Aluminum-plated steel sheet for hot stamping
The aluminum-plated steel sheet with a carbon-rich and rutile-structured surface treatment film addresses the inefficiencies in heating times and high-temperature losses of existing methods, enhancing productivity through accelerated heating.
Patent Information
- Application Number
- JP2024503823
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-08-29
- Filing Date
- 2023-08-28
- Publication Date
- 2024-09-19
- Estimated Expiration
- 2043-08-28
AI Technical Summary
Existing hot stamping methods for steel plates require long heating times to reach desired temperatures, limiting productivity, and aluminum-plated steel sheets with organic coatings lose effectiveness at high temperatures, further hindering productivity improvements.
An aluminum-plated steel sheet with a surface treatment film containing a carbon-rich compound and a metal oxide or fluoride with a rutile structure, having specific concentration gradients, enhances the temperature increase rate during heating.
The proposed solution significantly accelerates the heating process, improving the productivity of hot stamping members by efficiently absorbing radiant heat and maintaining effectiveness at high temperatures.
Smart Images

Figure 0007553876000008 
Figure 0007553876000007 
Figure 0007553876000002
Abstract
Description
[Technical field]
[0001] The present invention relates to an aluminum-plated steel sheet for hot stamping. This application claims priority based on Japanese Patent Application No. 2022-135751, filed on August 29, 2022, the contents of which are incorporated herein by reference. [Background technology]
[0002] In recent years, there has been an increasing demand to reduce the consumption of chemical fuels in order to protect the environment and prevent global warming, and this demand is affecting various manufacturing industries. For example, automobiles, which are indispensable in daily life and activities as a means of transportation, are no exception, and there is a demand for improving fuel efficiency by reducing the weight of the vehicle body. However, in the case of automobiles, simply reducing the weight of the vehicle body may lead to a decrease in safety, such as a decrease in the strength of the vehicle body (for example, a decrease in crash resistance), which is not desirable from the perspective of product quality. Therefore, when reducing the weight of a vehicle body, it is necessary to do so appropriately while ensuring safety.
[0003] Many of the structures of automobiles are formed from iron, particularly steel plates. Therefore, reducing the weight of steel plates is effective in reducing the weight of the vehicle body. Moreover, such requests for reducing the weight of steel plates are made not only in the automobile manufacturing industry but also in various other manufacturing industries. In order to meet such requests, it is possible to simply reduce the weight of the steel plates by reducing the thickness of the steel plates. However, reducing the thickness of the steel plates leads to a decrease in the strength of the vehicle body. Therefore, in recent years, research and development has been conducted on steel plates that can maintain or increase the mechanical strength of the vehicle body made of steel plates by increasing the mechanical strength of the steel plates, even if they are thinner than the conventional steel plates that were used previously.
[0004] Generally, materials with high mechanical strength tend to show a decrease in shape fixability during forming such as bending. Therefore, when a material with high mechanical strength is processed into a complex shape, the processing itself becomes difficult. One of the means for solving such problems regarding formability is the so-called "hot stamping method (also called hot pressing method, hot pressing method, high temperature pressing method, or die quenching method)."
[0005] In the hot stamping method, the material to be formed is heated to a high temperature to transform (austenitize) it into a structure called austenite, and the heated and softened steel plate is pressed to form it, and then cooled after forming. According to this hot stamping method, the material is once heated to a high temperature to soften it, so that the material can be easily pressed. Furthermore, the mechanical strength of the material can be increased by the quenching effect caused by cooling after forming. Therefore, the hot stamping method can produce a formed product with good shape fixability and high mechanical strength.
[0006] For example, Patent Document 1 discloses a technique for manufacturing a molded product that can be used as an automobile part by processing a galvannealed steel sheet by a hot stamping method. Furthermore, Patent Documents 2 and 3 disclose a technique for shortening the time required for heating to a desired temperature by applying a coating mainly composed of an organic substance such as a carbon pigment onto an aluminum-plated steel sheet. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2003-126921 A [Patent Document 2] JP 2011-149084 A [Patent Document 3] Special Publication No. 2017-518438 Summary of the Invention [Problem to be solved by the invention]
[0008] Here, the hot stamping method described in Patent Document 1 requires heating the steel sheet to be processed to 700 to 1000° C. Therefore, time must be secured for heating the steel sheet to the desired temperature, and improvement in productivity has been insufficient. In addition, in the aluminum-plated steel sheets described in Patent Documents 2 and 3, the carbon pigments and the like contained in the films on the steel sheets are all organic substances, and therefore, when the aluminum-plated steel sheet is heated to a high temperature range of 750° C. or higher, all of these organic substances disappear. Therefore, even in the techniques described in Patent Documents 2 and 3, improvement in productivity was insufficient.
[0009] The present invention has been made in consideration of the above problems, and an object of the present invention is to provide a steel sheet for hot stamping that can further improve the productivity of hot stamped members. [Means for solving the problem]
[0010] In order to solve the above problems, the present inventors have conducted extensive research. As a result, they have found that when manufacturing a hot stamped member using a steel sheet for hot stamping, if the heating rate when the steel sheet is heated to a desired temperature (for example, Ac3 point or higher) can be increased, the heating time can be shortened, which contributes to improving productivity. Specifically, they have found that the heating rate can be significantly increased by providing a surface treatment film on a plating layer, the surface treatment film containing compound A having a carbon concentration of 80 mass% or more and compound B which is an oxide or fluoride of metal element M and has a rutile structure, and controlling the concentration range of metal element M to a predetermined range. The gist of the present invention, which was completed based on these findings, is as follows.
[0011] [1] An aluminum-plated steel sheet for hot stamping according to one aspect of the present invention comprises: A base steel plate; An aluminum plating layer provided on at least one surface of the base steel sheet; and a surface treatment film provided on the aluminum plating layer, The surface treatment film is A compound A containing carbon; Compound B is an oxide or fluoride of metal element M and has a rutile structure; The carbon concentration of the compound A is 80% by mass or more, The concentration of the metal element M satisfies the following formula (1) and formula (2). 1≦C bM ≦40...Equation (1) 1.5≦C bM / C tM ≦10.0...Equation (2) Here, when the average thickness of the surface treatment film is H (μm), C in the above formula (2) tM is the concentration of the metal element M at a position 0.05H from the surface of the surface treatment film, in mass %, C in the above formula (1) and (2) bM is the concentration of the metal element M at a position 0.95H from the surface of the surface treatment film, in mass %. [2] In the aluminum-plated steel sheet for hot stamping according to the above [1], a content of the compound A may be 30% or more and 80% or less at a position 0.90H from the surface of the surface treatment film. [3] In the aluminum-plated steel sheet for hot stamping according to the above [1] or [2], the compound B may be TiO2. Effect of the Invention
[0012] According to the above aspect of the present invention, it is possible to provide a steel sheet for hot stamping that can further improve the productivity of hot stamped members. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a schematic cross-sectional view of an aluminum-plated steel sheet for hot stamping according to one embodiment of the present invention. [Diagram 2] FIG. 1 is a schematic cross-sectional view of an aluminum-plated steel sheet for hot stamping according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] A preferred embodiment of the present invention will be described in detail below. Note that the present invention is not limited to the configuration disclosed in this embodiment, and various modifications are possible without departing from the spirit of the present invention. In addition, the numerical ranges described below include lower and upper limits. Numerical values indicated as "greater than" or "less than" are not included in the numerical range.
[0015] (Aluminum-plated steel sheet for hot stamping) The aluminum-plated steel sheet for hot stamping (hereinafter also referred to as "HS aluminum-plated steel sheet") according to an embodiment of the present invention makes it possible to increase the temperature rise rate when the HS aluminum-plated steel sheet is heated when a hot stamped member is manufactured using the aluminum-plated steel sheet for HS. In other words, by using the aluminum-plated steel sheet for HS according to the present embodiment, which can increase the temperature rise rate during heating, it becomes possible to improve the productivity of hot stamped members.
[0016] In the present embodiment, the aluminum-plated steel sheet for hot stamping has a surface treatment film containing a predetermined compound on at least one surface of the plated steel sheet on which an aluminum plating layer is formed, in order to improve the temperature rise rate when the aluminum-plated steel sheet for HS is heated. By providing a surface treatment film containing a predetermined compound on at least one surface of the plated steel sheet on which an aluminum plating layer is formed, the temperature rise rate of the obtained aluminum-plated steel sheet for HS can be increased when the sheet is heated. The surface treatment film may be formed on both surfaces of the plated steel sheet on which the aluminum plating layer is formed, or only on one surface. The surface treatment film may be formed on the entire surface of the plated steel sheet on which the aluminum plating layer is formed, or may be a part of the surface. From the viewpoint of further improving the productivity of the hot stamp member, it is preferable that the surface treatment film is formed on the entire surface of the plated steel sheet on which the aluminum plating layer is formed.
[0017] In the aluminum-plated steel sheet for hot stamping according to this embodiment, the type of steel sheet (base steel sheet) serving as the base material is not particularly limited. Examples of the base steel sheet include various hot-rolled steel sheets and cold-rolled steel sheets. The plated steel sheet constituting the aluminum-plated steel sheet for hot stamping according to this embodiment has a plating layer on at least one surface of such a base steel sheet. Examples of the plated steel sheet include steel sheets that have been subjected to hot-dip aluminum plating. However, the plating layer according to this embodiment is not limited to hot-dip aluminum plating as long as it is applicable to hot stamping.
