Compositions for silicon-containing films and methods of using the compositions

Silazane precursors with a specific formula are used in ALD and CVD processes to deposit silicon-containing films with low dielectric constants and high oxygen ash resistance, addressing stability and purity issues in semiconductor manufacturing.

JP7554755B2Active Publication Date: 2024-09-20VERSUM MATERIALS US LLC
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2021544513
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-02-01
Filing Date
2020-02-03
Publication Date
2024-09-20
Estimated Expiration
2040-02-03

AI Technical Summary

Technical Problem

Existing methods for depositing silicon-containing films with high carbon content face challenges in achieving low dielectric constants and high oxygen ash resistance, while also requiring compositions and processes that ensure stability and purity for semiconductor manufacturing.

Method used

The use of silazane precursors with a specific formula, containing only one organic amino group, in deposition processes such as ALD and CVD, to form silicon-containing films like silicon oxide, silicon nitride, and silicon carbide, which are free from impurities and have controlled carbon content, ensuring stability and purity.

Benefits of technology

The described methods enable the deposition of silicon-containing films with low dielectric constants and high oxygen ash resistance, providing improved stability and purity suitable for semiconductor applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554755000004
    Figure 0007554755000004
  • Figure 0007554755000009
    Figure 0007554755000009
  • Figure 0007554755000035
    Figure 0007554755000035
Patent Text Reader

Abstract

Described herein are precursors and methods for forming silicon-containing films. In one embodiment, the precursors are selected from the group consisting of compounds of Formula I: The precursor to TIFF2022518595000034.tif5464 is provided.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to U.S. Provisional Application No. 62 / 800,085, filed February 1, 2019, the entire contents of which are incorporated herein by reference thereto for all possible purposes.

[0002] Described herein are compositions and methods for the manufacture of electronic devices.More specifically, described herein are compounds for the deposition of low dielectric constant (<4.0) and high oxygen ashing resistance silicon-containing films, including but not limited to amorphous silicon, crystalline silicon, silicon oxide, silicon oxycarbide, silicon nitride, silicon oxynitride, and silicon oxycarbonitride, and compositions and methods comprising the compounds. [Background technology]

[0003] There is a need in the art to provide compositions and methods of using the compositions for depositing doped silicon-containing films with high carbon content (e.g., carbon content of about 10 at% or greater as measured by X-ray photoelectron spectroscopy (XPS)) for certain applications in the electronics industry.

[0004] US Patent No. 8,575,033 describes a method for the deposition of silicon carbide films on a substrate surface. The method includes the use of a gas-phase carbosilane precursor and can use a plasma-enhanced atomic layer deposition process.

[0005] US 2013 / 022496 teaches a method for forming a dielectric film having Si-C bonds on a semiconductor substrate by atomic layer deposition (ALD). The method includes (i) adsorbing a precursor on a surface of the substrate; (ii) reacting the adsorbed precursor with a reactant gas at the surface; and (iii) repeating steps (i) and (ii) to form a dielectric film having at least Si-C bonds on the substrate.

[0006] WO 14 / 134476 describes a method for the deposition of films containing SiCN and SiCON. A particular method includes exposing a substrate surface to a first and a second precursor, the first precursor being of the formula (X y H 3-y Si) z CH 4-z , (X y H 3-y Si)(CH2)(SiX p H 2-p )(CH2)(SiX y H 3-y ) or (X y H 3-y Si)(CH2) n (SiX y H 3-y ), where x is a halogen, y has a value from 1 to 3, z has a value from 1 to 3, p has a value from 0 to 2, and n has a value from 2 to 5, and the second precursor comprises a reducible amine. Certain methods further comprise exposing the substrate surface to an oxygen source to provide a film comprising carbon-doped silicon oxide.

[0007] Hirose, Y., Mizuno, K., Mizuno, N., Okubo, S., Okubo, S., Yanagida, K., and Yanagita, K. et al., (2014), "Method of manufacturing semiconductor device, substrate processing apparatus, and recording medium", U.S. Patent Application Publication No. 2014 / 287596, describes a method of manufacturing a semiconductor device that includes forming a thin film containing silicon, oxygen, and carbon on a substrate by performing a predetermined number of cycles, the cycles including supplying a precursor gas containing silicon, carbon, and a halogen element and having a Si-C bond, and a first catalytic gas to the substrate; and supplying an oxidizing gas and a second catalytic gas to the substrate.

[0008] Hirose, Y., Mizuno, N., Yanagita, K., and Okubo, S., et al. (2014), "Method of manufacturing semiconductor device, substrate processing apparatus, and recording medium", U.S. Patent No. 9,343,290, describes a method of manufacturing a semiconductor device, including forming an oxide film on a substrate by performing a cycle a predetermined number of times. The cycle includes supplying a precursor gas to the substrate; and supplying ozone gas to the substrate. In the act of supplying the precursor gas, the precursor gas is supplied to the substrate without a catalytic gas being supplied to the substrate, and in the act of supplying the ozone gas, the ozone gas is supplied to the substrate with an amine-based catalytic gas being supplied to the substrate.

[0009] US Pat. No. 9,349,586 discloses thin films having desirable etch resistance and low dielectric constant.

[0010] US 2015 / 0044881 describes a method for forming a film containing highly doped carbon with high controllability. A method for manufacturing a semiconductor device includes forming a film containing silicon, carbon and a predetermined element on a substrate by performing a cycle a predetermined number of times. The predetermined element is one of nitrogen and oxygen. The cycle includes supplying a precursor gas containing at least 2 silicon atoms / mol, carbon, and a halogen element and having a Si-C bond to the substrate, and supplying a modifying gas containing the predetermined element to the substrate.

[0011] The reference entitled "Highly Stable Ultrathin Carbosiloxane Films by Molecular Layer Deposition", Han, Z. et al., Journal of Physical Chemistry C, 2013, 117, 19967, teaches growing carbosiloxane films using 1,2-bis[(dimethylamino)dimethylsilyl]ethane and ozone. Thermal stability shows that the films are stable below 40°C with only slight thickness loss at 60°C.

[0012] Liu et al., Jpn. J. Appl. Phys., 1999, Vol. 38, 3482-3486, teach the use of H2 plasma for polysilsesquioxane deposited by spin-on techniques. H2 plasma provides films with stable dielectric constants, improves the thermal stability of the films, and makes them less damaged during O2 ashing (plasma) treatment.

[0013] Kim et al., Journal of the Korean Physical Society, 2002, Vol. 40, 94, teaches that H2 plasma treatment on PECVD SiOC films improves leakage current density (by 4-5 orders of magnitude) while increasing the dielectric constant from 2.2 to 2.5. The SiOC films after H2 plasma are less damaged during the O2 ashing process.

[0014] Posseme et al., Solid State Phenomena, 2005, Vol. 103-104, 337, teaches different H2 / inert plasma treatments for SiOC PECVD films. The dielectric constant k does not improve after H2 plasma treatment, suggesting no bulk modification.

[0015] The disclosures of the aforementioned patents, patent applications and publications are incorporated herein by reference. Summary of the Invention

[0016] Two SiR 2Described herein is a silicon precursor comprising a silazane compound having one organic amino group linked to the X2 group, a composition comprising the precursor, and a method of using the precursor to form a film containing silicon, such as, but not limited to, silicon oxide, carbon-doped silicon oxide, silicon nitride, silicon oxynitride, silicon carbide, silicon carbonitride, and combinations thereof, on at least a portion of a substrate.In addition, described herein is a composition comprising a silazane that is substantially free of at least one species selected from organic amines, higher molecular weight species, and trace metals.The composition may further comprise a solvent.Also disclosed herein is a method of forming a film or coating containing silicon on a processed object, such as a semiconductor wafer.In one embodiment of the method described herein, a film containing silicon and oxygen is deposited on a substrate using a silazane precursor and an oxygen-containing source in a deposition chamber under conditions to produce a silicon oxide film or a carbon-doped silicon oxide film on the substrate. In another embodiment of the method described herein, a film containing silicon and nitrogen is deposited on a substrate in a deposition chamber using a silazane precursor and a nitrogen-containing precursor under conditions for producing a silicon nitride film on the substrate.In a further embodiment, the silazane precursor described herein can also be used as a dopant for metal-containing films, such as but not limited to metal oxide films or metal nitride films.In the compositions and methods described herein, a silazane having the formula described herein is used as at least one of the silicon-containing precursors.

[0017] In one embodiment, the silicon precursor described herein has the following formula I: [ka] wherein R 1 Linear or branched C1-C 10 Alkyl groups, linear or branched, C3-C 10 Alkenyl group, linear or branched C3-C 10Alkynyl groups, C3-C 10 Cyclic alkyl groups, C2-C6 dialkylamino groups, electron-withdrawing groups and C6-C 10 aryl groups; R 2 is hydrogen, linear or branched C1-C 10 Alkyl groups, linear or branched C2-C6 alkenyl groups, linear or branched C3-C6 alkynyl groups, C3-C 10 Cyclic alkyl groups, C2-C6 dialkylamino groups, C6-C 10 Aryl groups, linear or branched C1-C6 fluorinated alkyl groups, electron-withdrawing groups, C4-C 10 two SiR groups selected from the group consisting of aryl groups and halides selected from the group consisting of Cl, Br, and I; X is a halide selected from the group consisting of Cl, Br, and I; 2 It includes at least one silazane precursor that includes only one organoamino group linked to an X2 group.

[0018] In another embodiment, (a) Formula I: [ka] wherein R 1 Linear or branched C1-C 10 Alkyl groups, linear or branched, C3-C 10 Alkenyl group, linear or branched C3-C 10 Alkynyl groups, C3-C 10 Cyclic alkyl groups, C2-C6 dialkylamino groups, electron-withdrawing groups and C6-C 10 aryl groups; R 2 is hydrogen, linear or branched C1-C 10 Alkyl groups, linear or branched C2-C6 alkenyl groups, linear or branched C3-C6 alkynyl groups, C3-C 10 Cyclic alkyl groups, C2-C6 dialkylamino groups, C6-C 10 Aryl groups, linear or branched C1-C6 fluorinated alkyl groups, electron-withdrawing groups, C4-C 10two SiR groups selected from the group consisting of aryl groups and halides selected from the group consisting of Cl, Br, and I; X is a halide selected from the group consisting of Cl, Br, and I; 2 a silicon precursor as described herein comprising at least one silazane precursor comprising only one organoamino group linked to an X2 group; (b) at least one solvent; In certain embodiments of the compositions described herein, exemplary solvents include, but are not limited to, ethers, tertiary amines, alkyl hydrocarbons, aromatic hydrocarbons, siloxanes, tertiary amino ethers, and combinations thereof.In certain embodiments, the difference between the boiling point of silicon compound and the boiling point of solvent is 40°C or less, less than about 30°C, in some cases less than about 20°C, and most preferably less than 10°C.

[0019] In another embodiment, a method for forming a silicon-containing film on at least one surface of a substrate, comprising: providing at least one surface of a substrate in a reaction chamber; Formula I below: [ka] wherein R 1 Linear or branched C1-C 10 Alkyl groups, linear or branched, C3-C 10 Alkenyl group, linear or branched C3-C 10 Alkynyl groups, C3-C 10 Cyclic alkyl groups, C2-C6 dialkylamino groups, electron-withdrawing groups and C6-C 10 aryl groups; R 2 is hydrogen, linear or branched C1-C 10 Alkyl groups, linear or branched C2-C6 alkenyl groups, linear or branched C3-C6 alkynyl groups, C3-C 10 Cyclic alkyl groups, C2-C6 dialkylamino groups, C6-C 10Aryl groups, linear or branched C1-C6 fluorinated alkyl groups, electron-withdrawing groups, C4-C 10 two SiR groups selected from the group consisting of aryl groups and halides selected from the group consisting of Cl, Br, and I; X is a halide selected from the group consisting of Cl, Br, and I; 2 forming a silicon-containing film on at least one surface by a deposition process selected from a chemical vapor deposition process and an atomic layer deposition process using at least one silazane precursor containing only one organoamino group linked to an X2 group; A method is provided that includes:

[0020] In another aspect, a method of forming a silicon oxide film or a carbon doped silicon oxide film by an atomic layer deposition process or ALD-like process, comprising: a. providing a substrate in a reactor; b. Formula I: [ka] wherein R 1 Linear or branched C1-C 10 Alkyl groups, linear or branched, C3-C 10 Alkenyl group, linear or branched C3-C 10 Alkynyl groups, C3-C 10 Cyclic alkyl groups, C2-C6 dialkylamino groups, electron-withdrawing groups and C6-C 10 aryl groups; R 2 is hydrogen, linear or branched C1-C 10 Alkyl groups, linear or branched C2-C6 alkenyl groups, linear or branched C3-C6 alkynyl groups, C3-C 10 Cyclic alkyl groups, C2-C6 dialkylamino groups, C6-C 10 Aryl groups, linear or branched C1-C6 fluorinated alkyl groups, electron-withdrawing groups, C4-C 10 two SiR groups selected from the group consisting of aryl groups and halides selected from the group consisting of Cl, Br, and I; X is a halide selected from the group consisting of Cl, Br, and I;2 introducing into a reactor at least one silazane precursor containing only one organoamino group linked to an X2 group; c. purging the reactor with a purge gas; d. introducing an oxygen-containing source into the reactor; e. purging the reactor with a purge gas; wherein steps b through e are repeated until a film of a desired thickness is obtained.

[0021] In a further aspect, there is provided a method of forming a film selected from a silicon oxide film and a carbon-doped silicon oxide film on at least one surface of a substrate using a CVD process, comprising: a. providing a substrate in a reactor; b. Formula I: [ka] wherein R 1 Linear or branched C1-C 10 Alkyl groups, linear or branched, C3-C 10 Alkenyl group, linear or branched C3-C 10 Alkynyl groups, C3-C 10 Cyclic alkyl groups, C2-C6 dialkylamino groups, electron-withdrawing groups and C6-C 10 aryl groups; R 2 is hydrogen, linear or branched C1-C 10 Alkyl groups, linear or branched C2-C6 alkenyl groups, linear or branched C3-C6 alkynyl groups, C3-C 10 Cyclic alkyl groups, C2-C6 dialkylamino groups, C6-C 10 Aryl groups, linear or branched C1-C6 fluorinated alkyl groups, electron-withdrawing groups, C4-C 10 two SiR groups selected from the group consisting of aryl groups and halides selected from the group consisting of Cl, Br, and I; X is a halide selected from the group consisting of Cl, Br, and I; 2introducing into a reactor at least one silazane precursor containing only one organoamino group linked to an X2 group; c. providing an oxygen-containing source to deposit a film on at least one surface; In certain embodiments, R 1 and R 2 In some other embodiments, R 1 and R 2 is different.

[0022] In another aspect, a method of forming a silicon nitride film by an atomic layer deposition process includes the steps of: a. providing a substrate in a reactor; b. Formula I: [ka] wherein R 1 Linear or branched C1-C 10 Alkyl groups, linear or branched, C3-C 10 Alkenyl group, linear or branched C3-C 10 Alkynyl groups, C3-C 10 Cyclic alkyl groups, C2-C6 dialkylamino groups, electron-withdrawing groups and C6-C 10 aryl groups; R 2 is hydrogen, linear or branched C1-C 10 Alkyl groups, linear or branched C2-C6 alkenyl groups, linear or branched C3-C6 alkynyl groups, C3-C 10 Cyclic alkyl groups, C2-C6 dialkylamino groups, C6-C 10 Aryl groups, linear or branched C1-C6 fluorinated alkyl groups, electron-withdrawing groups, C4-C 10 two SiR groups selected from the group consisting of aryl groups and halides selected from the group consisting of Cl, Br, and I; X is a halide selected from the group consisting of Cl, Br, and I; 2 introducing into a reactor at least one silazane precursor containing only one organoamino group linked to an X2 group; c. purging the reactor with a purge gas; d. introducing a nitrogen-containing source into the reactor; e. purging the reactor with a purge gas wherein steps b through e are repeated until a silicon nitride film of a desired thickness is obtained. 1 and R 2 In some other embodiments, R 1 and R 2 is different.

