Release film

The release film with a melamine and polymer crosslinked network structure addresses the challenges of peeling force variability and stability in MLCC production, ensuring consistent and reliable peeling performance and defect prevention.

JP7554798B2Active Publication Date: 2024-09-20TORAY ADVANCED MATERIALS KOREA INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2022141454
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-09-07
Filing Date
2022-09-06
Publication Date
2024-09-20
Estimated Expiration
2042-09-06

AI Technical Summary

Technical Problem

Existing release films for MLCCs face challenges in achieving a diverse range of peeling forces and stability over time, leading to issues such as premature peeling of ceramic slurry or cracking of green sheets due to inappropriate peeling forces, and solvent residues causing defects like orange peel-like stains and low solvent resistance.

Method used

A release film comprising a base film with a release layer formed by a specific release coating composition, containing a melamine component, a polymer component, and an acid catalyst, which forms a crosslinked network structure to achieve a wide range of peeling forces and excellent stability, using a formulation that includes a melamine component with a weight average molecular weight of 3,000 to 30,000 and a polymer component with polar functional groups, and a crosslinked network structure.

Benefits of technology

The release film achieves a wide range of peeling forces and exhibits excellent stability over time, improving the reliability of MLCC production by preventing defects and maintaining consistent peeling performance, even after prolonged storage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554798000008
    Figure 0007554798000008
  • Figure 0007554798000010
    Figure 0007554798000010
  • Figure 0007554798000009
    Figure 0007554798000009
Patent Text Reader

Abstract

To provide a release film which can realize various ranges of peel force and exhibit excellent temporal stability.SOLUTION: The release film comprises: a substrate film; and a release layer formed by applying a release coating composition to at least one face of the substrate film. The release layer satisfies the formula (1) defined by 0.5≤Pb / Pa≤10.0 (where Pa is the maximum absorption peak strength in the region of the wave number greater than or equal to 1450 cm-1 and less than 1650 cm-1 in the FT-IR spectrum ; and Pb is the maximum absorption peak strength in the region of wave number greater than or equal to 1650 cm-1 and less than or equal to 1850 cm-1 in the FT-IR spectrum.)SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to release films. [Background technology]

[0002] Release films are generally used as protective films to which an adhesive coating is adhered to protect the adhesive component from foreign matter in the atmosphere or unwanted adherents, and generally have a structure in which a release layer is formed on a polyester base film.

[0003] In particular, release films are used as carrier films for thinly and uniformly applying ceramic slurry to green sheets that make up MLCCs (Multi-Layer Ceramic Capacitors). MLCCs are a type of capacitor used to store electricity and stabilize current. They are widely used in portable electronic devices due to their small size and large capacitance, and their demand has increased significantly recently due to the popularity of smartphones and tablet PCs. Such MLCCs are completed by alternately laminating tens or hundreds of layers of green sheets and internal metal electrodes, and then connecting external electrodes, and their size varies from less than 1 mm to several nm.

[0004] The green sheets used in MLCCs are formed by uniformly applying a ceramic slurry to a carrier film support and then firing it. The carrier film used to form the green sheets is made of a biaxially oriented polyester film base material that has excellent mechanical strength, dimensional stability, heat resistance, and price competitiveness, and one side of the base material is a release film with a polymer silicone release layer applied to it.

[0005] Recently, due to the trend of miniaturization and high capacity of MLCC, there is a demand for further thinning of green sheets and lamination of ceramic slurries in more layers, but if the peel strength of the release film used in manufacturing MLCC is too low, the ceramic slurry may peel off the release film first. Conversely, if the peel strength of the release film is too high, cracks, breaks, etc. may occur in the green sheet when the release film is removed from the ceramic green sheet. Therefore, the release film used in MLCC is required to have physical properties that allow it to be peeled off with an appropriate peel strength.

[0006] In addition, if the organic solvent used in the production of the ceramic slurry does not volatilize sufficiently and remains in the release layer, orange peel-like stains appear on the surface of the green sheet, but this problem occurs when the release layer has low solvent resistance and the ceramic slurry solvent remains in the release layer in addition to being caused by roughness, and improvement was necessary. Preventing defects in the green sheet as described above leads to improved reliability of MLCCs, so the function of the release film is very important in the production of MLCCs. Summary of the Invention [Problem to be solved by the invention]

[0007] The present disclosure provides a technique for a release film. The present disclosure aims to provide a release film that can achieve a wide range of peeling forces and exhibit excellent stability over time. [Means for solving the problem]

[0008] In one aspect, the present disclosure can provide a release film.

[0009] In one aspect, the release film includes a base film; and a release layer formed by applying a release coating composition to at least one surface of the base film, and the release layer may be a release film that satisfies the following formula (1).

[0010] Formula (1)

[0011] 0.5≦P b / P a <= 10.0

[0012] P a : In the FT-IR spectrum, the wave number is 1450 cm -1 More than 1650cm -1 Maximum absorption peak intensity in the region below

[0013] P b : In the FT-IR spectrum, the wave number is 1650 cm -1 over 1850cm -1 Maximum absorption peak intensity in the following region

[0014] In one aspect, the release film can satisfy one or more of the following conditions (1) to (4).

[0015] conditions

[0016] (1) When a TESA 7475 tape is attached to the release layer of the release film and the peel strength is measured at a peel speed of 0.3 m / min at 180° peeling, the peel strength is 30 to 50 gf / in.

[0017] (2) When a TESA 7475 tape is attached to the release layer of the release film, and after 24 hours at room temperature, the peel strength at 180° peeling is measured at a peel speed of 0.3 m / min., the peel strength at room temperature for one day is 200 to 250 gf / in.

[0018] (3) When the peel strength of the release film is measured at a peel speed of 0.5 m / min at 90° peeling from the green sheet, the peel strength of the release film from the green sheet is 1 to 100 gf / in.

[0019] (4) RF 90 / RF1≧0.9 (where RF1 and RF 90are the peel strengths of the release film to the green sheet measured after storing the release film with the green sheet attached for 24 hours (1 day) and 90 days at room temperature of 23°C and humidity of 50%.

[0020] In one aspect, the silicon content in the release layer measured using an X-ray fluorescence (XRF) analyzer is 0.001 to 0.015 g / m 2 may be also possible.

[0021] In one aspect, the release film may have a residual adhesion rate of 94% or more.

[0022] In one aspect, the release layer may have a surface energy of 21 to 30 dyne / cm.

[0023] In one aspect, the release layer may have a residual amount of volatile organic compounds of 5 ppm or less.

[0024] In one aspect, the release coating composition may include a melamine component that is a melamine compound of Formula 1, an oligomer thereof, a polymer thereof, or a combination thereof; a polymer component that contains a polar functional group and has a weight average molecular weight of 3,000 to 30,000; and an acid catalyst.

[0025] [Chemical formula 1]

[0026] [ka]

[0027] (In the formula, X represents a hydrogen atom, -CHOH, or -CH-OR, and may be the same or different. R represents an alkyl group having 1 to 8 carbon atoms, and may be the same or different. At least one X is -CH-O-CH.)

[0028] In one aspect, the melamine component may have a total acid value of 390 to 780 mg KOH / g.

[0029] In one aspect, the polymer component may be one or more selected from the group consisting of polyesters, polyurethanes, polyvinyl resins, polyethylene terephthalates, acrylates, methacrylates, combinations thereof, and copolymers thereof.

[0030] In one aspect, the polymer component is a polyethylene terephthalate copolymer, which may be a copolymer including terephthalic acid; ethylene glycol; and one or more of isophthalic acid, diethylene glycol, monopropylene glycol, and cyclohexylene dimethanol.

[0031] In one aspect, the polar functional group may be one or more selected from the group consisting of a hydroxyl group, a carboxyl group, an amino group, an amine group, a carbonyl group, an acryl group, an acryloyl group, a nitrile group, a vinyl group, a halogen group, a urethane group, and an ester group.

[0032] In one aspect, the polymeric component may contain two or more polar functional groups that are different from each other.

