Soundproofing materials
The soundproofing material with slits in the polyurethane foam addresses the bending issue by expanding to adhere closely to the floor, improving soundproofing and vibration damping properties.
Patent Information
- Application Number
- JP2020104512
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-06-17
- Publication Date
- 2024-09-24
- Estimated Expiration
- 2040-06-17
AI Technical Summary
Conventional soundproofing materials made of polyurethane foam integrated with a skin material suffer from shrinkage-induced bending, leading to gaps between the foam and the floor surface, which compromises soundproofing and vibration damping properties.
A soundproofing material with slits formed in the polyurethane foam opposite to the skin material side, combined with a compression hardness of 500N or more, ensures the foam adheres closely to the floor surface by expanding outward under weight, eliminating bending and enhancing soundproofing and vibration damping.
The slits in the polyurethane foam allow it to flatten and adhere closely to the floor, achieving effective soundproofing and vibration damping by preventing gaps and ensuring stable contact.
Smart Images

Figure 0007555202000008 
Figure 0007555202000007 
Figure 0007555202000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a soundproofing material. [Background technology]
[0002] 2. Description of the Related Art Conventionally, soundproofing materials used as floor silencers or the like placed on the floor of a vehicle include those made of polyurethane foam integrated with a skin, which is formed by foaming polyurethane foam on the back surface of a skin material.
[0003] The following Patent Document 1 describes an automobile floor carpet in which an impact material made of a skinless urethane resin foam is integrally molded on the back surface of the carpet.
[0004] In addition, the following Patent Document 2 describes a fabric with a breathability of 3.0 ft on the back of the surface. 3 / min or more, the foam layer hardness is 8kg / 314cm 2 The document describes a soundproofing material consisting of a polyurethane foam molded product with an integral skin, in which the following polyurethane foam (25% ILD) is integrally molded: [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Publication No. 10-71884 [Patent Document 2] Japanese Patent Application Publication No. 11-5499 Summary of the Invention [Problem to be solved by the invention]
[0006] However, in soundproofing materials such as automotive floor carpets made of polyurethane foam integrated with a skin as shown in Patent Documents 1 and 2, the polyurethane foam molded integrally with the skin shrinks due to natural cooling after the integral molding of the skin. At that time, since one side of the polyurethane foam is fixed to the skin, shrinkage is inhibited on the skin side, and shrinkage mainly occurs on the side opposite to the skin material 30. Due to this shrinkage, the polyurethane foam bends toward the polyurethane foam 83 side opposite to the skin material 81, as in the conventional soundproofing material 80 shown in (10-1) of Fig. 10. Reference numeral 84 denotes the surface of the polyurethane foam 83 opposite to the skin material 81.
[0007] When soundproofing material 80 bent toward polyurethane foam 83 is placed with surface 84 of polyurethane foam 83 on floor surface 90 of an automobile or the like, a gap 95 due to the bending of polyurethane foam 83 is generated between surface 84 of polyurethane foam 83 and floor surface 90, as shown in FIG. 10 (10-2), and polyurethane foam 83 cannot adhere closely to floor surface 90. As a result, the soundproofing properties (including vibration damping properties) that should be obtained by the adhesion between polyurethane foam 83 and floor surface 90 cannot be obtained.
[0008] The present invention has been made in consideration of the above-mentioned points, and has as its object to provide a soundproofing material made of polyurethane foam with an integrated skin, which eliminates the bending state that occurs after integral molding of the skin toward the polyurethane foam opposite the skin when the soundproofing material is placed on the floor of an automobile or the like, and which provides good soundproofing properties (including vibration control properties) by ensuring close contact between the polyurethane foam and the floor of the automobile or the like. [Means for solving the problem]
[0009] First aspectThe soundproofing material has a skin material integrally molded on one side of a polyurethane foam, the soundproofing material having a compression hardness of 500 N or more, the compression hardness being measured as the load at 50% compression when a sample of 200 mm square x 20 mm thick is compressed to 80% of its thickness using a φ80 mm compression tool at a test speed of 50 mm / min, and the polyurethane foam has a slit formed from the surface opposite the skin material to the skin material side.
[0010] Second Aspect teeth, First aspect The skin material is made of a fiber aggregate.
[0011] Third aspect teeth, First aspect or Second Aspect In the present invention, the skin material has an impregnated and hardened layer of polyurethane foam raw material formed at the boundary with the polyurethane foam, and the slits are formed up to the position of the impregnated and hardened layer.
[0012] Fourth aspect teeth, First aspect from Third aspect Either one In the above, the skin material including the impregnated hardened layer has an air permeability (1) based on JIS K6400-7B method: 2012 of 5 to 80 cc / cm 2 / sec.
[0013] Fifth aspect teeth, First aspect from Fourth aspect Either one The soundproofing material is characterized in that the loss factor ratio, calculated as loss factor ratio = (loss factor without double-sided tape attached) / (loss factor with double-sided tape attached to the entire surface), is 0.6 or more. Effect of the Invention
[0014] The soundproofing material of the present invention bends toward the polyurethane foam side opposite to the skin due to shrinkage of the polyurethane foam after integral molding of the skin. However, in the soundproofing material of the present invention, slits are formed in the polyurethane foam from the surface opposite the skin toward the skin, so that when the soundproofing material is placed on the floor of an automobile or the like, the weight of the soundproofing material, or the weight of the mat placed on the soundproofing material and the weight of the soundproofing material itself, presses the soundproofing material against the floor, causing the slits to widen on the surface side of the polyurethane foam opposite the skin, and the surface side of the polyurethane foam opposite the skin spreads outward and becomes flat. This allows the polyurethane foam of the soundproofing material to adhere closely to the floor, etc., providing good soundproofing effects (including vibration damping effects).
[0015] In addition, the soundproofing material of the present invention is relatively hard because its compression hardness is 500N or more, which is measured by compressing a sample of 200mm square x 20mm thick to 80% of the sample thickness at a test speed of 50mm / min using a φ80mm compression tool and measuring the load at 50% compression. Therefore, if the slits of the present invention are not formed in the polyurethane foam, the polyurethane foam will not be flattened by the weight of the soundproofing material, or the weight of the mat placed on the soundproofing material and the weight of the soundproofing material, and a gap will be generated between the polyurethane foam and the floor surface, etc., and a good soundproofing effect will not be obtained. In addition, since the soundproofing material of the present invention has the above-mentioned hardness, when a passenger sits on the soundproofing material, his / her feet will not be buried and he / she can move stably. [Brief description of the drawings]
[0016] [Figure 1] 1 is a rear perspective view of a soundproofing material according to one embodiment of the present invention with slits widened; FIG. [Diagram 2] 2 is a cross-sectional view taken along line AA and BB in FIG. 1. [Diagram 3] FIG. 2 is a cross-sectional view showing an example of use of the soundproofing material of FIG. 1. [Figure 4] FIG. 11 is a rear perspective view of a soundproofing material according to another embodiment with slits widened. [Diagram 5] 5 is a cross-sectional view taken along CC in FIG. 4. [Figure 6] 4 is a cross-sectional view showing a process of integrally molding the surface of the soundproofing material up to a midway point. FIG. [Figure 7] 4A to 4C are cross-sectional views showing the remaining steps in integrally molding the surface of the soundproofing material. [Figure 8] 4 is a cross-sectional view showing a step of forming a slit in the manufacture of a soundproofing material. FIG. [Figure 9] 1 is a table showing the formulations, configurations, and physical properties of examples and comparative examples. [Figure 10] 1 is a cross-sectional view showing a problem with a conventional soundproofing material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, an embodiment of the present invention will be described. A soundproofing material 10 of the embodiment shown in Fig. 1 and Fig. 2 is made of an integral skin polyurethane foam in which a skin material 30 is integrally formed on one side of a polyurethane foam 20. The soundproofing material 10 is suitable as a carpet or the like to be placed on the floor of an automobile or the like, and a surface 21 of the polyurethane foam 20 opposite to the skin material 30 is placed on the floor of the automobile or the like.
