Nanocrystal synthesis, capping and dispersion

By synthesizing colloidal semiconductor nanocrystals with controlled size and surface passivation, the challenge of non-uniform nanocrystal distribution in nanocomposites is addressed, resulting in improved optical, mechanical, and physical properties through uniform dispersion.

JP7554787B2Active Publication Date: 2024-09-20US BANK TRUST CO NAT ASSOC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2022018392
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2010-10-27
Filing Date
2022-02-09
Publication Date
2024-09-20
Estimated Expiration
2031-04-25

AI Technical Summary

Technical Problem

Existing methods for producing nanocomposites often result in non-uniform distributions of nanocrystals with significant agglomeration, leading to adverse effects on the optical, mechanical, and physical properties of the composite materials.

Method used

The synthesis of colloidal semiconductor nanocrystals with controlled size and surface passivation using capping agents, followed by dispersion in solvents and polymers to form high-quality nanocomposites with uniform distribution and minimal agglomeration.

Benefits of technology

Achieves well-dispersed nanocrystals in nanocomposites, maintaining or enhancing the optical, mechanical, and physical properties of the materials, thereby improving their performance and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554787000009
    Figure 0007554787000009
  • Figure 0007554787000010
    Figure 0007554787000010
  • Figure 0007554787000001
    Figure 0007554787000001
Patent Text Reader

Abstract

A method for preparing semiconductor nanocrystals by solvothermal synthesis and a capping method for improving the dispersibility of those nanocrystals in solvents and other media are provided. [Solution] Nanoparticle precursors are dissolved or mixed in at least one solvent and heated to a temperature in the range of 250°C to 350°C. A capping agent is added, if necessary. The resulting nanocrystals have small particle sizes (1-10 nm) with minimal agglomeration and can be synthesized in high yields. The capping agent on the as-synthesized nanocrystals and on the nanocrystals that have undergone cap exchange reactions results in the formation of stable suspensions in polar and nonpolar solvents, which can then be used to form high-quality nanocomposite films.
Need to check novelty before this filing date? Find Prior Art

Description

Detailed Description of the Invention

[0001] This application claims the benefit of U.S. Provisional Application Nos. 61 / 327,313 and 61 / 407,063, filed April 23, 2010 and October 27, 2010, respectively, the entire contents of each of which are incorporated herein by reference. [Technical field]

[0002] Described herein is the preparation of capped colloidal semiconductor nanocrystals and the dispersion of those crystals in polymer solutions and films. The colloidal semiconductor nanocrystals are highly monodisperse with nanocrystal sizes between 1-10 nm. These nanocrystals can be used to form nanocomposites containing high loading densities of uniformly dispersed capped semiconductor nanocrystals. Nanocrystal suspensions can be formed in a variety of solvents, and nanocomposites made from the suspensions can be optically transparent with little or no scattering.

[0003] STATEMENT REGARDING FEDERALLY SPONSORED RESEARCH OR DEVELOPMENT This research was supported in part by Department of Commerce Cooperative Agreements Nos. 70NANB7H7014 and 70NANB10H012 and the National Science Foundation Grant No. 0724417. [Background technology]

[0004] Nanocrystals are single crystals of a substance with at least one dimension of the crystal less than 1 micron in size. Nanocrystals may retain the optical, mechanical and physical properties of their bulk counterparts or may exhibit completely different properties. Nanocrystals can be produced by a wide range of methods, some of which include liquid synthesis, solvothermal synthesis, gas phase synthesis, aerosol synthesis, pyrolysis, flame pyrolysis, laser pyrolysis, ball milling, and laser ablation.

[0005] Nanocrystals can be dispersed in a variety of media or combinations of media, including (but not limited to) liquids, gels, glasses, polymers, and solids. Dispersed nanocrystals may impart all or some of the properties of the nanocrystals to the dispersion, or may impart properties to the dispersion that are different from those of any of the individual components. The quality of the dispersion formed between the nanocrystals and the medium may have a significant effect on the properties of the final dispersion. The quality of the dispersion of nanocrystals in the medium may be described as governed by a complex interplay between a set of parameters, including (but not limited to) the chemical properties of the nanocrystal surface (or effective nanocrystal surface), the size and shape of the nanocrystal, the physical properties of the nanocrystal, the chemical properties of the dispersing medium, and the physical properties of the dispersing medium. Well-dispersed nanocrystals may be defined as nanocrystals that are uniformly distributed throughout the medium with minimal amounts of nanocrystal agglomerates present. If the nanocrystals are not well-dispersed in the medium, the optical, mechanical, and physical properties of the nanocrystals may be altered or the properties of the medium may be adversely affected.

[0006] Nanocomposites are nanocrystal dispersions consisting of nanocrystals dispersed in a matrix, including polymers, ceramics, and glasses. Nanocomposites can be made by mixing either nanocrystals in powder form or nanocrystals already dispersed in another medium with a matrix precursor component. A non-exhaustive list of possible matrix components for use in forming nanocomposites includes monomers, oligomers, polymers, prepolymer resins, ceramics, preceramics, and glasses. Nanocomposites are an extension of the well-known range of composites, and are intended to address the needs of micron-sized particles used in composites. Nanocrystals can be considered as a replacement for micron-sized or larger fillers. In both composites and nanocomposites, the optical, mechanical and physical properties of nanocomposites may be modified using fillers, but due to the small size of the fillers used in nanocomposites, the detrimental effects of including fillers in the matrix will be relatively small or not strong. The list of possible detrimental effects that may occur in composites includes reduced structural integrity, reduced mechanical strength, reduced mechanical stability, reduced flexibility, reduced optical transparency, and reduced thermal stability. To more fully realize the potential of using nanocrystals as a replacement for micron-sized or larger fillers, the nanocrystals need to be able to disperse well in the matrix. This is due to the fact that aggregated nanocrystals in a composite will be as detrimental or even worse than aggregate-sized fillers. Thus, a composite made of strongly aggregated 5 nm particles with aggregate sizes larger than 1 micron in all dimensions will not work as a nanocomposite.

[0007] Typical procedures for producing nanocomposites often result in a distribution of nanocrystals in the medium that is not well dispersed. The distribution of nanocrystals is often non-uniform and can contain a large amount of aggregates. One key to producing well-dispersed nanocomposites is to use nanocrystals that are not aggregated before starting to mix with the matrix or medium.

[0008] There are two main types of agglomerates that are often discussed in the literature. Hard agglomerates are clusters of nanocrystals, in which the nanocrystals are relatively strongly bonded to each other. Hard agglomerates may result from particles coming into contact during or after formation, when the material is still at high temperature. The other type of agglomerates, soft agglomerates, are usually formed after synthesis or at relatively low temperatures. The general consensus is that soft agglomerates can be easily broken and separated during processing and therefore can be made well dispersed, whereas hard agglomerates cannot be broken without great difficulty and therefore are not a suitable source of well dispersed nanocrystals. To form a well dispersed dispersion of nanocrystals, it is preferable to avoid both types of agglomerations.

[0009] The aggregation of nanocrystals is controlled by the surface chemistry (or effective surface chemistry) of the nanocrystals. In dispersions, interparticle forces (e.g., electrostatic, van der Waals, and entropic forces) between the surfaces of the nanocrystals tend to form aggregates. These interparticle forces are particularly important in nanocrystals due to the large surface to volume ratio for these particles. To avoid aggregation in dispersions, it is desirable for the surfaces of the nanocrystals to be passivated (or stabilized). One method that can be used to passivate the surface of the nanocrystals involves the introduction of ligand ions or molecules. These ligands (also called capping agents or caps) are added to the surface of the nanocrystals, thereby forming a new effective surface of the nanocrystal. This effective surface is the surface of a shell created by completely (or partially) covering the surface with ligands. The chemistry of this effective surface can be changed to create a different chemical environment from the actual or initial surface of the nanocrystals, thereby avoiding or reducing aggregation and facilitating dispersion. These passivating ligands can help prevent aggregation in a variety of ways: electrostatic passivation, which uses like charges to repel the nanocrystals, and steric passivation, which uses clumping molecules to physically keep the nanocrystal surfaces apart, are two examples of surface passivation methods.

[0010] According to most typical nanocrystal synthesis methods, such as aerosol synthesis, pyrolysis, flame pyrolysis, laser pyrolysis, ball milling, and laser ablation, the nanocrystals described herein can be synthesized by the following methods: Nanocrystals are produced without any type of surface passivation. In fact, many of these methods produce nanocrystals that are tightly packed as hard aggregates. Even in cases where the synthesis does not produce aggregated nanocrystals, metal oxide nanocrystals without surface passivation tend to aggregate due to interparticle forces.

[0011] Liquid synthesis of colloidal nanocrystals of metal oxides is a method to produce nanocrystals with at least partial surface passivation during synthesis. Liquid synthesis is carried out in a solvent with or without the presence of a capping agent. The nanocrystals are at least partially protected against aggregation by the capping agent during or after synthesis. If the synthesis is carried out in a coordinating solvent, the solvent molecules or its products may act as capping agents to passivate the surface. After liquid synthesis, the nanocrystals are protected from forming aggregates by the partial or complete coverage of the nanocrystals by the solvent, products of the solvent, added capping agents, and / or combinations thereof.

[0012] After the nanocrystals are synthesized by liquid synthesis, the still-passivated surface can be modified by a process known as cap exchange or ligand exchange, in which one ligand or capping agent is at least partially replaced by another. In this process, the nanocrystals are usually dispersed in a solvent with the desired capping agent. In some cases, the temperature of the suspension is elevated to further the exchange process. The cap exchange results in either the addition of a new capping agent to a portion of the nanocrystal's surface, or the replacement of a portion of the previous surface passivating agent by a new capping agent, or some combination of these. The new capping agent may be selected to obtain chemical compatibility between the available nanocrystal surface and the solvent or other medium selected for the final dispersion or application.

[0013] As-synthesized nanocrystals produced by other methods and not surface passivated can also be exposed to a capping agent. This may result in some of the nanocrystal surface being covered by the capping agent, but the process will not disrupt and separate any previously formed aggregates (both hard and soft). These aggregates of oxide nanocrystals are different from the very weakly bound aggregates of surface passivated nanocrystals, where the passivating agent forms a porous spacer between the nanocrystals. In the weakly bound aggregates, the spacer layer between the nanocrystals provided by surface passivation is important because many of the surface-to-surface forces that cause aggregation are short-range interactions that can be reduced by increasing the separation of the nanocrystals. However, in the absence of surface passivation, once the nanocrystal surfaces are bound, such as by forming hard aggregates, short-range forces dominate and the nanocrystals are difficult to separate again.

[0014] Surface-passivated nanocrystal aggregates that can be broken down may form during various points in the preparation of the dispersion, such as when washing the particles, drying the powder, etc. One advantage of using liquid synthesis to produce colloidal nanocrystals is that surface passivation of the as-synthesized nanocrystals can be used to prevent or reduce the formation of both hard and soft aggregates at all stages of nanocrystal processing from synthesis to post-synthetic processing, ultimately resulting in the formation of high quality dispersions. Summary of the Invention

[0015] To obtain high quality nanocomposites, the size of the nanocrystalline particles is advantageously less than 10 nm in at least one dimension, and preferably has a very narrow grain size. The nanocrystals are advantageously of a size distribution and of a particular particle shape (rod, sphere, etc.). Additionally, the surface chemistry of the nanocrystals is advantageously sufficiently passivated to prevent or reduce agglomeration and to increase or improve compatibility with solvents and / or matrix materials, thus enabling or improving dispersion of the nanocrystals into nanocomposites or other nanocrystal-containing substrates.

[0016] Nanocrystals as disclosed herein are also recognized in the art to include, for example, nanoparticles, quantum dots, and colloidal particles, and may include crystalline and / or amorphous particles having sizes ranging from hundreds of nanometers to less than 1 nm. Due to their small size, nanocrystals can have dramatically different physical properties compared to bulk forms of similar materials, for example, due to quantum effects and / or large area-to-volume ratios. Nanocrystals as disclosed herein may be useful in applications ranging from metallurgy to chemical sensors, and in industries ranging from pharmaceuticals to paints and cosmetic fabrics. Microelectronic and optical applications are also contemplated.

[0017] Colloidal semiconductor nanocrystals are chemically synthesized on the nanometer scale, with ligands or capping agents on the surface of the nanocrystals that provide both dispersibility and stability in solution. In the basic chemical synthesis method, semiconductor nanocrystal precursors react or decompose in the presence of a stabilizing organic capping agent or solvent. Varying the size of the nanocrystals can be achieved by altering the reaction time or temperature profile, adjusting the order of precursor addition, or by changing the concentration of the chemical precursors, or by changing the concentration ratio of the chemical precursors, and / or by changing the capping agent.

