Laminate, cured product, and electronic component
The laminate of ultra-thin copper foil with a resin layer containing specific components addresses blistering and drilling issues, enhancing laser processing and reducing dielectric loss for finer circuit patterns.
Patent Information
- Application Number
- JP2021527658
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-06-27
- Filing Date
- 2020-06-23
- Publication Date
- 2024-09-20
- Estimated Expiration
- 2040-06-23
AI Technical Summary
The conventional methods for forming circuit patterns using resin-coated copper foil face issues such as blister formation during solder reflow, especially with thinner foils, and difficulty in achieving uniform thickness and laser processing, while also experiencing increased transmission loss due to higher frequencies.
A laminate comprising an ultra-thin copper foil with a thickness of 0.1 to 6 μm, a resin layer containing an epoxy resin, a compound with an active ester group, and an inorganic filler, with a specific ratio of epoxy groups to active ester groups in the resin layer, providing excellent laser drilling workability and reflow resistance, and a cured product with a low dielectric loss tangent.
The laminate achieves improved laser drilling precision, reflow resistance, and reduced dielectric loss, enabling the formation of fine circuits with excellent adhesion and thermal stability.
Smart Images

Figure 0007554745000019 
Figure 0007554745000015 
Figure 0007554745000014
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminate, a cured product, and an electronic component. [Background technology]
[0002] Resin coated copper foil (RCC), which is a laminate of copper foil and a curable resin layer, is used as a material for forming electronic components such as printed wiring boards (for example, Patent Document 1). As a conventionally used resin coated copper foil, one having a curable resin layer prepared by applying an epoxy resin composition to copper foil is widely known.
[0003] In recent years, in order to further miniaturize circuit patterns, the MSAP (Modified Semi-Additive Process) method has been increasingly used instead of the conventional subtractive method. For example, there is a method for manufacturing build-up wiring boards in which a resin-coated copper foil is laminated by heat lamination so that the resin layer side is in contact with a circuit board on which a circuit pattern has been formed, and then the copper foil is thermally cured, followed by laser processing, desmearing, plating, etc. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2006-89595 A Summary of the Invention [Problem to be solved by the invention]
[0005] When a circuit is formed using the resin-coated copper foil by the above-mentioned manufacturing method, there is a problem that defects such as blistering are likely to occur during solder reflow. Moreover, such defects during solder reflow are more noticeable as the copper foil of the resin-coated copper foil becomes thinner.
[0006] If the copper foil is made thicker to prevent defects during solder reflow, laser processing becomes difficult. Therefore, it was considered to first make the copper foil of the resin-coated copper foil thicker, heat-press the resin-coated copper foil, thin the copper foil with an etching solution, and then perform laser processing. However, it is difficult to form a thin film with a uniform thickness, and therefore there was a problem that the opening diameter becomes non-uniform when holes are drilled with a laser.
[0007] Furthermore, in recent years, with the adoption of high-speed communications, i.e., higher frequencies, transmission loss has tended to increase, and therefore materials for electronic components are required to have low dielectric tangents that can suppress transmission loss.
[0008] Therefore, an object of the present invention is to provide a laminate having an ultra-thin copper foil and a resin layer, which has excellent laser drilling processability and reflow resistance and in which the cured product of the resin layer has a low dielectric tangent, a cured product of the resin layer of the laminate, and an electronic component having the cured product. [Means for solving the problem]
[0009] As a result of intensive research aimed at achieving the above object, the present inventors discovered that the above problem could be solved by providing an ultra-thin copper foil with a carrier foil with a resin layer containing an epoxy resin, a compound having an active ester group, and an inorganic filler, and thus completed the invention.
[0010] That is, the laminate of the present invention is a laminate having at least a carrier foil, an ultrathin copper foil having a thickness of 0.1 to 6 μm, and a resin layer, in that order, and is characterized in that the resin layer contains (A) an epoxy resin, (B) a compound having an active ester group, and (C) an inorganic filler.
[0011] In the laminate of the present invention, the ratio of the total amount of epoxy groups in the epoxy resin (A) to the total amount of active ester groups in the compound (B) having an active ester group in the resin layer is preferably 0.20 to 0.60.
[0012] In the laminate of the present invention, the blending amount of the (C) inorganic filler is preferably 50% by mass or more, based on 100% by mass of the nonvolatile components in the resin layer.
[0013] In the laminate of the present invention, the compound (B) having an active ester group is represented by the following general formula (1): TIFF0007554745000001.tif22164 (wherein X1 are each independently a group having a benzene ring or a naphthalene ring, k represents 0 or 1, and n is an average of 0.25 to 1.5 for the repeating units).
[0014] In the laminate of the present invention, the compound (B) having an active ester group is represented by the following general formula (2): TIFF0007554745000002.tif31164 (In formula (2), X2 is independently represented by the following formula (3): A group represented by TIFF0007554745000003.tif25164 or the following formula (4): A group represented by TIFF0007554745000004.tif39164, m is an integer from 1 to 6, each n is independently an integer from 1 to 5, and each q is independently an integer from 1 to 6; In formula (3), k's each independently represent an integer of 1 to 5, In formula (4), Y is a group represented by formula (3) above (wherein k is an integer of 1 to 5, and t is an integer of 0 to 5). and a compound having a structure represented by the following formula (1) and both terminals of which are monovalent aryloxy groups.
[0015] In the laminate of the present invention, the ratio of the total amount of epoxy groups in the epoxy resin (A) to the total amount of active ester groups in the compound (B) having an active ester group in the resin layer is preferably 0.20 to 0.50.
[0016] In the laminate of the present invention, the resin layer preferably has a dielectric loss tangent of 0.01 or less after curing.
[0017] The electronic device of the present invention is characterized by having a cured product obtained by curing the resin layer of the laminate. Effect of the Invention
[0018] According to the present invention, it is possible to provide a laminate having an ultra-thin copper foil and a resin layer, which has excellent laser drilling processability and reflow resistance and in which the cured product of the resin layer has a low dielectric tangent, a cured product of the resin layer of the laminate, and an electronic component having the cured product. [Brief description of the drawings]
[0019] [Figure 1] 1 is a schematic cross-sectional view showing one embodiment of a laminate of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] The laminate of the present invention is a laminate having at least a carrier foil, an ultra-thin copper foil having a thickness of 0.1 to 6 μm, and a resin layer in this order, characterized in that the resin layer contains (A) an epoxy resin, (B) a compound having an active ester group, and (C) an inorganic filler. Since the ultra-thin copper foil is supported on the carrier foil, the laminate is easy to handle, and the laminate is easy to manufacture and laminate. In addition, since it is not necessary to thin the copper foil by etching after thermocompression bonding, which causes unevenness in the film thickness, the laminate is also excellent in laser drilling processability. Furthermore, by combining the ultra-thin copper foil having a thickness of 0.1 to 6 μm with the resin layer containing the components (A) to (C), a cured product having excellent reflow resistance and low dielectric loss tangent can be obtained. In this specification, when the surface of the ultra-thin copper foil is roughened, the uneven portion is not included in the thickness. In other words, when the ultra-thin copper foil is roughened, the thickness of the ultra-thin copper foil is the thickness of the part excluding the unevenness of the roughened surface, that is, the thickness of the bulk (base) part excluding the profile of the roughened surface.
[0021] 1 is a schematic cross-sectional view showing one embodiment of the laminate of the present invention. The laminate 1 has a carrier foil 2, an ultrathin copper foil 3, and a resin layer 4 laminated in this order.
[0022] In the laminate of the present invention, the ratio of the total amount of epoxy groups of the epoxy resin (A) in the resin layer to the total amount of active ester groups of the compound having an active ester group (B) is preferably 0.20 to 0.60, and a cured product having high heat resistance, low dielectric tangent, and low linear thermal expansion coefficient can be obtained. In general, when a large amount of a compound having an active ester group is blended, the crosslink density of the cured product decreases, the glass transition temperature (Tg) of the cured product decreases, and the heat resistance is considered to deteriorate. Therefore, usually, an excessive amount of a compound having an active ester group is not blended in excess of the epoxy equivalent of the epoxy resin in the composition, but even if the compound is blended in the above specific amount, it is unexpectedly possible to obtain a cured product having a high glass transition temperature (Tg), low dielectric tangent, and low linear thermal expansion coefficient. As a result, a cured product having excellent reflow resistance and low dielectric tangent can be obtained. Although the detailed mechanism is not clear, it is considered that when the ratio of the compound having an active ester group, preferably the compound having an active ester group having the structure of the following general formula (1) or (2), is increased, the volume ratio of the active ester structure, i.e., the aromatic ester structure having a rigidity and high molecular orientation, increases, thereby controlling the movement of the chain portion between the crosslinking points, and thus improving the glass transition temperature. The total amount of epoxy groups in the (A) epoxy resin can be obtained by dividing the amount of the (A) epoxy resin contained in the composition by the epoxy equivalent of the (A) epoxy resin. The total amount of active ester groups in the (B) compound having an active ester group can be obtained by dividing the amount of the (B) compound having an active ester group contained in the composition by the active ester equivalent of the (B) compound having an active ester group. The upper limit of the ratio of the total amount is preferably 0.50 or less, more preferably 0.40 or less, and particularly preferably 0.30 or less, since a cured product with a lower dielectric tangent can be obtained.
