Coating composition for forming oxygen barrier layer, laminate, method for removing oxygen barrier layer, and method for recovering substrate
A coating composition using polyurethane resin and layered clay mineral forms an oxygen barrier layer that can be easily removed, addressing the recycling challenge of laminated plastic films by maintaining adhesion and laminate strength, thus promoting environmental conservation.
Patent Information
- Application Number
- JP2023193626
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-11-15
- Filing Date
- 2023-11-14
- Publication Date
- 2024-09-19
- Estimated Expiration
- 2043-11-14
AI Technical Summary
Existing plastic films used for food and toiletry product packaging, which are laminates with an oxygen barrier layer, are difficult to recycle due to the challenge of removing the oxygen barrier layer while maintaining the required physical properties and adhesion, leading to inefficient recycling and resource waste.
A coating composition containing polyurethane resin and layered clay mineral with specific hydroxyl and acid values, and a solid content ratio, forming an oxygen barrier layer that can be easily removed with an alkaline solution, maintaining excellent adhesion and laminate strength.
The solution enables the formation of a laminate with excellent oxygen barrier and fragrance retention properties, allowing easy removal and recycling of the plastic film, contributing to environmental conservation and resource efficiency.
Smart Images

Figure 0007554337000001 
Figure 0007554337000002 
Figure 0007554337000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a coating composition for forming an oxygen barrier layer, a laminate, a method for removing the oxygen barrier layer of the laminate, and a method for recovering the substrate of the laminate. More specifically, the present invention relates to a coating composition for forming an oxygen barrier layer used for a laminate comprising, for example, a first substrate and an oxygen barrier layer, and also to a coating composition for forming an oxygen barrier layer used for, for example, a laminate having a first substrate and a second substrate and comprising the first substrate and the second substrate and the oxygen barrier layer. The laminate of the present invention using the coating composition for forming an oxygen barrier layer of the present invention can be widely used in large quantities as a film packaging product, and is excellent in the removal property of the oxygen barrier layer from the laminate as described above. This contributes to the recycling of substrates, and is a technology useful for environmental conservation that is expected to contribute to the effective use of resources. [Background technology]
[0002] For example, for packaging materials (packaging materials) for food packaging and packaging materials for toiletry products, it is required to prevent oxidation of the food contained therein and deterioration of the products contained therein, such as moisturizers and shampoos, so films with excellent oxygen barrier properties are used. In order to impart oxygen barrier properties to films, various methods have been conceived, proposed, and implemented. For example, Patent Document 1 proposes providing a coating layer of a specific material composition on the deposition layer surface of a deposition film in which a metal deposition layer is provided on a substrate film. In addition, Patent Document 2 proposes a coating liquid using a resin containing a specific polyvinyl alcohol and a specific polyacrylic acid as a coating liquid for forming a gas barrier layer, and proposes a coating film used as a gas barrier layer formed from the coating liquid, and a laminate including the coating film and a substrate.
[0003] In response to the recent problem of global warming, the applicant has proposed various methods for producing polyhydroxyurethane resins as a groundbreaking technology for synthesizing useful resins using carbon dioxide as a material. Among these, the applicant has proposed an aqueous dispersion composition in which polyhydroxyurethane resins and clay minerals are well-composite-dispersed in water, which can be used as a resin for forming a film in water-based paints and coating agents (see Patent Document 3). This aqueous dispersion composition is a good dispersion of clay minerals, which are known to improve gas barrier properties (low oxygen permeability), in water, and by using this, a film with superior gas barrier properties, for example, a laminate in which an oxygen barrier layer is formed on a substrate film, can be easily produced.
[0004] In recent years, excessive consumption of plastic products has become a social issue, and in view of the problem of the depletion of finite petroleum resources and the adverse effects of waste on living organisms, there is a demand for recycling plastic films that have been used once and reusing them as plastic films from the viewpoint of effective utilization of resources and preservation of the global environment, etc. In particular, plastic films used as packaging materials for food, toiletry products, etc. are consumed in large quantities and discarded in large quantities, so if this plastic film could be recycled easily, it is expected that the amount of discarded plastic film could be significantly reduced, which would be extremely useful. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 8-318591 [Patent Document 2] Patent No. 7060946 [Patent Document 3] Patent No. 6813338 Summary of the Invention [Problem to be solved by the invention]
[0006] However, for example, film packaging (containers) made of plastic film for packaging food or toiletry products are required to have various properties such as oxygen barrier property and aroma retention property, and therefore, most of them are not made of a single layer made of plastic film, but are made of a laminate made of various functional material layers such as an oxygen barrier layer, a pattern layer, and a metal layer. For example, in the case of plastic film for packaging food or toiletry products, a laminate is made in which an oxygen barrier layer is provided on the entire surface of the plastic film as a base material in order to prevent oxidation and deterioration of the items contained inside. Therefore, when recycling the plastic film used as the base material from a film packaging made of such a laminate, it is necessary to remove the oxygen barrier layer formed on the entire surface of the base material and recover it as a single plastic film. Furthermore, in order to reuse the plastic film recovered after use as a film packaging for food packaging or toiletry products, it is necessary for the recycled film to exhibit physical properties that satisfy various required performances. However, there was a problem in that it was difficult to obtain a recycled film that could be reused for packaging from a laminate having the structure described above in a simple manner, and it was difficult to obtain a recycled film that satisfied various required performance requirements.
[0007] Therefore, the object of the present invention is to provide a coating composition for forming an oxygen barrier layer having a new structure, which can form a laminate having a structure in which at least the oxygen barrier layer can be easily removed from a laminate having a first substrate and an oxygen barrier layer having low oxygen permeability, excellent oxygen barrier properties, and excellent adhesion, and can be made into a recycled film in a simple manner. Another object of the present invention is to provide a coating composition for forming an oxygen barrier layer having a new structure, which can form a laminate having at least the oxygen barrier layer can be easily removed from a laminate having excellent lamination strength, which is composed of a first substrate, a second substrate, and an excellent oxygen barrier layer having low oxygen permeability, and can be made into a recycled film in a simple manner. Hereinafter, in order to distinguish between embodiments, a laminate having a so-called surface-printed structure, which has an oxygen barrier layer (coating film) made of a first substrate and the coating composition of the present invention, is also called "laminate-1". Moreover, a laminate having a so-called laminate structure, which has first and second substrates and an oxygen barrier layer (coating film) made of the coating composition of the present invention, is also referred to as "laminate-2."
[0008] In the present invention, a functional layer provided to impart various required performance to a plastic film (substrate) used for packaging materials for food, toiletry products, etc. is called an "oxygen barrier layer" as a representative example of oxygen barrier property among various performances required for a plastic film. A plastic film with low oxygen permeability exhibits good oxygen barrier properties, but the present invention also aims to have another required performance, good aroma retention, by simultaneously achieving low permeability for, for example, the aroma applied to the item contained inside. In other words, the film packaging having an oxygen barrier layer in the present invention means that it has at least good oxygen barrier properties and aroma retention properties. Here, if the "aroma retention properties" of the film packaging are insufficient, the aroma of the item contained inside will leak out to the outside, causing the problem of odor transfer to other products, so realizing "aroma retention properties" is also an important technical issue for film packaging for food, toiletry products, etc. [Means for solving the problem]
[0009] The above object can be achieved by the present invention, which provides the following coating composition for forming an oxygen barrier layer. [1] A coating composition for forming an oxygen barrier layer, comprising a polyurethane resin and a layered clay mineral, The polyurethane resin has a hydroxyl value of 100 to 400 mgKOH / g and an acid value of 15 to 70 mgKOH / g; The average aspect ratio of the layered clay mineral is 150 to 350; 1. A coating composition for forming an oxygen barrier layer, wherein a ratio of solids in the polyurethane resin and the layered clay mineral is 100:1 to 100:35 on a mass basis.
