Method for producing granular boron nitride and granular boron nitride
The heat treatment of boron nitride with calcium and rare earth oxides produces granular boron nitride with a shell structure, enhancing thermal conductivity and reducing the need for expensive rare earth metals, addressing anisotropy issues in resin composites.
Patent Information
- Application Number
- JP2020549724
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-03-28
- Filing Date
- 2020-02-13
- Publication Date
- 2024-09-20
- Estimated Expiration
- 2040-02-13
AI Technical Summary
Existing methods for producing boron nitride compositions with resin materials face challenges in improving thermal conductivity, particularly in the thickness direction, due to anisotropy issues and the high cost of rare earth metals like yttrium, which are used to enhance thermal conductivity but are expensive.
A method involving the heat treatment of boron nitride powder with calcium compounds and rare earth element oxides in a non-oxidizing gas atmosphere to produce granular boron nitride, which includes a shell structure that enhances thermal conductivity while reducing the amount of rare earth metals needed.
The method results in improved thermal conductivity of molded products, suppressing anisotropy and maintaining good moldability, even when used in large amounts, with reduced reliance on expensive rare earth metals.
Smart Images

Figure 0007554473000019 
Figure 0007554473000010 
Figure 0007554473000016
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a granular boron nitride composition and the granular boron nitride composition obtained by the method.Furthermore, the present invention relates to a resin composition comprising the granular boron nitride composition and a resin, a molded product comprising granular boron nitride and a resin obtained by molding such a resin composition, and a method for producing the same. [Background technology]
[0002] Boron nitride (hereinafter referred to as "BN") is an insulating ceramic and is known to have various crystal types, such as c-BN, which has a diamond structure, h-BN, which has a graphite structure, and t-BN, which has a turbostratic structure.
[0003] Among these, h-BN is relatively easy to synthesize and has excellent thermal conductivity, solid lubricity, chemical stability, and heat resistance, so attempts have been made to increase the thermal conductivity of resin materials that have extremely low thermal conductivity by mixing them with fillers. Such resin materials are used in the electrical and electronic fields as heat dissipation components for integrated circuits.
[0004] However, h-BN has a layered structure similar to graphite and has large crystal anisotropy. Macroscopically, h-BN is granular, but microscopically, it is a layered structure of plate-shaped crystals. Since the plate-shaped crystal planes corresponding to the a-axis direction of the crystal are connected by strong covalent bonds, it exhibits a high thermal conductivity of nearly 400 W / mK. On the other hand, since the plate thickness direction corresponding to the c-axis direction is layered by weak van der Waals force bonds, it only exhibits a low thermal conductivity of about 1 to 2 W / mK.
[0005] When a resin composition containing such boron nitride is molded to produce a molded product, the plate-like boron nitride is oriented in the plate direction of the molded product, which is the flow direction of the resin composition during molding, and the resulting molded product has a problem in that it has excellent thermal conductivity in the plate direction but only low thermal conductivity in the thickness direction. Therefore, it is desirable to improve the anisotropy of such granular BN.
[0006] For example, JP 2013-147363 A discloses a method for producing metal oxide-containing boron nitride, which comprises mixing boron nitride with an oxide of at least one rare earth metal selected from yttrium, cerium, and ytterbium, and carbon, and heat-treating the mixture under a non-oxidizing gas atmosphere. Even when the boron nitride produced by this method is mixed in a large amount with a resin material to form a resin composition for the purpose of improving thermal conductivity, solid lubricity, chemical stability, heat resistance, etc., the boron nitride produced by this method can improve the thermal conductivity in the thickness direction of the molded body while maintaining good moldability as a resin composition.
[0007] It has been described that the thermal conductivity of boron nitride can be improved by producing the boron nitride by the above-mentioned method, but compared with the inherent thermal conductivity of the above-mentioned boron nitride, there is still room for improvement in the thermal conductivity that can be improved. Also, there is a problem that rare earth metal components such as yttrium are relatively expensive. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2013-147363 A Summary of the Invention [Problem to be solved by the invention]
[0009] Therefore, when mixing boron nitride with a resin material and using it to manufacture a molded product, it is desirable to further increase the thermal conductivity. Also, when using rare earth metal components such as yttrium, it is desirable to reduce the amount of the rare earth metal components used. [Means for solving the problem]
[0010] As a result of intensive research into the above problems, the present inventors have found that by heat-treating boron nitride, particularly boron nitride powder, in the presence of a calcium compound and a rare earth oxide as sintering aids, it is possible to produce granular boron nitride that can solve at least one of the above problems. It has been found that by heat-treating boron nitride powder in the presence of a calcium compound in addition to a rare earth oxide, it is possible to produce granular boron nitride having a large particle size.
[0011] In a first aspect, the present invention provides a method for producing a semiconductor device comprising the steps of: (1) a boron nitride component comprising boron nitride; (2) a rare earth component comprising an oxide and / or a precursor compound of at least one rare earth element selected from yttrium, cerium, and ytterbium; and (3) A calcium component comprising calcium oxide and / or calcium carbonate. The present invention provides a method for producing a granular boron nitride composition, comprising the step of heat-treating a mixture comprising the above components in a non-oxidizing gas atmosphere.
[0012] In a second aspect, the present invention provides a granular boron nitride composition obtained by the above-mentioned production method. In addition to the granular boron nitride obtained by heat treatment, this composition contains other compounds derived from the components (1) to (3) contained in the mixture. Such other compounds are mainly rare earth element oxides and calcium oxide, but may also contain small amounts of composite oxides derived from elements present in the system (e.g., Y-Ca-BO composite oxide).
[0013] In a third aspect, the present invention provides granular boron nitride contained in the above-mentioned granular boron nitride composition. This granular boron nitride can be obtained by subjecting the above-mentioned composition to a washing treatment using an acid to remove at least a portion of the calcium oxide and rare earth element oxides and most, preferably substantially all, of the calcium oxide. Thus, in a fourth aspect, the present invention provides a method for producing granular boron nitride, which method is characterized by acid washing the granular boron nitride composition of the second aspect.
[0014] In a fifth aspect, the present invention provides a resin composition comprising the granular boron nitride composition according to the second aspect or the granular boron nitride composition according to the third aspect and a resin material. In a sixth aspect, the present invention provides a molding method characterized by using such a resin material for molding, and in a seventh aspect, the present invention provides a molded article obtained by such a molding method. Effect of the Invention
[0015] When the granular boron nitride obtained by the manufacturing method of the present invention is mixed with a resin material to form a resin composition, the thermal conductivity of the resulting molded body is improved. In a preferred embodiment, the anisotropy of the thermal conductivity of the molded body is suppressed. Even when a large amount is mixed, the thermal conductivity of the resulting molded body can be improved while maintaining good moldability.
[0016] An example of a molded article is a heat dissipation sheet that requires insulation, thermal conductivity, and moldability. For example, it is suitable for use in the electrical and electronic fields. The granular boron nitride composition or granular boron nitride of the present invention can be used as a filler that can be blended into thermally conductive pastes, thermally conductive adhesives, compositions for thermally conductive molded articles, etc. [Brief description of the drawings]
[0017] [Figure 1]FIG. 1 shows a table and a graph of experimental results showing the relationship between the average particle size of the granular boron nitride of the present invention and the proportion (percent by mass) of the sum of the rare earth component (2) and the calcium component (3) (i.e., (2) + (3)) in the mixture to be heat treated. [Diagram 2] FIG. 2 shows a table and a graph of experimental results showing the relationship between the specific surface area of the granular boron nitride of the present invention and the proportion (percent by mass) of the sum of the rare earth component (2) and the calcium component (3) (i.e., (2) + (3)) in the mixture to be heat-treated. [Diagram 3] FIG. 3 shows a table and a graph of experimental results showing the relationship between the thermal conductivity in the thickness direction of a molded body obtained using a resin composition containing granular boron nitride of the present invention and the proportion (mass percent) of the sum of the rare earth component (2) and the calcium component (3) (i.e., (2) + (3)) in the mixture to be heat-treated. [Figure 4] FIG. 4 shows a table and a graph of experimental results showing the relationship between the thermal conductivity in the planar direction (direction perpendicular to the thickness direction) of a molded body obtained using a resin composition containing granular boron nitride of the present invention and the proportion (mass percent) of the sum of the rare earth component (2) and the calcium component (3) (i.e., (2) + (3)) in the mixture to be heat-treated. [Diagram 5] FIG. 5 shows a table and graph of experimental results showing the relationship between the degree of orientation of granular boron nitride in a molded body formed using a resin composition containing granular boron nitride of the present invention and the sum (i.e., (2)+(3)) of the rare earth component (2) and calcium component (3) in the mixture heat-treated when producing the granular boron nitride. [Figure 6] FIG. 6 is a typical SEM photograph of the granular boron nitride of the present invention obtained in Example 6 (but after washing). [Figure 7] FIG. 7 is a typical SEM photograph of the particulate boron nitride composition of the present invention obtained in Example 6 (before washing). [Figure 8] FIG. 8 shows SEM and EDS photographs (for N element and Y element) of the particulate boron nitride containing yttrium oxide of the present invention obtained in Example 36 (but after washing). [Figure 9] FIG. 9 shows SEM and EDS photographs (for N element, Ca element and Y element) of the particulate boron nitride composition of the present invention obtained in Example 11 (before washing). [Figure 10] FIG. 10 shows an SEM photograph and an EDS photograph (for N element) of the granular boron nitride of the present invention (after washing) obtained in Example 12. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Next, an embodiment of the present invention will be described in detail.
[0019] In the method for producing a granular boron nitride composition of the present invention, in a preferred embodiment, the boron nitride contained in the boron nitride component (1) is hexagonal boron nitride (h-BN) having a graphite structure, and in one embodiment, the boron nitride is preferably powdered (or finely granular) boron nitride, preferably h-BN. As such boron nitride component (1), a hexagonal boron nitride that is generally commercially available can be used.
[0020] The oxide of the rare earth element contained in the rare earth component (2) is, for example, yttrium oxide, cerium oxide, or ytterbium oxide, and the precursor of the oxide of the rare earth element means a compound that gives such an oxide in a preliminary heat treatment and / or heat treatment carried out prior to the heat treatment. As such rare earth component (2), for example, commercially available products such as yttrium oxide and cerium oxide can be used.
[0021] The calcium component (3) comprises calcium oxide and / or calcium carbonate, and as such calcium component (3), calcium oxide, calcium carbonate, etc. that are generally commercially available can be used.
[0022] In one preferred embodiment, the ratio of the total mass of the rare earth element oxide and its precursor (if present) in the rare earth component (2) and calcium oxide and calcium hydroxide (if present) in the calcium component (3) to the total mass of boron nitride (BN) in the boron nitride component (1), the rare earth element oxide (e.g., YO) and its precursor (if present) in the rare earth component (2), and calcium oxide (CaO) and calcium hydroxide (if present) in the calcium component (3) contained in the mixture to be heat treated (e.g., (YO+CaO) / (BN+YO+CaO)) is generally 5% to 60% (thus, boron nitride is 95 to 40%), preferably 6% to 50% (thus, boron nitride is 94 to 50%), more preferably 7 to 42%, particularly preferably 14 to 42%, for example 14 to 35%.
[0023] In another preferred embodiment, the ratio of rare earth elements in the rare earth component (2) to calcium elements in the calcium component (3) (e.g., the number of Y elements: the number of Ca elements) based on the number of elements in the mixture to be heat-treated is preferably 1:0.25 to 1:4, more preferably 1:0.5 to 1:3, particularly preferably 1:0.7 to 1:2.5, for example, 1:1 to 1:2.
