Lightweight reinforced thermoplastic composite articles containing bicomponent fibers - Patents.com

Thermoplastic composite articles with bicomponent fibers enhance mechanical properties, addressing performance gaps in traditional materials by utilizing a core-shell arrangement with specific melting point differences, suitable for automotive and architectural uses.

JP7554196B2Active Publication Date: 2024-09-19AZDEL INC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2021544584
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-07-15
Filing Date
2020-01-31
Publication Date
2024-09-19
Estimated Expiration
2040-01-31

AI Technical Summary

Technical Problem

Thermoplastic composite articles lacking bicomponent fibers often fail to achieve optimal mechanical properties and performance in automotive and architectural applications, necessitating improved materials that address unique considerations not present in traditional steel or metal articles.

Method used

The development of thermoplastic composite articles incorporating bicomponent fibers, which include a core-shell arrangement with a core material having a melting point at least 20 degrees Celsius higher than the thermoplastic material, and a shell material with a melting point similar to the thermoplastic, enhancing mechanical properties such as peak load, stiffness, and flexural modulus.

Benefits of technology

The inclusion of bicomponent fibers in thermoplastic composites significantly improves mechanical properties, including peak load, stiffness, and flexural modulus, making them suitable for applications like vehicle headliners and furniture panels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554196000023
    Figure 0007554196000023
  • Figure 0007554196000015
    Figure 0007554196000015
  • Figure 0007554196000010
    Figure 0007554196000010
Patent Text Reader

Abstract

Lightweight reinforced thermoplastic articles are described having a core layer containing bicomponent fibers. In some examples, the core layer contains a thermoplastic material, reinforcing fibers, bicomponent fibers, and a lofting agent. After molding of the composite article, improvements in one or more of peak load, stiffness, flexural strength, and flexural modulus can be achieved for a specific molded thickness.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] (Priority Application) This application claims priority to and the benefit of U.S. Provisional Patent Application No. 62 / 800,314, filed February 1, 2019, and U.S. Provisional Patent Application No. 62 / 874,036, filed July 15, 2019, the entire disclosures of each of which are incorporated herein by reference.

[0002] Certain embodiments relate to thermoplastic composite articles that include bicomponent fibers. In some cases, thermoplastic composite articles having bicomponent fibers may provide improved performance over thermoplastic composite articles lacking bicomponent fibers. [Background technology]

[0003] Certain automotive and architectural applications often use thermoplastic-based materials in place of traditional steel or metal articles, which can present unique considerations that do not arise with steel or metal articles. Summary of the Invention

[0004] Certain embodiments are described herein to illustrate several configurations of thermoplastic composite articles having bicomponent fibers. It will be within the ability of one of ordinary skill in the art, given the benefit of this disclosure, to produce other configurations of thermoplastic composite articles including bicomponent fibers.

[0005] In one embodiment, a molded porous composite article includes a lofted core layer including a web formed from reinforcing fibers, bicomponent fibers, a lofting agent, and a thermoplastic material, the web including a porosity of about 20% to about 80%, the bicomponent fibers including a core-shell configuration, the shell material of the shell of the core-shell configuration including a melting point substantially similar to the melting point of the thermoplastic material, the core material of the core of the core-shell configuration including a melting point at least 20 degrees Celsius higher than the melting point of the thermoplastic material, and the molded porous composite article includes a peak load of 10 N to about 40 N in the machine direction and a peak load of about 6 N to about 30 N in the cross direction at a molded thickness of about 2 mm to about 4 mm in both the machine direction and the cross direction when tested according to SAE J949_200904.

[0006] In certain embodiments, the bicomponent fiber includes a shell that includes a polyolefin and a core that includes a polyester or a polyamide. In other examples, the bicomponent fiber includes a shell that includes a polyolefin and a core that includes a polyester. In some examples, the polyolefin includes polyethylene. In other examples, the polyethylene is linear low density polyethylene. In some embodiments, the polyester includes polyethylene terephthalate. In other examples, the polyamide includes nylon.

[0007] In some cases, the thermoplastic material is polypropylene, the shell polyolefin comprises linear low density polyethylene, the loft agent comprises expandable microspheres, and the core polyester comprises polyethylene terephthalate.

[0008] In other cases, the thermoplastic material is polypropylene, the shell polyolefin comprises linear low density polyethylene, the loft agent comprises expandable microspheres, and the core polyamide comprises nylon.

[0009] In a particular example, the thermoplastic material includes polypropylene, the reinforcing fibers include glass fibers, the bicomponent fibers include linear low density polyethylene in the shell, the melting point of the polyester or polyamide in the core is at least 20 degrees Celsius higher than the melting point of the thermoplastic material, and the loft agent includes expandable microspheres.

[0010] In some examples, the molded composite article further comprises a stiffness in the machine direction of about 10 N / cm to about 50 N / cm and a stiffness in the cross direction of about 7 N / cm to about 30 N / cm when tested according to SAE J949_200904.

[0011] In other examples, the molded composite article further comprises a flexural strength in the machine direction of from about 6 MPa to about 17 MPa and a flexural strength in the transverse direction of from about 4 MPa to about 11 MPa when tested according to SAE J949_200904.

[0012] In a further example, the molded composite article further comprises a flexural modulus in the machine direction of from about 800 MPa to about 2000 MPa and a flexural modulus in the transverse direction of from about 500 MPa to about 1300 MPa when tested according to SAE J949_200904.

[0013] In certain cases, the molded composite article further comprises a stiffness in the machine direction of about 10 N / cm to about 50 N / cm and a stiffness in the transverse direction of about 7 N / cm to about 30 N / cm when tested according to SAE J949_200904, and a flexural strength in the machine direction of about 6 MPa to about 17 MPa and a flexural strength in the transverse direction of about 4 MPa to about 11 MPa when tested according to SAE J949_200904.

[0014] In some embodiments, the molded composite article further comprises a stiffness in the machine direction of about 10 N / cm to about 50 N / cm and a stiffness in the transverse direction of about 7 N / cm to about 30 N / cm when tested per SAE J949_200904, and a flexural modulus in the machine direction of about 800 MPa to about 2000 MPa and a flexural modulus in the transverse direction of about 500 MPa to about 1300 MPa when tested per SAE J949_200904.

[0015] In certain examples, the molded composite article further comprises a flexural strength in the machine direction of about 6 MPa to about 17 MPa, and a flexural modulus in the machine direction of about 800 MPa to about 2000 MPa and a flexural modulus in the transverse direction of about 500 MPa to about 1300 MPa, when tested according to SAE J949_200904.

[0016] In some examples, the molded composite article further comprises a stiffness in the machine direction of about 10 N / cm to about 50 N / cm and a stiffness in the transverse direction of about 7 N / cm to about 30 N / cm when tested according to SAE J949_200904, and a flexural strength in the machine direction of about 6 MPa to about 17 MPa and a flexural strength in the transverse direction of about 4 MPa to about 11 MPa when tested according to SAE J949_200904, and a flexural modulus in the machine direction of about 800 MPa to about 2000 MPa and a flexural modulus in the transverse direction of about 500 MPa to about 1300 MPa when tested according to SAE J949_200904.

[0017] In certain embodiments, the article is configured as an automobile headliner, an automobile interior component, as a cubicle panel, or as a furniture panel.

[0018] In another embodiment, a molded porous composite article includes a lofted core layer including a web formed from reinforcing fibers, bicomponent fibers, a lofting agent, and a thermoplastic material, the web including a porosity of about 20% to about 80%, the bicomponent fibers including a core-shell configuration, a shell material of the shell of the core-shell configuration including a melting point substantially similar to a melting point of the thermoplastic material, and a core material of the core of the core-shell configuration including a melting point at least 20 degrees Celsius higher than a melting point of the thermoplastic material, and the molded porous composite article includes a stiffness in the machine direction of about 10 N / cm to about 50 N / cm and a stiffness in the cross direction of about 7 N / cm to about 30 N / cm when tested according to SAE J949_200904.

[0019] In some examples, the molded composite article further comprises a flexural strength in the machine direction of from about 6 MPa to about 17 MPa and a flexural strength in the transverse direction of from about 4 MPa to about 11 MPa when tested according to SAE J949_200904.

[0020] In other examples, the molded composite article further comprises a flexural modulus in the machine direction of from about 800 MPa to about 2000 MPa and a flexural modulus in the transverse direction of from about 500 MPa to about 1300 MPa when tested according to SAE J949_200904.

[0021] In additional examples, the molded composite article further comprises a flexural strength in the machine direction of about 6 MPa to about 17 MPa and a flexural strength in the transverse direction of about 4 MPa to about 11 MPa when tested per SAE J949_200904, and a flexural modulus in the machine direction of about 800 MPa to about 2000 MPa and a flexural modulus in the transverse direction of about 500 MPa to about 1300 MPa when tested per SAE J949_200904.

[0022] In another embodiment, a molded porous composite article comprises a lofted core layer comprising reinforcing fibers, bicomponent fibers, a lofting agent, and a web formed from a thermoplastic material, wherein the web comprises a porosity of about 20% to about 80%, the bicomponent fibers comprise a core-shell configuration, wherein a shell material of the shell of the core-shell configuration comprises a melting point substantially similar to a melting point of the thermoplastic material, and wherein a core material of the core of the core-shell configuration comprises a melting point at least 20 degrees Celsius higher than a melting point of the thermoplastic material, and wherein the molded porous composite article comprises a flexural strength in the machine direction of about 6 MPa to about 17 MPa and a flexural strength in the transverse direction of about 4 MPa to about 11 MPa when tested according to SAE J949_200904.

[0023] In certain examples, the molded composite article further comprises a flexural modulus in the machine direction of about 800 MPa to about 2000 MPa and a flexural modulus in the transverse direction of about 500 MPa to about 1300 MPa when tested according to SAE J949_200904.

[0024] In an additional embodiment, a molded porous composite article comprises a lofted core layer comprising reinforcing fibers, bicomponent fibers, a lofting agent, and a web formed from a thermoplastic material, wherein the web comprises a porosity of about 20% to about 80%, the bicomponent fibers comprise a core-shell configuration, wherein a shell material of the shell of the core-shell configuration comprises a melting point substantially similar to a melting point of the thermoplastic material, and wherein a core material of the core of the core-shell configuration comprises a melting point at least 20 degrees Celsius higher than a melting point of the thermoplastic material, and wherein the molded porous composite article comprises a flexural modulus in the machine direction of about 800 MPa to about 2000 MPa and a flexural modulus in the transverse direction of about 500 MPa to about 1300 MPa when tested according to SAE J949_200904.