[0018] The chemical nature of the capping agent influences and / or controls several parameters of the system in the preparation of nanocrystals and / or nanocomposites, such as the growth rate, shape and dispersibility of the nanocrystals in various solvents and solids, as well as the excited state lifetime of the charge carriers in the nanocrystals. The flexibility of the effects produced in this chemical synthesis is demonstrated by the fact that one capping agent is often selected for its growth-controlling properties, and then partially or completely replaced after the synthesis for another capping agent has been performed. This replacement may be done for various reasons, such as (but not limited to) to make the nanocrystal-medium interface more suitable for a given application or to modify the optical properties of the nanocrystal.

[0019] Described below are synthetic methods for producing colloidal semiconductor nanocrystals of zinc oxide (ZnO), yttrium oxide (Y2O3), hafnium oxide (HfO2), zirconium oxide (ZrO2), hafnium-zirconium oxide (HfO2:ZrO2), and titanium-zirconium oxide (TiO2:ZrO2), as well as capping and cap exchange of these nanocrystals, dispersion of these materials in solvents and polymers, and formation of nanocomposites.

[0020] Functionalized organosilanes are a common class of organic compounds used to present the surface of nanocrystalline oxide materials as capping agents. These organosilanes typically consist of a head moiety and a tail moiety. The head of the functionalized organosilane is typically either a trialkoxysilane or trichlorosilane group, but di- and mono-substituted alkoxysilanes and chlorosilanes are also possible. The head is anchored to the oxide surface by covalent bonding with hydroxyl (-OH) or -OR groups (R is an alkyl or aryl group) present on the surface, which eliminates alcohol, alkyl chloride, water, or HCl as by-products. The tail of the functionalized organosilane can be one or more of alkyl chains of various lengths, aryl groups, or ether groups, amines, thiols, or carboxylic acids. The above may include.

[0021] Figure 1 shows a typical addition of an organosilane to the surface of a nanocrystal via an alcohol elimination reaction, in which a nanocrystal with a polar surface containing -OH groups (101) reacts with an organosilane (102) to form an organosilane-capped nanocrystal (103).

[0022] Other classes of organic compounds used as capping agents to passivate the surfaces of oxide materials include organocarboxylic acids and organoalcohols. The head of the organocarboxylic acid is a carboxylic acid (-COOH) group, and the head of the organoalcohol is an -OH group. The head is anchored to the oxide surface by covalent bonding with hydroxyl (-OH) or -OR groups (R is alkyl or aryl) present on the surface, which allows alcohol or water to be eliminated as a by-product. The tails of the functionalized organocarboxylic acids and organoalcohols can consist of alkyl chains of various lengths, aryl groups, ether groups, amines, thiols, or carboxylic acids.

[0023] The use of capping agents such as functionalized organosilanes, alcohols or carboxylic acids on colloidal nanocrystals can impart several desirable properties, such as controlling the compatibility of the nanocrystals with various dispersing solvents, e.g., polar and non-polar media, thereby reducing the aggregation of the nanocrystals.

[0024] The disclosure further includes methods for modifying the surface of nanocrystals with organosilanes, organoalcohols, and / or organocarboxylic acids, including attaching a capping agent during nanocrystal synthesis or attaching a capping agent after synthesis by ligand exchange of at least a portion of the capping agent initially present on the nanocrystal with a second capping agent, which reactions can be carried out under ambient conditions, heating conditions, and / or elevated temperature and pressure conditions.

[0025] The disclosure further includes nanocomposites comprising a matrix and nanocrystals, where the nanocrystals are, for example, mixed, stirred, or dispersed in the matrix. Nanocomposites according to the disclosure can be prepared, for example, by melt blending, in situ polymerization, and / or solvent blending of the nanocrystals and the matrix material or precursors of the matrix. This can be done.

[0026] In melt blending, nanocrystals are mixed with a polymer in a molten state using mechanical forces. In in situ polymerization, nanocrystals are mixed with a monomer, which are then polymerized to form a composite. In solvent blending, a solvent is used to disperse both the nanocrystals and the polymer, and a uniform dispersion of the polymer and nanocrystals is achieved by removing the solvent.

[0027] The disclosure includes a preparation method for the nanocomposite material, which includes solvent mixing of a polymer or a polymer precursor with nanocrystals capped with a functionalized organosilane, organic acid or organoalcohol, and in situ polymerization of the capped nanocrystals with monomers of the polymer. [Brief description of the drawings]

[0028] [Figure 1] FIG. 1 illustrates the attachment of organosilanes to the surface of nanocrystals by elimination of alcohol. [Diagram 2] FIG. 2 illustrates in block diagram form the processing steps of the present disclosure for forming the nanocomposite materials described herein. [Diagram 3] FIG. 3 illustrates silane-capped colloidal semiconductor nanocrystals in a polymer film. [Figure 4] FIG. 4 shows a TEM image of nanocrystals synthesized from zirconium butoxide. [Diagram 5] FIG. 5 shows the XRD patterns of ZrO2 nanocrystals synthesized from zirconium propoxide by removing 1-propanol before, during and after the reaction. [Figure 6] FIG. 6 shows TEM images of ZrO2 nanocrystals synthesized from zirconium propoxide by removing 1-propanol a) before and b) after the reaction. [Figure 7] FIG. 7 shows TEM images of ZrO2 nanocrystals with various sizes. [Figure 8] Figure 8 shows the TEM image of the as-synthesized HfO2 nanocrystals with rice-like morphology. [Figure 9] Figure 9 shows a TEM image of 2-5 nm HfO2 nanocrystals. [Figure 10] FIG. 10 shows a TEM image of ZnO nanocrystals. [Figure 11] FIG. 11 shows the UV-visible spectrum of the ZnO / SOG nanocomposite spin-coated film. [Figure 12] FIG. 12 shows the TEM image of the ZnO / PMMA nanocomposite. [Figure 13] Figure 13 shows the TEM image of HfO2 / SOG nanocomposite. [Figure 14] Figure 14 shows the surface roughness of the ZrO2 film measured by AFM. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0029] The synthetic methods for preparing high quality semiconducting metal oxide nanocrystals described herein include synthetic methods in which metal oxide precursors are mixed or dissolved in at least one solvent and reacted for a period of time, in some cases the use of pressure or heat may be required.

[0030] Surprisingly, at least for the synthesis of ZrO2 and HfO2 nanocrystals, as illustrated in the Examples, adding water to the solvent results in smaller particles than reactions carried out without added water. By controlling the amount of water added to the solvent, the average particle size of the nanocrystals can be controlled.

[0031] The metal oxide precursor may be one or more of the following alkoxides: zirconium ethoxide (Zr(OCH2CH3)4), zirconium n-propoxide (Zr(OCH2CH2CH3)4), zirconium isopropoxide (Zr(OCH(CH3)2)4), zirconium n-butoxide (Zr(OCH2CH2CH2CH3)4), zirconium t-butoxide (Zr(OC(CH3)3)4), hafnium ethoxide (Hf(OCH2CH3)4), hafnium n-propoxide (Hf(OCH2CH2CH3)4), hafnium t-butoxide (Zr(OC(CH3)3)4). Hafnium isopropoxide (Hf(OCH(CH3)2)4), hafnium butoxide (Hf(OCH2CH2CH2CH3)4), hafnium t-butoxide (Hf(OC(CH3)3)4), titanium ethoxide (Ti(OCH2CH3)4), titanium n-propoxide (Ti(OCH2CH2CH3)4), titanium isopropoxide (Ti(OCH(CH3)2)4), titanium t-butoxide (Ti(OC(CH3)3)4), titanium n-butoxide (Ti(OCH2CH2CH2CH3)4), zinc ethoxide (Zn(OCH2 CH3)2), zinc n-propoxide (Zn(OCH2CH2CH3)2), zinc isopropoxide Zinc butoxide (Zn(OCH(CH3)2)2), zinc butoxide (Zn(OCH2CH2CH2 CH3)2); acetate or acetylacetonate, for example zirconium acetate Zr(OOCCH3)4, Zr(CH3COC HCOCH3)4), zinc acetate (Zn(OOCCH3)2), zinc acetylacetonate Zn(CH3COCHCOCH3)2), Hafnium acetate (Hf(OOCCH 3) 4); Halides (halides), for example, zirconium chloride (ZrCl4), di Zirconium fluoride (ZrF4), zirconium iodide (ZrI4), zirconium bromide (ZrBr4), hafnium bromide (HfBr4), hafnium chloride (HfCl4), hafnium iodide (HfI4), titanium chloride (TiCl4), titanium bromide (TiBr4), titanium iodide (TiI4), titanium fluoride (TiF4), zinc chloride (ZnCl2), zinc bromide (ZnBr2), zinc iodide (ZnI2), zinc fluoride (ZnF2), or other organometallic compounds.

[0032] Solvents useful in the present disclosure include benzyl alcohol, phenol, oleyl alcohol, toluene, butanol, propanol, isopropanol, ethanol, water, propylene glycol monomethyl ether (PGME), propylene glycol methyl ether acetate (PGMEA), ethyl lactate (EL), and 2-propoxy-propanol (PnP), acetone, tetrahydrofuran, cyclic ketones, and mixtures thereof.

[0033] Optionally, the surface of the nanocrystal of the present disclosure is capped with at least one capping agent, such as an organosilane, an organoalcohol, or an organocarboxylic acid. Examples of organosilanes of the present disclosure include n-propyltrimethoxysilane, n-propyltriethoxysilane, n-octyltrimethoxysilane, n-octyltriethoxysilane, phenyltrimethoxysilane, 2-[methoxy(polyethyleneoxy)propyl]-trimethoxysilane, methoxy(triethyleneoxy)propyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-(methacrylopropyl) ... (yloxy)propyltrimethoxysilane, 3-isocyanatopropyltriethoxysilane Examples of suitable silanes include 3-isocyanatopropyltrimethoxysilane, 3-isocyanatopropyltrimethoxysilane, and glycidoxypropyltrimethoxysilane.

[0034] Examples of organoalcohols of the present disclosure include heptanol, hexanol, octanol, benzyl alcohol, phenol, ethanol, propanol, butanol, oleyl alcohol, dodecyl alcohol, octadecanol, and triethylene glycol monomethyl ether.

[0035] Examples of organocarboxylic acids of the present disclosure include octanoic acid, acetic acid, propionic acid, 2-[ 2-(2-methoxyethoxy)ethoxy]acetic acid, oleic acid, and benzoic acid. The capped colloidal semiconductor nanocrystals of the present disclosure are optionally removed from and redispersed in a solvent such as water, tetrahydrofuran, ethanol, methanol, acetonitrile, PGMEA, PGPE, PGME, cyclic ketones, ethyl lactate, acetone, naphtha, hexane, heptane, toluene, or mixtures thereof.

[0036] Semiconductor nanocrystals can be incorporated into a matrix to form a nanocomposite. Matrix materials of the present disclosure include poly(acrylonitrile-butadiene-styrene) (ABS), poly(methyl methacrylate) (PMMA), celluloid, cellulose acetate, poly(ethylene-vinyl acetate) (EVA), poly(ethylene-vinyl alcohol) (EVOH), fluoroplastics, polyacrylates, polyacrylonitrile, polyvinyl alcohol ... Polyamide (PAN), Polyamide (PA or Nylon), Polyamide-imide (PAI), Polyaryletherketone (PAEK), polybutadiene (PBD), polybutylene (PB), polybutylene terephthalate (PBT), polycaprolactone (PCL), polychlorotrifluoroethylene (PCTFE), polyethylene terephthalate (PET), polycyclohexylene dimethylene terephthalate (PCT), polycarbonate (PC), polyhydroxyalkanoates (PHAs), polyketone (PK), polyester, poly Polyethylene (PE), polyether ether ketone (PEEK), polyether ketone ketone (PEKK), polyetherimide (PEI), polyether sulfone (PES), polyethylene chlorinate (PEC), polyimide (PI), polylactic acid (PLA), polymethylpentene (PMP), polyphenylene oxide (PPO), polyphenylene sulfide (PPS), polyphthalamide (PPA), polypropylene (PP), polystyrene (PS), polysulfone (PSU), polytrimethylene terephthalate (PTT), polyurethane (PU), polyvinyl acetate (PVA), polyvinyl chloride Examples of suitable solvents include polyvinyl chloride (PVC), polyvinylidene chloride (PVDC), poly(styrene-acrylonitrile) (SAN), spin-on-glass (SOG) polymers (e.g., siloxane spin-on polymers in ethanol), propylene glycol methyl ether acetate (PGMEA), isopropyl alcohol, or mixtures of these solvents, JSR Micro Topcoat (NFCTCX014 in 4-methyl-2-pentanol), JSR Micro Photoresist (ARF1682J-19), and silicones (e.g., polydimethylsiloxane (PDMS) and polymethylphenylsiloxane).

