Method for depositing material onto a substrate
The remote plasma sputtering method addresses the challenges of controlling plasma deposition by optimizing working distance and pressure to form crystalline films with enhanced battery performance on flexible substrates.
Patent Information
- Application Number
- JP2022528178
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-11-15
- Filing Date
- 2020-11-13
- Publication Date
- 2024-09-24
- Estimated Expiration
- 2040-11-13
AI Technical Summary
The deposition of materials using plasma deposition is challenging due to the difficulty in controlling the process to achieve the required properties and structure of the deposited material on the substrate, often resulting in undesirable outcomes such as substrate damage and formation of high-energy oxide states.
A method of depositing materials using plasma sputtering techniques where a plasma is generated remotely from the target, with a controlled working distance and pressure to optimize the adatom energy, allowing for the formation of crystalline films without annealing steps, particularly suited for layered oxide structures.
This method enables the formation of crystalline films with desirable properties, such as layered oxide structures, which enhance the performance of solid-state batteries by facilitating faster charging and higher capacity, while using flexible substrates like PET or PEN without substrate deformation.
Smart Images

Figure 0007555408000018 
Figure 0007555408000043 
Figure 0007555408000013
Abstract
Description
[Technical field]
[0001] The present invention relates to the deposition of material onto a substrate. More particularly, but not by way of limitation, the present invention relates to a method for depositing material onto a substrate. The present invention also relates to a method for determining an optimum operating distance and / or optimum operating pressure for a remote plasma deposition system, a method for manufacturing a battery, and the battery. [Background technology]
[0002] Deposition of materials using plasma deposition is well known to those skilled in the art. In certain circumstances, such deposition can be difficult to control and optimization of deposition conditions is desired to ensure that the material deposited on the substrate has the required properties and / or structure. The present invention seeks to alleviate the above problems. Alternatively or additionally, the present invention seeks to provide an improved method of depositing materials. Summary of the Invention
[0003] The present disclosure relates to methods of depositing materials using plasma sputtering techniques.
[0004] More specifically, the present disclosure relates to a method for depositing materials using plasma sputtering techniques, where the plasma is generated remote from the material being sputtered.
[0005] According to a first aspect of the present invention there is provided a method of depositing material on a substrate, the method comprising: generating a plasma remote from one or more plasma targets suitable for plasma sputtering, wherein at least one distinct region of the one or more targets comprises an alkali metal, an alkaline earth metal, an alkali metal-containing compound, an alkaline earth metal-containing compound, or a combination thereof; exposing one or more plasma targets to a plasma thereby sputtering material from the one or more targets; Depositing a sputtered material on a substrate, the working distance between the target and the substrate being: system This includes being within + / - 50% of the theoretical mean free path of the
[0006] Without wishing to be bound by theory, it is believed that the working distance affects the "adatom" energy of the sputtered material as it is deposited on the substrate. system It is believed that if the working distance is longer than the mean free path of , the ions in the sputtering flux will have a higher chance of colliding with each other before reaching the substrate, resulting in a relatively low adatom energy. system If the mean free path of the adatom is shorter than 0.1, the adatom energy will be relatively high.
[0007] The definition of mean free path is the average distance traveled by ions in a plasma from one collision to the next. The mean free path is calculated based on the interaction volume (which varies with the working distance) and the number of molecules per unit volume (which varies with the working pressure).
[0008] The working distance is arbitrary. system 50% to 150% of the theoretical mean free path of system 70% to 120% of the theoretical mean free path of system This is 80% to 100% of the theoretical mean free path.
[0009] The working distance is optionally 3.0 cm or more, optionally 4.0 cm or more, optionally 5.0 cm or more, optionally 6.0 cm or more, optionally 7.0 cm or more, and optionally 8.0 cm or more. The working distance is optionally 20 cm or less, optionally 15 cm or less, optionally 13 cm or less, optionally 12.0 cm or less, optionally 10.0 cm or less, and optionally 9.0 cm or less. The working distance between the target and the substrate is optionally 3.0 cm to 20.0 cm, optionally 4.0 cm to 15.0 cm, optionally 5.0 cm to 13.0 cm, optionally 6.0 cm to 12.0 cm, optionally 7.0 cm to 10.0 cm, and optionally 8.0 cm to 9.0 cm.
[0010] The working distance may be less than the mean free path of the sputtered material.
