Preparation method of high-hardness flame-retardant ultrathin fiberboard

Through the combination technology of modified biomass fibers and flame retardant, the problem of insufficient hardness and flame retardancy of ultra-thin fiberboard was solved, and high-hardness flame retardant ultra-thin fiberboard was prepared, suitable for electronic circuit printing pads and packaging fields, with Good physical and mechanical properties and safety.

CN119017499AActive Publication Date: 2024-11-26GUANGXI UNIV

Patent Information

Application Number
CN202411465806.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-21
Publication Date
2024-11-26
Estimated Expiration
2044-10-21

AI Technical Summary

Technical Problem

The existing ultra-thin fiberboard has low hardness and poor flame retardant effect, which limits its application in electronic circuit printing pads and packaging fields, and lacks high-hardness flame retardant ultra-thin fiberboard technology that is easy to mass production.

Method used

Use biomass fibers as raw materials to make fiber slurry by peeling, shaving, water washing, steaming and hot grinding, add modified reinforcement powder and synergistic flame retardant, and use spray technology to uniformly apply adhesives and composite additives. Perform hot pressing and sanding treatment to prepare high-hardness flame-retardant ultra-thin fiberboard.

Benefits of technology

The surface hardness and flame retardant properties of the fiberboard are improved, and the effect of self-extinguishing is achieved in the air. It also has insect-proof and corrosion-proof properties, and the density and physical and mechanical properties meet relevant standards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119017499A_ABST
    Figure CN119017499A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a high-hardness flame-retardant ultrathin fiberboard, which belongs to the technical field of fiberboard production, and comprises the following steps: step 1, biomass fiber preparation; 2, inorganic mineral powder is modified through a coupling agent to obtain modified reinforced powder, or the obtained modified reinforced powder is further added into an aqueous solution containing metal ions, and a composite additive is prepared; step 3, fiber sizing: adding an adhesive and modified reinforced powder; or an adhesive and a composite additive; or an adhesive, a synergistic flame retardant and a composite additive are added to the surface of the biomass fiber; step 4, drying the obtained biomass fibers; and 5, the obtained dry fibers are subjected to paving, pre-pressing and hot pressing to be made into the high-hardness flame-retardant ultrathin fiberboard. The flame retardant property of the ultrathin fiberboard can be enhanced, and the physical and mechanical properties such as the surface hardness of the board can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of artificial board production, specifically to the technical field of fiberboard production, and in particular to a method for preparing a high-hardness flame-retardant ultra-thin fiberboard. Background Art

[0002] Ultra-thin fiberboard is widely used in the finishing field of artificial boards such as particleboard and plywood. In this finishing decoration field, the main materials used for veneer treatment are thin veneers of precious tree species, melamine impregnated decorative paper, resin film, etc. With the development of the artificial board industry, the existing technology has developed ultra-thin fiberboard with a thickness of less than 1.5mm, which has the advantages of flat surface and can be cut as needed. It can replace large-format natural wood veneer, technical veneer and other veneer substrates, and has been well developed in the fields of particleboard and plywood veneer, greatly expanding the new uses and new fields of fiberboard. However, with the increasing demand and application scenarios of ultra-thin fiberboard, such as in the fields of electronic circuit printing pads, packaging, etc., some problems have been gradually discovered. The thickness standards of ultra-thin fiberboard for electronic circuit printing pads include 0.4mm, 0.6mm, 0.8mm, 1.0mm, 1.2mm, etc. However, the ultra-thin fiberboard has low hardness and poor flame retardant effect, which limits its application field. Therefore, improving the hardness and flame retardant properties of ultra-thin fiberboard is of great significance to expanding its application areas, and is also one of the important ways for the fiberboard industry to develop high-value and differentiated products.

[0003] After searching, there are not many patent technologies related to improving the hardness and flame retardant properties of ultra-thin fiberboards. High-hardness flame-retardant ultra-thin fiberboards for electronic circuit printing pads and packaging fields are even rarer. Therefore, it is very necessary to design a high-hardness flame-retardant ultra-thin fiberboard that is easy to mass-produce and its industrial production process. Summary of the invention

[0004] In view of the above problems, an object of the present invention is to provide a method for preparing a high-hardness flame-retardant ultra-thin fiberboard with high surface hardness and good flame retardant performance.

[0005] In order to achieve the purpose and other advantages of the present invention, the preparation method of the high-hardness flame-retardant ultra-thin fiberboard provided by the present invention comprises: Step 1: Biomass fiber preparation: In one embodiment, small-diameter wood, branch wood, bamboo wood and wood processing residues are selected as biomass fiber raw materials, and biomass fiber slurry is prepared after peeling, chipping, washing, steaming and hot grinding; Step 2: Preparation of composite additives: In one embodiment, the inorganic mineral powder is modified by a coupling agent to obtain a modified and reinforced powder, which is then added to an aqueous solution containing metal ions and stirred thoroughly to prepare a composite additive; Step 3: Fiber sizing: In one embodiment, after the biomass fiber slurry is obtained by steaming and hot grinding, the fiber slurry is sent to a glue application pipeline or a glue mixing device, and then the adhesive, the synergistic flame retardant and the composite auxiliary agent are sprayed by a metering pump through a nozzle arranged on the pipeline, and evenly sprayed onto the fiber surface; Step 4: Fiber drying: In one embodiment, the fibers are dried by hot air ducts; Step 5: Preparation of high-hardness flame-retardant ultra-thin fiberboard: In one embodiment, the obtained dry fibers are laid, pre-pressed, and surface humidified, and then subjected to hot pressing, edge trimming, heat dissipation curing, and sanding to produce the high-hardness flame-retardant ultra-thin fiberboard.