[0037] Examples of nanocrystals include (but are not limited to) CuCl, CuBr, CuI, AgCl, AgBr, AgI, Ag2S, Ag2Te, Al2O3, Ga2O3, In2O3, FeO, Fe2O3, Fe3O4, TiO2, MgO, Eu2O3, CrO2, CaO, MgO, ZnO, Mg x Zinc 1-x O, SiO2, Cu2O, Zr2O3, ZrO2, SnO2, ZnS, HgS, Fe2S, Cu2S, CuIn2S2, MoS2, In2S3, Bi2S3, GaP, GaAs, GaSb, InP, InAs, In x Ga 1-x As, SiC, Si 1-x Ge x, CaF2, YF3, YSi2, GaInP2, Cd3P2, CuIn2Se2, In2Se3, HgI2, PbI2, ZnSe, CdS, CdSe, CdTe, HgTe, CdHgTe, PbS, BN, AlN, GaN, InN, Al x Ga 1-x N, Si3N4, ZrN, Y2O3, HfO2, Sc2O3, and mixtures or alloys thereof, where x can be a value between 0.01 and 0.99.

[0038] The present disclosure provides a method of producing nanocrystals, the method comprising dissolving precursors of the nanocrystals in at least one solvent, thereby forming a solution, and optionally at least one of heating and increasing the pressure of the solution, and reacting the precursors or reacting the precursors with at least one solvent of the solution, thereby forming nanocrystals.

[0039] The nanocrystals may be capped with at least one agent, thereby increasing the solubility or dispersibility of the nanocrystals in at least one solvent or other medium, or any combination of solvents and other media.

[0040] In the methods of the present disclosure, the nanocrystals may be capped with at least one agent, which may include at least one organosilane, organoalcohol, or organocarboxylic acid, which will result in uniform dispersion of the nanocrystals in various media, such as hydrophobic or hydrophilic media, by generating an effective nanocrystal surface formed by a full or partial shell of capping agents whose tail groups have a polarity compatible with the medium.

[0041] The capping method of the present disclosure may include capping the nanocrystals with at least one capping agent in solution before, during, or after said reaction of the precursors is carried out. The method of the present disclosure may further include purifying and / or isolating the nanocrystals before or after carrying out the capping method of the present disclosure.

[0042] The disclosed method includes capping as-synthesized nanocrystals, purified nanocrystals, and / or isolated nanocrystals with at least one capping agent, thereby producing at least partially capped nanocrystals. The at least partially purified capped nanocrystals may be further purified and / or isolated according to the disclosed method. The nanocrystals and capped nanocrystals may be dispersed in a substance, including a solvent, a polymer, or any combination thereof, in the disclosed method. FIG. 2 is a block diagram illustrating the formation of a colloidal suspension. In this illustrated method, nanocrystals are synthesized (101), capped or cap-exchanged with at least one capping agent (102), purified (103), and mixed with a solvent or polymer solution (104).

[0043] The present disclosure further includes methods for fully or partially replacing organic moieties or other capping agents already present on the surface of nanocrystals, resulting from capping reactions carried out prior to the synthesis or otherwise of the nanocrystals, with functionalized organosilanes, organoalcohols and organocarboxylic acids in a capping reaction.

[0044] The functionalized capping agent is covalently attached to the colloidal semiconductor nanocrystals according to aspects of the present disclosure during synthesis of the colloidal semiconductor nanocrystals. In some cases, the functionalized capping agent is covalently attached to the semiconductor in this disclosure by removing pre-existing organic components from the surface of the semiconductor nanocrystal with an acid, and then covalently attaching the functionalized capping agent to the surface of the semiconductor nanocrystal. Examples of acids for removing pre-existing organic components include, for example, strong acids (e.g., HCl, HNO3, and / or H2SO4), weak acids (e.g., H3PO4), and / or organic acids (e.g., acetic acid).

[0045] Alternatively, the nanocrystals are functionalized with a capping agent without forming a covalent bond. The present disclosure includes nanocrystals and at least partially capped nanocrystals produced by the methods described herein.

[0046] The methods of the present disclosure further include methods of forming a film or coating comprising dispersing the nanocrystals or at least partially capped nanocrystals of the present disclosure in another substance to form a dispersion and applying the dispersion to a surface by methods of application including spin coating, spraying, dipping, screen printing, rolling, painting, printing, inkjet printing, evaporative deposition, and / or vapor deposition.

[0047] The methods of the present disclosure include forming a nanocomposite, which includes combining the nanocrystals or at least partially capped nanocrystals of the present disclosure with another material, thereby forming the nanocomposite. Figure 3 is a depiction illustrating nanocrystals (102) capped with a capping agent (101) and dispersed in a polymer matrix (103).

[0048] The methods of the present disclosure include forming a nanocomposite, which may be accomplished, for example, by curing, polymerizing, laminating, extruding, injection molding, casting, spin coating, dip coating, brushing, spraying, and / or printing.

[0049] The present disclosure further includes methods for forming a homogenous mixture of nanocomposite components using a variety of different methods, which components are then assembled into a final composite suitable for a desired application.

[0050] The nanocrystals or at least partially capped nanocrystals of the present disclosure may be zinc oxide, hafnium oxide, zirconium oxide, titanium zirconium oxide, hafnium dioxide, It may be formed from zinc oxide, yttrium oxide, or other semiconductor materials. EXAMPLES

[0051] The products and methods of the present disclosure are illustrated by the following non-limiting examples. Example 1 Nanocrystal synthesis and capping Zirconium oxide (ZrO 2 ) Nanocrystal Synthesis Zirconium oxide nanocrystals with sizes in the range of 1-10 nm can be prepared from precursors such as zirconium(IV) n-butoxide, zirconium n-propoxide, zirconium isopropoxide or zirconium ethoxide. Depending on the desired end product, zirconium n-butoxide or zirconium n-propoxide may be advantageously used as precursors.

[0052] In a typical process, a zirconium alkoxide precursor, such as (but not limited to) zirconium n-butoxide, zirconium n-propoxide, zirconium isopropoxide isopropanol, or zirconium ethoxide, is mixed with a solvent or mixture of solvents including benzyl alcohol, phenol, oleyl alcohol, butanol, propanol, isopropanol, water, tetrahydrofuran, ethanol, methanol, acetonitrile, toluene, PGMEA, PGPE, PGME, 2-methyl-1-propanol, or triethylene glycol monomethyl ether, and sealed in an autoclave. The reaction mixture is heated to a temperature between 250-350°C. Once the reaction mixture reaches the set temperature, it is maintained at that temperature for a period of time ranging from 20 minutes to 24 hours, depending in part on the solvent or mixture of solvents and / or the temperature of the reaction. The as-synthesized zirconium oxide nanocrystals are collected as a milky white suspension.

[0053] In a further example, zirconium oxide nanocrystals were prepared from a mixture of 30 mmol of zirconium isopropoxide isopropanol or zirconium ethoxide with 300 mL of benzyl alcohol in an inert atmosphere sealed inside an autoclave. The reaction mixture was heated to 350°C at a heating rate of 10°C / min. When the reaction mixture reached 350°C, the temperature was maintained for 20-60 minutes. After the autoclave was cooled to room temperature, a milky solution of as-synthesized ZrO2 nanocrystals was collected.

[0054] In a further example, 45 mmol of zirconium isopropoxide isopropanol or zirconium ethoxide was mixed with 300 mL of benzyl alcohol and transferred to an autoclave to prepare zirconium oxide nanocrystals in an inert atmosphere. The reaction mixture was heated to 300-350°C at a heating rate of 10°C / min for 1-2 hours. The pressure of the reaction reaches 100-500 psi. After the reaction was completed and the reactor was cooled to room temperature, a milky solution of as-synthesized zirconium oxide nanocrystals was collected.

[0055] A typical synthesis procedure using zirconium n-butoxide as a precursor is as follows: 21.58 g of 80% (w / w) zirconium(IV) n-butoxide in 1-butanol solution. The zirconium(IV) n-butoxide (containing 17.26 g or 45 mmol of zirconium(IV) n-butoxide) was mixed with 300 ml of benzyl alcohol in a glove box and then transferred into a glass-lined autoclave. The set-up was sealed under an argon atmosphere to prevent contamination by oxygen and moisture. The autoclave was then heated to 325°C and held at this temperature for 1 hour and then cooled to room temperature. A milky solution of as-synthesized zirconium oxide nanocrystals was recovered.

[0056] Zirconium n-butoxide was prepared as a solution in 1-butanol (80% w / w). 1-Butanol can be synthesized under vacuum and / or under heat (at 30-50 °C). It can be removed from the precursor before synthesis, during synthesis by releasing the autoclave pressure when the temperature reaches about 100°C, or after the reaction is complete. Figure 4 shows a TEM image of nanocrystals obtained from a reaction carried out without removal of 1-butanol. The nanocrystals are spherical and about 5 nm in diameter.

[0057] A typical synthesis method using zirconium n-propoxide as a precursor is as follows: 21.06 g of 70% (w / w) zirconium(IV) n-propoxide in 1-propanol solution. 14.74 g or 45 mmol of zirconium(IV) n-propoxide was mixed with 300 ml of benzyl alcohol in a glove box and then transferred into an autoclave. The set-up was sealed under an argon atmosphere to prevent contamination by oxygen and moisture. The autoclave was then heated to 325° C. and held at this temperature for 1 hour and then cooled to room temperature. A milky solution of as-synthesized zirconium oxide nanocrystals was recovered.

[0058] Zirconium n-propoxide was used as a solution in 1-propanol (70% w / w). It should be noted that 1-propanol can be removed from the precursors prior to synthesis under vacuum and / or with heating (at 30-60 °C). It can be removed during synthesis by releasing the autoclave pressure when the temperature reaches about 100 °C, or it can be removed after synthesis. Nanocrystals obtained from reactions in which 1-propanol is removed from the precursors before, during, or after the reaction resulted in ZrO2 nanocrystals of about 5 nm. These nanocrystals have the same crystal structure as shown by the XRD patterns of the respective nanocrystals shown in Figure 5. Based on a comparison of the TEM images shown in Figure 6a for nanocrystals obtained with removal before the reaction and Figure 6b for those without removal of 1-propanol, the nanocrystals obtained by removing 1-propanol before or during the reaction are more spherical and more monodisperse.

[0059] To increase the yield of the reaction without affecting the quality of the nanocrystals, the concentration of precursors such as zirconium isopropoxide isopropanol, zirconium ethoxide, zirconium n-propoxide or zirconium n-butoxide can be increased by 5-20 times without changing the amount of solvent used.

[0060] ZrO2 nanocrystals can be synthesized in a variety of solvents and solvent mixtures. By varying the solvent used in the synthesis method, the surface properties of the nanocrystals can be changed and in some cases the nanocrystals can be capped well enough that further surface modification is not necessary to obtain a dispersion with minimal scattering. Alternative solvents include (but are not limited to) 1-hexanol, oleyl alcohol, oleylamine, trioctylamine, and methyltriethylene glycol. Alternative solvent mixtures include (but are not limited to) benzyl alcohol with 1-hexanol, oleyl alcohol, triethylene glycol monomethyl ether, and trioctylamine.

[0061] ZrO2 may be synthesized in a variety of ways to prepare nanocrystals with hydrophobic surface chemistry. This may be useful for applications that benefit from the use of a hydrophobic solvent to generate a nanocrystal dispersion. An example of a synthesis method for producing ZrO2 nanocrystals with a hydrophobic surface is as follows: The solvent for synthesizing ZrO2 nanocrystals contains a mixture of oleyl alcohol and benzyl alcohol in various volume ratios. The volume ratio of oleyl alcohol to benzyl alcohol for carrying out the reaction can be selected from the following non-limiting example ratios: 1:3, 1:1, or pure oleyl alcohol. In a typical reaction, 3 mmol of zirconium isopropoxy is added to 100 mL of ... Cidoisopropanol is added to a 20 ml mixture containing 10 ml of anhydrous benzyl alcohol and 10 ml of oleyl alcohol in an inert atmosphere. The mixture is stirred for about 1 hour. The reaction mixture is then added to an autoclave reactor under an inert atmosphere. The reactor is then heated to 325°C and maintained at 325°C for 1 hour with stirring. After cooling, the nanocrystals are precipitated from the solution using ethanol.

[0062] The exemplary synthesis method described herein is carried out in an autoclave at a temperature that may be higher than the boiling point of some of the solvents used. This can be done at pressures ranging from 100 to 900 psi, typically at about 250 psi. To eliminate the high pressures that would normally be present in the synthesis of ZrO2 nanocrystals, a solvent or mixture of solvents with a higher boiling point may be used. One non-limiting example of a solvent with a high boiling point is Dowtherm MX (Dow Chemicals), a mixture of alkylated aromatic compounds. Dowtherm MX can be used alone or in combination with other solvents such as benzyl alcohol. When used alone for the synthesis of ZrO2 nanocrystals, the pressure in the autoclave reactor is less than 100 psi, and typically less than 20 psi.

[0063] A typical example of the synthesis of ZrO2 nanocrystals carried out in a mixture of benzyl alcohol and Dowtherm MX is as follows: 100 ml of Dowtherm MX, 8.13 mmol of zirconium isopropoxide isopropanol and 30 ml of anhydrous benzyl alcohol are mixed in a 250 ml flask in a glove box for 30 minutes with a magnetic stirrer at 500 rpm. The mixture is then loaded into a 600 ml glass-lined Parr autoclave reactor. The reactor is then sealed in the glove box. The reaction mixture is heated to 325 °C with stirring at a heating rate of 10 °C / min and maintained at this temperature for 1 hour with stirring. After cooling to room temperature, a milky suspension of ZrO2 nanocrystals is obtained.

