Compositions Comprising Semiconducting Light-Emitting Nanoparticles Having Thiol-Functional Surface Ligands - Patent application

Compositions with semiconducting luminescent nanoparticles using a specific ligand and solvent improve dispersion and stability, addressing issues of initial quantum yield and optical density, enabling better performance at higher concentrations.

JP7554384B2Active Publication Date: 2024-09-20SAMSUNG ELECTRONICS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2019567741
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2017-06-08
Filing Date
2018-06-05
Publication Date
2024-09-20
Estimated Expiration
2038-06-05

AI Technical Summary

Technical Problem

Existing compositions of semiconducting luminescent nanoparticles face issues with dispersion, initial quantum yield, long-term stability, optical density, and dispersion at higher concentrations, necessitating improved formulations.

Method used

The development of compositions comprising semiconducting luminescent nanoparticles with a specific chemical formula (I) and a first material as a ligand, such as methoxy-PEG thiol, which is attached to the core or shell layer, and a solvent like propylene glycol alkyl ether acetate, enhancing dispersion and stability.

Benefits of technology

The new compositions exhibit improved dispersion, initial quantum yield, long-term stability, and higher optical density, allowing for better performance at higher concentrations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554384000021
    Figure 0007554384000021
  • Figure 0007554384000007
    Figure 0007554384000007
  • Figure 0007554384000009
    Figure 0007554384000009
Patent Text Reader

Abstract

The present invention relates to compositions comprising nanoparticles.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] Technical Field The present invention relates to compositions, formulations, uses of compositions, uses of formulations, optical media, and optical devices comprising semiconducting luminescent nanoparticles. [Background technology]

[0002] Background technology Semiconducting, luminescent nanoparticles comprising a core and at least one ligand, and compositions comprising semiconducting, luminescent nanoparticles, are known in the prior art. For example, J. Am. Chem. Soc. 9804, 132, 2010 discloses bis(DHLA)-PEG-OCH3 capped CdSe / ZnS and CdSe / CdZnS / ZnS QDs. J. Am. Chem. Soc. 739, 126, 2004 discloses CsSe nanoparticles bearing thioalkyl and thioalkylated oligo(ethylene glycol) ligands for the recognition of chymotrypsin (ChT). And QD beads with Zn-DDT (1-dodecanethiol) polymer are published in US 2016 / 0289552 A1. [Prior art documents] [Patent documents]

[0003] 1.US 2016-0289552 A1 [Non-patent literature]

[0004] 2. J. Am. Chem. Soc. 9804, 132 , 2010 3. J. Am. Chem. Soc. 739, 126 , 2004 Summary of the Invention [Problem to be solved by the invention]

[0005] SUMMARY OF THE PRESENT APPLICATION However, the present inventors have now discovered that there are still one or more significant problems for which improvement is desirable, as listed below.

[0006] 1. New compositions or formulations comprising one or more semiconducting, luminescent nanoparticles that exhibit improved dispersibility of the semiconducting, luminescent nanoparticles in the composition or formulation are desired. 2. New compositions or formulations are required that include one or more semiconducting luminescent nanoparticles that exhibit improved initial quantum yields of the semiconducting luminescent nanoparticles in the composition or formulation.

[0007] 3. New compositions or formulations are required that include one or more semiconducting, luminescent nanoparticles that exhibit long-term stability and stable quantum yield of the semiconducting, luminescent nanoparticles in the composition or formulation. 4. New compositions or formulations comprising one or more semiconducting, luminescent nanoparticles that exhibit higher optical density ("OD") at the excitation wavelength are desired. 5. New compositions or formulations comprising one or more semiconducting, luminescent nanoparticles that exhibit better dispersibility of the semiconducting, luminescent nanoparticles at higher concentrations are required. [Means for solving the problem]

[0008] The present inventors aimed to solve one or more of the problems 1 to 5 above. A first material is then formed having the following chemical formula (I): XYZ - (I) wherein X represents an attaching group containing one or two S atoms, preferably the attaching group is [ka] [ka] where "#" represents the point of attachment to the group Y, and "*" represents the point of attachment to the surface of the core or the outermost surface of the shell layer of the semiconducting, luminescent nanoparticle;

[0009] Y is a single bond, an alkylene group having 1 to 15 carbon atoms, or an alkenylene group having 1 to 15 carbon atoms, or a (poly)alkoxylene group having 1 to 15 carbon atoms, preferably Y is a (poly)alkoxylene group having 1 to 15 carbon atoms;

[0010] Z is -[CH(R 1 )-CH(R 2 )-Q] x -R 3 and Here, R 1 is H or a methyl group, and R 2 is H or a methyl group, Q is an oxygen atom, a nitrogen atom or a sulfur atom, preferably Q is an oxygen atom, R 3 is H or a methyl group, x is an integer, preferably x ranges from 1 to 300, more preferably from 2 to 200, even more preferably from 4 to 100; or

[0011] Z is -[(CHR 1 ) n -Q)] x -R 3 and where n is 2 or 3, Q is an oxygen atom, a nitrogen atom or a sulfur atom, preferably Q is an oxygen atom, and R 1 is H or a methyl group, and R 3 is H or a methyl group, n is 1 to 5, preferably 1 to 3, more preferably n is 2, and x is an integer, preferably x ranges from 1 to 300, more preferably from 2 to 200, even more preferably from 4 to 100;

[0010] Novel compositions have been discovered comprising, consisting essentially of, or consisting of at least one semiconducting, luminescent nanoparticle comprising at least one core, optionally one or more shell layers, a first material, and a second material, represented by the formula:

[0012] In another aspect, the present invention also provides the composition of the present invention, and At least one solvent, preferably it is an ethylene glycol monoalkyl ether, such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, and ethylene glycol monobutyl ether; a diethylene glycol dialkyl ether, such as diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dipropyl ether, and diethylene glycol dibutyl ether; a propylene glycol monoalkyl ether, such as propylene glycol monomethyl ether (PGME), propylene glycol monoethyl ether, and propylene glycol monopropyl ether; a methyl cellosolve acetate and an ethyl cellosolve acetate. ethylene glycol alkyl ether acetates such as sorb acetate; propylene glycol alkyl ether acetates such as propylene glycol monomethyl ether acetate (PGMEA), propylene glycol monoethyl ether acetate, and propylene glycol monopropyl ether acetate; ketones such as methyl ethyl ketone, acetone, methyl amyl ketone, methyl isobutyl ketone, and cyclohexanone; alcohols such as ethanol, propanol, butanol, hexanol, cyclohexanol, ethylene glycol, and glycerin; esters such as ethyl 3-ethoxypropionate, methyl 3-methoxypropionate, and ethyl lactate; and cyclic esters such as gamma butyrolactone;The present invention relates to a novel formulation comprising at least one of the following: a solvent selected from one or more members of the group consisting of chlorinated hydrocarbons such as chloroform, dichloromethane, chlorobenzene, and dichlorobenzene; preferably the solvent is selected from one or more members of the group consisting of propylene glycol alkyl ether acetates, alkyl acetates, ethylene glycol monoalkyl ethers, propylene glycol, and propylene glycol monoalkyl ethers; preferably the solvent is selected from one or more members of the group consisting of propylene glycol alkyl ether acetates such as propylene glycol monomethyl ether acetate (PGMEA), alkyl acetates such as butyl acetate, ethylene glycol monoalkyl ethers such as ethylene glycol monobutyl ether, propylene glycol, or propylene glycol monoalkyl ethers such as methoxypropanol; more preferably the solvent is selected from propylene glycol alkyl ether acetates;

