Asphalt composition, asphalt composition production device, asphalt composition production system, and asphalt composition production method

A specially formulated asphalt composition with SEBS and polyethylene wax achieves lower melting temperatures, reducing odor and smoke, and ensures stable mixing and flexibility, addressing the issues of high-temperature instability and lump formation in existing compositions.

JP7554744B2Active Publication Date: 2024-09-20IDEMITSU KOSAN CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2021527522
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-06-19
Filing Date
2020-05-28
Publication Date
2024-09-20
Estimated Expiration
2040-05-28

AI Technical Summary

Technical Problem

Existing asphalt compositions used in waterproofing applications require high melting temperatures, leading to smoke and odor issues, and result in unstable mixing due to the addition of high softening point waxes, causing lump formation and reduced flexibility.

Method used

An asphalt composition with specific properties, including penetration, softening point, viscosity, Fraas embrittlement point, and particle size, is formulated using a hydrogenated elastomer and wax, specifically styrene-ethylene/butadiene-styrene block copolymer (SEBS) and polyethylene or polyester wax, to achieve a lower melting temperature and stable mixing.

Benefits of technology

The composition allows for reduced melting temperatures, minimizing odor and smoke, ensuring stable mixing, and maintaining flexibility and adhesion even in high-temperature environments, thus enhancing waterproof performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554744000005
    Figure 0007554744000005
  • Figure 0007554744000004
    Figure 0007554744000004
  • Figure 0007554744000002
    Figure 0007554744000002
Patent Text Reader

Abstract

[Problem] To provide a technology that relates to an asphalt composition which has a low melting temperature, while being capable of achieving desired mixing stability. [Solution] An asphalt composition according to the present disclosure is characterized by having a penetration of from 17 to 40 (inclusive), a softening point of 97°C or more, a viscosity at 200°C of 250 mPa∙s or less, a Fraass embrittlement point of -15°C or less, a sagging length of 8 mm or less and a heating stability of 5°C or less, and is also characterized in that the particles of the composition have a maximum particle diameter of less than 1 mm.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an asphalt composition that makes it possible to reduce the temperature during melting, an apparatus for producing an asphalt composition, a system for producing an asphalt composition, and a method for producing an asphalt composition. [Background technology]

[0002] In waterproofing work, asphalt compositions are often used as waterproofing materials or adhesives that are attached to waterproof sheets. The asphalt compositions used in such waterproofing work are often used outdoors. For example, in the asphalt waterproofing thermal method used in waterproofing work on roofs, etc., blown asphalt is melted at the construction site, and the molten blown asphalt is attached to a waterproofing sheet to form a waterproof layer.

[0003] However, in the above-mentioned construction method, the asphalt composition is melted to about 260°C, which causes the light components contained in the asphalt to evaporate, resulting in the emission of smoke and odor, and there are concerns that this may have a negative impact on the working environment of workers and on the surrounding area of ​​the construction site.

[0004] Conventionally, the technology of Patent Document 1 has been proposed as a technology for suppressing odors generated when melting an asphalt composition used in waterproofing work, etc. However, in the technology disclosed in Patent Document 1, a high softening point wax is added, which may cause the generation of large lumps (also called lumps or aggregates) or particles, making it difficult to mix stably. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2007-238956 A Summary of the Invention [Problem to be solved by the invention]

[0006] Therefore, the present disclosure has been devised in consideration of the above-mentioned points, and an object of the present disclosure is to provide a technology relating to an asphalt composition that has a low melting temperature and is capable of obtaining the desired mixing stability. [Means for solving the problem]

[0007] According to one embodiment of the present disclosure, the composition has a penetration of 17 to 40, a softening point of 97°C or higher, a viscosity at 200°C of 250 mPa·s or lower, a Fraas embrittlement point of -15°C or lower, a sagging length of 8 mm or lower, and a heat stability of 5°C or lower, and the particle size of the composition is less than 1 mm in maximum diameter. The asphalt composition comprises a base asphalt, a hydrogenated elastomer, and a wax, the hydrogenated elastomer being 9.0% by mass or more and 10.5% by mass or less, and the wax being 3.0% by mass or more and 5.5% by mass or less, the hydrogenated elastomer has a styrene content of 27.0% by mass or more and 35.0% by mass or less, the wax has a crystallinity of 70% or more and a melt viscosity at 150°C of 100 mPa·s or less, the hydrogenated elastomer is a styrene-ethylene / butadiene-styrene block copolymer (SEBS) having a 20% toluene solution viscosity of 0.3 Pa·s or more and 0.8 Pa·s or less, and the wax is polyethylene or polyester to which an acid has been added. It is possible to provide techniques relating to asphalt compositions. Effect of the Invention

[0008] According to the present disclosure, it is possible to provide a technology relating to an asphalt composition that has a low melting temperature and is capable of obtaining desired mixing stability. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a schematic diagram showing an example of an asphalt composition and an asphalt composition production device and production system that can be suitably used in this embodiment. [Diagram 2] FIG. 1 is a diagram showing an example of an asphalt composition and a process for producing the asphalt composition that can be suitably used in this embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] As described above, the inventors have conducted extensive research into the component composition and content ratio of an asphalt composition, as well as into the manufacturing method of the asphalt composition. As a result, they have discovered a new technology for an asphalt composition that has a low melting temperature and can obtain a desired mixing stability by mixing a specific hydrogenated elastomer and wax in a range of a predetermined mass % with asphalt, and have completed the technology of the present disclosure.

[0011] Hereinafter, the asphalt composition, the asphalt composition manufacturing apparatus, and the asphalt composition manufacturing method according to the present embodiment will be described in detail. In the following description, materials added to the base asphalt to produce the asphalt composition of the present disclosure, such as hydrogenated elastomers and waxes, may be collectively referred to as additives.

[0012] The asphalt composition in this embodiment contains SEBS and wax in the base asphalt. In addition, the asphalt composition in this disclosure may contain aromatic oils, such as extracts obtained by solvent extraction of deasphalted oil obtained by deasphalting the residual oil obtained by vacuum distillation of crude oil, in the base asphalt. The preferred properties and contents of each component composition are as follows.

[0013] Penetration: 17 or more and 40 or less, Softening point: 97℃ or higher, Viscosity at 200℃: 250mPa·s or less, Frass embrittlement point: -15℃ or less, Sagging length: 8mm or less, Heating stability: 5℃ or less And, The particle size of the composition is less than 1 mm in maximum diameter; It is.

[0014] Hydrogenated elastomer: 9.0% by mass or more and 10.5% by mass or less Wax: 3.0% by mass or more and 5.5% by mass or less The hydrogenated elastomer has a styrene content of 27.0% by mass or more and 35.0% by mass or less, and a 20% toluene solution viscosity of 0.3 Pa·s or more and 0.8 Pa·s or less. The wax has a crystallinity of 70% or more and a melt viscosity at 150°C of 100 mPa·s or less.

