Adhesive sheet

The adhesive sheet with a polyorganosiloxane and (meth)acrylic copolymer structure offers low initial adhesive strength and rapid high-strength increase at mild temperatures, addressing inefficiencies in existing adhesive technologies and expanding application possibilities.

JP7555271B2Active Publication Date: 2024-09-24NITTO DENKO CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020565715
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-01-08
Filing Date
2019-12-26
Publication Date
2024-09-24
Estimated Expiration
2039-12-26

AI Technical Summary

Technical Problem

Existing adhesive sheets require high temperatures or prolonged periods to achieve significant adhesive strength, which can be impractical or damaging to certain materials, and lack efficient methods for rapid strength increase at mild temperatures.

Method used

A pressure-sensitive adhesive sheet comprising a pressure-sensitive adhesive layer with Polymer A and Polymer B, a copolymer of a monomer with a polyorganosiloxane skeleton and a (meth)acrylic monomer, allowing for low initial adhesive strength and rapid increase to high strength upon mild heating around 50°C.

Benefits of technology

The adhesive sheet provides good reworkability at initial attachment and efficiently increases adhesive strength within a short time through mild heating, enhancing productivity and applicability to temperature-sensitive materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555271000008
    Figure 0007555271000008
  • Figure 0007555271000007
    Figure 0007555271000007
  • Figure 0007555271000009
    Figure 0007555271000009
Patent Text Reader

Abstract

The present invention provides a novel pressure-sensitive adhesive sheet that can exhibit good reworkability initially after being attached to an adherend, and can then significantly increase its adhesive strength in a short period of time by mild heating at about 50°C. The pressure-sensitive adhesive sheet includes a pressure-sensitive adhesive layer. The pressure-sensitive adhesive layer includes polymer A and polymer B, which is a copolymer of a monomer having a polyorganosiloxane skeleton and a (meth)acrylic monomer. The pressure-sensitive adhesive sheet has an adhesive strength N of 5 N / 25 mm or more. 50 Here, the adhesive force N 50 refers to the adhesive strength measured at 23°C after laminating to a stainless steel plate and holding at 50°C for 15 minutes.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a pressure-sensitive adhesive sheet. This application claims priority to Japanese Patent Application No. 2019-001349, filed on January 8, 2019, the entire contents of which are incorporated herein by reference. [Background technology]

[0002] Adhesive sheets are used for purposes such as bonding between adherends, fixing an article to an adherend, and reinforcing an adherend by firmly adhering to the adherend. Conventionally, adhesive sheets that exhibit high adhesive strength from the initial stage of application have been used for such purposes. Recently, as in Patent Documents 1 to 3, adhesive sheets that exhibit low adhesive strength at the initial stage of application to an adherend and can then significantly increase their adhesive strength have been proposed. Adhesive sheets with such characteristics exhibit reworkability (reworkability) that is useful for suppressing a decrease in yield due to incorrect or failed application of the adhesive sheet before the increase in adhesive strength, and can exhibit strong adhesiveness suitable for the original purpose of use of the adhesive sheet after the increase in adhesive strength. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 2014-224227 [Patent Document 2] Japanese Patent No. 5890596 [Patent Document 3] Japanese Patent No. 5951153 Summary of the Invention [Problem to be solved by the invention]

[0004] The adhesive sheets described in the above-mentioned prior art documents are configured to exhibit low adhesive strength at the beginning of application, and to increase the adhesive strength to a predetermined value or more by exposure to a high temperature of about 80°C or by taking a period of about 2 days. This allows the increase in adhesive strength to be reliably controlled. Meanwhile, the use of this type of adhesive sheet includes use in the manufacturing process of products, and in such applications, it may be advantageous to increase the adhesive strength by a simpler process from the viewpoint of improving the efficiency (production efficiency) of the manufacturing process. For example, if an adhesive sheet capable of increasing the adhesive strength in a short time by heating closer to room temperature (mild heating) is provided, the adhesive strength increasing process can be efficiently, uniformly and reliably performed, which may be advantageous in terms of improving production efficiency. An adhesive sheet having such characteristics can be applied to an adherend that is not desirable to be exposed to high temperatures, and new applications can be expected. Therefore, the present invention aims to provide a novel adhesive sheet that can exhibit good reworkability at the beginning of application to an adherend, and can then significantly increase the adhesive strength in a short time by mild heating at about 50°C. [Means for solving the problem]

[0005] According to the present specification, there is provided a pressure-sensitive adhesive sheet including a pressure-sensitive adhesive layer. The pressure-sensitive adhesive layer includes a polymer A and a polymer B which is a copolymer of a monomer having a polyorganosiloxane skeleton and a (meth)acrylic monomer. The pressure-sensitive adhesive sheet has an adhesive strength N of 5 N / 25 mm or more. 50 Here, the adhesive strength N 50 refers to the adhesive strength measured at 23°C after laminating to a stainless steel plate and holding at 50°C for 15 minutes.

[0006] The pressure-sensitive adhesive sheet having the above-mentioned structure can exhibit good reworkability at the initial stage of application due to the action of the polymer B having a polyorganosiloxane skeleton. Thereafter, the adhesive strength can be increased to a predetermined value or more by mild heating at about 50°C.

[0007] In some preferred embodiments, the adhesive sheet has an adhesive strength of N 23 The adhesive strength is 3N / 25mm or less. An adhesive sheet that satisfies this characteristic exhibits good reworkability because the adhesive strength is kept low at the beginning of application. In other words, it is possible to preferably achieve both initial light peelability (reworkability) and an increase in adhesive strength after mild heating.

[0008] In some preferred embodiments, the adhesive sheet has an adhesive strength N 50 The adhesive strength (N) is measured after the tape is attached to a stainless steel plate and kept at 23°C for 30 minutes. 23 Thus, the adhesive strength N 23 Adhesive strength N 50 More than 5 times (N 50 / N 23 ≧5), the adhesive sheet exhibits good reworkability at the initial stage of application, and the adhesive strength can be significantly increased by subsequent heating or the like.

[0009] The pressure-sensitive adhesive sheet according to some embodiments has an adhesive strength (N) measured at 23°C after being attached to a stainless steel plate and kept at 80°C for 5 minutes. 80 The adhesive strength N 50 (i.e., N 80 / N 50 ≦2). A pressure-sensitive adhesive sheet that satisfies this characteristic has a sufficient increase in adhesive strength with mild heating at around 50°C, and therefore does not need to be exposed to a higher temperature (specifically, heating at around 80°C) to obtain strong adhesive strength. With a pressure-sensitive adhesive sheet that satisfies this characteristic, adhesive strength can be increased to a desired level more efficiently than before.

[0010] The pressure-sensitive adhesive layer preferably has a storage modulus G'(150°C) at 150°C of 10,000 Pa or more and 90,000 Pa or less. A pressure-sensitive adhesive layer that satisfies the above-mentioned storage modulus at 150°C is likely to exhibit good adhesive properties and polymer B is likely to move within the pressure-sensitive adhesive layer, so that an increase in adhesive strength after mild heating can be preferably achieved based on the mobility.

[0011] In the technology disclosed herein, the polymer A contained in the adhesive layer is typically chemically crosslinked. This allows the adhesive sheet to exhibit good adhesive properties. In addition, in a configuration in which the degree of crosslinking is limited so that the storage modulus G' (150°C) is a predetermined value or less, the adhesive strength after mild heating can be preferably increased based on the mobility of the polymer B in the adhesive layer. In some embodiments, the adhesive layer may contain more than 0 parts by weight and not more than 10 parts by weight of a crosslinking agent relative to 100 parts by weight of the polymer A. By using a crosslinking agent, chemical crosslinking that satisfies the desired properties can be preferably achieved, and a storage modulus G' (150°C) within a predetermined range can be preferably achieved.

[0012] In some embodiments, the weight average molecular weight of the polymer B may be 100,000 or more. Even in embodiments in which a polymer B having a Mw of a certain level or more is used, the effects of the technology disclosed herein can be preferably achieved.

[0013] In some preferred embodiments, the weight average molecular weight of the polymer B may be less than 80,000. By using a polymer B having an Mw less than a predetermined value, an increase in adhesive strength after mild heating can be preferably achieved.

[0014] In some embodiments, the content of the polymer B in the pressure-sensitive adhesive layer can be, for example, in the range of 0.5 parts by weight to 50 parts by weight relative to 100 parts by weight of the polymer A. With a content in the above range, an increase in adhesive strength after mild heating can be preferably realized.

[0015] The polymer A is preferably an acrylic polymer. The adhesive layer containing the polymer A, which is an acrylic polymer, and the polymer B, which is a copolymer of a monomer having a polyorganosiloxane skeleton and a (meth)acrylic monomer, can preferably realize an increase in adhesive strength after mild heating.

[0016] In some embodiments, the acrylic polymer preferably contains a monomer having a nitrogen atom-containing ring as a monomer unit. Polymer A containing a monomer unit having a nitrogen atom-containing ring is preferably used in combination with polymer B to realize an increase in adhesive strength after mild heating.

[0017] In some preferred embodiments, the monomer components for preparing the polymer B include, as the (meth)acrylic monomer (monomer M2), a monomer having a homopolymer glass transition temperature of 50° C. or higher in a ratio of 60% by weight or less. In the polymer B, the copolymerization ratio of the monomer M2 having a Tg of 50° C. or higher is limited to a predetermined value or less, so that an increase in adhesive strength after mild heating can be preferably realized based on the mobility of the polymer B at around 50° C. As the monomer M2, a (meth)acrylic acid alkyl ester (i.e., an alkyl (meth)acrylate) having a homopolymer Tg of 50° C. or higher can be preferably used.

[0018] The adhesive sheet disclosed herein can be implemented in a form that includes a support substrate having a first surface and a second surface, and the adhesive layer is laminated on at least the first surface of the support substrate, that is, in the form of an adhesive sheet with a substrate. Such an adhesive sheet with a substrate can have good handling and processability. For example, a resin film having a thickness of 30 μm or more can be preferably used as the support substrate.

[0019] The present specification also provides a pressure-sensitive adhesive sheet including a pressure-sensitive adhesive layer. The pressure-sensitive adhesive layer includes polymer A and polymer B, which is a copolymer of a monomer having a polyorganosiloxane skeleton and a (meth)acrylic monomer. The pressure-sensitive adhesive layer has a storage modulus G'(150°C) of 10,000 Pa or more and 90,000 Pa or less at 150°C. A pressure-sensitive adhesive sheet including a pressure-sensitive adhesive layer satisfying the above-mentioned storage modulus at 150°C can exhibit good reworkability due to the action of polymer B, and can then increase its adhesive strength by mild heating at about 50°C. [Brief description of the drawings]

[0020] [Figure 1] 1 is a cross-sectional view illustrating a schematic configuration of a pressure-sensitive adhesive sheet according to an embodiment. [Diagram 2] FIG. 4 is a cross-sectional view illustrating a schematic configuration of a pressure-sensitive adhesive sheet according to another embodiment. [Diagram 3] FIG. 4 is a cross-sectional view illustrating a schematic configuration of a pressure-sensitive adhesive sheet according to another embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Preferred embodiments of the present invention will be described below. Matters necessary for carrying out the present invention other than those specifically mentioned in this specification can be understood by those skilled in the art based on the teachings on carrying out the invention described in this specification and the common general technical knowledge at the time of filing. The present invention can be carried out based on the contents disclosed in this specification and the common general technical knowledge in the relevant field. In the following drawings, the same reference numerals may be used to denote components or parts having the same function, and duplicated descriptions may be omitted or simplified. In addition, the embodiments shown in the drawings are schematic in order to clearly explain the present invention, and do not necessarily accurately represent the size or scale of the product actually provided.

[0022] In addition, in this specification, the term "acrylic polymer" refers to a polymer containing a monomer unit derived from a (meth)acrylic monomer in the polymer structure, and typically refers to a polymer containing a monomer unit derived from a (meth)acrylic monomer at a ratio of more than 50% by weight. In addition, the term "(meth)acrylic monomer" refers to a monomer having at least one (meth)acryloyl group in one molecule. Here, the term "(meth)acryloyl group" refers to an acryloyl group and a methacryloyl group in a comprehensive sense. Therefore, the concept of the (meth)acrylic monomer here can include both a monomer having an acryloyl group (acrylic monomer) and a monomer having a methacryloyl group (methacrylic monomer). Similarly, in this specification, "(meth)acrylic acid" refers to acrylic acid and methacrylic acid, and "(meth)acrylate" refers to acrylate and methacrylate in a comprehensive sense.

[0023] <Structural example of adhesive sheet> The pressure-sensitive adhesive sheet disclosed herein is configured to include a pressure-sensitive adhesive layer. The pressure-sensitive adhesive sheet disclosed herein may be in the form of a substrate-attached pressure-sensitive adhesive sheet in which the pressure-sensitive adhesive layer is laminated on one or both sides of a supporting substrate, or may be in the form of a substrate-less pressure-sensitive adhesive sheet that does not have a supporting substrate. Hereinafter, the supporting substrate may be simply referred to as a "substrate".

[0024] The structure of an adhesive sheet according to an embodiment is shown in FIG. 1. The adhesive sheet 1 is configured as a substrate-attached single-sided adhesive sheet including a sheet-like supporting substrate 10 having a first surface 10A and a second surface 10B, and an adhesive layer 21 provided on the first surface 10A side. The adhesive layer 21 is fixed to the first surface 10A side of the supporting substrate 10. The adhesive sheet 1 is used by attaching the adhesive layer 21 to an adherend. The adhesive sheet 1 before use (i.e., before attachment to an adherend) may be a component of a release-liner-attached adhesive sheet 100 in which the surface (adhesive surface) 21A of the adhesive layer 21 is in contact with a release liner 31, at least the side facing the adhesive layer 21 being a release surface (release surface), as shown in FIG. As the release liner 31, for example, one configured to be a release surface by providing a release layer made of a release treatment agent on one side of a sheet-like substrate (liner substrate), may be preferably used. Alternatively, the adhesive sheet 1 may be in a form (roll form) in which release liner 31 is omitted, supporting substrate 10 having second surface 10B as the release surface is used, and adhesive sheet 1 is rolled up so that adhesive surface 21A is in contact with second surface 10B of supporting substrate 10. When adhering adhesive sheet 1 to an adherend, release liner 31 or second surface 10B of supporting substrate 10 is peeled off from adhesive surface 21A, and the exposed adhesive surface 21A is pressure-bonded to the adherend.

[0025] The structure of an adhesive sheet according to another embodiment is shown in FIG. 2. The adhesive sheet 2 is configured as a substrate-attached double-sided adhesive sheet including a sheet-like supporting substrate 10 having a first surface 10A and a second surface 10B, an adhesive layer 21 provided on the first surface 10A side, and an adhesive layer 22 provided on the second surface 10B side. The adhesive layer (first adhesive layer) 21 is fixed to the first surface 10A of the supporting substrate 10, and the adhesive layer (second adhesive layer) 22 is fixed to the second surface 10B of the supporting substrate 10. The adhesive sheet 2 is used by attaching the adhesive layers 21 and 22 to different locations on an adherend. The locations to which the adhesive layers 21 and 22 are attached may be locations on different members, or may be different locations within a single member. As shown in Fig. 2, the adhesive sheet 2 before use may be a component of an adhesive sheet with a release liner 200 in which the surface (first adhesive surface) 21A of the adhesive layer 21 and the surface (second adhesive surface) 22A of the adhesive layer 22 are in contact with release liners 31, 32, each of which has a release surface on at least the side facing the adhesive layers 21, 22. As the release liners 31, 32, for example, a sheet-like substrate (liner substrate) may be preferably used, in which a release layer made of a release treatment agent is provided on one side of the substrate, so that the one side serves as the release surface. Alternatively, the release liner 32 may be omitted, and a release liner 31, both of which have release surfaces, may be used, which is superimposed on the adhesive sheet 2 and wound in a spiral shape to form an adhesive sheet with a release liner in which the second adhesive surface 22A is in contact with the back surface of the release liner 31 (roll form).