[0018] The polyurethane foam 20 is a foam obtained from polyurethane foam raw material, and has slits 25 formed from a surface 21 opposite to the skin material 30 toward the skin material 30 by slit processing.
[0019] In addition, the polyurethane foam 20 has a density (JIS K7222:2005) of 30 to 95 kg / m 3 The thickness is preferably 1 to 40 mm. If the density of the polyurethane foam 20 is too low, the hardness will be too low, and conversely, if the density is too high, the weight will be too heavy. If the polyurethane foam 20 is too thin, the gap between the upper and lower surfaces in the molding space (cavity) of the mold used for integrally molding the skin will be narrowed, making it impossible to fill with the polyurethane foam raw material, and it will be impossible to mold the polyurethane foam. Conversely, if the polyurethane foam is too thick, the soundproofing material 10 will be bulky and heavy.
[0020] The polyurethane foam raw material contains at least a polyol component, a catalyst, a blowing agent, and an isocyanate. The polyol component preferably contains a polyether polyol and a polymer polyol, or is preferably composed of only a polymer polyol.
[0021] Examples of the polyether polyol include polyhydric alcohols such as ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol, butylene glycol, neopentyl glycol, glycerin, pentaerythritol, trimethylolpropane, sorbitol, and sucrose, and polyether polyols in which an alkylene oxide such as ethylene oxide or propylene oxide is added to the polyhydric alcohol.
[0022] The polyether polyol is preferably a polyether polyol having a functionality of 2 to 8, a hydroxyl value of 20 to 168 mgKOH / g, and a number average molecular weight of 168 to 20000. The ethylene oxide content (EO ratio) of the polyether polyol is preferably 5 to 90%. The ethylene oxide content (EO ratio) of the polyether polyol is the content of ethylene oxide units when the total amount of one raw material composition unit is taken as 100% by weight.
[0023] The polymer polyol is obtained by polymerizing an ethylenically inactive compound in a polyether polyol. By including the polymer polyol in the polyol component, the effect of improving the breathability and hardness can be obtained. The polymer polyol preferably has a functionality of 3 to 8, a hydroxyl value of 20 to 60 mgKOH / g, and a number average molecular weight of 2000 to 8000. The ethylene oxide content (EO rate) of the polymer polyol is preferably 3 to 50%. The ethylene oxide content (EO rate) of the polymer polyol is the content of ethylene oxide units when the total amount of one raw material composition unit is taken as 100% by weight. The weight proportion of the polymer polyol in the polyol component is preferably from 20 to 100%, more preferably from 50 to 100%, with the remainder being polyether polyol.
[0024] The catalyst may be one known for use in polyurethane foams. Examples of the catalyst include amine catalysts such as triethylamine, triethylenediamine, diethanolamine, dimethylaminomorpholine, N-ethylmorpholine, tetramethylguanidine, and imidazole-based compounds, tin catalysts such as stannous octoate and dibutyltin dilaurate, and metal catalysts (also called organometallic catalysts) such as phenylmercury propionate and lead octenate. A combination of multiple catalysts may be used. The general amount of catalyst is about 0.2 to 4 parts by weight per 100 parts by weight of the polyol component.
[0025] The foaming agent is not particularly limited, but water is preferred. The amount of water used as the foaming agent is preferably about 2 to 10 parts by weight, more preferably 3 to 7 parts by weight, based on 100 parts by weight of the polyol component.
[0026] The isocyanate may be any of aromatic, alicyclic, and aliphatic isocyanates, and may be a bifunctional isocyanate having two isocyanate groups in one molecule, or a trifunctional or higher isocyanate having three or more isocyanate groups in one molecule, and these may be used alone or in combination.
[0027] For example, bifunctional isocyanates include 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, m-phenylene diisocyanate, p-phenylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 2,2'-diphenylmethane diisocyanate, xylylene diisocyanate, 3,3'-dimethyl-4,4'-biphenylene diisocyanate, 3,3'-dimethoxy-4,4'- Examples of the isocyanate include aromatic isocyanates such as biphenylene diisocyanate, alicyclic isocyanates such as cyclohexane-1,4-diisocyanate, isophorone diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, and methylcyclohexane diisocyanate, and aliphatic isocyanates such as butane-1,4-diisocyanate, hexamethylene diisocyanate, isopropylene diisocyanate, methylene diisocyanate, and lysine isocyanate.
[0028] Examples of trifunctional or higher isocyanates include 1-methylbenzene-2,4,6-triisocyanate, 1,3,5-trimethylbenzene-2,4,6-triisocyanate, biphenyl-2,4,4'-triisocyanate, diphenylmethane-2,4,4'-triisocyanate, methyldiphenylmethane-4,6,4'-triisocyanate, 4,4'-dimethyldiphenylmethane-2,2',5,5'tetraisocyanate, triphenylmethane-4,4',4"-triisocyanate, polymeric MDI, and the like. Other urethane prepolymers can also be used. The isocyanate is, Each of them is not limited to one type, and may be one or more types. For example, one type of aliphatic isocyanate and two types of aromatic isocyanate may be used, or two types of aromatic isocyanate and urethane prepolymer may be used, or three or more types of isocyanate may be used. The isocyanate index is preferably 90 to 130, more preferably 95 to 120. The isocyanate index is an index used in the field of polyurethane, and is a numerical value that represents the equivalent ratio of the isocyanate group of the isocyanate to the active hydrogen group in the raw material (for example, the active hydrogen group contained in the hydroxyl group of polyols and the active hydrogen group of water as a blowing agent, etc.) expressed as a percentage.
[0029] The polyol component may optionally contain a foam stabilizer and additives. The foam stabilizer may be any foam stabilizer that is used in polyurethane foam, including silicone foam stabilizers, fluorine-containing compound foam stabilizers, and known surfactants. The amount of foam stabilizer is preferably 0 to 2 parts by weight per 100 parts by weight of the polyol component.
[0030] Examples of the additives include a linking agent, a crosslinking agent, a pigment, a filler, a flame retardant, an antioxidant, and an ultraviolet absorbing agent. Examples of the opening agent include polyether polyols with a high EO addition ratio, polyethylene glycols, and silicone foam stabilizers that increase air permeability (having foam breaking properties). When a opening agent is used, the amount of the opening agent is preferably 0.5 to 20 parts by weight per 100 parts by weight of polyol. The opening agent is not limited to one type, and two or more types may be used. Examples of the crosslinking agent include glycerin, trimethylolpropane, 1,2,4-butanetriol, 2-methyl-2,3,4-butanetriol, triethanolamine, pentaerythritol, etc., and one or more of them may be used in combination. Preferred crosslinking agents include glycerin, pentaerythritol, diethanolamine, etc., which have 2 to 4 functional groups, a molecular weight of 92 to 136, and a hydroxyl value of 1066 to 1826 mgKOH / g. When a crosslinking agent is used, the amount of the crosslinking agent is preferably 1 to 6 parts by weight per 100 parts by weight of the polyol component. The crosslinking agent may have an ethylene oxide content (EO ratio) of more than 0%. For example, ethylenediamine-based (functional group number: 4, molecular weight: 280, hydroxyl value 800 mg KOH / g, EO ratio 40%), trimethylolpropane-based (functional group: 3, molecular weight: 183, hydroxyl value 920 mg KOH / g, EO ratio 50%), etc.
[0031] Examples of the pigment include carbon black and titanium oxide. Examples of the filler include graphite, alumina, and melamine.