[0015] The details of each component composition and the reasons for limiting the content thereof will be explained below. Note that mass% here may be read as weight%.

[0016] (Hydrogenated elastomer) The hydrogenated elastomer preferably used in the asphalt composition of this embodiment is a thermoplastic elastomer added as a reinforcing material to the base asphalt. The hydrogenated elastomer particularly preferably used in this embodiment is a styrene-ethylene / butadiene-styrene block copolymer (SEBS) in which the double bonds in the butadiene block of a styrene-butadiene-styrene block copolymer (SBS) have been completely hydrogenated, and the hydrogenated elastomer will be described below assuming that SEBS is used. The performance of SEBS can be estimated mainly from its styrene content and the viscosity of a 20% toluene solution at 25°C.

[0017] The content of SEBS preferably used in this embodiment is 9.0% by mass or more and 10.5% by mass or less with respect to the total mass of the asphalt composition. If the content of SEBS is less than 9.0% by mass with respect to the total mass of the asphalt composition, the furth embrittlement point does not satisfy -15°C or less, and low-temperature flexibility decreases. In addition, if the content of SEBS exceeds 10.5% by mass with respect to the total mass of the asphalt composition, a predetermined viscosity cannot be secured at about 200°C, and workability deteriorates when performing waterproofing work. Therefore, a melting temperature of about 260°C or more is required, and the melting temperature cannot be reduced. As a result, the odor generated during melting cannot be suppressed. For this reason, the content of SEBS used in this embodiment is preferably 9.0% by mass or more and 10.5% by mass or less with respect to the total mass of the asphalt composition.

[0018] Moreover, the SEBS has a styrene content of 27.0% by mass or more and 35.0% by mass or less relative to the SEBS mass. If the styrene content is less than 27.0% by mass relative to the SEBS mass, a predetermined softening point cannot be ensured and waterproof performance cannot be exhibited. If the styrene content exceeds 35.0% by mass relative to the SEBS mass, mixing cannot be performed stably. Therefore, the SEBS used in this embodiment preferably has a styrene content of 27.0% by mass or more and 35.0% by mass or less relative to the SEBS mass.

[0019] Furthermore, the SEBS preferably used in this embodiment has a 20% toluene solution viscosity of 0.3 Pa·s or more and 0.8 Pa·s or less. The 20% toluene solution viscosity is a value measured by using toluene as a solvent and dissolving a specific sample in a solution at 20 mass% of the solution with a Brookfield (BF) type viscometer at 25°C. If the SEBS has a 20% toluene solution viscosity of less than 0.3 Pa·s, the softening point of the asphalt composition cannot be effectively increased. If the SEBS has a 20% toluene solution viscosity of more than 0.8 Pa·s, the viscosity of the asphalt composition increases too much, and there is a risk that the temperature cannot be reduced when performing waterproofing work. For this reason, the SEBS preferably used in this embodiment has a 20% toluene solution viscosity of 0.3 Pa·s or more and 0.8 Pa·s or less.

[0020] In this embodiment, only one type of SEBS may be mixed, or two or more types of SEBS having specific molecular structures may be selected and mixed. Mixing only one type of SEBS is preferable to selecting and mixing two or more types of SEBS, since it is possible to eliminate the complication of selecting and mixing two or more types of SEBS and reduce the manufacturing labor.

[0021] (wax) The wax preferably used in the asphalt composition in this embodiment is polyethylene or polyethylene to which an acid has been added. The reason for mixing wax is to reduce the melt viscosity and improve the high-temperature rigidity, and these performances match the properties of wax. On the other hand, wax does not have properties useful for improving the flexibility of an asphalt composition at low temperatures. In other words, when wax is added, the low-temperature flexibility is reduced. According to the present invention, the reduction in low-temperature flexibility caused by mixing wax is compensated for by adding SEBS.

[0022] Wax includes not only normal paraffin with a straight chain structure, but also those with numerous branched structures. The degree of branching is indicated by the degree of crystallinity. The degree of crystallinity is the ratio of amorphous parts to crystalline parts in the wax, and the higher the degree of crystallinity, the less branching there is.

[0023] The wax preferably used in this embodiment has a crystallinity of 70% or more. If the wax has a crystallinity of less than 70%, the melt viscosity increases in an amount expected to increase the softening point of the asphalt composition, and workability deteriorates. Therefore, a melting temperature of about 260°C is required, and the melting temperature cannot be reduced. As a result, the odor generated during melting cannot be suppressed. For this reason, the wax preferably used in this embodiment has a crystallinity of 70% or more.

[0024] The degree of crystallinity can be determined by first measuring the amount of endotherm observed at the melting point (around 100°C) of a sample of the asphalt composition to be evaluated using differential scanning calorimetry (DSC), and then calculating the ratio of this to the theoretical heat of fusion of the wax, as shown in the following formula. Crystallinity (%) = (measured heat absorption (J / g) / heat of wax fusion (J / g)) x 100

[0025] The content of the wax preferably used in this embodiment is 3.0% by mass or more and 5.5% by mass or less with respect to the total mass of the asphalt composition. If the content of the wax is less than 3.0% by mass with respect to the total mass of the asphalt composition, the specified softening point cannot be ensured and waterproof performance cannot be exhibited. If the content of the wax exceeds 5.5% by mass, mixing cannot be performed stably. In addition, the effects of reducing the melt viscosity and improving the high-temperature rigidity are saturated. For this reason, the content of the wax used in this embodiment is preferably 3.0% by mass or more and 5.5% by mass or less with respect to the total mass of the asphalt composition.

[0026] The wax preferably used in this embodiment has a melt viscosity at 150°C of 100 mPa·s or less. If the melt viscosity of the wax at 150°C exceeds 100 mPa·s, the melt viscosity of the asphalt composition increases, and workability deteriorates. Therefore, a melt temperature of about 260°C is required, and the melt temperature cannot be reduced. As a result, the odor generated during melting cannot be suppressed. For this reason, the wax used in this embodiment preferably has a melt viscosity at 150°C of 100 mPa·s or less.

[0027] The asphalt composition according to the present disclosure may contain rosin. Examples of rosin include gum rosin, disproportionated gum rosin, wood rosin, and tall oil rosin. These rosins can be classified into the above-mentioned gum rosin and wood rosin depending on the difference in origin, raw material, and extraction method, but the rosin preferably used in the present invention is sufficient as long as it is obtained as a residue component during steam distillation of pine resin. These rosins are mixtures containing abietic acid, palustric acid, neoabietic acid, dehydroabietic acid, pimaric acid, sandaracopimaric acid, isopimaric acid, and the like as components. These rosins usually soften at about 80°C and melt at about 90 to 100°C. Rosin contains various resin acids such as abietic acid, dehydroabietic acid, dihydroabietic acid, tetrahydroabietic acid, palustric acid, neoabietic acid, and levopimaric acid, and these resin acids may be purified and used alone.

