Tungsten acid solution and its manufacturing method, tungsten oxide powder and its manufacturing method

A room-temperature produced tungstic acid solution with controlled particle size and organic additives enhances tungsten oxide stability and solubility, addressing high-cost heating issues in existing methods.

JP7554935B2Active Publication Date: 2024-09-20MITSUI MINING & SMELTING CO LTD
View PDF 19 Cites 0 Cited by

Patent Information

Application Number
JP2023534886
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-08-04
Filing Date
2022-06-24
Publication Date
2024-09-20
Estimated Expiration
2042-06-24

AI Technical Summary

Technical Problem

Existing methods for producing tungsten oxide require high-temperature heating of ammonia water, leading to increased manufacturing costs and instability of tungsten oxide solutions.

Method used

A tungstic acid solution with a particle size of 20 nm or less, containing 0.1 to 40% tungsten by mass, is produced at room temperature using a reverse neutralization method with ammonia and an organic nitrogen compound, ensuring stability and solubility.

Benefits of technology

The solution achieves high stability and solubility, allowing for efficient production of tungsten oxide powder with improved properties and reduced energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007554935000001
    Figure 0007554935000001
Patent Text Reader

Abstract

A tungstic acid solution according to the present invention contains tungsten in an amount of 0.1 to 40.0% by mass in terms of WO3 content and has a particle diameter (D50) of 20 nm or less when measured by a particle diameter distribution measurement employing a dynamic light scattering method. A method for producing a tungstic acid solution according to the present invention comprises: a step for adding an acidic aqueous tungsten solution containing tungsten in an amount of 1 to 100 g / L in terms of WO3 content to an aqueous ammonia solution having a concentration of 10 to 30% by mass to produce tungsten-containing precipitates; and a step for adding an organic nitrogen compound to a tungsten-containing precipitate slurry that is a slurry-like product of the tungsten-containing precipitates to produce a tungstic acid solution.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a tungstic acid solution and a method for producing the same, a tungsten oxide powder and a method for producing the same. [Background technology]

[0002] Tungsten has the highest melting point among metals, a relatively large electrical resistance as a metal, and high hardness, and is widely used in industrial and medical fields. For example, if tungsten trioxide can be made into a solution, it will be easy to coat, and it has been studied that it will be easy to combine it with multiple elements and add properties suited to the application. For example, Patent Document 1 discloses tungsten oxide that is dissolved in ammonia water heated to 70°C. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2015-44739 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, the tungsten oxide disclosed in Patent Document 1 requires equipment for heating the highly concentrated ammonia water having a concentration of 25% to 70° C., making it difficult to reduce the production cost.

[0005] In view of the above problems, the present invention provides a tungstic acid solution that can be dissolved at room temperature and has excellent solution stability, a method for producing the same, and a tungsten oxide powder and a method for producing the same. [Means for solving the problem]

[0006] The tungstic acid solution of the present invention, which has been made to solve the above problems, is a tungstic acid solution containing 0.1 to 40 mass% of tungsten in terms of WO3, and is characterized in that the particle size (D50) measured by particle size distribution measurement using a dynamic light scattering method is 20 nm or less. The tungstic acid solution of the present invention preferably contains 0.1 to 40 mass% of tungsten in terms of WO3, since the solution stability of the solution is improved.Moreover, the tungstic acid solution of the present invention more preferably contains 20 to 30 mass% of tungsten in terms of WO3.

[0007] Here, the tungstic acid concentration in the tungstic acid solution is calculated by diluting the solution with dilute hydrochloric acid as necessary, and measuring the weight fraction of W in terms of tungsten oxide (WO3) by ICP emission spectrometry (Agilent Technologies: AG-5110). Note that the tungstic acid in the tungstic acid solution of the present invention does not necessarily exist in the form of WO3. The content of tungstic acid is shown in terms of WO3 based on the convention for showing the concentration of tungstic acid.

[0008] Here, it is presumed that the tungstic acid in the tungstic acid solution of the present invention exists in the solution as a polytungstic acid polynuclear complex ion in which tungsten atoms and oxygen atoms are multi-stage condensed in the solution.

[0009] In addition, the particle diameter (D50) measured by dynamic light scattering is preferably 20 nm or less from the viewpoint of stability over time, more preferably 10 nm or less, even more preferably 2 nm or less, particularly preferably 1 nm or less, and even more preferably below the detection limit of less than 1 nm. Thus, the particle diameter (D50) of the present invention is a solution in which the particle diameter (D50) is 20 nm or less by dynamic light scattering. For example, the particle diameter (D50) of tungstic acid particles in the tungstic acid solution of the present invention measured by dynamic light scattering is preferably 20 nm or less from the viewpoint of stability over time, more preferably 10 nm or less, even more preferably 2 nm or less, particularly preferably 1 nm or less, and even more preferably below the detection limit of less than 1 nm.

[0010] Here, the dynamic light scattering method is a method in which a solution such as a suspension solution is irradiated with light such as a laser beam to measure the light scattering intensity from a group of particles undergoing Brownian motion, and the particle size and distribution are obtained from the temporal variation of the intensity. Specifically, the particle size distribution is evaluated in accordance with JIS Z 8828:2019 "Particle Size Analysis - Dynamic Light Scattering Method" using a zeta potential, particle size, and molecular weight measurement system (manufactured by Otsuka Electronics Co., Ltd.: ELSZ-2000ZS). In addition, in order to remove dust and the like in the solution to be measured immediately before the measurement, the solution is filtered with a filter having a pore size of 2 μm, and ultrasonic treatment is performed for 3 minutes with an ultrasonic cleaner (manufactured by As One Co., Ltd.: VS-100III). Furthermore, the liquid temperature of the solution, which is the measurement mode, was adjusted to 25 ° C. The particle size (D50) refers to the median diameter (D50), which is the particle size that shows the 50% cumulative value of the cumulative distribution curve.

[0011] In the present invention, the term "solution" is not limited to a solute dispersed or mixed in a solvent in a monomolecular state, but also includes an aggregate in which a plurality of molecules are attracted to each other by intermolecular interactions, such as (1) polymer molecules, (2) solvated molecules, (3) molecular clusters, and (4) colloidal particles dispersed in a solvent.