[0023] The resin layer, ultrathin copper foil, and carrier foil of the laminate of the present invention will be described below. In this specification, when a numerical range is expressed with "~", it means a range including the numerical range (i.e., . . or more . . . or less).
[0024] [Resin layer] The resin layer contains (A) an epoxy resin, (B) a compound having an active ester group, and (C) an inorganic filler. The resin layer can be obtained by applying and drying a resin composition containing (A) an epoxy resin, (B) a compound having an active ester group, and (C) an inorganic filler.
[0025] [(A) Epoxy resin] The (A) epoxy resin is a resin having an epoxy group, and any of those known in the art can be used. Examples include bifunctional epoxy resins having two epoxy groups in the molecule, and polyfunctional epoxy resins having many epoxy groups in the molecule. In addition, hydrogenated bifunctional epoxy resins may be used. The (A) epoxy resin may be any of solid epoxy resins, semi-solid epoxy resins, and liquid epoxy resins. In this specification, the solid epoxy resin refers to an epoxy resin that is solid at 40°C, the semi-solid epoxy resin refers to an epoxy resin that is solid at 20°C and liquid at 40°C, and the liquid epoxy resin refers to an epoxy resin that is liquid at 20°C. The liquid state is determined in accordance with the "Method of Confirming Liquid State" in Appendix 2 of the Ministerial Ordinance on the Testing and Properties of Hazardous Materials (Ministry of Home Affairs Ordinance No. 1 of 1989). For example, the method described in paragraphs 23 to 25 of JP 2016-079384 A is used. The (A) epoxy resin may be used alone or in combination of two or more types.
[0026] In the present invention, as described above, the ratio of the total amount of epoxy groups in the epoxy resin (A) in the resin layer to the total amount of active ester groups in the compound having an active ester group (B) is preferably 0.20 to 0.60, and in this case, it is preferable that the epoxy resin (A) contains at least one of a liquid epoxy resin having three or more functionalities and a semi-solid epoxy resin having three or more functionalities. When a liquid epoxy resin having three or more functionalities or a semi-solid epoxy resin having three or more functionalities is contained, the glass transition temperature can be improved while maintaining a low dielectric tangent. As a commercially available product of such a liquid epoxy resin having three or more functionalities, for example, TEPIC-VL manufactured by Nissan Chemical Industries, Ltd., jER630 manufactured by Mitsubishi Chemical Corporation, etc. can be used. In addition, as a commercially available product of such a semi-solid epoxy resin having three or more functionalities, for example, jER604 manufactured by Mitsubishi Chemical Corporation can be used.
[0027] The epoxy equivalent of the (A) epoxy resin is preferably 100 to 5000 g / eq., and more preferably 150 to 3000 g / eq. For example, the (A) epoxy resin may contain a liquid or semi-solid epoxy resin having an epoxy equivalent of 350 to 1000 g / eq.
[0028] (A) Epoxy resin is not limited to the above, and examples of solid epoxy resins include naphthalene type epoxy resins such as EPICLON HP-4700 manufactured by DIC Corporation, naphthalene skeleton-containing novolac type epoxy resins such as NC-7000 manufactured by Nippon Kayaku Co., Ltd., naphthol aralkyl type epoxy resins such as ESN-475V manufactured by Nippon Steel Chemical & Material Co., Ltd., epoxidized products of condensation products of phenols and aromatic aldehydes having a phenolic hydroxyl group (trisphenol type epoxy resins) such as EPPN-502H manufactured by Nippon Kayaku Co., Ltd., dicyclopentadiene type epoxy resins such as EPICLON HP-7200H manufactured by DIC Corporation, biphenyl aralkyl type epoxy resins such as NC-3000H and NC-3000L manufactured by Nippon Kayaku Co., Ltd., and EPICLON Examples of such epoxy resins include novolac epoxy resins such as N680 and EOCN-104S manufactured by Nippon Kayaku Co., Ltd.; biphenyl epoxy resins such as YX-4000 manufactured by Mitsubishi Chemical Co., Ltd.; phosphorus-containing epoxy resins such as TX0712 manufactured by Nippon Steel Chemical & Materials Co., Ltd.; and tris(2,3-epoxypropyl)isocyanurate such as TEPIC manufactured by Nissan Chemical Co., Ltd. By including a solid epoxy resin, the glass transition temperature of the cured product is increased and the heat resistance is excellent. When the ratio of the total amount of epoxy groups of the (A) epoxy resin in the resin layer to the total amount of active ester groups of the (B) compound having an active ester group is 0.20 to 0.60, among the solid epoxy resins, a cured product having a higher Tg, excellent reflow resistance, and low dielectric tangent is obtained, and therefore, an aralkyl epoxy resin such as ESN-475V or NC3000H, i.e., an epoxy resin containing a divalent group in which an alkylene group and an arylene group are bonded, is preferred. Examples of the alkylene group include a methylene group, a methylmethylene group, an ethylene group, a propylene group, a trimethylene group, etc. Examples of the arylene group include a phenylene group, a biphenylene group, a naphthylene group, etc.
[0029] Examples of semi-solid epoxy resins include bisphenol A type epoxy resins such as EPICLON860, EPICLON900-IM, EPICLON EXA-4816, and EPICLON EXA-4822 manufactured by DIC Corporation, Epotohto YD-134 manufactured by Nippon Steel Chemical & Materials Co., Ltd., jER834 and jER872 manufactured by Mitsubishi Chemical Co., Ltd., and ELA-134 manufactured by Sumitomo Chemical Co., Ltd.; naphthalene type epoxy resins such as EPICLON HP-4032 manufactured by DIC Corporation; phenol novolac type epoxy resins such as EPICLON N-740 manufactured by DIC Corporation, and aromatic amino epoxy resins such as jER604 manufactured by Mitsubishi Chemical Co., Ltd. By including a semi-solid epoxy resin, the glass transition temperature (Tg) of the cured product is high, the coefficient of linear thermal expansion (CTE) is low, and the crack resistance is excellent. By including a semi-solid epoxy resin, the storage stability of the dry film is excellent, and cracking and peeling can be prevented.
[0030] Examples of liquid epoxy resins include aromatic aminoepoxy resins such as bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol AF type epoxy resins, phenol novolac type epoxy resins, tert-butyl-catechol type epoxy resins, glycidylamine type epoxy resins, and aminophenol type epoxy resins, alicyclic epoxy resins, and heterocyclic epoxy resins. By including a liquid epoxy resin, the flexibility of the laminate is excellent.
[0031] The epoxy resin (A) is preferably a combination of a solid epoxy resin and at least one of a liquid epoxy resin and a semi-solid epoxy resin. A solid epoxy resin, a liquid epoxy resin, and a semi-solid epoxy resin may also be used in combination.
[0032] The blending amount of the (A) epoxy resin is preferably 50% by mass or less, more preferably 40% by mass or less, and particularly preferably 30% by mass or less, since a cured product with a lower dielectric tangent can be obtained when the non-volatile components in the resin layer are taken as 100% by mass. From the viewpoint of the strength of the cured product, the lower limit is preferably 1% by mass or more, and more preferably 3% by mass or more.
[0033] The resin layer of the laminate of the present invention may contain a thermosetting resin other than the epoxy resin (A) as long as the effects of the present invention are not impaired. For example, a known and commonly used thermosetting resin such as an isocyanate compound, a blocked isocyanate compound, an amino resin, a benzoxazine resin, a carbodiimide resin, a cyclocarbonate compound, a polyfunctional oxetane compound, an episulfide resin, or a maleimide resin can be used.
[0034] [(B) Compound having an active ester group] (B) The compound having an active ester group is preferably a compound having two or more active ester groups in one molecule. The compound having an active ester group can generally be obtained by a condensation reaction between a carboxylic acid compound and a hydroxy compound. Among them, a compound having an active ester group obtained by using a phenol compound or a naphthol compound as a hydroxy compound is preferable. Examples of the phenol compound or naphthol compound include hydroquinone, resorcin, bisphenol A, bisphenol F, bisphenol S, phenolphthaline, methylated bisphenol A, methylated bisphenol F, methylated bisphenol S, phenol, o-cresol, m-cresol, p-cresol, catechol, α-naphthol, β-naphthol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucin, benzenetriol, dicyclopentadienyl diphenol, and phenol novolak. The (B) compound having an active ester group may be a naphthalenediol alkyl / benzoic acid type. The (B) compound having an active ester group may be used alone or in combination of two or more. The (B) compound having an active ester group is preferably one having a benzene, α-naphthol, β-naphthol, or dicyclopentadiene skeleton.
[0035] When the non-volatile components in the resin layer are taken as 100% by mass, the upper limit of the compound having an active ester group is preferably 50% by mass or less, more preferably 45% by mass or less, and particularly preferably 40% by mass or less, from the viewpoint of the strength of the cured product. In addition, the lower limit is preferably 5% by mass or more, and more preferably 10% by mass or more, in order to obtain a cured product with a lower dielectric tangent.
