Corrosion-resistant aerial cable

By using materials such as modified polyethylene and nano-zinc oxide in the sheath layer of overhead cables, the problem of insufficient corrosion resistance and antibacterial properties of cables in harsh environments is solved, and higher resistance to oxidation and aging is achieved. flammability, improving the overall performance of the cable.

CN118852811AInactive Publication Date: 2024-10-29天津市华夏电缆有限公司

Patent Information

Application Number
CN202411327911.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-10-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing overhead cables have problems with insufficient corrosion resistance, flame retardancy, aging resistance and antibacterial properties under harsh climatic conditions. Especially in areas with abundant rain and long sun exposure, their mechanical properties and waterproofing need to be improved.

Method used

Using a sheath layer composed of polyvinyl chloride resin, modified polyethylene, modified fillers, heat stabilizers, lubricants and ultraviolet absorbers, the modified polyethylene is prepared through efficient stirring and melt grafting technology, and is added to the sheath Nano-zinc oxide and benzothiazolinone structures are added to the layer to enhance the corrosion resistance and antibacterial properties of the cable.

Benefits of technology

It significantly improves the oxidative aging resistance, flame retardancy, mechanical properties and antibacterial properties of the cable, meets the corrosion resistance requirements of the cable in harsh environments, and improves its stability in high temperatures and water.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a corrosion-resistant aerial cable, and relates to the technical field of cables, the corrosion-resistant aerial cable comprises a conductor, an insulating layer and a sheath layer from inside to outside, and the sheath layer comprises the following raw materials in parts by weight: 90-110 parts of polyvinyl chloride resin, 10-15 parts of modified polyethylene, 8-10 parts of a modified filler, 2-4 parts of a heat stabilizer, 0.2-0.4 part of a lubricant, 3-5 parts of a plasticizer and 0.6-0.8 part of an ultraviolet light absorber. And the modified polyethylene has good corrosion resistance and meets the corrosion resistance requirement of the cable. The synthesized modified polyethylene contains a potassium sulfonate group and phenothiazine structure, so that the oxidation aging resistance and flame retardance of the cable are improved. The synthesized modified filler comprises nano zinc oxide, a benzothiazolinone structure and a dehydroabietic acid structure, so that the mechanical property, the antibacterial property and the waterproof property of the cable are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cables, and in particular to a corrosion-resistant overhead cable. Background Art

[0002] Overhead cables are overhead conductors equipped with an insulating layer and a protective sheath. They are a new high-voltage power transmission method between overhead conductors and underground cables. According to their structure, they can be divided into hard aluminum wire structure, hard-drawn copper wire structure, aluminum alloy wire structure, steel core or aluminum alloy core support structure and self-supporting three-core composite structure. They have the main characteristics of high power supply reliability, good power supply safety, easy installation and maintenance, and reasonable economy.

[0003] Patent application number 202310124413.X discloses an overhead cable with a corrosion-resistant outer shell and a preparation method thereof. With polyvinyl chloride resin as the matrix, low-density polyethylene, modified particles, etc. are added to obtain an overhead cable with excellent anti-aging and corrosion resistance, but there are still some shortcomings: (1) The low-density polyethylene molecular chain has a small polarity, and its compatibility and dispersion with the polyvinyl chloride resin matrix with a large molecular chain polarity is poor; (2) Polyvinyl chloride has certain flame retardant properties, but does not meet the current requirements for halogen-free flame retardant properties of cables, and polyethylene has poor flame retardant properties. In some areas with harsh climates such as excessive rainfall and long sunshine time, higher requirements are also put forward for the mechanical properties, waterproofness, anti-aging and antibacterial properties of overhead cables to resist external forces. Therefore, a suitable modification method is needed to solve the problems encountered by current overhead cables during use. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a corrosion-resistant overhead cable.

[0005] The purpose of the present invention can be achieved through the following technical solutions: A corrosion-resistant overhead cable comprises, from the inside to the outside, a conductor, an insulating layer and a sheath layer, wherein the conductor is located in the innermost layer, the insulating layer is coated on the outer periphery of the conductor, and the sheath layer is coated on the outer periphery of the insulating layer; The conductor is made of a plurality of aluminum alloy wires twisted together; the insulating layer is made of nylon insulating material; The sheath layer comprises the following raw materials in parts by weight: 90-110 parts of polyvinyl chloride resin, 10-15 parts of modified polyethylene, 8-10 parts of modified filler, 2-4 parts of heat stabilizer, 0.2-0.4 parts of lubricant, 3-5 parts of plasticizer and 0.6-0.8 parts of ultraviolet absorber; the heat stabilizer is a mixture of calcium stearate and zinc stearate in a mass ratio of 1:1, the lubricant is stearic acid, the plasticizer is epoxy soybean oil, and the ultraviolet absorber is 2-(2'-hydroxy-5'-methylphenyl)benzotriazole; The preparation of the corrosion-resistant overhead cable comprises the following steps: Step S1: adding polyvinyl chloride resin and modified polyethylene into a mixer, stirring at a high speed of 900-1000 r / min, adding modified filler, heat stabilizer, lubricant, plasticizer and ultraviolet absorber while stirring, stirring for 30-40 minutes, reducing the speed to 600-700 r / min, stirring and heating to 120° C., and discharging after 3 minutes to obtain a sheath layer material; Step S2: twisting a plurality of aluminum alloy wires to form a conductor; extruding nylon insulating material on the outer periphery of the conductor to form an insulating layer; and finally extruding the sheath layer material on the outer periphery of the insulating layer to form a sheath layer, thereby obtaining a corrosion-resistant overhead cable.