[0032] Specific examples of the flame retardant include halogenated diphenyl ethers such as degabromdiphenyl ether and octabromdiphenyl ether, halogen compounds such as halogenated polycarbonates, inorganic compounds such as antimony trioxide, antimony tetraoxide, antimony pentoxide, sodium pyroantimonate, and aluminum hydroxide, triazine ring-containing compounds, metal hydroxides, phosphate flame retardants, condensed phosphate flame retardants, phosphate flame retardants, inorganic phosphorus flame retardants, dialkylphosphinates, silicone flame retardants, metal oxides, boric acid compounds, and expandable graphite.
[0033] Examples of the antioxidant include naphthylamines, diphenylamines, p-phenyldiamines, quinolines, hydroquinone derivatives, monophenols, thiobisphenols, hindered phenols, and phosphites.
[0034] Examples of the ultraviolet absorber include 2-hydroxybenzophenones such as 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-octoxybenzophenone, and 5,5'-methylenebis(2-hydroxy-4-methoxybenzophenone); 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole, and 2-(2'-hydroxy-3',5'- 2-(2'-hydroxyphenyl)benzotriazoles such as 2-(2'-hydroxy-5'-tert-octylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-dicumylphenyl)benzotriazole, 2,2'-methylenebis(4-tert-octyl-6-(benzotriazolyl)phenol), 2-(2'-hydroxy-3'-tert-butyl-5'-carboxyphenyl)benzotriazole; phenyl Benzoates such as ricinate, resorcinol monobenzoate, 2,4-ditert-butylphenyl-3,5-ditert-butyl-4-hydroxybenzoate, 2,4-ditert-amylphenyl-3,5-ditert-butyl-4-hydroxybenzoate, hexadecyl-3,5-ditert-butyl-4-hydroxybenzoate; substituted oxanilides such as 2-ethyl-2'-ethoxyoxanilide, 2-ethoxy-4'-dodecyloxanilide; ethyl-α-cyano-β,β-diphenylacrylate, methyl cyanoacrylates such as aryl-2-cyano-3-methyl-3-(p-methoxyphenyl)acrylate; and triaryltriazines such as 2-(2-hydroxy-4-octoxyphenyl)-4,6-bis(2,4-di-tert-butylphenyl)-s-triazine, 2-(2-hydroxy-4-methoxyphenyl)-4,6-diphenyl-s-triazine, and 2-(2-hydroxy-4-propoxy-5-methylphenyl)-4,6-bis(2,4-di-tert-butylphenyl)-s-triazine.
[0035] The slits 25 formed in the polyurethane foam 20 are provided to prevent the polyurethane foam 20, which is integrally molded with the skin material 30, from bending toward the opposite side to the skin material 30 due to natural cooling after the integral molding of the skin.
[0036] The bending of the soundproofing material 10 is eliminated by the slits 25 when, as shown in FIG. 3, the soundproofing material 10 is placed on the floor surface 37 of an automobile or the like with the polyurethane foam 20 side facing, and the soundproofing material 10 is pressed against the floor surface 37 by the weight of the soundproofing material 10 or by the weight of the mat 39 placed on top of the soundproofing material 10 and the weight of the soundproofing material 10 itself, causing the slits 25 to widen on the surface 21 side of the polyurethane foam 20 opposite the skin material 30, and flattening the polyurethane foam 20 from its bent state.
[0037] The elimination of bending will now be described in more detail. Since the surface 30 side of the polyurethane foam 20 is fixed to the surface 30, the slits 25 are prevented from expanding or only expand slightly on the surface 30 side. On the other hand, the surface 21 of the polyurethane foam 20 opposite the surface 30 is not fixed to the surface 30, etc. and is open, so the slits 25 expand more on the surface 21 side opposite the surface 30 than on the surface 30 side. As a result, the surface 21 side opposite the surface 30 of the polyurethane foam 20 expands outward, and the bending of the polyurethane foam 20 is eliminated.
[0038] In order to facilitate good expansion of the slits 25, it is preferable that the slits 25 are formed from the surface 21 of the polyurethane foam 20 on the side opposite the skin 30, through the polyurethane foam 20 to the boundary with the skin 30. If the slits 25 are formed only partway through the polyurethane foam 20, there is a risk that the slits 25 will tear (break) from the ends inside the polyurethane foam 25 when they are expanded.
[0039] The slits may be in the form of a lattice-shaped slit 25 in the soundproofing material 10 shown in Figs. 1 and 2, or in the form of parallel slits 250 in the soundproofing material 100 shown in Figs. 4 and 5, or in other forms. In particular, in the case of the lattice-shaped slits 25 shown in Figs. 1 and 2, the soundproofing material 10 can be more effectively unbent than in the case of the parallel slits 250 shown in Figs. 4 and 5. In Fig. 4, reference numeral 200 denotes polyurethane foam, 300 denotes a skin material, 310 denotes a first layer in the skin material 30, 330 denotes a second layer in the skin material, and 340 denotes an impregnated hardened layer. Reference numeral 210 denotes the surface of the polyurethane foam 200 opposite to the skin material 300. The first layer, the second layer, and the impregnated hardened layer will be described later. The distance between the slits 25 may be appropriately determined, and may be, for example, 5 to 150 mm, and more preferably 10 to 100 mm.
[0040] When the bending of the polyurethane foam 20 is eliminated, the polyurethane foam 20 adheres closely to the floor surface 37, and the soundproofing material 10 exhibits good soundproofing properties (including vibration damping properties).
[0041] The skin material 30 may be a fiber aggregate such as nonwoven fabric or felt, and felt is particularly preferred from the viewpoints of light weight and soundproofing (sound absorption). An impregnated and cured layer 34 of polyurethane foam raw material is formed on the boundary between the skin material 30 and the polyurethane foam 20.
[0042] The impregnated and hardened layer 34 is formed by impregnating and hardening the skin material 30 at the boundary with the polyurethane foam 20 with polyurethane foam raw material for foaming the polyurethane foam 20 during integral skin molding of the polyurethane foam 20 and the skin material 30. The impregnated and hardened layer 34 suppresses the elongation of the polyurethane foam 20 on the skin material 30 side, and allows the slits 25 to be opened more on the surface 21 side of the polyurethane foam 20 opposite the skin material 30 than on the skin material 30 side, thereby making it possible to effectively eliminate bending of the polyurethane foam 20.
[0043] The skin material 30 may be either a single layer or a laminate of multiple layers. The covering material 30 of the embodiment is made of a two-layer nonwoven fabric sheet composed of a first layer 31 and a second layer 33. The first layer 31 faces away from the polyurethane foam 20, while the second layer 33 faces the polyurethane foam 20.
[0044] Either the first layer 31 or the second layer 33 is made of a fiber having a diameter of 2 to 4d and has a basis weight of 90 g / m 2 More than 90g / m 2 More than 500g / m 2 The other layer has a basis weight of 100 g / m 2 More than 100g / m 2 More than 500g / m 2 When the skin 30 is constructed in this manner, one layer is densely composed of fine fibers, so that the viscous polyurethane foam raw material impregnated in the skin 30 is less likely to seep out of the skin 30. One of the two layers is filled with 35 g / m of acrylic ester resin. 2 More than 35g / m 2 More than 100g / m 2 The layer impregnated with the acrylic ester resin has spaces between the fibers filled with the acrylic ester resin, making it difficult for the polyurethane foam raw material to pass through the skin material 30, and making it even more difficult for the polyurethane foam raw material to seep out. The acrylic ester resin can be impregnated into the skin material 30 by applying an emulsion of the acrylic ester resin to the surface of the skin material 30, or by scattering acrylic ester resin powder on the surface of the skin material 30 and applying a heated roller or hot air to the surface.
[0045] By adjusting the basis weight of the first layer 31 and the second layer 33 and the impregnation of the acrylic ester resin, the air permeability (1) based on JIS K6400-7B method: 2012 of the skin material 30 including the impregnated hardened layer 34 is set to 5 to 80 cc / cm 2The air permeability (1) of the skin material 30 including the impregnated hardened layer 34 based on JIS K6400-7B method: 2012 can be set to 5 to 80 cc / cm 2 / sec, the soundproofing (sound absorption) properties of the soundproofing material 10 can be improved.