[0010] Preferred forms of the above-mentioned coating composition for forming an oxygen barrier layer are as follows. [2] The coating composition for forming an oxygen barrier layer according to the above [1], wherein the layered clay mineral has a particle size of 1.0 to 20 μm. [3] The coating composition for forming an oxygen barrier layer according to the above [1] or [2], wherein the polyurethane resin has a weight average molecular weight of 10,000 to 1,200,000. [4] The coating composition for forming an oxygen barrier layer according to any one of the above [1] to [3], wherein the polyurethane resin is a polyhydroxyurethane resin which is a reaction product of a cyclic carbonate compound, which is a reaction product of an epoxy compound and carbon dioxide, and a polyamine. [5] The coating composition for forming an oxygen barrier layer according to any one of the above [1] to [4], further comprising an epoxy compound as a curing agent. [6] The coating composition for forming an oxygen barrier layer according to any one of the above [1] to [5], which is used for forming an oxygen barrier layer of a laminate film.
[0011] As another embodiment, the present invention provides the following laminate. [7] A laminate comprising an oxygen barrier layer formed on a first substrate, the oxygen barrier layer being made of a coating composition for forming an oxygen barrier layer according to any one of the above [1] to [6].
[0012] Preferable forms of the above-mentioned laminate include the following. [8] The laminate according to the above [7], wherein the first substrate is made of any polyolefin-based resin. [9] The laminate according to the above [7] or [8], wherein the first substrate is made of recycled materials that have been recovered after being used once.
[10] The laminate according to any one of the above [7] to [9], further comprising a first and a second substrate formed by laminating, in this order, an adhesive layer and a second substrate on the oxygen barrier layer formed on the first substrate.
[11] The laminate according to the above
[10] , wherein the second substrate is made of at least one resin selected from the group consisting of polyolefin resins, polyester resins and nylon resins.
[12] The laminate according to the above
[10] or
[11] , wherein the first substrate and / or the second substrate are made of recycled materials that have been recovered after being used once.
[0013] As another embodiment, the present invention provides a method for removing an oxygen barrier layer, which is described below.
[13] A method for removing an oxygen barrier layer from a laminate comprising a first substrate and an oxygen barrier layer made of the coating composition for forming an oxygen barrier layer according to any one of the above [1] to [6], or from a laminate comprising the first substrate, a second substrate, and the oxygen barrier layer, the method comprising the step of removing the oxygen barrier layer from the laminate using an alkaline solution.
[0014] As another embodiment, the present invention provides a method for recovering a substrate, as described below.
[14] A method for recovering a substrate, comprising removing an oxygen barrier layer from a laminate comprising a first substrate and an oxygen barrier layer formed on the first substrate, the oxygen barrier layer being made of the coating composition for forming an oxygen barrier layer according to any one of [1] to [6] above, or a laminate comprising the first substrate, a second substrate, and the oxygen barrier layer, the method comprising the step of removing the oxygen barrier layer from the laminate using an alkaline solution. Effect of the Invention
[0015] According to the present invention, it is possible to provide a coating composition for forming an oxygen barrier layer, which exhibits excellent oxygen barrier properties (including aroma retention) with low oxygen permeability and is capable of forming an oxygen barrier layer in which the formed coating film exhibits excellent release properties. In addition, the oxygen barrier layer having the above-mentioned excellent functions formed by the coating composition for forming an oxygen barrier layer of the present invention has excellent adhesion to the substrate, and when formed into a laminate having a laminate structure, it also has excellent laminate strength. Therefore, according to the present invention, it is possible to provide a laminate having excellent oxygen barrier properties, for example, a film packaging having good oxygen barrier properties and aroma retention. In addition, it is possible to provide a laminate in which the oxygen barrier layer constituting the laminate exhibits excellent adhesion and good release properties from the substrate, enabling the recycling of the substrate film. In addition, according to the present invention, it is also possible to provide a laminate having a laminate structure having excellent laminate strength in addition to the above-mentioned excellent properties, and a film packaging made of the laminate. Furthermore, according to a preferred embodiment of the coating composition for forming an oxygen barrier layer of the present invention, which uses a polyhydroxyurethane resin made from carbon dioxide as a raw material, in addition to the above, it is possible to provide a coating composition for forming an oxygen barrier layer that is useful from the viewpoint of global environmental conservation, which can contribute to solving the problem of global warming and can form a more stable and excellent oxygen barrier layer. Furthermore, according to the study by the present inventors, by using a resin having a hydroxyl value specified in the present invention as a polyurethane resin, a more specific example being a material such as a polyhydroxyurethane resin, it is possible to vapor-deposit a metal or metal oxide such as aluminum or silica directly onto the formed oxygen barrier layer. As a result, according to the present invention, an excellent effect in terms of production is obtained, which is that it is not necessary to provide a primer as a base. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The present invention will be described in detail below with reference to preferred embodiments for carrying out the present invention. However, the present invention is not limited to the following embodiments. The coating composition for forming an oxygen barrier layer of the present invention (hereinafter, may be simply referred to as "coating composition") contains a polyurethane resin and a layered clay mineral, the polyurethane resin has a hydroxyl value of 100 to 400 mgKOH / g and an acid value of 15 to 70 mgKOH / g, the layered clay mineral has an average aspect ratio of 150 to 350, and the ratio of solids in the polyurethane resin and the layered clay mineral is 100:1 to 100:35 by mass.
[0017] The coating composition for forming an oxygen barrier layer of the present invention is used to form an oxygen barrier layer of a laminate (laminate-1) in which an oxygen barrier layer is formed on a first substrate (sometimes referred to as substrate 1), or a laminate (laminate-2) having an oxygen barrier layer with a first and second substrate (sometimes referred to as substrate 2). These laminates have a remarkable effect that the oxygen barrier layer formed on the first substrate can be easily removed, which was not realized in conventional laminates, and a recyclable plastic film (substrate) can be easily obtained. Furthermore, when the coating composition of the present invention is applied to a laminate having two substrates, a first and a second substrate (a laminate having a laminate structure), it has a remarkable effect that the oxygen barrier layer formed on the first substrate can be easily removed, and a laminate having excellent laminate strength can be obtained.
[0018] Hereinafter, each component constituting the coating composition for forming an oxygen barrier layer of the present invention will be described. [Polyurethane resin] The polyurethane resin constituting the coating composition of the present invention must have a hydroxyl value of 100 to 400 mgKOH / g and an acid value of 15 to 70 mgKOH / g. The method for synthesizing the polyurethane resin having the above-mentioned characteristics used in the present invention is not particularly limited, and it can be easily produced by utilizing a conventionally known method. For example, a synthesis method by reacting a bifunctional cyclic carbonate compound with a polyamine can be used (see, for example, U.S. Patent No. 3,072,613). In the present invention, it is particularly preferable to use a polyhydroxyurethane resin obtained by reacting a cyclic carbonate compound obtained by reacting an epoxy compound with carbon dioxide with a polyamine (see, for example, Japanese Patent No. 6,224,529). Specifically, by using a polyhydroxyurethane resin having a hydroxyl value of 100 to 400 mgKOH / g and an acid value of 15 to 70 mgKOH / g as the polyurethane resin constituting the coating composition of the present invention, an oxygen barrier layer having excellent oxygen barrier properties and aroma retention properties, and a laminate having excellent oxygen barrier properties and the oxygen barrier layer, for example, a film packaging product made of the laminate, can be more stably obtained. Details of the polyhydroxyurethane resin suitable as the polyurethane resin constituting the present invention will be described later.