[0013] In another aspect, the present invention also provides a method for preparing a compound having the following formula (I): XYZ - (I) wherein X represents an attaching group containing one or two S atoms, preferably the attaching group is

[0014] [ka] [ka]

[0015] where "#" represents the point of attachment to the group Y, and "*" represents the point of attachment to the surface of the core or the outermost surface of the shell layer of the semiconducting, luminescent nanoparticle; Y is a single bond, an alkylene group having 1 to 15 carbon atoms, or an alkenylene group having 1 to 15 carbon atoms, or a (poly)alkoxylene group having 1 to 15 carbon atoms, preferably Y is a (poly)alkoxylene group having 1 to 15 carbon atoms;

[0016] Z is -[CH(R 1 )-CH(R 2 )-Q] x -R 3 and Here, R 1 is H or a methyl group, and R 2 is H or a methyl group, Q is an oxygen atom, a nitrogen atom or a sulfur atom, preferably Q is an oxygen atom, R 3 is H or a methyl group, x is an integer, preferably x ranges from 1 to 300, more preferably from 2 to 200, even more preferably from 4 to 100; or

[0017] Z is -[(CHR 1 ) n -Q)] x -R 3 and where n is 2 or 3, Q is an oxygen atom, a nitrogen atom or a sulfur atom, preferably Q is an oxygen atom, and R 1 is H or a methyl group, and R 3 is H or a methyl group, n is 1 to 5, preferably 1 to 3, more preferably n is 2, and x is an integer, preferably x ranges from 1 to 300, more preferably from 2 to 200, even more preferably from 4 to 100; the core, optionally one or more shell layers, at least one first material, preferably the first material as a ligand, is placed on the surface of the core or on the outermost surface of the shell layer; and

[0018] at least one solvent, preferably it is an ethylene glycol monoalkyl ether, such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, and ethylene glycol monobutyl ether; a diethylene glycol dialkyl ether, such as diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dipropyl ether, and diethylene glycol dibutyl ether; a propylene glycol monoalkyl ether, such as propylene glycol monomethyl ether (PGME), propylene glycol monoethyl ether, and propylene glycol monopropyl ether;

[0019] ethylene glycol alkyl ether acetates, such as methyl cellosolve acetate and ethyl cellosolve acetate; propylene glycol alkyl ether acetates, such as propylene glycol monomethyl ether acetate (PGMEA), propylene glycol monoethyl ether acetate, and propylene glycol monopropyl ether acetate; ketones, such as methyl ethyl ketone, acetone, methyl amyl ketone, methyl isobutyl ketone, and cyclohexanone; alcohols, such as ethanol, propanol, butanol, hexanol, cyclohexanol, ethylene glycol, and glycerin; esters, such as ethyl 3-ethoxypropionate, methyl 3-methoxypropionate, and ethyl lactate; and cyclic esters, such as gamma butyrolactone; chlorinated hydrocarbons, such as chloroform, dichloromethane, chlorobenzene, and dichlorobenzene,

[0020] Preferably, the solvent is propylene glycol alkyl ether acetate, alkyl acetate, ethylene glycol monoalkyl ether, propylene glycol, and propylene glycol monoalkyl ether, preferably the solvent is selected from one or more members of the group consisting of propylene glycol alkyl ether acetate such as propylene glycol monomethyl ether acetate (PGMEA), alkyl acetate such as butyl acetate, ethylene glycol monobutyl ether, ethylene glycol monoalkyl ether, propylene glycol, or propylene glycol monoalkyl ether such as methoxypropanol, more preferably the solvent is selected from propylene glycol alkyl ether acetate.

[0021] In another aspect, the invention relates to the use of the composition or formulation in an electronic device, an optical device, in a biomedical device or for making an electronic, optical or biomedical device.

[0022] In another aspect, the invention further relates to an optical medium comprising said composition or formulation.

[0023] In another aspect, the present invention also provides a method for preparing a compound having the following formula (I): XYZ - (I) wherein X represents an attaching group containing one or two S atoms, preferably the attaching group is [ka] [ka]

[0024] where "#" represents the point of attachment to the group Y, and "*" represents the point of attachment to the surface of the core or the outermost surface of the shell layer of the semiconducting, luminescent nanoparticle;

[0025] Y is a single bond, an alkylene group having 1 to 15 carbon atoms, or an alkenylene group having 1 to 15 carbon atoms, or a (poly)alkoxylene group having 1 to 15 carbon atoms, preferably Y is a (poly)alkoxylene group having 1 to 15 carbon atoms;

[0026] Z is -[CH(R 1 )-CH(R 2 )-Q] x -R 3 and Here, R 1 is H or a methyl group, and R 2 is H or a methyl group, Q is an oxygen atom, a nitrogen atom or a sulfur atom, preferably Q is an oxygen atom, R 3 is H or a methyl group, x is an integer, preferably x ranges from 1 to 300, more preferably from 2 to 200, even more preferably from 4 to 100; or

[0027] Z is -[(CHR1) n -Q)] x -R 3 and where n is 2 or 3, Q is an oxygen atom, a nitrogen atom or a sulfur atom, preferably Q is an oxygen atom, and R 1 is H or a methyl group, and R 3 is H or a methyl group, n is 1 to 5, preferably 1 to 3, more preferably n is 2, and x is an integer, preferably x ranges from 1 to 300, more preferably from 2 to 200, even more preferably from 4 to 100; and at least one organic layer comprising a core, optionally one or more shell layers, and at least one luminescent nanoparticle comprising a first material, preferably said one organic layer is a light emitting layer, more preferably the medium further comprises one or more layers selected from the group consisting of a hole injection layer, a hole transport layer, an electron blocking layer, a hole blocking layer, an electron blocking layer and an electron injection layer.

[0028] In another aspect, the present invention also relates to an optical device comprising at least one optical medium according to the present invention.

[0029] Detailed Description of the Invention In accordance with the present invention, in one embodiment, the composition comprises a first material having the following chemical formula (I): XYZ - (I) wherein X represents an attaching group containing one or two S atoms, preferably the attaching group is [ka] [ka] where "#" represents the point of attachment to the group Y and "*" represents the point of attachment to the surface of the core or the outermost surface of the shell layer of the semiconducting, luminescent nanoparticle;

[0030] Y is a single bond, an alkylene group having 1 to 15 carbon atoms, or an alkenylene group having 1 to 15 carbon atoms, or a (poly)alkoxylene group having 1 to 15 carbon atoms, preferably Y is a (poly)alkoxylene group having 1 to 15 carbon atoms;

[0031] Z is -[CH(R 1 )-CH(R 2 )-Q]x -R 3 and Here, R 1 is H or a methyl group, and R 2 is H or a methyl group, Q is an oxygen atom, a nitrogen atom or a sulfur atom, preferably Q is an oxygen atom, R 3 is H or a methyl group, x is an integer, preferably x ranges from 1 to 300, more preferably from 2 to 200, even more preferably from 4 to 100; or

[0032] Z is -[(CHR 1 ) n -Q)] x -R 3 and where n is 2 or 3, Q is an oxygen atom, a nitrogen atom or a sulfur atom, preferably Q is an oxygen atom, and R 1 is H or a methyl group, and R 3 is H or a methyl group, n is 1 to 5, preferably 1 to 3, more preferably n is 2, and x is an integer, preferably x ranges from 1 to 300, more preferably from 2 to 200, even more preferably from 4 to 100; The at least one semiconducting luminescent nanoparticle may comprise, consist essentially of, or consist of, at least one semiconducting luminescent nanoparticle comprising at least a core, optionally one or more shell layers, a first material, and a second material, as represented by the formula:

[0033] Preferably, the first material represented by formula (I) is located on the surface of the core or on the outermost surface of the shell layer as a ligand of the semiconducting luminescent nanoparticles. Preferably, the composition comprises a plurality of semiconducting luminescent nanoparticles.