[0024] The heat treatment is carried out in a non-oxidizing gas atmosphere. The non-oxidizing gas atmosphere means an atmosphere that does not contain oxygen, and is, for example, an atmosphere that contains one or more of nitrogen gas, helium gas, argon gas, ammonia gas, hydrogen gas, methane gas, propane gas, and carbon monoxide gas. The crystallization rate after dissolution of boron nitride varies depending on the type of gas used in this atmosphere. For example, with argon gas, the crystallization rate may be slow, and the heat treatment time may be extended. In order to perform crystallization in a short time, it is particularly preferable to use nitrogen gas or a mixed gas in which nitrogen gas is used in combination with other gases. In one embodiment of the present invention, the heat treatment is carried out in a nitrogen gas atmosphere. It is preferable that the mixture to be heat-treated is in a non-oxidizing atmosphere even until it reaches a predetermined heat treatment temperature described later. In this specification, the non-oxidizing gas atmosphere may be a so-called vacuum state or reduced pressure state that does not substantially contain gas or contains almost no gas.
[0025] In the method of the present invention, the boron nitride component (1) may contain oxygen, and in that case (for example, when it is contained in the form of boron oxide), the mixture may contain carbon in an amount of 1% to 5% based on the mass of boron nitride in the boron nitride component (1) if necessary (for example, to convert at least a portion of the boron oxide to boron nitride). In another embodiment, the mixture does not contain carbon unless there is a substantial adverse effect. In addition, when a commercially available product known as "boron nitride" is used as the boron nitride component (1), the amount of oxygen contained is not so large (for example, generally 5% or less, for example 4% by mass based on the mass of the boron nitride component (1)), so there is usually no need to use carbon, but the mixture may contain carbon if necessary (for example, when the amount of oxygen is large).
[0026] The granular boron nitride contained in the granular boron nitride composition of the present invention preferably has an average particle size of 9 to 25 μm, more preferably 10 to 20 μm, for example 12 to 15 μm, and the specific surface area of the granular material is preferably 2 to 10 m. 2 / g, more preferably 4 to 8m 2 / g, e.g. 5~6m 2The above average particle size and specific surface area are values measured by the following methods:
[0027] (Average particle size) 0.02 to 0.04 g of the obtained granular material was placed in 20 ml of soapy water (1 g of kitchen liquid detergent (Kitchen Fresh, manufactured by Sankyo Yushi) mixed with 500 ml of pure water) as a dispersion medium, and the mixture was stirred for 5 minutes with an ultrasonic cleaner to disperse the granular material. Then, a volume-based particle size accumulation diagram was created using a laser diffraction particle size distribution measuring device (Shimadzu Corporation: SALD-2100), and the particle size at a particle size accumulation rate of 50% (Dv50) was taken as the average particle size (or simply referred to as "particle size"). The average particle size referred to in this specification is a value obtained by this measurement method regardless of the aggregation state of the particles, and may be the average particle size of primary particles or the average particle size of secondary particles depending on the properties of the particles. In some cases, it is the average particle size measured in a state where both primary particles and secondary particles are mixed.
[0028] (specific surface area) The specific surface area of powdered granular boron nitride was measured using a gas adsorption analyzer (AUTOSORB-1, Quantachrome Instruments LLC). The samples were dried at 110°C for 12 hours before the measurement. The Brunauer-Emmett-Teller (BET) method, a typical method for calculating the surface area of granular materials (0.5-1.0 g), was used. Using the multipoint BET method, the specific surface area was calculated from a three-point BET plot where P / P0 = 0.1, 0.2, and 0.3 (where P is the gas pressure of the adsorbate at adsorption equilibrium, and P0 is the saturated vapor pressure of the adsorbate at the adsorption temperature).
[0029] The granular boron nitride of the present invention produced by heat treatment is believed to be produced by dissolving boron nitride in the liquid phase produced by first melting calcium oxide in addition to rare earth element oxide during heat treatment, and then precipitating from the liquid phase. This is not bound by any theory, but based on the inventors' knowledge and experience regarding the production of boron nitride and new findings obtained regarding the above-mentioned production method, particularly the results of SEM photographs of the resulting granules, the production of the granules can be considered as follows. Note that this is only one possible way of thinking. The present invention, which is capable of obtaining boron nitride granules by heat treatment under specific conditions, is not limited in any way by the suitability of this idea.
[0030] In the method for producing the granular boron nitride composition of the present invention, when the mixture is heat-treated, the rare earth element oxide and calcium oxide are preferentially melted to form a liquid phase, in which the granular boron nitride is dissolved. As this dissolution progresses, the boron nitride concentration in the liquid phase increases and becomes supersaturated, resulting in the precipitation of boron nitride (recrystallization). While boron nitride is precipitated in this way, other boron nitride particles are newly dissolved in the liquid phase and become supersaturated, resulting in further precipitation of boron nitride. By repeating this dissolution-precipitation process, the precipitated boron nitride is bonded to form a bent shape. Since there is a liquid phase in which boron nitride is dissolved inside and outside the bent shape of the boron nitride, the supersaturation-precipitation process is repeated there, and the boron nitride crystals grow further, the bent shape becomes thicker and longer, and the boron nitride crystals gradually grow. The bent boron nitride thus grown combines with other bent boron nitride crystals grown in the same way, and grows further inside and outside of them, eventually forming a shape surrounded by a wall having a certain thickness, i.e., a roughly spherical or granular shell of boron nitride crystals. In this sense, the boron nitride obtained by heat treatment is referred to as "granular boron nitride" in this specification.
[0031] Thus, the granular boron nitride of the present invention has a strong shell structure formed by boron nitride in the form of a relatively thick wall. This shell structure is a rounded shape, i.e., a granular shape, as a whole particle. In the strict sense, it is a so-called spherical, spheroidal, or polyhedral shape, and generally has a complex combination of these shapes. Usually, this granular material has a relatively small aspect ratio, preferably 1 to 3, more preferably 1 to 2, and is clearly different from granular materials with a large aspect ratio such as boron nitride having a graphite structure.
[0032] An example of a typical SEM photograph of the granular boron nitride of the present invention is shown in FIG. 6. These photographs are of the granular boron nitride obtained in Example 6 described later. A detailed observation of these photographs reveals that the granular boron nitride is so-called granular, having an apparent shape of a polyhedron (or sphere) as a whole, constituted by curved walls. An SEM photograph was also taken of the granular boron nitride composition of the present invention in a state before removing the oxide. The photograph is shown in FIG. 7. As can be seen by comparing the two, there is substantially no difference from that after removing the oxide. One possible explanation for this is that the liquid phase component consisting of the added oxide remains mainly in the granular boron nitride having a shell structure.
[0033] In the granular boron nitride of the present invention, the shell structure may contain other granular boron nitride or a part thereof. FIG. 10 shows SEM photographs of two different fields of view of a cross section of the granular boron nitride obtained in Example 12 described later mixed with an epoxy resin and cured, and EDS photographs of the nitrogen element in the photographs. In FIG. 10, the upper photograph is the SEM photograph. The lower photograph shows the results of mapping analysis of the granular boron nitride in this state for the N element using EDS (energy dispersive X-ray analysis), and is an EDS photograph. The EDS photograph corresponding to the upper left photograph is the lower left photograph, and the EDS photograph corresponding to the upper right photograph is the lower right photograph. It can be seen that the nitrogen element (whitish part) and therefore boron nitride are present inside the shell structure of boron nitride, which appears to shine white in the SEM photograph, as can be confirmed in the EDS photograph.
[0034] As is clear, granular boron nitride is also present inside the shell structure of granular boron nitride. In the embodiment on the left side of the photograph in FIG. 10, the granular boron nitride inside is columnar (hence, planar in three dimensions), and the inside of the shell structure of granular boron nitride located on the outside is divided, for example, divided into two. On the other hand, in the embodiment on the right side of the photograph in FIG. 10, the granular boron nitride inside fills a part of the inside of the shell structure of granular boron nitride located on the outside. The granular boron nitride thus included may be a part of the shell structure that has not yet reached the stage of forming a shell structure (for example, at least one or a part of the surface constituting the shell), or a smaller shell structure. The surface constituting the shell structure may be a substantially flat surface constituting the shell structure, or a curved surface. In one embodiment, the granular boron nitride inside the shell structure is thus considered to be generated by newly precipitating and growing boron nitride inside the already formed shell structure or a part of it. In another embodiment, it is believed that the grown granular boron nitride or a part thereof is bonded with other granular boron nitride or a part thereof, and a part of the granular boron nitride is contained therein. In this way, the granular boron nitride containing other granular boron nitride increases the thermal conduction path, and therefore is believed to contribute to increasing the thermal conductivity of the granular boron nitride. In addition, the presence of other granular boron nitride inside is believed to have the effect of suppressing or preventing deformation when pressure is applied to the granular boron nitride from the outside.
[0035] In the present invention, as described above, when boron nitride precipitates from the liquid phase to form a shell, one of the main features is that rare earth oxide and calcium oxide are present as the liquid phase, and as a result, the resulting granular boron nitride has a thicker shell and a smaller aspect ratio. This makes it possible to produce granular boron nitride with superior crush strength compared to various known boron nitride aggregates. Specifically, as described below, when a resin composition is obtained by blending the composition with a resin material and then molded, the orientation degree of the granular boron nitride in the molded body can be about 85% or less, preferably 70% or less, more preferably 20 to 65%, for example 25 to 60%. When the particle size of the granular boron nitride particles is small, the resistance to hot press pressure is strong, so that the granular particles do not collapse and show a low orientation degree of the (00L) plane, but in order for the resin material to have a high thermal conductivity, granular boron nitride with a large particle size is desirable so that a long high heat conduction path can be provided. However, as the grain size of granular boron nitride increases, the grains tend to collapse during hot pressing, which may increase the degree of orientation of the (00L) plane.
[0036] As described above, the shell is formed, and the granular boron nitride composition of the present invention comprises a component that is finally solidified inside the shell by cooling after heating. This component is mainly composed of rare earth element oxide and calcium oxide, but may comprise various compounds, particularly composite oxides, as described above. In addition to such components, as described above, it may also comprise a portion of boron nitride that constitutes the shell structure of the granular boron nitride or a part of it. In the method for producing the granular boron nitride composition of the present invention, the ratios of boron, rare earth element and calcium elements contained in the granular boron nitride composition obtained by heat treatment are substantially the same as the ratios of these elements contained in the mixture. Therefore, the amounts of rare earth element oxide and calcium oxide contained in the granular boron nitride composition are equal to the amounts of oxides derived from rare earth element and calcium contained in the mixture.
[0037] Thus, in one embodiment, the granular boron nitride composition contains, in addition to boron nitride, typically 3 to 40%, preferably 5 to 37%, more preferably 8 to 35%, for example 12 to 32%, of rare earth element oxide, and 1 to 30%, preferably 2 to 26%, more preferably 5 to 22%, for example 8 to 15%, of calcium oxide, based on the mass of the composition.
[0038] Such oxides can be reduced by acid washing as described above, for example, by using an acid aqueous solution to react the oxides with an acid to convert them into water-soluble salts, which are then dissolved in water and removed. For example, when the granular boron nitride composition is used as a thermally conductive filler, the thermal conductivity of oxides is usually small, so it is preferable to reduce the oxides contained in the granular boron nitride composition to a level that does not substantially adversely affect the thermal conductivity. For example, calcium oxide can be preferentially removed by acid washing, so that substantially the entire amount of calcium oxide is removed, and rare earth element oxides are partially removed. The granular boron nitride composition is acid washed so that the amount of rare earth element oxide contained therein is, for example, 0.1 to 30%, preferably 1 to 15%, more preferably 2 to 12%, for example 3 to 10%, based on its mass.