[0036] Among the compounds having an active ester group (B), the following compounds having an active ester group (B1) and (B2) can be preferably used. In addition, the compound having an active ester group (B2) is more preferred because it can lower the dielectric tangent of the cured product.
[0037] (B1) The compound having an active ester group (B1) has a structure obtained by reacting (b1) a phenolic resin having a molecular structure in which phenols are bonded via an aliphatic cyclic hydrocarbon group, (b2) an aromatic dicarboxylic acid or its halide, and (b3) an aromatic monohydroxy compound. It is preferable that the compound has a structure obtained by reacting in a ratio of 0.05 to 0.75 mol of the phenolic hydroxyl group in the phenolic resin (b1) and 0.25 to 0.95 mol of the aromatic monohydroxy compound (b3) per 1 mol of the carboxyl group or acid halide group in the aromatic dicarboxylic acid (b2) or its halide.
[0038] Here, in the (b1) phenolic resin, the molecular structure in which phenols are connected via an aliphatic cyclic hydrocarbon group includes a structure obtained by polyaddition reaction of an unsaturated aliphatic cyclic hydrocarbon compound containing two double bonds in one molecule with a phenol. Here, examples of the phenols include phenol and substituted phenols in which one or more alkyl groups, alkenyl groups, allyl groups, aryl groups, aralkyl groups, or halogen groups are substituted. Specific examples include cresol, xylenol, ethylphenol, isopropylphenol, butylphenol, octylphenol, nonylphenol, vinylphenol, isopropenylphenol, allylphenol, phenylphenol, benzylphenol, chlorophenol, bromophenol, naphthol, and dihydroxynaphthalene, but are not limited thereto. Mixtures of these may also be used. Among these, phenol is particularly preferred because of its excellent fluidity and curability.
[0039] Specific examples of unsaturated alicyclic hydrocarbon compounds include dicyclopentadiene, tetrahydroindene, 4-vinylcyclohexene, 5-vinylnorbon-2-ene, α-pinene, β-pinene, and limonene. Among these, dicyclopentadiene is preferred in terms of balance of properties, particularly heat resistance and hygroscopicity. Since dicyclopentadiene is contained in petroleum fractions, industrial dicyclopentadiene may contain other aliphatic or aromatic dienes as impurities. However, in consideration of heat resistance, curability, moldability, and the like, it is desirable for the product to have a purity of dicyclopentadiene of 90% by mass or more.
[0040] Next, the (b2) aromatic dicarboxylic acid or its halide may be an aromatic dicarboxylic acid such as isophthalic acid, terephthalic acid, 1,4-, 2,3-, or 2,6-naphthalenedicarboxylic acid, or an acid halide thereof such as an acid fluoride, an acid chloride, an acid bromide, or an acid iodide. Among these, an acid chloride of an aromatic dicarboxylic acid is preferable because of its particularly good reactivity, and among these, isophthalic acid dichloride and terephthalic acid dichloride are particularly preferable, and isophthalic acid dichloride is particularly preferable.
[0041] Examples of aromatic monohydroxy compounds include phenol, alkylphenols such as o-cresol, m-cresol, p-cresol, and 3,5-xylenol, aralkylphenols such as o-phenylphenol, p-phenylphenol, 2-benzylphenol, 4-benzylphenol, and 4-(α-cumyl)phenol, and naphthols such as α-naphthol and β-naphthol. Among these, α-naphthol and β-naphthol are preferred because they lower the dielectric tangent of the cured product.
[0042] The (B1) active ester compound has a structure obtained by reacting (b1) a phenol resin, (b2) an aromatic dicarboxylic acid or its halide, and (b3) an aromatic monohydroxy compound, and in particular has a structure represented by the following general formula (1): TIFF0007554745000005.tif22164 (wherein X1 is a group having a benzene ring or a naphthalene ring, k is 0 or 1, and n is the average value of the repeating units and is 0.05 to 2.5.) The structure represented by the formula (1) is particularly preferred because it provides a low dielectric tangent of the cured product and a low solution viscosity when dissolved in an organic solvent. The group having a benzene ring or a naphthalene ring is not particularly limited and may be a phenyl group, a naphthyl group, or the like, and the benzene ring or the naphthalene ring may be bonded to the molecular end via another atom, or may have a substituent. In addition, it is preferred that the (B1) active ester compound has a naphthalene ring at its molecular end.
[0043] In particular, the value of n in the above general formula (1), i.e., the average number of repeating units, is preferably in the range of 0.25 to 1.5, since the solution viscosity is low and the laminate can be easily produced. Also, in the above general formula (1), the value of k is preferably 0, from the viewpoints of high heat resistance and low dielectric tangent.
[0044] Here, n in the above general formula (1) can be determined as follows. [How to determine n in general formula (1)] By GPC measurement performed under the following conditions, the ratios (β1 / α1, β2 / α2, β3 / α3, β4 / α4) of the styrene-equivalent molecular weights (α1, α2, α3, α4) corresponding to n=1, n=2, n=3, n=4 and the theoretical molecular weights (β1, β2, β3, β4) corresponding to n=1, n=2, n=3, n=4 are calculated, and the average value of these (β1 / α1 to β4 / α4) is calculated. The number average molecular weight (Mn) calculated by GPC is multiplied by this average value to obtain the average molecular weight. Next, the value of n is calculated by taking the molecular weight of the general formula (1) as the average molecular weight.
[0045] (GPC measurement conditions) Measurement equipment: Tosoh Corporation "HLC-8220 GPC" Column: Tosoh guard column "H XL -L” +Tosoh Corporation "TSK-GEL G2000HXL" +Tosoh Corporation "TSK-GEL G2000HXL" +Tosoh Corporation "TSK-GEL G3000HXL" +Tosoh Corporation "TSK-GEL G4000HXL" Detector: RI (differential refractive index) Data processing: Tosoh Corporation "GPC-8020 Model II Version 4.10" Measurement conditions: Column temperature 40℃ Developing solvent: Tetrahydrofuran Flow rate 1.0ml / min Standard: In accordance with the measurement manual for the above-mentioned "GPC-8020 Model II Version 4.10," the following monodisperse polystyrene with known molecular weight was used. (Polystyrene used) Tosoh "A-500" Tosoh "A-1000" Tosoh "A-2500" Tosoh "A-5000" Tosoh "F-1" Tosoh "F-2" Tosoh "F-4" Tosoh "F-10" Tosoh "F-20" Tosoh "F-40" Tosoh "F-80" Tosoh "F-128" Sample: A tetrahydrofuran solution (1.0 mass % in terms of resin solid content) filtered through a microfilter (50 μl).
[0046] Specifically, the method of reacting (b1) a phenol resin, (b2) an aromatic dicarboxylic acid or its halide, and (b3) an aromatic monohydroxy compound can be carried out by reacting these components in the presence of an alkali catalyst. Examples of the alkali catalyst that can be used here include sodium hydroxide, potassium hydroxide, triethylamine, pyridine, etc. Among these, sodium hydroxide and potassium hydroxide are particularly preferred because they can be used in the form of an aqueous solution and provide good productivity.
[0047] Specifically, the reaction may be carried out by mixing (b1) a phenol resin, (b2) an aromatic dicarboxylic acid or its halide, and (b3) an aromatic monohydroxy compound in the presence of an organic solvent, and reacting the mixture while continuously or intermittently dropping the alkali catalyst or its aqueous solution. In this case, the concentration of the aqueous alkali catalyst is preferably in the range of 3.0 to 30%. Examples of organic solvents that can be used here include toluene and dichloromethane.
[0048] After the reaction is completed, in the case of using an aqueous solution of an alkaline catalyst, the reaction liquid is allowed to stand for liquid separation, the aqueous layer is removed, and the remaining organic layer is washed repeatedly until the aqueous layer becomes nearly neutral, thereby obtaining the target resin.
[0049] The compound having an active ester group (B1) thus obtained is usually obtained as a solution in an organic solvent, and therefore it can be mixed as it is with other compounding components, and further, the amount of organic solvent can be appropriately adjusted to produce the desired curable resin composition. The active ester compound (B1) is characterized by having a low melt viscosity when dissolved in an organic solvent to form a resin solution; specifically, when the active ester resin is made into a toluene solution with a non-volatile content of 65%, the solution viscosity is 300 to 10,000 mPa·s (25°C).
[0050] (B2) The compound having an active ester group of (B2) is represented by the following general formula (2): It has a resin structure having a structural moiety represented by TIFF0007554745000006.tif31164, and both ends of the structural moiety are monovalent aryloxy groups.
[0051] (In formula (2), X2 each independently represents the following formula (3): A group represented by TIFF0007554745000007.tif25164 or the following formula (4): each n is independently an integer of 1 to 5; each q is independently an integer of 0 to 6; in formula (3), each k is independently an integer of 1 to 5; and in formula (4), Y is a group represented by formula (3) above (each k is independently an integer of 1 to 5); and each t is independently an integer of 0 to 5).
[0052] The compound having an active ester group of (B2) is represented by the general formula (2) The partial structure represented by TIFF0007554745000009.tif29164 is preferably a structure derived from a modified naphthalene compound having a hydroxyl group equivalent of 170 to 200 g / eq.