[0028] Also, instead of using rosin as it is, any one or more of abietic acid, dehydroabietic acid, neoabietic acid, pimaric acid, isopimaric acid, palustric acid, etc. may be added alone.

[0029] (Base asphalt) The base asphalt preferably used in the asphalt composition of this embodiment is composed of straight asphalt obtained as residual oil obtained by vacuum distillation of crude oil, asphalt obtained by deasphalting the residual oil of vacuum distillation of crude oil with propane or the like (propane deasphalting process) (also called SDA: Solvent Deasphalting, SDA bitumen, SDA pitch, etc., hereinafter referred to as SDA), blown asphalt into which air is introduced by blowing, etc. The base asphalt may be composed of straight asphalt and SDA. In addition, the base asphalt may further include an extract (solvent extracted oil) obtained by solvent extraction of the solvent deasphalted oil obtained by deasphalting the residual oil of vacuum distillation of crude oil with propane or the like in the above composition. In addition, instead of this extract, it may be composed of aromatic oil. This aromatic oil is, for example, specified in JIS K 6200, and is a hydrocarbon process oil containing at least 35 mass% aromatic hydrocarbons.

[0030] The base asphalt preferably used in this embodiment is produced by any of the above-mentioned vacuum distillation method, blowing (air blowing method), and mixing method (blending method). That is, this base asphalt contains one or more of SDA, straight asphalt, blown asphalt, and extract.

[0031] SDA is obtained by deasphalting vacuum distillation residual oil using propane or a mixture of propane and butane as a solvent.

[0032] For example, SDA has a penetration of 13 (1 / 10 mm) at 25°C, a softening point of 61.5°C, and a density of 1066 kg / m at 15°C under JIS K 2207. 3 Alternatively, the above-mentioned may be used.

[0033] In addition, for example, straight asphalt has a penetration of 65 (1 / 10 mm) at 25°C, a softening point of 48.5°C, and a density of 1034 kg / m at 15°C according to JIS K 2207. 3 Alternatively, the above-mentioned may be used.

[0034] Extract is an oil extracted when heavy lubricating oil is obtained as refined oil by solvent extraction using a polar solvent from the solvent deasphalted oil obtained by deasphalting the residual oil from the vacuum distillation of crude oil using propane or the like. Extract has a kinetic viscosity of 61.2 mm at 100°C. 2 / s, kinetic viscosity at 40°C is 3970mm 2 / s, density at 15°C is 976.4 kg / m 3 In addition, the content of the extract preferably used in this embodiment is preferably 3.0 mass% or less with respect to the total mass of the asphalt composition. Here, if the content of the extract exceeds 3.0 mass%, there is a risk of causing a decrease in the sagging resistance of the asphalt composition as a final product. Note that the asphalt composition according to the present disclosure does not necessarily contain an extract.

[0035] The asphalt composition having the above-mentioned component composition is melted and applied to a waterproof sheet such as asphalt roofing, and is used in waterproofing work on roofs, etc. Here, a manufacturing device and a manufacturing system for the asphalt composition having the above-mentioned component composition will be described with reference to FIG.

[0036] An asphalt production plant 100 as a production system for an asphalt composition composed of the above-mentioned component composition is mainly composed of a base asphalt container 101 for storing and preserving the base asphalt, and a mixing container 102 for mixing the base asphalt with various additives such as the above-mentioned SEBS and wax. Here, the asphalt production plant 100 may be composed of any one or all of a product container 103 for storing and preserving the asphalt composition produced by mixing, an agitator (mixing device) 105 provided in the mixing container 102, an additive supplying device 106 for supplying various additives, and a control device (control unit) 108 for controlling at least the agitator 105 and the additive supplying device 106.

[0037] In addition, the base asphalt container 101 and the mixing container 102 are connected by a first supply piping 104, and a predetermined amount of base asphalt maintained at a predetermined temperature is supplied from the base asphalt container 101 to the mixing container 102 via the first supply piping 104.

[0038] Similarly, the mixing container 102 and the product container 103 are connected by a second supply pipe 107, and the asphalt composition produced in the mixing container 102 is transferred to the product container 103 and stored and maintained at a predetermined temperature for a predetermined period of time.

[0039] The mixing vessel 102 is provided with an additive supplying device 106 for supplying various additives such as SEBS and wax, and an agitating device (mixing device) 105 for agitating the base asphalt and additives at a predetermined rotation speed. The mixing vessel 102 and the agitating device 105 mainly constitute an asphalt composition manufacturing device. The additive supplying device 106 and the control device 108 described below may also be included in the asphalt composition manufacturing device.

[0040] The control device 108 is a device for controlling the temperature management and supply amount of various materials, and is electrically connected to the agitator 105 and the additive supply device 106 by wire or wirelessly.

[0041] The control device 108 also has at least a storage device (storage unit) 110 such as an HDD or CD that stores predetermined parameters, a processing device (processing unit) 109 such as a CPU that reads out each parameter and performs processing to control the target device, and an input device (input unit) 111 using a UI or the like for inputting each parameter, necessary data, and signals for performing necessary processing. The control device 108 may also have an output device such as a display or printer (not shown). The processing device 109, storage device 110, and input device 111 are electrically connected to each other.

[0042] Next, the manufacturing process of the asphalt composition having the above-mentioned component composition will be described with reference to FIG.

[0043] (Base asphalt production process: S101) Straight asphalt supplied to base asphalt container 101 is mixed with an extract if necessary, and the mixture is stirred and mixed for a predetermined period of time by a stirring device (not shown) under conditions such as a temperature of 140° C. or higher and a rotation speed of 1,000 rpm or higher and 4,000 rpm or lower, to produce base asphalt as an asphalt material (S101).

[0044] (Additive mixing process: S102) Next, a predetermined amount of the above-mentioned base asphalt is transferred to a mixing vessel 102, and predetermined amounts of SEBS and wax are added by an additive supplying device 106. The mixture is stirred and mixed in an agitating device 105 for a predetermined period of time under conditions of, for example, a temperature of 160° C. to 240° C. and a rotation speed of 2,000 rpm to 6,000 rpm, to produce an asphalt composition (S102).

[0045] (Asphalt composition (product) storage process: S103) Next, the produced asphalt composition is transferred to a product container 103 for temporary storage and preservation (S103). At this time, the temperature in the product container may be controlled by, for example, a control device 108 so as to maintain a predetermined temperature.