[0039] Thus, the present invention provides a granular boron nitride having a shell structure, and also provides another granular boron nitride obtained by removing at least rare earth element oxides and / or calcium oxide from the above-mentioned granular material, preferably a major part of the calcium oxide, more preferably substantially all of the calcium oxide. That is, the more preferred granular material comprises boron, nitrogen, oxygen and rare earth elements, and is substantially free of calcium. The granular material has a strong shell structure formed by boron nitride and contains a small amount of rare earth element oxide in addition to boron nitride. The removal of the oxides may be carried out by any other suitable method other than washing with an acid, as long as the filler properties of the granular boron nitride are not unduly affected. Washing with an acid is advantageous in that the oxides can be substantially removed without adversely affecting the granular boron nitride.
[0040] As described above, the present invention provides a resin composition comprising granular boron nitride, preferably having an oxide content reduced by washing, particularly granular boron nitride substantially free of calcium oxide, and a resin material. The resin composition contains granular boron nitride in an amount of preferably 10 to 90%, more preferably 15 to 88%, for example 30 to 85%, particularly 50 to 82% by mass based on the total mass of the resin composition. When these ranges are expressed as volume percentages, they correspond to about 5 to 80 volume%, about 10 to 70 volume%, and about 15 to 50 volume%, respectively, although they may differ slightly depending on the apparent density of the granular material. If the amount of granular boron nitride is too small, the probability that the granular boron nitride particles are in contact with each other decreases, and thermal conduction may be insufficient. Conversely, if the amount is too large, the resin material as a matrix becomes excessively small, which may adversely affect the strength and voltage resistance of the molded body. In another embodiment, the resin composition may comprise the particulate boron nitride composition of the present invention in place of the particulate boron nitride described above in similar proportions.
[0041] <Granular boron nitride composition and method for producing granular boron nitride> The method for producing a granular boron nitride composition of the present invention is characterized by comprising a step of heat-treating a mixture comprising a boron nitride component (1) comprising boron nitride (BN, preferably hexagonal boron nitride (h-BN)), a rare earth component (2) comprising an oxide of at least one rare earth element selected from yttrium, cerium and ytterbium and / or a precursor thereof, and a calcium component (3) in a non-oxidizing gas atmosphere.
[0042] In the method for producing a granular boron nitride composition of the present invention, when the rare earth component (2) contains a precursor of an oxide of at least one rare earth element selected from yttrium, cerium and ytterbium, the precursor is converted to the corresponding rare earth element oxide in the heat treatment step or in a preheating or calcination step which may be carried out beforehand as necessary. When the calcium component (3) contains calcium carbonate, it is similarly converted to calcium oxide. The converted product contributes to the precipitation and growth of granular boron nitride crystals as a rare earth element oxide or calcium oxide.
[0043] The method for producing the granular boron nitride composition of the present invention is carried out, for example, by mixing the raw material components (1), (2) and (3) to obtain a mixture, which is then heated under a non-oxidizing gas atmosphere, for example at 1800 to 2100°C. The mixture may contain other components as necessary, for example components that are inevitably contained when producing the raw material components. For example, when the boron nitride component (1) contains excessive oxygen (for example, when it contains 5 mass% or more of oxygen because it contains boron oxide), the mixture may contain carbon, and the oxygen can be reduced by reduction using carbon (which may result in the production of boron nitride).
[0044] In order to promote uniform mixing of the mixture, a suitable dispersion medium (e.g., ethanol, acetone, etc.) may be used, and the mixture is mixed uniformly with 5 to 20 times the amount of the dispersion medium by mass in a homogenizer to form a slurry or paste. After drying, this is calcined (pre-baked or fired) in air as necessary to obtain a powder in which the components constituting the mixture are uniformly mixed, and then heat-treated at 1800 to 2100°C in a non-oxidizing gas atmosphere.
[0045] <Boron nitride component (1)> Examples of the boron nitride component (1) used in the present invention include commercially available h-BN, commercially available t-BN, BN produced by a reduction nitridation method of a boron compound and ammonia, and BN synthesized from a boron compound and a nitrogen-containing compound such as melamine, and the like, and can be used without any particular restrictions. In one embodiment, it is preferable to use h-BN. Such a boron nitride component (1) preferably contains at least 90% boron nitride by mass, preferably at least 95%, and more preferably at least 96%. As long as it does not impair the effects of the present invention, it may contain other boron compounds (e.g., boron oxide), other elements or components, etc. that are inevitably mixed in when producing boron nitride. The boron nitride constituting the boron nitride component (1) is preferably h-BN, but may contain other boron nitrides. The ratio of h-BN to boron nitride may be preferably at least 90%, more preferably at least 95%, for example at least 96%, particularly at least 98%, and the remainder is other boron nitrides. Boron nitride may be commercially available in the form of fine particles or powder. For example, Nisshin Refratec Co., Ltd. sells boron nitride having a primary particle size of 50 nm, an aggregate particle size of 3 μm, and a specific surface area of 160 m. 2 / g boron nitride powder is commercially available as "ABN." MARUKA Corporation also sells h-BN in powder form as "AP170S."
[0046] In the method for producing the granular boron nitride composition of the present invention, from the viewpoint of growth of the h-BN crystals, oxygen may be present to a certain extent in the boron nitride component (1) containing the raw material h-BN and the like. In the present invention, for example, the total oxygen concentration of the boron nitride component (1) may be 1% by mass to 10% by mass, and it is generally preferable to use one having a total oxygen concentration of 5% by mass or less. When the total oxygen concentration is within the above range, the primary particle size of the boron nitride particles is generally small and many of the crystals are underdeveloped, and when mixed with other components used in the present invention and subjected to heat treatment, it is preferable because it is easily dissolved. If the total oxygen concentration is excessively high, when the granular boron nitride composition obtained after heat treatment is used as a thermally conductive filler, it is in a state containing oxides, so that high thermal conductivity may not be achieved, which is not preferable. In that case, the amount of oxygen can be reduced by adding carbon to the mixture as described above. Alternatively, the granular boron nitride composition may be washed to reduce the amount of oxides. Furthermore, if the total oxygen concentration of the boron nitride component (1) is excessively low, the purity and crystallinity of boron nitride are already good, so that it may be difficult to dissolve in the liquid phase, and as a result, changes such as the crystal growth of boron nitride may be small, and it may be difficult to form an aggregate structure. The total oxygen concentration in the boron nitride component (1) as a raw material can be measured by the inert gas fusion-infrared absorption method using an oxygen / nitrogen analyzer manufactured by Horiba, Ltd.
[0047] There is no particular restriction on the particle size of the boron nitride, preferably granular boron nitride, constituting the boron nitride component (1). If the particle size is excessively large, a non-uniform mixed state is likely to occur when preparing the mixture, so it is preferable that the average particle size of the boron nitride, particularly granular boron nitride, contained in the boron nitride component (1) is 5 μm or less. There is no particular restriction on the lower limit of the average particle size, but it is usually 0.1 μm or more. As described above, the average particle size can be measured by dispersing the granular boron nitride, which is the raw material, in an appropriate solvent and using a laser diffraction / scattering type particle size distribution analyzer.
[0048] <Rare Earth Components (2)> When the rare earth component (2) used in the production method of the present invention contains a precursor of an oxide of a rare earth element, this is converted to a rare earth element oxide in the heat treatment step or in a calcination step that may be carried out beforehand as necessary, and this oxide acts to stably precipitate and grow granular boron nitride. Components that are originally oxides contained in the rare earth component (2) also act in the same way.
[0049] In addition, the rare earth component (2) used in the manufacturing method of the present invention is preferably heat-resistant to the heat treatment conditions because it is heat-treated together with the boron nitride component (1). In the present invention, rare earth oxides such as yttrium oxide, cerium oxide, ytterbium oxide, and / or precursors thereof are used as the rare earth component (2). Among these, yttrium oxide is particularly suitable from the viewpoints of thermal conductivity and heat resistance as an oxide, and stably precipitating granular boron nitride and growing it to have strength. As the rare earth component (2) containing such an oxide, a commercially available oxide can be used. In general, a commercially available oxide with a purity of 99% by mass or more can be used as the rare earth component (2). In addition, at least one rare earth compound selected from yttrium, cerium, and ytterbium used as a precursor to generate such an oxide may be in any suitable form, for example, in the form of a liquid sol, a water-soluble salt such as a nitrate, and is converted to a rare earth oxide in the heat treatment step or a calcination step that may be performed before the heat treatment step as necessary.
[0050] In the rare earth component (2) used in the production method of the present invention, the oxide is at least one selected from yttrium oxide, cerium oxide, and ytterbium oxide, and the precursor thereof provides such an oxide of a rare earth element. For example, at least one selected from inorganic acid salts and organic acid salts, such as acetates, nitrates, carbonates, citrates, oxalates, and sulfates of rare earth elements, and chlorides, etc., can be exemplified. Among these, from the viewpoint of ease of availability, etc., yttrium oxide, acetates, nitrates, carbonates, citrates, oxalates, sulfates, etc. of yttrium are preferably used. In a preferred embodiment, yttrium oxide, yttrium nitrate, yttrium carbonate, yttrium citrate, yttrium oxalate, yttrium sulfate, etc. are used.
[0051] As the rare earth component (2), one selected from the rare earth element oxides and their precursor metal compounds may be used alone, or in another embodiment, two or more may be used in combination. In addition to the rare earth element oxides and / or their precursors as described above, the rare earth component (2) may contain other components that are inevitably contained during the production of the granular boron nitride produced in the present invention, for example, as long as they do not substantially have an adverse effect on the granular boron nitride produced in the present invention.
[0052] <Calcium component (3)> The calcium component (3) used in the production method of the present invention includes at least one selected from calcium oxide and calcium carbonate. Calcium carbonate is converted to calcium oxide in the heat treatment step of the present invention or in a calcination step that may be performed beforehand as necessary. The calcium component (3) may be in any suitable form, such as a solid (e.g., powder), a dispersion liquid, etc. Although the present invention is not bound by any theory and does not limit the present invention, in consideration of the results of the Examples and Comparative Examples described below, such calcium component (3) is considered to have a function of melting prior to boron nitride in the heat treatment step, as with the rare earth element oxides described above, to provide a liquid phase in which the already-existing boron nitride can be dissolved, and then to provide a solvent in which boron nitride crystallizes (i.e., recrystallizes) in the liquid phase. During such crystallization, it is considered that the crystals of boron nitride grow larger and then aggregate and bond to form a shell structure having a larger particle size. As such calcium component (3), calcium oxide and calcium carbonate that are commercially available can be used. Generally, calcium having a purity of 90% by mass or more (e.g., 93% or more, 95% or more, etc.) is commercially available and can be used as calcium (2). In addition to the above-mentioned calcium oxide and calcium carbonate, calcium component (3) may contain other components that are inevitably contained in the production of the granular boron nitride produced in the present invention, so long as they do not substantially adversely affect the product.
[0053] <Amount of each ingredient used> In a preferred embodiment, as described above, the ratio of rare earth elements in the rare earth component (2) to calcium elements in the calcium component (3), based on the number of elements in the mixture to be heat treated, is preferably 1:0.25 to 1:4, more preferably 1:0.5 to 1:3, particularly preferably 1:0.7 to 1:2.5, for example 1:1 to 1:2. If the amount of calcium is too small, the effect of the calcium oxide component in providing a large particle size to the granular boron nitride may be insufficient, and if the amount of calcium is too large, there will be too little rare earth element oxide, and the effect, particularly the effect of firmly binding the granular boron nitride, may be insufficient.