[0046] In a more preferred embodiment of the skin 30, the second layer 33 on the polyurethane foam 20 side is made of fibers with a fiber diameter of 2 to 4d and a basis weight of 90 g / m 2 The above composition, and the acrylic ester resin is 35 g / m 2 When the skin material 30 is constructed in this manner, the second layer 33 that comes into contact with the polyurethane foam raw material during the production of the soundproofing material 10 is densely packed with fine fibers, and the acrylic ester resin is impregnated at 35 g / m 2 Since the polyurethane foam raw material is impregnated to the extent that the amount of the polyurethane foam raw material that is impregnated (seeped into) second layer 33 can be restricted so as not to become excessive. Also, impregnated and cured layer 34 formed by the impregnation and curing of the polyurethane foam raw material in the portion of second layer 33 that contacts polyurethane foam 20 can suppress the penetration of the raw material into second layer 33.
[0047] The basis weight of the first layer 31 on the opposite side to the polyurethane foam 20 is 100 g / m 2 By doing so, it is possible to effectively prevent the first layer 31 from being impregnated with the raw material for the urethane foam, and ensure the breathability of the skin material 30. Furthermore, it is preferable to improve the abrasion resistance of the surface of the first layer 31 by making the fiber diameter 5d or more. The first layer 31 and the second layer 33 are integrated together by adhesion or needle punching.
[0048] The soundproofing material 10 preferably has a compression hardness of 500 N or more, more preferably 650 to 1200 N, as measured by the load at 50% compression when a sample of 200 mm square and 20 mm thick is compressed to 80% of its thickness in a compression jig of φ80 mm at a test speed of 50 mm / min. If the compression hardness of the soundproofing material 10 is too low, for example, when the upper surface of the soundproofing material 10 is pressed by the foot of a passenger, the pressed portion will sink, making it difficult to walk or causing an unstable posture.
[0049] A method for producing the soundproofing material 10 using an example of the two-layer skin material 30 will be described with reference to Figs. 6 to 8. The soundproofing material 10 can be produced by molding using a metal mold 40. The metal mold 40 is composed of a lower mold 41 and an upper mold 43, and the skin material 30 is attached to either the lower mold 41 or the upper mold 43. The skin material 30 is attached so that the first layer 31 faces the mold surface of one of the molds and the second layer 33 faces inside the mold. When the skin material 30 is attached to the upper mold 43, a locking means consisting of a locking pin or the like for removably holding the skin material 30 is provided on the mold surface of the upper mold 43. In the illustrated example, the skin material 30 is attached to the mold surface of the upper mold 43 as shown in FIG. 6 (6-1).
[0050] Before attaching the skin material 30 to the mold surface of the mold 40, a mold release agent 38 is applied to the mold surface of the mold 40. The mold release agent 38 preferably contains a linear hydrocarbon wax in order to facilitate making the floor side (sound source side) surface of the polyurethane foam 20 open-celled. Making the floor side (sound source side) surface of the polyurethane foam 20 open-celled can further improve soundproofing (sound absorption). Examples of the linear hydrocarbon wax include paraffin wax, Fischer-Tropsch wax, and Sasol wax. Solvent-based release agents dispersed in an organic solvent, and water-based release agents dispersed in water using an emulsifier can be used.
[0051] A release agent 38 is applied to the surface of the mold 40, and the skin 30 is attached. Then, as shown in FIG. 6 (6-2), polyurethane foam raw material 20a is mixed and injected into the mold 40, and the mold is closed to cause the polyurethane foam raw material 20a to foam in the molding space between the second layer 33 of the skin 30 and the surface of the lower part 41 of the mold 40.
[0052] The polyurethane foam raw material 20a injected into the mold 40 fills the molding space between the second layer 33 of the skin material 30 and the mold surface of the lower part of the mold 40 by foaming, and forms the polyurethane foam 20 integrally with the skin material 30, as shown in Figure 6 (6-3). At that time, a part of the polyurethane foam raw material 20a impregnates and hardens in the second layer 33 of the skin material 30, forming an impregnated and hardened layer 34 at the boundary with the polyurethane foam 20.
[0053] Thereafter, as shown in FIG. 7, upper die 43 is separated from lower die 41 to open mold 40, and integrally molded body 10A having skin 30 molded integrally with one side of polyurethane foam 20 as shown in FIG. 1 is taken out.
[0054] 8, the slits 25 are formed by slitting on the surface 21 of the polyurethane foam 20 on the side opposite the skin material 30 of the integrally molded body 10A. Reference numeral 51 denotes a lower platen, 53 a die, and 55 a slit forming blade provided downward on the die 53. In the slitting, the skin material 30 of the integrally molded body 10A faces the lower platen 51, the surface 21 of the polyurethane foam 20 on the side opposite the skin material 30 faces the die 55, the polyurethane foam 20 is placed on the upper surface of the lower platen 51, the die 53 located above the polyurethane foam 20 is lowered, and the slit forming blade 55 is inserted into the surface 21 of the polyurethane foam 20 to form the slits 25, thereby obtaining the soundproofing material 10. EXAMPLES
[0055] Using a polyurethane foam raw material having the composition shown in Fig. 9, a 500 mm square x 20 mm thick integral skin molded body was formed by a molding method using a mold 40 shown in Fig. 6 to Fig. 7, and then lattice-shaped slits were formed through the polyurethane foam until they met the impregnated and cured layer by the slit processing shown in Fig. 8, to obtain the soundproofing materials of Examples 1 to 10. The slit interval was 100 mm. In Comparative Examples 1 to 4, no slit processing was performed, and the samples had no slits.
[0056] The numerical values of each component in the composition in Fig. 9 indicate parts by weight. The mold was heated with warm water, and the lower mold 41 and the upper mold 43 were heated to 70°C. As a mold release agent, linear hydrocarbon wax (product name: URH-520, manufactured by Konishi Co., Ltd.) was sprayed onto the mold surface at 10 to 30 g / m 2 It was applied.
[0057] The components constituting the composition of FIG. 9 are as follows: Polyol-1: Polyether polyol, functionality 3.6, number average molecular weight 5500, hydroxyl value 31.5 mg KOH / g, EO ratio 15% Polyol-2: Polyether polyol, functionality 3, number average molecular weight 5000, hydroxyl value 34 mg KOH / g, EO ratio 14% Polyol-3: Polyether polyol, functionality 3, number average molecular weight 7000, hydroxyl value 26 mg KOH / g, EO ratio 14% Polyol-4: Polyether polyol, functionality 3, number average molecular weight 700, hydroxyl value 245 mg KOH / g, EO ratio 0% Polyol-5: Polymer polyol, functionality 3, number average molecular weight 5000, hydroxyl value 25 mg KOH / g, EO ratio 0%, solids concentration 32% Polyol-6: Polymer polyol, functionality 3, number average molecular weight 3000, hydroxyl value 31 mgKOH / g, EO ratio 40%, solids concentration 32% Foaming agent: Water Amine catalyst 1: Diethanolamine Amine catalyst 2: Aliphatic tertiary amine composition [bis(2-dimethylaminoethyl) ether / dipropylene glycol] Amine catalyst 3: DABCO 33LSI EVONIK Foam stabilizer: Organic modified siloxane, product name: B8715LF2, EVONIC Additives: Polyether polyol, molecular weight 5000, functionality 3, hydroxyl value 34mgKOH, EO ratio 70% Isocyanate 1 (ISO-1): Polymeric MDI, NCO% 31.5% Isocyanate 2 (ISO-2): 4,4'-MDI / urethane prepolymer = 75-85 / 15-25, NCO% 26.5% Isocyanate 3 (ISO-3): Crude MDI, NCO%: 31.7%
[0058] For each of the Examples and Comparative Examples, the thickness of the impregnated and cured layer in the second layer, the hardness of the soundproofing material, the vibration damping property of the soundproofing material, the density of the polyurethane foam, the air permeability (1) of the skin material including the impregnated and cured layer, the reverberation room sound absorption coefficient, the reverberation room sound absorption coefficient of the polyurethane foam, and the sound transmission loss of the soundproofing material were calculated or measured.