[0012] In addition, the tungstic acid solution of the present invention is preferably an aqueous solution. Since the tungstic acid in the tungstic acid solution of the present invention has high dispersibility in water and good solubility in water, pure water can be used as the solvent.

[0013] The tungstic acid solution of the present invention is characterized by containing ammonia and an organic nitrogen compound. The tungstic acid solution of the present invention contains ammonia and organic nitrogen compounds in addition to tungstic acid. The "ammonia" and "organic nitrogen compounds" of the present invention include those ionized in the tungstic acid solution of the present invention. As will be described in detail in the method for producing the tungstic acid solution of the present invention later, in the production process, an acidic tungsten solution is added to ammonia water by reverse neutralization to produce a tungsten-containing precipitate slurry, ammonium tungstate hydrous cake, and then an organic nitrogen compound is added and mixed to produce the tungstic acid solution of the present invention. Therefore, it is considered that the substituted ammonia and organic nitrogen compounds exist in the solution as cations.

[0014] Methods for measuring the ammonia concentration in the solution include adding sodium hydroxide to the solution to distill and separate the ammonia and quantifying the ammonia concentration using an ion meter, quantifying the N2 content in a gasified sample using a thermal conductivity meter, the Kjeldahl method, gas chromatography (GC), ion chromatography, and gas chromatography-mass spectrometry (GC-MS).

[0015] On the other hand, examples of organic nitrogen compounds include aliphatic amines, aromatic amines, amino alcohols, amino acids, polyamines, quaternary ammonium compounds, guanidine compounds, and azole compounds.

[0016] Examples of aliphatic amines include methylamine, dimethylamine, trimethylamine, ethylamine, methylethylamine, diethylamine, triethylamine, methyldiethylamine, dimethylethylamine, n-propylamine, di-n-propylamine, tri-n-propylamine, isopropylamine, diisopropylamine, triisopropylamine, n-butylamine, di-n-butylamine, tri-n-butylamine, isobutylamine, diisobutylamine, triisobutylamine, tert-butylamine, n-pentamine, n-hexylamine, cyclohexylamine, piperidine, and the like.

[0017] Examples of aromatic amines include aniline, phenylenediamine, and diaminotoluene. Examples of amino alcohols include methanolamine, ethanolamine, propanolamine, butanolamine, pentanolamine, dimethanolamine, diethanolamine, trimethanolamine, methylmethanolamine, methylethanolamine, methylpropanolamine, methylbutanolamine, ethylmethanolamine, ethylethanolamine, ethylpropanolamine, dimethylmethanolamine, dimethylethanolamine, dimethylpropanolamine, methyldimethanolamine, methyldiethanolamine, diethylmethanolamine, trishydroxymethylaminomethane, bis(2-hydroxyethyl)aminotris(hydroxymethyl)methane, and aminophenol. Examples of amino acids include alanine, arginine, aspartic acid, and EDTA. Examples of polyamines include polyamines and polyetheramines.

[0018] Examples of quaternary ammonium include alkylimidazolium, pyridinium, pyrrolidium, tetraalkylammonium, etc. Specific examples of alkylimidazolium include 1-methyl-3-methylimidazolium, 1-ethyl-3-methylimidazolium, 1-propyl-3-methylimidazolium, 1-butyl-3-methylimidazolium, 1-hexyl-3-methylimidazolium, 1-methyl-2,3-dimethylimidazolium, 1-ethyl-2,3-dimethylimidazolium, 1-propyl-2,3-dimethylimidazolium, 1-butyl-2,3-dimethylimidazolium, etc. Specific examples of pyridinium and pyrrolidium include N-butyl-pyridinium, N-ethyl-3-methyl-pyridinium, N-butyl-3-methyl-pyridinium, N-hexyl-4-(dimethylamino)-pyridinium, N-methyl-1-methylpyrrolidinium, and N-butyl-1-methylpyrrolidinium. Specific examples of tetraalkylammonium include tetramethylammonium, tetraethylammonium, tetrabutylammonium, and ethyl-dimethyl-propylammonium. Examples of anions that form salts with the above-mentioned cations include OH, - , Cl - , Br - , I - , BF4 - , HSO4 - etc.

[0019] Examples of the guanidine compound include guanidine, diphenylguanidine, and ditolylguanidine. Examples of the azole compound include imidazole compounds and triazole compounds. Specific examples of the imidazole compound include imidazole, 2-methylimidazole, and 2-ethyl-4-methylimidazole. Specific examples of the triazole compound include 1,2,4-triazole, 1,2,4-triazole-3-methyl carboxylate, and 1,2,3-benzotriazole.

[0020] Methods for measuring the concentration of organic nitrogen compounds in the solution include gas chromatography (GC), liquid chromatography (LC), mass spectrometry (MS), gas chromatography-mass spectrometry (GC-MS), and liquid chromatography-mass spectrometry (LC-MS). In addition, a method for quantifying the N2 content in the gasified sample using a thermal conductivity meter may be used in combination.

[0021] In the tungstic acid solution of the present invention, the organic nitrogen compound is preferably an aliphatic amine and / or a quaternary ammonium. When the organic nitrogen compound is an aliphatic amine and / or a quaternary ammonium, these organic nitrogen compounds are highly volatile and easy to remove when complexed with multiple elements to impart properties suited to the intended use.

[0022] Here, the organic nitrogen compound is preferably an aliphatic amine, since it has low toxicity. Specifically, it is more preferable that the organic nitrogen compound is an aliphatic amine having 1 to 4 carbon atoms, and particularly preferable that the organic nitrogen compound is an aliphatic amine having 1 to 2 carbon atoms. Examples of the aliphatic amine include methylamine and dimethylamine.

[0023] In addition, the organic nitrogen compound is preferably a quaternary ammonium, which is not only highly soluble but also highly inhibits crystallization and sol formation. For example, tetraalkylammonium salts are preferred, tetraalkylammonium hydroxide salts are more preferred, tetramethylammonium hydroxide and tetraethylammonium are particularly preferred, and tetramethylammonium hydroxide (TMAH) is also particularly preferred.

