Composite Materials

The composite member addresses the peeling and absorption limitations of previous structures by using an inorganic matrix with dispersed elastic bodies, achieving uniform impact absorption and durability through a dense, stable structure.

JP7555011B2Active Publication Date: 2024-09-24PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2021550435
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-30
Filing Date
2020-08-27
Publication Date
2024-09-24
Estimated Expiration
2040-08-27

AI Technical Summary

Technical Problem

Existing composite structures with ceramic and fiber bundles suffer from material mismatch in thermal expansion coefficients leading to peeling and limited impact absorption, particularly from the ceramic layer side, and have insufficient shock absorption properties.

Method used

A composite member comprising an inorganic matrix made of inorganic substances with dispersed elastic bodies, where the tensile modulus of the dispersion is between 100 Pa and 3.5 GPa, and a porosity of 20% or less, ensuring uniform impact absorption and stability over time.

Benefits of technology

The composite member effectively absorbs impacts from all directions, maintains structural integrity, and prevents peeling, with enhanced shock absorption and durability due to the dispersed elastic bodies and dense inorganic matrix.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555011000005
    Figure 0007555011000005
  • Figure 0007555011000007
    Figure 0007555011000007
  • Figure 0007555011000010
    Figure 0007555011000010
Patent Text Reader

Abstract

A composite member (100) equipped with an inorganic matrix section (10) comprising an inorganic material, and an elastic dispersion element (20) which is present in a dispersed state inside the inorganic matrix section (10), wherein the tensile elasticity of the material constituting the dispersion element (20) is 100Pa to 3.5GPa, inclusive. The porosity in a cross-section of the inorganic matrix section (10) of said composite member (100) is 20% or less.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composite member. [Background technology]

[0002] Ceramics are known to have high strength and high heat resistance, but are also difficult to distort. Therefore, when a load (shock) is applied to ceramics, their ability to absorb the load is small, and sudden destruction can occur. In order to improve these characteristics, research has been actively conducted into imparting shock absorption properties to ceramics.

[0003] Patent Document 1 discloses a composite structure that is lightweight, difficult to break, and has excellent shock absorption properties. Specifically, Patent Document 1 discloses a composite structure in which a fiber bundle layer in which composite fiber bodies are bundled and which is composed of a long core material and a coating layer that covers the outer periphery of the core material and has a different composition from the core material, and a single ceramic layer are laminated. It is described that this configuration allows the propagation direction of cracks generated by impact to be deflected by contact with the composite fiber body, thereby providing a high shock absorption effect. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2005-281035 A Summary of the Invention

[0005] However, in the composite structure of Patent Document 1, the fiber bundle layer and the single ceramic layer are made of different materials, which results in a difference in thermal expansion coefficient between them. Therefore, there is a possibility that the fiber bundle layer will peel off from the single ceramic layer after long-term use. Furthermore, since the composite structure of Patent Document 1 has a laminated structure, it has an effect of absorbing impacts from the fiber bundle layer side, but does not have sufficient effect of absorbing impacts from the single ceramic layer side. Therefore, the composite structure needs to be shaped so that the fiber bundle layer side can absorb impacts, which causes a problem that there are limitations on the impact absorbing shape.

[0006] The present invention has been made in view of the problems inherent in the conventional techniques, and an object of the present invention is to provide a composite member that is stable over a long period of time and capable of absorbing impact as a whole.

[0007] In order to solve the above problems, a composite member according to an embodiment of the present invention includes an inorganic matrix portion made of an inorganic substance, and an elastic dispersion portion that exists in a dispersed state inside the inorganic matrix portion, and the tensile modulus of the material that constitutes the dispersion portion is 100 Pa to 3.5 GPa. The composite member has a porosity of 20% or less in a cross section of the inorganic matrix portion. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a cross-sectional view that illustrates an example of a composite member according to this embodiment. [Diagram 2] Fig. 2(a) is a schematic enlarged view of a cross section of a composite member according to this embodiment, and Fig. 2(b) is a schematic cross-sectional view of the vicinity of grain boundaries of a particle group of an inorganic substance. [Diagram 3] FIG. 3 is a cross-sectional view that diagrammatically illustrates another example of a composite member according to the present embodiment. [Figure 4] FIG. 4 is a cross-sectional view that diagrammatically illustrates another example of a composite member according to the present embodiment. [Diagram 5]FIG. 5 is a schematic diagram for explaining a method for measuring the impact absorbency in Example 1. As shown in FIG. [Figure 6] Fig. 6(a) is a diagram showing a secondary electron image at position 1 in the test sample of Example 1-3, and Fig. 6(b) is a diagram showing binarized data of the secondary electron image at position 1 in the test sample of Example 1-3. [Figure 7] Fig. 7(a) is a diagram showing a secondary electron image at position 2 in the test sample of Example 1-3, and Fig. 7(b) is a diagram showing binarized data of the secondary electron image at position 2 in the test sample of Example 1-3. [Figure 8] Fig. 8(a) is a diagram showing a secondary electron image at position 3 in the test sample of Example 1-3, and Fig. 8(b) is a diagram showing binarized data of the secondary electron image at position 3 in the test sample of Example 1-3. [Figure 9] Fig. 9(a) is a diagram showing a secondary electron image at position 1 in the test sample of Example 2. Fig. 9(b) is a diagram showing binarized data of the secondary electron image at position 1 in the test sample of Example 2. [Figure 10] Fig. 10(a) is a diagram showing a secondary electron image at position 2 in the test sample of Example 2. Fig. 10(b) is a diagram showing binarized data of the secondary electron image at position 2 in the test sample of Example 2. [Figure 11] Fig. 11(a) is a diagram showing a secondary electron image at position 3 in the test sample of Example 2. Fig. 11(b) is a diagram showing binarized data of the secondary electron image at position 3 in the test sample of Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, a composite member according to the present embodiment will be described with reference to the drawings. Note that the dimensional ratios in the drawings are exaggerated for the convenience of explanation and may differ from the actual ratios.

[0010] [Composite material] As shown in Fig. 1, the composite member 100 of the present embodiment includes an inorganic matrix portion 10 made of an inorganic substance, and a dispersion 20 that exists in a dispersed state inside the inorganic matrix portion 10. As shown in Fig. 2, the inorganic matrix portion 10 is made of a plurality of particles 11 made of an inorganic substance, and the inorganic matrix portion 10 is formed by bonding the inorganic substance particles 11 to each other.

