Binder composition for non-aqueous electrolyte secondary battery, negative electrode for non-aqueous electrolyte secondary battery, non-aqueous electrolyte secondary battery, and method for producing the same
The binder composition for non-aqueous electrolyte secondary batteries, containing specific monomers and copolymers, addresses the peeling issue and enhances low-temperature performance by maintaining surface tension and adhesion, thereby improving battery output and stability.
Patent Information
- Application Number
- JP2020132579
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-08-04
- Publication Date
- 2024-09-24
- Estimated Expiration
- 2040-08-04
AI Technical Summary
Non-aqueous electrolyte secondary batteries face issues with increased resistance and reduced battery output and life characteristics at low temperatures due to oxidation-reduction reactions at the electrode interface, and the negative electrode active material layer tends to peel off from the current collector during charging, especially in pouch batteries.
A binder composition for non-aqueous electrolyte secondary batteries is developed, comprising an aromatic vinyl monomer, unsaturated carboxylic acid alkyl ester monomer, (meth)acrylic acid monomer, and unsaturated carboxylic acid amide monomer, along with a hydrophobic copolymer and a water-soluble copolymer, which improves adhesion and suppresses peeling, maintaining a dynamic surface tension of 65 to 75 mN/m to prevent bubble generation.
The binder composition enhances battery output at low temperatures and prevents the negative electrode active material layer from peeling off during initial charging, improving coating stability and reducing defects.
Smart Images

Figure 0007555213000005 
Figure 0007555213000004 
Figure 0007555213000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a binder composition for a non-aqueous electrolyte secondary battery, a negative electrode slurry for a non-aqueous electrolyte secondary battery, a negative electrode for a non-aqueous electrolyte secondary battery, and a non-aqueous electrolyte secondary battery. [Background technology]
[0002] A non-aqueous electrolyte secondary battery has a problem that the resistance of the electrolyte and the resistance of the oxidation-reduction reaction at the electrode interface increase at low temperatures, resulting in a decrease in the battery output and life characteristics. In response to this problem, as in Patent Documents 1 and 2, it has been considered to improve the life characteristics of the battery at room temperature or low temperature and to reduce the internal resistance by devising a binder composition for non-aqueous electrolyte secondary batteries. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] WO2015 / 045522 publication [Patent Document 2] JP 2016-042408 A Summary of the Invention [Problem to be solved by the invention]
[0004] Therefore, the inventors tried to produce a negative electrode active material layer using a binder composition for a non-aqueous electrolyte secondary battery containing a styrene-acrylic acid ester-based polymer as described in Patent Documents 1 and 2, and found that there were problems in that air bubbles were generated when the slurry for the negative electrode active material layer was applied to the negative electrode current collector, which made the negative electrode prone to coating defects, and that the negative electrode active material layer was prone to peeling off from the negative electrode current collector after the first charge. In particular, in pouch batteries sealed with an aluminum laminate film or the like, pressure or heat may be applied from the outside during the initial charge in order to form a stable coating at the interface between the electrode and the electrolyte and to suppress distortion of the battery, and therefore, in pouch batteries and the like, the problem of the negative electrode active material layer peeling off from the negative electrode current collector during the initial charge becomes more pronounced.
[0005] The present invention has been made in view of the above problems, and has as its main object to provide a binder composition for a nonaqueous electrolyte secondary battery that improves battery output at low temperatures as compared to conventional methods and can realize a negative electrode active material layer that is easily applied to and adheres to a negative electrode current collector. [Means for solving the problem]
[0006] That is, the binder composition for non-aqueous electrolyte secondary batteries according to the present invention contains a hydrophobic copolymer containing units derived from one or more monomers selected from the group consisting of aromatic vinyl monomers, unsaturated carboxylic acid alkyl ester monomers, (meth)acrylic acid monomers, and unsaturated carboxylic acid amide monomers, and a water-soluble copolymer containing units derived from (meth)acrylic acid monomers and units derived from (meth)acrylonitrile monomers, dispersing the hydrophobic copolymer in an aqueous solution. In addition, the dynamic surface tension of the binder composition for non-aqueous electrolyte secondary batteries at a solid content of 3 mass% and a lifetime of 5 seconds according to the maximum bubble pressure method is 65 mN / m or more and 75 mN / m or less.
[0007] Such a binder composition for a non-aqueous electrolyte secondary battery contains a hydrophobic copolymer containing units derived from one or more monomers selected from the group consisting of an aromatic vinyl monomer, an unsaturated carboxylic acid alkyl ester monomer, a (meth)acrylic acid monomer, and an unsaturated carboxylic acid amide monomer, and a water-soluble copolymer containing units derived from a (meth)acrylic acid monomer and a (meth)acrylonitrile monomer, and therefore can improve battery output at low temperatures. In addition, the dynamic surface tension of an aqueous dispersion with a solid content of 3% by mass at a lifetime of 5 seconds as measured by the maximum bubble pressure method is 65 mN / m or more and 75 mN / m or less, so that the generation of bubbles can be suppressed when the negative electrode active material is applied. Furthermore, since the binder composition contains the hydrophobic copolymer and the water-soluble copolymer, peeling of the negative electrode active material layer from the negative electrode current collector during the initial charge can be suppressed compared to the case where a binder composition containing only a styrene-acrylic acid ester-based polymer is used.
[0008] The content of the water-soluble copolymer in the binder composition for non-aqueous electrolyte secondary batteries is preferably 15% by mass or more and 45% by mass or less, and the content of the hydrophobic copolymer is preferably 55% by mass or more and 85% by mass or less. The content of the water-soluble copolymer of 15% by mass or more is preferable because it can improve the stability of the hydrophobic copolymer during the polymerization reaction and during storage. In addition, the content of the water-soluble copolymer of 45% by mass or less is preferable because it can prevent the negative electrode active material layer from cracking or peeling when the negative electrode active material layer is coated, dried, and rolled.
[0009] The water-soluble copolymer preferably has a content of units derived from a (meth)acrylic acid monomer of 35% by mass or more and 65% by mass or less, a content of units derived from a (meth)acrylonitrile monomer of 35% by mass or more and 65% by mass or less, and a content of units derived from other monomers copolymerizable with the units derived from the (meth)acrylic acid monomer and / or the units derived from the (meth)acrylonitrile monomer of 0% by mass or more and 20% by mass or less. If the content of units derived from a (meth)acrylic acid monomer in the water-soluble copolymer is 35% by mass or more, the solubility of the water-soluble copolymer in water can be improved. As a result, the stability of the hydrophobic copolymer during polymerization reaction and storage can be improved, which is preferable. If the content of units derived from a (meth)acrylic acid monomer in the water-soluble copolymer is 65% by mass or less, the negative electrode active material layer is less likely to crack or peel when the negative electrode active material layer is coated, dried, and rolled, which is preferable.