[0033] In one aspect, the acid catalyst is hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, oxalic acid, nitric acid, formic acid, methanesulfonic acid, trifluoromethanesulfonic acid, isoprene sulfonic acid, camphorsulfonic acid, hexanesulfonic acid, octanesulfonic acid, nonanesulfonic acid, decane sulfonic acid, hexadecanesulfonic acid, dinonylnaphthalenesulfonic acid, dinonylnaphthalenedisulfonic acid, benzenesulfonic acid, alkylbenzenesulfonic acid, paratoluenesulfonic acid, melamine zinc iodide (melamine ZnI2), melamine trisulfonic acid (melamine trisulfonic acid), melamine iodide (melamine ZnI2), melamine trisulfonic acid ... acid;MTSA), cumene sulfonic acid, dodecylbenzene sulfonic acid, naphthalene sulfonic acid, nonylnaphthalene sulfonic acid, methyl acid phosphate, ethyl acid phosphate, propyl acid phosphate, isopropyl acid phosphate, butyl acid phosphate, butoxyethyl acid phosphate, octyl acid phosphate, 2-ethylhexyl acid phosphate, decyl acid phosphate, lauryl acid phosphate, stearyl acid phosphate, oleyl acid phosphate, behenyl acid phosphate, phenyl acid phosphate, nonylphenyl acid phosphate, cyclohexyl acid phosphate and the acid phosphate may be one or more selected from the group consisting of bisphenol A acid phosphate, phenoxyethyl acid phosphate, alkoxypolyethylene glycol acid phosphate, bisphenol A acid phosphate, dimethyl acid phosphate, diethyl acid phosphate, dipropyl acid phosphate, diisopropyl acid phosphate, dibutyl acid phosphate, dioctyl acid phosphate, di-2-ethylhexyl acid phosphate, dilauryl acid phosphate, distearyl acid phosphate, diphenyl acid phosphate, bisnonylphenyl acid phosphate sulfonium salt, benzothiazolium salt, ammonium salt, and phosphonium salt.

[0034] In one aspect, the weight ratio of the melamine component to the acid catalyst in the release coating composition may be 100:5 to 100:30, 100:10 to 100:20, or 100:10 to 100:15.

[0035] In one aspect, the release coating composition may comprise 0.2 to 1.0 wt % of a melamine component based on the total weight of the entire composition, or 0.01 to 5 wt % of a polymer component based on the total weight of the entire composition.

[0036] In one aspect, the weight ratio of the melamine component and the polymer component in the release coating composition may be 100:3 to 100:70 based on the solid content.

[0037] In one aspect, the release coating composition may further comprise one or more of an antistatic agent, a conductivity enhancer, a pH adjuster, a surfactant, and an antifouling agent.

[0038] In one aspect, the antistatic agent may be one or more selected from the group consisting of PEDOT, PEDOT:PSS, polyaniline, polypyrrole, quaternary ammonium salts, sulfonates, and phosphates.

[0039] In one aspect, the pH adjusting agent may be one or more selected from the group consisting of sodium hydroxide, potassium hydroxide, calcium hydroxide, and aqueous ammonia.

[0040] In one aspect, the surfactant may be a cationic surfactant, an anionic surfactant, an amphoteric surfactant, a nonionic surfactant, a silicone surfactant, a modified silicone surfactant, a fluorosurfactant, or a combination thereof.

[0041] In one aspect, the antifouling agent may be one or more selected from the group consisting of fluorine, fluorine-containing silane-based compounds, fluorine-containing organic compounds, and self-emulsifying silicones.

[0042] In one aspect, the antifouling agent is a self-emulsifying silicone, which may be a silicone monomer containing a hydroxyl group.

[0043] In one aspect, the release coating composition may include, based on the total weight of the entire composition, 0.1 to 30 wt % of an antistatic agent, 0.01 to 0.3 wt % of a pH adjuster, 0.05 to 0.2 wt % of a surfactant, or 0.1 to 0.3 wt % of an antifouling agent.

[0044] In one aspect, the release coating composition may further comprise an oxazoline-based curing agent.

[0045] In one aspect, the release coating composition includes water or a combination of water and an organic solvent, and the weight ratio of the water to the organic solvent may be 50:50 or more, 60:40 or more, 70:30 or more, 80:20 or more, 90:10 or more, 95:5 or more, or 99:1 or more.

[0046] In one aspect, the melamine component and the polymer component containing a polar functional group may form a crosslinked network structure with each other after curing.

[0047] In one aspect, the release film is used in pressure sensitive adhesives, semi-curable adhesives, ceramic sheets for multilayer ceramic capacitors, semi-curable resins for printed circuits, or prepregs. Effect of the Invention

[0048] The release film according to one aspect of the present disclosure can realize a wide range of peel strength during production of the release film and can exhibit excellent stability over time, and this effect is even better than that of a release film produced using a silicone-based release coating composition. [Brief description of the drawings]

[0049] [Figure 1a] 1 is a photograph relating to a first peeling test of a release film, and a diagram showing a method of the first peeling test. [Figure 1b] 1 is a photograph showing a result of a first peeling test of a release film. [Diagram 2] 1 is a graph showing the results of FT-IR spectrum measurement of a release film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0050] Various aspects or examples described in this document are exemplified for the purpose of clearly explaining the technical idea of ​​the present disclosure, and are not intended to limit it to a specific embodiment. The technical idea of ​​the present disclosure includes various modifications, equivalents, alternatives, and aspects or examples selectively combined from all or part of each aspect or example described in this document. In addition, the scope of the technical idea of ​​the present disclosure is not limited to the various aspects or examples presented below and the specific description thereof.

[0051] Terms used in this document, including technical or scientific terms, may have the meaning commonly understood by one of ordinary skill in the art to which this disclosure belongs, unless otherwise defined.

[0052] 1. Base film

[0053] In one aspect of the present disclosure, the base film constituting the release film can be a known film that is widely used in the field of conventional release films, and is not limited thereto.

[0054] In one aspect, the substrate film may be formed from a polyester-based polymer, but the substrate film to which the release coating composition is applied is not limited to a polyester-based film. Specifically, the polyester-based polymer may be, but is not limited to, a polyethylene terephthalate polymer, a polybutylene terephthalate polymer, a polyethylene naphthalate polymer, a polyphenylene sulfide polymer, a polyether ether ketone polymer, a polyphthalamide polymer, a polyimide polymer, a polysulfone polymer, a polyethersulfone polymer, a polyetherimide polymer, or a combination thereof.

[0055] In one aspect, the polyester-based polymer may be a polyester obtained by the condensation reaction of an aromatic dicarboxylic acid and an aliphatic glycol. In one aspect, the aromatic dicarboxylic acid may be, but is not limited to, isophthalic acid, phthalic acid, terephthalic acid, 2,6-naphthalenedicarboxylic acid, adipic acid, sebacic acid, an oxycarboxylic acid (e.g., p-oxybenzoic acid, etc.), or a combination thereof. In one aspect, the aliphatic glycol may be, but is not limited to, ethylene glycol, diethylene glycol, propylene glycol, butanediol, 1,4-cyclohexanedimethanol, neopentyl glycol, or a combination thereof.

[0056] In one aspect, the polyester polymer may be a combination of two or more of the aromatic dicarboxylic acids and aliphatic glycols, or a copolymer containing a third component, but in consideration of heat resistance, chemical resistance, mechanical strength, and economic efficiency, it may be more preferable to use polyethylene terephthalate. In another aspect, it may be more preferable to use a biaxially stretched polyethylene terephthalate film as the base film.

[0057] In one aspect, the substrate film may have a thickness of 10 to 200 μm, but is not limited thereto.

[0058] In one aspect, the release coating composition can be applied to at least one side of a substrate film to form a release layer.

[0059] In one aspect, the release coating composition may include a melamine component that is a melamine compound of Formula 1, an oligomer thereof, a polymer thereof, or a combination thereof; a polymer component that contains a polar functional group and has a weight average molecular weight of 3,000 to 30,000; and an acid catalyst.

[0060] [Chemical formula 1]

[0061] [ka]

[0062] (In the formula, X represents a hydrogen atom, -CHOH, or -CH-OR, and may be the same or different. R represents an alkyl group having 1 to 8 carbon atoms, and may be the same or different. At least one X is -CH-O-CH.)

[0063] 2. Melamine ingredients

[0064] In one aspect of the present disclosure, the release coating composition forming the release layer constituting the release film uses a melamine component as a main chain component constituting the release layer after curing, and when a melamine component is used, a hard release layer coating film can be obtained due to high crosslink density, and a level of hardness exceeding that of a silicone-based release coating composition can be achieved. This is because in the release film for the ceramic green sheet manufacturing process for manufacturing MLCC, it is effective to harden the release layer coating film in order to adjust the peel force to a desired level.

[0065] In one aspect, the melamine component is not particularly limited, but is generally produced by the reaction of melamine with formaldehyde, and the methylol melamine thus produced can be reacted with an alcohol having an appropriate carbon number under acid catalysis conditions to obtain an alkyl etherified melamine compound.

[0066] In one aspect, the melamine component may refer to a melamine compound having the structure of Formula 1 below, an oligomer thereof, a polymer thereof, and / or a combination thereof.

[0067] [Chemical formula 1]

[0068] [ka]

[0069] Here, X represents a hydrogen atom, -CH2OH, or -CH2-OR, and may be the same or different. R represents an alkyl group having 1 to 8 carbon atoms, and may be the same or different. At least one X may be -CH2-O-CH3.

[0070] In one aspect, all of the X's may be -CH2-O-CH3, and the melamine component may be a full ether type methylated melamine, a melamine oligomer and / or a melamine polymer.

