Composite Materials
A composite member with an inorganic matrix and dispersed organic fibers addresses the strength and durability issues of cement molded bodies by minimizing porosity and preventing fiber oxidation, enhancing mechanical properties.
Patent Information
- Application Number
- JP2021550427
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-30
- Filing Date
- 2020-08-25
- Publication Date
- 2024-09-24
- Estimated Expiration
- 2040-08-25
AI Technical Summary
Cement molded bodies exhibit insufficient mechanical strength due to the presence of numerous pores, which also lead to oxidative deterioration of fibers over time.
A composite member is created by directly bonding organic fibers to an inorganic matrix made of metal oxides or hydroxides without an adhesive, with a porosity of 20% or less, ensuring the fibers are dispersed within the matrix to enhance mechanical strength and prevent oxidation.
The composite member maintains high mechanical strength and stability over time by reducing fiber oxidation, achieved through a dense inorganic matrix structure that minimizes contact with oxygen and water vapor.
Smart Images

Figure 0007555010000005 
Figure 0007555010000004 
Figure 0007555010000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a composite member. [Background technology]
[0002] Ceramics are known to have high strength and high heat resistance, but are also difficult to distort. Therefore, when a load is applied to ceramics, their ability to absorb the load is small, and sudden destruction can occur. In order to improve these characteristics, research has been actively conducted into improving the strength of ceramics by blending fibers.
[0003] Patent Document 1 discloses a cement admixture that contains a cellulose nanofiber-containing masterbatch (A) obtained by micronizing cellulose in a polyester resin, a maleic anhydride copolymer resin (B), and water (C). It also describes that by adding the cement admixture to a cement composition, the cellulose nanofibers can be uniformly dispersed in the cement composition, and as a result, the strength of cement molded bodies such as concrete and mortar is improved. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2015-155357 A Summary of the Invention
[0005] However, since cement molded bodies are mainly composed of hydrates and have many pores, there is a problem that the mechanical strength of the resulting molded body is insufficient even if fibers are blended in. In addition, when a cement molded body has many pores, the fibers come into contact with the air, and there is a problem that the fibers are oxidized and deteriorated over long-term use.
[0006] The present invention has been made in view of the problems associated with the prior art, and an object of the present invention is to provide a composite material that is stable over a long period of time and has excellent mechanical strength even when organic fibers are used.
[0007] In order to solve the above problems, a composite member according to an embodiment of the present invention includes an inorganic matrix portion constituted by an inorganic material containing at least one of a metal oxide and a metal oxide hydroxide, and organic fibers that are directly bonded to the inorganic matrix portion without an adhesive material different from the inorganic material that constitutes the inorganic matrix portion and that exist in a dispersed state within the inorganic matrix portion. The composite member has a porosity of 20% or less in a cross section of the inorganic matrix portion. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a cross-sectional view that illustrates an example of a composite member according to this embodiment. [Diagram 2] Fig. 2(a) is a schematic enlarged view of a cross section of the composite member of Fig. 1. Fig. 2(b) is a cross-sectional view that shows a schematic view of the vicinity of grain boundaries of a particle group of an inorganic substance. [Diagram 3] FIG. 3 is a cross-sectional view that diagrammatically illustrates another example of a composite member according to the present embodiment. [Figure 4] FIG. 4 is a cross-sectional view that diagrammatically illustrates another example of a composite member according to the present embodiment. [Diagram 5] Fig. 5(a) is a diagram showing a secondary electron image at position 1 in the test sample of Example 2. Fig. 5(b) is a diagram showing binarized data of the secondary electron image at position 1 in the test sample of Example 2. [Figure 6] Fig. 6(a) is a diagram showing a secondary electron image at position 2 in the test sample of Example 2. Fig. 6(b) is a diagram showing binarized data of the secondary electron image at position 2 in the test sample of Example 2. [Figure 7]Fig. 7(a) is a diagram showing a secondary electron image at position 3 in the test sample of Example 2. Fig. 7(b) is a diagram showing binarized data of the secondary electron image at position 3 in the test sample of Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, a composite member according to the present embodiment will be described with reference to the drawings. Note that the dimensional ratios in the drawings are exaggerated for the convenience of explanation and may differ from the actual ratios.
[0010] [Composite material] 1, the composite material 100 of this embodiment includes an inorganic matrix portion 10 and organic fibers 20 that are directly bonded to the inorganic matrix portion 10 without an adhesive material different from the inorganic material that constitutes the inorganic matrix portion 10. In the composite material 100, the organic fibers 20 are bonded to the inorganic matrix portion 10 while being dispersed inside the inorganic matrix portion 10.
[0011] As shown in FIG. 2, the inorganic matrix portion 10 is composed of a plurality of particles 11 made of an inorganic substance, and the inorganic matrix portion 10 is formed by bonding the inorganic substance particles 11 to each other.
[0012] The inorganic material constituting the inorganic matrix portion 10 preferably contains at least one metal element selected from the group consisting of alkali metals, alkaline earth metals, transition metals, base metals, and metalloids. In this specification, the alkaline earth metals include calcium, strontium, barium, and radium, as well as beryllium and magnesium. The base metals include aluminum, zinc, gallium, cadmium, indium, tin, mercury, thallium, lead, bismuth, and polonium. The metalloids include boron, silicon, germanium, arsenic, antimony, and tellurium. Among these, it is preferable that the inorganic material contains at least one metal element selected from the group consisting of zinc, aluminum, and magnesium. The inorganic material containing these metal elements can easily form a connection portion derived from the inorganic material by a pressurized and heated method, as described below.
