Sinter manufacturing method
By measuring and controlling the surface recess volume of sintered ore, the method addresses the challenge of simultaneously assessing cold strength and reducibility, achieving balanced properties in the produced sintered ore.
Patent Information
- Application Number
- JP2020202693
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-07
- Publication Date
- 2024-09-24
- Estimated Expiration
- 2040-12-07
AI Technical Summary
Existing methods fail to simultaneously measure the porosity of coarse and fine pores in sintered ore, which are crucial for determining its cold strength and reducibility, and lack correlation between surface recess volume and these properties.
A method involving measuring the volume of surface recesses of sintered ore using an imaging device and adjusting the amount of coagulant, limestone, and production rate to achieve a surface recess volume of 1000 to 1300 μm³/μm², thereby predicting both cold strength and reducibility.
Enables the production of sintered ore with excellent cold strength and reducibility by using a single measurement method, ensuring a balanced pore structure through controlled adjustments.
Smart Images

Figure 0007554979000004 
Figure 0007554979000005 
Figure 0007554979000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing sintered ore. [Background technology]
[0002] The manufacturing method of sintered ore is roughly as follows. First, the raw materials for sintering, which are the raw materials for sintered ore, are mixed in a predetermined ratio to prepare a mixed raw material, which is then granulated with water. The raw materials for sintering are composed of main raw materials, miscellaneous raw materials, auxiliary raw materials necessary for the sintering reaction and component adjustment, carbonaceous materials (solid fuel, coagulant) as a heat source, and return ore. The main raw materials are, for example, iron ores for sintering, such as fine ore and pulverized ore. The miscellaneous raw materials are, for example, iron-containing recycled raw materials, such as iron-making dust, steel-making dust, and scale. The auxiliary raw materials are, for example, limestone, dolomite, converter slag, serpentine, silica stone, and peridotite. The carbonaceous materials are, for example, coke powder and anthracite.
[0003] Next, the granulated mixture of raw materials is charged in layers onto the sintering pallet (strand) of the sintering machine. Next, the solid fuel in the raw material packed bed is ignited from the surface of the raw material packed bed, and suction and ventilation are performed in the thickness direction from the top to the bottom of the raw material packed bed. This causes the combustion zone of the raw material packed bed to gradually shift to the lower layer side, and the sintering reaction (i.e., the firing of the mixed raw materials) progresses. After firing, the sintered cake in the sintering pallet is crushed and sized to a predetermined particle size suitable for sintered ore for blast furnaces. Sintered ore is produced by the above process.
[0004] Sintered ore is porous, and its porosity strongly affects the cold strength and reducibility of sintered ore. For this reason, various methods have been proposed to measure the porosity of sintered ore (including the porosity inside the sintered ore).
[0005] Specifically, methods for measuring the porosity of sintered ore include the mercury method (JIS_M8716), water method (JIS_K2151), paraffin method, plasticine method (Tetsu-to-Hagane, 68 (1982), 2215.), and PAC method (Tetsu-to-Hagane, 93 (1997), 109.). Since mercury has come to be avoided due to environmental concerns, fine pores are measured by the water method, and coarse pores by the PAC method. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2018-31735 A Summary of the Invention [Problem to be solved by the invention]
[0007] As mentioned above, the porosity of sintered ore strongly influences the cold strength and reducibility of sintered ore. To explain in more detail, it is considered that the cold strength of sintered ore is governed by the porosity of relatively coarse pores, and the reducibility of sintered ore is governed by the porosity of relatively fine pores. The pore size (diameter) of this boundary is considered to be 0.1 to 0.5 mm. In other words, a pore structure that contains many pores of 0.1 mm or less and few pores of 0.5 mm or more is considered to be a preferable pore structure that achieves both the cold strength and reducibility of sintered ore.
[0008] In order to evaluate the cold strength and reducibility of sintered ore in a short period of time, it is preferable to measure the porosity of coarse pores and the porosity of fine pores simultaneously (i.e., to measure the porosity of a wide range of pores). However, the above-mentioned measurement method could not measure the porosity of coarse pores and the porosity of fine pores simultaneously.