[0018] Conventionally, most of the steel sheets used for automotive frame parts and the like have been hot-rolled steel sheets, cold-rolled steel sheets, or plated steel sheets coated with aluminum, zinc, etc. These conventional steel sheets have low emissivity, and therefore have a low rate of temperature rise due to radiant heating.
[0019] In the aluminum-plated steel sheet for hot stamping of this embodiment, a predetermined surface treatment film, which will be described later, is applied to the entire surface of at least one surface of the plating layer, thereby making it possible to increase the temperature rise rate during hot stamp heating. Specifically, the productivity of hot stamped members can be further improved by heating an aluminum-plated steel sheet for HS use having a predetermined surface treatment film and hot stamping the heated aluminum-plated steel sheet for hot stamping.
[0020] <Surface treatment film> FIG. 1 shows a schematic cross-sectional view of a surface portion of one of the surfaces of an aluminum-plated steel sheet for hot stamping according to this embodiment.
[0021] As shown in FIG. 1, the aluminum-plated steel sheet 10 for hot stamping according to this embodiment has, for example, a base steel sheet 11, an aluminum plating layer (Al plating layer) 12 provided on at least one surface of the base steel sheet 11, and a surface treatment film 13 provided on the aluminum plating layer 12. In the aluminum-plated steel sheet 10 for hot stamping according to this embodiment, the surface on the side to which the surface treatment film 13 is applied (i.e., the surface of the surface treatment film 13) has a high emissivity. Therefore, the temperature rise rate during hot stamp heating is high, and as a result, the productivity of the hot stamped member can be further improved. Note that FIG. 1 is a schematic diagram for explanation, and the dimensions of the surface treatment film 13 and the aluminum plating layer 12, etc. do not necessarily show a preferred embodiment, and are not limited to the dimensions of FIG. 1, etc.
[0022] The surface treatment film 13 according to this embodiment contains compound A, which contains carbon, and compound B, which is an oxide or fluoride of metal element M and has a rutile structure. The surface treatment film 13 according to this embodiment may further contain a binder component as necessary. The surface treatment film 13 according to this embodiment may also contain silica. Furthermore, in this embodiment, the temperature rise rate (heating efficiency) during hot stamp heating can be improved by adjusting the contents of compound A and compound B in the surface treatment film 13, the concentration distribution of metal element M, the application and drying methods of the surface treatment film 13, and the film thickness, etc.
[0023] Moreover, in the surface treatment film 13 according to this embodiment, the compound B has a predetermined concentration distribution. Specifically, the concentration of the metal element M constituting the compound B in the film has a concentration distribution (concentration gradient) in which the concentration in the film is higher on the plating layer side than on the surface side of the film in the film thickness direction. The presence of the metal element M in such a predetermined concentration distribution makes it possible to further increase the heating efficiency of the surface treatment film 13. When the hot stamp steel sheet according to this embodiment is hot stamp heated, the radiant heat from the heating atmosphere can be efficiently absorbed. In addition, heat can also be efficiently absorbed by thermal conduction due to contact with the heated atmospheric gas. As a result, it becomes possible to quickly heat the entire surface treatment film. The constituent elements of the surface treatment film 13 will be described in detail below.
[0024] [Compound A] The carbon concentration of compound A contained in the surface treatment film 13 is 80% by mass or more. If the carbon concentration of compound A is less than 80% by mass, when the HS aluminum-plated steel sheet is heated in the hot stamping process, compound A may be decomposed and oxidized even at a relatively low temperature, and compound A may disappear from the film. If compound A disappears from the film, the effect of improving the temperature rise characteristic cannot be maintained up to a high temperature. Therefore, the carbon concentration of compound A is set to 80% by mass or more. Preferably, the carbon concentration of compound A is 82% by mass or more, and preferably 85% by mass or more. The carbon concentration of compound A may be 100% by mass. Examples of compound A include carbon black (CB), graphite, and soot.
[0025] The carbon concentration of compound A can be measured by cross-sectional analysis of the surface treatment film using a transmission electron microscope (TEM), energy dispersive X-ray spectroscopy (EDS), and electron beam diffraction. Specifically, the spectrum of characteristic X-rays when irradiated with an electron beam is measured, the detection intensity for each energy is calculated, and the elements constituting the compound to be measured can be identified from the energy value. Then, using a calibration curve that has been created in advance from the relationship between a substance with a known element concentration and the corresponding detection intensity data, the concentration of each element in the compound to be measured is calculated from the detection intensity of each element constituting the compound. Measurements are performed at 10 locations within the same compound, and if all elements have a maximum concentration within the range of 1.0 to 1.3 times the minimum value, the compound is considered to be the same. In other words, measurements are performed at 10 locations in one compound observed by TEM-EDS, and if the maximum concentration value of all elements constituting the compound is within the range of 1.0 to 1.3 times the minimum value, the compound is considered to be the same. The TEM observation sample is prepared by the FIB sampling method using a focused ion beam (FIB) processing and observation device (e.g., "NB5000" manufactured by Hitachi High-Technologies Corporation). The accelerating voltage during processing is 40 kV.
[0026] The carbon concentration of compound A is defined as follows. In a cross-sectional analysis of a surface treatment film, the carbon concentration of compound A is determined as the median value between the maximum and minimum carbon concentrations measured at 10 points in the same compound within a range surrounded by the film thickness and a length of 5 μm in the direction perpendicular to the film thickness. If multiple compounds A exist within the above range, the median value is calculated for each compound A, and the average value of the median values obtained is determined as the carbon concentration of compound A. In this manner, the concentration of elements such as carbon that constitute compound A can be analyzed. Compound A, which is mainly composed of carbon, and compound B, which is an oxide or fluoride of metal element M, can be distinguished by the difference in carbon concentration.
[0027] Furthermore, in this embodiment, the content of compound A having a carbon concentration of 80 mass % or more is preferably 10 to 90% or 20 to 90%, and more preferably 30 to 80%, at a position 0.90H from the surface of the surface treatment coating (hereinafter also referred to as the "interface side position P." This interface side position P can be said to be a position 0.10H from the interface between the surface treatment coating and the Al plating layer), where H (μm) is the average thickness of the surface treatment coating.
[0028] Compound A having a carbon concentration of 80% by mass or more has a large effect of absorbing radiant heat. In addition, since such compound A has a high carbon concentration, it is unlikely to be decomposed by heating or disappear from the surface treatment film due to volatilization. Therefore, even if the temperature of the outermost surface of the HS aluminum-plated steel sheet rises due to heating in hot stamping, the absorption of radiant heat can be increased up to a high temperature range. In order to obtain such an effect, it is effective to increase the content of compound A. In this embodiment, the content of compound A at the interface side position P is preferably 10% or more or 20% or more, more preferably 30% or more, so that the temperature rise rate during hot stamp heating can be further improved. On the other hand, compound A itself in the surface treatment film does not have the effect of increasing the film adhesion. Therefore, it is preferable to suppress the content of compound A at the interface side position P, which is the Al plating layer side, in the surface treatment film, to a predetermined amount or less. Specifically, the content of compound A at the interface side position P is preferably 90% or less, more preferably 80% or less, so that the adhesion between the surface treatment film and the Al plating layer is improved. The mechanism by which the content of compound A at interface position P is improved by preferably setting it to 90% or less, and more preferably 80% or less, is thought to be that chemical and physical bonds between the highly polar rutile compound and binder resin contained in the surface treatment film and the aluminum plating layer can be secured, resulting in an effect of improving the film adhesion.
[0029] The content of compound A at position P on the interface side is determined by the following method. First, compound A having a carbon concentration of 80% or more is detected by EDS at interface position P through TEM observation. For example, when the average thickness H of the surface treatment film is 5 μm, the "0.90H position" is a position 4.5 μm deep (thickness) from the surface of the surface treatment film (i.e., a position 0.5 μm deep (thickness) from the interface between the surface treatment film and the Al plating layer toward the film side). Next, in the TEM image of the sample described below, when 10 points are observed at 30 nm intervals in a direction perpendicular to the thickness direction of the surface treatment film layer (parallel to the interface between the aluminum plating layer and the surface treatment film, perpendicular to the thickness direction of the sample), if the presence of the compound A is observed at three points, the content of compound A at the interface side position P is defined as 30%. Similarly, if the presence of the compound A is observed at four points, the content of compound A is defined as 40%, and so on. Therefore, if compound A with a carbon concentration of 80% or more is observed at three or more and eight or less points, it means that the content of compound A is 30 to 80%. The TEM observation sample used in calculating the content of compound A is prepared by the FIB sampling method using a focused ion beam (FIB) processing and observation device (e.g., "NB5000" manufactured by Hitachi High-Tech Corporation). The acceleration voltage during processing is 40 kV. The thickness of the sample is 100 nm ± 10 nm. As described above, the content of compound A is a percentage (%) calculated from the ratio (= number of points where compound A is present / 10) of the number of points where compound A is observed (present) among 10 points in a specific direction (parallel to the surface of the surface treatment film and perpendicular to the thickness direction of the sample) in a TEM image of a sample with a thickness of 100±10 nm. Therefore, the unit of content is neither volume % nor area %, but dimensionless %.
[0030] [Compound B] Compound B is an oxide or fluoride of metal element M and has a rutile structure. Examples of metal element M include Ti, V, Mn, Ru, Cs, Ir, Ge, Cu, Ag, and Ni. If necessary, only one or more of the above elements may be the metal element M. Examples of such compound B include TiO2, VO2, β-MnO2, RuO2, CsO2, IrO2, GeO2, CuO2, AgO2, and NiF2. If necessary, only one or more of the above compounds may be the compound B.