[0011] The inorganic material constituting the inorganic matrix portion 10 preferably contains at least one metal element selected from the group consisting of alkali metals, alkaline earth metals, transition metals, base metals, and metalloids. In this specification, the alkaline earth metals include calcium, strontium, barium, and radium, as well as beryllium and magnesium. The base metals include aluminum, zinc, gallium, cadmium, indium, tin, mercury, thallium, lead, bismuth, and polonium. The metalloids include boron, silicon, germanium, arsenic, antimony, and tellurium. Among these, it is preferable that the inorganic material contains at least one metal element selected from the group consisting of zinc, aluminum, and magnesium. The inorganic material containing these metal elements can easily form a connection portion derived from the inorganic material by a pressurized and heated method, as described below.

[0012] The inorganic substance preferably contains at least one of the oxides and hydroxide oxides of the above metal elements. The inorganic substance more preferably contains at least one of the oxides and hydroxide oxides of the above metal elements as a main component. That is, the inorganic substance preferably contains at least one of the oxides and hydroxide oxides of the above metal elements in an amount of 50 mol% or more, more preferably 80 mol% or more. The oxides of the above metal elements include phosphates, silicates, aluminates, and borates in addition to compounds in which only oxygen is bonded to a metal element. Since such inorganic substances are highly stable against oxygen and water vapor in the atmosphere, by dispersing the dispersion 20 inside the inorganic matrix portion 10, the contact of the dispersion 20 with oxygen and water vapor can be suppressed, and deterioration of the dispersion 20 can be suppressed.

[0013] It is particularly preferable that the inorganic substance constituting the inorganic matrix portion 10 is an oxide. When the inorganic substance is an oxide of the above-mentioned metal element, a more durable composite member 100 can be obtained. The oxide of the metal element is preferably a compound in which only oxygen is bonded to the metal element.

[0014] The inorganic material constituting the inorganic matrix portion 10 is preferably polycrystalline. In other words, it is preferable that the inorganic material particles 11 are crystalline particles, and the inorganic matrix portion 10 is formed by agglomerating a large number of particles 11. By using the inorganic material constituting the inorganic matrix portion 10 as a polycrystalline material, it is possible to obtain a composite member 100 having high durability compared to a case where the inorganic material is amorphous. It is more preferable that the inorganic material particles 11 are crystalline particles containing at least one metal element selected from the group consisting of alkali metals, alkaline earth metals, transition metals, base metals, and semimetals. It is also preferable that the inorganic material particles 11 are crystalline particles containing at least one of the oxides and hydroxide oxides of the above metal elements. It is more preferable that the inorganic material particles 11 are crystalline particles containing at least one of the oxides and hydroxide oxides of the above metal elements as a main component.

[0015] The inorganic material constituting the inorganic matrix portion 10 is preferably boehmite. Boehmite is an aluminum oxyhydroxide represented by the formula AlOOH. Boehmite is insoluble in water and hardly reacts with acids or alkalis at room temperature, so it has high chemical stability, and has a high dehydration temperature of about 500°C, so it also has excellent heat resistance. In addition, since boehmite has a specific gravity of about 3.07, when the inorganic matrix portion 10 is made of boehmite, it is possible to obtain a composite member 100 that is lightweight and has excellent chemical stability.

[0016] When the inorganic material constituting the inorganic matrix portion 10 is boehmite, the particles 11 may be particles consisting of only a boehmite phase, or may be particles consisting of a mixed phase of boehmite and aluminum oxide or aluminum hydroxide other than boehmite. For example, the particles 11 may be particles consisting of a mixture of a phase consisting of boehmite and a phase consisting of gibbsite (Al(OH)3).

[0017] In addition, it is preferable that the inorganic substance constituting the inorganic matrix portion 10 does not contain a hydrate of a calcium compound. The calcium compounds referred to here are tricalcium silicate (alite, 3CaO·SiO2), dicalcium silicate (belite, 2CaO·SiO2), calcium aluminate (3CaO·Al2O3), calcium aluminoferrite (4CaO·Al2O3·Fe2O3), and calcium sulfate (CaSO4·2H2O). When the inorganic substance constituting the inorganic matrix portion 10 contains a hydrate of the above calcium compound, the porosity of the cross section of the inorganic matrix portion obtained may exceed 20%. Therefore, it is preferable that the inorganic substance does not contain a hydrate of the above calcium compound. In addition, it is preferable that the inorganic substance constituting the inorganic matrix portion 10 does not contain phosphate cement, zinc phosphate cement, or calcium phosphate cement. By not including these cements in the inorganic substance, it is possible to make the porosity of the obtained composite member 20% or less.

[0018] The average particle diameter of the inorganic particles 11 constituting the inorganic matrix portion 10 is not particularly limited. However, the average particle diameter of the particles 11 is preferably 300 nm or more and 50 μm or less, more preferably 300 nm or more and 30 μm or less, even more preferably 300 nm or more and 10 μm or less, and particularly preferably 300 nm or more and 5 μm or less. When the average particle diameter of the inorganic particles 11 is within this range, the particles 11 are firmly bonded to each other, and the strength of the inorganic matrix portion 10 can be increased. In addition, when the average particle diameter of the inorganic particles 11 is within this range, the ratio of pores present inside the inorganic matrix portion 10 is 20% or less, as described later, and therefore deterioration of the dispersion 20 can be suppressed. In addition, in this specification, the value of "average particle diameter" is a value calculated as the average particle diameter of particles observed in several to several tens of fields of view using an observation means such as a scanning electron microscope (SEM) or a transmission electron microscope (TEM), unless otherwise specified.

[0019] The shape of the inorganic particles 11 is not particularly limited, but may be, for example, spherical. The particles 11 may be whisker-like (needle-like) particles or scale-like particles. Compared with spherical particles, whisker-like particles or scale-like particles have a higher contact with other particles, and the strength of the inorganic matrix portion 10 is likely to be improved. Therefore, by using particles having such a shape as the particles 11, it is possible to increase the strength of the entire composite member 100. Note that, as the whisker-like particles 11, for example, particles containing at least one of zinc oxide (ZnO) and aluminum oxide (Al2O3) can be used.

[0020] The dispersion 20 dispersed inside the inorganic matrix portion 10 is preferably made of an elastic material. By dispersing the elastic dispersion 20 inside the inorganic matrix portion 10, it is possible to improve the impact absorption of the composite material 100. In other words, by dispersing the dispersion 20 inside, the composite material 100 becomes more likely to deform when a load (impact) is applied from the outside, and therefore it becomes possible to reduce and absorb the load.