[0034] -Second Ingredient In some embodiments of the invention, the second material is selected from one or more members of the group consisting of organic light-emitting materials, inorganic light-emitting materials, charge transporting materials such as electron transporting organic materials, scattering particles, host materials, semiconducting inorganic materials, and matrix materials, preferably the matrix material is selected from one or more members of the group consisting of poly-(meth)acrylates, (meth)acrylate monomers, silicon polymers, epoxy polymers, preferably the matrix first material is an acrylate monomer, a methacrylate monomer, a poly-acrylate, a poly-methacrylate, or a mixture thereof, more preferably the matrix material is a poly-acrylate, a poly-methacrylate, or a mixture thereof.

[0035] In a preferred embodiment of the invention, the second material is a matrix material selected from one or more members of the group consisting of poly-(meth)acrylates, (meth)acrylate monomers, silicon polymers, epoxy polymers, preferably the matrix material is an acrylate monomer, a methacrylate monomer, a poly-acrylate, a poly-methacrylate, or a mixture thereof, more preferably the matrix material is a poly-acrylate, a poly-methacrylate, or a mixture thereof.

[0036] Thus, in some embodiments of the invention, the composition comprises a ligand having the following formula (I): XYZ - (I) wherein X represents an attaching group comprising one or two S atoms, preferably the attaching group comprises one or two thiol groups, more preferably it is [ka] or preferably the attachment group is [ka] where "#" represents the point of attachment to the group Y, and "*" represents the point of attachment to the surface of the core or the outermost surface of the shell layer of the semiconducting, luminescent nanoparticle;

[0037] Y is a single bond, an alkylene group having 1 to 15 carbon atoms, or an alkenylene group having 1 to 15 carbon atoms, or a (poly)alkoxylene group having 1 to 15 carbon atoms, preferably Y is a (poly)alkoxylene group having 1 to 15 carbon atoms;

[0038] Z is -[CH(R 1 )-CH(R 2 )-Q] x -R 3 and Here, R 1 is H or a methyl group, and R 2 is H or a methyl group, Q is an oxygen atom, a nitrogen atom or a sulfur atom, preferably Q is an oxygen atom, R 3 is H or a methyl group, x is an integer, preferably x ranges from 1 to 300, more preferably from 2 to 200, even more preferably from 4 to 100; or

[0039] Z is -[(CHR 1 ) n -Q)] x -R 3 and In the formula, n is 2 or 3, Q is an oxygen atom, a nitrogen atom or a sulfur atom, preferably Q is an oxygen atom, and R 1 is H or a methyl group, and R 3 is H or a methyl group, n is 1 to 5, preferably 1 to 3, more preferably n is 2, and x is an integer, preferably x ranges from 1 to 300, more preferably from 2 to 200, even more preferably from 4 to 100; a semiconducting luminescent nanoparticle comprising at least a core, optionally one or more shell layers, and at least one ligand as a first material located on a surface of the core or on an outermost surface of the shell layer, and

[0040] At least one matrix material selected from one or more members of the group consisting of poly-(meth)acrylates, (meth)acrylate monomers, silicon polymers, epoxy polymers, preferably the matrix material is an acrylate monomer, a methacrylate monomer, a poly-acrylate, a poly-methacrylate, or a mixture thereof, more preferably the matrix material is a poly-acrylate, a poly-methacrylate, or a mixture thereof.

[0041] -Matrix material In accordance with the present invention, in some embodiments, the composition comprises at least one matrix material selected from one or more members of the group consisting of poly-(meth)acrylates, (meth)acrylate monomers, silicon polymers, epoxy polymers, preferably the matrix material is an acrylate monomer, a methacrylate monomer, a poly-acrylate, a poly-methacrylate, or a mixture thereof, more preferably the matrix material is a poly-acrylate, a poly-methacrylate, or a mixture thereof.

[0042] In some embodiments of the present invention, the matrix material comprises poly-(meth)acrylates and / or (meth)acrylate monomers. In accordance with the present invention, the term "poly-(meth)acrylate" refers to a general term for a polymer obtained by polymerization of monomers selected from the group consisting of acrylic acid, methacrylic acid, acrylates, methacrylates, and any combination thereof.

[0043] Preferably, the poly-(meth)acrylate is a poly-acrylate or a poly-methacrylate, and preferably, the (meth)acrylate monomer is an acrylate monomer or a methacrylate monomer. The poly-(meth)acrylate of the present invention may further contain other monomer units not mentioned above, so long as the poly-(meth)acrylate exhibits the effects of the present invention.

[0044] In accordance with the present invention, the weight average molecular weight of the poly-(meth)acrylate is not specifically limited. Preferably it is in the range of 2,000-100,000, more preferably it is in the range of 3,000-30,000. As poly-(meth)acrylate one or more known poly-acrylates or poly-methacrylates may be used.

[0045] In a preferred embodiment of the present invention, silane-modified poly-(meth)acrylates, which include repeat units containing acidic groups to achieve good polymerization reaction with polysiloxanes, may be used alone or in mixtures. As examples of silane-modified poly-(meth)acrylates, siloxy- and / or silanol-substituted poly-acrylates or poly-methacrylates, polyacrylates or poly-methacrylates reacted with silane coupling agents containing carbon-carbon unsaturated bonds, silicone oligomers, or silicone oils may preferably be used.

[0046] Without wishing to be bound by theory, it is believed that silane-modified poly-(meth)acrylates can lead to improved solubility of polysiloxanes. More preferably, a copolymer made from a silane coupling agent and a poly-(meth)acrylate may be used.

[0047] In the present specification, as an example of a silane coupling agent, KBM-1003, KME-1003, KBM-1403 or KBM-5103 (from Shinetsu Co.) may be preferably used, and as an example of a silicone oil, X-22-174DX, X-22-2426, X-22-2475 or X-22-1602 (from Shinetsu Co.) may be preferably used.

[0048] According to the present invention, the number of unsaturated bonds is not specifically limited. From the viewpoint of a balance between better reactivity and compatibility with siloxane, the double bond equivalent (ethylenically unsaturated bond equivalent) value in the (meth)acrylic polymer is preferably in the range of 10 to 500 g / eq.

[0049] As the (meth)acrylic polymer including a repeat unit containing an acidic group, the (meth)acrylic polymer includes a side chain selected from the group consisting of a carboxyl group, a sulfo group, or a phenol-type hydroxyl group. It is believed that (meth)acrylic polymers that include repeat units that contain acidic groups may lead to better solubility of the uncured portions of the photosensitive composition in the developer.

[0050] According to the present invention, the number of acidic groups is not specifically limited. From the viewpoint of a balance between better reactivity and storage stability of the photosensitive composition, the acid value of the (meth)acrylic polymer is preferably in the range of 50 to 500 mg of KOH based on 1 g of the (meth)acrylic polymer.