[0013] It is more preferable that the inorganic material contains at least one of the oxides and hydroxide oxides of the above metal elements as a main component. That is, it is preferable that the inorganic material contains at least one of the oxides and hydroxide oxides of the above metal elements in an amount of 50 mol% or more, and more preferably 80 mol% or more. The oxides of the above metal elements include phosphates, silicates, aluminates, and borates in addition to compounds in which only oxygen is bonded to a metal element. Since such inorganic materials are highly stable against oxygen and water vapor in the atmosphere, by dispersing the organic fibers 20 inside the inorganic matrix portion 10, it is possible to suppress the contact of the organic fibers 20 with oxygen and water vapor, and thus suppress deterioration of the organic fibers 20.
[0014] It is particularly preferable that the inorganic substance constituting the inorganic matrix portion 10 is an oxide. When the inorganic substance is an oxide of the above-mentioned metal element, a more durable composite member 100 can be obtained. The oxide of the metal element is preferably a compound in which only oxygen is bonded to the metal element.
[0015] The inorganic material constituting the inorganic matrix portion 10 is preferably polycrystalline. In other words, it is preferable that the inorganic material particles 11 are crystalline particles, and the inorganic matrix portion 10 is formed by agglomerating a large number of particles 11. By using the inorganic material constituting the inorganic matrix portion 10 as a polycrystalline material, it is possible to obtain a composite member 100 having high durability compared to a case where the inorganic material is amorphous. It is more preferable that the inorganic material particles 11 are crystalline particles containing at least one metal element selected from the group consisting of alkali metals, alkaline earth metals, transition metals, base metals, and semimetals. It is also preferable that the inorganic material particles 11 are crystalline particles containing at least one of the oxides and hydroxide oxides of the above metal elements. It is more preferable that the inorganic material particles 11 are crystalline particles containing at least one of the oxides and hydroxide oxides of the above metal elements as a main component.
[0016] The inorganic material constituting the inorganic matrix portion 10 is preferably boehmite. Boehmite is an aluminum oxyhydroxide represented by the formula AlOOH. Boehmite is insoluble in water and hardly reacts with acids or alkalis at room temperature, so it has high chemical stability, and has a high dehydration temperature of about 500°C, so it also has excellent heat resistance. In addition, since boehmite has a specific gravity of about 3.07, when the inorganic matrix portion 10 is made of boehmite, it is possible to obtain a composite member 100 that is lightweight and has excellent chemical stability.
[0017] When the inorganic material constituting the inorganic matrix portion 10 is boehmite, the particles 11 may be particles consisting of only a boehmite phase, or may be particles consisting of a mixed phase of boehmite and aluminum oxide or aluminum hydroxide other than boehmite. For example, the particles 11 may be particles consisting of a mixture of a phase consisting of boehmite and a phase consisting of gibbsite (Al(OH)3).
[0018] As described above, it is more preferable that the inorganic substance constituting the inorganic matrix portion 10 contains at least one of an oxide and an oxide hydroxide as a main component. Therefore, it is preferable that the inorganic matrix portion 10 also contains at least one of an oxide and an oxide hydroxide as a main component. In other words, it is preferable that the inorganic matrix portion 10 contains at least one of an oxide and an oxide hydroxide in an amount of 50 mol% or more, more preferably 80 mol% or more. However, it is preferable that the inorganic matrix portion 10 does not substantially contain hydrates. In this specification, "the inorganic matrix portion does not substantially contain hydrates" means that the inorganic matrix portion 10 is not intentionally made to contain hydrates. Therefore, when hydrates are mixed into the inorganic matrix portion 10 as unavoidable impurities, the condition "the inorganic matrix portion does not substantially contain hydrates" is satisfied. Note that boehmite is an oxyhydroxide, and is not included in the hydrates in this specification.
[0019] It is preferable that the inorganic substance constituting the inorganic matrix portion 10 does not contain a hydrate of a calcium compound. The calcium compounds referred to here are tricalcium silicate (alite, 3CaO·SiO2), dicalcium silicate (belite, 2CaO·SiO2), calcium aluminate (3CaO·Al2O3), calcium aluminoferrite (4CaO·Al2O3·Fe2O3), and calcium sulfate (CaSO4·2H2O). When the inorganic substance constituting the inorganic matrix portion 10 contains a hydrate of the calcium compound, the porosity of the cross section of the inorganic matrix portion of the obtained composite member may exceed 20%, resulting in a decrease in strength. Therefore, it is preferable that the inorganic substance does not contain a hydrate of the calcium compound. In addition, it is preferable that the inorganic substance constituting the inorganic matrix portion 10 does not contain phosphate cement, zinc phosphate cement, or calcium phosphate cement. When the inorganic substance does not contain these cements, the porosity of the cross section of the inorganic matrix portion decreases, thereby increasing the mechanical strength.
[0020] The average particle diameter of the inorganic particles 11 constituting the inorganic matrix portion 10 is not particularly limited. However, the average particle diameter of the particles 11 is preferably 300 nm or more and 50 μm or less, more preferably 300 nm or more and 30 μm or less, even more preferably 300 nm or more and 10 μm or less, and particularly preferably 300 nm or more and 5 μm or less. When the average particle diameter of the inorganic particles 11 is within this range, the particles 11 are firmly bonded to each other, and the strength of the inorganic matrix portion 10 can be increased. In addition, when the average particle diameter of the inorganic particles 11 is within this range, the ratio of pores present inside the inorganic matrix portion 10 is 20% or less, and therefore, it is possible to suppress oxidation deterioration of the organic fibers 20. In addition, in this specification, the value of "average particle diameter" is, unless otherwise specified, a value calculated as the average particle diameter of particles observed in several to several tens of fields of view using an observation means such as a scanning electron microscope (SEM) or a transmission electron microscope (TEM).
[0021] The shape of the inorganic particles 11 is not particularly limited, but may be, for example, spherical. The particles 11 may be whisker-like (needle-like) particles or scale-like particles. Compared with spherical particles, whisker-like particles or scale-like particles have a higher contact with other particles, and the strength of the inorganic matrix portion 10 is likely to be improved. Therefore, by using particles having such a shape as the particles 11, it is possible to increase the strength of the entire composite member 100. Note that, as the whisker-like particles 11, for example, particles containing at least one of zinc oxide (ZnO) and aluminum oxide (Al2O3) can be used.
