Thermoplastic starch and its manufacturing method

The continuous mixer and single screw extruder method for thermoplastic starch production maintains molecular weight and reduces wear, addressing the limitations of conventional extrusion by using a low shear process and specific ingredient ratios, resulting in high-quality starch with improved properties.

JP7554201B2Active Publication Date: 2024-09-19GREEN DOT BIOPLASTICS INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021553764
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-15
Filing Date
2020-03-13
Publication Date
2024-09-19
Estimated Expiration
2040-03-13

AI Technical Summary

Technical Problem

Conventional twin screw extrusion processes for producing thermoplastic starch result in loss of molecular weight and increased machinery wear, leading to high costs and reduced physical strength, while alternative methods involve complex processes with excessive water addition and downstream processing.

Method used

A continuous mixer is used to gelatinize starch with a low shear process, followed by a single screw extruder to form thermoplastic starch without significant molecular weight change, using a composition of 50-75% starch, 15-30% plasticizer, and 5-20% water, operated at specific temperatures and pressures.

Benefits of technology

The process maintains starch molecular weight, reduces machinery wear, and eliminates the need for downstream moisture removal, producing high-quality thermoplastic starch with improved elongation properties and lower costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554201000002
    Figure 0007554201000002
  • Figure 0007554201000003
    Figure 0007554201000003
  • Figure 0007554201000001
    Figure 0007554201000001
Patent Text Reader

Abstract

A thermoplastic starch material and method for its manufacture are provided. The method involves mixing a starch material, a plasticizer, and water in a low-shear mixer under conditions that result in substantial gelatinization of the starch material. The melt formed in the mixer is discharged into an extruder for final processing. The method prevents degradation of the starch material, thereby resulting in the formation of a thermoplastic starch material with high strength, due at least in part to preservation of the molecular weight characteristics of the starch, and improved elasticity due to the ability to use higher moisture contents than conventional processes.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] Related Applications This application claims the benefit of U.S. Provisional Patent Application No. 62 / 819,006, filed March 15, 2018, which is incorporated herein by reference in its entirety.

[0002] 2. Background of the Invention FIELD OF THEINVENTION The present invention relates generally to a thermoplastic starch material and a method for producing the material, which includes a low shear digestion stage located upstream of the extrusion device from which the material is ultimately obtained. The method of the present invention allows for the efficient production of high quality thermoplastic starch products from low cost starting materials.

[0003] Description of the Prior Art Historically, the most common method of producing thermoplastic starch (TPS) was to use a conventional twin screw extruder (TTSE). Starch, water, and plasticizers were added to the TTSE, and heat generated by a heating element in the barrel and friction in the screw caused gelatinization of the starch, thereby creating a thermoplastic material. This process involved the creation of high pressure and high shear conditions in the extruder, which ultimately resulted in loss of starch molecular weight, which adversely affected the physical strength of the thermoplastic starch material. It was discovered that this adverse effect could be mitigated by increasing the water content of the melt. However, there are practical limits to the amount of water that can be used and the amount of water that can be used to chop the material into pellets as it exits the extruder. If the water content is too high, the polymer becomes too soft. At the same time, the materials and conditions used can cause significant wear on the machinery, often resulting in the use of more expensive materials to build the extruder. This also increases the already high capital costs of the TTSE equipment.

[0004] Because of these problems, other processes for producing TPS have been developed. One such process is described in U.S. Patent No. 6,136,097. These solutions often involve complex processes with many steps and many downstream facilities required. They all require the addition of large amounts of water to the starch in the cooking stage of the process, which is then removed. Once this water is removed, further processing must occur to render the TPS into a usable form. Summary of the Invention

[0005] Certain embodiments of the present invention overcome the above problems by providing a simple, efficient, low-cost method using a continuous mixer to produce thermoplastic starch products at higher quality and lower cost than traditional extrusion processes.