[0031] The temperature rise rate during hot stamping can be increased by including compound B having a rutile compound structure in the coating. The reason for this is not clear, but is presumed to be as follows. The rutile structure is a structure in which anions have a distorted hexagonal close packing, and cations are arranged in the 6-coordinated spaces (6-coordinated gaps). When compound B having such a rutile structure is contained in a coating, it is presumed that the heating rate during hot stamping can be increased because the ionic distance becomes such that radiation from infrared or near-infrared electromagnetic waves, which is the main heating factor during hot stamping, is active. The crystal structure of compound B and the type of compound (whether it is an oxide or a fluoride) can be determined by cross-sectional analysis of the surface treatment film using TEM, EDS, and electron diffraction. Specifically, the electron diffraction image obtained when irradiated with an electron beam is compared with a pre-existing database. If the compound is classified as a rutile structure, it can be determined that the compound has a rutile structure. In addition, the compound can be identified from the ratio of element concentrations using EDS, and if the ratio of oxygen or fluorine is 10 mass% or more, it can be determined that the compound is an oxide or a fluoride.
[0032] In this embodiment, the concentration of the metal element M in the compound B satisfies the following formula (1) and the following formula (2).
[0033] 1≦C bM ≦40...Equation (1) 1.5≦C bM / C tM ≦10.0...Equation (2) Here, when the average thickness of the surface treatment film is H (μm), C in the above formula (2) tM is the concentration (mass%) of the metal element M at a position 0.05H from the surface of the surface treatment film 13, and C in the above formula (1) and the above formula (2) is bM is the concentration (mass %) of the metal element M at a position 0.95H from the surface of the surface treatment film 13.
[0034] As shown in FIG. 1, when the thickness of the surface treatment film 13 is H (μm), the concentration C of the metal element M at 0.95H from the surface of the surface treatment film 13 is bM is, in mass%, 1% or more and 40% or less. C bM If C is less than 1%, it becomes difficult to improve the temperature rise characteristics, especially in the high temperature range, during heating in hot stamping. bM must be 1% or more. bM is preferably 5% or more, more preferably 8% or more. bM By making C 8% or more, the temperature rise rate during hot stamping can be further increased. bM When the concentration of the compound B exceeds 40%, the rate of temperature rise during heating in hot stamping becomes saturated, while the adhesion between the surface treatment film 13 and the Al plating layer 12 decreases. This is because the compound B is relatively hard, and the concentration C bM This is because, when C increases, the ability of the surface treatment film 13 to conform to the fine irregularities on the surface of the Al plating layer 12 decreases. bM This allows the temperature rise rate during hot stamping to be increased and also improves the coating adhesion. bM is preferably 35% or less, more preferably 30% or less, and further preferably 20% or less. bM By making the content of the aluminum plating layer 12 equal to or less than 20%, the adhesion of the surface treatment film 13 to the aluminum plating layer 12 can be further improved.
[0035] In addition, as shown in the above formula (2), C bM / C tM is 1.5 to 10.0. The concentration of the metal element M is high near the interface between the Al plating layer 12 and the surface treatment film 13, and C bM / C tM When the ratio is 1.5 or more, the metallic luster on the surface of the Al plating layer 12 can be concealed and the reflection of radiant heat can be suppressed. bM / C tM is preferably 2.0 or more, more preferably 3.0 or more. bM / C tM If C exceeds 10.0, the heat absorption on the surface side of the surface treatment film 13 is insufficient, and as a result, the temperature rise rate during hot stamping cannot be increased. bM / C tM is set to 10.0 or less. This allows the reflection of radiant heat on the surface of the Al plating layer 12 and the heat absorption state on the surface side of the surface treatment film 13 to be appropriately controlled, thereby increasing the temperature rise rate. bM / C tM is preferably 8.0 or less, and more preferably 6.0 or less.
[0036] Concentration (mass%) of metal element M at 0.05H from the surface of the surface treatment film 13 tM , and the concentration C of the metal element M at 0.95H from the surface of the surface treatment film 13 bM As shown in FIG. 1, when the thickness of the surface treatment film 13 is H (μm), it can be measured by fluorescent X-ray analysis and glow discharge optical emission spectroscopy (GDS). Below, C bM and C tM We will now explain in detail how to calculate this.
[0037] First, the average concentration (mass %) of the metal element M is determined as follows. Using aluminum-plated steel sheets with surface treatment films containing compound A and compound B (oxide or fluoride of metal element M), the detection intensity of metal element M (kcps, 10 3The adhesion amount (g / m2) of the metal element M in the surface treatment film is measured in advance using fluorescent X-rays in accordance with JIS K 0119 (2008). 2 A calibration curve of the detection intensity (kcps) of the metal element M is prepared in advance. Using this calibration curve, the amount of metal element M attached in the surface treatment film, P (g / m), was calculated from the detection intensity (kcps) of metal element M obtained by X-ray fluorescence analysis. 2 ) is obtained. When determining the detection intensity of the metal element M in the surface treatment film by fluorescent X-ray analysis, the concentration of the metal element M in the base steel does not have an effect, i.e., it can be ignored. In other words, since fluorescent X-rays are significantly attenuated by the metal elements in the aluminum plating layer and the surface treatment film, elements in the base steel at positions deeper than the aluminum plating layer and the surface treatment film can be considered not to have an effect on the detection intensity of the metal element M in the surface treatment film.
[0038] Next, the metal element M is measured in the depth direction of the surface treatment film 13 by GDS, and the location where the strength of the metal element M is less than half on the base steel sheet side from the depth (thickness) position showing the maximum strength is defined as the interface between the surface treatment film and the Al plating layer, and the thickness of the surface treatment film 13 is obtained. This thickness is measured at five locations, and the average value of the thicknesses obtained is defined as the thickness H (μm) of the surface treatment film 13. The adhesion amount P of the metal element M is divided by H and multiplied by 100 to obtain "P×100 / H", which is regarded as the average concentration (mass %) of the metal element M in the surface treatment film in the entire depth direction.
[0039] Meanwhile, the concentration of the metal element M at any position in the depth direction of the surface treatment film can be determined by utilizing the fact that the relationship between the average value of the intensity of the metal element M from the surface of the surface treatment film to the interface with the Al plating layer measured by GDS and the above average concentration P×100 / H is proportional to one to one. That is, the average concentration (mass%) of the metal element M in the entire film thickness, P×100 / H, and the average value α of the intensity of the metal element M from the surface to the interface with the Al plating layer can each be determined. In contrast, if the intensity (kcps) of metal element M at any position X in the depth direction is β, the concentration C of metal element M at that position X is XM (mass %) can be calculated using the proportional relationship according to the following formula (3).
[0040] C XM = P / H × 100 × (β / α) (3) The average concentration (mass%) of metal element M in 0.05H obtained using this formula (3) is C tM The concentration (mass%) of metal element M at a position 0.95H from the surface is C bM Let us assume that.
[0041] In this embodiment, compound B is preferably rutile-type TiO2. When compound B is rutile-type TiO2, the temperature rise rate during hot stamping can be further increased. The reason for this is unclear, but is presumed to be as follows. Compared to compounds such as Al2O3 that are normally formed on the surface of the aluminum plating layer during the heating process of hot stamping, rutile TiO2 can maintain a high emissivity even in the high temperature range of 300°C to 900°C. Therefore, it is presumed that the amount of heat input by radiation can be increased. Furthermore, when the temperature is raised to a higher temperature range, a composite oxide of rutile TiO2 and Al2O3 may be formed. The emissivity of this composite oxide of rutile TiO2 and Al2O3 is also higher than that of other oxides, and it is presumed that this is also a factor that can further increase the heating rate during hot stamping.
[0042] Compound B is an oxide or fluoride of metal element M, but compound B may be composed of two or more compounds. For example, the surface treatment film may contain TiO2 and VO2 as compound B. When the surface treatment film contains two or more compounds as compound B, it is sufficient that the compound with the highest content has the desired concentration and distribution that satisfies the above (1) and (2).
[0043] In addition, when a laminated film is formed by separately preparing a treatment liquid containing compound A, a treatment liquid containing compound B, which is an oxide or fluoride of metal element M and has a rutile structure, and a treatment liquid containing an organic or inorganic substance such as a resin serving as a binder component, and separately applying these treatment liquids onto an aluminum plating layer, compound B does not exist in the predetermined concentration distribution as described above. In addition, when attempting to form a multi-layered surface treatment film using multiple treatment liquids in this way, the second layer must be formed after the first layer is formed, which increases the size of the manufacturing equipment and increases the manufacturing cost. Therefore, the surface treatment film 13 of this embodiment needs to have a single layer structure, not a multi-layer structure.
[0044] The aluminum-plated steel sheet 10 for hot stamping according to this embodiment is provided with the surface treatment film 13 having the above-mentioned characteristics, and thus can improve the temperature rise rate during hot stamping. Therefore, by using the aluminum-plated steel sheet 10 for hot stamping according to this embodiment as a material, the productivity of hot stamped materials can be improved.
[0045] Although it is not clear why the provision of the surface treatment film 13 according to this embodiment enables the heating rate of the steel sheet to be improved during hot stamping, one possible reason for this is the presence of a large number of bonds that are active against infrared rays with wavelengths of 1 to 10 μm, which are particularly effective in absorbing radiant heat.