[0022] As described above, in the composite member 100, the inorganic matrix portion 10 is preferably composed of a group of inorganic particles. That is, the inorganic matrix portion 10 is preferably composed of a plurality of particles 11 made of an inorganic material, and the inorganic particles 11 are preferably bonded to each other to form the inorganic matrix portion 10. In this case, the particles 11 may be in a state of point contact with each other, or may be in a state of surface contact in which the particle faces of the particles 11 are in contact with each other. The organic fibers 20 are preferably present in a state of being dispersed substantially uniformly inside the inorganic matrix portion 10. However, the organic fibers 20 are preferably present at the grain boundaries of the inorganic particles 11. As shown in FIG. 2, the organic fibers 20 are unevenly distributed between the adjacent inorganic particles 11, so that the organic fibers 20 are deformed so as to fill the gaps between the inorganic particles 11. Therefore, it is possible to further reduce the proportion of pores present inside the inorganic matrix portion 10.
[0023] In the composite member 100, when the inorganic matrix portion 10 is composed of a group of inorganic particles, an organic fiber 20 may be present between adjacent inorganic particles 11. However, as shown in FIG. 2, an amorphous portion 30 containing a non-crystalline inorganic compound may be present between adjacent inorganic particles 11 in addition to the organic fiber 20. The presence of the amorphous portion 30 bonds adjacent inorganic particles 11 to each other via the amorphous portion 30, so that the strength of the inorganic matrix portion 10 can be further increased. It is preferable that the amorphous portion 30 is present so as to be in contact with at least the surface of the inorganic particle 11. In addition to being present between adjacent inorganic particles 11, the amorphous portion 30 may be present between the inorganic particle 11 and the organic fiber 20, and between adjacent organic fibers 20.
[0024] The amorphous portion 30 preferably contains an amorphous inorganic compound. Specifically, the amorphous portion 30 may be a portion consisting of only an amorphous inorganic compound, or may be a portion consisting of a mixture of an amorphous inorganic compound and a crystalline inorganic compound. The amorphous portion 30 may also be a portion in which a crystalline inorganic compound is dispersed inside an amorphous inorganic compound.
[0025] The inorganic particle 11 and the amorphous portion 30 preferably contain the same metal element, and the metal element is at least one selected from the group consisting of alkali metals, alkaline earth metals, transition metals, base metals, and metalloids. In other words, the inorganic compound constituting the particle 11 and the amorphous inorganic compound constituting the amorphous portion 30 preferably contain at least the same metal element. In addition, the inorganic compound constituting the particle 11 and the amorphous inorganic compound constituting the amorphous portion 30 may have the same chemical composition, or may have different chemical compositions. Specifically, when the metal element is zinc, the inorganic compound constituting the particle 11 and the amorphous inorganic compound constituting the amorphous portion 30 may both be zinc oxide (ZnO). Alternatively, the inorganic compound constituting the particle 11 is ZnO, but the amorphous inorganic compound constituting the amorphous portion 30 may be a zinc-containing oxide other than ZnO.
[0026] In addition, when the amorphous portion 30 is a portion consisting of a mixture of amorphous inorganic compounds and crystalline inorganic compounds, the amorphous inorganic compounds and the crystalline inorganic compounds may have the same chemical composition or may have different chemical compositions.
[0027] In the composite material 100, the particles 11 and the amorphous portion 30 preferably contain an oxide of at least one metal element selected from the group consisting of alkali metals, alkaline earth metals, transition metals, base metals, and metalloids. Such an oxide of a metal element has high durability, and therefore can prevent the organic fibers 20 from contacting oxygen and water vapor for a long period of time, thereby suppressing deterioration of the organic fibers 20.
[0028] The oxide of the metal element contained in both the particles 11 and the amorphous portion 30 is preferably at least one selected from the group consisting of zinc oxide, magnesium oxide, and a complex of zinc oxide and magnesium oxide. As described later, by using the oxide of these metal elements, it becomes possible to form the amorphous portion 30 by a simple method.
[0029] As described above, the inorganic substance constituting the inorganic matrix portion 10 may be boehmite. In this case, the particles 11 of the inorganic matrix portion 10 may be particles consisting of only a boehmite phase, or may be particles consisting of a mixed phase of boehmite and aluminum oxide or aluminum hydroxide other than boehmite. In this case, it is preferable that adjacent particles 11 are bonded via at least one of an aluminum oxide and an aluminum hydroxide. In other words, it is preferable that the particles 11 are not bonded via an organic binder consisting of an organic compound, and are not bonded via an inorganic binder consisting of an inorganic compound other than an aluminum oxide and an aluminum hydroxide. In addition, when adjacent particles 11 are bonded via at least one of an aluminum oxide and an aluminum hydroxide, the aluminum oxide and the aluminum hydroxide may be crystalline or amorphous.
[0030] When the inorganic matrix part 10 is made of boehmite, the proportion of the boehmite phase is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more. By increasing the proportion of the boehmite phase, it is possible to obtain an inorganic matrix part 10 that is lightweight and has excellent chemical stability and heat resistance. The proportion of the boehmite phase in the inorganic matrix part 10 can be determined by measuring the X-ray diffraction pattern of the inorganic matrix part 10 by X-ray diffraction method and then performing Rietveld analysis.