[0006] The modified polyethylene is prepared by the following steps: Step A1: Add potassium 2-carboxyl-5-nitrobenzenesulfonate to DMF, add dichlorothionyl under stirring, and reflux and stir at 50°C for 4-5h to obtain an acyl chloride product; add 10H-phenothiazine-3,7-diamine, potassium carbonate and dimethyl sulfoxide to a flask to obtain a mixed solution 1, and then add the above-mentioned acyl chloride product to dimethyl sulfoxide to obtain a mixed solution 2, slowly dropwise add the mixed solution 2 to the mixed solution 1 in a 0°C ice-water bath, and after the dropwise addition is completed, heat to 40°C, stir and react at a constant temperature for 8-10h, and distill under reduced pressure to obtain an amide product; Further, the dosage ratio of potassium 2-carboxy-5-nitrobenzenesulfonate, DMF, and dichlorothionyl is 0.2 mol: 120 mL: 0.22-0.25 mol; the dosage ratio of 10H-phenothiazine-3,7-diamine, potassium carbonate, and dimethyl sulfoxide is 0.1 mol: 0.005-0.007 mol: 45-55 mL; the dosage ratio of the acyl chloride product and dimethyl sulfoxide is 0.1 mol: 130-140 mL; the dosage ratio of the mixed solution 1 and the mixed solution 2 is 50-60 mL: 135-145 mL; During the reaction of step A1, the carboxyl group of potassium 2-carboxy-5-nitrobenzenesulfonate reacts with thionyl chloride to generate an acyl chloride product; the acyl chloride of the acyl chloride product reacts with the primary amino group of 10H-phenothiazine-3,7-diamine to obtain a nitro-containing amide product; Step A2: Add the amide product and ethyl acetate into a three-necked flask, heat to 45-55°C, start reflux stirring, then add sodium dithionite, and reflux stirring for 1-1.5h to obtain the amino product; Further, the usage ratio of the amide product, ethyl acetate, and sodium dithionite is 0.1 mol: 190-210 mL: 0.2-0.25 mol; During the reaction of step A2, the nitro group of the amide product is reduced to an amino group to obtain an amino product; Step A3: adding the amino product, potassium carbonate and dimethyl sulfoxide into a flask to obtain a mixed solution 3, then adding methacryloyl chloride into dimethyl sulfoxide to obtain a mixed solution 4, slowly dropping the mixed solution 4 into the mixed solution 3 in an ice-water bath at 0°C, after the dropping is complete, heating to 40°C, stirring at a constant temperature to react for 8-10 hours, and distilling under reduced pressure to obtain a functional monomer; Further, the usage ratio of the amino product, potassium carbonate and dimethyl sulfoxide is 0.1 mol: 0.007-0.009 mol: 195-215 mL; the usage ratio of methacryloyl chloride and dimethyl sulfoxide is 0.2 mol: 50-60 mL; the usage ratio of mixed solution 3 and mixed solution 4 is 200-220 mL: 55-65 mL; During the reaction of step A3, methacryloyl chloride reacts with the primary amino group of the amino product to obtain a functional monomer containing a terminal carbon-carbon double bond; Step A4: low-density polyethylene, functional monomers and dicumyl peroxide were mixed and stirred for 20 minutes, melt-grafted in a twin-screw extruder at 180° C., and extruded after 5 minutes to obtain modified polyethylene; Furthermore, the dosage ratio of low-density polyethylene, functional monomer, and dicumyl peroxide is 100 g: 12 g: 0.12 g, and the screw speed frequency of the extruder is 5 Hz; During the reaction of step A4, the functional monomer is grafted into the low-density polyethylene by a melt grafting method to obtain modified polyethylene.

[0007] The modified filler is prepared by the following steps: Step B1: Add nano zinc oxide to toluene, ultrasonically disperse for 30 minutes, then add 16-nor-15-oxodehydroabietic acid and N,N'-dicyclohexyldiimide under stirring at room temperature, heat to 110-120°C, reflux and stir for 48-51 hours, then centrifuge for 10-15 minutes, centrifuge the lower precipitate once with isopropanol and anhydrous ethanol respectively, and finally vacuum dry the lower precipitate at 80°C for 12 hours to obtain modified zinc oxide; Further, the dosage ratio of nano zinc oxide, toluene, 16-nor-15-oxodehydroabietic acid, N,N'-dicyclohexyldiimide, isopropanol and anhydrous ethanol is 5g; 110mL: 12g: 2g: 10mL: 10mL; During the reaction of step B1, nano zinc oxide and 16-nor-15-oxo-dehydroabietic acid undergo a topological reaction to generate dehydroabietic acid-modified nano zinc oxide, i.e., modified zinc oxide; Step B2: In a nitrogen atmosphere, add modified zinc oxide and methylenetriphenylphosphine to anhydrous tetrahydrofuran, and reflux and stir at 40-50° C. for 3-4 hours to obtain modified zinc oxide containing a terminal double bond; Further, the usage ratio of modified zinc oxide, methylenetriphenylphosphine and anhydrous tetrahydrofuran is 8 g: 0.1 mol: 75-85 mL; During the reaction of step B2, the keto carbonyl group in the modified zinc oxide undergoes a ylide reaction with methylenetriphenylphosphine to generate a modified zinc oxide containing a terminal double bond; Step B3: Add the modified zinc oxide containing a terminal double bond to dichloromethane, start stirring, then add 3-chloroperoxybenzoic acid, and stir at room temperature for 4-5 hours to obtain an epoxy product; add 6-amino-2(3H)benzothiazolone and the epoxy product to a round-bottom flask, then add dimethyl sulfoxide, stir at 60°C for 24 hours, filter, and dry to obtain a modified filler; Further, the dosage ratio of modified zinc oxide containing terminal double bonds, dichloromethane and 3-chloroperoxybenzoic acid is 13-15 g: 60-70 mL: 0.1 mol; the dosage ratio of 6-amino-2 (3H) benzothiazolone, epoxy product and dimethyl sulfoxide is 33-35 g: 32-36 g: 140-160 mL; During the reaction of step B3, the carbon-carbon double bond in the modified zinc oxide containing a terminal double bond is oxidized to an epoxy group to obtain an epoxy product; the amino group of 6-amino-2(3H)benzothiazolone reacts with the epoxy group of the epoxy product to obtain a modified filler.