[0021] In the composite member 100, the tensile modulus of the material constituting the dispersion 20 is preferably 100 Pa or more and 3.5 GPa or less. The tensile modulus of the material constituting the dispersion 20 is more preferably 1000 Pa or more and 0.5 GPa or less. By using a dispersion 20 having such a tensile modulus, the inorganic matrix portion 10 becomes easily deformed, and the impact absorption of the composite member 100 can be improved. The tensile modulus of the material constituting the dispersion 20 can be measured in accordance with Japanese Industrial Standard JIS K7161-1.

[0022] The material constituting the dispersion 20 is not particularly limited as long as it satisfies the above-mentioned tensile modulus, but the material is preferably a resin. In other words, the dispersion 20 preferably contains a resin, and more preferably has a resin as the main component. When the dispersion 20 is made of a resin, the resin is more likely to absorb impacts and vibrations through the inorganic matrix portion 10, and the inorganic matrix portion 10 is more likely to deform, so that it is possible to improve the impact absorption of the composite member 100. The resin constituting the dispersion 20 is not particularly limited as long as it satisfies the above-mentioned tensile modulus, but at least one of the resins shown in Tables 1 and 2 can be used, for example. Tables 1 and 2 also show typical tensile moduli of each resin in a state where no filler is added.

[0023] [Table 1]

[0024] [Table 2]

[0025] As described above, in the composite member 100, the inorganic matrix portion 10 is preferably composed of a group of inorganic particles. That is, the inorganic matrix portion 10 is preferably composed of a plurality of particles 11 made of an inorganic material, and the inorganic particles 11 are preferably bonded to each other to form the inorganic matrix portion 10. In this case, the particles 11 may be in a state of point contact with each other, or may be in a state of surface contact in which the particle surfaces of the particles 11 are in contact with each other. The dispersion 20 is preferably present in a state of being dispersed substantially uniformly inside the inorganic matrix portion 10. However, the dispersion 20 is preferably present at the grain boundaries of the inorganic particles 11. As shown in FIG. 2, the dispersion 20 is unevenly distributed between the adjacent inorganic particles 11, and the dispersion 20 is deformed so as to fill the gaps between the inorganic particles 11. Therefore, it is possible to further reduce the proportion of pores present inside the inorganic matrix portion 10.

[0026] In the composite member 100, when the inorganic matrix portion 10 is composed of a group of inorganic particles, the dispersion 20 may be present between adjacent inorganic particles 11. However, as shown in FIG. 2, in addition to the dispersion 20, an amorphous portion 30 containing an amorphous inorganic compound may be present between adjacent inorganic particles 11. The presence of the amorphous portion 30 bonds adjacent inorganic particles 11 to each other via the amorphous portion 30, so that the strength of the inorganic matrix portion 10 can be further increased. It is preferable that the amorphous portion 30 is present so as to be in contact with at least the surface of the inorganic particle 11. In addition to being present between adjacent inorganic particles 11, the amorphous portion 30 may be present between the inorganic particle 11 and the dispersion 20, and between adjacent dispersions 20.

[0027] The amorphous portion 30 preferably contains an amorphous inorganic compound. Specifically, the amorphous portion 30 may be a portion consisting of only an amorphous inorganic compound, or may be a portion consisting of a mixture of an amorphous inorganic compound and a crystalline inorganic compound. The amorphous portion 30 may also be a portion in which a crystalline inorganic compound is dispersed inside an amorphous inorganic compound.

[0028] The inorganic particle 11 and the amorphous portion 30 preferably contain the same metal element, and the metal element is at least one selected from the group consisting of alkali metals, alkaline earth metals, transition metals, base metals, and metalloids. In other words, the inorganic compound constituting the particle 11 and the amorphous inorganic compound constituting the amorphous portion 30 preferably contain at least the same metal element. In addition, the inorganic compound constituting the particle 11 and the amorphous inorganic compound constituting the amorphous portion 30 may have the same chemical composition, or may have different chemical compositions. Specifically, when the metal element is zinc, the inorganic compound constituting the particle 11 and the amorphous inorganic compound constituting the amorphous portion 30 may both be zinc oxide (ZnO). Alternatively, the inorganic compound constituting the particle 11 is ZnO, but the amorphous inorganic compound constituting the amorphous portion 30 may be a zinc-containing oxide other than ZnO.

[0029] In addition, when the amorphous portion 30 is a portion consisting of a mixture of amorphous inorganic compounds and crystalline inorganic compounds, the amorphous inorganic compounds and the crystalline inorganic compounds may have the same chemical composition or may have different chemical compositions.

[0030] In the composite material 100, the particles 11 and the amorphous portion 30 preferably contain an oxide of at least one metal element selected from the group consisting of alkali metals, alkaline earth metals, transition metals, base metals, and metalloids. Such oxides of metal elements are highly durable, and therefore can prevent the dispersion 20 from coming into contact with oxygen and water vapor for a long period of time, thereby preventing deterioration of the dispersion 20.

[0031] The oxide of the metal element contained in both the particles 11 and the amorphous portion 30 is preferably at least one selected from the group consisting of zinc oxide, magnesium oxide, and a complex of zinc oxide and magnesium oxide. As described later, by using the oxide of these metal elements, it becomes possible to form the amorphous portion 30 by a simple method.

[0032] As described above, the inorganic substance constituting the inorganic matrix portion 10 may be boehmite. In this case, the particles 11 of the inorganic matrix portion 10 may be particles consisting of only a boehmite phase, or may be particles consisting of a mixed phase of boehmite and aluminum oxide or aluminum hydroxide other than boehmite. In this case, it is preferable that adjacent particles 11 are bonded via at least one of an aluminum oxide and an aluminum hydroxide. In other words, it is preferable that the particles 11 are not bonded via an organic binder consisting of an organic compound, and are not bonded via an inorganic binder consisting of an inorganic compound other than an aluminum oxide and an aluminum hydroxide. In addition, when adjacent particles 11 are bonded via at least one of an aluminum oxide and an aluminum hydroxide, the aluminum oxide and the aluminum hydroxide may be crystalline or amorphous.

[0033] When the inorganic matrix part 10 is made of boehmite, the proportion of the boehmite phase is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more. By increasing the proportion of the boehmite phase, it is possible to obtain an inorganic matrix part 10 that is lightweight and has excellent chemical stability and heat resistance. The proportion of the boehmite phase in the inorganic matrix part 10 can be determined by measuring the X-ray diffraction pattern of the inorganic matrix part 10 by X-ray diffraction method and then performing Rietveld analysis.