[0031] In the composite material 100, the porosity in the cross section of the inorganic matrix portion 10 is preferably 20% or less. That is, when the cross section of the inorganic matrix portion 10 is observed, the average value of the ratio of pores per unit area is preferably 20% or less. When the porosity is 20% or less, the organic fibers 20 can be sealed inside the dense inorganic material. Therefore, the contact rate between the organic fibers 20 and oxygen and water vapor from the outside of the composite material 100 is reduced, so that corrosion of the organic fibers 20 can be suppressed and the characteristics of the organic fibers 20 can be maintained for a long period of time. The porosity in the cross section of the inorganic matrix portion 10 is preferably 15% or less, more preferably 10% or less, and even more preferably 5% or less. The smaller the porosity in the cross section of the inorganic matrix portion 10, the more the contact between the organic fibers 20 and oxygen and water vapor is suppressed, so that it is possible to prevent oxidation deterioration of the organic fibers 20.
[0032] In this specification, the porosity can be obtained as follows. First, the cross section of the inorganic matrix portion 10 is observed to distinguish the inorganic matrix portion 10, the organic fibers 20, and the pores. Then, the unit area and the area of the pores in the unit area are measured to obtain the ratio of the pores per unit area. After obtaining the ratio of the pores per unit area at a plurality of points, the average value of the ratio of the pores per unit area is defined as the porosity. When observing the cross section of the inorganic matrix portion 10, an optical microscope, a scanning electron microscope (SEM), or a transmission electron microscope (TEM) can be used. The unit area and the area of the pores in the unit area may be measured by binarizing an image observed by a microscope.
[0033] In the composite member 100, the organic fiber 20 is a fibrous material made of an organic compound, and has high strength based on its molecular weight. At least one of vegetable fiber and animal fiber can be used as such organic fiber 20. Examples of vegetable fiber include wood fiber, cotton, hemp, and kenaf. Examples of animal fiber include silk, wool, and cashmere.
[0034] Also, at least one of regenerated fibers, semi-synthetic fibers, and synthetic fibers may be used as the organic fibers 20. Examples of regenerated fibers include rayon and lyocell. Examples of semi-synthetic fibers include acetate and triacetate. Examples of synthetic fibers include polyamide fibers, polyester fibers, polyacrylonitrile fibers, polyolefin fibers, polyfluoroethylene fibers, polyvinyl chloride fibers, polyvinylidene chloride fibers, polyvinyl alcohol fibers, and polyurethane fibers.
[0035] The fiber length of the organic fibers 20 is not particularly limited, but is preferably 1 nm to 10 mm, and more preferably 10 nm to 1 mm. The fiber diameter of the organic fibers 20 is also not particularly limited, but is preferably 1 nm to 1 mm, and more preferably 5 nm to 500 μm. When the organic fibers 20 have such fiber length and fiber diameter, they are highly dispersed inside the inorganic matrix portion 10, and the mechanical strength of the composite material 100 can be further increased.
[0036] As described above, it is preferable that the organic fiber 20 is a petroleum-derived or plant-derived material. When the organic fiber 20 is a fiber obtained by processing petroleum or a fiber obtained by processing a plant, it is possible to obtain a composite member 100 suitable for industrial production because the fiber can be obtained stably.
[0037] The organic fibers 20 preferably have a hydrophilic surface. Specifically, the organic fibers 20 preferably have a hydrophilic functional group on the surface. Since the organic fibers 20 are hydrophilic, when water is used as a solvent in the manufacturing process of the composite member 100, the organic fibers 20 are less likely to aggregate, and the organic fibers 20 can be highly dispersed in the inorganic matrix portion 10. If necessary, the surfaces of the organic fibers 20 may be treated to make them hydrophilic. Specifically, the surfaces of the organic fibers 20 may be treated with a silane coupling agent to make them hydrophilic.
[0038] The organic fibers 20 are preferably cellulose nanofibers (CNF). Since cellulose nanofibers are characterized by being lightweight, high strength, and low thermal expansion, when dispersed inside the inorganic matrix portion 10, they adhere to the multiple particles 11 and suppress damage to the inorganic matrix portion 10. Furthermore, since cellulose nanofibers have a high affinity for water, when water is used as a solvent in the manufacturing process, the cellulose nanofibers are easily defibrated, enabling them to be highly dispersed in the inorganic matrix portion 10.
[0039] The cellulose nanofiber is not particularly limited, but it is preferable to use one obtained by a method that promotes nano-fibrillation of the raw material pulp. Specifically, the cellulose nanofiber may be a carboxymethylated cellulose nanofiber in which a carboxymethyl group has been introduced onto the surface. In addition, the cellulose nanofiber may be a TEMPO-oxidized cellulose nanofiber in which a carboxy group has been introduced onto the surface using TEMPO (2,2,6,6-tetramethylpiperidine-1-oxyl radical) as a catalyst.
[0040] In the composite member 100 of the present embodiment, as shown in FIG. 1, the organic fibers 20 are dispersed inside the inorganic matrix portion 10 in a state where they are directly fixed to the inorganic matrix portion 10. As described above, the inorganic matrix portion 10 itself is formed by bonding inorganic particles 11 together, so it has high hardness but is prone to brittle fracture. However, by dispersing the organic fibers 20 inside the inorganic matrix portion 10, the inorganic particles 11 are easily connected to each other by the organic fibers 20. In other words, by dispersing the organic fibers 20 in the inorganic matrix portion 10, the organic fibers 20 are entangled with each other and also with the particles 11. Therefore, even if an external force is applied to the inorganic matrix portion 10, the occurrence of cracks and the like can be suppressed. In addition, even if a crack occurs in the inorganic matrix portion 10, the organic fibers 20 are dispersed to connect the cracked surfaces and suppress the breakage of the inorganic matrix portion 10.
[0041] Moreover, the composite material 100 has a cross-sectional porosity of 20% or less. This reduces the contact rate between oxygen and water vapor and the organic fibers 20, thereby suppressing oxidative decomposition of the organic fibers 20 and enabling the mechanical strength of the composite material 100 to be maintained over a long period of time. Furthermore, the inorganic matrix portion 10 has few internal pores and the inorganic material is dense, allowing the composite material 100 to have high strength.