[0051] -First Ingredient According to the present invention, the first material, preferably the ligand of the semiconducting luminescent nanoparticles, is represented by the following formula (I): XYZ - (I) wherein X represents an attaching group containing one or two S atoms, preferably the attaching group is [ka] [ka] where "#" represents the point of attachment to the group Y, and "*" represents the point of attachment to the surface of the core or the outermost surface of the shell layer of the semiconducting, luminescent nanoparticle;

[0052] Y is a single bond, an alkylene group having 1 to 15 carbon atoms, or an alkenylene group having 1 to 15 carbon atoms, or a (poly)alkoxylene group having 1 to 15 carbon atoms, preferably Y is a (poly)alkoxylene group having 1 to 15 carbon atoms;

[0053] Z is -[CH(R 1 )-CH(R 2 )-Q] x -R 3 and Here, R 1 is H or a methyl group, and R 2 is H or a methyl group, Q is an oxygen atom, a nitrogen atom or a sulfur atom, preferably Q is an oxygen atom, R 3 is H or a methyl group, x is an integer, preferably x ranges from 1 to 300, more preferably from 2 to 200, even more preferably from 4 to 100; or

[0054] Z is -[(CHR 1 ) n -Q)] x -R 3 and where n is 2 or 3, Q is an oxygen atom, a nitrogen atom or a sulfur atom, preferably Q is an oxygen atom, and R 1 is H or a methyl group, and R 3 is H or a methyl group, n is 1 to 5, preferably 1 to 3, more preferably n is 2, and x is an integer, preferably x ranges from 1 to 300, more preferably from 2 to 200, even more preferably from 4 to 100; It is expressed as:

[0055] In some embodiments of the present invention, the first material is preferably placed as a ligand on the surface of the core or on the outermost surface of the shell layer of the semiconducting luminescent nanoparticle. In some embodiments of the present invention, the surface of the core, or the outermost surface of one or more shell layers of the outermost surface of the semiconducting luminescent nanoparticles may be partially or completely coated with a material as a ligand.

[0056] In some embodiments of the present invention, at least two materials represented by formula (I) as ligands are attached to the surface of the core or the outermost surface of the shell layer, and preferably, a plurality of said ligands are attached to the surface of the core or the outermost surface of the shell layer. According to the invention, in some embodiments, the content of the first material, preferably as a ligand, is in the range of 1% to 80% by weight, more preferably in the range of 20% to 70% by weight, and even more preferably in the range of 40% to 65% by weight, with respect to the total weight of the semiconducting luminescent nanoparticles.

[0057] In a preferred embodiment of the invention, the weight average molecular weight (Mw) of the first material, preferably as a ligand, is in the range of from 200 g / mol to 30,000 g / mol, preferably in the range of from 250 g / mol to 2,000 g / mol, more preferably in the range of from 400 g / mol to 1,000 g / mol.

[0058] The molecular weights Mw are determined by means of GPC (=gel permeation chromatography) relative to a polystyrene internal standard. In a preferred embodiment, preferably as a ligand, the material has the following formula (Ia) or (Ib): [ka] It is expressed as:

[0059] More preferably, Z is -[(CHR 1 ) n -Q)]x -R 3 where n is 2 or 3, Q is an oxygen atom, a nitrogen atom or a thiol atom, preferably Q is an oxygen atom, and R 1 is H or a methyl group, and R 3 is H or a methyl group, n is 1 to 5, preferably 1 to 3, more preferably n is 2, and x is an integer, preferably x ranges from 1 to 700, more preferably from 2 to 350, even more preferably from 4 to 200.

[0060] Preferably, Y is selected from the group in Table 1 below. [Table 1] where "*" represents the point of attachment to groups X and Z.

[0061] Publicly available polyethylene glycol (PEG) thiols, polypropylene glycol thiols, and derivatives thereof (eg, from Sigma-Aldrich) may be preferably used as the ligands described above. -Semiconductive luminescent nanoparticles According to the present invention, the term "semiconductor" means a material that has, at room temperature, an electrical conductivity between that of a conductor (such as copper) and that of an insulator (such as glass). Preferably, a semiconductor is a material whose electrical conductivity increases with temperature. The term "nano-sized" means a size between 0.1 nm and 999 nm, preferably between 1 nm and 150 nm, more preferably between 3 nm and 50 nm.

[0062] Thus, in accordance with the present invention, "semiconductive luminescent nanoparticles" is taken to mean luminescent materials, preferably semiconductors, having electrical conductivity at room temperature between that of a conductor (such as copper) and that of an insulator (such as glass) with a size between 0.1 and 999 nm, preferably 1 nm to 150 nm, more preferably 3 nm to 50 nm, the electrical conductivity of which increases with temperature, and the size of which is between 0.1 and 999 nm, preferably 0.5 nm to 150 nm, more preferably 1 nm to 50 nm.

[0063] According to the present invention, the term "size" refers to the average diameter of the longest axis of the semiconducting nano-sized luminescent particles. The average diameter of the semiconducting nano-sized luminescent particles is calculated based on 100 semiconducting luminescent nanoparticles in the TEM images produced by a Tecnai G2 Spirit Twin T-12 Transmission Electron Microscope.

[0064] In a preferred embodiment of the present invention, the semiconducting luminescent nanoparticles of the present invention are quantum-sized materials. In accordance with the present invention, the term "quantum size" refers to the size of the semiconducting material itself, without any ligands or other surface modifications, and may represent quantum confinement effects, for example as described in ISBN: 978-3-662-44822-9.

[0065] For example, CdS, CdSe, CdTe, ZnS, ZnSe, ZnSeS, ZnTe, ZnO, GaAs, GaP, GaSb, HgS, HgSe, HgSe, HgTe, InAs, InP, InPS, InPZnS, InPZn, InPZnSe, InCdP, InPCdS, InPCdSe, InGaP, InGaPZn, InSb, AlAs, AlP, AlSb, Cu2S, Cu2Se, CuInS2, CuInSe2, Cu2(ZnSn)S4, Cu2(InGa)S4, TiO2 alloys and any combination thereof may be used.

[0066] In a preferred embodiment of the invention, the core comprises one element from group 13 of the periodic table and one element from group 15 of the periodic table, preferably the group 13 element is In and the group 15 element is P, more preferably the core is selected from the group consisting of InP, InPZn, InPZnS, and InGaP.

[0067] In accordance with the present invention, the shape of the core of the semiconducting luminescent nanoparticles and the type of shape of the synthesized semiconducting luminescent nanoparticles are not specifically limited. For example, spherical, elongated, star-shaped, polyhedral, pyramidal, tetrapod-shaped, tetrahedral, platelet-shaped, conical, and irregularly shaped core and / or semiconducting luminescent nanoparticles may be synthesized.

[0068] In some embodiments of the invention, the average diameter of the core ranges from 1.5 nm to 3.5 nm. The average core diameter is calculated based on 100 semiconducting luminescent nanoparticles in TEM images produced by a Tecnai G2 Spirit Twin T-12 Transmission Electron Microscope.

[0069] In some embodiments of the invention, the shell layer comprises or consists of a first element from Group 12 of the periodic table and a second element from Group 16 of the periodic table, preferably where the first element is Zn or Cd and the second element is S, Se, or Te.