[0034] In the composite member 100, the porosity in the cross section of the inorganic matrix portion 10 is preferably 20% or less. That is, when the cross section of the inorganic matrix portion 10 is observed, the average value of the ratio of pores per unit area is preferably 20% or less. When the porosity is 20% or less, the dispersion 20 can be sealed inside the dense inorganic material. Therefore, the contact rate between the dispersion 20 and oxygen and water vapor from the outside of the composite member 100 is reduced, so that it is possible to suppress oxidative decomposition of the dispersion 20 and maintain the elasticity of the dispersion 20 for a long period of time. The porosity in the cross section of the inorganic matrix portion 10 is preferably 15% or less, more preferably 10% or less, and even more preferably 5% or less. The smaller the porosity in the cross section of the inorganic matrix portion 10, the more the contact between the dispersion 20 and oxygen and water vapor is suppressed, so that it is possible to prevent deterioration of the dispersion 20.

[0035] In this specification, the porosity can be obtained as follows. First, the cross section of the inorganic matrix portion 10 is observed to distinguish the inorganic matrix portion 10, the dispersion 20, and the pores. Then, the unit area and the area of ​​the pores in the unit area are measured to obtain the ratio of the pores per unit area. After obtaining the ratio of the pores per unit area at multiple points, the average value of the ratio of the pores per unit area is defined as the porosity. When observing the cross section of the inorganic matrix portion 10, an optical microscope, a scanning electron microscope (SEM), or a transmission electron microscope (TEM) can be used. In addition, the unit area and the area of ​​the pores in the unit area may be measured by binarizing an image observed with a microscope.

[0036] The shape of the composite member 100 is not particularly limited, but may be, for example, a plate-like shape. The thickness t of the composite member 100 (inorganic matrix portion 10) is not particularly limited, but may be, for example, 50 μm or more. As described below, the composite member 100 is formed by a pressurized and heated method, so that a thick composite member 100 can be easily obtained. The thickness t of the composite member 100 (inorganic matrix portion 10) may be 1 mm or more, and may also be 1 cm or more. The upper limit of the thickness t of the composite member 100 (inorganic matrix portion 10) is not particularly limited, but may be, for example, 50 cm.

[0037] In the composite member 100, it is preferable that the dispersion 20 does not exist continuously from the surface 10a of the inorganic matrix portion 10 to the inside, and does not exist in a film form on the surface 10a of the inorganic matrix portion 10. Specifically, it is preferable that the dispersion 20 exists in a dispersed state inside the inorganic matrix portion 10. In addition, a part of the dispersion 20 may segregate inside the inorganic matrix portion 10. However, as shown in FIG. 3, it is preferable that the segregated dispersion 20a does not exist continuously from the surface 10a to the inside of the inorganic matrix portion 10. When the dispersion 20a is made of a resin, the dispersion 20a existing on the surface 10a of the inorganic matrix portion 10 may be deteriorated by contact with oxygen and water vapor in the air. The dispersion 20a existing continuously from the surface 10a to the inside of the inorganic matrix portion 10 may also be deteriorated due to oxidative deterioration of the dispersion 20a existing on the surface 10a. Therefore, from the viewpoint of suppressing deterioration of the dispersion 20, it is preferable that the dispersion 20 does not exist continuously from the surface 10a to the inside of the inorganic matrix portion 10.

[0038] Moreover, with regard to the dispersion 20 dispersed in the inorganic matrix part 10, it is preferable that a part of the dispersion 20 is not present in a film form on the surface 10a of the inorganic matrix part 10. When the dispersion 20 is made of a resin, the film-like dispersion 20 is exposed to oxygen and water vapor in the air, and therefore may be oxidized and deteriorated.

[0039] In the composite member 100, it is preferable that the inorganic matrix portion 10 does not have voids 10b that communicate from the surface 10a to the inside of the inorganic matrix portion 10. The dispersion 20 inside the inorganic matrix portion 10 is covered with inorganic particles 11, and is therefore unlikely to be oxidized and deteriorated. However, as shown in FIG. 4, when voids 10b are present in the inorganic matrix portion 10, oxygen and water vapor may reach the inside of the inorganic matrix portion 10 through the voids 10b and come into contact with the dispersion 20 inside the inorganic matrix portion 10. Therefore, from the viewpoint of suppressing the oxidative deterioration of the dispersion 20, it is preferable that the inorganic matrix portion 10 does not have voids 10b that communicate from the surface 10a to the inside.

[0040] Thus, the composite member 100 of the present embodiment includes an inorganic matrix portion 10 made of an inorganic substance, and a dispersion 20 that exists in a dispersed state inside the inorganic matrix portion 10 and has elasticity. The material that constitutes the dispersion 20 has a tensile modulus of 100 Pa or more and 3.5 GPa or less. The composite member 100 has a porosity of 20% or less in the cross section of the inorganic matrix portion 10. In the composite member 100, the dispersion 20 having a predetermined tensile modulus is dispersed inside the inorganic matrix portion 10, thereby increasing the elasticity of the entire composite member 100. Therefore, even if an impact is applied from the outside, the composite member 100 can deform in response to the impact and absorb the impact. In addition, since the dispersion 20 is dispersed throughout the inorganic matrix portion 10, the composite member 100 as a whole has impact absorption properties. Therefore, the composite member 100 can absorb impacts from all directions.

[0041] Moreover, the composite material 100 has a cross-sectional porosity of 20% or less. This reduces the contact rate between oxygen and water vapor and the dispersion 20, thereby suppressing oxidative decomposition of the dispersion 20 and enabling the elasticity of the composite material 100 to be maintained for a long period of time. Furthermore, the inorganic matrix portion 10 has few internal pores and the inorganic material is dense, allowing the composite material 100 to have high strength.

[0042] As described above, in the composite fiber body of Patent Document 1, the fiber bundle layer may peel off due to the difference in thermal expansion coefficient between the fiber bundle layer and the single ceramic layer. However, in the composite member 100, the dispersion 20 is highly dispersed inside the inorganic matrix portion 10, so that the peeling problem is unlikely to occur. In other words, in the composite member 100, the inorganic matrix portion 10 is arranged so as to encase the dispersion 20, so that the entire surface of the dispersion 20 comes into contact with the inorganic matrix portion 10. As a result, the contact area between the inorganic matrix portion 10 and the dispersion 20 increases, so that peeling between them is suppressed, and high stability can be maintained for a long period of time.