[0046] According to the asphalt composition of the present embodiment, it is possible to reduce the possibility of water leakage due to insufficient attachment to the waterproof sheet caused by dripping occurring after construction.

[0047] Furthermore, according to the asphalt composition of the present embodiment, even when the asphalt composition is used in an environment where the outside air reaches high temperatures, such as in summer or in tropical or subtropical regions, and the asphalt composition itself reaches a high temperature of around 80°C, it is possible to suppress softening of the asphalt composition used as an adhesive and reduce the possibility of the asphalt composition being unable to exhibit its waterproofing performance.

[0048] Furthermore, according to the asphalt composition of this embodiment, it is possible to suppress the formation of lumps (also called lumps, aggregates, etc.) having a particle diameter of 1 mm or more formed in the composition, and it is possible to avoid variations in the quality of the generated asphalt composition due to the formation of lumps, and a decrease in waterproof performance due to water penetration from the lumps or granules. In other words, it is possible to uniformly disperse the mixture of the asphalt composition (also called mixing stability and dispersion uniformity).

[0049] Furthermore, according to the asphalt composition of the present embodiment, it is possible to suppress the occurrence of brittle fracture at low temperatures, thereby reducing the possibility of water leakage.

[0050] As described above, according to the asphalt composition of the present embodiment, it is possible to exhibit waterproof performance, to suppress the odor generated when the asphalt composition melts, and to ensure mixing stability. EXAMPLES

[0051] The present embodiment will be specifically described below with reference to examples and comparative examples.

[0052] Samples were prepared by mixing straight asphalt 60-80, extract, SEBS, wax, SBS, etc. in the blending ratios shown in Examples 1-24 and Comparative Examples 1-36 in Tables 1 and 2. In the following tables and explanations, the viscosity of a 20% toluene solution refers to the viscosity of a 20% toluene solution at 25°C.

[0053] [Table 1]

[0054] [Table 2]

[0055] Regarding SEBS, samples SEBS1 to SEBS7 were prepared. The properties of each are as follows: SEBS1: Styrene content 30.0% by mass, 20% toluene solution viscosity 1.5 Pa s SEBS2: Styrene content 31.0% by mass, 20% toluene solution viscosity 60.0 Pa s SEBS3: Styrene content 13.0% by mass, 20% toluene solution viscosity 1.5 Pa s SEBS4: Styrene content 67.0% by mass, 20% toluene solution viscosity 0.3 Pa s SEBS5: Styrene content 42.0% by mass, 20% toluene solution viscosity 1.0 Pa s SEBS6: Styrene content 29.0% by mass, 20% toluene solution viscosity 0.4 Pa s SEBS7: Styrene content 30.0% by mass, 20% toluene solution viscosity 0.5 Pa s Among these, SEBS6 and SEBS7 satisfy the styrene content and 20% toluene solution viscosity specified in the above-mentioned embodiment, and SEBS1 to SEBS5 are all samples for comparison purposes.

[0056] As a sample for comparison, SBS (styrene-butadiene-styrene copolymer) was prepared. The properties of SBS are as follows. SBS is the starting material for the production of SEBS, and SEBS is obtained by adding hydrogen to the double bonds in the SBS molecule to make them single bonds. SBS: styrene content 30.0% by mass, 20% toluene solution viscosity 0.5 Pa s

[0057] Regarding the wax, polyethylene or polyethylene to which acid has been added was prepared as samples, Wax 1 to Wax 4. The properties of each are as follows: Wax 1: Crystallinity 73.5%, melt viscosity at 150°C 5 mPa·s, calorific value 216 J / g Wax 2: Crystallinity 74.5%, melt viscosity at 150°C 15 mPa·s, calorific value 219 J / g Wax 3: Crystallinity 70.1%, melt viscosity at 150°C 4300 mPa·s, calorific value 206 J / g Wax 4: Crystallinity 54.4%, melt viscosity at 150°C 340 mPa·s, calorific value 160 J / g Of these, waxes that satisfy the crystallinity and melt viscosity at 150° C. specified in the above-mentioned embodiment are waxes 1 and 2, and waxes 3 and 4 are both samples for comparative examples.

[0058] In each of Examples 1 to 24 and Comparative Examples 1 to 36, the penetration was adjusted to 17 to 40 (1 / 10 mm) using straight asphalt 60 to 80 and extract. The extract had a kinetic viscosity of 480 mm at 60°C. 2 / s, density at 15°C is 976.4 kg / m 3 In addition, for Comparative Examples 1 to 4, three types of asphalt for waterproofing work obtained in accordance with JIS K 2207 were used.

[0059] Next, the test methods used in the present invention will be described.

[0060] The mixing stability is a test for confirming the particle size of the lump-like composition that occurs in the asphalt composition due to improper mixing. Specifically, the asphalt composition after mixing was spread to a thickness of 1 mm on a release paper, and the presence or absence of lumps or particles with a maximum diameter of 1 mm or more (presence or absence of lumps with a maximum diameter of 1 mm or more) was visually confirmed, and the diameter of the lumps or particles confirmed by visual inspection was measured with a measuring means such as a vernier caliper or a scale to confirm the presence or absence of lumps or particles with a maximum diameter of 1 mm or more. The samples used in the mixing stability test were each mixed with the materials in Tables 1 and 2 in a homomixer so as to have the respective mixing ratios of Examples 1 to 24 and Comparative Examples 1 to 36 in Tables 1 and 2, and maintained at about 200°C, and various additives such as SEBS and wax were added. The mixing was performed for 3 hours with the homomixer rotating at 3500 rpm. The production amount at that time was 0.9 kg. In the above, it has been explained that the mixing stability is confirmed by visual inspection. However, in addition to visual inspection, it is also possible to check the portion that passes through a sieve with 1 mm mesh size to confirm whether or not lumps with a diameter of 1 mm or more are present. Therefore, it does not matter which method is used to evaluate the mixing stability.

[0061] The penetration (25°C) was measured according to JIS K 2207 "Petroleum asphalt - Penetration test method".

[0062] The softening point was measured according to JIS K 2207 "Petroleum asphalt - softening point test method".

[0063] The viscosity (200°C) was measured under the conditions of JPI-5S-54-99 "Asphalt - Viscosity test method using a rotational viscometer" at a measurement temperature of 200°C, using a spindle SC4-21, and a spindle rotation speed of 20 rpm.

[0064] The sagging length was measured according to JIS K 2207 "Petroleum asphalt - sagging test method".

[0065] The frass embrittlement point was measured according to JIS K 2207 "Petroleum asphalt - frass embrittlement point test method".

[0066] Heat stability was measured according to JIS K 2207 "Petroleum asphalt - Heat stability test method".

[0067] The effects of the asphalt composition defined in this embodiment were verified below.