[0046] In addition to the above-mentioned compound A and compound B, the surface treatment film 13 according to this embodiment may contain various resins and additives as binder components. By containing a resin, the adhesion between the surface treatment film 13 and the Al plating layer 12 can be improved. Examples of additives contained in the surface treatment film 13 include a leveling agent, an antifoaming agent, a colorant, a viscosity adjuster, and an ultraviolet absorbing agent. The coating liquid for forming the surface treatment film 13 is preferably obtained by dispersing or dissolving each of the above-mentioned components in water or a solvent.
[0047] In this embodiment, specific methods for applying the surface treatment film 13 include, but are not limited to, coating and lamination. The surface treatment film 13 may be applied to only one side of the aluminum-plated steel sheet, or may be applied to both sides of the aluminum-plated steel sheet.
[0048] When applying the surface treatment film 13 to the entire surface of the aluminum plating layer 12 by coating, a treatment liquid is first prepared, which contains, for example, compound A having a carbon concentration of 80% by weight or more and compound B which is an oxide or fluoride of metal element M and has a rutile structure. The treatment liquid is then applied to the entire surface of the aluminum plating layer 12 by a roll coater, curtain coater, inkjet, or the like, and the volatile components in the treatment liquid are then dried to apply the surface treatment film 13. Coating by inkjet is particularly preferred because the film thickness can be changed continuously.
[0049] Here, in the past (for example, Patent Document 2, etc.), when a surface treatment film contains organic matter such as a carbon pigment, when the plated steel sheet is heated to a high temperature range (for example, 750°C or higher), all of the organic matter disappears, resulting in a problem of deterioration in the temperature rise characteristics (temperature rise rate). However, the present inventors have found that in the case of the surface treatment film 13 according to this embodiment, it is possible to efficiently heat to a high temperature range even if the organic matter disappears. Although the mechanism by which it is possible to heat to a high temperature range even if the organic matter disappears in this way is not clear, it is presumed that the compound B (oxide or fluoride of metal element M) contained in the film increases the heat input by radiation at high temperatures.
[0050] [Binder component (resin)] The content of the binder component (resin) that can be contained in the surface treatment film 13 according to this embodiment is preferably 40 volume % or more relative to the total volume of the surface treatment film 13. As the binder component, various known resins can be used.
[0051] The resin as the binder component is not particularly limited. For example, polyurethane resin, polyester resin, acrylic resin, epoxy resin, fluororesin, polyamide resin, polyolefin resin, and polymer compounds obtained by hydrolysis and condensation polymerization of silane coupling agents can be mentioned. Examples of the resin include resins crosslinked with butylated melamine resin, methylated melamine resin, butylmethyl mixed melamine resin, urea resin, isocyanate resin, or a crosslinking agent component of a mixed system thereof. In addition, electron beam curable resins and ultraviolet ray curable resins can also be mentioned. Among these, the resin as the binder component is preferably one or more of polyester resin, epoxy resin, acrylic resin, and polyurethane resin. These resins as the binder component may be used alone or in a mixture of two or more.
[0052] When a polyurethane resin is used as the binder component, for example, the polyurethane resin is preferably a polyether polyurethane resin, because the use of a polyether polyurethane resin can prevent the occurrence of hydrolysis caused by acid or alkali, compared with a polyester polyurethane resin, and because the use of a polyether polyurethane resin can suppress the formation of a hard and brittle film, compared with a polycarbonate polyurethane resin, thereby ensuring adhesion during processing and corrosion resistance of the processed part.
[0053] Whether or not polyurethane resin is contained can be determined by detecting the 3330 cm -1 (NH telescopic), 1730cm -1 (C=O expansion and contraction), 1530cm -1 (CN), 1250cm -1 It can be judged based on whether the characteristic absorption of (CO) is observed. In addition, the polyurethane resin content can also be determined from the obtained characteristic absorption intensity by creating a calibration curve showing the relationship between the content and the characteristic absorption intensity using a sample with a known content.
[0054] In addition, for resins other than the above polyurethane resins, it is possible to determine the presence or absence and the amount of the resin in the same manner as for the above polyurethane resins by focusing on the characteristic absorption derived from the functional group specific to each resin. Water or a solvent can be used as a component in the treatment liquid for dispersing or dissolving the resin.
[0055] [Additives] The surface treatment film 13 according to this embodiment can contain various additives, such as a leveling agent, a water-soluble solvent, a metal stabilizer, an etching inhibitor, etc., as additives used in preparing the treatment liquid prior to film formation, within a range that does not impair the effects of the present invention.
[0056] The leveling agent may be a nonionic or cationic surfactant, such as a polyethylene oxide or polypropylene oxide adduct, or an acetylene glycol compound.
[0057] Examples of the water-soluble solvent include alcohols such as ethanol, isopropyl alcohol, t-butyl alcohol, and propylene glycol; cellosolves such as ethylene glycol monobutyl ether and ethylene glycol monoethyl ether; esters such as ethyl acetate and butyl acetate; and ketones such as acetone, methyl ethyl ketone, and methyl isobutyl ketone.
[0058] Examples of metal stabilizers include chelating compounds such as EDTA (ethylenediaminetetraacetic acid) and DTPA (diethylenetriaminepentaacetic acid).
[0059] Etch inhibitors include, for example, amine compounds such as ethylenediamine, triethylenepentamine, guanidine, and pyrimidine.
[0060] The contents of the binder components and additives can be measured in the same manner as in the case of the compounds A and B.
[0061] [silica] The surface treatment film 13 according to this embodiment may contain silica. When silica is contained, the content of silica is 0.01 to 0.3 g / m 2 Silica is preferably 0.01 g / m 2 With a silica content of 0.3 g / m or more, it is possible to prevent scratches on the coating due to contact with other steel sheets or equipment. 2 If the content exceeds 0.3 g / m, the temperature increase effect cannot be expected, while the cost is high, which is undesirable from an economic standpoint. In addition, since silica is a substance with low electrical conductivity, it is not preferable to add silica at a content of more than 0.3 g / m. 2 If the silica content exceeds 0.10 g / m, this is not preferable in terms of weldability after hot stamping. When silica is contained, the smaller the silica content in the surface treatment film 13, the better. The silica content of the surface treatment film is more preferably 0.10 g / m 2 More preferably, it is 0.05 g / m or less. 2 The following is the result.
[0062] [Thickness of surface treatment film] The average film thickness H of the surface treatment film 13 containing the above components is preferably, for example, 0.5 to 15.0 μm. When the average thickness of the surface treatment film 13 is less than 0.5 μm, the absorption of radiant heat is insufficient, and therefore the temperature rise rate during hot stamping cannot be sufficiently increased. On the other hand, when the average thickness of the surface treatment film 13 exceeds 15.0 μm, the heat capacity of the surface treatment film 13 itself becomes large, and becomes a barrier to the transfer of heat to the aluminum plating layer 12. As a result, the temperature rise rate cannot be sufficiently increased, and the cost increases, which is not preferable from the viewpoint of economy. The temperature rise rate can be increased by setting the average thickness of the surface treatment film 13 in the range of 0.5 to 15.0 μm. The average thickness of the surface treatment film 13 is more preferably 1.0 to 7.0 μm.
[0063] <Surface treatment film> As shown in Fig. 2, a base treatment film (chemical conversion layer) 14 may be provided between the surface treatment film 13 and the aluminum plating layer 12 in order to improve the adhesion of the surface treatment film 13. Note that Fig. 2 is a schematic diagram for explanation, and the dimensions of the surface treatment film 13, the aluminum plating layer 12, the base treatment film 14, etc. do not necessarily represent a preferred embodiment, and are not limited to the dimensions in Fig. 2.
[0064] The base treatment film 14 may contain one or more selected from resin, silane coupling agent, zirconium compound, silica, phosphoric acid and its salt, fluoride, and vanadium compound. The inclusion of these substances further improves the film-forming properties after application of the chemical conversion treatment agent, the barrier properties (density) of the film against corrosive factors such as moisture and corrosive ions, and the adhesion of the film to the plating surface, thereby contributing to raising the corrosion resistance of the film. In particular, when the chemical conversion treatment layer contains one or more of a silane coupling agent and a zirconium compound, a cross-linked structure is formed in the film, and the bond with the plating surface is also strengthened, thereby improving the adhesion and barrier properties of the film. Furthermore, when the base treatment film 14 contains one or more of silica, phosphoric acid and its salts, fluorides, and vanadium compounds, these act as inhibitors to form a precipitate film or a passivation film on the plating surface or the surface of the base steel sheet, thereby improving corrosion resistance.
[0065] [Adhesion amount of base treatment film 14] The amount of the base treatment film 14 on one side of the plating layer is 10 to 1000 mg / m in terms of solid content. 2 The coating weight of the base coating 14 is preferably 10 mg / m 2 If the coating weight is less than 1000 mg / m, sufficient adhesion and corrosion resistance cannot be ensured. 2 If it exceeds this value, the adhesion during processing may decrease. The amount of the base treatment film 14 on one side of the plating layer is more preferably 20 to 800 mg / m 2 , and more preferably 50 to 600 mg / m 2 It is.
[0066] <Aluminum plating layer> The aluminum-plated steel sheet 10 for hot stamping according to this embodiment preferably has an aluminum plating layer 12 on at least one surface of the base steel sheet 11. By having the aluminum plating layer 12, it is possible to further improve the corrosion resistance after painting after hot stamping. In addition, by having the aluminum plating layer 12 between the base steel sheet 11 and the surface treatment film 13, it is possible to prevent iron scale from being generated by heating during hot stamping. Iron scale contaminates the heating furnace and adheres to rolls used for transportation, which is a burden in manufacturing. Therefore, when iron scale is generated, a process such as shot blasting is required to remove the iron scale, which is not economically preferable.