[0043] In the composite member 100, the Young's modulus of the material constituting the inorganic matrix portion 10 is preferably greater than that of the material constituting the dispersion 20. Since the inorganic matrix portion 10 itself is made of an inorganic substance, it has a large Young's modulus and is difficult to distort, making it difficult to absorb impact. However, since the Young's modulus between the inorganic matrix portion 10 and the dispersion 20 is in such a relationship, impact through the inorganic matrix portion is easily absorbed by the dispersion, and the inorganic matrix portion is easily deformed, making it possible to absorb the impact. The Young's modulus can be determined by a tensile test at room temperature.

[0044] In the composite material 100, the dispersion 20 preferably contains a resin, and the inorganic substance is at least one of a metal oxide and a metal oxide hydroxide. When the dispersion 20 is made of a resin, the impact through the inorganic matrix portion 10 is easily absorbed by the dispersion 20, and the inorganic matrix portion 10 is easily deformed, so that it is possible to improve the impact absorption of the composite material 100. In addition, metal oxides and metal oxide hydroxides are highly stable against oxygen and water vapor in the atmosphere. Therefore, when the inorganic substance of the inorganic matrix portion is made of a metal oxide and a metal oxide hydroxide, the oxygen permeability of the inorganic matrix portion is reduced and the gas barrier property is improved, so that the contact of the dispersion with oxygen and water vapor can be suppressed, and deterioration of the dispersion can be suppressed.

[0045] In the composite material 100, the inorganic matrix portion 10 preferably has a larger volume ratio than the dispersion 20. By increasing the volume ratio of the inorganic matrix portion 10 compared to the dispersion 20, the dispersion 20 is more likely to be surrounded by the inorganic particles 11. Therefore, from the viewpoint of further suppressing deterioration of the dispersion 20, it is preferable that the inorganic matrix portion 10 has a larger volume ratio than the dispersion 20.

[0046] [Manufacturing method for composite materials] Next, a method for producing the composite member 100 according to this embodiment will be described. The composite member 100 can be produced by pressurizing and heating a mixture of inorganic particles and dispersion 20 in a state containing a solvent. By using such a pressurizing and heating method, the inorganic substances are bonded to each other, so that an inorganic matrix portion 10 having the dispersion 20 dispersed therein can be formed.

[0047] Specifically, first, a mixed powder is prepared by mixing a powder of the inorganic substance with a powder of the dispersion body 20. The method of mixing the powder of the inorganic substance with the powder of the dispersion body 20 is not particularly limited, and the powder can be mixed in a dry or wet manner. The powder of the inorganic substance and the powder of the dispersion body 20 may be mixed in air or in an inert atmosphere.

[0048] Next, a solvent is added to the mixed powder. The solvent is not particularly limited, but for example, a solvent capable of dissolving a part of the inorganic substance when the mixed powder is pressurized and heated can be used. In addition, a solvent capable of reacting with the inorganic substance to generate an inorganic substance different from the inorganic substance can be used. As such a solvent, at least one selected from the group consisting of an acidic aqueous solution, an alkaline aqueous solution, water, an alcohol, a ketone, and an ester can be used. As the acidic aqueous solution, an aqueous solution having a pH of 1 to 3 can be used. As the alkaline aqueous solution, an aqueous solution having a pH of 10 to 14 can be used. As the acidic aqueous solution, an aqueous solution of an organic acid is preferably used. As the alcohol, an alcohol having a carbon number of 1 to 12 is preferably used.

[0049] The mixture containing the inorganic substance, the dispersion 20, and the solvent can be prepared by mixing the powder of the inorganic substance and the powder of the dispersion 20, and then adding the solvent, as described above. However, the method of preparing the mixture containing the inorganic substance, the dispersion 20, and the solvent is not limited to this method. In the method of preparing the mixture, the dispersion 20 and the solvent are first mixed. At this time, the dispersion 20 may or may not be dissolved in the solvent. Then, the powder of the inorganic substance may be added to the mixture of the dispersion 20 and the solvent to prepare the mixture containing the inorganic substance, the dispersion 20, and the solvent.

[0050] Next, the mixture containing the inorganic material, the dispersion 20, and the solvent is filled into the inside of the mold. After the mixture is filled into the mold, the mold may be heated as necessary. Then, pressure is applied to the mixture inside the mold, so that the inside of the mold is put into a high-pressure state. At this time, the inorganic material and the dispersion 20 are densified, and at the same time, the particles of the inorganic material are bonded to each other.

[0051] Here, when a solvent that dissolves a part of the inorganic substance is used, the inorganic compound that constitutes the inorganic substance dissolves in the solvent under high pressure. The dissolved inorganic compound penetrates into the gaps between the inorganic substance and the dispersion 20, the gaps between the inorganic substances, and the gaps between the dispersions 20. Then, by removing the solvent in the mixture in this state, connections derived from the inorganic substance are formed between the inorganic substance and the dispersion 20, between the inorganic substances, and between the dispersions 20. Also, when a solvent that reacts with the inorganic substance to generate an inorganic substance different from the inorganic substance is used, the inorganic compound that constitutes the inorganic substance reacts with the solvent under high pressure. Then, the other inorganic substance generated by the reaction is filled into the gaps between the inorganic substance and the dispersion 20, the gaps between the inorganic substances, and the gaps between the dispersions 20, and connections derived from the other inorganic substance are formed.

[0052] The heating and pressurizing conditions of the mixture containing the inorganic substance, the dispersion 20, and the solvent are not particularly limited as long as the dissolution of the surface of the inorganic substance proceeds when a solvent that dissolves a part of the inorganic substance is used. In addition, the heating and pressurizing conditions of the mixture are not particularly limited as long as the reaction between the inorganic substance and the solvent proceeds when a solvent that reacts with the inorganic substance to produce an inorganic substance different from the inorganic substance is used. For example, it is preferable to heat the mixture containing the inorganic substance, the dispersion 20, and the solvent to 50 to 300°C, and then pressurize it at a pressure of 10 to 600 MPa. The temperature at which the mixture containing the inorganic substance, the dispersion 20, and the solvent is heated is more preferably 80 to 250°C, and even more preferably 100 to 200°C. In addition, the pressure at which the mixture containing the inorganic substance, the dispersion 20, and the solvent is pressurized is more preferably 50 to 400 MPa, and even more preferably 50 to 200 MPa.

[0053] Then, the molded body is removed from the inside of the mold to obtain the composite material 100. Note that the connection parts derived from the inorganic substance, which are formed between the inorganic substance and the dispersion 20, between the inorganic substances, and between the dispersions 20, are preferably the amorphous parts 30 described above.