[0009] Incidentally, the volume of surface recesses is known as a parameter for evaluating the shape of sintered ore. Methods for measuring the volume of surface recesses include a method using X-ray CT (Tetsu-to-Hagane, 71 (1985), S873) and a method assuming the use of a laser range finder (Patent Document 1). However, these documents do not present any correlation between the volume of surface recesses of sintered ore and the cold strength and reducibility of sintered ore.
[0010] Therefore, the present invention has been made in consideration of the above problems, and an object of the present invention is to provide a new and improved method for producing sintered ore, which is capable of predicting both the cold strength and reducibility of sintered ore by a single measurement method, and using the results to produce sintered ore having excellent both cold strength and reducibility. [Means for solving the problem]
[0011] In order to solve the above problem, according to one aspect of the present invention, there is provided a method for producing sintered ore, measuring a volume of a surface recess of the produced sintered ore, and 1040~1270 μm 3 / μm 2 and adjusting at least one of the amount of the agglomerating agent, the amount of the limestone, and the productivity of the sintered ore so that the values fall within the range.
[0012] Here, in the process of measuring the surface recess volume, the sintered ore placed on the installation stand is imaged with an imaging device to obtain an image depicting the three-dimensional shape of the sintered ore, the cross-sectional shape of the sintered ore is obtained from the image, maximum points are identified from the curve showing the cross-sectional shape of the sintered ore, line segments are drawn connecting these maximum points, and a straight line is further drawn that passes through the maximum point and is inclined at a predetermined angle θ from the line segment, and the surface recess volume is measured by integrating the surface recess area surrounded by the straight line at the top and the curve, and the surface recess volume is measured by dividing the surface recess area by the installation stand projected area obtained by projecting the sintered ore onto the installation stand.
[0013] In addition, the mixing amount of the agglomerating agent may be adjusted by adjusting the amount of the agglomerating agent discharged from the raw material hopper of the agglomerating agent.
[0014] The amount of limestone mixed may be adjusted by adjusting the amount of limestone discharged from a limestone raw material hopper.
[0015] In addition, the productivity of sintered ore may be adjusted by carrying out at least one of a process for adjusting the sintering negative pressure and a process for adjusting the layer thickness. Effect of the Invention
[0016] According to the above-described aspects of the present invention, it is possible to predict both the cold strength and reducibility of sintered ore using a single measurement method (i.e., measuring the volume of surface recesses), and to produce sintered ore having excellent both cold strength and reducibility using the results. [Brief description of the drawings]
[0017] [Figure 1] 1 is a schematic diagram showing an overview of a sintered ore manufacturing apparatus according to an embodiment of the present invention; [Diagram 2] FIG. 2 is an explanatory diagram showing an outline of a method for determining the volume of a surface recess; [Diagram 3] 1 is a graph showing the correlation between the volume of a surface recess and cold strength and reducibility. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] A preferred embodiment of the present invention will be described in detail below with reference to the accompanying drawings. Each raw material used in this embodiment is an aggregate of many particles. Unless otherwise specified, the name of each raw material refers to the aggregate of particles that constitute the raw material. A numerical range expressed using "~" means a range that includes the numerical values written before and after "~" as the lower and upper limits. A numerical value indicated as "greater than" or "less than" does not fall within the numerical range.
[0019] <1. Investigation by the present inventor> First, the inventor's investigation will be described. As the sintering of sintered ore progresses, the cold strength of the sintered ore increases and the reducibility decreases. On the other hand, the degree of sintering of sintered ore is also strongly reflected in the unevenness of its surface. In other words, as the sintering of sintered ore progresses, the unevenness decreases. From this, the inventor considered that the surface concave volume, which is an index of the unevenness of the surface of sintered ore, has a good correspondence relationship with both the cold strength and reducibility of sintered ore.
[0020] Therefore, the present inventors investigated the relationship between the surface recess volume of various sintered ores (a specific method for measuring the surface recess volume will be described later) and SI (cold strength) and RI (reducibility). 3 / μm 2 It was confirmed that when the range is within this range, both the SI and the RI become good (see Examples). The present invention was made based on such findings. Hereinafter, a method for producing sintered ore according to this embodiment will be described.