[0019] As described above, the polyurethane resin constituting the coating composition of the present invention has a hydroxyl value of 100 to 400 mgKOH / g. The hydroxyl value is preferably 120 to 350 mgKOH / g, more preferably 150 to 300 mgKOH / g. Furthermore, it is more preferable to use a polyurethane resin having a hydroxyl value of 170 to 250 mgKOH / g. By using a polyurethane resin having a hydroxyl value in the above range, an oxygen barrier layer having high oxygen barrier properties is formed, and a laminate having excellent oxygen barrier properties and aroma retention properties, for example, a film packaging body made of the laminate, can be obtained. If the hydroxyl value of the polyurethane resin is less than the lower limit of the above range, the oxygen barrier properties and aroma retention properties of the formed oxygen barrier layer are poor, while if it exceeds the upper limit of the above range, the resin becomes hard, which is undesirable in the following respects. According to the inventors' investigations, particularly when made into a laminate, the adhesion between the first substrate and the oxygen barrier layer in "Laminate-1" is poor, and when made into a laminate film in "Laminate-2", the laminate strength is poor.
[0020] The acid value of the polyurethane resin constituting the coating composition of the present invention must be 15 to 70 mgKOH / g. It is also preferable that it is 15 to 60 mgKOH / g, 20 to 55 mgKOH / g, and more preferably 30 to 50 mgKOH / g, 35 to 45 mgKOH / g. If the acid value of the polyurethane resin is less than the lower limit, the releasability is poor, and the miscibility with water is reduced, resulting in another problem of poor stability as an emulsion. Regarding the releasability, for example, as shown in Comparative Example 6, the peeling test results when a polyurethane resin having an acid value of 10 mgKOH / g was used showed that the peeling of the coating film was less than 10%. This point will be described later. On the other hand, if the acid value of the polyurethane resin exceeds the upper limit, it is not preferable in terms of a decrease in water resistance. According to the study by the present inventors, by using a polyurethane resin having an acid value within the above range, an oxygen barrier layer having excellent releasability can be obtained.
[0021] The weight average molecular weight of the polyurethane resin is preferably 10,000 to 1,200,000, more preferably 30,000 to 200,000, and further preferably 50,000 to 100,000. According to the study by the present inventors, when a polyurethane resin having a weight average molecular weight of less than 10,000 is used, physical properties such as water resistance may be reduced. On the other hand, according to the study by the present inventors, when a polyurethane resin having a weight average molecular weight of more than 12,000,000 is used, the laminate strength when made into a laminate film, which is "laminate-2", may be reduced. According to the study by the present inventors, by using a polyurethane resin having a weight average molecular weight within the above range, a laminate having both physical properties such as water resistance and laminate strength and adhesion, and a film packaging body made of the laminate can be obtained.
[0022] The content of the polyurethane resin constituting the coating composition of the present invention is preferably 10 to 80% by mass. If the content of the polyurethane resin is less than 10% by mass, the drying speed may decrease when the coating composition is printed or applied as a coating liquid, and there is a concern of a decrease in productivity. On the other hand, since the viscosity of the coating liquid may increase, it is preferable that the content of the polyurethane resin does not exceed 80% by mass. From the above, it is preferable that the content of the polyurethane resin is 10% by mass or more because if it is less than 10% by mass, there is a concern of a decrease in productivity due to a decrease in the drying speed during printing, and it is preferable that it does not exceed 80% by mass because the viscosity of the coating liquid increases.
[0023] (Polyhydroxyurethane resin) As mentioned above, it is preferable to use a polyhydroxyurethane resin synthesized as follows as the polyurethane resin used in the present invention. The polyhydroxyurethane resin is obtained by reacting a cyclic carbonate compound obtained by reacting an epoxy compound with carbon dioxide with a polyamine. The polyhydroxyurethane resin obtained by this synthesis method has a characteristic structure having a hydroxyl group (hydroxy group) in the main chain. An example of a polyhydroxyurethane resin that can be suitably used in the coating composition of the present invention is shown below.
[0024] In the coating composition of the present invention, for example, a polyhydroxyurethane resin having a repeating unit represented by the following general formula (1) as a basic structure and a chemical structural portion having a carboxy group represented by the following general formula (6) can be preferably used. TIFF0007554337000001.tif44170 [In the general formula (1), -X- is a direct bond, an aliphatic hydrocarbon group having 1 to 30 carbon atoms, an alicyclic hydrocarbon group having 4 to 40 carbon atoms, or an aromatic hydrocarbon group having 6 to 40 carbon atoms, and the structure of these groups may contain any of an ether bond, an amino bond, a sulfonyl bond, and an ester bond, or any of a hydroxyl group, a halogen atom, and a polyalkylene glycol chain having 2 to 6 carbon atoms and repeating units of 1 to 30 as a substituent. Y- is an aliphatic hydrocarbon group having 1 to 15 carbon atoms, an alicyclic hydrocarbon group having 4 to 15 carbon atoms, or an aromatic hydrocarbon group having 6 to 15 carbon atoms, and the structure of these groups may contain any of an ether bond, a sulfonyl bond, or a hydroxyl group and a halogen atom as a substituent. -Z1- and -Z2- each independently represent at least one structure selected from the group consisting of the following formula (2), formula (3), general formula (4) and general formula (5), and two or more structures selected from these formulas (2) to (5) may be mixed either within a repeating unit or between repeating units. In addition, in any of the formulas (2) to (5) selected, the right bond is bonded to an oxygen atom, and the left bond is bonded to X, and when X is a direct bond, it is bonded to the left bond of the other Z.] TIFF0007554337000002.tif98170 [In general formula (4) or (5), R represents a hydrogen atom or a methyl group.] TIFF0007554337000003.tif60170 [In the general formula (6), -W- is an aliphatic hydrocarbon group having 1 to 30 carbon atoms, an alicyclic hydrocarbon group having 4 to 40 carbon atoms, or an aromatic hydrocarbon group having 6 to 40 carbon atoms, and the structure of these groups may contain any one of an ether bond, an amino bond, a sulfonyl bond, and an ester bond, or any one of a hydroxyl group, a halogen atom, and a polyalkylene glycol chain having 2 to 6 carbon atoms and 1 to 30 repeating units as a substituent. Y- is a moiety that bonds to the urethane structure having a bond in the general formula (1), and may be selected from those that can be selected as Y- in the general formula (1). -V- is a hydrocarbon group having 1 to 10 carbon atoms, or an aromatic hydrocarbon group having 6 to 10 carbon atoms, and the structure of these groups may contain an oxygen atom or a nitrogen atom.]
[0025] [Layered clay minerals] The coating composition of the present invention is characterized in that it contains a polyurethane resin having a specific hydroxyl value and a specific acid value as defined in the present invention as described above, and a specific layered clay mineral as described below, and the ratio of solid content of the polyurethane resin to the layered clay mineral is 100:1 to 100:35 by mass. The layered clay mineral will be described below.