[0068] In order to suppress the odor that is generated when the asphalt composition melts, it is necessary to reduce the melting temperature. However, by reducing the melting temperature, there is a risk that it will not be possible to ensure a viscosity sufficient for construction. Therefore, a viscosity sufficient for construction is required, for example, when melted at around 220°C, without increasing the melting temperature to around 260°C as in the past. In this study, it was determined that construction is possible when the viscosity (200°C) of the asphalt composition is 250 mPa·s or less, and it was evaluated that the melting temperature can be reduced.

[0069] In addition, if sagging occurs after application of the asphalt composition, it may not be attached properly to the waterproof sheet, and the waterproof performance may not be achieved. For this reason, it is necessary to ensure a certain level of sagging resistance for the asphalt composition. In this study, it was evaluated that sagging resistance can be ensured when the sagging length measured according to JIS K 2207 is 8 mm or less.

[0070] In addition, since the asphalt composition applied to the waterproof layer is often applied outdoors, the temperature may rise to about 80°C in environments where the outside air may reach high temperatures, such as in summer, tropical regions, or subtropical regions. If used in such a high-temperature environment, the waterproof layer may deform and may not be able to perform its waterproofing performance. For this reason, the asphalt composition applied to the waterproof layer needs to have a specified softening point. In this study, it was evaluated that deformation resistance can be ensured when the softening point of the asphalt composition is 97°C or higher. In order to ensure higher deformation resistance, it is desirable for the softening point of the asphalt composition to be 100°C or higher.

[0071] In addition, if the flexibility of an asphalt composition deteriorates at low temperatures, such as 0°C to -10°C, cracks may occur and the waterproofing performance may not be achieved. For this reason, it is necessary for the asphalt composition to ensure a certain level of low-temperature flexibility. In this study, it was evaluated that low-temperature flexibility can be ensured when the furth embrittlement point measured according to JIS K 2207 is -15°C or lower.

[0072] In addition, if lumps or particles occur during mixing of the asphalt composition, the quality will vary greatly, and water may seep in through the lumps or particles, which may reduce the waterproofing performance. For this reason, the asphalt composition needs to be able to be mixed stably. In this study, the mix stability was evaluated as good when no lumps or particles with a diameter of 1 mm or more were observed in the mix stability test. In Tables 1 and 2, when no lumps or particles with a diameter of 1 mm or more were observed in the mix stability test, the mix stability was indicated as "○", and when lumps or particles with a diameter of 1 mm or more were observed in the mix stability test, the mix stability was indicated as "×".

[0073] In addition, asphalt compositions may be kept in a heated and molten state for more than one hour during waterproofing work. If the asphalt product changes in quality and the furth embrittlement point rises, i.e., the low-temperature flexibility deteriorates, the low-temperature flexibility of the waterproofing material is significantly impaired, the possibility of cracking increases, and the waterproofing performance cannot be achieved. Here, the Frass embrittlement point is measured before and after the heat stability test, and if the difference is within 5°C, the material has sufficient performance as a waterproof material and maintains its low-temperature flexibility.

[0074] That is, the asphalt compositions according to the examples and comparative examples were examined as to whether they satisfied the conditions (1) to (6) shown in the following Table 3. In Tables 1 and 2, when all of the conditions (1) to (6) were satisfied, the overall evaluation was indicated as "◯", and when any of the conditions (1) to (6) were not satisfied, the overall evaluation was indicated as "×".

[0075] [Table 3]

[0076] In all of Examples 1 to 24, the SEBS content, the styrene content of SEBS, the viscosity of a 20% toluene solution of SEBS, the wax content, the degree of crystallinity of the wax, the melt viscosity of the wax at 150°C, and the extract content were within the ranges specified in the above-mentioned embodiment.

[0077] As a result, Examples 1 to 24 satisfy all of the above conditions (1) to (6).

[0078] That is, in Examples 1 to 24, the sagging length measured according to JIS K 2207 was 8 mm or less. This makes it possible to suppress the occurrence of sagging after construction. As a result, it is possible to ensure the desired sagging resistance.

[0079] In addition, in Examples 1 to 24, the softening point of the asphalt composition measured by JIS K 2207 is 97°C or higher. This makes it possible to suppress deformation of the waterproof layer even in environments where the outside air may reach high temperatures, such as in summer, tropical regions, or subtropical regions. This makes it possible to ensure the desired deformation resistance. Furthermore, in Examples 1, 2, 4 to 9, 11 to 14, and 20 to 24, the softening point is 100°C or higher. This makes it possible to ensure higher deformation resistance.

[0080] Moreover, in Examples 1 to 24, the furth embrittlement point measured according to JIS K 2207 is -15°C or lower. This makes it possible to suppress deterioration of the properties of the asphalt composition at low temperatures (for example, 0°C to -10°C), thereby ensuring the desired low-temperature flexibility.

[0081] Moreover, in Examples 1 to 24, the viscosity (200°C) was 250 mPa·s or less. This allows the viscosity to be secured so that the composition can be applied even if it is melted at, for example, about 220°C, without having to raise the melting temperature to about 260°C as in the past. This allows the melting temperature to be lowered, and the odor generated when the asphalt composition melts can be suppressed.

[0082] Furthermore, in the mixing stability test, no lumps or particles with a diameter of 1 mm or more were observed in Examples 1 to 24. This means that mixing can be stably performed without the generation of lumps or particles during mixing, and the desired mixing stability can be ensured.

[0083] Moreover, the results of the heat stability test for Examples 1 to 24 were 5° C. or less. This means that even if the product is kept in a heat-molten state for one hour or more, the product maintains its low-temperature flexibility. This reduces the possibility of cracking, and the product can exhibit waterproof performance.

[0084] As a result, the asphalt composition of the present embodiment can exhibit waterproof performance, can suppress the odor generated when the asphalt composition melts, and can ensure mixing stability.

[0085] In Comparative Example 1, three types of waterproofing asphalt were used as the asphalt composition. As a result, the viscosity (200°C) exceeded 250 mPa·s. Therefore, a melting temperature of about 260°C was required, and the melting temperature could not be reduced. As a result, the odor generated during melting could not be suppressed.

[0086] Comparative Example 2 uses waterproofing asphalt type 3 and wax 2, but does not use SEBS. As a result, the viscosity (200°C) exceeded 250 mPa·s. This requires a melting temperature of about 260°C, and the melting temperature cannot be reduced. This makes it impossible to suppress the odor generated during melting.

[0087] Comparative Example 3 used waterproofing asphalt type 3 and wax 2, but did not use SEBS. As a result, the viscosity (200°C) exceeded 250 mPa·s. This required a melting temperature of about 260°C, and the melting temperature could not be reduced. This meant that the odor generated during melting could not be suppressed.