[0006] Preferably, the present invention provides four ways of adding the composite auxiliary agent. The first way is that after the composite auxiliary agent and the adhesive are evenly mixed in step 3, they are applied in multiple times in the glue application pipeline or the glue mixing device; the second way is that in step 3, the composite auxiliary agent and the adhesive are applied alternately in the glue application pipeline or the glue mixing device for multiple times; the third way is that after the fiber is dried, the modified reinforced powder or the modified reinforced powder and the flame retardant are evenly stirred and applied at the flame retardant adding device under the cyclone separator; the fourth way is that after pre-pressing in step 5, the upper and lower surfaces of the slab are subjected to high-pressure spraying treatment using a water suspension of the composite auxiliary agent in a surface wetting process.

[0007] Furthermore, the biomass fiber in step 1 of the present invention is a biomass material fiber of eucalyptus, poplar, fir, miscellaneous wood, bamboo, wheat straw, cotton straw or bagasse, etc. Preferably, it is a fiber of eucalyptus, poplar, fir or miscellaneous wood, and the bark content does not exceed 5% of the total fiber amount.

[0008] Furthermore, a waterproofing agent is added in the hot grinding stage described in step 1 or the sizing stage described in step 3 of the present invention to improve the moisture-proof performance of the product. The waterproofing agent is a paraffin emulsion with a high solid content of 50%, and the addition amount is 1-3% of the absolute dry fiber mass.

[0009] Further, the inorganic mineral powder in step 2 of the present invention includes inorganic mineral powders such as light calcium carbonate, heavy calcium carbonate, quartz powder (silicon dioxide), alumina, montmorillonite, bentonite, kaolin, attapulgite or aluminum silicate powder. The particle size of the inorganic mineral powder is 100-800 meshes; if the mesh number is too large, the cost is high, the particle size is too small and it is not easy to disperse, and it is easy to deposit on the lower surface of the slab after paving, and the glue consumption is large, and powder aggregation and glue spot defects are prone to occur, thereby reducing the mechanical properties of the board; if the inorganic powder mesh number is too small, its particle size is too large, and it is easy to precipitate in the aqueous phase dispersion due to gravity, resulting in uneven application of the reinforcing powder, because its particle size is too large, it is not conducive to the construction of a uniform and continuous bonding network structure of fibers and adhesives in the slab after paving. At the same time, the excessively large powder particle size may cause wear on the paving belt and hot pressing equipment. Preferably, the particle size of the inorganic mineral powder is 325 mesh to 400 mesh.

[0010] Furthermore, the coupling agent in step 2 of the present invention includes any one or more of silane coupling agents KH-550, KH-560, KH-570 and titanate coupling agents 110, 201, 401. Preferably, silane coupling agent KH-560 is used.

[0011] Furthermore, the method of treating inorganic mineral powder with a coupling agent in step 2 of the present invention includes stirring treatment in water phase at room temperature; or heating and stirring treatment at 60-90°C; or diluting the coupling agent 5 times with a 95% ethanol solution, and then dropping it into the inorganic mineral powder for high-speed mixing and stirring treatment in a high-speed stirrer, and the temperature is controlled at 90-120°C. Preferably, heating and stirring treatment at 60-90°C is used. The amount of the coupling agent is 0.5-5% of the total weight of the inorganic mineral material powder.

[0012] Furthermore, the metal ion described in step 2 of the present invention is a metal ion capable of forming a metal complex; obtained by an aqueous solution of a metal chloride, the metal chloride comprising any one or more of ferric chloride, aluminum chloride, zinc chloride, titanium tetrachloride, cupric chloride, ferrous chloride, manganese dichloride, nickel chloride and calcium chloride. Among them, aluminum chloride is preferably used because of its low cost, safety and environmental protection. The amount of metal chloride added is 0.5-1.5% of the absolute dry fiber mass.

[0013] Further, the main components of the synergistic flame retardant described in step three of the present invention are 3.5 hydrated zinc borate, melamine and phytic acid; or 3.5 hydrated zinc borate, ammonium polyphosphate and phytic acid; or 3.5 hydrated zinc borate, ammonium polyphosphate, melamine and phytic acid. Phytic acid has a strong chelating effect and can form a coordination with metal ions, so it can fix metal ions and improve its bonding performance with the adhesive, which is beneficial to improve the easy loss problem of inorganic flame retardants and contribute to the synergistic flame retardant effect of metal chlorides and flame retardants. The synergistic flame retardant is prepared from the following raw materials in parts by weight: 3-10 parts of 3.5-water zinc borate, 3-10 parts of melamine, and 1-5 parts of phytic acid; or 3-8 parts of 3.5-water zinc borate, 5-8 parts of ammonium polyphosphate, and 1-3 parts of phytic acid; or 3-8 parts of 3.5-water zinc borate, 3-5 parts of ammonium polyphosphate, 1-3 parts of melamine, and 1-3 parts of phytic acid; preferably, 5-8 parts of 3.5-water zinc borate, 3-5 parts of melamine, and 1-3 parts of phytic acid. The addition amount of the synergistic flame retardant is 5-30% of the absolute dry fiber mass.