[0006] According to one embodiment of the present invention, a process for producing thermoplastic starch is provided. The process includes mixing a composition comprising about 50% to about 75% by weight starch, about 15% to about 30% by weight plasticizer, and about 5% to about 20% by weight water in a continuous mixer. The mixing step includes operating the mixer at a temperature of about 150°F to about 200°F to gelatinize the starch and form a melt. The melt is then discharged from the continuous mixer and fed to a single screw extruder. The extruder is operated at a temperature of about 150°F to about 250°F. The melt is then extruded through a die at a die pressure of about 1500 psi to about 2500 psi.

[0007] According to yet another embodiment of the present invention, there is provided a process for producing thermoplastic starch. The process includes mixing a composition comprising about 50% to about 75% by weight of non-pregelatinized native or modified starch, about 15% to about 30% by weight of glycerin, and about 5% to about 20% by weight of water in a heated twin screw continuous mixer. The mixing step includes operating the mixer at a temperature of about 150°F to about 200°F to gelatinize the starch and form a melt. The melt exits the continuous mixer as a rope and is fed directly into a single screw extruder. The single screw extruder is operated at a temperature of about 150°F to about 250°F. The melt is then extruded through a die at a die pressure of about 1500 psi to about 2500 psi. The mixing and extrusion steps do not substantially change the molecular weight of the starch added to the mixer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention generally relates to a process for the manufacture of thermoplastic starch (TPS). The TPS can be formed into pellets, sheets, or films to produce articles, or the TPS can be compounded with other plastic materials, such as biodegradable plastics, before being formed into a final product. In a particular embodiment, the process according to the invention comprises, consists of, or consists essentially of two steps. In the first step, ingredients including starch, one or more plasticizers, and water are mixed in a continuous mixer under heating. In the second step, the melt exiting the mixer is extruded to form the TPS.

[0009] As described in more detail below, the present invention advantageously provides a process in which inexpensive, uncooked, native or modified starch can be combined with a plasticizer and cooked before being extruded. It has been discovered that cooking or gelatinizing the starch upstream of the extruder imparts favorable properties to the TPS, such as improved elongation properties, without substantially affecting the molecular weight properties of the starch, which would result in a loss of strength of the TPS. As used herein, the term "gelatinized" refers to cooking of starch in which the starch molecules are opened to allow water molecules to penetrate into the starch. The process of gelatinization transforms the starch molecules from their native or crystalline form to an amorphous state.

[0010] In certain embodiments, the continuous mixer includes an elongated twin-shaft mixer, preferably of the type shown and described in U.S. Patent No. 7,350,690, the entirety of which is incorporated herein by reference. In a particularly preferred embodiment, each of the mixer screws includes a Levenhertz flight disposed upstream of a standard screw flight. Also, in certain embodiments, the continuous mixer has a compression ratio of about 3:1. In certain embodiments, the L / D ratio of the mixer (the ratio of the length to the diameter of the mixing screw) is about 10:1 or less.

[0011] Typically, a continuous mixer is configured to receive both dry and liquid ingredients, blend or mix them under heat, and then discharge the mixed ingredients through an adjustable aperture outlet. By increasing the size of the mixer outlet, the material in the mixer can exit more freely, thereby experiencing less heat, back pressure, and mixing shear. However, if more heat and mixing is required, the aperture can be adjusted smaller. Additionally, the design of the screw in the barrel can also adjust the amount of mixing and shear-induced heat.

[0012] The starch component fed to the mixer includes starch obtained from plant sources such as cereal plants (e.g., corn, wheat, rice, barley, triticale and sorghum), tubers (e.g., potato and cassava), legumes (e.g., pea, soybean and bean), or starch derived from other non-food cellulosic materials and biomass. Most preferably, the starch is native wheat, corn or potato starch. However, it is within the scope of the present invention for modified starches (e.g., pregelatinized starches or high amylose starches) to be used, so long as the modifications to the starch do not interfere with its ability to be gelatinized in the mixer.