[0054] Here, as a method for manufacturing an inorganic member made of ceramics, a sintering method has been conventionally known. The sintering method is a method for obtaining a sintered body by heating an aggregate of solid powder made of an inorganic substance at a temperature lower than the melting point. However, in the sintering method, the solid powder is heated to, for example, 1000°C or higher. Therefore, even if an attempt is made to obtain a composite member made of an inorganic substance and a resin dispersion using the sintering method, the dispersion is carbonized by heating at a high temperature, and therefore the composite member cannot be obtained. However, in the manufacturing method of the composite member 100 of this embodiment, a mixture obtained by mixing a powder of an inorganic substance and a powder of the dispersion 20 is heated at a low temperature of 300°C or less, so that the carbonization of the dispersion 20 is unlikely to occur. Therefore, the dispersion 20 can be stably dispersed inside the inorganic matrix portion 10 made of an inorganic substance, and impact absorption properties can be imparted.

[0055] Furthermore, in the manufacturing method of the present embodiment, the mixture obtained by mixing the powder of the inorganic substance and the powder of the dispersion 20 is pressurized while being heated, so that the inorganic substance aggregates to form a dense inorganic matrix portion 10. As a result, the number of pores inside the inorganic matrix portion 10 is reduced, so that the composite member 100 having high strength can be obtained while suppressing the oxidative deterioration of the dispersion 20.

[0056] Next, a method for producing the composite member 100 in which the inorganic material constituting the inorganic matrix portion 10 is boehmite will be described. The composite member 100 in which the inorganic material is boehmite can be produced by mixing hydraulic alumina, the dispersion 20, and a solvent containing water, and then pressurizing and heating the mixture. Hydraulic alumina is an oxide obtained by heat-treating aluminum hydroxide, and contains ρ-alumina. Such hydraulic alumina has the property of bonding and hardening through a hydration reaction. Therefore, by using a pressurized heating method, the hydration reaction of hydraulic alumina progresses, and the hydraulic alumina bonds to each other, while the crystal structure changes to boehmite, and the composite member 100 can be formed.

[0057] Specifically, first, a mixture is prepared by mixing hydraulic alumina powder, the dispersion 20, and a water-containing solvent. The water-containing solvent is preferably pure water or ion-exchanged water. However, the water-containing solvent may contain an acidic substance or an alkaline substance in addition to water. Furthermore, the water-containing solvent may contain water as a main component, and may contain, for example, an organic solvent (e.g., alcohol, etc.).

[0058] The amount of the solvent added to the hydraulic alumina is preferably an amount that allows the hydration reaction of the hydraulic alumina to proceed sufficiently, and is preferably 20 to 200 mass % and more preferably 50 to 150 mass % relative to the hydraulic alumina.

[0059] Next, a mixture of hydraulic alumina, the dispersion 20, and a solvent containing water is filled into the inside of a mold. After the mixture is filled into the mold, the mold may be heated as necessary. Then, pressure is applied to the mixture inside the mold, and the inside of the mold is put into a high-pressure state. At this time, hydraulic alumina is highly packed, and the hydraulic alumina particles are bonded to each other, thereby increasing the density. Specifically, by adding water to hydraulic alumina, the hydraulic alumina undergoes a hydration reaction, and boehmite and aluminum hydroxide are generated on the surface of the hydraulic alumina particles. Then, by applying pressure to the mixture while heating it inside the mold, the generated boehmite and aluminum hydroxide diffuse between adjacent hydraulic alumina particles, and the hydraulic alumina particles are gradually bonded to each other. Thereafter, a dehydration reaction proceeds due to heating, and the crystal structure changes from aluminum hydroxide to boehmite. It is presumed that such hydration reaction of hydraulic alumina, mutual diffusion between hydraulic alumina particles, and dehydration reaction proceed almost simultaneously.

[0060] Then, by removing the molded body from inside the mold, a composite material 100 can be obtained in which the dispersion 20 is highly dispersed while multiple particles 11 are bonded to each other via at least one of aluminum oxide and hydroxide oxide.

[0061] The heating and pressurizing conditions of the mixture obtained by mixing hydraulic alumina, the dispersion 20, and the solvent containing water are not particularly limited as long as the reaction between hydraulic alumina and the solvent proceeds. For example, it is preferable to pressurize the mixture obtained by mixing hydraulic alumina, the dispersion 20, and the solvent containing water at a pressure of 10 to 600 MPa while heating it to 50 to 300°C. The temperature at which the mixture obtained by mixing hydraulic alumina, the dispersion 20, and the solvent containing water is heated is more preferably 80 to 250°C, and even more preferably 100 to 200°C. The pressure at which the mixture obtained by mixing hydraulic alumina, the dispersion 20, and the solvent containing water is pressurized is more preferably 50 to 600 MPa, and even more preferably 200 to 600 MPa.

[0062] Thus, the manufacturing method of the composite member 100 includes a step of mixing the powder of the inorganic substance with the powder of the dispersion 20 to obtain a mixture, and a step of adding a solvent that dissolves the inorganic substance or a solvent that reacts with the inorganic substance to the mixture, and then pressurizing and heating the mixture. The manufacturing method of the composite member 100 also includes a step of mixing the dispersion 20 with a solvent that dissolves the inorganic substance or a solvent that reacts with the inorganic substance, a step of mixing the powder of the inorganic substance with a solvent containing the dispersion 20 to obtain a mixture, and a step of pressurizing and heating the mixture. The heating and pressurizing conditions of the mixture are preferably a temperature of 50 to 300°C and a pressure of 10 to 600 MPa. In the manufacturing method of the present embodiment, the composite member 100 is molded under such low-temperature conditions, so that carbonization of the dispersion 20 is suppressed and a ceramic member having impact absorption properties can be obtained.

[0063] Furthermore, a method for producing a composite member 100 in which the inorganic substance is boehmite includes a step of mixing hydraulic alumina, the dispersion 20, and a solvent containing water to obtain a mixture, and a step of pressurizing and heating the mixture. The heating and pressurizing conditions for the mixture are preferably a temperature of 50 to 300°C and a pressure of 10 to 600 MPa. In this production method, the composite member 100 is molded under low-temperature conditions, and therefore the obtained member is mainly composed of the boehmite phase. Therefore, a composite member 100 that is lightweight and has excellent chemical stability can be obtained by a simple method.