[0014] Furthermore, the adhesive in step three of the present invention includes urea-formaldehyde resin adhesive (UF), melamine urea-formaldehyde resin adhesive (MUF), isocyanate adhesive (MDI) and soy protein adhesive. Among them, melamine urea-formaldehyde resin adhesive and isocyanate adhesive are preferred. Metal ions can form coordination bonds with amide groups (—CO—NH—) in MUF, hydroxyl groups (—OH) in biomass fibers, etc., to improve the dispersibility of the modified and reinforced powder and the cross-linking degree of the adhesive, thereby improving the surface hardness of the ultra-thin fiberboard.

[0015] Furthermore, the amount of the composite auxiliary agent added in step three of the present invention accounts for 3-20% of the absolute dry fiber mass of the fiber slurry, and the more preferred amount is 5-12%; if MUF adhesive is used, the amount added is 8-16% of the total mass of the absolute dry fiber and inorganic mineral powder, and the more preferred amount is 10-14%; if MDI adhesive is used, the amount added is 3-5% of the total mass of the absolute dry fiber and inorganic mineral powder, and the more preferred amount is 3-4%. If the amount of glue applied is too low, the adhesive cannot be evenly distributed on the surface of the fiber and powder, resulting in insufficient mechanical properties of the board, and the thickness of the board rebounds greatly after hot pressing; excessive use of adhesive will also increase production costs and board surface adhesive spot defects.

[0016] Furthermore, the fiber sizing method described in step three of the present invention is that after the composite additive and the adhesive are evenly mixed, they are applied multiple times in the glue application pipeline or glue mixing device; or the composite additive and the adhesive are applied alternately multiple times in the glue application pipeline or glue mixing device respectively.

[0017] Furthermore, in step 4 of the present invention, the hot air duct is used for drying, and the temperature of the drying medium in the drying duct is 110-250° C., preferably 130-150° C., and finally the moisture content of the fiber is controlled at 9-12%.

[0018] Furthermore, the paving method described in step five of the present invention includes one of mechanical forming, airflow forming or mechanical-airflow forming.

[0019] Furthermore, the hot pressing temperature described in step five of the present invention is 180~210℃, and a four-stage hot pressing method is adopted: the first stage is the contact zone, and the hot pressing unit pressure is 0.03~0.1MPa, which is mainly used for the smooth entry of the slab into the hot press; the second stage, the hot pressing unit pressure is 4.0~6.0MPa, which is mainly used for plate thickness determination; the third stage, the hot pressing unit pressure is 0.8~1.2MPa, which is mainly used to remove water vapor evaporated during the hot pressing process to prevent defects such as bubbling and bursting; the fourth stage, the hot pressing unit pressure is 1.0~3.5MPa, which is mainly to allow the adhesive to completely cure and cross-link and improve the strength of the plate.

[0020] Furthermore, the sanding in step five is double-sided sanding with a margin of 0.05-0.15 mm, which is used to remove the pre-cured layer on the surface of the plate.

[0021] Furthermore, the best way to add the composite auxiliary agent of the present invention is to apply the composite auxiliary agent and the adhesive in the glue application pipeline or glue mixing device in multiple times.

[0022] Furthermore, the present invention simultaneously uses an adhesive to glue the biomass fiber to obtain fibers that are only glued but not applied with composite additives and synergistic flame retardants, and the fibers that are only glued but not applied with composite additives and synergistic flame retardants after drying are used as the core layer, and the dry fibers obtained in step four are used as two surface layers for layered paving, and the mass ratio of the fibers that are only glued but not applied with composite additives and synergistic flame retardants to the dry fibers obtained in step four is 1:1; or all the dry fibers obtained in step four are used for paving.

[0023] The present invention has at least the following beneficial effects: 1. The present invention forms coordination crosslinks with metal ions and biomass fibers, adhesives, and inorganic mineral powders modified by coupling agents, which are used to disperse inorganic mineral powders and improve the interface compatibility between inorganic mineral powders and biomass fibers. In addition, inorganic mineral powders are used as reinforcing materials to increase the surface hardness of the board and prepare ultra-thin fiberboards with high hardness.

[0024] 2. The inorganic mineral powder used in the present invention is a kind of covering flame retardant. By preparing a synergistic flame retardant and using multiple flame retardant mechanisms with inorganic mineral powder and metal chloride, the surface of the fiberboard is rapidly dehydrated and carbonized to form a carbonized layer, thereby avoiding the smoldering phenomenon of the board and reducing the emission of toxic gases. The high-hardness flame-retardant ultra-thin fiberboard prepared by the present invention can achieve the effect of self-extinguishing in the air.

[0025] 3. The metal chloride and zinc borate used in the present invention have certain insect-proof and anti-corrosion effects, so the prepared ultra-thin fiberboard has certain insect-proof and anti-corrosion effects.