[0024] Furthermore, the organic nitrogen compound may be a mixture of two or more selected from aliphatic amines, aromatic amines, amino alcohols, amino acids, polyamines, quaternary ammonium, guanidine compounds, and azole compounds, rather than one selected from them. For example, a mixture of two types of compounds, an aliphatic amine and a quaternary ammonium compound, is preferred in that it can increase solubility while suppressing the amount of addition so as not to increase toxicity.

[0025] Specifically, examples of such mixtures include mixtures of two organic nitrogen compounds, such as methylamine and tetramethylammonium hydroxide (TMAH), dimethylamine and tetramethylammonium hydroxide (TMAH), and methylamine and dimethylamine, and mixtures of three organic nitrogen compounds, such as methylamine, dimethylamine, and tetramethylammonium hydroxide (TMAH).

[0026] In the tungstic acid solution of the present invention, it is more preferable that the aliphatic amine is methylamine or dimethylamine, and the quaternary ammonium is tetramethylammonium hydroxide (TMAH). The aliphatic amine is preferably methylamine or dimethylamine, since it has low toxicity as described above. The quaternary ammonium is preferably tetramethylammonium hydroxide (TMAH), since it has high solubility as described above, and also has high crystallization inhibition and high solization inhibition. Furthermore, tetramethylammonium hydroxide (TMAH) is particularly preferable, since it has high crystallization inhibition and high solization inhibition.

[0027] The tungstic acid solution of the present invention preferably has a pH of 6 or more and 13 or less. The tungstic acid solution of the present invention has better solution stability when its pH is 6 or more and 13 or less. The pH is more preferably 6 or more and 9 or less, and even more preferably 6 or more and 8 or less. The tungstic acid solution of the present invention has a higher basicity of the organic nitrogen compound contained in the solution, and the stronger the bond with the polytungstic acid polynuclear complex ion, the more the H in the polytungstic acid polynuclear complex ion is bonded. + It is presumed that the pH tends to decrease due to the release of

[0028] The tungstic acid solution of the present invention may contain oxide powders such as Nb, Ta, Ti, Mo, Si, Zr, Zn, Al, Y, V, and La-based (La, Ce, Nd, Eu, Gd, Dy, Yb) as additives. Since the tungstic acid solution of the present invention is a homogeneous solution, even if these oxide powders are in a suspended state, improvement in homogeneity and improvement in reactivity (reaction rate) are expected. In addition, if these oxide powders are dissolved in the tungstic acid solution of the present invention to form a homogeneous solution, the composite element can be in the most reactive state.

[0029] Furthermore, the tungstic acid solution of the present invention may contain components (referred to as "other components") other than components derived from tungsten or tungstic acid and components derived from ammonia and organic nitrogen compounds, within a range that does not impair the action and effect of the solution. Examples of other components include Nb, Ta, Ti, Mo, Si, Zr, Zn, Al, Y, V, and La-based (La, Ce, Nd, Eu, Gd, Dy, Yb). However, the other components are not limited to these. The content of other components in the tungstic acid solution of the present invention is preferably less than 5% by mass, more preferably less than 4% by mass, and even more preferably less than 3% by mass. It is assumed that the tungstic acid solution of the present invention contains unavoidable impurities, not intentionally. The content of unavoidable impurities is preferably less than 0.01% by mass.

[0030] The tungsten oxide powder of the present invention is characterized by containing tungstic acid particles contained in a tungstic acid solution. The tungsten oxide powder of the present invention contains tungsten acid particles contained in the above-mentioned tungstic acid solution. The method for producing the tungsten oxide powder of the present invention will be described later.

[0031] The above-mentioned method for producing the tungstic acid solution of the present invention will be described below.

[0032] The method for producing a tungstic acid solution of the present invention includes the steps of: adding an acidic tungsten aqueous solution containing 1-100 g / L of tungsten calculated as WO3 to a 10-30 mass % ammonia aqueous solution to generate a tungsten-containing precipitate; and adding an organic nitrogen compound to the tungsten-containing precipitate slurry obtained by turning the tungsten-containing precipitate into a slurry to generate a tungstic acid solution.

[0033] First, in the step of adding an acidic tungsten aqueous solution containing 1-100g / L of tungsten in terms of WO3 to a 10-30 mass% ammonia aqueous solution to generate a tungsten-containing precipitate, the acidic tungsten aqueous solution refers to a tungsten sulfate aqueous solution obtained by solvent extraction of a solution in which tungsten is dissolved in an acidic aqueous solution containing sulfuric acid. Note that, unless otherwise specified, tungsten referred to in this specification includes tungsten oxide.

[0034] Here, it is preferable to adjust the tungsten sulfate aqueous solution to contain 1 to 100 g / L of tungsten in terms of WO3 by adding water (e.g., pure water). In this case, it is preferable that the tungsten concentration is 1 g / L or more in terms of WO3, since it becomes a tungsten acid compound hydrate that is easily soluble in water, and in consideration of productivity, it is more preferable that it is 10 g / L or more, and even more preferable that it is 20 g / L or more. On the other hand, it is preferable that the tungsten concentration is 100 g / L or less in terms of WO3, since it becomes a tungsten acid compound hydrate that is easily soluble in water, and in order to more reliably synthesize a tungsten acid compound hydrate that is easily soluble in water, it is more preferable that it is 90 g / L or less, even more preferable that it is 80 g / L or less, and particularly preferable that it is 70 g / L or less. In addition, the pH of the tungsten sulfate aqueous solution is preferably 2 or less, and more preferably 1 or less, from the viewpoint of completely dissolving tungsten or tungsten oxide.

[0035] When the tungsten sulfate aqueous solution is added to the ammonia aqueous solution, in the so-called reverse neutralization method, it is preferable to add the tungsten sulfate aqueous solution to a 10 mass % to 30 mass % ammonia aqueous solution, that is, to obtain a slurry of a tungsten acid compound hydrate, that is, a slurry of a tungsten-containing precipitate, by the reverse neutralization method.