[0010] If the other monomer contains, for example, a sulfonic acid group-containing ethylenically unsaturated monomer, the sulfonic acid group-containing ethylenically unsaturated monomer functions as a reactive surfactant during the production of the binder composition for non-aqueous electrolyte secondary batteries, so that even if the content of the water-soluble copolymer is reduced, the polymerization reaction of the hydrophobic copolymer and the dispersion stability during storage can be improved. As a result, compared to the case where a reactive surfactant is not added, it is preferable because the negative electrode active material layer is less likely to crack or peel when coated, dried, and rolled. A non-reactive surfactant may be used to improve the dispersion stability during the polymerization reaction and storage of the hydrophobic copolymer. However, a non-reactive surfactant tends to lower the surface tension, and the dynamic surface tension of an aqueous dispersion with a solid content of 3% by mass at a lifetime of 5 seconds measured by the maximum bubble pressure method may not be 65 mN / m or more. Therefore, in order to make the dynamic surface tension 65 mN / m or more, it is preferable not to use a non-reactive surfactant.
[0011] Specific examples of the sulfonic acid group-containing ethylenically unsaturated monomer include sodium (meth)acrylic acid 2-ethylsulfonate, sodium methacryloyloxypolyoxypropylene sulfate, and phenyl ether methacrylate sulfate.
[0012] The viscosity of an aqueous solution of the water-soluble copolymer with a solid content of 10% by mass is preferably 500 mPa·s or more and 3000 mPa·s or less. By setting the viscosity of the aqueous solution to 500 mPa·s or more, peeling of the negative electrode active material layer during the initial charge can be further suppressed, which is preferable. In addition, by setting the viscosity to 3000 mPa·s or less, the viscosity of the negative electrode coating slurry does not become too high, and there is no need to reduce the solid content concentration to adjust the viscosity, which is preferable because it reduces the drying time and improves productivity. Effect of the Invention
[0013] According to the present invention, the battery contains a hydrophobic copolymer containing units derived from one or more monomers selected from the group consisting of aromatic vinyl monomers, unsaturated carboxylic acid alkyl ester monomers, (meth)acrylic acid monomers, and unsaturated carboxylic acid amide monomers, and a water-soluble copolymer containing units derived from a (meth)acrylic acid monomer and a unit derived from a (meth)acrylonitrile monomer, thereby making it possible to improve battery output at low temperatures. In addition, since the dynamic surface tension at a lifetime of 5 seconds using the maximum bubble pressure method with a solid content of 3 mass % is 65 mN / m or more and 75 mN / m or less, the generation of bubbles when the negative electrode active material is applied can be suppressed.
[0014] Furthermore, since the battery contains the hydrophobic copolymer and the water-soluble copolymer, peeling of the negative electrode active material from the negative electrode current collector during initial charging can be suppressed. [Brief description of the drawings]
[0015] [Figure 1] 1 is a side cross-sectional view illustrating a schematic configuration of a lithium-ion secondary battery. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings. In this specification and drawings, components having substantially the same functional configurations are denoted by the same reference numerals and redundant explanations are omitted.
[0017] <1. Nonaqueous electrolyte secondary battery> A specific configuration of a nonaqueous electrolyte secondary battery according to one embodiment of the present invention will be described.
[0018] The lithium ion secondary battery 1 shown in FIG. 1 is an example of the nonaqueous electrolyte secondary battery 1 according to the present embodiment. As shown in FIG. 1, the lithium ion secondary battery 1 includes a positive electrode 10, a negative electrode 20, a separator 30, and a nonaqueous electrolyte. The charge voltage (oxidation-reduction potential) of the lithium ion secondary battery 1 is, for example, 4.0 V (vs. Li / Li+) or more and 5.0 V or less, particularly 4.2 V or more and 5.0 V or less. The shape of the lithium ion secondary battery 1 is not particularly limited, and may be, for example, any of a cylindrical shape, a square shape, a laminate shape, a button shape, or the like.
[0019] (1-1. Positive electrode) The positive electrode 10 includes a positive electrode current collector 11 and a positive electrode active material layer 12 . The positive electrode current collector 11 may be any conductive material, for example, a plate or foil, and is preferably made of aluminum, stainless steel, nickel-plated steel, or the like. The positive electrode active material layer 12 contains at least a positive electrode active material, and may further contain a conductive agent and a positive electrode binder.
[0020] The positive electrode active material is, for example, a transition metal oxide or solid solution oxide containing lithium, and is not particularly limited as long as it is a material that can electrochemically absorb and release lithium ions. Examples of transition metal oxides containing lithium include Li·Co-based composite oxides such as LiCoO2, LiNi x Co y M.N. z Examples of the solid solution oxide include Li·Ni·Co·MN-based composite oxides such as LiO2, Li·Ni-based composite oxides such as LiNiO2, and Li·MN-based composite oxides such as LiMN2O4. a M.N. x Co y Ni z O2 (1.150≦a≦1.430, 0.45≦x≦0.6, 0.10≦y≦0.15, 0.20≦z≦0.28), LiMN 1.5 Ni 0.5O4, etc. The content (content ratio) of the positive electrode active material is not particularly limited as long as it is a content that is applicable to the positive electrode active material layer 12 of the nonaqueous electrolyte secondary battery 1. These compounds may be used alone or in combination.
[0021] The conductive agent is not particularly limited as long as it is capable of increasing the conductivity of the positive electrode 10. Specific examples of the conductive agent include those containing one or more materials selected from carbon black, natural graphite, artificial graphite, and fibrous carbon. Examples of carbon black include furnace black, channel black, thermal black, ketjen black, and acetylene black. Examples of fibrous carbon include carbon nanotubes, graphene, and carbon nanofibers. The content of the conductive material is not particularly limited, and may be any content that is applicable to the positive electrode active material layer 12 of the nonaqueous electrolyte secondary battery 1.
[0022] Examples of the positive electrode binder include fluorine-containing resins such as polyvinylidene fluoride, ethylene-containing resins such as styrene-butadiene rubber, ethylene-propylene-diene terpolymer, acrylonitrile-butadiene rubber, fluororubber, polyvinyl acetate, polymethylmethacrylate, polyethylene, polyvinyl alcohol, carboxymethyl cellulose or a carboxymethyl cellulose derivative (such as a salt of carboxymethyl cellulose), or nitrocellulose. The positive electrode binder is not particularly limited as long as it can bind the positive electrode active material and the conductive agent onto the positive electrode current collector 11.
[0023] (1-2. Negative electrode) The negative electrode 20 includes a negative electrode current collector 21 and a negative electrode active material layer 22. The negative electrode current collector 21 may be any conductive material, and is preferably, for example, in the form of a plate or foil, and is made of copper, stainless steel, nickel-plated steel, or the like. The negative electrode active material layer 22 contains, for example, a binder composition for a non-aqueous electrolyte secondary battery, a negative electrode active material, and a water-soluble polymer compound.
[0024] The binder composition for a non-aqueous electrolyte secondary battery, together with the water-soluble polymer compound, serves to bind the negative electrode active material layer 22 onto the negative electrode current collector 21 . The content of the binder composition for a non-aqueous electrolyte secondary battery in the negative electrode active material layer 22 is preferably, for example, 0.5 mass % or more and 3.5 mass % or less. If the content of the binder composition for a non-aqueous electrolyte secondary battery is 0.5 mass % or more, it is possible to obtain a negative electrode 20 in which the negative electrode active material layer 22 is less likely to crack or peel off when the negative electrode active material layer 22 is coated, dried, and rolled, which is preferable. On the other hand, if the content of the binder composition for a non-aqueous electrolyte secondary battery is 3.5 mass % or less, it is possible to obtain a negative electrode 20 with good cycle performance without excessively increasing the electrode resistance, which is preferable.