[0021] <2. Sintered ore manufacturing equipment> Next, the configuration of a sintered ore manufacturing apparatus 1 according to this embodiment will be described with reference to Fig. 1. The manufacturing apparatus 1 is an apparatus for carrying out the sintered ore manufacturing method according to this embodiment.
[0022] The manufacturing apparatus 1 includes a plurality of raw material hoppers 10, conveyors 20a, 20b, a drum mixer 30, a granulated material hopper 40, a drum feeder 50, a chute 60, an ignition furnace 80, a pallet 100, a measuring device 200, and a control device 300.
[0023] The raw material hoppers 10 are filled with different raw materials for sintering, and each of them feeds a predetermined amount of raw materials for sintering to the conveyor 20a. The raw materials for sintering are composed of main raw materials, miscellaneous raw materials, auxiliary raw materials necessary for sintering reaction and component adjustment, carbonaceous material (solid fuel, coagulant) as a heat source, and return ore. The main raw materials are, for example, iron ore for sintering, such as fine ore and powdered ore. The miscellaneous raw materials are, for example, iron-containing recycled raw materials such as iron-making dust, steel-making dust, and scale. The auxiliary raw materials are, for example, limestone, dolomite, converter slag, serpentine, silica stone, and olivine. The carbonaceous material is, for example, coke powder and anthracite. The raw material hopper 10a feeds the coagulant. The amount of coagulant fed by the raw material hopper 10a may be controlled by the control device 300. The multiple raw material hoppers 10 also include a raw material hopper 10 that cuts out limestone, and the amount of limestone cut out from this raw material hopper 10 may also be controlled by the control device 300.
[0024] The cut raw material for sintering is mixed on the conveyor 20a to form a mixed raw material, which is then supplied to the drum mixer 30. The drum mixer 30 granulates the mixed raw material together with water to produce a granulated product of the mixed raw material. Note that the device for granulating the mixed raw material is not limited to the drum mixer 30, and any device capable of granulating the mixed raw material may be used.
[0025] The produced granulated material is transported by the conveyor 20b to the granulated material hopper 40. The granulated material stored in the granulated material hopper 40 is fed to the chute 60 by the drum feeder 50 and falls down the chute 60. Thereafter, the granulated material is packed in layers on the pallet 100 to form the raw material packed layer 70.
[0026] The raw material packed bed 70 is transported to the right in the figure by the pallet 100. When the raw material packed bed 70 reaches the ignition furnace 80, the surface of the raw material packed bed 70 is ignited by the ignition furnace 80. After that, the raw material packed bed 70 is ventilated by suction from the top to the bottom in the thickness direction (the negative pressure at this time is also called sintering negative pressure). This causes the combustion zone of the raw material packed bed 70 to gradually move downward, and the sintering reaction (i.e., sintering of the blended raw materials) progresses. After sintering, the sintered cake 90 on the pallet is crushed and sized by the crusher 110 to a predetermined particle size suitable for sintered ore. Through the above process, sintered ore (sintered ore X) is produced.
[0027] The measuring device 200 measures the volume of the surface recessed portion of the sintered ore. A specific measuring method will be described later. The control device 300 controls (adjusts) the amount of the coagulating material discharged from the raw material hopper 10a, for example, based on the measured surface recessed portion volume. Details will be described later.
[0028] Next, the processing by the measuring device 200 will be described. The measuring device 200 includes, as its hardware configuration, an installation stand, an imaging device (consisting of an imaging section and a lens), and a calculation device. A plurality of sintered ores (e.g., 100 pieces of sintered ores. Of course, the number of pieces to be installed is not limited to 100) are installed on the installation stand. Here, it is preferable to install the sintered ores on the installation stand so that a plurality of pieces of sintered ores are not piled up (i.e., one piece of sintered ore is installed on each part of the installation stand).
[0029] The imaging device is installed above the installation table and captures images of the exposed surfaces (surfaces exposed to the imaging device) of the multiple sintered ores installed on the installation table, thereby obtaining captured images of the exposed surfaces of the multiple sintered ores.