[0088] Comparative Example 4 uses waterproofing asphalt type 3 and wax 2, and does not use SEBS. As a result, the furath embrittlement point did not satisfy the requirement of -15°C or less. Therefore, the low-temperature flexibility of the asphalt composition cannot be ensured, and the waterproofing performance cannot be exhibited.

[0089] In Comparative Example 5, SEBS1 and Wax 1 were used. The amount of Wax 1 used in Comparative Example 5 was less than 3.0% by mass relative to the total mass of the asphalt composition. As a result, the mixing stability was reduced and the viscosity (200°C) exceeded 250 mPa·s. For this reason, a melting temperature of about 260°C was required, and the melting temperature could not be reduced. As a result, the odor generated during melting could not be suppressed. The sagging length of Comparative Example 5 was not measured because the mixing stability was reduced.

[0090] In Comparative Example 6, SEBS2 and Wax 1 were used. The amount of Wax 1 used in Comparative Example 6 was less than 3.0% by mass relative to the total mass of the asphalt composition. As a result, the mixing stability was reduced and the viscosity (200°C) exceeded 250 mPa·s. This required a melting temperature of about 260°C, which meant that the melting temperature could not be reduced and the odor generated during melting could not be suppressed. In addition, the softening point was less than -97°C, which meant that deformation resistance could not be secured and waterproof performance could not be achieved. The sagging length in Comparative Example 6 was not measured because the mixing stability was reduced.

[0091] In Comparative Example 7, SEBS6 and Wax 1 were used. The amount of Wax 1 used in Comparative Example 7 was less than 3.0% by mass with respect to the total mass of the asphalt composition. As a result, the softening point was less than 97°C. Therefore, deformation resistance could not be ensured, and waterproof performance could not be exhibited.

[0092] In Comparative Example 8, SEBS3 and Wax 1 were used. The amount of Wax 1 used in Comparative Example 8 was less than 3.0% by mass with respect to the total mass of the asphalt composition. As a result, the viscosity (200°C) exceeded 250 mPa·s. This required a melting temperature of about 260°C, which meant that the melting temperature could not be reduced and the odor generated during melting could not be suppressed. In addition, the softening point was less than 97°C, which meant that deformation resistance could not be ensured and waterproof performance could not be achieved.

[0093] In Comparative Example 9, SEBS6 and Wax 1 were used. The amount of SEBS6 used in Comparative Example 9 was less than 9.0% by mass relative to the total mass of the asphalt composition, and the amount of Wax 1 was less than 3.0% by mass relative to the total mass of the asphalt composition. As a result, the softening point was less than 97°C. Therefore, deformation resistance could not be ensured and waterproof performance could not be exhibited. Furthermore, the furth embrittlement point of -15°C or less was not satisfied, which deteriorated flexibility at low temperatures and caused cracks to occur, preventing waterproof performance.

[0094] In Comparative Example 10, SEBS6 and wax 1 were used. The amount of SEBS6 used in Comparative Example 10 was less than 9.0% by mass relative to the total mass of the asphalt composition. As a result, the softening point was less than 97°C. Therefore, deformation resistance could not be ensured and waterproof performance could not be achieved. Furthermore, the frass embrittlement point of -15°C or less was not satisfied, which deteriorated flexibility at low temperatures and caused cracks, preventing waterproof performance.

[0095] In Comparative Example 11, SEBS6 and Wax 1 were used. The amount of SEBS6 used in Comparative Example 11 was less than 9.0% by mass relative to the total mass of the asphalt composition. As a result, the softening point was less than 97°C. Therefore, deformation resistance could not be ensured and waterproof performance could not be achieved. Furthermore, the frass embrittlement point of -15°C or less was not satisfied, which deteriorated flexibility at low temperatures and caused cracks to occur, preventing waterproof performance.

[0096] In Comparative Example 12, SEBS6 and Wax 1 were used. The amount of SEBS6 used in Comparative Example 12 was less than 9.0% by mass relative to the total mass of the asphalt composition. As a result, the softening point was less than 97°C. Therefore, deformation resistance could not be ensured and waterproof performance could not be achieved. Furthermore, the frass embrittlement point of -15°C or less was not satisfied, which deteriorated flexibility at low temperatures and caused cracks to occur, preventing waterproof performance.

[0097] In Comparative Example 13, SEBS6 and Wax 1 were used. The amount of SEBS6 used in Comparative Example 13 was less than 9.0% by mass relative to the total mass of the asphalt composition. As a result, the softening point was less than 97°C. Therefore, deformation resistance could not be ensured and waterproof performance could not be achieved. Furthermore, the frass embrittlement point of -15°C or less was not satisfied, which deteriorated flexibility at low temperatures and caused cracks to occur, preventing waterproof performance.

[0098] In Comparative Example 14, SEBS6 and Wax 2 were used. The amount of SEBS6 used in Comparative Example 14 was less than 9.0% by mass relative to the total mass of the asphalt composition. As a result, the softening point was less than 97°C. Therefore, deformation resistance could not be ensured and waterproof performance could not be achieved. Furthermore, the frass embrittlement point of -15°C or less was not satisfied, which deteriorated flexibility at low temperatures and caused cracks to occur, preventing waterproof performance.

[0099] In Comparative Example 15, SEBS6 and Wax 2 were used. The amount of SEBS6 used in Comparative Example 15 was less than 9.0% by mass relative to the total mass of the asphalt composition. As a result, the softening point was less than 97°C. Therefore, deformation resistance could not be ensured and waterproof performance could not be exhibited. Furthermore, the frass embrittlement point of -15°C or less was not satisfied, which deteriorated flexibility at low temperatures and caused cracks to occur, preventing waterproof performance.

[0100] In Comparative Example 16, SEBS6 and Wax 2 were used. The amount of SEBS6 used in Comparative Example 16 was less than 9.0% by mass relative to the total mass of the asphalt composition, and the amount of Wax 2 was more than 5.5% by mass relative to the total mass of the asphalt composition. As a result, the softening point was less than 97°C. Therefore, deformation resistance could not be ensured, and waterproof performance could not be exhibited. In addition, the furth embrittlement point of -15°C or less was not satisfied, which deteriorated flexibility at low temperatures, caused cracks, and prevented waterproof performance from being exhibited. Furthermore, the mixing stability was also reduced, so that water could penetrate through the lumps and grains that were generated during mixing, and waterproof performance could be reduced.

[0101] In Comparative Example 17, SEBS6 and Wax 2 were used. The amount of SEBS6 used in Comparative Example 17 was less than 9.0% by mass relative to the total mass of the asphalt composition, and the amount of Wax 2 was more than 5.5% by mass relative to the total mass of the asphalt composition. As a result, the frass embrittlement point of -15°C or less was not satisfied, and low-temperature flexibility could not be ensured. Therefore, waterproof performance could not be achieved. Furthermore, the mixing stability was reduced, so water could seep in through the lumps and granules that were generated during mixing, which could reduce waterproof performance.