[0025] The negative electrode active material is not particularly limited as long as it can electrochemically absorb and release lithium ions. Examples of the negative electrode active material include graphite active materials (artificial graphite, natural graphite, a mixture of artificial graphite and natural graphite, natural graphite coated with artificial graphite, etc.), Si-based active materials or Sn-based active materials (for example, a mixture of fine particles of silicon (Si) or tin (Sn) or an oxide thereof and a graphite active material, fine particles of silicon or tin, and an alloy based on silicon or tin), metallic lithium, and Li4Ti5O 12 Examples of the negative electrode active material include titanium oxide compounds such as SiO, lithium nitride, etc. One of the above-mentioned materials may be used alone or two or more of them may be used in combination. The oxide of silicon is SiO x It is expressed as (0≦x≦2).
[0026] The content of the negative electrode active material in the negative electrode active material layer 22 of this embodiment is preferably 90% by mass or more and 99% by mass or less, and more preferably 94% by mass or more and 98% by mass or less. If the content of the negative electrode active material in the negative electrode active material layer 22 is 94% by mass or more, the electrode resistance does not become excessively large, and the negative electrode 20 having good cycle performance can be obtained. On the other hand, if the content of the negative electrode active material in the negative electrode active material layer 22 is 98% by mass or less, the negative electrode 20 having better adhesion and good cycle performance can be obtained, which is preferable.
[0027] The water-soluble polymer compound is, for example, an alkali metal salt of carboxymethylcellulose. The content of the water-soluble polymer compound in the negative electrode active material layer 22 is preferably, for example, 0.5% by mass or more and 2.5% by mass or less. If the content of the water-soluble polymer compound is 0.5% by mass or more, it is preferable because good viscosity can be imparted to the slurry for coating the negative electrode active material layer 22. On the other hand, if the content of the water-soluble polymer compound is 3.5% by mass or less, excessive viscosity is not imparted to the slurry for coating the negative electrode active material layer 22, so that the slurry can be coated in a high solid content state and efficiently dried to obtain the negative electrode 20, which is preferable.
[0028] The coating amount of the negative electrode active material layer 22 is 5 mg / cm in surface density. 2 More than 25mg / cm 2 It is preferable that the concentration is 10 mg / cm or less. 2 More than 20mg / cm 2 It is more preferable that the coating be as follows (for single-sided coating): The thickness of the negative electrode active material layer 22 on one side is preferably, for example, 50 μm or more and 150 μm or less. By setting the coating amount and thickness of the negative electrode active material layer 22 within this range, the charge / discharge capacity of the nonaqueous electrolyte secondary battery can be increased, which is preferable.
[0029] The negative electrode 20 may further contain a conductive agent. As the conductive agent, those exemplified for the positive electrode 10 can be used.
[0030] (1-3. Separator) The separator 30 is not particularly limited, and may be any material that can be used as the separator 30 of the lithium ion secondary battery 1. As the separator 30, it is preferable to use a porous film, a nonwoven fabric, or the like that exhibits excellent high-rate discharge performance, either alone or in combination. Examples of the resin constituting the separator 30 include polyolefin resins such as polyethylene and polypropylene, polyester resins such as polyethylene terephthalate and polybutylene terephthalate, polyvinylidene difluoride, vinylidene fluoride-hexafluoropropylene copolymer, vinylidene difluoride-perfluorovinyl ether copolymer, vinylidene difluoride-tetrafluoroethylene copolymer, vinylidene difluoride-trifluoroethylene copolymer, vinylidene difluoride- ... copolymer, vinylidene difluoride-hexafluoroacetone copolymer, vinylidene difluoride-ethylene copolymer, vinylidene difluoride-propylene copolymer, vinylidene difluoride-trifluoropropylene copolymerExamples of the porosity of separator 30 include vinylidene fluoride-tetrafluoroethylene-hexafluoropropylene copolymer, vinylidene difluoride-tetrafluoroethylene copolymer, vinylidene difluoride-ethylene-tetrafluoroethylene copolymer, etc. The porosity of separator 30 is not particularly limited, and the porosity of separator 30 of conventional lithium ion secondary battery 1 can be arbitrarily applied.
[0031] The surface of the separator 30 may have a heat-resistant layer containing inorganic particles to improve heat resistance, or a layer containing an adhesive to bond with the electrodes and fix the battery element. Examples of the inorganic particles include Al2O3, AlOOH, Mg(OH)2, and SiO2. Examples of the adhesive include vinylidene fluoride-hexafluoropropylene copolymer, acid-modified vinylidene fluoride polymer, and styrene-(meth)acrylic acid ester copolymer.
[0032] (1-4.Non-aqueous electrolyte) The non-aqueous electrolyte can be used without any particular limitation as long as it is the same as the non-aqueous electrolyte conventionally used in the lithium ion secondary battery 1. The non-aqueous electrolyte has a composition in which an electrolyte salt is contained in a non-aqueous solvent.Examples of the non-aqueous solvent include cyclic carbonates such as propylene carbonate, ethylene carbonate, butylene carbonate, chloroethylene carbonate, and vinylene carbonate; cyclic esters such as γ-butyrolactone and γ-valerolactone; chain carbonates such as dimethyl carbonate, diethyl carbonate, and ethylmethyl carbonate; methylformate, methylacetate, methylbutyrate, ethylpropionate, and propylpropionate. Chain esters such as tetrahydrofuran or a derivative thereof, 1,3-dioxane, 1,4-dioxane, 1,2-dimethoxyethane, 1,4-dibutoxyethane, or methyldiglyme, ethers such as ethylene glycol monopropyl ether and propylene glycol monopropyl ether, nitriles such as acetonitrile and benzonitrile, dioxolane or a derivative thereof, ethylene sulfide, sulfolane, sultone or a derivative thereof, or the like can be used alone or in combination of two or more of them.When two or more kinds of solvents are mixed and used, the mixing ratio of each solvent may be the same as that used in the conventional lithium ion secondary battery 1.
[0033] Examples of electrolyte salts include LiClO4, LiBF4, LiAsF6, LiPF6, and LIPF6-x (C n F 2n+1 )x[where 1 <x<6、n=1or2]、LiSCN、LiBr、LiI、Li2SO4、Li2B 10 Cl 10 , NaClO4, NaI, NaSCN, NaBr, KClO4, KSCN and other inorganic ion salts containing one of lithium (Li), sodium (Na) or potassium (K), LiCF3SO3, LiN(CF3SO2)2, LiN(C2F5SO2)2, LiN(CF3SO2)(C4F9SO2), LiC(CF3SO2)3, LiC(C2F5SO2)3, (CH3)4NBF4, (CH3)4NBr, (C2H5)4NClO4, (C2H5)4NI, (C3H7)4NBr, (n-C4H9)4NClO4, (n-C4H9)4NI, (C2H5)4N-maleate, (C2H5)4N-benzoate, (C2H5)4N-phtalate, lithium stearyl sulfonic acid Examples of the ionic compounds include organic ion salts such as lithium, octyl sulfonic acid lithium, and dodecyl benzenesulfonic acid lithium. These ionic compounds can be used alone or in combination of two or more. The concentration of the electrolyte salt may be the same as that of the nonaqueous electrolyte used in the conventional lithium ion secondary battery 1, and is not particularly limited. In this embodiment, it is preferable to use a nonaqueous electrolyte containing the above-mentioned lithium compound (electrolyte salt) at a concentration of about 0.8 mol / L or more and 1.5 mol / L or less.