[0011] Without wishing to be bound by theory, if the working distance is too short, the energy of the sputtered material may be high enough to deform or damage the substrate. Such high energy sputter flex may also cause the formation of undesirable high energy oxide states due to plasma induced induction during the sputter flex. Desirably, the working distance is longer than a lower limit defined by when substrate damage and / or the formation of undesirable oxide states is observed.
[0012] The working distance may be from 3.0 cm to 20.0 cm.
[0013] The working distance may be from 5.0 cm to 15 cm, within which the material may be deposited with relatively high adatom energies and with fewer undesirable oxidized compounds formed in the film.
[0014] The working distance may be from 6.0 cm to 14.0 cm. The working distance may be from 7.0 cm to 13.0 cm.
[0015] The working distance may be between 8.0 cm and 12.0 cm, within which crystalline materials occur in primary crystallite platelets, particularly layered oxide materials.
[0016] The working distance may be 8.0 cm to 9.0 cm, within which a higher proportion of the crystalline material is of the layered oxide structure.
[0017] The operating pressure may be defined as the chamber pressure prior to ignition of the remote plasma. The operating pressure may be constant throughout the deposition process or may vary slightly as the target is unloaded or consumed during deposition. .
[0018] Applicants have found that it is possible to form a crystalline film of a material directly on a substrate. By "directly" it is meant that the film forms a crystalline film substantially without an annealing step. This has been shown to be true even for materials that form high energy crystalline structures that otherwise require an annealing step. This method has been shown to be effective for a wide range of substrate materials.
[0019] In a remote plasma system, the plasma is generated away from the plasma target. In conventional plasma deposition, it is the bias of the target that creates and maintains the plasma. In a remote plasma deposition system, the plasma is generated elsewhere and then directed to the target by various electric and / or magnetic fields. The bias of the target allows for control of the sputtering rate.
[0020] The deposited material may be crystalline. At least a portion of the deposited material, and optionally the entire deposited material, may have a hexagonal crystal structure. At least a portion of the deposited material, and optionally the entire deposited material, may have a crystalline "layered oxide" structure. Such a "layered oxide" structure is important when fabricating solid-state batteries. The layered oxide structure allows the alkali metal ions to more easily deintercalate from the crystal structure, resulting in faster charging, higher capacity solid-state batteries.
[0021] The layered oxide framework may generally be defined by the formula ABO2, where A is typically an alkali metal ion, an alkaline earth metal ion or a mixture, and B is typically one or more redox active transition metals, one or more transition metals or a mixture thereof. Metal elements of the so-called "post-transition metal" group, such as aluminum, may also be included in the layered oxide framework.
[0022] The advantage of forming a crystalline material without the need for an annealing step is that a relatively low melting point substrate can be used. The substrate may comprise a polymer. The substrate may be flexible. The substrate may comprise polyethylene terephthalate (PET) or polyethylene naphthalate (PEN). PEN and PET are semi-crystalline in structure and therefore fairly flexible and have relatively high tensile strength. During the plasma deposition process, the temperature of the substrate may not exceed 200 degrees at any point.
[0023] The deposition may occur in a reactive atmosphere that includes oxygen.
[0024] The operating pressure is optionally 0.0005mBar or more, optionally 0.00065mBar or more, optionally 0.0010mBar or more, optionally 0.0020mBar or more, optionally 0.0030mBar or more, optionally 0.0040mBar or more, and optionally 0.0045mBar or more. The operating pressure is optionally 0.0100mBar or less, optionally 0.0090mBar or less, optionally 0.0080mBar or less, optionally 0.0070mBar or less, and optionally 0.0065mBar or less. The operating pressure is optionally from 0.0005mBar to 0.0100mBar, optionally from 0.0020mBar to 0.0090mBar, optionally from 0.0030mBar to 0.0080mBar, optionally from 0.0040mBar to 0.0070mBar, and optionally from 0.0045mBar to 0.0065mBar.
[0025] The operating pressure may be from 0.0010 mBar to 0.0065 mBar. Higher operating pressures within this range may result in higher deposition rates because they result in more bombardment of process ions (usually Ar+) on the surface of the target, and therefore material is sputtered from the target at a faster rate.
[0026] When the operating pressure is between 0.0010 mBar and 0.0065 mBar, the crystal size (size of the crystal platelets) of the resulting crystalline material can be between 8 nm and 65 nm. Larger crystal sizes usually result in a thin film with a higher percentage of ordered material, since a lower percentage of the film is composed of material with irregular grain boundaries. This is important for thin film batteries, since larger crystal sizes usually result in a thin film battery with a higher usable capacity. Crystal sizes within this range can be observed when the alkali metal-containing material optionally includes at least one of the following compounds (described here with non-specific stoichiometry): LiCoO, LiCoAlO, LiNiCoAlO, LiMnO, LiNiMnO, LiNiMnCoO, LiNiO, LiNiCoO.