[0023] In a further embodiment, there is provided a method of forming a silicon nitride film on at least one surface of a substrate using a CVD process, comprising: a. providing a substrate in a reactor; b. Formula I: [ka] wherein R 1 Linear or branched C1-C 10 Alkyl groups, linear or branched, C3-C 10 Alkenyl group, linear or branched C3-C 10 Alkynyl groups, C3-C 10 Cyclic alkyl groups, C2-C6 dialkylamino groups, electron-withdrawing groups and C6-C 10 aryl groups; R 2 is hydrogen, linear or branched C1-C 10 Alkyl groups, linear or branched C2-C6 alkenyl groups, linear or branched C3-C6 alkynyl groups, C3-C 10 Cyclic alkyl groups, C2-C6 dialkylamino groups, C6-C 10 Aryl groups, linear or branched C1-C6 fluorinated alkyl groups, electron-withdrawing groups, C4-C 10 two SiR groups selected from the group consisting of aryl groups and halides selected from the group consisting of Cl, Br, and I; X is a halide selected from the group consisting of Cl, Br, and I; 2introducing into a reactor at least one silazane precursor containing only one organoamino group linked to an X2 group; c. providing a nitrogen-containing source, wherein the at least one silazane precursor reacts with the nitrogen-containing source to deposit a film on the at least one surface; In certain embodiments, R 1 and R 2 In some other embodiments, R 1 and R 2 is different.

[0024] In a further embodiment of the methods described herein, a method for forming an amorphous or crystalline silicon or silicon carbide film on at least one surface of a substrate is provided. In this embodiment, the method includes: a. placing one or more substrates in a reactor and heating the reactor to one or more temperatures ranging from ambient temperature to about 1000°C; b. Formula I: [ka] wherein R 1 Linear or branched C1-C 10 Alkyl groups, linear or branched, C3-C 10 Alkenyl group, linear or branched C3-C 10 Alkynyl groups, C3-C 10 Cyclic alkyl groups, C2-C6 dialkylamino groups, electron-withdrawing groups and C6-C 10 aryl groups; R 2 is hydrogen, linear or branched C1-C 10 Alkyl groups, linear or branched C2-C6 alkenyl groups, linear or branched C3-C6 alkynyl groups, C3-C 10 Cyclic alkyl groups, C2-C6 dialkylamino groups, C6-C 10 Aryl groups, linear or branched C1-C6 fluorinated alkyl groups, electron-withdrawing groups, C4-C 10two SiR groups selected from the group consisting of aryl groups and halides selected from the group consisting of Cl, Br, and I; X is a halide selected from the group consisting of Cl, Br, and I; 2 introducing at least one silazane precursor containing only one organic amino group linked to an X2 group; c. providing a reducing agent source into the reactor to at least partially react with the at least one silazane precursor to deposit a silicon-containing film on the one or more substrates; The reducing agent is selected from the group consisting of hydrogen, hydrogen plasma, and hydrogen chloride. In certain embodiments of the CVD method, the reactor is maintained at a pressure between 10 mTorr and 760 Torr during the introducing step. The above steps define one cycle for the method described herein, and the cycle of steps can be repeated until a film of the desired thickness is obtained. In some embodiments, R 1 and R 2 is the same as R 1 and R 2 is different.

[0025] In another aspect, a method for depositing an amorphous or crystalline silicon or silicon carbide film by an atomic layer deposition process or a cyclic chemical vapor deposition process, comprising: a. providing a substrate in a reactor; b. Formula I: [ka] wherein R 1 Linear or branched C1-C 10 Alkyl groups, linear or branched, C3-C 10 Alkenyl group, linear or branched C3-C 10 Alkynyl groups, C3-C 10 Cyclic alkyl groups, C2-C6 dialkylamino groups, electron-withdrawing groups and C6-C 10 aryl groups; R 2 is hydrogen, linear or branched C1-C 10Alkyl groups, linear or branched C2-C6 alkenyl groups, linear or branched C3-C6 alkynyl groups, C3-C 10 Cyclic alkyl groups, C2-C6 dialkylamino groups, C6-C 10 Aryl groups, linear or branched C1-C6 fluorinated alkyl groups, electron-withdrawing groups, C4-C 10 two SiR groups selected from the group consisting of aryl groups and halides selected from the group consisting of Cl, Br, and I; X is a halide selected from the group consisting of Cl, Br, and I; 2 Introducing into the reactor at least one silazane precursor containing only one organoamino group linked to an X2 group. and step b is repeated until a film of a desired thickness is obtained. In certain embodiments, the thickness of the film is 1 Å or more, 1-10,000 Å, 1-1,000 Å, or 1-100 Å. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] The silazane precursors described herein are used to form stoichiometric and non-stoichiometric silicon-containing films, including but not limited to amorphous silicon, crystalline silicon, silicon oxide, silicon oxycarbide, silicon nitride, silicon oxynitride, and silicon oxycarbonitride. These precursors can also be used as dopants, for example, for metal-containing films. Typically, silazane precursors used in semiconductor processes are high-purity volatile liquid chemicals that are vaporized and transported as gases to a deposition chamber or reactor to deposit silicon-containing films by CVD or ALD processes for semiconductor devices. The selection of precursor materials for deposition depends on the desired resulting silicon-containing material or film. For example, the precursor material can be selected for its chemical element content, its chemical element stoichiometric ratio, and / or the resulting silicon-containing film or coating formed under CVD. The precursor material can also be selected for various other characteristics, such as cost, relatively low toxicity, handling characteristics, ability to maintain liquid phase at room temperature, volatility, molecular weight, and / or other considerations. In certain embodiments, the precursors described herein can be delivered to the reactor system in any of a number of ways, preferably using a pressurizable stainless steel vessel equipped with suitable valves and fittings to allow for the delivery of liquid phase precursors to the deposition chamber or reactor.

[0027] The silazane precursors described herein exhibit a balance of reactivity and stability that makes them ideally suited as CVD or ALD precursors in microelectronic device fabrication processes. With respect to reactivity, the silazanes in the present invention contain two SiR groups that aid in the silazane precursor reacting with hydroxyl surfaces during ALD processes. 2It has an X2 group. Certain precursors may have boiling points that are too high to be vaporized, transported to a reactor, and deposited as a film on a substrate, and therefore it is preferred to select smaller organic amino groups as well as smaller alkyl groups to provide precursors with boiling points below 250°C, preferably below 200°C. As disclosed in the prior art, having two or more organic amino groups allows the boiling point to be raised significantly; precursors with higher relative boiling points require that, under a given vacuum, the transport containers and lines need to be heated above the boiling point of the precursor to prevent condensates or particles from forming in the container, line, or both. With regard to stability, other precursors may form silane (SiH4) or disilane (Si2H6) as they decompose. Silanes can be pyrophoric or spontaneously combust at room temperature, resulting in safety and handling issues. Additionally, the formation of silane or disilane and other by-products reduces the purity level of the precursor, and as little as a 1-2% change in chemical purity may be deemed unacceptable for reliable semiconductor manufacturing. In certain embodiments, the silazane precursor having formula I described herein has 2 wt. % or less, 1 wt. % or less, or 0.5 wt. % or less of impurities (e.g., free organic amines, X-SiR 2 X2 species, or higher molecular weight disproportionation products), which indicates storage stability. In addition to the advantages mentioned above, in certain embodiments, for example, using ALD deposition methods, ALD-like deposition methods, PEALD deposition methods, or CCVD deposition methods, for depositing silicon oxide films, silicon nitride films, or silicon films, the silazane precursors described herein can deposit high density materials at relatively low deposition temperatures, for example, 1000° C. or less, 800° C. or less, 700° C. or less, 500° C. or less, 400° C. or less, 300° C. or less, 200° C. or less, 100° C. or less, or 50° C. or less.

[0028] In one embodiment, a composition for forming a silicon-containing film is described herein, comprising a silazane having formula I described herein and at least one solvent. Without intending to be bound by a particular theory, it is believed that the composition described herein can provide one or more advantages compared to current silicon precursors, such as hexachlorodisilane and dichlorosilane. These advantages include better use of the silazane in semiconductor processes, better stability during long-term storage, cleaner evaporation by flash vaporization, and / or an overall more stable direct liquid injection (DLI) chemical vapor deposition process. The weight percentage of the silazane in the composition can be 1-99 wt%, with the remainder being at least one solvent, which does not react with the silazane and has a boiling point close to that of the silazane. With respect to the latter, the difference in boiling point between the silazane and the at least one solvent in the composition is 40° C. or less, more preferably 20° C. or less or 10° C. or less.

[0029] In one embodiment, the compound of formula I: [ka] wherein R 1 Linear or branched C1-C 10 Alkyl groups, linear or branched, C3-C 10 Alkenyl group, linear or branched C3-C 10 Alkynyl groups, C3-C 10 Cyclic alkyl groups, C2-C6 dialkylamino groups, electron-withdrawing groups and C6-C 10 aryl groups; R 2 is hydrogen, linear or branched C1-C 10 Alkyl groups, linear or branched C2-C6 alkenyl groups, linear or branched C3-C6 alkynyl groups, C3-C 10 Cyclic alkyl groups, C2-C6 dialkylamino groups, C6-C 10 Aryl groups, linear or branched C1-C6 fluorinated alkyl groups, electron-withdrawing groups, C4-C 10two SiR groups selected from the group consisting of aryl groups and halides selected from the group consisting of Cl, Br, and I; X is a halide selected from the group consisting of Cl, Br, and I; 2 At least one silazane precursor is provided that contains only one organoamino group linked to an X2 group.

[0030] In the formula and throughout the specification, the term "alkyl" refers to a straight or branched chain functional group having 1-10 or 1-6 carbon atoms. Exemplary alkyl groups include, but are not limited to, methyl, ethyl, propyl, isopropyl, butyl, isobutyl, sec-butyl, tert-butyl, pentyl, iso-pentyl, tert-pentyl, hexyl, iso-hexyl, and neo-hexyl. In certain embodiments, the alkyl groups may have one or more functional groups attached thereto, such as, but not limited to, alkoxy groups, dialkylamino groups, or combinations thereof. In other embodiments, the alkyl groups do not have one or more functional groups attached thereto.

[0031] In the formulas and throughout the specification, the term "cyclic alkyl" refers to a cyclic functional group having 3 to 10, 4 to 10, or 5 to 10 carbon atoms. Exemplary cyclic alkyl groups include, but are not limited to, cyclobutyl, cyclopentyl, cyclohexyl, and cyclooctyl groups.

[0032] In the formula and throughout the specification, the term "aryl" refers to an aromatic cyclic functional group having 5 to 12 carbon atoms or 6 to 10 carbon atoms. Exemplary aryl groups include, but are not limited to, phenyl, benzyl, chlorobenzyl, tolyl, and o-xylyl.

[0033] In the formulae and throughout the specification, the term "alkenyl group" means a group having one or more carbon-carbon double bonds and having 3 to 10, 3 to 6, or 3 to 4 carbon atoms.

[0034] In the formulae and throughout the specification, the term "alkynyl group" refers to a group having one or more carbon-carbon triple bonds and having 3 to 10, 3 to 6, or 3 to 4 carbon atoms.

[0035] In the formulas and throughout the specification, the term "organoamino group" means a group having an alkyl group attached to a nitrogen atom and having 1 to 10, 2 to 6, or 2 to 4 carbon atoms. Exemplary organic amino groups include, but are not limited to, methylamino, ethylamino, n-propylamine, iso-propylamino, n-butylamino, iso-butylamino, sec-butylamino, tert-butylamino.

[0036] In the formulas and throughout the specification, the term "dialkylamino group" refers to a group having two alkyl groups attached to a nitrogen atom, where each alkyl group has, for example, 1 to 10, 2 to 6, or 2 to 4 carbon atoms. Exemplary dialkylamino groups include, but are not limited to, dimethylamino, diethylamino, ethylmethylamino, di-n-propylamine, di-iso-propylamino, di-n-butylamino, di-iso-butylamino, di-sec-butylamino, di-tert-butylamino.

[0037] As used herein, the term "electron-withdrawing group" refers to an atom or group thereof that acts to withdraw electrons from a Si-N bond. Examples of suitable electron-withdrawing groups or substituents include, but are not limited to, nitrile (CN). In certain embodiments, the electron-withdrawing substituent may be adjacent to or proximal to the N in any one of formulas I. Further non-limiting examples of electron-withdrawing groups include F, Cl, Br, I, CN, NO2, RSO, and / or RSO2, where R is C1-C 10 The alkyl group may be, for example but not limited to, a methyl group, or another group.

[0038] In certain embodiments, one or more of the alkyl, alkenyl, alkynyl, alkoxy, dialkylamino, aryl and / or electron-withdrawing groups in formula I may be substituted or have one or more atoms or groups of atoms substituted, for example, at the position of a hydrogen atom. Exemplary substituents include, but are not limited to, oxygen, sulfur, halogen atoms (e.g., F, Cl, I, or Br), nitrogen, and phosphorus.

[0039] In certain embodiments, at least one silazane precursor having formula I has one or more substituents that include an oxygen or nitrogen atom.

[0040] The unique structure of the precursor of formula I described herein is believed to enable deposition temperatures of 1000° C. or less, 700° C. or less, 500° C. or less, 400° C. or less, 300° C. or less, 200° C. or less, 100° C. or less, or 25° C. or less.

[0041] Table 1 shows two SiR 2 Examples of silicon precursors having one organoamino group linked to the X2 group are listed. Table 1. Two SiR 2 Silicon precursors with X2 groups [Table 1-1] [Table 1-2] [Table 1-3] [Table 1-4] [Table 1-5] [Table 1-6] [Table 1-7]

[0042] Preferably, the silazane precursor according to the present invention and compositions comprising the silazane precursor according to the present invention are substantially free of organic amines or halide ions. As used herein, the term "substantially free" means less than 5 ppm (by weight), preferably less than 3 ppm, more preferably less than 1 ppm, and most preferably 0 ppm, of halide ions (or halides), e.g., chloride, fluoride, bromide and iodide. As used herein, the term "free" means 0 ppm when referring to halide ions or other impurities. Chloride is known to act as a decomposition catalyst for silazanes. Significant levels of chloride in the final product can decompose silazane precursors. The slow decomposition of silazanes can directly affect the film deposition process making it difficult for semiconductor manufacturers to meet film specifications. In addition, shelf life or stability is negatively affected by the higher silazane decomposition rate, thus making it difficult to guarantee a shelf life of 1 to 2 years. Accelerated decomposition of silazanes therefore raises safety and performance concerns regarding the formation of gaseous by-products which are flammable and / or spontaneously combustible. 10 The silicon precursor compounds having formula I include, but are not limited to, organic amines and organic diamines. Preferably, the silicon precursor compounds having formula I include, but are not limited to, metal ions, such as Li + , Na + , K + , Mg 2+ , Ca 2+ , Al 3+ , Fe 2+ , Fe 2+ , Fe 3+ , Ni 2+ , Cr 3+Substantially free. As used herein, the term "substantially free" means less than 5 ppm (by weight), preferably less than 3 ppm, more preferably less than 1 ppm, and most preferably less than 0.1 ppm, when measured by ICP-MS, when referring to Li, Na, K, Mg, Ca, Al, Fe, Ni, Cr. In some embodiments, the silicon precursor compound having formula I is free of metal ions, such as Li + , Na + , K + , Mg 2+ , Ca 2+ , Al 3+ , Fe 2+ , Fe 2+ , Fe 3+ , Ni 2+ , Cr 3+ As used herein, the term "free" of metal impurities, when referring to Li, Na, K, Mg, Ca, Al, Fe, Ni, Cr, precious metals, such as volatile Ru or Pt complexes derived from ruthenium or platinum catalysts used in the synthesis, means less than 1 ppm (by weight), preferably less than 0.1 ppm, as measured by ICP-MS or other analytical methods for measuring metals.