[0034] In addition, various additives may be added to the non-aqueous electrolyte. Examples of such additives include negative electrode additives, positive electrode additives, ester additives, carbonate additives, sulfate additives, phosphate additives, borate additives, acid anhydride additives, and electrolyte additives. Any one of these may be added to the non-aqueous electrolyte, or multiple types of additives may be added to the non-aqueous electrolyte.
[0035] <2. Method for Manufacturing Nonaqueous Electrolyte Secondary Battery According to the Present Embodiment> Next, a method for manufacturing the lithium ion secondary battery 1 will be described. The positive electrode 10 is produced as follows. First, a positive electrode active material, a conductive agent, and a positive electrode binder are mixed in a desired ratio and dispersed in a solvent (e.g., N-methyl-2-pyrrolidone) to form a positive electrode mixture slurry. Next, the positive electrode mixture slurry is applied onto a positive electrode current collector 11 and dried to form a positive electrode active material layer 12. The application method is not particularly limited. Examples of the application method include a knife coater method, a gravure coater method, a reverse roll coater, and a slit die coater. The following application steps are also performed in the same manner. Next, the positive electrode active material layer 12 is pressed to a desired density by a press machine. In this way, the positive electrode 10 is produced.
[0036] The negative electrode 20 is also produced in the same manner as the positive electrode 10. First, a mixture of materials constituting the negative electrode active material layer 22 is dispersed in a solvent (e.g., water) to produce a negative electrode mixture slurry (hereinafter also referred to as a slurry for a non-aqueous electrolyte battery negative electrode). Next, the negative electrode mixture slurry is applied onto the negative electrode current collector 21 and dried to form the negative electrode active material layer 22. Next, the negative electrode active material layer 22 is pressed by a press machine to a desired density. In this way, the negative electrode 20 is produced.
[0037] Next, the separator 30 is sandwiched between the positive electrode 10 and the negative electrode 20 to prepare an electrode structure. Next, the electrode structure is processed into a desired shape (e.g., cylindrical, rectangular, laminated, button, etc.) and inserted into a container of the desired shape. Next, a nonaqueous electrolyte is injected into the container, so that the electrolyte is impregnated into each pore in the separator 30 and the gaps in the positive electrode 10 and the negative electrode 20. In this way, a lithium ion secondary battery 1 is prepared.
[0038] <3. Characteristic configuration of the binder composition according to this embodiment> The binder composition for a non-aqueous electrolyte secondary battery according to this embodiment is a water-dispersed binder composition for a non-aqueous electrolyte secondary battery, which contains a hydrophobic copolymer and a water-soluble copolymer that disperses the hydrophobic copolymer in an aqueous solution, and is characterized in that the dynamic surface tension of an aqueous dispersion having a solid content of 3 mass % at a lifetime of 5 seconds as measured by a maximum bubble pressure method is 65 mN / m or more and 75 mN / m or less.
[0039] (3-1. Hydrophobic Copolymer) The hydrophobic copolymer contains units derived from one or more monomers selected from the group consisting of aromatic vinyl monomers, unsaturated carboxylic acid alkyl ester monomers, (meth)acrylic acid monomers, and unsaturated carboxylic acid amide monomers. Examples of aromatic vinyl compounds include styrene, p-methylstyrene, m-methylstyrene, o-methylstyrene, ot-butylstyrene, mt-butylstyrene, pt-butylstyrene, p-chlorostyrene, o-chlorostyrene, etc. Among these, styrene is preferred. Examples of the unsaturated carboxylic acid alkyl ester monomer include methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, isopropyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isobutyl (meth)acrylate, pentyl (meth)acrylate, n-hexyl (meth)acrylate, isoamyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, and isobornyl (meth)acrylate. Examples of the (meth)acrylic acid monomer include methacrylic acid, acrylic acid, itaconic acid, fumaric acid, and maleic acid. Examples of the unsaturated carboxylic acid amide monomer include (meth)acrylamide, (meth)N-methylacrylamide, (meth)N-dimethylacrylamide, (meth)N-hydroxymethylacrylamide, (meth)N-butoxymethylacrylamide, and (meth)isobutoxymethylacrylamide. Other copolymerizable monomers include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, 2-acryloyloxyethyl-2-hydroxyethyl-phthalic acid, ethoxy-diethylene glycol (meth)acrylate, methoxy-triethylene glycol (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, phenoxy-polyethylene glycol (meth)acrylate, phenoxydiethylene glycol (meth)acrylate, phenoxyethyl (meth)acrylate, methoxyethyl (meth)acrylate, glycidyl (meth)acrylate, (meth)acrylonitrile, 2-acrylamido-2-methylpropanesulfonic acid, and 2-methacryloyloxyethyl acid phosphate.
[0040] The content of the hydrophobic copolymer in the binder composition for a non-aqueous electrolyte secondary battery according to this embodiment is preferably 55% by mass or more and 85% by mass or less. If the content of the hydrophobic copolymer is 55% by mass or more, the flexibility of the binder composition for a non-aqueous electrolyte secondary battery and the negative electrode active material layer 22 using the same can be further improved, and the occurrence of cracks during coating and drying in the negative electrode active material layer 22 can be suppressed, which is preferable. If the content of the hydrophobic copolymer is 85% by mass or less, the content of the water-soluble copolymer can be 15 wt% or more. As a result, the storage stability of the negative electrode mixture slurry can be further improved, which is preferable.
[0041] (3-2.Water-soluble copolymer) The water-soluble copolymer contains units derived from a (meth)acrylic acid monomer and units derived from a (meth)acrylonitrile monomer. The water-soluble copolymer preferably has, for example, a content of units derived from a (meth)acrylic acid monomer of 35% by mass or more and 65% by mass or less, a content of units derived from a (meth)acrylonitrile monomer of 35% by mass or more and 65% by mass or less, and a content of units derived from other monomers copolymerizable with the (meth)acrylic acid monomer and / or (meth)acrylonitrile of 0% by mass or more and 20% by mass or less.
[0042] If the content of the units derived from the (meth)acrylic acid monomer in the water-soluble copolymer is 35% by mass or more, the water-soluble copolymer becomes easily soluble in water, and the dispersibility of the negative electrode active material and the storage stability of the negative electrode mixture slurry can be further improved, which is preferable. Also, if the content of the structural units derived from the (meth)acrylic acid monomer in the water-soluble copolymer is 65% by mass or less, the occurrence of cracks in the electrode can be further suppressed during the coating and drying process of the negative electrode mixture slurry, which is preferable.