[0053] In order to clarify the relationship between m and n in formula (2), several patterns are shown below as examples, but the active ester resin (B2) is not limited to these. For example, when m=1, formula (2) represents the structure of formula (2-I) below.
[0054] TIFF0007554745000010.tif29164
[0055] In formula (2-I), n is an integer of 1 to 5, and each q is independently an integer of 0 to 6. As with the relationship between m and n, when n is 2 or more, each q is independently an integer of 0 to 6.
[0056] Furthermore, for example, when m=2, formula (2) represents a structure of the following formula (2-II).
[0057] TIFF0007554745000011.tif29167
[0058] In formula (2-II), n is independently an integer of 1 to 5, and q is independently an integer of 0 to 6. As with the relationship between m and n, when n is 2 or more, each q is independently an integer of 0 to 6.
[0059] The compound having an active ester group (B2) has a naphthylene ether structural moiety in the main molecular skeleton, and therefore can impart superior heat resistance and flame retardancy to the cured product. TIFF0007554745000012.tif23167, the cured product can have excellent dielectric properties. In addition, the resin structure of the compound having an active ester group (B2) has aryloxy groups at both ends, which improves the thermal decomposition resistance of the cured product to a sufficient degree even in multilayer printed circuit board applications.
[0060] The compound having an active ester group (B2) preferably has a softening point in the range of 100 to 200° C., particularly 100 to 190° C., in order to provide a cured product with excellent heat resistance.
[0061] In the compound having an active ester group (B2), m in formula (2) is an integer of 1 to 6. Of these, m is preferably an integer of 1 to 5. Also, n in formula (2) is each independently an integer of 1 to 5. Of these, n is preferably an integer of 1 to 3. In formula (2), the relationship between m and n is described for confirmation. For example, when m is an integer of 2 or more, n is 2 or more, and in that case, each n is an independent value. As long as it is within the numerical range of n, it may be the same value or different values.
[0062] In the compound having an active ester group of (B2), when q in formula (2) is 1 or more, X2 substitutes at any position in the naphthalene ring structure.
[0063] The aryloxy groups at both ends of the resin structure may be derived from monohydric phenol compounds such as phenol, cresol, pt-butylphenol (para-tertiary butylphenol), 1-naphthol, 2-naphthol, etc. Among these, from the viewpoint of thermal decomposition resistance of the cured product, a phenoxy group, a tolyloxy group, or a 1-naphthyloxy group is preferred, and a 1-naphthyloxy group is more preferred.
[0064] The method for producing the compound having an active ester group (B2) will be described in detail below. The method for producing a compound having an active ester group (B2) comprises a step of reacting a dihydroxynaphthalene compound with benzyl alcohol in the presence of an acid catalyst to obtain a benzyl-modified naphthalene compound (hereinafter, this step may be abbreviated as "step 1"), and then a step of reacting the obtained benzyl-modified naphthalene compound with an aromatic dicarboxylic acid chloride and a monohydric phenol compound (hereinafter, this step may be abbreviated as "step 2").
[0065] That is, in step 1, the dihydroxynaphthalene compound is reacted with benzyl alcohol in the presence of an acid catalyst to obtain a benzyl-modified naphthalene compound having a naphthylene structure as the main skeleton, phenolic hydroxyl groups at both ends of the main skeleton, and a benzyl group pendantly bonded to the aromatic nucleus of the naphthylene structure. It should be noted here that, in general, when a dihydroxynaphthalene compound is converted into naphthylene ether under an acid catalyst, it is extremely difficult to control the molecular weight, and a high molecular weight product is obtained, whereas the above-mentioned production method, by using benzyl alcohol in combination, can suppress such an increase in molecular weight, and a resin suitable for electronic material applications can be obtained.
[0066] Furthermore, by adjusting the amount of benzyl alcohol used, the content of benzyl groups in the benzyl-modified naphthalene compound can be adjusted, and the melt viscosity of the benzyl-modified naphthalene compound can also be adjusted. That is, the reaction ratio of the dihydroxynaphthalene compound and the benzyl alcohol can usually be selected from a range in which the reaction ratio of the dihydroxynaphthalene compound and the benzyl alcohol (dihydroxynaphthalene compound) / (benzyl alcohol) is 1 / 0.1 to 1 / 10 on a molar basis, but from the perspective of the balance between heat resistance, flame retardancy, dielectric properties, and thermal decomposition resistance, the reaction ratio of the dihydroxynaphthalene compound and the benzyl alcohol (dihydroxynaphthalene compound) / (benzyl alcohol) on a molar basis is preferably in a range of 1 / 0.5 to 1 / 4.0.
[0067] Examples of the dihydroxynaphthalene compound that can be used herein include 1,2-dihydroxynaphthalene, 1,3-dihydroxynaphthalene, 1,4-dihydroxynaphthalene, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 1,7-dihydroxynaphthalene, 1,8-dihydroxynaphthalene, 2,3-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, 2,7-dihydroxynaphthalene, etc. Among these, 1,6-dihydroxynaphthalene or 2,7-dihydroxynaphthalene is preferred, and 2,7-dihydroxynaphthalene is more preferred, since the flame retardancy of the cured product of the obtained benzyl-modified naphthalene compound is further improved, and the dielectric tangent of the cured product is also lowered, resulting in improved dielectric properties.
[0068] Examples of the acid catalyst that can be used in the reaction of the dihydroxynaphthalene compound with benzyl alcohol in step 1 include inorganic acids such as phosphoric acid, sulfuric acid, and hydrochloric acid; organic acids such as oxalic acid, benzenesulfonic acid, toluenesulfonic acid, methanesulfonic acid, and fluoromethanesulfonic acid; and Friedel-Crafts catalysts such as aluminum chloride, zinc chloride, stannous chloride, ferric chloride, and diethyl sulfate.
[0069] The amount of the acid catalyst used can be appropriately selected depending on the target modification rate, etc., but for example, in the case of an inorganic acid or an organic acid, it is preferably in the range of 0.001 to 5.0 parts by mass, preferably 0.01 to 3.0 parts by mass, per 100 parts by mass of the dihydroxynaphthalene compound, and in the case of a Friedel-Crafts catalyst, it is preferably in the range of 0.2 to 3.0 mol, preferably 0.5 to 2.0 mol, per 1 mol of the dihydroxynaphthalene compound.
[0070] The reaction of the dihydroxynaphthalene compound with benzyl alcohol in the step 1 can be carried out without a solvent, or can be carried out in a solvent in order to increase the homogeneity in the reaction system. Examples of such solvents include mono- or diethers of ethylene glycol or diethylene glycol, such as ethylene glycol dimethyl ether, ethylene glycol diethyl ether, ethylene glycol dipropyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dipropyl ether, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monopropyl ether, and diethylene glycol monobutyl ether; non-polar aromatic solvents, such as benzene, toluene, and xylene; aprotic polar solvents, such as dimethylformamide and dimethylsulfoxide; and chlorobenzene.
[0071] A specific method for carrying out the reaction of the step 1 is to dissolve the dihydroxynaphthalene compound, benzyl alcohol and the acid catalyst in the absence of a solvent or in the presence of the solvent, and carry out the reaction under temperature conditions of 60 to 180°C, preferably about 80 to 160°C. The reaction time is not particularly limited, but is preferably 1 to 10 hours. Thus, the reaction can be specifically carried out by maintaining the temperature for 1 to 10 hours. In addition, it is preferable to distill off the water generated during the reaction from the system using a fractionating column or the like, since the reaction proceeds quickly and productivity is improved.
[0072] In addition, if the resulting benzyl-modified naphthalene compound is significantly colored, an antioxidant or a reducing agent may be added to the reaction system to suppress coloration. Examples of the antioxidant include hindered phenol compounds such as 2,6-dialkylphenol derivatives, divalent sulfur compounds, and phosphorous ester compounds containing a trivalent phosphorus atom. Examples of the reducing agent include hypophosphorous acid, phosphorous acid, thiosulfuric acid, sulfurous acid, hydrosulfite, or salts thereof.
[0073] After the reaction is completed, the acid catalyst is removed by neutralization, washing with water or decomposition, and the target resin having a phenolic hydroxyl group can be separated by a general operation such as extraction, distillation, etc. The neutralization and washing can be performed according to a conventional method, and for example, a basic substance such as sodium hydroxide, potassium hydroxide, sodium carbonate, ammonia, triethylenetetramine, or aniline can be used as a neutralizing agent.
[0074] Specific examples of the aromatic dicarboxylic acid chloride include acid chlorides of phthalic acid, isophthalic acid, terephthalic acid, 2,6-naphthalenedicarboxylic acid, 1,6-naphthalenedicarboxylic acid, and 2,7-naphthalenedicarboxylic acid. Among these, isophthalic acid chloride and terephthalic acid chloride are preferred from the viewpoint of the balance between solvent solubility and heat resistance.
[0075] Specific examples of the monohydric phenol compound include phenol, cresol, pt-butylphenol, 1-naphthol, 2-naphthol, etc. Among them, phenol, cresol, and 1-naphthol are preferred because of their good reactivity with carboxylic acid chloride, and 1-naphthol is more preferred because of their good thermal decomposition resistance.