[0067] The type of the aluminum plating layer is not particularly limited, and the composition constituting the aluminum plating layer includes aluminum plating, Al-Si plating, Al-Si-Mg, Al-Si-Ca plating, etc. For example, the aluminum plating layer may have a chemical composition (average chemical composition) containing, in mass%, Al: 80.0 to 95.0%, Si: 2.0 to 15.0%, Fe: 1 to 15.0%, Cr: 0% or more and less than 1.0%, Mo: 0% or more and less than 1.0%, Zn: 0% or more and less than 1.0%, V: 0% or more and less than 1.0%, Ti: 0% or more and less than 1.0%, Sn: 0% or more and less than 1.0%, Ni: 0% or more and less than 1.0%, Cu: 0% or more and less than 1.0%, W: 0% or more and less than 1.0%, Bi: 0% or more and less than 1.0%, Mg: 0% or more and less than 1.0%, Ca: 0% or more and less than 1.0%, and the remainder being impurities.
[0068] If the Al content in the aluminum plating layer is less than 80.0%, the corrosion resistance after hot stamping (corrosion resistance in the hot stamped body) deteriorates. Therefore, the Al content is preferably 85.0% or more. The Al content is more preferably 88.0% or more. On the other hand, if the Al content in the aluminum plating layer exceeds 95.0%, the plating adhesion may deteriorate. Therefore, the Al content is preferably 95.0% or less. The Al content is more preferably 92.0% or less.
[0069] If the Si content in the aluminum plating layer is less than 2.0%, the plating adhesion may deteriorate. Therefore, the Si content is preferably 2.0% or more. The Si content is more preferably 3.0% or more, and further preferably 4.0% or more. On the other hand, if the Si content in the aluminum plating layer is more than 15.0%, the plating adhesion may deteriorate. Therefore, the Si content is preferably 15.0% or less. The Si content is more preferably 13.0% or less.
[0070] The Fe content is preferably 1.0% or more and 15.0% or less.
[0071] The chemical composition of the aluminum plating layer can be measured by X-ray fluorescence spectrometry in accordance with JIS GK 0119:2008. In other words, the relationship between X-ray intensity and content is determined in advance using a sample with a known content of the target element. From the calibration curve created based on this, the content of each element in the unknown sample, i.e., the chemical composition, can be determined.
[0072] [Amount of aluminum plating layer] The aluminum plating layer 12 is applied to one or both sides of the base steel sheet 11. The coating weight is 5 g / m 2 ~140g / m 2 It is preferable that: Adhesion weight per side is 5g / m 2If the adhesion amount is less than 140 g / m2, iron scale will form on the surface of the base steel sheet during the heating process of hot stamping, and a process to remove the scale will be required. 2 If the coating weight of the aluminum plating layer 12 is more than 5 g / m per side, it is not preferable from the viewpoint of productivity because it takes time to proceed with the alloying reaction between Al and Fe in the hot stamp heating step, which is necessary to improve the corrosion resistance after painting. 2 ~140g / m 2 is preferred.
[0073] <Base material steel plate> Next, the base steel sheet 11 of the aluminum-plated steel sheet 10 for hot stamping according to this embodiment will be described. There are no particular limitations on the base steel sheet 11 as long as it is a steel sheet that can be suitably used in the hot stamping method. The chemical composition of the base steel sheet 11 applicable to the aluminum-plated steel sheet 10 for hot stamping according to this embodiment is, for example, in mass %, as follows: C: 0.03-0.60%, Si: 0.01 to 0.60%, Mn: 0.50-3.00%, P: 0.050% or less, S: 0.020% or less, Al: 0.100% or less, Ti: 0.01 to 0.10%, B: 0.0001~0.0100%, N: 0.010% or less, Cr: 0-1.00%, Ni: 0-2.00%, Cu: 0-1.000%, Mo: 0-1.00%, V: 0~1.00%, Nb: 0-1.00%, Sn: 0-1.00%, W: 0 to 1.00%, Ca: 0 to 0.010%, REM: 0-0.30% The balance may be Fe and impurities. Moreover, examples of the form of the base steel sheet 11 include a steel sheet such as a hot-rolled steel sheet or a cold-rolled steel sheet. Hereinafter, the preferred range of each element in the base steel sheet 11 of the aluminum-plated steel sheet 10 for hot stamping and the reasons therefor will be described in detail. In the following description of the chemical composition of the base steel sheet 11, the designation "%" means "mass %" unless otherwise specified.
[0074] [C:0.03~0.60%] C is contained to ensure the desired mechanical strength. When the C content is 0.03% or more, a sufficient improvement in mechanical strength is obtained, and the effect of containing C is fully obtained. Therefore, the C content is preferably 0.03% or more. The C content is more preferably 0.20% or more. On the other hand, when the C content is 0.60% or less, the strength of the steel sheet can be hardened and improved while the decrease in elongation and reduction of area can be suppressed. Therefore, the C content is preferably 0.60% or less. The C content is more preferably 0.40% or less.
[0075] [Si: 0.01~0.60%] Si is one of the strength-improving elements that improve mechanical strength, and is contained in order to secure the desired mechanical strength, similar to C. When the Si content is 0.01% or more, the strength-improving effect is fully exerted, and sufficient improvement in mechanical strength is obtained. Therefore, the Si content is preferably 0.01% or more. The Si content is more preferably 0.10% or more. On the other hand, since Si is also an easily oxidizable element, when the Si content is 0.60% or less, the decrease in wettability during hot-dip Al plating due to the influence of Si oxide formed on the steel sheet surface layer is suppressed, and the occurrence of bare spots can be suppressed. Therefore, the Si content is preferably 0.60% or less. The Si content is more preferably 0.40% or less.
[0076] [Mn: 0.50~3.00%] Mn is one of the strengthening elements that strengthen steel, and is also one of the elements that enhance hardenability. Furthermore, Mn is an element that is effective in preventing hot embrittlement caused by S, which is one of the impurities. When the Mn content is 0.50% or more, these effects can be sufficiently obtained. Therefore, in order to reliably exhibit the above effects, the Mn content is preferably 0.50% or more. The Mn content is more preferably 0.80% or more. On the other hand, since Mn is an austenite forming element, when the Mn content is 3.00% or less, the amount of retained austenite phase does not become too large, and a decrease in strength is suppressed. Therefore, the Mn content is preferably 3.00% or less. The Mn content is more preferably 1.50% or less.
[0077] [P:0.050% or less] P is an impurity contained in steel. By making the P content 0.050% or less, it is possible to suppress the P contained in the steel sheet from segregating to the grain boundaries of the steel sheet and reducing the toughness of the base material of the hot stamped body, and to suppress the reduction in the delayed fracture resistance of the steel sheet. Therefore, the P content is preferably 0.050% or less, and it is preferable to make the P content as small as possible. If necessary, the P content may be 0.045% or less or 0.040% or less. The lower limit of the P content is 0%, but the lower limit may be 0.001% or 0.005%.
[0078] [S:0.020% or less] S is an impurity contained in steel. By making the S content 0.020% or less, it is possible to suppress the S contained in the steel sheet from forming sulfides that reduce the toughness of the steel sheet, and to suppress the reduction in the delayed fracture resistance of the steel sheet. Therefore, the S content is preferably 0.020% or less, and it is preferable to make the S content as small as possible. If necessary, the S content may be made 0.015% or less or 0.010% or less. The lower limit of the S content is 0%, but the lower limit may be made 0.001% or 0.002%.
[0079] [Al:0.100% or less] Al is generally used for the purpose of deoxidizing steel. On the other hand, by making the Al content 0.100% or less, the increase in Ac3 point of the steel sheet is suppressed, so that the heating temperature required to ensure the hardenability of the steel during hot stamping can be reduced, which is desirable for hot stamping production. Therefore, the Al content of the steel sheet is preferably 0.100% or less, more preferably 0.050% or less, and further preferably 0.030% or less. The lower limit of the Al content is 0%, but the lower limit may be 0.001%, 0.003%, or 0.007%.
[0080] [Ti: 0.01~0.10%] Ti is one of the strength enhancing elements. When the Ti content is 0.01% or more, the strength improving effect and the oxidation resistance improving effect can be sufficiently obtained. Therefore, in order to reliably realize the above effects, the Ti content is preferably 0.01% or more. The Ti content is more preferably 0.03% or more. On the other hand, when the Ti content is 0.10% or less, for example, the formation of carbides and nitrides is suppressed, the softening of the steel can be suppressed, and the desired mechanical strength can be sufficiently obtained. Therefore, the Ti content is preferably 0.10% or less. The Ti content is more preferably 0.08% or less.
[0081] [B:0.0001~0.0100%] B acts during quenching to improve strength. When the B content is 0.0001% or less, such a strength improving effect can be sufficiently obtained. Therefore, the B content is preferably 0.0001% or more. The B content is more preferably 0.0010% or more. On the other hand, when the B content is 0.0100% or less, the formation of inclusions is reduced, embrittlement of the steel sheet is suppressed, and a decrease in fatigue strength can be suppressed. Therefore, the B content is preferably 0.0100% or less. The B content is more preferably 0.0040% or less.