[0043] If the content of the structural unit derived from (meth)acrylonitrile in the water-soluble copolymer is 35% by mass or more, this is preferable because it can further improve the adhesion of the negative electrode active material layer 22 to the negative electrode current collector 21. If the content of the structural unit derived from (meth)acrylonitrile in the water-soluble copolymer is 65% by mass or less, this is preferable because it makes the water-soluble copolymer more soluble in water, and it is easier to improve the dispersibility of the negative electrode active material and the storage stability of the negative electrode mixture slurry.
[0044] When the content of structural units derived from (meth)acrylic acid-based monomers and other monomers copolymerizable with (meth)acrylonitrile in the water-soluble copolymer is 20 mass% or less, it is possible to suppress the occurrence of electrode cracks during the application and drying process of the negative electrode mixture slurry and the peeling of the negative electrode active material from the negative electrode current collector 21 during the initial charge.
[0045] The (meth)acrylic acid monomer preferably contains at least one selected from the group consisting of (meth)acrylic acid, metal salts of (meth)acrylic acid, ammonium salts of (meth)acrylic acid, and amine salts of (meth)acrylic acid.
[0046] As the metal salt of (meth)acrylic acid, for example, it is preferable to use an alkali metal salt of acrylic acid. Specific examples of the metal salt of acrylic acid include sodium acrylate, lithium acrylate, potassium acrylate, calcium acrylate, magnesium acrylate, sodium methacrylate, lithium methacrylate, potassium methacrylate, calcium methacrylate, etc. Among these, it is more preferable to use sodium acrylate.
[0047] Examples of the ammonium salt of (meth)acrylic acid include ammonia-neutralized (meth)acrylic acid, monoethanolamine-neutralized (meth)acrylic acid, diethanolamine-neutralized (meth)acrylic acid, hydroxylamine-neutralized (meth)acrylic acid, etc. Among these, it is more preferable to use ammonia-neutralized (meth)acrylic acid.
[0048] The other monomer copolymerizable with the (meth)acrylic acid monomer and (meth)acrylonitrile in the water-soluble copolymer preferably contains, for example, a sulfonic acid group-containing ethylenically unsaturated monomer. Specific examples of the sulfonic acid group-containing ethylenically unsaturated monomer include sodium (meth)acrylic acid 2-ethylsulfonate, sodium methacryloyloxypolyoxypropylene sulfate, and phenyl ether methacrylate sulfate.
[0049] The viscosity of an aqueous solution of the water-soluble copolymer having a solid content of 10% by mass is preferably in the range of 500 mPa·s or more and 3000 mPa·s or less. It is preferable that the viscosity of the water-soluble copolymer is 500 mPa s or more, since this can improve the adhesion of the negative electrode active material layer 22 to the negative electrode current collector 21. It is also preferable that the viscosity of the water-soluble copolymer is 3000 mPa s or less, since this does not impart excessive viscosity to the slurry for coating the negative electrode active material layer 22, and therefore the slurry can be coated in a high solid content state, and the negative electrode 20 can be obtained by efficiently drying.
[0050] The manufacturing method for achieving the above viscosity is not particularly limited, but the viscosity may be increased by using a divinyl monomer. As the divinyl monomer, N,N'-methylenebisacrylamide, ethylene glycol dimethacrylate, N,N'-ethylenebis[2-(vinylsulfonyl)acetamide], N,N'-trimethylenebis[2-(vinylsulfonyl)acetamide], etc. can be used.
[0051] The content of the water-soluble copolymer in the binder composition for a non-aqueous electrolyte secondary battery is preferably 15% by mass or more and 45% by mass or less. If the content of the water-soluble copolymer is 15% by mass or more, the stability of the hydrophobic copolymer during the polymerization reaction and during storage can be improved, and if the content of the water-soluble copolymer is 45% by mass or less, the negative electrode active material layer 22 is less likely to crack or peel off when the negative electrode active material layer 22 is coated, dried, and rolled, so this is preferable.
[0052] <4. Method for producing binder composition for non-aqueous electrolyte secondary battery according to the present embodiment> The binder composition for a non-aqueous electrolyte secondary battery according to this embodiment can be produced, for example, by the following steps or procedures. (4-1. Synthesis of Water-Soluble Copolymer) In a flask, acrylic acid monomers, acrylonitrile, and other polymerizable monomers as necessary are mixed and thoroughly stirred in an aqueous solution containing sodium hydroxide and / or ammonia as necessary. The atmosphere in the flask is then replaced with nitrogen and heated to 60°C. When the temperature of the solution reaches 60°C, a reaction initiator is added to start polymerization. By reacting with stirring, an aqueous solution of a water-soluble copolymer can be obtained. As the other polymerizable monomer, a reactive surfactant such as a sulfonic acid group-containing ethylenically unsaturated monomer may be further added, if necessary. The sulfonic acid group-containing ethylenically unsaturated monomer includes, for example, one or more selected from the group consisting of sodium (meth)acrylic acid 2-ethylsulfonate, sodium methacryloyloxypolyoxypropylene sulfate, and phenyl ether methacrylate sulfate. Use of these reactive surfactants as the other polymerizable monomers is preferable because it is possible to stably disperse the hydrophobic copolymer in water while further reducing the amount of the water-soluble copolymer added during synthesis of the hydrophobic copolymer described below or during storage of the binder for nonaqueous electrolyte secondary batteries.
[0053] (4-2. Synthesis of binder composition for non-aqueous electrolyte secondary battery) The aqueous solution of the water-soluble copolymer obtained as described above and the monomers that are the raw materials for the hydrophobic copolymer are placed in a flask, and then the atmosphere in the flask is replaced with nitrogen and heated to 60° C. When the temperature of the solution reaches 60° C., a reaction initiator is added to initiate polymerization. By carrying out a polymerization reaction while stirring in the presence of the water-soluble copolymer, the hydrophobic copolymer is synthesized in a state where it is stably dispersed in water, and an aqueous solution of a binder composition for non-aqueous electrolyte secondary batteries is obtained.
[0054] Examples of reaction initiators for the water-soluble copolymer and the hydrophobic copolymer that can be used include azo compounds such as α,α'-azobisisobutyronitrile and 2,2'-azobis(2-methyl-N-2-hydroxyethylpropionamide), and persulfates such as ammonium persulfate and potassium persulfate.