[0064] [Applications of composite materials] Next, the use of the composite member 100 according to this embodiment will be described. As described above, the composite member 100 according to this embodiment can be formed into a thick plate, and is also excellent in shock absorption. In addition, the composite member 100 has high mechanical strength, and can be cut in the same way as general ceramic members, and can also be surface-treated. Therefore, the composite member 100 can be suitably used as an indoor structural member. Specifically, the composite member 100 can absorb the shock when a person falls, and therefore can be used as a flooring material, for example, a flooring material for a water area or a flooring material for a bath. In addition, the composite member 100 can also be used as a member around steps and stairs.

[0065] Furthermore, since the composite member 100 has shock absorbing properties, it is possible to improve the feel when touched by a person. Therefore, the composite member 100 can be applied to parts that are touched by a person. Specifically, the composite member 100 can be applied to toilet seats, bathtubs, and washbasins.

[0066] In addition, since the composite member 100 can suppress water splashing, it can also be applied to components related to plumbing. Specifically, the composite member 100 can be applied to toilets. In addition, the composite member 100 has the potential to suppress not only water splashing but also water noise.

[0067] As described above, the composite material 100 has shock absorbing properties and can therefore be suitably used as a protective material for devices. Specifically, the composite material 100 can be used not only as an absorbing material that protects a device from shocks and vibrations received from the outside, but also as a member that absorbs vibrations, sounds, high frequencies, and the like generated inside the device.

[0068] The composite member 100 can be suitably used as a building member. The building member is not particularly limited, but examples thereof include exterior wall materials (siding) and roofing materials. By using the composite member 100 as a roofing material, splashing of rain and rain noise can be suppressed. In addition, examples of building members include materials for roads and materials for exterior gutters. By using the composite member 100 as a road material, in addition to suppressing splashing of rain and water noise, it is possible to absorb impacts on pedestrians and improve the feeling of walking.

[0069] The composite member of this embodiment will be described in more detail below with reference to examples, but this embodiment is not limited thereto. EXAMPLES

[0070] [Preparation of test samples] (Example 1-1) First, hydraulic alumina BK-112 manufactured by Sumitomo Chemical Co., Ltd. was prepared as hydraulic alumina. The hydraulic alumina had a median particle size of 16 μm. The X-ray diffraction pattern of this hydraulic alumina was measured by X-ray diffraction method, and it was found to be a mixture of boehmite (AlOOH) and gibbsite (aluminum hydroxide, Al(OH)3). The hydraulic alumina also contained ρ-alumina.

[0071] Furthermore, as polymethyl methacrylate (PMMA), cross-linked polymethyl methacrylate, grade: MBX-5, manufactured by Sekisui Chemical Co., Ltd. was prepared. The cross-linked polymethyl methacrylate had an average particle size of 5 μm.

[0072] Next, hydraulic alumina and PMMA were weighed out so that hydraulic alumina:PMMA=95% by volume:5% by volume, and then the hydraulic alumina and PMMA were mixed using an agate mortar and pestle. Furthermore, ion-exchanged water was weighed out so that the ratio was 80% by mass relative to the hydraulic alumina, and then mixed with the hydraulic alumina and PMMA to obtain a mixture.

[0073] The mixture was then placed in a cylindrical molding die (Φ10) having an internal space, and heated and pressurized under conditions of 400 MPa, 180°C, and 20 minutes to obtain a test sample for this example.

[0074] (Example 1-2) A test sample of this example was obtained in the same manner as in Example 1-1, except that the components were weighed out so that hydraulic alumina:PMMA=90 volume %:10 volume %.

[0075] (Examples 1-3) First, as polyethylene (PE), micronized modified HD polyethylene wax CERAFLOUR (registered trademark) 950 manufactured by BYK was prepared. The polyethylene had an average particle size (D50) of 9 μm.

[0076] Next, the same hydraulic alumina and PE as in Example 1-1 were weighed out so that the ratio of hydraulic alumina to PE was 93% by volume to 7% by volume, and then the hydraulic alumina and PE were mixed using an agate mortar and pestle. Furthermore, ion-exchanged water was weighed out so that the ratio was 80% by mass relative to the hydraulic alumina, and then mixed with the hydraulic alumina and PE to obtain a mixture.

[0077] The mixture was then placed in a cylindrical molding die (Φ10) having an internal space, and heated and pressurized under conditions of 400 MPa, 180°C, and 20 minutes to obtain a test sample for this example.

[0078] (Comparative Example 1-1) Ion-exchanged water was weighed out so that the amount was 80 mass% relative to the same hydraulic alumina as in Example 1-1, and then the hydraulic alumina and the ion-exchanged water were mixed using an agate mortar and pestle to obtain a mixture. The mixture was then placed inside a cylindrical molding die (Φ10) having an internal space. The mixture was then heated and pressurized under conditions of 400 MPa, 180°C, and 20 minutes to obtain a test sample of this example.

[0079] Table 3 shows the mixing ratios of hydraulic alumina, PMMA, and PE in the test samples obtained in Examples 1-1 to 1-3 and Comparative Example 1-1.

[0080] [Table 3]

[0081] [evaluation] (Porosity measurement) First, a cross-section of the cylindrical test sample of Example 1-3 was subjected to cross-section polishing (CP processing). Next, a secondary electron image of the cross-section of the test sample was observed at a magnification of 20,000 times using a scanning electron microscope (SEM). Secondary electron images obtained by observing three positions (positions 1 to 3) on the cross-section of the test sample of Example 1-3 are shown in Figures 6(a), 7(a), and 8(a).

[0082] Next, the SEM images of the three fields of view were binarized to clarify the pores. The binarized images of the secondary electron images of Fig. 6(a), Fig. 7(a) and Fig. 8(a) are shown in Fig. 6(b), Fig. 7(b) and Fig. 8(b), respectively. Then, the area ratio of the pores was calculated from the binarized images, and the average value was taken as the porosity. Specifically, from Fig. 6(b), the area ratio of the pores at position 1 was 1.4%. From Fig. 7(b), the area ratio of the pores at position 2 was 1.1%. From Fig. 8(b), the area ratio of the pores at position 3 was 1.7%. Therefore, the porosity of the test sample of Example 1-3 was 1.4%, which is the average value of the area ratios of the pores at positions 1 to 3.

[0083] 6, 7, and 8, it can be seen that the porosity of the test sample of Example 1-3 is less than 10%, so that the dispersion is prevented from contacting the air and water vapor, and oxidation deterioration is suppressed. The dispersion 20 shown in Figs. 6, 7, and 8 is a polyethylene aggregate. Although it cannot be confirmed in these figures, fine polyethylene is dispersed between the boehmite particles 11.