[0036] The ammonia concentration of the aqueous ammonia solution used for reverse neutralization is preferably 10% by mass to 30% by mass. When the ammonia concentration is 10% by mass, tungsten is less likely to remain undissolved, and tungsten or tungsten oxide can be completely dissolved in water. On the other hand, when the ammonia concentration is 30% by mass or less, it is preferable because it is close to a saturated aqueous ammonia solution.

[0037] From this viewpoint, the ammonia concentration of the aqueous ammonia solution is preferably 10% by mass or more, more preferably 15% by mass or more, even more preferably 20% by mass or more, and particularly preferably 25% by mass, while the ammonia concentration is preferably 30% by mass or less, more preferably 29% by mass or less, and even more preferably 28% by mass or less.

[0038] In the reverse neutralization, the amount of tungsten sulfate aqueous solution added to the ammonia water is preferably such that the molar ratio of NH3 / WO3 is 0.1 or more and 300 or less, more preferably 5 or more and 200 or less. In addition, the tungsten sulfate aqueous solution added to the ammonia water is preferably such that the molar ratio of NH3 / SO4 2- The molar ratio of NH3 / SO4 is preferably 3.0 or more, more preferably 10.0 or more, and even more preferably 20.0 or more. On the other hand, from the viewpoint of cost reduction, the NH3 / SO4 2- The molar ratio of is preferably 200 or less, more preferably 150 or less, and even more preferably 100 or less.

[0039] In the reverse neutralization, the time for adding the tungsten sulfate aqueous solution to the ammonia water is preferably within 1 minute, more preferably within 30 seconds, and even more preferably within 10 seconds. That is, it is preferable to add the tungsten sulfate aqueous solution to the ammonia water in as short a time as possible, for example, all at once, rather than gradually adding the tungsten sulfate aqueous solution over a long period of time, and to carry out the neutralization reaction. In addition, in the reverse neutralization, since the acidic tungsten sulfate aqueous solution is added to the alkaline ammonia water, the neutralization reaction can be carried out while maintaining a high pH. The tungsten sulfate aqueous solution and the ammonia water can be used at room temperature.

[0040] The sulfur content is then removed from the slurry of the tungsten-containing precipitate obtained by the reverse neutralization method to produce a tungsten-containing precipitate from which the sulfur content has been removed. Since the slurry of the tungsten-containing precipitate obtained by the reverse neutralization method contains, as impurities, sulfate ions that remain without reacting with tungsten or tungsten oxide and sulfur content in the form of hydrogen sulfate ions, it is preferable to remove these.

[0041] Any method for removing sulfur may be used, and for example, a method using a membrane such as reverse osmosis filtration, ultrafiltration, or microfiltration using ammonia water or pure water, centrifugation, or other known methods may be used. Note that, when removing sulfur from the slurry of the tungsten-containing precipitate, temperature control is not particularly required, and the removal may be performed at room temperature.

[0042] Specifically, the slurry of the tungsten-containing precipitate obtained by the reverse neutralization method is decanted using a centrifuge, and washing is repeated until the conductivity of the slurry of the tungsten-containing precipitate becomes 500 μS / cm or less, thereby obtaining a tungsten-containing precipitate from which the sulfur content has been removed. The conductivity was measured by adjusting the liquid temperature of the slurry of the tungsten-containing precipitate to 25° C., immersing the measuring part of a conductivity meter (ASCON2 manufactured by AS ONE CORPORATION) in the supernatant liquid of the slurry of the precipitate, and reading the value after the conductivity value stabilized.

[0043] The cleaning solution used to remove the sulfur content is preferably ammonia water. Specifically, ammonia water of 5.0 mass% or less is preferable, ammonia water of 4.0 mass% or less is more preferable, ammonia water of 3.0 mass% or less is even more preferable, and ammonia water of 2.5 mass% is particularly preferable. When the ammonia water is 5.0 mass% or less, ammonia and ammonium ions are appropriate for the sulfur content, and unnecessary cost increases can be avoided.

[0044] Next, in the step of adding an organic nitrogen compound to the tungsten-containing precipitate slurry obtained by making the tungsten-containing precipitate into a slurry, the tungsten-containing precipitate slurry is obtained by diluting the tungsten-containing precipitate from which sulfur has been removed with pure water or the like to make a slurry. The tungsten concentration of the tungsten-containing precipitate slurry from which sulfur has been removed is measured by taking a part of the slurry, drying it at 110°C for 24 hours, and then firing it at 1,000°C for 4 hours to produce WO3. The weight of the WO3 thus produced can be measured, and the tungsten concentration of the slurry can be calculated from the weight.

[0045] The tungsten-containing precipitate slurry from which the sulfur content has been removed is mixed with an organic nitrogen compound to obtain the tungstic acid solution of the present invention.

[0046] Specifically, the obtained tungsten-containing precipitate slurry is added to an organic nitrogen compound so that the tungsten concentration in the final mixture is 0.1 to 40 mass% in terms of WO3, and then mixed with pure water. The mixture is stirred while maintaining the liquid temperature at room temperature (25°C) for 1 hour, thereby obtaining a colorless and transparent tungstic acid solution of the present invention.

[0047] The organic nitrogen compound mixed with the tungsten-containing precipitation slurry is preferably an aliphatic amine and / or a quaternary ammonium.

[0048] Here, from the viewpoint of solubility, the aliphatic amine is preferably mixed so that the aliphatic amine concentration in the tungsten-containing precipitation slurry is 40 mass% or less. From the same viewpoint, the aliphatic amine is preferably mixed so that the aliphatic amine concentration in the tungsten-containing precipitation slurry is 0.1 mass% or more, more preferably 20 mass% or more. The aliphatic amine is more preferably methylamine or dimethylamine.

[0049] On the other hand, from the viewpoint of solubility, the quaternary ammonium is preferably mixed so that the quaternary ammonium concentration in the tungsten-containing precipitation slurry is 40 mass% or less. From the same viewpoint, the quaternary ammonium is preferably mixed so that the quaternary ammonium concentration in the tungsten-containing precipitation slurry is 0.1 mass% or more, and more preferably 20 mass% or more. The quaternary ammonium is more preferably tetramethylammonium hydroxide (TMAH).