[0013] According to certain embodiments of the present invention, the plasticizer component may be any suitable material known to improve the flexibility of polymer resin materials. Exemplary plasticizers include various modified or unmodified vegetable oils, fatty acids, polyols, ethers, thioethers, inorganic and organic esters, acetals, and their derivatives. Particularly preferred plasticizers include organic acid derived plasticizers, especially organic acid ester plasticizers (e.g., citric acid derived plasticizers), adipic acid derivatives such as tridecyl adipate adipate, benzoic acid derivatives such as isodecyl benzoate, and glycerin.

[0014] The ingredients blended in the mixer can also include one or more optional solid or liquid ingredients, such as those selected from the group consisting of glycerol monostearate, metal stearates, internal or external lubricants, natural fibers, fillers, reinforcing materials, additional starches having higher or lower molecular weight than the primary starch component, and sugars.

[0015] In a preferred embodiment of the present invention, the ingredients may be added and blended in a mixer at the approximate levels set forth in Table 1.

[0016] [Table 1]

[0017] In certain embodiments, the ingredients are mixed in a mixer at a temperature of about 150°F to about 200°F and a mixer screw speed of 140-250 rpm, preferably 150-200 rpm, to gelatinize the starch and form a melt. The pressure in the mixer is at or near atmospheric pressure. In certain embodiments, the pressure in the mixer is less than 5 bar, less than 3 bar, less than 2 bar, about 1 bar, or from about 1 bar to about 2 bar. The mixer provides relatively low shear to the melt so as not to overcook the starch or substantially affect the molecular weight of the starch. In certain embodiments, the shear rate during mixing is about 590 s -1 ~about 280 -1 Also, in certain embodiments, the amount of mechanical energy input to the ingredients in the mixer is about 75 to about 150 Wh / kg, about 85 to about 145 Wh / kg, or about 90 to about 130 Wh / kg. However, in other embodiments, the amount of mechanical energy applied to the ingredients in the mixer is less than 100 J / g, or less than 90 J / g, or less than 80 J / g. As mentioned above, the main function of the mixer is to cook or gelatinize the starch, and the majority of the starch gelatinization that occurs in the manufacturing process occurs in the mixer. It is preferred to cook at least 70%, preferably at least 80%, and more preferably at least 90% of the starch in the mixer. In certain embodiments, the starch is fully gelatinized in the mixer (maximum possible gelatinization is achievable).

[0018] The melt exits the barrel of the mixer through an adjustable opening as a thick strand or rope. The rope of homogeneous, molten material then travels a short distance into the feed throat of the extruder. The melt temperature of the rope exiting the mixer is preferably about 190°F to about 200°F. The rope preferably travels a relatively short distance (e.g., less than 36 inches) into the inlet of the extruder. During this short period of time, at least a portion of the excess moisture in the melt, if any, flashes off.

[0019] In a preferred embodiment, the extruder used in this second step of the process is a common single screw extruder sized to feed the output of the mixer, but it is within the scope of the invention to use other types of extruders and screw configurations. The extruder can be set to provide the additional heat and time necessary to complete the gelatinization of the starch that began in the mixer, and to vent the material to ensure the removal of excess moisture and compaction of the melt. The action of the extruder also ensures that the TPS material has the correct product structure. The loss of excess moisture means that it can produce fully gelatinized strands of starch that can be cut into pellets in a die or easily produce any extrudable shape (profiles, sheets, films, etc.) without any further downstream processing or processing required, as disclosed in U.S. Pat. No. 6,136,097, the entirety of which is incorporated herein by reference.