[0054] As described above, in the mixture to be heat-treated, the ratio of the amount of rare earth element oxide contained in the rare earth component (2) (in the case of a precursor, converted to the corresponding rare earth element oxide) and the amount of calcium oxide contained in the calcium component (3) (in the case of calcium carbonate, converted to calcium oxide) to the amount of boron nitride, the amount of rare earth element oxide, and the amount of calcium oxide in the mixture, i.e., (amount of rare earth oxide+amount of calcium oxide) / (amount of boron nitride+amount of rare earth oxide+amount of calcium oxide), is generally 5% to 60% (thus, boron nitride is 95 to 40%), preferably 6% to 50% (thus, boron nitride is 94 to 50%), more preferably 7 to 42%, particularly preferably 14 to 42%, for example 14 to 35%.
[0055] If the content is less than this range, the effect of stabilizing the shell structure of the granular boron nitride by the rare earth element oxide and calcium oxide during the heat treatment is reduced. As a result, when the obtained granular boron nitride composition or granular boron nitride is kneaded with a resin material, the shell structure is easily collapsed. When such granular boron nitride is used as a thermally conductive filler for molding, the viscosity of the resin composition melted for molding increases. Therefore, a larger force acts on the resin composition during molding, and the effect of stabilizing the shell structure tends to decrease. Also, if the content is greater than this range, the amount of boron nitride contained in the obtained granular boron nitride composition is excessively small. As a result, when the granular boron nitride composition is used as a thermally conductive filler, the effect of improving thermal conductivity may be reduced.
[0056] <Carbon> In the method for producing granular boron nitride of the present invention, when the boron nitride component (1) contains excessive oxygen, the mixture may further contain carbon as necessary. As carbon, carbon black, graphite, and carbon precursors that can be carbon sources at high temperatures can be used, but carbon black is preferred from the viewpoint of ease of availability. As carbon black, carbon black produced by the furnace method, channel method, etc., acetylene black, etc. can be used. The average particle size (average particle size on a volume basis) of these carbon blacks is arbitrary, but is preferably 0.01 to 20 μm.
[0057] Also, instead of or in addition to the above-mentioned carbon, a carbon precursor may be used. For example, synthetic resin condensates such as phenolic resin, melamine resin, epoxy resin, and furanphenolic resin, hydrocarbon compounds such as pitch and tar, and organic compounds such as cellulose, sucrose, polyvinylidene chloride, and polyphenylene can be used as precursors. Among these, those with low metal impurities such as phenolic resin, cellulose, and polyphenylene are particularly preferred. These may be used alone or in combination of two or more.
[0058] The amount of carbon used (when a carbon precursor is used, the amount of carbon generated from it) is preferably 5% by mass or less, more preferably 3% by mass or less, based on the boron nitride component (1) on a mass basis. The presence of carbon during the heat treatment can prevent the presence of excessive oxygen. As a result, the shell structure of the granular boron nitride obtained by the oxide during the heat treatment becomes stronger. If more carbon is used than this amount, the stability of the shell structure may be impaired. By reducing the amount of carbon used, the amount of carbon remaining after the heat treatment can be minimized, and therefore, when used as a thermally conductive filler, the effect on the insulating properties of the granular boron nitride can be suppressed. In this sense, it is preferable to be able to omit the use of carbon. Therefore, in the method for producing an aggregate of the present invention, the mixture does not contain carbon.
[0059] <Other ingredients> In the method for producing granular boron nitride of the present invention, the mixture containing components (1) to (3) may contain other components as long as they do not adversely affect the production method and the granular boron nitride produced. Examples of such other components include one or more inorganic aluminum compounds such as aluminum nitride, aluminum hydroxide, and aluminum oxide (alumina). By using these compounds in combination, the thermal conductivity of the obtained granular boron nitride is not impaired and the aggregate structure can be further stabilized.
[0060] However, if the amount of other components is too large, the boron nitride content in the produced granular boron nitride will be too low, and the effect of improving thermal conductivity when used as a thermally conductive filler may be insufficient. Therefore, when other components are used in combination, the amount of the other components used is generally preferably 5% or less, for example 0.1 to 3%, based on the boron nitride component (1) by mass.
[0061] <Mixing of raw material components (1) to (3)> In the method for producing granular boron nitride of the present invention, the method for mixing the boron nitride component (1), rare earth component (2) and calcium component (3) that make up the mixture, as well as the carbon and other components that are included as necessary as described above, is not particularly limited, and for example, dry mixing or wet mixing can be used.
[0062] For dry mixing, a horizontal cylindrical mixer, V-type mixer, double cone type mixer, ribbon type mixer, single-axis rod or pin rotor type mixer, paddle type mixer, conical screw mixer, high-speed flow type mixer, rotating disk type mixer, Muller type mixer, air current agitation type mixer or the like can be used, while for wet mixing, in addition to manual agitation and mixing, general mixers such as an automatic mortar, ball mill, Bonny mixer, internal mixer, three-roll mixer, co-kneader, votator, high-speed flow mixer, ultrasonic homogenizer or the like can be used.
[0063] For more uniform mixing, wet mixing is preferably used. Although there is no limitation on the solvent (dispersion medium) used in wet mixing, from the viewpoints of ease of drying and simplification of the apparatus, organic solvents such as pure water, alcohols such as ethanol, methanol, and propanol, and ketones such as acetone are preferred, and in another embodiment, a mixed solvent of water and these organic solvents is preferred.
[0064] The amount of organic solvent such as pure water, alcohol, or ketone used is preferably 5 to 20 times, and particularly 5 to 10 times, the mass of the boron nitride component (1) since too much will increase the load during drying performed later, and too little will make it difficult to achieve uniform mixing.
[0065] <Drying and grinding> When wet mixing is employed for mixing the components as described above, it is preferable to dry the mixture to remove the solvent and pulverize the dried product, and then, if necessary, calcinate it and then carry out a heat treatment.
[0066] There is no particular limitation on the method for carrying out this drying, and heating drying, heating vacuum drying, etc. may be used. In general, heating drying is preferred. In small-scale, heating vacuum drying is usually used. In the case of heating drying, the conditions are preferably a heating temperature of 100 to 120°C and a heating time of about 12 to 48 hours. If the heating temperature is too low or the heating time is too short, sufficient drying cannot be performed, and conversely, if the heating temperature is too high or the heating time is too long, it is not preferable in terms of heating costs. In the case of heating vacuum drying, the solvent is distilled off using an evaporator at a temperature of about 50°C.
[0067] The crushing after drying may be performed using a mortar or a ball mill. The degree of crushing is not important as long as the powder is crushed to the extent that no large lumps with an average particle size of 100 μm or more exist. The average particle size can be measured in the same manner as the average particle size described above.
[0068] The drying and pulverization may be performed in an air atmosphere, but it is preferable to perform the drying and pulverization in dry air with a humidity of 50% or less in order to prevent moisture absorption.
[0069] <Caking> When a metal salt such as a nitrate, acetate, or oxalate is used as a precursor of the rare earth oxide of the rare earth component (2), the precursor may be calcined (or pre-calcined, i.e., a heat treatment at a lower temperature prior to the heat treatment) to convert it to an oxide prior to the heat treatment. The same applies when calcium carbonate is used as the calcium component (3), and it is converted to calcium oxide.
[0070] This calcination may be carried out by heating at a temperature of 500 to 700°C for about 1 to 5 hours in an oxidizing atmosphere such as air. If the heating temperature during calcination is too low or the heating time is too short, the conversion will be insufficient, and acids or nitrogen oxides will be generated during the calcination, which will damage the apparatus, and this is not preferred. If a heating furnace capable of evacuating decomposition gases during heating is used, the calcination step may be omitted, and calcination can be performed simultaneously with the subsequent heat treatment. Also, if the heating temperature during calcination is too high or the heating time is too long, the boron nitride contained in the boron nitride component (1) may be oxidized, which is not preferred. If the heating furnace is equipped with an exhaust system, oxidation can be avoided by evacuating the air inside the furnace. In this case, oxidation of boron nitride due to high heating temperatures and long heating times does not pose a problem.
[0071] <Heat treatment> The heat treatment temperature is usually 1800 to 2100°C, preferably 1900 to 2100°C, and more preferably 2000 to 2100°C. If the heat treatment temperature is lower than this range, the crystallization of h-BN becomes insufficient, and amorphous parts with underdeveloped crystallization remain, resulting in a small effect of improving thermal conductivity when used as a thermally conductive filler. If the heat treatment temperature exceeds the upper limit, the rare earth element oxide evaporates and decomposes, making it impossible to maintain the shell structure, and decomposition of boron nitride may occur.
[0072] The heat treatment time is usually 5 to 20 hours, and preferably 5 to 15 hours. If the heat treatment time is shorter than this range, the crystal growth will be insufficient, and if it is longer than this range, there is a risk of partial decomposition of h-BN.
[0073] In order to carry out the heat treatment under a non-oxidizing gas atmosphere, the inside of the furnace is preferably heated while being evacuated by a vacuum pump, and the evacuation is continued until the amount of decomposition gases caused by heating is reduced, and then the temperature is increased to a desired temperature while introducing a non-oxidizing gas. The temperature at which the evacuation is carried out by the vacuum pump is approximately 200 to 700°C, for example, approximately 600°C, and the degree of vacuum is increased by 10 degrees to the desired temperature. -1The mixture may be heated at a rate of about 20°C / min while maintaining the pressure at about 1 Pa. Thereafter, a non-oxidizing gas is introduced up to atmospheric pressure and continues to be introduced until the end of the heat treatment. The flow rate of the non-oxidizing gas depends on the size of the furnace, but is usually no problem if it is 1 ml / min or more. After the introduction of the non-oxidizing gas, the mixture is heated to about 1100°C at a rate of 20 to 100°C / min, and then heated from 1100°C to a predetermined heat treatment temperature at a rate of 2 to 20°C / min. After heating at this temperature for the above-mentioned heat treatment time, it is preferable to lower the temperature to room temperature at a rate of, for example, about 5 to 50°C / min. Naturally, the method for producing granular boron nitride of the present invention also includes a step of cooling the heat-treated mixture to room temperature.
[0074] The calcination furnace for carrying out the heat treatment may be a batch furnace such as a muffle furnace, a tubular furnace, an atmosphere furnace, or a multipurpose high-temperature furnace, or a continuous furnace such as a rotary kiln, a screw conveyor furnace, a tunnel furnace, a belt furnace, a pusher furnace, or a vertical continuous furnace, and may be used according to the purpose.
[0075] If this heat treatment is carried out in an oxidizing gas atmosphere, most of the boron nitride contained in the boron nitride component (1) will be converted to boron oxide, etc., so it is necessary to carry out the heat treatment in a non-oxidizing gas atmosphere.
[0076] <Washing of Granular Boron Nitride Composition (Production of Granular Boron Nitride)> In the granular boron nitride composition of the present invention obtained as described above, rare earth element oxides and calcium oxide remain. In addition, composite oxides of elements constituting these oxides (calcium yttrium borate (CaYBO4), etc.) and borate compounds (calcium borate (CaB2O4), etc.) may also be contained and remain. Since the thermal conductivity of these residues is often smaller than that of boron nitride, in a preferred embodiment, the thermal conductivity of the granular boron nitride is improved by removing and reducing the residues. Therefore, if necessary, the residues may be removed from the granular boron nitride composition obtained by the above-mentioned method. This removal can be performed by washing the granular boron nitride composition with an acid aqueous solution. In more detail, the oxides are removed by using a reaction that converts the residues into their corresponding water-soluble salts, dissolving the salts in the water present to obtain an aqueous salt solution, and removing this. Examples of the acid used include organic acids and inorganic acids, and for example, hydrochloric acid, nitric acid, sulfuric acid, etc. may be used.