[0026] The structure of a pressure-sensitive adhesive sheet according to yet another embodiment is shown in FIG. 3. The pressure-sensitive adhesive sheet 3 is configured as a substrate-less double-sided pressure-sensitive adhesive sheet made of a pressure-sensitive adhesive layer 21. The pressure-sensitive adhesive sheet 3 is used by attaching a first adhesive surface 21A, which is configured by one surface (first surface) of the pressure-sensitive adhesive layer 21, and a second adhesive surface 21B, which is configured by the other surface (second surface) of the pressure-sensitive adhesive layer 21, to different locations on an adherend. As shown in FIG. 3, the pressure-sensitive adhesive sheet 3 before use may be a component of a pressure-sensitive adhesive sheet with a release liner 300 in a form in which the first adhesive surface 21A and the second adhesive surface 21B are in contact with release liners 31 and 32, each of which has a release surface at least on the side facing the pressure-sensitive adhesive layer 21. Alternatively, the release liner 32 may be omitted, and a release liner 31, both of which have release surfaces, may be used, and the release liner and the pressure-sensitive adhesive sheet 3 may be superimposed and rolled in a spiral shape to form a pressure-sensitive adhesive sheet with a release liner in a form in which the second adhesive surface 21B is in contact with the back surface of the release liner 31 (roll form).

[0027] The concept of adhesive sheet here may include those called adhesive tape, adhesive film, adhesive label, etc. The adhesive sheet may be in a roll form or in a sheet form, and may be cut, punched, or the like into an appropriate shape depending on the application or mode of use. The adhesive layer in the technology disclosed herein is typically formed continuously, but is not limited thereto, and may be formed in a regular or random pattern such as a dotted or striped pattern.

[0028] <Adhesive layer> The pressure-sensitive adhesive sheet disclosed herein includes a pressure-sensitive adhesive layer containing polymer A and polymer B, which is a copolymer of a monomer having a polyorganosiloxane skeleton and a (meth)acrylic monomer. Such a pressure-sensitive adhesive layer may be formed from a pressure-sensitive adhesive composition containing polymer A, which is a complete or partial polymer of monomer raw material A, and polymer B. The form of the pressure-sensitive adhesive composition is not particularly limited, and may be in various forms, such as a solvent type, a water-dispersed type, a hot melt type, or an active energy ray curable type (e.g., a photocurable type).

[0029] (Polymer A) As the polymer A, one or more of various polymers that exhibit rubber elasticity at room temperature, such as acrylic polymers, rubber polymers, polyester polymers, urethane polymers, polyether polymers, silicone polymers, polyamide polymers, and fluorine polymers, known in the field of pressure-sensitive adhesives, can be used. In the pressure-sensitive adhesive sheet disclosed herein, the polymer A is typically the main component of the polymer components contained in the pressure-sensitive adhesive layer, i.e., a component that accounts for more than 50% by weight, and may be a component that accounts for, for example, 75% by weight or more of the above polymer components. In some embodiments, the polymer A may be a component that accounts for more than 50% by weight of the entire pressure-sensitive adhesive layer, and may be a component that accounts for 70% by weight or more.

[0030] Glass transition temperature T of polymer A A is not particularly limited and can be selected so as to obtain preferred properties in the pressure-sensitive adhesive sheet disclosed herein. A A polymer A having a T of less than 0° C. can be preferably used. Since a pressure-sensitive adhesive containing such a polymer A exhibits appropriate fluidity (e.g., mobility of the polymer chain contained in the pressure-sensitive adhesive), it is suitable for realizing a pressure-sensitive adhesive sheet whose adhesive strength increases to a predetermined value or more upon mild heating. The pressure-sensitive adhesive sheet disclosed herein has a T A may be preferably carried out with polymer A at less than -10°C, less than -20°C, less than -30°C or less than -35°C. A may be less than -40°C or less than -50°C. A There is no particular restriction on the lower limit of T. From the viewpoint of material availability and improving the cohesive strength of the adhesive layer, T A Preferably, the polymer A has a temperature of −80° C. or higher, −70° C. or higher, or −65° C. or higher. A may be, for example, -63°C or higher, -55°C or higher, -50°C or higher, or -45°C or higher.

[0031] In this specification, the glass transition temperature (Tg) of a polymer refers to a nominal value described in literature, catalogs, etc., or a Tg calculated by the Fox formula based on the composition of the monomer raw materials used in the preparation of the polymer. The Fox formula is a relational expression between the Tg of a copolymer and the glass transition temperature Tgi of a homopolymer obtained by homopolymerizing each of the monomers constituting the copolymer, as shown below. 1 / Tg=Σ(Wi / Tgi) In the above Fox formula, Tg represents the glass transition temperature (unit: K) of the copolymer, Wi represents the weight fraction (copolymerization ratio by weight) of monomer i in the copolymer, and Tgi represents the glass transition temperature (unit: K) of a homopolymer of monomer i. When the target polymer for which Tg is specified is a homopolymer, the Tg of the homopolymer and the Tg of the target polymer are the same.

[0032] The glass transition temperature of the homopolymer used to calculate Tg is a value listed in a publicly known document. Specifically, the values ​​are listed in "Polymer Handbook" (3rd Edition, John Wiley & Sons, Inc., 1989). For monomers for which multiple values ​​are listed in the Polymer Handbook, the highest value is used.

[0033] As the glass transition temperature of a homopolymer of a monomer not described in the Polymer Handbook, a value obtained by the following measurement method is used. Specifically, 100 parts by weight of monomer, 0.2 parts by weight of 2,2'-azobisisobutyronitrile, and 200 parts by weight of ethyl acetate as a polymerization solvent are charged into a reactor equipped with a thermometer, a stirrer, a nitrogen inlet tube, and a reflux condenser tube, and stirred for 1 hour while passing nitrogen gas through it. After removing oxygen from the polymerization system in this way, the temperature is raised to 63°C and the reaction is carried out for 10 hours. Then, the mixture is cooled to room temperature to obtain a homopolymer solution with a solid content concentration of 33% by weight. Then, the homopolymer solution is cast and applied onto a release liner, and dried to prepare a test sample (sheet-shaped homopolymer) with a thickness of about 2 mm. This test sample was punched out into a disk with a diameter of 7.9 mm, sandwiched between parallel plates, and the viscoelasticity was measured in shear mode using a viscoelasticity tester (TA Instruments Japan, model name "ARES") while applying a shear strain of 1 Hz at a temperature range of -70°C to 150°C and a heating rate of 5°C / min. The temperature corresponding to the peak top temperature of tan δ was taken as the Tg of the homopolymer.

[0034] Although not particularly limited, the weight average molecular weight (Mw) of the polymer A is usually about 20×10 4 It is appropriate that the Mw of polymer A is 30×10 or more. With polymer A having such Mw, a PSA exhibiting good cohesive properties is likely to be obtained. From the viewpoint of obtaining higher cohesive strength, in some embodiments, the Mw of polymer A is, for example, 30×10 4 It may be 40×10 or more. 4 More than 50 x 10 is fine. 4 More than 60 x 10 is fine. 4 More than 80 x 10 is fine. 4 The Mw of polymer A is usually about 500×10 4 It is appropriate that the Mw of polymer A is not too high. Polymer A with such an Mw is likely to form an adhesive that exhibits moderate fluidity (mobility of polymer chains), and is therefore suitable for realizing an adhesive sheet that has low adhesive strength at the initial stage of application and high adhesive strength after mild heating. It is also preferable from the viewpoint of improving compatibility with polymer B that the Mw of polymer A is not too high. In some embodiments, the Mw of polymer A is, for example, 250×10 4 may be less than or equal to 200 x 10 4Less than 150×10 is fine. 4 The following is also fine.

[0035] In this specification, the Mw of polymer A and polymer B described later can be determined in terms of polystyrene by gel permeation chromatography (GPC). More specifically, the Mw can be measured according to the method and conditions described in the examples described later.

[0036] An acrylic polymer can be preferably used as polymer A in the pressure-sensitive adhesive sheet disclosed herein. When an acrylic polymer is used as polymer A, good compatibility with polymer B tends to be easily obtained. Good compatibility between polymer A and polymer B is preferable because it can contribute to reducing the initial adhesive strength and improving the adhesive strength after heating through improving the mobility of polymer B in the pressure-sensitive adhesive layer.

[0037] The acrylic polymer may be, for example, a polymer containing 50% by weight or more of monomer units derived from (meth)acrylic acid alkyl esters, that is, a polymer in which 50% by weight or more of the total amount of the monomer component (monomer raw material A) for preparing the acrylic polymer is a (meth)acrylic acid alkyl ester. The (meth)acrylic acid alkyl ester may be a monomer unit having 1 to 20 carbon atoms (i.e., C 1-20 Of the monomer raw materials A, (meth)acrylic acid alkyl esters having linear or branched alkyl groups are preferably used. 1-20 The proportion of alkyl ester may be, for example, 50% by weight or more, 60% by weight or more, or 70% by weight or more. For the same reason, the proportion of (meth)acrylic acid C in the monomer raw material A is preferably 10% by weight or more. 1-20 The proportion of alkyl ester may be, for example, 99.9% by weight or less, 98% by weight or less, or 95% by weight or less. 1-20The proportion of alkyl esters may be, for example, 90% by weight or less, 85% by weight or less, or 80% by weight or less.

[0038] (Meth)acrylic acid C 1-20 Non-limiting examples of alkyl esters include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl ... and isopropyl (meth)acrylate. Examples of such acrylates include isooctyl, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, nonadecyl (meth)acrylate, and eicosyl (meth)acrylate.

[0039] Among these, at least (meth)acrylic acid C 1-18 It is preferable to use an alkyl ester, and at least (meth)acrylic acid C 1-14 It is more preferred to use alkyl esters. In some embodiments, the acrylic polymer is (meth)acrylic acid C 4-12 Alkyl ester (preferably acrylic acid C 4-10 Alkyl esters, such as acrylic acid C 6-10The (meth)acrylic acid C may contain at least one selected from the group consisting of n-butyl acrylate (BA) and 2-ethylhexyl acrylate (2EHA) as a monomer unit. For example, an acrylic polymer containing one or both of n-butyl acrylate (BA) and 2-ethylhexyl acrylate (2EHA) is preferred, and an acrylic polymer containing at least 2EHA is particularly preferred. 1-18 Examples of alkyl esters include methyl acrylate, methyl methacrylate (MMA), n-butyl methacrylate (BMA), 2-ethylhexyl methacrylate (2EHMA), isostearyl acrylate (ISTA), and the like.

[0040] The monomer raw material A may contain, as the main component, an alkyl (meth)acrylate ester and, if necessary, another monomer (copolymerizable monomer) that can be copolymerized with the alkyl (meth)acrylate ester. As the copolymerizable monomer, a monomer having a polar group (e.g., a carboxyl group, a hydroxyl group, a nitrogen atom-containing ring, etc.) can be suitably used. The monomer having a polar group can be useful for introducing a crosslinking point into the acrylic polymer or for increasing the cohesive force of the acrylic polymer. The copolymerizable monomer can be used alone or in combination of two or more kinds.

[0041] Non-limiting examples of copolymerizable monomers include the following: Hydroxyl group-containing monomers: for example, hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)methyl (meth)acrylate. Monomers having a nitrogen atom-containing ring: for example, N-vinyl-2-pyrrolidone, N-methylvinylpyrrolidone, N-vinylpyridine, N-vinylpiperidone, N-vinylpyrimidine, N-vinylpiperazine, N-vinylpyrazine, N-vinylpyrrole, N-vinylimidazole, N-vinyloxazole, N-(meth)acryloyl-2-pyrrolidone, N-(meth)acryloylpiperidine, N-(meth)acryloylpyrrolidine, N-vinylmorpholine, N-vinyl-3-morpholinone, N-vinyl-2-caprolactam, N-vinyl-1,3-oxazin-2-one, N-vinyl-3,5-morpholinedione, N-vinylpyrazole, N-vinylisoxazole, N-vinylthiazole, N-vinylisothiazole, N-vinylpyridazine, etc.; For example, monomers having a succinimide skeleton, such as N-(meth)acryloyloxymethylene succinimide, N-(meth)acryloyl-6-oxyhexamethylene succinimide, and N-(meth)acryloyl-8-oxyhexamethylene succinimide; Maleimides, such as, for example, N-cyclohexylmaleimide, N-isopropylmaleimide, N-laurylmaleimide, N-phenylmaleimide, and the like; and For example, itaconimides such as N-methylitaconimide, N-ethylitaconimide, N-butylitaconimide, N-octylitaconimide, N-2-ethylhexylitaconimide, N-cyclohexylitaconimide, and N-laurylitaconimide. Carboxy group-containing monomers: for example, acrylic acid, methacrylic acid, carboxyethyl acrylate, carboxypentyl acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, isocrotonic acid, and the like. Acid anhydride group-containing monomers: for example, maleic anhydride, itaconic anhydride. Epoxy group-containing monomers: for example, epoxy group-containing acrylates such as glycidyl (meth)acrylate and 2-ethyl glycidyl ether (meth)acrylate, allyl glycidyl ether, and glycidyl ether (meth)acrylate. Cyano group-containing monomers: for example, acrylonitrile, methacrylonitrile, etc. Isocyanate group-containing monomers: for example, 2-isocyanatoethyl (meth)acrylate. Amide group-containing monomers: for example, (meth)acrylamide; N,N-dialkyl(meth)acrylamides such as N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N,N-dipropyl(meth)acrylamide, N,N-diisopropyl(meth)acrylamide, N,N-di(n-butyl)(meth)acrylamide, and N,N-di(t-butyl)(meth)acrylamide; N-alkyl(meth)acrylamides such as N-ethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, N-butyl(meth)acrylamide, and Nn-butyl(meth)acrylamide; N-vinyl carboxylic acid amides such as N-vinylacetamide; monomers having a hydroxyl group and an amide group, for example, N-(2-hydroxyethyl)(meth)acrylamide; N-hydroxyalkyl (meth)acrylamides such as N-(2-hydroxypropyl) (meth)acrylamide, N-(1-hydroxypropyl) (meth)acrylamide, N-(3-hydroxypropyl) (meth)acrylamide, N-(2-hydroxybutyl) (meth)acrylamide, N-(3-hydroxybutyl) (meth)acrylamide, and N-(4-hydroxybutyl) (meth)acrylamide; monomers having an alkoxy group and an amide group, for example, N-alkoxyalkyl (meth)acrylamide such as N-methoxymethyl (meth)acrylamide, N-methoxyethyl (meth)acrylamide, and N-butoxymethyl (meth)acrylamide; and others, such as N,N-dimethylaminopropyl (meth)acrylamide and N-(meth)acryloylmorpholine. Aminoalkyl (meth)acrylates: for example, aminoethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, N,N-diethylaminoethyl (meth)acrylate, and t-butylaminoethyl (meth)acrylate. Alkoxy group-containing monomers: for example, alkoxyalkyl (meth)acrylates such as 2-methoxyethyl (meth)acrylate, 3-methoxypropyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, propoxyethyl (meth)acrylate, butoxyethyl (meth)acrylate, and ethoxypropyl (meth)acrylate; alkoxyalkylene (meth)acrylates such as methoxyethylene glycol (meth)acrylate and methoxypolypropylene glycol (meth)acrylate. Monomers containing a sulfonic acid group or a phosphoric acid group: for example, styrene sulfonic acid, allyl sulfonic acid, sodium vinyl sulfonate, 2-(meth)acrylamido-2-methylpropanesulfonic acid, (meth)acrylamidopropanesulfonic acid, sulfopropyl (meth)acrylate, (meth)acryloyloxynaphthalenesulfonic acid, 2-hydroxyethyl acryloyl phosphate, etc. (Meth)acrylic acid esters having an alicyclic hydrocarbon group: for example, cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, and the like. (Meth)acrylic acid esters having an aromatic hydrocarbon group: for example, phenyl (meth)acrylate, phenoxyethyl (meth)acrylate, benzyl (meth)acrylate, and the like. Vinyl ethers: for example, vinyl alkyl ethers such as methyl vinyl ether and ethyl vinyl ether. Vinyl esters: for example, vinyl acetate, vinyl propionate, etc. Aromatic vinyl compounds: for example, styrene, α-methylstyrene, vinyltoluene, etc. Olefins: For example, ethylene, butadiene, isoprene, isobutylene, etc. Other examples include heterocyclic ring-containing (meth)acrylates such as tetrahydrofurfuryl (meth)acrylate, halogen atom-containing (meth)acrylates such as vinyl chloride and fluorine atom-containing (meth)acrylates, silicon atom-containing (meth)acrylates such as silicone (meth)acrylate, and (meth)acrylic acid esters obtained from alcohols derived from terpene compounds.