[0020] In certain embodiments, the extruder barrel temperature is set at about 130°F to about 170°F, or about 140°F to about 160°F, or about 150°F, but can be operated over a much wider range, such as about 150°F to about 250°F, preferably about 180°F to about 220°F. The melt is extruded through the die at a pressure of about 1500 psi to about 2500 psi, preferably about 1800 psi to about 2200 psi. In certain embodiments, the extrudate has a die temperature of about 175°F to about 220°F, about 185°F to about 205°F, or about 190°F. The extruder die may be configured to form the extruded melt into a sheet or film, or to prepare the extruded melt to pass through a pelletizer, whereby the extruded melt is formed into pellets. In certain embodiments, some water may be driven off from the melt during passage through the die, but most typically no released steam is visually observed. In certain embodiments, the L / D ratio of the extruder (ratio of the length to diameter of the extruder screw) is about 10:1 or less.

[0021] It is an advantage of certain embodiments of the invention with respect to the mixing and extrusion process that the molecular weight of the starch component initially added to the mixer is not substantially altered. In preferred embodiments, the number average molecular weight, weight average molecular weight, peak molecular weight, and polydispersity (Mw / Mn) of the starch are altered by less than 5%, less than 3%, or less than 1%. In certain embodiments, the starch present in the TPS has a molecular weight (Mw, Mn, or Mp) that is at least 90%, at least 95%, or at least 98% of the molecular weight of the starch initially added to the mixer. In certain embodiments, the finished TPS product exiting the extruder is transparent or translucent. However, it is within the scope of the invention to add colorants to the melt during mixing or prior to extrusion, if desired. It is also an advantage of certain embodiments of the invention that the evacuation (e.g., vacuuming) and evaporation of moisture from within the material being mixed and extruded is not required.

[0022] The TPS produced according to the present invention can be used alone to make articles, or can be blended with other plastics and polymers, especially biodegradable polymers, and then molded into articles using various means known to those skilled in the art, such as injection molding. Additional modified or complexed polymers with which the TPS can be blended include plasticizers such as polyols and polyol derivatives, esters, ester-modified thermoplastic cellulose polymers, urethane prepolymers, diacids, or other compounds that can impart desired properties to the starch component. In other embodiments, the modified or complexed polymers can include water-soluble polymers such as polycaprolactone (PCL), aromatic copolyesters (PBAT), aliphatic polyesters (PBS), polyvinyl alcohol (PVOH), or polyesters of renewable origin such as polylactates (PLA), microbial polyhydroxyalkanoates (PHAs), or cellulose derivatives.

[0023] In addition to the above, in certain embodiments, it is preferred that no fibers or fibrous materials are added to the material processed in the mixer and / or extruder. In certain embodiments, it is preferred that the material processed in the mixer and / or extruder does not contain wood fibers, wood flour, or any other type of cellulosic material. In certain embodiments, it is preferred that the material processed in the mixer and / or extruder does not contain inorganic mineral fillers.

[0024] Working Example The following examples illustrate preferred thermoplastic starch materials and methods for making said materials according to the present invention, however, it should be understood that these examples are given by way of illustration and that nothing therein should be taken as a limitation on the overall scope of the invention.

[0025] Example 1 In this example, the TPS material was made from wheat starch (MIDSOL 50 from MGP Ingredients), glycerin (industrial / technical grade 99.7% from KIC Group), and water. These ingredients were mixed and extruded using a continuous mixer and single screw extruder, Model 2FR from Technical Process and Engineering, Inc. The mixer configuration is generally described in U.S. Patent No. 7,350,960. Dry ingredients were added to the continuous mixer using a loss-in-weight powder feeder from Brabender. Water was added using a peristaltic pump for liquids.

[0026] The continuous mixer temperatures were set at 188°F at the feed section and 190°F at the discharge section. The mixer screw speed was set at 240 rpm. The rotor used in the mixer was a low shear TPEI #17 rotor. Glycerin and water were mixed to form a solution in a ratio of 67% glycerin and 33% water by weight. Starch was fed to the mixer at 30 lbs / hr and the liquid solution was fed at 25 lbs / hr. The resulting mixture contained 54.5% starch, 30.5% glycerin, and 15% water by weight.