[0050] Furthermore, the organic nitrogen compound to be mixed with the tungsten-containing precipitation slurry may be a mixture of two or more of aliphatic amines or quaternary ammonium, rather than one of them. For example, a mixture of two or more organic nitrogen compounds such as methylamine and tetramethylammonium hydroxide (TMAH), dimethylamine and tetramethylammonium hydroxide (TMAH), or methylamine and dimethylamine, or a mixture of three or more organic nitrogen compounds such as methylamine, dimethylamine, and tetramethylammonium hydroxide (TMAH) may be used, and may be appropriately changed according to the application.

[0051] The method for producing tungsten oxide powder from the above-mentioned tungstic acid solution of the present invention will be described below.

[0052] The method for producing a tungsten oxide powder of the present invention is characterized by having a step of drying and calcining the tungstic acid solution obtained by the above-mentioned method for producing a tungsten acid solution of the present invention to produce a tungsten oxide powder.

[0053] First, the tungstic acid solution obtained by the above-mentioned method for producing a tungstic acid solution of the present invention is placed in a stationary furnace and dried in the air at a heating temperature of about 110°C for 7 hours to remove moisture from the tungstic acid solution of the present invention, thereby obtaining an intermediate product of a tungsten oxide powder containing tungsten oxide particles contained in the tungstic acid solution of the present invention. The tungstic acid solution may also be placed in a vacuum drying furnace with an internal pressure set to 0.01 MPa, heated to 60°C or higher, and vacuum dried for 6 hours.

[0054] Next, the intermediate product (also called dried powder) of the tungsten oxide powder containing the obtained tungsten oxide particles is placed in a stationary furnace, heated to 650°C or higher, and fired for 1 to 3 hours to obtain tungsten oxide powder. The heating temperature is preferably 500°C or higher and 2,000°C or lower. When the heating temperature is 500°C or higher and 2,000°C or lower, it is a temperature sufficient for the growth of tungsten oxide particles, and the firing cost can be suppressed, and the fired product obtained by firing does not become a hard lump, so that the labor and cost increase of crushing can be avoided. Furthermore, the heating temperature is more preferably 700°C or higher and 1,500°C or lower, and even more preferably 900°C or higher and 1,500°C or lower. Moreover, the firing time is preferably 0.5 hours to 72 hours. When the firing time is 0.5 hours to 72 hours, it is a time sufficient for the growth of tungsten oxide particles, and unnecessary costs can be suppressed. Furthermore, the firing time is more preferably 0.5 to 50 hours, and further preferably 0.5 to 30 hours.

[0055] The sintered product may be pulverized and used as the tungsten oxide powder. Regardless of whether or not the sintered product is pulverized, the sintered product may be classified using a sieve, and the undersize (fine grain side) obtained may be used as the tungsten oxide powder. The oversize (coarse grain side) may be pulverized again and classified for use. It is also possible to combine pulverization and classification using a vibrating sieve into which iron balls coated with nylon or fluororesin are charged as pulverizing media. By combining classification and pulverization in this way, even if there are tungsten oxide particles that are too large after roasting, they can be removed. Specifically, when classifying using a sieve, it is preferable to use one with an opening of 150 μm to 1,000 μm. If the opening is 150 μm to 1,000 μm, the proportion of oversize particles is not too high, so that re-pulverization is not repeated, and tungsten oxide powder that needs re-pulverization is not classified to the undersize.

[0056] The composite tungstic acid composition of the present invention is characterized by having the above-mentioned tungstic acid solution of the present invention and at least one element selected from the group consisting of Si, Al, Ti, Zn, Sn, Y, Ce, Ba, Sr, P, S, La, Gd, Nd, Eu, Dy, Yb, Nb, Li, Na, K, Mg, Ca, Zr, Mo, and Ta. It is presumed that the composite tungstic acid composition of the present invention is present in a solution as ions in an ionic state in which tungstic acid and at least one element selected from the group are ionically bonded. Here, the composite tungstic acid composition of the present invention is not limited to the "solution" in the present invention, and also includes those in which a precipitate occurs in the "solution". The tungstic acid concentration in the composite tungstic acid composition of the present invention can be calculated by diluting the composition appropriately with dilute hydrochloric acid as necessary, and measuring the W weight fraction in terms of WO3 by ICP emission spectrometry (manufactured by Agilent Technologies: AG-5110). Similarly to the W weight fraction, the concentration of at least one element selected from the group in the composite tungstic acid composition of the present invention can also be calculated.

[0057] In addition, the method for producing a composite tungstic acid composition of the present invention includes a step of mixing the tungstic acid solution produced by the above-mentioned method for producing a tungstic acid solution of the present invention with at least one element selected from the group consisting of Si, Al, Ti, Zn, Sn, Y, Ce, Ba, Sr, P, S, La, Gd, Nd, Eu, Dy, Yb, Nb, Li, Na, K, Mg, Ca, Zr, Mo, and Ta to produce a composite tungstic acid composition. The above-mentioned tungstic acid solution of the present invention and at least one element selected from the group are mixed and stirred while maintaining the liquid temperature at an appropriate temperature for a predetermined time, thereby obtaining the composite tungstic acid composition of the present invention. Here, the at least one element selected from the group, which is mixed with the tungstic acid solution produced by the above-mentioned method for producing a tungstic acid solution of the present invention, may be in various forms such as oxides, hydroxides, metal complexes, and salts made of polyoxometalates and peroxo complexes.

[0058] The tungstic acid film of the present invention is characterized by containing tungstic acid particles contained in the tungstic acid solution. The tungstic acid film of the present invention, i.e., the tungstic acid formed film, contains tungstic acid particles contained in the above-mentioned tungstic acid solution.

[0059] The method for producing a tungstic acid film of the present invention is characterized by comprising the steps of applying a tungstic acid solution obtained by the method for producing a tungstic acid solution of the present invention described above, baking the solution, and forming a tungstic acid film.