[0042] When such a copolymerizable monomer is used, the amount of the copolymerizable monomer is not particularly limited, but is usually appropriate to be 0.01% by weight or more of the monomer raw material A. From the viewpoint of better exerting the effect of using the copolymerizable monomer, the amount of the copolymerizable monomer may be 0.1% by weight or more of the monomer raw material A, or may be 1% by weight or more. In addition, the amount of the copolymerizable monomer may be 50% by weight or less of the monomer raw material A, and is preferably 45% by weight or less. This can prevent the cohesive force of the adhesive from becoming too high, and can improve the tackiness at room temperature (25°C). In some embodiments, the amount of the copolymerizable monomer may be 40% by weight or less of the monomer raw material A, or may be 35% by weight or less.

[0043] In some embodiments, the monomer raw material A may contain a monomer having a nitrogen atom-containing ring. By using a monomer having a nitrogen atom-containing ring, the cohesive strength and polarity of the adhesive can be adjusted, and the adhesive strength after mild heating can be suitably improved. By including a monomer having a nitrogen atom-containing ring in the monomer raw material A, the compatibility between the polymer A formed from the monomer raw material A and the polymer B tends to be improved. This makes it easier to obtain an adhesive sheet that can greatly increase the adhesive strength by mild heating.

[0044] The monomer having a nitrogen atom-containing ring may be appropriately selected from the above examples, and may be used alone or in combination of two or more. In some embodiments, the monomer raw material A preferably contains at least one monomer selected from the group consisting of N-vinyl cyclic amides represented by the following general formula (M1) as the monomer having a nitrogen atom-containing ring. The monomer raw material A may contain only one or two or more of such N-vinyl cyclic amides as the monomer having a nitrogen atom-containing ring.

[0045] [ka] Here, R in the above general formula (M1)1 is a divalent organic group.

[0046] Specific examples of N-vinyl cyclic amides include N-vinyl-2-pyrrolidone, N-vinyl-2-piperidone, N-vinyl-3-morpholinone, N-vinyl-2-caprolactam, N-vinyl-1,3-oxazin-2-one, N-vinyl-3,5-morpholinedione, etc. Particularly preferred are N-vinyl-2-pyrrolidone and N-vinyl-2-caprolactam.

[0047] The amount of the monomer having a nitrogen atom-containing ring used is not particularly limited, and is usually appropriate to be 0.01% by weight or more (preferably 0.1% by weight or more, for example 0.5% by weight or more) of the monomer raw material A. In some embodiments, the amount of the monomer having a nitrogen atom-containing ring used may be 1% by weight or more, 5% by weight or more, 10% by weight or more, or 12% by weight or more of the monomer raw material A. In addition, from the viewpoint of improving the tackiness at room temperature (25° C.) and improving the flexibility at low temperatures, the amount of the monomer having a nitrogen atom-containing ring used is usually appropriate to be 40% by weight or less of the monomer raw material A, and may be 30% by weight or less, 20% by weight or less, or 18% by weight or less.

[0048] In some preferred embodiments, the monomer raw material A includes a hydroxyl group-containing monomer. The use of the hydroxyl group-containing monomer can adjust the cohesive strength and polarity of the adhesive, and can favorably improve the adhesive strength after mild heating. In addition, the hydroxyl group-containing monomer can provide a reaction site with a crosslinking agent (e.g., an isocyanate-based crosslinking agent) described later, and can increase the cohesive strength of the adhesive through a crosslinking reaction.

[0049] Suitable examples of hydroxyl group-containing monomers include 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, N-(2-hydroxyethyl)(meth)acrylamide, etc. Among these, preferred examples include 2-hydroxyethyl acrylate (HEA), 4-hydroxybutyl acrylate (4HBA), and N-(2-hydroxyethyl)acrylamide (HEAA).

[0050] The amount of the hydroxyl group-containing monomer used is not particularly limited, and is usually appropriate to be 0.01% by weight or more (preferably 0.1% by weight or more, for example 0.5% by weight or more) of the monomer raw material A. In some embodiments, the amount of the hydroxyl group-containing monomer used may be 1% by weight or more, 5% by weight or more, or 10% by weight or more of the monomer raw material A. In addition, from the viewpoint of the mobility of the polymer B in the adhesive layer, improvement of the tackiness at room temperature (25°C), and improvement of the flexibility at low temperatures, the amount of the hydroxyl group-containing monomer used is usually appropriate to be 40% by weight or less of the monomer raw material A, and may be 30% by weight or less, 20% by weight or less, 10% by weight or less, or 5% by weight or less.

[0051] In some embodiments, a monomer having a nitrogen atom-containing ring (e.g., N-vinyl cyclic amide) and a hydroxyl group-containing monomer can be used in combination as a copolymerizable monomer. In this case, the total amount of the monomer having a nitrogen atom-containing ring and the hydroxyl group-containing monomer can be, for example, 0.1% by weight or more of the monomer raw material A, 1% by weight or more, 5% by weight or more, 10% by weight or more, 15% by weight or more, 20% by weight or more, or 25% by weight or more. In addition, the total amount of the monomer having a nitrogen atom-containing ring and the hydroxyl group-containing monomer can be, for example, 50% by weight or less of the monomer raw material A, and preferably 40% by weight or less.

[0052] In an embodiment in which the monomer raw material A contains a combination of a monomer having a nitrogen atom-containing ring and a hydroxyl group-containing monomer, the content of the monomer having a nitrogen atom-containing ring in the monomer raw material A (W N ) and the content of hydroxyl group-containing monomers (W OH The relationship (weight basis) between W and W is not particularly limited. N / W OH For example, W may be 0.01 or more, and is usually 0.05 or more. It may be 0.1 or more, 0.2 or more, 0.5 or more, or 0.7 or more. N / W OH may be, for example, 100 or less, and is usually suitably 20 or less, may be 10 or less, may be 5 or less, may be 2 or less, or may be 1.5 or less.

[0053] In some embodiments, it is preferable that the monomer raw material A does not contain a monomer (monomer S1) having a polyorganosiloxane skeleton, which is preferably used as a constituent of the monomer raw material B described later, or the content of the monomer is less than 10% by weight (more preferably less than 5% by weight, for example less than 2% by weight) of the monomer raw material A. With a monomer raw material A having such a composition, a pressure-sensitive adhesive sheet that preferably achieves both initial reworkability and strong adhesion after the adhesive strength increases can be preferably realized. For the same reason, in some other embodiments, it is preferable that the monomer raw material A does not contain monomer S1, or if it contains monomer S1, its content (weight basis) is lower than the content of monomer S1 in the monomer raw material B.

[0054] The method for obtaining the polymer A is not particularly limited, and various polymerization methods such as solution polymerization, emulsion polymerization, bulk polymerization, suspension polymerization, and photopolymerization can be appropriately adopted. In some embodiments, the solution polymerization method can be preferably adopted. The polymerization temperature when carrying out the solution polymerization can be appropriately selected depending on the type of monomer and solvent used, the type of polymerization initiator, and the like, and can be, for example, about 20°C to 170°C (typically about 40°C to 140°C).

[0055] The initiator used for the polymerization can be appropriately selected from conventionally known thermal polymerization initiators, photopolymerization initiators, etc., depending on the polymerization method. The polymerization initiator can be used alone or in combination of two or more kinds.

[0056] Examples of the thermal polymerization initiator include azo-based polymerization initiators (e.g., 2,2'-azobisisobutyronitrile, 2,2'-azobis-2-methylbutyronitrile, 2,2'-azobis(2-methylpropionic acid) dimethyl, 4,4'-azobis-4-cyanovaleric acid, azobisisovaleronitrile, 2,2'-azobis(2-amidinopropane) dihydrochloride, 2,2'-azobis[2-(5-methyl-2 -imidazolin-2-yl)propane]dihydrochloride, 2,2'-azobis(2-methylpropionamidine)disulfate, 2,2'-azobis(N,N'-dimethyleneisobutylamidine)dihydrochloride, etc.); persulfates such as potassium persulfate; peroxide-based polymerization initiators (e.g., dibenzoyl peroxide, t-butyl permaleate, lauroyl peroxide, etc.); redox-based polymerization initiators, etc. The amount of the thermal polymerization initiator used is not particularly limited, but can be, for example, within the range of 0.01 to 5 parts by weight, preferably 0.05 to 3 parts by weight, relative to 100 parts by weight of the monomer component (monomer raw material A) used in the preparation of the acrylic polymer.

[0057] The photopolymerization initiator is not particularly limited, but for example, a benzoin ether-based photopolymerization initiator, an acetophenone-based photopolymerization initiator, an α-ketol-based photopolymerization initiator, an aromatic sulfonyl chloride-based photopolymerization initiator, a photoactive oxime-based photopolymerization initiator, a benzoin-based photopolymerization initiator, a benzyl-based photopolymerization initiator, a benzophenone-based photopolymerization initiator, a ketal-based photopolymerization initiator, a thioxanthone-based photopolymerization initiator, an acylphosphine oxide-based photopolymerization initiator, etc. can be used. The amount of the photopolymerization initiator used is not particularly limited, but for example, it can be in the range of 0.01 to 5 parts by weight, preferably 0.05 to 3 parts by weight, relative to 100 parts by weight of the monomer raw material A.

[0058] In some embodiments, the polymer A may be included in the adhesive composition for forming the adhesive layer in the form of a partial polymer (polymer syrup) obtained by irradiating a mixture of the monomer raw material A and a polymerization initiator as described above with ultraviolet (UV) light to polymerize a part of the monomer component. The adhesive composition containing such a polymer syrup may be applied to a predetermined substrate and irradiated with ultraviolet light to complete the polymerization. That is, the polymer syrup may be regarded as a precursor of the polymer A. The adhesive layer disclosed herein may be formed, for example, using an adhesive composition containing the polymer syrup and the polymer B.

[0059] (Polymer B) The polymer B in the technology disclosed herein is a copolymer of a monomer having a polyorganosiloxane skeleton (hereinafter also referred to as "monomer S1") and a (meth)acrylic monomer. The polymer B suppresses the adhesive strength at the initial stage of attachment to an adherend due to the low polarity and mobility of the polyorganosiloxane structure derived from the monomer S1, and can function as an adhesive strength increase retarder that increases the adhesive strength to the adherend by heating. The monomer S1 is not particularly limited, and any monomer containing a polyorganosiloxane skeleton can be used. The monomer S1 promotes uneven distribution of the polymer B on the surface of the adhesive layer in the adhesive sheet before use (before attachment to an adherend) due to the low polarity derived from its structure, and exhibits light peelability (low adhesiveness) at the initial stage of attachment. The monomer S1 can preferably be one having a structure having a polymerizable reactive group at one end. By copolymerizing such a monomer S1 with a (meth)acrylic monomer, a polymer B having a polyorganosiloxane skeleton in the side chain is formed. Polymer B having such a structure tends to have low initial adhesion and high adhesion after mild heating due to the mobility and ease of movement of the side chain. In some embodiments, the monomer S1 may preferably have a polymerizable reactive group at one end and no functional group at the other end that causes a crosslinking reaction with polymer A. Polymer B in which monomer S1 having such a structure is copolymerized tends to have low initial adhesion and high adhesion after heating due to the mobility of the polyorganosiloxane structure derived from monomer S1.

[0060] As the monomer S1, for example, a compound represented by the following general formula (1) or (2) can be used. More specifically, examples of the silicone oil having a reactive end, manufactured by Shin-Etsu Chemical Co., Ltd., include X-22-174ASX, X-22-2426, X-22-2475, and KF-2012. The monomer S1 can be used alone or in combination of two or more. [ka] [ka] Here, R in the above general formulas (1) and (2) 3 is hydrogen or methyl, and R 4 is a methyl group or a monovalent organic group, and m and n are integers of 0 or greater.

[0061] The functional group equivalent of the monomer S1 can be an appropriate value within a range in which the desired effect is achieved by using the monomer S1, and is not limited to a specific range. From the viewpoint of sufficiently suppressing the initial adhesive strength, the functional group equivalent is, for example, 100 g / mol or more, 200 g / mol or more, or 300 g / mol or more (for example, 500 g / mol or more), preferably 700 g / mol or more, more preferably 800 g / mol or more, even more preferably 850 g / mol or more, and particularly preferably 1500 g / mol or more. In some embodiments, from the viewpoint of achieving both low adhesive strength at the initial stage of application and increased adhesive strength after mild heating, the functional group equivalent may be 3000 g / mol or more, 4500 g / mol or more, 6000 g / mol or more, 9000 g / mol or more, 12000 g / mol or more, or 15000 g / mol or more (for example, 16000 g / mol or more). The functional group equivalent of the monomer S1 may be, for example, 50000 g / mol or less. From the viewpoint of sufficiently increasing the adhesive strength, the functional group equivalent is, for example, preferably 30000 g / mol or less, more preferably 20000 g / mol or less. In some embodiments, the functional group equivalent of the monomer S1 may be less than 18000 g / mol, less than 15000 g / mol, less than 10000 g / mol, less than 6000 g / mol, or less than 5000 g / mol. When the functional group equivalent of the monomer S1 is within the above range, it is easy to adjust the compatibility (for example, compatibility with the base polymer) and mobility in the adhesive layer to an appropriate range, and it is easy to realize an adhesive layer that achieves both initial low adhesion and increased adhesive strength after mild heating.

[0062] Non-limiting examples of suitable ranges of functional group equivalent weight of monomer S1 include 700 g / mol to 50,000 g / mol, 700 g / mol to 30,000 g / mol, 700 g / mol to 20,000 g / mol, 700 g / mol to less than 18,000 g / mol, 700 g / mol to less than 15,000 g / mol, 800 g / mol to less than 10,000 g / mol, 850 g / mol to less than 6,000 g / mol, and 1,500 g / mol to less than 5,000 g / mol. In some embodiments, suitable ranges for the functional group equivalent weight of monomer S1 may be from 3000 g / mol to 50000 g / mol, from 6000 g / mol to 50000 g / mol, from 12000 g / mol to 50000 g / mol, or from 15000 g / mol to 50000 g / mol.

[0063] Here, the term "functional group equivalent" refers to the weight of the main skeleton (e.g., polydimethylsiloxane) bound to one functional group. The unit g / mol is calculated based on 1 mol of functional group. The functional group equivalent of the monomer S1 can be calculated, for example, based on nuclear magnetic resonance (NMR). 1 It can be calculated from the H-NMR (proton NMR) spectrum intensity. 1 The functional group equivalent weight (g / mol) of monomer S1 was calculated based on the H-NMR spectrum intensity as follows: 1 This can be done based on a general structural analysis technique involving H-NMR spectrum analysis, and if necessary, by referring to the description in Japanese Patent No. 5951153.

[0064] In addition, when two or more kinds of monomers having different functional group equivalents are used as the monomer S1, the functional group equivalent of the monomer S1 can be an arithmetic average value. That is, when n kinds of monomers having different functional group equivalents (monomer S11, monomer S12, ..., monomer S1 n The functional group equivalent of the monomer S1 consisting of (a) can be calculated by the following formula. Functional group equivalent of monomer S1 (g / mol) = (functional group equivalent of monomer S11 × amount of monomer S11 + functional group equivalent of monomer S12 × amount of monomer S12 + + monomer S1n Functional group equivalent weight × monomer S1 n (amount of monomer S11 + amount of monomer S12 + + monomer S1 n (amount of mixture)

[0065] The content of the monomer S1 can be an appropriate value within a range in which the desired effect is exhibited using the monomer S1, and is not limited to a specific range. In some embodiments, the content of the monomer S1 may be, for example, 5% by weight or more of the total amount of the monomer components (monomer raw material B) for preparing the polymer B, and is preferably 10% by weight or more from the viewpoint of better exhibiting the effect as an adhesive strength increase retarder, and may be 15% by weight or more, or may be 20% by weight or more. In addition, the content of the monomer S1 in the monomer raw material B may be, for example, 80% by weight or less, and is suitably 60% by weight or less, and may be 50% by weight or less, 40% by weight or less, or may be 30% by weight or less from the viewpoint of polymerization reactivity and compatibility. If the content of the monomer S1 is less than 5% by weight, the initial adhesive strength may not be sufficiently suppressed. If the content of the monomer S1 is more than 60% by weight, the increase in adhesive strength may be insufficient.

[0066] The monomer raw material B contains, in addition to the monomer S1, a (meth)acrylic monomer copolymerizable with the monomer S1. By copolymerizing one or more (meth)acrylic monomers with the monomer S1, the mobility of the polymer B in the adhesive layer can be suitably adjusted. Copolymerizing the monomer S1 with the (meth)acrylic monomer can also be useful for improving the compatibility between the polymer B and the polymer A (e.g., an acrylic polymer).