[0025] Additional aspects, examples, embodiments, and configurations are described in more detail below.

[0026] Particular aspects, embodiments, and examples are described below with reference to the accompanying figures. [Brief description of the drawings]

[0027] [Figure 1] 1 is an illustration of a core-shell fiber arrangement, with some examples. [Diagram 2] 1 is an illustration of a parallel fiber arrangement, according to certain embodiments. [Figure 3A] 14A-14C are illustrations of parallel fiber arrangements with shells, according to several examples. [Figure 3B] 14A-14C are illustrations of parallel fiber arrangements with shells, according to several examples. [Figure 4] 1 is an illustration of a core layer with some examples. [Diagram 5] 1 illustrates a process that can be used to produce a core layer, according to some examples. [Figure 6] 1 illustrates another process that can be used to produce a core layer, according to a particular example. [Figure 7] 1 is an illustration of an article including a core layer and a skin layer, according to some examples. [Figure 8] 1 is an illustration of an article including a core layer and two skin layers, according to some examples. [Figure 9] 1 is an illustration of an article including a core layer, a skin layer, and a decorative layer, according to some examples. [Figure 10] 1 is an illustration of an automobile headliner, with some examples. [Figure 11] 1 is an illustration of a rear trim piece for an automobile, with several examples. [Figure 12] 1 is an illustration of an article of furniture, according to some embodiments. [Figure 13] 1 is another illustration of an article of furniture according to some embodiments. [Figure 14] 1 is another illustration of an article of furniture according to some embodiments. [Figure 15] 1 is another illustration of an article of furniture according to some embodiments. [Figure 16] 1 shows a photograph of a molded part produced using a hybrid lightweight reinforced thermoplastic sheet. [Figure 17]1 is a graph showing the tensile modulus measured in the machine direction (MD) and cross direction (CD) for several samples. [Figure 18] 1 is a graph showing the tensile strength measured in the machine direction (MD) and cross direction (CD) for several samples. [Figure 19A] 1 is a graph comparing peak load in the machine direction for various samples. [Figure 19B] 1 is a graph comparing peak load in the transverse direction for various samples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0028] It will be appreciated by those skilled in the art that the depictions and layers in the figures are provided for illustrative purposes only, and no specific thicknesses, materials, dimensions, etc. are intended to be implied or required unless expressly stated in the description herein in connection with that specific illustration.

[0029] Specific examples of composite articles are described herein that include combinations of thermoplastic materials and different fibers to provide improved properties. In some examples, one or more of peak load, stiffness, flexural strength, and flexural modulus may be improved.

[0030] In certain embodiments, the articles produced herein are described in certain cases as lightweight reinforced thermoplastic (LWRT) articles. In general, the articles include a core layer including a web formed from a thermoplastic material, reinforcing fibers, bicomponent fibers, and optionally a lofting agent. The presence of the combined materials can aid in enhanced properties.

[0031] In certain configurations, the bicomponent fibers of the core layer may include two or more different materials that can be arranged in many different ways. For example, the bicomponent fibers can be configured as a core-shell arrangement, a side-by-side arrangement, or a combination of these arrangements with the shell surrounding the side-by-side arrangement of the fibers. The different fibers can be extruded, coextruded, drawn, or produced in a manner similar to that used to produce the fibers. In some examples, the produced fibers can be coated with another material to provide a shell around the core fibers. When there are multiple fibers in the shell, the fibers can be coaxial, e.g., left untwisted, or crossed or twisted as desired.

[0032] Referring to FIG. 1, an illustration showing a cross section through a core-shell arrangement of a bicomponent fiber is shown. The bicomponent fiber 100 includes a core material 110 surrounded by a shell material 120. Although each of the components 110, 120 may not be truly fibers, the core 110 and shell 120 materials together form a fiber. Alternatively, each of the materials 110, 120 can be considered a fiber. The shell material 120 does not have to completely surround or be symmetrical around the core material 110. Without wishing to be bound by any particular theory, the shell material 120 is selected to be compatible with the thermoplastic material, e.g., thermoplastic resin, used to generate the core layer. For example, the melting point of the shell material 120 can be about the same or the same as the melting point of the thermoplastic material of the core layer. In some examples, the melting points of the shell material 120 and the thermoplastic material can differ by about 1 degree to about 10 degrees Celsius and the materials can still be considered compatible.

[0033] In certain embodiments, the core material 110 typically comprises a higher melting point than the shell material 120 and the thermoplastic material. For example, when the core layer is formed, the shell material 120 and the thermoplastic material may be melted or softened to form the web of the core layer. The core material 110 typically remains solid and does not melt or soften to any substantial extent during processing of the material to form the core layer.

[0034] In certain examples, the melting point of the core material 110 is at least 15 degrees Celsius higher than the melting point of the shell material 120 or the melting point of the thermoplastic material. In some examples, the melting point of the core material 110 is at least 20 degrees Celsius higher than the melting point of the shell material 120 or the melting point of the thermoplastic material. In other examples, the melting point of the core material 110 is at least 25 degrees Celsius higher than the melting point of the shell material 120 or the melting point of the thermoplastic material. In other examples, the melting point of the core material 110 is at least 30 degrees Celsius higher than the melting point of the shell material 120 or the melting point of the thermoplastic material. In certain examples, the melting point of the core material 110 is at least 35 degrees Celsius higher than the melting point of the shell material 120 or the melting point of the thermoplastic material. In certain embodiments, the melting point of the core material 110 is at least 40 degrees Celsius higher than the melting point of the shell material 120 or the melting point of the thermoplastic material. In other embodiments, the melting point of the core material 110 is at least 45 degrees Celsius higher than the melting point of the shell material 120 or the melting point of the thermoplastic material. In other embodiments, the melting point of the core material 110 is at least 50 degrees Celsius higher than the melting point of the shell material 120 or the melting point of the thermoplastic material.

[0035] In certain configurations, the materials present in the shell 120 and the core 110 are not the same material. For example, the shell material 120 may include a polyolefin and the core material 110 may include a material having a melting point higher than the melting point of the polyolefin of the shell material 120. In other cases, the core material 110 may include a polyester, polyamide, or copolyamide and the shell material 120 may include a material having a melting point lower than the melting point of the polyester, polyamide, or copolyamide in the core material 110. In additional examples, the shell material 120 may include a polyolefin and the core material 110 may include a polyester, polyamide, or copolyamide. In some examples, the shell material 120 includes a polyolefin and the core material 110 includes a polyester. In other examples, the shell material 120 includes a polyolefin and the core material 110 includes a polyamide. In some examples, the shell material 120 includes a polyolefin and the core material includes a copolyamide.

[0036] In some examples, the polyolefin of the shell material 120 may be polyethylene, polypropylene, or other olefin-based polymers and copolymers. In some embodiments, the polyolefin material of the shell 120 may be considered a linear low density polyolefin. For example, the polyolefin material of the shell 120 may be linear low density polyethylene (LLDPE) or low density polyethylene (LDPE). While the exact material properties may vary, linear low density polyethylene has a viscosity of approximately 0.91 g / cm 3 ~Approx. 0.94g / cm 3 In some examples, the melting point of the LLDPE or LDPE may be at least 15 degrees Celsius lower than the melting point of the core material 110. In certain examples, the melting point of the LLDPE or LDPE may be at least 20 degrees Celsius lower than the melting point of the core material 110. In other examples, the melting point of the LLDPE or LDPE may be at least 25 degrees Celsius lower than the melting point of the core material 110. In certain examples, the melting point of the LLDPE or LDPE may be at least 30 degrees Celsius lower than the melting point of the core material 110. In other examples, the melting point of the LLDPE or LDPE may be at least 35 degrees Celsius lower than the melting point of the core material 110. In certain examples, the melting point of the LLDPE or LDPE may be at least 40 degrees Celsius lower than the melting point of the core material 110. In other examples, the melting point of the LLDPE or LDPE may be at least 45 degrees Celsius lower than the melting point of the core material 110. In some examples, the melting point of the LLDPE or LDPE may be at least 50 degrees Celsius lower than the melting point of the core material 110 .

[0037] In other examples, the core material 110 may include a polyester that includes terephthalate monomer units. For example, the polyester may be polyethylene terephthalate, polybutylene terephthalate, or polynaphthalene terephthalate. In certain examples, the melting point of the polyester that includes terephthalate monomer units in the core material 110 may be at least 15 degrees higher than the melting point of the material in the shell material 120. In some examples, the melting point of the polyester that includes terephthalate monomer units in the core material 110 may be at least 20 degrees higher than the melting point of the material in the shell material 120. In certain examples, the melting point of the polyester that includes terephthalate monomer units in the core material 110 may be at least 25 degrees higher than the melting point of the material in the shell material 120. In other examples, the melting point of the polyester that includes terephthalate monomer units in the core material 110 may be at least 30 degrees higher than the melting point of the material in the shell material 120. In certain examples, the melting point of the polyester that includes terephthalate monomer units in the core material 110 may be at least 35 degrees higher than the melting point of the material in the shell material 120. In some examples, the melting point of the polyester including terephthalate monomer units in the core material 110 may be at least 40 degrees higher than the melting point of the material in the shell material 120. In other examples, the melting point of the polyester including terephthalate monomer units in the core material 110 may be at least 45 degrees higher than the melting point of the material in the shell material 120. In additional examples, the melting point of the polyester including terephthalate monomer units in the core material 110 may be at least 50 degrees higher than the melting point of the material in the shell material 120.

[0038] In some embodiments, the core material 110 may include a polyamide or copolyamide. For example, the core material 110 may include nylon, nylon 66, aramid, polyesteramide, polyetheramide, polyetheresteramide, or other polyamide-containing copolymer. In certain examples, the melting point of the polyamide or copolyamide in the core material 110 may be at least 15 degrees higher than the melting point of the material in the shell material 120. In some examples, the melting point of the polyamide or copolyamide in the core material 110 may be at least 20 degrees higher than the melting point of the material in the shell material 120. In certain examples, the melting point of the polyamide or copolyamide in the core material 110 may be at least 25 degrees higher than the melting point of the material in the shell material 120. In other examples, the melting point of the polyamide or copolyamide in the core material 110 may be at least 30 degrees higher than the melting point of the material in the shell material 120. In certain examples, the melting point of the polyamide or copolyamide in the core material 110 may be at least 35 degrees higher than the melting point of the material in the shell material 120. In some examples, the melting point of the polyamide or copolyamide in core material 110 may be at least 40 degrees higher than the melting point of the material in shell material 120. In other examples, the melting point of the polyamide or copolyamide in core material 110 may be at least 45 degrees higher than the melting point of the material in shell material 120. In additional examples, the melting point of the polyamide or copolyamide in core material 110 may be at least 50 degrees higher than the melting point of the material in shell material 120.