[0082] [N:0.010% or less] N is an impurity contained in steel. By making the N content 0.010% or less, the formation of nitrides due to N contained in the steel plate is suppressed, and the deterioration of the toughness of the steel plate can be suppressed. Furthermore, when B is contained in the steel plate, the N contained in the steel plate is suppressed from combining with B to reduce the amount of solid-solubilized B, and the deterioration of the hardenability improving effect of B can be suppressed. Therefore, the N content is preferably 0.010% or less, and it is more preferable to make the N content as small as possible.
[0083] The base steel sheet of the hot stamping steel sheet according to this embodiment may further contain, as an optional element, one or more elements selected from the group consisting of Cr, Mo, Ni, Cu, V, Nb, Sn, W, Ca and REM. The lower limit of the content of these elements is 0%.
[0084] [Cr:0~1.00%] Cr is an element that improves the hardenability of steel sheet. In order to fully obtain this effect, the Cr content is preferably 0.01% or more. On the other hand, by setting the Cr content to 1.00% or less, the effect can be fully obtained while suppressing an increase in costs. Therefore, when Cr is contained, the Cr content is preferably 1.00% or less. If necessary, the Cr content may be 0.70% or less or 0.50% or less.
[0085] [Ni:0~2.00%] Ni is an element that enhances the hardenability of steel and enables the strength of the steel plate member after hardening to be stably ensured. In order to fully exert such effects, it is preferable that the Ni content is 0.10% or more. On the other hand, by making the Ni content 2.00% or less, the above effects can be sufficiently obtained while improving economic efficiency. Therefore, when Ni is contained, the Ni content is preferably 2.00% or less. If necessary, the Ni content may be 1.20% or less, 0.80% or less, or 0.50% or less.
[0086] [Cu:0~1.000%] Cu is an element that enhances the hardenability of steel and enables the strength of the steel plate member after hardening to be stably secured. Cu also improves pitting corrosion resistance in a corrosive environment. In order to fully exert such effects, it is preferable that the Cu content is 0.100% or more. On the other hand, by making the Cu content 1.000% or less, the above effects can be sufficiently obtained while improving economic efficiency. Therefore, when Cu is contained, it is preferable that the Cu content is 1.000% or less. If necessary, the Cu content may be 0.600% or less, 0.400% or less, or 0.200% or less.
[0087] [Mo:0~1.00%] Mo is an element that enhances the hardenability of steel and enables the strength of the steel plate member after hardening to be stably ensured. In order to fully exert such effects, the Mo content is preferably 0.10% or more. On the other hand, by making the Mo content 1.00% or less, the above effects can be sufficiently obtained while improving economic efficiency. Therefore, when Mo is contained, the Mo content is preferably 1.00% or less. If necessary, the Mo content may be 0.60% or less, 0.40% or less, or 0.20% or less.
[0088] [V:0~1.00%] V is an element that enhances the hardenability of steel and enables the strength of the steel plate member after hardening to be stably ensured. In order to fully exert this effect, it is preferable that the V content is 0.10% or more. On the other hand, by making the V content 1.00% or less, the above-mentioned effect can be sufficiently obtained while improving economic efficiency. Therefore, when V is contained, the V content is preferably 1.00% or less. If necessary, the V content may be 0.60% or less, 0.40% or less, or 0.20% or less.
[0089] [Nb: 0-1.00%] Nb is an element that enhances the hardenability of steel and enables the strength of the steel plate member after hardening to be stably ensured. In order to fully exert such effects, the Nb content is preferably 0.01% or more. On the other hand, by making the Nb content 1.00% or less, the above effects can be fully obtained while improving economic efficiency. Therefore, when Nb is contained, the Nb content is preferably 1.00% or less. If necessary, the Nb content may be 0.50% or less, 0.20% or less, or 0.10% or less.
[0090] [Sn: 0~1.00%] Sn is an element that improves pitting corrosion resistance in a corrosive environment. In order to fully exert this effect, the Sn content is preferably 0.01% or more. On the other hand, by making the Sn content 1.00% or less, the decrease in grain boundary strength can be suppressed, and the decrease in toughness can be suppressed. Therefore, when Sn is contained, the Sn content is preferably 1.00% or less. If necessary, the Sn content may be 0.40% or less, 0.10% or less, or 0.05% or less.
[0091] [W:0~1.00%] W is an element that enhances the hardenability of steel and enables the strength of the steel plate member after hardening to be stably secured. W also improves pitting corrosion resistance in a corrosive environment. In order to fully exert such effects, it is preferable that the W content is 0.01% or more. On the other hand, by making the W content 1.00% or less, the above effects can be sufficiently obtained while improving economic efficiency. Therefore, when W is contained, it is preferable that the W content is 1.00% or less. If necessary, the W content may be 0.60% or less, 0.40% or less, or 0.20% or less.
[0092] [Ca: 0~0.010%] Ca is an element that has the effect of refining inclusions in steel and improving toughness and ductility after quenching. In order to fully exert such effects, the Ca content is preferably 0.001% or more, and more preferably 0.002% or more. On the other hand, by making the Ca content 0.010% or less, the effect can be sufficiently obtained while the cost can be suppressed. Therefore, when Ca is contained, the Ca content is preferably 0.010% or less, and more preferably 0.004% or less. If necessary, the Ca content may be 0.008% or less, 0.006% or less, or 0.0004% or less.
[0093] [REM:0~0.30%] REM, like Ca, is an element that has the effect of refining inclusions in steel and improving toughness and ductility after quenching. In order to fully exert such effects, the REM content is preferably 0.001% or more, and more preferably 0.002% or more. On the other hand, by making the REM content 0.30% or less, the effect can be sufficiently obtained while the cost can be suppressed. Therefore, when REM is contained, the REM content is preferably 0.30% or less, and more preferably 0.20% or less. If necessary, the Ca content may be 0.10% or less, 0.05% or less, or 0.02% or less.
[0094] Here, REM refers to Sc, Y and lanthanoids, a total of 17 elements, and the above REM content means the total content of these elements. REM is added to molten steel using, for example, an Fe-Si-REM alloy, which includes, for example, Ce, La, Nd, and Pr.
[0095] The balance other than the above components is Fe and impurities. In addition to the above components, the base steel sheet 11 may contain impurities that are mixed in during the manufacturing process, etc., as long as the effects of the present invention are not impaired. Examples of such impurities include Zn (zinc) and Co (cobalt).
[0096] The chemical composition of the base steel sheet 11 of the aluminum-plated steel sheet 10 for hot stamping described above may be measured by a general analytical method. For example, it may be measured using ICP-AES (Inductively Coupled Plasma-Atomic Emission Spectrometry). C and S may be measured using a combustion-infrared absorption method, N may be measured using an inert gas fusion-thermal conductivity method, and O may be measured using an inert gas fusion-non-dispersive infrared absorption method. When the steel sheet for hot stamping has a plating layer on its surface, the plating layer on the surface may be removed by mechanical grinding before the chemical composition is analyzed.
[0097] Of the surface of the plated steel sheet consisting of the base steel sheet 11 having the above-mentioned chemical composition and the aluminum plating layer 12, the portion to which the surface treatment film 13 is applied can be made into a hot stamped member having high tensile strength by heating and quenching using a hot stamping method. In addition, in the hot stamping method, since press working can be performed in a softened state at high temperature, it can be easily formed.
[0098] (Method of manufacturing aluminum-plated steel sheet for hot stamping) Hereinafter, an example of a method for producing the aluminum-plated steel sheet for hot stamping according to the present embodiment will be described. Note that the method for producing the aluminum-plated steel sheet for hot stamping according to the present embodiment is not particularly limited as long as the aluminum-plated steel sheet for hot stamping according to the present embodiment has the above-mentioned configuration. The following production method is one example for producing the aluminum-plated steel sheet for hot stamping according to the present embodiment, and is a suitable example of the method for producing the aluminum-plated steel sheet for hot stamping according to the present embodiment.
[0099] <Base material steel plate> The base steel sheet to be subjected to aluminum plating is not particularly limited as long as it is a steel sheet suitable for hot stamping. Examples of the form of the base steel sheet include hot-rolled steel sheets and cold-rolled steel sheets.
[0100] <Formation of aluminum plating layer> The method for forming the aluminum plating layer includes, but is not limited to, a hot-dip plating method, an electroplating method, a physical vapor deposition method, a chemical vapor deposition method, etc. The aluminum plating layer is formed on the surface of the base steel sheet by a known method.
[0101] <Method of manufacturing surface treatment film> The method for producing the surface treatment film is not particularly limited, but for example, the film-forming components are mixed, stirred with a disperser, and the mixed treatment liquid dissolved or dispersed is applied onto the plating layer, followed by drying. The mixed treatment liquid is produced, for example, by preparing a treatment liquid of compound A and a treatment liquid of compound B, respectively, adjusting the pH, and then mixing each treatment liquid with other optional components such as resin. The specific details will be explained below.
[0102] Compound A contained in the surface treatment film includes carbon black, graphite, soot, etc. In the manufacturing method of the surface treatment film, it is preferable to use a treatment liquid in which powder of these is dispersed in water or the like.
[0103] Compound A is pulverized by a machine or the like so that the powder diameter (particle size) is between 30 and 300 nm, and then compound A is put into a treatment liquid containing sodium hydroxide and adjusted to pH 9.0 to 13.0. Then, by carrying out a pretreatment in which the treatment liquid containing compound A is stirred at 50 to 80°C for 1 to 4 days, compound A with a particle size of 30 to 300 nm can be more stably dispersed in the treatment liquid. In addition, when the surface treatment film is formed, compound A can be uniformly present in the film layer, thereby improving the temperature rise characteristic.