[0043] The method used to form silicon-containing film or coating is a deposition process. Examples of suitable deposition processes for the method disclosed herein include, but are not limited to, cyclic CVD (CCVD), MOCVD (metal organic CVD), thermal chemical vapor deposition, plasma enhanced chemical vapor deposition (PECVD), high density PECVD, photon assisted CVD, plasma-photon assisted (PPECVD), low temperature chemical vapor deposition, chemical assisted vapor deposition, hot filament chemical vapor deposition, CVD of liquid polymer precursors, deposition from supercritical fluids and low energy CVD (LECVD). In certain embodiments, the metal-containing film is deposited by atomic layer deposition (ALD), plasma enhanced ALD (PEALD) or plasma enhanced cyclic CVD (PECCVD) process. As used herein, the term "chemical vapor deposition process" refers to any process in which a substrate is exposed to one or more volatile precursors that react and / or decompose on the substrate surface to produce a desired deposit. As used herein, the term "atomic layer deposition process" refers to a self-limiting (e.g., the amount of film material deposited in each reaction cycle is constant), continuous surface chemical reaction that deposits a film of material on a substrate of various compositions. Although the precursors, reagents and sources used herein may sometimes be described as "gaseous", it is understood that the precursors may be either liquids or solids that are transported into the reactor by direct vaporization, bubbling or sublimation, with or without an inert gas. In some cases, the vaporized precursors may pass through a plasma generator. In one embodiment, the silicon-containing film is deposited using an ALD process. In another embodiment, the silicon-containing film is deposited using a CCVD process. In a further embodiment, the silicon-containing film is deposited using a thermal CVD process. As used herein, the term "reactor" includes, but is not limited to, a reaction chamber or a deposition chamber.

[0044] In certain embodiments, the method disclosed herein avoids pre-reaction of precursors by using ALD or CCVD methods that separate precursors before and / or during introduction into the reactor. In this regard, deposition techniques, such as ALD or CCVD processes, are used to deposit silicon-containing films. In one embodiment, the film is deposited by ALD process by exposing the substrate surface to an oxygen-containing source, a nitrogen-containing source, or other precursor or agent instead of one or more silicon-containing precursors. The growth of the film proceeds by self-limiting control of surface reactions, pulse length of each precursor or agent, and deposition temperature. However, once the substrate surface is saturated, the growth of the film stops.

[0045] In certain embodiments, the methods described herein further include one or more additional silicon-containing precursors other than the silazane precursor having formula I above. Further examples of silicon-containing precursors are monoaminosilanes (e.g. di-iso-propylaminosilane, di-sec-butylaminosilane, phenylmethylaminosilane); organosilicon compounds such as trisilylamine (TSA); monoaminosilanes (di-iso-propylaminosilane, di-sec-butylaminosilane, phenylmethylaminosilane); siloxanes (e.g. hexamethyldisiloxane (HMDSO), dimethylsiloxane (DMSO) and hexachlorodisiloxane (HCDSO)); organosilanes (e.g. methylsilane, dimethylsilane, diethylsilane, vinyltrimethylsilane, trimethylsilane, tetramethylsilane, ethylsilane, disilylmethane, 2,4-disilapentane, 1,4-disilabutane, 2,5-disilahexane, 2,2-disilylpropane, 1,3,5-trisilacyclohexane, and fluorinated derivatives of these compounds); phenyl containing organosilicon compounds (e.g. dimethylphenylsilane and diphenylmethylsilane); oxygen-containing organosilicon compounds such as dimethyldimethoxysilane, 1,3,5,7-tetramethylcyclotetrasiloxane, 1,1,3,3-tetramethyldisiloxane, 1,3,5,7-tetrasila-4-oxo-heptane, 2,4,6,8-tetrasila-3,7-dioxo-nonane, 2,2-dimethyl-2,4,6,8-tetrasila-3,7-dioxo Examples of suitable siloxanes include, but are not limited to, 1,3,5,7,9-pentamethylcyclopentasiloxane, 1,3,5,7-tetrasila-2,6-dioxo-cyclooctane, hexamethylcyclotrisiloxane, 1,3-dimethyldisiloxane, 1,3,5,7,9-pentamethylcyclopentasiloxane, hexamethoxydisiloxane, and fluorinated derivatives of these compounds.

[0046] In certain embodiments, depending on the deposition method, one or more silicon-containing precursors can be introduced into the reactor at a predetermined molar volume, or from about 0.1 to about 1000 micromoles. In this or other embodiments, the silicon-containing precursor and / or silazane precursor can be introduced into the reactor for a predetermined period of time. In certain embodiments, the period is from about 0.001 to about 500 seconds.

[0047] In certain embodiments, the silicon-containing film deposited using the methods described herein is formed in the presence of oxygen using an oxygen-containing source, an agent or precursor that contains oxygen. The oxygen-containing source may be introduced into the reactor in the form of at least one oxygen-containing source and / or may be present incidentally in other precursors used in the deposition process. Suitable oxygen-containing source gases may include, for example, water (H2O) (e.g., deionized water, purified water, and / or distilled water), oxygen (O2), oxygen plasma, ozone (O3), NO, NO2O, NO2, carbon monoxide (CO), carbon dioxide (CO2), and combinations thereof. In certain embodiments, the oxygen-containing source comprises an oxygen-containing source gas introduced into the reactor at a flow rate of about 1 to about 2000 square cubic centimeters (sccm) or about 1 to about 1000 sccm. The oxygen-containing source may be introduced for a time period ranging from about 0.1 to about 100 seconds. In one particular embodiment, the oxygen-containing source comprises water having a temperature of 10° C. or higher. In the embodiment where the film is deposited by ALD or cyclic CVD process, the precursor pulse can have a pulse duration longer than 0.01 seconds, the oxygen-containing source can have a pulse duration shorter than 0.01 seconds, while the water pulse can have a pulse duration shorter than 0.01 seconds.In yet another embodiment, the purge period between pulses can be as short as 0 seconds, or pulse continuously without purge in between.The oxygen-containing source or agent is provided in a molecular amount less than 1:1 ratio to the silicon precursor, so that at least some carbon is retained in the as-deposited silicon-containing film.

[0048] In certain embodiments, the silicon-containing film comprises silicon and nitrogen. In these embodiments, the silicon-containing film deposited using the methods described herein is formed in the presence of a nitrogen-containing source. The nitrogen-containing source may be introduced into the reactor in the form of at least one nitrogen-containing source and / or may be present incidentally in other precursors used in the deposition process. Suitable nitrogen-containing source gases may include, for example, ammonia, hydrazine, monoalkylhydrazine, dialkylhydrazine, nitrogen, nitrogen / hydrogen, ammonia plasma, nitrogen plasma, nitrogen / hydrogen plasma, and mixtures thereof. In certain embodiments, the nitrogen-containing source comprises an ammonia plasma or a hydrogen / nitrogen plasma source gas introduced into the reactor at a flow rate of about 1 to about 2000 square cubic centimeters (sccm) or about 1 to about 1000 sccm. The nitrogen-containing source may be introduced for a time period ranging from about 0.1 to about 100 seconds. In embodiments where the film is deposited by ALD or cyclic CVD processes, the precursor pulse may have a pulse duration longer than 0.01 seconds, the nitrogen-containing source may have a pulse duration shorter than 0.01 seconds, while the water pulse may have a pulse duration shorter than 0.01 seconds. In yet another embodiment, the purge period between the pulses may be as short as 0 seconds, or pulsed continuously with no purge in between.

[0049] The deposition methods disclosed herein may include one or more purge gases. The purge gases used to purge unconsumed reactants and / or reaction by-products are inert gases that do not react with the precursors. Exemplary purge gases include, but are not limited to, argon (Ar), nitrogen (N2), helium (He), neon, hydrogen (H2), and mixtures thereof. In certain embodiments, a purge gas, such as Ar, is fed into the reactor at a flow rate of about 10 to about 2000 sccm for about 0.1 to 1000 seconds, thus purging unreacted materials and any by-products that may remain in the reactor.

[0050] Each step of supplying the precursor, oxygen-containing source, nitrogen-containing source and / or other precursor, source gas and / or reagent can be performed with varying times for supplying them to vary the stoichiometric composition of the resulting silicon-containing film.

[0051] Energy is applied to at least one of the precursor, nitrogen-containing source, reducing agent, other precursor, or combination thereof to induce reaction and form silicon-containing film or coating on the substrate.Such energy can be provided by, but not limited to, thermal, plasma, pulsed plasma, helicon plasma, high-density plasma, inductively coupled plasma, X-ray, electron beam, photon, remote plasma, and combinations thereof.In certain embodiments, a secondary RF frequency source can be used to modify the plasma characteristics at the substrate surface.In embodiments where deposition includes plasma, the plasma generation process can include a direct plasma generation process in which plasma is generated directly in the reactor, or alternatively, a remote plasma generation process in which plasma is generated outside the reactor and fed into the reactor.

[0052] Silazane precursors and / or other silicon-containing precursors can be transported to reaction chambers, for example, CVD or ALD reactors, in a variety of ways. In one embodiment, a liquid transport system can be utilized. In an alternative embodiment, a unit that combines liquid transport and flash vaporization processes, such as a turbo vaporizer manufactured by MSP Corporation of Shoreview, MN, can be used, allowing low volatility materials to be transported volumetrically, which results in reproducible transport and deposition without pyrolysis of the precursor. In liquid transport formulations, the precursors described herein can be transported in a substantially liquid form, or alternatively, can be used in solvent formulations or compositions that include the precursors. Thus, in certain embodiments, precursor formulations can include at least one solvent component with suitable properties that can be desirable and advantageous in a given end-use application of forming a film on a substrate.

[0053] For embodiments in which a precursor having formula I is used in a composition comprising a solvent and at least one silazane precursor having formula I as described herein, the solvent or mixture thereof selected does not react with the silazane. The amount of solvent is 0.5 wt% to 99.5 wt% or 10 wt% to 75 wt% by weight of the composition. In this or other embodiments, the solvent has a boiling point (bp) close to the bp of the silazane of formula I, or the difference between the bp of the solvent and the bp of the organoaminosilane of formula I is 40° C. or less, 30° C. or less, 20° C. or less, or 10° C. Alternatively, the difference between the boiling points is a range that includes any one or more of the following endpoints: 0, 10, 20, 30, or 40° C. Examples of suitable ranges of bp difference include, but are not limited to, 0° C. to 40° C., 20° C. to 30° C., or 10° C. to 30° C. Examples of suitable solvents in the composition include, but are not limited to, ethers (e.g., 1,4-dioxane, dibutyl ether), tertiary amines (e.g., pyridine, 1-methylpiperidine, 1-ethylpiperidine, N,N'-dimethylpiperazine, N,N,N',N'-tetramethylethylenediamine), nitriles (e.g., benzonitrile), alkyl hydrocarbons (e.g., octane, nonane, dodecane, ethylcyclohexane), aromatic hydrocarbons (e.g., toluene, mesitylene), tertiary amino ethers (e.g., bis(2-dimethylaminoethyl) ether), or mixtures thereof.

[0054] In another embodiment, a container for depositing silicon-containing films comprising one or more silazane precursors having formula I is described herein.In one particular embodiment, the container comprises at least one pressurizable (preferably made of stainless steel) container with suitable valves and fittings that allow the transport of one or more precursors to a reactor for CVD or ALD process.In this embodiment or other embodiments, the silazane precursor having formula I is provided in a pressurizable container made of stainless steel, and the purity of the precursor is 98 wt% or more or 99.5 wt% or more, which is suitable for many semiconductor applications.In certain embodiments, such a container may have a means for mixing the precursor with one or more additional precursors, if desired.In these embodiments or other embodiments, the contents of the container can be premixed with the additional precursors.Alternatively, the silazane precursor and / or other precursors can be kept in separate containers or in a single container with a separation means for keeping the silazane precursor and other precursors separate during storage.

[0055] In one embodiment of the method described herein, a cyclic deposition process, such as CCVD, ALD or PEALD, can be used, using at least one silicon-containing precursor selected from a silazane precursor having a formula described herein, and optionally a nitrogen-containing source, such as ammonia, hydrazine, monoalkylhydrazine, dialkylhydrazine, nitrogen, nitrogen / hydrogen, ammonia plasma, nitrogen plasma, nitrogen / hydrogen plasma, and the like.

[0056] In certain embodiments, the gas lines connecting the precursor canister to the reaction chamber are heated to one or more temperatures according to the process requirements, and the container of the silazane precursor having formula I described herein is maintained at one or more temperatures for bubbling.In other embodiments, the solution containing at least one silicon-containing precursor having formula described herein is injected into a vaporizer maintained at one or more temperatures for direct liquid injection.

[0057] A flow of argon and / or other gases can be used as a carrier gas to facilitate the transport of the vapor phase of at least one silazane precursor to the reaction chamber during precursor pulse.In a particular embodiment, the pressure of the reaction chamber process is about 10 Torr or less.In another embodiment, the pressure of the reaction chamber process is about 5 Torr or less.

[0058] In a typical ALD or CCVD process, a substrate, such as, but not limited to, silicon oxide, carbon-doped silicon oxide, flexible substrates, or metal nitride substrates, is initially exposed to a silicon-containing precursor and heated in a heater stage in a reaction chamber to chemically adsorb silazane to the surface of the substrate. A purge gas, such as nitrogen, argon, or other inert gas, purges unabsorbed excess silazane from the process chamber. After sufficient purging, an oxygen-containing source can be introduced into the reaction chamber to react with the adsorbed surface, and then another gas purge is performed to remove reaction by-products from the chamber. The cycle of the process can be repeated to achieve the desired film thickness. In another embodiment, pumping under vacuum can be used to remove unabsorbed excess silazane from the process chamber, and after sufficient evacuation under pumping, an oxygen-containing source can be introduced into the reaction chamber to react with the adsorbed surface, and then another pump purge is performed to remove reaction by-products from the chamber. In yet another embodiment, the silazane and the oxygen-containing source can be co-flowed into a reaction chamber and reacted on the substrate surface to deposit silicon oxide, carbon-doped silicon oxide. In certain embodiments of cyclic CVD, no purge step is used.

[0059] In this or other embodiments, it is considered that the steps of the method described herein can be performed in various orders, and can be performed sequentially or simultaneously (e.g., during at least a portion of another step), and any combination thereof. Each step of supplying precursor and nitrogen-containing source gas can be performed with different durations for supplying them to vary the stoichiometric composition of the resulting silicon-containing film.