[0064] A typical example of the procedure for the synthesis of ZrO2 nanocrystals using only Dowtherm MX as solvent is as follows: 100 ml of Dowtherm MX and 3.15 g of zirconium isopropoxide isopropanol are mixed in a 250 ml flask in a glove box for 30 minutes with a magnetic stirrer at 500 rpm. The mixture is then loaded into a 600 ml glass-lined Parr reactor. The reactor is then sealed in the glove box before proceeding to the reaction. The reaction mixture is heated to 325°C with a heating rate of 10°C / min while stirring and maintained at this temperature for 1 hour while stirring. After cooling to room temperature, a milky suspension of ZrO2 nanocrystals is obtained.

[0065] Alternatively, precursors other than zirconium(IV) isopropoxide isopropanol may be used to synthesize ZrO2 nanocrystals in solvents with boiling points higher than the reaction temperature or in mixtures of these solvents with benzyl alcohol. These alternative precursors include (but are not limited to) zirconium(IV) ethoxide, zirconium(IV) n-propoxide, and zirconium(IV) n-butoxide.

[0066] 1-5nm ZrO 2 Synthesis of nanocrystals By controlling the amount of water in the reaction mixture during the solvothermal synthesis, ZrO2 nanocrystals with average diameters of 1-5 nm, preferably 1-3 nm, can be synthesized. These small size nanocrystals (1-5 nm) may be desirable for increased specific surface area over larger nanocrystals (6-10 nm) or for applications where smaller physical dimensions are beneficial. A typical example of the experimental procedure for synthesizing these nanocrystals is as follows: In a vial, 30 ml of benzyl alcohol and 0.5 ml of ethanol are added. 0.08 mL of water (4.44 mmol) was stirred for 1 hour and transferred into the glove box. In the glove box, 4.49 mmol of zirconium(IV) isopropoxide isopropanol (Zr(OPr i)4(HOPr i ))-, (~1:1 water to precursor ratio) was stirred with benzyl alcohol solution for 4 hours. The precursor was completely dissolved in the solvent and a clear solution was obtained. The reaction mixture was then transferred to an autoclave and sealed in the vessel. The reaction mixture was then heated to 325 °C for 1 hour with stirring (250 °C in 15 min, 265 °C in 3 min, 280 °C in 3 min, 295 °C in 3 min, 310 °C in 3 min, 325 °C in 3 min). After cooling to room temperature, a white slurry and a faint yellow solution were obtained. The XRD pattern of the solid matched that of ZrO2 and TEM images of the nanocrystals showed that the size of the particles was about 3 nm. Figure 7a, b, c and d show the TEM images of the nanocrystals obtained from precursor to water molar ratios of 1:1, 1:2, 1:3 and 1:4, respectively, in the reaction mixture. FIG. 7 shows that the particle size becomes smaller as the water-to-precursor ratio increases, with a water-to-precursor ratio of 1:4 yielding the smallest average particle size (~2 nm) among typical ratios of 1:1, 1:2, 1:3, and 1:4.

[0067] Alternatively, precursors other than zirconium(IV) isopropoxide isopropanol can be used to synthesize ZrO2 nanocrystals with average diameters of 1-5 nm, preferably 1-3 nm. These alternative precursors may include zirconium(IV) ethoxide, zirconium(IV) n-propoxide, and zirconium(IV) n-butoxide.

[0068] The heating temperature and time of the exemplary synthesis method described here for synthesizing ZrO2 nanocrystals can be adjusted to vary the reaction temperature from 250-350°C and the reaction time from 20 minutes to 24 hours. Reactions conducted at the lower end of the temperature range will require longer heating times to complete the synthesis, and reactions conducted at the higher end of the temperature range will require shorter times.

[0069] Titanium zirconium oxide (TiO 2 -ZrO 2 ) Nanocrystal Synthesis By modifying the synthetic method to obtain ZrO2 nanocrystals, metal oxide nanocrystals containing both zirconium and titanium atoms can be synthesized. These TiO2-ZrO2 metal oxide nanocrystals have the same chemical and physical properties as ZrO2 and TiO2. These can be used in a variety of applications requiring a combination of crystalline, crystalline, or optical properties (or some combination of these). involves replacing the zirconium precursor with a mixture containing both titanium and zirconium precursors in benzyl alcohol. Nanocrystals with various Ti / Zr atomic ratios can be produced by adjusting the concentrations of the titanium and zirconium precursors relative to one another while keeping the overall concentration of the metal precursors constant. In this manner, TiO2-ZrO2 nanocrystals can be synthesized with Ti:Zr ratios of 1:3, 1:2, and 1:1, which are non-limiting examples.

[0070] A typical method for synthesizing TiO2-ZrO2 nanocrystals with a Ti:Zr ratio of 1:1 was used. The procedure is as follows: 15 mmol of zirconium isopropoxide isopropanol and 15 mmol of titanium isopropoxide were dissolved in 30 ml of anhydrous benzyl alcohol under inert atmosphere. The reaction mixture was then charged into an autoclave reactor under inert atmosphere. The reactor was heated to 300°C and maintained at 300°C for 1 hour with stirring. The resulting nanocrystals were precipitated from the solution with ethanol. TEM images showed that the TiO2-ZrO2 nanocrystals had a size of about 5 nm. Elementary analysis confirmed that the Ti / Zr atomic ratio in the sample was roughly consistent with that of the two precursors.

[0071] A typical method for synthesizing TiO2-ZrO2 nanocrystals with a Ti:Zr ratio of 1:2 was used. The procedure is as follows: 20 mmol of zirconium isopropoxide isopropanol and 10 mmol of titanium isopropoxide were dissolved in 30 ml of anhydrous benzyl alcohol under inert atmosphere. The reaction mixture was then charged into an autoclave reactor under inert atmosphere. The reactor was heated to 300°C and maintained at 300°C for 1 hour with stirring. The resulting nanocrystals were precipitated from the solution with ethanol.

[0072] Alternatively, a mixture of titanium and zirconium, other than a mixture of zirconium isopropoxide and titanium isopropoxide, may be used to synthesize TiO2-ZrO2 nanocrystals with various values ​​of x. The mixture of materials may include: zirconium ethoxide, zirconium n-propoxide, and zirconium n-butoxide as non-limiting examples of zirconium precursors, and titanium ethoxide, titanium n-propoxide, and titanium n-butoxide as titanium precursors.

[0073] Hafnium zirconium oxide (HfO 2 -ZrO 2 ) Nanocrystal Synthesis Metal oxide nanocrystals containing both zirconium and hafnium atoms in a single nanocrystal can be synthesized. HfO2-ZrO2 with a hafnium to zirconium atomic ratio of 1:1 can be synthesized by mixing 2 mmol of hafnium isopropoxide in isopropanol and 2 mmol of zirconium chloride with 10 grams of trioctylphosphine oxide. O2 oxide nanocrystals can be produced in an inert atmosphere. The reaction mixture is then heated to 100°C at a heating rate of 10°C / min under inert atmosphere with vigorous stirring. After stirring at 100°C for 1 hour, the trioctylphosphine oxide melts, and the hafnium and zirconium precursors dissolve in the molten trioctylphosphine oxide. The solution is then rapidly heated to 350°C at a heating rate of 10°C / min and maintained at 350°C for 2 hours. A white powder forms, and the solution becomes milky white. After 2 hours, the reaction mixture is allowed to cool. When the reaction mixture reaches 70°C, acetone is added to precipitate the nanocrystals. The resulting hafnium and zirconium oxide nanomaterials are rod-like in shape (i.e., "nanorods").

[0074] In a further embodiment, hafnium zirconium oxide nanocrystals can be prepared with a range of values ​​for the hafnium to zirconium atomic ratio. For example, nanocrystals with a 1:4 Hf:Zr ratio can be prepared as follows: 0.8 mmol of hafnium isopropoxide isopropanol, 1.2 mmol of zirconium isopropoxide isopropanol, 2 mmol of zirconium chloride, and 10 grams of trioctylphosphine oxide are mixed in an inert atmosphere. The order of feeding is arbitrary. The reaction mixture is heated to 100°C at a heating rate of 10°C / min under inert atmosphere with vigorous stirring. The solution is then rapidly heated to 350°C at a heating rate of 10°C / min and maintained at 350°C for 2 hours. A white powder is formed and the solution becomes milky white. After 2 hours, the reaction mixture is allowed to cool. When the reaction mixture reaches 70°C, acetone is added to precipitate the HfO2-ZrO2 nanocrystals. The precipitate is separated by centrifugation. The hafnium zirconium oxide nanomaterials range in shape from spheres to rods (i.e., "nanorods").

[0075] Hafnium oxide (HfO 2 ) Nanocrystal Synthesis Hafnium oxide nanocrystals having sizes ranging from 1 to 10 nm have been synthesized in an inert atmosphere using a solvothermal synthesis method, for example: hafnium alkoxide precursors (such as, but not limited to, hafnium isopropionate, hafnium alkoxide precursors ... A sample of hafnium oxide (isopropanol or hafnium ethoxide) was mixed with an organic alcohol (e.g., but not limited to, benzyl alcohol or 2-methyl-1-propanol) and sealed in an autoclave. The reaction mixture was heated to 250-350°C. After the reaction mixture reached the set temperature, the temperature was maintained for a set time, which can range from 20 minutes to 24 hours. The as-synthesized hafnium oxide nanocrystals were obtained as a milky suspension. Figure 8 shows a TEM image of the synthesized HfO2 nanocrystals, which have a rice-like shape and are less than 10 nm in size.

[0076] In the disclosed method for producing 6 g of hafnium oxide nanocrystals, a 30 mmol sample of hafnium ethoxide or hafnium isopropoxide isopropanol is mixed with 300 milliliters of benzyl alcohol in an inert atmosphere and then transferred to an autoclave. The reaction mixture is heated to 300-350°C at a heating rate of 10°C / min for 1-2 hours. The pressure in the autoclave is kept below 500 psi (~35 atm) during the reaction. After the reaction time has elapsed and the reactor is allowed to return to room temperature, a milky solution of as-synthesized hafnium oxide nanocrystals is obtained.

[0077] Alternatively, precursors other than hafnium(IV) isopropoxide, isopropanol, or hafnium ethoxide may be used to synthesize HfO2 nanocrystals in solvents with boiling points higher than the reaction temperature, or in mixtures of these solvents with benzyl alcohol. These alternative precursors include (but are not limited to) hafnium(IV) n-propoxide, and hafnium(IV) n-butoxide.

[0078] 1-5 nm HfO 2 Synthesis of nanocrystals By controlling the amount of water in the reaction mixture during the solvothermal synthesis, HfO2 nanocrystals with diameters between 1-5 nm, preferably 1-3 nm, can be synthesized. These small size nanocrystals may be desirable for increased specific surface area over larger nanocrystals, or for applications where smaller physical dimensions are beneficial. A typical example of an experimental procedure for adding water to produce hafnium oxide nanocrystals in the 1-5 nm size range is as follows: 30 ml of benzyl alcohol and 0.1 ml of water are stirred in a vial for 3 hours, then transferred into a dry box. In the dry box, 4.45 mmol of Hf(OPr i )4(HOPr i ) (2.113 g) is stirred overnight in a solution of water and benzyl alcohol with a 1:1 molar ratio of water to hafnium isopropoxide. The precursor dissolves completely in the solvent mixture. The reaction mixture is transferred to an autoclave and sealed in the vessel. The reaction mixture is then heated to 325 °C using a heating mantle while stirring for 1 h. After cooling to room temperature, a white slurry and a faintly yellow solution is obtained. Figure 9 shows a TEM image of nanocrystals with sizes of 2-5 nm.

[0079] Alternatively, HfO2 nanocrystals with diameters of 1-5 nm, preferably 1-3 nm, can be synthesized starting from precursors other than hafnium isopropoxide isopropanol. These alternative precursors would include (but are not limited to) hafnium ethoxide, hafnium n-propoxide, and hafnium n-butoxide.

[0080] The ratio of hafnium alkoxide to water can range from 1:1 to 1:4. The heating temperature and time of the exemplary synthesis method described herein for synthesizing HfO2 nanocrystals can be adjusted to vary the reaction temperature from 250 to 350 °C and the reaction time from 20 minutes to 24 hours. Reactions conducted at the lower end of the temperature range require longer heating times, and reactions conducted at the higher end of the temperature range require shorter heating times. It will take a short time.