[0030] More specifically, the imaging device sequentially measures the surface shape of the sintered ore by a focusing method (for example, "High-speed three-dimensional shape measurement by focusing method" Ishihara Mitsuhiro, Sasaki Hiromi, Journal of the Japan Society of Precision Engineering Vol. 63, No. 1, 1997). As the imaging device, for example, an imaging device with a field of view of 4 mm x 4 mm, a horizontal resolution of 10 μm, and a depth resolution of 0.4 μm can be used. Here, the focusing method is a method of identifying the three-dimensional position of the surface of the object by detecting the positional relationship between a lens that focuses on the surface of the object and the object. The method of measuring the three-dimensional shape of the object (here, sintered ore) by the focusing method is described in the above non-patent document, so a detailed description will be omitted in this specification. Therefore, the above-mentioned captured image depicts the three-dimensional shapes of the exposed surfaces of multiple sintered ores. Note that the method of obtaining the three-dimensional shape of the exposed surface of the sintered ore is not limited to this, and for example, X-ray CT may be used.
[0031] The arithmetic device includes a CPU, a ROM, a RAM, a communication device, etc. The CPU reads and executes a program recorded in the ROM. The RAM is used as a working area for the CPU. The communication device communicates with the control device 300. Specifically, the arithmetic device measures the volume of the surface recess based on an image captured by the imaging device.
[0032] Hereinafter, a method for measuring the surface recess volume will be described based on FIG. 2. Since the detailed method for measuring the surface recess volume is described in Patent Document 1, only an outline will be described here. The surface recess volume is the volume of a depression formed by the surface unevenness of sintered ore. The calculation device selects any one sintered ore X from the captured image and obtains a cross-sectional shape (cross-sectional shape parallel to the thickness direction) of the sintered ore X as shown in FIG. 2(a). A curve X1 corresponding to the shape of the exposed surface of the sintered ore X is drawn on this cross-sectional shape. Next, the calculation device identifies a maximum point A of the curve X1 and draws a plurality of line segments L1 connecting the maximum points A as shown in FIG. 2(b). Next, the calculation device draws a straight line L2 that passes through the maximum point A and is inclined at an angle θ from the line segment L1 toward the sintered ore X direction. Here, the angle θ may be 5 degrees or more and 15 degrees or less, following Patent Document 1 (JP Patent Publication 2018-31735).
[0033] Next, as shown in Fig. 2(c), the calculation device leaves only the topmost straight line L2 on the cross-sectional shape and deletes the others. Here, none of the other straight lines L2, line segments L1, or curves X1 exist above the topmost straight line L2. In other words, the straight line L2 that satisfies these characteristics becomes the topmost straight line L2.
[0034] Next, as shown in FIG. 2(d), the calculation device regards the area surrounded by the uppermost straight line L2 and curve X1 as the surface recessed area X2, and calculates the area of the surface recessed area X2 (if there are multiple surface recessed areas X2, the sum of the areas of these areas). Next, the calculation device repeats the above-mentioned process in a direction perpendicular to the paper surface of FIG. 2, and calculates the area of the surface recessed area X2 for different cross-sectional shapes. Next, the calculation device calculates the accumulated surface recessed area by accumulating (i.e., integrating) the calculated areas of the surface recessed areas X2. The calculation device measures the accumulated surface recessed areas of all sintered ores placed on the setting table, and calculates the sum of these. Meanwhile, the calculation device measures the setting table projection areas (projected areas when the sintered ores are projected in a direction perpendicular to the setting table) of all sintered ores placed on the setting table, and calculates the sum of these. Next, the calculation device divides the sum of the accumulated surface recessed areas by the sum of the setting table projection areas to calculate the surface recessed volume (μm 3 / μm 2 The calculation device outputs the measured (calculated) surface recess volume to the control device 300.
[0035] The control device 300 includes a CPU, a ROM, a RAM, a communication device, and the like. The CPU reads and executes a program recorded in the ROM. The RAM is used as a work area for the CPU. The communication device communicates with the measurement device 200. Specifically, the control device 300 receives a signal indicating that the measured surface recess volume is within the range of 1000 to 1300 μm 3 / μm 2 At least one of the amount of the coagulant, the amount of limestone, and the productivity of sintered ore is adjusted so that the value falls within the range.