[0104] Furthermore, the carbon concentration of compound A in the coating can be increased by heating the treatment solution with a pH of 9.0 to 13.0 containing compound A at 50 to 80°C for 1 to 4 days (i.e., by satisfying the above-mentioned pretreatment conditions). When the treatment solution is subjected to the pretreatment, areas with low carbon concentration on the outside of the particles of compound A (e.g., areas with high ratios of oxygen (O), nitrogen (N), sulfur (S), etc.) are dissolved by the treatment solution containing sodium hydroxide, leaving areas with high carbon concentration on the inside of the particles. This can also increase the carbon concentration of compound A in the coating. On the other hand, when the above pretreatment conditions are not satisfied (for example, when the stirring time is less than one day), the amount of dissolution in the area with low carbon concentration on the outside of the compound A particles decreases, and the carbon concentration of compound A in the coating decreases relatively. Therefore, in order to sufficiently increase the carbon concentration of compound A in the coating, it is necessary to control the pretreatment conditions before applying the treatment liquid.
[0105] Similarly, it is preferable to use a treatment liquid in which compound B, which is an oxide or fluoride of metal element M and has a rutile structure, is in the form of a powder or dispersed in water or a solvent.
[0106] Compound B is pulverized by a machine or the like to a powder diameter (particle size) of 10 to 300 nm, and then introduced into a treatment liquid containing sodium fluoride and adjusted to pH 3 to 7, and pre-treated by stirring at 50 to 80°C for 4 to 24 hours. This allows compound B with a particle size of 10 to 300 nm to be more stably dispersed in the treatment liquid. As a result, when a surface treatment film is formed, compound B can be present in the film in the form described below, thereby improving the temperature rise characteristic.
[0107] The surface treatment film of this embodiment can be obtained by using a mixed treatment liquid in which a binder component (resin) is appropriately added to the raw materials and treatment liquid screened in this manner.
[0108] The method for producing the mixed treatment liquid by combining the treatment liquid of compound A and the treatment liquid of compound B is not particularly limited, but for example, the treatment liquid containing compound A and the treatment liquid containing compound B obtained by the above method are mixed, stirred with a disperser to dissolve or disperse, and then a binder (resin) or silica is added as necessary. In order to improve the solubility or dispersibility of each film-forming component, a known hydrophilic solvent or the like may be added as necessary. An acid, an alkali, or the like may be added to the treatment liquid for pH adjustment within a range that does not impair its performance. The method for producing the mixed treatment liquid will now be described in detail.
[0109] In order to realize a surface treatment film that satisfies the above formulas (1) and (2), first, compound A and compound B are each dispersed in water or a mixed solution of water and a solvent such as ethanol, and each treatment liquid is prepared by the above-mentioned preparation method. Then, a binder component (such as a resin) and the treatment liquid of compound A are mixed, and then the treatment liquid of compound B is mixed to prepare a mixed treatment liquid. The treatment liquid of compound B having a pH of 3 to 7 is stirred at 30 to 50°C for 4 to 25 hours, and then the pH of the treatment liquid of compound B is adjusted to 8 or more using ammonia water or the like just before mixing with the treatment liquid of compound A. In addition, when silica is to be contained in the surface treatment film, it is preferable to add silica after mixing the treatment liquid of compound B with the mixed liquid. In order to make the content of compound A at the interface side position P of the surface treatment coating 30% or more, the concentration (content) of compound A in the mixed treatment liquid is made 15% by mass or more in terms of dry weight (mass) ratio. In order to make the content of compound A at the interface side position P of the surface treatment coating 80% or less, the concentration (content) of compound A in the mixed treatment liquid is made 50% by mass or less in terms of dry weight (mass) ratio. In order to satisfy the formulas (1) and (2) regarding the concentration of the metal element M, the concentration (content) of the compound B in the mixed treatment liquid is set to 3 to 50 mass % in terms of dry weight (mass) ratio. The total concentration (content) of compound A and compound B in the mixed treatment solution is 18 to 90% in terms of dry weight (mass) ratio. Next, the obtained mixed treatment liquid is stirred at 150 rpm to 300 rpm immediately before coating, and the mixed treatment liquid after stirring is preferably applied within 5 seconds.
[0110] In order to realize a surface treatment film that satisfies the above formulas (1) and (2), a shear rate of 10 -3 The dynamic viscosity of the mixed treatment liquid at 1000 rpm is 3 to 16 mPa·s and the surface tension is 20 to 60 mN / m. When the dynamic viscosity is less than 3 mPa s, C in formula (2) bM / C tM If the dynamic viscosity exceeds 10.0, the desired heating rate may not be obtained. Therefore, the dynamic viscosity of the mixed treatment liquid is set to 3 mPa·s or more, and preferably 6 mPa·s or more. On the other hand, if the dynamic viscosity exceeds 16 mPa·s, C in formula (2) bM / C tM If the dynamic viscosity of the mixed treatment liquid is less than 1.5, the desired heating rate may not be obtained. Therefore, the dynamic viscosity of the mixed treatment liquid is set to 16 mPa·s or less, and preferably 12 mPa·s or less.
[0111] In addition, if the surface tension of the mixed treatment liquid is less than 20 mN / m, C bM is less than 1 mass %, and the desired heating rate cannot be obtained. Therefore, the surface tension of the mixed treatment liquid is set to 20 mN / m or more, and preferably 30 mN / m or more. On the other hand, if the surface tension exceeds 60 mN / m, the desired heating rate cannot be obtained. Therefore, the surface tension of the mixed treatment liquid is set to 60 mN / m or less, and preferably 40 mN / m or less.
[0112] To form the surface treatment film layer, a treatment liquid is applied onto the aluminum plating layer (or the chemical conversion layer) and the applied film is dried by heating. The method of applying the treatment liquid is not particularly limited, and generally known application methods such as roll coating and immersion are possible.
[0113] In order to control the compound B to have a predetermined concentration distribution as represented by formulas (1) and (2), the ultimate heating and drying temperature after coating is set to 55° C. to 120° C. Here, the "ultimate temperature" refers to the temperature of the surface of the base steel sheet. If the temperature is less than 55°C, the evaporation rate of the water is slow and sufficient film formation cannot be achieved, which may result in insufficient film adhesion. Furthermore, if the temperature is too low, the evaporation rate of the treatment solution is slow, so that the metal element M in compound B is concentrated on the Al plating layer side, and bM / C tM becomes excessively high. As a result, heat absorption on the surface side of the surface treatment film 13 becomes insufficient, and there is a risk of deterioration in temperature rise characteristics during hot stamping. On the other hand, if the ultimate temperature exceeds 120°C, the binder component may be denatured due to thermal decomposition or the like, and adhesion and corrosion resistance may decrease. The ultimate temperature is more preferably 65 to 100°C.
[0114] In addition, assuming that the time taken for the temperature of the base steel sheet surface to reach 65°C from 25°C is t1 (if it does not reach 65°C, the final temperature of the base material) and the time taken for the temperature to drop from 65°C (or the final temperature of the base material) to 40°C by cooling is t2, t1 is set to 1.5 to 14.0 seconds, t2 is set to 0.5 to 8.6 seconds, and t1 / t2 is set to the range of 0.35 to 10.0. As a result, the concentration distribution C of compound B in the surface treatment film is bM / C tM This makes it easier to control the temperature, and the temperature rise rate is further improved.
[0115] Furthermore, when the time it takes for the temperature of the surface of the base steel sheet to reach 55° C. from 25° C. is t3, t3 is set to 5.0 to 12.0 seconds. This allows the content of compound A at the interface side position P to be 30 to 80%.
[0116] The method for heating and drying the treatment liquid after application is not particularly limited, and examples thereof include hot air, induction heating, near infrared rays, direct flame, etc., either alone or in combination. Water or a solvent can be used as a component in the treatment liquid for dispersing or dissolving the resin.
[0117] (Method of manufacturing hot stamped parts) Various hot stamped members, such as automotive frame parts, can be produced using an aluminum-plated steel sheet for hot stamping having the above-mentioned surface treatment film applied to the entire surface of at least one surface.
[0118] First, for example, an aluminum-plated steel sheet having a surface treatment film is subjected to various processes such as cutting or punching by a press to obtain an aluminum-plated steel sheet for hot stamping according to this embodiment. The aluminum-plated steel sheet for hot stamping according to the present embodiment can also be obtained by providing a surface treatment film on an aluminum-plated steel sheet that has been cut, punched by pressing, etc. In addition, by partially reducing the thickness of the surface treatment film, it is possible to facilitate electrical conduction and improve spot weldability, for example, in applications in which multiple steel sheets are welded together before hot stamping.
[0119] The aluminum-plated steel sheet for hot stamping to which the surface treatment film is applied as described above is hot stamped. Examples of the heating device include an electric heating furnace, a gas heating furnace, a far-infrared furnace, and a normal heating device equipped with an infrared heater. The surface on which the surface treatment film is applied to increase the emissivity has a high heating rate because of a large heat transfer effect due to radiation. Therefore, the temperature is quickly raised to a temperature equal to or higher than the Ac3 point at which the metal structure transforms into the austenite phase. As a result, in the manufacturing method for the hot stamped member according to this embodiment, the productivity of the hot stamped member can be further improved by shortening the heating time. In this embodiment, the specific heating conditions are not particularly limited, and it is sufficient to appropriately control the heating device to be used.