[0026] 4. The high-hardness flame-retardant ultra-thin fiberboard prepared by the preparation method of the present invention has a thickness of 0.8-1.4 mm and a density of 900-1100 kg / m 3 The moisture content is 5~12%, and the relevant physical and mechanical properties meet the requirements of T / CNFPIA 3007-2019 "Ultra-thin High-density Fiberboard" group standard.

[0027] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is a diagram showing the mechanism of preparing high-hardness flame-retardant ultra-thin fiberboard by metal ion coordination reinforcement of the present invention.

[0029] Figure 2 Figures 2 and 3 are the microscopic morphologies and elemental analysis diagrams of the fibers after sizing of Comparative Example 1 and Example 2; (a) and (b) are the microscopic morphologies of the fibers after sizing of Comparative Example 1 and Example 2, respectively; (c) (d) (e) (f) are the elemental analysis diagrams of C, O, Si and Al based on Figure (b), respectively.

[0030] Figure 3 This is a surface diagram of the ultra-thin fiberboard of comparative example 3; wherein (a) is the upper surface and (b) is the lower surface. DETAILED DESCRIPTION

[0031] The present invention is further described in detail below in conjunction with embodiments so that those skilled in the art can implement the invention with reference to the description.

[0032] Example 1 A method for preparing a high-hardness flame-retardant ultra-thin fiberboard, comprising: S1: Eucalyptus is selected as the biomass fiber raw material, which is made into fiber pulp after peeling, chipping, washing, cooking and hot grinding.

[0033] S2: First, prepare the silane coupling agent KH-560 into a 10% aqueous solution by mass, and heat and stir it at 70°C for 30 minutes. Then add SiO2 powder and continue to heat and stir it for 1 hour. Finally, filter, dry and crush to obtain the modified and reinforced powder. The amount of silane coupling agent KH-560 added is 5% of the mass of SiO2 powder. The mesh number of the modified and reinforced powder is 325 mesh.

[0034] S3: The modified reinforcing powder and melamine modified urea-formaldehyde resin adhesive are uniformly and alternately applied to the fiber slurry through the sizing device. The amount of modified reinforcing powder is 10% of the absolute dry fiber mass; the amount of MUF adhesive is 12% of the total mass of the absolute dry fiber and modified reinforcing powder.

[0035] S4: The fiber slurry after sizing is dried through a hot air duct. The temperature of the drying medium in the drying duct is 130-150°C, so that its final moisture content is 8%~12%.

[0036] S5: After the obtained dry fiber is assembled and pre-pressed, it is hot pressed, trimmed, heat-dissipated and sanded to make the high-hardness ultra-thin fiberboard. Among them, the hot pressing temperature is 180~210℃, and a four-stage hot pressing method is adopted: the first stage is the contact zone, and the hot pressing unit pressure is 0.03~0.1MPa, which is mainly used for the smooth entry of the slab into the hot press; the second stage, the hot pressing unit pressure is 4.0~6.0MPa, which is mainly used for the thickness of the board; the third stage, the hot pressing unit pressure is 0.8~1.2MPa, which is mainly used to remove the evaporated water vapor during the hot pressing process to prevent defects such as bubbling and bursting; the fourth stage, the hot pressing unit pressure is 1.0~3.5MPa, mainly to allow the adhesive to completely cure and cross-link, and improve the strength of the board. The hot pressing speed of the continuous hot press is 1400~1600mm / s. Sanding is double-sided sanding with a margin of 0.05~0.15mm.

[0037] Example 2 (The difference from Example 1 is that the metal ion AlCl3 is used to compound the modified and reinforced powder as a composite auxiliary agent.) A method for preparing a high-hardness flame-retardant ultra-thin fiberboard, comprising: S1: Eucalyptus is selected as the biomass fiber raw material, which is made into fiber pulp after peeling, chipping, washing, cooking and hot grinding.

[0038] S2: First, prepare the silane coupling agent KH-560 into a 10% aqueous solution by mass, and heat and stir it at 70°C for 30 minutes. Then add SiO2 powder and continue to heat and stir it for 1 hour. Finally, filter, dry and crush to obtain the modified and reinforced powder. The amount of silane coupling agent KH-560 added is 5% of the mass of SiO2 powder. The mesh number of the modified and reinforced powder is 325 mesh.

[0039] S3: AlCl3 particles are prepared into a 5% aqueous solution. The modified and enhanced powder is added into the AlCl3 solution to prepare a composite auxiliary agent suspension.

[0040] S4: The composite additive and melamine modified urea-formaldehyde resin adhesive are uniformly and alternately applied to the fiber slurry through the sizing device. The amount of modified reinforcing powder is 10% of the absolute dry fiber mass; the amount of AlCl3 is 1% of the absolute dry fiber mass; the amount of MUF adhesive is 12% of the total mass of the absolute dry fiber and modified reinforcing powder.

[0041] S5: The fiber slurry after sizing is dried through a hot air duct. The temperature of the drying medium in the drying duct is 130-150°C, so that its final moisture content is 8%~12%.