[0071] In one aspect, various commercially available and widely used products can be used as the melamine component, such as, but not limited to, Cymel 300, Cymel 301, Cymel 303LF, Cymel 350, or Cymel 370N (all products of Allnes Corporation). Commercially available products can be used alone or in combination of two or more.

[0072] In one aspect, the content of the melamine component may be about 0.2 to about 1.0 wt% based on the total weight of the entire composition, specifically about 0.2 to about 0.8 wt%, about 0.3 to about 0.7 wt%, about 0.4 to about 0.6 wt%, or about 0.5 to about 0.6 wt%. If the melamine component is used too little below the minimum value, the desired hardening effect, i.e., the effect of maintaining the release layer hard and reducing the peeling force of the green sheet of the release film, may be weakened, and the peeling force may not be adjusted as desired. In addition, if the melamine hardening is not performed properly, the stability over time of the release film may decrease, so the content of the melamine component should satisfy the content ratio with the acid catalyst mentioned below.

[0073] In one aspect, the total acid number of the melamine component may be 390 to 780 mgKOH / g, specifically, 400 KOH / g or more, 450 KOH / g or more, 500 KOH / g or more, 550 KOH / g or more, 600 KOH / g or more, 650 KOH / g or more, 700 KOH / g or more, or 750 KOH / g or more, or 730 KOH / g or less, 680 KOH / g or less, 630 KOH / g or less, 580 KOH / g or less, 530 KOH / g or less, 480 KOH / g or less, or 430 KOH / g or less, but is not limited thereto.

[0074] 3. Polymer component

[0075] In one aspect of the present disclosure, the polymer component may be used as a binder or release force modifier in the release coating composition. Since the molecular weight of the monomer of the melamine component is low, it forms a fine crosslinked structure after curing and has a high crosslink density. However, if a polymer component having a relatively large molecular weight and a long chain structure is cured together, the polymer having a long chain structure is bonded between the fine crosslinked structures of the melamine component, and the hardness is relieved, so that the softness of the release layer can be increased. As the softness increases, the release force of the release film also increases, and the present disclosure has the effect of achieving a wide range of release forces, particularly a wide range of release forces of green sheets, by combining the melamine component and the polymer component.

[0076] The melamine component may have a total of up to 6 functional groups. The polymer component bonds between the melamine components so that the melamine components cannot bond to each other, and a long chain structure may form a coarse crosslinked network structure, and the formed melamine component-polymer component copolymer and this structure may increase the softness of the release layer and increase the stability over time.

[0077] Generally, in a silicone-based release film, a silicone polymer component is added to increase the release force, but if the content of the silicone polymer component exceeds 50 wt % based on the total weight of the entire composition, serious problems occur in stability over time. This is because the silicone polymer component that should be present on the surface of the release layer is impregnated into the inside of the release layer over time. Unlike conventional silicone-based release films, the release coating composition of the present disclosure is a copolymer of the melamine component and the polymer component as described above, forming a crosslinked network structure, so that the functional group exhibiting releasability can be continuously maintained without being impregnated from the surface of the release layer into the inside, thereby exhibiting excellent stability over time.

[0078] In one aspect, the polymer component is not limited as long as it is a polymer having a long chain structure and is bonded with the melamine component to form a crosslinked network structure and provide softness. For example, the polymer component may be one or more selected from the group consisting of polyester, polyurethane, polyvinyl resin, polyethylene terephthalate, acrylate, methacrylate, combinations thereof, and copolymers thereof, but is not limited thereto. Here, the polyethylene terephthalate copolymer (co-PET) is not limited as long as it is a copolymer having polyethylene terephthalate as the main repeating unit, but may be, for example, a copolymer containing terephthalic acid; ethylene glycol; and one or more of isophthalic acid, diethylene glycol, monopropylene glycol, and cyclohexylene dimethanol.

[0079] In one aspect, the polymer component may contain a polar functional group, or may contain two or more different polar functional groups.

[0080] In one aspect, the polar functional group is not limited as long as it can react with the functional group present in the melamine component to form a crosslinking bond, for example, the polar functional group may be one or more selected from the group consisting of a hydroxyl group, a carboxyl group, an amino group, an amine group, a carbonyl group, an acryl group, an acryloyl group, a nitrile group, a vinyl group, a halogen group, a urethane group, and an ester group, but is not limited thereto.

[0081] In one embodiment, the polymer component may have a weight average molecular weight of about 3,000 to about 30,000, about 5,000 to about 30,000, about 8,000 to about 30,000, about 10,000 to about 30,000, about 10,500 to about 30,000, about 10,500 to about 20,000, about 11,000 to about 15,000, about 11,000 to about 14,000, about 11,000 to about 13,000, or about 11,000 to about 12,000. The higher the weight average molecular weight of the polymer component, the greater the softness of the release layer after curing.

[0082] In one embodiment, the content of the polymer component may be 0.01 to 5 wt%, 0.1 to 4 wt%, 1 to 3.5 wt%, 1.5 to 3 wt%, or 2 to 3 wt% based on the total weight of the entire composition. If the polymer component is used in an excessive amount exceeding the above maximum value, the melamine component cannot be cured sufficiently, and the uncured polymer component or melamine component rises to the surface of the release layer, so that the rub-off characteristics of the release film (i.e., the adhesive strength or adhesion of the release layer to the base film) may be poor. If the polymer component is used too little below the above minimum value, the crosslinked network structure due to the curing reaction may not be sufficiently formed, and the desired release force or stability over time may not be achieved.

[0083] 4. Acid Catalyst

[0084] In one aspect, the acid catalyst is not limited as long as it is known to catalyze the crosslinking reaction of the melamine component or the crosslinking reaction of the melamine component and the polymer component, and can be appropriately selected and used.For example, the acid catalyst may be an inorganic acid such as hydrochloric acid, sulfuric acid, nitric acid, or phosphoric acid; an acid catalyst may be an inorganic acid such as oxalic acid, nitric acid, formic acid, methanesulfonic acid, trifluoromethanesulfonic acid, isoprene sulfonic acid, camphorsulfonic acid, hexanesulfonic acid, octanesulfonic acid, nonanesulfonic acid, decane sulfonic acid, hexadecanesulfonic acid, dinonylnaphthalenesulfonic acid, dinonylnaphthalenedisulfonic acid, benzenesulfonic acid, alkylbenzenesulfonic acid, paratoluenesulfonic acid, melamine zinc iodide (melamine ZnI2), melamine trisulfonic acid (melamine trisulfonic acid), acid;MTSA), cumene sulfonic acid, dodecylbenzene sulfonic acid, naphthalene sulfonic acid, nonylnaphthalene sulfonic acid, methyl acid phosphate, ethyl acid phosphate, propyl acid phosphate, isopropyl acid phosphate, butyl acid phosphate, butoxyethyl acid phosphate, octyl acid phosphate, 2-ethylhexyl acid phosphate, decyl acid phosphate, lauryl acid phosphate, stearyl acid phosphate, oleyl acid phosphate, behenyl acid phosphate, phenyl acid phosphate, nonylphenyl acid phosphate, cyclohexyl acid phosphate, phenoxy Organic acids such as ethyl acid phosphate, alkoxy polyethylene glycol acid phosphate, bisphenol A acid phosphate, dimethyl acid phosphate, diethyl acid phosphate, dipropyl acid phosphate, diisopropyl acid phosphate, dibutyl acid phosphate, dioctyl acid phosphate, di-2-ethylhexyl acid phosphate, dilauryl acid phosphate, distearyl acid phosphate, diphenyl acid phosphate, bisnonylphenyl acid phosphate, etc.; thermal acid generators such as sulfonium salts, benzothiazolium salts, ammonium salts, phosphonium salts, etc. can be used, but are not limited thereto. The acid catalyst component can be used alone or in combination of two or more.

[0085] In one aspect, the weight ratio of the melamine component to the acid catalyst may be 100:5 to 100:30, 100:10 to 100:20, or 100:10 to 100:15, or may be a weight ratio between the upper and lower limits described above. If the content of the acid catalyst is used too low below the minimum value of the weight ratio, the curing reaction may not occur sufficiently, and if it is used in an excessive amount exceeding the maximum value, over-curing may occur, and in both cases, poor stability over time may result. Therefore, in order to achieve excellent stability over time, it is better for the weight ratio of the melamine component to the acid catalyst to satisfy the above range.

[0086] 5. Solvent

[0087] In one aspect, the release coating composition may be a water-based release coating composition. In one aspect, water-based can mean an aqueous solution or dispersion, and can mean that the solvent component of the composition is water alone or a combination of water and an organic solvent, as described below.