[0055] <5. Effects of this embodiment> According to the binder composition for non-aqueous electrolyte secondary batteries configured as described above, the binder composition contains a hydrophobic copolymer containing units derived from one or more monomers selected from the group consisting of aromatic vinyl monomers, unsaturated carboxylic acid alkyl ester monomers, (meth)acrylic acid monomers, and unsaturated carboxylic acid amide monomers, and the shell contains a water-soluble copolymer containing units derived from a (meth)acrylic acid monomer and a unit derived from a (meth)acrylonitrile monomer, so that the battery output at low temperatures can be improved. In addition, since the hydrophobic copolymer is synthesized in the presence of the water-soluble copolymer, it is not necessary to add a non-reactive surfactant separately when producing the binder composition for non-aqueous electrolyte secondary batteries. As a result, the decrease in dynamic surface tension of the aqueous dispersion of the binder composition for non-aqueous electrolyte secondary batteries having a solid content of 3% by mass at a lifetime of 5 seconds as measured by the maximum bubble pressure method can be suppressed and maintained in the range of 65 mN / m to 75 mN / m, compared to the case where a non-reactive surfactant is added separately. Since the dynamic surface tension of the aqueous dispersion of the binder composition for non-aqueous electrolyte secondary batteries having a solid content of 3% by mass at a lifetime of 5 seconds measured by the maximum bubble pressure method can be maintained at 65 mN / m or more and 75 mN / m or less, the generation of bubbles can be suppressed when applying the negative electrode active material. The dynamic surface tension is preferably 70 mN / m or more and 73 mN / m or less, and more preferably 71.5 mN / m or more and 72.0 mN / m or less. Furthermore, since the binder composition contains the hydrophobic copolymer and the water-soluble copolymer having the above-mentioned composition, the peeling of the negative electrode active material layer 22 from the negative electrode current collector 21 during the initial charge can be suppressed. It is considered that this peeling suppression effect is due to the fact that the adhesive strength to the current collector is not reduced even in the high-temperature electrolyte during the initial charge due to the inclusion of the water-soluble copolymer having the above-mentioned composition. In addition, since the content of the water-soluble copolymer in the binder composition for non-aqueous electrolyte secondary batteries can be suppressed to 45 mass % or less, cracks during coating and drying of the negative electrode active material layer can be reduced compared to a binder composition consisting only of a water-soluble copolymer containing units derived from a (meth)acrylic acid-based monomer and units derived from a (meth)acrylonitrile monomer. EXAMPLES
[0056] The present invention will be described in more detail below with reference to specific examples. However, the following examples are merely examples of the present invention, and the present invention is not limited to the following examples. In the present example, binders for non-aqueous electrolyte secondary batteries of Examples 1 and 2 and Comparative Examples 1 and 2 were prepared, secondary batteries were fabricated using them, and these secondary batteries were evaluated. Each of the examples and comparative examples will be described below.
[0057] <Example 1> (Synthesis of Water-soluble Copolymer) In a 2000 ml separable flask equipped with a mechanical stirrer, a stirring rod, and a thermometer, 60.0 g of acrylic acid, 75.0 g of acrylonitrile, 15.0 g of sodium ethyl methacrylic acid 2-sulfonate, 0.225 g of N,N'-methylenebisacrylamide, 166.52 ml of 4 mol / l aqueous sodium hydroxide solution, and 653.26 g of ion-exchanged water were placed and stirred at 450 rpm. After stirring, the system was replaced with nitrogen, and the jacket temperature was set to 85°C and the temperature was raised. When the temperature in the system reached 60°C, an aqueous initiator solution in which 3338 mg of 2,2'-azobis(2-methyl-N-2-hydroxyethylpropionamide) was dissolved in 30.0 g of ion-exchanged water was added. With the jacket temperature set to 85°C, stirring was continued for 12 hours from the addition of the initiator, to obtain a pale yellow aqueous solution. This pale yellow aqueous solution is an aqueous solution containing a water-soluble copolymer. The non-volatile content of the aqueous solution after the reaction was measured and found to be 15.2% by mass. The pale yellow aqueous solution was then concentrated by heating under reduced pressure to remove the unreacted monomers. Ammonia water and ion-exchanged water were then added to adjust the solid content and pH of the aqueous polymer solution, yielding a water-soluble copolymer aqueous solution with a solid content of 7% by mass and a pH of 7.5. The solution was stirred at 25°C and a shear rate of 100 s -1 The viscosity of the 7% by mass water-soluble copolymer solution was 606 mPa·s. The measurement was performed using an Anton Paar rheometer MCR102 at a rotation speed of 100 rpm.
[0058] (Synthesis of binder composition for non-aqueous electrolyte secondary battery) In a 1000 ml separable flask equipped with a mechanical stirrer, a stirring rod, and a thermometer, 321.43 g of the water-soluble copolymer aqueous solution having a solid content of 7% by mass and a pH of 7.5, 26.25 g of styrene and 26.25 g of 2-ethylhexyl acrylate, which are raw materials for the hydrophobic copolymer, and 121.07 g of ion-exchanged water were charged and stirred at 550 rpm. After stirring, the system was replaced with nitrogen, and the jacket temperature was set to 70 ° C. and the temperature was raised. When the temperature in the system reached 60 ° C., an initiator aqueous solution in which 489 mg of ammonium persulfate was dissolved in 5.0 g of ion-exchanged water was added. With the jacket temperature set to 70 ° C., stirring was continued for 12 hours from the addition of the initiator to obtain a milky white dispersion. This milky white dispersion is a liquid containing a binder composition for non-aqueous electrolyte secondary batteries. This liquid is a binder composition for non-aqueous electrolyte secondary batteries in a stable dispersion state in water, in which the hydrophobic copolymer formed by copolymerization of styrene and 2-ethylhexyl acrylate, which were added as raw materials for the hydrophobic copolymer, is covered with the water-soluble copolymer. The non-volatile content of the aqueous solution after the reaction was measured and found to be 15.0% by mass. The milky white dispersion was then concentrated by heating and vacuum distillation to remove unreacted monomers. Ammonia water and ion-exchanged water were then added to adjust the solid content concentration and pH, and a dispersion of a binder composition for non-aqueous electrolyte secondary batteries containing 10% by mass of solids and having a pH of 7.5 was obtained. 25°C, shear rate 100 s -1 The viscosity of the dispersion with a solid content of 10 mass % was 355 mPa s.
[0059] <Example 2> (Synthesis of binder composition for non-aqueous electrolyte secondary battery) In a 1000 ml separable flask equipped with a mechanical stirrer, a stirring rod, and a thermometer, 357.14 g of the water-soluble copolymer aqueous solution with a solid content of 7% by mass and pH 7.5 prepared in Example 1, 18.75 g of styrene and 18.75 g of 2-ethylhexyl acrylate, which are raw materials for the hydrophobic copolymer, and 100.36 g of ion-exchanged water were charged and stirred at 550 rpm. After stirring, the system was replaced with nitrogen, and the jacket temperature was set to 70 ° C. and the temperature was raised. When the temperature in the system reached 60 ° C., an initiator aqueous solution in which 408 mg of ammonium persulfate was dissolved in 5.0 g of ion-exchanged water was added. With the jacket temperature set to 70 ° C., stirring was continued for 12 hours from the addition of the initiator to obtain a milky white dispersion. This milky white dispersion is a liquid containing a binder composition for non-aqueous electrolyte secondary batteries. This liquid is a binder composition for non-aqueous electrolyte secondary batteries in a stable dispersion state in water, in which the hydrophobic copolymer produced by copolymerization of styrene and 2-ethylhexyl acrylate, which were added as raw materials for the hydrophobic copolymer, is covered with the water-soluble copolymer. The non-volatile content of the aqueous solution after the reaction was measured and found to be 12.5% by mass. The milky white dispersion was then concentrated by heating and vacuum distillation to remove unreacted monomers. Ammonia water and ion-exchanged water were then added to adjust the solid content concentration and pH, and a dispersion of a binder composition for non-aqueous electrolyte secondary batteries containing 10% by mass of solids and having a pH of 7.5 was obtained. 25°C, shear rate 100 s -1 The viscosity of the binder composition dispersion for a non-aqueous electrolyte secondary battery having a solid content of 10 mass % was 398 mPa·s.