[0042] The shape of the composite member 100 is not particularly limited, but may be, for example, a plate shape. The thickness t of the composite member 100 (inorganic matrix portion 10) is also not particularly limited, but may be, for example, 50 μm or more. The thickness t of the composite member 100 may be 1 mm or more, and may also be 1 cm or more. The upper limit of the thickness t of the composite member 100 is not particularly limited, but may be, for example, 50 cm.
[0043] In the composite member 100, it is preferable that the organic fibers 20 are not present continuously from the surface 10a of the inorganic matrix portion 10 to the inside, and are not present in the form of a film on the surface 10a of the inorganic matrix portion 10. Specifically, it is preferable that the organic fibers 20 are present in a dispersed state inside the inorganic matrix portion 10. In addition, a part of the organic fibers 20 may be segregated inside the inorganic matrix portion 10. However, it is preferable that the organic fibers 20a are not present continuously from the surface 10a to the inside of the inorganic matrix portion 10 as shown in FIG. 3. The organic fibers 20a present on the surface 10a of the inorganic matrix portion 10 may be deteriorated by contact with oxygen and water vapor in the air. The organic fibers 20a present continuously from the surface 10a to the inside of the inorganic matrix portion 10 may also be deteriorated due to oxidative deterioration of the organic fibers 20a present on the surface 10a. Therefore, from the viewpoint of suppressing deterioration of the organic fibers 20, it is preferable that the organic fibers 20 are not present continuously from the surface 10a to the inside of the inorganic matrix portion 10.
[0044] In the composite member 100, it is preferable that the inorganic matrix portion 10 does not have voids 10b that communicate from the surface 10a to the inside of the inorganic matrix portion 10. The organic fibers 20 inside the inorganic matrix portion 10 are covered with inorganic particles 11, and therefore are not easily oxidized and deteriorated. However, as shown in FIG. 4, when voids 10b are present in the inorganic matrix portion 10, oxygen and water vapor may reach the inside of the inorganic matrix portion 10 through the voids 10b and come into contact with the organic fibers 20 inside the inorganic matrix portion 10. Therefore, from the viewpoint of suppressing the oxidative deterioration of the organic fibers 20, it is preferable that the inorganic matrix portion 10 does not have voids 10b that communicate from the surface 10a to the inside.
[0045] In the composite member 100, the inorganic matrix portion 10 preferably has a larger volume ratio than the organic fibers 20. Specifically, the ratio of the volume of the organic fibers 20 to the volume of the inorganic matrix portion 10 ([volume of organic fibers] / [volume of inorganic matrix portion]) is preferably less than 20%. By increasing the volume ratio of the inorganic matrix portion 10 compared to the organic fibers 20, the organic fibers 20 are more likely to be covered with inorganic particles 11. Therefore, from the viewpoint of further suppressing deterioration of the organic fibers 20, it is preferable that the inorganic matrix portion 10 has a larger volume ratio than the organic fibers 20.
[0046] Thus, the composite member 100 of the present embodiment includes an inorganic matrix portion 10 that is made of an inorganic material containing at least one of a metal oxide and a metal hydroxide oxide. The composite member 100 further includes organic fibers 20 that are directly fixed to the inorganic matrix portion 10 without using an adhesive material different from the inorganic material that constitutes the inorganic matrix portion 10 and that are dispersed within the inorganic matrix portion 10. The porosity of the cross section of the inorganic matrix portion 10 in the composite member 10 is 20% or less. In the composite member 100, the organic fibers 20 are dispersed within the inorganic matrix portion 10, so that the inorganic material particles 11 are connected to each other by the organic fibers 20, and the mechanical strength and toughness of the composite member 100 can be improved. Furthermore, since the porosity of the cross section of the composite member 100 is 20% or less, contact between oxygen and water vapor and the organic fibers 20 is suppressed, and the organic fibers 20 can be dispersed stably for a long period of time.
[0047] [Manufacturing method for composite materials] Next, a method for producing the composite member according to this embodiment will be described. The composite member can be produced by pressurizing and heating a mixture of inorganic particles and organic fibers 20 in a solvent-containing state. By using such a pressurizing and heating method, the inorganic substances are bonded to each other to form the inorganic matrix portion 10.
[0048] Specifically, first, a mixture is prepared by mixing an inorganic powder with the organic fibers 20. There is no particular limitation on the method of mixing the inorganic powder with the organic fibers 20, and the mixture can be performed by a dry method or a wet method. The inorganic powder and the organic fibers 20 may be mixed in air or in an inert atmosphere.
[0049] Here, the powder of the inorganic substance has an average particle diameter D 50Preferably, the particle diameter is in the range of 300 nm to 50 μm. Such inorganic substances are not only easy to handle, but also have a relatively large specific surface area, so that the contact area between particles becomes large when the mixture is pressurized. Therefore, it acts to increase the binding force between the inorganic substances, and it becomes possible to improve the density of the inorganic matrix portion 10.
[0050] Next, a solvent is added to the mixture. The solvent is not particularly limited, but for example, a solvent capable of dissolving a part of the inorganic substance when the mixture is pressurized and heated can be used. In addition, a solvent capable of reacting with the inorganic substance to generate an inorganic substance different from the inorganic substance can be used. As such a solvent, at least one selected from the group consisting of an acidic aqueous solution, an alkaline aqueous solution, water, an alcohol, a ketone, and an ester can be used. As the acidic aqueous solution, an aqueous solution having a pH of 1 to 3 can be used. As the alkaline aqueous solution, an aqueous solution having a pH of 10 to 14 can be used. As the acidic aqueous solution, an aqueous solution of an organic acid is preferably used. As the alcohol, an alcohol having a carbon number of 1 to 12 is preferably used.