[0076] Specifically, the method for reacting the benzyl-modified naphthalene compound, the aromatic dicarboxylic acid chloride and the monohydric phenol compound can be carried out by reacting these components in the presence of an alkali catalyst.
[0077] Examples of the alkali catalyst that can be used here include sodium hydroxide, potassium hydroxide, triethylamine, pyridine, etc. Among these, sodium hydroxide and potassium hydroxide are particularly preferred because they can be used in the form of an aqueous solution and provide good productivity.
[0078] Specifically, the reaction can be carried out by mixing the above-mentioned components in the presence of an organic solvent and continuously or intermittently dropping the alkali catalyst or its aqueous solution into the mixture. In this case, the concentration of the aqueous alkali catalyst solution is preferably in the range of 3.0 to 30% by mass. Examples of organic solvents that can be used here include toluene, dichloromethane, and chloroform.
[0079] After the reaction is completed, in the case of using an aqueous solution of an alkaline catalyst, the reaction liquid is allowed to stand for liquid separation, the aqueous layer is removed, and the remaining organic layer is washed repeatedly until the aqueous layer becomes nearly neutral, thereby obtaining the target resin.
[0080] The compound having an active ester group (B2) thus obtained preferably has a softening point of 100 to 200° C., since this increases the solubility in organic solvents.
[0081] The resin layer may contain a curing agent other than the compound having an active ester group (B) within a range that does not impair the effects of the present invention. Examples of the curing agent include a compound having a phenolic hydroxyl group, a polycarboxylic acid and an acid anhydride thereof, a compound having a cyanate ester group, a compound having a maleimide group, and an alicyclic olefin polymer.
[0082] ((C) Inorganic filler) The resin layer of the laminate of the present invention contains (C) an inorganic filler. In addition, by blending (C) an inorganic filler, the curing shrinkage of the obtained cured product is suppressed, the CTE is low, and the thermal properties such as adhesion, hardness, and crack resistance can be improved by matching the thermal strength with the conductor layer such as copper surrounding the insulating layer. As the inorganic filler, a conventionally known inorganic filler can be used, and is not limited to a specific one. For example, extender pigments such as barium sulfate, barium titanate, amorphous silica, crystalline silica, fused silica, and spherical silica, talc, clay, Neuburg silica particles, boehmite, magnesium carbonate, calcium carbonate, titanium oxide, aluminum oxide, aluminum hydroxide, silicon nitride, aluminum nitride, and calcium zirconate, and metal powders such as copper, tin, zinc, nickel, silver, palladium, aluminum, iron, cobalt, gold, and platinum can be mentioned. The inorganic filler is preferably a spherical particle. Among them, silica is preferable, as it suppresses the curing shrinkage of the curable composition, has a lower CTE, and improves properties such as adhesion and hardness. The average particle size (median size, D50) of the inorganic filler is preferably 0.01 to 10 μm. From the viewpoint of slit processability, the inorganic filler is preferably silica having an average particle size of 0.01 to 3 μm. In this specification, the average particle size of the inorganic filler is an average particle size including not only the particle size of the primary particles but also the particle size of the secondary particles (aggregates). The average particle size can be determined by a laser diffraction particle size distribution measuring device and a measuring device using a dynamic light scattering method. An example of a measuring device using the laser diffraction method is Microtrac MT3300EXII manufactured by Microtrac-Bell, and an example of a measuring device using the dynamic light scattering method is Nanotrac Wave II UT151 manufactured by Microtrac-Bell.
[0083] (C) The inorganic filler is preferably a surface-treated inorganic filler. The surface treatment may be a surface treatment with a coupling agent or a surface treatment without introducing an organic group, such as an alumina treatment. The surface treatment method of the inorganic filler is not particularly limited, and a publicly known and commonly used method may be used, and the surface of the inorganic filler may be treated with a surface treatment agent having a curable reactive group, for example, a coupling agent having a curable reactive group as an organic group.
[0084] The surface treatment of the inorganic filler is preferably a surface treatment with a coupling agent. As the coupling agent, silane-based, titanate-based, aluminate-based, zircoaluminate-based, and other coupling agents can be used. Among them, silane-based coupling agents are preferred. Examples of such silane-based coupling agents include vinyltrimethoxysilane, vinyltriethoxysilane, N-(2-aminomethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-anilinopropyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, and N-phenyl-3-aminopropyltrimethoxysilane, which can be used alone or in combination. These silane coupling agents are preferably immobilized in advance on the surface of the inorganic filler by adsorption or reaction. The amount of the coupling agent to be used per 100 parts by mass of the inorganic filler is, for example, 0.5 to 10 parts by mass.
[0085] The curable reactive group is preferably a thermosetting reactive group. Examples of the thermosetting reactive group include a hydroxyl group, a carboxyl group, an isocyanate group, an amino group, an imino group, an epoxy group, an oxetanyl group, a mercapto group, a methoxymethyl group, a methoxyethyl group, an ethoxymethyl group, an ethoxyethyl group, and an oxazoline group. Among them, at least one of an amino group and an epoxy group is preferable. The surface-treated inorganic filler may have a photocurable reactive group in addition to the thermosetting reactive group.
[0086] In addition, the surface-treated inorganic filler may be contained in the resin layer in a surface-treated state, and the inorganic filler and the surface treatment agent may be separately blended into the resin composition forming the resin layer to surface-treat the inorganic filler in the composition, but it is preferable to blend the inorganic filler that has been surface-treated in advance. By blending the inorganic filler that has been surface-treated in advance, it is possible to prevent a decrease in crack resistance, etc. due to the surface treatment agent that was not consumed in the surface treatment that may remain when blended separately. When performing surface treatment in advance, it is preferable to blend a preliminary dispersion in which the inorganic filler is pre-dispersed in a solvent or a curable resin, and the surface-treated inorganic filler is pre-dispersed in a solvent and the preliminary dispersion is blended into the composition, or it is more preferable to pre-disperse the surface-untreated inorganic filler in a solvent, perform sufficient surface treatment, and then blend the preliminary dispersion into the composition.
[0087] The (C) inorganic filler may be blended with the epoxy resin or the like in a powder or solid state, or may be mixed with a solvent or dispersant to form a slurry and then blended with the epoxy resin or the like.
[0088] The inorganic filler (C) may be used alone or in a mixture of two or more. The amount of the inorganic filler (C) is preferably 30% by mass or more, more preferably 50% by mass or more, even more preferably 60% by mass or more, and particularly preferably 65% by mass or more, from the viewpoint of low CTE, assuming that the non-volatile components in the resin layer are 100% by mass. Also, from the viewpoint of toughness of the cured film, the amount is preferably 90% by mass or less, more preferably 85% by mass or less.
[0089] (Cure accelerator) The resin layer may contain a curing accelerator, which accelerates the thermosetting reaction and is used to further improve properties such as adhesion, chemical resistance, and heat resistance. Specific examples of such curing accelerators include imidazole and its derivatives; guanamines such as acetoguanamine and benzoguanamine; polyamines such as diaminodiphenylmethane, m-phenylenediamine, m-xylylenediamine, diaminodiphenylsulfone, dicyandiamide, urea, urea derivatives, melamine, and polybasic hydrazides; organic acid salts and / or epoxy adducts thereof; amine complexes of boron trifluoride; triazine derivatives such as ethyldiamino-S-triazine, 2,4-diamino-S-triazine, and 2,4-diamino-6-xylyl-S-triazine; amines such as trimethylamine, triethanolamine, N,N-dimethyloctylamine, N-benzyldimethylamine, pyridine, dimethylaminopyridine, N-methylmorpholine, hexa(N-methyl)melamine, 2,4,6-tris(dimethylaminophenol), tetramethylguanidine, and m-aminophenol; polyvinylphenol, polyvinylphenol bromine, phenol, and the like. organic phosphines such as tributylphosphine, triphenylphosphine, tris-2-cyanoethylphosphine; phosphonium salts such as tri-n-butyl(2,5-dihydroxyphenyl)phosphonium bromide, hexadecyltributylphosphonium chloride; quaternary ammonium salts such as benzyltrimethylammonium chloride, phenyltributylammonium chloride; the above-mentioned polybasic acid anhydrides; photocationic polymerization catalysts such as diphenyliodonium tetrafluoroborate, triphenylsulfonium hexafluoroantimonate, 2,4,6-triphenylthiopyrylium hexafluorophosphate; styrene-maleic anhydride resins; equimolar reactants of phenylisocyanate and dimethylamine, equimolar reactants of organic polyisocyanates such as tolylene diisocyanate and isophorone diisocyanate and dimethylamine, and conventionally known curing accelerators such as metal catalysts.Among the curing accelerators, imidazole and its derivatives, and dimethylaminopyridine are preferred, and imidazole and its derivatives are more preferred since they give a cured product with a higher Tg and a lower dielectric tangent.
[0090] The curing accelerator can be used alone or in combination of two or more. The amount of the curing accelerator is preferably 5% by mass or less, more preferably 3% by mass or less, from the viewpoint of storage stability of the resin layer before the thermosetting reaction, when the total amount of the epoxy resin (A) and the compound having an active ester group (B) in the resin layer is taken as 100% by mass, and is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, from the viewpoint of curability.