[0027] A narrower range of crystal sizes can be obtained using a working pressure of 0.0010 mBar to 0.0065 mBar when the working distance is 8.0 to 9.0 cm. The crystal size can be 14 nm to 25 nm. This is evidence that within these parameters, it is possible to form a narrow, predictable thin film range of films. This can be important because it can make the deposition step more predictable and repeatable on an industrial scale.
[0028] Without wishing to be bound by theory, it is believed that the layered oxide structure requires a high activation energy to form. system Therefore, there may be a lower limit for the operating pressure, below which the desired layered oxide structure does not occur. system The operating pressure must be above the lower limit defined by the pressure at which the desired layered oxide structure does not form, so that there is sufficient activation energy for the desired layered oxide structure to form within the range of 1000 to 2000 K. For example, when the alkali metal-containing compound is LiCoO2, the characteristic X-ray diffraction peak for the layered oxide structure appears at 19 degrees 2θ (related to the (003) plane). system If the operating pressure is too low, the desired layered oxide structure may not develop and this characteristic peak may not appear.
[0029] The operating pressure is 1.2e -3 Preferably, the operating pressure is 4.6e -3 It may be mBar or more.
[0030] At high operating pressures, the substrate may begin to be damaged. system The energy in the plasma may be high. Damage may be caused by plasma induced temperature increases. Preferably, the operating pressure is below an upper limit, the upper limit being defined by the pressure at which observable damage is caused to the substrate. Preferably, the operating pressure is below 0.0065 mBar.
[0031] When present, the alkali metal may be preferably one or more of Li, Na, K, Cs, Rb, optionally one or more of Li, Na or K, optionally Li or Na, and optionally Li. Lithium ions are sometimes used as the conductive species in the cathode of solid-state batteries. When present, the alkaline earth metal may optionally be one or more of magnesium, calcium, strontium or barium, optionally one or more of magnesium, calcium and barium, and optionally one or both of magnesium and calcium.
[0032] The one or more transition metals and / or the one or more redox-active transition metals may be from Period 4, Period 5 of the Periodic Table. The following description relates to transition metals that may be redox-active or transition metals that may not be redox-active. At least one transition metal, and optionally each transition metal, may optionally be selected from the group consisting of Fe, Co, Mn, Ni, Ti, Nb, and V.
[0033] The material to be deposited on the substrate has the empirical formula A a M1 b M2 cO2, where A is an alkali metal (optionally lithium), M1 is one or more transition metals (optionally one or more of cobalt, nickel, niobium, vanadium, and manganese) (b is the total number of transition metals), M2 is aluminum, a is 0.5 to 1.5, and z is 0 to 0.5.
[0034] Optionally, a is 1, b is 1, and c is 0. Optionally, M1 is one of cobalt, nickel, vanadium, niobium, and manganese.
[0035] Optionally, a is greater than 1 and A is lithium. In this case, the material is sometimes known as a "lithium-rich" material. Such lithium-rich materials include: [ka] For example, x=0, 0.06, 0.12, 0.2, 0.3 and 0.4.
[0036] Other such materials include [ka] where y is greater than 0.12 and less than or equal to 0.4.
[0037] Other such materials include [ka] In the formula, x is a value between 0.175 and 0.325, and y is a value between 0.05 and 0.35.
[0038] [ka] are other such materials, where x is 0 to 0.4, y is 0.1 to 0.4, and z is 0.02 to 0.3.
[0039] The alkali metal containing material may include lithium. The alkali metal containing material may include at least one of the following compounds (described herein with non-specific stoichiometry): LiCoO, LiCoAlO, LiNiCoAlO, LiMnO, LiNiMnO, LiNiMnCoO, LiNiO, and LiNiCoO.
[0040] The method includes moving the substrate and depositing the sputtered material onto the substrate, thereby forming material on the substrate. For example, material may be deposited onto a first portion of the substrate, then the substrate may be moved and material may be deposited onto a second portion of the substrate.
[0041] This facilitates the production of relatively large areas of material in a fairly short period of time.
[0042] The substrate may comprise or be in the form of a sheet, optionally elongated, sheet. Such a sheet may be provided in roll or stack format. Preferably, the substrate is provided as a roll. This facilitates simple and safe storage and handling of the substrate.