[0070] In a preferred embodiment of the present invention, the shell layer is represented by the following formula (II): ZnS x Se y Te z、 -(II) In formula (II), 0≦x≦1, 0≦y≦1, 0≦z≦1, and x+y+z=1. Preferably, the shell layer is ZnSe, ZnS x Se y , ZnSe y Te z or ZnS x Te zIt is expressed as: In some embodiments of the present invention, the shell layer is an alloyed shell layer or a graded shell layer, and preferably the graded shell layer is ZnS x Se y , ZnSe y Te z , or ZnS x Te z and more preferably it is ZnS x Se y It is.

[0071] In some embodiments of the present invention, the semiconducting luminescent nanoparticles further comprise a second shell layer, preferably the second shell layer comprises or consists of a third element from group 12 of the periodic table and a fourth element from group 16 of the periodic table, more preferably the third element is Zn and the fourth element is S, Se, or Te, provided that the fourth element and the second element are not the same.

[0072] In a preferred embodiment of the present invention, the second shell layer is represented by the following formula (II'): ZnS x Se y Te z、 (II') In formula (II'), 0≦x≦1, 0≦y≦1, 0≦z≦1, and x+y+z=1. Preferably, the shell layer is ZnSe, ZnS x Se y , ZnSe y Te z , or ZnS x Te z where the shell layer and the second shell layer are not the same.

[0073] In some embodiments of the present invention, the second shell layer may be an alloyed shell layer. In some embodiments of the present invention, the semiconducting luminescent nanoparticles may further comprise one or more additional shell layers above the second shell layer as a multishell. In accordance with the present invention, the term "multishell" refers to a stacked shell layer consisting of three or more shell layers.

[0074] For example, CdSe / CdS, CdSeS / CdZnS, CdSeS / CdS / ZnS, ZnSe / CdS, CdSe / ZnS, InP / ZnS, InP / ZnSe, InP / ZnSe / ZnS, InZnP / ZnS, InZnP / ZnSe, InZnP / ZnSe / ZnS, InGaP / ZnS, InGaP / ZnSe, InGaP / ZnSe / ZnS, InZnPS / ZnS, InZnPSZnSe, InZnPS / ZnSe / ZnS, ZnSe / CdS, ZnSe / ZnS or any combination thereof may be used. Preferably, InP / ZnS, InP / ZnSe, InP / ZnSe / ZnS, InZnP / ZnS, InZnP / ZnSe, InZnP / ZnSe / ZnS, InGaP / ZnS, InGaP / ZnSe, InGaP / ZnSe / ZnS.

[0075] In some embodiments of the present invention, the composition comprises two or more semiconducting luminescent nanoparticles. In some embodiments of the present invention, the composition comprises a plurality of semiconducting luminescent nanoparticles.

[0076] In some embodiments of the present invention, the total amount of semiconducting luminescent nanoparticles ranges from 0.1 wt.% to 90 wt.%, preferably from 5 wt.% to 70 wt.%, more preferably from 20 wt.% to 50 wt.%, based on the total amount of the composition.

[0077] -Additional Ligands In some embodiments of the present invention, the semiconducting luminescent nanoparticles may optionally include different types of ligands in addition to the material represented by Formula (I).

[0078] Thus, in some embodiments of the present invention, the outermost surface of the core or shell layer of the semiconducting luminescent nanoparticles may be coated with one or more additional ligands, if desired, along with the ligand represented by formula (I).

[0079] When one or more of the additional ligands are attached to the outermost surface of the core or shell layer(s) of the semiconducting luminescent nanoparticles, the amount of the ligands represented by formula (I) is in the range of 30 wt.% to 99.9 wt.%, preferably in the range of 50 wt.% to 95 wt.%, and more preferably in the range of 60 wt.% to 90 wt.%, of the total ligands attached to the outermost surface of the shell layer(s).

[0080] In some embodiments of the present invention, the composition may further comprise one or more additives. Preferably, the additive is selected from the group consisting of the further ligands.

[0081] Without wishing to be bound by theory, it is believed that such surface ligands lead to the nanosized fluorescent material being more easily dispersed in a solvent.

[0082] Commonly used surface ligands include phosphines and phosphine oxides such as trioctylphosphine oxide (TOPO), trioctylphosphine (TOP), and tributylphosphine (TBP); phosphonic acids such as dodecylphosphonic acid (DDPA), tridecylphosphonic acid (TDPA), octadecylphosphonic acid (ODPA), and hexylphosphonic acid (HPA); amines such as oleylamine, dedecylamine (DDA), tetradecylamine (TDA), hexadecylamine (HDA), and octadecylamine (ODA), oleylamine (OLA), thiols such as 1-octadecene (ODE), hexadecanethiol, and hexanethiol; mercaptocarboxylic acids such as mercaptopropionic acid and mercaptoundecanoic acid; oleic acid, stearic acid, myristic acid; carboxylic acids such as acetic acid, and also any combination thereof. Polyethyleneimine (PEI) may also be preferably used.

[0083] Examples of surface ligands are described, for example, in International Patent Application Publication No. WO 2012 / 059931A.

[0084] -Additional materials In some embodiments of the present invention, the composition may further comprise at least one additional material, preferably the additional material is selected from the group consisting of an organic light-emitting material, an inorganic light-emitting material, a charge transport material, a scattering particle, a light-transmitting polymer, an antioxidant, a radical quencher, a polymerization initiator, and an additional ligand.

[0085] For example, the activator is Sc 3+ ,Y 3+ , La 3+ , Ce 3+ ,Pr 3+ , Nd 3+ , Pm 3+ , Sm 3+ ,EU 3+ , Gd 3+ , Tb 3+ , Dy 3+ , Ho 3+ , Er 3+ , Tm 3+ , Yb 3+ , Lu 3+ , Bi 3+ , Pb 2+ , Mn 2+ , Yb 2+ , Sm 2+ ,EU 2+ , Dy 2+ , Ho 2+ and any combination thereof, and the inorganic fluorescent material may be selected from the group consisting of sulfides, thiogallates, nitrides, oxynitrides, silicates, aluminates, apatites, borates, oxides, phosphates, halophosphates, sulfates, tungstenates, tantalates, vanadates, molybdates, niobates, titanates, germanates, halide based phosphors, and any combination thereof.

[0086] Such suitable inorganic fluorescent materials as described above may be well-known fluorescent materials, including nano-sized phosphors, quantum-sized materials as described in, for example, Handbook of Phosphors, 2nd Edition (CRC Press, 2006), pp. 155-pp. 338 (W.M. En, S. Shionoya and H. Yamamoto), WO2011 / 147517A, WO2012 / 034625A, and WO2010 / 095140A.

[0087] According to the present invention, any known type of material may be preferably used as the organic light-emitting material, charge transport material, such as well-known organic fluorescent materials, organic host materials, organic dyes, organic electron transport materials, organometallic complexes, and organic hole transport materials.

[0088] As examples of scattering particles, small particles of inorganic oxides such as SiO2, SnO2, CuO, CoO, Al2O3TiO2, Fe2O3, Y2O3, ZnO, MgO, etc.; organic particles such as polymerized polystyrene, polymerized PMMA; inorganic hollow oxides such as hollow silica, or any combination of these may preferably be used. -Transparent polymer A wide variety of known transparent polymers suitable for optical devices may preferably be used in accordance with the present invention. In accordance with the present invention, the term "transparent" means that at least approximately 60% of incident light is transmitted at the thickness used in the optical medium and at the wavelength or range of wavelengths used during operation of the optical medium. Preferably, it is greater than 70%, more preferably greater than 75%, and most preferably it is greater than 80%.