[0091] (Thermoplastic resin (polymer resin)) The resin layer may further contain a thermoplastic resin in order to improve the mechanical strength of the resulting cured film. The thermoplastic resin is preferably soluble in a solvent. When it is soluble in a solvent, the flexibility of the resin layer is improved, and the occurrence of cracks and powder fall can be suppressed. Examples of the thermoplastic resin include thermoplastic polyhydroxypolyether resins, phenoxy resins which are condensates of epichlorohydrin and various bifunctional phenolic compounds, or phenoxy resins in which the hydroxyl groups of the hydroxyether moiety present in the skeleton are esterified using various acid anhydrides or acid chlorides, polyvinyl acetal resins, polyamide resins, polyamideimide resins, block copolymers, and the like. The thermoplastic resins may be used alone or in combination of two or more. Among these thermoplastic resins, phenoxy resins are preferred because they can improve the glass transition temperature while maintaining a low dielectric tangent. Polyvinyl acetal resins are preferred from the viewpoint of reducing the roughness of the cured surface after desmearing.
[0092] The polyvinyl acetal resin can be obtained, for example, by acetalizing a polyvinyl alcohol resin with an aldehyde.The aldehyde is not particularly limited, and examples thereof include formaldehyde, acetaldehyde, propionaldehyde, butyl aldehyde, amyl aldehyde, hexyl aldehyde, heptyl aldehyde, 2-ethylhexyl aldehyde, cyclohexyl aldehyde, furfural, benzaldehyde, 2-methylbenzaldehyde, 3-methylbenzaldehyde, 4-methylbenzaldehyde, p-hydroxybenzaldehyde, m-hydroxybenzaldehyde, phenylacetaldehyde, and β-phenylpropionaldehyde, with butyl aldehyde being preferred.
[0093] Specific examples of phenoxy resins include FX280 and FX293 manufactured by Nippon Steel Chemical & Material Co., Ltd., and YX8100, YX6954, YL6954, YL6974, and YX7200 manufactured by Mitsubishi Chemical Co., Ltd. Specific examples of polyvinyl acetal resins include S-LEC KS series manufactured by Sekisui Chemical Co., Ltd., polyamide resins include KS5000 series manufactured by Hitachi Chemical Co., Ltd., and BP series manufactured by Nippon Kayaku Co., Ltd., and polyamideimide resins include KS9000 series manufactured by Hitachi Chemical Co., Ltd. The amount of the thermoplastic resin is preferably 0.1% by mass or more, and more preferably 0.3% by mass or more, from the viewpoint of the mechanical strength of the cured film obtained, when the total of (A) epoxy resin and (B) compound having an active ester group in the resin layer is taken as 100% by mass. In addition, from the viewpoint of the dielectric properties of the cured film, it is preferably 30% by mass or less, and more preferably 20% by mass or less.
[0094] (rubber particles) The resin layer may contain rubber particles as necessary. Examples of such rubber particles include polybutadiene rubber, polyisopropylene rubber, urethane-modified polybutadiene rubber, epoxy-modified polybutadiene rubber, acrylonitrile-modified polybutadiene rubber, carboxyl-modified polybutadiene rubber, acrylonitrile-butadiene rubber modified with carboxyl or hydroxyl groups, and crosslinked rubber particles thereof, core-shell type rubber particles, etc., and one type may be used alone or two or more types may be used in combination. These rubber particles are added to improve the flexibility of the resulting cured film, improve crack resistance, enable surface roughening treatment with an oxidizing agent, and improve adhesion strength with copper foil, etc.
[0095] The average particle size of the rubber-like particles is preferably in the range of 0.005 to 15 μm, more preferably in the range of 0.2 to 10 μm. The average particle size of the rubber-like particles in the present invention can be measured by the same method as that for the average particle size of the inorganic filler.
[0096] (Flame retardant) The resin layer may contain a flame retardant. Examples of the flame retardant include hydrated metals such as aluminum hydroxide and magnesium hydroxide, red phosphorus, ammonium phosphate, ammonium carbonate, zinc borate, zinc stannate, molybdenum compounds, bromine compounds, chlorine compounds, phosphate esters, phosphorus-containing polyols, phosphorus-containing amines, melamine cyanurate, melamine compounds, triazine compounds, guanidine compounds, and silicon polymers. The flame retardants may be used alone or in combination of two or more.
[0097] (Organic solvent) The organic solvent is not particularly limited, and examples thereof include ketones, aromatic hydrocarbons, glycol ethers, glycol ether acetates, esters, alcohols, aliphatic hydrocarbons, petroleum-based solvents, etc. More specifically, ketones such as methyl ethyl ketone, cyclohexanone, methyl butyl ketone, and methyl isobutyl ketone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; glycol ethers such as cellosolve, methyl cellosolve, butyl cellosolve, carbitol, methyl carbitol, butyl carbitol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, propylene glycol monomethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol diethyl ether, and triethylene glycol monoethyl ether; ethyl acetate, butyl acetate, isobutyl acetate, ethyl Examples of suitable organic solvents include esters such as ethylene glycol monoethyl ether acetate, dipropylene glycol methyl ether acetate, propylene glycol methyl ether acetate, propylene glycol ethyl ether acetate, and propylene glycol butyl ether acetate; alcohols such as ethanol, propanol, 2-methoxypropanol, n-butanol, isobutyl alcohol, isopentyl alcohol, ethylene glycol, and propylene glycol; aliphatic hydrocarbons such as octane and decane; petroleum solvents such as petroleum ether, petroleum naphtha, hydrogenated petroleum naphtha, and solvent naphtha, as well as N,N-dimethylformamide (DMF), tetrachloroethylene, and turpentine. In addition, organic solvents such as Swazol 1000 and Swazol 1500 manufactured by Maruzen Petrochemical Co., Ltd., Solvesso 100 and Solvesso 150 manufactured by Standard Oil Osaka Sales Co., Ltd., Solvent #100 and Solvent #150 manufactured by Sankyo Chemical Co., Ltd., Shellsol A100 and Shellsol A150 manufactured by Shell Chemicals Japan Ltd., and Ipzol 100 and Ipzol 150 manufactured by Idemitsu Kosan Co., Ltd. may also be used. The organic solvents may be used alone or in combination of two or more.
[0098] The amount of residual solvent in the resin layer is preferably 0.5 to 10.0% by mass. If the amount of residual solvent is 10.0% by mass or less, bumping during thermal curing is suppressed, and the surface flatness is improved. In addition, the melt viscosity is prevented from dropping too much, causing the resin to flow, and the flatness is improved. If the amount of residual solvent is 0.5% by mass or more, the flowability during lamination is good, and the flatness and embeddability are improved.
[0099] (Other Ingredients) The resin layer may further contain, as necessary, organic fillers such as silicon powder, fluorine powder, nylon powder, etc.; conventionally known colorants such as phthalocyanine blue, phthalocyanine green, iodine green, disazo yellow, crystal violet, titanium oxide, carbon black, naphthalene black, etc.; conventionally known thickeners such as asbestos, orben, bentone, finely powdered silica, etc.; antifoaming agents and / or leveling agents such as silicone-based, fluorine-based, and polymer-based agents; adhesion imparting agents such as thiazole-based, triazole-based, and silane coupling agents, etc.; and conventionally known titanate-based and aluminum-based additives.
[0100] [Ultra-thin copper foil] In the present invention, the thickness of the ultra-thin copper foil is 0.1 to 6 μm. The method of forming the ultra-thin copper foil is not particularly limited, and it can be formed by a known method such as a wet film formation method such as electroless copper plating and electrolytic copper plating, a dry film formation method such as sputtering and chemical vapor deposition, or a combination of these. From the viewpoint of easy control of the thickness of the ultra-thin copper foil, an electrolytic plating method is preferred. For example, after forming an auxiliary metal layer such as a nickel layer on a carrier foil, it is immersed in a copper solution with a copper concentration of 20 to 100 g / L and a sulfuric acid concentration of 100 to 300 g / L, and a current density of 5 to 30 A / dm 2 By electrolysis at 4000 K, an ultra-thin copper foil can be formed.
[0101] The surface of the ultra-thin copper foil is preferably roughened. The roughening treatment is not particularly limited, and may be performed by a known, commonly used method. For example, the roughening treatment can be performed by carrying out a burnt plating process for depositing fine copper particles on the ultra-thin copper foil, and a cover plating process for preventing the deposited fine copper particles from falling off. For example, in the burnt plating process, an acidic copper sulfate solution containing a copper concentration of 10 g / L and a sulfuric acid concentration of 120 g / L is used, and the solution temperature is 25° C., the current density is 15 A / dm 2 In the subsequent plating process, an acidic copper sulfate solution containing 70 g / L of copper and 120 g / L of sulfuric acid was used at a solution temperature of 40°C and a current density of 15 A / dm 2 The electrodeposition may be carried out under the smooth plating conditions.