[0026] The layered clay mineral used in the coating composition of the present invention is a material having a layered structure, which is composed of a large number of sheets of silicate minerals having a layered structure laminated together. What is important in the coating composition of the present invention is that a specific layered clay mineral having an average aspect ratio of 150 to 350 is used as the layered clay mineral to be used in combination with the polyurethane resin having the above-mentioned characteristics. The layered clay mineral constituting the present invention must have an average aspect ratio of 150 to 350. In addition, the average aspect ratio is preferably 170 to 330, more preferably 190 to 310, and even more preferably 210 to 290. If the average aspect ratio is less than the lower limit, the oxygen barrier property of the coating film formed by the coating composition of the present invention is poor, while if the average aspect ratio exceeds the upper limit, thixotropy is expressed, and the adhesion and lamination strength of the coating film are reduced, which is not preferable. According to the studies of the present inventors, by using a layered clay mineral having an average aspect ratio in the above range as a component of the coating composition of the present invention, it is surprisingly possible to form an oxygen barrier layer having excellent oxygen barrier properties and aroma retention properties, and to form a laminate having the oxygen barrier layer that is useful as a material for forming a film packaging. The "aspect ratio of the layered clay mineral" in the present invention is the value of the planar diameter of the clay mineral particle relative to the thickness of the particle.
[0027] The average aspect ratio of the layered clay mineral defined in the present invention is a value measured and calculated by the following procedure. It is an arithmetic average value obtained by using the aspect ratio values measured for 20 or more particles randomly selected from clay mineral particles observed by a scanning electron microscope (SEM). The aspect ratio for one clay mineral particle was obtained as follows. Using an SEM image of one clay mineral particle, the planar diameter and thickness of the particle were measured, and the aspect ratio was calculated by dividing the measured planar diameter by the measured thickness. At that time, the major axis of the clay mineral particle was used as the planar diameter. The thickness of the particle can be almost the same, but the measured value of the thicker part was used. In the specification of the present invention, the arithmetic average value obtained from the aspect ratios measured for each of 20 clay mineral particles was used as the average aspect ratio. According to the study by the present inventors, an objective average aspect ratio can be obtained by using the aspect ratios of 10 or more, more preferably about 20, randomly selected clay mineral particles.
[0028] The layered clay mineral constituting the present invention is preferably one having a particle size of 1.0 μm to 20 μm. The particle size is more preferably 3 μm to 15 μm, and even more preferably 3 μm to 12 μm. The particle size of the layered clay mineral described above is the value of the median diameter (50% particle size) obtained by laser diffraction / scattering type particle size distribution measurement. If the particle size is smaller than the above value, sufficient barrier properties may not be exhibited. On the other hand, if the particle size is too large than the above range, the adhesion and lamination strength may decrease. According to the study by the present inventors, by using a layered clay mineral having a particle size within the above range, a laminate that combines physical properties such as water resistance and barrier properties, and a film packaging product made of the laminate can be obtained.
[0029] Examples of the layered clay minerals constituting the present invention include montmorillonite, saponite, hectorite, vermiculite, kaolinite, and mica. According to the study by the present inventors, montmorillonite, saponite, and mica are particularly preferred. These layered clay minerals can be either natural or synthetic. In addition, a mixture of multiple types of clay minerals such as those listed above may be used.
[0030] Specific examples of such layered clay minerals include Benton EW, Benton MA, Benton AD (all manufactured by Rheox Corporation), Kunipia F, Kunipia G, Kunigel VA, Sumecton SA (all manufactured by Kunimine Kogyo Co., Ltd.), Lucentite SWN, Lucentite SWF, Somasif ME (all manufactured by Katakura Coop Agri Co., Ltd.), Sanbentonite KG-1, Sanbentonite K-1, Sanbentonite KA-1 (all manufactured by Sanbentonite Kogyo Co., Ltd.), and the like.
[0031] [Ratio of polyurethane resin and layered clay mineral solids] The coating composition for forming an oxygen barrier layer of the present invention is characterized in that the ratio of the solid content of the polyurethane resin to the layered clay mineral is 100:1 to 100:35 on a mass basis. This ratio is more preferably 100:2 to 100:35, and even more preferably 100:10 to 100:35. If the solid content ratio of the polyurethane resin to the layered clay mineral is less than 100:1, sufficient barrier properties are not exhibited. On the other hand, if it exceeds 100:35, it is not preferable because the fluidity, adhesion to the substrate, and laminate strength are poor when the coating composition is used as a coating liquid. According to the study by the present inventors, the coating composition of the present invention, by setting the solid content ratio of the polyurethane resin to the layered clay mineral within the above range, can realize the formation of an oxygen barrier layer that has excellent laminate strength when made into a laminate film corresponding to the "laminate-2" of the above-mentioned configuration, and also has excellent adhesion to the substrate in the "laminate-1" and "laminate-2".
[0032] [Hardening agent] In the coating composition of the present invention, a curing agent is also blended as a component other than the polyurethane resin and layered clay mineral described above, which is a preferred embodiment. According to the coating composition of the present invention having a configuration in which a curing agent is blended, a crosslinked coating film can be formed on the first substrate. The oxygen barrier layer formed by the coating composition of the present invention in which a curing agent is blended becomes a crosslinked coating film, and thus excellent effects can be obtained in terms of adhesion, laminate strength, and water resistance. There is no particular limitation on the curing agent that can be used in the present invention. For example, polyisocyanates, blocked isocyanates, epoxy compounds, metal chelate compounds such as aluminum and titanium, melamine resins, aldehyde compounds, carbodiimides, etc. can be used. Among these, it is preferable to use an epoxy compound as a curing agent.
[0033] [solvent] The coating composition of the present invention may contain an appropriate solvent as necessary, as a component other than the polyurethane resin and layered clay mineral described above. Examples of the solvent used in the present invention include water; lower alcohols such as methanol, ethanol, n-propanol, isopropanol, and n-butanol; ketone-based organic solvents such as methyl ethyl ketone and methyl isobutyl ketone; and ester-based organic solvents such as ethyl acetate, n-propyl acetate, isopropyl acetate, and n-butyl acetate. These solvents may be used alone or in combination of two or more.
[0034] In the coating composition of the present invention, among the above-mentioned solvents, it is particularly preferable to use a mixed solvent containing water and isopropanol as the main component. The reasons for using such a mixed solvent are as follows. First, by using water as a solvent, the problems of odor and performance deterioration due to residual organic solvents can be eliminated, and a coating composition with reduced environmental impact can be obtained. In addition, by using isopropanol as a solvent, when forming an oxygen barrier layer on the substrate 1 to form a laminate, the coating composition has excellent leveling and defoaming properties, and the drying time after applying the coating composition to the substrate 1 can be shortened, which are advantages in manufacturing.
[0035] [Other additives] The coating composition of the present invention may contain various additives as appropriate in accordance with the required properties, other than those described above. Examples of additives that can be used include wax, fatty acid amide, silica, dispersant, leveling agent, defoamer, antioxidant, light stabilizer, ultraviolet absorber, and rheology adjuster.
[0036] [Method of producing coating composition] The method for producing the coating composition of the present invention is not particularly limited, and can be produced by a conventionally known production method. For example, a method of adding a specific polyurethane resin specified in the present invention to an aqueous dispersion obtained by dispersing the layered clay mineral specified in the present invention in a mixed solvent containing water in advance can be mentioned. In addition, a method of mixing and dispersing the polyurethane resin, layered clay mineral, and solvent at once is also possible. The method for dispersing the layered clay mineral is not particularly limited, and can be appropriately selected from, for example, a disperser, a roller mill, a ball mill, a pebble mill, an attritor, a sand mill, and a paint conditioner.
[0037] [Laminate] Next, a laminate characterized by being formed of the coating composition of the present invention and having the above-described excellent functionality as an oxygen barrier layer will be described.