[0089] In a preferred embodiment of the present invention, any type of known transparent polymer may be used, for example as described in WO 2016 / 134820A. According to the present invention, the term "polymer" means a material having repeating units and having a weight average molecular weight (Mw) of 1000 g / mol or more.

[0090] The molecular weights Mw are determined by means of GPC (=gel permeation chromatography) relative to a polystyrene internal standard. In some embodiments of the present invention, the glass transition temperature (Tg) of the transparent polymer is 70°C or more and 250°C or less.

[0091] Tg is measured based on the change in heat capacity observed in differential scanning calorimetry, such as that described in http: / / pslc.ws / macrog / dsc.htm; Rickey J Seyler, Assignment of the Glass Transition, ASTM Publication Code Number (PCN) 04-012490-50. For example, poly(meth)acrylates, epoxies, polyurethanes, polysiloxanes may be preferably used as transparent polymers for the transparent matrix material.

[0092] In a preferred embodiment of the present invention, the weight average molecular weight (Mw) of the polymer as the transparent matrix material is in the range of from 1,000 to 300,000 g / mol, more preferably it is from 10,000 to 250,000 g / mol.

[0093] -Formulation In another aspect, the present invention provides a composition comprising at least and at least one solvent, ethylene glycol monoalkyl ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, and ethylene glycol monobutyl ether; diethylene glycol dialkyl ethers such as diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dipropyl ether, and diethylene glycol dibutyl ether; propylene glycol monoalkyl ethers such as propylene glycol monomethyl ether (PGME), propylene glycol monoethyl ether, and propylene glycol monopropyl ether; methyl cellosolve acetate and ethyl cellosolve acetate; propylene glycol alkyl ether acetates such as propylene glycol monomethyl ether acetate (PGMEA), propylene glycol monoethyl ether acetate, and propylene glycol monopropyl ether acetate; ketones such as methyl ethyl ketone, acetone, methyl amyl ketone, methyl isobutyl ketone, and cyclohexanone; alcohols such as ethanol, propanol, butanol, hexanol, cyclohexanol, ethylene glycol, and glycerin; esters such as ethyl 3-ethoxypropionate, methyl 3-methoxypropionate, and ethyl lactate; and cyclic esters such as gamma-butyrolactone;at least one solvent selected from one or more members of the group consisting of chlorinated hydrocarbons such as chloroform, dichloromethane, chlorobenzene, and dichlorobenzene, preferably the solvent is propylene glycol alkyl ether acetate, alkyl acetate, ethylene glycol monoalkyl ether, propylene glycol, and propylene glycol monoalkyl ether, preferably the solvent is selected from one or more members of the group consisting of propylene glycol alkyl ether acetate such as propylene glycol monomethyl ether acetate (PGMEA), alkyl acetate such as butyl acetate, ethylene glycol monoalkyl ether such as ethylene glycol monobutyl ether, propylene glycol, or propylene glycol monoalkyl ether such as methoxypropanol, more preferably the solvent is selected from propylene glycol alkyl ether acetate;

[0094] In another aspect, the present invention also provides a method for preparing a compound having the following formula (I): XYZ - (I) wherein X represents an attaching group containing one or two S atoms, preferably the attaching group is [ka] [ka] [ka] where "#" represents the point of attachment to the group Y, and "*" represents the point of attachment to the surface of the core or the outermost surface of the shell layer of the semiconducting, luminescent nanoparticle;

[0095] Y is a single bond, an alkylene group having 1 to 15 carbon atoms, or an alkenylene group having 1 to 15 carbon atoms, or a (poly)alkoxylene group having 1 to 15 carbon atoms, preferably Y is a (poly)alkoxylene group having 1 to 15 carbon atoms;

[0096] Z is -[CH(R 1 )-CH(R 2 )-Q] x -R 3 and Here, R 1 is H or a methyl group, and R 2 is H or a methyl group, Q is an oxygen atom, a nitrogen atom or a sulfur atom, preferably Q is an oxygen atom, R 3 is H or a methyl group, x is an integer, preferably x ranges from 1 to 300, more preferably from 2 to 200, even more preferably from 4 to 100; or

[0097] Z is -[(CHR 1 ) n -Q)] x -R 3 and where n is 2 or 3, Q is an oxygen atom, a nitrogen atom or a sulfur atom, preferably Q is an oxygen atom, and R 1 is H or a methyl group, and R 3 is H or a methyl group, n is 1 to 5, preferably 1 to 3, more preferably n is 2, and x is an integer, preferably x ranges from 1 to 300, more preferably from 2 to 200, even more preferably from 4 to 100; At least one semiconducting luminescent nanoparticle comprising a core, optionally one or more shell layers, at least one first material, preferably the first material being placed as a ligand on the surface of the core or on the outermost surface of the shell layer,

[0098] and At least one solvent, preferably it is an ethylene glycol monoalkyl ether, such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, and ethylene glycol monobutyl ether; a diethylene glycol dialkyl ether, such as diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dipropyl ether, and diethylene glycol dibutyl ether; a propylene glycol monoalkyl ether, such as propylene glycol monomethyl ether (PGME), propylene glycol monoethyl ether, and propylene glycol monopropyl ether; a methyl cellosolve acetate and an ethyl cellosolve acetate. ethylene glycol alkyl ether acetates such as sorb acetate; propylene glycol alkyl ether acetates such as propylene glycol monomethyl ether acetate (PGMEA), propylene glycol monoethyl ether acetate, and propylene glycol monopropyl ether acetate; ketones such as methyl ethyl ketone, acetone, methyl amyl ketone, methyl isobutyl ketone, and cyclohexanone; alcohols such as ethanol, propanol, butanol, hexanol, cyclohexanol, ethylene glycol, and glycerin; esters such as ethyl 3-ethoxypropionate, methyl 3-methoxypropionate, and ethyl lactate; and cyclic esters such as gamma butyrolactone;The present invention also relates to a formulation comprising, consisting essentially of, or consisting of one or more members of the group consisting of chlorinated hydrocarbons such as chloroform, dichloromethane, chlorobenzene, and dichlorobenzene, preferably the solvent is propylene glycol alkyl ether acetate, alkyl acetate, ethylene glycol monoalkyl ether, propylene glycol, and propylene glycol monoalkyl ether, preferably the solvent is selected from one or more members of the group consisting of propylene glycol alkyl ether acetate such as propylene glycol monomethyl ether acetate (PGMEA), alkyl acetate such as butyl acetate, ethylene glycol monoalkyl ether such as ethylene glycol monobutyl ether, propylene glycol, or propylene glycol monoalkyl ether such as methoxypropanol, more preferably the solvent is selected from propylene glycol alkyl ether acetate;

[0099] Details of the semiconducting luminescent nanoparticles and the first material, preferably as a ligand, are described in the sections "Semiconducting luminescent nanoparticles" and "First material."

[0100] In some embodiments, the formulation may further comprise additional ingredients, details of which are described in the "Additional Ingredients" section.

[0101] -use In another aspect, the invention relates to the use of the composition or formulation in an electronic device, an optical device, in a biomedical device or for making an electronic, optical or biomedical device.