[0067] Examples of (meth)acrylic monomers that can be used for the monomer raw material B include (meth)acrylic acid alkyl esters. For example, one or more of the monomers exemplified above as (meth)acrylic acid alkyl esters that can be used when the polymer A is an acrylic polymer can be used as a constituent of the monomer raw material B. In some embodiments, the monomer raw material B is (meth)acrylic acid C 4-12 Alkyl ester (preferably (meth)acrylic acid C 4-10 Alkyl esters, such as (meth)acrylic acid C 6-10 In some other embodiments, the monomer feedstock B may contain at least one of methacrylic acid C 1-18 Alkyl ester (preferably methacrylic acid C 1-14 Alkyl esters, such as methacrylic acid C 1-10 The monomer raw material B may contain, as a (meth)acrylic monomer, one or more selected from the group consisting of MMA, BMA, and 2EHMA.

[0068] Other examples of the (meth)acrylic monomer include (meth)acrylic acid esters having an alicyclic hydrocarbon group. For example, cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, 1-adamantyl (meth)acrylate, etc. can be used. In some embodiments, the monomer raw material B can contain at least one selected from dicyclopentanyl methacrylate, isobornyl methacrylate, and cyclohexyl methacrylate as the (meth)acrylic monomer.

[0069] The content of the (meth)acrylic acid alkyl ester and the (meth)acrylic acid ester having an alicyclic hydrocarbon group in the monomer raw material B may be, for example, 10% by weight or more and 95% by weight or less, 20% by weight or more and 95% by weight or less, 30% by weight or more and 90% by weight or less, 40% by weight or more and 90% by weight or less, or 50% by weight or more and 85% by weight or less. From the viewpoint of the ease of increasing the adhesive strength by mild heating, the use of the (meth)acrylic acid alkyl ester may be advantageous. In some embodiments, the content of the (meth)acrylic acid ester having an alicyclic hydrocarbon group may be less than 50% by weight, less than 30% by weight, less than 15% by weight, less than 10% by weight, or less than 5% by weight of the monomer raw material B. The (meth)acrylic acid ester having an alicyclic hydrocarbon group may not be used.

[0070] In some preferred embodiments, the (meth)acrylic monomer, which is a component of the monomer raw material B, may contain a monomer M2 having a homopolymer Tg of 50° C. or more. In the polymer B, the monomer S1 and the monomer M2 are copolymerized to suitably control the mobility and mobility of the polyorganosiloxane structure portion with increasing temperature, and it is easy to achieve both initial light peelability (reworkability) and an increase in adhesive strength after mild heating. In some embodiments, the Tg of the homopolymer of the monomer M2 may be 60° C. or more, 70° C. or more, 80° C. or more, or 90° C. or more. In addition, the upper limit of the Tg of the homopolymer of the monomer M2 is not particularly limited, but from the viewpoint of ease of synthesis of the polymer B, it is usually appropriate that it is 200° C. or less. In some embodiments, the Tg of the homopolymer of the monomer M2 may be, for example, 180° C. or less, 150° C. or less, or 120° C. or less.

[0071] As the monomer M2, for example, from among the (meth)acrylic monomers exemplified above, those that satisfy the conditions of Tg of the homopolymer can be used. For example, one or more monomers selected from the group consisting of (meth)acrylic acid alkyl esters and (meth)acrylic acid esters having an alicyclic hydrocarbon group can be used. As the (meth)acrylic acid alkyl ester, a methacrylic acid alkyl ester having an alkyl group with 1 to 4 carbon atoms can be preferably used.

[0072] In an embodiment in which the monomer raw material B contains the monomer M2, the content of the monomer M2 may be, for example, 5% by weight or more, 10% by weight or more, 15% by weight or more, 20% by weight or more, 25% by weight or more, or 30% by weight or more of the monomer raw material B. In some embodiments, the content of the monomer M2 may be 35% by weight or more, 40% by weight or more, 45% by weight or more, 50% by weight or more, or 55% by weight or more of the monomer raw material B. In addition, the content of the monomer M2 may be, for example, 90% by weight or less, and is usually suitably 80% by weight or less, preferably 75% by weight or less, may be 70% by weight or less, or may be 65% by weight or less. In some preferred embodiments, the content of the monomer M2 is 60% by weight or less (for example, 50% by weight or less, typically 42% by weight or less). In polymer B, the copolymerization ratio of monomer M2 having a Tg of 50° C. or more is limited to a predetermined value or less, so that an increase in adhesive strength after mild heating can be preferably achieved based on the mobility of polymer B at around 50° C. From the same viewpoint, the content of monomer M2 in monomer raw material B may be 35% by weight or less, 25% by weight or less, or 15% by weight or less (for example, 5% by weight or less).

[0073] The content of the monomer M2 can be preferably applied, for example, to an embodiment in which the monomer M2 is composed of one or more monomers selected from the group consisting of (meth)acrylic acid alkyl esters and the (meth)acrylic acid esters having an alicyclic hydrocarbon group, or an embodiment in which the monomer M2 is composed of one or more monomers selected from (meth)acrylic acid alkyl esters (e.g., methacrylic acid alkyl esters). One preferred example of such an embodiment is an embodiment in which the monomer M2 is composed of MMA.

[0074] In some embodiments, the (meth)acrylic monomer may include a monomer M3 having a homopolymer Tg of less than 50° C. (typically, −20° C. or more and less than 50° C.). Use of the monomer M3 makes it easier to obtain a pressure-sensitive adhesive sheet that has a good balance between adhesive strength and cohesive strength after the adhesive strength is increased. From the viewpoint of making it easier to exert such effects, it is preferable to use the monomer M3 in combination with the monomer M2.

[0075] As the monomer M3, for example, one having a homopolymer Tg that satisfies the conditions can be used from among the (meth)acrylic monomers exemplified above. For example, one or more monomers selected from the group consisting of (meth)acrylic acid alkyl esters can be used.

[0076] In an embodiment in which the monomer raw material B contains the monomer M3, the content of the monomer M3 may be, for example, 5% by weight or more, 10% by weight or more, 15% by weight or more, 20% by weight or more, 25% by weight or more, 30% by weight or more, or 35% by weight or more of the monomer raw material B. The content of the monomer M3 is usually suitably 70% by weight or less, 60% by weight or less, or 50% by weight or less of the monomer raw material B. The above content of the monomer M3 can be preferably applied, for example, to an embodiment in which the monomer M3 is composed of one or more monomers selected from (meth)acrylic acid alkyl esters (e.g., methacrylic acid alkyl esters).

[0077] In some embodiments of the pressure-sensitive adhesive sheet disclosed herein, the monomer raw material B preferably contains 30% by weight or less of a monomer having a homopolymer Tg of higher than 170°C. Here, in this specification, the content of a monomer is X% by weight or less, unless otherwise specified, and includes an embodiment in which the content of the monomer is 0% by weight, that is, an embodiment in which the monomer is not substantially contained. In addition, the term "substantially not contained" means that the monomer is not used at least intentionally. When the copolymerization ratio of a monomer having a homopolymer Tg of higher than 170°C is high, the mobility of polymer B tends to be insufficient, and it may be difficult to increase the adhesive strength by heating to a temperature range higher than 50°C.

[0078] In some embodiments, the monomer raw material B preferably contains at least MMA as a (meth)acrylic monomer. According to the polymer B in which MMA is copolymerized, N 50 It is easy to obtain a pressure-sensitive adhesive sheet with a large diameter. The proportion of MMA in the total amount of (meth)acrylic monomers contained in monomer raw material B may be, for example, 5% by weight or more, 10% by weight or more, 20% by weight or more, 30% by weight or more, or 40% by weight or more. In some embodiments, the proportion of MMA in the total amount of the (meth)acrylic monomers may be, for example, more than 50% by weight, more than 55% by weight, more than 60% by weight, more than 65% by weight, or more than 70% by weight. In addition, the proportion of MMA in the total amount of the (meth)acrylic monomers is usually appropriately 95% by weight or less, and may be 90% by weight or less, or 85% by weight or less. In some preferred embodiments, the proportion of MMA in the total amount of the (meth)acrylic monomers may be 75% by weight or less, 65% by weight or less, 60% by weight or less, or 55% by weight or less (e.g., 50% by weight or less) from the viewpoint of increasing adhesive strength after mild heating.

[0079] Other examples of monomers that may be included together with monomer S1 as a monomer unit constituting polymer B include the carboxyl group-containing monomers, acid anhydride group-containing monomers, hydroxyl group-containing monomers, epoxy group-containing monomers, cyano group-containing monomers, isocyanate group-containing monomers, amide group-containing monomers, monomers having a nitrogen atom-containing ring (N-vinyl cyclic amide, monomers having a succinimide skeleton, maleimides, itaconimides, etc.), aminoalkyl (meth)acrylates, vinyl esters, vinyl ethers, olefins, (meth)acrylic acid esters having an aromatic hydrocarbon group, heterocyclic ring-containing (meth)acrylates, halogen atom-containing (meth)acrylates, and (meth)acrylic acid esters obtained from terpene compound derivative alcohols, which are exemplified above as monomers that may be used when polymer A is an acrylic polymer.

[0080] Further examples of monomers that may be included together with the monomer S1 as a monomer unit constituting the polymer B include oxyalkylene di(meth)acrylates such as ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, and tripropylene glycol di(meth)acrylate; monomers having a polyoxyalkylene skeleton, such as polyethylene glycol and polypropylene glycol, having a polymerizable functional group such as a (meth)acryloyl group, a vinyl group, or an allyl group at one end of the polyoxyalkylene chain and an ether structure (alkyl ether, aryl ether, aryl alkyl ether, or the like) at the other end; methoxyethyl (meth)acrylate, ethoxyethyl (meth)acrylate, and propoxyethyl (meth)acrylate; Alkoxyalkyl (meth)acrylates such as butoxyethyl (meth)acrylate and ethoxypropyl (meth)acrylate; salts such as alkali metal (meth)acrylate; polyvalent (meth)acrylates such as trimethylolpropane tri(meth)acrylate; halogenated vinyl compounds such as vinylidene chloride and 2-chloroethyl (meth)acrylate; oxazoline group-containing monomers such as 2-vinyl-2-oxazoline, 2-vinyl-5-methyl-2-oxazoline and 2-isopropenyl-2-oxazoline; aziridine group-containing monomers such as (meth)acryloylaziridine and 2-aziridinylethyl (meth)acrylate; hydroxyl group-containing vinyl monomers such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate and adducts of lactones and 2-hydroxyethyl (meth)acrylate; fluorine-containing vinyl monomers such as fluorine-substituted (meth)acrylic acid alkyl esters; reactive halogen-containing vinyl monomers such as 2-chloroethyl vinyl ether and vinyl monochloroacetate;Examples of the vinyl monomer include organosilicon-containing vinyl monomers such as vinyltrimethoxysilane, γ-(meth)acryloxypropyltrimethoxysilane, allyltrimethoxysilane, trimethoxysilylpropylallylamine, and 2-methoxyethoxytrimethoxysilane; and macromonomers having a radical polymerizable vinyl group at the monomer end obtained by polymerizing a vinyl group. These may be copolymerized with monomer S1 either alone or in combination of two or more.

[0081] In some embodiments, the polymer B may preferably be one that does not have a functional group that undergoes a crosslinking reaction with the polymer A. In other words, the polymer B is preferably included in the adhesive layer in a form that is not chemically bonded to the polymer A. The adhesive layer containing the polymer B in such a form has good mobility of the polymer B when heated, and is suitable for improving the adhesive strength increase ratio. The functional group that undergoes a crosslinking reaction with the polymer A may vary depending on the type of functional group possessed by the polymer A, and may be, for example, an epoxy group, an isocyanate group, a carboxy group, an alkoxysilyl group, an amino group, etc.

[0082] The Mw of polymer B is not particularly limited. The Mw of polymer B may be, for example, 1000 or more, or 5000 or more. From the viewpoint of favorably exhibiting an increase in adhesive strength after mild heating, the Mw of polymer B may be, for example, 10,000 or more, 12,000 or more, 15,000 or more, or 20,000 or more. In some embodiments, the Mw of polymer B may be 50,000 or more, 80,000 or more, 100,000 or more, or 120,000 or more (for example, 150,000 or more). The upper limit of the Mw of polymer B is, for example, 500,000 or less, 350,000 or less, 350,000 or less, or less than 100,000. From the viewpoint of adjusting the compatibility and mobility within the adhesive layer within an appropriate range and favorably exhibiting an increase in adhesive strength after mild heating, the Mw of polymer B may be less than 80,000, less than 70,000, less than 50,000, less than 40,000, less than 20,000, or even less than 10,000.

[0083] In some preferred embodiments, the Mw of polymer B is preferably lower than the Mw of polymer A. This makes it easier to realize a pressure-sensitive adhesive sheet that has both good reworkability at the initial stage of application and increased adhesive strength after mild heating. The Mw of polymer B may be, for example, 0.8 times or less, 0.75 times or less, 0.5 times or less, 0.3 times or less, 0.1 times or less, 0.05 times or less, or 0.03 times or less (e.g., 0.02 times or less) the Mw of polymer A.

[0084] Polymer B can be prepared, for example, by polymerizing the above-mentioned monomers by a known method such as solution polymerization, emulsion polymerization, bulk polymerization, suspension polymerization, or photopolymerization.

[0085] A chain transfer agent can be used as necessary to adjust the molecular weight of polymer B. Examples of the chain transfer agent to be used include compounds having a mercapto group, such as octyl mercaptan, lauryl mercaptan, t-nonyl mercaptan, t-dodecyl mercaptan, mercaptoethanol, and α-thioglycerol; thioglycolic acid esters, such as thioglycolic acid, methyl thioglycolate, ethyl thioglycolate, propyl thioglycolate, butyl thioglycolate, t-butyl thioglycolate, 2-ethylhexyl thioglycolate, octyl thioglycolate, isooctyl thioglycolate, decyl thioglycolate, dodecyl thioglycolate, thioglycolic acid ester of ethylene glycol, thioglycolic acid ester of neopentyl glycol, and thioglycolic acid ester of pentaerythritol; and α-methylstyrene dimer.

[0086] The amount of the chain transfer agent used is not particularly limited, but is usually 0.05 to 20 parts by weight, preferably 0.1 to 15 parts by weight, and more preferably 0.2 to 10 parts by weight, per 100 parts by weight of the monomer. By adjusting the amount of the chain transfer agent added in this manner, a polymer B having a suitable molecular weight can be obtained. The chain transfer agent can be used alone or in combination of two or more kinds.

[0087] As a means for adjusting the molecular weight of polymer B, various conventionally known means including the use of the chain transfer agent can be used alone or in appropriate combination. The same applies to the molecular weight of polymer A. Non-limiting examples of such means include selection of a polymerization method, selection of the type and amount of a polymerization initiator, selection of a polymerization temperature, selection of the type and amount of a polymerization solvent in a solution polymerization method, selection of light irradiation intensity in a photopolymerization method, etc. A person skilled in the art would understand how to obtain a polymer having a desired molecular weight based on the description of the present specification including the specific examples described below and the common general technical knowledge at the time of filing of the present application.

[0088] In the pressure-sensitive adhesive sheet disclosed herein, the amount of polymer B used relative to 100 parts by weight of polymer A used can be, for example, 0.1 parts by weight or more, and from the viewpoint of obtaining a higher effect, it may be 0.5 parts by weight or more, 1 part by weight or more, or 2 parts by weight or more. In some embodiments, from the viewpoint of improving reworkability, the amount of polymer B used can be, for example, 3 parts by weight or more, 4 parts by weight or more, or 5 parts by weight or more. In addition, the amount of polymer B used relative to 100 parts by weight of polymer A used can be, for example, 75 parts by weight or less, 60 parts by weight or less, or 50 parts by weight or less. From the viewpoint of avoiding an excessive decrease in the cohesive force of the pressure-sensitive adhesive layer, in some embodiments, the amount of polymer B used relative to 100 parts by weight of polymer A can be, for example, 40 parts by weight or less, and may be 35 parts by weight or less, 30 parts by weight or less, or 25 parts by weight or less. In order to obtain a higher adhesive strength after heating, in some embodiments, the amount of polymer B used may be 20 parts by weight or less, 17 parts by weight or less, 15 parts by weight or less, 12 parts by weight or less, 10 parts by weight or less, 8 parts by weight or less, 6 parts by weight or less, or 4 parts by weight or less (for example, 3 parts by weight or less).