[0059] The thickness of the impregnated and hardened layer in the second layer was measured using a scanning electron microscope (SEM: manufactured by JEOL Ltd.) at a magnification of 35x on a 500mm square x 20mm thick soundproofing material, and the thickness was calculated as the average of five points (including the maximum and minimum).
[0060] To measure the hardness of the soundproofing material, a sample of 500mm square x 20mm thick soundproofing material was cut to 200mm square x 20mm thick, placed with the skin material on top, and compressed using a φ80mm compression tool at a compression speed of 50mm / min until the displacement was 80% of the thickness (sample displacement 16mm, remaining sample thickness 4mm), and the loads at 25%, 50% and 75% compression were read as the measured values. The hardness of the soundproofing material was evaluated by measuring the load at 50% compression and giving a rating of "◎" if the compressive hardness was 1000N or more, "◯" if it was 500N or more but less than 1000N, and "×" if it was less than 500.
[0061] The vibration damping performance (loss factor ratio) of the soundproofing material was measured by placing a 1mm thick metal plate (soundproofing material) under the polyurethane foam and a 1mm thick rubber sheet on the skin of a 30 x 300mm soundproofing material sample, measuring the loss factor at approximately 650Hz based on JIS K 7391:2008, and calculating the loss factor ratio for vibration damping evaluation using the following formula. Loss coefficient ratio = (loss coefficient without double-sided tape attached) / (loss coefficient with double-sided tape attached to the entire surface) The "loss factor without double-sided tape" is the loss factor measured when the metal plate is placed under the polyurethane foam without using double-sided tape, whereas the "loss factor with double-sided tape attached to the entire surface" is the loss factor measured when the metal plate and polyurethane foam are attached to each other with double-sided tape over the entire surface of the bonding surface. The vibration damping performance (loss factor ratio) was evaluated as "◎" if it was 0.80 or more, "〇" if it was 0.60 or more and less than 0.80, "△" if it was 0.40 or more and less than 0.6, and "×" if it was less than 0.40.
[0062] The density of the polyurethane foam was measured in accordance with JIS K7222:2005 by cutting a 500 mm square x 20 mm thick soundproofing material into a 100 mm square x 20 mm thick piece, removing the skin portion from the resulting cut piece (or the skin portion including the impregnated hardened layer, if an impregnated hardened layer was present).
[0063] The air permeability (2) and (3) of the skin layer and center layer of polyurethane foam were measured by cutting a 500 mm square x 20 mm thick soundproofing material into a 100 mm square x 20 mm thick piece, removing the skin part (if an impregnated layer exists, the skin part including the impregnated layer) from the cut piece, and slicing the sample into a size of 40 mm square or more x 3 mm thick to separate it into the skin layer (the surface side of the polyurethane foam) and the center layer (the center part in terms of thickness), and measuring the air permeability according to JIS K 6400-7B method: 2012 with the surface closer to the surface facing down. At this time, the clamp aperture was 5 cm 2(φ approx. 25 mm) was used. In order to convert the thickness, the air permeability (2) and (3) were calculated using the following formula. Calculated ventilation volume [(cc / cm 2 / sec)·mm] = JIS measured airflow rate [cc / cm 2 / sec] × thickness of measurement area [mm]
[0064] The air permeability of the skin material including the impregnated hardened layer (1) was measured by cutting a 500 mm square x 20 mm thick soundproofing material into a 100 mm square x 20 mm thick piece, cutting out the skin part (if an impregnated hardened layer exists, the skin part including the impregnated hardened layer) from the resulting cut piece, placing the impregnated hardened layer on the bottom of the sample, and measuring the air permeability of the sample over a measurement area of 38 cm in accordance with JIS K6400-7B method: 2012. 2 Measurements were taken using a diameter of approximately 70 mm.
[0065] The sound absorption coefficient of the skin material, including the impregnated hardened layer, was measured in a reverberation room (approximately 30 m) using four soundproofing materials 10, each 500 mm square and 20 mm thick. 3 ) and the test was performed on the surface of the skin material (non-sound source surface) based on JIS A 1409. All gaps between the samples and between the sample and the jig were sealed with aluminum tape. The reverberation room sound absorption coefficient was determined by averaging the measured sound absorption coefficients at each frequency (500, 630, 800, 1000, 1250, 1600, 2000, 2500, 3150, 4000, 5000, 6300 Hz). The reverberation room sound absorption coefficient of the soundproofing material 10 corresponds to the average sound absorption coefficient for the surface of the skin material including the impregnated hardened layer. The reverberation chamber sound absorption rate of skin materials including the impregnated hardened layer was evaluated as "◎" if it was 65% or more, "〇" if it was 50% or more but less than 65%, "△" if it was 35% or more but less than 50%, and "×" if it was less than 35%.
[0066] The sound transmission loss of soundproofing materials was measured based on JIS A1441-1:2007. The sound source reverberation room was 36 m 3 , the anechoic chamber is 20m 3 The measurement area is 400 × 400 mm (0.16 m 2The polyurethane foam on the floor side of the 500mm square x 20mm thick soundproofing material is covered with a 0.8mm thick steel plate (soundproofing material) and a 1mm thick rubber sheet (soundproofing material) (1700g / m 2 ) was layered on top of each other, the periphery of the soundproofing material was fixed with a 50mm wide frame, and any gaps were sealed with clay. Sound was then incident on the iron plate side as the sound source, and the numerical values at 1600 Hz were measured at four centrally separated scattered points (100mm pitch) 100mm away from the surface of the rubber sheet. In terms of transmission loss, "Configuration A" is a configuration in which the urethane foam is attached to a metal plate, i.e., the skin is adhered to a rubber sheet, and "Configuration B" is a configuration in which the skin is adhered to a metal plate, i.e., the urethane foam is adhered to a rubber sheet. The transmission loss was evaluated as "◎" if it was 44.2 dB or more, "◯" if it was 42.2 dB or more but less than 44.2 dB, and "×" if it was less than 42.2 dB.
[0067] A comprehensive evaluation was performed for each example and each comparative example. The comprehensive evaluation was determined to be the lowest evaluation among the individual evaluations. For example, if all the evaluations were "◎", the comprehensive evaluation was "◎", if at least one of the evaluations was "◯" and the rest were "◎", the comprehensive evaluation was "◯", if at least one of the evaluations was "△" and the rest were "◯" or "◎", the comprehensive evaluation was "△", and if at least one of the evaluations was "×" and the rest were "△", "◯", or "◎", the comprehensive evaluation was "×".
[0068] In Example 1, a polyurethane foam raw material containing 30 parts by weight of polyol-1 (polyether polyol), 70 parts by weight of polyol-6 (polymer polyol), 5.10 parts by weight of foaming agent, 2.71 parts by weight of amine catalyst-1, 0.39 parts by weight of amine catalyst-2, 0 parts by weight of foam stabilizer, 0 parts by weight of additive, isocyanate ISO-1:ISO-2=22:78, and isocyanate index 105 was used. The first layer was made of 6d PET fiber as a skin material, and the basis weight was 150 g / m. 2 , the second layer is 3D PET fiber, basis weight 100g / m 2 , acrylic ester resin is 50g / m 2 Impregnated with 300g / m2 2The skin material used was
[0069] The results of Example 1 were as follows: the thickness of the impregnated hardened layer was 1 mm; the soundproofing material was constructed as an integrated skin with slits; the hardness of the soundproofing material at 25% compression was 570 N, the hardness at 50% compression was 1110 N, and the hardness at 75% compression was 3100 N; the hardness of the soundproofing material was rated as "◎"; the vibration damping property of the soundproofing material (loss coefficient ratio without a rubber sheet placed on it) was 0.60; the vibration damping property was rated as [◯]; and the density of the polyurethane foam was 55 kg / m 3 The air permeability of the polyurethane foam is 78 (cc / cm 2 / sec)·mm, and the airflow rate of the central layer (3) is 287(cc / cm 2 / sec)·mm, and the air permeability of the skin material including the impregnated hardened layer (1) is 20.8cc / cm 2 / sec, the reverberation chamber sound absorption coefficient of the skin material including the impregnated hardened layer was 71%, the reverberation chamber sound absorption coefficient of the skin material including the impregnated hardened layer was rated as "◎", the soundproofing material had a sound transmission loss of [A] (a configuration in which the urethane foam is adhered to a metal plate and the skin material is adhered to a rubber sheet), the soundproofing material had a sound transmission loss of 49.2dB, and the soundproofing material was rated as "◎". Overall rating: "〇", and the soundproofing (vibration control, sound absorption) properties were good.