[0060] Specifically, the tungstic acid solution obtained by the above-mentioned method for producing the tungstic acid solution of the present invention is dropped onto a substrate using a syringe while being filtered, for example, with a filter having a pore size of 2 μm, as necessary, and then coated by spin coating (1,500 rpm, 30 seconds).Then, the substrate coated with the tungstic acid solution of the present invention is placed in a stationary furnace, heated to 700° C. or higher, and baked for 1 hour, thereby obtaining the tungstic acid film of the present invention.

[0061] The composite tungstic acid film of the present invention is characterized by containing composite tungstic acid particles contained in the composite tungstic acid composition. The composite tungstic acid film of the present invention, i.e., the composite tungstic acid formed film, contains the composite tungstic acid particles contained in the above-mentioned composite tungstic acid solution.

[0062] The method for producing a composite tungstic acid film of the present invention is characterized by having a step of applying and baking a composite tungstic acid composition obtained by the above-mentioned method for producing a composite tungstic acid composition of the present invention to produce a composite tungstic acid film.

[0063] Specifically, the composite tungstic acid composition obtained by the above-mentioned method for producing the composite tungstic acid composition of the present invention is dropped onto a substrate using a syringe while being filtered, for example, with a filter having a pore size of 2 μm, as required, and is applied by spin coating (1,500 rpm, 30 seconds).Then, the substrate coated with the composite tungstic acid composition of the present invention is placed in a stationary furnace, heated to 700° C. or higher, and baked for 1 hour, thereby obtaining the composite tungstic acid film of the present invention.

[0064] The tungstic acid solution of the present invention may contain additives such as dispersants, pH adjusters, colorants, thickeners, wetting agents, and binder resins depending on the intended use. Effect of the Invention

[0065] The tungstic acid solution of the present invention has a high concentration and is excellent in solution stability. BEST MODE FOR CARRYING OUT THEINVENTION

[0066] The tungstic acid solution according to the embodiment of the present invention will be further described below with reference to the following examples. However, the present invention is not limited to the following examples.

[0067] Example 1 100 g of tungsten trioxide was dissolved in 200 g of 55 mass% sulfuric acid aqueous solution, and ion-exchanged water was added to obtain a tungsten sulfate aqueous solution containing 100 g / L of tungsten in terms of WO3. 200 mL of this tungsten sulfate aqueous solution was added to 1 L of ammonia water (NH3 concentration 25 mass%) in less than 1 minute (NH3 / WO3 molar ratio = 170.47, NH3 / SO4 2- The reaction solution was a slurry of a tungstic acid compound hydrate, in other words, a slurry of a tungsten-containing precipitate.

[0068] The reaction solution was then decanted using a centrifuge and washed until the electrical conductivity was 500 μS / cm or less, to obtain a tungsten-containing precipitate from which the sulfur content had been removed. In this case, ammonia water was used as the washing liquid.

[0069] Furthermore, the tungsten-containing precipitate from which the sulfur was removed was diluted with pure water to obtain a tungsten-containing precipitate slurry from which the sulfur was removed. A portion of the tungsten-containing precipitate slurry from which the sulfur was removed was dried at 110°C for 24 hours and then fired at 1,000°C for 4 hours to produce WO3, and the WO3 concentration in the tungsten-containing precipitate slurry from which the sulfur was removed was calculated from its weight.

[0070] Then, the tungsten-containing precipitate slurry from which the sulfur content had been removed and diluted with pure water was mixed with 2% by mass of methylamine and pure water so that the tungsten concentration of the final mixture was 10% by mass in terms of WO3, and the mixture was stirred and held for 1 hour while maintaining the liquid temperature at room temperature (25°C), thereby obtaining a colorless and transparent aqueous tungstic acid solution according to Example 1. The pH of the obtained aqueous tungstic acid solution according to Example 1 was 8.2.

[0071] Example 2 In Example 2, a similar manufacturing method to that of Example 1 was carried out, except that 2 mass% methylamine and pure water were mixed so that the tungsten concentration of the final mixture was 0.1 mass% in terms of WO3, to obtain a colorless and transparent tungstic acid aqueous solution according to Example 2. The pH of the obtained tungstic acid aqueous solution according to Example 2 was 8.5.

[0072] Example 3 In Example 3, a similar manufacturing method to that of Example 1 was carried out, except that 2 mass% methylamine and pure water were mixed so that the tungsten concentration of the final mixture was 30 mass% in terms of WO3, to obtain a colorless and transparent tungstic acid aqueous solution according to Example 3. The pH of the obtained tungstic acid aqueous solution according to Example 3 was 8.3.

[0073] Example 4 In Example 4, the same manufacturing method as in Example 1 was carried out, except that 2 mass% dimethylamine was mixed with the tungsten-containing precipitate slurry from which sulfur was removed and diluted with pure water, instead of 2 mass% methylamine, to obtain a colorless and transparent tungstic acid aqueous solution according to Example 5. The pH of the obtained tungstic acid aqueous solution according to Example 5 was 7.0.

[0074] Example 5 In Example 5, the same manufacturing method as in Example 1 was carried out, except that 2 mass% tetramethylammonium hydroxide (TMAH) was mixed with the tungsten-containing precipitate slurry from which sulfur was removed and diluted with pure water, instead of 2 mass% methylamine, to obtain a colorless and transparent tungstic acid aqueous solution according to Example 6. The pH of the obtained tungstic acid aqueous solution according to Example 6 was 6.9.

[0075] Example 6 In Example 6, the tungsten concentration of the final mixture was 30 mass% in terms of WO3, and the sulfur-removed tungsten-containing precipitate slurry was diluted with pure water and mixed with 2 mass% tetramethylammonium hydroxide (TMAH) instead of 2 mass% methylamine, and the same manufacturing method as in Example 1 was carried out to obtain a colorless and transparent tungstic acid aqueous solution according to Example 6. The pH of the obtained tungstic acid aqueous solution according to Example 6 was 6.8.