[0042] S6: After the obtained dry fiber is assembled and pre-pressed, it is hot pressed, trimmed, heat-dissipated and sanded to make the high-hardness ultra-thin fiberboard. Among them, the hot pressing temperature is 180~210℃, and a four-stage hot pressing method is adopted: the first stage is the contact zone, and the hot pressing unit pressure is 0.03~0.1MPa, which is mainly used for the smooth entry of the slab into the hot press; the second stage, the hot pressing unit pressure is 4.0~6.0MPa, which is mainly used for the thickness of the board; the third stage, the hot pressing unit pressure is 0.8~1.2MPa, which is mainly used to remove the evaporated water vapor during the hot pressing process to prevent defects such as bubbling and bursting; the fourth stage, the hot pressing unit pressure is 1.0~3.5MPa, which is mainly to allow the adhesive to completely cure and cross-link and improve the strength of the board. The hot pressing speed of the continuous hot press is 1400~1600mm / s. Sanding is double-sided sanding with a margin of 0.05~0.15mm.

[0043] Example 3 (The difference from Example 2 is that the inorganic mineral powder is Al2O3.) A method for preparing a high-hardness flame-retardant ultra-thin fiberboard, comprising: S1: Eucalyptus is selected as the biomass fiber raw material, which is made into fiber pulp after peeling, chipping, washing, cooking and hot grinding.

[0044] S2: First, prepare the silane coupling agent KH-560 into a 10% aqueous solution by mass, and heat and stir it at 70°C for 30 minutes. Then add Al2O3 powder and continue heating and stirring for 1 hour. Finally, filter, dry and crush to obtain the modified and reinforced powder. The amount of silane coupling agent KH-560 added is 5% of the mass of Al2O3 powder. The mesh size of the modified and reinforced powder is 325 mesh.

[0045] S3: AlCl3 particles are prepared into a 5% aqueous solution. The modified and enhanced powder is added into the AlCl3 solution to prepare a composite auxiliary agent suspension.

[0046] S4: The waterproofing agent, composite additive and melamine modified urea-formaldehyde resin adhesive are uniformly and alternately applied to the fiber slurry through the sizing device. The amount of modified reinforcing powder is 10% of the absolute dry fiber mass; the amount of AlCl3 is 1% of the absolute dry fiber mass; the amount of MUF adhesive is 12% of the total mass of the absolute dry fiber and modified reinforcing powder.

[0047] S5: The fiber slurry after sizing is dried through a hot air duct. The temperature of the drying medium in the drying duct is 130-150°C, so that its final moisture content is 8%~12%.

[0048] S6: After the obtained dry fiber is assembled and pre-pressed, it is hot pressed, trimmed, heat-dissipated and sanded to make the high-hardness ultra-thin fiberboard. Among them, the hot pressing temperature is 180~210℃, and a four-stage hot pressing method is adopted: the first stage is the contact zone, and the hot pressing unit pressure is 0.03~0.1MPa, which is mainly used for the smooth entry of the slab into the hot press; the second stage, the hot pressing unit pressure is 4.0~6.0MPa, which is mainly used for the thickness of the board; the third stage, the hot pressing unit pressure is 0.8~1.2MPa, which is mainly used to remove the evaporated water vapor during the hot pressing process to prevent defects such as bubbling and bursting; the fourth stage, the hot pressing unit pressure is 1.0~3.5MPa, which is mainly to allow the adhesive to completely cure and cross-link and improve the strength of the board. The hot pressing speed of the continuous hot press is 1400~1600mm / s. Sanding is double-sided sanding with a margin of 0.05~0.15mm.

[0049] Example 4 (The difference from Example 2 is that a synergistic flame retardant is used.) A method for preparing a high-hardness flame-retardant ultra-thin fiberboard, comprising: S1: Eucalyptus is selected as the biomass fiber raw material, which is made into fiber pulp after peeling, chipping, washing, cooking and hot grinding.

[0050] S2: First, prepare the silane coupling agent KH-560 into a 10% aqueous solution by mass, and heat and stir it at 70°C for 30 minutes. Then add SiO2 powder and continue to heat and stir it for 1 hour. Finally, filter, dry and crush to obtain the modified and reinforced powder. The amount of silane coupling agent KH-560 added is 5% of the mass of SiO2 powder. The mesh size of the modified and reinforced powder is 325 mesh.

[0051] S3: AlCl3 particles are prepared into a 5% aqueous solution. The modified and enhanced powder is added into the AlCl3 solution to prepare a composite auxiliary agent suspension.

[0052] S4: The waterproofing agent, synergistic flame retardant, composite auxiliary agent and melamine modified urea-formaldehyde resin adhesive are respectively and alternately applied to the fiber slurry through the sizing device. The amount of synergistic flame retardant is 8% of the absolute dry fiber mass; the amount of modified reinforcing powder is 10% of the absolute dry fiber mass; the amount of AlCl3 is 1% of the absolute dry fiber mass; the amount of MUF adhesive is 12% of the total mass of the absolute dry fiber and the modified reinforcing powder. The synergistic flame retardant is prepared from the following raw materials in parts by weight: 5-8 parts of 3.5-water zinc borate, 3-5 parts of melamine, and 1-3 parts of phytic acid.