[0081] Synthesis of zinc oxide (ZnO) nanocrystals Organosilane-capped zinc oxide nanocrystals were prepared as follows: 2.7 grams of zinc acetate dihydrate was dissolved in 140 milliliters of ethanol and heated to 80°C with stirring. After the zinc acetate was completely dissolved and the solution became clear, the reaction mixture was cooled in an ice-water bath. In a separate flask, a 0.72 gram sample of lithium hydroxide monohydrate was mixed with 60 milliliters of ethanol and sonicated for 30 minutes. The lithium hydroxide and ethanol solution was added dropwise to the zinc acetate dihydrate and ethanol solution in the ice-water bath at a rate of 3 drops per second. After the entire lithium hydroxide and ethanol solution was added, the reaction mixture was allowed to warm to room temperature and stirred for 1 hour. A 0.25 gram sample of methoxy(triethyleneoxypropyl)trimethoxysilane was mixed with 5 milliliters of ethanol and then injected into the reaction mixture. The entire reaction mixture was stirred at room temperature for 12 hours, which resulted in the synthesis of organosilane-capped zinc oxide nanocrystals. These nanocrystals were spherical and had diameters in the range of 3-6 nm.

[0082] In a further example, large size (5 nm or more but less than 10 nm) organosilane-capped zinc oxide nanocrystals were prepared as follows: 2.7 grams of zinc acetate dihydrate was dissolved in 140 ml of ethanol and heated to 80° C. with stirring. After the zinc acetate was completely dissolved and the solution was clear, the reaction mixture was cooled in an ice-water bath. In a separate flask, a 0.72 gram sample of lithium hydroxide monohydrate was mixed with 60 milliliters of ethanol and sonicated for 30 minutes. This solution was added dropwise at a rate of 3 drops per second to the zinc acetate dihydrate and ethanol solution in the ice-water bath. After all of the lithium hydroxide and ethanol solution was added, the reaction mixture was placed in a 60° C. water bath and stirred for 1 hour. A 0.25 gram sample of methoxytri(ethyleneoxy)propyltrimethoxysilane was mixed with 5 milliliters of ethanol and then injected into the reaction mixture. The entire reaction mixture was stirred at 60° C. for 12 hours, which resulted in the synthesis of organosilane-capped zinc oxide nanocrystals with diameters of 5 nm or more and less than 10 nm.

[0083] A method for producing organosilane-capped zinc oxide nanocrystals is provided. A 21.28 gram sample of zinc acetate dihydrate is dissolved in 1080 ml of ethanol and heated to 80° C. with stirring. After the zinc acetate is completely dissolved and the solution is clear, the reaction mixture is cooled in an ice-water bath. In a separate flask, a 5.76 gram sample of lithium hydroxide monohydrate is mixed with 480 ml of ethanol and sonicated for 30 minutes. This solution is added dropwise to the zinc acetate dihydrate and ethanol solution in the ice-water bath. After the entire lithium hydroxide and ethanol solution is added, the reaction mixture is allowed to warm to room temperature and stirred for 0.5 hours. A 2.0 gram sample of methoxytri(ethyleneoxy)propyltrimethoxysilane is mixed with 15 milliliters of ethanol and then injected into the reaction mixture. The entire reaction mixture is stirred at room temperature for 16 hours, which results in the synthesis of organosilane-capped zinc oxide nanocrystals. These nanocrystals are spherical and have diameters between 3 and 6 nm.

[0084] Alternatively, methoxytri(ethyleneoxy)propyltrimethoxysilane, four times more concentrated with respect to ethanol, was added to the reaction mixture during the synthesis of 3–6 nm and 5–10 nm ZnO nanocrystals, which increased the degree of capping and dispersibility of the nanocrystals in polar solvents.

[0085] ZnO nanocrystals can be synthesized by different liquid synthesis methods. A typical synthesis is as follows: As follows: 50 mmol of zinc acetate dihydrate was added to 500 ml of absolute ethanol in a flask. The zinc acetate was completely dissolved by heating the flask to 80° C. in a water bath. Separately, 200 mmol of lithium hydroxide monohydrate was dissolved in 125 ml of methanol (or ethanol) by vigorous stirring at room temperature. The LiOH solution was then poured into the refluxing Zn(Ac)2 solution. After the addition, the heat was turned off and the reaction mixture was cooled in air for 20 min. A clear solution resulted. The solution was then reheated to 80° C. for 30 min, which resulted in the formation of a white precipitate. The precipitate was separated from the solution by centrifuging at 4500 rpm at 4° C. for 20 min and washed with THF. A TEM image of the product is shown in FIG. 10.

[0086] Alternatively, in the above reaction used to produce ZnO nanocrystals, the molar ratio of lithium hydroxide to zinc salt can be varied from 1:1.4 to 1:4. Alternatively, KOH or NaOH can be used as a substitute for lithium hydroxide in the above reaction used to produce ZnO nanocrystals.

[0087] Yttrium oxide (Y 2 O 3 ) Nanocrystal Synthesis Yttrium oxide nanocrystals were prepared from 1 gram of yttrium oleate and 5.96 grams of dodecylamine. These were mixed and purged with inert gas for 10 minutes. The reaction mixture was then heated to 70°C in 20 minutes with stirring under an inert atmosphere, maintained at 70°C for 20 minutes, then heated to 259°C in an additional 20 minutes, and maintained at 259°C for 2 hours. The reaction mixture was then cooled. At 70°C, 20 ml of ethanol was added to the reaction mixture, which precipitated the yttrium oxide nanocrystals.

[0088] In another example, yttrium oxide nanodisks (disk-shaped nanocrystals) with a diameter of 20 nanometers were produced from a mixture of 1 gram of yttrium oleate and 5 ml of oleylamine. These were mixed and purged with an inert gas such as argon for 10 minutes. The reaction mixture was then heated to 70° C. in 20 minutes while stirring under an inert gas atmosphere, maintained at 70° C. for 20 minutes, heated to 250° C. in 20 minutes, and finally maintained at 250° C. for 2 hours. The reaction mixture was then cooled. At 70° C., 20 milliliters of ethanol was added to the reaction mixture, which precipitated the yttrium oxide nanodisks.

[0089] In another example, yttrium oxide nanodisks with a diameter of 10 nanometers were prepared from 2 grams of yttrium oleate and 25 ml of oleylamine. They were mixed and purged with argon for 10 minutes. The reaction mixture was then heated to 70°C in 20 minutes with stirring under the protection of argon, maintained at 70°C for 20 minutes, heated to 280°C in 20 minutes, and finally maintained at 280°C for 2 hours. The reaction mixture was then cooled. At 70°C, 20 milliliters of ethanol was added to the reaction mixture, which precipitated the yttrium oxide nanodisks.

[0090] In a further example, yttrium oxide nanodisks with a diameter of 10 nanometers were prepared from 2 grams of yttrium oleate and 25 ml of oleylamine. These were mixed and purged with argon for 10 minutes. The reaction mixture was then heated to 70°C in 20 minutes with stirring under the protection of argon, maintained at 70°C for 20 minutes, heated to 230°C in 20 minutes, and finally maintained at 230°C for 2 hours. The reaction mixture was then cooled. At 70°C, 20 milliliters of ethanol was added to the reaction mixture, which precipitated the yttrium oxide nanodisks.

[0091] In a further example, yttrium oxide nanocrystals were prepared by mixing 2.15 grams of yttrium oleate and 23 grams of dodecylamine, and The mixture was purged with inert gas for 10 minutes. The reaction mixture was then heated to 70°C in 20 minutes with stirring under an inert atmosphere, maintained at 70°C for 20 minutes, then heated to 259°C in 20 minutes, and maintained at 259°C for 2 hours. The reaction mixture was then cooled. At 70°C, 20 milliliters of ethanol was added to the reaction mixture, which precipitated yttrium oxide nanocrystals. The product had a flake-like shape, and the flakes had a thickness of 2 nm.

[0092] Example 2 Removal of ligands from the surface of nanocrystals Treatment of the surface of as-synthesized HfO2 and ZrO2 nanocrystals with hydrochloric acid may be necessary to remove any organic components or capping agents on the surface of the nanocrystals before allowing any further modification. A typical method involves suspending the as-synthesized or purified nanocrystals in water by stirring and adjusting the suspension to a pH of 1 with a 1M hydrochloric acid solution. Upon addition of hydrochloric acid, the solution changes from a milky suspension to a clear solution. To further proceed with the reaction, the solution may be stirred overnight at room temperature. The solution is added to tetrahydrofuran, which precipitates a white solid. After centrifugation, the precipitate can be collected. The process of resuspending the particles in tetrahydrofuran, then centrifuging the mixture, and collecting the precipitate may be repeated until the pH of the supernatant is in the range of 5-7.

[0093] Example 3 Nanocrystal cap exchange ZrO 2 , HfO 2 and TiO 2 -ZrO 2 Nanocrystal cap exchange ZrO2, HfO2 and TiO2-ZrO2 nanocrystals were synthesized and then capped. To perform the cap exchange, the as-synthesized nanocrystals are transferred into a round bottom flask. The as-produced nanocrystals can be capped by the solvent or by reaction by-products present during synthesis. It may be desirable to exchange the capping molecules of the nanocrystals for various reasons, including but not limited to increasing the dispersibility in the solvent or some other matrix, imparting different optical properties, or imparting different chemical properties at the surface of the nanocrystals. The cap exchange process may include dispersing or suspending the as-synthesized nanocrystals in a solvent or reaction mixture with a specific amount of capping agent. The reaction may be carried out at an elevated temperature and for a specific length of time to facilitate the cap exchange. Capping methods for performing cap exchange on as-synthesized ZrO2, HfO2 and TiO2-ZrO2 nanocrystals are described. Non-limiting choices for blocking agents include methoxytri(ethyleneoxy)propyltrimethoxysilane, 2-[2-(2-methoxyethoxy)ethoxy]acetic acid, 3-(methacryloyl) (phenyloxy)propyltrimethoxysilane, and other silanes, carboxylic acids and alkoxy The cap exchange can be carried out in benzyl alcohol or other solvent or mixture of solvents.

[0094] Cap exchange of as-synthesized ZrO2, HfO2 and TiO2-ZrO2 nanocrystals The capping of methoxytri(ethyleneoxy)propyltrimethoxysilane on as-synthesized nanocrystals can be carried out using methoxytri(ethyleneoxy)propyltrimethoxysilane as a capping agent. Methoxytri(ethyleneoxy)propyltrimethoxysilane may be injected into a reaction vessel (typically a round-bottom flask) containing the as-synthesized nanocrystal reaction mixture. The weight ratio of methoxytri(ethyleneoxy)propyltrimethoxysilane to as-synthesized nanocrystals may range from 1:5 to 3:2. The mixture is then heated to 80-150°C for as short as 10 minutes or as long as 3 hours. A typical procedure for cap exchange of methoxy(triethyleneoxy)propyltrimethoxysilane on as-synthesized nanocrystals is as follows: 1 g of methoxytri(ethyleneoxy)propyltrimethoxysilane is added to a round-bottom flask containing a reaction mixture containing 5 g of as-synthesized ZrO2, HfO2 or TiO2-ZrO2 nanocrystals. The methoxy(triethyleneoxy)propyltrimethoxysilane capping agent was added. The mixture was continuously stirred during the addition of the capping agent. The suspension was heated to 80-150°C and maintained at this temperature with continued stirring for 10 minutes to 1 hour. The reaction mixture was then cooled to room temperature.

[0095] Alternatively, capping of ZrO2, HfO2 and TiO2-ZrO2 nanocrystals using methoxy(triethyleneoxy)propyltrimethoxysilane as a capping agent was performed. , may be performed on suspensions of nanocrystals other than the as-synthesized reaction mixture. Similar reactions can be performed on suspensions of nanocrystals, including (but not limited to) suspensions containing nanocrystals that have previously been cap-exchanged, suspensions containing as-synthesized nanocrystals that have previously been purified, suspensions containing nanocrystals from which the capping agent has been removed by acid treatment, and suspensions containing nanocrystals that have been transferred to another solvent. Alternative solvents for cap exchange can be selected from (but are not limited to): benzyl alcohol, propylene glycol monomethyl ether (PGME), propylene glycol methyl ether acetate (PGMEA), ethyl lactate (EL), and 2-propoxy-propanol (PnP), acetone, tetrahydrofuran, phenol, oleyl alcohol, toluene, butanol, propanol, isopropanol, ethanol, water, and mixtures thereof.

[0096] Cap exchange of as-synthesized ZrO2, HfO2 and TiO2-ZrO2 nanocrystals can be accomplished using 2-[2-(2-methoxyethoxy)ethoxy]acetic acid as a capping agent. 2-[2-(2-methoxyethoxy)ethoxy]acetic acid may be injected into a reaction vessel (typically a round-bottom flask) containing the as-synthesized nanocrystal reaction mixture. The amount of 2-[2-(2-methoxyethoxy)ethoxy]acetic acid should be at least 0.4 g and at most 1.0 g per gram of as-synthesized ZrO2, HfO2 or TiO2-ZrO2 nanocrystals. The mixture may then be kept at a low temperature of around 20° C. or heated to around 50° C. for a period of time as short as 30 minutes or as long as 3 hours. A typical procedure for the capping reaction of 2-[2-(2-methoxyethoxy)ethoxy]acetic acid on the as-synthesized nanocrystals is as follows: 2 g of 2-[2-(2-methoxyethoxy)ethoxy]acetic acid is added to a round bottom flask containing the reaction mixture containing 5 g of as-synthesized nanocrystals. Add 100 mL of 1,0 ... The mixture is then allowed to stand at room temperature while continuing to stir.