[0089] The pressure-sensitive adhesive layer may contain a polymer (optional polymer) other than polymer A and polymer B as necessary, to the extent that the performance of the pressure-sensitive adhesive sheet disclosed herein is not significantly impaired. The amount of such an optional polymer used is usually appropriately 20% by weight or less of the total polymer components contained in the pressure-sensitive adhesive layer, and may be 15% by weight or less, or may be 10% by weight or less. In some embodiments, the amount of the optional polymer used may be 5% by weight or less, 3% by weight or less, or may be 1% by weight or less of the total polymer components. The pressure-sensitive adhesive layer may be substantially free of polymers other than polymer A and polymer B.

[0090] (Crosslinking agent) In the pressure-sensitive adhesive layer, a crosslinking agent may be used as necessary for the purpose of adjusting the cohesive force, etc. As the crosslinking agent, a crosslinking agent known in the field of pressure-sensitive adhesives may be used, and examples thereof include epoxy-based crosslinking agents, isocyanate-based crosslinking agents, silicone-based crosslinking agents, oxazoline-based crosslinking agents, aziridine-based crosslinking agents, silane-based crosslinking agents, alkyl etherified melamine-based crosslinking agents, and metal chelate-based crosslinking agents. In particular, isocyanate-based crosslinking agents, epoxy-based crosslinking agents, and metal chelate-based crosslinking agents are preferably used. The crosslinking agents may be used alone or in combination of two or more.

[0091] Specifically, examples of isocyanate-based crosslinking agents include tolylene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, xylylene diisocyanate, hydrogenated xylylene diisocyanate, diphenylmethane diisocyanate, hydrogenated diphenylmethane diisocyanate, tetramethylxylylene diisocyanate, naphthalene diisocyanate, triphenylmethane triisocyanate, polymethylene polyphenyl isocyanate, and adducts of these with polyols such as trimethylolpropane. Alternatively, a compound having at least one isocyanate group and one or more unsaturated bonds in one molecule, specifically 2-isocyanatoethyl (meth)acrylate, etc., can also be used as an isocyanate-based crosslinking agent. These can be used alone or in combination of two or more.

[0092] Examples of epoxy crosslinking agents include bisphenol A, epichlorohydrin type epoxy resins, ethylene glycidyl ether, polyethylene glycol diglycidyl ether, glycerin diglycidyl ether, glycerin triglycidyl ether, 1,6-hexanediol glycidyl ether, trimethylolpropane triglycidyl ether, diglycidylaniline, diamine glycidylamine, N,N,N',N'-tetraglycidyl-m-xylylenediamine, and 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, etc. These may be used alone or in combination of two or more.

[0093] Examples of the metal chelate compound include metal components such as aluminum, iron, tin, titanium, nickel, etc., and chelate components such as acetylene, methyl acetoacetate, ethyl lactate, etc. These may be used alone or in combination of two or more.

[0094] The amount of the crosslinking agent used is not particularly limited, and can be, for example, more than 0 parts by weight relative to 100 parts by weight of polymer A. The amount of the crosslinking agent used can be, for example, 0.01 parts by weight or more relative to 100 parts by weight of polymer A, and is preferably 0.05 parts by weight or more. By increasing the amount of the crosslinking agent used, the adhesive strength at the initial stage of application is suppressed, and reworkability tends to be improved. In some embodiments, the amount of the crosslinking agent used relative to 100 parts by weight of polymer A may be 0.1 parts by weight or more, may be 0.5 parts by weight or more, or may be 0.8 parts by weight or more. On the other hand, from the viewpoint of obtaining an increase in adhesive strength after mild heating while allowing the mobility of polymer B to an appropriate extent, the amount of the crosslinking agent used relative to 100 parts by weight of polymer A is usually appropriately 15 parts by weight or less, may be 10 parts by weight or less, or may be 5 parts by weight or less.

[0095] The technology disclosed herein can be preferably implemented in an embodiment using at least an isocyanate-based crosslinking agent as a crosslinking agent. From the viewpoint of achieving both good reworkability at the initial stage of application and increased adhesive strength after mild heating, in some embodiments, the amount of the isocyanate-based crosslinking agent used relative to 100 parts by weight of polymer A can be, for example, 0.01 parts by weight or more, or 0.05 parts by weight or more, or 0.1 parts by weight or more, or 0.2 parts by weight or more (for example, 0.3 parts by weight or more), or, for example, 5 parts by weight or less, or 3 parts by weight or less, or 1.5 parts by weight or less, or 1.2 parts by weight or less, or 0.8 parts by weight or less (for example, 0.6 parts by weight or less).

[0096] Although not particularly limited, when an isocyanate-based crosslinking agent is used in a configuration in which the adhesive layer contains a hydroxyl group-containing monomer as a monomer unit, the amount of the isocyanate-based crosslinking agent used W NCO The amount of hydroxyl group-containing monomer used W OH is based on weight, W OH / W NCO The amount can be set so that the ratio of the hydroxyl group-containing monomer to the isocyanate-based crosslinking agent is 2 or more. In this way, by increasing the amount of the hydroxyl group-containing monomer used relative to the isocyanate-based crosslinking agent, a crosslinked structure suitable for greatly increasing the adhesive strength after mild heating relative to the adhesive strength at the initial stage of application can be formed. In some embodiments, W OH / W NCO may be 3 or more, 5 or more, 10 or more, 20 or more, 30 or more, or 50 or more. OH / W NCO The upper limit of W is not particularly limited, and from the viewpoint of obtaining a degree of crosslinking that allows for a moderate movement of polymer B by mild heating, OH / W NCO may be, for example, 500 or less, 200 or less, 100 or less, or 50 or less.

[0097] In order to make any of the above-mentioned crosslinking reactions proceed more effectively, a crosslinking catalyst may be used. As the crosslinking catalyst, for example, a tin catalyst (particularly dioctyltin dilaurate) can be preferably used. The amount of the crosslinking catalyst used is not particularly limited, but can be, for example, about 0.0001 to 1 part by weight relative to 100 parts by weight of polymer A.

[0098] The adhesive layer may contain a polyfunctional monomer as required. The polyfunctional monomer may be used in place of the crosslinking agent as described above or in combination with the crosslinking agent, and may be useful for purposes such as adjusting the cohesive strength. For example, the polyfunctional monomer may be preferably used in the adhesive layer formed from the photocurable adhesive composition. Examples of the polyfunctional monomer include ethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, ethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,12-dodecanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, tetramethylolmethane tri(meth)acrylate, allyl (meth)acrylate, vinyl (meth)acrylate, divinylbenzene, epoxy acrylate, polyester acrylate, urethane acrylate, butyl diol (meth)acrylate, and hexyl diol di(meth)acrylate. Among them, trimethylolpropane tri(meth)acrylate, 1,6-hexanediol di(meth)acrylate, and dipentaerythritol hexa(meth)acrylate can be preferably used. The polyfunctional monomers can be used alone or in combination of two or more.

[0099] The amount of the polyfunctional monomer used varies depending on its molecular weight, the number of functional groups, etc., but is usually appropriate to be in the range of about 0.01 to 3.0 parts by weight relative to 100 parts by weight of polymer A. In some embodiments, the amount of the polyfunctional monomer used may be, for example, 0.02 parts by weight or more, or 0.03 parts by weight or more, relative to 100 parts by weight of polymer A. By increasing the amount of the polyfunctional monomer used, the adhesive strength at the initial stage of application tends to be suppressed and reworkability tends to be improved. On the other hand, from the viewpoint of ensuring the mobility of polymer B while controlling its movement with a crosslinked network to adjust the increase in adhesive strength after mild heating, the amount of the polyfunctional monomer used may be 2.0 parts by weight or less, 1.0 parts by weight or less, or 0.5 parts by weight or less, relative to 100 parts by weight of polymer A.

[0100] (tackifier resin) The adhesive layer may contain a tackifier resin as necessary. The tackifier resin is not particularly limited, but may be, for example, a rosin-based tackifier resin, a terpene-based tackifier resin, a phenol-based tackifier resin, a hydrocarbon-based tackifier resin, a ketone-based tackifier resin, a polyamide-based tackifier resin, an epoxy-based tackifier resin, or an elastomer-based tackifier resin. The tackifier resin may be used alone or in combination of two or more.

[0101] Examples of rosin-based tackifying resins include unmodified rosins (raw rosins) such as gum rosin, wood rosin, and tall oil rosin; modified rosins obtained by modifying these unmodified rosins through polymerization, disproportionation, hydrogenation, or the like (polymerized rosin, stabilized rosin, disproportionated rosin, fully hydrogenated rosin, partially hydrogenated rosin, and other chemically modified rosins); and various rosin derivatives. Examples of the rosin derivative include: Rosin phenolic resin obtained by adding phenol to rosins (unmodified rosin, modified rosin, various rosin derivatives, etc.) using an acid catalyst and then thermally polymerizing the mixture; rosin ester resins such as rosin ester compounds (unmodified rosin esters) obtained by esterifying unmodified rosin with alcohols, and modified rosin ester compounds (polymerized rosin ester, stabilized rosin ester, disproportionated rosin, fully hydrogenated rosin, partially hydrogenated rosin, etc.) obtained by esterifying modified rosins such as polymerized rosin, stabilized rosin ester, disproportionated rosin ester, fully hydrogenated rosin ester, partially hydrogenated rosin ester, etc.) with alcohols; Unsaturated fatty acid modified rosin resins, which are made by modifying unmodified rosin or modified rosin (polymerized rosin, stabilized rosin, disproportionated rosin, fully hydrogenated rosin, partially hydrogenated rosin, etc.) with unsaturated fatty acids; unsaturated fatty acid modified rosin ester resin obtained by modifying a rosin ester resin with an unsaturated fatty acid; Unmodified rosin, modified rosin (polymerized rosin, stabilized rosin, disproportionated rosin, fully hydrogenated rosin, partially hydrogenated rosin, etc.), unsaturated fatty acid modified rosin resin, or rosin alcohol resin in which the carboxyl group in unsaturated fatty acid modified rosin ester resin has been reduced; Examples of the metal salts include unmodified rosin, modified rosin, and metal salts of rosin-based resins such as various rosin derivatives (particularly rosin ester-based resins).

[0102] Examples of terpene-based tackifying resins include terpene-based resins such as α-pinene polymers, β-pinene polymers, and dipentene polymers, as well as modified terpene-based resins obtained by modifying these terpene-based resins (phenol-modified, aromatic-modified, hydrogen-modified, hydrocarbon-modified, etc.) (e.g., terpene-phenolic resins, styrene-modified terpene resins, aromatic-modified terpene resins, hydrogenated terpene resins, etc.).

[0103] Examples of phenol-based tackifying resins include condensates of various phenols (e.g., phenol, m-cresol, 3,5-xylenol, p-alkylphenol, resorcin, etc.) with formaldehyde (e.g., alkylphenol-based resins, xylene formaldehyde-based resins, etc.), resols obtained by addition reaction of the above-mentioned phenols with formaldehyde using an alkali catalyst, and novolaks obtained by condensation reaction of the above-mentioned phenols with formaldehyde using an acid catalyst.

[0104] Examples of hydrocarbon-based tackifying resins include various hydrocarbon resins such as aliphatic hydrocarbon resins, aromatic hydrocarbon resins, aliphatic cyclic hydrocarbon resins, aliphatic / aromatic petroleum resins (styrene-olefin copolymers, etc.), aliphatic / alicyclic petroleum resins, hydrogenated hydrocarbon resins, coumarone resins, and coumarone-indene resins.

[0105] Commercially available polymerized rosin esters that can be preferably used include those available from Arakawa Chemical Industries, Ltd. under the trade names "PENSEL D-125," "PENSEL D-135," "PENSEL D-160," "PENSEL KK," and "PENSEL C," but are not limited to these.

[0106] Examples of commercially available terpene phenol resins that can be preferably used include those manufactured by Yasuhara Chemical Co., Ltd. under the trade names "YS Polystar S-145," "YS Polystar G-125," "YS Polystar N125," and "YS Polystar U-115," those manufactured by Arakawa Chemical Industries, Ltd. under the trade names "Tamanol 803L" and "Tamanol 901," and those manufactured by Sumitomo Bakelite Co., Ltd. under the trade name "Sumilite Resin PR-12603," but are not limited to these.

[0107] The content of the tackifier resin is not particularly limited and can be set so as to exhibit appropriate adhesive performance depending on the purpose and application. The content of the tackifier resin (when two or more tackifier resins are contained, the total amount thereof) relative to 100 parts by weight of polymer A can be, for example, about 5 to 500 parts by weight.

[0108] The tackifier resin preferably has a softening point (softening temperature) of about 80° C. or higher (preferably about 100° C. or higher, for example about 120° C. or higher). A tackifier resin having a softening point equal to or higher than the above-mentioned lower limit makes it easier to obtain a pressure-sensitive adhesive sheet having high adhesive strength after heating. The upper limit of the softening point is not particularly limited, and may be, for example, about 200° C. or lower (typically 180° C. or lower). The softening point of the tackifier resin can be measured based on the softening point test method (ring and ball method) specified in JIS K2207.

[0109] In addition, the adhesive layer in the technology disclosed herein may contain, as necessary, known additives that can be used in adhesives, such as leveling agents, plasticizers, softeners, colorants (dyes, pigments, etc.), fillers, antistatic agents, antioxidants, UV absorbers, antioxidants, light stabilizers, and preservatives, provided that the effects of the present invention are not significantly impeded.

[0110] The adhesive layer constituting the adhesive sheet disclosed herein may be a cured layer of an adhesive composition. That is, the adhesive layer may be formed by applying (for example, coating) an aqueous dispersion type, solvent type, photocurable type, hot melt type, or other adhesive composition to a suitable surface, and then appropriately carrying out a curing treatment. When two or more types of curing treatments (drying, crosslinking, polymerization, cooling, etc.) are performed, these can be performed simultaneously or in multiple stages. In an adhesive composition using a partial polymer (polymer syrup) of a monomer raw material, typically, a final copolymerization reaction is performed as the curing treatment. That is, the partial polymer is subjected to a further copolymerization reaction to form a complete polymer. For example, in the case of a photocurable adhesive composition, light irradiation is performed. If necessary, a curing treatment such as crosslinking or drying may be performed. For example, if a photocurable adhesive composition needs to be dried, it is recommended to perform photocuring after drying. In an adhesive composition using a complete polymer, typically, a treatment such as drying (heat drying) or crosslinking is performed as the curing treatment as necessary.

[0111] The pressure-sensitive adhesive composition can be applied using a conventional coater such as a gravure roll coater, a reverse roll coater, a kiss roll coater, a dip roll coater, a bar coater, a knife coater or a spray coater.

[0112] The thickness of the adhesive layer is not particularly limited, and can be, for example, 1 μm or more. In some embodiments, the thickness of the adhesive layer may be, for example, 3 μm or more, 5 μm or more, 8 μm or more, 10 μm or more, 15 μm or more, 20 μm or more, or more than 20 μm. The adhesive strength after heating tends to increase due to the increase in the thickness of the adhesive layer. In addition, in some embodiments, the thickness of the adhesive layer may be, for example, 300 μm or less, 200 μm or less, 150 μm or less, 100 μm or less, 70 μm or less, 50 μm or less, or 40 μm or less. It may be advantageous for the adhesive layer not to be too thick in terms of thinning the adhesive sheet and preventing cohesive failure of the adhesive layer. In addition, in the case of an adhesive sheet having a first adhesive layer and a second adhesive layer on the first surface and the second surface of the substrate, the thickness of the adhesive layer described above may be applied to at least the thickness of the first adhesive layer. The thickness of the second pressure-sensitive adhesive layer can be selected from a similar range. In the case of a substrate-less pressure-sensitive adhesive sheet, the thickness of the pressure-sensitive adhesive sheet is the same as the thickness of the pressure-sensitive adhesive layer.

[0113] The storage modulus G'(150°C) of the adhesive layer at 150°C is appropriately set within a range in which the adhesive strength increases to a predetermined value or more after mild heating, and is not limited to a specific range. In some embodiments, the storage modulus G'(150°C) of the adhesive layer can be 5000 Pa or more, and from the viewpoint of obtaining good adhesive properties such as low adhesive strength at the initial stage of application, it is preferably 10,000 Pa or more, more preferably 15,000 Pa or more, and even more preferably 20,000 Pa or more (e.g., 25,000 Pa or more), and may be 30,000 Pa or more, 40,000 Pa or more, or 50,000 Pa or more. In addition, the storage modulus G'(150°C) can be, for example, 300,000 Pa or less, 200,000 Pa or less, 150,000 Pa or less, or 100,000 Pa or less. In some preferred embodiments, the storage modulus G'(150°C) is 90,000 Pa or less, or may be 70,000 Pa or less, 50,000 Pa or less, 40,000 Pa or less, or 30,000 Pa or less, from the viewpoint of favorably increasing the adhesive strength after mild heating as a degree of crosslinking that allows for moderate movement of polymer B in the adhesive layer. The storage modulus G'(150°C) of the adhesive layer can be adjusted by the type and amount of crosslinking agent used, the molecular weight and molecular structure of polymer A, etc. The storage modulus G'(150°C) of the adhesive layer is measured by the method described in the Examples below.