[0088] In one aspect, since the aqueous release coating composition is aqueous-based, when forming a release layer, it can drastically reduce the emission of volatile organic compounds (VOCs) and meet the requirements for environmental friendliness. Furthermore, it can be easily used by mixing with aqueous additives such as aqueous antistatic agents, and has the advantage that both antistatic properties and releasability of the release film can be achieved with a one-component liquid preparation.

[0089] In one aspect, the release coating composition may further comprise an aqueous solvent. The aqueous solvent may be water or a combination of water and an organic solvent. The mixing ratio of the water to the organic solvent may be 50:50 or more, 60:40 or more, 70:30 or more, 80:20 or more, 85:15 or more, 90:10 or more, 95:5 or more, or 99:1 or more by weight.

[0090] In one aspect, the organic solvent may be a known organic solvent widely used in the field of release films, and is not particularly limited as long as it is a solvent that is compatible with water. For example, the organic solvent may be one or more selected from the group consisting of isopropyl alcohol, isobutyl alcohol, hexane, acetone, ethyl acetate, ethylene glycol, propylene glycol, butyl glycol, dipropylene glycol, polyethylene glycol, gamma-butyrolactone, and combinations thereof, but is not limited thereto.

[0091] 6. Other Ingredients

[0092] In one aspect, the release coating composition may further include one or more of an antistatic agent, a conductivity enhancer, a pH adjuster, a surfactant, and an antifouling agent, as long as the physical properties (e.g., frame) of the release layer to be achieved are not changed.

[0093] (1) Antistatic agents and conductivity enhancers

[0094] In one aspect of the present disclosure, the antistatic agent not only imparts antistatic properties to the release layer, but also has the effect of preventing the adsorption of foreign matter. The ceramic green sheet manufacturing process includes a process of cutting and slicing the ceramic green sheet, and since the ceramic green sheet is in the form of an accumulation of beads like grains, the beads fall off during the cutting process of the green sheet. Therefore, the antistatic property can prevent the beads from falling off due to static electricity during the process of cutting the release film together with the ceramic green sheet, thereby contributing to the processability of the ceramic green sheet manufacturing process.

[0095] In one aspect, the antistatic agent may be a known antistatic agent widely used in the field of release films, and is not particularly limited.For example, the antistatic agent may be selected from the group consisting of PEDOT (Poly(3,4-ethylenedioxythiophene)), PEDOT:PSS (poly(3,4-ethylenedioxythiophene) polystyrene sulfonate), polyaniline, polypyrrole, quaternary ammonium salts, sulfonates, and phosphates, but is not limited thereto.

[0096] In one aspect, the antistatic agent may be included in the release coating composition in the form of an aqueous solution containing an antistatic agent component that is a solid content (the solid content may be 1.0% to 2.0% or 1.5% to 2.0%), and in this case, the content of the aqueous solution containing the antistatic agent may be about 0.1 to about 30 wt%, about 1 to about 25 wt%, or about 5 to about 20 wt% based on the total weight of the entire composition, and may be a content that exists between the upper and lower limits described above. If the content of the antistatic agent is used in an excessive amount exceeding the maximum value, it may induce defects in the appearance of the release layer, and such defects may be seen as blue spots.

[0097] In one aspect, the antistatic agent is contained in the above amount, and can impart a surface resistance of about 10^4 to 10^10 ohm / sq to the release layer.

[0098] In one aspect, the release coating composition further includes a conductivity enhancer to achieve a desired level of surface resistance, i.e., antistatic performance. Such a conductivity enhancer can play a role in supporting the performance of the antistatic agent, and by using the conductivity enhancer, a desired level of surface resistance of the release layer can be achieved even with a smaller amount of the antistatic agent.

[0099] In one aspect, the content of the conductivity enhancer may be about 1 to 20 wt%, about 1 to 15 wt%, about 1 to 10 wt%, about 1 to 8 wt%, about 1.5 to 8 wt%, about 1.5 to 6 wt%, about 2 to 6 wt%, about 2.5 to 6 wt%, about 3 to 6 wt%, or about 4 to 6 wt% based on the total weight of the entire composition. If the content of the conductivity enhancer is used in an excessive amount exceeding the above maximum value, it may hinder the curing of the release layer, and the appearance and rub-off properties of the release layer may not be achieved to a desired level, and if the content of the conductivity enhancer is used too little below the above minimum value, the effect may be insufficient.

[0100] In one aspect, the conductivity enhancer may be a known conductivity enhancer that has been widely used in the field of release films, and is not particularly limited. For example, the conductivity enhancer may be selected from the group consisting of ethylene glycol, dimethyl sulfoxide, N-methyl-2-pyrrolidone, propylene glycol, butyl glycol, dipropylene glycol dimethyl ether, gamma-butyrolactone, sulfolane, dimethyl carbonate, and sorbitol, but is not limited thereto.

[0101] (2) pH adjuster

[0102] In one aspect of the present disclosure, the pH adjuster can adjust the pH of the entire composition to a desired level. The release coating composition may contain an antistatic agent that exhibits acidity, and if the composition becomes acidic, neutral or basic components such as surfactants or polymer components may not function sufficiently, so in this case, pH adjustment is necessary. If the pH of the entire release coating composition is not adjusted, the stability of the composition itself over time may rapidly deteriorate, and the appearance of the release layer may deteriorate depending on the time elapsed after the composition is prepared. For example, when the release coating composition is prepared and immediately applied to a substrate film to form a release layer, the appearance of the release layer is good, but when the release layer is formed about 4 hours after preparation, the appearance of the release layer may become mottled.

[0103] In one aspect, the pH adjuster may be a known pH adjuster widely known in the field of release films, and is not particularly limited.For example, the pH adjuster may be one or more selected from the group consisting of sodium hydroxide, potassium hydroxide, calcium hydroxide, and aqueous ammonia, but is not limited thereto.The pH adjuster may be a basic pH adjuster.

[0104] In one aspect, the content of the pH adjuster may be 0.05 to 0.3 wt %, 0.1 to 0.3 wt %, or 0.15 to 0.25 wt % based on the total weight of the entire composition, and may be a content between the upper and lower limits described above. If the pH adjuster is used in an excessive amount exceeding the maximum value, it may interfere with the curing of the release layer.

[0105] (3) Surfactants

[0106] In one aspect of the present disclosure, the surfactant may improve the wetting property or the coatability of the release coating composition to the substrate film, and may improve the compatibility of the melamine component and the polymer component. In one aspect, when water is used as the sole solvent in the aqueous release coating composition, two or more different surfactants may be used.

[0107] In one aspect, the surfactant may be a component capable of lowering the surface tension as a known surfactant widely known in the field of release films, and is not particularly limited. For example, the surfactant may be a cationic surfactant, an anionic surfactant, an amphoteric surfactant, a nonionic surfactant, a silicon-based surfactant, a modified silicon-based surfactant, a fluorine-based surfactant, or a combination thereof, but is not limited thereto.

[0108] In one aspect, the cationic surfactant can be, for example, but not limited to, an alkyltrimethylammonium salt, a dialkyldimethylammonium salt, or an alkylbenzyldimethylammonium salt.

[0109] In one aspect, the anionic surfactant may be, for example, but not limited to, a fatty acid salt, an alkylbenzene sulfonate, an alkyl sulfonate, an alkyl ether sulfonate ester salt, an alkyl polyoxyethylene sulfonate, or a monoalkyl phosphate.

[0110] In one aspect, the amphoteric surfactant can be, for example, but not limited to, an alkyl dimethylamine oxide, or an alkyl carboxybetaine.

[0111] In one aspect, the nonionic surfactant may be, for example, but is not limited to, fatty acid ethanolamide, polyoxyethylene alkyl ether, polyoxyethylene alkylphenyl ether, sorbitol, sorbitan, sorbitan fatty acid ester, polyoxyethylene sorbitan fatty acid ester, polyoxyethylene fatty acid ester, glycerin fatty acid ester, propylene glycol fatty acid ester, or polyoxyalkylene modified silicones.

[0112] In one aspect, the silicone surfactant may be, for example, but not limited to, polyether-modified silicone or polyglycerin-modified silicone. The structure of such modified silicone may be classified into side chain modified type, both end modified type (ABA type), one end modified type (AB type), both end side chain modified type, linear block type (ABn type), branched type, etc., and modified silicone of any of these structures may be used.

[0113] In one aspect, the content of the surfactant may be 0.05 to 0.2 wt %, 0.1 to 0.2 wt %, or 0.15 to 0.2 wt % based on the total weight of the entire composition, and may be a content between the upper and lower limits described above.

[0114] (4) Antifouling agents

[0115] In one aspect of the present disclosure, the antifouling agent can adjust the surface energy of the release layer to impart antifouling properties. If the difference in surface energy between the substrate film and the release layer is small, the wettability and peelability of the release layer to the substrate film may decrease, but the antifouling agent can reduce the surface energy of the release layer to prevent this. Furthermore, since the melamine component contained in the release coating composition of the present disclosure has almost no slip property (sliding property), the antifouling agent can impart slip property to the release layer.