[0102] In Comparative Example 18, SEBS6 and Wax 2 were used. The amount of SEBS6 used in Comparative Example 18 was less than 9.0% by mass relative to the total mass of the asphalt composition, and the amount of Wax 2 was more than 5.5% by mass relative to the total mass of the asphalt composition. As a result, the frass embrittlement point of -15°C or less was not satisfied, low-temperature flexibility could not be secured, and waterproof performance could not be achieved. Furthermore, the mixing stability was also reduced, so water could penetrate through lumps and granules that were generated during mixing, which may reduce waterproof performance.

[0103] In Comparative Example 19, SEBS6, Wax 2, and Wax 3 were used. The amount of SEBS6 used in Comparative Example 19 was less than 9.0% by mass relative to the total mass of the asphalt composition, and the total amount of Wax 2 and Wax 3 was more than 5.5% by mass relative to the total mass of the asphalt composition. As a result, the frass embrittlement point of -15°C or less was not satisfied, low-temperature flexibility could not be secured, and waterproof performance could not be achieved. Furthermore, the mixing stability was also reduced, so that water could penetrate through the lumps and granules that were generated during mixing, and waterproof performance could be reduced.

[0104] In Comparative Example 20, SEBS6, Wax 2, and Wax 3 were used. The amount of SEBS6 used in Comparative Example 20 was less than 9.0% by mass relative to the total mass of the asphalt composition, and the total amount of Wax 2 and Wax 3 was more than 5.5% by mass relative to the total mass of the asphalt composition. As a result, the furth embrittlement point of -15°C or less was not satisfied, low-temperature flexibility could not be secured, and waterproof performance could not be achieved. Furthermore, the mixing stability was also reduced, so that water could penetrate through the lumps and granules that were generated during mixing, and waterproof performance could be reduced.

[0105] In Comparative Example 21, SEBS6, Wax 2, and Wax 4 were used. The amount of SEBS6 used in Comparative Example 21 was less than 9.0% by mass relative to the total mass of the asphalt composition, and the total amount of Wax 2 and Wax 4 was more than 5.5% by mass relative to the total mass of the asphalt composition. As a result, the frass embrittlement point of -15°C or less was not satisfied, low-temperature flexibility could not be secured, and waterproof performance could not be achieved. Furthermore, the mixing stability was reduced, so water could penetrate through lumps and granules that were generated during mixing, which could reduce waterproof performance.

[0106] In Comparative Example 22, SEBS6, Wax 2, and Wax 4 were used. The amount of SEBS6 used in Comparative Example 22 was less than 9.0% by mass relative to the total mass of the asphalt composition, and the total amount of Wax 2 and Wax 4 was more than 5.5% by mass relative to the total mass of the asphalt composition. As a result, the frass embrittlement point of -15°C or less was not satisfied, low-temperature flexibility could not be secured, and waterproof performance could not be achieved. Furthermore, the mixing stability was reduced, so water could penetrate through the lumps and granules that were generated during mixing, which could reduce waterproof performance.

[0107] In Comparative Example 23, SEBS6 and Wax 2 were used. The amount of SEBS6 used in Comparative Example 23 was less than 9.0% by mass relative to the total mass of the asphalt composition, and the amount of Wax 2 was more than 5.5% by mass relative to the total mass of the asphalt composition. As a result, the frass embrittlement point of -15°C or less was not satisfied, low-temperature flexibility could not be secured, and waterproof performance could not be achieved. Furthermore, the mixing stability was reduced, and water could penetrate through the lumps and granules, which may reduce waterproof performance.

[0108] In Comparative Example 24, SEBS6 and Wax 2 were used. The amount of SEBS6 used in Comparative Example 24 was less than 9.0% by mass relative to the total mass of the asphalt composition. As a result, the frass embrittlement point of -15°C or less was not satisfied. Therefore, low-temperature flexibility could not be ensured, and waterproof performance could not be exhibited.

[0109] In Comparative Example 25, SEBS4 and Wax 2 were used. The SEBS4 used in Comparative Example 25 had a styrene content of more than 35.0% by mass relative to the SEBS mass. The styrene content was less than 9.0% by mass relative to the total mass of the asphalt composition. As a result, in the mixing stability test, lumps and grains with a diameter of 1 mm or more were generated. Therefore, mixing stability could not be ensured. In addition, the Frass embrittlement point of -15°C or less was not satisfied. Therefore, low-temperature flexibility could not be ensured, and waterproof performance could not be exhibited. Furthermore, the softening point was less than 97°C. Therefore, deformation resistance could not be ensured, and waterproof performance could not be exhibited.

[0110] In Comparative Example 26, SEBS4 and Wax 2 were used. The SEBS4 used in Comparative Example 26 had a styrene content of more than 35.0% by mass relative to the SEBS mass. The SEBS4 content was 9.0% by mass or more and less than 10.5% by mass relative to the total mass of the asphalt composition. As a result, in the mixing stability test, lumps and grains with a diameter of 1 mm or more were generated. Therefore, mixing stability could not be ensured. Furthermore, the furth embrittlement point of -15°C or less was not satisfied. Therefore, low-temperature flexibility could not be ensured, and waterproof performance could not be exhibited.

[0111] In Comparative Example 27, SEBS6 and Wax 2 were used. The amount of Wax 2 used in Comparative Example 27 was less than 3.0% by mass relative to the total mass of the asphalt composition. As a result, the sagging length exceeded 8 mm, sagging resistance could not be ensured, sagging occurred even after construction, and adhesion to the waterproof sheet was insufficient, failing to exhibit waterproof performance.

[0112] In Comparative Example 28, SEBS6 and Wax 2 were used. The amount of Wax 2 used in Comparative Example 28 was less than 3.0% by mass relative to the total mass of the asphalt composition. As a result, the sagging length exceeded 8 mm, sagging resistance could not be ensured, sagging occurred even after construction, and adhesion to the waterproof sheet was insufficient, failing to exhibit waterproof performance.

[0113] In Comparative Example 29, SEBS7 and Wax 1 were used. The amount of SEBS7 used in Comparative Example 29 was more than 10.5% by mass relative to the total mass of the asphalt composition. As a result, the viscosity (200°C) exceeded 250 mPa·s. For this reason, a melting temperature of about 260°C was required, and the melting temperature could not be reduced. As a result, the odor generated during melting could not be suppressed.

[0114] In Comparative Example 30, SEBS4 and Wax 1 were used. The SEBS4 used in Comparative Example 30 had a styrene content of more than 35.0% by mass relative to the mass of SEBS. As a result, in the mixed stability test, lumps and grains with a diameter of 1 mm or more were generated. For this reason, mixed stability could not be ensured.