[0114] Although not particularly limited, the gel fraction of the adhesive constituting the adhesive layer is usually in the range of 20.0% to 99.0%, and preferably in the range of 30.0% to 90.0%. By setting the gel fraction in the above range, it is possible to preferably realize an increase in adhesive strength after mild heating. The gel fraction is measured by the following method.

[0115] [Measurement of gel fraction] About 0.1 g of the adhesive sample (weight Wg1) is wrapped in a porous polytetrafluoroethylene film (weight Wg2) with an average pore size of 0.2 μm in a purse shape, and the opening is tied with a string (weight Wg3). As the porous polytetrafluoroethylene film, the product name "Nitoflon (registered trademark) NTF1122" (Nitto Denko Corporation, average pore size 0.2 μm, porosity 75%, thickness 85 μm) or an equivalent product is used. The wrapper is immersed in 50 mL of ethyl acetate and kept at room temperature (typically 23 ° C) for 7 days to elute the sol content (ethyl acetate soluble content) in the adhesive out of the film. Next, the wrapper is taken out, the ethyl acetate adhering to the outer surface is wiped off, and the wrapper is dried at 130 ° C for 2 hours, and the weight of the wrapper (Wg4) is measured. By substituting each value into the following formula, the gel fraction G of the adhesive is calculated. C can be calculated. Gel fraction G C (%) = [(Wg4-Wg2-Wg3) / Wg1] x 100

[0116] <Supporting base material> The pressure-sensitive adhesive sheet according to some embodiments may be in the form of a substrate-attached pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer on one or both sides of a support substrate. The material of the support substrate is not particularly limited, and can be appropriately selected according to the purpose and mode of use of the pressure-sensitive adhesive sheet. Non-limiting examples of substrates that can be used include plastic films such as polyolefin films mainly composed of polyolefins such as polypropylene and ethylene-propylene copolymers, polyester films mainly composed of polyesters such as polyethylene terephthalate and polybutylene terephthalate, and polyvinyl chloride films mainly composed of polyvinyl chloride; foam sheets made of foams such as polyurethane foam, polyethylene foam, and polychloroprene foam; woven and nonwoven fabrics made by single or mixed spinning of various fibrous materials (natural fibers such as hemp and cotton, synthetic fibers such as polyester and vinylon, semi-synthetic fibers such as acetate, etc.); papers such as Japanese paper, fine paper, craft paper, and crepe paper; metal foils such as aluminum foil and copper foil; and the like. The substrate may be a composite of these. Examples of such composite substrates include substrates having a structure in which a metal foil and the above-mentioned plastic film are laminated together, and plastic substrates reinforced with inorganic fibers such as glass cloth.

[0117] As the substrate of the adhesive sheet disclosed herein, various film substrates can be preferably used. The film substrate may be a porous substrate such as a foam film or a nonwoven fabric sheet, or may be a nonporous substrate, or may be a substrate having a structure in which a porous layer and a nonporous layer are laminated. In some embodiments, the film substrate may preferably be one that includes a resin film that can independently maintain its shape (self-supporting or independent) as a base film. Here, the term "resin film" refers to a resin film that has a nonporous structure and typically does not substantially contain air bubbles (voidless). Therefore, the resin film is a concept that is distinguished from foam films and nonwoven fabrics. As the resin film, one that can independently maintain its shape (self-supporting or independent) can be preferably used. The resin film may be a single-layer structure, or may be a multi-layer structure of two or more layers (for example, a three-layer structure).

[0118] Examples of resin materials constituting the resin film include polyester, polyolefin, polyamide (PA) such as nylon 6, nylon 66, and partially aromatic polyamide, polyimide (PI), polyamideimide (PAI), polyetheretherketone (PEEK), polyethersulfone (PES), polyphenylene sulfide (PPS), polycarbonate (PC), polyurethane (PU), ethylene-vinyl acetate copolymer (EVA), fluororesin such as polytetrafluoroethylene (PTFE), acrylic resin, polyacrylate, polystyrene, polyvinyl chloride, and polyvinylidene chloride. The resin film may be formed using a resin material containing only one of these resins, or may be formed using a resin material containing two or more of them blended together. The resin film may be unstretched or stretched (for example, uniaxially or biaxially stretched).

[0119] Suitable examples of resin materials constituting the resin film include polyester-based resin, PPS resin, and polyolefin-based resin. Here, polyester-based resin refers to a resin containing more than 50% by weight of polyester. Similarly, PPS resin refers to a resin containing more than 50% by weight of PPS, and polyolefin-based resin refers to a resin containing more than 50% by weight of polyolefin.

[0120] As the polyester-based resin, typically used is a polyester-based resin containing, as a main component, a polyester obtained by polycondensation of a dicarboxylic acid and a diol.

[0121] Examples of dicarboxylic acids constituting the polyester include phthalic acid, isophthalic acid, terephthalic acid, 2-methylterephthalic acid, 5-sulfoisophthalic acid, 4,4'-diphenyldicarboxylic acid, 4,4'-diphenyletherdicarboxylic acid, 4,4'-diphenylketonedicarboxylic acid, 4,4'-diphenoxyethanedicarboxylic acid, 4,4'-diphenylsulfonedicarboxylic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, and the like. Examples of the dicarboxylic acids include aromatic dicarboxylic acids such as cyclohexanedicarboxylic acid, cyclohexanedicarboxylic acid, and aromatic dicarboxylic acids such as 1,2-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, and 1,4-cyclohexanedicarboxylic acid; aliphatic dicarboxylic acids such as malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, and dodecanoic acid; unsaturated dicarboxylic acids such as maleic acid, maleic anhydride, and fumaric acid; and derivatives thereof (for example, lower alkyl esters of the above dicarboxylic acids such as terephthalic acid); and the like. These can be used alone or in combination of two or more. From the viewpoint of strength, aromatic dicarboxylic acids are preferred. Among them, preferred dicarboxylic acids include terephthalic acid and 2,6-naphthalenedicarboxylic acid. For example, it is preferred that 50% by weight or more (for example, 80% by weight or more, typically 95% by weight or more) of the dicarboxylic acids constituting the polyester are terephthalic acid, 2,6-naphthalenedicarboxylic acid, or a combination of these. The dicarboxylic acid may consist essentially of terephthalic acid, essentially of 2,6-naphthalenedicarboxylic acid, or essentially of terephthalic acid and 2,6-naphthalenedicarboxylic acid.

[0122] Examples of the diol constituting the polyester include aliphatic diols such as ethylene glycol, diethylene glycol, polyethylene glycol, propylene glycol, polypropylene glycol, 1,3-propanediol, 1,5-pentanediol, neopentyl glycol, 1,4-butanediol, 1,6-hexanediol, 1,8-octanediol, and polyoxytetramethylene glycol; alicyclic diols such as 1,2-cyclohexanediol, 1,4-cyclohexanediol, 1,1-cyclohexanedimethylol, and 1,4-cyclohexanedimethylol; aromatic diols such as xylylene glycol, 4,4'-dihydroxybiphenyl, 2,2-bis(4'-hydroxyphenyl)propane, and bis(4-hydroxyphenyl)sulfone; and the like. These can be used alone or in combination of two or more. Among them, aliphatic diols are preferred from the viewpoint of transparency, and ethylene glycol is particularly preferred. The proportion of the aliphatic diol (preferably ethylene glycol) in the diol constituting the polyester is preferably 50% by weight or more (e.g., 80% by weight or more, typically 95% by weight or more). The diol may be substantially composed of ethylene glycol alone.

[0123] Specific examples of polyester resins include polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polyethylene naphthalate (PEN), and polybutylene naphthalate.

[0124] As the polyolefin resin, one type of polyolefin can be used alone, or two or more types of polyolefins can be used in combination. The polyolefin can be, for example, a homopolymer of an α-olefin, a copolymer of two or more types of α-olefins, or a copolymer of one or more types of α-olefins and other vinyl monomers. Specific examples include polyethylene (PE), polypropylene (PP), poly-1-butene, poly-4-methyl-1-pentene, ethylene-propylene copolymers such as ethylene-propylene rubber (EPR), ethylene-propylene-butene copolymers, ethylene-butene copolymers, ethylene-vinyl alcohol copolymers, and ethylene-ethyl acrylate copolymers. Both low density (LD) polyolefins and high density (HD) polyolefins can be used. Examples of polyolefin resin films include non-oriented polypropylene (CPP) film, biaxially oriented polypropylene (OPP) film, low-density polyethylene (LDPE) film, linear low-density polyethylene (LLDPE) film, medium-density polyethylene (MDPE) film, high-density polyethylene (HDPE) film, polyethylene (PE) film made by blending two or more types of polyethylene (PE), and PP / PE blend film made by blending polypropylene (PP) and polyethylene (PE).

[0125] Specific examples of resin films that can be preferably used as the base film of the adhesive sheet disclosed herein include PET film, PEN film, PPS film, PEEK film, CPP film and OPP film. Examples of base films that are preferred from the viewpoint of strength and dimensional stability include PET film, PEN film, PPS film and PEEK film. From the viewpoint of easy availability of the substrate, PET film and PPS film are particularly preferred, and PET film is particularly preferred.

[0126] The resin film may contain known additives such as light stabilizers, antioxidants, antistatic agents, colorants (dyes, pigments, etc.), fillers, slip agents, antiblocking agents, etc., as necessary, within the range that does not significantly impair the effects of the present invention. The amount of additives to be added is not particularly limited, and can be appropriately set depending on the application of the pressure-sensitive adhesive sheet, etc.

[0127] The method for producing the resin film is not particularly limited, and may be any of the conventionally known general resin film forming methods, such as extrusion molding, inflation molding, T-die casting, and calendar roll molding.

[0128] The substrate may be substantially composed of such a base film. Alternatively, the substrate may include an auxiliary layer in addition to the base film. Examples of the auxiliary layer include an optical property adjusting layer (e.g., a coloring layer, an anti-reflection layer), a printing layer or a lamination layer for imparting a desired appearance to the substrate, an antistatic layer, an undercoat layer, a peeling layer, and other surface treatment layers.

[0129] The thickness of the substrate is not particularly limited and may be selected according to the purpose and mode of use of the pressure-sensitive adhesive sheet. The thickness of the substrate may be, for example, 1000 μm or less. In some embodiments, from the viewpoint of the handleability and processability of the pressure-sensitive adhesive sheet, the thickness of the substrate may be, for example, 500 μm or less, 300 μm or less, 250 μm or less, or 200 μm or less. In some embodiments, from the viewpoint of miniaturization and weight reduction of the product to which the pressure-sensitive adhesive sheet is applied, the thickness of the substrate may be, for example, 160 μm or less, 130 μm or less, 100 μm or less, 90 μm or less, 80 μm or less, 60 μm or less, 50 μm or less, 25 μm or less, 10 μm or less, or 5 μm or less. When the thickness of the substrate is reduced, the flexibility of the pressure-sensitive adhesive sheet and its ability to follow the surface shape of the adherend tend to improve. In addition, from the viewpoint of handling and processability, the thickness of the substrate may be, for example, 2 μm or more, 5 μm or more, 10 μm or more, 20 μm or more, 25 μm or more, or more than 25 μm. In some embodiments, the thickness of the substrate may be, for example, 30 μm or more, 35 μm or more, 55 μm or more, 70 μm or more, 75 μm or more, 90 μm or more, or 120 μm or more. For example, in a pressure-sensitive adhesive sheet that can be used for purposes such as reinforcing, supporting, and cushioning an adherend, a substrate having a thickness of 30 μm or more can be preferably used.

[0130] The first surface of the substrate may be subjected to a conventionally known surface treatment, such as a corona discharge treatment, a plasma treatment, an ultraviolet irradiation treatment, an acid treatment, an alkali treatment, or the formation of an undercoat layer by applying an undercoat agent (primer), if necessary. Such a surface treatment may be a treatment for improving the anchoring property of the pressure-sensitive adhesive layer to the substrate. For example, in a pressure-sensitive adhesive sheet having a substrate containing a resin film as a base film, a substrate subjected to such an anchoring property improvement treatment may be preferably used. The above surface treatments may be applied alone or in combination. The composition of the primer used to form the undercoat layer is not particularly limited, and may be appropriately selected from known ones. The thickness of the undercoat layer is not particularly limited, but is usually appropriate to be about 0.01 μm to 1 μm, and preferably about 0.1 μm to 1 μm. Other treatments that may be applied to the first surface of the substrate as necessary include an antistatic layer forming treatment, a colored layer forming treatment, a printing treatment, and the like.

[0131] When the pressure-sensitive adhesive sheet disclosed herein is in the form of a single-sided pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer only on the first surface of the substrate, the second surface of the substrate may be subjected to a conventionally known surface treatment such as a release treatment or an antistatic treatment, if necessary. For example, by surface treating the back surface of the substrate with a release treatment agent (typically by providing a release layer made of a release treatment agent), the unwinding force of the pressure-sensitive adhesive sheet wound into a roll can be reduced. As the release treatment agent, a silicone-based release treatment agent, a long-chain alkyl-based release treatment agent, an olefin-based release treatment agent, a fluorine-based release treatment agent, a fatty acid amide-based release treatment agent, molybdenum sulfide, silica powder, etc. can be used. In addition, for the purpose of improving printability, reducing light reflectivity, improving overlapping adhesion, etc., the second surface of the substrate may be subjected to a corona discharge treatment, a plasma treatment, an ultraviolet irradiation treatment, an acid treatment, an alkali treatment, etc. In addition, in the case of a double-sided pressure-sensitive adhesive sheet, the second surface of the substrate may be subjected to a surface treatment similar to those exemplified above as the surface treatment that can be applied to the first surface of the substrate, if necessary. The surface treatment applied to the first surface of the substrate and the surface treatment applied to the second surface may be the same or different.

[0132] <Adhesive sheet> (Characteristics of adhesive sheet, etc.) The adhesive sheet disclosed herein has an adhesive strength of 5N / 25mm or more. 50 , that is, the adhesive strength measured at 23°C after being attached to a stainless steel plate and held at 50°C for 15 minutes. An adhesive sheet that satisfies this characteristic has an adhesive strength that increases to a predetermined value or more when it is attached to an adherend and then mildly heated at about 50°C. According to the technology disclosed herein, it is possible to obtain strong adhesive strength by mild heating, so that the adhesive strength N 50 can be 7N / 25mm or more, for example, 10N / 25mm or more, further 13N / 25mm or more, 15N / 25mm or more, 17N / 25mm or more, 19N / 25mm or more, 21N / 25mm or more, 23N / 25mm or more (for example, 25N / 25mm or more). 50 There is no particular upper limit to the adhesive strength N. In some embodiments, from the viewpoint of ease of production of the adhesive sheet and economic efficiency, 50 may be, for example, 70N / 25mm or less, 50N / 25mm or less, or 40N / 25mm or less.

[0133] Adhesive strength (N) measured after bonding to a stainless steel plate and keeping at 23°C for 30 minutes 23 is not particularly limited, and in some embodiments, the adhesive strength N 23 may be, for example, 3 N / 25 mm or less, preferably 2.5 N / 25 mm or less, more preferably less than 2 N / 25 mm, may be 1.5 N / 25 mm or less, may be 1.2 N / 25 mm or less, or may be 1 N / 25 mm or less. 23 A low adhesive strength N is preferable from the viewpoint of reworkability. 23 The lower limit of the adhesive strength N is not particularly limited, and may be, for example, 0.01 N / 25 mm or more. 23 In order to improve the adhesive strength after heating, it is usually appropriate that the adhesive strength N 23may be, for example, 0.2 N / 25 mm or more, 0.5 N / 25 mm or more, 0.8 N / 25 mm or more, or 1.0 N / 25 mm or more (for example, 1.5 N / 25 mm or more).