[0027] The mixture was passed through a continuous mixer at the conditions described above and exited as a continuous molten rope. The temperature of the molten rope was measured several times and was between 190°F and 200°F. The molten rope was directed into a single screw extruder using a 3:1 compression screw. The single screw extruder temperatures were set at 220°F at the barrel and 230°F at the die. The screw speed was 10 rpm and the thermoplastic starch was extruded into strands and then strand pelletized without the use of a water bath.

[0028] Example 2 In this example, the TPS material was made from wheat starch (MIDSOL 50 from MGP Ingredients), glycerin (industrial / technical grade 99.7% from KIC Group), and water. These ingredients were mixed and extruded using a continuous mixer and single screw extruder, Model 2FR from Technical Process and Engineering, Inc. The mixer configuration is generally described in U.S. Patent No. 7,350,960. Dry ingredients were added to the continuous mixer using a loss-in-weight powder feeder from Brabender. Water was added using a peristaltic pump for liquids.

[0029] The continuous mixer temperatures were set at 155°F in the feed section and 180°F in the discharge section. The screw speed was set at 145 rpm. The rotor used in the mixer was a low shear TPEI #17 rotor. Glycerin and water were mixed to form a solution in a ratio of 67% glycerin and 33% water by weight. Starch was fed to the mixer at 35 lbs / hr and the liquid solution was fed at 15 lbs / hr. The resulting mixture contained 70% starch, 20.1% glycerin, and 9.9% water by weight.

[0030] The mixture was passed through a continuous mixer under the conditions described above and emerged as a continuous molten rope. The temperature of the molten rope was measured several times and was between 200°F and 210°F. The molten rope was directed into a single screw extruder using a 3:1 compression screw. The single screw extruder temperatures were set at 150°F at the barrel and 200°F at the die. The screw speed was 8 rpm. A die pressure of 2100 psi was achieved using a die with three 0.125 inch diameter holes. A hot face pelletizer was attached to the face of the die and the extrudate was pelletized.

[0031] Example 3 In this example, the TPS material was made from pregelatinized wheat starch (PREGEL 10 from MGP Ingredients), glycerin (industrial / technical grade 99.7% from KIC Group), and water. These ingredients were mixed and extruded using a continuous mixer and single screw extruder, Model 2FR from Technical Process and Engineering, Inc. The mixer configuration is generally described in U.S. Patent No. 7,350,960. Dry ingredients were added to the continuous mixer using a loss-in-weight powder feeder from Brabender. Water was added using a peristaltic pump for liquids.

[0032] The continuous mixer temperatures were set at 150°F in the feed section and 185°F in the discharge section. The screw speed was set at 117 rpm. The rotor used in the mixer was a low shear TPEI #17 rotor. Glycerin and water were mixed to form a solution in a ratio of 67% glycerin and 33% water by weight. Starch was fed to the mixer at 35 lbs / hr and the liquid solution was fed at 15 lbs / hr. The resulting mixture contained 70% starch, 20.1% glycerin, and 9.9% water by weight.

[0033] The mixture was passed through a continuous mixer under the conditions described above and emerged as a continuous molten rope. The temperature of the molten rope was measured several times and found to be stable at approximately 190°F. The molten rope was directed into a single screw extruder using a 3:1 compression screw. The single screw extruder temperatures were set at 180°F at the barrel and 200°F at the die. The screw speed was 12 rpm. A die with three holes, 0.125 inches in diameter, was used to obtain a die pressure of 1,900-2,100 PSI. A hot face pelletizer was attached to the face of the die and the extrudate was pelletized.

[0034] Molecular weight evaluation To determine if any significant changes in the molecular weight of the starch occurred due to the TPS manufacturing process, two samples were sent to an independent laboratory for testing. The first sample was the raw wheat starch (MIDSOL 50) used in Examples 1 and 2. The second sample was the TPS made in Example 2. The laboratory developed a method to analyze the molecular weight of the starch in the two materials.