[0115] In Comparative Example 31, SEBS5 and Wax 1 were used. The SEBS5 used in Comparative Example 31 had a styrene content of more than 35.0% by mass relative to the mass of SEBS. As a result, in the mixed stability test, lumps and grains with a diameter of 1 mm or more were generated. For this reason, the mixed stability could not be ensured.

[0116] In Comparative Example 32, SEBS7 and Wax 1 were used. The amount of SEBS7 used in Comparative Example 32 was more than 10.5% by mass relative to the total mass of the asphalt composition, and the amount of Wax 1 used was more than 5.5% by mass relative to the total mass of the asphalt composition. As a result, the viscosity (200°C) exceeded 250 mPa·s. For this reason, a melting temperature of about 260°C was required, and the melting temperature could not be reduced. As a result, the odor generated during melting could not be suppressed.

[0117] In Comparative Example 33, SEBS7 and Wax 1 were used. The amount of SEBS7 used in Comparative Example 33 was more than 10.5% by mass relative to the total mass of the asphalt composition, and the amount of Wax 1 used was more than 5.5% by mass relative to the total mass of the asphalt composition. As a result, the viscosity (200°C) exceeded 250 mPa·s. For this reason, a melting temperature of about 260°C was required, and the melting temperature could not be reduced. As a result, the odor generated during melting could not be suppressed.

[0118] In Comparative Example 34, SBS and Wax 1 were used. SEBS was not blended in Comparative Example 34. As a result, the difference in the furth embrittlement point before and after the heat stability test was 13°C. This means that the low-temperature flexibility is greatly impaired by heating for melting during waterproofing work, increasing the possibility of cracking, and waterproofing performance cannot be achieved.

[0119] In Comparative Example 35, SEBS7 and Wax 3 were used. The Wax 3 used in Comparative Example 35 had a melt viscosity of more than 100 mPa·s at 150°C. As a result, the viscosity (200°C) exceeded 250 mPa·s. This required a melting temperature of about 260°C, and the melting temperature could not be reduced. As a result, the odor generated during melting could not be suppressed.

[0120] In Comparative Example 36, SEBS7 and Wax 4 were used. The Wax 4 used in Comparative Example 35 had a crystallinity of less than 70% and a melt viscosity at 150°C of more than 100 mPa·s. As a result, the viscosity (200°C) exceeded 250 mPa·s. For this reason, a melting temperature of about 260°C was required, and the melting temperature could not be reduced. As a result, the odor generated during melting could not be suppressed. In addition, the sagging length exceeded 8 mm. For this reason, sagging resistance could not be ensured, and waterproof performance could not be exhibited. [Explanation of symbols]

[0121] 100: Asphalt manufacturing plant 101: Base asphalt container 102: Mixing container 103: Product container 104: First supply pipe 105: Stirring device 106: Additive supply device 107: Second supply pipe 108: Control device 109: Processing equipment 110: Storage device 111: Input device

Claims

1. Penetration: 17 or more and 40 or less, Softening point: 97℃ or higher, Viscosity at 200 ° C: 250 mPa s or less, Frass embrittlement point: -15°C or less, Sagging length: 8mm or less Heating stability: 5℃ or less And, the particle size of the composition is less than 1 mm in maximum diameter; The composition comprises a base asphalt, a hydrogenated elastomer, and a wax; The hydrogenated elastomer: 9.0% by mass or more and 10.5% by mass or less, The wax: 3.0% by mass or more and 5.5% by mass or less; The hydrogenated elastomer has a styrene content of 27.0% by mass or more and 35.0% by mass or less, The wax has a crystallinity of 70% or more and a melt viscosity at 150°C of 100 mPa s or less, The hydrogenated elastomer is a styrene-ethylene / butadiene-styrene block copolymer (SEBS) having a 20% toluene solution viscosity of 0.3 Pa·s or more and 0.8 Pa·s or less, The asphalt composition, wherein the wax is a polyethylene or polyester to which an acid has been added.

2. The wax: 3.0% by mass or more and 4.0% by mass or less The asphalt composition of claim 1.

3. The hydrogenated elastomer has a styrene content of 27.0% by mass or more and 30.0% by mass or less. The asphalt composition according to claim 1 or 2.

4. An apparatus for producing the asphalt composition according to any one of claims 1 to 3.

5. A system for producing an asphalt composition according to any one of claims 1 to 3.

6. The composition comprises a base asphalt, a hydrogenated elastomer, and a wax; The hydrogenated elastomer: 9.0% by mass or more and 10.5% by mass or less, The wax: 3.0% by mass or more and 5.5% by mass or less; The hydrogenated elastomer has a styrene content of 27.0% by mass or more and 35.0% by mass or less, The wax has a crystallinity of 70% or more and a melt viscosity at 150° C. of 100 mPa s or less, The hydrogenated elastomer is a styrene-ethylene / butadiene-styrene block copolymer (SEBS) having a 20% toluene solution viscosity of 0.3 Pa·s or more and 0.8 Pa·s or less, The asphalt composition, wherein the wax is a polyethylene or polyester to which an acid has been added.

7. The wax: 3.0% by mass or more and 4.0% by mass or less The asphalt composition of claim 6.

8. The hydrogenated elastomer has a styrene content of 27.0% by mass or more and 30.0% by mass or less. The asphalt composition according to claim 6 or 7.

9. An apparatus for producing an asphalt composition according to any one of claims 6 to 8.

10. A system for producing an asphalt composition according to any one of claims 6 to 8.

11. The method includes a step of mixing 9.0% by mass or more and 10.5% by mass or less of a hydrogenated elastomer and 3.0% by mass or more and 5.5% by mass or less of a wax with a base asphalt to produce an asphalt composition, The asphalt composition comprises the base asphalt, the hydrogenated elastomer, and the wax, The hydrogenated elastomer has a styrene content of 27.0% by mass or more and 35.0% by mass or less, The wax has a crystallinity of 70% or more and a melt viscosity at 150° C. of 100 mPa s or less, The hydrogenated elastomer is a styrene-ethylene / butadiene-styrene block copolymer (SEBS) having a 20% toluene solution viscosity of 0.3 Pa·s or more and 0.8 Pa·s or less, The wax is polyethylene or polyester to which an acid has been added. A method for producing an asphalt composition, comprising the steps of:

Citation Information

Patent Citations

  • Improved asphalt for heat construction method capable of being used at low temperature

    JP2007238956A

  • Low-carbon additive for medium-temperature asphalt mixtures, medium-temperature asphalt produced using the same, and method for producing medium-temperature asphalt mixtures.

    JP2012500329A

  • Modified asphalt composition for waterproof construction

    JP2013173824A