[0102] The ten-point average roughness Rz of the resin layer side surface of the ultra-thin copper foil is preferably 4.0 μm or less from the viewpoint of the formability of a fine circuit. More preferably, it is 3.0 μm or less, and even more preferably, it is 2.5 μm or less. In addition, from the viewpoint of adhesion with the resin layer, it is preferably 0.5 μm or more, and more preferably 1.0 μm or more. Here, the ten-point average roughness Rz is a parameter that can be determined in accordance with JIS B 0601:2001, and refers to the sum of the average height of the top five peaks in order from the highest peak to the fifth highest peak in the roughness curve of the reference length, and the average depth of the bottom five valleys in order from the deepest valley to the fifth deepest valley. The ten-point average roughness Rz can be measured by using a commercially available three-dimensional surface structure analysis microscope (e.g., zygo New View 5032 (manufactured by Zygo)) and commercially available analysis software (e.g., Metro Pro Ver.8.0.2) with a low-frequency filter set to a condition of 11 μm. At this time, the non-measurement surface of the foil is fixed in contact with the sample stage, and six points of a 108 μm x 144 μm field of view are selected within a 1 cm square area of the sample piece and measured, and the average value obtained from the six measurement points is used as the representative value.
[0103] [Carrier foil] The method of forming the carrier foil is not particularly limited, and examples thereof include copper foil, aluminum foil, stainless steel (SUS) foil, and resin film with a metal coating on the surface, and copper foil is preferred. The copper foil may be electrolytic copper foil or rolled copper foil. The thickness of the carrier foil is usually 250 μm or less, and preferably 9 to 200 μm.
[0104] The ultra-thin copper foil and carrier foil may be commercially available products. For example, MT18Ex, MT18FL, MT18SD-H, etc., which are ultra-thin copper foils with carrier foils manufactured by Mitsui Mining & Smelting Co., Ltd., may be used.
[0105] [Laminate] The laminate of the present invention may have a carrier foil, an ultra-thin copper foil having a thickness of 0.1 to 6 μm, and a resin layer in this order, and may further have other layers as necessary. For example, a release layer or an auxiliary metal layer may be provided between the carrier foil and the ultra-thin copper foil, or a protective film may be provided on the resin layer.
[0106] The release layer may be either an organic release layer or an inorganic release layer. The organic components of the organic release layer include nitrogen-containing organic compounds such as triazole compounds, sulfur-containing organic compounds, carboxylic acids, etc. Examples of the inorganic components of the inorganic release layer include Ni, Mo, Co, Cr, Fe, Ti, W, P, Zn, chromate-treated films, etc.
[0107] The auxiliary metal layer is preferably a layer made of nickel and / or cobalt, and such an auxiliary metal layer provides good stability in the peel strength of the carrier foil.
[0108] The protective film is provided on the resin layer for the purpose of preventing dust and the like from adhering to the surface of the resin layer and improving the handling. As the protective film, for example, polyester films such as polyethylene terephthalate and polyethylene naphthalate, polyimide films, polyamideimide films, polyethylene films, polytetrafluoroethylene films, polypropylene films, polystyrene films, and other thermoplastic resin films, and surface-treated paper can be used, among which polyester films, polyethylene films, and polypropylene films are preferred. The thickness of the protective film is not particularly limited, but is appropriately selected within the range of approximately 5 to 150 μm depending on the application. The surface of the protective film on which the resin layer is provided may be subjected to a release treatment.
[0109] The method for producing the laminate of the present invention is not particularly limited, and the laminate can be produced, for example, by applying a resin composition containing (A) an epoxy resin, (B) a compound having an active ester group, and (C) an inorganic filler onto a commercially available ultra-thin copper foil with a carrier foil, and drying the composition to form a resin layer as a dried coating film.
[0110] The laminate of the present invention is preferably a resin-coated copper foil (RCC) used for manufacturing a multilayer wiring board. A conventionally known method may be used as a method for manufacturing an electronic component using the laminate of the present invention. The method for curing the resin layer of the laminate of the present invention is not particularly limited, and may be cured by a conventionally known method, for example, by heating at 150 to 230°C. Examples of a method for manufacturing a printed wiring board using the laminate of the present invention include the following method. The laminate of the present invention is laminated by heat lamination so that the resin layer side is in contact with a circuit board on which a circuit pattern is formed, and then thermally cured. The thermal curing may be performed in an oven or by hot plate pressing. Next, a circuit may be formed by a modified semi-additive process (MSAP) method using the ultra-thin copper foil as all or part of the wiring layer, and a build-up wiring board may be manufactured. A build-up wiring board in which a circuit is formed by removing the ultra-thin copper foil and using a semi-additive process (SAP) method may be manufactured. Printed wiring boards may also be manufactured by direct build-up on wafer, which alternates between laminating resin-coated copper foil and forming circuits on semiconductor integrated circuits. A coreless build-up method may also be used, in which resin layers and conductor layers are alternately laminated without using a core substrate. The carrier foil may be peeled off after lamination, heat curing, laser processing, or desmearing.
[0111] The laminate of the present invention can be preferably used for forming a permanent protective film for electronic components, particularly multilayer printed wiring boards, and can be preferably used for forming an interlayer insulating layer. The cured resin layer of the laminate of the present invention has excellent dielectric properties, and can therefore be suitably used for high-frequency applications where transmission loss is an issue. Specific examples of high-frequency applications include substrates for millimeter-wave radar and millimeter-wave sensors for autonomous driving, motherboards for mobile devices compatible with high-speed communication, SLPs (Substrate-Like PCBs) for forming circuits by the modified semi-additive process (MSAP) method, application processors (AP) for mobile devices and personal computers, HDI (high-density interconnect) substrates and PKG (package) substrates for smartphones, tablets, and personal computers, highly multilayer substrates for servers and routers for base stations, and substrates for antennas. A wiring board may be formed by laminating wiring using the laminate of the present invention. The electronic components may be used for applications other than printed wiring boards, such as passive components such as inductors. Furthermore, according to the laminate of the present invention, even when the total amount of active ester groups is large, that is, when the ratio of the total amount of epoxy groups in the epoxy resin (A) / the total amount of active ester groups in the compound (B) having an active ester group in the resin layer is 0.20 to 0.60, a fine pattern can be formed with good adhesion on an insulating layer, and the laminate is suitable for circuit formation applications with a line / space of 35 μm or less / 35 μm or less.
[0112] The dielectric dissipation factor of the cured product of the present invention is not particularly limited, but according to the present invention it is possible to obtain a cured product with a low dielectric dissipation factor, for example, 0.005 or less, or even 0.003 or less, or even 0.002 or less. EXAMPLES
[0113] The present invention will be specifically described below with reference to examples and comparative examples, but it goes without saying that the present invention is not limited to the following examples. In the following, "parts" and "%" are all based on mass unless otherwise specified.
[0114] <Synthesis of compounds having active ester groups> (Synthesis Example 1: Synthesis of Compound Having Active Ester Group (B-1)) In a flask equipped with a thermometer, a dropping funnel, a cooling tube, a fractionating tube, and a stirrer, 203.0g of isophthalic acid chloride (molar number of acid chloride groups: 2.0 mol) and 1338g of toluene were charged, and the system was reduced in pressure and replaced with nitrogen to dissolve. Next, 96.0g (0.67 mol) of α-naphthol and 220g of dicyclopentadiene phenol resin (molar number of phenolic hydroxyl groups: 1.33 mol) were charged, and the system was reduced in pressure and replaced with nitrogen to dissolve. Then, 1.12g of tetrabutylammonium bromide was dissolved, and while applying nitrogen gas purge, the system was controlled to 60°C or less, and 400g of 20% sodium hydroxide aqueous solution was dropped over 3 hours. Stirring was then continued under these conditions for 1.0 hour. After the reaction was completed, the mixture was allowed to stand and separated, and the aqueous layer was removed. Water was then added to the toluene phase in which the reactants were dissolved, and the mixture was stirred and mixed for about 15 minutes, and the mixture was allowed to stand and separated, and the aqueous layer was removed. This operation was repeated until the pH of the aqueous layer reached 7. Thereafter, water was removed by decanting, and an active ester resin (B-1) was obtained in a toluene solution state with a non-volatile content of 65%. The ester group equivalent of the obtained active ester resin (B-1) calculated as solid content was 223 g / eq.