[0035] Solutions containing the samples were prepared at approximately 0.8 mg / ml concentration using the mobile phase DMSO+DMAC (4:1)+0.1% LiBr as diluent. The sample solutions were placed in a 50°C oven for 2 hours to aid in elution, then removed from the oven and allowed to acclimate to ambient temperature for 16 hours. Upon visual inspection, the samples appeared to be completely dissolved in the diluent and did not precipitate at room temperature. All samples were filtered through 0.45 μm nylon filters. The samples filtered easily without resistance. All samples were analyzed using a Waters 2695 Alliance Separation Module System. The system was equipped with a polyester copolymer column set with refractive index detection. A series of narrow pullulan standards were used for calibration. The calibration standards ranged from 180 to 1.22 M Daltons. The results of the molecular weight tests are shown in Table 2.

[0036] [Table 2] Mn = number average molecular weight; Mw = weight average molecular weight; Mp = peak molecular weight; PDI = polydispersity index

[0037] As can be seen, there was minimal change in molecular weight before and after treatment. The starch contained in the TPS material showed a slight increase in Mn of 3%. The Mw of the starch contained in the TPS material showed a decrease of 0.5%. The Mp of the starch contained within the TPS material was nearly identical to that of native starch, as was the PDI. These results demonstrate that the process of preparing the TPS did not cause any significant damage to the molecular weight of the starch.

[0038] Physical property evaluation The physical properties of the thermoplastic starch prepared in Example 2 were compared with those of a sample of thermoplastic starch made using a conventional twin screw extruder (CTPS), i.e., without an elongated mixer upstream of the extruder. Both thermoplastic starches contained the same ingredients. The thermoplastic starch was then blended with a biodegradable polyester, polybutylene adipate terephthalate (PBAT), available from BASF and known under the trade name ECOFLEX.

[0039] Compounding was done in a 35mm twin screw extruder. The feed zone of the barrel was heated to 380°F and the remainder of the barrel zone was 360°F. The screw speed was 220 rpm and the total feed rate of the ingredients was 60 lbs / hr. The formulation for both compounded materials was 70% PBAT and 30% TPS.

[0040] The resulting compounds were injection molded into standard tensile bars and then tested for tensile properties, the results of which are shown in Table 3.

[0041] [Table 3]

[0042] As the above data shows, there are significant differences between the two materials: the TPS from Example 2 exhibits higher modulus, elongation, break stress and yield stress than the conventionally produced CTPS, indicating that a stronger, yet more elastic material can be produced.

[0043] Tensile tests were also performed on samples from Examples 1 and 3. As before, using the process conditions described above, TPS samples were compounded in PBAT at a ratio of 30% TPS to 70% PBAT.

[0044] With reference to the above examples, the main differences between the TPS of Examples 1-3 are as follows: The TPS from Example 1 was made with native wheat starch and contained 30% glycerin and 15% water. The TPS from Example 2 was also made with native wheat starch, but contained 20% glycerin and 10% water. The TPS from Example 3 was also made with 20% glycerin and 10% water, but contained pre-cooked wheat starch instead of native starch. Thus, by comparing Example 1 and Example 2, the effect of higher liquid levels on the TPS material can be observed. Also, the gelatinization level achieved in the mixing process can be determined by comparison with the pre-gelatinized starch in Example 3. Lower strength and elasticity should indicate a lower degree of gelatinization. The results are shown in Table 4.

[0045] [Table 4]

[0046] This data shows that because the liquid acts as a plasticizer in the TPS, the higher liquid level of the TPS from Example 1 produced a much less stiff and more elastic composite than those of the TPS from Examples 2 and 3. The nearly identical results of the TPS from Examples 2 and 3 also indicate that the gelatinization level of the native starch in the mixer was close to 100% of the pregelatinized starch.