[0039] In certain examples, the shell material 120 may include a polyethylene, such as LLDPE, and the core material 110 may include a polyester or a polyamide. For example, the core material 110 may include nylon, polyethylene terephthalate, polybutylene terephthalate, polynaphthalene terephthalate, or a combination thereof. In certain examples, the melting point of the polyester or polyamide in the core material 110 may be at least 15 degrees higher than the melting point of the polyethylene material in the shell material 120. In some examples, the melting point of the polyester or polyamide in the core material 110 may be at least 20 degrees higher than the melting point of the polyethylene material in the shell material 120. In certain examples, the melting point of the polyester or polyamide in the core material 110 may be at least 25 degrees higher than the melting point of the polyethylene material in the shell material 120. In other examples, the melting point of the polyester or polyamide in the core material 110 may be at least 30 degrees higher than the melting point of the polyethylene material in the shell material 120. In certain examples, the melting point of the polyester or polyamide in the core material 110 may be at least 35 degrees higher than the melting point of the polyethylene material in the shell material 120. In some examples, the melting point of the polyester or polyamide in the core material 110 may be at least 40 degrees higher than the melting point of the polyethylene material in the shell material 120. In other examples, the melting point of the polyester or polyamide in the core material 110 may be at least 45 degrees higher than the melting point of the polyethylene material in the shell material 120. In additional examples, the melting point of the polyester or polyamide in the core material 110 may be at least 50 degrees higher than the melting point of the polyethylene material in the shell material 120.

[0040] In other cases, the bicomponent fibers present in the LWRT article may include a left-right fiber arrangement. Referring to FIG. 2, an illustration showing a cross section through a side-by-side fiber arrangement of a bicomponent fiber is shown. The bicomponent fiber 200 includes a first fiber 210 arranged on the side of a second fiber 220. The fibers 210, 220 may be twisted around each other or remain untwisted and run approximately coaxially with each other throughout the fiber 200. While not wishing to be bound by any particular theory, the melting point of the material of one of the fibers 210, 220 is typically approximately the same or the same as the melting point of the thermoplastic material of the core layer. In some instances, the melting points of the fibers 210, 220 and one of the thermoplastic materials may differ by about 1 degree to about 10 degrees Celsius and the materials can still be considered compatible.

[0041] In certain embodiments, the fibers 210 typically include a higher melting point than the other fibers 220 and the thermoplastic material. For example, when the core layer is formed, the fibers 220 and the thermoplastic material may be melted or softened to form the web of the core layer. The fibers 210 typically remain solid and do not melt and soften to any substantial extent during processing of the material to form the core layer. In certain examples, the melting point of the fibers 210 is at least 15 degrees Celsius higher than the melting point of the fibers 220 or the melting point of the thermoplastic material. In some examples, the melting point of the fibers 210 is at least 20 degrees Celsius higher than the melting point of the fibers 220 or the melting point of the thermoplastic material. In other examples, the melting point of the fibers 210 is at least 25 degrees Celsius higher than the melting point of the fibers 220 or the melting point of the thermoplastic material. In other examples, the melting point of the fibers 210 is at least 30 degrees Celsius higher than the melting point of the fibers 220 or the melting point of the thermoplastic material. In certain instances, the melting point of the fibers 210 is at least 35 degrees Celsius higher than the melting point of the fibers 220 or the melting point of the thermoplastic material. In certain embodiments, the melting point of the fibers 210 is at least 40 degrees Celsius higher than the melting point of the fibers 220 or the melting point of the thermoplastic material. In other embodiments, the melting point of the fibers 210 is at least 45 degrees Celsius higher than the melting point of the fibers 220 or the melting point of the thermoplastic material. In other embodiments, the melting point of the fibers 210 is at least 50 degrees Celsius higher than the melting point of the fibers 220 or the melting point of the thermoplastic material.

[0042] In certain configurations, the materials present in fibers 210, 220 are not the same material. For example, fiber 220 may include a polyolefin and fiber 210 may include a material having a melting point higher than the melting point of the polyolefin of shell material 120. In other cases, fiber 210 may include a polyester, polyamide, or copolyamide and fiber 220 may include a material having a melting point lower than the melting point of the polyester, polyamide, or copolyamide in fiber 210. In additional examples, fiber 220 may include a polyolefin and fiber 210 may include a polyester, polyamide, or copolyamide. In some examples, fiber 220 includes a polyolefin and fiber 210 includes a polyester. In other examples, fiber 220 includes a polyolefin and fiber 210 includes a polyamide. In some examples, fiber 220 includes a polyolefin and fiber 210 includes a copolyamide.

[0043] In some examples, the polyolefin of the fibers 220 may be polyethylene, polypropylene, or other olefin-based polymers and copolymers. In some embodiments, the polyolefin material of the fibers 220 may be considered a linear low density polyolefin. For example, the polyolefin material of the fibers 220 may be linear low density polyethylene (LLDPE) or low density polyethylene (LDPE). While the exact material properties may vary, linear low density polyethylene has a viscosity of about 0.91 g / cm 3 ~Approx. 0.94g / cm 3In some examples, the melting point of the LLDPE or LDPE may be at least 15 degrees Celsius lower than the melting point of the fibers 210. In certain examples, the melting point of the LLDPE or LDPE may be at least 20 degrees Celsius lower than the melting point of the fibers 210. In other examples, the melting point of the LLDPE or LDPE may be at least 25 degrees Celsius lower than the melting point of the fibers 210. In certain examples, the melting point of the LLDPE or LDPE may be at least 30 degrees Celsius lower than the melting point of the core material 110. In other examples, the melting point of the LLDPE or LDPE may be at least 35 degrees Celsius lower than the melting point of the fibers 210. In certain examples, the melting point of the LLDPE or LDPE may be at least 40 degrees Celsius lower than the melting point of the fibers 210. In other examples, the melting point of the LLDPE or LDPE may be at least 45 degrees Celsius lower than the melting point of the fibers 210. In some examples, the melting point of the LLDPE or LDPE may be at least 50 degrees Celsius lower than the melting point of the fibers 210.

[0044] In other examples, the fiber 210 may include a polyester that includes terephthalate monomer units. For example, the polyester may be polyethylene terephthalate, polybutylene terephthalate, or polynaphthalene terephthalate. In certain examples, the melting point of the polyester that includes terephthalate monomer units in the fiber 210 may be at least 15 degrees higher than the melting point of the material in the fiber 220. In some examples, the melting point of the polyester that includes terephthalate monomer units in the fiber 210 may be at least 20 degrees higher than the melting point of the material in the fiber 220. In certain examples, the melting point of the polyester that includes terephthalate monomer units in the fiber 210 may be at least 25 degrees higher than the melting point of the material in the fiber 220. In other examples, the melting point of the polyester that includes terephthalate monomer units in the fiber 210 may be at least 30 degrees higher than the melting point of the material in the fiber 220. In certain examples, the melting point of the polyester that includes terephthalate monomer units in the fiber 210 may be at least 35 degrees higher than the melting point of the material in the fiber 220. In some examples, the melting point of the polyester including terephthalate monomer units in fibers 210 may be at least 40 degrees higher than the melting point of the material in fibers 220. In other examples, the melting point of the polyester including terephthalate monomer units in fibers 210 may be at least 45 degrees higher than the melting point of the material in fibers 220. In an additional example, the melting point of the polyester including terephthalate monomer units in fibers 210 may be at least 50 degrees higher than the melting point of the material in fibers 220.

[0045] In some embodiments, the fiber 210 may include a polyamide or copolyamide. For example, the fiber 210 may include nylon, nylon 66, aramid, polyesteramide, polyetheramide, polyetheresteramide, or other polyamide-containing copolymer. In certain examples, the melting point of the polyamide or copolyamide in the fiber 210 may be at least 15 degrees higher than the melting point of the material in the fiber 220. In some examples, the melting point of the polyamide or copolyamide in the fiber 210 may be at least 20 degrees higher than the melting point of the material in the fiber 220. In certain examples, the melting point of the polyamide or copolyamide in the fiber 210 may be at least 25 degrees higher than the melting point of the material in the fiber 220. In other examples, the melting point of the polyamide or copolyamide in the fiber 210 may be at least 30 degrees higher than the melting point of the material in the fiber 220. In certain examples, the melting point of the polyamide or copolyamide in the fiber 210 may be at least 35 degrees higher than the melting point of the material in the fiber 220. In some examples, the melting point of the polyamide or copolyamide in fibers 210 may be at least 40 degrees higher than the melting point of the material in fibers 220. In other examples, the melting point of the polyamide or copolyamide in fibers 210 may be at least 45 degrees higher than the melting point of the material in fibers 220. In additional examples, the melting point of the polyamide or copolyamide in fibers 210 may be at least 50 degrees higher than the melting point of the material in fibers 220.

[0046] In certain examples, the fiber 220 may include polyethylene, such as LLDPE, and the fiber 210 may include polyester or polyamide. For example, the fiber 210 may include nylon, polyethylene terephthalate, polybutylene terephthalate, polynaphthalene terephthalate, or combinations thereof. In certain examples, the melting point of the polyester or polyamide in the fiber 210 may be at least 15 degrees higher than the melting point of the polyethylene material in the fiber 220. In some examples, the melting point of the polyester or polyamide in the core fiber 210 may be at least 20 degrees higher than the melting point of the polyethylene material in the fiber 220. In certain examples, the melting point of the polyester or polyamide in the fiber 210 may be at least 25 degrees higher than the melting point of the polyethylene material in the fiber 220. In other examples, the melting point of the polyester or polyamide in the fiber 210 may be at least 30 degrees higher than the melting point of the polyethylene material in the fiber 220. In certain examples, the melting point of the polyester or polyamide in the fiber 210 may be at least 35 degrees higher than the melting point of the polyethylene material in the fiber 220. In some examples, the melting point of the polyester or polyamide in fibers 210 may be at least 40 degrees higher than the melting point of the polyethylene material in fibers 220. In other examples, the melting point of the polyester or polyamide in fibers 210 may be at least 45 degrees higher than the melting point of the polyethylene material in fibers 220. In additional examples, the melting point of the polyester or polyamide in fibers 210 may be at least 50 degrees higher than the melting point of the polyethylene material in fibers 220.