[0097] Alternatively, cap exchange of ZrO2, HfO2 and TiO2-ZrO2 nanocrystals using 2-[2-(2-methoxyethoxy)ethoxy]acetic acid as a capping agent was performed using the synthesized Similar reactions may be performed on suspensions of nanocrystals other than the as-synthesized reaction mixture. Similar reactions may be performed on suspensions of ZrO2, HfO2 or TiO2-ZrO2 nanocrystals, including (but not limited to) suspensions containing nanocrystals that have been previously cap-exchanged, suspensions containing as-synthesized nanocrystals that have been previously purified, suspensions containing nanocrystals from which the capping agent has been removed by acid treatment, and suspensions containing nanocrystals that have been transferred to another solvent. Alternative solvents for the capping reaction can be selected from (but are not limited to): benzyl alcohol, propylene glycol monomethyl ether (PGME), propylene glycol methyl ether acetate (PGMEA), ethyl lactate (EL), and 2-propoxy-propanol (PnP), acetone, tetrahydrofuran, phenol, oleyl alcohol, toluene, butanol, propanol, isopropanol, ethanol, water, cyclic ketones, and mixtures thereof.

[0098] Cap exchange of as-synthesized ZrO2, HfO2 and TiO2-ZrO2 nanocrystals The capping agent used was 3-(methacryloyloxy)propyltrimethoxysilane. The cap exchange of 3-(methacryloyloxy)propyltrimethoxysilane on as-synthesized nanocrystals can be carried out by injecting the 3-(methacryloyloxy)propyltrimethoxysilane into a reaction vessel (typically a round-bottom flask) containing the as-synthesized nanocrystal reaction mixture. The amount of 3-(methacryloyloxy)propyltrimethoxysilane can be as little as 0.8 g and as much as 1.5 g per gram of as-synthesized nanocrystals. The mixture is then heated to 120°C for as little as 30 minutes and as long as 1 hour. A typical procedure for cap exchange of 3-(methacryloyloxy)propyltrimethoxysilane on as-synthesized nanocrystals is as follows: A round-bottom flask containing a reaction mixture containing 5 g of as-synthesized ZrO2, HfO2 or TiO2-ZrO2 nanocrystals is poured into the flask. Add 4 g of 3-(methacryloyloxy)propyltrimethoxysilane. Stir the mixture continuously during the addition of the capping agent. Heat the suspension to 120° C. and maintain at this temperature while continuing to stir for 1 hour. Then cool the reaction mixture to room temperature.

[0099] Alternatively, cap exchange of ZrO2, HfO2 and TiO2-ZrO2 nanocrystals using 3-(methacryloyloxy)propyltrimethoxysilane as a capping agent was The reaction may be carried out on suspensions of nanocrystals other than the as-synthesized reaction mixture. Similar reactions may be carried out on suspensions of nanocrystals, including (but not limited to) suspensions containing previously cap-exchanged nanocrystals, suspensions containing previously purified as-synthesized nanocrystals, suspensions containing nanocrystals from which the capping agent has been removed by acid treatment, and suspensions containing nanocrystals transferred to another solvent. Alternative solvents for dispersing the nanocrystals during the cap-exchange reaction may be selected from (but are not limited to): benzyl alcohol, propylene glycol monomethyl ether (PGME), propylene glycol methyl ether acetate (PGMEA), ethyl lactate (EL), and 2-propoxy-propanol (PnP), acetone, tetrahydrofuran, phenol, oleyl alcohol, toluene, butanol, propanol, isopropanol, ethanol, water, cyclic ketones, and mixtures thereof.

[0100] Cap exchange of as-synthesized ZrO2, HfO2 and TiO2-ZrO2 nanocrystals can be carried out using 3-(methacryloyloxy)propyltrimethoxysilane and methoxy(triethyleneoxy)propyltrimethoxysilane as capping agents. A typical cap exchange reaction of ZrO2 nanocrystals is as follows: 500 mg of as-synthesized ZrO2 was mixed with 25 mg of 3-(methacryloyloxy)propyltrimethoxysilane in 5 ml of PGMEA at 100 °C for 1 h. Then, 150 mg of methoxy(triethyleneoxy)propyltrimethoxysilane was added to the suspension, and the mixture was stirred at 100 °C for another 1 h. The resulting mixture was washed with heptane, and the white precipitate was collected.

[0101] The as-synthesized nanocrystals of ZrO2, HfO2 and TiO2-ZrO2 exhibited hydrophobic The nanocrystals may be capped to facilitate dispersion in solvents and matrices. The cap exchange process may involve dispersing or suspending the as-synthesized nanocrystals with a certain amount of capping agent or with the capping agent in a relatively hydrophobic solvent, where the hydrophobic solvent is selected from solvents including (but not limited to) naphtha, toluene, heptane, pentane, decane, chloroform. The cap exchange reaction may be carried out at room temperature or at elevated temperatures for times ranging from minutes to days to facilitate the cap exchange. Capping to make the surfaces of as-synthesized ZrO2, HfO2 and TiO2-ZrO2 nanocrystals more compatible with hydrophobic solvents and media The agents of choice include (but are not limited to) stearic acid, oleic acid, and octadecyltrimethoxysilane. In a typical reaction, 2 g of oleic acid is added to a suspension containing 2 g of as-synthesized nanocrystals in 20 ml of toluene. The mixture is stirred continuously during and after the addition of the capping agent. The reaction mixture is allowed to react for a few minutes to a few hours and then purified.

[0102] Cap exchange of as-synthesized ZrO2, HfO2 and TiO2-ZrO2 nanocrystals This may be done using methoxypoly(ethyleneoxy)propyltrimethoxysilane as a capping agent. Alternatively, ZrO2, HfO2 and TiO2-ZrO2 nanocrystals using methoxypoly(ethyleneoxy)propyltrimethoxysilane as a capping agent may be prepared. The cap exchange of nanocrystals may be carried out on suspensions of nanocrystals other than the as-synthesized reaction mixture. Similar reactions can be carried out on suspensions of nanocrystals, including (but not limited to) suspensions containing previously cap-exchanged nanocrystals, suspensions containing previously purified as-synthesized nanocrystals, suspensions containing nanocrystals from which the capping agent has been removed by acid treatment, and suspensions containing nanocrystals transferred to another solvent. Alternative solvents for dispersing the nanocrystals during the cap exchange reaction can be selected from (but are not limited to): benzyl alcohol, propylene glycol monomethyl ether (PGME), propylene glycol methyl ether acetate (PGMEA), ethyl lactate (EL), and 2-propoxy-propanol (PnP), acetone, tetrahydrofuran, phenol, oleyl alcohol, toluene, butanol, propanol, isopropanol, ethanol, water, cyclic ketones, and mixtures thereof.

[0103] Cap exchange of yttrium oxide nanocrystals. Organosilane-capped yttrium oxide nanocrystals can be prepared by a cap exchange process using as-synthesized yttrium oxide nanocrystals and methoxy(triethyleneoxy)propyltrimethoxysilane. The as-synthesized yttrium oxide nanocrystals and methoxytri(ethyleneoxy)propyltrimethoxysilane were mixed in tetrahydrofuran. The mixture was then heated to 200°C for 2-4 hours in an autoclave. After the reaction time, the mixture was cooled to room temperature.

[0104] Alternatively, the cap exchange process may be carried out with other organosilanes, organocarboxylic acids, and organoalcohols. Similar reactions can be carried out with suspensions of nanocrystals, including (but not limited to) suspensions containing previously cap-exchanged nanocrystals, suspensions containing previously purified as-synthesized nanocrystals, suspensions containing nanocrystals from which the capping agent has been removed by acid treatment, and suspensions containing nanocrystals transferred to another solvent. Alternative solvents for dispersing the nanocrystals during the cap exchange reaction can be selected from (but are not limited to): benzyl alcohol, propylene glycol monomethyl ether (PGME), propylene glycol methyl ether acetate (PGMEA), ethyl lactate (EL), and 2-propoxy-propanol (PnP), acetone, phenol, oleyl alcohol, toluene, butanol, propanol, isopropanol, ethanol, water, cyclic ketones, and mixtures thereof.

[0105] Cap exchange of ZnO nanocrystals If ZnO nanocrystals are synthesized without adding a capping agent during synthesis, the nanocrystals can be capped after synthesis is complete using 3-(methacryloyloxy)propyltrimethoxysilane, methoxytri(ethyleneoxy)propyltrimethoxysilane, 2,2,2-methyoxyethyoxyethyoxyacetic acid, or a combination of these materials. Capping with 2,2,2-methyoxyethyoxyethyoxyacetic acid can be performed at room temperature, or with the aid of sonication, or by heating the suspension to 80° C., or with a combination of both heating and sonication. A typical procedure is as follows: After synthesis, 4 g of the as-synthesized precipitate is poured into a round-bottom flask and cooled to 30° C. for 1 hour. The nanocrystals are redispersed in PGMEA in 500 ml of 10 ...

[0106] Example 4 Nanocrystal purification As-synthesized ZrO 2 , HfO 2 and TiO 2 -ZrO 2 Nanocrystals After autoclave synthesis of ZrO2, HfO2 and TiO2-ZrO2 nanocrystals The collected suspension of as-synthesized milky white nanocrystals can be purified. In a typical method, the suspension of nanocrystals is mixed with ethanol and centrifuged (8000 rpm, 30 min) to separate the nanocrystals. After decanting and discarding the supernatant, the white precipitate is collected. The wet nanocrystals are suspended in additional ethanol by sonication, stirring, or shaking, and the suspension is centrifuged again. These resuspension steps of adding ethanol, centrifugation, and collecting the resulting powder are repeated about four more times, thereby obtaining purified nanocrystals.

[0107] ZrO with hydrophobic surface 2 Nanocrystals To purify the nanocrystals, they are dispersed in hexane and then precipitated using ethanol as an antisolvent. The resulting mixture is then centrifuged and The nanocrystals are then collected, and this purification process is repeated three times, resulting in nanocrystals that are easily dispersed in hydrophobic solvents such as naphtha or heptane.

[0108] ZrO 2 , HfO 2 and TiO 2 -ZrO 2 Nanocrystals After synthesis, capping and / or cap exchange, the ZrO2, HfO2 and TiO2-ZrO2 nanocrystals may be purified or further purified. One typical purification of nanocrystals after synthesis in a mixture of alcohol or benzyl alcohol and other solvents is as follows: THF is added to the reaction mixture in a volume ratio of 2:1 THF to reaction mixture, and then heptane is added in a volume ratio of 7-9:1 heptane to reaction mixture. The reaction of the nanocrystal suspension to THF and heptane may be adjusted based on the concentration of nanocrystals in the suspension. This causes the nanocrystals to precipitate, which are then centrifuged. After centrifugation and decanting the supernatant, an additional amount of THF or PGMEA is added to disperse the nanocrystals, and then heptane is added. The ratio of heptane to THF or PGMEA may be 2:1 or 3:1. The cycle of sonication, centrifugation and decantation is repeated 2-5 times, thereby purifying the nanocrystals.

[0109] ZnO nanocrystals As-synthesized, capped and / or cap-exchanged zinc oxide nanocrystals can be purified or further purified to obtain optically clear suspensions in polar solvents. This process removes at least a portion of the by-products of the synthesis or cap-exchange reactions. A typical method for purifying ZnO nanocrystals is as follows: 200 ml of a suspension of zinc oxide nanocrystals in ethanol (~1 g ZnO) is mixed with 400-500 ml of heptane to form a white precipitate that is collected by centrifugation, and the supernatant is then decanted and discarded. A sample of 20-60 ml of ethanol is then used to redisperse the white precipitate in solution using 5 min of sonication, and a sample of 40-50 ml of heptane is again used to precipitate the product. The white precipitate is collected by centrifugation, followed by a second decantation and discarding of the supernatant. The ethanol redispersion and heptane precipitation steps are repeated twice. This was repeated several times to obtain purified nanocrystals.

[0110] In a further example, the capped zinc oxide nanocrystals were purified to obtain a redispersible dry powder. A 200 ml suspension of organosilane-capped zinc oxide nanocrystals in ethanol (~1 g ZnO) was mixed with 400-500 ml heptane to form a white precipitate. The white precipitate was collected by centrifugation and the supernatant was then decanted and discarded. The white solid was then redispersed with a 20 ml sample of ethanol, assisted by sonication for 5 minutes. The product was again precipitated with 40-50 ml of heptane. The white precipitate was collected by centrifugation and the procedure of redispersion with ethanol and precipitation with heptane was (preferably) repeated two more times, after a second decantation and discarding of the supernatant. A 5 ml sample of pentane was then added to the washed organosilane-capped ZnO nanocrystals and sonicated for 5 minutes. The resulting mixture was then centrifuged again and the precipitate was again collected. After discarding the supernatant, the solid was dried in air or under vacuum, thereby obtaining a dry white precipitate, which was a powder of ZnO nanocrystals.