[0070] Example 2 is the same as Example 1, except that the soundproofing material of Example 1 was used and a 1 mm thick rubber sheet was placed on the surface of its skin to measure the vibration damping properties of the soundproofing material. The soundproofing material had a structure of transmission loss [A] (a structure in which the urethane foam is adhered to a metal plate and the skin is adhered to the rubber sheet).
[0071] The results of Example 2 are similar to those of Example 1, except for the vibration damping properties of the soundproofing material. In Example 2, the vibration damping property of the soundproofing material (loss factor ratio with rubber sheet placed) is 0.95, the vibration damping property evaluation is [◎], and the overall evaluation is [◎]. The vibration damping result of the soundproofing material is better in Example 2 with rubber sheet placed than in Example 1 without rubber sheet placed. From this vibration damping result, it can be understood that in Example 2, the soundproofing material is pressed more strongly by the weight of the rubber sheet placed on the surface of the skin material than in Example 1 (without rubber sheet placed), and as a result, the slits of the polyurethane foam are expanded more than in Example 1 (without rubber sheet placed) on the side opposite the skin material, and the polyurethane foam is expanded more outward than in Example 1 (without rubber sheet placed) on the side opposite the skin material, and thus the bending of the soundproofing material is eliminated, and it is adhered to the metal plate more reliably than in Example 1.
[0072] In Example 3, the foaming agent in Example 1 was used at 5.76 parts by weight, the amine catalyst-1 at 3.06 parts by weight, the amine catalyst-2 at 0.45 parts by weight, the foam stabilizer at 0.31 parts by weight, and the additive at 2.27 parts by weight, but the other components were the same as in Example 1.
[0073] The results of Example 3 were as follows: the thickness of the impregnated hardened layer was 1 mm; the soundproofing material was constructed as an integrated skin with slits; the hardness of the soundproofing material at 25% compression was 700 N, the hardness at 50% compression was 1400 N, and the hardness at 75% compression was 3900 N; the hardness of the soundproofing material was rated as "◎"; the vibration damping property of the soundproofing material (loss coefficient ratio without a rubber sheet placed on it) was 0.59; the vibration damping property was rated as [◯]; and the density of the polyurethane foam was 55 kg / m 3 The air permeability of the polyurethane foam is 39 (cc / cm 2 / sec)·mm, and the central layer air permeability (3) is 70(cc / cm 2 / sec)·mm, and the air permeability of the skin material including the impregnated hardened layer (1) is 11.7cc / cm 2 / sec, the reverberation chamber sound absorption coefficient of the skin material including the impregnated hardened layer was 65%, the reverberation chamber sound absorption coefficient of the skin material including the impregnated hardened layer was rated as "◎", the soundproofing material had a sound transmission loss of [A] (a configuration in which the urethane foam is adhered to a metal plate and the skin material is adhered to a rubber sheet), the soundproofing material had a sound transmission loss of 47.2dB, and the soundproofing material was rated as "◎". Overall rating: "〇", and the soundproofing (vibration control, sound absorption) properties were good.
[0074] Example 4 is the same as Example 3, except that the soundproofing material of Example 3 was used and a 1 mm thick rubber sheet was placed on the surface of its skin to measure the vibration damping properties of the soundproofing material. The soundproofing material had a structure of transmission loss [A] (a structure in which the urethane foam is adhered to a metal plate and the skin is adhered to the rubber sheet).
[0075] The results of Example 4 are similar to those of Example 3, except for the vibration damping properties of the soundproofing material. In Example 4, the vibration damping property of the soundproofing material (loss factor ratio with rubber sheet placed) is 0.93, the vibration damping property evaluation is [◎], and the overall evaluation is [◎]. The vibration damping result of the soundproofing material is better in Example 4 with rubber sheet placed than in Example 3 without rubber sheet placed. From this vibration damping result, it can be understood that in Example 4, the soundproofing material is pressed more strongly by the weight of the rubber sheet placed on the surface of the skin material than in Example 3 (without rubber sheet placed), and as a result, the slits of the polyurethane foam are expanded more than in Example 3 (without rubber sheet placed) on the side opposite the skin material, and the polyurethane foam is expanded more outward than in Example 3 (without rubber sheet placed) on the side opposite the skin material, and thus the bending of the soundproofing material is eliminated, and it is more reliably adhered to the metal plate than in Example 3.
[0076] In Example 5, the foaming agent in Example 1 was 5.88 parts by weight, the amine catalyst-1 was 3.13 parts by weight, the amine catalyst-2 was 0.45 parts by weight, the foam stabilizer was 0 parts by weight, the additive was 9.84 parts by weight, and the isocyanate was ISO-1:ISO-2=0:100, and the rest was the same as in Example 1.
[0077] The results of Example 5 are as follows: the thickness of the impregnated hardened layer is 1 mm, the soundproofing material is constructed as an integrated skin with slits, the hardness of the soundproofing material at 25% compression is 375 N, the hardness at 50% compression is 650 N, the hardness at 75% compression is 1500 N, the hardness of the soundproofing material is rated as "good", the vibration damping property of the soundproofing material (loss coefficient ratio without placing a rubber sheet) is 0.64, the vibration damping property is rated as "good", and the density of the polyurethane foam is 55 kg / m 3 The air permeability of the polyurethane foam is 276 (cc / cm 2 / sec)·mm, and the central layer air permeability (3) is 352(cc / cm 2 / sec)·mm, and the air permeability of the skin material including the impregnated hardened layer (1) is 72cc / cm 2 / sec, the reverberation chamber sound absorption coefficient of the skin material including the impregnated hardened layer was 73%, the reverberation chamber sound absorption coefficient of the skin material including the impregnated hardened layer was rated as "◎", the soundproofing material had a sound transmission loss of [A] (a configuration in which the urethane foam is adhered to a metal plate and the skin material is adhered to a rubber sheet), the soundproofing material had a sound transmission loss of 50.2 dB, and the soundproofing material was rated as "◎". Overall rating: "〇", and the soundproofing (vibration control, sound absorption) properties were good.
[0078] Example 6 is the same as Example 5, except that the soundproofing material of Example 5 was used and a 1 mm thick rubber sheet was placed on the surface of its skin to measure the vibration damping properties of the soundproofing material. The soundproofing material had a structure of transmission loss [A] (a structure in which the urethane foam is adhered to a metal plate and the skin is adhered to the rubber sheet).