[0060] In another embodiment of the method disclosed herein, the film containing both silicon and nitrogen is formed by: a. providing a substrate in an ALD reactor; b. Formula I: [ka] wherein R 1 Linear or branched C1-C 10 Alkyl groups, linear or branched, C3-C 10 Alkenyl group, linear or branched C3-C 10 Alkynyl groups, C3-C 10 Cyclic alkyl groups, C2-C6 dialkylamino groups, electron-withdrawing groups and C6-C 10 aryl groups; R 2 is hydrogen, linear or branched C1-C 10 Alkyl groups, linear or branched C2-C6 alkenyl groups, linear or branched C3-C6 alkynyl groups, C3-C 10 Cyclic alkyl groups, C2-C6 dialkylamino groups, C6-C 10 Aryl groups, linear or branched C1-C6 fluorinated alkyl groups, electron-withdrawing groups, C4-C 10 two SiR groups selected from the group consisting of aryl groups and halides selected from the group consisting of Cl, Br, and I; X is a halide selected from the group consisting of Cl, Br, and I; 2 introducing at least one silazane precursor containing only one organoamino group linked to an X2 group into an ALD reactor to chemisorb the at least one silazane precursor onto the substrate; c. purging the reactor of any unreacted at least one silazane precursor using a purge gas; d. providing a nitrogen-containing source into the reactor to react with the chemisorbed at least one silazane precursor; e. optionally purging or pumping away any unreacted nitrogen-containing source; The film is formed using an ALD, PEALD, CCVD or PECCVD deposition method including: Steps b-e are repeated until the desired thickness of the film containing both silicon and nitrogen is reached. In one particular embodiment of the above invention, for high temperature deposition of silicon nitride or carbon doped silicon nitride, the substrate temperature is 600°C-850°C, 650°C-800°C or 700°C-800°C. In another embodiment, for low temperature deposition of silicon nitride or carbon doped silicon nitride, especially for X=I, the substrate temperature is 20°C-500°C, 20°C-400°C or 50°C-400°C.

[0061] In another aspect, a method of forming a film selected from a silicon oxide film and a carbon doped silicon oxide film by a PEALD or PECCVD deposition process, comprising: a. providing a substrate in a reactor; b. Formula I: [ka] wherein R 1 Linear or branched C1-C 10 Alkyl groups, linear or branched, C3-C 10 Alkenyl group, linear or branched C3-C 10 Alkynyl groups, C3-C 10 Cyclic alkyl groups, C2-C6 dialkylamino groups, electron-withdrawing groups and C6-C 10 aryl groups; R 2 is hydrogen, linear or branched C1-C 10 Alkyl groups, linear or branched C2-C6 alkenyl groups, linear or branched C3-C6 alkynyl groups, C3-C 10Cyclic alkyl groups, C2-C6 dialkylamino groups, C6-C 10 Aryl groups, linear or branched C1-C6 fluorinated alkyl groups, electron-withdrawing groups, C4-C 10 two SiR groups selected from the group consisting of aryl groups and halides selected from the group consisting of Cl, Br, and I; X is a halide selected from the group consisting of Cl, Br, and I; 2 introducing oxygen into a reactor along with at least one silazane precursor containing only one organoamino group linked to an X2 group; c. purging the reactor with a purge gas along with oxygen; d. introducing an oxygen-containing plasma; e. purging or pumping the reactor with a purge gas; and steps b to e are repeated until a film of a desired thickness is obtained. In some embodiments of the present invention, for low temperature deposition of silicon oxide, the substrate temperature is 20°C to 500°C, 20°C to 400°C, or 50°C to 400°C.

[0062] In another embodiment of the method disclosed herein, the silicon-containing film comprises: a. providing a substrate in a reactor; b. Formula I: [ka] wherein R 1 Linear or branched C1-C 10 Alkyl groups, linear or branched, C3-C 10 Alkenyl group, linear or branched C3-C 10 Alkynyl groups, C3-C 10 Cyclic alkyl groups, C2-C6 dialkylamino groups, electron-withdrawing groups and C6-C 10 aryl groups; R 2 is hydrogen, linear or branched C1-C 10 Alkyl groups, linear or branched C2-C6 alkenyl groups, linear or branched C3-C6 alkynyl groups, C3-C 10Cyclic alkyl groups, C2-C6 dialkylamino groups, C6-C 10 Aryl groups, linear or branched C1-C6 fluorinated alkyl groups, electron-withdrawing groups, C4-C 10 two SiR groups selected from the group consisting of aryl groups and halides selected from the group consisting of Cl, Br, and I; X is a halide selected from the group consisting of Cl, Br, and I; 2 introducing at least one silazane precursor containing only one organoamino group linked to an X2 group into a reactor to chemisorb the at least one silazane precursor onto the substrate; c. purging the at least one unreacted silazane precursor with a purge gas; d. providing an oxygen-containing source to the silazane precursor on the heated substrate to react with the at least one chemisorbed silazane precursor; e. optionally purging or pumping away any unreacted oxygen-containing source; The nanotubes are formed using ALD deposition methods including

[0063] In another embodiment, a method for forming a silicon nitride film or a silicon carbonitride film by a PEALD or PECCVD process comprises the steps of: a. providing a substrate in a reactor; b. a nitrogen-containing source and a compound of Formula I: [ka] wherein R 1 Linear or branched C1-C 10 Alkyl groups, linear or branched, C3-C 10 Alkenyl group, linear or branched C3-C 10 Alkynyl groups, C3-C 10 Cyclic alkyl groups, C2-C6 dialkylamino groups, electron-withdrawing groups and C6-C 10 aryl groups; R 2 is hydrogen, linear or branched C1-C 10Alkyl groups, linear or branched C2-C6 alkenyl groups, linear or branched C3-C6 alkynyl groups, C3-C 10 Cyclic alkyl groups, C2-C6 dialkylamino groups, C6-C 10 Aryl groups, linear or branched C1-C6 fluorinated alkyl groups, electron-withdrawing groups, C4-C 10 two SiR groups selected from the group consisting of aryl groups and halides selected from the group consisting of Cl, Br, and I; X is a halide selected from the group consisting of Cl, Br, and I; 2 introducing into a reactor at least one silazane precursor containing only one organoamino group linked to an X2 group; c. purging the reactor with a purge gas; d. introducing a nitrogen-containing plasma; e. purging or pumping the reactor with a purge gas; wherein steps b to e are repeated until a film of desired thickness is obtained. In one particular embodiment of the above invention, for low temperature deposition of silicon nitride or silicon oxycarbonitride, especially for X=I, the substrate temperature is 20° C.-500° C., 20° C.-400° C. or 50° C.-400° C.

[0064] The above steps define one cycle for the method described herein; the cycle can be repeated until a silicon-containing film of desired thickness is obtained.It is considered that in this embodiment or other embodiments, the steps of the method described herein can be carried out in various orders, and can be carried out sequentially or simultaneously (e.g., during at least a portion of another step), and any combination thereof.Each step of supplying precursor and oxygen-containing source can be carried out with different durations for supplying them to vary the stoichiometric composition of the silicon-containing film obtained, but always use oxygen in less than stoichiometric amount with respect to available silicon.

[0065] For multi-component silicon-containing films, other precursors, such as silicon-containing precursors, nitrogen-containing precursors, reducing agents, or other agents, can be alternately introduced into the reactor chamber.

[0066] In a further embodiment of the method described herein, the silicon-containing film is deposited using a thermal CVD process. In this embodiment, the method comprises: a. placing one or more substrates in a reactor and heating the reactor to one or more temperatures ranging from ambient temperature to about 1000°C; b. Formula I: [ka] wherein R 1 Linear or branched C1-C 10 Alkyl groups, linear or branched, C3-C 10 Alkenyl group, linear or branched C3-C 10 Alkynyl groups, C3-C 10 Cyclic alkyl groups, C2-C6 dialkylamino groups, electron-withdrawing groups and C6-C 10 aryl groups; R 2 is hydrogen, linear or branched C1-C 10 Alkyl groups, linear or branched C2-C6 alkenyl groups, linear or branched C3-C6 alkynyl groups, C3-C 10 Cyclic alkyl groups, C2-C6 dialkylamino groups, C6-C 10 Aryl groups, linear or branched C1-C6 fluorinated alkyl groups, electron-withdrawing groups, C4-C 10 two SiR groups selected from the group consisting of aryl groups and halides selected from the group consisting of Cl, Br, and I; X is a halide selected from the group consisting of Cl, Br, and I; 2 introducing at least one silazane precursor containing only one organic amino group linked to an X2 group; c. providing an oxygen-containing source into the reactor to at least partially react with the at least one silazane precursor to deposit a silicon-containing film on the one or more substrates; In a particular embodiment of the CVD method, during the introducing step, the reactor is held at a pressure between 10 mTorr and 760 Torr. The above steps define one cycle for the method described herein; the cycle can be repeated until a silicon-containing film of a desired thickness is obtained. It is understood that in this or other embodiments, the steps of the method described herein can be performed in various orders, sequentially or simultaneously (e.g., during at least a portion of another step), and any combination thereof. Each step of supplying the precursor and oxygen-containing source can be performed for different periods of time to supply them to vary the stoichiometric composition of the resulting silicon-containing film, but always uses oxygen in a less than stoichiometric amount relative to the available silicon.

[0067] In a further embodiment of the method described herein, an amorphous or crystalline silicon film is deposited using a precursor of formula I described herein. In this embodiment, the method comprises: a. placing one or more substrates in a reactor and heating the reactor to one or more temperatures ranging from ambient temperature to about 1000°C; b. Formula I: [ka] wherein R 1 Linear or branched C1-C 10 Alkyl groups, linear or branched, C3-C 10 Alkenyl group, linear or branched C3-C 10 Alkynyl groups, C3-C 10 Cyclic alkyl groups, C2-C6 dialkylamino groups, electron-withdrawing groups and C6-C 10 aryl groups; R 2 is hydrogen, linear or branched C1-C 10 Alkyl groups, linear or branched C2-C6 alkenyl groups, linear or branched C3-C6 alkynyl groups, C3-C 10 Cyclic alkyl groups, C2-C6 dialkylamino groups, C6-C 10Aryl groups, linear or branched C1-C6 fluorinated alkyl groups, electron-withdrawing groups, C4-C 10 two SiR groups selected from the group consisting of aryl groups and halides selected from the group consisting of Cl, Br, and I; X is a halide selected from the group consisting of Cl, Br, and I; 2 introducing at least one silazane precursor containing only one organic amino group linked to an X2 group; c. providing a source of reducing agent into the reactor to at least partially react with the at least one silazane precursor to deposit a silicon-containing film on the one or more substrates, wherein the reducing agent is selected from the group consisting of hydrogen, hydrogen plasma, and hydrogen chloride; In certain embodiments of the CVD method, during the introducing step, the reactor is held at a pressure between 10 mTorr and 760 Torr. The above steps define one cycle for the method described herein; the cycle can be repeated until a film of the desired thickness is obtained.

[0068] For multi-component silicon-containing films, other precursors, such as silicon-containing precursors, nitrogen-containing precursors, oxygen-containing sources, reducing agents, and / or other agents, can be alternately introduced into the reactor chamber.

[0069] In a further embodiment of the method described herein, the silicon-containing film is deposited using a thermal CVD process. In this embodiment, the method comprises: a. placing one or more substrates in a reactor and heating the reactor to one or more temperatures ranging from ambient temperature to about 1000°C; b. Formula I: [ka] wherein R 1 Linear or branched C1-C 10 Alkyl groups, linear or branched, C3-C 10 Alkenyl group, linear or branched C3-C 10 Alkynyl groups, C3-C 10Cyclic alkyl groups, C2-C6 dialkylamino groups, electron-withdrawing groups and C6-C 10 aryl groups; R 2 is hydrogen, linear or branched C1-C 10 Alkyl groups, linear or branched C2-C6 alkenyl groups, linear or branched C3-C6 alkynyl groups, C3-C 10 Cyclic alkyl groups, C2-C6 dialkylamino groups, C6-C 10 Aryl groups, linear or branched C1-C6 fluorinated alkyl groups, electron-withdrawing groups, C4-C 10 two SiR groups selected from the group consisting of aryl groups and halides selected from the group consisting of Cl, Br, and I; X is a halide selected from the group consisting of Cl, Br, and I; 2 introducing at least one silazane precursor containing only one organic amino group linked to an X2 group; d. providing a nitrogen-containing source into the reactor to at least partially react with the at least one silazane precursor to deposit a silicon-containing film on the one or more substrates; In certain embodiments of the CVD method, during the introducing step, the reactor is maintained at a pressure between 10 mTorr and 760 Torr.

[0070] In a further embodiment of the method described herein, a silicon-containing film, which may be amorphous or crystalline, and in one embodiment is a silicon carbonitride film, is deposited using a precursor of formula I described herein. In this embodiment, the method includes: a. placing one or more substrates in a reactor and heating the reactor to one or more temperatures ranging from ambient temperature to about 1000°C; b. Formula I: [ka] wherein R 1 Linear or branched C1-C 10 Alkyl groups, linear or branched, C3-C 10 Alkenyl group, linear or branched C3-C 10Alkynyl groups, C3-C 10 Cyclic alkyl groups, C2-C6 dialkylamino groups, electron-withdrawing groups and C6-C 10 aryl groups; R 2 is hydrogen, linear or branched C1-C 10 Alkyl groups, linear or branched C2-C6 alkenyl groups, linear or branched C3-C6 alkynyl groups, C3-C 10 Cyclic alkyl groups, C2-C6 dialkylamino groups, C6-C 10 Aryl groups, linear or branched C1-C6 fluorinated alkyl groups, electron-withdrawing groups, C4-C 10 two SiR groups selected from the group consisting of aryl groups and halides selected from the group consisting of Cl, Br, and I; X is a halide selected from the group consisting of Cl, Br, and I; 2 introducing at least one silazane precursor represented by one of the following silazane precursors containing only one organic amino group linked to an X2 group; c. purging the reactor with a purge gas; d. providing a plasma source into the reactor to at least partially react with the at least one silazane precursor to deposit a silicon-containing film on the one or more substrates; e. purging the reactor with a purge gas; Includes.

[0071] In the method described above, steps b to e define one cycle, and the cycle can be repeated until a film of a desired thickness is obtained. The thickness of the film is about 0.1 Å to about 1000 Å, about 0.1 Å to about 100 Å, or about 0.1 Å to about 10 Å. The plasma source is selected from the group consisting of hydrogen and argon-containing plasma, hydrogen and helium-containing plasma, argon plasma, helium plasma, other noble gas (e.g., neon (Ne), krypton (Kr) and xenon (Xe)) plasma, and combinations thereof. In one particular embodiment of the method, the silicon-containing film comprises silicon carbonitride.