[0008] Beneficial effects of the invention: The invention discloses a corrosion-resistant overhead cable, which includes a conductor, an insulating layer and a sheath layer from the inside to the outside, and the sheath layer includes the following raw materials: polyvinyl chloride resin, modified polyethylene, modified filler, heat stabilizer, lubricant, plasticizer and ultraviolet absorber. Both the modified polyethylene and polyethylene have good corrosion resistance and meet the requirements of cable corrosion resistance.

[0009] The modified polyethylene is obtained by melt grafting a functional monomer containing a phenothiazine structure, a potassium sulfonate group, an amide group, and a terminal carbon-carbon double bond with a low-density polyethylene; the introduction of the amide group and the secondary amine group in the phenothiazine structure increases the polarity of the low-density polyethylene molecular chain, thereby enhancing its compatibility and dispersibility with the polyvinyl chloride resin; the phenothiazine structure has the functions of a peroxyl radical terminator and a peroxide decomposer in the oxidative degradation reaction of the polymer, and is grafted into the polyethylene chain, dispersed along with the dispersion of the modified polyethylene in the matrix, avoiding the migration of small molecular phenothiazine compounds, and can quickly terminate the degradation of the polymer, so that the cable sheath layer has good anti-oxidation and aging properties; the sulfur element in the potassium sulfonate group generates non-combustible gases such as sulfur dioxide when burned, diluting the concentration of combustible gases, and solidifies in the carbon layer in the form of potassium sulfate and potassium sulfite compounds to form a dense and thick protective carbon layer, reducing heat transfer in the combustion site, and synergistically effectively preventing further combustion of the matrix in the gas phase and the solid phase, while inhibiting the release of smoke; adding the modified polyethylene improves the anti-oxidation and aging properties and the flame retardancy of the cable.

[0010] The modified filler includes nano zinc oxide, benzothiazolinone structure and dehydroabietic acid structure; the nano zinc oxide can slowly release zinc ions that can enter the microbial cells, and the zinc ions react with functional groups such as carboxyl and thiol in the microorganisms to destroy the cell structure and electron transfer system of the microorganisms, thereby killing the bacteria. After the bacteria are killed, the zinc ions can be freed from the dead cells and continue to play an antibacterial role; the agglomeration phenomenon of the nano zinc oxide in the modified filler is improved, and the dispersion in the matrix is ​​more uniform, thereby improving the mechanical properties and antibacterial properties of the sheath layer After the benzothiazolinone structure comes into contact with microorganisms, it can quickly penetrate into the cells and play a bactericidal role by breaking the bonds between bacteria and algae proteins. It has the advantages of small addition amount, fast onset and strong bactericidal power, which makes up for the shortcomings of slow antibacterial speed of inorganic antibacterial agents such as nano zinc oxide, and synergistically improves the antibacterial property with oxidized zinc; dehydroabietic acid is a derivative of rosin. Due to the tricyclic diterpene structure in its molecule, it has strong hydrophobicity, so that the sheath layer has good waterproofness; adding the modified filler improves the mechanical properties, antibacterial and waterproof properties of the cable. DETAILED DESCRIPTION

[0011] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0012] Embodiment 1: A modified polyethylene, the preparation of which comprises the following steps: Step A1: Add potassium 2-carboxyl-5-nitrobenzenesulfonate to DMF, add dichlorothionyl under stirring, and reflux and stir at 50°C for 4 hours to obtain an acyl chloride product; add 10H-phenothiazine-3,7-diamine, potassium carbonate and dimethyl sulfoxide to a flask to obtain a mixed solution 1, and then add the above-mentioned acyl chloride product to dimethyl sulfoxide to obtain a mixed solution 2. In a 0°C ice-water bath, slowly drop the mixed solution 2 into the mixed solution 1. After the dropwise addition is completed, the temperature is raised to 40°C, and the reaction is stirred at a constant temperature for 8 hours, and the mixture is reduced. The amide product was obtained by distillation under reduced pressure; the dosage ratio of potassium 2-carboxy-5-nitrobenzenesulfonate, DMF, and dichlorothionyl was 0.2 mol: 120 mL: 0.22 mol; the dosage ratio of 10H-phenothiazine-3,7-diamine, potassium carbonate, and dimethyl sulfoxide was 0.1 mol: 0.005 mol: 45 mL; the dosage ratio of the acyl chloride product and dimethyl sulfoxide was 0.1 mol: 130 mL; the dosage ratio of the mixed solution 1 and the mixed solution 2 was 50 mL: 135 mL; Step A2: Add the amide product and ethyl acetate into a three-necked flask, heat to 45°C, start reflux stirring, then add sodium dithionite, and reflux stirring for 1 hour to obtain the amino product; the dosage ratio of the amide product, ethyl acetate, and sodium dithionite is 0.1 mol: 190 mL: 0.2 mol; Step A3: adding the amino product, potassium carbonate and dimethyl sulfoxide into a flask to obtain a mixed solution 3, then adding methacryloyl chloride into dimethyl sulfoxide to obtain a mixed solution 4, slowly dropping the mixed solution 4 into the mixed solution 3 in an ice water bath at 0°C, after the dropping is completed, heating to 40°C, stirring at a constant temperature for 8 hours, and distilling under reduced pressure to obtain a functional monomer; the amount ratio of the amino product, potassium carbonate and dimethyl sulfoxide is 0.1 mol: 0.007 mol: 195 mL; the amount ratio of methacryloyl chloride and dimethyl sulfoxide is 0.2 mol: 50 mL; the amount ratio of the mixed solution 3 to the mixed solution 4 is 200 mL: 55 mL; Step A4: After mixing and stirring low-density polyethylene, functional monomers and diisopropylbenzene peroxide for 20 minutes, melt-grafting is carried out in a twin-screw extruder at 180° C., and extruding after 5 minutes to obtain modified polyethylene; the amount ratio of low-density polyethylene, functional monomers and diisopropylbenzene peroxide is 100g:12g:0.12g, and the screw speed frequency of the extruder is 5Hz.