[0036] Details will be described in the Examples, but the surface recess volume is 1000 to 1300 μm 3 / μm 2 When the above condition is satisfied, the sintered ore has both excellent cold strength and reducibility. The volume of the surface recesses of the sintered ore decreases as the sintering of the sintered ore progresses. In other words, as the sintering of the sintered ore progresses, the sintered ore itself becomes stronger and the surface unevenness decreases. Here, since the surface unevenness is a reaction interface, the smaller the surface unevenness, the smaller the reaction interface and the lower the reducibility. On the other hand, when the sintering of the sintered ore has not progressed much, the sintered ore itself becomes brittle, but the surface unevenness becomes large. When the volume of the surface recesses is 1000 to 1300 μm 3 / μm 2 In this case, it can be said that the balance between the surface irregularities (i.e., reducibility) and the cold strength is excellent. In this way, it is possible to predict the reducibility and cold strength of sintered ore using a single parameter, the surface concave volume.
[0037] In addition, the increase in the amount of coagulant, the increase in the amount of limestone, or the increase in the production rate of sinter (t / m 2 By decreasing the sintering rate (times per minute / day), the sintering of the sintered ore is promoted (progresses more easily), and the volume of the concave portions on the surface of the sintered ore is reduced. Incidentally, the productivity can be reduced by decreasing the sintering negative pressure or by increasing the thickness of the raw material packed bed 70. Either operation reduces the amount of air passing through the sintering bed, which in turn reduces the rate of combustion, thereby reducing the productivity.
[0038] Conversely, a decrease in the amount of agglomerant or limestone added, or an increase in the production rate of sintered ore inhibits sintering of the sintered ore (makes it more difficult to proceed), and the volume of the surface recesses of the sintered ore increases.
[0039] Therefore, the control device 300 detects the surface recess volume of 1000 to 1300 μm 3 / μm 2 If the surface concave volume is 1000μm, no action is taken. 3 / μm 2If the surface concave volume is less than 1300 μm, sintering has progressed too far, and the sintered ore has sufficient cold strength but insufficient reducibility. Therefore, the control device 300 performs at least one of the following actions to increase the surface concave volume: reducing the amount of coagulant, reducing the amount of limestone, and increasing the productivity of sintered ore. 3 / μm 2 If the temperature is higher, the surface unevenness is large (i.e., the reaction interface is large), so the reducibility is sufficient but the cold strength is insufficient. Therefore, the control device 300 performs at least one of the following actions to reduce the volume of the surface recesses: increasing the amount of the coagulant, increasing the amount of the limestone, and decreasing the productivity of the sintered ore.
[0040] Table 1 shows an example of the change in the volume of the surface recesses due to each action. The numerical values for each raw material in the table are in mass%, but the mass% of the return ore and coke (a type of agglomerating agent) are outside the range (mass% relative to the total mass of iron ore, limestone, quicklime, and olivine). Sintered ore was produced using manufacturing equipment 1. When measuring the volume of the surface recesses, the angle θ shown in Figure 2 was set to 10 degrees.
[0041] Compared to condition S, condition T aims to increase the amount of agglomeration material, condition U aims to increase the amount of limestone, and condition V aims to decrease the production rate. Under all conditions, the volume of surface depressions decreased compared to condition S. In addition, in condition V, the production rate of sintered ore was decreased by lowering the firing negative pressure.
[0042] [Table 1]
[0043] Therefore, by the processing by the measuring device 200 and the control device 300, the volume of the surface recesses of the sintered ore is 1000 to 1300 μm 3 / μm 2 This allows the sintered ore to have excellent cold strength and reducibility.
[0044] <3. Manufacturing method of sintered ore> Next, a method for producing sintered ore using the above-mentioned sintered ore production apparatus 1 will be described with reference to Fig. 1 and Fig. 2. The method for producing sintered ore includes a first step of producing sintered ore, a second step of measuring the volume of the surface recesses of the produced sintered ore, and a second step of measuring the volume of the surface recesses of the produced sintered ore when the measured volume of the surface recesses is 1000 to 1300 µm. 3 / μm 2 and a third step of adjusting at least one of the mixing amount of the agglomerating agent, the mixing amount of limestone, and the productivity of sintered ore so that the values fall within the ranges.
[0045] (3-1. First step) The first step is as follows. First, a predetermined amount of sintering raw material is fed from a plurality of raw material hoppers 10 to a conveyor 20a. Here, the raw material hoppers 10a feed the agglomeration material. The amount of the agglomeration material fed by the raw material hoppers 10a may be controlled by the control device 300.