[0038] (Laminate-1) Laminate-1, which is one embodiment of the present invention, is characterized by comprising a first substrate and an oxygen barrier layer formed from the coating composition of the present invention. Here, the thickness of the oxygen barrier layer formed on the substrate is not particularly limited, but in the case of a laminate applied to a film packaging body, it is, for example, about 0.5 to 3 μm. Laminate-1 may further have layers other than the first substrate and the oxygen barrier layer, for example, a pattern layer made of a printing ink, a deposition layer made by depositing a metal or a metal oxide such as aluminum or silica, etc.
[0039] According to the study by the present inventors, by using a polyurethane resin having a hydroxyl value with the characteristics specified in the present invention that constitutes the coating composition of the present invention, it becomes possible to directly vapor-deposit aluminum, silica, etc. on the oxygen barrier layer formed by the coating composition. Since aluminum, silica, etc. can be directly vapor-deposited on the oxygen barrier layer, an excellent effect in terms of production is obtained that a vapor-deposited layer can be easily formed in the production of a laminate. In contrast, in the conventional technology, when a vapor-deposited layer formed by vapor-depositing aluminum, silica, etc. is formed, a primer layer as a base must be formed, which causes a problem of complicated processes. According to the study by the present inventors, when a polyhydroxyurethane resin, for example, is used as a polyurethane resin with the characteristics specified in the present invention, the above-mentioned effects can be obtained more stably.
[0040] Examples of the laminate structure included in the laminate-1 include a structure in which an oxygen barrier layer specific to the present invention is provided on the surface of a first substrate, and a structure in which an oxygen barrier layer specific to the present invention is provided on the surface of a first substrate having a pattern layer. When preparing the laminate-1 having the above-mentioned structure, for example, the useful oxygen barrier layer described above can be easily produced by applying the coating composition of the present invention and then removing the volatile components. Here, the method of applying the coating composition of the present invention is not particularly limited, and the coating composition can be easily and stably applied by using, for example, a gravure coater, a knife coater, a reverse coater, a bar coater, a spray coater, a slit coater, or the like. The thickness of the oxygen barrier layer constituting the present invention formed on the surface of the first substrate is not particularly limited depending on its use, but considering the releasability of the formed oxygen barrier layer, it is, for example, about 0.5 to 3 μm, more preferably about 1 to 2 μm.
[0041] (Laminate-2) Next, the laminate-2, which is one embodiment of the present invention and has a different structure from the laminate-1 described above, will be described. As described above, the laminate-1 is characterized by having a first substrate and an oxygen barrier layer formed from the coating composition of the present invention, while the laminate-2 is characterized by having a second substrate. That is, the laminate-2 of the present invention is a laminate having a structure including a first substrate, a second substrate, and a specific oxygen barrier layer formed from the coating composition of the present invention, and has a form of a so-called laminate film. The laminate-2 may have a first substrate, a second substrate, and other layers other than the specific oxygen barrier layer. For example, the other layers may include a pattern layer made of a printing ink, an adhesive layer made of an adhesive, and a deposition layer formed by depositing a metal or metal oxide such as aluminum or silica. More specifically, the laminate-2 may be in the form of a laminate film in which an adhesive layer and a second substrate are further laminated in this order on the specific oxygen barrier layer formed on the first substrate. As described above, the oxygen barrier layer formed from the coating composition of the present invention has the advantage that aluminum, silica, etc. can be directly vapor-deposited on the oxygen barrier layer. Therefore, according to the present invention, the laminate-2 having the vapor-deposited layer can be easily obtained.
[0042] When the laminate-2 is a laminate film having the above-mentioned configuration, it can be easily manufactured, for example, by the following method. First, an adhesive is applied to the surface of the specific oxygen barrier layer of the laminate-1 of the present invention manufactured as described above, thereby laminating and forming an adhesive layer, and then a second substrate is attached onto the adhesive layer to manufacture a laminate film. By making a laminate film having such a configuration, it is possible to obtain a laminate film of the laminate-2 having a configuration in which, in addition to the performance realized by the laminate-1, other desired functions are added.
[0043] (base material) Examples of the substrate 1 or substrate 2 used in the laminate of the present invention having the above-described configuration include plastic films appropriately selected from polyethylenes such as high density polyethylene (HDPE), low density polyethylene (LDPE), linear low density polyethylene (LLDPE), polypropylene, polyesters such as polyethylene terephthalate (PET) and polybutylene terephthalate (PBT), nylon (NY), and the like. As the substrate 1 for forming the oxygen barrier layer made of the coating composition of the present invention, it is preferable to use polyolefin films such as polyethylenes and polypropylene among those listed above. In this case, it is preferable to use a corona-treated film. In addition, any of the substrates used in the production of the laminate of the present invention may be made of recycled materials that have been used once as a printed matter and then recovered. In addition, any of the substrates used in the production of the laminate of the present invention may be stretched or unstretched. Furthermore, the substrate may be one on which a metal or metal oxide such as silica, alumina, or aluminum is vapor-deposited, or one on which the vapor-deposited surface is coated with a paint such as polyvinyl alcohol.
[0044] [Method of removing the oxygen barrier layer (coating film) from the substrate] The method for removing an oxygen barrier layer (coating film) of the present invention is characterized by having a step of immersing a laminate-1 in which an oxygen barrier layer made of the coating composition for forming an oxygen barrier layer of the present invention is formed on a first substrate, or a laminate-2 in which an oxygen barrier layer formed by laminating a first substrate and a second substrate is formed, in an alkaline aqueous solution to remove the oxygen barrier layer from the first substrate. According to the removal method of the present invention, as described above, the coating film formed on the first substrate can be removed in a good condition by a very simple method. Examples of the alkaline aqueous solution used above include ammonia water, sodium hydroxide aqueous solution, potassium hydroxide aqueous solution, calcium hydroxide, sodium hydrogen carbonate, potassium hydrogen carbonate, sodium carbonate, potassium carbonate, and aqueous solutions. Among them, it is preferable to use a sodium hydroxide aqueous solution, which is widely used.
[0045] The conditions for immersing the laminate of the present invention in an alkaline aqueous solution are not particularly limited, but it is preferable to determine the concentration, temperature, immersion time, etc. of the alkaline aqueous solution to be used by observing the state in which the coating film formed on the substrate is removed. As the alkaline aqueous solution, it is preferable to use an alkaline aqueous solution having a concentration of, for example, about 1 to 5% by mass. According to the study by the present inventors, for example, when removing the coating film using an aqueous sodium hydroxide solution having a concentration of about 1.5 mass percent, a good peeling (removal) of the coating film can be performed by a very simple and quick treatment of immersing the laminate in an aqueous solution at a temperature of about 40°C to 80°C for a short period of time of about 5 to 30 minutes. More specifically, in the case of a laminate-1 formed by forming a coating film on a first substrate, for example, the laminate-1 is put into an aqueous sodium hydroxide solution of 1.5 mass percent, and is immersed therein, and the coating film can be peeled off from the substrate 1 and removed in a good state by treating with stirring at 40°C for about 5 minutes. In the case of a laminate-2 having a first and second substrate, for example, the coating film can be peeled off from the first substrate and detached in a good condition from the first substrate by immersing the laminate-2 in a 1.5 mass percent aqueous solution of sodium hydroxide and stirring at 80° C. for about 30 minutes. Details of the above-mentioned detachment test will be described later.