[0134] Adhesive strength (N) measured at 23°C after bonding to a stainless steel plate and holding at 80°C for 5 minutes 80 is not particularly limited, and in some embodiments, the adhesive strength N 80 may be, for example, 5 N / 25 mm or more, 7 N / 25 mm or more, 10 N / 25 mm or more, 13 N / 25 mm or more, 15 N / 25 mm or more, 17 N / 25 mm or more, 20 N / 25 mm or more, 25 N / 25 mm or more, or 30 N / 25 mm or more (e.g., 35 N / 25 mm or more). Also, from the viewpoint of ease of production and economic efficiency of the pressure-sensitive adhesive sheet, in some embodiments, the adhesive strength N 80 may be, for example, 70N / 25mm or less, 50N / 25mm or less, or 40N / 25mm or less.

[0135] Adhesive force N 23 Adhesive strength N against [N / 25mm] 50 [N / 25mm] ratio, i.e., adhesive strength increase ratio N 50 / N 23 is not particularly limited, and in some embodiments, N 50 / N 23 is suitably 2 or more (for example, 3 or more), preferably 5 or more, more preferably 8 or more, may be 10 or more, 12 or more, 15 or more, 18 or more, or 20 or more. 50 / N 23 A pressure-sensitive adhesive sheet with a large N exhibits good reworkability at the initial stage of application, and the adhesive strength can be significantly increased by subsequent heating or the like. 50 / N 23 The upper limit of N is not particularly limited, and is usually 100 or less, may be 80 or less, 60 or less, or may be 50 or less, and from the viewpoint of ease of production of the PSA sheet and economic efficiency, is typically 30 or less, and may be 20 or less.50 / N 23 may be, for example, 18 or less, 15 or less, or 12 or less.

[0136] Adhesive force N 50 Adhesive strength N against [N / 25mm] 80 [N / 25mm] ratio, i.e., adhesive strength increase ratio N 80 / N 50 is not particularly limited, and in some embodiments, N 80 / N 50 is suitably 3 or less, and preferably 2 or less, for example 1.8 or less, or 1.5 or less (for example 1.3 or less). With a pressure-sensitive adhesive sheet that satisfies this characteristic, the adhesive strength can be sufficiently increased by mild heating at about 50°C, and there is no need to expose the sheet to a higher temperature (specifically, heating to about 80°C) in order to obtain the desired adhesive strength. 80 / N 50 The lower limit is not particularly limited, and in some embodiments, from the viewpoint of ease of production of the PSA sheet and economic efficiency, it may be, for example, 1 or more, 1.2 or more, 1.4 or more, or 1.6 or more.

[0137] Here, the adhesive strength N 23 [N / 25mm] is determined by pressing the tape against a stainless steel (SUS) plate as an adherend, leaving it in an environment of 23°C and 50% RH for 30 minutes, and then measuring the 180° peel adhesive strength in the same environment (i.e., at 23°C) at a peel angle of 180° and a tensile speed of 300mm / min. Adhesive force N 50 [N / 25mm] is determined by pressing the tape against a stainless steel plate as an adherend, holding it in a 50°C environment for 15 minutes, and then leaving it in a 23°C, 50% RH environment for 30 minutes, and then measuring the 180° peel adhesive strength in the same environment at a peel angle of 180° and a tensile speed of 300mm / min. Adhesive force N 80[N / 25mm] is determined by pressing the tape against a stainless steel plate as the adherend, heating it at 80°C for 5 minutes, and then leaving it in an environment of 23°C and 50% RH for 30 minutes, and then measuring the 180° peel adhesive strength in the same environment at a peel angle of 180° and a tensile speed of 300mm / min. The adhesive strength of the adherend is N 23 ,N 50 ,N 80 In both measurements, SUS304BA plate is used. When making the measurements, if necessary, the pressure-sensitive adhesive sheet to be measured can be reinforced by attaching an appropriate backing material (for example, a PET film with a thickness of about 25 μm). Adhesive strength N 23 ,N 50 ,N 80 More specifically, it can be measured according to the method described in the Examples below.

[0138] The adhesive strength after heating of the adhesive sheet disclosed herein represents one characteristic of the adhesive sheet and does not limit the use of the adhesive sheet. In other words, the use of the adhesive sheet disclosed herein is not limited to the use of the adhesive sheet at 50°C for 15 minutes, and the adhesive sheet can be used in a mode in which heating to a temperature above room temperature (usually 20°C to 30°C, typically 23°C to 25°C) is not particularly performed. Even in such a use mode, the adhesive strength increases over the long term, and strong bonding can be achieved. In addition, the adhesive sheet disclosed herein can be heated at a temperature above 30°C (for example, 50°C) or higher at any timing after attachment to promote an increase in adhesive strength. The heating temperature in such a heat treatment is not particularly limited, and can be set in consideration of workability, economy, heat resistance of the substrate of the adhesive sheet or the adherend, and the like. The heating temperature may be, for example, less than 150°C, 120°C or less, 100°C or less, 80°C or less, or 70°C or less. The heating temperature can be, for example, 40°C or higher, 45°C or higher, 50°C or higher, 55°C or higher, 60°C or higher, or 70°C or higher, and may be 80°C or higher, or 100°C or higher. The heating time is not particularly limited, and may be, for example, 1 hour or less, 30 minutes or less, 10 minutes or less, or 5 minutes or less. The heating time may be, for example, 1 minute or more, 3 minutes or more, 7 minutes or more, or 15 minutes or more. Alternatively, the heating treatment may be performed for a longer period of time as long as no significant thermal deterioration occurs in the pressure-sensitive adhesive sheet or the adherend. The heating treatment may be performed all at once, or may be performed in multiple steps.

[0139] (Adhesive sheet with substrate) When the pressure-sensitive adhesive sheet disclosed herein is in the form of a pressure-sensitive adhesive sheet with a substrate, the thickness of the pressure-sensitive adhesive sheet may be, for example, 1000 μm or less, 600 μm or less, 350 μm or less, or 250 μm or less. In view of the miniaturization, weight reduction, thinning, etc. of the product to which the pressure-sensitive adhesive sheet is applied, in some embodiments, the thickness of the pressure-sensitive adhesive sheet may be, for example, 200 μm or less, 175 μm or less, 140 μm or less, 120 μm or less, or 100 μm or less (for example, less than 100 μm). In addition, in view of the handleability, etc., the thickness of the pressure-sensitive adhesive sheet may be, for example, 5 μm or more, 10 μm or more, 15 μm or more, 20 μm or more, 25 μm or more, or 30 μm or more. In some embodiments, the thickness of the pressure-sensitive adhesive sheet may be, for example, 50 μm or more, 60 μm or more, 80 μm or more, 100 μm or more, or 120 μm or more. There is no particular upper limit to the thickness of the pressure-sensitive adhesive sheet. The thickness of the adhesive sheet refers to the thickness of the portion attached to the adherend. For example, in the adhesive sheet 1 having the configuration shown in FIG. 1, the thickness refers to the thickness from the adhesive surface 21A of the adhesive sheet 1 to the second surface 10B of the substrate 10, and does not include the thickness of the release liner 31.

[0140] The pressure-sensitive adhesive sheet disclosed herein can be suitably implemented, for example, in an embodiment in which the thickness Ts of the support substrate is greater than the thickness Ta of the pressure-sensitive adhesive layer, that is, in an embodiment in which Ts / Ta is greater than 1. Although not particularly limited, Ts / Ta may be, for example, 1.1 or more, 1.2 or more, 1.5 or more, or 1.7 or more. For example, in a pressure-sensitive adhesive sheet that can be used for purposes such as reinforcing, supporting, and cushioning an adherend, an increase in Ts / Ta tends to make it easier to exhibit good effects even when the pressure-sensitive adhesive sheet is made thinner. In some embodiments, Ts / Ta may be 2 or more (e.g., greater than 2), 2.5 or more, or 2.8 or more. In addition, Ts / Ta may be, for example, 50 or less, or 20 or less. From the viewpoint of making it easier to exhibit high post-heating adhesive strength even when the pressure-sensitive adhesive sheet is made thinner, Ts / Ta may be, for example, 10 or less, 8 or less, or 5 or less.

[0141] The adhesive layer is preferably fixed to the support substrate. Here, the term "fixed" refers to the adhesive layer having sufficient anchoring properties to the support substrate to such an extent that, in an adhesive sheet whose adhesive strength has increased after being attached to an adherend, peeling does not occur at the interface between the adhesive layer and the support substrate when the adhesive sheet is peeled off from the adherend. A substrate-attached adhesive sheet in which the adhesive layer is fixed to the support substrate can firmly integrate the adherend and the support substrate. A preferred example of an adhesive sheet in which the adhesive layer is fixed to the substrate is an adhesive sheet in which peeling (anchor failure) does not occur between the adhesive layer and the support substrate when the adhesive strength after heating is measured as described above. An adhesive sheet having an adhesive strength of 15 N / 25 mm or more after heating and no anchor failure occurs when the adhesive strength after heating is measured is a preferred example of an adhesive sheet in which the adhesive layer is fixed to the substrate.

[0142] The adhesive sheet disclosed herein can be preferably produced by a method including, for example, contacting a liquid adhesive composition with a first surface of a substrate and curing the adhesive composition on the first surface to form an adhesive layer in this order. The curing of the adhesive composition can involve one or more of drying, crosslinking, polymerization, cooling, etc. of the adhesive composition. According to the method of curing a liquid adhesive composition on the first surface of a substrate to form an adhesive layer, the adhesive layer can be more anchored to the substrate than the method of placing the adhesive layer on the first surface by attaching the cured adhesive layer to the first surface of the substrate. By utilizing this, an adhesive sheet in which the adhesive layer is fixed to the substrate can be preferably produced.

[0143] In some embodiments, the method of contacting the liquid pressure-sensitive adhesive composition with the first surface of the substrate can be a method of directly applying the pressure-sensitive adhesive composition to the first surface of the substrate. By contacting the first surface (adhesive surface) of the pressure-sensitive adhesive layer cured on the first surface of the substrate with a release surface, a pressure-sensitive adhesive sheet can be obtained in which the second surface of the pressure-sensitive adhesive layer is fixed to the first surface of the substrate and the first surface of the pressure-sensitive adhesive layer is in contact with the release surface. The release surface can be the surface of a release liner, the back surface of a substrate that has been subjected to a release treatment, or the like.

[0144] In addition, for example, in the case of a photocurable pressure-sensitive adhesive composition using a partial polymer (polymer syrup) of a monomer raw material, the pressure-sensitive adhesive composition may be applied to a release surface, and then the applied pressure-sensitive adhesive composition may be covered with a first surface of a substrate to bring the uncured pressure-sensitive adhesive composition into contact with the first surface of the substrate, and in this state, the pressure-sensitive adhesive composition sandwiched between the first surface of the substrate and the release surface may be irradiated with light to cure it, thereby forming a pressure-sensitive adhesive layer.

[0145] The above-mentioned methods are not intended to limit the manufacturing method of the adhesive sheet disclosed herein. In manufacturing the adhesive sheet disclosed herein, any suitable method capable of adhering the adhesive layer to the first surface of the substrate can be used alone or in combination of two or more. Examples of such methods include the above-mentioned method of curing a liquid adhesive composition on the first surface of the substrate to form an adhesive layer, and the method of performing a surface treatment on the first surface of the substrate to enhance the anchoring property of the adhesive layer. For example, when the anchoring property of the adhesive layer to the substrate can be sufficiently improved by a method such as providing an undercoat layer on the first surface of the substrate, the adhesive sheet may be manufactured by laminating the cured adhesive layer to the first surface of the substrate. In addition, the anchoring property of the adhesive layer to the substrate can be improved by selecting the material of the substrate or the composition of the adhesive. In addition, the anchoring property of the adhesive layer to the substrate can be improved by applying a temperature higher than room temperature to an adhesive sheet having an adhesive layer on the first surface of the substrate. The temperature applied to enhance the anchoring property may be, for example, about 35°C to 80°C, about 40°C to 70°C or higher, or about 45°C to 60°C.

[0146] When the pressure-sensitive adhesive sheet disclosed herein is in the form of a pressure-sensitive adhesive sheet having a first pressure-sensitive adhesive layer provided on a first surface of a substrate and a second pressure-sensitive adhesive layer provided on a second surface of the substrate (i.e., a double-sided adhesive substrate-attached pressure-sensitive adhesive sheet), the first pressure-sensitive adhesive layer and the second pressure-sensitive adhesive layer may be of the same configuration or of different configurations. When the first pressure-sensitive adhesive layer and the second pressure-sensitive adhesive layer have different configurations, the difference may be, for example, a difference in composition or structure (thickness, surface roughness, formation area, formation pattern, etc.). For example, the second pressure-sensitive adhesive layer may be a pressure-sensitive adhesive layer that does not contain polymer B. In addition, the surface of the second pressure-sensitive adhesive layer (second adhesive surface) has an adhesive strength N 50 may be less than 5N / 25mm, may be less than 3N / 25mm, may be less than 1.5N / 25mm, or may be less than 1N / 25mm.

[0147] <Adhesive sheet with release liner> The adhesive sheet disclosed herein may take the form of an adhesive product in which the surface (adhesive surface) of an adhesive layer is in contact with the release surface of a release liner. Thus, this specification may provide an adhesive sheet with a release liner (adhesive product) that includes any of the adhesive sheets disclosed herein and a release liner having a release surface in contact with the adhesive surface of the adhesive sheet.

[0148] The thickness of the release liner is not particularly limited, but is usually about 5 μm to 200 μm. When the thickness of the release liner is within the above range, it is preferable because it is easy to attach to the adhesive layer and easy to peel from the adhesive layer. In some embodiments, the thickness of the release liner may be, for example, 10 μm or more, 20 μm or more, 30 μm or more, or 40 μm or more. In addition, from the viewpoint of facilitating peeling from the adhesive layer, the thickness of the release liner may be, for example, 100 μm or less, or 80 μm or less. The release liner may be subjected to a known antistatic treatment such as a coating type, a kneading type, or a deposition type, as necessary.

[0149] The release liner is not particularly limited, and for example, a release liner having a release layer on the surface of a liner substrate such as a resin film or paper (which may be paper laminated with a resin such as polyethylene), or a release liner made of a resin film formed from a low-adhesion material such as a fluorine-based polymer (polytetrafluoroethylene, etc.) or a polyolefin resin (polyethylene, polypropylene, etc.) can be used. Since the surface smoothness is excellent, a release liner having a release layer on the surface of a resin film as a liner substrate, or a release liner made of a resin film formed from a low-adhesion material can be preferably used. The resin film is not particularly limited as long as it is a film that can protect the adhesive layer, and examples thereof include a polyethylene film, a polypropylene film, a polybutene film, a polybutadiene film, a polymethylpentene film, a polyvinyl chloride film, a vinyl chloride copolymer film, a polyester film (PET film, PBT film, etc.), a polyurethane film, and an ethylene-vinyl acetate copolymer film. The release layer can be formed using known release agents such as silicone-based release agents, long-chain alkyl-based release agents, olefin-based release agents, fluorine-based release agents, fatty acid amide-based release agents, molybdenum sulfide, silica powder, etc. The use of silicone-based release agents is particularly preferred.

[0150] The thickness of the release layer is not particularly limited, but is usually about 0.01 μm to 1 μm, and preferably about 0.1 μm to 1 μm. The method for forming the release layer is not particularly limited, and a known method can be appropriately adopted depending on the type of release treatment agent used, etc.

[0151] <Application> The pressure-sensitive adhesive sheet provided by this specification can exhibit good reworkability, for example, in the initial stage after being attached to an adherend, and can contribute to suppressing a decrease in yield and improving the quality of products containing the pressure-sensitive adhesive sheet. The pressure-sensitive adhesive sheet can have a significantly increased adhesive strength by aging (which can be mild heating at about 50°C, aging, a combination of these, etc.). For example, by heating at a desired timing, the pressure-sensitive adhesive sheet can be firmly attached to the adherend. Taking advantage of these characteristics, the pressure-sensitive adhesive sheet disclosed herein can be preferably used in various fields for purposes such as fixing, joining, molding, decoration, protection, reinforcement, support, and shock mitigation of members contained in various products.