[0046] The cut raw material for sintering is mixed on the conveyor 20a to form a mixed raw material, which is then supplied to the drum mixer 30. The drum mixer 30 granulates the mixed raw material together with water to produce a granulated product of the mixed raw material.
[0047] The produced granulated material is transported by the conveyor 20b to the granulated material hopper 40. The granulated material stored in the granulated material hopper 40 is fed to the chute 60 by the drum feeder 50 and falls down the chute 60. Thereafter, the granulated material is packed in layers on the pallet 100 to form the raw material packed layer 70.
[0048] The raw material packed bed 70 is transported to the right in the figure by the pallet 100. When the raw material packed bed 70 reaches the ignition furnace 80, the surface of the raw material packed bed 70 is ignited by the ignition furnace 80. Then, suction ventilation is performed from the top to the bottom of the raw material packed bed 70 in the thickness direction. This causes the combustion zone of the raw material packed bed 70 to gradually move downward, and the sintering reaction progresses. After firing, the sintered cake 90 on the pallet is crushed and sized by the crusher 110 to a predetermined particle size suitable for sintered ore. Sintered ore (sintered ore X) is produced by the above process.
[0049] (3-2. Second step) The second step is as follows. First, a plurality of iron ores are placed on a placement table. Next, the imaging device captures images of the exposed surfaces (surfaces exposed to the imaging device side) of the plurality of sintered ores placed on the placement table. This results in an image of the exposed surfaces of the plurality of sintered ores being captured. Here, the captured image depicts the three-dimensional shapes of the exposed surfaces of the plurality of sintered ores. Details are as described above.
[0050] Next, the calculation device measures the surface recess volume based on the captured image captured by the imaging device. As described above in detail, first, the calculation device selects any one sintered ore X from the captured image and obtains the cross-sectional shape of the sintered ore X as shown in FIG. 2(a). Next, the calculation device identifies the maximum point A of the curve X1 and draws a plurality of line segments L1 connecting the maximum points A as shown in FIG. 2(b). Next, the calculation device draws a straight line L2 that passes through the maximum point A and is inclined at an angle θ from the line segment L1 toward the sintered ore X. Here, the angle θ may be 5 degrees or more and 15 degrees or less, following Patent Document 1 (JP Patent Publication 2018-31735).
[0051] Next, as shown in Fig. 2(c), the calculation device leaves only the topmost straight line L2 on the cross-sectional shape and deletes the others. Next, as shown in Fig. 2(d), the calculation device determines the area surrounded by the topmost straight line L2 and curve X1 as the surface recess region X2, and calculates the area of the surface recess region X2. Next, the calculation device repeats the above-mentioned process in a direction perpendicular to the paper surface of Fig. 2, and calculates the area of the surface recess region X2 for different cross-sectional shapes. Next, the calculation device calculates the accumulated surface recess area by accumulating (i.e., integrating) the areas of the calculated surface recess regions X2.
[0052] The calculation device measures the integrated surface recess areas of all the sintered ores placed on the setting table and calculates the sum of these. Meanwhile, the calculation device measures the setting table projected areas of all the sintered ores placed on the setting table and calculates the sum of these. Next, the calculation device divides the sum of the integrated surface recess areas by the sum of the setting table projected areas to calculate the surface recess volume (μm3 / μm 2 The calculation device outputs the measured (calculated) surface recess volume to the control device 300.
[0053] (3-3. Third step) The third step is as follows. The control device 300 detects whether the measured surface recess volume is within the range of 1000 to 1300 μm 3 / μm 2 At least one of the amount of the coagulant, the amount of limestone, and the productivity of sintered ore is adjusted so that the value falls within the range.
[0054] Specifically, the control device 300 detects a surface recess volume of 1000 to 1300 μm 3 / μm 2 If the surface recess volume is less than 1000 μm, no action is taken. 3 / μm 2 If the surface recess volume is lower than 1300 μm, at least one of the following actions is taken to increase the surface recess volume: reducing the amount of coagulant mixed, reducing the amount of limestone mixed, and increasing the productivity of sintered ore. 3 / μm 2 If the surface concavity volume is higher, at least one of the following actions is taken to reduce the surface concavity volume: increasing the amount of coagulant, increasing the amount of limestone, and decreasing the productivity of sintered ore.