[0072] In one embodiment of the method described herein, the silicon oxynitride or silicon oxycarbonitride film is deposited using a thermal ALD process. In this embodiment, the method includes: a. placing one or more substrates having surface features in an ALD reactor and heating the reactor to one or more temperatures in a range from about 600° C. to about 800° C., and optionally maintaining the reactor at a pressure of 100 Torr or less; b. 1,1,1,3,3,3-hexachloro-2-methyldisilazane, 1,1,1,3,3,3-hexachloro-2-ethyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-propyldisilazane, 1,1,1,3,3,3-hexachloro-2-isopropyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-butyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-propyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-butyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-butyldisilazane, 1,1,1,3,3,3-hexachloro -2-iso-butyldisilazane, 1,1,1,3,3-pentachloro-2-methyldisilazane, 1,1,1,3,3-pentachloro-2-ethyldisilazane, 1,1,1,3,3-pentachloro-2-n-propyldisilazane, 1,1,1,3,3-pentachloro-2-iso-propyldisilazane, 1,1,1,3,3-pentachloro-2-methyl-3-methyldisilazane, 1,1,1,3,3-pentachloro-2-ethyl-3-methyldisilazane, 1,1,1,3,3-pentachloro-2-n-propyl-3-methyldisilazane, 1,1,1, 3,3-Pentachloro-2-iso-propyl-3-methyldisilazane, 1,1,1,3,3,3-Hexabromo-2-methyldisilazane, 1,1,1,3,3,3-Bromo-2-ethyldisilazane, 1,1,1,3,3,3-Bromo-2-n-propyldisilazane, 1,1,1,3,3,3-Bromo-2-n-propyldisilazane, 1,1,1,3,3,3-Bromo-2-n-propyldisilazane, 1,1,1,3,3,3-Bromo-2-n-butyldisilazane, 1,1,1,3,3,3-Bromo-2-sec-butyldisilazane, 1,1,1 ,3,3,3-Bromo-2-iso-butyldisilazane, 1,1,1,3,3,3-Bromo-2-tert-butyldisilazane, 1,1,1,3,3,3-Hexaiodo-2-methyldisilazane, 1,1,1,3,3,3-Iodo-2-ethyldisilazane, 1,1,1,3,3,3-Iodo-2-n-propyldisilazane, 1,1,1,3,3,3-Iodo-2-n-butyldisilazane, 1,1,1,3,3,3-Iodo-2-iso-propyldisilazane, 1,1,1,3,3,3-Iodo-2-sec-butyldisilazane, 1,1,1,3,3,3-iodo-2-tert-butyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-methyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-tetrachloro-2-ethyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-n-propyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-isopropyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-n-butyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-isobutyldisilazane Silazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-sec-butyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-tert-butyldisilazane, 1,1,3,3-tetrachloro-2-methyldisilazane, 1,1,3,3-tetrachloro-2-ethyldisilazane, 1,1,3,3-tetrachloro-n-propyldisilazane, 1,1,3,3-tetrachloro-2-iso-propyldisilazane, 1,1,3,3-tetrachloro-2-n-butyldisilazane, 1,3,3-tetrachloro-2-iso-butyldisilazane , 1,1,3,3-tetrachloro-2-sec-butyldisilazane, 1,1,3,3-tetrachloro-2-tert-butyldisilazane, 1,1,3,3-tetrabromo-2-methyldisilazane, 1,1,3,3-tetrabromo-2-ethyldisilazane, 1,1,3,3-tetrabromo-n-propyldisilazane, 1,1,3,3-tetrabromo-2-iso-propyldisilazane, 1,1,3,3-tetrabromo-2-n-butyldisilazane, 1,1,3,3-tetrabromo-2-iso-butyldisilazane, 1,1,3,3-tetrabromo-2- sec-butyldisilazane, 1,1,3,3-tetrachloro-2-tert-butyldisilazane, 1,1,3,3-tetraiodo-2-methyldisilazane, 1,1,3,3-tetraiodo-2-ethyldisilazane, 1,1,3,3-tetraiodo-n-propyldisilazane, 1,1,3,3-tetraiodo-2-iso-propyldisilazane, 1,1,3,3-tetraiodo-2-n-butyldisilazane, 1,1,3,3-tetraiodo-2-iso-butyldisilazane, 1,1,3,3-tetraiodo-2-sec-butyldisilazane, 1,1,3,introducing into the reactor at least one silazane selected from the group consisting of 3-tetraiodo-2-tert-butyldisilazane, 1,1,3,3-tetrachloro-2-cyclopentyldisilazane, 1,1,3,3-tetrachloro-2-cyclohexyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-cyclopentyldisilazane, and 1,1,3,3-tetrachloro-1,3-dimethyl-2-cyclohexyldisilazane; c. purging the reactor with an inert gas, thereby removing unreacted silicon precursor and forming a composition comprising the purge gas and the silicon precursor; d. providing a nitrogen source into the reactor to react with the surface to form a silicon carbonitride film; e. purging with an inert gas to remove reaction by-products; f. providing an oxygen-containing source into the reactor; g. purging with an inert gas to remove reaction by-products; Steps b through g are repeated to provide a silicon oxynitride or silicon oxycarbonitride of the desired thickness.

[0073] In one embodiment of the method described herein, a carbon-doped silicon oxide film or silicon oxide film having a carbon content of 0 at% to 20 at% is deposited using a thermal ALD process and a hydrogen-containing plasma to improve the film's properties. In this embodiment, the method includes: h. placing one or more substrates having surface features into a reactor and heating the reactor to one or more temperatures ranging from ambient temperature to about 550° C., and optionally maintaining the reactor at a pressure of 100 Torr or less; i. 1,1,1,3,3,3-hexachloro-2-methyldisilazane, 1,1,1,3,3,3-hexachloro-2-ethyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-propyldisilazane, 1,1,1,3,3,3-hexachloro-2-isopropyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-butyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-propyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-butyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-butyldisilazane, -2-iso-butyldisilazane, 1,1,1,3,3-pentachloro-2-methyldisilazane, 1,1,1,3,3-pentachloro-2-ethyldisilazane, 1,1,1,3,3-pentachloro-2-n-propyldisilazane, 1,1,1,3,3-pentachloro-2-iso-propyldisilazane, 1,1,1,3,3-pentachloro-2-methyl-3-methyldisilazane, 1,1,1,3,3-pentachloro-2-ethyl-3-methyldisilazane, 1,1,1,3,3-pentachloro-2-n-propyl-3-methyldisilazane, 1,1,1, 3,3-Pentachloro-2-iso-propyl-3-methyldisilazane, 1,1,1,3,3,3-Hexabromo-2-methyldisilazane, 1,1,1,3,3,3-Bromo-2-ethyldisilazane, 1,1,1,3,3,3-Bromo-2-n-propyldisilazane, 1,1,1,3,3,3-Bromo-2-n-propyldisilazane, 1,1,1,3,3,3-Bromo-2-n-propyldisilazane, 1,1,1,3,3,3-Bromo-2-n-butyldisilazane, 1,1,1,3,3,3-Bromo-2-sec-butyldisilazane, 1,1,1 ,3,3,3-Bromo-2-iso-butyldisilazane, 1,1,1,3,3,3-Bromo-2-tert-butyldisilazane, 1,1,1,3,3,3-Hexaiodo-2-methyldisilazane, 1,1,1,3,3,3-Iodo-2-ethyldisilazane, 1,1,1,3,3,3-Iodo-2-n-propyldisilazane, 1,1,1,3,3,3-Iodo-2-n-butyldisilazane, 1,1,1,3,3,3-Iodo-2-iso-propyldisilazane, 1,1,1,3,3,3-Iodo-2-sec-butyldisilazane, 1,1,1,3,3,3-iodo-2-tert-butyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-methyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-tetrachloro-2-ethyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-n-propyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-isopropyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-n-butyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-isobutyldisilazane Silazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-sec-butyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-tert-butyldisilazane, 1,1,3,3-tetrachloro-2-methyldisilazane, 1,1,3,3-tetrachloro-2-ethyldisilazane, 1,1,3,3-tetrachloro-n-propyldisilazane, 1,1,3,3-tetrachloro-2-iso-propyldisilazane, 1,1,3,3-tetrachloro-2-n-butyldisilazane, 1,3,3-tetrachloro-2-iso-butyldisilazane , 1,1,3,3-tetrachloro-2-sec-butyldisilazane, 1,1,3,3-tetrachloro-2-tert-butyldisilazane, 1,1,3,3-tetrabromo-2-methyldisilazane, 1,1,3,3-tetrabromo-2-ethyldisilazane, 1,1,3,3-tetrabromo-n-propyldisilazane, 1,1,3,3-tetrabromo-2-iso-propyldisilazane, 1,1,3,3-tetrabromo-2-n-butyldisilazane, 1,1,3,3-tetrabromo-2-iso-butyldisilazane, 1,1,3,3-tetrabromo-2- sec-butyldisilazane, 1,1,3,3-tetrachloro-2-tert-butyldisilazane, 1,1,3,3-tetraiodo-2-methyldisilazane, 1,1,3,3-tetraiodo-2-ethyldisilazane, 1,1,3,3-tetraiodo-n-propyldisilazane, 1,1,3,3-tetraiodo-2-iso-propyldisilazane, 1,1,3,3-tetraiodo-2-n-butyldisilazane, 1,1,3,3-tetraiodo-2-iso-butyldisilazane, 1,1,3,3-tetraiodo-2-sec-butyldisilazane, 1,1,3,introducing into the reactor at least one silazane selected from the group consisting of 3-tetraiodo-2-tert-butyldisilazane, 1,1,3,3-tetrachloro-2-cyclopentyldisilazane, 1,1,3,3-tetrachloro-2-cyclohexyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-cyclopentyldisilazane, and 1,1,3,3-tetrachloro-1,3-dimethyl-2-cyclohexyldisilazane; j. purging the reactor with an inert gas, thereby removing unreacted silicon precursor and forming a composition comprising the purge gas and the silicon precursor; k. providing a nitrogen source into the reactor to react with the surface to form a silicon carbonitride film; l. purging with an inert gas to remove reaction by-products; m. repeating steps c through f to provide a carbon doped silicon nitride of a desired thickness; n. providing a post-deposition treatment of the carbon-doped silicon nitride film with an oxygen source, either in situ or in a separate chamber, at one or more temperatures ranging from about ambient temperature to 1000°C or from about 100°C to 400°C, to convert the carbon-doped silicon nitride film to a carbon-doped silicon oxide film; o. providing a post-deposition exposure of the carbon doped silicon oxide film to a hydrogen containing plasma to improve at least one of the properties of the film; p. Optionally, post-deposition processing the carbon-doped silicon oxide film using a spike anneal at a temperature of 400-1000° C. or a UV light source. In this or other embodiments, the UV exposure step can occur either during film deposition or after deposition is completed.

[0074] In one embodiment, the substrate comprises at least one feature comprising a patterned trench having an aspect ratio of 1:9 or greater, an opening of 180 nm or less.

[0075] In one embodiment of the method described herein, a carbon-doped silicon oxide film having a carbon content of 0 at% to 30 at% is deposited using a thermal ALD process and a hydrogen-containing plasma to improve the film's properties. a. placing one or more substrates having surface features into a reactor (e.g., in a conventional ALD reactor); b. heating the reactor to one or more temperatures ranging from ambient temperature to about 550° C., and optionally maintaining the reactor at a pressure of 100 Torr or less; c. 1,1,1,3,3,3-hexachloro-2-methyldisilazane, 1,1,1,3,3,3-hexachloro-2-ethyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-propyldisilazane, 1,1,1,3,3,3-hexachloro-2-isopropyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-butyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-propyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-butyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-butyldisilazane, 1,1,1,3,3,3-hexachloro -2-iso-butyldisilazane, 1,1,1,3,3-pentachloro-2-methyldisilazane, 1,1,1,3,3-pentachloro-2-ethyldisilazane, 1,1,1,3,3-pentachloro-2-n-propyldisilazane, 1,1,1,3,3-pentachloro-2-iso-propyldisilazane, 1,1,1,3,3-pentachloro-2-methyl-3-methyldisilazane, 1,1,1,3,3-pentachloro-2-ethyl-3-methyldisilazane, 1,1,1,3,3-pentachloro-2-n-propyl-3-methyldisilazane, 1,1,1, 3,3-Pentachloro-2-iso-propyl-3-methyldisilazane, 1,1,1,3,3,3-Hexabromo-2-methyldisilazane, 1,1,1,3,3,3-Bromo-2-ethyldisilazane, 1,1,1,3,3,3-Bromo-2-n-propyldisilazane, 1,1,1,3,3,3-Bromo-2-n-propyldisilazane, 1,1,1,3,3,3-Bromo-2-n-propyldisilazane, 1,1,1,3,3,3-Bromo-2-n-butyldisilazane, 1,1,1,3,3,3-Bromo-2-sec-butyldisilazane, 1,1,1 ,3,3,3-Bromo-2-iso-butyldisilazane, 1,1,1,3,3,3-Bromo-2-tert-butyldisilazane, 1,1,1,3,3,3-Hexaiodo-2-methyldisilazane, 1,1,1,3,3,3-Iodo-2-ethyldisilazane, 1,1,1,3,3,3-Iodo-2-n-propyldisilazane, 1,1,1,3,3,3-Iodo-2-n-butyldisilazane, 1,1,1,3,3,3-Iodo-2-iso-propyldisilazane, 1,1,1,3,3,3-Iodo-2-sec-butyldisilazane, 1,1,1,3,3,3-iodo-2-tert-butyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-methyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-tetrachloro-2-ethyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-n-propyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-isopropyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-n-butyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-isobutyldisilazane Silazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-sec-butyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-tert-butyldisilazane, 1,1,3,3-tetrachloro-2-methyldisilazane, 1,1,3,3-tetrachloro-2-ethyldisilazane, 1,1,3,3-tetrachloro-n-propyldisilazane, 1,1,3,3-tetrachloro-2-iso-propyldisilazane, 1,1,3,3-tetrachloro-2-n-butyldisilazane, 1,3,3-tetrachloro-2-iso-butyldisilazane , 1,1,3,3-tetrachloro-2-sec-butyldisilazane, 1,1,3,3-tetrachloro-2-tert-butyldisilazane, 1,1,3,3-tetrabromo-2-methyldisilazane, 1,1,3,3-tetrabromo-2-ethyldisilazane, 1,1,3,3-tetrabromo-n-propyldisilazane, 1,1,3,3-tetrabromo-2-iso-propyldisilazane, 1,1,3,3-tetrabromo-2-n-butyldisilazane, 1,1,3,3-tetrabromo-2-iso-butyldisilazane, 1,1,3,3-tetrabromo-2- sec-butyldisilazane, 1,1,3,3-tetrachloro-2-tert-butyldisilazane, 1,1,3,3-tetraiodo-2-methyldisilazane, 1,1,3,3-tetraiodo-2-ethyldisilazane, 1,1,3,3-tetraiodo-n-propyldisilazane, 1,1,3,3-tetraiodo-2-iso-propyldisilazane, 1,1,3,3-tetraiodo-2-n-butyldisilazane, 1,1,3,3-tetraiodo-2-iso-butyldisilazane, 1,1,3,3-tetraiodo-2-sec-butyldisilazane, 1,1,3,introducing into the reactor at least one silazane selected from the group consisting of 3-tetraiodo-2-tert-butyldisilazane, 1,1,3,3-tetrachloro-2-cyclopentyldisilazane, 1,1,3,3-tetrachloro-2-cyclohexyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-cyclopentyldisilazane, and 1,1,3,3-tetrachloro-1,3-dimethyl-2-cyclohexyldisilazane; d. purging the reactor with an inert gas; e. providing a nitrogen source into the reactor to react with the surface to form a carbon doped silicon nitride film; f. purging the reactor with an inert gas to remove reaction by-products; g. repeating steps c through f to provide a carbon doped silicon nitride of a desired thickness; h. providing a post-deposition treatment of the carbon-doped silicon nitride film with an oxygen source, either in situ or in a separate chamber, at one or more temperatures ranging from about ambient temperature to 1000° C. or from about 100° C. to 400° C., to convert the carbon-doped silicon nitride film to a carbon-doped silicon oxide film; i. providing a post-deposition exposure of the carbon-doped silicon oxide film to a hydrogen-containing plasma to improve at least one of the film's physical properties; j. Optionally, post-deposition processing the carbon-doped silicon oxide film using a thermal anneal at a temperature of 400-1000° C. or a UV light source. In this or other embodiments, the UV exposure step can occur either during film deposition or after deposition is completed.