[0053] S5: The fiber slurry after sizing is dried through a hot air duct. The temperature of the drying medium in the drying duct is 130-150°C, so that its final moisture content is 8%~12%.

[0054] S6: After the obtained dry fiber is assembled and pre-pressed, it is hot pressed, trimmed, heat-dissipated and sanded to make the high-hardness ultra-thin fiberboard. Among them, the hot pressing temperature is 180~210℃, and a four-stage hot pressing method is adopted: the first stage is the contact zone, and the hot pressing unit pressure is 0.03~0.1MPa, which is mainly used for the smooth entry of the slab into the hot press; the second stage, the hot pressing unit pressure is 4.0~6.0MPa, which is mainly used for the thickness of the board; the third stage, the hot pressing unit pressure is 0.8~1.2MPa, which is mainly used to remove the evaporated water vapor during the hot pressing process to prevent defects such as bubbling and bursting; the fourth stage, the hot pressing unit pressure is 1.0~3.5MPa, which is mainly to allow the adhesive to completely cure and cross-link and improve the strength of the board. The hot pressing speed of the continuous hot press is 1400~1600mm / s. Sanding is double-sided sanding with a margin of 0.05~0.15mm.

[0055] Example 5 (The difference from Example 4 is that fibers with only sizing but no composite additive and synergistic flame retardant are also prepared at the same time. After drying, the fibers with only sizing but no composite additive and synergistic flame retardant are used as the core layer, and the modified fibers are used as two surface layers for layered laying.) A method for preparing a high-hardness flame-retardant ultra-thin fiberboard, comprising: S1: Eucalyptus is selected as the biomass fiber raw material, which is made into fiber pulp after peeling, chipping, washing, cooking and hot grinding.

[0056] S2: First, prepare the silane coupling agent KH-560 into a 10% aqueous solution by mass, and heat and stir it at 70°C for 30 minutes. Then add SiO2 powder and continue to heat and stir it for 1 hour. Finally, filter, dry and crush to obtain the modified and reinforced powder. The amount of silane coupling agent KH-560 added is 5% of the mass of SiO2 powder. The mesh size of the modified and reinforced powder is 325 mesh.

[0057] S3: AlCl3 particles are prepared into a 5% aqueous solution. The modified and enhanced powder is added into the AlCl3 solution to prepare a composite auxiliary agent suspension.

[0058] S4: The waterproofing agent, the synergistic flame retardant, the composite auxiliary agent and the melamine modified urea-formaldehyde resin adhesive are respectively and alternately applied to the fiber slurry through a sizing device to obtain a modified fiber slurry. The amount of the synergistic flame retardant is 8% of the absolute dry fiber mass; the amount of the modified reinforcing powder is 10% of the absolute dry fiber mass; the amount of AlCl3 is 1% of the absolute dry fiber mass; the amount of the MUF adhesive is 12% of the total mass of the absolute dry fiber and the modified reinforcing powder. The synergistic flame retardant is prepared from the following raw materials in parts by weight: 5-8 parts of 3.5-water zinc borate, 3-5 parts of melamine, and 1-3 parts of phytic acid.

[0059] The melamine modified urea-formaldehyde resin adhesive is uniformly applied to the fiber slurry through a sizing device to obtain a fiber slurry with only sizing applied but without composite additives and synergistic flame retardants, and the amount of the MUF adhesive used is 12% of the absolute dry fiber mass.

[0060] S5: The modified fiber slurry after sizing and the fiber slurry only sizing without applying the composite additive and the synergistic flame retardant are dried through a hot air duct respectively, and the temperature of the drying medium in the drying duct is 130-150°C, so that the final moisture content is 8%-12%, and the modified dry fiber and the dried fiber only sizing without applying the composite additive and the synergistic flame retardant are obtained respectively.

[0061] S6: The dried fibers that are only glued but not applied with composite additives and synergistic flame retardants are used as the core layer, and the modified dry fibers are used as the surface layer, and they are laid in layers. The mass ratio of the modified dry fibers to the dried fibers that are only glued but not applied with composite additives and synergistic flame retardants is 1:1. After assembly and pre-pressing, hot pressing, edge trimming, heat dissipation curing and sanding are performed to make the high-hardness flame-retardant ultra-thin fiberboard. Among them, the hot pressing temperature is 180~210℃, and a four-stage hot pressing method is adopted: the first stage is the contact zone, the hot pressing unit pressure is 0.03~0.1MPa, which is mainly used for the slab to enter the hot press smoothly; the second stage, the hot pressing unit pressure is 4.0~6.0MPa, which is mainly used for plate thickness determination; the third stage, the hot pressing unit pressure is 0.8~1.2MPa, which is mainly used to remove the evaporated water vapor during the hot pressing process to prevent defects such as bubbling and bursting; the fourth stage, the hot pressing unit pressure is 1.0~3.5MPa, mainly to allow the adhesive to completely cure and crosslink, and improve the strength of the plate. The hot pressing speed of the continuous hot press is 1400~1600mm / s. Sanding is double-sided sanding with a margin of 0.05~0.15mm.

[0062] Comparative Example 1 (The difference from Example 1 is that the reinforced powder is not modified) A method for preparing a high-hardness ultra-thin fiberboard, comprising: S1: Eucalyptus is selected as the biomass fiber raw material, which is made into fiber pulp after peeling, chipping, washing, cooking and hot grinding.