[0055] Therefore, by the processing by the measuring device 200 and the control device 300, the volume of the surface recesses of the sintered ore is 1000 to 1300 μm 3 / μm 2 This allows the sintered ore to have excellent cold strength and reducibility. In other words, it is possible to predict both the cold strength and reducibility of the sintered ore using a single measurement method (i.e., measurement of the surface recess volume), and to manufacture sintered ore having excellent cold strength and reducibility using the result.
[0056] Furthermore, processing by the measuring device 200 (i.e., measurement of the surface recess volume) can be performed faster (outputting the surface recess volume in a short time) than the methods described in the Background Art section. Therefore, processing by the measuring device 200 can be performed online. FIG. 1 shows one embodiment of processing performed online. By performing processing by the measuring device 200 online, operational actions can be taken by the control device 300 without any time lag, and stabilization of quality can be expected. Of course, processing by the measuring device 200 may be performed offline or on-site (within the same steelworks). EXAMPLES
[0057] Next, an example of this embodiment will be described. In this example, the mixing amount of the agglomerating agent was changed, and the change in the volume of the surface recesses and the associated change in the cold strength and reducibility of the sintered ore were investigated.
[0058] <1. Example> (1-1. Adjustment of raw material mix) Iron ores A to E, limestone, quicklime, olivine, return ore, and coke (a type of agglomerating agent) shown in Table 2 below were prepared, and these were blended at the blending ratios (mass%) shown in Table 2 below to prepare blended raw materials 1 to 3. Here, the blending ratios of return ore and coke were the outside numbers (mass% relative to the total mass of iron ore, limestone, quicklime, and olivine). More specifically, the coke blending ratio C1 was 4.7 or 5.0 mass%, the coke blending ratio C2 was 4.4 or 4.7 mass%, and the coke blending ratio C3 was 4.5 or 4.8 mass%. In other words, the blended raw materials 1 to 3 are each divided into two types of blended raw materials with different coke blending ratios, so a total of six types of blended raw materials are prepared.
[0059] [Table 2]
[0060] (1-2. Overview of sintering experiment equipment) In this example, a so-called pot test was carried out. Table 3 shows an overview of the main sintering experimental equipment used in the pot test.
[0061] [Table 3]
[0062] (1-3. Sintering experiment method) The pot test (sintering experiment) was carried out as follows. First, the blended raw materials were mixed at 25 rpm for 1 minute using a drum mixer. Next, 6.8 mass% moisture was added to the drum mixer and granulated for 4 minutes. Next, the granulated material was charged from the top of the floor of the sintering pot to the surface of the sintering pot. Next, the surface of the packed bed of the granulated material was heated and ignited in an ignition furnace for 60 [sec], and the negative pressure (constant): 11.8 [kPa] in the wind box was set to sinter the packed bed of raw materials.
[0063] The time from the start of ignition to the point at which the temperature measured in the wind box reached its highest point was considered to be the sintering completion time. After sintering was completed, the sinter cake was removed from the sintering pot and crushed by dropping it from a height of 2 m five times to produce sintered ore. The sintered ore produced was classified using a sieve with 5.0 mm openings. Sintered ore with a particle size larger than 5 mm, specifically sintered ore on the sieve, was considered to be the sintered ore product.
[0064] (1-4. Evaluation of sintered ore) The sintered ore product was classified using sieves with 21 mm and 19 mm openings to obtain sintered ores with particle sizes greater than 19 mm and less than 21 mm (i.e., sintered ores that remained on the 19 mm opening sieve and dropped through the 21 mm opening sieve). These sintered ores were used to evaluate the JIS-RI, which is an index of reducibility, and the surface recess volume. The surface recess volume was measured using the measuring device 200 described in the above embodiment. The angle θ shown in FIG. 2 was set to 10 degrees.