[0079] The results of Example 6 are the same as those of Example 5, except for the results of the vibration-damping properties of the soundproofing material. In Example 6, the vibration-damping properties of the soundproofing material (loss factor ratio with a rubber sheet placed) are 0.96, the vibration-damping properties are evaluated as [◎], and the overall evaluation is [◎]. The results of the vibration-damping properties of the soundproofing material are better in Example 6 with a rubber sheet placed than in Example 5 without a rubber sheet placed. From the results of the vibration-damping properties, it can be understood that in Example 6, the soundproofing material is pressed more strongly by the weight of the rubber sheet placed on the surface of the skin material than in Example 5 (without a rubber sheet placed), and thus the slits of the polyurethane foam are expanded more than in Example 5 (without a rubber sheet placed) on the side opposite the skin material, and the polyurethane foam is expanded outward more than in Example 5 (without a rubber sheet placed) on the side opposite the skin material, thereby eliminating the bending of the soundproofing material, and is more reliably adhered to the metal plate than in Example 5.
[0080] In Example 7, a polyurethane foam raw material containing 100 parts by weight of polyol 6 (polymer polyol), 6.41 parts by weight of blowing agent, 3.33 parts by weight of amine catalyst-1, 0.37 parts by weight of amine catalyst-2, 0 parts by weight of foam stabilizer, 2.47 parts by weight of additive, isocyanate ISO-1:ISO-2=0:100, and isocyanate index 105 was used. The first layer was made of 6d PET fiber as a skin material, and the basis weight was 150 g / m. 2 , the second layer is 3D PET fiber, basis weight 100g / m 2 , acrylic ester resin is 50g / m 2 Impregnated with 300g / m2 2 The skin material used was
[0081] The results of Example 7 were as follows: the thickness of the impregnated hardened layer was 1 mm, the soundproofing material was constructed as an integrated skin with slits, the hardness of the soundproofing material at 25% compression was 529 N, the hardness of the soundproofing material at 50% compression was 1024 N, the hardness of the soundproofing material at 75% compression was 3933 N, the hardness of the soundproofing material was rated as "◎", the vibration damping property of the soundproofing material (loss coefficient ratio without placing a rubber sheet) was 0.62, the vibration damping property was rated as [◯], and the density of the polyurethane foam was 55 kg / m 3 The air permeability of the polyurethane foam is 36 (cc / cm 2 / sec)·mm, and the central layer air permeability (3) is 55(cc / cm 2 / sec)·mm, and the air permeability of the skin material including the impregnated hardened layer (1) is 8.23cc / cm 2 / sec, the reverberation chamber sound absorption coefficient of the skin material including the impregnated hardened layer was 59%, the reverberation chamber sound absorption coefficient of the skin material including the impregnated hardened layer was rated as "◎", the soundproofing material had a sound transmission loss of [A] (a configuration in which the urethane foam is adhered to a metal plate and the skin material is adhered to a rubber sheet), the soundproofing material had a sound transmission loss of 44.2dB, and the soundproofing material sound transmission loss was rated as "◎". Overall rating: "〇", and the soundproofing (vibration control, sound absorption) properties were good.
[0082] Example 8 is the same as Example 7, except that the soundproofing material of Example 7 was used and a 1 mm thick rubber sheet was placed on the surface of its skin to measure the vibration damping properties of the soundproofing material. The soundproofing material had a structure of transmission loss [A] (a structure in which the urethane foam is adhered to a metal plate and the skin is adhered to the rubber sheet).
[0083] The results of Example 8 are the same as those of Example 7, except for the results of the vibration-damping properties of the soundproofing material. In Example 8, the vibration-damping properties of the soundproofing material (loss factor ratio with a rubber sheet placed) are 0.95, the vibration-damping properties are evaluated as [◎], and the overall evaluation is [◎]. The results of the vibration-damping properties of the soundproofing material are better in Example 8 with a rubber sheet placed than in Example 7 without a rubber sheet placed. From the results of the vibration-damping properties, it can be understood that in Example 8, the soundproofing material is pressed more strongly by the weight of the rubber sheet placed on the surface of the skin material than in Example 7 (without a rubber sheet placed), and thus the slits of the polyurethane foam are expanded more than in Example 7 (without a rubber sheet placed) on the side opposite the skin material, and the polyurethane foam is expanded outward more than in Example 7 (without a rubber sheet placed) on the side opposite the skin material, thereby eliminating the bending of the soundproofing material, and is more reliably adhered to the metal plate than in Example 7.
[0084] Example 9 is the same as Example 1, except that the soundproofing material of Example 1 is used and the transmission loss configuration of the soundproofing material is [B] (a configuration in which the skin material is adhered to a metal plate and the urethane foam is adhered to a rubber sheet).
[0085] The results of Example 9 are the same as those of Example 1, except for the results of the vibration damping and transmission loss of the soundproofing material. In Example 9, the vibration damping of the soundproofing material (loss coefficient ratio without placing a rubber sheet) was 0.62, the vibration damping was evaluated as [◯], the transmission loss of the soundproofing material was 47.2 dB, the transmission loss of the soundproofing material was evaluated as "◎", and the overall evaluation was "◯", and the soundproofing (vibration damping, sound absorption) properties were good.
[0086] Example 10 is the same as Example 9, except that the soundproofing material of Example 9 (same as Example 1) was used, and a 1 mm-thick rubber sheet was placed on the surface of the skin material to measure the vibration damping properties of the soundproofing material. The structure of the soundproofing material's transmission loss was [B] (a structure in which the skin material is in close contact with a metal plate and the urethane foam is in close contact with the rubber sheet).
[0087] The results of Example 10 are the same as those of Example 9, except for the results of the vibration-damping properties of the soundproofing material. In Example 10, the vibration-damping properties of the soundproofing material (loss factor ratio with a rubber sheet placed) are 0.95, the vibration-damping properties are evaluated as [◎], and the overall evaluation is [◎]. The results of the vibration-damping properties of the soundproofing material are better in Example 10 with a rubber sheet placed than in Example 9 without a rubber sheet placed. From the results of the vibration-damping properties, it can be understood that in Example 10, the soundproofing material is pressed more strongly by the weight of the rubber sheet placed on the surface of the skin material than in Example 9 (without a rubber sheet placed), and thus the slits of the polyurethane foam are expanded more than in Example 7 (without a rubber sheet placed) on the side opposite the skin material, and the polyurethane foam is expanded outward more than in Example 7 (without a rubber sheet placed) on the side opposite the skin material, thereby eliminating the bending of the soundproofing material, and is more reliably adhered to the metal plate than in Example 9.
[0088] In Examples 1 to 10, as the air permeabilities (2) and (3) of the polyurethane foam (skin layer, center layer) increase, the transmission loss of the soundproofing material tends to increase, resulting in a high soundproofing effect. In particular, Example 5, which has the largest air permeabilities (2) and (3) of the skin layer and center layer of the polyurethane foam, has the highest transmission loss of the soundproofing material among Examples 1 to 10 and is excellent in soundproofing effect.
[0089] Comparative Example 1 is the same as Example 1, except that no slits were formed in the polyurethane foam similar to that in Example 1. The configuration of the soundproofing material's transmission loss is [A] (configuration in which the polyurethane foam is adhered to a metal plate and the skin material is adhered to a rubber sheet).
[0090] The results of Comparative Example 1 are the same as those of Example 1, except for the vibration-damping properties of the soundproofing material, the air permeability of the polyurethane foam skin layer (2), the air permeability of the central cavity (3), and the transmission loss of the soundproofing material. In Comparative Example 1, the vibration-damping properties of the soundproofing material (loss coefficient ratio without a rubber sheet placed) was 0.29, the vibration-damping properties were evaluated as [×], and the air permeability of the polyurethane foam skin layer (2) was 64 (cc / cm 2 / sec)·mm, and the central layer airflow (3) is 267(cc / cm 2 / sec)·mm, the soundproofing material had a transmission loss of 47.2 dB, the soundproofing material was rated as having a transmission loss of "◎", and the overall rating was [×]. The vibration damping results for the soundproofing material were worse in Comparative Example 1 without slits than in Example 1 with slits. Since no slits were formed in the polyurethane foam in Comparative Example 1, the soundproofing material was measured in a state in which it remained bent toward the polyurethane foam due to the contraction of the polyurethane foam after integral molding of the skin, and since the polyurethane foam of the soundproofing material did not adhere to the metal plate, the vibration damping properties of Comparative Example 1 (without slits) were worse than those of Example 1 (with slits).