[0060] <Comparative Example 1> (Synthesis of binder composition for non-aqueous electrolyte secondary battery) In a 1000 ml separable flask equipped with a mechanical stirrer, a stirring rod, and a thermometer, 0.45 g of sodium dodecylbenzenesulfonate, which is a non-reactive (low molecular weight) surfactant, 18.75 g of styrene and 18.75 g of 2-ethylhexyl acrylate, which are raw materials for the hydrophobic copolymer, and 100.36 g of ion-exchanged water were charged and stirred at 550 rpm. After stirring, the system was replaced with nitrogen, and the jacket temperature was set to 70 ° C. and the temperature was raised. When the temperature in the system reached 60 ° C., an initiator aqueous solution in which 408 mg of ammonium persulfate was dissolved in 5.0 g of ion-exchanged water was added. Stirring was continued for 12 hours from the addition of the initiator with the jacket temperature set to 70 ° C. to obtain a milky white dispersion. This milky white dispersion is a liquid containing a binder composition for non-aqueous electrolyte secondary batteries. In this liquid, the hydrophobic copolymer is dispersed in water by being covered with sodium dodecylbenzenesulfonate, which is a non-reactive surfactant. The non-volatile content of the aqueous solution after the reaction was measured and found to be 26.0% by mass. The milky white dispersion was then concentrated by heating and vacuum distillation to remove unreacted monomers. Ammonia water and ion-exchanged water were then added to adjust the solid content concentration and pH, to obtain a binder composition dispersion for non-aqueous electrolyte secondary batteries containing 10% by mass of solids and having a pH of 7.5. 25°C, shear rate 100 s -1 The viscosity of the binder composition dispersion for non-aqueous electrolyte secondary batteries having a solid content of 10 mass % was 398 mPa·s.
[0061] <Comparative Example 2> As the binder composition for a non-aqueous electrolyte secondary battery, a commercially available modified styrene butadiene rubber (hereinafter also referred to as modified SBR) was used.
[0062] <Measurement of dynamic surface tension> The dynamic surface tension of the binder composition for non-aqueous electrolyte secondary batteries prepared to a solid content of 3% was measured by measuring the change over time by the maximum bubble pressure method using a dynamic surface tensiometer BP-D5L manufactured by Kyowa Interface Science Co., Ltd., and the value at the time of a lifetime of 5000 msec was taken as the dynamic surface tension. The results are shown in Table 1 below.
[0063] [Table 1]
[0064] <Anode coating evaluation> (Negative electrode production) A negative electrode mixture slurry was prepared by dissolving and dispersing graphite, a binder composition for non-aqueous electrolyte secondary batteries, and a sodium salt of carboxymethylcellulose in an aqueous solvent at a mass ratio of 97.5:1.5:1 of solid content. The negative electrode mixture slurry was then applied to both sides of a copper foil current collector having a thickness of 10 μm, and then dried. The dried coating layer was rolled to prepare a double-sided negative electrode. The density of the negative electrode active material layer after rolling was 1.65 g / cm3, and the coating amount was 11 mg / cm2 on both sides. (Anode coating evaluation) For the rolled double-sided negative electrodes prepared as described above, the number of dents thought to be coating defects caused by bubbles in five randomly selected 15 cm square areas was counted. The results are shown in Table 2.
[0065] [Table 2]
[0066] <Evaluation of peeling during first charge> (Preparation of positive electrode) A positive electrode mixture slurry was prepared by dissolving and dispersing lithium cobalt oxide, carbon black, and polyvinylidene fluoride (PVDF) in N-methylpyrrolidone at a mass ratio of 97.5:1.2:1.3 in solid content. The positive electrode mixture slurry was then applied to one side of an aluminum foil current collector with a thickness of 12 μm and then dried. The dried coating layer was rolled to prepare a single-sided positive electrode. The density of the positive electrode active material layer after rolling was 4.15 g / cm3, and the coating amount was 19.5 mg / cm2.
[0067] (Preparation of non-aqueous electrolyte secondary battery) After welding aluminum and nickel lead wires to the above-mentioned single-sided positive electrode and double-sided negative electrode, the single-sided positive electrode was folded in half so that the positive electrode active material layer was on the inside, and the polyethylene porous separator was folded in half and placed inside the folded positive electrode. The double-sided negative electrode was placed further inside the separator so that the positive electrode and the negative electrode faced each other through the separator, and these were stored in an aluminum laminate film with the lead wires drawn out to the outside. An electrolyte was poured into this and the battery was sealed under reduced pressure to prepare a secondary battery before initial charging. The electrolyte used was a solution of 1M LiPF6 dissolved in a solvent made of ethylene carbonate / ethyl propionate mixed in a volume ratio of 3:7.
[0068] (Evaluation of peeling during first charge) After injecting the electrolyte, the secondary battery was left to stand at 25°C for 12 hours before initial charging, and was sandwiched between two 500μm porous PTFE sheets. In this state, a constant current charge was performed at 1 / 5 CA (1CA is a 1-hour discharge rate) of the design capacity up to 4.4V while applying a pressure of 0.8MPa with a heat press set at 60°C, and then a constant voltage charge was performed at 4.4V up to 1 / 20 CA. After that, the secondary battery was allowed to cool to room temperature and the pressure was released, and the secondary battery was disassembled in a glove box, and the state of the negative electrode was visually observed. The results are shown in Table 3.
[0069] [Table 3]
[0070] <Low temperature output evaluation> After the injection, the secondary battery was left to stand at 25 ° C for 12 hours before initial charging, sandwiched between two 500 μm porous PTFE sheets, and while applying a pressure of 0.8 MPa with a heat press set at 60 ° C, it was charged at a constant current to 4.4 V at 1 / 5 CA (1 CA is a 1-hour discharge rate) of the design capacity, and then charged at a constant voltage to 1 / 20 CA at 4.4 V. Thereafter, it was allowed to cool to room temperature, the pressure was released, and it was sandwiched between two Bakelite plates and discharged at a constant current to 3.0 V at 1 / 5 CA at 25 ° C. Then, constant current charging to 4.4 V at 1 / 5 CA of the design capacity, constant voltage charging to 1 / 20 CA at 4.4 V, and constant current discharging to 3.0 V at 1 / 2 CA were repeated three times. Furthermore, after constant current charging at 1 / 5 CA to 4.4 V and constant voltage charging at 4.4 V to 1 / 20 CA, the secondary battery was transferred to a thermostatic chamber at -10°C and left for 3 hours to cool to the same temperature as the set temperature. After that, constant current discharging was performed at 1 / 2 CA to 3.0 V. The discharge capacity at this time was divided by the third discharge capacity of 1 / 2 CA discharge performed at 25°C to calculate the discharge capacity retention rate at -10°C relative to 25°C. The results are shown in Table 4.