[0076] Comparative Example 1 In Comparative Example 1, the above-mentioned slurry of tungsten-containing precipitate was concentrated using an ultrafiltration device until the tungsten concentration of the slurry was 10 mass% in terms of WO3, and the slurry was washed until the electrical conductivity was 500 μS / cm or less, thereby obtaining a translucent sol (suspension solution). Then, this mixture was stirred and held for 1 hour while maintaining the liquid temperature at room temperature (25°C), thereby obtaining a tungstic acid aqueous solution of a translucent sol (suspension solution) according to Comparative Example 1. The pH of the obtained tungstic acid aqueous solution according to Comparative Example 1 was 7.3.

[0077] Comparative Example 2 In Comparative Example 2, the same manufacturing method as in Example 1 was carried out, except that 22 mass% methylamine was mixed with the tungsten-containing precipitate slurry from which sulfur was removed and diluted with pure water, instead of 2 mass% methylamine, to obtain a tungstic acid aqueous solution of a translucent sol (suspension solution) according to Comparative Example 2. The pH of the obtained tungstic acid aqueous solution according to Comparative Example 2 was 6.7.

[0078] The following physical properties were measured for the tungstic acid aqueous solutions obtained in Examples 1 to 6 and Comparative Examples 1 and 2. The measured physical property values ​​and the measurement methods for the physical property values ​​are shown below, and the measurement results are shown in Table 1.

[0079] <Elemental analysis> If necessary, the sample was appropriately diluted with dilute hydrochloric acid, and the W weight fraction in terms of WO3 was measured by ICP emission spectrometry (Agilent Technologies: AG-5110).

[0080] Dynamic Light Scattering The particle size distribution was evaluated by dynamic light scattering in accordance with JIS Z 8828:2019 using a zeta potential, particle size, and molecular weight measurement system (Otsuka Electronics Co., Ltd.: ELSZ-2000ZS). In addition, the mixture was filtered through a filter with a pore size of 2 μm, and the dispersion treatment using the ultrasonic waves described above was performed. The particle size (D50) refers to the median size (D50), which is the particle size that shows the 50% cumulative value of the cumulative distribution curve. The "initial particle size D50 (nm)" in Table 1 refers to the tungstic acid particle size (D50) in a tungsten aqueous solution adjusted to a liquid temperature of 25 ° C immediately after generation. In addition, the "particle size over time D50 (nm)" in Table 1 refers to the tungstic acid particle size (D50) in a tungsten aqueous solution after being left to stand for one month in an incubator set at room temperature of 25 ° C.

[0081] Quantitative analysis of ammonia 25 ml of sodium hydroxide solution (30 g / 100 ml) was added to 1 to 5 ml of the sample solution, and the mixture was boiled and distilled. The distillate (about 200 ml) was poured into a container containing 20 ml of pure water and 0.5 ml of sulfuric acid to separate ammonia. Next, the separated ammonia was transferred to a 250 ml measuring flask and the volume was adjusted to 250 ml with pure water. Furthermore, 10 ml of the solution adjusted to 250 ml was taken into a 100 ml measuring flask, 1 ml of sodium hydroxide solution (30 g / 100 mL) was added to the taken solution, and the volume was adjusted to 100 ml with pure water. The solution thus obtained was quantitatively analyzed using an ion meter (main unit: HORITA F-53, electrode: HORIBA 500 2A) to measure the ammonium ion concentration (mass%) contained in the solution.

[0082] <pH measurement> The sample at 25°C was measured using a tabletop pH meter (Horiba Ltd.: F-71S: standard ToupH electrode).

[0083] <Stability test over time> The tungstic acid aqueous solutions of Examples 1 to 6 and Comparative Examples 1 and 2 were left to stand for one month in an incubator set at room temperature 25°C, and then visually observed for the presence or absence of a significant increase in particle size. Those in which no significant increase in particle size was observed, specifically, those in which the initial particle size was 200 nm or less and the particle size increase after one month was 20% or less, were evaluated as having stability over time and were marked as "○ (GOOD)". Those in which a significant increase in particle size or precipitation was observed, specifically, those in which the initial particle size was more than 200 nm or the particle size increase after one month was more than 20%, were evaluated as not having stability over time and were marked as "× (BAD)". In addition, the particle diameter over time (D50) of the tungstic acid particles in the tungstic acid aqueous solutions of Examples 1 to 6 and Comparative Examples 1 and 2 after standing for one month was measured using the dynamic light scattering method described above.

[0084] <Film-forming test> The appearance of the coating film formed on the surface of the glass substrate, which is a substitute for the current collector plate, was evaluated by observing it with an optical microscope. The tungstic acid aqueous solutions of Examples 1 to 6 and Comparative Examples 1 and 2 were dropped onto a 15 mm x 15 mm glass substrate using a syringe, and applied by spin coating (1,500 rpm, 30 seconds). The applied area was then air-dried with high-pressure air to form a coating film on the glass substrate. The formed coating film was observed with an optical microscope at 100 times magnification, and those in which no bubbles, uneven coating, or cracks were observed were evaluated as having excellent film-forming properties and were evaluated as "○ (GOOD)", and those in which even one of the following was observed were evaluated as not having excellent film-forming properties and were evaluated as "× (BAD)".

[0085] [Table 1]

[0086] As shown in Table 1, the tungstic acid aqueous solutions according to Examples 1 to 6 had excellent solution stability during long-term storage when the tungstic acid concentration in the aqueous solution was 0.1 to 40 mass%. On the other hand, the tungstic acid aqueous solution according to Comparative Example 1 was observed to have precipitates after being left to stand for one month under the test conditions of the above-mentioned stability test over time. The tungstic acid aqueous solution according to Comparative Example 2 was observed to have precipitates.

[0087] In addition, the tungstic acid aqueous solutions according to Examples 1 to 6, when the tungstic acid particle diameter (D50) in the aqueous solution was 20 nm or less by dynamic light scattering, gave good results in the results of the stability test over time. Specifically, even after one month had passed, the tungstic acid aqueous solutions according to Examples 1 to 6 showed almost no increase in particle size from the initial particle diameter (D50) of tungstic acid over time, and were excellent in stability over time. On the other hand, the tungstic acid aqueous solution of the translucent sol (suspension solution) according to Comparative Example 1 showed an increase of about 10 times in the particle diameter (D50) of tungstic acid over time from the initial particle diameter (D50), and furthermore, precipitates were observed. The tungstic acid aqueous solution according to Comparative Example 2 showed precipitates.