[0116] In one aspect, the antifouling agent may be one or more selected from the group consisting of fluorine, fluorine-containing silane-based compounds, fluorine-containing organic compounds, and self-emulsifying silicones, but is not limited thereto. In one aspect, the self-emulsifying silicones may be silicone monomers containing one or more hydroxyl groups, but is not limited thereto.

[0117] In one aspect, the content of the antifouling agent may be 0.1 to 0.3 wt%, 0.15 to 0.25 wt%, or 0.2 to 0.25 wt% based on the total weight of the entire composition, and may be a content between the upper and lower limits described above. If the content of the antifouling agent is excessively less than the minimum value, problems may occur in which stain marks remain when the release film is peeled off, and problems may occur in which green sheet slurry particles remain on the release layer after the release film is peeled off from the green sheet.

[0118] (5) Oxazoline-based curing agents

[0119] In one aspect of the present disclosure, the oxazoline-based curing agent can induce a curing reaction of a polar functional group of a polymer component, for example, a carboxy group, an aromatic thiol group, or a phenol group, and thus can improve the rub-off property or solvent resistance of the release film. Specifically, the polar functional group present in the polymer component may have a lower priority in curing than the curing between the hydroxyl groups involved in the bond between the melamine components or the curing between the hydroxyl groups of the melamine component and the silicon component (e.g., self-emulsifying silicon) contained in the release coating composition, and therefore the polar functional group of the polymer component may not be able to fully participate in the curing reaction. In this case, the polymer component containing the polar functional group exists on the cured structure composed of melamine-melamine or melamine-silicon with a weak binding force of about the van der Waals force, which may cause a problem of weakened solvent resistance of the release layer. When an oxazoline-based curing agent is used, the polar functional group can be made to participate in the curing reaction, and thus a crosslinked body between the polymer components or a crosslinked body between the polymer component and the melamine component is further formed, thereby improving the rub-off property or solvent resistance of the release film.

[0120] In one aspect, the oxazoline-based curing agent may be a compound or polymer containing an oxazoline group, and may be any known component that is widely used in the field of release films without any particular limitation. Examples of oxazoline-based curing agent-containing monomers that can be used for the preparation of the oxazoline-based curing agent include, but are not limited to, 2-vinyl-2-oxazoline, 2-vinyl-4-methyl-2-oxazoline, 2-vinyl-5-methyl-2-oxazoline, 2-isopropenyl-2-oxazoline, 2-isopropenyl-4-methyl-2-oxazoline, 2-isopropenyl-5-ethyl-2-oxazoline, or combinations thereof. Examples of other monomers that can be used for the preparation of the oxazoline-based curing agent include, but are not limited to, any monomer that can form a copolymer with the above-mentioned oxazoline-based curing agent, and may be, but are not limited to, alkyl (meth)acrylate, acrylic acid, methacrylic acid, ethylene, propylene, vinyl chloride, or styrene.

[0121] In one aspect, commercially available oxazoline curing agents may include, but are not limited to, products of Nippon Shokubai Co., Ltd. under the names WS-300, WS-500, WS-700, K-2010E, K2020E, K2030E, or RPS-1005.

[0122] 7. Properties of release film

[0123] In one aspect of the present disclosure, a release film may be prepared by applying a release coating composition to at least one surface of a substrate film to form a release layer, and the release film thus prepared may have the following physical properties. The following physical properties may be measured by the methods described in the experimental examples.

[0124] In one aspect, the release layer constituting the release film can satisfy the following formula (1).

[0125] Formula (1)

[0126] 0.5≦P b / P a <= 10.0

[0127] P a : In the FT-IR spectrum, the wave number is 1450 cm -1 More than 1650cm -1 Maximum absorption peak intensity in the region below

[0128] P b : In the FT-IR spectrum, the wave number is 1650 cm -1 over 1850cm -1 Maximum absorption peak intensity in the following region

[0129] The FT-IR spectrum of the release layer can be measured by the method described in Experimental Example 8.

[0130] P b / P aThe value is not particularly limited as long as it satisfies the above range, but may be, for example, 0.55 or more, or 0.6 or more, or 9.95 or less, or 9.9 or less, or 9.85 or less, or 9.8 or less, or 9.75 or less, or 9.7 or less, or 9.65 or less, or 9.6 or less.

[0131] P b is a peak due to a polar functional group contained in the polymer component, and a is a peak due to NCN bending of the melamine component, and b / P a When the value is within the above range, the release film exhibits excellent stability over time and can achieve a wide range of peel strength of the green sheet through the inclusion of a polymer component containing a polar functional group and melamine. In addition, the release film can achieve excellent residual adhesion rate and stability over time while increasing the peel strength of the green sheet. b / P a If the value exceeds 10.0, the content of the polymer component containing a polar functional group (eg, co-PET) becomes too high, and residues may remain when the green sheet is peeled off, making complete transfer difficult.

[0132] In one aspect, the release film may satisfy one or more of the following conditions (1) to (4).

[0133] conditions

[0134] (1) When a TESA 7475 tape is attached to the release layer of the release film and the peel strength is measured at a peel speed of 0.3 m / min at 180° peeling, the peel strength is 30 to 50 gf / in.

[0135] (2) When a TESA 7475 tape is attached to the release layer of the release film, and after 24 hours at room temperature, the peel strength at 180° peeling is measured at a peel speed of 0.3 m / min., the peel strength at room temperature for one day is 200 to 250 gf / in.

[0136] (3) When the peel strength of the release film is measured at a peel speed of 0.5 m / min at 90° peeling from the green sheet, the peel strength of the release film from the green sheet is 1 to 100 gf / in.

[0137] (4) RF 90 / RF1≧0.9 (where RF1 and RF 90 are the peel strengths of the release film to the green sheet measured after storing the release film with the green sheet attached for 24 hours (1 day) and 90 days at room temperature of 23°C and humidity of 50%.

[0138] In one aspect, the release film may exhibit a tape immediate peel force of 30 to 50 gf / in, or may exhibit a peel force of a value between the upper and lower limits described above, for example, 32 gf / in or more, 34 gf / in or more, 36 gf / in or more, 38 gf / in or more, 40 gf / in or more, 42 gf / in or more, 44 gf / in or more, 46 gf / in or more, or 48 gf / in or more, or 48 gf / in or less, 46 gf / in or less, 44 gf / in or less, 42 gf / in or less, 40 gf / in or less, 38 gf / in or less, 36 gf / in or less, 34 gf / in or less, or 32 gf / in or less.

[0139] In one aspect, the release film may have a tape room temperature peel strength of 200 to 250 gf / in after 1 day, or may have a peel strength between the upper and lower limits described above, for example, 210 gf / in or more, 220 gf / in or more, 230 gf / in or more, or 240 gf / in or more, or 240 gf / in or less, 230 gf / in or less, 220 gf / in or less, or 210 gf / in or less. Such a release film satisfies the peel strength of a heavy or extra heavy release release film and can be used in a variety of fields that require this.

[0140] In one aspect, the release film may exhibit a peel strength of the green sheet of 1 to 100 gf / in, 4 to 98 gf / in, 10 to 70 gf / in, 20 to 60 gf / in, or 20 to 50 gf / in, or may exhibit a peel strength between the upper and lower limits described above. The peel strength of the green sheet may be measured by the method described in Experimental Example 1, and may exhibit a peel strength for a green sheet having a thickness of 3 μm. In one aspect, the release film exhibits a wide peel strength for the green sheet, and this range corresponds to a physical property that cannot be achieved by conventional silicone release films. In particular, in order to achieve a peel strength of at least 4 gf / in for a green sheet having a thickness of 3 μm, a large amount of silicone resin must be added to the silicone release film to increase the peel strength. In this case, if the content of the silicone resin exceeds 50 wt % based on the total weight of the release coating composition, serious problems may occur in terms of stability over time, as described above. Therefore, the release film according to one aspect of the present disclosure or the release coating composition used to produce such a release film has the advantage that it can be used in a very diverse range of industrial fields because it exhibits excellent stability over time and can achieve a wide range of green sheet peel strengths by combining a melamine component and a polymer component.

[0141] For example, when manufacturing MLCCs for IT, the green sheet thickness is about 2.3 μm or less, for high quality MLCCs, a green sheet with a thickness of about 0.6 to 0.8 μm is used, and when manufacturing MLCCs for industrial / electrical equipment, a green sheet with a thickness of about 3 μm or more may be used. If the thickness of the green sheet is low, the peeling force of the green sheet itself is high, and if the thickness is high, the peeling force of the green sheet itself is low. Therefore, the thicker the green sheet, the greater the need for a release film with a high level of peeling force.