[0047] Example 4 In this example, the TPS material was made from wheat starch (MIDSOL 50 from MGP Ingredients), glycerin (industrial / technical grade 99.7% from KIC Group), and water. These ingredients were mixed and extruded using a continuous mixer and single screw extruder, Model 2FR from Technical Process and Engineering, Inc. The mixer configuration is generally described in U.S. Patent No. 7,350,960. Dry ingredients were added to the continuous mixer using a loss-in-weight powder feeder from Ktron. Water was added using a peristaltic pump for liquids.

[0048] The continuous mixer temperatures were set at 180°F in the feed section and 190°F in the discharge section. The screw speed was set at 300 RPM. The rotor used in the mixer was a low shear TPEI #7 rotor. Glycerin and water were mixed to form a solution in a ratio of 67% glycerin, 33% water. Starch was fed to the mixer at 30 lbs / hr and the liquid solution was fed at 20 lbs / hr. The resulting mixture contained 60% starch, 26.8% glycerin, and 13.2% water by weight.

[0049] The mixture was passed through a continuous mixer at the conditions described above and exited as a continuous molten rope. The specific energy of the mixer was calculated to be about 64 watts per kilogram x hours at these conditions. The temperature of the molten rope was 165°F. The molten rope was directed to a single screw extruder with a 3:1 compression ratio screw. The single screw extruder was set at 180°F-190°F on the barrel and 200°F at the die. The screw speed was 10 RPM. The thermoplastic starch was extruded into strands and then strand pelletized without the use of a water bath.

[0050] Molecular weight evaluation To determine if any significant changes in molecular weight occurred due to the TPS manufacturing process, two samples were sent to an independent laboratory for testing. The first sample was the raw wheat starch used in this example. The second sample was the TPS made in this example. The method used by the laboratory to analyze the molecular weight of the starch in the two materials is described in Example 3 above. The results of the molecular weight testing are shown in Table 5.

[0051] [Table 5]

[0052] The results of this example show that the total energy input to the TPS material in the mixer can be reduced (as indicated by the rope temperature exiting the mixer) compared to the previous example, while achieving a similar molecular weight profile.

[0053] Example 5 In this example, the TPS material was made from wheat starch (MIDSOL 50 from MGP Ingredients), glycerin (industrial / technical grade 99.7% from KIC Group), and water. These ingredients were mixed and extruded using a continuous mixer and single screw extruder, Model 2FR from Technical Process and Engineering, Inc. The mixer configuration is generally described in U.S. Patent No. 7,350,960. Dry ingredients were added to the continuous mixer using a loss-in-weight powder feeder from Ktron. Water was added using a peristaltic pump for liquids.

[0054] The continuous mixer temperatures were set at 140°F at the feed section and 195°F at the discharge section. The screw speed was set at 950 RPM. The rotor used was a low shear TPEI #7 rotor. Glycerin and water were mixed to form a solution in a ratio of 67% glycerin, 33% water. Starch was fed to the mixer at 120 lbs / hr and the liquid solution was fed at 80 lbs / hr. The resulting mixture contained 60% starch, 26.8% glycerin, and 13.2% water by weight.

[0055] The mixture passed through a continuous mixer at the conditions described above and exited as a continuous molten rope. The specific energy of the mixer was calculated to be about 64 watts per kilogram x hour at these conditions. The molten rope then entered a single screw extruder with a 3:1 compression ratio screw. The single screw extruder temperatures were set at 200°F-220°F on the barrel and 220°F at the die. The screw speed was 35 RPM. The thermoplastic starch was extruded into strands and then strand pelletized without the use of a water bath.

[0056] Molecular weight evaluation To determine if any significant changes in molecular weight occurred due to the TPS manufacturing process, two samples were sent to an independent laboratory for testing. The first sample was the raw wheat starch used in this example. The second sample was the TPS made in this example. The method used by the laboratory to analyze the molecular weight of the starch in the two materials is described in Example 3 above. The results of the molecular weight testing are shown in Table 6.