[0051] Next, the mixture containing the inorganic material, the organic fibers 20, and the solvent is filled into the inside of the mold. After the mixture is filled into the mold, the mold may be heated as necessary. Then, pressure is applied to the mixture inside the mold, so that the inside of the mold is put into a high-pressure state. At this time, the inorganic material and the organic fibers 20 are densified, and at the same time, the particles of the inorganic material are bonded to each other.
[0052] Here, when a solvent that dissolves a part of the inorganic substance is used, the inorganic compound that constitutes the inorganic substance dissolves in the solvent under high pressure. The dissolved inorganic compound penetrates into the gaps between the inorganic substance and the organic fiber 20, the gaps between the inorganic substances, and the gaps between the organic fibers 20. Then, by removing the solvent in the mixture in this state, connections derived from the inorganic substance are formed between the inorganic substance and the organic fiber 20, between the inorganic substances, and between the organic fibers 20. Also, when a solvent that reacts with the inorganic substance to generate an inorganic substance different from the inorganic substance is used, the inorganic compound that constitutes the inorganic substance reacts with the solvent under high pressure. Then, the other inorganic substance generated by the reaction is filled into the gaps between the inorganic substance and the organic fiber 20, the gaps between the inorganic substances, and the gaps between the organic fibers 20, and connections derived from the other inorganic substance are formed.
[0053] The heating and pressurizing conditions of the mixture containing the inorganic substance, the organic fiber 20, and the solvent are not particularly limited as long as the dissolution of the surface of the inorganic substance proceeds when a solvent that dissolves a part of the inorganic substance is used. In addition, the heating and pressurizing conditions of the mixture are not particularly limited as long as the reaction between the inorganic substance and the solvent proceeds when a solvent that reacts with the inorganic substance to produce an inorganic substance different from the inorganic substance is used. For example, it is preferable to heat the mixture containing the inorganic substance, the organic fiber 20, and the solvent to 50 to 300°C, and then pressurize it at a pressure of 10 to 600 MPa. The temperature at which the mixture containing the inorganic substance, the organic fiber 20, and the solvent is heated is more preferably 80 to 250°C, and even more preferably 100 to 200°C. In addition, the pressure at which the mixture containing the inorganic substance, the organic fiber 20, and the solvent is pressurized is more preferably 50 to 400 MPa, and even more preferably 50 to 200 MPa. By limiting the heating temperature to within this range, it is possible to suppress the deterioration or loss of the organic fibers and obtain a desired composite member in which the inorganic matrix portion and the organic fibers are combined. Also, by limiting the pressure to within this range, it is possible to obtain a dense composite member in which internal distortion is suppressed.
[0054] The composite member can be obtained by removing the molded body from the inside of the mold. Note that the connection parts derived from the inorganic material, which are formed between the inorganic material and the organic fibers 20, between the inorganic materials, and between the organic fibers 20, are preferably the amorphous parts 30 described above.
[0055] Here, as a method for manufacturing an inorganic member made of ceramics, a sintering method has been conventionally known. The sintering method is a method for obtaining a sintered body by heating an aggregate of solid powder made of an inorganic substance at a temperature lower than the melting point. However, in the sintering method, the solid powder is heated to, for example, 1000°C or higher. Therefore, even if an attempt is made to obtain a composite member made of an inorganic substance and organic fibers using the sintering method, the organic fibers are carbonized by heating at a high temperature, and therefore the composite member cannot be obtained. However, in the manufacturing method for the composite member of this embodiment, a mixture obtained by mixing the powder of the inorganic substance and the organic fibers 20 is heated at a low temperature of 300°C or less, so that the organic fibers 20 are unlikely to be carbonized. Therefore, the organic fibers 20 can be directly fixed to the inorganic matrix portion 10 made of an inorganic substance.
[0056] Furthermore, in the manufacturing method of this embodiment, the mixture obtained by mixing the powder of the inorganic substance and the organic fibers 20 is pressurized while being heated, so that the inorganic substance aggregates to form a dense inorganic matrix portion 10. As a result, the number of pores inside the inorganic matrix portion 10 is reduced, and a composite member 100 having high strength can be obtained.
[0057] Next, a method for manufacturing the composite member 100 in which the inorganic material constituting the inorganic matrix portion 10 is boehmite will be described. The composite member 100 in which the inorganic material is boehmite can be manufactured by mixing hydraulic alumina, organic fibers 20, and a solvent containing water, and then pressurizing and heating the mixture. Hydraulic alumina is an oxide obtained by heat-treating aluminum hydroxide, and contains ρ-alumina. Such hydraulic alumina has the property of bonding and hardening through a hydration reaction. Therefore, by using a pressurized and heated method, the hydration reaction of hydraulic alumina progresses, and the hydraulic alumina bonds to each other, while the crystal structure changes to boehmite, and the inorganic matrix portion 10 can be formed.
[0058] Specifically, first, hydraulic alumina powder, organic fibers 20, and a water-containing solvent are mixed to prepare a mixture. The water-containing solvent is preferably pure water or ion-exchanged water. However, the water-containing solvent may contain an acidic substance or an alkaline substance in addition to water. Furthermore, the water-containing solvent may contain water as a main component, and may contain, for example, an organic solvent (e.g., alcohol, etc.).
[0059] The amount of the solvent added to the hydraulic alumina is preferably an amount that allows the hydration reaction of the hydraulic alumina to proceed sufficiently, and is preferably 20 to 200 mass % and more preferably 50 to 150 mass % relative to the hydraulic alumina.