[0013] Embodiment 2: A modified polyethylene, the preparation of which comprises the following steps: Step A1: Add potassium 2-carboxy-5-nitrobenzenesulfonate to DMF, add dichlorothionyl under stirring, and reflux and stir at 50°C for 4.5 hours to obtain an acyl chloride product; add 10H-phenothiazine-3,7-diamine, potassium carbonate and dimethyl sulfoxide to a flask to obtain a mixed solution 1, and then add the above-mentioned acyl chloride product to dimethyl sulfoxide to obtain a mixed solution 2. In a 0°C ice-water bath, slowly drop the mixed solution 2 into the mixed solution 1. After the dropwise addition is completed, the temperature is raised to 40°C, and the reaction is stirred at a constant temperature for 9 hours. The amide product was obtained by distillation under reduced pressure; the dosage ratio of potassium 2-carboxy-5-nitrobenzenesulfonate, DMF, and dichlorothionyl was 0.2 mol: 120 mL: 0.23 mol; the dosage ratio of 10H-phenothiazine-3,7-diamine, potassium carbonate, and dimethyl sulfoxide was 0.1 mol: 0.006 mol: 50 mL; the dosage ratio of the acyl chloride product and dimethyl sulfoxide was 0.1 mol: 135 mL; the dosage ratio of the mixed solution 1 and the mixed solution 2 was 55 mL: 140 mL; Step A2: Add the amide product and ethyl acetate into a three-necked flask, heat to 50°C, start reflux stirring, then add sodium dithionite, and reflux stirring to react for 1.3 hours to obtain the amino product; the dosage ratio of the amide product, ethyl acetate, and sodium dithionite is 0.1 mol: 200 mL: 0.23 mol; Step A3: adding the amino product, potassium carbonate and dimethyl sulfoxide into a flask to obtain a mixed solution 3, then adding methacryloyl chloride into dimethyl sulfoxide to obtain a mixed solution 4, slowly dropping the mixed solution 4 into the mixed solution 3 in an ice water bath at 0°C, after the dropping is completed, heating to 40°C, stirring at a constant temperature for 9 hours, and distilling under reduced pressure to obtain a functional monomer; the amount ratio of the amino product, potassium carbonate and dimethyl sulfoxide is 0.1 mol: 0.008 mol: 205 mL; the amount ratio of methacryloyl chloride and dimethyl sulfoxide is 0.2 mol: 55 mL; the amount ratio of the mixed solution 3 to the mixed solution 4 is 210 mL: 60 mL; Step A4: After mixing and stirring low-density polyethylene, functional monomers and diisopropylbenzene peroxide for 20 minutes, melt-grafting is carried out in a twin-screw extruder at 180° C., and extruding after 5 minutes to obtain modified polyethylene; the amount ratio of low-density polyethylene, functional monomers and diisopropylbenzene peroxide is 100g:12g:0.12g, and the screw speed frequency of the extruder is 5Hz.

[0014] Embodiment 3: A modified polyethylene, the preparation of which comprises the following steps: Step A1: Add potassium 2-carboxyl-5-nitrobenzenesulfonate to DMF, add dichlorothionyl under stirring, and reflux and stir at 50°C for 5 hours to obtain an acyl chloride product; add 10H-phenothiazine-3,7-diamine, potassium carbonate and dimethyl sulfoxide to a flask to obtain a mixed solution 1, and then add the above-mentioned acyl chloride product to dimethyl sulfoxide to obtain a mixed solution 2. In a 0°C ice-water bath, slowly drop the mixed solution 2 into the mixed solution 1. After the dropwise addition is completed, the temperature is raised to 40°C, and the reaction is stirred at a constant temperature for 10 hours. The amide product was obtained by distillation under reduced pressure; the dosage ratio of potassium 2-carboxy-5-nitrobenzenesulfonate, DMF, and dichlorothionyl was 0.2 mol: 120 mL: 0.25 mol; the dosage ratio of 10H-phenothiazine-3,7-diamine, potassium carbonate, and dimethyl sulfoxide was 0.1 mol: 0.007 mol: 55 mL; the dosage ratio of the acyl chloride product and dimethyl sulfoxide was 0.1 mol: 140 mL; the dosage ratio of the mixed solution 1 and the mixed solution 2 was 60 mL: 145 mL; Step A2: Add the amide product and ethyl acetate into a three-necked flask, heat to 55°C, start reflux stirring, then add sodium dithionite, and reflux stirring for 1.5h to obtain the amino product; the dosage ratio of the amide product, ethyl acetate, and sodium dithionite is 0.1mol:210mL:0.25mol; Step A3: adding the amino product, potassium carbonate and dimethyl sulfoxide into a flask to obtain a mixed solution 3, then adding methacryloyl chloride into dimethyl sulfoxide to obtain a mixed solution 4, slowly dropping the mixed solution 4 into the mixed solution 3 in an ice water bath at 0°C, after the dropping is completed, heating to 40°C, stirring at a constant temperature for 10 hours, and distilling under reduced pressure to obtain a functional monomer; the amount ratio of the amino product, potassium carbonate and dimethyl sulfoxide is 0.1 mol: 0.009 mol: 215 mL; the amount ratio of methacryloyl chloride and dimethyl sulfoxide is 0.2 mol: 60 mL; the amount ratio of the mixed solution 3 to the mixed solution 4 is 220 mL: 65 mL; Step A4: After mixing and stirring low-density polyethylene, functional monomers and diisopropylbenzene peroxide for 20 minutes, melt-grafting is carried out in a twin-screw extruder at 180° C., and extruding after 5 minutes to obtain modified polyethylene; the amount ratio of low-density polyethylene, functional monomers and diisopropylbenzene peroxide is 100g:12g:0.12g, and the screw speed frequency of the extruder is 5Hz.