[0071] [Table 4]
[0072] (Consideration) From the results of Tables 1 and 2, when the dynamic surface tension of a binder composition for a nonaqueous electrolyte secondary battery prepared to have a solid content of 3% was measured, if the value at a lifetime of 5000 msec was 65 mN / m or more and 75 mN / m or less, bubbles were unlikely to be generated when the negative electrode active material layer was applied, and the formation of dents in the negative electrode that are thought to be coating defects could be suppressed. Moreover, the results in Table 3 show that by using the binder compositions for nonaqueous electrolyte secondary batteries of Examples 1 and 2, peeling of the negative electrode active material layer from the negative electrode current collector during the initial charge can be suppressed. Furthermore, as can be seen from the results in Table 4, the battery output at low temperatures could be improved compared to the case where modified SBR, which is a conventional binder composition for non-aqueous electrolyte secondary batteries, was used. It was confirmed that the same results as those in Table 4 could be obtained when various different types of modified SBR of Comparative Example 2 were tried. In summary, it has been found that the use of the binder composition for a nonaqueous electrolyte secondary battery according to the present invention can improve battery output at low temperatures and suppress coating defects in the negative electrode due to peeling of the negative electrode active material from the negative electrode current collector and generation of bubbles during coating.
[0073] In the above-mentioned examples, sodium ethyl methacrylate 2-sulfonate, which functions as a reactive surfactant, was used as the raw material for the water-soluble polymer, but such a reactive surfactant is not necessarily required. For example, the value at the time of the lifetime of the binder composition for non-aqueous electrolyte secondary batteries of 5000 msec can be maintained in the range of 65 mN / m to 75 mN / m by making the content of the water-soluble copolymer in the binder composition for non-aqueous electrolyte secondary batteries 40 mass % or more.
[0074] If the dynamic surface tension of a binder composition for a non-aqueous electrolyte secondary battery is measured and the value at a lifetime of 5000 msec is 65 mN / m or more and 75 mN / m or less, bubbles are less likely to occur when the negative electrode active material layer is coated, and the formation of dents that are thought to be coating defects in the negative electrode can be suppressed. The reason for this is currently under investigation, but one possibility is that it is related to the surface tension during the time from when the negative electrode mixture slurry is coated until it dries and becomes fixed. If the surface tension of the coated surface is high within this time, the bubbles that have occurred cannot be stabilized and will quickly disappear, resulting in a good coating surface. On the other hand, if the interface is stabilized, the bubbles that have occurred will not disappear and will continue to dry, resulting in defects in the dried coating surface.
[0075] As described above, the binder composition for non-aqueous electrolyte secondary batteries according to the present invention is an aqueous dispersion type in which the hydrophobic copolymer is stably dispersed in an aqueous solution by the water-soluble copolymer. Although the specific structure of this binder composition for non-aqueous electrolyte secondary batteries is currently under investigation, one possibility is that the water-soluble copolymer is located on the surface of the hydrophobic copolymer, thereby stably dispersing the hydrophobic copolymer in water. In addition, since the hydrophobic copolymer and the hydrophilic copolymer do not separate even when centrifugal separation is performed, it is believed that at least a portion of the hydrophobic copolymer and the hydrophilic copolymer are bonded to each other through some kind of chemical interaction. [Explanation of symbols]
[0076] 1. Lithium-ion secondary battery 10...Positive electrode 20...Negative electrode 30 Separator
Claims
1. a hydrophobic copolymer containing units derived from one or more monomers selected from the group consisting of an aromatic vinyl monomer, an unsaturated carboxylic acid alkyl ester monomer, a (meth)acrylic acid monomer, and an unsaturated carboxylic acid amide monomer; A water-soluble copolymer that contains a unit derived from a (meth)acrylic acid monomer and a unit derived from a (meth)acrylonitrile monomer and disperses the hydrophobic copolymer in an aqueous solution; 1. A binder composition for a non-aqueous electrolyte secondary battery, comprising: a binder composition having a solid content of 3 mass % and a dynamic surface tension of 65 mN / m or more and 75 mN / m or less at a lifetime of 5 seconds according to a maximum bubble pressure method.
2. 2. The binder composition for a non-aqueous electrolyte secondary battery according to claim 1, wherein the dynamic surface tension is 70 mN / m or more and 73 mN / m or less.
3. 3. The binder composition for a nonaqueous electrolyte secondary battery according to claim 1, wherein the content of the water-soluble copolymer is 15% by mass or more and 45% by mass or less, and the content of the hydrophobic copolymer is 55% by mass or more and 85% by mass or less.
4. 4. The binder composition for a non-aqueous electrolyte secondary battery according to claim 1, wherein the water-soluble copolymer has a content of units derived from a (meth)acrylic acid-based monomer of 35% by mass or more and 65% by mass or less, a content of units derived from a (meth)acrylonitrile monomer of 35% by mass or more and 65% by mass or less, and a content of units derived from other monomers copolymerizable with the units derived from the (meth)acrylic acid-based monomer and / or the units derived from the (meth)acrylonitrile monomer of 0% by mass or more and 20% by mass or less.
5. 5. The binder composition for a non-aqueous electrolyte secondary battery according to claim 4, wherein the other monomer comprises a sulfonic acid group-containing ethylenically unsaturated monomer.
6. 6. The binder composition for a non-aqueous electrolyte secondary battery according to claim 5, wherein the sulfonic acid group-containing ethylenically unsaturated monomer comprises at least one selected from the group consisting of sodium 2-ethyl (meth)acrylate sulfonate, sodium methacryloyloxypolyoxypropylene sulfate, and phenyl ether methacrylate sulfate.
7. 7. The binder composition for a non-aqueous electrolyte secondary battery according to claim 1, wherein an aqueous solution of the water-soluble copolymer having a solid content of 10% by mass has a viscosity of 500 mPa·s or more and 3000 mPa·s or less.
8. A negative electrode for a non-aqueous electrolyte secondary battery, comprising the binder composition for a non-aqueous electrolyte secondary battery according to claim 1 and a negative electrode active material.
9. 9. The negative electrode for a non-aqueous electrolyte secondary battery in accordance with claim 8, further comprising a water-soluble polymer compound.
10. 10. The negative electrode for a non-aqueous electrolyte secondary battery according to claim 9, wherein the water-soluble polymer compound is an alkali metal salt of carboxymethyl cellulose.
11. A non-aqueous electrolyte secondary battery comprising the negative electrode according to claim 8 .
12. A method for producing a water-dispersed binder composition for non-aqueous electrolyte secondary batteries, comprising synthesizing a hydrophobic copolymer containing units derived from one or more monomers selected from the group consisting of aromatic vinyl monomers, unsaturated carboxylic acid alkyl ester monomers, (meth)acrylic acid monomers, and unsaturated carboxylic acid amide monomers in the presence of a water-soluble copolymer containing units derived from a (meth)acrylic acid monomer and a (meth)acrylonitrile monomer.
Citation Information
Patent Citations
Manufacturing method of lithium secondary battery electrode binder, and lithium secondary battery electrode binder
JP2016042408A
Lithium ion secondary battery positive electrode
JP2019133908A
Binder aqueous solution for lithium ion battery, slurry for lithium ion battery electrode and manufacturing method therefor, lithium ion battery electrode, and lithium ion battery
JP2020043064A
Binder composition for nonaqueous battery electrodes, slurry for nonaqueous battery electrodes, nonaqueous battery electrode, and nonaqueous battery
WO2015045522A1
Separator for non-aqueous secondary battery, manufacturing method therefor, and non-aqueous secondary battery
WO2016110894A1