[0046] [How to recover substrate material] The method for recovering a substrate of the present invention is a method for recovering a substrate by removing an oxygen barrier layer (coating film) from a laminate-1 in which an oxygen barrier layer made of the coating composition for forming an oxygen barrier layer of the present invention is formed on a first substrate, or a laminate-2 in which an oxygen barrier layer formed by laminating a first substrate and a second substrate is formed, and is characterized by having a step of immersing the laminate in an alkaline aqueous solution to remove the oxygen barrier layer from the substrate. By carrying out the extremely simple and rapid oxygen barrier layer removal method of the present invention described above, the oxygen barrier layer (coating film) can be removed (peeled off) from the first substrate very easily and quickly. As a result, the coating film is easily peeled off from the first substrate, and the coating film removed from the substrate remains in the alkaline aqueous solution in which the laminate is immersed, and a first substrate from which the coating film has been removed in a good state is obtained. For example, if the coating film is 80% or more peeled off from the first substrate, it is possible to use the substrate as a recycled film simply by cleaning the recovered substrate surface. EXAMPLES
[0047] The present invention will be specifically described below based on examples and comparative examples, but the present invention is not limited to these examples. In the examples and comparative examples, "parts" and "%" are based on mass unless otherwise specified.
[0048] [Production Example 1: Synthesis of cyclic carbonate-containing compound (IA)] 100 parts of bisphenol A diglycidyl ether with an epoxy equivalent of 192 (trade name: jER828, manufactured by Japan Epoxy Resins Co., Ltd.), 20 parts of sodium iodide (manufactured by Wako Pure Chemical Industries, Ltd.), and 100 parts of N-methyl-2-pyrrolidone were charged into a reaction vessel equipped with a stirrer and a reflux condenser with an air opening. Then, carbon dioxide was continuously blown in while stirring, and the reaction was carried out at 100°C for 10 hours. Then, 1400 parts of isopropanol was added to the solution after the reaction was completed, and the reaction product was precipitated as a white precipitate and filtered off. The obtained precipitate was recrystallized with toluene to obtain 52 parts of white powder (yield 42%).
[0049] The white powder obtained above was analyzed by a Fourier transform infrared spectrophotometer (FT-IR) FT-720 (trade name, manufactured by Horiba, Ltd.; the same device was used in the following production examples). -1 The absorption due to the epoxy group of the nearby raw material disappeared, while the absorption at 1800 cm -1 Absorption from the carbonyl of the carbonate group, which is not present in the raw material, was confirmed near the peak. In addition, analysis by high performance liquid chromatography (HPLC) LC-2000 (product name, manufactured by JASCO Corporation, column FinepakSIL C18-T5; mobile phase acetonitrile + water) showed that the peak of the raw material disappeared and a new peak appeared on the high polarity side, and the purity was 98%. In addition, as a result of DSC measurement (differential scanning calorimetry), the melting point was 178 ° C, and the melting point range was ± 5 ° C.
[0050] From the above, this powder was confirmed to be a compound with the structure shown in the following formula, in which cyclic carbonate groups were introduced by the reaction of epoxy groups with carbon dioxide. This was abbreviated as IA. The proportion of carbon dioxide-derived components in the chemical structure of IA was 20.5% (calculated value).
[0051] TIFF0007554337000004.tif38170
[0052] [Production Example 2: Production of carboxyl group-containing polyhydroxyurethane resin] In a reaction vessel equipped with a stirrer and a reflux condenser with an air opening and capable of vacuum distillation, 22.4 parts of bisphenol A diglycidyl ether (trade name: jER828, manufactured by Japan Epoxy Resins Co., Ltd.), 33.9 parts of hexamethylenediamine (manufactured by Tokyo Chemical Industry Co., Ltd.), and 112 parts of tetrahydrofuran (THF) as a reaction solvent were added and reacted for 12 hours while stirring at a temperature of 60° C. Next, 100 parts of the cyclic carbonate-containing compound IA obtained in Production Example 1 were added, and the reaction was carried out for 24 hours while stirring at a temperature of 60° C.
[0053] The resin solution after the reaction was analyzed by FT-IR. -1The absorption due to the carbonyl group of the cyclic carbonate observed in the vicinity has completely disappeared, and a new absorption at 1760 cm -1 Absorption due to the carbonyl group of the urethane bond was confirmed near the amine value. The amine value measured using the resulting resin solution was 41.93 mg KOH / g, calculated as a value of 100% resin (measured in accordance with JIS K-1557).
[0054] Next, 140 parts of tetrahydrofuran (THF) was added to this resin solution to dilute it, and then 11.5 parts of maleic anhydride (Tokyo Chemical Industry Co., Ltd.) was added and the reaction was carried out at room temperature. -1 The reaction was terminated when it was confirmed that the peak had disappeared.
[0055] Next, 7.8 parts of 28% ammonia water was added into the reaction vessel to neutralize the carboxyl group. Then, 453 parts of ion-exchanged water was gradually added while stirring at room temperature to perform phase inversion emulsification. Next, the reaction vessel was heated to 50°C, reduced pressure, and THF was distilled off to obtain an aqueous dispersion in which the polyhydroxyurethane resin was dispersed in water. The obtained aqueous dispersion was adjusted so that the solid content was 30%. As a result, the aqueous dispersion was uniform in appearance. In addition, the hydroxyl value of the obtained polyhydroxyurethane resin was 187 mgKOH / g, the acid value was 40 mgKOH / g, and the weight average molecular weight was 71,000. The obtained polyhydroxyurethane resin is abbreviated as PU-1.
[0056] [Production Example 3: Production of Polyurethane Resins PU-2 to PU-6 and PU-8 to PU-10] Aqueous dispersions with a solid content of 30% of polyurethane resins PU-2 to PU-6 and PU-8 to PU-10 with different hydroxyl values were prepared by the same method as in Production Example 2. As shown in Table 2, PU-9 has a larger hydroxyl value than that specified in the present invention, and PU-10 has a smaller hydroxyl value than that specified in the present invention. In addition, PU-8 has a smaller acid value than that specified in the present invention. PU-7 is a commercially available polyurethane resin (manufactured by Dainichiseika Color & Chemicals Co., Ltd.) that does not have a hydroxyl group.
[0057] [Preparation of aqueous dispersions A-1 to A-6 of layered clay minerals] As the aqueous dispersion A-4 of the layered clay mineral, a commercially available dispersion (solid content 8% by mass) in which mica A-4 (average aspect ratio = 264, median diameter = 8 µm) was dispersed in water was used.
[0058] Table 1 shows the average aspect ratio and median diameter of each of the micas A-1 to A-3, A-5, and A-6, each of which has a different average aspect ratio and median diameter, 8 parts each was mixed with 92 parts water, and the mixture was filled into a container together with glass beads and dispersed for 1 hour in a paint conditioner to obtain aqueous dispersions A-1 to A-3, A-5, and A-6 of layered clay minerals. The solid content of each of the obtained aqueous dispersions of layered clay minerals was 8 mass%.
[0059] [Preparation of aqueous dispersion B-1 of layered clay mineral] Using mica B (average aspect ratio = 55, median diameter = 4 μm), 8 parts of mica B and 92 parts of water were mixed, filled into a container together with glass beads, and dispersed in a paint conditioner for 1 hour to obtain a layered clay mineral aqueous dispersion B-1. The solid content of the obtained layered clay mineral aqueous dispersion B-1 was 8 mass%.
[0060] [Preparation of aqueous dispersions B-2 and B-3 of layered clay minerals] Aqueous dispersions of layered clay minerals with a solid content of 8% by mass, B-2 and B-3, were prepared in the same manner as in the above-mentioned manufacturing example, except that the formulations were as shown in Table 1. The properties of each layered clay mineral used are summarized in Table 1. Table 1 also lists mica A-4 constituting aqueous dispersion A-4. The average aspect ratio and median diameter shown in Table 1 are values measured by the method described above.