[0015] Embodiment 4: A modified filler, the preparation of which comprises the following steps: Step B1: Add nano zinc oxide to toluene, ultrasonically disperse for 30 minutes, then add 16-nor-15-oxo-dehydroabietic acid and N, N'-dicyclohexyl diimide at room temperature with stirring, heat to 110°C, reflux and stir for 48 hours, then centrifuge for 10 minutes, centrifuge the lower precipitate once with isopropanol and anhydrous ethanol respectively, and finally vacuum dry the lower precipitate at 80°C for 12 hours to obtain modified zinc oxide; the dosage ratio of nano zinc oxide, toluene, 16-nor-15-oxo-dehydroabietic acid, N, N'-dicyclohexyl diimide, isopropanol and anhydrous ethanol is 5g; 110mL: 12g: 2g: 10mL: 10mL; Step B2: In a nitrogen atmosphere, add modified zinc oxide and methylene triphenylphosphine to anhydrous tetrahydrofuran, and reflux and stir at 40°C for 3 hours to obtain modified zinc oxide containing a terminal double bond; the amount ratio of modified zinc oxide, methylene triphenylphosphine and anhydrous tetrahydrofuran is 8g:0.1mol:75mL; Step B3: Add the modified zinc oxide containing a terminal double bond to dichloromethane, start stirring, then add 3-chloroperoxybenzoic acid, and stir to react at room temperature for 4 hours to obtain the epoxy product; add 6-amino-2(3H)benzothiazolone and the epoxy product to a round-bottom flask, then add dimethyl sulfoxide, stir to react at 60°C for 24 hours, filter, and dry to obtain the modified filler; the amount ratio of the modified zinc oxide containing a terminal double bond, dichloromethane and 3-chloroperoxybenzoic acid is 13g:60mL:0.1mol; the amount ratio of 6-amino-2(3H)benzothiazolone, epoxy product and dimethyl sulfoxide is 33g:32g:140mL.

[0016] Embodiment 5: A modified filler, the preparation of which comprises the following steps: Step B1: Add nano zinc oxide to toluene, ultrasonically disperse for 30 minutes, then add 16-nor-15-oxo-dehydroabietic acid and N, N'-dicyclohexyl diimide at room temperature with stirring, heat to 115°C, reflux and stir for 49 hours, then centrifuge for 13 minutes, centrifuge the lower precipitate once with isopropanol and anhydrous ethanol respectively, and finally vacuum dry the lower precipitate at 80°C for 12 hours to obtain modified zinc oxide; the dosage ratio of nano zinc oxide, toluene, 16-nor-15-oxo-dehydroabietic acid, N, N'-dicyclohexyl diimide, isopropanol and anhydrous ethanol is 5g; 110mL: 12g: 2g: 10mL: 10mL; Step B2: In a nitrogen atmosphere, add modified zinc oxide and methylene triphenylphosphine to anhydrous tetrahydrofuran, and reflux and stir at 45°C for 3.5 hours to obtain modified zinc oxide containing a terminal double bond; the amount ratio of modified zinc oxide, methylene triphenylphosphine and anhydrous tetrahydrofuran is 8g:0.1mol:80mL; Step B3: Add the modified zinc oxide containing a terminal double bond to dichloromethane, start stirring, then add 3-chloroperoxybenzoic acid, and stir to react at room temperature for 4.5 hours to obtain the epoxy product; add 6-amino-2(3H)benzothiazolone and the epoxy product to a round-bottom flask, then add dimethyl sulfoxide, stir to react at 60°C for 24 hours, filter, and dry to obtain the modified filler; the amount ratio of the modified zinc oxide containing a terminal double bond, dichloromethane and 3-chloroperoxybenzoic acid is 14g:65mL:0.1mol; the amount ratio of 6-amino-2(3H)benzothiazolone, epoxy product and dimethyl sulfoxide is 34g:34g:150mL.