[0115] (Synthesis Example 2: Synthesis of Compound Having Active Ester Group (B-2)) In a flask equipped with a thermometer, dropping funnel, condenser, distillation tube, and stirrer, 320g (2.0 mol) of 2,7-dihydroxynaphthalene, 184g (1.7 mol) of benzyl alcohol, and 5.0g of paratoluenesulfonic acid monohydrate were charged and stirred at room temperature while blowing in nitrogen. The temperature was then raised to 150°C and the mixture was stirred for 4 hours while distilling off the water produced. After the reaction was completed, 900g of methyl isobutyl ketone and 5.4g of 20% aqueous sodium hydroxide solution were added to neutralize the mixture, and the aqueous layer was removed by separation. The mixture was washed three times with 280g of water, and the methyl isobutyl ketone was removed under reduced pressure to obtain 460g of a benzyl-modified naphthalene compound (B-2 intermediate). The obtained benzyl-modified naphthalene compound (B-2 intermediate) was a black solid with a hydroxyl equivalent of 180g / eq. In a flask equipped with a thermometer, a dropping funnel, a cooling tube, a fractionating tube, and a stirrer, 203.0 g of isophthalic acid chloride (molar number of acid chloride groups: 2.0 mol) and 1400 g of toluene were charged, and the system was reduced in pressure and replaced with nitrogen to dissolve. Next, 96.0 g (0.67 mol) of α-naphthol and 240 g of benzyl-modified naphthalene compound (B-2 intermediate) (molar number of phenolic hydroxyl groups: 1.33 mol) were charged, and the system was reduced in pressure and replaced with nitrogen to dissolve. Then, 0.70 g of tetrabutylammonium bromide was dissolved, and while applying nitrogen gas purge, the system was controlled to 60°C or less, and 400 g of 20% aqueous sodium hydroxide solution was dropped over 3 hours. Then, stirring was continued under these conditions for 1.0 hour. After the reaction was completed, the mixture was left to stand for liquid separation, and the aqueous layer was removed. Further, water was added to the toluene layer in which the reactants were dissolved, and the mixture was stirred and mixed for 15 minutes, and the mixture was allowed to stand and separated to remove the aqueous layer. This operation was repeated until the pH of the aqueous layer reached 7. Thereafter, water was removed by decanting to obtain an active ester resin (B-2) in a toluene solution state with a non-volatile content of 65 mass%. The ester group equivalent of the obtained active ester resin (B-2) calculated as the solid content was 230 g / eq.
[0116] <Preparation of Curable Resin Composition> Curable resin compositions were prepared by kneading and mixing the various components shown in the "resin layer" of the examples and comparative examples in Tables 1 and 2 in the ratios (parts by mass) shown in Tables 1 and 2. The values in the tables indicate parts by mass (converted into non-volatile content).
[0117] <Measurement of dielectric dissipation factor (DF)> Using a film applicator, the curable resin composition was applied to the glossy side of copper foil (F2-WS, 18 μm thick, manufactured by Furukawa Electric Co., Ltd.) for each Example and Comparative Example, dried at 90° C. for 10 minutes in a hot air circulation drying oven, and then cured at 200° C. for 60 minutes. The copper foil was then peeled off to produce a cured film (cured film) with a thickness of about 40 μm. The obtained cured film was cut to a measurement size (50 mm x 60 mm), and the dielectric loss tangent at 10 GHz at 23° C. was measured using an SPDR dielectric resonator and a network analyzer (both manufactured by Agilent Technologies), and evaluated according to the following criteria. ◎: Less than 0.003 〇: 0.003 or more and less than 0.010 ×: 0.010 or more
[0118] <Production of RCC (Resin-Coated Copper Foil) with Carrier Foil> Using a film applicator, the curable resin compositions of Examples 1 to 14 and Comparative Example 1 were each applied to the laminate surface (copper foil roughness Rz = 2 μm) of an extremely thin copper foil with a carrier (MT18Ex manufactured by Mitsui Mining & Smelting Co., Ltd., 3 μm thick), and dried at 90°C for 10 minutes in a hot air circulation drying oven to produce RCC (resin-coated copper foil) with a carrier foil having a resin layer thickness of about 40 μm.
[0119] <Production of RCC (Resin-Coated Copper Foil)> Using a film applicator, the curable resin compositions of Comparative Examples 2 and 3 were each applied to the laminate surface (copper foil roughness Rz = 2 μm) of an electrolytic copper foil (3EC-M2S-VLP manufactured by Mitsui Mining & Smelting Co., Ltd., 18 μm thick), and dried at 90°C for 10 minutes in a hot air circulation drying oven to produce RCC (resin-coated copper foil) having a resin layer thickness of about 40 μm.
[0120] <Evaluation of Laser Drilling Processability> (i) In the case of the RCC with carrier foil of Examples 1 to 14 and Comparative Example 1 prepared above The surface of the substrate was laminated with the resin layer side of the RCC, and after thermocompression bonding at 4.0 MPa and 200°C for 90 minutes, the carrier foil was peeled off to produce a copper-clad laminate for evaluation. (ii) In the case of the RCC of Comparative Examples 2 and 3 prepared above The surface of the substrate was laminated with the resin layer side of the RCC, and after thermocompression bonding at 4.0 MPa and 200°C for 90 minutes, the entire surface of the copper foil of the laminate was etched using a cupric chloride-based etching solution so that the thickness of the copper foil became about 3 μm to produce a copper-clad laminate for evaluation. Thereafter, the copper-clad laminate prepared in (i) and (ii) above was subjected to laser drilling using a carbon dioxide laser under the conditions of a pulse width of 12 μsec, pulse energy of 8 mJ, and laser beam diameter of 97 μm. The diameters of the 10 holes formed by the laser drilling were measured in the x and y directions, and the average value was calculated to determine the hole diameter after processing. Holes where the difference between the maximum and minimum values of the hole diameters after processing (out of 10) was less than 3 μm were judged as ◎, and those of 3 μm or more were judged as ×.
[0121] <Evaluation of reflow resistance> First, the copper-clad laminate was cut into a size of 10 cm x 10 cm and repeatedly treated 10 times in a reflow furnace (maximum temperature of 285°C). After the treatment, the specimen was visually inspected to determine whether there was any appearance defect such as blistering, and whether there was any appearance defect such as blistering.
[0122] [Table 1]
[0123] [Table 2]
[0124] *1: DIC EXA-835LV (mixture of bisphenol A epoxy resin and bisphenol F epoxy resin, liquid, epoxy equivalent: 165g / eq.) *2: NC-3000H manufactured by Nippon Kayaku Co., Ltd. (biphenyl aralkyl type epoxy resin, solid, epoxy equivalent: 290g / eq.) *3: Active ester resin B-1 synthesized in Synthesis Example 1 above (active ester equivalent: 223 g / eq.) *4: Active ester resin B-2 synthesized in Synthesis Example 2 above (active ester equivalent: 230 g / eq.) *5: DIC TD-2090 (phenol novolac, hydroxyl equivalent: 105g / eq.) *6: Phenylaminosilane-treated SO-C2 (spherical silica, average particle size: 0.5 μm) manufactured by Admatechs *7: Mitsubishi Chemical jER YX7200B35 (phenoxy resin) *8: 2E4MZ (2-ethyl-4-methylimidazole) manufactured by Shikoku Kasei Co., Ltd. *9: Thickness of copper foil before etching. After etching, it is about 3μm.
[0125] From the results shown in the above table, it is clear that the laminate of the present invention is excellent in laser drilling processability and reflow resistance, and the cured product of the resin layer has a low dielectric tangent. [Explanation of symbols]
[0126] 1. Laminate 2 Carrier foil 3 Ultra-thin copper foil 4 Resin layer
Claims
1. A laminate having at least a carrier foil, an ultra-thin copper foil having a thickness of 0.1 to 6 μm, and a resin layer in this order, the resin layer contains (A) an epoxy resin, (B) a compound having an active ester group, and (C) an inorganic filler, a ratio of the total amount of epoxy groups in the epoxy resin (A) to the total amount of active ester groups in the compound (B) having an active ester group in the resin layer is 0.20 to 0.60; The compound (B) having an active ester group is represented by the following general formula (1): (wherein X 1 's each independently represent a group having a benzene ring or a naphthalene ring, k represents 0 or 1, and n represents an average of 0.25 to 1.5 in the repeating units).
2. A laminate having at least a carrier foil, an ultra-thin copper foil having a thickness of 0.1 to 6 μm, and a resin layer, in that order, the resin layer contains (A) an epoxy resin, (B) a compound having an active ester group, and (C) an inorganic filler, a ratio of the total amount of epoxy groups in the epoxy resin (A) to the total amount of active ester groups in the compound (B) having an active ester group in the resin layer is 0.20 to 0.60; The compound (B) having an active ester group is represented by the following general formula (2): In formula (2), X 2 each independently represents the following formula (3): or a group represented by the following formula (4): is a group represented by m is an integer from 1 to 6, each n is independently an integer from 1 to 5, and each q is independently an integer from 1 to 6; In formula (3), k is independently an integer from 1 to 5, In formula (4), Y is a group represented by formula (3) above (wherein k is an integer of 1 to 5, and t is an integer of 0 to 5). and both ends of the structure are monovalent aryloxy groups.
3. 3. The laminate according to claim 1, wherein the blending amount of the inorganic filler (C) is 50% by mass or more, based on 100% by mass of non-volatile components in the resin layer.
4. The laminate according to any one of claims 1 to 3, characterized in that a ratio of a total amount of epoxy groups in the epoxy resin (A) to a total amount of active ester groups in the compound (B) having an active ester group in the resin layer is 0.20 to 0.
50.
5. 5. The laminate according to claim 1, wherein the resin layer has a dielectric loss tangent of 0.01 or less after curing.
6. 6. An electronic component comprising a cured product obtained by curing the resin layer of the laminate according to claim 1.
Citation Information
Patent Citations
Epoxy resin composition, prepreg using composition, and laminated plate using composition
CN106916282A
Build-up resin composition and its application
JP2006089595A
Production method of cured product, cured product, and multilayer board
JP2013075948A
Curable composition, cured product and printed circuit board
JP2014189751A
Method for manufacturing wiring board
JP2017059728A