[0047] Referring to Figure 3A, an illustration showing a cross section through a parallel fiber arrangement of bicomponent fibers with a shell surrounding the parallel fiber arrangement is shown. For example, fiber 300 includes a shell 320 surrounding two fibers 310, 315. In Figure 3A, fibers 310, 315 can include the same or similar composition. For example, each of fibers 310, 315 can independently include the same material as described in connection with core material 110 of Figure 1, e.g., each of fibers 310, 315 can independently include polyamide, polyester, or other polymer.

[0048] In certain embodiments, the shell material 320 may include a polyolefin. In some examples, the polyolefin of the shell material 320 may be polyethylene, polypropylene, or other olefin-based polymers and copolymers. In some embodiments, the polyolefin material of the shell 320 may be considered a linear low density polyolefin. For example, the polyolefin material of the shell 320 may be linear low density polyethylene (LLDPE) or low density polyethylene (LDPE). While the exact material properties may vary, linear low density polyethylene has a viscosity of approximately 0.91 g / cm 3 ~Approx. 0.94g / cm 3 In some examples, the melting point of the LLDPE or LDPE may be at least 15 degrees Celsius lower than the melting point of the fibers 310, 315. In certain examples, the melting point of the LLDPE or LDPE may be at least 20 degrees Celsius lower than the melting point of the fibers 310, 315. In other examples, the melting point of the LLDPE or LDPE may be at least 25 degrees Celsius lower than the melting point of the fibers 310, 315. In certain examples, the melting point of the LLDPE or LDPE may be at least 30 degrees Celsius lower than the melting point of the fibers 310, 315. In other examples, the melting point of the LLDPE or LDPE may be at least 35 degrees Celsius lower than the melting point of the fibers 310, 315. In certain examples, the melting point of the LLDPE or LDPE may be at least 40 degrees Celsius lower than the melting point of the fibers 310, 315. In other examples, the melting point of the LLDPE or LDPE may be at least 45 degrees Celsius lower than the melting point of the fibers 310, 315. In some examples, the melting point of the LLDPE or LDPE may be at least 50 degrees Celsius lower than the melting point of the fibers 310, 315.

[0049] In certain examples, the fibers 310, 315 may independently comprise polyester or polyamide. In some cases, the fibers 310, 315 may independently comprise nylon, polyethylene terephthalate, polybutylene terephthalate, polynaphthalene terephthalate, or combinations thereof. In certain examples, the melting point of the polyester or polyamide in the fibers 310, 315 may be at least 15 degrees higher than the melting point of the polyethylene material in the shell material 320. In some examples, the melting point of the polyester or polyamide in the fibers 310, 315 may be at least 20 degrees higher than the melting point of the polyethylene material in the shell material 320. In certain examples, the melting point of the polyester or polyamide in the fibers 310, 315 may be at least 25 degrees higher than the melting point of the polyethylene material in the shell material 320. In other examples, the melting point of the polyester or polyamide in the fibers 310, 315 may be at least 30 degrees higher than the melting point of the polyethylene material in the shell material 320. In certain examples, the melting point of the polyester or polyamide in the fibers 310, 315 may be at least 35 degrees higher than the melting point of the polyethylene material in the shell material 320. In some examples, the melting point of the polyester or polyamide in the fibers 310, 315 may be at least 40 degrees higher than the melting point of the polyethylene material in the shell material 320. In other examples, the melting point of the polyester or polyamide in the fibers 310, 315 may be at least 45 degrees higher than the melting point of the polyethylene material in the shell material 320. In additional examples, the melting point of the polyester or polyamide in the fibers 310, 315 may be at least 50 degrees higher than the melting point of the polyethylene material in the shell material 320.

[0050] FIG. 3A shows two parallel fibers that may have the same composition, but this configuration is not required. For example, referring to FIG. 3B, a parallel arrangement of fibers 360, 365 surrounded by a shell 370 is shown. The fibers 360, 365 do not have to have the same composition as each other, but the melting point of each of the fibers 360, 365 is typically higher than the melting point of the shell 370 in the fiber arrangement 350. In one configuration, one of the fibers 360, 365 is an inorganic fiber, such as a reinforcing fiber, as described below, e.g., glass fiber, graphite fiber, carbon fiber, etc., and the other of the fibers 360, 365 is an organic fiber, e.g., containing one or more covalently bonded carbon-hydrogen groups. Packaging the inorganic and organic fibers in a shell may simplify the addition of fibers during processing of the material to form the core layer. In another example, the fibers 360, 365 may each be an organic fiber having a different composition.

[0051] In certain embodiments, the shell material 370 may include a polyolefin. In some examples, the polyolefin of the shell material 370 may be polyethylene, polypropylene, or other olefin-based polymers and copolymers. In some embodiments, the polyolefin material of the shell 370 may be considered a linear low density polyolefin. For example, the polyolefin material of the shell 370 may be linear low density polyethylene (LLDPE) or low density polyethylene (LDPE). While the exact material properties may vary, linear low density polyethylene has a viscosity of approximately 0.91 g / cm 3 ~Approx. 0.94g / cm 3In some examples, the melting point of the LLDPE or LDPE may be at least 15 degrees Celsius lower than the melting point of the fibers 360, 365. In certain examples, the melting point of the LLDPE or LDPE may be at least 20 degrees Celsius lower than the melting point of the fibers 360, 365. In other examples, the melting point of the LLDPE or LDPE may be at least 25 degrees Celsius lower than the melting point of the fibers 360, 365. In certain examples, the melting point of the LLDPE or LDPE may be at least 30 degrees Celsius lower than the melting point of the fibers 360, 365. In other examples, the melting point of the LLDPE or LDPE may be at least 35 degrees Celsius lower than the melting point of the fibers 360, 365. In certain examples, the melting point of the LLDPE or LDPE may be at least 40 degrees Celsius lower than the melting point of the fibers 360, 365. In other examples, the melting point of the LLDPE or LDPE may be at least 45 degrees Celsius lower than the melting point of the fibers 360, 365. In some instances, the melting point of the LLDPE or LDPE may be at least 50 degrees Celsius lower than the melting point of the fibers 360, 365.

[0052] In certain examples, the fibers 360, 365 may independently comprise polyester or polyamide, or one of the fibers 360, 365 may be an inorganic reinforcing fiber. In some cases, the fibers 360, 365 may independently comprise nylon, polyethylene terephthalate, polybutylene terephthalate, polynaphthalene terephthalate, or combinations thereof. In certain examples, the melting point of the material in the fibers 360, 365 may be at least 15 degrees higher than the melting point of the polyethylene material in the shell material 370. In some examples, the melting point of the material in the fibers 360, 365 may be at least 20 degrees higher than the melting point of the polyethylene material in the shell material 370. In certain examples, the melting point of the material in the fibers 360, 365 may be at least 25 degrees higher than the melting point of the polyethylene material in the shell material 370. In other examples, the melting point of the material in the fibers 360, 365 may be at least 30 degrees higher than the melting point of the polyethylene material in the shell material 370. In certain examples, the melting point of the material in the fibers 360, 365 may be at least 35 degrees higher than the melting point of the polyethylene material in the shell material 320. In some examples, the melting point of the material in the fibers 360, 365 may be at least 40 degrees higher than the melting point of the polyethylene material in the shell material 370. In other examples, the melting point of the material in the fibers 360, 365 may be at least 45 degrees higher than the melting point of the polyethylene material in the shell material 370. In additional examples, the melting point of the material in the fibers 360, 365 may be at least 50 degrees higher than the melting point of the polyethylene material in the shell material 370.

[0053] In a particular embodiment, referring to FIG. 4, a core layer 410 is shown that includes a thermoplastic material, a reinforcing fiber, a bicomponent fiber, and a lofting agent. As discussed further below, the combination of these materials can provide improved mechanical properties. Although not true for all configurations, the lofting agent is typically trapped within the voids or pores of the core layer 410. The core layer 410 may first be formed as a prepreg, which is generally a precursor to the core layer 410 and is not necessarily fully formed. For ease of illustration, the core layer is described below, but the properties of the core layer may also be the same as the prepreg. The core layer 410 includes a porous structure that allows gas to flow through the core layer. For example, the core layer can be set to 0-30%, 10-40%, 20-50%, 30-60%, 40-70%, 50-80%, 60-90%, 0-40%, 0-50%, 0-60%, 0-70%, 0-80%, 0-90%, 10-50%, 10-60%, 10-70%, 10-80%, 10-90%, 10-95%, 20-60%, 20-70%, 20-80%, 20-95%, 20-10%, 20-15%, 20-25%, 20-30%, 20-40%, 20-50%, 20-60%, 20-70%, 20-80%, 20-95%, 20-15%. The core layer 410 may include a void content or porosity of 0%, 20% to 95%, 30% to 70%, 30% to 80%, 30% to 90%, 30% to 95%, 40% to 80%, 40% to 90%, 40% to 95%, 50% to 90%, 50% to 95%, 60% to 95%, 70% to 80%, 70% to 90%, 70% to 95%, 80% to 90%, 80% to 95%, or any exemplary value within these exemplary ranges. In some cases, the core layer 410 includes a porosity or void content of greater than 0%, e.g., up to about 95% that is not fully consolidated. Unless otherwise indicated, references to a core layer including a particular void content or porosity are based on the total volume of the core layer, and not necessarily the total volume of the core layer plus any other materials or layers bonded to the core layer.

[0054] In certain embodiments, improved mechanical properties may be achieved by including polymeric bicomponent fibers in the core layer 410. For example, increasing the amount of reinforcing fibers in the core layer 410 may often degrade certain mechanical properties. The inclusion of bicomponent fibers in the core layer may improve, for example, one or more of peak load values, stiffness values, flexural strength values, and flexural modulus values ​​for a selected molded thickness. These values ​​may be measured, for example, using SAE J949 dated April 2009 (also referred to as SAEJ949_200904). Briefly, the SAE J949 protocol used subjects samples to a three-point bend test and measures various performance values.