[0102] -Optical media In another aspect, the present invention further relates to an optical medium comprising at least one composition or formulation, preferably the optical medium comprises at least one composition.

[0103] In some embodiments of the present invention, the optical medium may be an optical sheet, such as a color filter, a color conversion film, a remote fluorescent tape, or another film or filter. In accordance with the present invention, the term "sheet" encompasses films and / or layers, such as structured media.

[0104] In another aspect, the present invention also provides a method for preparing a compound having the following formula (I): XYZ - (I) wherein X represents an attaching group containing one or two S atoms, preferably the attaching group is [ka] [ka]

[0105] where "#" represents the point of attachment to the group Y, and "*" represents the point of attachment to the surface of the core or the outermost surface of the shell layer of the semiconducting, luminescent nanoparticle;

[0106] Y is a single bond, an alkylene group having 1 to 15 carbon atoms, or an alkenylene group having 1 to 15 carbon atoms, or a (poly)alkoxylene group having 1 to 15 carbon atoms, preferably Y is a (poly)alkoxylene group having 1 to 15 carbon atoms;

[0107] Z is -[CH(R 1 )-CH(R 2 )-Q] x -R 3 and Here, R 1 is H or a methyl group, and R 2 is H or a methyl group, Q is an oxygen atom, a nitrogen atom or a sulfur atom, preferably Q is an oxygen atom, R 3is H or a methyl group, x is an integer, preferably x ranges from 1 to 300, more preferably from 2 to 200, even more preferably from 4 to 100; or

[0108] Z is -[(CHR 1 ) n -Q)] x -R 3 and where n is 2 or 3, Q is an oxygen atom, a nitrogen atom or a sulfur atom, preferably Q is an oxygen atom, and R 1 is H or a methyl group, and R 3 is H or a methyl group, n is 1 to 5, preferably 1 to 3, more preferably n is 2, and x is an integer, preferably x ranges from 1 to 300, more preferably from 2 to 200, even more preferably from 4 to 100; and at least one organic layer comprising at least one core, optionally one or more shell layers, and at least one semiconducting, luminescent nanoparticle comprising a first material, preferably said one organic layer is a light emitting layer, more preferably the medium further comprises one or more layers selected from the group consisting of a hole injection layer, a hole transport layer, an electron blocking layer, a hole blocking layer, an electron blocking layer and an electron injection layer.

[0109] In some embodiments of the present invention, the organic layer comprises at least one emissive nanoparticle, a first material, and a host material, preferably the host material is an organic host material. In a preferred embodiment, the organic layer comprises a plurality of light-emitting nanoparticles and a first material.

[0110] -Optical devices In another aspect, the present invention further relates to an optical device comprising at least one optical medium of the present invention. In some embodiments of the present invention, the optical device may be a liquid crystal display device (LCD), an organic light emitting diode (OLED), a backlight unit for an optical display, a light emitting diode device (LED), a microelectromechanical system (hereinafter "MEMS"), an electrowetting display, or an electrophoretic display, a light emitting device, and / or a solar cell. The term "radiation" refers to the emission of electromagnetic waves by electronic transitions in atoms and molecules.

[0111] Technical Effects of the Invention 1. The present invention provides novel compositions or formulations comprising one or more semiconducting, luminescent nanoparticles that exhibit improved dispersibility of the semiconducting, luminescent nanoparticles in the composition or formulation. 2. The present invention provides novel compositions or formulations comprising one or more semiconducting luminescent nanoparticles that exhibit improved initial quantum yields of the semiconducting luminescent nanoparticles in the composition or formulation.

[0112] 3. The present invention provides novel compositions or formulations comprising one or more semiconducting luminescent nanoparticles that exhibit long term stability and stable quantum yield of the semiconducting luminescent nanoparticles in the composition or formulation. 4. The present invention provides novel compositions or formulations comprising one or more semiconducting, luminescent nanoparticles that exhibit higher optical density ("OD") at an excitation wavelength. 5. The present invention provides novel compositions or formulations comprising one or more semiconducting, luminescent nanoparticles that exhibit better dispersibility of the semiconducting, luminescent nanoparticles at higher concentrations.

[0113] The following Examples 1-2 provide a description of the invention as well as a detailed description of its preparation.

[0114] Working Example Example 1: Preparation of compositions containing semiconducting luminescent nanoparticles Red InP-based quantum materials (hereinafter "QM") are prepared as described in US 7,588,828 B in toluene.

[0115] -ligand exchange Place 0.5 g of the red InP-based quantum material in 8.3 mL toluene solution in a flask and evaporate the toluene under reduced pressure. The QM is then dispersed in 17 mL of anhydrous tetrahydrofuran (hereinafter "THF"). And the resulting dispersion is mixed with 1 g of methoxy-PEG thiol (from Sigma Aldrich) dissolved in 17 mL of THF in a reaction vessel. The resulting mixture is then refluxed at 85°C for 19 hours in a N2 atmosphere. After stirring for 19 hours, the THF is evaporated under reduced pressure. Then, 5 mL of PGMEA is added to the resulting mixture, and the resulting solution is refluxed at 150°C for 4.5 hours in a N2 atmosphere.

[0116] Isolation of -QM and methoxy-PEG thiol from solution The QM obtained in the ligand exchange process is precipitated by adding 4.5 mL of octane. After centrifugation, the resulting sediment is dispersed in 5 mL of PGMEA. The resulting QM is then precipitated by adding 6 mL of octane and centrifuging. The resulting sediment is redispersed in 5 mL of PGMEA, then 7 mL of octane is added and it is centrifuged.

[0117] After centrifugation, the resulting sediment is dried under reduced pressure. Finally, 0.61 g of a dark red material is obtained, which is the QM with methoxy-PEG thiol ligand.

[0118] Preparation of compositions containing QMs bearing -methoxy-PEG thiol ligands The obtained QM stabilized with methoxy-PEG thiol ligand is dispersed in PGMEA at a concentration of 30 wt.% based on the total amount of the composition, and stored at 5° C. under N2 atmosphere for QY measurement. Sample 1 is then subjected to QY measurement. The QM stabilized with methoxy-PEG thiol ligand is uniformly dispersed in PGMEA.

[0119] Comparative Example 1: Preparation of compositions containing semiconducting luminescent nanoparticles Red InP-based quantum materials (hereinafter "QM") are prepared in toluene in the same manner as described in US Pat. No. 7,588,828 B.

[0120] -ligand exchange A 1.7 mL toluene solution of 0.1 g of red InP-based quantum material is placed in a flask and the toluene is evaporated under reduced pressure. The QM is then dispersed in 2.5 mL of chloroform and mixed with 0.27 g of Disperbyk-170® (from BYK Japan KK) dissolved in 5 mL of chloroform. The resulting mixture was allowed to stir at 80° C. for 2 h under N2 atmosphere. It is then allowed to cool to room temperature.

[0121] Preparation of compositions containing -QM After cooling to room temperature, 0.4 g of PGMEA is added and the chloroform is evaporated under vacuum. The concentration of the resulting QM stabilized with Disperbyk-170® in PGMEA solution is 30 wt.% based on the total amount of the composition, and it is stored at 5° C. under N2 atmosphere for QY measurement. Samples 2 and 3 are then subjected to QY measurement.

[0122] Example 2 Quantum yield calculation The absolute quantum yields of the samples obtained in Example 1 and Comparative Example 1 are measured by a Hamamatsu instrument via a relative technique.