[0060] Next, a mixture of hydraulic alumina, organic fibers 20, and a solvent containing water is filled into the inside of the mold. After the mixture is filled into the mold, the mold may be heated as necessary. Then, pressure is applied to the mixture inside the mold, and the inside of the mold is put into a high-pressure state. At this time, hydraulic alumina is highly packed, and the hydraulic alumina particles are bonded to each other, thereby increasing the density. Specifically, by adding water to hydraulic alumina, the hydraulic alumina undergoes a hydration reaction, and boehmite and aluminum hydroxide are generated on the surfaces of the hydraulic alumina particles. Then, by applying pressure to the mixture while heating it inside the mold, the generated boehmite and aluminum hydroxide diffuse between adjacent hydraulic alumina particles, and the hydraulic alumina particles are gradually bonded to each other. Thereafter, a dehydration reaction proceeds due to heating, and the crystal structure changes from aluminum hydroxide to boehmite. It is presumed that such hydration reaction of hydraulic alumina, mutual diffusion between hydraulic alumina particles, and dehydration reaction proceed almost simultaneously.
[0061] Then, by removing the molded body from inside the mold, a composite material 100 can be obtained in which the organic fibers 20 are fixed while the multiple particles 11 are bonded to each other via at least one of aluminum oxide and hydroxide oxide.
[0062] The heating and pressurizing conditions of the mixture of hydraulic alumina, organic fiber 20, and a solvent containing water are not particularly limited as long as the reaction between hydraulic alumina and the solvent proceeds. For example, it is preferable to pressurize the mixture of hydraulic alumina, organic fiber 20, and a solvent containing water at a pressure of 10 to 600 MPa while heating it to 50 to 300°C. The temperature at which the mixture of hydraulic alumina, organic fiber 20, and a solvent containing water is heated is more preferably 80 to 250°C, and even more preferably 100 to 200°C. The pressure at which the mixture of hydraulic alumina, organic fiber 20, and a solvent containing water is pressed is more preferably 50 to 600 MPa, and even more preferably 200 to 600 MPa.
[0063] As described above, the method for producing a composite member includes a step of mixing powder of an inorganic substance with organic fibers 20 to obtain a mixture, and a step of adding a solvent that dissolves the inorganic substance or a solvent that reacts with the inorganic substance to the mixture, and then pressurizing and heating the mixture. The heating and pressurizing conditions for the mixture are preferably a temperature of 50 to 300°C and a pressure of 10 to 600 MPa. In the production method of this embodiment, the composite member 100 is molded under such low-temperature conditions, so that carbonization of the organic fibers 20 is suppressed, and the organic fibers 20 can be directly fixed to the inorganic matrix portion 10.
[0064] Furthermore, a method for producing a composite member 100 in which the inorganic substance is boehmite includes a step of mixing hydraulic alumina, organic fibers 20, and a solvent containing water to obtain a mixture, and a step of pressurizing and heating the mixture. The heating and pressurizing conditions for the mixture are preferably a temperature of 50 to 300°C and a pressure of 10 to 600 MPa. In this production method, the composite member 100 is molded under low-temperature conditions, and therefore the obtained member is mainly composed of the boehmite phase. Therefore, a composite member 100 that is lightweight and has excellent chemical stability can be obtained by a simple method.
[0065] [Applications of composite materials] Next, applications of the composite member 100 according to this embodiment will be described. As described above, the composite member 100 has high mechanical strength and can be formed into a plate with a large thickness, and therefore can be used in structures. The structures including the composite member 100 are preferably housing equipment, housing components, building materials, and buildings. Housing equipment, housing components, building materials, and buildings are structures that are in high demand in people's lives, and therefore the use of the composite member 100 in structures can be expected to have the effect of creating a new, large market.
[0066] The composite member of this embodiment can be used as a building member. In other words, the building member of this embodiment includes the composite member 100. A building member is a member manufactured for construction, and in this embodiment, the composite member 100 can be used for at least a part of it. As described above, the composite member 100 can be made into a plate shape with a large thickness, and has high strength and durability. Therefore, the composite member 100 can be suitably used as a building member. Examples of building members include exterior wall materials (siding) and roofing materials. Examples of building members also include materials for roads and materials for exterior gutters.
[0067] Furthermore, the composite material of this embodiment can also be used as an interior material. In other words, the interior material of this embodiment includes the composite material 100. Examples of the interior material include a bathtub, a kitchen counter, a washstand, and a flooring material. EXAMPLES
[0068] The composite member of this embodiment will be described in more detail below with reference to examples, but this embodiment is not limited thereto.
[0069] [Preparation of test samples] Example 1 As inorganic particles, the average particle size D 50 Zinc oxide particles with a diameter of about 1 μm (manufactured by Kojundo Chemical Laboratory Co., Ltd., purity 99.99%) were prepared. In addition, cellulose nanofibers manufactured by Nippon Paper Industries Co., Ltd., Cellenpia (registered trademark) CS-01 (carboxymethylated cellulose nanofiber) were prepared as organic fibers. Then, cellulose nanofiber powder was weighed out so that it was 5% by volume relative to the zinc oxide particles, and the zinc oxide particles and organic fiber powder were mixed using an agate mortar and pestle to obtain a mixed powder.
[0070] Next, the obtained mixed powder was put into a cylindrical molding die (Φ10) having an internal space. Furthermore, 1M acetic acid was added to the mixed powder filled inside the molding die so that the amount was 20 mass% relative to the zinc oxide particles. Then, the mixed powder containing the acetic acid was heated and pressurized under conditions of 100 MPa, 150°C, and 30 minutes to obtain a test sample of this example.
[0071] Example 2 A test sample of this example was obtained in the same manner as in Example 1, except that the cellulose nanofiber powder was added so as to be 10% by volume relative to the zinc oxide particles.
[0072] Example 3 A test sample of this example was obtained in the same manner as in Example 1, except that the cellulose nanofiber powder was added so as to be 15% by volume relative to the zinc oxide particles.
[0073] Comparative Example 1 A test sample of this example was obtained in the same manner as in Example 1, except that no cellulose nanofiber powder was added.