[0055] In certain embodiments, the thermoplastic material of the core layer 410 may at least partially comprise one or more of polyethylene, polypropylene, polystyrene, acrylonitrile styrene, butadiene, polyethylene terephthalate, polybutylene terephthalate, polybutylene tetrachlorate, and polyvinyl chloride, both plasticized and unplasticized, as well as blends of these materials with each other or with other polymeric materials. Other suitable thermoplastics include, but are not limited to, polyarylene ethers, polycarbonates, polyester carbonates, thermoplastic polyesters, polyimides, polyetherimides, polyamides, acrylonitrile-butyl acrylate-styrene polymers, amorphous nylons, polyarylene ether ketones, polyphenylene sulfides, polyarylsulfones, polyethersulfones, liquid crystal polymers, poly(1,4 phenylene) compounds commercially known as PARMAX®, high heat polycarbonates such as Bayer's APEC® PC, high temperature nylons, and silicones, as well as alloys and blends of these materials with each other or with other polymeric materials. The virgin thermoplastic material used to form the core layer may be used in powder form, resin form, rosin form, fiber form, or other suitable form. Various forms of exemplary thermoplastic materials are described herein, but are also described, for example, in U.S. Patent Application Publication Nos. 2013 / 0244528 and 2012 / 0065283. The exact amount of thermoplastic material present in the core layer 410 may vary, with exemplary amounts ranging from about 20% to about 80% by weight. As described herein, the material of the core layer 410 may be selected such that its melting point is approximately the same as one of the materials in the bicomponent fiber and less than the melting point of another material in the bicomponent fiber. Exemplary melting point ranges for the thermoplastic material include, but are not limited to, about 120 degrees Celsius to about 260 degrees Celsius. Thermoplastic materials that melt between 100 degrees Celsius and 315 degrees Celsius may also be used if desired.

[0056] In certain examples, the reinforcing fibers of the core layer described herein can include glass fibers, carbon fibers, graphite fibers, synthetic organic fibers, such as para-aramid and meta-aramid fibers, nylon fibers, polyester fibers, or organic fibers with particularly high modulus, such as any high melt flow index resin suitable for use as fibers, natural fibers, such as hemp, sisal, jute, flax, coir, kenaf, and cellulosic fibers, mineral fibers, such as basalt, mineral wool (e.g., rock wool or slag wool), wollastonite, alumina silica, and the like, or mixtures thereof, metal fibers, metallized natural and / or synthetic fibers, ceramic fibers, yarn fibers, or mixtures thereof. In some cases, one type of reinforcing fiber can be used with mineral fibers, such as fibers formed by spinning or drawing molten minerals. Exemplary mineral fibers include, but are not limited to, mineral wool fibers, glass wool fibers, stone wool fibers, and ceramic wool fibers. In some examples, the reinforcing fibers can be selected to be inorganic fibers, such as fibers that do not contain covalently bonded carbon-hydrogen groups.

[0057] In some embodiments, any of the aforementioned reinforcing fibers may be chemically treated prior to use to provide the fibers with desired functional groups or to impart other physical properties. The total fiber content in the core layer (reinforcing fibers + bicomponent fibers) may be about 20% to about 90% by weight of the core layer, more specifically, about 30% to about 70% by weight of the core layer. Typically, the total fiber content of a composite article including a core layer varies from about 20% to about 90% by weight of the composite, more specifically, about 30% to about 80% by weight, e.g., about 40% to about 70% by weight. The specific size and / or orientation of the reinforcing fibers used may depend, at least in part, on the polymeric material used and / or the desired properties of the resulting core layer. Suitable additional fiber types, fiber sizes, and amounts will be readily selected by one of ordinary skill in the art given the benefit of this disclosure. In a non-limiting illustration, the reinforcing fibers dispersed in the thermoplastic material to provide the core layer generally have a diameter greater than about 5 micrometers, more specifically, between about 5 micrometers and about 22 micrometers, and a length between about 5 mm and about 200 mm. More specifically, the diameter of the reinforcing fibers can be between about 5 micrometers and about 22 micrometers, and the length of the fibers can be between about 5 mm and about 75 mm. In some configurations, the flame retardant material can be present in fibrous form. For example, the core layer can include a thermoplastic material, a reinforcing fiber, a bicomponent fiber, and a fiber including a flame retardant material.

[0058] In some configurations, the core layer 410 may be a substantially halogen-free or halogen-free layer to meet regulations regarding hazardous material requirements for certain applications. In other cases, the core layer 410 may include halogenated flame retardants (which may be present in the flame retardant material or may be additionally added to the flame retardant material), such as halogenated flame retardants including one or more of F, Cl, Br, I, and At, or compounds containing such halogens, such as tetrabromobisphenol-A polycarbonate, or monohalo-, dihalo-, trihalo-, or tetrahalo-polycarbonates. In some cases, the thermoplastic material used in the core layer 410 may include one or more halogens to impart some degree of flame retardancy without the addition of a separate flame retardant. For example, the thermoplastic material may be halogenated in addition to the flame retardant material being present, or virgin thermoplastic material may be halogenated and used on its own. If a halogenated flame retardant is present, it is desirably present in an amount of flame retardant that may vary depending on other components present. For example, the halogenated flame retardant present in addition to the flame retardant material may be present at about 0.1 weight percent to about 40 weight percent (based on the weight of the prepreg), more specifically, about 0.1 weight percent to about 15 weight percent, such as about 5 weight percent to about 15 weight percent. If desired, two different halogenated flame retardants may be added to the core layer 410. In other cases, a non-halogenated flame retardant may be added, such as a flame retardant containing one or more of N, P, As, Sb, Bi, S, Se, and Te. In some embodiments, the non-halogenated flame retardant may include a phosphorus-containing material, so that the core layer 410 may be more environmentally friendly. When a non-halogenated or substantially halogen-free flame retardant is present, the flame retardant is desirably present in an amount of the flame retardant that may vary depending on other components present. For example, the substantially halogen-free flame retardant can be present from about 0.1 weight percent to about 40 weight percent (based on the weight of the prepreg), more specifically, from about 5 weight percent to about 40 weight percent, such as from about 5 weight percent to about 15 weight percent, based on the weight of the core layer.If desired, two different substantially halogen-free flame retardants may be added to the core layer 410. In certain cases, the core layer 410 described herein may include one or more halogenated flame retardants in combination with one or more substantially halogen-free flame retardants. When two different flame retardants are present, the combination of the two flame retardants may be present in an amount of flame retardant that may vary depending on the other components present. For example, the total weight of the flame retardants present may be from about 0.1 weight percent to about 40 weight percent (based on the weight of the prepreg or core), more specifically, from about 5 weight percent to about 40 weight percent, e.g., from about 2 weight percent to about 14 weight percent, based on the weight of the core layer. The flame retardants used in the core layer described herein may be added to the mixture including the thermoplastic material, bicomponent fiber, and reinforcing fiber (prior to placement of the mixture on a wire screen or other processing component) or may be added after the core layer 410 is formed.

[0059] As described herein, the core layer 410 may include a lofting agent present in the pores or voids of the core layer. The lofting agent may take the form of expandable microspheres that may increase in volume upon exposure to heat or other stimuli. For example, the thickness of the core layer 410 may be increased by expanding the lofting agent. The exact amount of lofting agent present in the core layer 410 may vary, with exemplary amounts including, but not limited to, about 0.5 weight percent to about 30 weight percent.

[0060] In certain embodiments, the exact amount of bicomponent fibers in the core layer described herein may vary. Generally, the weight percent of bicomponent fibers in the core layer may vary from about 2 weight percent to about 30 weight percent. In some examples, about equal amounts of bicomponent fibers and reinforcing fibers are present in the core layer. In some examples, the overall basis weight of the core layer 410 may vary from about 500 gsm to about 3500 gsm. In some examples, a lighter core layer with suitable mechanical properties may be more desirable to reduce overall weight, for example, the basis weight of the core layer 410 may vary from about 750 gsm to about 1500 gsm or from about 750 gsm to about 1250 gsm.

[0061] In certain embodiments, the core layer and / or articles described herein can be prepared using reinforcing fibers, bicomponent fibers, lofting agents, and thermoplastic materials, generally as shown in FIG. 5. To produce the core layer, the thermoplastic materials, reinforcing fibers, bicomponent fibers, lofting agents, and optionally other materials can be added or metered in step 510 to a dispersed foam contained in an open-top mixing tank fitted with an impeller to provide an aqueous dispersion of the materials. Without wishing to be bound by any particular theory, the presence of trapped air pockets in the foam can aid in the dispersion of the reinforcing fibers, bicomponent fibers, thermoplastic materials, lofting agents, and any other materials. In some examples, the dispersed mixture of fibers, lofting agents, and thermoplastic materials can be pumped through a dispersion manifold to a headbox positioned above the wire section of a papermaking machine. For example, the aqueous mixture can be deposited in step 520 on a moving wire screen or other support element. The dispersed mixture is then provided to a moving support, such as a wire screen, using pressure to continuously produce a uniform, fibrous wet-laid web with the lofting agent trapped in the web, where the foam, but not the fibers, or the thermoplastic material can be removed. The wet-laid web can be passed through a dryer at a suitable temperature to reduce the moisture content and melt or soften at least one of the thermoplastic and bicomponent fibers to provide a core layer in step 530. As the hot web exits the dryer, an optional surface or skin layer, such as, for example, a textured film, can be laminated onto the web by passing the web of reinforcing fibers, bicomponent fibers, thermoplastic materials, lofting agents, and textured film through the nip of a set of heated rollers. If desired, additional layers, such as, for example, another film layer, a scrim layer, can also be attached to one or both sides of the web with the textured film to facilitate handling of the resulting composite. The composite can then be passed through a tension roll and continuously cut (cut) to a desired size for later formation into a final composite article.Further information regarding the preparation of such complexes, including suitable materials and processing conditions used to form such complexes, is described, for example, in U.S. Pat. Nos. 6,923,494, 4,978,489, 4,944,843, 4,964,935, 4,734,321, 5,053,449, 4,925,615, 5,609,966, and U.S. Patent Application Publication Nos. US2005 / 0082881, US2005 / 0228108, US2005 / 0217932, US2005 / 0215698, US2005 / 0164023, and US2005 / 0161865.