[0123] The quantum yields of Samples 1 to 3 were evaluated with an absolute PL quantum yield measurement system C9920-02 (Hamamatsu), and the following equation was used: Quantum yield (QY) = number of photons emitted by the sample / number of photons absorbed by the sample Tables 2 and 3 show the results of the QY measurements.

[0124]

Table 2

Claims

1. A method for producing a semiconductor device comprising the steps of: (a) providing a semiconductor device having a semiconductor substrate and a semiconductor material that is a semiconductor material having a semiconductor substrate and a semiconductor material; the core comprises one element from group 13 of the periodic table and one element from group 15 of the periodic table; The first material has the following formula (I): XYZ-(I) wherein X represents an attaching group containing one or two S atoms, preferably the attaching group is 【Chemistry 1】 【Chemistry 2】 where "#" represents the point of attachment to Y, and "*" represents the point of attachment to the surface of the core or the outermost surface of the shell layer of the semiconducting, luminescent nanoparticle; Y is a single bond, an alkylene group having 1 to 15 carbon atoms, or an alkenylene group having 1 to 15 carbon atoms, or a (poly)alkoxylene group having 1 to 15 carbon atoms, preferably Y is a (poly)alkoxylene group having 1 to 15 carbon atoms; Z is -[CH(R 1 )-CH(R 2 ) -Q] x -R 3 and Here, R 1 is H or a methyl group, R 2 is H or a methyl group, Q is an oxygen atom, a nitrogen atom or a sulfur atom, preferably Q is an oxygen atom, R 3 is H or a methyl group; x is an integer, preferably x ranges from 1 to 300, more preferably from 2 to 200, even more preferably from 4 to 100; or Z is -[(CHR 1 ) n -Q)] x -R 3 and where n is 2 or 3, Q is an oxygen atom, a nitrogen atom or a sulfur atom, preferably Q is an oxygen atom, and R 1 is H or a methyl group, R 3 is H or a methyl group; n is 1 to 5, preferably 1 to 3, more preferably n is 2; and x is an integer, preferably x ranges from 1 to 300, more preferably from 2 to 200, even more preferably from 4 to 100. and A composition wherein the second material is selected from one or more members of the group consisting of organic light emitting materials, inorganic light emitting materials, charge transporting materials such as electron transporting organic materials, scattering particles, semiconducting inorganic materials, and matrix materials, and the matrix material is selected from one or more members of the group consisting of poly-(meth)acrylates, (meth)acrylate monomers, silicon polymers, epoxy polymers.

2. The composition of claim 1, wherein the second material is a matrix material selected from one or more members of the group consisting of poly-(meth)acrylates, (meth)acrylate monomers, silicon polymers, epoxy polymers.

3. 3. The composition of claim 1 or 2, wherein the group 13 element is In and the group 15 element is P, more preferably the core is selected from the group consisting of InP, InPZn, InPZnS, and InGaP.

4. At least one of the shell layers contains a first element from group 12 of the periodic table, preferably the first element is Zn or Cd; and The composition of any one of claims 1 to 3, comprising a second element of group 16 of the periodic table, preferably the second element is S, Se or Te.

5. At least one shell layer is represented by the following formula (II): ZnS x Se y Te z、 -(II) The composition according to any one of claims 1 to 4, wherein 0≦x≦1, 0≦y≦1, 0≦z≦1, and x+y+z=1, preferably 0≦x≦1, 0≦y≦1, z=0, and x+y=1.

6. The composition according to any one of claims 1 to 5, wherein the shell layer of the semiconducting luminescent nanoparticles is a double shell layer.

7. 7. The composition of any one of claims 1 to 6, wherein the composition further comprises at least one additional material, preferably the additional material is selected from the group consisting of an organic light emitting material, an inorganic light emitting material, a charge transport material, a scattering particle, a light transparent polymer, an antioxidant, a radical quencher, a polymerization initiator, and an additional ligand.

8. The composition of any one of claims 1 to 7, wherein the composition comprises a plurality of semiconducting luminescent nanoparticles.

9. The composition according to any one of claims 1 to 8, wherein the total amount of the semiconducting luminescent nanoparticles ranges from 0.1 wt. % to 90 wt. %, preferably from 5 wt. % to 70 wt. %, more preferably from 20 wt. % to 50 wt. %, based on the total amount of the composition.

10. The composition according to any one of claims 1 to 9, and At least one solvent, preferably it is an ethylene glycol monoalkyl ether, such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, and ethylene glycol monobutyl ether; a diethylene glycol dialkyl ether, such as diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dipropyl ether, and diethylene glycol dibutyl ether; a propylene glycol monoalkyl ether, such as propylene glycol monomethyl ether (PGME), propylene glycol monoethyl ether, and propylene glycol monopropyl ether; a methyl cellosolve acetate and an ethyl cellosolve acetate. ethylene glycol alkyl ether acetates such as sorb acetate; propylene glycol alkyl ether acetates such as propylene glycol monomethyl ether acetate (PGMEA), propylene glycol monoethyl ether acetate, and propylene glycol monopropyl ether acetate; ketones such as methyl ethyl ketone, acetone, methyl amyl ketone, methyl isobutyl ketone, and cyclohexanone; alcohols such as ethanol, propanol, butanol, hexanol, cyclohexanol, ethylene glycol, and glycerin; esters such as ethyl 3-ethoxypropionate, methyl 3-methoxypropionate, and ethyl lactate; and cyclic esters such as gamma butyrolactone;A formulation comprising: a solvent selected from one or more members of the group consisting of chlorinated hydrocarbons such as chloroform, dichloromethane, chlorobenzene, and dichlorobenzene, preferably the solvent is propylene glycol alkyl ether acetate, alkyl acetate, ethylene glycol monoalkyl ether, propylene glycol, and propylene glycol monoalkyl ether, preferably the solvent is selected from one or more members of the group consisting of propylene glycol alkyl ether acetate such as propylene glycol monomethyl ether acetate (PGMEA), alkyl acetate such as butyl acetate, ethylene glycol monobutyl ether, ethylene glycol monoalkyl ether such as propylene glycol, propylene glycol or propylene glycol monoalkyl ether such as methoxypropanol, more preferably the solvent is selected from propylene glycol alkyl ether acetate;

11. Use of a composition according to any one of claims 1 to 9 or a formulation according to claim 10 in an electronic device, an optical device, in a biomedical device or for making an electronic device, an optical device or a biomedical device.

12. Optical medium comprising at least the composition according to any one of claims 1 to 9 or the formulation according to claim 10.

13. 10. An optical medium comprising at least one organic layer comprising at least one luminescent nanoparticle comprising the composition according to any one of claims 1 to 9, preferably said one organic layer is a light emitting layer, more preferably the medium further comprises one or more layers selected from the group consisting of a hole injection layer, a hole transport layer, an electron blocking layer, a hole blocking layer, an electron blocking layer and an electron injection layer.

14. 14. Optical medium according to claim 13, wherein the organic layer comprises at least one luminescent nanoparticle and a first material according to claim 13, and a host material, preferably the host material is an organic host material.

15. An optical device comprising at least one optical medium according to any one of claims 12 to 14.

Citation Information

Patent Citations

  • Semiconductor nanoparticle capping agent

    JP2011513508A

  • Semiconductor nanoparticles and thin film containing the same

    US20040007169A1