[0063] S2: The reinforcing powder (SiO2) and melamine-modified urea-formaldehyde resin adhesive are alternately and evenly applied to the fiber slurry through the sizing device. The amount of reinforcing powder is 10% of the absolute dry fiber mass; the amount of MUF adhesive is 12% of the total mass of the absolute dry fiber and reinforcing powder.

[0064] S3: The sizing biomass fiber is dried through a hot air duct to obtain dry fiber. The temperature of the drying medium in the drying duct is 130-150° C., so that the final moisture content is 8%-12%.

[0065] S4: After the obtained dry fiber is assembled and pre-pressed, it is hot pressed, trimmed, heat-dissipated and sanded to make the high-hardness ultra-thin fiberboard. Among them, the hot pressing temperature is 180~210℃, and a four-stage hot pressing method is adopted: the first stage is the contact zone, and the hot pressing unit pressure is 0.03~0.1MPa, which is mainly used for the smooth entry of the slab into the hot press; the second stage, the hot pressing unit pressure is 4.0~6.0MPa, which is mainly used for the thickness of the board; the third stage, the hot pressing unit pressure is 0.8~1.2MPa, which is mainly used to remove the evaporated water vapor during the hot pressing process to prevent defects such as bubbling and bursting; the fourth stage, the hot pressing unit pressure is 1.0~3.5MPa, which is mainly to allow the adhesive to completely cure and cross-link and improve the strength of the board. The hot pressing speed of the continuous hot press is 1400~1600mm / s. Sanding is double-sided sanding with a margin of 0.05~0.15mm.

[0066] Comparative Example 2 The difference from Example 4 is that the mesh size of the modified reinforced powder is 100 meshes, and the other steps are the same to obtain a high-hardness flame-retardant ultra-thin fiberboard.

[0067] Comparative Example 3 The difference from Example 4 is that the mesh size of the modified reinforced powder is 800 meshes, and the other steps are the same to obtain a high-hardness flame-retardant ultra-thin fiberboard.

[0068] Comparative Example 4 The difference from Example 4 is that the method of adding the composite auxiliary agent is replaced by: after the composite auxiliary agent and the adhesive are evenly mixed, they are applied in multiple times in the glue application pipeline or glue mixing device.

[0069] Comparative Example 5 Different from Example 4, the method of adding the composite auxiliary agent is replaced by: after pre-pressing, a water suspension of the composite auxiliary agent is used in a surface wetting process to perform high-pressure spray treatment on the upper and lower surfaces of the slab.

[0070] Data analysis Table 1 shows the physical and mechanical properties of the ultra-thin fiberboards prepared in the examples and comparative examples. Through the test of the surface Shore hardness, it can be found that the addition of inorganic mineral powders can significantly improve the hardness of the ultra-thin fiberboard. Compared with comparative example 1, the performance of Example 1 is significantly improved, proving that the addition of coupling agents is beneficial to improving the interfacial compatibility between the fiber and the mineral powder. Compared with Example 1, the internal bonding strength of Example 2 is improved, and the water absorption thickness expansion rate is reduced, proving that the metal ions increase the cross-linking degree of the adhesive through coordination, making the interior of the slab denser, thereby improving the performance of the ultra-thin board. According to Figure 2 Analysis shows that the inorganic mineral powder is firmly adhered to the fiber surface and dispersed evenly, and the metal ions are distributed in the fiber through coordination. In Example 4, by adding a small amount of synergistic flame retardant, the limiting oxygen index value can reach 31% when other physical and mechanical properties are similar, which is 48% higher than that of Comparative Example 1, and significantly higher than other embodiments, indicating that the obtained ultra-thin fiberboard has good flame retardancy. Example 5 has excellent physical and mechanical properties while maintaining high surface hardness and good flame retardancy through layered paving. In Comparative Example 3, since the mesh size of the inorganic mineral powder is too large, most of the powder is deposited on the lower surface of the ultra-thin fiberboard. The hardness of the upper surface (HD) is 71, and the hardness of the lower surface is 80. There is a large difference in hardness between the upper and lower surfaces. Figure 3 The surface diagram of the ultra-thin fiberboard of Comparative Example 3, wherein (a) is the upper surface and (b) is the lower surface. After the composite additive and the adhesive are evenly mixed in Comparative Example 4, the viscosity of the adhesive increases and the curing time is shortened. The ultra-thin fiberboard of Comparative Example 5 is prone to blistering defects and causes greater wear on the steel belt of the press.

[0071] Table 1 Physical and mechanical properties of ultra-thin fiberboards prepared in the examples and comparative examples Although the embodiments of the present invention have been disclosed above, they are not limited to the applications listed in the specification and the embodiments. They can be applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily realized.

Claims

1. A method for preparing a high-hardness flame-retardant ultra-thin fiberboard, characterized in that: include: Step 1: preparing biomass fibers; Step 2: The inorganic mineral powder is modified by a coupling agent to obtain a modified and reinforced powder, or the obtained modified and reinforced powder is further added to an aqueous solution containing metal ions to prepare a composite additive; Step 3, fiber sizing: adding adhesive and modified reinforcing powder; or adhesive and composite additive; or adhesive, synergistic flame retardant and composite additive to the surface of the biomass fiber; Step 4, drying the obtained biomass fiber; Step 5: The obtained dry fibers are laid, pre-pressed and hot-pressed to form the high-hardness flame-retardant ultra-thin fiberboard.