[0111] Another method is provided for purifying the as-synthesized organosilane-capped zinc oxide nanocrystals to obtain an optically clear suspension in a polar solvent. A 1.6 L suspension of the prepared organosilane-capped zinc oxide nanocrystals in ethanol (containing more than 8 g ZnO) is mixed with 3.2-4.0 L heptane, forming a white precipitate. The white precipitate is collected by centrifugation, and the supernatant is then decanted and discarded. The white precipitate is then redispersed with a sample of 60 ml ethanol, assisted by sonication for 5 min. The product is again precipitated with 120-150 ml heptane. The white precipitate is collected by centrifugation, and after a second decantation and discarding of the supernatant, less than 8 g of organosilane-capped ZnO nanocrystals are obtained. To achieve even higher purity, the ethanol redispersion and heptane precipitation procedure is repeated two more times to obtain a white precipitate.

[0112] Y 2 O 3 Nanocrystals The purification of the as-synthesized Y2O3 nanocrystals is as follows: the as-synthesized reaction mixture was precipitated by adding ethanol to the reaction mixture in a volume ratio of 4:1. The suspension was centrifuged at 9000 rpm for 20 min, after which the supernatant was decanted and discarded to recover the precipitate. The precipitate was then suspended in 2 ml of chloroform by sonication (>1 min) and reprecipitated by adding 2 ml of ethanol. The suspension was centrifuged at 9000 rpm for 30 min, after which the supernatant was again decanted and discarded to recover the precipitate. The precipitate was dispersed in 3 ml of hexane by sonication (>2 min) and reprecipitated with 2 ml of ethanol, the supernatant was decanted and discarded to recover the precipitate. This redispersion and precipitation procedure with hexane and ethanol was repeated once more. After this purification procedure, the yttrium oxide nanocrystals can be dispersed in several solvents such as chloroform, hexane, toluene and tetrahydrofuran.

[0113] The purification of Y2O3 nanocrystals after the cap exchange reaction is as follows: the nanocrystals are precipitated with pentane and centrifuged at 9000 rpm for 20 min. The precipitate is redispersed in tetrahydrofuran, precipitated with hexane and centrifuged at 9000 rpm for 20 min to remove excess capping agent and by-products. The precipitate can be dispersed in various solvents such as tetrahydrofuran, chloroform and toluene, and mixtures of solvents such as hexane and ethanol.

[0114] Example 5 Nanocomposite Formation Formation of nanocomposite suspensions and nanocomposite layers from capped ZnO nanocrystals and polymers The capped and purified ZnO nanocrystals in the form of white precipitate or nanocrystalline powder can be dispersed in many polar solvents, including but not limited to tetrahydrofuran, ethanol, methanol, acetonitrile, PGMEA, PGME, PGPE, ethyl lactate, cyclic ketones, and acetone, to form optically transparent suspensions. These optically transparent suspensions can be mixed with various polymer solutions to form uniformly dispersed ZnO / polymer nanocomposites using solvent blends. The dispersion solvent for the nanocrystals may be selected based on the chemical compatibility of the capping agent and the polymer. A solvent system suitable for dispersing both the nanocrystals and the polymer is preferred. To form a composite solution with the desired nanocrystal to polymer ratio, the nanocrystals dispersed in the selected solvent are mixed with a separately prepared solution of the polymer, preferably in the same solvent or a different solvent, or a combination of solvents compatible with the selected solvent. These polymers include but are not limited to PMMA, JSR Topcoat, JSR Micro( (California) brand acrylate-based photoresist, Honeywell Spray These include pin-on-glass polymers (silicon-based polymers from Honeywell Electronic Materials, California), PEO (polyethylene oxide), epoxy resins, silicones (eg, polydimethylsiloxane (PDMS) and polymethylphenylsiloxane), and epoxy resins.

[0115] A typical method for forming the nanocomposite suspension involves adding a 38 milligram sample of the purified, capped ZnO nanocrystal powder to a 0.5 gram Honeywell Electronic A solution of spin-on glass (SOG) polymer and ethanol ( The mixture was sonicated for 30 min to obtain an optically transparent suspension.

[0116] Similarly, highly transparent films were obtained using epoxy or acrylic polymers or spin-on glasses with ZrO2 nanocrystals having an average size of 5 nm. The loading of the nanocrystals by weight can be varied from 0.01 percent to 90 percent, resulting in optically transparent suspensions and films.

[0117] Nanocomposite films were prepared by spin-coating a suspension of capped ZnO nanocrystals with an average particle size of 3-4 nm with SOG in ethanol onto a 2-inch quartz disk at a rotation speed of 500 rpm to ensure uniformity of the resulting nanocomposite film. The optical density (OD) (absorbance) of the film was measured at various points along three radial directions using UV-Vis spectroscopy. Measurements were taken at 0, 3, 5, 8, 12, 16, and 20 mm from the center of the disk, which was defined as 0 mm. The exciton peak showed a maximum at 330 nm, and the deviation of the OD at 330 nm was less than 2.0% for all measurements.

[0118] A suspension of capped ZnO nanocrystals mixed with SOG in ethanol was also used to spin coat films onto three 1-inch quartz disks at 300, 500, and 700 rpm, respectively. To remove residual ethanol, these films were baked in air at 80° C. for 1 min. The resulting films were visually transparent with no obvious haze or dullness. The nominal content of ZnO nanocrystals in the SOG polymer nanocomposite was determined to be 72.0 wt %, calculated from the nanocomposite composition. Figure 11 shows the UV-visible spectra of the resulting films. All of these nanocomposite films have bandgaps with a maximum wavelength of about 330 nm, which corresponds to the exciton peak of ZnO. Increasing the spin speed at which the films were applied from 300 to 700 rpm decreased the optical density (OD) (absorbance) of the films due to the decrease in film thickness. The nanocomposite films were highly transparent at visible wavelengths, as indicated by the lack of scattering above 350 nm and the presence of a sharp exciton peak in the UV-visible spectrum.

[0119] The method of forming the nanocomposite involves solvent mixing the purified capped zinc oxide nanocrystals of the present disclosure with PMMA in tetrahydrofuran. The purified capped ZnO nanocrystals were dispersed in tetrahydrofuran and then mixed with a solution of PMMA and THF. Figure 12 shows a TEM of the nanocomposite spun onto a CuTEM grid. The scale bar on the TEM image is 10 nm, and the 4-5 nm capped ZnO nanocrystals are uniformly dispersed in the PMMA matrix without forming any aggregates. The inset shows a close-up of a single nanocrystal in the nanocomposite.

[0120] Nanocomposite films were prepared by spin coating 2-inch silicon wafers with organosilane-capped ZnO nanocrystals dispersed in a solution of PMMA and THF at a spin speed of 500 rpm. Film thickness measurements were performed with a Dektak profilometer, in which intermittent scratches were made on the film to determine the film thickness. A distance of 1 mm was measured, which indicated a uniform film thickness of less than 300 nm and a thickness variation of less than 3% over this range.

[0121] Another example of a method for forming a nanocomposite of the present disclosure includes dispersing the purified capped zinc oxide nanocrystals of the present disclosure with an epoxy polymer in tetrahydrofuran. 500 mg of purified organosilane capped ZnO nanocrystals were dispersed in 2 ml of tetrahydrofuran and mixed with 1.5 g of epoxy EPON® resin 862 (diglycidyl ether of bisphenol F), which is a low viscosity liquid epoxy resin, and 0.3 g of Epikure® W hardener (Epikure W is an aromatic diamine hardener for epoxy resins). The mixture was transferred into a mold and cured for 12 hours, then post-cured at 150° C. for 3 hours.

[0122] Another example of a method of forming a nanocomposite of the present disclosure involves manually mixing EPON862 resin with hardener W (or hardener 3295) in a weight ratio of 5:1. To this mixture, ZnO or ZrO2 capped with methoxytri(ethyleneoxy)propyltrimethoxysilane is then added. The weight ratio of nanocrystals to epoxy mixture can range from 1:1000 to 10:1. A small amount of THF (up to 200% by weight of the composite mixture) was added to reduce the viscosity of the nanocrystal and epoxy resin mixture. The mixture is then sonicated for less than 5 minutes in an ultrasonic bath or with a Hielscher UP200S sonication probe. After sonication, the composite mixture (2 grams to 4 grams) was then poured into an aluminum dish (4 cm diameter, which acts as a mold). The dish was then placed in a vacuum oven. A vacuum was applied to remove the THF and air bubbles. The oven was then heated to 80° C. under vacuum overnight (less than 10 hours). The resulting composite was post-cured at 150° C. for an additional 3 hours and removed from the vacuum oven.

[0123] Another example of a method for forming a nanocomposite of the present disclosure is as follows: Epoxy resin EPON 862 and hardener 3274 are premixed by hand in a weight ratio of 10:4. 3-(methacryloyloxy)propyltrimethoxysilane-capped ZrO2 nanocrystals are then added to the epoxy resin at a loading of 0.01-99.99 wt%. A small amount (up to 200 wt% of the composite mixture) of ZrO2 nanocrystals capped with 3-(methacryloyloxy)propyltrimethoxysilane is added to the epoxy resin to reduce the viscosity of the nanocrystal-epoxy resin mixture. Acetone was added. The mixture was then sonicated in a sonication bath or with a Hielscher UP200S sonication probe for less than 5 minutes. The mixed composite mixture (2 grams to 4 grams) was then poured into an aluminum dish (4 cm diameter, which served as a mold). The dish was then placed in a vacuum oven. A vacuum was applied to remove the acetone and air bubbles. The resulting composite was cured at room temperature for 24 hours and removed from the vacuum oven.

[0124] A typical procedure for spin-coating composite films of 3-(methacryloyloxy)propyltrimethoxysilane-capped nanoparticles and epoxy is as follows: Epoxy resin EPON 862 and hardener 3274 are manually premixed in a weight ratio of 10:4. The desired amount of capped nanocrystals is then added to the epoxy resin at a loading of 1-99.99 wt%. Acetone is added, thereby preparing a spin-coating solution with an appropriate solid content (ranging from 10 wt% to 50 wt%). The mixture is then sonicated for 5 min in a sonication bath. This solution can then be used directly for spin-coating. By varying the spin speed, various film thicknesses ranging from hundreds of nanometers to several micrometers can be obtained.

[0125] Another example of forming a nanocomposite of the present disclosure involves solvent mixing the purified capped zinc oxide nanocrystals of the present disclosure with a photoresist from JSR Micro Inc. The coated and capped ZnO nanocrystals were dispersed in PGMEA to form a clear suspension, which was then mixed with a JSR photoresist solution. After being spun onto a surface, the resulting suspension formed a nanocomposite film.

[0126] In a further embodiment, the nanocomposite of the present disclosure is prepared by solvent mixing the purified capped zinc oxide nanocrystals of the present disclosure with a topcoat polymer from JSR Micro Inc. As-purified, organosilane-capped ZnO nanocrystals were dispersed in 4-methyl-2-pentanol, which is also the solvent in the JSR topcoat polymer solution. A dispersion was formed by mixing the nanocrystal suspension with the topcoat solution. The dispersion can be used to form a nanocomposite film by spin-coating onto a surface.

[0127] The disclosed method involves dispersing purified capped zinc oxide nanocrystals in water. The purified capped ZnO nanocrystals were dispersed in water by mixing the purified ZnO wet precipitate with water and ultrasonicating to form a clear suspension. This suspension was mixed with JSR water-based topcoat solution (NFC545-34).

[0128] In a further example, nanocomposites of the present disclosure are formed by dispersing methoxytri(ethyleneoxy)propyltrimethoxysilane-capped HfO2 nanocrystals in ethanol to form a suspension, and mixing the suspension with a solution of SOG and ethanol. Figure 13 shows TEM images of nanocomposites prepared by spin-coating the suspension onto a CuTEM grid. The inset in this figure shows a close-up of the nanocrystals. These images show that the 4-5 nm rice-shaped HfO2 nanocrystals are uniformly dispersed in the SOG matrix, with no visible agglomerates forming.

[0129] A further embodiment for forming the nanocomposite of the present disclosure is the methoxytri(ethy) ZrO2 nanocrystals and acrylic acid capped with (phenyloxy)propyltrimethoxysilane The process involves dispersing a polymer based on the polymer matrix in a mixture of PGMEA and PGME, thereby forming a nanocomposite suspension. Films of this suspension are fabricated by spin coating onto a quartz disk and a silicon wafer. The nanocrystal content in the suspension is less than 80 wt%. The film is fabricated after filtering the nanocomposite suspension through a 200 nm filter. Figure 14 shows an AFM image showing the surface roughness of a nanocomposite film prepared by spin-coating the suspension onto a quartz disk. The root mean square (RMS) roughness value for this film was 0.521 nm.