[0062] In another configuration, the core layer and / or articles described herein can be prepared using reinforcing fibers, bicomponent fibers, and thermoplastic materials, generally as shown in FIG. 6. To produce the core layer, the thermoplastic materials, reinforcing fibers, bicomponent fibers, and optionally other materials can be added or metered in step 610 to a dispersed foam contained in an open-top mixing tank fitted with an impeller to provide an aqueous dispersion. Without wishing to be bound by any particular theory, the presence of trapped air pockets in the foam can aid in the dispersion of the reinforcing fibers, bicomponent fibers, thermoplastic materials, and any other materials. In some examples, the dispersed mixture of fibers and thermoplastic materials can be pumped through a dispersion manifold to a headbox positioned above the wire section of a papermaking machine. For example, the aqueous mixture can be deposited in step 620 on a moving wire screen or other support element to provide a wet-laid web. The dispersed mixture can then be provided to a moving support, such as a wire screen, using pressure to continuously produce a uniform fibrous wet-laid web, while the foam, but not the fibers, or the thermoplastic materials can be removed. The lofting agent can then be deposited or sprayed on top of the wet web in step 625 to provide a wet web containing the lofting agent. The wet web containing the deposited lofting agent can be passed through a dryer, optionally under vacuum or by applying pressure and heat at a suitable temperature to reduce the moisture content and melt or soften at least one of the thermoplastic material and the bicomponent fiber to provide a core layer in step 630. As the hot web exits the dryer, an optional surface or skin layer, such as, for example, a textured film, can be laminated onto the web by passing the web of reinforcing fibers, bicomponent fibers, thermoplastic material, lofting agent, and textured film through the nip of a set of heated rollers. If desired, additional layers, such as, for example, another film layer, a scrim layer, can also be attached to one or both sides of the web with the textured film to facilitate handling of the resulting composite.The composite may then be passed through tension rolls and subsequently cut (cut) to the desired size for later formation into the final composite article.

[0063] In certain embodiments, the core layer described herein can be used with a skin layer to provide a composite article. With reference to FIG. 7, a skin layer 720 is shown disposed on a first surface of the core layer 410 to provide a composite article 700. The skin layer 720 can include, for example, a film, a scrim (e.g., a fiber-based scrim), a frim (film + scrim), a foil, a woven fabric, a nonwoven fabric, or can be present as an inorganic coating, an organic coating, or a thermosetting coating disposed on the core layer. In other cases, the layer 720 can include a limiting oxygen index greater than about 22 as measured by ISO 4589, 1996. When a fiber-based scrim is present as (or as part of) the skin layer 720, the fiber-based scrim can include at least one of glass fibers, aramid fibers, graphite fibers, carbon fibers, inorganic mineral fibers, metal fibers, metallized synthetic fibers, and metallized inorganic fibers. If a thermosetting coating is present as (or as part of) layer 720, the coating may include at least one of unsaturated polyurethane, vinyl ester, phenolic, and epoxy. If an inorganic coating is present as (or as part of) layer 720, the inorganic coating may include a mineral containing a cation selected from Ca, Mg, Ba, Si, Zn, Ti, and Al, or may include at least one of gypsum, calcium carbonate, and mortar. If a nonwoven fabric is present as (or as part of) layer 720, the nonwoven fabric may include a thermoplastic material, a thermosetting binder, inorganic fibers, metal fibers, metallized inorganic fibers, and metallized synthetic fibers. If desired, an intermediate layer (not shown) may be present between the core layer and the skin layer 720. For example, an adhesive layer or other layer of material may be present between the core layer 410 and the skin layer 720.

[0064] In some examples, the composite article may also include a second skin layer disposed on another surface of the core layer. With reference to FIG. 8, a composite article 800 is shown including skin layers 720, 820 sandwiching the core layer 410. Layer 820 may be the same as or different from layer 720. In some cases, layer 820 may include, for example, a film, a scrim (e.g., fiber-based scrim), a flim (film + scrim), a foil, a woven fabric, a nonwoven fabric, or may be present as an inorganic coating, an organic coating, or a thermoset coating disposed on the core layer. In other cases, layer 820 may include a limiting oxygen index greater than about 22 as measured by ISO 4589, 1996. When a fiber-based scrim is present as (or as part of) layer 820, the fiber-based scrim may include at least one of glass fibers, aramid fibers, graphite fibers, carbon fibers, inorganic mineral fibers, metal fibers, metallized synthetic fibers, and metallized inorganic fibers. If a thermosetting coating is present as (or as part of) layer 820, the coating may include at least one of unsaturated polyurethane, vinyl ester, phenolic, and epoxy. If an inorganic coating is present as (or as part of) layer 820, the inorganic coating may include a mineral containing a cation selected from Ca, Mg, Ba, Si, Zn, Ti, and Al, or may include at least one of gypsum, calcium carbonate, and mortar. If a nonwoven fabric is present as (or as part of) layer 820, the nonwoven fabric may include a thermoplastic material, a thermosetting binder, inorganic fibers, metal fibers, metallized inorganic fibers, and metallized synthetic fibers. If desired, an intermediate layer (not shown) may be present between the core layer and the skin layer 820. For example, an adhesive layer or other layer of material may be present between the core layer 410 and the skin layer 820.

[0065] In certain configurations, the composite article can include a decorative layer disposed on a surface of the core layer or on a skin layer. With reference to FIG. 9, an article 900 is shown including a decorative layer 830 disposed on a skin layer 720. Although not shown, the decorative layer can be disposed on the opposite surface of the core layer 410 or on the skin layer 820 shown in FIG. 8. In some examples, the decorative layer 930 can be configured as a decorative layer, a texturing layer, a coloring layer, or the like. For example, the decorative layer 930 can be formed from a thermoplastic film, such as, for example, polyvinyl chloride, polyolefin, thermoplastic polyester, thermoplastic elastomer, or the like. The decorative layer 930 can also be a multi-layer structure including a foam core formed from, for example, polypropylene, polyethylene, polyvinyl chloride, polyurethane, or the like. Fabrics can be bonded to the foam core, such as natural and synthetic fibers, organic fiber nonwovens after needle punching or the like, brushed fabrics, knit goods, flock fabrics, or woven fabrics made from other such materials. Fabrics can also be bonded to the foam core with thermoplastic adhesives, including pressure sensitive adhesives and hot melt adhesives such as polyamides, modified polyolefins, urethanes, and polyolefins. The decorative layer 930 may also be produced using spunbond, thermal bond, spunlace, meltblown, wet laid processes, and / or dry laid processes. Insulating or acoustical layers may also be bonded to one or more surfaces of the articles described herein, and the insulating or acoustical layers may be, for example, open cell or closed cell foams, open-ended or closed, as desired.

[0066] In certain embodiments, the LWRT articles described herein can be molded to a specific thickness. Although not necessarily in all cases, the molding temperature can be selected to increase the total volume of the lofting agent, thereby increasing the thickness of the LWRT article. LWRT articles without lofting agents can also loft to some degree during molding if compressed during the formation of the LWRT article. The exact molded thickness can vary as desired, with typical molded thicknesses ranging from about 1 cm to about 10 cm in the machine and cross directions, although other molded thicknesses can also be used.

[0067] In certain embodiments, the presence of bicomponent fibers, reinforcing fibers, loft agents, and thermoplastic materials in the core layer of an LWRT article, as described herein, can provide improved mechanical properties for a selected molding thickness.

[0068] In certain embodiments, an LWRT article comprising a core layer and a skin layer may comprise a peak load value of about 10 N / cm to about 40 N / cm in the machine direction and about 5 N / cm to about 30 N / cm in the cross direction when measured by SAE J949_200904 at a molded thickness of 1.5 cm to 4 cm in the machine direction and cross direction.

[0069] In certain embodiments, an LWRT article comprising a core layer and a skin layer may comprise a stiffness value of about 6 N / cm to about 50 N / cm in the machine direction and about 3 N / cm to about 30 N / cm in the cross direction when measured by SAE J949_200904 at a molded thickness of 1.5 cm to 4 cm in the machine direction and cross direction.

[0070] In certain embodiments, the LWRT article, including the core layer and the skin layers, has a compressibility of about 6 N / m in the machine direction when measured by SAE J949_200904 at a molded thickness of 1.5 cm to 4 cm in the machine direction and cross direction. 2 ~about 20N / m 2 , and approximately 4 N / m in the transverse direction 2 ~Approx. 12N / m 2The bending strength value may include

[0071] In some examples, the LWRT article, including the core layer and the skin layers, has a compressibility of about 800 N / m in the machine direction when measured according to SAE J949_200904 at a molded thickness of 1.5 cm to 4 cm in the machine direction and cross direction. 2 ~Approx. 1800N / m 2 , and about 500 N / m in the transverse direction 2 ~Approx. 1600N / m 2 The flexural modulus may include

[0072] In certain embodiments, the core layers and articles described herein can be used in architectural and automotive applications, such as, for example, headliners, rear window trim, trunk trim, office partition panels, cabinet back panels, automotive interior panels, or other automotive interior articles.

[0073] In certain embodiments, referring to FIG. 10, the articles described herein can be present in a headliner of a vehicle. Exemplary vehicles include, but are not limited to, automobiles, trucks, trains, subways, recreational vehicles, airplanes, ships, submarines, spacecraft, and other vehicles capable of transporting people or cargo. In some cases, the headliner typically includes a core layer including at least one prepreg, or bicomponent fiber, reinforcing fiber, thermoplastic material, lofting agent, one or more optional skin layers, and a decorative layer, such as a decorative fabric, disposed on or over the core layer. The decorative layer may also optionally include foam, insulation, or other materials in addition to being aesthetically and / or visually pleasing. An illustration of a top view of a headliner is shown in FIG. 10. The headliner 1000 includes a body 1010 and an opening 1020, for example, for a sunroof, moonroof, or the like. The body of the headliner 1010 may be produced using one or more core layers as described herein and a molding machine in which a decorative fabric is placed on the surface of the core layer and pressed in a desired mold to convert the article into a headliner of the desired shape. The opening 1020 may then be provided by trimming the headliner 1000. Non-visible surfaces of the headliner, such as the surface that mounts against the roof of the vehicle, may include one or more additional layers or adhesives as desired. The overall shape and geometry of the headliner may be selected based on the area of ​​the vehicle to which the headliner will be bonded. For example, the length of the headliner may be sized and positioned to span from the windshield to the rear windshield, and the width of the headliner may be sized and positioned to span from the left side of the vehicle to the right side of the vehicle. In some examples, the core layer of the headliner 1000 may include 20% to 80% by weight of reinforcing fibers and bicomponent fibers (collectively) and 20% to 80% by weight of thermoplastic material. In other embodiments, the reinforcing fibers include glass fibers and the thermoplastic material includes a polyolefin. The bicomponent fibers may include a core-shell configuration or other configurations as described herein.In some examples, an automotive headliner may provide peak load values, stiffness values, flexural strength values, and / or flexural modulus values ​​as discussed herein with respect to the core layer.