[0084] (Shock Absorption Test) For each test sample of Examples 1-1 to 1-3 and Comparative Example 1-1, a hollow resin ball was dropped and impacted, and the rebound height of the hollow resin ball was measured to evaluate the impact absorption. Specifically, as shown in Fig. 5, a hollow resin ball 210 was dropped from a height of 10 cm onto the surface of a test sample 200 of each example having a diameter φ of 10 mm, and impacted. Then, the height H when the hollow resin ball 210 rebounded from the surface of the test sample 200 was measured. The hollow resin ball used was a resin sphere having a mass of 0.15 g and a diameter of 3 mm.

[0085] The higher the impact absorption of the test sample, the more the rebound force of the hollow resin ball is absorbed, and therefore the lower the height H. The results of the impact absorption test for the test samples of each example are also shown in Table 3.

[0086] As shown in Table 3, the test sample of Comparative Example 1-1, which did not contain a dispersion, had a rebound height of 4 cm when the hollow resin balls rebounded. In contrast, the test samples of Examples 1-1 and 1-2, in which PMMA was added as a dispersion, had a rebound height of 1 cm or less when the hollow resin balls rebounded. Moreover, the test sample of Example 1-3, in which PE was added as a dispersion, had a rebound height of 2 cm when the hollow resin balls rebounded.

[0087] It is thus clear that by dispersing the dispersion in the inorganic matrix portion made of boehmite particles, it is possible to impart impact absorption properties to the composite material. In addition, since the dispersion is covered by the inorganic matrix portion and is not easily deteriorated by oxidation, it is possible to impart elasticity stably over a long period of time. EXAMPLES

[0088] [Preparation of test samples] As inorganic particles, the average particle size D 50Zinc oxide particles (manufactured by Kojundo Chemical Laboratory Co., Ltd., purity 99.99%) having a diameter of about 1 μm were prepared. In addition, the same polyethylene particles as in Example 1-3 were prepared as a dispersion. Then, the polyethylene particles were weighed out so as to be 7% by volume relative to the zinc oxide particles, and the zinc oxide particles and the polyethylene particles were wet-mixed with acetone using an agate mortar and pestle to obtain a mixed powder.

[0089] Next, the obtained mixed powder was put into a cylindrical molding die (Φ10) having an internal space. Furthermore, 1M acetic acid was added to the mixed powder filled inside the molding die so that 200 μL per 1 g of zinc oxide particles was added. Then, the mixed powder containing the acetic acid was heated and pressurized under conditions of 50 MPa, 150° C., and 30 minutes to obtain a test sample of this example.

[0090] [evaluation] (Porosity measurement) First, a cross-section polisher was applied to the cylindrical cross-section of the test sample of Example 2. Next, a secondary electron image was observed at a magnification of 20,000 times using a scanning electron microscope for the cross-section of the test sample. Secondary electron images obtained by observing three positions (positions 1 to 3) on the cross-section of the test sample of Example 2 are shown in Figures 9(a), 10(a), and 11(a).

[0091] Next, the SEM images of the three fields of view were binarized to clarify the pores. The binarized images of the secondary electron images of Fig. 9(a), Fig. 10(a) and Fig. 11(a) are shown in Fig. 9(b), Fig. 10(b) and Fig. 11(b), respectively. Then, the area ratio of the pores was calculated from the binarized images, and the average value was taken as the porosity. Specifically, from Fig. 9(b), the area ratio of the pores at position 1 was 0.44%. From Fig. 10(b), the area ratio of the pores at position 2 was 2.1%. From Fig. 11(b), the area ratio of the pores at position 3 was 0.86%. Therefore, the porosity of the test sample of Example 2 was 1.1%, which is the average value of the area ratio of the pores at positions 1 to 3.

[0092] 9, 10 and 11, it can be seen that the porosity of the test sample of Example 2 is also less than 10%, so that the dispersion is prevented from coming into contact with the air and water vapor, and oxidation deterioration is suppressed.

[0093] The contents of this embodiment have been described above based on examples, but the present embodiment is not limited to these descriptions, and it will be obvious to those skilled in the art that various modifications and improvements are possible.

[0094] The entire contents of Patent Application No. 2019-178441 (filing date: September 30, 2019) are incorporated herein by reference. [Industrial Applicability]

[0095] According to the present disclosure, it is possible to provide a composite member that is stable over the long term and is capable of absorbing impact as a whole. [Explanation of symbols]

[0096] 10 Inorganic matrix part 10a Surface of inorganic matrix part 11 Inorganic particles 20 Dispersion 100 Composite Materials

Claims

1. an inorganic matrix portion formed by bonding together a plurality of particles of an inorganic material containing boehmite or zinc oxide as a main component; a dispersion that is present in a dispersed state inside the inorganic matrix portion, has elasticity, and contains a resin as a main component; The tensile modulus of the material constituting the dispersion is 100 Pa or more and 3.5 GPa or less, the particles of the inorganic material are bonded to each other via connecting portions that are derived from the inorganic material and are formed between the inorganic material and the dispersion, between the inorganic materials, and between the dispersions; the inorganic matrix portion has a cross-sectional porosity of 20% or less; A composite member, wherein the inorganic material does not include a hydrate of a calcium compound.

2. 2. The composite member according to claim 1, wherein the material constituting the dispersion has a tensile modulus of elasticity of 1000 Pa or more and 0.5 GPa or less.

3. The composite material according to claim 1 , wherein a Young's modulus of a material constituting the inorganic matrix portion is greater than a Young's modulus of a material constituting the dispersion.

4. The composite material according to claim 1 , wherein the dispersion is not present continuously from the surface to the inside of the inorganic matrix portion and is not present in the form of a film on the surface of the inorganic matrix portion.

5. The composite material according to claim 1 , wherein the inorganic matrix portion has a volume ratio larger than that of the dispersion.

6. The composite member according to claim 1 , wherein the inorganic matrix portion has a cross-sectional porosity of 10% or less.

7. The composite member according to claim 1 , wherein the connecting portion is an amorphous portion containing a non-crystalline inorganic compound.

8. The composite member according to claim 7 , wherein the particles of the inorganic substance and the amorphous portion contain the same metal element.

Citation Information

Patent Citations

  • Laying repairing method for molten metal vessel

    JP1983011378A

  • Manufacture of leathery sheet material

    JP1985059182A

  • Hydraulic cement

    JP1991115148A

  • Cement type arc resistant material and its production

    JP1992130041A

  • Fe-cr alloy excellent in workability and pitting corrosion resistance

    JP1994049604A