[0130] in-situ polymerization Nanocomposites of ZrO2 nanocrystals and polymethylmethacrylate can be prepared by in situ polymerization of nanocrystals at least partially capped with methyl methacrylate (MMA) and 3-(methacryloyloxy)propyltrimethoxysilane. A typical synthesis procedure for this nanocomposite is as follows: 500 mg of MMA and 2 mg of AlBN are dissolved in 9 g of toluene and the solution is heated to 100 °C. 0.5 g of ZrO2 nanocrystals capped with a mixture of both 3-(methacryloyloxy)propyltrimethoxysilane and methoxytri(ethyleneoxy)propyltrimethoxysilane are dispersed in 1 g of THF. This dispersion is added dropwise into the solution of MMA and toluene. The mixture is maintained at 100 °C for 16 hours. The reaction mixture is slightly opaque. The resulting precipitate is recovered by anti-solvent precipitation using methanol. The precipitate is then redispersed in THF, thereby forming a 12 wt % dispersion. Thermogravimetric analysis (TGA) of the product indicates that approximately 38% by weight of the solids content of this dispersion is from the capping agent and PMMA.

[0131] Another example of a nanocomposite formed by in situ polymerization of ZrO2 nanocrystals and polymethylmethacrylate is as follows: 9 g of toluene is heated to 100°C. (ethyloxy)propyltrimethoxysilane and methoxytri(ethyleneoxy)propyltrimethoxysilane 0.5 g of ZrO2 nanocrystals capped with trimethoxysilane, 0.5 g of MMA and 2 mg of AlBN are added to 1 g of THF. This mixture is added dropwise into hot toluene. The mixture is maintained at 100°C for 16 hours, and the reaction mixture becomes slightly opaque. The resulting nanocomposite is recovered by anti-solvent precipitation using methanol. The precipitate is then redispersed in THF, thereby forming a 5 wt% dispersion. According to TGA of the product, about 31 wt% of the solid content of this dispersion is due to the capping agent and PMMA. [Mode of the invention] [1] 1. A method for producing nanocrystals, comprising: dissolving or mixing said nanocrystal precursors in at least one solvent, thereby forming a solution; Optionally, at least one of heating and increasing the pressure of the solution; and reacting said precursor or reacting said precursor with said at least one solvent of said solution, thereby forming said nanocrystals; The method comprising: [2] 2. The method of claim 1, wherein the nanocrystals are capped with at least one agent, thereby increasing the solubility or dispersibility of the nanocrystals in the at least one solvent or other substance. [3] 3. The method of claim 2, wherein the at least one agent comprises at least one organosilane, organocarboxylic acid, or organoalcohol. [4] 3. The method of claim 2, wherein the at least one agent for capping the nanocrystals is contained in a solution. [5] 5. The method of claim 4, wherein the at least one agent for capping the nanocrystals is contacted with the solution before, during, or after the reacting is performed. [6] 2. The method of claim 1, further comprising purifying and / or isolating the nanocrystals. [7] 7. The method of claim 6, further comprising capping the purified and / or separated nanocrystals with at least one capping agent, thereby producing at least partially capped nanocrystals. [8] 8. The method of claim 7, further comprising purifying and / or isolating the at least partially capped nanocrystals. [9] 7. The method of claim 6, further comprising contacting the nanocrystals with an additional solvent.

[10] 9. The method of claim 8, further comprising contacting the at least partially capped nanocrystals with an additional solvent.

[11] 10. The method of claim 9, wherein the additional solvent comprises at least one solvent of claim 1.

[12] 11. The method of claim 10, wherein the additional solvent comprises at least one solvent of claim 1.

[13] 13. The method of any of claims 6 to 12, wherein the nanocrystals or at least partially capped nanocrystals are dispersed in a further substance.

[14] 14. The method of claim 13, wherein the additional substance is a polymer.

[15] 15. A nanocrystal or at least a partially capped nanocrystal formed by the method according to any one of 1 to 14 above.

[16] A method of forming a film or coating, comprising dispersing the nanocrystals or at least partially capped nanocrystals described in paragraph 15 in a further substance to form a dispersion, and applying the dispersion to a surface.

[17] 17. The method of claim 16, wherein the applying comprises spin coating, spraying, dipping, screen printing, rolling, painting, printing, ink jet printing, evaporative deposition, and / or vapor deposition.

[18] 16. A method of forming a nanocomposite, comprising combining the nanocrystal or at least a partially capped nanocrystal of claim 15 with an additional substance, thereby forming the nanocomposite.

[19] 19. The method of any one of claims 1 to 14 or 16 to 18, wherein the nanocrystals or the at least partially capped nanocrystals are comprised of zinc oxide, hafnium oxide, zirconium oxide, hafnium-zirconium oxide, titanium-zirconium oxide and / or yttrium oxide or other semiconductor material.

[20] The at least one solvent is benzyl alcohol, phenol, oleyl alcohol , toluene, butanol, propanol, isopropanol, ethanol, methanol, water, propylene glycol monomethyl ether (PGME), propylene glycol methyl ether acetate (PGMEA), ethyl lactate (EL), and 2-propoxy-propanol (PnP), acetonitrile, acetone, tetrahydrofuran, cyclic ketones, and mixtures thereof. [twenty one] The at least one agent may be selected from the group consisting of n-propyltrimethoxysilane, n-propyltriethoxysilane, n-octyltrimethoxysilane, n-octyltriethoxysilane, phenyltrimethoxysilane, 2-[methoxy(polyethyleneoxy)propyl]-trimethoxysilane, methoxytri(ethyleneoxy)propyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-(methacryloyl ... Trimethoxysilane, 3-isocyanatopropyltriethoxy 21. The method according to any one of 2 to 5, 7, 8, 10, 12 to 14 or 16 to 20, comprising at least one of silane, 3-isocyanatopropyltrimethoxysilane, and glycidoxypropyltrimethoxysilane, heptanol, hexanol, octanol, benzyl alcohol, phenol, ethanol, propanol, butanol, oleyl alcohol, dodecyl alcohol, octadecanol, and triethylene glycol monomethyl ether, octanoic acid, acetic acid, propionic acid, 2-[2-(2-methoxyethoxy)ethoxy]acetic acid, oleic acid, benzoic acid, or mixtures thereof. [twenty two] The further materials include the polymers poly(acrylonitrile-butadiene-styrene) (ABS), poly(methyl methacrylate) (PMMA), celluloid, cellulose acetate, poly(ethylene-vinyl acetate) (EVA), poly(ethylene-vinyl alcohol) (PVA), and the like. (EVOH), Fluoroplastics, Polyacrylates (Acrylic), Polyacrylonitrile (PAN), Polyamides (PA or Nylon), Polyamide-imides (PAI) , polyaryletherketone (PAEK), polybutadiene (PBD), polybutylene (PB), polybutylene terephthalate (PBT), polycaprolactone (PCL), polychlorotrifluoroethylene (PCTFE), polyethylene terephthalate (PET), polycyclohexylene dimethylene terephthalate (PCT), polycarbonate (PC), polyhydroxyalkanoates (PHAs), polyketone (PK), polyester, polyethylene (PE), polyetheretherketone (PEEK), polyetherketoneketone (PEKK), polyetherimide (PEI), polyethersulfone (PES), polyethylene chlorinate (PEC), polyimide (PI), polylactic acid (PLA), polymer Poly(vinyl chloride) (PVC), polyvinylidene chloride (PVDC), poly(styrene-acrylonitrile) (SAN), spin-on glass (SOG) polymers, siloxane spin-on polymers in ethanol, propylene glycol methyl ether acetate (PGMEA), isopropyl alcohol, or a mixture of these solvents, JSR Micro Topcoat (NFC TCX014 in 4-methyl-2-pentanol), JSR Micro Photoresist (ARF1682J-19), 22. The method according to any one of 13 to 21, comprising a matrix material such as silicone, polydimethylsiloxane (PDMS) or polymethylphenylsiloxane, or a mixture thereof. [twenty three] 2. The method of claim 1, wherein the at least one solvent further comprises water. [twenty four] 24. The method of claim 23, wherein the water is present in a molar ratio of water to precursor ranging from 1:1 to 4:1. [twenty five] 25. The method of claim 24, wherein the nanocrystals are in the average size range of 1 nm to 5 nm.

Claims

1. 1. A method for solvothermal production of nanocrystals, comprising: dissolving or mixing at least one precursor of said nanocrystals in at least one solvent, thereby forming a solution; heating said solution to a temperature in the range of 250° C. to 350° C., thereby forming said nanocrystals, wherein said nanocrystals comprise at least one of hafnium oxide, zirconium oxide, hafnium zirconium oxide, and titanium zirconium oxide, and said precursor comprises at least one of an alkoxide, an acetate, an acetylacetonate, and a halide. The method.

2. The method of claim 1 , wherein the nanocrystals are capped with at least one agent to increase the solubility or dispersibility of the nanocrystals.

3. The at least one agent may be selected from the group consisting of n-propyltrimethoxysilane, n-propyltriethoxysilane, n-octyltrimethoxysilane, n-octyltriethoxysilane, phenyltrimethoxysilane, 2-[methoxy(polyethyleneoxy)propyl]-trimethoxysilane, methoxytri(ethyleneoxy)propyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-(methacryloyloxy)propyltrimethoxysilane, 3-isocyanatopropyltriethoxysilane, 3. The method of claim 2, wherein the solvent comprises at least one of the following: dimethylformamide, dimethyl silane, dimethyl ether ...

4. The method of claim 1 , wherein water is present in the solution.

5. The method of claim 2 , wherein the at least one agent for capping the nanocrystals is contained in the solution.

6. The method of claim 1, wherein the nanocrystals are in the average size range of 1 nm to 10 nm.

7. The method of claim 2 , further comprising purifying and / or isolating the nanocrystals.

8. The method of claim 7, further comprising dispersing the purified and / or separated nanocrystals in a solvent or polymer.

9. 2. The method of claim 1, wherein the at least one solvent comprises benzyl alcohol, phenol, oleyl alcohol, toluene, butanol, propanol, isopropanol, ethanol, methanol, propylene glycol monomethyl ether (PGME), propylene glycol methyl ether acetate (PGMEA), ethyl lactate (EL), and 2-propoxy-propanol (PnP), acetonitrile, acetone, tetrahydrofuran, a cyclic ketone, or a mixture thereof.

10. The precursor is zirconium ethoxide (Zr(OCH 2 CH 3 ) 4 ), zirconium n-propoxide (Zr(OCH 2 CH 2 CH 3 ) 4 ), zirconium isopropoxide (Zr(OCH(CH 3 ) 2 ) 4 ), zirconium n-butoxide (Zr(OCH 2 CH 2 CH 2 CH 3 ) 4 ), zirconium t-butoxide (Zr(OC(CH 3 ) 3 ) 4 ), hafnium ethoxide (Hf(OCH 2 CH 3 ) 4 ), hafnium n-propoxide (Hf(OCH 2 CH 2 CH 3 ) 4 ), hafnium isopropoxide (Hf(OCH(CH 3 ) 2 ) 4 ), hafnium butoxide (Hf(OCH 2 CH 2 CH 2 CH 3 ) 4 ), hafnium t-butoxide (Hf(OC(CH 3 ) 3 ) 4 ), titanium ethoxide (Ti(OCH 2 CH 3 ) 4 ), titanium n-propoxide (Ti(OCH 2 CH 2 CH 3 ) 4 ), titanium isopropoxide (Ti(OCH(CH 3 ) 2 ) 4 ), titanium t-butoxide (Ti(OC(CH 3 ) 3 ) 4 ), titanium n-butoxide (Ti(OCH 2 CH 2 CH 2 CH 3 ) 4 ), zirconium acetate (Zr(OOCCH 3 ) 4 ), zirconium acetylacetonate (Zr(CH 3 COCHCOCH 3 ) 4 ), Hafnium acetate (Hf(OOCCH 3 ) 4 ), zirconium chloride (ZrCl 4 ), zirconium fluoride (ZrF 4 ), zirconium iodide (ZrI 4 ), zirconium bromide (ZrBr 4 ), hafnium bromide (HfBr 4 ), hafnium chloride (HfCl 4 ), hafnium iodide (HfI 4 ), titanium chloride (TiCl 4 ), titanium bromide (TiBr 4 ), titanium iodide (TiI 4 ), titanium fluoride (TiF 4 2. The method of claim 1, wherein the compound is selected from the group consisting of:

11. The method of claim 1, wherein the solution pressure is in the range of 100 to 900 psi.

12. The method of claim 2, further comprising dispersing the at least partially capped nanocrystals in at least one solvent or other medium to form a dispersion, and applying the dispersion to a surface to form a film or coating.

13. The method of claim 12, wherein the applying comprises spin coating, spraying, dipping, screen printing, rolling, painting, printing, inkjet printing, evaporative deposition, and / or vapor deposition.

14. The method of claim 1 , wherein the nanocrystals have an average size in the range of 1 nm to 5 nm.

Citation Information

Patent Citations

  • Zirconium oxide nanoparticle and method for producing the same

    JP2008044835A

  • Method for manufacturing catalytic carrier for cleaning exhaust gas

    JP2008289985A

  • Coating liquid for forming transparent film for synthetic resin lens, and synthetic resin lens

    JP2009162848A