[0076] In yet another further embodiment of the methods described herein, the silicon-containing film is deposited using a thermal ALD process with a catalyst comprising ammonia or an organic amine. In this embodiment, the method comprises: a. placing one or more substrates having surface features into a reactor; b. heating the reactor to one or more temperatures ranging from ambient temperature to about 150° C., and optionally maintaining the reactor at a pressure of 100 Torr or less; c. 1,1,1,3,3,3-hexachloro-2-methyldisilazane, 1,1,1,3,3,3-hexachloro-2-ethyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-propyldisilazane, 1,1,1,3,3,3-hexachloro-2-isopropyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-butyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-propyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-butyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-butyldisilazane, 1,1,1,3,3,3-hexachloro -2-iso-butyldisilazane, 1,1,1,3,3-pentachloro-2-methyldisilazane, 1,1,1,3,3-pentachloro-2-ethyldisilazane, 1,1,1,3,3-pentachloro-2-n-propyldisilazane, 1,1,1,3,3-pentachloro-2-iso-propyldisilazane, 1,1,1,3,3-pentachloro-2-methyl-3-methyldisilazane, 1,1,1,3,3-pentachloro-2-ethyl-3-methyldisilazane, 1,1,1,3,3-pentachloro-2-n-propyl-3-methyldisilazane, 1,1,1, 3,3-Pentachloro-2-iso-propyl-3-methyldisilazane, 1,1,1,3,3,3-Hexabromo-2-methyldisilazane, 1,1,1,3,3,3-Bromo-2-ethyldisilazane, 1,1,1,3,3,3-Bromo-2-n-propyldisilazane, 1,1,1,3,3,3-Bromo-2-n-propyldisilazane, 1,1,1,3,3,3-Bromo-2-n-propyldisilazane, 1,1,1,3,3,3-Bromo-2-n-butyldisilazane, 1,1,1,3,3,3-Bromo-2-sec-butyldisilazane, 1,1,1 ,3,3,3-Bromo-2-iso-butyldisilazane, 1,1,1,3,3,3-Bromo-2-tert-butyldisilazane, 1,1,1,3,3,3-Hexaiodo-2-methyldisilazane, 1,1,1,3,3,3-Iodo-2-ethyldisilazane, 1,1,1,3,3,3-Iodo-2-n-propyldisilazane, 1,1,1,3,3,3-Iodo-2-n-butyldisilazane, 1,1,1,3,3,3-Iodo-2-iso-propyldisilazane, 1,1,1,3,3,3-Iodo-2-sec-butyldisilazane, 1,1,1,3,3,3-iodo-2-tert-butyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-methyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-tetrachloro-2-ethyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-n-propyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-isopropyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-n-butyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-isobutyldisilazane Silazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-sec-butyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-tert-butyldisilazane, 1,1,3,3-tetrachloro-2-methyldisilazane, 1,1,3,3-tetrachloro-2-ethyldisilazane, 1,1,3,3-tetrachloro-n-propyldisilazane, 1,1,3,3-tetrachloro-2-iso-propyldisilazane, 1,1,3,3-tetrachloro-2-n-butyldisilazane, 1,3,3-tetrachloro-2-iso-butyldisilazane , 1,1,3,3-tetrachloro-2-sec-butyldisilazane, 1,1,3,3-tetrachloro-2-tert-butyldisilazane, 1,1,3,3-tetrabromo-2-methyldisilazane, 1,1,3,3-tetrabromo-2-ethyldisilazane, 1,1,3,3-tetrabromo-n-propyldisilazane, 1,1,3,3-tetrabromo-2-iso-propyldisilazane, 1,1,3,3-tetrabromo-2-n-butyldisilazane, 1,1,3,3-tetrabromo-2-iso-butyldisilazane, 1,1,3,3-tetrabromo-2- sec-butyldisilazane, 1,1,3,3-tetrachloro-2-tert-butyldisilazane, 1,1,3,3-tetraiodo-2-methyldisilazane, 1,1,3,3-tetraiodo-2-ethyldisilazane, 1,1,3,3-tetraiodo-n-propyldisilazane, 1,1,3,3-tetraiodo-2-iso-propyldisilazane, 1,1,3,3-tetraiodo-2-n-butyldisilazane, 1,1,3,3-tetraiodo-2-iso-butyldisilazane, 1,1,3,3-tetraiodo-2-sec-butyldisilazane, 1,1,3,introducing at least one silazane selected from the group consisting of 3-tetraiodo-2-tert-butyldisilazane, 1,1,3,3-tetrachloro-2-cyclopentyldisilazane, 1,1,3,3-tetrachloro-2-cyclohexyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-cyclopentyldisilazane, and 1,1,3,3-tetrachloro-1,3-dimethyl-2-cyclohexyldisilazane, and a catalyst into a reactor; d. purging the reactor with an inert gas; e. providing water vapor into the reactor to react with the precursor and catalyst to form an as-deposited film of carbon doped silicon oxide; f. purging the reactor with an inert gas to remove reaction by-products; g. repeating steps c through f to provide a carbon doped silicon oxide of a desired thickness; h. providing a post-deposition exposure of the treated film to a hydrogen-containing plasma to improve at least one of the film's properties; i. Optionally, post-deposition processing the carbon-doped silicon oxide film using a spike anneal at a temperature of 400-1000° C. or a UV light source; In this or other embodiments, the UV exposure step can occur either during film deposition or after deposition is completed.

[0077] In this or other embodiments, the catalyst is selected from Lewis bases such as pyridine, piperazine, ammonia, triethylamine or other organic amines. The amount of Lewis base vapor is at least 1 equivalent relative to the amount of silicon precursor vapor during step c.

[0078] In certain embodiments in which the film is treated with a plasma, the plasma source is selected from the group consisting of a hydrogen plasma, a hydrogen and helium containing plasma, and a hydrogen and argon containing plasma. The hydrogen plasma lowers the dielectric constant of the film and improves its damage resistance to subsequent plasma ashing processes, while still keeping the carbon content in the bulk nearly unchanged.

[0079] Throughout this specification, the term "ALD or ALD-like" refers to a process that includes, but is not limited to, the following processes: a) sequentially introducing each reactant, including a silicon precursor and a reactive gas, into a reactor, such as a single-wafer ALD reactor, a semi-batch ALD reactor, or a batch furnace ALD reactor; b) exposing each reactant, including a silicon precursor and a reactive gas, to a substrate by moving or rotating the substrate into different compartments of the reactor, each compartment being separated by an inert gas curtain, i.e., a spatial ALD reactor or a roll-to-roll ALD reactor.

[0080] Throughout this specification, the term "ashing" refers to a process of removing photoresist or carbon hardmask in a semiconductor manufacturing process using a plasma containing an oxygen source, such as an O2 / inert gas plasma, an O2 plasma, a CO2 plasma, a CO plasma, an H2 / O2 plasma, or combinations thereof.

[0081] Throughout this specification, the term "damage resistance" refers to the properties of a film after an oxygen ashing process. Good or high damage resistance is defined as the following film properties after oxygen ashing: dielectric constant of the film lower than 4.5; carbon content in the bulk (greater than 50 Å deep into the film) within 5 at% of before ashing; less than 50 Å of the film is damaged as observed by the difference in dilute HF etch rate between the film near the surface (less than 50 Å deep) and the bulk (greater than 50 Å deep).

[0082] In certain embodiments, the silazane precursors having formula I described herein can also be used as dopants for metal-containing films, such as, but not limited to, metal oxide films or metal nitride films. In these embodiments, the metal-containing films are deposited using ALD or CVD processes, such as, but not limited to, ALD or CVD processes described herein using metal alkoxide, metal amide, or volatile organometallic precursors. Examples of suitable metal alkoxide precursors that can be used with the methods disclosed herein include, but are not limited to, Group 3-6 metal alkoxides, Group 3-6 metal complexes having both alkoxy and alkyl-substituted cyclopentadienyl ligands, Group 3-6 metal complexes having both alkoxy and alkyl-substituted pyrrolyl ligands, Group 3-6 metal complexes having both alkoxy and diketonate ligands, and Group 3-6 metal complexes having both alkoxy and ketoester ligands.Examples of suitable metal amide precursors that can be used with the methods disclosed herein include, but are not limited to, tetrakis(dimethylamino)zirconium (TDMAZ), tetrakis(diethylamino)zirconium (TDEAZ), tetrakis(ethylmethylamino)zirconium (TEMAZ), tetrakis(dimethylamino)hafnium (TDMAH), tetrakis(diethylamino)hafnium (TDEAH), tetrakis(ethylmethylamino)hafnium (TEMAH), tetrakis(dimethylamino)titanium (TDMAT), tetrakis(diethylamino)titanium (TDEAT), tetrakis(ethylmethylamino)titanium (TEMAT), tert-butyliminotri(diethylamino)tantalum (TBTDET), tert-butyliminotri(dimethylamino)tantalum (T BTDMT), tert-butylimino tri(ethylmethylamino)tantalum (TBTEMT), ethylimino tri(diethylamino)tantalum (EITDET), ethylimino tri(dimethylamino)tantalum (EITDMT), ethylimino tri(ethylmethylamino)tantalum (EITEMT), tert-amylimino tri(dimethylamino)tantalum (TAIMAT), tert-amylimino tri(diethylamino)tantalum, pentakis(dimethylamino)tantalum, tert-amylimino tri(ethylmethylamino)tantalum, bis(tert-butylimino)bis(dimethylamino)tungsten (BTBMW), bis(tert-butylimino)bis(diethylamino)tungsten, bis(tert-butylimino)bis(ethylmethylamino)tungsten, and combinations thereof. Examples of suitable organometallic precursors that can be used with the methods disclosed herein include, but are not limited to, Group 3 metal cyclopentadienyls or alkylcyclopentadienyls. Exemplary Group 3-6 metals herein include, but are not limited to, Y, La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Er, Yb, Lu, Ti, Hf, Zr, V, Nb, Ta, Cr, Mo, and W.

[0083] In certain embodiments, the resulting silicon-containing film or coating can be subjected to post-deposition treatments, such as, but not limited to, plasma treatments, chemical treatments, ultraviolet light exposure, electron beam exposure, and / or other treatments that affect one or more properties of the film.

[0084] In certain embodiments, the silicon-containing films described herein have a dielectric constant of 6 or less. In these or other embodiments, the films can have a dielectric constant of about 5 or less, about 4 or less, or about 3.5 or less. However, it is believed that films having other dielectric constants (e.g., higher or lower) can be formed depending on the desired end use of the film. Examples of silicon-containing films or silicon-containing films formed using the silazane precursors and processes described herein are of the formula Si x O y C z N v H w and Si ranges from about 10% to about 40%, O ranges from about 0% to about 65%, C ranges from about 0% to about 75% or about 0% to about 50%, N ranges from about 0% to about 75% or about 0% to about 50%, and H ranges from about 0% to about 50% atomic percent weight percent, with x+y+z+v+w=100 atomic percent weight percent. Another example of a silicon-containing film formed using the silazane precursors and processes described herein is silicon carbonitride, with a carbon content of 1 at% to 80 at%, as measured by XPS. Yet another example of a silicon-containing film formed using the silazane precursors and processes described herein is amorphous silicon, with a sum of both the nitrogen content and the carbon content of less than 10 at%, preferably less than 5 at%, and most preferably less than 1 at%, as measured by XPS.

[0085] As described above, the method described herein can be used to deposit silicon-containing film on at least a portion of a substrate.Examples of suitable substrates include, but are not limited to, silicon, germanium-doped silicon, germanium, SiO2, Si3N4, OSG, FSG, silicon carbide, hydrogenated silicon carbide, silicon nitride, hydrogenated silicon nitride, silicon carbonitride, hydrogenated silicon carbonitride, boron nitride, anti-reflective coating, photoresist, flexible substrate, organic polymer, porous organic and inorganic material, metal, such as copper and aluminum, and diffusion barrier layer, such as, but not limited to, TiN, Ti(C)N, TaN, Ta(C)N, Ta, W or WN.The film is compatible with various subsequent processing steps, such as chemical mechanical planarization (CMP) and anisotropic etching process.

[0086] The deposited films have applications including, but not limited to, computer chips, optical devices, magnetic information storage devices, coatings on supporting materials or substrates, microelectromechanical systems (MEMS), nanoelectromechanical systems, thin film transistors (TFTs), light emitting diodes (LEDs), organic light emitting diodes (OLEDs), IGZO, and liquid crystal displays (LCDs).

[0087] The following examples illustrate methods for preparing silazane precursors and for depositing silicon-containing films described herein, but are not intended to be limiting in any way. EXAMPLES

[0088] Example 1a. Synthesis of 1,1,1,3,3,3-hexachloro-2-methyldisilazane

[0089] Heptamethyldisilazane (20 g, 0.11 mol), silicon tetrachloride (155 g, 0.91 mol), and pyridine (0.45 g, 0.0057 mol) were combined in a 100 mL glass bottle and stirred at 70-80 °C for 5 days. When the mixture was analyzed by gas chromatography-mass spectrometry (GC-MS), the desired product, 1,1,1,3,3,3-hexachloro-2-methyldisilazane, was identified by the following mass peaks: m / z = 296 (M+), 261, 212, 175, 162, 135, 126, 98, 63.

[0090] Example 1b. Alternative synthesis of 1,1,1,3,3,3-hexachloro-2-methyldisilazane

[0091] A solution of methylamine (100 mL of a 1.0 M solution in THF, 0.1 mol) is added dropwise at -20°C to a 1 L three-neck round bottom flask containing a stirred mixture of 0.4 mol silicon tetrachloride, 0.22 mol triethylamine, and 300 mL hexane. The resulting slurry is stirred while warmed to room temperature and filtered to remove the white solids. The filtrate is purified by vacuum distillation to give the desired product, 1,1,1,3,3,3-hexachloro-2-methyldisilazane.

[0092] Example 2. Synthesis of 1,1,3,3-tetrachloro-1,3-dimethyl-2-methyldisilazane

[0093] In a 500 mL round bottom flask, heptamethyldisilazane (88.7 g, 0.506 mol) and trichloromethylsilane (302 g, 2.02 mol) were stirred at room temperature for one week. To this mixture, HCl solution (85 mL of a 1.0 M solution in Et2O, 0.085 mol) was added and the reaction mixture was heated to about 50° C. for five days. The translucent mixture was filtered and purified by vacuum distillation to give 48 g of purified 1,1,3,3-tetrachloro-1,3-dimethyl-2-methyldisilazane. The boiling point was measured to be 199° C. by differential scanning calorimetry (DSC). GC-MS showed the following peaks: m / z=256 (M+), 242, 220, 212, 204, 190, 177, 142, 126, 113, 106, 92, 79, 63.

[0094] Example 2b. Alternative synthesis of 1,1,3,3-tetrachloro-1,3-dimethyl-2-methyldisilazane

[0095] A solution of methylamine (100 mL of a 1.0 M solution in THF, 0.1 mol) is added dropwise to a 1 L three-necked round bottom flask containing a stirred mixture of trichloromethylsilane (0.4 mol), triethylamine (0.22 mol), and hexanes (300 mL) at -20°C. The resulting slurry is stirred while warmed to room temperature and filtered to remove the white solids. The filtrate is purified by vacuum distillation to give the desired product, 1,1,3,3-tetrachloro-1,3-dimethyl-2-methyldisilazane.

[0096] Example 3. Thermal stability of 1,1,3,3-tetrachloro-1,3-dimethyl-2-methyldisilazane

[0097] Two 1 mL samples of purified 1,1,3,3-tetrachloro-1,3-dimethyl-2-methyldisilazane were heated in sealed 3.8 mL stainless steel tubes at 80° C. for 7 days. The heated samples were cooled to room temperature and analyzed by gas chromatography (GC). The analysis of 1,1,3,3-tetrachloro-1,3-dimethyl-2-methyldisilazane decreased from 95.72% to an average of 95.69%, indicating that 1,1,3,3-tetrachloro-1,3-dimethyl-2-methyldisilazane has excellent thermal stability and is suitable as a precursor for vapor deposition processes.

[0098] Example 3a. Synthesis of 1,1,3,3-tetrachloro-2-methyldisilazane

[0099] In a 500 mL round bottom flask, heptamethyldisilazane (0.5 mol) and trichlorosilane (2 mol) are stirred at either room temperature or elevated temperature for one week. Optionally, pyridine or HCl (1.0 M in Et2O) is added to the reaction mixture to promote complete conversion. The translucent mixture is filtered and purified by vacuum distillation to provide purified 1,1,3,3-tetrachloro-2-methyldisilazane.