[0057] [Table 6]

[0058] The results of this example demonstrate that the process can be scaled up (increasing the throughput from 50 lbs / hr as in Example 4 to 200 lbs / hr in this example) without affecting the molecular weight profile of the material.

Claims

1. 1. A process for producing thermoplastic starch comprising the steps of: mixing a composition comprising about 50 to about 75% by weight starch, about 15 to about 30% by weight plasticizer, and about 5 to about 20% by weight water in a continuous mixer, operating the mixer at a temperature of about 150° F. to about 200° F. to gelatinize the starch and form a melt; discharging the melt from the continuous mixer and feeding the melt to an extruder; operating said extruder at a temperature of from about 150° F. to about 250° F.; and extruding said melt through a die at a die pressure of about 1500 psi to about 2500 psi.

2. 2. The process of claim 1, wherein the plasticizer is selected from the group consisting of glycerin, citric acid-based plasticizers, modified or unmodified vegetable oils, and fatty acids.

3. 3. The process of claim 2, wherein the plasticizer is glycerin.

4. 2. The process of claim 1, wherein the starch is selected from the group consisting of native or modified wheat starch, native or modified corn starch, and native or modified potato starch.

5. The process of claim 1 , wherein the continuous mixer comprises an elongated twin-shaft mixer.

6. The process described in claim 5, wherein each of the mixer screws includes a Lewenhertz thread flight positioned upstream of a standard screw flight.

7. 6. The process of claim 5, wherein the continuous mixer has a compression ratio of about 3:

1.

8. 2. The process of claim 1, wherein the shear rate during mixing is from about 590 s-1 to about 280 s-1.

9. 10. The process of claim 1, wherein the melt exits the continuous mixer as a rope.

10. 10. The process of claim 1, wherein one or more additional solid or liquid ingredients are added to the continuous mixer along with the starch, plasticizer, and water.

11. 11. The process of claim 10, wherein the one or more additional solid or liquid ingredients are selected from the group consisting of glycerol monostearate, metal stearates, internal or external lubricants, natural fibers, fillers, reinforcing materials, additional starches having higher or lower molecular weight than the starch, and sugars.

12. The process of claim 1 , wherein one or more lubricants and / or additional plasticizers are added to the melt in the extruder.

13. 10. The process of claim 1 further comprising pelletizing the extruded melt upon exiting the extruder die.

14. 10. The process of claim 1, wherein the extruder die is configured to form the melt into a sheet or film.

15. 10. The process of claim 1, wherein the mixing and extruding steps do not substantially change the molecular weight of the starch added to the mixer.

16. 1. A process for producing thermoplastic starch comprising the steps of: mixing a composition comprising about 50% to about 75% by weight of non-pregelatinized native or modified starch, about 15% to about 30% by weight of glycerin, and about 5% to about 20% by weight of water in a heated twin-shaft continuous mixer, operating the mixer at a temperature of about 150° F. to about 200° F. to gelatinize the starch and form a melt; discharging the melt from the continuous mixer as a rope and feeding the melt directly into a single screw extruder; operating the single screw extruder at a temperature of about 150° F. to about 250° F.; and extruding the melt through a die at a die pressure of about 1500 psi to about 2500 psi; A process for producing thermoplastic starch, wherein the mixing and extrusion steps do not substantially change the molecular weight of the starch added to the mixer.

Citation Information

Patent Citations

  • Biodegradable plalstic composition containing gelatinized starch and production thereof

    JP1993331315A

  • Biodegradable plastic molding

    JP1996188671A

  • Melt processable starch composition

    JP2000327840A

  • Starch-containing biodegradable plastic and method of producing same

    US5256711A

  • Melt processable starch compositions

    US6709526B1