[0142] However, in the case of conventional release films, it is difficult to achieve a peel strength of 4 gf / in or more based on a green sheet having a thickness of 3 μm, and even if the peel strength is increased, there is a problem that the stability over time is significantly reduced in the process of increasing the peel strength. In contrast, the release film according to one aspect of the present disclosure can have excellent stability over time while exhibiting a peel strength of 1 to 100 gf / in from a green sheet.

[0143] Therefore, the release film according to one aspect of the present disclosure has the advantage of being able to realize a certain range of heavy release force based on the immediate tape peel force or the room temperature tape peel force after 1 day while realizing various green sheet peel strength grades, and therefore one release film can be used as a release film for manufacturing green sheets for various purposes, and can also be used in industrial fields that require heavy release force based on the tape peel strength, so it can be used for various purposes. That is, the release force of a conventional release film for a green sheet is inversely proportional to the thickness of the green sheet, and there are limitations to its control, but the release film according to one aspect of the present disclosure can be used to achieve a desired release force even when the thickness of the green sheet is various by adjusting the ratio of the melamine component and the polymer component, or by adjusting the P ratio. b / P a By adjusting the range, it is possible to have a peel force of the green sheet in a variety of ranges (i.e., 1 to 100 gf / in) required in various industrial fields without being restricted by thickness. Therefore, the release film according to one aspect of the present disclosure can be used in various industrial fields by satisfying all of the various ranges of peel force required according to the thickness range of the green sheet used in various industrial fields.

[0144] In one aspect, the release film has an RF of 0.9 or more, 0.91 or more, 0.92 or more, 0.93 or more, 0.94 or more, 0.95 or more, 0.96 or more, 0.97 or more, or 0.98 or more, or an RF of 1.2 or less, 1.18 or less, 1.16 or less, 1.14 or less, 1.12 or less, 1.10 or less, 1.08 or less, 1.06 or less, 1.04 or less, or 1.08 or less. 90 / RF1, and the RF value lying between the upper and lower limits described above. 90It may also indicate the value of / RF1. 90 The value of / RF1 may be measured by the method described in Experimental Example 1, and may indicate stability over time for a 3 μm thick green sheet through the rate of change over time of the peel force of the green sheet after 90 days. In one aspect, the release film exhibits excellent stability over time, and this range corresponds to physical properties that cannot be achieved from conventional silicone release films. Thus, the release film according to one aspect of the present disclosure or the release coating composition used to manufacture such a release film has the advantage that it can be used in a very diverse range of industrial fields because it exhibits excellent stability over time and can achieve a wide range of green sheet peel forces by combining a melamine component and a polymer component.

[0145] In one aspect, the release film has a release layer with a silicon content of about 0.001 to about 0.015 g / m2 as measured using an X-ray fluorescence analyzer. 2 may be also possible.

[0146] In one aspect, the release film may exhibit a residual adhesion rate of about 94%, about 95%, or about 96% or more, and the residual adhesion rate may be measured by the method described in Experimental Example 4. In general, in the process of peeling off the release film, an adhesive such as a pressure sensitive adhesive (PSA) or an optically clear adhesive (OCA) is applied onto the release film, and then the release film is peeled off. However, in this process of peeling off the release film, a problem may occur in which uncured components present in the release layer of the release film are transferred and interfere with the adhesive properties of the adhesive. The release film of the present disclosure has an advantage that it can be used in fields where high standards are required because it satisfies a residual adhesion rate of about 95% or more.

[0147] In one aspect, the release film may have a surface energy of about 21 to about 30 dyne / cm or about 25 to about 27 dyne / cm, or may have a surface energy value between the upper and lower limits described above. The surface energy of the release layer may be measured by the method described in Experimental Example 5.

[0148] In one aspect, the release film may have a residual amount of volatile organic compounds of about 5 ppm or less, which allows it to be utilized as an environmentally friendly material.

[0149] In one aspect, the release film may be used in pressure sensitive adhesives, semi-curable adhesives, ceramic sheets for multilayer ceramic capacitors, semi-curable resins for printed circuits, or prepregs.

[0150] 8.Release film manufacturing method

[0151] In one aspect of the present disclosure, the method for producing a release film is not particularly limited as long as it is a method for forming a release layer using a release coating composition. For example, the release coating composition is applied to at least one surface of a substrate film, and the coating is heated and dried to harden the melamine component and the polymer component contained in the release coating composition to form a release layer, thereby obtaining a release film.

[0152] In one aspect, the method of applying the release coating composition may be a known method widely used in the field of release films, such as, but not limited to, gravure coating, bar coating, spray coating, spin coating, knife coating, roll coating, die coating, in-line coating, off-line coating, and the like.

[0153] In one aspect, the applied release coating composition may be thermally cured by drying by heating, and in this case, the heating temperature may be 110° C. to 160° C., 120° C. to 160° C., 130° C. to 160° C., 140° C. to 160° C., 150° C. to 160° C., 145° C. to 155° C., or 150° C. to 155° C., or may be a temperature within the range described above. In one aspect, the heating time may be 5 seconds to 60 seconds, 10 seconds to 40 seconds, 15 seconds to 30 seconds, or 20 seconds to 25 seconds, or may be a time within the range described above.

[0154] In one aspect, a post-curing process may be additionally included to cure the uncured components after the heat drying of the release coating composition. For example, the post-curing process may involve winding the release film produced by heat drying into a roll and treating it at 40°C to 60°C for 1 to 5 days. The treatment temperature may be 40°C to 60°C, 45°C to 55°C, 47°C to 53°C, 49°C to 53°C, 50°C to 53°C, or 50°C to 51°C, and the treatment time may be 1 to 5 days, 1.5 to 4.5 days, 2 to 4 days, 2.5 to 3.5 days, or 3 to 3.5 days. When the post-curing process is performed, the stability over time of the physical properties (e.g., peel strength, residual adhesion rate, or rub-off property) of the release film is improved.

[0155] In one aspect, the release layer of the release film can be formed to a dry thickness of 0.01 to 2 μm, or 50 nm to 500 nm.

[0156] The present disclosure will be further clarified through the above-mentioned aspects and the following experimental examples or examples. Hereinafter, the present disclosure will be described in detail through the examples described with reference to the attached tables so that those skilled in the art can easily understand and realize the present disclosure. However, these experimental examples or examples are provided to exemplify the present disclosure, and the scope of the present disclosure is not limited to these experimental examples or examples.

[0157] [Example]

[0158] 1. Preparation of release coating composition

[0159] The following components were mixed to prepare release coating compositions, with the exception that the content of the co-PET compound corresponding to the polymer component was different based on 100 parts by weight of the melamine component according to Table 1.

[0160] - Melamine component (manufacturer: Allnex, product name: CYMEL(R) 303 LF Resin) 0.5% by weight

[0161] - Polymer component (co-PET compound: a compound made by mixing 52% by weight of terephthalic acid, 45% by weight of ethylene glycol, and 3% by weight of isophthalic acid, with a solid content of 25% by weight, and added in the form of a liquid containing 70% by weight of water and 5% by weight of isopropyl alcohol)

[0162] - Melamine catalyst (manufacturer: Allnex, product name: Cymel(R) 4040 Catalyst) 0.06% by weight

[0163] - PEDOT aqueous solution (manufacturer: Heraus, product name: Clevios PT2) 20% by weight

[0164] - 9% ammonia water (manufacturer: Doksan Pharmaceutical Co., Ltd.) 0.05% by weight

[0165] - Surfactant (manufacturer: BYK, product name: BYK348) 0.01% by weight

[0166] - Antifouling agent (manufacturer: Silicone DNA, product name: SD3667) 0.2% by weight

[0167] - Distilled water remaining

[0168] 2.Production of release film

[0169] The release coating composition thus produced was applied to at least one side of a 50 μm thick polyethylene terephthalate substrate film (manufacturer: Toray Advanced Materials, product name: XD500) using a bar coater, and then the composition was heated and dried in a hot air dryer at 150° C. for 30 seconds to harden the film, producing a release film having a release layer formed on the substrate.

[0170] [Comparative Example]

[0171] 1. Preparation of release coating composition

[0172] The release coating compositions were prepared in the same manner as in the Examples, but in Comparative Example 1, the polymer component (co-PET compound) was omitted, and in Comparative Examples 2 to 5, an existing controlled release additive (CRA) (Shin-Etsu Co., Ltd., product name: X-62-185) was added in the amount of 50%, 20%, 40%, and 60% based on the melamine component, respectively, instead of the polymer component.

[0173] 2.Production of release film

[0174] A release film having a release layer formed thereon was prepared using the release coating composition of the comparative example in the same manner as in the above example.