[0100] Example 3b. Alternative synthesis of 1,1,3,3-tetrachloro-2-methyldisilazane

[0101] A solution of methylamine (100 mL of a 1.0 M solution in THF, 0.1 mol) is added dropwise to a 1 L three-neck round bottom flask containing a stirred mixture of trichlorosilane (0.4 mol), triethylamine (0.22 mol), and hexanes (300 mL) at -20°C. The resulting slurry is stirred while warmed to room temperature and filtered to remove the white solids. The filtrate is purified by vacuum distillation to give the desired product, 1,1,3,3-tetrachloro-1,3-dimethyl-2-methyldisilazane.

[0102] Example 4. Precursor thermal stability of 1,1,1,3,3,3-hexachloro-2-methyldisilazane to 1,1,1,3,3,3-hexachloro-disilazane

[0103] 1,1,1,3,3,3-Hexachloro-disilazane and 1,1,1,3,3,3-Hexachloro-2-methyldisilazane as silazane precursors were introduced into the ALD chamber with the following steps: (a) introducing the silicon precursor for 10 seconds; (b) purging with nitrogen. Steps (a) and (b) were repeated for 300 cycles. The thickness and refractive index (RI) of the film were measured using a FilmTek 2000SE ellipsometer by fitting the reflectance data from the film to a predefined physical model (e.g., Lorentz Oscillator model). Table 2 summarizes the films formed by thermal deposition of the silazane precursors at substrate temperatures of 650°C and 700°C, respectively, showing that 1,1,1,3,3,3-Hexachloro-2-methyldisilazane has less decomposition and is therefore a better precursor for high-temperature ALD applications.

[0104] Table 2. Pyrolysis of silazane precursors [Table 2]

[0105] Example 5. High Temperature ALD of Silicon Nitride Using 1,1,1,3,3,3-Hexachloro-2-methyldisilazane

[0106] 1,1,1,3,3,3-Hexachloro-disilazane as a silazane precursor and 1,1,1,3,3,3-Hexachloro-2-methyldisilazane were introduced into the ALD chamber with the following steps: (a) silicon precursor introduction for 10 seconds; (b) purging with nitrogen; (c) ammonia introduction for 24 seconds; (d) purging with nitrogen. Steps (a)-(d) are repeated multiple cycles to obtain a film thick enough for analysis. The thickness and refractive index (RI) of the film were measured using a FilmTek 2000SE ellipsometer by fitting the reflectance data from the film to a predefined physical model (e.g., Lorentz Oscillator model). Wet etch rates were performed using a 1% solution of 49% hydrofluoric (HF) acid in deionized water (approximately 0.5 wt% HF). For each batch, the solution concentration was confirmed using a thermal oxide wafer as a reference. The wet etch rate (WER) of a typical thermal oxide wafer for 0.5 wt% HF in deionized water is 0.5 Å / s. The film thickness before and after etching was used to calculate the wet etch rate. Table 3 lists the growth rates per cycle (GPC) and shows that 1,1,1,3,3,3-hexachloro-2-methyldisilazane is suitable for ALD silicon nitride at temperatures above 650°C, while 1,1,1,3,3,3-hexachloro-disilazane with NH groups is resistant to chemical vapor deposition at 700°C, i.e., the GPC is greater than 3.0 Å / cycle.

[0107] Table 3. Comparison of silicon nitride growth rates using 1,1,1,3,3,3-hexachloro-2-methyldisilazane and 1,1,1,3.3.3-hexachloro-disilazane [Table 3]

[0108] Example 6. High Temperature ALD of Silicon Oxynitride Using 1,1,1,3,3,3-Hexachloro-2-methyldisilazane

[0109] 1,1,1,3,3,3-hexachloro-2-methyldisilazane as a silazane precursor was introduced into the ALD chamber with the following steps: (a) silicon precursor introduction for 10 seconds; (b) purging with nitrogen; (c) ammonia introduction for 24 seconds; (d) purging with nitrogen; (e) water vapor introduction for 2 or 5 seconds; (f) purging with nitrogen. Steps (a)-(f) were repeated for 200 cycles. The results are listed in Table 4 and show that 1,1,1,3,3,3-hexachloro-2-methyldisilazane is suitable for ALD silicon oxynitride at temperatures higher than 700° C.

[0110] Table 4. Growth rate and some physical properties of silicon oxynitride using 1,1,1,3,3,3-hexachloro-2-methyldisilazane [Table 4] The present invention can be embodied in the following manner. (Appendix 1) Formula I below: [ka] wherein R 1 is linear or branched C 1 ~C 10 Alkyl group, linear or branched C 3 ~C 10 Alkenyl group, linear or branched C 3 ~C 10 Alkynyl group, C 3 ~C 10 Cyclic alkyl groups, C 2 ~C 6 Dialkylamino group, electron-withdrawing group and C 6 ~C 10 aryl groups; R 2 is hydrogen, linear or branched C 1 ~C 10 Alkyl group, linear or branched C 3 ~C 6 Alkenyl group, linear or branched C 2 ~C 6 Alkynyl group, C 3 ~C10 Cyclic alkyl groups, C 2 ~C 6 Dialkylamino group, C 6 ~C 10 Aryl groups, linear or branched C 1 ~C 6 Fluorinated alkyl groups, electron-withdrawing groups, C 4 ~C 10 1. A composition comprising a silazane precursor, wherein X is selected from the group consisting of an aryl group and a halide selected from the group consisting of Cl, Br, and I; and X is a halide selected from the group consisting of Cl, Br, and I, and which is free of organic amines, halide ions, and metal ions. (Appendix 2) The silazane precursor is 1,1,1,3,3,3-hexachloro-2-methyldisilazane, 1,1,1,3,3,3-hexachloro-2-ethyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-propyldisilazane, 1,1,1,3,3,3-hexachloro-2-isopropyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-butyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-propyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-butyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-butyldisilazane, 1,1,1,3,3,3-hexachloro-2-iso-butyldisilazane, 1,1,1,3,3,3-hexabromo-2-methyldisilazane, 1,1,1,3,3-pentachloro-2-methyldisilazane, 1,1,1,3,3-pentachloro-2-ethyldisilazane, 1,1,1,3,3-pentachloro-2-n-propyldisilazane, 1,1,1,3,3-pentachloro-2-iso-propyldisilazane, 1,1,1,3,3-pentachloro-2-methyl-3-methyldisilazane, 1,1,1,3,3-pentachloro-2-ethyl-3-methyldisilazane, 1,1,1,3,3 -Pentachloro-2-n-propyl-3-methyldisilazane, 1,1,1,3,3-pentachloro-2-iso-propyl-3-methyldisilazane, 1,1,1,3,3,3-bromo-2-ethyldisilazane, 1,1,1,3,3,3-bromo-2-n-propyldisilazane, 1,1,1,3,3,3-bromo-2-n-propyldisilazane, 1,1,1,3,3,3-bromo-2-n-propyldisilazane, 1,1,1,3,3,3-bromo-2-n-butyldisilazane, 1,1,1,3,3,3-bromo-2-sec-butyldisilazane, 1,1 ,1,3,3,3-Bromo-2-iso-butyldisilazane, 1,1,1,3,3,3-Bromo-2-tert-butyldisilazane, 1,1,1,3,3,3-Hexaiodo-2-methyldisilazane, 1,1,1,3,3,3-Iodo-2-ethyldisilazane, 1,1,1,3,3,3-Iodo-2-n-propyldisilazane, 1,1,1,3,3,3-Iodo-2-n-butyldisilazane, 1,1,1,3,3,3-Iodo-2-iso-propyldisilazane, 1,1,1,3,3,3-Iodo-2-sec-butyldisilazane, 1,1,1,3,3,3-iodo-2-tert-butyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-methyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-tetrachloro-2-ethyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-n-propyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-isopropyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-n-butyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-isobutyldisilazane Silazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-sec-butyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-tert-butyldisilazane, 1,1,3,3-tetrachloro-2-methyldisilazane, 1,1,3,3-tetrachloro-2-ethyldisilazane, 1,1,3,3-tetrachloro-n-propyldisilazane, 1,1,3,3-tetrachloro-2-iso-propyldisilazane, 1,1,3,3-tetrachloro-2-n-butyldisilazane, 1,3,3-tetrachloro-2-iso-butyldisilazane , 1,1,3,3-tetrachloro-2-sec-butyldisilazane, 1,1,3,3-tetrachloro-2-tert-butyldisilazane, 1,1,3,3-tetrabromo-2-methyldisilazane, 1,1,3,3-tetrabromo-2-ethyldisilazane, 1,1,3,3-tetrabromo-n-propyldisilazane, 1,1,3,3-tetrabromo-2-iso-propyldisilazane, 1,1,3,3-tetrabromo-2-n-butyldisilazane, 1,1,3,3-tetrabromo-2-iso-butyldisilazane, 1,1,3,3-tetrabromo-2- sec-butyldisilazane, 1,1,3,3-tetrachloro-2-tert-butyldisilazane, 1,1,3,3-tetraiodo-2-methyldisilazane, 1,1,3,3-tetraiodo-2-ethyldisilazane, 1,1,3,3-tetraiodo-n-propyldisilazane, 1,1,3,3-tetraiodo-2-iso-propyldisilazane, 1,1,3,3-tetraiodo-2-n-butyldisilazane, 1,1,3,3-tetraiodo-2-iso-butyldisilazane, 1,1,3,3-tetraiodo-2-sec-butyldisilazane, 1,1,3,The composition of claim 1, wherein the silazane is selected from the group consisting of 3-tetraiodo-2-tert-butyldisilazane, 1,1,3,3-tetrachloro-2-cyclopentyldisilazane, 1,1,3,3-tetrachloro-2-cyclohexyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-cyclopentyldisilazane, and 1,1,3,3-tetrachloro-1,3-dimethyl-2-cyclohexyldisilazane. (Appendix 3) (a) Formula I:

change

change

change

Claims

1. A composition for forming a silicon-containing film, comprising: 【Chemistry 1】 wherein R 1 is selected from the group consisting of methyl, ethyl, propyl, isopropyl, butyl, isobutyl, sec-butyl, tert-butyl, cyclopentyl, and cyclohexyl; R 2 is selected from the group consisting of hydrogen, methyl, and a halide selected from the group consisting of Cl, Br, and I; and X is a halide selected from the group consisting of Cl, Br, and I, and the composition is free of organic amines, halide ions, and metal ions.

2. The silazane precursor is 1,1,1,3,3,3-hexachloro-2-methyldisilazane, 1,1,1,3,3,3-hexachloro-2-ethyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-propyldisilazane, 1,1,1,3,3,3-hexachloro-2-iso-propyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-butyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-propyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-butyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-butyldisilazane, 1,1,1,3,3,3-hexabromo-2-methyldisilazane, 1,1,1,3,3-pentachloro-2-methyldisilazane, 1,1,1,3,3-pentachloro-2-ethyldisilazane, 1,1,1,3,3-pentachloro-2-n-propyldisilazane, 1,1,1,3,3-pentachloro-2-iso-propyldisilazane, 1,1,1,3,3-pentachloro-2-methyl-3-methyldisilazane, 1,1,1,3,3-pentachloro-2-ethyl-3-methyldisilazane, 1,1,1,3,3-pentachloro -2-n-propyl-3-methyldisilazane, 1,1,1,3,3-pentachloro-2-iso-propyl-3-methyldisilazane, 1,1,1,3,3,3-bromo-2-ethyldisilazane, 1,1,1,3,3,3-bromo-2-n-propyldisilazane, 1,1,1,3,3,3-bromo-2-n-butyldisilazane, 1,1,1,3,3,3-bromo-2-sec-butyldisilazane, 1,1,1,3,3,3-bromo-2-iso-butyldisilazane, 1,1,1,3,3,3-bromo-2-tert-butyldisilazane, 1,1,1,3,3,3- Hexaiodo-2-methyldisilazane, 1,1,1,3,3,3-iodo-2-ethyldisilazane, 1,1,1,3,3,3-iodo-2-n-propyldisilazane, 1,1,1,3,3,3-iodo-2-n-butyldisilazane, 1,1,1,3,3,3-iodo-2-iso-propyldisilazane, 1,1,1,3,3,3-iodo-2-sec-butyldisilazane, 1,1,1,3,3,3-iodo-2-tert-butyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-methyldisilazane, 1,1,3,3-tetrachloro-1,3-Dimethyl-tetrachloro-2-ethyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-n-propyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-iso-propyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-n-butyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-iso-butyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-sec-butyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-tert-butyl Disilazane, 1,1,3,3-tetrachloro-2-methyldisilazane, 1,1,3,3-tetrachloro-2-ethyldisilazane, 1,1,3,3-tetrachloro-n-propyldisilazane, 1,1,3,3-tetrachloro-2-iso-propyldisilazane, 1,1,3,3-tetrachloro-2-n-butyldisilazane, 1,3,3-tetrachloro-2-iso-butyldisilazane, 1,1,3,3-tetrachloro-2-sec-butyldisilazane, 1,1,3,3-tetrachloro-2-tert-butyldisilazane, 1,1,3,3-tetrabromo-2-methyldisilazane 1,1,3,3-tetrabromo-2-ethyldisilazane, 1,1,3,3-tetrabromo-n-propyldisilazane, 1,1,3,3-tetrabromo-2-iso-propyldisilazane, 1,1,3,3-tetrabromo-2-n-butyldisilazane, 1,1,3,3-tetrabromo-2-iso-butyldisilazane, 1,1,3,3-tetrabromo-2-sec-butyldisilazane, 1,1,3,3-tetrachloro-2-tert-butyldisilazane, 1,1,3,3-tetraiodo-2-methyldisilazane, 1,1,3,3-tetraiodo-2-methyldisilazane, -ethyldisilazane, 1,1,3,3-tetraiodo-n-propyldisilazane, 1,1,3,3-tetraiodo-2-iso-propyldisilazane, 1,1,3,3-tetraiodo-2-n-butyldisilazane, 1,1,3,3-tetraiodo-2-iso-butyldisilazane, 1,1,3,3-tetraiodo-2-sec-butyldisilazane, 1,1,3,3-tetraiodo-2-tert-butyldisilazane, 1,1,3,3-tetrachloro-2-cyclopentyldisilazane, 1,1,3,3-tetrachloro-2-cyclohexyldisilazane, 1,1,3,The composition according to claim 1, which is selected from the group consisting of 3-tetrachloro-1,3-dimethyl-2-cyclopentyldisilazane and 1,1,3,3-tetrachloro-1,3-dimethyl-2-cyclohexyldisilazane.

3. A composition for forming a silicon-containing film, comprising: (a) Formula I: 【Chemistry 2】 wherein R 1 is selected from the group consisting of methyl, ethyl, propyl, isopropyl, butyl, isobutyl, sec-butyl, tert-butyl, cyclopentyl, and cyclohexyl; R 2 at least one silazane in which X is selected from the group consisting of hydrogen, methyl, and a halide selected from the group consisting of Cl, Br, and I; and X is a halide selected from Cl, Br, and I; (b) a solvent having a boiling point, the difference between the boiling point of the solvent and the boiling point of the at least one silazane being 40° C. or less; and being substantially free of organic amines, halide ions and metal ions.