[0091] Comparative Example 2 is the same as Comparative Example 1, except that the same soundproofing material (without slits) as in Comparative Example 1 was used, and a 1 mm-thick rubber sheet was placed on the surface of the skin to measure the vibration damping properties of the soundproofing material. The soundproofing material had the configuration of transmission loss [A] (a configuration in which the urethane foam is adhered to a metal plate, and the skin is adhered to the rubber sheet).
[0092] Comparative Example 2 is similar to Comparative Example 1 except for the results of the vibration damping of the soundproofing material. In Comparative Example 2, the vibration damping of the soundproofing material (with rubber sheet placed) was 0.57, the vibration damping evaluation was [△], and the overall evaluation was [△]. The results of the vibration damping of the soundproofing material were better in Comparative Example 2 with a rubber sheet placed than in Comparative Example 1 without a rubber sheet placed. In Comparative Example 2, the weight of the rubber sheet placed on the surface of the skin material pressed the soundproofing material more strongly than in Comparative Example 1 (without rubber sheet placed), and as a result, the contact area between the polyurethane foam and the device was larger than in Comparative Example 1 (without rubber sheet placed), and the vibration damping was better than in Comparative Example 1, and the vibration damping was evaluated as "△".
[0093] In Comparative Example 3, 65 parts by weight of polyol-2 (polyether polyol), 15 parts by weight of polyol-3 (polyether polyol), 10 parts by weight of polyol-4 (polyether polyol), 10 parts by weight of polyol-5 (polymer polyol), 3.30 parts by weight of blowing agent, 0 part by weight of amine catalyst-1, 0.1 part by weight of amine catalyst-2, 0.6 parts by weight of amine catalyst-3, 0.25 parts by weight of foam stabilizer, 2 parts by weight of additive, 100 parts by weight of ISO-3 isocyanate, and an isocyanate index of 90 were used as the polyurethane foam raw material, and the same skin material as in Examples 1 and 2 was used as the skin material.
[0094] The results of Comparative Example 3 were as follows: the thickness of the impregnated hardened layer was 1 mm, the soundproofing material was constructed as an integrated skin, there were no slits, the hardness of the soundproofing material at 25% compression was 16 N, the hardness at 50% compression was 30 N, and the hardness at 75% compression was 114 N, the hardness was rated "x", the vibration damping property of the soundproofing material (loss coefficient ratio without rubber sheet placed) was 0.70, the vibration damping property was rated [◯], and the density of the polyurethane foam was 70 kg / m 3 The air permeability of the polyurethane foam skin layer (2) is 53 (cc / cm 2 / sec)·mm, and the central layer airflow (3) is 131(cc / cm 2 / sec)·mm, and the air permeability of the skin material including the impregnated hardened layer (1) is 3.10cc / cm 2 / sec, the reverberation chamber sound absorption coefficient of the skin material including the impregnated hardened layer was 32%, the reverberation chamber sound absorption coefficient of the skin material including the impregnated hardened layer was rated "x", the soundproofing material had a sound transmission loss configuration of [A] (configuration in which urethane foam is adhered to a metal plate and the skin material is adhered to a rubber sheet), the soundproofing material had a sound transmission loss of 51.5 dB, the soundproofing material had a sound transmission loss rating of "◎", and the overall rating was "x". Comparative Example 3 had low hardness, slightly poor vibration damping, and a poor reverberation chamber sound absorption coefficient of the skin material including the impregnated hardened layer.
[0095] In Comparative Example 3, since the hardness of the soundproofing material was low, even though the polyurethane foam was bent toward the polyurethane foam due to shrinkage after being integrally molded with the skin, when the soundproofing material was placed on the equipment, the soundproofing material was pushed by its own weight, and even though no slits were formed in the polyurethane foam, the polyurethane foam spread outward on the side opposite the skin material, resulting in a larger contact area between the polyurethane foam and the equipment than in the other Comparative Examples, and the vibration damping properties of the soundproofing material were better than those of the other Comparative Examples.
[0096] Comparative Example 4 is the same as Comparative Example 3, except that the same soundproofing material (without slits) as in Comparative Example 3 was used, and a 1 mm-thick rubber sheet was placed on the surface of the skin material to measure the vibration damping properties of the soundproofing material. The soundproofing material had the configuration of transmission loss [A] (a configuration in which the urethane foam is adhered to a metal plate, and the skin material is adhered to the rubber sheet).
[0097] The results of Comparative Example 4 are similar to those of Comparative Example 3, except for the results of the vibration damping of the soundproofing material. In Comparative Example 4, the vibration damping of the soundproofing material (loss factor ratio with rubber sheet placed) is 0.97, the vibration damping evaluation is [◎], and the overall evaluation is [×]. The results of the vibration damping of the soundproofing material were better in Comparative Example 4 with the rubber sheet placed than in Comparative Example 3 without the rubber sheet placed.
[0098] In the soundproofing material of Comparative Example 4, the weight of the rubber sheet placed on the surface of the skin material pressed the soundproofing material more strongly than in Comparative Example 3 (no rubber sheet placed), resulting in a larger contact area between the polyurethane foam and the device than in Comparative Example 3 (no rubber sheet placed), and resulting in better vibration damping properties than in Comparative Example 3.
[0099] In this way, the soundproofing material of the present invention can correct the bending that occurs after the skin is integrally molded toward the polyurethane foam opposite the skin by expanding the slits formed in the polyurethane foam when the soundproofing material is placed on the floor of an automobile or the like, so that the polyurethane foam adheres closely to the floor surface, providing good soundproofing properties (including vibration control properties). [Explanation of symbols]
[0100] 10, 100 Soundproofing material 20, 200 Polyurethane foam 20a polyurethane foam raw material 25, 250 slits 30, 300 Skin material 31, 310 1st layer 33, 330 Second layer 34, 340 impregnated hardened layer 40 Mold 41 Lower mold 43 Upper mold 38 Release Agent
Claims
1. In soundproofing materials in which a skin material is integrally molded onto one side of a polyurethane foam, The soundproofing material has a compression hardness of 500 N or more, the compression hardness being measured by compressing a 200 mm square x 20 mm thick sample to 80% of the sample thickness at a test speed of 50 mm / min using a φ80 mm compression tool and measuring the load at 50% compression; The polyurethane foam has a slit formed from a surface opposite to the skin toward the skin, A soundproofing material characterized by satisfying at least one of the following requirements A to B. A: The air permeability (2) of sample A sliced to a thickness of 3 mm from the side opposite to the skin of the polyurethane foam is 36 to 276 (cc / cm 2 / sec) mm, B: The central layer from which the skin material and sample A were removed was sliced to a thickness of 3 mm to obtain sample B. The air permeability (3) of the sample B was 55 to 352 (cc / cm 2 / sec)·mm.
2. the skin material has an impregnated and cured layer of polyurethane foam raw material formed at the boundary with the polyurethane foam, 2. The soundproofing material according to claim 1, wherein the slits are formed up to the position of the impregnated and hardened layer.
3. The air permeability (1) of the skin material including the impregnated hardened layer based on JIS K6400-7B method: 2012 is 5 to 80 cc / cm 2 3. The soundproofing material according to claim 2, wherein the thickness of said soundproofing material is 1 / sec.
4. 4. The soundproofing material according to claim 1, wherein a loss factor ratio of the soundproofing material is 0.6 or more when loss factor ratio = (loss factor when no double-sided tape is attached) / (loss factor when double-sided tape is attached to the entire surface).
Citation Information
Patent Citations
Floor carpet for automobile
JP1998071884A
Sound insulating material
JP1999005499A
Floor mat
JP2001260734A
Structure for installing floor carpet
JP2001310671A
Composite panel and its manufacturing method
JP2002371702A