[0175] [Experimental Example 1] Measurement of peel strength and stability over time of green sheet

[0176] A ceramic slurry was produced by adding 69 parts by mass of toluene and 46 parts by mass of ethanol to 50 parts by mass of barium titanate (BaTiO3; manufactured by Sakai Chemical Industry Co., Ltd., product name: BT-03), 5 parts by mass of polyvinyl butyral (manufactured by Sekisui Chemical Co., Ltd., product name: S-LEC B·KBM-2), and 2 parts by mass of dioctyl phthalate (manufactured by Kanto Chemical Co., Ltd., product name: dioctyl phthalate grade 1). The mixture was mixed and dispersed in a ball mill.

[0177] In the examples and comparative examples, the ceramic slurry was uniformly applied to the surface of the release layer of the release film that had been stored at room temperature for 48 hours after production using an applicator. The release film was then dried in a dryer at 80°C for 1 minute. Finally, a ceramic green sheet with a thickness of 3 μm was obtained on the release film, and a release film with a ceramic green sheet attached was produced.

[0178] The release film with the ceramic green sheet attached was stored for 24 hours and 90 days under conditions of room temperature of 23°C and humidity of 50%. After that, an acrylic adhesive tape (manufactured by Nitto Denko Corporation, product name: 31B tape) was attached to the surface of the ceramic green sheet opposite to the release film, and in this state, it was cut to a width of 25 mm to be used as a measurement sample.

[0179] The adhesive tape side of the measurement sample was fixed to a flat plate, and then the release film was peeled off from the ceramic green sheet at a peel angle of 90° and a peel speed of 500 mm / min using a tensile tester (AR-1000 from ChemInstrument) to measure the peel force (gf / 25 mm). The average value of the results of five measurements is shown in Table 1.

[0180] In addition, the peel strength after storage for 90 days (RF1) was compared to that after storage for 24 hours (RF2). 90 ) ratio (RF 90 / RF1) was measured to show stability over time.

[0181] [Experimental Example 2] Measurement of tape peeling force

[0182] The release strength of the release films prepared by applying the release coating compositions prepared in the above Examples and Comparative Examples was evaluated using TESA 7475 tape (manufactured by TESA, Germany), which is a standard tape widely used in the technical field of the present disclosure.

[0183] The standard tape, TESA7475 tape, was attached to the release coating surface of the release layer using a 2 kg roller, and the peel force was measured after 20 minutes at room temperature or after 24 hours at room temperature. The peel force was measured five times using a ChemInstrument AR-1000 device at a peel angle of 180° and a peel speed of 12 in / min, and the average value was calculated.

[0184] [Experimental Example 3] Measurement of silicon content

[0185] The silicon content in the release layer of the release film produced in the above Examples and Comparative Examples was measured using an X-ray fluorescence analyzer (XRF) (manufactured by OXFORD, product name: LAB X-3500).

[0186] [Experimental Example 4] Measurement of residual adhesion rate

[0187] The release film measurement samples prepared in the above examples and comparative examples were stored at 25°C and 65% RH for 24 hours, and then Nitto 31B tape, which is a standard tape, was attached to the release coating surface. The samples were then heated at room temperature with a tape of 20 g / cm 2 The tape was then adhered to the release coating surface for 24 hours under a load of 1000 g / m2. The tape was then collected without contamination and adhered to a flat and clean polyethylene terephthalate (PET) film surface. The tape was then reciprocated once with a 2 kg tape roller, after which the peel force was measured.

[0188] For comparison, a Nitto 31B tape that had never been used was adhered to a flat, clean PET film surface, and then the tape was pressed back and forth once with a 2 kg tape roller, after which the peel force was measured.

[0189] The peel force was measured as follows, and the residual adhesion rate was calculated according to Equation 1.

[0190] Measurement equipment: ChemInstrument AR-1000 equipment

[0191] Measurement method: 180° peel angle, peel speed 30mm / min

[0192]

[0193] Residual adhesion rate (%) = [peeling force of adhesive tape that was peeled off after being attached to the surface of the release layer / peeling force of adhesive tape that was not in contact with the surface of the release layer] x 100

[0194] [Experimental Example 5] Measurement of surface energy

[0195] Distilled water and diiodomethane were dropped onto the release coating surface of the release films prepared in the above examples and comparative examples using a contact angle tester (KRUSS, product name: DSA-100) to measure the contact angle of each. The measured contact angle values ​​were then substituted into the Owens-Wendt model to calculate the surface energy.

[0196] [Experimental Example 6] Rub-off test

[0197] The release layer of each of the release films prepared in the above Examples and Comparative Examples was rubbed 10 times with a thumb, and the degree of change in the surface of the release layer was observed with the naked eye. As a result, the rub-off characteristics were evaluated as follows.

[0198] ◎: No change after evaluation

[0199] ○: There is slight pressure, but no problem with use.

[0200] △: When the surface of the release layer is dimly

[0201] ×: When the release layer peeled off

[0202] The results obtained from the above experimental examples are shown in Table 1 below.

[0203] [Table 1-1] [Table 1-2]

[0204] According to the results of Table 1, the release film obtained using the release coating composition according to one aspect of the present disclosure exhibited excellent stability over time and achieved a wide range of peel strengths for green sheets compared to the comparative examples, and therefore has the advantage of being applicable in a variety of industrial fields.

[0205] In the case of Comparative Examples 2 to 5, which are release films that have a heavy peel strength in the prior art, the peel strength from a 3μm green sheet could not exceed 4gf / in, and even if it did exceed this limit, the stability over time was very poor, because the content of CRA, which corresponds to silicone resin, was too high as described above. In contrast, in the Examples, a heavy peel strength exceeding 4gf / in, which was previously unattainable, was achieved by combining a melamine component and a polymer component.

[0206] In the examples according to one aspect of the present disclosure, the peel strength of the green sheet was almost the same as that of the first day after production even when the peel strength was measured on the green sheet 90 days after production, and the green sheet showed excellent stability over time, whereas the comparative example showed a relatively poor stability over time, with the peel strength of the green sheet decreasing over time. This is because the melamine component and the polymer component in the examples form a crosslinked network structure after curing, whereas the comparative example is unable to form such a structure.

[0207] It was also confirmed that the examples according to one aspect of the present disclosure exhibited a residual adhesion rate of at least 94% and excellent rub-off properties.

[0208] [Experimental Example 7] First peel test

[0209] A folding tester (Flexigo, Foldy-100-1C) was used to replicate and evaluate the degree of peeling of the release film. The release film with the ceramic green sheet manufactured in Experimental Example 1 attached was fixed with tape on a fixed plate and a moving plate, and the degree to which the green sheet peeled off from the release film was compared by repeating the process 1 to 100 times at a speed of 1.5 times / sec. The results are shown in Figure 1.

[0210] 1b, in the case of Example 2, even after repeated application, there was almost no peeling, and only a small amount of peeling occurred at the edge after 30 repetitions. In contrast, in the case of Comparative Example 2, a lifting phenomenon was observed after application, and peeling occurred, and a considerable amount of peeling occurred after the first repetition. As the repetitions were repeated, peeling continued to occur, and the peeled area increased.

[0211] These results indicate that the release film manufactured using the release coating composition according to one aspect of the present disclosure can achieve a relatively high green sheet peel strength and has excellent stability over time, compared to release films that have a heavy peel strength in the prior art. In the case of the prior art release film, the CRA content can be increased to achieve a higher green sheet peel strength, but the increased CRA content can cause problems with poor stability over time. However, the present disclosure achieves a wide range of green sheet peel strength and excellent stability over time by using a combination of a melamine component and a polymer component, making it much more advantageous for use in the relevant industrial field.

[0212] In addition, the release film of the present disclosure exhibits far superior peeling properties and stability over time compared to conventional release films, even when the same peeling force is realized. In particular, the thicker the green sheet, the higher the peeling force required, but in the case of conventional release films, if such a peeling force is achieved, the stability over time becomes very poor, and when the release film with the green sheet attached is stored in a rolled state, peeling may occur in which the release film floats up even with a small physical impact. In contrast, the release film of the present disclosure realizes various levels of peeling force for green sheets while at the same time exhibiting excellent stability over time, so it can be used on thick green sheets without the problems of conventional release films.

[0213] [Experimental Example 8] Measurement of FT-IR spectrum

[0214] The FT-IR spectrum of the release layer prepared with the release coating composition of Example 2 and Comparative Example 1 was measured. Specifically, using a Bruker VERTEX70 device, the release coating composition of the Example and Comparative Example was applied to a glass plate, dried and cured at 150°C for 30 seconds in a hot air dryer, and then 0.1 g of the coating layer was sampled with a ceramic knife and the spectrum was measured using the ATR method of the measuring device. The FT-IR spectrum measurement results are shown in Figure 2.

[0215] According to FIG. 2, unlike Comparative Example 1, the release layer prepared from the release coating composition of the present disclosure has a viscosity of 1650 cm -1 over 1850cm -1 It can be seen that the following regions show high absorption peak intensities. Meanwhile, the P b / P a The values ​​are shown in Table 2 below.