[0077] The washing with the acid aqueous solution can be carried out by dispersing the granular boron nitride composition in the acid aqueous solution under stirring. The composition is then filtered, washed with water to remove the remaining acid, and then dried to obtain granular boron nitride. Calcium oxide and borate compounds (if present) can be easily removed substantially in their entirety by acid washing. The total amount of rare earth element oxides contained in the obtained granular boron nitride is preferably 0.1 to 30%, preferably 1 to 15%, more preferably 3 to 10%, based on the mass of the granular boron nitride. The remaining rare earth element oxides can be easily adjusted by appropriately selecting the washing conditions (e.g., the concentration of the acid, the amount of the aqueous solution used for washing, and / or the number of washings).
[0078] The amount of rare earth oxide in the granular boron nitride composition can be measured as follows: 1 g of the acid-washed granular boron nitride composition was added to 60 g of 1N hydrochloric acid solution in a Teflon-lined pressure vessel, sealed, and treated at 100°C for 11 hours. The resulting slurry was filtered through a membrane filter, and the filtrate was diluted 200 times with pure water to obtain a solution, which was then analyzed for the concentration of rare earth elements (e.g., yttrium) using an ICP (ion inductively coupled plasma) emission spectrometer (Shimadzu Corporation, ICPS-7510), and the amount of rare earth element oxide (e.g., Y2O3) contained in the composition was calculated based on the concentration. The filter cake was also analyzed by XRD to confirm that there was no peak of rare earth element oxide.
[0079] The particles filtered out were confirmed to be granular boron nitride (h-BN) by X-ray diffraction patterns. In addition, SEM observations showed that the c-planes of the boron nitride crystals were bent to form polyhedrons (or roughly spherical shapes). The shell structure of granular boron nitride was investigated using a sample for SEM observation made by adding granular boron nitride to epoxy resin, hardening it, and etching it with an argon ion beam. When granular boron nitride particles are sliced by etching, the stacked c-planes of boron nitride are connected in a circular shape to form a shell, and it can be confirmed by SEM observation that substances other than boron nitride are present within the shell.
[0080] For example, the SEM photograph of the granular boron nitride in the sliced state (granular boron nitride (containing about 8.65% yttrium oxide) obtained in Example 36 (an example in which oxide partially remains) described later) is shown in the upper left of FIG. 8. The results of mapping analysis of the granular boron nitride in this state using EDS (energy dispersive X-ray analysis) are shown in the upper right (N element) and lower left (Y element) of FIG. 8. Combining these mapping results with the SEM photograph, it can be seen that the nitrogen element is present in the polygonal periphery (or approximately circumferential) part (i.e., the ring-shaped part) of the N element, and the Y element is present inside the nitrogen element. From these results, it can be understood that the N element (i.e., boron nitride) forms a shell structure, and Y (i.e., yttrium oxide) is present inside the shell structure. That is, the granular boron nitride of the present invention is composed of a shell part composed of boron nitride, and a rare earth element oxide remaining inside the shell in an amount according to the degree of washing.
[0081] FIG. 9 shows the results of a similar analysis of the granular boron nitride composition of the present invention obtained in Example 11 described later (i.e., before the washing treatment was carried out). The top left of FIG. 9 shows an SEM photograph, the top right shows the EDS mapping results for N element, the bottom left shows the EDS mapping results for Ca element, and the bottom right shows the EDS mapping results for Y element. As in FIG. 8, it can be seen that N element exists in a shell structure around the granular boron nitride crystals, and calcium element and yttrium element exist inside (i.e., oxides of these elements exist). It can also be seen that the amount of oxides is reduced by the washing treatment.
[0082] <Granular boron nitride composition> The granular boron nitride composition of the present invention can be preferably produced by the above-mentioned method for producing the granular boron nitride composition of the present invention, and contains boron nitride, an oxide of at least one rare earth element selected from yttrium, cerium and ytterbium, and calcium oxide, and preferably the boron nitride has a graphite structure. The amount of these oxides can be reduced by acid washing as described above.
[0083] The shell structure of the granular boron nitride composition of the present invention is reinforced by rare earth element oxide and calcium oxide, and as a result, the strength (e.g., crushing strength) when pressure is applied is improved. Therefore, it can be blended into a resin material for the purpose of improving the thermal conduction anisotropy and improving the thermal conductivity. Furthermore, since the solid lubrication derived from the granular boron nitride is maintained, even when it is blended into a resin material, it is possible to maintain good moldability as a resin composition, and when a molded body is produced, a heat conduction path in the thickness direction is easily formed in the molded body due to the shell structure. As a result, the thermal conductivity in the thickness direction of the molded body can be increased. In addition, the granular boron nitride of the present invention also has chemical stability, heat resistance, etc. derived from boron nitride.
[0084] When the boron nitride component contains oxygen, the oxygen is generally contained as boron oxide (B2O3). In this case, the boron oxide reacts with the rare earth element oxide and calcium oxide to become an oxide (e.g., a complex oxide such as CaYBO4) and form a liquid phase. When a heat treatment is carried out in the manufacturing method of the granular boron nitride composition of the present invention, this oxide forms a liquid phase in which the boron nitride contained in the boron nitride component (1) dissolves, similar to the rare earth element oxide and calcium oxide. It is considered that the shell structure can be strengthened when granular boron nitride is generated during recrystallization of boron nitride. Note that, similar to the rare earth element oxide, the above-mentioned complex oxide can also be reduced depending on the conditions of washing with an acid, and the amount can be substantially entirely removed.
[0085] The content of rare earth element oxide in the granular boron nitride composition of the present invention, when the above-mentioned washing is not performed (i.e., when only the heat treatment and the subsequent cooling are performed), is substantially equal to the sum of the amounts of rare earth element oxide and oxide derived from its precursor (if the precursor is present) contained in the mixture heat-treated in the above-mentioned method for producing a granular boron nitride composition of the present invention, and the content of calcium oxide is similarly substantially equal to the sum of the amounts of calcium oxide and oxide derived from calcium carbonate (if the precursor is present) contained in the mixture heat-treated. Usually, the boron nitride content of the granular boron nitride composition is preferably 40 to 95%, more preferably 50 to 90%, for example 55 to 85%, based on the total mass of boron nitride, rare earth element oxide and calcium oxide in the granular boron nitride composition.
[0086] <Resin composition containing granular boron nitride> The resin composition of the present invention, particularly a thermally conductive resin composition, comprises the above-mentioned granular boron nitride of the present invention and a resin material. That is, as described above, the granular boron nitride of the present invention is suitably used as a thermally conductive filler in the resin composition. In some cases, it is also possible to use a granular boron nitride composition instead of the granular boron nitride.
[0087] <Resin materials> The resin material that functions as the resin that will form the matrix in the resin composition is not particularly limited, and may be, for example, a curable resin, a thermoplastic resin, etc. The curable resin may be any crosslinkable resin such as a thermosetting, photocurable, or electron beam curable resin, but in terms of heat resistance, water absorption, dimensional stability, etc., a thermosetting resin is preferred, and an epoxy resin is particularly optimal.
[0088] The epoxy resin may be an epoxy resin having only one type of structural unit, or a combination of multiple epoxy resins having different structural units. The epoxy resin may be used together with an epoxy resin curing agent and a curing accelerator, if necessary.
[0089] Here, in order to reduce voids in the cured product and obtain a cured product with high thermal conductivity in addition to coatability or film-forming property and adhesiveness, it is preferable that the epoxy resin contains at least a phenoxy resin (hereinafter referred to as "epoxy resin (A)") described below. In particular, the mass ratio of epoxy resin (A) to the total amount of epoxy resins is preferably in the range of 5 to 95 mass%, more preferably 10 to 90 mass%, and even more preferably 20 to 80 mass%, but is not limited to these amounts.
[0090] The phenoxy resin generally refers to a resin obtained by reacting epihalohydrin with a dihydric phenol compound, or a resin obtained by reacting a divalent epoxy compound with a dihydric phenol compound, but in the present invention, among these, a phenoxy resin that is a high molecular weight epoxy resin having a mass average molecular weight of 10,000 or more is referred to as epoxy resin (A). The mass average molecular weight is a value measured by gel permeation chromatography in terms of polystyrene.
[0091] As the epoxy resin (A), a phenoxy resin having at least one skeleton selected from the group consisting of a naphthalene skeleton, a fluorene skeleton, a biphenyl skeleton, an anthracene skeleton, a pyrene skeleton, a xanthene skeleton, an adamantane skeleton, and a dicyclopentadiene skeleton is preferred. Among them, a phenoxy resin having a fluorene skeleton and / or a biphenyl skeleton is particularly preferred because it further enhances heat resistance. These may be used alone or in combination of two or more.
[0092] The epoxy resin other than the epoxy resin (A) is preferably an epoxy resin having two or more epoxy groups in the molecule (hereinafter, sometimes referred to as "epoxy resin (B)"). For example, various epoxy resins such as bisphenol A type epoxy resin, bisphenol F type epoxy resin, naphthalene type epoxy resin, phenol novolac type epoxy resin, cresol novolac type epoxy resin, phenol aralkyl type epoxy resin, biphenyl type epoxy resin, triphenylmethane type epoxy resin, dicyclopentadiene type epoxy resin, glycidyl ester type epoxy resin, glycidyl amine type epoxy resin, polyfunctional phenol type epoxy resin, etc. These may be used alone or in combination of two or more.
[0093] From the viewpoint of controlling the melt viscosity, the epoxy resin (B) has a mass average molecular weight of preferably 100 to 5000, more preferably 200 to 2000. If the mass average molecular weight is less than 100, the heat resistance tends to be poor, and if it is more than 5000, the melting point of the epoxy resin tends to be high, and the workability tends to be reduced.
[0094] Furthermore, the epoxy resin according to the present invention may contain an epoxy resin (hereinafter, "other epoxy resin") other than the epoxy resin (A) and the epoxy resin (B) within a range that does not impair the object of the present invention. The content of the other epoxy resin is usually 50 mass % or less, preferably 30 mass % or less, based on the total of the epoxy resin (A) and the epoxy resin (B).
[0095] In the resin composition of the present invention, the proportion of the epoxy resin (A) in the total epoxy resins including the epoxy resin (A) and the epoxy resin (B) is, as described above, preferably 5 to 95 mass%, preferably 10 to 90 mass%, and more preferably 20 to 80 mass%, with the total being 100 mass%. Note that, "total epoxy resins including the epoxy resin (A) and the epoxy resin (B)" means the total of the epoxy resin (A) and the epoxy resin (B) when the epoxy resins contained in the resin composition of the present invention are only the epoxy resin (A) and the epoxy resin (B), and means the total of the epoxy resin (A), the epoxy resin (B), and the other epoxy resins when the epoxy resins further contain other epoxy resins.
[0096] By having the proportion of epoxy resin (A) equal to or greater than the lower limit, the effect of improving thermal conductivity by blending epoxy resin (A) can be fully obtained, and the desired high thermal conductivity can be obtained. By having the proportion of epoxy resin (A) equal to or less than the upper limit, and in particular by having epoxy resin (B) account for 10 mass% or more of the total epoxy resins, the effect of blending epoxy resin (B) can be fully obtained, and the curing property and physical properties of the cured product can be sufficiently obtained.