[0017] Embodiment 6: A modified filler, the preparation of which comprises the following steps: Step B1: Add nano zinc oxide to toluene, ultrasonically disperse for 30 minutes, then add 16-nor-15-oxo-dehydroabietic acid and N, N'-dicyclohexyl diimide at room temperature with stirring, heat to 120°C, reflux and stir for 51 hours, then centrifuge for 15 minutes, centrifuge the lower precipitate once with isopropanol and anhydrous ethanol respectively, and finally vacuum dry the lower precipitate at 80°C for 12 hours to obtain modified zinc oxide; the dosage ratio of nano zinc oxide, toluene, 16-nor-15-oxo-dehydroabietic acid, N, N'-dicyclohexyl diimide, isopropanol and anhydrous ethanol is 5g; 110mL: 12g: 2g: 10mL: 10mL; Step B2: In a nitrogen atmosphere, add modified zinc oxide and methylene triphenylphosphine to anhydrous tetrahydrofuran, and reflux and stir at 50° C. for 4 h to obtain modified zinc oxide containing a terminal double bond; the amount ratio of modified zinc oxide, methylene triphenylphosphine and anhydrous tetrahydrofuran is 8 g: 0.1 mol: 85 mL; Step B3: Add the modified zinc oxide containing a terminal double bond to dichloromethane, start stirring, then add 3-chloroperoxybenzoic acid, and stir to react at room temperature for 5 hours to obtain the epoxy product; add 6-amino-2(3H)benzothiazolone and the epoxy product to a round-bottom flask, then add dimethyl sulfoxide, stir to react at 60°C for 24 hours, filter, and dry to obtain the modified filler; the amount ratio of the modified zinc oxide containing a terminal double bond, dichloromethane and 3-chloroperoxybenzoic acid is 15g:70mL:0.1mol; the amount ratio of 6-amino-2(3H)benzothiazolone, epoxy product and dimethyl sulfoxide is 35g:36g:160mL.

[0018] Embodiment 7: A corrosion-resistant overhead cable, comprising a conductor, an insulating layer and a sheath layer from the inside to the outside, wherein the conductor is located in the innermost layer, the insulating layer is coated on the outer periphery of the conductor, and the sheath layer is coated on the outer periphery of the insulating layer; the conductor is formed by twisting a plurality of aluminum alloy wires; the insulating layer is made of nylon insulating material; the sheath layer comprises the following raw materials in parts by weight: 90 parts of polyvinyl chloride resin, 10 parts of modified polyethylene, 8 parts of modified filler, 2 parts of heat stabilizer, 0.2 parts of lubricant, 3 parts of plasticizer and 0.6 parts of ultraviolet absorber; the heat stabilizer is prepared by mixing calcium stearate and zinc stearate in a mass ratio of 1:1, the lubricant is stearic acid, the plasticizer is epoxy soybean oil, and the ultraviolet absorber is 2-(2'-hydroxy-5'-methylphenyl)benzotriazole; The preparation of the corrosion-resistant overhead cable comprises the following steps: Step S1: adding polyvinyl chloride resin and the modified polyethylene obtained in Example 1 into a mixer, stirring at a high speed of 900 r / min, adding the modified filler, heat stabilizer, lubricant, plasticizer and ultraviolet absorber obtained in Example 4 while stirring, stirring for 30 minutes, reducing the speed to 600 r / min, stirring and heating to 120° C., and discharging the material after 3 minutes to obtain a sheath layer material; Step S2: twisting a plurality of aluminum alloy wires to form a conductor; extruding nylon insulating material on the outer periphery of the conductor to form an insulating layer; and finally extruding the sheath layer material on the outer periphery of the insulating layer to form a sheath layer, thereby obtaining a corrosion-resistant overhead cable.

[0019] Embodiment 8: A corrosion-resistant overhead cable, comprising a conductor, an insulating layer and a sheath layer from the inside to the outside, wherein the conductor is located in the innermost layer, the insulating layer is coated on the outer periphery of the conductor, and the sheath layer is coated on the outer periphery of the insulating layer; the conductor is formed by twisting a plurality of aluminum alloy wires; the insulating layer is made of nylon insulating material; the sheath layer comprises the following raw materials in parts by weight: 100 parts of polyvinyl chloride resin, 13 parts of modified polyethylene, 9 parts of modified filler, 3 parts of heat stabilizer, 0.3 parts of lubricant, 4 parts of plasticizer and 0.7 parts of ultraviolet absorber; the heat stabilizer is prepared by mixing calcium stearate and zinc stearate in a mass ratio of 1:1, the lubricant is stearic acid, the plasticizer is epoxy soybean oil, and the ultraviolet absorber is 2-(2'-hydroxy-5'-methylphenyl)benzotriazole; The preparation of the corrosion-resistant overhead cable comprises the following steps: Step S1: adding polyvinyl chloride resin and the modified polyethylene obtained in Example 2 into a mixer, stirring at a high speed of 900 r / min, adding the modified filler, heat stabilizer, lubricant, plasticizer and ultraviolet absorber obtained in Example 5 while stirring, stirring for 35 minutes, reducing the speed to 600 r / min, stirring and heating to 120° C., and discharging after 3 minutes to obtain a sheath layer material; Step S2: twisting 16 aluminum alloy wires to form a conductor; extruding nylon insulation material on the outer periphery of the conductor to form an insulation layer; and finally extruding the sheath layer material on the outer periphery of the insulation layer to form a sheath layer, thereby obtaining a corrosion-resistant overhead cable.