[0216] [Table 2]

[0217] Thus, the release film produced using the release coating composition of the present disclosure has a viscosity of 1450 cm -1 More than 1650cm -1 The maximum absorption peak intensity in the region less than P a , 1650cm -1 over 1850cm -1 The maximum absorption peak intensity in the following region is P b When P is 0.5 or less, b / P a It can be confirmed that the formula of ≦10.0 is satisfied. In addition, in such a range, b / P a By satisfying the above values, it can be confirmed that excellent stability over time is exhibited as shown in Table 1, and the peel force of the green sheet can be achieved in a wide range.

Claims

1. A substrate film; and a release layer formed by applying a release coating composition to at least one surface of the substrate film; The release coating composition comprises a melamine component which is a melamine compound of Formula 1, an oligomer thereof, a polymer thereof, or a combination thereof; a polymer component which contains a polar functional group and has a weight average molecular weight of 3,000 to 30,000; and an acid catalyst, the polymer component does not include a silicone polymer component; The polymer component is at least one selected from the group consisting of polyester, polyurethane, polyvinyl resin, polyethylene terephthalate, acrylate, methacrylate, combinations thereof, and copolymers thereof; the polar functional group is at least one selected from the group consisting of a hydroxyl group, a carboxyl group, an amino group, an amine group, a carbonyl group, an acryl group, an acryloyl group, a nitrile group, a vinyl group, a halogen group, a urethane group, and an ester group; The release layer is a release film that satisfies the following formula (1). Formula (1) 0.5≦P b / P a ≦10.0 P a In the FT-IR spectrum, the wave number is 1450 cm -1 More than 1650cm -1 Maximum absorption peak intensity in the region below P b In the FT-IR spectrum, the wave number is 1650 cm -1 1850cm or more -1 Maximum absorption peak intensity in the following region [Chemical formula 1] 【Chemistry 1】 (Wherein, X is a hydrogen atom, —CH 2 OH, or -CH 2 Each of the R groups may be the same or different. Each of the R groups may be the same or different. At least one of the X groups is -CH 2 -O-CH 3 (It is)

2. The release film satisfies one or more of the following conditions (1) to (4): The release film according to claim 1 . conditions (1) When a TESA 7475 tape is attached to the release layer of the release film and the peel strength is measured at 180° peeling at a peel speed of 0.3 m / min, the peel strength is 30 to 50 gf / in. (2) When TESA 7475 tape is attached to the release layer of the release film, and after 24 hours at room temperature, the peel strength at 180° peeling is measured at a peel speed of 0.3 m / min., and the peel strength at room temperature for one day is 200 to 250 gf / in. (3) When the peel strength of the release film is measured at a peel speed of 0.5 m / min at 90° peeling from the green sheet, the peel strength of the release film from the green sheet is 1 to 100 gf / in. (4) RF 90 / RF 1 ≧0.9 (where RF 1 and RF 90 are the peeling forces of the release film to the green sheet measured after storing the release film with the green sheet attached thereto for 24 hours (1 day) and for 90 days under conditions of room temperature of 23°C and humidity of 50%)

3. The silicon content in the release layer, as measured using an X-ray fluorescence (XRF) analyzer, is 0.001 to 0.015 g / m 2 That is, The release film according to claim 1 .

4. The residual adhesion rate of the release film is 94% or more. The release film according to claim 1 .

5. The surface energy of the release layer is 21 to 30 dyne / cm. The release film according to claim 1 .

6. The residual amount of volatile organic compounds in the release layer is 5 ppm or less. The release film according to claim 1 .

7. The total acid value of the melamine component is 390 to 780 mg KOH / g. The release film according to claim 1 .

8. the polymer component is a polyethylene terephthalate copolymer, The polyethylene terephthalate copolymer is a copolymer comprising terephthalic acid; ethylene glycol; and one or more of isophthalic acid, diethylene glycol, monopropylene glycol, and cyclohexylene dimethanol. The release film according to claim 1 .

9. The polymer component contains two or more different polar functional groups. The release film according to claim 1 .

10. The acid catalyst may be hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, oxalic acid, nitric acid, formic acid, methanesulfonic acid, trifluoromethanesulfonic acid, isoprene sulfonic acid, camphorsulfonic acid, hexanesulfonic acid, octanesulfonic acid, nonanesulfonic acid, decane sulfonic acid, hexadecanesulfonic acid, dinonylnaphthalenesulfonic acid, dinonylnaphthalenedisulfonic acid, benzenesulfonic acid, alkylbenzenesulfonic acid, paratoluenesulfonic acid, melamine zinc iodide (melamine ZnI 2 ), melamine trisulfonic acid (MTSA), cumene sulfonic acid, dodecylbenzene sulfonic acid, naphthalene sulfonic acid, nonylnaphthalene sulfonic acid, methyl acid phosphate, ethyl acid phosphate, propyl acid phosphate, isopropyl acid phosphate, butyl acid phosphate, butoxyethyl acid phosphate, octyl acid phosphate, 2-ethylhexyl acid phosphate, decyl acid phosphate, lauryl acid phosphate, stearyl acid phosphate, oleyl acid phosphate, behenyl acid phosphate, phenyl acid phosphate, nonylphenyl acid phosphate, cyclohexyl acid phosphate acid phosphate, phenoxyethyl acid phosphate, alkoxypolyethylene glycol acid phosphate, bisphenol A acid phosphate, dimethyl acid phosphate, diethyl acid phosphate, dipropyl acid phosphate, diisopropyl acid phosphate, dibutyl acid phosphate, dioctyl acid phosphate, di-2-ethylhexyl acid phosphate, dilauryl acid phosphate, distearyl acid phosphate, diphenyl acid phosphate, bisnonylphenyl acid phosphate sulfonium salt, benzothiazolium salt, ammonium salt, and phosphonium salt; The release film according to claim 1 .

11. In the release coating composition, the weight ratio of the melamine component to the acid catalyst is 100:5 to 100:30; The release film according to claim 1 .

12. The release coating composition comprises 0.2 to 1.0 wt % of a melamine component based on the total weight of the entire composition; or Contains 0.01 to 5 wt% of a polymer component based on the total weight of the entire composition; The release film according to claim 1 .

13. In the release coating composition, the weight ratio of the melamine component and the polymer component is 100:3 to 100:70 based on the solid content. The release film according to claim 1 .

14. The release coating composition further comprises one or more of an antistatic agent, a conductivity enhancer, a pH adjuster, a surfactant, and an antifouling agent. The release film according to claim 1 .

15. The antistatic agent is at least one selected from the group consisting of PEDOT, PEDOT:PSS, polyaniline, polypyrrole, quaternary ammonium salts, sulfonates, and phosphates; The release film according to claim 14.

16. The pH adjuster is at least one selected from the group consisting of sodium hydroxide, potassium hydroxide, calcium hydroxide, and aqueous ammonia. The release film according to claim 14.

17. The surfactant is a cationic surfactant, an anionic surfactant, an amphoteric surfactant, a nonionic surfactant, a silicone surfactant, a modified silicone surfactant, a fluorosurfactant, or a combination thereof. The release film according to claim 14.

18. The antifouling agent is at least one selected from the group consisting of fluorine, fluorine-containing silane-based compounds, fluorine-containing organic compounds, and self-emulsifying silicones; The release film according to claim 14.

19. The antifouling agent is a self-emulsifying silicone, The self-emulsifying silicone is a silicone monomer containing a hydroxyl group; The release film according to claim 18.

20. The release coating composition is based on the total weight of the entire composition. 0.1 to 30% by weight of an antistatic agent, 0.01 to 0.3 wt. % of a pH adjuster, 0.05 to 0.2% by weight of a surfactant, or 0.1 to 0.3 wt. % of an antifouling agent; The release film according to claim 14.

21. The release coating composition further comprises an oxazoline-based curing agent; The release film according to claim 1 .

22. the release coating composition comprises water or a combination of water and an organic solvent; The mixing ratio of the water and the organic solvent is such that the water content is 50% by weight or more based on the total weight of the water and the organic solvent. The release film according to claim 1 .

23. The melamine component and the polymer component containing a polar functional group form a crosslinked network structure after curing. The release film according to claim 1 .

24. The release film is used in adhesives, semi-curing adhesives, ceramic sheets for multilayer ceramic capacitors, semi-curing resins for printed circuits, or prepregs. The release film according to claim 1 .

Citation Information

Patent Citations

  • Composition of antistatic release agent and release film

    JP2012241130A

  • Release film for ceramic green sheet manufacturing process

    JP2017105092A

  • Thermosetting release coating agent and laminate film

    JP2020050863A

  • Release film for manufacturing ceramic green sheet

    JP2021079699A

  • Release film

    JP2021091127A