[0074] In certain cases, the core layer can also be used to manufacture other automotive interior components, including panels, trim pieces, and the like. An illustration of a rear window trim 1100 (top view) is shown in FIG. 11. The trim 1100 can include one or more of the core layers described herein, optionally with skin layers and / or decorative layers. In some examples, the core layer of an automotive component, such as a trim piece, can include 20% to 80% by weight of reinforcing fibers and bicomponent fibers (collectively) and 20% to 80% by weight of a thermoplastic material. In other embodiments, the reinforcing fibers include glass fibers and the thermoplastic material includes a polyolefin. The bicomponent fibers can include a core-shell arrangement or other arrangements as described herein. In some examples, the automotive trim or interior component can provide peak load values, stiffness values, flexural strength values, and / or flexural modulus values ​​as discussed herein in connection with the core layer.

[0075] In other configurations, the bicomponent fibers described herein can be used in non-automotive articles, such as furniture. For example, referring to FIG. 12, a display cabinet 1200 is shown including a top surface 1110, sides 1212, 1214 coupled to a front surface 1210, and a back surface 1220 coupled to the sides 1212, 1214. The surfaces 1210, 1212, 1214, and 1220 together form an interior storage area accessible to a user. Although not shown, the cabinet 1200 can include a front surface, e.g., a glass surface or other material for viewing the contents of the cabinet. Alternatively, a door or other device can be attached to the cabinet 1200 to shield the contents within the cabinet 1200 from view. One or more surfaces of the cabinet 1200 can be configured as an LWRT article, having a core layer including a TP material, reinforcing fibers, and bicomponent fibers. In some examples, the back surface 1220 can include a core layer including a web of reinforcing fibers and bicomponent fibers held together by a thermoplastic material. When two or more surfaces of the article 1200 include bicomponent fibers in layers, the layers do not have to have the same composition, thickness, or number of layers. In some examples, the core layer of the furniture article 1200 may include 20% to 80% by weight of reinforcing fibers and bicomponent fibers (collectively) and 20% to 80% by weight of a thermoplastic material. In other embodiments, the reinforcing fibers include glass fibers and the thermoplastic material includes a polyolefin. The bicomponent fibers may include a core-shell configuration or other configurations. In some examples, the furniture article 1200 or a panel thereof may provide peak load values, stiffness values, flexural strength values, and / or flexural modulus values ​​as discussed herein in connection with the core layer.

[0076] In some configurations, the furniture article can be configured to receive at least one drawer. For example, with reference to FIG. 13, a cabinet 1300 is shown to include a drawer 1310 and a back 1320. The back 1320 can include, for example, an LWRT article as described herein, such as one having bicomponent fibers. Other surfaces of the cabinet 1300 can also include an LWRT article as described herein. In other configurations, the furniture article 1300 can be configured to receive (or can include) at least one door. With reference to FIG. 14, a cabinet 1400 includes a door 1410 and a back 1420. The back 1420 can include, for example, an LWRT article as described herein. Other surfaces of the cabinet 1400 can also include an LWRT article as described herein. If desired, the exterior surface of the door 1410 can include an LWRT as described herein. If the cabinet includes a door, the door need not be closable by hinges 1412, 1414. Alternatively, the door can be configured as a sliding door 1510, as shown in cabinet 1500 in FIG.

[0077] To further illustrate some of the aspects of the technology described herein, certain specific examples are described.

[0078] Example 1 Several samples were prepared and tested to determine the properties of composite articles containing bicomponent fibers. The materials used in the tested samples and their numbering are shown in Table 1 below. PP stands for polypropylene. The polymer fibers tested are core-shell bicomponent fibers with LLDPE in the shell and polyethylene terephthalate in the core. [Table 1]

[0079] Example 2 The composite article of Example 1 was molded to different thicknesses. Table 2 below lists some of the different thicknesses for different articles. MD represents the longitudinal direction of the specimen, which corresponds to the machine direction, and CD represents the longitudinal direction of the specimen, which corresponds to the cross-machine direction. [Table 2]

[0080] Example 3 The peak load values ​​of the test specimens were measured using SAE J949_200904. A three-point bend test was used with the film side of the test specimen facing the load in the three-point bend test. The measured peak load values ​​for the tested specimens are shown in Table 3 below. [Table 3]

[0081] For all samples tested, the peak load values ​​in the machine and cross directions generally increase as the molded wall thickness increases. Comparing the peak load values ​​of samples with microspheres (ST-12244 and ST-12245) and samples without microspheres (ST-12242 and ST-12243), the peak load is generally higher for the microsphere-based samples of similar thickness. For example, at 2.6 cm thickness, the 990 gsm ST-12242b sample had peak load values ​​of 25.2 and 17.0 in the machine and cross directions, respectively. At 2.5 cm thickness, the 990 gsm ST-12244a sample had peak load values ​​of 32.2 and 21.1 in the machine and cross directions, respectively. Similar results are observed, for example, for the 790 gsm sample, where the MD and CD peak load values ​​for ST-12245a are greater than the MD and CD peak load values ​​for ST-12243c. These results are consistent with a combination of thermoplastic, reinforcing fibers, polymeric fibers, and microspheres providing improved peak load at a selected basis weight and molded thickness.

[0082] Example 4 The stiffness values ​​of the test specimens were measured using SAE J949_200904. A three-point bending test was used with the film side of the test specimen facing the load in the three-point bending test. The measured stiffness values ​​for the tested specimens are shown in Table 4 below. [Table 4]

[0083] Stiffness was generally lower for lighter products containing fewer fibers. Comparing stiffness values ​​for samples with microspheres (ST-12244 and ST-12245) and samples without microspheres (ST-12242 and ST-12243), stiffness was the same or higher for microsphere-based samples of similar thickness. For example, at a molded thickness of about 2.6 cm, the 990 gsm ST-12242b sample had a stiffness value of 21.0 in the machine direction. At a molded thickness of 2.5 cm, the 990 gsm ST-12244a sample had a stiffness value of 22.2. For these same samples, stiffness in the cross direction was reduced in the presence of microspheres. For the 790 gsm sample, the MD and CD stiffness values ​​for ST-12245a (10.1 and 7.6) are less than the MD and CD stiffness values ​​for ST-12243c (15.1 and 12.7). These results are consistent with the bicomponent fibers and microspheres providing an article that is the same or softer than without the microspheres.

[0084] Example 5 The flexural strength values ​​of the test samples were measured using SAE J949_200904. A three-point bending test was used with the film side of the test sample facing the load in the three-point bending test. The measured flexural strength values ​​for the tested samples are shown in Table 5 below. [Table 5]

[0085] Flexural strength generally decreased as mold thickness increased. Flexural strength was also generally lower for lighter articles containing fewer fibers. Comparing the flexural strength of samples with microspheres (ST-12244 and ST-12245) and samples without microspheres (ST-12242 and ST-12243), the flexural strength was the same or higher for microsphere-based samples of similar thickness. For example, at a mold thickness of about 2.6 cm, the 990 gsm ST-12242b sample had a flexural strength of 11.3 in the machine direction. At a mold thickness of 2.5 cm, the 990 gsm ST-12244a sample had a flexural strength of 15.1. For these same samples, the flexural strength in the transverse direction increased slightly in the presence of microspheres. For the 790 gsm samples, the MD and CD flexural strength values ​​for ST-12245a (14.5 and 10.2) were much higher than the MD and CD flexural strength values ​​for ST-12243c (8.9 and 6.3). These results are consistent with the bicomponent fibers and microspheres providing comparable or greater flexural strength.

[0086] Example 6 The flexural modulus values ​​of the test samples were measured using SAE J949_200904. A three-point bending test was used with the film side of the test sample facing the load in the three-point bending test. The measured flexural modulus values ​​for the tested samples are shown in Table 6 below. [Table 6]

[0087] The flexural modulus strength generally decreased with increasing mold thickness. Comparing the flexural modulus of samples with microspheres (ST-12244 and ST-12245) and samples without microspheres (ST-12242 and ST-12243), the flexural modulus was the same or higher for microsphere-based samples of similar thickness. For example, at a mold thickness of about 2.6 cm, the 990 gsm ST-12242b sample had a flexural modulus of 1389.6 in the machine direction. At a mold thickness of 2.5 cm, the 990 gsm ST-12244a sample had a flexural modulus of 1582.8. For these same samples, the flexural strength in the transverse direction increased in the presence of microspheres. For the 790 gsm sample, the MD and CD flexural modulus values ​​for ST-12245a (1546.7 and 1204.8) were much higher than the MD and CD flexural modulus values ​​for ST-12243c (1195.5 and 914.3). These results are consistent with the bicomponent fibers and microspheres providing comparable or higher flexural moduli.

[0088] Example 7 Glass / bicomponent polymer fiber hybrid LWRT (H-LWRT) and standard glass fiber LWRT (S-LWRT) sheets were produced by using the same wet-laid process. Polyolefin resin, chopped glass fiber, and bicomponent polymer fiber for H-LWRT were dispersed in water. The aqueous suspension of well-dispersed resin and fiber was transferred to a web forming section and an expansion agent was added to the continuous web. The resulting web was drained, heated, laminated with facing materials (scrim and film) and consolidated to produce flat LWRT composite sheets. By adjusting the manufacturing parameters, materials of various basis weights (areal densities) can be produced. The control sample (S-LWRT) was 650 g / m 2 This has a basis weight of 568 g / m2 for HLWRT. 2 It was about 14.4% heavier than

[0089] After being heated above the melting point of the resin, the material increases in thickness due to the release of residual stresses from the bent fibers as well as the expansion / lofting agents. Thus, all materials can be molded to thicknesses of 3.5-7 mm, which is thicker than the as-produced state / thickness (Table 1). Figure 16 shows one exemplary part molded from a sample B (H-LWRT) sheet. The material shows excellent formability to accommodate complex shapes in the mold.