[0097] The epoxy resin curing agent may be appropriately selected according to the type of resin used. For example, an acid anhydride curing agent or an amine curing agent may be used. Examples of the acid anhydride curing agent include tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, hexahydrophthalic anhydride, and benzophenonetetracarboxylic anhydride. Examples of the amine curing agent include aliphatic polyamines such as ethylenediamine, diethylenetriamine, and triethylenetetramine, aromatic polyamines such as diaminodiphenylsulfone, diaminodiphenylmethane, diaminodiphenylether, and m-phenylenediamine, and dicyandiamide. These may be used alone or in combination of two or more. These epoxy resin curing agents are usually mixed with the epoxy resin in an equivalent ratio of 0.3 to 1.5.
[0098] The curing accelerator may be appropriately selected according to the type of resin or curing agent used. For example, the curing accelerator for the acid anhydride curing agent may be, for example, boron trifluoride monoethylamine, 2-ethyl-4-methylimidazole, 1-isobutyl-2-methylimidazole, or 2-phenyl-4-methylimidazole. These may be used alone or in combination of two or more. These curing accelerators are usually used in the range of 0.1 to 5 parts by mass per 100 parts by mass of the epoxy resin.
[0099] The resin material used in the resin composition of the present invention may be a thermoplastic resin. Examples of the thermoplastic resin include polyolefin resins such as polyethylene resin, polypropylene resin, and ethylene-vinyl acetate copolymer resin, polyester resins such as polyethylene terephthalate resin, polybutylene terephthalate resin, and liquid crystal polyester resin, polyvinyl chloride resin, phenoxy resin, acrylic resin, polycarbonate resin, polyphenylene sulfide resin, polyphenylene ether resin, polyamide resin, polyamideimide resin, polyimide resin, polyetheramideimide resin, polyetheramide resin, and polyetherimide resin. Also included are copolymers such as block copolymers and graft copolymers thereof. These may be used alone or in combination of two or more.
[0100] The resin material may be a rubber component, and examples of the rubber component include natural rubber, polyisoprene rubber, styrene-butadiene copolymer rubber, polybutadiene rubber, ethylene-propylene copolymer rubber, ethylene-propylene-diene copolymer rubber, butadiene-acrylonitrile copolymer rubber, isobutylene-isoprene copolymer rubber, chloroprene rubber, silicone rubber, fluororubber, chlorosulfonated polyethylene, polyurethane rubber, etc. These may be used alone or in combination of two or more.
[0101] <Amount of granular boron nitride> The amount of the granular boron nitride (or granular boron nitride composition) of the present invention contained in the resin composition of the present invention is, as described above, preferably 10 to 90% by mass of the resin composition, more preferably 15 to 88%, and even more preferably 30 to 85%. If the amount of granular boron nitride in the resin composition is less than this range, the viscosity of the resin composition (viscosity when melted) is low, and although the molding processability is good, the effect of improving thermal conductivity may be insufficient. If the amount of granular boron nitride in the resin composition is greater than this range, the viscosity of the resin composition when melted increases, and molding tends to become difficult.
[0102] <Other ingredients> The resin composition of the present invention may contain other components as long as the effect of the present invention can be obtained.Such components include functional resins obtained by imparting functionality to the above-mentioned resins such as liquid crystal epoxy resins, nitride particles such as aluminum nitride, silicon nitride, and fibrous boron nitride, insulating metal oxides such as alumina, fibrous alumina, zinc oxide, magnesium oxide, beryllium oxide, and titanium oxide, insulating carbon components such as diamond and fullerene, resin curing agents, resin curing accelerators, viscosity modifiers, and dispersion stabilizers.
[0103] In addition, from the viewpoint of decreasing the viscosity of the resin composition, the resin composition of the present invention may contain a solvent. As the solvent, a known solvent that dissolves a resin is used. Examples of such a solvent include methyl ethyl ketone, acetone, cyclohexanone, toluene, xylene, monochlorobenzene, dichlorobenzene, trichlorobenzene, phenol, and hexafluoroisopropanol. These may be used alone or in combination of two or more. The solvent is used in an amount of, for example, 0 to 10,000 parts by mass relative to 100 parts by mass of a resin such as an epoxy resin.
[0104] Furthermore, the resin composition of the present invention may contain inorganic fillers such as aluminum hydroxide and magnesium hydroxide, surface treatment agents such as silane coupling agents that improve the interfacial adhesive strength between the inorganic filler and the matrix resin, reducing agents, and the like, as long as the effects of the composition are not impaired.
[0105] With regard to the inorganic filler, the total amount of the particulate boron nitride of the present invention and the inorganic filler in the resin composition is preferably 90 mass % or less, in order to maintain moldability in the resin composition.
[0106] <Production and molding of resin compositions> The resin composition of the present invention can be obtained by uniformly mixing the granular boron nitride (or granular boron nitride composition) of the present invention, a resin material, and other components added as necessary by stirring or kneading. For the mixing, a general kneading device such as a mixer, a kneader, or a single-screw or twin-screw kneader can be used, and heating may be performed as necessary during mixing.
[0107] <Molded body> The molded article of the present invention is obtained by molding the resin composition of the present invention. The molding method of the molded article can be a method generally used for molding the resin composition, such as injection molding or mold molding, depending on the properties of the resin composition. In any molding method, the resin composition is heated as necessary to be fluidized or plasticized, and the resin composition is molded into a molded article using a mold or the like, so that some force acts on the fluidized resin composition. For example, pressure acts when the resin composition is filled into a mold. This is considered to apply whether the resin material is a curable resin (e.g., phenolic resin, epoxy resin, melamine resin, urea resin, etc.) or a thermoplastic resin (e.g., polyethylene, polypropylene, polyvinyl chloride, polystyrene, acrylic resin, etc.).
[0108] For example, when the resin composition of the present invention has plasticity and fluidity, the resin composition can be molded into a desired shape, for example, by curing the resin composition in a state filled in a mold. As a method for producing such a molded body, injection molding, injection compression molding, extrusion molding, and compression molding can be used. In addition, when the resin composition of the present invention is a thermosetting resin composition such as an epoxy resin or a silicone resin, the molding of the molded body, i.e., curing, can be performed under curing conditions according to each composition. Furthermore, when the resin composition of the present invention is a thermoplastic resin composition, the molding of the molded body can be performed at a temperature equal to or higher than the melting temperature of the thermoplastic resin and at a predetermined molding speed and pressure. The molded body of the present invention can also be obtained by cutting out the resin composition of the present invention into a desired shape from a solid bulk material molded or cured.
[0109] In the molded article of the present invention obtained as described above, although it depends on the blending amounts of resin material and granular boron nitride (or granular boron nitride composition), in one embodiment of a resin composition in which the amount of resin material is 65 to 85% by mass, the thermal conductivity in the direction parallel to the direction in which force is applied during molding is usually 10 to 25 W / (m·K), preferably 15 to 23 W / (m·K), more preferably 18 to 22 W / (m·K). Also, the thermal conductivity in the direction perpendicular to the direction in which pressure is applied during molding is usually 15 to 35 W / (m·K), preferably 20 to 30 W / (m·K), more preferably 22 to 27 W / (m·K).
[0110] Therefore, when a resin composition is prepared using the granular boron nitride of the present invention and then molded to produce a molded body, the thermal conductivity in the parallel direction is generally preferably 70 to 120%, more preferably 80 to 110%, and particularly 90 to 105% of the thermal conductivity in the perpendicular direction, and the anisotropy of the molded body with respect to thermal conduction can be significantly suppressed, and in some cases, the anisotropy can be substantially eliminated. This tendency also applies when a molded body is obtained by mixing the granular nitrogen composition of the present invention with a resin material instead of granular boron nitride, in that the thermal conductivity in the parallel direction is similarly smaller than the thermal conductivity in the perpendicular direction. That is, anisotropy can be suppressed even when the granular boron nitride contains an oxide, particularly a rare earth element oxide, a Ca-rare earth element-BO composite oxide, etc. In a particularly preferred embodiment, the resin composition contains 65 to 85 mass% of granular boron nitride, and in that case, the ratio of the thermal conductivity in the parallel direction to the thermal conductivity in the perpendicular direction is at least about 90 to 105%. EXAMPLES
[0111] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to such examples.
[0112] [Raw materials used] The specifications of the raw materials used in the following Examples and Comparative Examples are as follows. <Boron nitride component (1)> Boron nitride powder: Mitsui Chemicals, Inc., product name: MBN-250 (Total oxygen concentration: 4% by mass, average particle size: 1.8 μm) <Rare Earth Components (2)> Fine yttrium oxide powder: Manufactured by Japan Yttrium Co., Ltd. Y2O399.9%, average particle size 0.91μm Fine powdered cerium oxide: manufactured by Nippon Yttrium Co., Ltd. CeO299.9%, average particle size 0.58μm <Calcium component (3)> Powdered calcium oxide: manufactured by Adachi Lime Industry Co., Ltd. CaO 98.5%, average particle size 150μm <Epoxy resin materials> Epoxy resin: Mitsubishi Chemical Corporation, product name: JER828, Epoxy resin hardener: Mitsubishi Chemical Corporation, product name: YH306 Epoxy curing accelerator: Mitsubishi Chemical Corporation, product name: EMI24 Mixing ratio (mass basis) JER828:YH306:EMI24=100:80:2
[0113] [Production of granular boron nitride composition and granular boron nitride] <Example 1> To a 300 ml beaker, 20 g of boron nitride powder as the boron nitride component (1), 1.70 g of Y2O3 powder (3.6 vol. % of the total amount of mixed powder before heat treatment) as the rare earth component (2), and 0.42 g of CaO powder (1.4 vol. % of the total amount of mixed powder before heat treatment) as the calcium component (3) were added, and 150 ml of ethanol was further added. In order to mix uniformly, ultrasonic treatment was performed for 5 minutes using an ultrasonic homogenizer (IKA U200 Controls) to obtain a slurry of the mixture.
[0114] The ethanol in the resulting slurry was removed using an evaporator, and a dried powder was obtained as a mixture. This powder was placed in a boron nitride crucible and heat-treated using a multipurpose high-temperature furnace (Fuji Denpa Kogyo Co., Ltd., Hi-Multi 5000) to obtain a granular boron nitride composition. In addition to boron nitride, this composition contained Ca-YBO-based composite oxides such as CaYBO4. It is believed that the BO in this composite oxide is derived from the boron nitride powder used as the raw material containing 4% by weight of oxygen.
[0115] The heat treatment was performed by increasing the temperature from room temperature to 1100°C at 20°C / min, then increasing the temperature from 1100 to 1900°C at 10°C / min, holding at 1900°C for 10 hours, and then decreasing the temperature to room temperature at 20°C / min. The heat treatment atmosphere was 1×10 -1 The furnace was then maintained at a vacuum of less than 1 Pa, and nitrogen gas was then introduced into the furnace up to atmospheric pressure, with the nitrogen gas flow rate maintained at 1 ml / min until the end of the heat treatment.
[0116] The mixture was heat-treated as described above to obtain a granular boron nitride composition of the present invention. The obtained composition was then washed to remove the oxides contained therein (yttrium oxide, calcium oxide). In detail, 2.5 g of the composition was added to 20 ml of 3N hydrochloric acid solution in a Teflon-lined sealed pressure vessel, and the mixture was reacted at 100°C for 11 hours to convert the oxides contained therein into water-soluble salts. The mixture was then washed with pure water and filtered to remove the salts, obtaining the granular boron nitride of the present invention. When the obtained granular boron nitride was subjected to XRD analysis, any remaining yttrium oxide and calcium oxide could not be detected.