[0020] Embodiment 9: A corrosion-resistant overhead cable, comprising a conductor, an insulating layer and a sheath layer from the inside to the outside, wherein the conductor is located in the innermost layer, the insulating layer is coated on the outer periphery of the conductor, and the sheath layer is coated on the outer periphery of the insulating layer; the conductor is formed by twisting a plurality of aluminum alloy wires; the insulating layer is made of nylon insulating material; the sheath layer comprises the following raw materials in parts by weight: 110 parts of polyvinyl chloride resin, 15 parts of modified polyethylene, 10 parts of modified filler, 4 parts of heat stabilizer, 0.4 parts of lubricant, 5 parts of plasticizer and 0.8 parts of ultraviolet absorber; the heat stabilizer is prepared by mixing calcium stearate and zinc stearate in a mass ratio of 1:1, the lubricant is stearic acid, the plasticizer is epoxy soybean oil, and the ultraviolet absorber is 2-(2'-hydroxy-5'-methylphenyl)benzotriazole; The preparation of the corrosion-resistant overhead cable comprises the following steps: Step S1: adding polyvinyl chloride resin and the modified polyethylene obtained in Example 3 into a mixer, stirring at a high speed of 1000 r / min, adding the modified filler, heat stabilizer, lubricant, plasticizer and ultraviolet absorber obtained in Example 6 while stirring, stirring for 40 minutes, reducing the speed to 700 r / min, stirring and heating to 120° C., and discharging after 3 minutes to obtain a sheath layer material; Step S2: twisting 18 aluminum alloy wires to form a conductor; extruding nylon insulation material on the outer periphery of the conductor to form an insulation layer; and finally extruding the sheath layer material on the outer periphery of the insulation layer to form a sheath layer, thereby obtaining a corrosion-resistant overhead cable.

[0021] Comparative Example 1: Compared with Example 9, the modified polyethylene is replaced with low-density polyethylene, and the rest is exactly the same as Example 9 to prepare a corrosion-resistant overhead cable.

[0022] Comparative Example 2: Compared with Example 9, the modified filler is replaced with the modified zinc oxide obtained in step B1 of Example 6, and the rest is exactly the same as Example 9 to prepare a corrosion-resistant overhead cable.

[0023] The corrosion-resistant overhead cable of the present invention is further tested for its effectiveness, and the test results are as follows.

[0024] In order to test the corrosion-resistant overhead cable of the present invention, the sheath layer materials for the overhead cables obtained in Examples 7-9 and Comparative Examples 1-2 were subjected to tensile strength and elongation at break tests according to GB / T2951.11-2008 "General Test Methods for Insulation and Sheath Materials of Electric and Optical Cables"; the sheath layer materials were aged at 80°C in an air box for 168h, and the tensile strength and elongation at break retention rates were tested according to the method of GB / T2951-2008; the oxygen index was measured according to GB / T2406.1-2008 "Determination of Combustion Behavior of Plastics by Oxygen Index Method"; the oxygen index was measured according to GB / T31 402-2015 "Test Method for Antibacterial Performance of Plastic Surface" uses Escherichia coli and Staphylococcus aureus as the test bacteria for antibacterial testing, and the size of the sheath material sample is 2mm×40mm×40mm; Waterproof performance test method: Take 150.0g of the cable samples obtained from Examples 7-9 and Comparative Examples 1-2 and immerse them in water (water temperature 15°C), seal both ends of the sample and extend 300mm out of the water surface. After soaking for one week, measure the weight after soaking and remove the sheath layer after soaking, and observe whether there is moisture on the outer surface of the cable after removing the sheath layer; and record the results in Table 1; Table 1: Test results

[0025] According to the data in Table 1, the material used for the sheath layer of the corrosion-resistant overhead cable of the present invention has good resistance to oxidation and aging, flame retardancy, mechanical properties, water resistance and antibacterial properties, thereby improving the resistance to oxidation and aging, flame retardancy, mechanical properties, water resistance and antibacterial properties of the cable; Comparison between Example 9 and Comparative Example 1 shows that modified polyethylene is used to introduce phenothiazine and potassium sulfonate groups to improve the resistance to oxidation and aging and flame retardancy of the cable; Comparison between Example 9 and Comparative Example 2 shows that modified fillers are used to introduce benzothiazolinone structures into nano zinc oxide, which cooperates with nano zinc oxide to quickly improve the antibacterial properties of the cable.

[0026] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

Claims

1. A corrosion-resistant overhead cable, characterized in that: The invention comprises a conductor, an insulating layer and a sheath layer from the inside to the outside, wherein the conductor is located in the innermost layer, the insulating layer is coated on the outer periphery of the conductor, and the sheath layer is coated on the outer periphery of the insulating layer; the sheath layer comprises the following raw materials in parts by weight: 90-110 parts of polyvinyl chloride resin, 10-15 parts of modified polyethylene, 8-10 parts of modified filler, 2-4 parts of heat stabilizer, 0.2-0.4 parts of lubricant, 3-5 parts of plasticizer and 0.6-0.8 parts of ultraviolet absorber; The modified polyethylene is prepared by the following steps: Step A1: Add potassium 2-carboxyl-5-nitrobenzenesulfonate to DMF, add dichlorothionyl under stirring, and reflux and stir at 50° C. for 4-5 hours to obtain an acyl chloride product; 10H-phenothiazine-3,7-diamine, potassium carbonate and dimethyl sulfoxide are added to a flask to obtain a mixed solution 1, and then the above-mentioned acyl chloride product is added to dimethyl sulfoxide to obtain a mixed solution 2. In a 0°C ice-water bath, the mixed solution 2 is slowly added dropwise to the mixed solution 1. After the addition is completed, the temperature is raised to 40°C, and the reaction is stirred at a constant temperature for 8-10 hours, and the amide product is obtained by distillation under reduced pressure; Step A2: Add the amide product and ethyl acetate into a three-necked flask, heat to 45-55°C, start reflux stirring, then add sodium dithionite, and reflux stirring for 1-1.5h to obtain the amino product; Step A3: adding the amino product, potassium carbonate and dimethyl sulfoxide into a flask to obtain a mixed solution 3, then adding methacryloyl chloride into dimethyl sulfoxide to obtain a mixed solution 4, slowly dropping the mixed solution 4 into the mixed solution 3 in an ice-water bath at 0°C, after the dropping is complete, heating to 40°C, stirring at a constant temperature to react for 8-10 hours, and distilling under reduced pressure to obtain a functional monomer; Step A4: low-density polyethylene, functional monomers and dicumyl peroxide are mixed and stirred for 20 minutes, melt-grafted in a twin-screw extruder at 180° C., and extruded after 5 minutes to obtain modified polyethylene.