[0090] Analytical properties including basis weight (areal density), as-formed thickness, and glass (ash) content were measured according to standard internal testing procedures. Tensile properties of 3 mm thick specimens were measured per ASTM D790. Flexural properties of molded specimens of 3.5, 4, 5.5, and 7 mm thickness were evaluated per ASTM D638. Table 7 shows the physical properties of S-LWRT and H-LWRT. [Table 7]

[0091] The control sample, S-LWRT, was 82 g / m2 lower than the two H-LWRT samples. 2 (14.4%) heavier. S-LWRT exhibits slightly lower thickness, indicating a slightly higher stabilization level. Samples A and B (H-LWRT) have different glass contents due to different weight percentages of the bicomponent polymer fibers.

[0092] Example 8 To evaluate the tensile properties of the samples shown in Table 7, the molded plaques with a thickness of 3.5 mm were cut into dog-bone tensile specimens by a punch press. Figure 17 is a graph showing the tensile modulus, and Figure 18 is a graph showing the tensile strength of sample A (H-LWRT), sample B (H-LWRT), and the control (S-LWRT). In terms of both tensile modulus and tensile strength, all three samples show significantly better results in the machine direction (MD) than in the cross-machine direction (CD). This can be attributed to the fiber orientation bias in favor of the machine direction, which occurs mainly in the headbox. The flow in the headbox is a mixture of both shear and elongation. The complex flow is characterized by shear close to the wall and can stretch toward the machine direction throughout the domain. As a result, the fibers can be strongly aligned toward the flow direction, leading to better mechanical performance in MD.

[0093] Sample B (H-LWRT) has the highest average tensile modulus in the MD, while the control (SLWRT) shows only a slightly higher average modulus than both samples A and B in the CD. In terms of tensile strength, all three samples perform very similarly in the MD. In the CD, sample A shows similar results to the control, and sample B is only slightly lower than the other two. In particular, the control (S-LWRT) has a higher average modulus of 82 g / m2 than both H-LWRT samples. 2 Heavy. It can be up to 82g / m without sacrificing tensile properties. 2 This means that the weight reduction of 100% is achieved by hybridizing bicomponent polymer fibers with glass fibers. The strength, especially in terms of tensile properties, depends heavily on the bond between the resin and the fiber. The bicomponent polymer fibers have components with a lower melting point than the matrix resin. During the heating and stabilization stage, the components with a lower melting point in the polymer fibers melt and bond to the glass fiber surface, which is believed to contribute to a better wet-out of the resin around the glass fiber.

[0094] Example 9 Flexural testing was performed on specimens molded at 3.5, 4, 5.5, and 7 mm. Figures 19A and 19B compare the peak load in both MD and CD between sample A (H-LWRT), sample B (HLWRT), and the control (S-LWRT). Similar to the tensile properties, the peak load results in MD are also better than those in CD. As thickness increases, the peak load drops due to increased porosity. Throughout the range of molded thicknesses, all three samples show very comparable peak load results. This includes up to 82 g / m without sacrificing the bending peak load. 2 is shown to be achieved by hybridizing bicomponent polymer fibers with glass fibers.

[0095] When introducing elements of the embodiments disclosed herein, the articles "a," "an," "the," and "said" are intended to mean that there is one or more elements. The terms "comprising," "including," and "having" are intended to be open-ended and mean that there may be additional elements other than the listed elements. Those skilled in the art will recognize, given the benefit of this disclosure, that various components of the embodiments may be interchanged or substituted for various components in other embodiments.

[0096] While particular aspects, examples, and embodiments have been described above, those of ordinary skill in the art, given the benefit of this disclosure, will recognize that additions, substitutions, modifications, and variations of the disclosed exemplary aspects, configurations, examples, and embodiments are possible.

Claims

1. A molded porous composite article comprising: a lofted core layer comprising inorganic reinforcing fibers, organic bicomponent fibers, a lofting agent comprising expandable microspheres, and a web formed from a polyolefin thermoplastic material, wherein the web comprises about 20% to about 80% porosity, the organic bicomponent fibers comprise a core-shell configuration, a core material of a core of the core-shell configuration comprises a melting point at least 20 degrees Celsius higher than the melting point of the thermoplastic material of the web, and the shell of the organic bicomponent fibers comprises a polyolefin, and wherein the molded porous composite article, when tested according to SAE J949_200904, comprises a peak load of 10N to about 40N in the machine direction and a peak load of about 6N to about 30N in the transverse direction at a molded thickness of about 2mm to about 4mm in both the machine and transverse directions.

2. The molded porous composite article of claim 1 , wherein the organic bicomponent fiber comprises a core comprising a polyamide.

3. The molded porous composite article of claim 1 , wherein the organic bicomponent fiber comprises a core comprising a polyester.

4. The molded porous composite article of claim 1, wherein the thermoplastic material of the web comprises polypropylene, the inorganic reinforcing fibers comprise glass fibers, and the organic bicomponent fibers comprise a polyester or polyamide in the core, and the molded composite article further comprises a flexural strength in the machine direction of about 6 MPa to about 17 MPa, a flexural modulus in the machine direction of about 800 MPa to about 2000 MPa, and a flexural modulus in the transverse direction of about 500 MPa to about 1300 MPa when tested according to SAE J949_200904.

5. The molded porous composite article of claim 1, wherein the thermoplastic material of the web comprises polypropylene, the inorganic reinforcing fibers comprise glass fibers, and the organic bicomponent fibers comprise a polyester or polyamide in the core, and wherein the molded composite article further comprises a stiffness in the machine direction of about 10 N / cm to about 50 N / cm and a stiffness in the transverse direction of about 7 N / cm to about 30 N / cm, when tested according to SAE J949_200904, a flexural strength in the machine direction of about 6 MPa to about 17 MPa and a flexural strength in the transverse direction of about 4 MPa to about 11 MPa, when tested according to SAE J949_200904, and a flexural modulus in the machine direction of about 800 MPa to about 2000 MPa and a flexural modulus in the transverse direction of about 500 MPa to about 1300 MPa, when tested according to SAE J949_200904.

6. The molded porous composite article of claim 3 , wherein the polyester comprises polyethylene terephthalate.

7. The molded porous composite article of claim 2 , wherein the polyamide comprises nylon.

8. The molded porous composite article of claim 3, wherein the thermoplastic material of the web is polypropylene, the inorganic reinforcing fibers are glass fibers, the polyolefin of the shell of the core-shell configuration comprises linear low density polyethylene, and the polyester of the core comprises polyethylene terephthalate.

9. The molded porous composite article of claim 2, wherein the thermoplastic material of the web is polypropylene, the inorganic reinforcing fibers are glass fibers, the polyolefin of the shell of the core-shell configuration comprises linear low density polyethylene, and the polyamide of the core comprises nylon.

10. The molded porous composite article of claim 1, wherein the thermoplastic material of the web comprises polypropylene, the inorganic reinforcing fibers comprise glass fibers, and the organic bicomponent fibers comprise a polyester or polyamide in the core, the melting point of the polyester or polyamide in the core being at least 20 degrees Celsius higher than the melting point of polypropylene of the thermoplastic material of the polyolefin of the web.

11. 11. The molded porous composite article of claim 10, wherein the molded composite article further comprises a stiffness in the machine direction of about 10 N / cm to about 50 N / cm and a stiffness in the cross direction of about 7 N / cm to about 30 N / cm when tested according to SAE J949_200904.

12. 11. The molded porous composite article of claim 10, wherein the molded composite article further comprises a flexural strength in the machine direction of about 6 MPa to about 17 MPa and a flexural strength in the transverse direction of about 4 MPa to about 11 MPa when tested according to SAE J949_200904.

13. 11. The molded porous composite article of claim 10, wherein the molded composite article further comprises a flexural modulus in the machine direction of about 800 MPa to about 2000 MPa and a flexural modulus in the transverse direction of about 500 MPa to about 1300 MPa when tested according to SAE J949_200904.

14. 11. The molded porous composite article of claim 10, wherein the molded composite article further comprises a stiffness in the machine direction of about 10 N / cm to about 50 N / cm and a stiffness in the transverse direction of about 7 N / cm to about 30 N / cm when tested according to SAE J949_200904, and a flexural strength in the machine direction of about 6 MPa to about 17 MPa and a flexural strength in the transverse direction of about 4 MPa to about 11 MPa when tested according to SAE J949_200904.

15. 11. The molded porous composite article of claim 10, wherein the molded composite article further comprises a stiffness in the machine direction of about 10 N / cm to about 50 N / cm and a stiffness in the transverse direction of about 7 N / cm to about 30 N / cm when tested according to SAE J949_200904, and a flexural modulus in the machine direction of about 800 MPa to about 2000 MPa and a flexural modulus in the transverse direction of about 500 MPa to about 1300 MPa when tested according to SAE J949_200904.

16. 11. The molded porous composite article of claim 10, wherein the molded composite article further comprises a flexural strength in the machine direction of about 6 MPa to about 17 MPa, and a flexural modulus in the machine direction of about 800 MPa to about 2000 MPa and a flexural modulus in the transverse direction of about 500 MPa to about 1300 MPa when tested according to SAE J949_200904.

17. 11. The molded porous composite article of claim 10, wherein the molded composite article further comprises a stiffness in the machine direction of about 10 N / cm to about 50 N / cm and a stiffness in the transverse direction of about 7 N / cm to about 30 N / cm when tested according to SAE J949_200904, a flexural strength in the machine direction of about 6 MPa to about 17 MPa and a flexural strength in the transverse direction of about 4 MPa to about 11 MPa when tested according to SAE J949_200904, and a flexural modulus in the machine direction of about 800 MPa to about 2000 MPa and a flexural modulus in the transverse direction of about 500 MPa to about 1300 MPa when tested according to SAE J949_200904.

18. The molded porous composite article of any one of claims 1 to 17, wherein the article is configured as an automobile headliner.

19. The molded porous composite article of any one of claims 1 to 17, wherein the article is configured as an interior automotive component.

20. The molded porous composite article of any one of claims 1 to 17, wherein the article is configured as a cubicle panel or a furniture panel.

Citation Information

Patent Citations

  • Heat-expandable nonwoven fabric

    JP2012107350A

  • Laminated nonwoven fabric

    JP2013221217A

  • Method for producing three-layer nonwoven fabric

    JP2015080899A

  • Composite articles including surface layers that provide enhanced formability

    WO2018111781A1