[0117] <Examples 2 to 6> The amount of Y2O3 added in Example 1 was 3.59 g (Example 2: 7.3 vol% of the total amount of mixed powder before heat treatment), 5.70 g (Example 3: 10.9 vol% of the total amount of mixed powder before heat treatment), 8.07 g (Example 4: 14.6 vol% of the total amount of mixed powder before heat treatment), 10.76 g (Example 5: 18.2 vol% of the total amount of mixed powder before heat treatment), and 13.84 g (Example 6: 21.9 vol% of the total amount of mixed powder before heat treatment). Granular boron nitride of the present invention was obtained by repeating Example 1, except that the amount of added was changed to 0.89 g (Example 2: 2.7 vol% of the total amount of mixed powder before heat treatment), 1.41 g (Example 3: 4.1 vol% of the total amount of mixed powder before heat treatment), 2.00 g (Example 4: 5.4 vol% of the total amount of mixed powder before heat treatment), 2.67 g (Example 5: 6.8 vol% of the total amount of mixed powder before heat treatment), and 3.44 g (Example 6: 8.1 vol% of the total amount of mixed powder before heat treatment). When the obtained granular boron nitride was subjected to XRD analysis, any remaining yttrium oxide and calcium oxide could not be detected.
[0118] In addition, in Examples 1 to 6, the ratio of the total volume of the oxides, Y2O3 and CaO, contained in the mixture powder before heat treatment to the volume of the mixture was 5 vol.% in Example 1, 10 vol.% in Example 2, 15 vol.% in Example 3, 20 vol.% in Example 4, 25 vol.% in Example 5, and 30 vol.% in Example 6.
[0119] <Examples 7 to 24> Granular boron nitride of the present invention was obtained by repeating Example 1 except for the conditions shown in Table 1 below. In Examples 7 to 12, the molar ratio of yttrium oxide and calcium oxide constituting the mixture was 1:2, in Examples 13 to 18, the molar ratio of yttrium oxide and calcium oxide constituting the mixture was 1:4, and in Examples 19 to 24, the molar ratio of yttrium oxide and calcium oxide constituting the mixture was 1:6.
[0120] <Example 25> The procedure of Example 1 was repeated except that 1.97 g of CeO2 powder was added instead of yttrium oxide and 0.64 g of CaO powder was used, and the composition was heated to obtain a granular boron nitride composition of the present invention, which was then washed to remove oxides to obtain granular boron nitride of the present invention. XRD analysis of the obtained granular boron nitride revealed that no residual cerium oxide or calcium oxide was detected.
[0121] <Examples 26 to 30> In Example 25, the amount of CeO2 added was 4.15 g (Example 26: 5.9 vol% of the total amount of mixed powder before heat treatment), 6.59 g (Example 27: 8.8 vol% of the total amount of mixed powder before heat treatment), 9.34 g (Example 28: 11.8 vol% of the total amount of mixed powder before heat treatment), 12.45 g (Example 29: 14.7 vol% of the total amount of mixed powder before heat treatment), and 16.01 g (Example 30: 17.6 vol% of the total amount of mixed powder before heat treatment). Granular boron nitride of the present invention was obtained by repeating Example 25, except that the amount of added was changed to 1.35 g (Example 26: 4.1 vol.% of the total amount of mixed powder before heat treatment), 2.15 g (Example 27: 6.2 vol.% of the total amount of mixed powder before heat treatment), 3.04 g (Example 28: 8.2 vol.% of the total amount of mixed powder before heat treatment), 4.06 g (Example 29: 10.3 vol.% of the total amount of mixed powder before heat treatment), and 5.22 g (Example 30: 12.4 vol.% of the total amount of mixed powder before heat treatment).
[0122] In addition, in the above Examples 25 to 30, the ratio of the total volume of the oxides, CeO2 and CaO, contained in the mixed powder before heat treatment to the volume of the mixture was 5 vol.% in Example 25, 10 vol.% in Example 26, 15 vol.% in Example 27, 20 vol.% in Example 28, 25 vol.% in Example 29, and 30 vol.% in Example 30.
[0123] <Examples 31 to 38> 3 g of the granular boron nitride composition containing the oxide after the heat treatment obtained in Example 3 was added to 65 ml of 3N hydrochloric acid solution, stirred for 11 hours at 25°C using a stirrer, filtered and dried to obtain a powder of a granular boron nitride composition from which calcium oxide components had been partially removed. The obtained powder was then added to 10 ml of 0.6N hydrochloric acid solution, and reacted for 11 hours at 100°C in a Teflon-lined sealed container to convert most of the contained oxides into water-soluble salts. Thereafter, the mixture was washed with pure water and filtered to remove the salts in the same manner as above to obtain the granular boron nitride of the present invention. In this acid treatment, the hydrochloric acid concentration used at 100°C was reduced compared to Example 3, so that Y2O3 partially remained, but other components were substantially removed. 1 g of the granular boron nitride obtained after filtration was added to 20 ml of 1N hydrochloric acid solution, and reacted in a Teflon-lined sealed container at 100°C for 11 hours. The filtrate was quantitatively analyzed by ICP and found to contain 1.01 mass% yttrium oxide, but the amount of calcium oxide was below the detection limit. Similarly, the granular boron nitride compositions containing the oxides after heat treatment obtained in Examples 4, 6, 9, 11, 12, 18, and 24 were similarly treated to obtain the granular boron nitride of the present invention in Examples 32 to 38, respectively.
[0124] <Comparative Example 1> In a 300 ml beaker, 20 g of boron nitride powder and 2.32 g of Y2O3 powder (5% by volume of the total mixed powder before heat treatment) were added, and 150 ml of ethanol was further added. In order to mix uniformly, an ultrasonic homogenizer (IKA U200 Controls) was used to perform ultrasonic treatment for 5 minutes to obtain a slurry of the mixture. The ethanol solvent of the obtained slurry was removed with an evaporator, and a dried powder was obtained as a mixture. This powder was subjected to a heat treatment of the mixture and then washed in the same manner as in Example 1 to obtain boron nitride.
[0125] <Comparative Examples 2 to 6> Comparative Example 1 was repeated, varying the amount of Y2O3 powder added.
[0126] <Comparative Example 7> Based on the description in JP 2017-14064, 44.41 g of H3BO3 powder (Wako Pure Chemical Industries, Ltd., special grade reagent), 12.48 g of CaO, and 200 ml of distilled water were added to a glass bottle (volume 250 ml) with a lid (CaO / B2O3 molar ratio = 0.62), the bottle was closed, and the mixture was stirred in an oil bath at 95°C for 2 hours to obtain Ca2B2O5·H2O and Ca3B 20 O 33 48.0 g of a mixture of composite oxides of H2O and H3BO3 was synthesized. 9.2 g of carbon powder (2300B manufactured by Mitsubishi Chemical Corporation) was added to this mixture so that the element ratio B / C was 0.79 relative to the B in the raw material H3BO3, and the mixture was mixed in a ball mill to obtain a powder mixture. The mixture was then heated and washed in the same manner as in Example 1 to obtain a multifaceted boron nitride structure.
[0127] <Comparative Example 8> Raw materials used A compact was produced using commercially available platelet-shaped boron nitride as the thermally conductive filler as follows: [Boron nitride component] Plate-shaped boron nitride powder: manufactured by Denki Kagaku Kogyo Co., Ltd., product name: Denka Boron Nitride GP (Total oxygen concentration: 0.1% by mass, average particle size: 8.0 μm, specific surface area: 8 m 2 / g) Boron nitride was added and mixed with an epoxy resin material to obtain a resin composition. The composition of the resin composition was 81.7% by mass (70% by volume) of granular boron nitride and 18.3% by mass (30% by volume) of epoxy resin material. The processing conditions not specifically mentioned were the same as those in the comparative example.
[0128] <Production of resin composition and molded article> The granular boron nitride of the present invention obtained in Examples 1 to 30 and the boron nitride obtained in Comparative Examples 1 to 7 were each added to and mixed with an epoxy resin material to obtain a resin composition. The composition of the resin composition on a mass basis was 81.7% (70% by volume) of granular boron nitride and 18.3% (30% by volume) of the epoxy resin material.
[0129] Specifically, 1.0 g of the obtained boron nitride, 0.1229 g of bisphenol A type liquid epoxy (base agent) (JER828, manufactured by Mitsubishi Chemical Corporation), 0.0983 g of tetrahydromethylphthalic anhydride (curing agent) (YH306, manufactured by Mitsubishi Chemical Corporation), 0.00246 g of 2-ethyl-4(5)-methylimidazole (curing accelerator) (EMI-24, manufactured by Mitsubishi Chemical Corporation), and 20 g of acetone (Saito, special grade, manufactured by Wako Pure Chemical Industries, Ltd.) were added to a 100 ml eggplant-shaped flask and mixed for 5 minutes using an ultrasonic homogenizer.
[0130] Next, the acetone was removed using an evaporator. After the removal, 0.8 g of the mixture containing the granular boron nitride and the epoxy resin material remaining in the eggplant-shaped flask as a resin composition was placed in a 15 mm diameter mold and hot pressed to thermally cure the resin composition, thereby obtaining a molded product.
[0131] The hot pressing conditions are as follows: Regarding boron nitride in Comparative Examples 1 to 6, Examples 1 to 4, 7 to 10, 13 to 16, 19 to 22, and 25 to 28 Hot pressing at 125℃ for 120 minutes under uniaxial pressure of 70MPa Regarding boron nitride in Comparative Example 7 and Examples 5, 6, 11, 12, 17, 18, 23, 24, 29, and 30 Hot pressing at 125°C under uniaxial pressure of 5 MPa for 60 minutes, followed by hot pressing for 60 minutes at a pressure of 70 MPa.
[0132] <Measurement of thermal conductivity of molded body> The density, specific heat and thermal diffusivity of the obtained molded body were measured, and the thermal conductivity of the molded body was calculated based on the following formula: Thermal conductivity = density x specific heat x thermal diffusivity
[0133] <Density measurement> The epoxy / boron nitride compact was measured by the Archimedes method in water, and the density was calculated by the following (Equation 1):
[0134]
number
[0135] <Measurement of specific heat> Using a differential scanning calorimeter (Netzsch DSC200F3 Maia), a constant heat was applied to a known reference material (sapphire in this measurement) and a molded body as a sample, and their temperatures were measured, and the temperature difference was measured to perform thermal analysis and obtain the specific heat. The specific heat of the sample was calculated using the following formula (2). The temperature measurement range was -50°C to 100°C, and the specific heat at 25°C, which is the same measurement temperature as the thermal diffusivity below, was used to calculate the thermal conductivity.
[0136]
number
[0137] <Measurement of thermal diffusivity> The thermal constants were measured using a xenon flash method thermal constant measurement device (Netzsch Xe Flash Analyzer LFA447 Nanoflash). Thermal conductivity (α) was calculated by irradiating a heat source onto the front surface of a molded body sample, measuring the temperature on the back surface, and calculating the time t 1 / 2 (s) and the sample thickness L (m) are calculated using the following formula (3):
[0138]
number
[0139] The thermal conductivity of the molded body was measured in the direction of pressure applied during hot pressing (pressing direction) and in a direction perpendicular thereto.