[0120] Next, the heated steel sheet is formed and cooled. The portion heated to or above the Ac3 point temperature at which the metal structure of the steel material transforms into the austenite phase is quenched at the same time as forming, thereby increasing the strength. This allows a hot stamped part with improved strength to be obtained. EXAMPLES
[0121] Examples of the present invention will be described below, but the conditions in the examples are merely examples of conditions adopted to confirm the feasibility and effects of the present invention, and the present invention is not limited to these examples. Various conditions may be adopted in the present invention as long as they do not deviate from the gist of the present invention and achieve the object of the present invention.
[0122] It is preferable to use a steel plate having high mechanical strength (meaning various properties related to mechanical deformation and destruction, such as tensile strength, yield point, elongation, reduction in area, hardness, impact value, fatigue strength, etc.) as the base steel plate. The chemical compositions of the base steel sheets before plating used in the hot stamping steel sheets shown in the following examples are shown in Table 1 below.
[0123] [Table 1]
[0124] For the base steel sheets (steel Nos. S1 to S10) having the chemical compositions shown in Table 1, steel sheets (base steel sheets) having a width of 100 mm, a length of 200 mm and a thickness of 2.3 mm were prepared, and an aluminum plating layer and a surface treatment film were applied to the entire surfaces of both sides of the base steel sheet by the method described below. Here, the notation "-" in Table 1 means that the content of the corresponding element is 0% in significant figures (numbers up to the least significant digit) defined in this embodiment.
[0125] First, an aqueous treatment liquid (solvent: water) containing at least one of carbon black (CB), graphite, and soot pulverized to a powder diameter (particle size) of 30 to 300 nm as compound A, and an aqueous treatment liquid (solvent: water) containing metal oxide or metal fluoride pulverized to a powder diameter (particle size) of 30 to 300 nm as compound B were separately prepared. Then, the respective treatment liquids were mixed, and a treatment liquid containing polyurethane resin was further added was applied onto the aluminum plating layer and dried to form a surface treatment film. The thickness of the surface treatment film was within the range of 1.0 to 2.5 μm, and the same type of film was applied to both sides.
[0126] Tables 2A and 2B show the manufacturing methods of the surface treatment film, including the types of compounds and additives used. In all manufacturing methods shown in Tables 2A and 2B, the polyurethane resin was added so that the ratio of the solid content in the treatment liquid was 10 to 92 mass%. In all manufacturing methods shown in Tables 2A and 2B, sodium fluoride was used as an additive when preparing compound B. In addition, when each treatment liquid of compound A and compound B was mixed, the dry weight ratio was adjusted to be as shown in Tables 2A and 2B. Note that the underlines in Tables 2A and 2B indicate conditions outside the preferred conditions of the manufacturing method of the present invention. The dynamic viscosity (mPa·s) shown in Tables 2A and 2B is calculated at a shear rate of 10 -3 The dynamic viscosity at 1000 nm / s is shown in Table 2. "Time t1", "Time t2", and "Time t3" shown in Table 2A and Table 2B respectively indicate "the time at which the temperature of the base steel plate surface reaches 65°C from 25°C", "the time at which the temperature of the base steel plate surface decreases from 65°C to 40°C", and "the time at which the temperature of the base steel plate surface reaches 55°C from 25°C".
[0127] [Table 2A]
[0128] [Table 2B]
[0129] Then, a thermocouple was connected to the surface of the aluminum-plated steel sheet (HS aluminum-plated steel sheet) to which the surface treatment film had been applied so that the temperature at each position could be measured. The HS aluminum-plated steel sheet was then heated in an electric heating furnace set at a temperature of 940°C, and when the surface temperature reached 930°C, the HS aluminum-plated steel sheet was removed from the heating furnace. The HS aluminum-plated steel sheet was then rapidly cooled using a flat die to obtain a hot stamped component.
[0130] In this example, the base steel sheet was plated with Al-10 mass% Si by hot-dip galvanization, and then the above-mentioned surface treatment film was applied. In the case of the hot-dip galvanization, the base steel sheet was immersed in a plating bath, and then the coating weight was reduced to 100 g / m per side by gas wiping. 2 was adjusted to.
[0131] The coating composition, temperature rise rate (temperature rise characteristics), and coating adhesion of the surface treatment coating were investigated. Note that hot stamped parts are not necessarily used as parts that are subjected to sliding, etc. Therefore, in this example, coating adhesion is not an essential characteristic that a hot stamped part should have, but is a characteristic that is preferable for the part to have.
[0132] The evaluation methods for each evaluation item were as follows.
[0133] (1) Temperature rise rate (temperature rise characteristics) (Score) The heating rate of each HS aluminum-plated steel sheet was calculated from the temperature change obtained from the thermocouple attached to the sheet and the heating time in the electric heating furnace, and an evaluation was performed. In detail, the heating rate from room temperature to 910°C was calculated, and the sheet was evaluated based on the following evaluation criteria. A score of 2 or higher was considered to be a pass.
[0134] (Score) 4: Heating rate of 5.7℃ / s or more 3: Heating rate: 4.3℃ / s or more and less than 5.7℃ / s 2: Heating rate: 3.5℃ / s or more but less than 4.3℃ / s 1: Heating rate less than 2.5℃ / s
[0135] (2) Film adhesion The obtained hot stamped molded body was placed in a rubbing tester (Imoto Manufacturing Co., Ltd., "Rubbing Tester 1509"), and absorbent cotton soaked in ethanol was rubbed with the following conditions: stroke distance: 100 mm, speed: 30 reciprocations per minute, load: 0.5 kgf / cm 2 After sliding (back and forth) 10 times with a brush, the film condition was evaluated according to the following criteria.
[0136] (Score) 3: No marks at all on the entire sliding surface. 2: There are slight marks on some of the sliding parts. 1: The coating disappears from the sliding parts.
[0137] <Example 1> In Table 3, B1 to B16 are invention examples, and b1 to b8 are comparative examples. In this example, when preparing the aqueous treatment liquid, carbon black (CB), graphite, soot powder, and an aqueous dispersion were used as compounds other than the binder component.
[0138] In Comparative Example b1, the carbon concentration of compound A was low at 71%. In Comparative Examples b2 to b4, compound B did not have a rutile structure. Comparative Examples b5 and b10 did not satisfy formula (1). Comparative Examples b6, b7, b8, and b9 did not satisfy formula (2). Comparative Examples b1 to b7, b9, and b10 were scored 1 for the heating rate, while Invention Examples B1 to B16 were scored 2 for the heating rate.
[0139] [Table 3]
[0140] <Example 2> As shown in Table 4, invention examples C2 to C11, in which the content of compound A at a position 0.90H from the surface of the surface treatment film (i.e., position P on the interface side) was 30 to 80%, had a superior heating rate to C1, in which the content of compound A at the same position was 20%.
[0141] [Table 4]
[0142] <Example 3> As shown in Table 5, Examples D6 to D9 in which Compound B was TiO2 had a superior heating rate to Examples D1 and D5 in which Compound B was IrO2 or GeO2.
[0143] [Table 5]
[0144] Although the preferred embodiment of the present invention has been described in detail above, the present invention is not limited to such an example. It is clear that a person having ordinary knowledge in the technical field to which the present invention pertains can conceive of various modified or altered examples within the scope of the technical ideas described in the claims, and it is understood that these also naturally fall within the technical scope of the present invention. [Industrial Applicability]
[0145] According to the above-described aspects of the present invention, it is possible to provide an aluminum-plated steel sheet for hot stamping that can further improve the productivity of hot stamped members, and therefore the present invention has high industrial applicability. [Explanation of symbols]
[0146] 10. Aluminum-plated steel sheets for hot stamping 11 Base steel plate 12 Aluminum plating layer 13 Surface treatment film 14 Surface preparation film
Claims
1. A base steel plate; An aluminum plating layer having an Al content of 80 mass% or more provided on at least one surface of the base steel sheet; and a surface treatment film provided on the aluminum plating layer, The surface treatment film is A compound A containing carbon; A compound B which is an oxide or fluoride of a metal element M and has a rutile structure; The carbon concentration of the compound A is 80% by mass or more, The aluminum-plated steel sheet for hot stamping, characterized in that the concentration of the metal element M satisfies the following formula (1) and the following formula (2): 1≦C bM ≦40・・・Formula (1) 1.5≦C bM / C tM ≦10.0・・・Formula (2) Here, when the average thickness of the surface treatment film is H, C in the above formula (2) tM is the concentration, in mass %, of the metal element M at a position 0.05H from the surface of the surface treatment film, C in the above formula (1) and the above formula (2) bM is the concentration of the metal element M at a position 0.95H from the surface of the surface treatment film, in mass %.
2. The aluminum-plated steel sheet for hot stamping according to claim 1, characterized in that a content of the compound A is 30 to 80% at a position 0.90H from the surface of the surface treatment film.
3. The compound B is TiO 2 The aluminum-plated steel sheet for hot stamping according to claim 1 or 2,
Citation Information
Patent Citations
Hot press formed product with high corrosion resistance
JP2003126921A
Al PLATED STEEL SHEET FOR HOT PRESS HAVING EXCELLENT TEMPERATURE RISING PROPERTY, AND METHOD FOR PRODUCING THE SAME
JP2011149084A
Method for manufacturing press hardened and coated steel parts at high production rates
JP2017518438A
Coated steel sheet having high corrosion resistance and method for manufacturing the same
KR1020190062944A
Layered blank for hot stamping, method for manufacturing layered hot stamping molded body, and layered hot stamping molded body
WO2019194308A1