[0061] TIFF0007554337000005.tif112170
[0062] [Example 1] As shown in Table 3-1, 56.25 parts of the aqueous dispersion A-4 of the layered clay mineral having a solid content of 8% described above, 50 parts of the polyhydroxyurethane resin having a solid content of 30% (abbreviated as PU-1 in the table) prepared in the previous Production Example 2, 12.4 parts of water, and 3.1 parts of isopropanol (IPA) were mixed to obtain a coating composition for forming an oxygen barrier layer in this example. The solid content ratio of the polyurethane resin to the layered clay mineral in the obtained coating composition was 100:30 by mass.
[0063] [Examples 2 to 15, Comparative Examples 1 to 8] The coating compositions for forming oxygen barrier layers of Examples 2 to 15 and Comparative Examples 1 to 8 were obtained in the same manner as in Example 1, except that the raw materials for preparation were blended as shown in Table 3 (Table 3-1 to Table 3-3) and Table 4 (Table 4-1, Table 4-2), respectively. The curing agent used in Example 6 was Denacol EX-614B (product name, manufactured by Nagase Chemtec Corporation: sorbitol polyglycidyl ether).
[0064] Table 2 shows the properties of the polyurethane resins used in preparing the coating compositions for forming oxygen barrier layers in the examples and comparative examples. As shown in Table 2, PU-7 has a hydroxyl value of 0 mgKOH / g, and PU-8 has an acid value of 10 mgKOH / g, both of which are polyurethane resins with hydroxyl and acid values outside the ranges specified in the present invention and were used in comparative examples. Furthermore, PU-9 has a hydroxyl value larger than that specified in the present invention, and PU-10 has a hydroxyl value smaller than that specified in the present invention, both of which were used in comparative examples.
[0065] TIFF0007554337000006.tif108170
[0066] <Evaluation> For the coating compositions of the Examples and Comparative Examples, laminates were formed and evaluated according to the following evaluation methods and criteria. [Preparation of Laminate-1 and Laminate-2] First, each of the coating compositions obtained above was applied to a 50 μm-thick HDPE (high density polyethylene) film (product name: HS31, manufactured by Tamapoly Co., Ltd.) used as substrate 1 using a bar coater #16, and dried at 40° C. for 24 hours to produce a printed matter in which an oxygen barrier layer (hereinafter also referred to as a coating film) was formed on substrate 1. The printed matter corresponds to a "laminate-1" called a surface print, in which a coating film made of each coating composition was formed on substrate 1, which is a polyolefin-based substrate.
[0067] In addition, adhesive was applied to each of the printed materials at a dry weight of 3 g / m2. 2 The adhesive was applied so that the thickness of the adhesive layer was 10:1, and the adhesive layer was laminated with LLDPE (low density polyethylene). The adhesive was made of a mixture of "Seikabond E-263" and "Seikabond C-75N" (trade names of Dainichiseika Chemicals Mfg. Co., Ltd.). The laminate-2 obtained as described above is a so-called laminated form in which an adhesive layer and LLDPE, which is a second polyolefin-based base material, are laminated in this order on the oxygen barrier layer constituting the laminate-1. The "laminate-1" and "laminate-2" obtained as described above were used as laminates for evaluation tests, and were evaluated according to the following methods and criteria. Table 3 shows the evaluation results for each laminate made using the coating composition for forming an oxygen barrier layer of the embodiment of the present invention. Table 4 shows the evaluation results for the laminate having a coating film made using the coating composition of the comparative example, which was similarly evaluated.
[0068] (Evaluation method and criteria) [Adhesion] The adhesion of the oxygen barrier layer (coating) formed on the surface of the substrate 1 of the "Laminate-1" for evaluation test obtained above was evaluated using the following evaluation method and criteria. Specifically, Cellotape (registered trademark) (12 mm width, manufactured by Nichiban Co., Ltd.) was applied to the coating surface of the "Laminate-1", and the appearance of the oxygen barrier layer (coating) when it was peeled off in one go was evaluated using the following criteria. In the present invention, an evaluation of ◯ or higher was judged to be practical.
[0069] [Evaluation Criteria] ◎: More than 90% of the coating remains on the substrate ○: 70% to less than 90% of the coating film remains on the substrate △: 30% to less than 70% of the coating film remains on the substrate ×: Less than 30% of the coating film remains on the substrate.
[0070] [Desorption test] Using the "Laminate-1" for evaluation test obtained above, a peeling test was performed on the oxygen barrier layer (coating film) formed on the substrate 1 to evaluate the releasability by the following evaluation method. Specifically, the "Laminate-1" was placed in a 1.5 mass percent aqueous solution of sodium hydroxide and stirred at 40°C for 30 minutes, and the peeling (detachment) state of the "oxygen barrier layer (coating film)" formed on the substrate 1 was evaluated by visual observation and evaluated according to the following criteria. In addition, for the "Laminate-2" for evaluation test, the detachment performance of the coating film was evaluated in the same manner as the evaluation method performed for the "Laminate-1", except that the "Laminate-2" was placed in a 1.5 mass percent aqueous solution of sodium hydroxide and stirred at 80°C for 30 minutes.
[0071] The evaluation results are summarized in Table 3. In the present invention, the evaluation of the detachment test indicates that the greater the degree of peeling (detachment) of the coating film, the better the quality. In the present invention, an evaluation of 0 or higher was determined to facilitate separation and recovery of the substrate due to the improved detachment performance of the formed coating film.
[0072] [Evaluation Criteria] ◎: 80% or more of the coating has peeled off. ○: 50% or more but less than 80% of the coating has peeled off. △: 10% or more but less than 50% of the coating has peeled off. ×: Less than 10% of the coating peeled off.
[0073] [Laminate strength] As mentioned above, the "Laminate-2" to be evaluated was a laminate for evaluation test, which was obtained by aging (curing) at 40°C for 48 hours after lamination. The laminate strength of this "Laminate-2" was measured by measuring the load when peeled at 180° with a tensile speed of 100 mm / min, and evaluated according to the following criteria using the measured value. In the present invention, a rating of △ or higher was judged to be practical.
[0074] [Evaluation Criteria] ◎: Load exceeds 1.0N / 15mm ○: Load exceeds 0.6N / 15mm and is 1.0N / 15mm or less △: Load is 0.4N / 15mm or more and 0.6N / 15mm or less ×: Less than 0.4N / 15mm
[0075] [Oxygen transmission rate (OTR)] The oxygen permeability of each of the "Laminate-1" and "Laminate-2" obtained as described above for the evaluation test was measured in accordance with JIS K-7126. An OX-TRAN2-22H (trade name, manufactured by MOCON) was used as the oxygen permeability measuring device. Evaluation was performed according to the following criteria. In the present invention, an evaluation of △ or higher indicates that the formed coating film effectively functions as an oxygen barrier layer and is practical.
[0076] [Evaluation Criteria] ◎: 1.0ml / m 2 · Less than ATM·day ○: 1.0ml / m 2 ·atm·day or more, 10ml / m 2 · Less than ATM·day △: 10ml / m 2 ·atm·day or more, 200ml / m 2 · Less than ATM·day ×:200ml / m 2 More than just ATM day
[0077] [Fragrance retention] The "Laminate-1" obtained as described above was used to form a coating film made of a coating composition that was applied to a substrate 1, and the fragrance retention obtained by this was evaluated using the following evaluation method and evaluation criteria. Specifically, first, three types of commercially available shampoo, fabric softener, and body soap with different fragrances, as shown below, were used as fragrance sources in each of the prepared metal containers, and 1g of each fragrance source was placed in each container. Then, the openings (20cm) of the metal containers containing the different fragrance sources were opened and the fragrance sources were removed. 2 ) was covered with "Laminate-1" to be the subject of the evaluation test, with the coating surface (test print) facing the inside of the container, and the opening was then sealed with paraffin to prepare a sample for the aroma retention evaluation test. Each of the evaluation test samples obtained as described above was placed in an aluminum-deposited nylon (NY) bag, sealed, and after 24 hours at 25°C, the "aroma retention" was evaluated based on the level of aroma inside the NY bag.