[0140] <Measurement of the degree of orientation of granular boron nitride in a green body> The strength of granular boron nitride (more specifically, its ability to resist external forces applied to granular boron nitride, i.e., its crushing strength) was evaluated by examining the degree of orientation of the (00L) plane of granular boron nitride in the epoxy resin material of a molded body obtained by hot pressing at a pressure of 70 MPa.
[0141] If the strength of the shell structure of the granular boron nitride contained in the compact is insufficient, the hot pressing will cause part of the shell structure to collapse, weakening the shell structure of the granular boron nitride and strengthening the layered structure. As a result, the a-axis of the broken boron nitride platelet crystals tends to be oriented perpendicular to the hot pressing direction, and the diffraction peaks of the (00L) planes of the boron nitride crystals, such as (002) and (004), will become higher.
[0142] That is, the height of the diffraction peak of the boron nitride (00L) plane can be used to estimate whether the platelet crystals of boron nitride are oriented parallel to the pressing direction. That is, if the crushing strength of granular boron nitride is insufficient, parts of the shell structure will break and the fragments will tend to line up in the pressing direction. In other words, the greater the proportion of fragments aligned in the pressing direction, the weaker the strength.
[0143] The degree of orientation of the boron nitride (00L) plane in the compact after hot pressing was measured by measuring the XRD diffraction pattern of the plane perpendicular to the pressing direction (i.e., the hot pressed surface or the pressed surface) using the Lotgering method, and was calculated using the following equation (4):
[0144]
number
[0145] The Lotgering method is a method for evaluating the degree of orientation of crystals, etc., using the degree of orientation (also called the Lotgering factor) calculated by formula (4). The Lotgering factor is 100% in the case of perfect orientation. In this formula (4), ΣI(hkl) is the sum of the X-ray diffraction intensities of all crystal planes (hkl) measured on a plane perpendicular to the pressing direction for a sample of a compact containing aggregates, and ΣI0(hkl) is the sum of the X-ray diffraction intensities of all crystal planes (hkl) measured for a sample of a compact obtained when non-oriented boron nitride is used instead of granular boron nitride. In addition, ΣI(00L) is the sum of X-ray diffraction intensities of crystallographically equivalent specific crystal faces (e.g., (00L) faces including (002) and (004) faces) measured for a molded body including aggregates, and ΣI0(00L) is the sum of X-ray diffraction intensities of the crystal faces of the (00L) faces measured for a non-oriented material having the same composition as the hybrid material of a specific face when the above-mentioned non-oriented boron nitride is used. The Lotgering method for evaluating the degree of orientation in this way is well known as a method for evaluating the degree of orientation of crystals, and reference can be made to, for example, JP 2011-37695 A.
[0146] <Conditions and Measurement Results of the Example> The conditions and various measurement results of the above-mentioned Examples and Comparative Examples are shown in the following Tables 1 to 5.
[0147] [Table 1]
[0148] [Table 2]
[0149] [Table 3]
[0150] [Table 4]
[0151] [Table 5]
[0152] The granular boron nitride obtained in each of the Examples has a considerably larger average particle size than the boron nitride of Comparative Examples 1 to 6 not using a calcium component, but the specific surface area is slightly smaller. The thermal conductivity of the molded body of the present invention obtained by molding the resin composition of the present invention using such granular boron nitride as a thermally conductive filler can achieve about 10 to 25 W / (m·K) in the direction in which force is applied, and 15 to 35 W / (m·K) in the direction perpendicular thereto. This thermal conductivity is higher than that of the molded body obtained by using the known granular boron nitride as a filler in the Comparative Example. Such a high thermal conductivity means that the granular boron nitride can form an effective heat conduction path due to its large particle size.
[0153] In the molded body of the present invention, the thermal conductivity in the parallel direction is at least about 60% of the thermal conductivity in the perpendicular direction, and the anisotropy of the thermal conductivity of the molded body containing this granular boron nitride is suppressed. In some cases, the particle size and the result may exceed 100%, and the anisotropy of the thermal conductivity may not be substantially observed.
[0154] The degree of orientation of granular boron nitride in a molded body affects the thermal conductivity of the molded body. Boron nitride that has become plate-like due to the force applied by the press during molding (or boron nitride that is originally plate-like) has a strong tendency to be oriented in a direction that is not parallel to the press direction, especially in a direction perpendicular to the press direction, and line up in the resin, so that the thermal conductivity in the direction parallel to the press direction during molding is significantly reduced, resulting in increased thermal conductivity anisotropy. For example, since commercially available plate-like particles are added to Comparative Example 8, the degree of orientation is high and the thermal conductivity in the direction parallel to the press direction is low.
[0155] In Comparative Example 7, instead of using plate-shaped boron nitride particles, synthetic polyhedral boron nitride particles are added. However, since the cohesive force of boron nitride crystals is weak, it is considered that the polyhedral structure collapses into plate-shaped boron nitride due to the force applied by press molding, and the plate-shaped boron nitride is oriented. Therefore, as in Comparative Example 8, it is considered that the thermal conductivity along the direction parallel to the press direction is low due to press molding.
[0156] The granular boron nitride produced in this embodiment uses rare earth oxide in the manufacturing method. Since rare earth oxide promotes the dissolution and reprecipitation of boron nitride, it is considered that it brings about a stronger cohesion force than the boron nitride having a polyhedral structure of Comparative Example 7 produced by adding only conventional alkaline earth oxide. In particular, it is considered that the shell part of the granular boron nitride produced in this embodiment tends to form a polyhedron or sphere from the integrated plate-like boron nitride, which is considered to be a factor in increasing the strength of the granular boron nitride. As a result, it is difficult to collapse against the force applied by press molding and convert to plate-like boron nitride. Therefore, the orientation degree of the molded body obtained by press molding using this is considerably smaller than the orientation degrees of Comparative Examples 7 and 8.
[0157] Furthermore, the inventors' investigations have shown that the higher the ratio of rare earth element oxides such as Y2O3 in the oxides in the mixture to be heat treated, the thicker the shell layer tends to be compared to the diameter of the granular boron nitride. This is thought to be the reason why the granular boron nitride of the present invention has a strong shape retention ability.
[0158] The granular boron nitride contained in the granular boron nitride particle composition contains an oxide therein before being washed with an acid. By changing the degree of acid washing, for example by lowering the acid concentration used for washing, the amount of rare earth element oxide remaining therein can be changed. If an oxide remains in the granular boron nitride, it is expected that the strength of the shell structure of the boron nitride formed, particularly the compressive strength, can be improved. That is, when a resin composition is obtained using such granular boron nitride and this is molded by hot pressing, it is considered that the granular boron nitride becomes difficult to collapse, and the orientation degree of the (00L) plane of the molded body becomes low. The results shown in Table 5 are in line with this idea, and from this viewpoint, the granular boron nitride of the present invention preferably contains 0.5 to 15 mass %, more preferably 3 to 10 mass %, particularly 4 to 8 mass % of rare earth element oxide.
[0159] Therefore, the resin composition of the present invention and a molded article produced by molding the composition can be suitably used as a thermally conductive filler in, for example, heat dissipation sheets, thermally conductive pastes, thermally conductive adhesives, and the like, which require thermal conductivity in the electrical and electronic fields.
[0160] This application claims priority to Japanese Patent Application No. 2019-064120 (filing date: March 28, 2019, title of invention: granular boron nitride manufacturing method and granular boron nitride), and by citing this patent application herein, the contents of this patent application constitute the specification of this application.
Claims
1. (1) a boron nitride component comprising boron nitride; (2) a rare earth component comprising an oxide and / or a precursor compound of at least one rare earth element selected from yttrium, cerium, and ytterbium; and ((3) Calcium component comprising calcium oxide and / or calcium carbonate The method includes a step of heat-treating the mixture comprising the steps of: The heat treatment comprises heating the mixture at 1800 to 2100° C. for 5 to 20 hours.
2. 2. A method for producing a granular boron nitride composition as described in claim 1, characterized in that the ratio of the total mass of the rare earth element oxide in the rare earth component (2) and the calcium oxide in the calcium component (3) to the total mass of boron nitride in the boron nitride component (1), the rare earth element oxide in the rare earth component (2), and the calcium oxide in the calcium component (3) contained in the mixture to be heat treated is 5% to 60%.
3. A method for producing a granular boron nitride composition according to claim 1 or 2, characterized in that the ratio of rare earth elements in the rare earth component (2) to calcium elements in the calcium component (3), based on the number of elements in the mixture to be heat treated, is 1:0.25 to 1:
4.
4. 4. The method for producing a granular boron nitride composition according to claim 1, wherein the boron nitride component (1) contains 5% by mass or less of oxygen.
5. Average particle size is 10-25 μm, specific surface area (calculated using the BET multipoint method) is 2-10 m 2 1. A granular boron nitride composition comprising: a granular boron nitride having a shell structure with a surface roughness of 100 nm / g; and an oxide of at least one rare earth element selected from yttrium, cerium, and ytterbium.
6. 6. The granular boron nitride composition according to claim 5, wherein the granular boron nitride has a shell structure with an aspect ratio of 1-3.
7. 7. The granular boron nitride composition according to claim 5, which contains, by mass, 3 to 40% of rare earth element oxide and 1 to 30% of calcium oxide.
8. A method for producing granular boron nitride, comprising treating a granular boron nitride composition obtained by the method for producing a granular boron nitride composition according to any one of claims 1 to 4 with acid washing to remove oxides.
9. 9. The method for producing granular boron nitride according to claim 8, wherein the oxides removed are substantially all calcium oxide and at least a portion of rare earth element oxides.
10. Average particle size is 10-25 μm, specific surface area (calculated using the BET multipoint method) is 2-10 m 2 / g.
11. Granular boron nitride according to claim 10, characterized in that it has a shell structure with an aspect ratio of 1-3.
12. 12. Granular boron nitride according to claim 10 or 11, characterized in that it contains 1% to 15% of rare earth element oxide, based on the mass of the granular boron nitride.
13. Granular boron nitride according to any one of claims 10 to 12, which is contained in the granular boron nitride composition according to any one of claims 5 to 7.
14. A resin composition comprising the granular boron nitride composition according to any one of claims 5 to 7 and a resin material.
15. 15. The resin composition according to claim 14, wherein the amount of the particulate boron nitride composition is 10 to 90% by weight of the resin composition.
16. A resin composition comprising the granular boron nitride according to any one of claims 10 to 13 and a resin material.
17. 17. The resin composition according to claim 16, wherein the amount of the particulate boron nitride is 10 to 90% by weight of the resin composition.
18. The resin composition according to any one of claims 14 to 17, characterized in that the resin material is an epoxy resin.
19. A method for producing a molded article, comprising molding the resin composition according to any one of claims 14 to 18.
20. A molded article produced by using the resin composition according to any one of claims 14 to 18.
21. The molded body according to claim 20, having a thermal conductivity of 10 to 25 W / (m·K) in a direction parallel to the direction in which pressure is applied during molding.
22. The molded body according to claim 20 or 21, having a thermal conductivity of 15 to 35 W / (m·K) in a direction perpendicular to the direction in which pressure is applied during molding.
Citation Information
Patent Citations
Polyolefin microporous film and lithium ion secondary battery
JP2011225736A
Powdery boron nitride composition, and composite material composition including the same
JP2013056789A
Boron nitride containing metal oxide and method of producing the same
JP2013147363A
Aggregated boron nitride particle, composition containing aggregated boron nitride particle, and three-dimensional integrated circuit having layer comprising composition
JP2013241321A
Boron nitride aggregates, methods for producing the same, and uses thereof
JP2015518808A