[0065] The sintered ore product was further classified using sieves with 20mm and 10mm openings to obtain sintered ore with particle sizes greater than 10mm and less than 20mm (i.e., sintered ore that remained on the 10mm opening sieve and dropped from the 20mm opening sieve). 10kg of these sintered ores were collected and dropped four times from a height of 2m. The sintered ore after dropping was classified using a 5mm sieve, and the proportion of sintered ore with particle sizes greater than 5mm (i.e., that remained on the 5mm opening sieve) (mass % relative to 10kg) was used as the cold strength.
[0066] <2. Comparative Example> (2-1. Adjustment of raw material mix) In the above-mentioned Table 2, the coke blending ratio C1 was 4.4 or 5.3 mass% (mass% relative to the total mass of iron ore, limestone, quicklime, and olivine), the coke blending ratio C2 was 4.1% or 5.0 mass% and the coke blending ratio C3 was 4.2 or 5.1 mass%. In other words, the raw material blends 1 to 3 are each divided into two types of raw material blends with different coke blending ratios, so a total of six types of raw material blends are prepared.
[0067] (2-2. Treatment of mixed raw materials) The blended raw materials were treated in the same manner as in the Example. The results of the Example and the Comparative Example are shown in FIG. 3. The horizontal axis of FIG. 3 is the surface recess volume (μm 3 / μm 2 ), and the vertical axis indicates cold strength (SI, mass%) or reducibility (RI, %). Point P10 indicates the correlation between the surface recess volume and cold strength, and graph L10 indicates the approximation curve of point P10 (approximation curve obtained by the least squares method). Point P20 indicates the correlation between the surface recess volume and reducibility, and graph L20 indicates the approximation curve of point P20 (approximation curve obtained by the least squares method).
[0068] In the embodiment, the surface recess volume is 1000 to 1300 μm 3 / μm 2 Therefore, the cold strength (SI) and reducibility (RI) are both high, whereas the surface recess volume is 1000 μm in the comparative example. 3 / μm 2 Less than or equal to 1300μm 3 / μm 2 Therefore, either the cold strength (SI) or reducibility (RI) was low.
[0069] Although the preferred embodiment of the present invention has been described in detail above, the present invention is not limited to such an example. It is clear that a person having ordinary knowledge in the technical field to which the present invention pertains can conceive of various modified or altered examples within the scope of the technical ideas described in the claims, and it is understood that these also naturally belong to the technical scope of the present invention.
Claims
1. producing sintered ore; Measuring the volume of a surface recess of the produced sinter; The measured surface recess volume is 1040 to 1270 μm 3 / μm 2 and adjusting at least one of the amount of the coagulant, the amount of the limestone, and the productivity of the sintered ore so that the values fall within the range.
2. In the step of measuring the volume of the surface recesses, The sintered ore placed on the installation table is imaged by an imaging device to obtain an image depicting a three-dimensional shape of the sintered ore; A cross-sectional shape of the sintered ore is obtained from the captured image, and a maximum point is identified from a curve representing the cross-sectional shape of the sintered ore; Draw a line segment connecting these maximum points, and then draw a straight line passing through the maximum points and tilted at a predetermined angle θ from the line segment. calculating an integrated surface recess area by integrating a surface recess area surrounded by the straight line and the curved line at the top; The method for producing sintered ore according to claim 1 , characterized in that the volume of the surface recesses is measured by dividing the integrated area of the surface recesses by a projected area of the installation table obtained by projecting the sintered ore onto the installation table.
3. 3. The method for producing sintered ore according to claim 1, further comprising adjusting an amount of the coagulating agent discharged from a raw material hopper for the coagulating agent to adjust a mixing amount of the coagulating agent.
4. The method for producing sintered ore according to any one of claims 1 to 3, characterized in that the blending amount of the limestone is adjusted by adjusting the amount of the limestone discharged from the limestone raw material hopper.
5. The method for producing sintered ore according to any one of claims 1 to 4, characterized in that the productivity of the sintered ore is adjusted by performing at least one of a process for adjusting the firing negative pressure and a process for adjusting the layer thickness.
Citation Information
Patent Citations
Process for producing sintered ore
EP2365101A1
Sintering operation method
JP1983204134A
Production of sintered raw material of iron ore
JP1985248826A
Operation of vertical furnace using sintered ore having good characteristic at high temperature
JP1999043709A
Method for operating blast furnace using sintered ore excellent in high temperature reducibility
JP2006028538A