[0074] The amounts of cellulose nanofibers added in the test samples of Examples 1 to 3 and Comparative Example 1 are summarized in Table 1.
[0075] [Table 1]
[0076] [Evaluation of test samples] (Bending strength measurement) The bending strength of each test sample was measured in accordance with the Japanese Industrial Standard JIS R1601 (room temperature bending strength test method for fine ceramics). The bending strength of the test sample was measured using the three-point bending strength test method of JIS R1601. The maximum stress value of each test sample is also shown in Table 1.
[0077] As shown in Table 1, it can be seen that the addition of cellulose nanofibers, which are organic fibers, increases the bending stress and improves the mechanical strength. In particular, when the amount of cellulose nanofibers added to zinc oxide is 5 to 10 volume %, it can be seen that the bending stress is improved by about 5 times compared to when cellulose nanofibers are not added.
[0078] (Density ratio measurement) First, the specific gravity was calculated from the volume and mass of the test sample of each example. Furthermore, the theoretical specific gravity of each test sample was calculated based on the specific gravity of zinc oxide being 5.6 and the specific gravity of cellulose nanofiber being 1.4. That is, in the case of the test sample of Example 1, the volume ratio of zinc oxide was 95% and the volume ratio of cellulose nanofiber was 5%, so the theoretical specific gravity was 5.6×0.95+1.4×0.05=5.39. The actual specific gravity relative to the theoretical specific gravity ([actual specific gravity] / [theoretical specific gravity]×100) was taken as the density ratio (%). The density ratio of each test sample is also shown in Table 1.
[0079] As shown in Table 1, as the amount of cellulose nanofiber added increases, the density ratio decreases. In other words, the actual specific gravity of the test sample decreases compared to the theoretical specific gravity. This is presumably because the pores increase as the proportion of cellulose nanofiber increases. Therefore, it is preferable to adjust the amount of organic fiber added so that the porosity does not exceed 20%.
[0080] (Porosity measurement) First, a cross-section of the cylindrical test sample of Example 2 was subjected to cross-section polisher processing (CP processing). Next, a secondary electron image of the cross-section of the test sample was observed at a magnification of 20,000 times using a scanning electron microscope (SEM). Secondary electron images obtained by observing three positions (positions 1 to 3) of the cross-section of the test sample of Example 2 are shown in Figures 5(a), 6(a), and 7(a). In the observed secondary electron images, the gray areas are zinc oxide (particles 11 of an inorganic substance), and the black areas are pores 40. Although not confirmed in Figures 5, 6, and 7, fine cellulose nanofibers are dispersed between the zinc oxide particles 11.
[0081] Next, the SEM images of the three fields of view were binarized to clarify the pores. The binarized images of the secondary electron images of Fig. 5(a), Fig. 6(a) and Fig. 7(a) are shown in Fig. 5(b), Fig. 6(b) and Fig. 7(b), respectively. The area ratio of the pores was calculated from the binarized images, and the average value was taken as the porosity. Specifically, from Fig. 5(b), the area ratio of the pores at position 1 was 4.6%. From Fig. 6(b), the area ratio of the pores at position 2 was 4.4%. From Fig. 7(b), the area ratio of the pores at position 3 was 1.6%. Therefore, the porosity of the test sample of Example 2 was 3.5%, which is the average value of the area ratio of the pores at positions 1 to 3.
[0082] 5, 6 and 7, it can be seen that since the porosity of the test sample of Example 2 is 20% or less, the organic fibers are prevented from coming into contact with the air and water vapor, and oxidation deterioration is suppressed.
[0083] The contents of this embodiment have been described above based on examples, but the present embodiment is not limited to these descriptions, and it will be obvious to those skilled in the art that various modifications and improvements are possible.
[0084] The entire contents of Patent Application No. 2019-178350 (filing date: September 30, 2019) are incorporated herein by reference. [Industrial Applicability]
[0085] According to the present disclosure, it is possible to provide a composite member which is stable over the long term and has excellent mechanical strength even when organic fibers are used. [Explanation of symbols]
[0086] 10 Inorganic matrix part 20 Organic Fiber 100 Composite Materials
Claims
1. an inorganic matrix portion formed by bonding together a plurality of particles of an inorganic material containing boehmite or zinc oxide as a main component; organic fibers derived from the inorganic material, directly bonded to the inorganic matrix portion via connecting portions formed between the inorganic material and the organic fibers, between the inorganic materials, and between the organic fibers, and further present in a dispersed state within the inorganic matrix portion; Equipped with the particles of the inorganic material are bonded to each other via connecting parts that are derived from the inorganic material and are formed between the inorganic material and the organic fibers, between the inorganic materials, and between the organic fibers; the inorganic matrix portion has a cross-sectional porosity of 20% or less; A composite member, wherein the inorganic material does not include a hydrate of a calcium compound.
2. The composite member according to claim 1 , wherein a ratio of a volume of the organic fibers to a volume of the inorganic matrix portion is less than 20%.
3. 3. The composite material according to claim 1, wherein the inorganic matrix portion has a cross-sectional porosity of 10% or less.
4. The composite member according to claim 1 , wherein the organic fibers are derived from petroleum or plants.
5. The composite member according to claim 1 , wherein the organic fiber is a cellulose nanofiber.
6. The composite member according to claim 1 , wherein the inorganic material is polycrystalline.
7. The composite member according to claim 1 , wherein the connecting portion is an amorphous portion containing a non-crystalline inorganic compound.
8. The composite member according to claim 7 , wherein the particles of the inorganic substance and the amorphous portion contain the same metal element.
Citation Information
Patent Citations
Laying repairing method for molten metal vessel
JP1983011378A
Hydraulic cement
JP1991115148A
Cement type arc resistant material and its production
JP1992130041A
Fe-cr alloy excellent in workability and pitting corrosion resistance
JP1994049604A
Inorganic plate and its production
JP1998101450A