[0088] The tungstic acid aqueous solutions according to Examples 1 to 6 had improved solution stability when the pH of the aqueous solutions was 6 or more and 13 or less. The tungstic acid aqueous solutions according to Examples 1 to 6 had increasing basicity in the order of methylamine, dimethylamine, and tetramethylammonium hydroxide (TMAH) contained in the aqueous solutions. As the basicity increases, the stronger the bond with the polytungstic acid polynuclear complex ion, and the more the H in the polytungstic acid polynuclear complex ion is dissolved. + It was estimated that the pH tends to decrease due to the release of

[0089] The tungstic acid aqueous solutions according to Examples 1 to 6 were observed under an optical microscope at 100x magnification to form coating films. As a result, no air bubbles, coating unevenness, or cracks were observed in the tungstic acid films formed from the tungstic acid aqueous solutions according to all Examples, and the aqueous solutions had excellent film-forming properties.

[0090] The inventions disclosed in this specification include, in addition to the configurations of each invention or embodiment, those that are specified by changing these partial configurations to other configurations disclosed in this specification, to the extent applicable, or those that are specified by adding other configurations disclosed in this specification to these configurations, or those that are specified as higher-level concepts by deleting these partial configurations to the extent that partial action and effects are obtained. [Industrial Applicability]

[0091] The tungstic acid aqueous solution according to the present invention is highly concentrated and has excellent solution stability, and is suitable as a coating agent or a composite material with multiple elements. Conventionally, tungstic acid composite materials and the like have been produced through high-temperature firing, whereas the tungstic acid aqueous solution according to the present invention can be produced at low temperatures (low energy) by mixing aqueous solutions, and is stable as a substance, which leads to the achievement of sustainable management, efficient use, and decarbonization (carbon neutrality) of natural resources.

Claims

1. Tungsten WO 3 A tungstic acid solution containing 0.1 to 30 mass% of tungstic acid in terms of Contains ammonia and organic nitrogen compounds (except for dopamine hydrochloride), The pH is 6 to 9, and the particle size (D50) measured by a particle size distribution measurement using a dynamic light scattering method is 20 nm or less; A tungstic acid solution, characterized in that the organic nitrogen compound is an aliphatic amine and / or a quaternary ammonium.

2. 2. The tungstic acid solution according to claim 1, wherein the tungstic acid solution is an aqueous solution.

3. The tungstic acid solution according to claim 1 or 2, characterized in that the particle diameter (D50) measured by particle diameter distribution measurement using a dynamic light scattering method after one month has elapsed is 20 nm or less.

4. 2. The tungstic acid solution according to claim 1, wherein the aliphatic amine is methylamine or dimethylamine, and the quaternary ammonium is tetramethylammonium hydroxide (TMAH).

5. The tungstic acid solution according to claim 1 or 2, characterized in that the particle diameter (D50) is 10 nm or less in the particle diameter distribution measurement.

6. The tungstic acid solution according to claim 1 or 2, characterized in that the particle diameter (D50) is 2 nm or less in the particle diameter distribution measurement.

7. The tungstic acid solution according to claim 1 or 2, characterized in that the particle diameter (D50) is 1 nm or less in the particle diameter distribution measurement.

8. Tungsten WO 3 adding an acidic tungsten aqueous solution containing 1 to 100 g / L of tungsten in terms of tungsten content to a 10 to 30 mass% ammonia aqueous solution to generate a tungsten-containing precipitate; adding an organic nitrogen compound to the tungsten-containing precipitate slurry obtained by forming the tungsten-containing precipitate into a slurry such that a molar ratio of the organic nitrogen compound to the tungsten is 1.49 or less to produce a tungstic acid solution; having The method for producing a tungstic acid solution, wherein the organic nitrogen compound is an aliphatic amine and / or a quaternary ammonium.

9. A method for producing a tungsten oxide powder, comprising the steps of drying and calcining the tungstic acid solution obtained by the method according to claim 8 to produce a tungsten oxide powder.

10. Tungsten WO 3 a tungstic acid solution containing 0.1 to 30 mass% of tungsten in terms of nitrogen and having a molar ratio of the organic nitrogen compound to the tungsten of 1.49 or less; At least one element selected from the group consisting of Si, Al, Ti, Zn, Sn, Y, Ce, Ba, Sr, P, S, La, Gd, Nd, Eu, Dy, Yb, Nb, Li, Na, K, Mg, Ca, Zr, Mo, and Ta; having A composite tungstic acid composition, characterized in that the organic nitrogen compound is an aliphatic amine and / or tetramethylammonium hydroxide (TMAH).

11. 9. A method for producing a composite tungstic acid composition, comprising the step of mixing the tungstic acid solution produced by the method for producing a tungstic acid solution according to claim 8 with at least one element selected from the group consisting of Si, Al, Ti, Zn, Sn, Y, Ce, Ba, Sr, P, S, La, Gd, Nd, Eu, Dy, Yb, Nb, Li, Na, K, Mg, Ca, Zr, Mo, and Ta to produce a composite composition.

12. A method for producing a tungstic acid film, comprising coating a tungstic acid solution according to claim 1 or 2 and baking the solution.

13. A method for producing a composite tungstic acid film, comprising coating the composite tungstic acid composition according to claim 10 and baking the composition.

Citation Information

Patent Citations

  • Boron-tungsten-iron-nickel alloy electroplating liquid

    CN101928968A

  • Preparation method and application of nano tungsten oxide water solution

    CN104556232A

  • Nano tungsten phosphide / carbon or tungsten nitride / carbon composite material and preparation method thereof

    CN110813338A

  • High-oxygen-resistant medium-temperature hydrolysis catalyst and preparation method thereof

    CN111744500A

  • Catalyst for purifying exhaust gas and its preparation

    JP1985222146A