[0152] The pressure-sensitive adhesive sheet disclosed herein can be preferably used as a reinforcing film that is attached to an adherend and reinforces the adherend, for example, in the form of a substrate-attached pressure-sensitive adhesive sheet in which a pressure-sensitive adhesive layer is provided on at least the first surface of a film-like substrate having a first surface and a second surface. In such a reinforcing film, a film substrate that includes a resin film as a base film can be preferably used. In addition, from the viewpoint of enhancing reinforcing performance, it is preferable that the pressure-sensitive adhesive layer is fixed to the first surface of the film-like substrate. For example, optical components used in optical products and electronic components used in electronic products are becoming highly integrated, smaller, lighter, and thinner, and multiple thin optical / electronic components with different linear expansion coefficients and thicknesses may be stacked. By attaching the above-mentioned reinforcing film to such components, it is possible to impart appropriate rigidity to the optical / electronic components. This makes it possible to suppress curling and curvature caused by stress that may occur between multiple components with different linear expansion coefficients and thicknesses during the manufacturing process and / or in the manufactured product. Furthermore, in the manufacturing process of optical products / electronic products, in the situation where thin optical / electronic components are subjected to shaping processing such as cutting as described above, by attaching a reinforcing film to the components, local stress concentration on the optical / electronic components accompanying processing can be alleviated, and the risk of cracks, breakage, peeling of laminated components, etc. Attaching a reinforcing member to an optical / electronic component and handling it can also be useful for alleviating local stress concentration during transportation, stacking, rotation, etc. of the components, and for preventing bending or bending due to the weight of the components. Furthermore, in the case of devices such as optical products and electronic products including the above-mentioned reinforcement film, when the devices are used by consumers in the market, even if the devices are subjected to unintentional stress such as when the devices are dropped, placed under a heavy object, or hit by a flying object, the inclusion of the reinforcement film in the devices can reduce stress on the devices. Therefore, the inclusion of the reinforcement film in the devices can improve the durability of the devices.

[0153] In addition, the adhesive sheet disclosed herein may be preferably used in an embodiment in which it is attached to a member constituting various portable devices (portable devices). Here, "portable" does not mean that it is merely portable, but that it has a level of portability that allows an individual (average adult) to carry it relatively easily. Examples of portable devices herein include mobile phones, smartphones, tablet computers, notebook computers, various wearable devices, digital cameras, digital video cameras, audio devices (portable music players, IC recorders, etc.), calculators (calculators, etc.), portable game devices, electronic dictionaries, electronic organizers, electronic books, in-vehicle information devices, portable radios, portable televisions, portable printers, portable scanners, portable modems, and other portable electronic devices, as well as mechanical wristwatches, pocket watches, flashlights, hand mirrors, and the like. Examples of members constituting the above portable electronic devices may include optical films and display panels used in image display devices such as thin-layer displays such as liquid crystal displays and film-type displays. The adhesive sheet disclosed herein may also be preferably used in an embodiment in which it is attached to various members in automobiles, home appliances, and the like. EXAMPLES

[0154] Some examples of the present invention will be described below, but it is not intended that the present invention be limited to those specific examples. In the following description, "parts" and "%" are by weight unless otherwise specified.

[0155] (Preparation of Polymer A1) In a reaction vessel equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube and a cooler, 60 parts of 2-ethylhexyl acrylate (2EHA), 15 parts of N-vinyl-2-pyrrolidone (NVP), 10 parts of methyl methacrylate (MMA), 15 parts of 2-hydroxyethyl acrylate (HEA), and 200 parts of ethyl acetate as a polymerization solvent were charged, and the mixture was stirred for 2 hours under a nitrogen atmosphere at 60°C, after which 0.2 parts of 2,2'-azobisisobutyronitrile (AIBN) was added as a thermal polymerization initiator, and the reaction was carried out at 60°C for 6 hours to obtain a solution of polymer A1. The Mw of this polymer A1 was 1.1 million.

[0156] (Preparation of Polymer B1) Into a reaction vessel equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube and a cooler, 40 parts of MMA, 20 parts of n-butyl methacrylate (BMA), 20 parts of 2-ethylhexyl methacrylate (2EHMA), 8.7 parts of a polyorganosiloxane skeleton-containing methacrylate monomer having a functional group equivalent of 900 g / mol (trade name: X-22-174ASX, manufactured by Shin-Etsu Chemical Co., Ltd.), 11.3 parts of a polyorganosiloxane skeleton-containing methacrylate monomer having a functional group equivalent of 4600 g / mol (trade name: KF-2012, manufactured by Shin-Etsu Chemical Co., Ltd.), 100 parts of ethyl acetate, and 0.5 parts of thioglycerol as a chain transfer agent were added, and the mixture was stirred for 1 hour under a nitrogen atmosphere at 70 ° C., after which 0.2 parts of AIBN were added as a thermal polymerization initiator, and the mixture was reacted at 70 ° C. for 2 hours, after which 0.1 parts by weight of AIBN was added as a thermal polymerization initiator, and then the mixture was reacted at 80 ° C. for 5 hours. In this way, a solution of polymer B1 was obtained. The Mw of this polymer B1 was 2.2×10 4 It was.

[0157] (Preparation of Polymer B2) The same procedure as for the preparation of polymer B1 was repeated except that thioglycerol was not used, and a polymer with a molecular weight of 16.5×10 was obtained. 4 Thus, a solution of polymer B2 was obtained.

[0158] The weight average molecular weight of each of the above-mentioned polymers was measured under the following conditions using a GPC device (HLC-8220GPC, manufactured by Tosoh Corporation) and calculated in terms of polystyrene. [GPC conditions] Sample concentration: 0.2 wt% (tetrahydrofuran (THF) solution) Sample injection volume: 10μL ·Eluent: THF ·Flow rate: 0.6mL / min ·Measurement temperature: 40℃ ·column: Sample column: TSKguardcolumn SuperHZ-H (1 column) + TSKgel SuperHZM-H (2 columns) Reference column: TSKgel SuperH-RC (1 column) Detector: Differential refractometer (RI)

[0159] <Preparation of adhesive sheet> (Example 1) To a solution of polymer A1, 2 parts of polymer B1 and 0.5 parts of an isocyanate-based crosslinking agent (product name: Takenate D110N, trimethylolpropane xylylene diisocyanate, manufactured by Mitsui Chemicals) were added per 100 parts of polymer A1 contained in the solution, and the mixture was mixed uniformly to prepare a pressure-sensitive adhesive composition C1. The adhesive composition C1 was directly applied to the first surface of a 75 μm thick polyethylene terephthalate (PET) film (manufactured by Toray Industries, Inc., product name "Lumirror") as a supporting substrate, and dried by heating at 110°C for 2 minutes to form an adhesive layer having a thickness of 15 μm. The release surface of a release liner was attached to the surface (adhesive surface) of this adhesive layer. As the release liner, MRQ25T100 (a release liner having a release layer made of a silicone-based release treatment agent on one side of a polyester film, thickness 25 μm) manufactured by Mitsubishi Chemical Corporation was used. In this way, the adhesive sheet according to Example 1 was obtained in the form of an adhesive sheet with a release liner in which the release surface of the release liner was in contact with the adhesive surface of the release liner.

[0160] (Example 2 to Example 4) Pressure-sensitive adhesive compositions C2 to C4 were prepared in the same manner as for the preparation of pressure-sensitive adhesive composition C1, except that the type of polymer B or the amount of crosslinking agent used was changed as shown in Table 1. Pressure-sensitive adhesive sheets according to Examples 2 to 4 were obtained in the same manner as for the preparation of the pressure-sensitive adhesive sheet according to Example 1, except that these pressure-sensitive adhesive compositions C2 to C4 were used, respectively, in the form of pressure-sensitive adhesive sheets with release liner in which the release surface of a release liner abutted against the pressure-sensitive adhesive surface of the pressure-sensitive adhesive sheet.

[0161] <Storage modulus G´(150℃)> The storage modulus G' (150°C) of the adhesive layer was determined by dynamic viscoelasticity measurement. Specifically, the adhesive layer was formed under basically the same conditions as in each example, except that the adhesive layer was formed on the release surface of a release liner instead of a PET film, and a plurality of such adhesive layers were stacked to form an adhesive layer with a thickness of about 2 mm. The obtained adhesive layer was punched into a disk shape with a diameter of 7.9 mm, and the sample was sandwiched and fixed between parallel plates, and dynamic viscoelasticity measurement was performed under the following conditions using a viscoelasticity tester (for example, "ARES" manufactured by TA Instruments Co., Ltd. or an equivalent product) to determine the storage modulus G' (150°C). The adhesive layer to be measured may be formed by applying the corresponding adhesive composition in a layer on the release surface of a release liner or the like, and drying or curing it. Measurement mode: Shear mode Temperature range: -50℃~200℃ Heating rate: 5℃ / min ·Measurement frequency: 1Hz

[0162] <Measurement of adhesive strength (23℃)> The adhesive sheet according to each example was cut together with the release liner into a 25 mm wide specimen, which was used as a test piece. A SUS plate (SUS304BA plate) cleaned with toluene was used as the adherend, and the adhesive strength N was measured in the following manner. 23 , adhesive force N 50 and adhesive strength N 80 was measured. (Adhesive force N 23 Measurement of Under standard conditions of 23°C and 50% RH, the release liner covering the adhesive surface of each test piece was peeled off, and the exposed adhesive surface was pressed against the adherend by rolling a 2 kg roller back and forth once. The test piece thus pressed against the adherend was left for 30 minutes under the above-mentioned standard conditions, and then the 180° peel adhesive strength (resistance to the above-mentioned tension) was measured in accordance with JIS Z0237 using a universal tension and compression tester (apparatus name "Tension and Compression Tester, TCM-1kNB" manufactured by Minebea Co., Ltd.) at a peel angle of 180° and a tensile speed of 300 mm / min. The measurement was performed three times, and the average value was taken as the adhesive strength N. 23 The values ​​are shown in Table 1 as [N / 25mm]. (Adhesive force N 50 Measurement of The above adhesive strength 23 The test piece was pressed against the adherend in the same manner as in the measurement of (1), and then held in a 50°C environment for 15 minutes, and then left in the above-mentioned standard environment for 30 minutes, after which the 180° peel adhesive strength was measured in the same manner. The measurement was carried out three times, and the average of these measurements was taken as the adhesive strength N. 50 The values ​​are shown in Table 1 as [N / 25mm]. (Adhesive force N 80 Measurement of The above adhesive strength 23 The test piece was pressed against the adherend in the same manner as in the measurement of (1), heated at 80°C for 5 minutes, and then left to stand for 30 minutes under the above-mentioned standard environment, after which the 180° peel adhesive strength was measured in the same manner. The measurement was carried out three times, and the average of these measurements was taken as the adhesive strength N 80 The adhesive strength is shown in Table 1 as [N / 25mm]. Note that the adhesive sheets according to Examples 1 to 4 all had an adhesive strength of N 80 It was confirmed that no anchor destruction occurred during measurements.

[0163] Based on these adhesion measurement results, the adhesion increase ratio N 80 / N 50 and N 50 / N 23 The results are shown in Table 1.

[0164] [Table 1]

[0165] As shown in Table 1, the pressure-sensitive adhesive sheets according to Examples 1 to 4 have a pressure-sensitive adhesive layer containing polymer A and polymer B, which is a copolymer of a monomer having a polyorganosiloxane skeleton and a (meth)acrylic monomer, and all of them have an adhesive strength N of 5 N / 25 mm or more. 50 These pressure sensitive adhesive sheets show good reworkability in the initial stage of application, and it is found that the adhesive strength can then be increased to a predetermined value or higher by mild heating at about 50°C. Also, particularly good results were obtained in Examples 1 to 3, which used pressure sensitive adhesive layers with a storage modulus G'(150°C) at 150°C of 10,000 Pa or more and 90,000 Pa or less. Specifically, the adhesive strength N23 While keeping the adhesive strength N 50 was able to be further improved.

[0166] Although the specific examples of the present invention have been described in detail above, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and changes of the specific examples exemplified above. [Explanation of symbols]

[0167] 1,2,3 Adhesive sheet 10 Supporting base material 10A front page 10B Second side 21 Adhesive layer (first adhesive layer) 21A Adhesive surface (first adhesive surface) 21B Adhesive surface (second adhesive surface) 22 Adhesive layer (second adhesive layer) 22A Adhesive surface (second adhesive surface) 31,32 Release liner 100,200,300 Adhesive sheet with release liner (adhesive product)

Claims

1. A pressure-sensitive adhesive sheet comprising a pressure-sensitive adhesive layer, The pressure-sensitive adhesive layer includes a polymer A, a polymer B which is a copolymer of a monomer having a polyorganosiloxane skeleton and a (meth)acrylic monomer, and a crosslinking agent, The polymer A is an acrylic polymer having a glass transition temperature of less than 0° C. The acrylic polymer is a polymer containing 50% by weight or more of monomer units derived from an alkyl (meth)acrylate ester, The (meth)acrylic acid alkyl ester is a (meth)acrylic acid alkyl ester having a linear or branched alkyl group having 1 to 18 carbon atoms, The (meth)acrylic acid alkyl ester includes 2-ethylhexyl acrylate, the acrylic polymer further contains, as a copolymerizable monomer copolymerizable with the (meth)acrylic acid alkyl ester, a monomer unit derived from at least one copolymerizable monomer selected from a monomer having a nitrogen atom-containing ring and a hydroxyl group-containing monomer; The monomer having a polyorganosiloxane skeleton is represented by general formula (1) or (2): 【Chemistry 1】 【Chemistry 2】 (In the general formulas (1) and (2), R 3 is hydrogen or a methyl group, R 4 is a methyl group or a monovalent organic group, and m and n are integers of 0 or more.) A compound represented by the formula: The content of the polymer B in the pressure-sensitive adhesive layer is 0.5 parts by weight or more and 20 parts by weight or less with respect to 100 parts by weight of the polymer A, The crosslinking agent includes an isocyanate-based crosslinking agent, The content of the isocyanate-based crosslinking agent is 0.1 parts by weight or more and 0.8 parts by weight or less based on 100 parts by weight of the polymer A, the pressure-sensitive adhesive layer does not contain any polymer other than the polymer A and the polymer B, or contains a polymer other than the polymer A and the polymer B in an amount of 10% by weight or less of the total polymer components contained in the pressure-sensitive adhesive layer; The pressure-sensitive adhesive layer has a storage modulus G'(150°C) of 10,000 Pa or more and 50,000 Pa or less at 150°C, Adhesive strength (N) measured at 23°C after bonding to a stainless steel plate and holding at 50°C for 15 minutes 50 is 5N / 25mm or more, Adhesive strength (N) measured after bonding to a stainless steel plate and keeping at 23°C for 30 minutes 23 The adhesive force N 50 The ratio (N 50 / N 23 ) is 12 or less, The adhesive strength N 50 Adhesive strength to N 80 The ratio (N 80 / N 50 ) is 1.5 or less, wherein the adhesive strength N 80 is the adhesive strength (N) measured at 23°C after bonding to a stainless steel plate and holding at 80°C for 5 minutes. 80 It's an adhesive sheet.

2. The adhesive strength N 23 The pressure-sensitive adhesive sheet according to claim 1, wherein the tension is 3 N / 25 mm or less.

3. The ratio (N 50 / N 23 3. The pressure-sensitive adhesive sheet according to claim 1 , wherein the molecular weight ratio (Mg / m2) is 5 or more.

4. The pressure-sensitive adhesive sheet according to any one of claims 1 to 3, wherein the polymer A contained in the pressure-sensitive adhesive layer is chemically crosslinked.

5. The pressure-sensitive adhesive sheet according to any one of claims 1 to 4, wherein the weight average molecular weight of the polymer B is 100,000 or more.

6. The pressure-sensitive adhesive sheet according to any one of claims 1 to 4, wherein the weight average molecular weight of the polymer B is less than 80,000.

7. The pressure-sensitive adhesive sheet according to any one of claims 1 to 6, wherein the acrylic polymer contains a monomer unit derived from a monomer having the nitrogen atom-containing ring.

8. The pressure-sensitive adhesive sheet according to any one of claims 1 to 7, wherein the monomer components for preparing the polymer B contain, as the (meth)acrylic monomer, a monomer having a homopolymer glass transition temperature of 50°C or higher in a proportion of 60% by weight or less.

9. The pressure-sensitive adhesive sheet according to any one of claims 1 to 8, comprising a supporting substrate having a first surface and a second surface, the pressure-sensitive adhesive layer being laminated on at least the first surface of the supporting substrate.

Citation Information

Patent Citations

  • DNA, recombined DNA, host polypeptide containing them and manufacture

    JP1983090596A

  • Premixing device for gasious fuel

    JP1984051153A

  • Adhesive composition, adhesive layer and adhesive sheet

    JP2014224227A

  • Adhesive sheet

    JP2019094385A

  • Adhesive sheet

    WO2018092904A1