2. A corrosion-resistant overhead cable according to claim 1, characterized in that: In step A1, the usage ratio of potassium 2-carboxy-5-nitrobenzenesulfonate, DMF, and dichlorothionyl is 0.2 mol: 120 mL: 0.22-0.25 mol; the usage ratio of 10H-phenothiazine-3,7-diamine, potassium carbonate, and dimethyl sulfoxide is 0.1 mol: 0.005-0.007 mol: 45-55 mL; the usage ratio of acyl chloride product and dimethyl sulfoxide is 0.1 mol: 130-140 mL; the usage ratio of mixed solution 1 and mixed solution 2 is 50-60 mL: 135-145 mL.

3. The corrosion-resistant overhead cable according to claim 1, characterized in that: In step A2, the usage ratio of the amide product, ethyl acetate and sodium dithionite is 0.1 mol:190-210 mL:0.2-0.25 mol.

4. The corrosion-resistant overhead cable according to claim 1, characterized in that: In step A3, the usage ratio of the amino product, potassium carbonate and dimethyl sulfoxide is 0.1 mol: 0.007-0.009 mol: 195-215 mL; the usage ratio of methacryloyl chloride and dimethyl sulfoxide is 0.2 mol: 50-60 mL; and the usage ratio of mixed solution 3 and mixed solution 4 is 200-220 mL: 55-65 mL.

5. The corrosion-resistant overhead cable according to claim 1, characterized in that: In step A4, the usage ratio of low-density polyethylene, functional monomer and dicumyl peroxide is 100 g:12 g:0.12 g, and the screw speed frequency of the extruder is 5 Hz.

6. The corrosion-resistant overhead cable according to claim 1, characterized in that: The modified filler is prepared by the following steps: Step B1: Add nano zinc oxide to toluene, ultrasonically disperse for 30 minutes, then add 16-nor-15-oxodehydroabietic acid and N,N'-dicyclohexyldiimide under stirring at room temperature, heat to 110-120°C, reflux and stir for 48-51 hours, then centrifuge for 10-15 minutes, centrifuge the lower precipitate once with isopropanol and anhydrous ethanol respectively, and finally vacuum dry the lower precipitate at 80°C for 12 hours to obtain modified zinc oxide; Step B2: In a nitrogen atmosphere, add modified zinc oxide and methylenetriphenylphosphine to anhydrous tetrahydrofuran, and reflux and stir at 40-50° C. for 3-4 hours to obtain modified zinc oxide containing a terminal double bond; Step B3: Add the modified zinc oxide containing a terminal double bond into dichloromethane, start stirring, then add 3-chloroperbenzoic acid, and stir at room temperature for 4-5 hours to obtain an epoxy product; Add 6-amino-2(3H)benzothiazolone and the epoxy product into a round-bottom flask, then add dimethyl sulfoxide, stir and react at 60°C for 24 hours, filter and dry to obtain the modified filler.

7. The corrosion-resistant overhead cable according to claim 6, characterized in that: In step B1, the usage ratio of nano zinc oxide, toluene, 16-nor-15-oxodehydroabietic acid, N,N'-dicyclohexyldiimide, isopropanol and anhydrous ethanol is 5g; 110mL:12g:2g:10mL:10mL.

8. The corrosion-resistant overhead cable according to claim 6, characterized in that: In step B2, the usage ratio of modified zinc oxide, methylenetriphenylphosphine and anhydrous tetrahydrofuran is 8 g:0.1 mol:75-85 mL.

9. The corrosion-resistant overhead cable according to claim 6, characterized in that: In step B3, the usage ratio of modified zinc oxide containing terminal double bonds, dichloromethane and 3-chloroperbenzoic acid is 13-15 g: 60-70 mL: 0.1 mol; the usage ratio of 6-amino-2(3H)benzothiazolone, epoxy product and dimethyl sulfoxide is 33-35 g: 32-36 g: 140-160 mL.

10. The corrosion-resistant overhead cable according to claim 1, characterized in that: The conductor is formed by twisting a plurality of aluminum alloy wires, and the insulating layer is made of nylon insulating material; the heat stabilizer is prepared by mixing calcium stearate and zinc stearate in a mass ratio of 1:1, the lubricant is stearic acid, the plasticizer is epoxy soybean oil, and the ultraviolet absorber is 2-(2'-hydroxy-5'-methylphenyl)benzotriazole.

Citation Information

Patent Citations

  • Aerial cable with corrosion-resistant shell and preparation method thereof

    CN115850885A

  • Anti-ultraviolet aging cable and preparation method thereof

    CN118562236A

Cited By

  • Waterproof and corrosion-resistant cable sheath material and preparation method thereof

    CN120554739A

  • A waterproof and corrosion-resistant cable sheath material and its preparation method

    CN120554739B

  • Weather-proof large-section aerial insulated cable and preparation method and application thereof

    CN121483746A

  • Weather-resistant large-section overhead insulated cable and preparation method and application thereof

    CN121483746B