4. The silazane precursor is 1,1,1,3,3,3-hexachloro-2-methyldisilazane, 1,1,1,3,3,3-hexachloro-2-ethyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-propyldisilazane, 1,1,1,3,3,3-hexachloro-2-iso-propyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-butyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-propyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-butyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-butyldisilazane, 1,1,1,3,3-pentachloro-2-methyldisilazane, 1,1,1,3,3-pentachloro-2-ethyldisilazane, 1,1,1,3,3-pentachloro-2-n-propyldisilazane, 1,1,1,3,3-pentachloro-2-iso-propyldisilazane, 1,1,1,3,3-pentachloro-2-methyl-3-methyldisilazane, 1,1,1,3,3-pentachloro-2-ethyl-3-methyldisilazane, 1,1,1,3,3-pentachloro-2-n-propyl-3-methyldisilazane, -pentachloro-2-iso-propyl-3-methyldisilazane, 1,1,1,3,3,3-hexabromo-2-methyldisilazane, 1,1,1,3,3,3-bromo-2-ethyldisilazane, 1,1,1,3,3,3-bromo-2-n-propyldisilazane, 1,1,1,3,3,3-bromo-2-n-butyldisilazane, 1,1,1,3,3,3-bromo-2-sec-butyldisilazane, 1,1,1,3,3,3-bromo-2-iso-butyldisilazane, 1,1,1,3,3,3-bromo-2-tert-butyldisilazane, 1,1,1,3,3,3- Hexaiodo-2-methyldisilazane, 1,1,1,3,3,3-iodo-2-ethyldisilazane, 1,1,1,3,3,3-iodo-2-n-propyldisilazane, 1,1,1,3,3,3-iodo-2-n-butyldisilazane, 1,1,1,3,3,3-iodo-2-iso-propyldisilazane, 1,1,1,3,3,3-iodo-2-sec-butyldisilazane, 1,1,1,3,3,3-iodo-2-tert-butyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-methyldisilazane, 1,1,3,3-tetrachloro-1,3-Dimethyl-tetrachloro-2-ethyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-n-propyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-iso-propyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-n-butyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-iso-butyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-sec-butyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-tert-butyl Disilazane, 1,1,3,3-tetrachloro-2-methyldisilazane, 1,1,3,3-tetrachloro-2-ethyldisilazane, 1,1,3,3-tetrachloro-n-propyldisilazane, 1,1,3,3-tetrachloro-2-iso-propyldisilazane, 1,1,3,3-tetrachloro-2-n-butyldisilazane, 1,3,3-tetrachloro-2-iso-butyldisilazane, 1,1,3,3-tetrachloro-2-sec-butyldisilazane, 1,1,3,3-tetrachloro-2-tert-butyldisilazane, 1,1,3,3-tetrabromo-2-methyldisilazane 1,1,3,3-tetrabromo-2-ethyldisilazane, 1,1,3,3-tetrabromo-n-propyldisilazane, 1,1,3,3-tetrabromo-2-iso-propyldisilazane, 1,1,3,3-tetrabromo-2-n-butyldisilazane, 1,1,3,3-tetrabromo-2-iso-butyldisilazane, 1,1,3,3-tetrabromo-2-sec-butyldisilazane, 1,1,3,3-tetrachloro-2-tert-butyldisilazane, 1,1,3,3-tetraiodo-2-methyldisilazane, 1,1,3,3-tetraiodo-2-methyldisilazane, -ethyldisilazane, 1,1,3,3-tetraiodo-n-propyldisilazane, 1,1,3,3-tetraiodo-2-iso-propyldisilazane, 1,1,3,3-tetraiodo-2-n-butyldisilazane, 1,1,3,3-tetraiodo-2-iso-butyldisilazane, 1,1,3,3-tetraiodo-2-sec-butyldisilazane, 1,1,3,3-tetraiodo-2-tert-butyldisilazane, 1,1,3,3-tetrachloro-2-cyclopentyldisilazane, 1,1,3,3-tetrachloro-2-cyclohexyldisilazane, 1,1,3,The composition according to claim 3, comprising at least one selected from the group consisting of 3-tetrachloro-1,3-dimethyl-2-cyclopentyldisilazane and 1,1,3,3-tetrachloro-1,3-dimethyl-2-cyclohexyldisilazane.

5. 4. The composition of claim 3, wherein the solvent comprises at least one selected from the group consisting of ethers, alkyl hydrocarbons, and aromatic hydrocarbons.

6. 1. A method for forming a silicon-containing film on at least one surface of a substrate by a deposition process selected from a chemical vapor deposition process and an atomic layer deposition process, comprising: providing at least one surface of a substrate in a reaction chamber; Formula I below: 【Chemistry 3】 wherein R 1 is selected from the group consisting of methyl, ethyl, propyl, isopropyl, butyl, isobutyl, sec-butyl, tert-butyl, cyclopentyl, and cyclohexyl; R 2 is selected from hydrogen, methyl, and a halide selected from the group consisting of Cl, Br, and I; and X is a halide selected from the group consisting of Cl, Br, and I; introducing a nitrogen-containing source into the reactor, where the at least one silazane precursor and the nitrogen-containing source react to form a film on the at least one surface; wherein the silazane is substantially free of organic amines, halide ions and metal ions.

7. The at least one silazane is selected from the group consisting of 1,1,1,3,3,3-hexachloro-2-methyldisilazane, 1,1,1,3,3,3-hexachloro-2-ethyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-propyldisilazane, 1,1,1,3,3,3-hexachloro-2-iso-propyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-butyldisilazane, 1,1,1,3,3,3-hexachloro-2-n ...butyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-butyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-butyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-butyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-propyldisilazane, 1,1,1,3,3,3-hex 3-Hexachloro-2-iso-butyldisilazane, 1,1,1,3,3-Pentachloro-2-methyldisilazane, 1,1,1,3,3-Pentachloro-2-ethyldisilazane, 1,1,1,3,3-Pentachloro-2-n-propyldisilazane, 1,1,1,3,3-Pentachloro-2-iso-propyldisilazane, 1,1,1,3,3-Pentachloro-2-methyl-3-methyldisilazane, 1,1,1,3,3-Pentachloro-2-ethyl-3-methyldisilazane, 1,1,1,3,3-Pentachloro-2-n-propyl-3-methyldisilazane, 1 , 1,1,3,3-pentachloro-2-iso-propyl-3-methyldisilazane, 1,1,1,3,3,3-hexabromo-2-methyldisilazane, 1,1,1,3,3,3-bromo-2-ethyldisilazane, 1,1,1,3,3,3-bromo-2-n-propyldisilazane, 1,1,1,3,3,3-bromo-2-n-butyldisilazane, 1,1,1,3,3,3-bromo-2-sec-butyldisilazane, 1,1,1,3,3,3-bromo-2-iso-butyldisilazane, 1,1,1,3,3,3-bromo-2-tert-butyldisilazane, 1, 1,1,3,3,3-hexaiodo-2-methyldisilazane, 1,1,1,3,3,3-iodo-2-ethyldisilazane, 1,1,1,3,3,3-iodo-2-n-propyldisilazane, 1,1,1,3,3,3-iodo-2-n-butyldisilazane, 1,1,1,3,3,3-iodo-2-iso-propyldisilazane, 1,1,1,3,3,3-iodo-2-sec-butyldisilazane, 1,1,1,3,3,3-iodo-2-tert-butyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-methyldisilazane, 1,1,3,3-Tetrachloro-1,3-dimethyl-tetrachloro-2-ethyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-n-propyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-iso-propyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-n-butyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-iso-butyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-sec-butyldisilazane, 1,1,3,3-tetrachloro-1,3 -dimethyl-2-tert-butyldisilazane, 1,1,3,3-tetrachloro-2-methyldisilazane, 1,1,3,3-tetrachloro-2-ethyldisilazane, 1,1,3,3-tetrachloro-n-propyldisilazane, 1,1,3,3-tetrachloro-2-iso-propyldisilazane, 1,1,3,3-tetrachloro-2-n-butyldisilazane, 1,3,3-tetrachloro-2-iso-butyldisilazane, 1,1,3,3-tetrachloro-2-sec-butyldisilazane, 1,1,3,3-tetrachloro-2-tert-butyldisilazane , 1,1,3,3-tetrabromo-2-methyldisilazane, 1,1,3,3-tetrabromo-2-ethyldisilazane, 1,1,3,3-tetrabromo-n-propyldisilazane, 1,1,3,3-tetrabromo-2-iso-propyldisilazane, 1,1,3,3-tetrabromo-2-n-butyldisilazane, 1,1,3,3-tetrabromo-2-iso-butyldisilazane, 1,1,3,3-tetrabromo-2-sec-butyldisilazane, 1,1,3,3-tetrachloro-2-tert-butyldisilazane, 1,1,3,3-tetraiodo-2- Methyldisilazane, 1,1,3,3-tetraiodo-2-ethyldisilazane, 1,1,3,3-tetraiodo-n-propyldisilazane, 1,1,3,3-tetraiodo-2-iso-propyldisilazane, 1,1,3,3-tetraiodo-2-n-butyldisilazane, 1,1,3,3-tetraiodo-2-iso-butyldisilazane, 1,1,3,3-tetraiodo-2-sec-butyldisilazane, 1,1,3,3-tetraiodo-2-tert-butyldisilazane, 1,1,3,3-tetrachloro-2-cyclopentyldisilazane, 1,1,3,The method according to claim 6, wherein the silazane is selected from the group consisting of 3-tetrachloro-2-cyclohexyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-cyclopentyldisilazane, and 1,1,3,3-tetrachloro-1,3-dimethyl-2-cyclohexyldisilazane.

8. 7. The method of claim 6, wherein the nitrogen-containing source is selected from the group consisting of ammonia, hydrazine, monoalkylhydrazine, dialkylhydrazine, nitrogen, nitrogen / hydrogen, ammonia plasma, nitrogen plasma, nitrogen / hydrogen plasma, and mixtures thereof.

9. 7. The method of claim 6, wherein the silicon-containing film is selected from the group consisting of silicon nitride and silicon carbonitride.

10. 1. A method for forming a silicon-containing film selected from an amorphous film and a crystalline film by a deposition process selected from plasma-enhanced atomic layer deposition and plasma-enhanced cyclic chemical vapor deposition, comprising: placing one or more substrates in a reactor and heating the reactor to one or more temperatures ranging from ambient temperature to about 1000° C.; Formula I below: 【Chemistry 4】 wherein R 1 is selected from the group consisting of methyl, ethyl, propyl, isopropyl, butyl, isobutyl, sec-butyl, tert-butyl, cyclopentyl, and cyclohexyl; R 2 introducing at least one silazane precursor, wherein X is selected from the group consisting of hydrogen, methyl, and a halide selected from the group consisting of Cl, Br, and I; and X is a halide selected from the group consisting of Cl, Br, and I, and the silazane is substantially free of organic amines, halide ions, and metal ions; purging the reactor with a purge gas; providing a plasma source into the reactor to at least partially react with the at least one silazane precursor to deposit a silicon-containing film on the one or more substrates; purging the reactor with a purge gas; A method comprising:

11. 11. The method of claim 10, wherein the plasma source is selected from the group consisting of a plasma comprising hydrogen and argon, a plasma comprising hydrogen and helium, an argon plasma, a helium plasma, and mixtures thereof.

12. The at least one silazane is selected from the group consisting of 1,1,1,3,3,3-hexachloro-2-methyldisilazane, 1,1,1,3,3,3-hexachloro-2-ethyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-propyldisilazane, 1,1,1,3,3,3-hexachloro-2-iso-propyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-butyldisilazane, 1,1,1,3,3,3-hexachloro-2-n ...butyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-butyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-butyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-butyldisilazane, 1,1,1,3,3,3-hexachloro-2-n-propyldisilazane, 1,1,1,3,3,3-hex 3-Hexachloro-2-iso-butyldisilazane, 1,1,1,3,3-Pentachloro-2-methyldisilazane, 1,1,1,3,3-Pentachloro-2-ethyldisilazane, 1,1,1,3,3-Pentachloro-2-n-propyldisilazane, 1,1,1,3,3-Pentachloro-2-iso-propyldisilazane, 1,1,1,3,3-Pentachloro-2-methyl-3-methyldisilazane, 1,1,1,3,3-Pentachloro-2-ethyl-3-methyldisilazane, 1,1,1,3,3-Pentachloro-2-n-propyl-3-methyldisilazane, 1 , 1,1,3,3-pentachloro-2-iso-propyl-3-methyldisilazane, 1,1,1,3,3,3-hexabromo-2-methyldisilazane, 1,1,1,3,3,3-bromo-2-ethyldisilazane, 1,1,1,3,3,3-bromo-2-n-propyldisilazane, 1,1,1,3,3,3-bromo-2-n-butyldisilazane, 1,1,1,3,3,3-bromo-2-sec-butyldisilazane, 1,1,1,3,3,3-bromo-2-iso-butyldisilazane, 1,1,1,3,3,3-bromo-2-tert-butyldisilazane, 1, 1,1,3,3,3-hexaiodo-2-methyldisilazane, 1,1,1,3,3,3-iodo-2-ethyldisilazane, 1,1,1,3,3,3-iodo-2-n-propyldisilazane, 1,1,1,3,3,3-iodo-2-n-butyldisilazane, 1,1,1,3,3,3-iodo-2-iso-propyldisilazane, 1,1,1,3,3,3-iodo-2-sec-butyldisilazane, 1,1,1,3,3,3-iodo-2-tert-butyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-methyldisilazane, 1,1,3,3-Tetrachloro-1,3-dimethyl-tetrachloro-2-ethyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-n-propyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-iso-propyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-n-butyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-iso-butyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-sec-butyldisilazane, 1,1,3,3-tetrachloro-1,3 -dimethyl-2-tert-butyldisilazane, 1,1,3,3-tetrachloro-2-methyldisilazane, 1,1,3,3-tetrachloro-2-ethyldisilazane, 1,1,3,3-tetrachloro-n-propyldisilazane, 1,1,3,3-tetrachloro-2-iso-propyldisilazane, 1,1,3,3-tetrachloro-2-n-butyldisilazane, 1,3,3-tetrachloro-2-iso-butyldisilazane, 1,1,3,3-tetrachloro-2-sec-butyldisilazane, 1,1,3,3-tetrachloro-2-tert-butyldisilazane , 1,1,3,3-tetrabromo-2-methyldisilazane, 1,1,3,3-tetrabromo-2-ethyldisilazane, 1,1,3,3-tetrabromo-n-propyldisilazane, 1,1,3,3-tetrabromo-2-iso-propyldisilazane, 1,1,3,3-tetrabromo-2-n-butyldisilazane, 1,1,3,3-tetrabromo-2-iso-butyldisilazane, 1,1,3,3-tetrabromo-2-sec-butyldisilazane, 1,1,3,3-tetrachloro-2-tert-butyldisilazane, 1,1,3,3-tetraiodo-2- Methyldisilazane, 1,1,3,3-tetraiodo-2-ethyldisilazane, 1,1,3,3-tetraiodo-n-propyldisilazane, 1,1,3,3-tetraiodo-2-iso-propyldisilazane, 1,1,3,3-tetraiodo-2-n-butyldisilazane, 1,1,3,3-tetraiodo-2-iso-butyldisilazane, 1,1,3,3-tetraiodo-2-sec-butyldisilazane, 1,1,3,3-tetraiodo-2-tert-butyldisilazane, 1,1,3,3-tetrachloro-2-cyclopentyldisilazane, 1,1,3,The method according to claim 10, wherein the silazane is selected from the group consisting of 3-tetrachloro-2-cyclohexyldisilazane, 1,1,3,3-tetrachloro-1,3-dimethyl-2-cyclopentyldisilazane, and 1,1,3,3-tetrachloro-1,3-dimethyl-2-cyclohexyldisilazane.

Citation Information

Patent Citations

  • Si, si'-diorganyl-n-alkyl-tetrachloro- disilazane and its production