[0078] The sensory test was conducted by three neutral panelists on the scent inside the NY bag, and was rated according to the following criteria. The sensory test was conducted under the condition that the evaluation of the majority of the three panelists would be adopted as the evaluation result. However, the evaluation results of the sensory test by the three panelists were all consistent, and no individual evaluations were made. The evaluation results are summarized in Tables 3 and 4. Furthermore, when an evaluation test of aroma retention was conducted on "Laminate-2" in the same manner as above, the same effect was obtained as when "Laminate-1" was used, and it was confirmed that "Laminate-2" also exhibits good aroma retention.
[0079] [Source of aroma] ·shampoo: Product name: Pantene Micellar Pure & Rose Water (P&G) Fabric softener: Product name: Lenor Super Deodorizer Fresh Green Scent (P&G) Body soap: Product name: Dove Peach & Sweet Pea (manufactured by Unilever)
[0080] [Evaluation Criteria] ◎: No scent at all 〇: Almost no scent △: The type of scent can be distinguished ×: Strong scent
[0081] TIFF0007554337000007.tif181170
[0082] TIFF0007554337000008.tif189170
[0083] TIFF0007554337000009.tif184170
[0084] TIFF0007554337000010.tif198170
[0085] TIFF0007554337000011.tif193170
[0086] [Example of use] (Evaluation of packaging made of laminate-2) Using the "Laminate-2" for evaluation test used previously in the evaluation, the second substrates of the Laminate-2 were overlapped and heat-sealed to obtain a bag-shaped package. The same evaluation test as that previously performed on the Laminate-2 was performed on each of the obtained packages. As a result, it was confirmed that the effects of the present invention described above could be obtained even with the packages after heat sealing.
[0087] [Examples of recovery and reuse of base materials] The coating composition for forming an oxygen barrier layer of Example 1 prepared above was used to form an oxygen barrier layer on the HDPE (high density polyethylene) film of substrate 1, and the laminate 2 was bonded to the laminate 1 with an adhesive to form a laminate 2 of LLDPE (low density polyethylene). The releasability of the oxygen barrier layer and whether each substrate 1 can be reused after the releasability were confirmed for the laminate 1 and the laminate 2. Specifically, as in the above-described releasability test, the laminate 1 was added to a 1.5 mass percent aqueous solution of sodium hydroxide and stirred at 40°C for 30 minutes to remove the oxygen barrier layer (coating film) formed on the substrate 1, and the laminate 2 was added to a 1.5 mass percent aqueous solution of sodium hydroxide and stirred at 80°C for 30 minutes to remove the oxygen barrier layer (coating film) formed on the substrate 1. Then, after "Laminate-1" and "Laminate-2" were pulled out of the sodium hydroxide aqueous solution and washed with water, visual observation confirmed that the oxygen barrier layer had been detached and removed in good condition from the substrate 1 of each laminate. Furthermore, for "Laminate-1," in which good detachment of the coating film was achieved under milder conditions than for "Laminate-2," the conditions for the detachment treatment were further relaxed, and "Laminate-1" was placed in a 1.5 mass percent aqueous solution of sodium hydroxide and stirred at 40°C for 5 minutes to detach the "oxygen barrier layer (coating film)" formed on the substrate 1. As a result, it was confirmed that good detachment of the coating film was achieved under these conditions as well.
[0088] The substrate 1 recovered after the above-mentioned coating film removal treatment was used to prepare strands using a twin-screw extruder, which were then cooled with water and crushed with a cutter to obtain pellets. The obtained pellets were pressed with a hot press to produce a sheet. When the produced sheet was visually observed, it was confirmed that the sheet had transparency. This means that the substrate can be recovered from the laminate in a simple manner, and the recovered substrate 1 can be recycled as it is.
Claims
1. A coating composition for forming an oxygen barrier layer, comprising a polyurethane resin and a layered clay mineral, The polyurethane resin has a hydroxyl value of 100 to 400 mgKOH / g and an acid value of 15 to 70 mgKOH / g; The layered clay mineral has an average particle size of 1.0 to 20 μm and an aspect ratio of 160 to 350; A coating composition for forming an oxygen barrier layer, characterized in that the ratio of solids in the polyurethane resin and the layered clay mineral is 100:1 to 100:35 on a mass basis.
2. 2. The coating composition for forming an oxygen barrier layer according to claim 1, wherein the layered clay mineral is at least one selected from the group consisting of montmorillonite, saponite, hectorite, vermiculite, kaolinite and mica.
3. 2. The coating composition for forming an oxygen barrier layer according to claim 1, wherein the polyurethane resin has a weight average molecular weight of 10,000 to 1,200,000.
4. 2. The coating composition for forming an oxygen barrier layer according to claim 1, wherein the polyurethane resin is a polyhydroxyurethane resin which is a reaction product of a cyclic carbonate compound which is a reaction product of an epoxy compound and carbon dioxide, and a polyamine.
5. The coating composition for forming an oxygen barrier layer according to any one of claims 1 to 4, further comprising an epoxy compound as a curing agent.
6. The coating composition for forming an oxygen barrier layer according to any one of claims 1 to 4, which is used for forming an oxygen barrier layer of a laminate film.
7. A laminate comprising an oxygen barrier layer formed on a first substrate, the oxygen barrier layer being made of the coating composition for forming an oxygen barrier layer according to any one of claims 1 to 4.
8. The laminate according to claim 7 , wherein the first substrate is made of any polyolefin-based resin.
9. The laminate according to claim 7 , wherein the first substrate is made of recycled material that has been recovered after one use.
10. The laminate according to claim 7, further comprising a first and a second substrate, the first and second substrates being formed by laminating an adhesive layer and a second substrate in this order on the oxygen barrier layer formed on the first substrate.
11. The laminate according to claim 10 , wherein the first substrate is made of any polyolefin-based resin.
12. The laminate according to claim 10 , wherein the first substrate and / or the second substrate is made of recycled materials that have been recovered after being used once.
13. A method for removing an oxygen barrier layer from a laminate comprising a first substrate and an oxygen barrier layer made of the coating composition for forming an oxygen barrier layer according to any one of claims 1 to 4, or from a laminate comprising the first substrate, a second substrate, and the oxygen barrier layer, the method comprising the step of removing the oxygen barrier layer from the laminate using an alkaline solution.
14. A method for recovering a substrate, comprising removing the oxygen barrier layer from a laminate comprising a first substrate and an oxygen barrier layer made of the coating composition for forming an oxygen barrier layer according to any one of claims 1 to 4, or from a laminate comprising the first substrate, a second substrate, and the oxygen barrier layer, to recover at least the first substrate, the method comprising the step of removing the oxygen barrier layer from the laminate using an alkaline solution.
Citation Information
Patent Citations
Barrier material having vapor deposition layer and laminated material using the same
JP1996318591A
Laminated and its manufacturing method
JP2002144515A
Barrier coating resin laminate and plastic container including the same
JP2014151631A
Gas-barrier coating agent and gas-barrier film
JP2014196419A
Polyhydroxyurethane water dispersion composition, gas barrier aqueous coating agent using the water dispersion composition and gas barrier film