2. The method for preparing the high-hardness flame-retardant ultra-thin fiberboard according to claim 1, characterized in that: The adding method of the composite additive includes any one of the following: 1) after the composite additive and the adhesive are evenly mixed, they are applied in multiple times in the glue application pipeline or the glue mixing device; 2) the composite additive and the adhesive are applied alternately in the glue application pipeline or the glue mixing device for multiple times; 3) the modified reinforced powder or the modified reinforced powder and the flame retardant are stirred and evenly applied at the flame retardant adding equipment below the cyclone separator in the paving molding process; 4) after pre-pressing, the upper and lower surfaces of the slab are subjected to high-pressure spray treatment using a water suspension of the composite additive in the surface wetting process.

3. The method for preparing the high-hardness flame-retardant ultra-thin fiberboard according to claim 1, characterized in that: The inorganic mineral powder includes any one or more of light calcium carbonate, heavy calcium carbonate, silicon dioxide, aluminum oxide, montmorillonite, bentonite, kaolin, attapulgite and aluminum silicate powder; the particle size of the inorganic mineral powder is 100-800 meshes.

4. The method for preparing the high-hardness flame-retardant ultra-thin fiberboard according to claim 1, characterized in that: The coupling agent is any one or more of silane coupling agents KH-550, KH-560, KH-570 and titanate coupling agents 110, 201, 401.

5. The method for preparing the high-hardness flame-retardant ultra-thin fiberboard according to claim 4, characterized in that: The method for treating the inorganic mineral powder with the coupling agent is heating and stirring at 60-90° C.; the amount of the coupling agent used is 0.5-5% of the total weight of the inorganic mineral powder.

6. The method for preparing the high-hardness flame-retardant ultra-thin fiberboard according to claim 1, characterized in that: The metal ions are metal ions that can form metal complexes; the metal ions are obtained by using an aqueous solution of metal chloride, and the metal chloride includes any one or more of ferric chloride, aluminum chloride, zinc chloride, titanium tetrachloride, cupric chloride, ferrous chloride, manganese dichloride, nickel chloride and calcium chloride; the added amount of the metal chloride is 0.5-1.5% of the absolute dry fiber mass.

7. The method for preparing the high-hardness flame-retardant ultra-thin fiberboard according to claim 1, characterized in that: The synergistic flame retardant is prepared from the following raw materials in parts by weight: 5-8 parts of 3.5-hydrated zinc borate, 3-5 parts of melamine, and 1-3 parts of phytic acid; or 5-8 parts of 3.5-hydrated zinc borate, 3-5 parts of ammonium polyphosphate, and 1-3 parts of phytic acid; or 3-8 parts of 3.5-hydrated zinc borate, 3-5 parts of ammonium polyphosphate, 1-3 parts of melamine, and 1-3 parts of phytic acid; the added amount of the synergistic flame retardant is 5-30% of the absolute dry fiber mass.

8. The method for preparing the high-hardness flame-retardant ultra-thin fiberboard according to claim 1, characterized in that: In step three, the fiber sizing method is to mix the composite additive and the adhesive evenly and then apply them multiple times in a glue application pipeline or a glue mixing device; or to apply the composite additive and the adhesive alternately multiple times in a glue application pipeline or a glue mixing device.

9. The method for preparing the high-hardness flame-retardant ultra-thin fiberboard according to claim 1, characterized in that: At the same time, an adhesive is used to apply glue to the biomass fiber to obtain a fiber that is only applied with glue but not applied with a composite additive and a synergistic flame retardant, and the fiber that is only applied with glue but not applied with a composite additive and a synergistic flame retardant after drying is used as a core layer; the dry fiber obtained in claim 1 is used as two surface layers for layered paving, and the mass ratio of the fiber that is only applied with glue but not applied with a composite additive and a synergistic flame retardant to the dry fiber obtained in claim 1 is 1:1; Or all the dry fibers obtained according to claim 1 are used for paving.

Citation Information

Patent Citations

  • Process for manufacturing prefinished hardboard

    CA1121529A

  • Processing method for temperature-resistant and flame-retardant wood composite fiber decorative plate

    CN107142763A

  • Production process of formaldehyde-free flame-retardant fiberboard

    CN113815082A

  • High-flame-retardant gypsum-based fiberboard and preparation method thereof

    CN115959877A

  • Woody molding and its production method

    JP2004314510A

Cited By

  • Composite flexible material, biomass fiber flexible material and preparation method and application thereof

    CN117005194A

  • Flame-retardant wrapping tape based on wide-range biomass fibers and preparation process thereof

    CN120645409A

  • Flame-retardant biomass fiber composite material and preparation method thereof

    CN120887671A

  • Surface-enhanced flame-retardant low-odor ultrathin fiberboard and preparation method thereof

    CN120985779A

  • Surface enhanced flame retardant low odor ultra-thin fiberboard and preparation method thereof