at the end of 500 dots is 1.4 times or more but less than 1.7 times the diameter of the electrode contact surface at the first dot. 4: 500 dots are performed, no current flow, and the diameter of the electrode contact surface when using pressure-sensitive paper at the end of 500 dots is 1.1 times or more but less than 1.4 times the diameter of the electrode contact surface at the first dot. 5: 500 dots are performed, no current flow, no electrode wear, or the diameter of the electrode contact surface when using pressure-sensitive paper at the end of 500 dots is less than 1.1 times the diameter of the electrode contact surface at the first dot. 3 and 4, 20A indicates test piece A, 20B indicates test piece B, 20C indicates joined test piece C, and 22 indicates a spot welded portion.

[0073]

[0074]

[0075]

[0076] From the above results, it can be seen that the surface-treated steel sheets of the present invention have superior corrosion resistance and weldability compared to the surface-treated steel sheets of the comparative examples. In Table 1, the notation "inorganic substance *1" indicates the composition ratio of "inorganic substances other than Zn-containing compounds including doped zinc oxide particles" to the coating film.

[0077] The disclosure of Japanese Patent Application No. 2023-056126 is incorporated herein by reference in its entirety. All documents, patent applications, and technical standards described herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard was specifically and individually indicated to be incorporated by reference.

Claims

1. Plating weight per side is 20-60g / m 2 and a coating film disposed on at least one main surface of the Zn-Al-Mg-plated steel sheet, wherein the coating film contains a binder resin, doped zinc oxide particles, and a rust inhibitor, the coating film has an average thickness of 0.5 to 3 μm, the doped zinc oxide particles have an average particle size of 0.1 to 2 μm, the doped zinc oxide particles are contained in an amount of 20 to 40 mass % relative to the coating film, and a content of inorganic substances other than a Zn-containing compound in the coating film is 0 to 1 mass % relative to the coating film.

2. The surface-treated steel sheet according to claim 1, wherein the rust inhibitor is an organic acid, and the content of the rust inhibitor is 1 to 20 mass % relative to the coating film.

3. The surface-treated steel sheet according to claim 1, further comprising an intermediate coating film between the Zn-Al-Mg-plated steel sheet and the coating film, the intermediate coating film containing a binder resin, a silane coupling agent, silica fine particles, a phosphate compound, and a fluorine compound, and the intermediate coating film has an average thickness of 0.1 to 0.5 μm.

4. The surface-treated steel sheet according to claim 1, wherein the chemical composition of the Zn-Al-Mg-based plating layer of the Zn-Al-Mg-plated steel sheet contains, on average, 4-22 mass% Al, 1.0-10 mass% Mg, with the balance being Zn and impurities.

Citation Information

Patent Citations

  • Airless tire and method for manufacturing the same

    JP2023056126A

  • Surface-treated steel sheet and coated member

    WO2018092244A1

  • MOLTEN Zn-Al-Mg GROUP PLATED SHEET STEEL, AND MOLTEN Zn-Al-Mg GROUP PLATED SHEET STEEL MANUFACTURING METHOD

    JP2018090885A

  • Coated metal plate for wall material, and wall material using the same

    JP2019105098A

  • Precoated steel sheet

    WO2020100286A1

Cited By

  • Surface-treated metal sheet and automotive component having the same

    JP7953253B2

  • Surface-treated metal sheet and automotive component having the same

    JPWO2026127066A1

  • Surface-treated metal sheet and automotive member comprising same

    WO2026127066A1