[0043] The substrate may be movably mounted to facilitate movement of the (optionally sheet-like) substrate. The substrate may be incorporated in a roll-to-roll arrangement. Upstream of the plasma deposition process, the substrate is held on a roller or drum. Downstream of the plasma deposition process, the substrate is held on a roller or drum. This facilitates simple and rapid manipulation of flexible sheets of substrate. Shutters may be provided to allow exposure of portions of the substrate to a remotely generated plasma.
[0044] There are many advantages to using a roll-to-roll arrangement, where sequential depositions are performed on a first portion of the substrate, followed by a second portion of the substrate, etc. This facilitates high material throughput and allows for large material areas to be deposited on one large substrate. One of the main advantages of roll-to-roll processing is that many depositions can occur without breaking vacuum. This saves time and energy compared to systems where the chamber must be returned to atmospheric pressure from vacuum after deposition in order to load a new substrate.
[0045] The upstream drum or rollers carrying the substrate may be located inside the process chamber or outside the chamber, and the downstream drum or rollers carrying the substrate may be located inside the chamber or outside the chamber.
[0046] The substrate may be provided in individual sheets that are handled and stored in a relatively flat sheet. The substrate may be in a planar form for depositing material thereon. This may be the case when the substrate is provided in individual sheets and not transported to and from a roll. The sheets may each be fixed on a carrier with greater structural rigidity. This may allow for thinner substrates to be used than if the substrate film was held on a roller. The substrate may be a sacrificial substrate. The substrate may be removed before the layer of material. Part or all of the substrate may be removed before incorporating the crystalline layer or a portion thereof into an electronic product package, component or other end product. For example, the layer of crystalline material may break away from the substrate. There may be another layer of intervening material between the base substrate and the crystalline material. This layer may break away from the crystalline material or aid in the separation of the crystalline material from the base substrate. Laser-based lift-off techniques may be used. The substrate may be removed by a process utilizing laser ablation.
[0047] Similar techniques are described in the prior art, for example in KR20130029488 which describes a method for making a battery that includes using a sacrificial substrate and a laser beam to obtain the battery layer. In other examples, other suitable processing regimes are used, provided that a sufficiently high product throughput is possible.
[0048] The substrate cannot exceed its temperature corrected yield strength at any point as it passes between the upstream and downstream rollers or drums. This is important because the roll-to-roll processing equipment needs to tension the substrate as it is transported through the various rolls, rollers, and drums. As the polymer warms up, the yield strength may begin to decrease. If the polymer heats up too much, it may begin to deform as it passes through the roll-to-roll equipment. This can lead to warping, clogging, and uneven deposition on the substrate. There is a gender.
[0049] The temperature of the substrate during the deposition process is optionally 500° C. or less, optionally 300° C. or less, optionally 200° C. or less, optionally 150° C. or less, optionally 120° C. or less, and optionally 100° C. or less. The methods of the present invention may be carried out at lower temperatures, which facilitate the use of substrates and other materials that cannot be used at higher temperatures. Additionally, at higher temperatures, substrate manipulation may be more difficult.
[0050] Measured on the surface opposite to the surface on which the material is deposited, averaged over 1 second, with an area of 1 cm 2 The maximum temperature reached on any given square of substrate material at any one time may be 500°C or less, optionally 300°C or less, optionally 200°C or less, optionally 150°C or less, optionally 120°C or less, and optionally 100°C or less.
[0051] At the end of the method, the thickness of the deposited alkali metal-containing compound is optionally 10 microns or less, optionally 1.0 micron or less.
[0052] The thickness of the substrate is optionally 1.6 microns or less. The thickness of the substrate as provided is optionally less than 1.0 microns.
[0053] When designing a solid-state battery on a substrate, it is beneficial to make it as thin as possible. This allows for the production of batteries with higher energy density. Preferably, a thinner substrate can be used, and if the thinner substrate meets the necessary conditions of relatively high temperature-corrected yield strength and high decomposition point, this substrate will be used in the present method. When the alkali metal-containing compound is LiCoO2, the crystals are optionally aligned with (101) and (110) planes substantially parallel to the substrate. This is beneficial because it means that the ion channels of the thin film are oriented perpendicular to the substrate, making it easier to intercalate and deintercalate ions from the battery. This improves the working capacity and charging speed of the battery.
[0054] The substrate optionally includes a current collecting layer. The current collecting layer may include an inert metal. The current collecting layer may be platinum. The current collecting layer may be nickel. The current collecting layer may be gold. The current collecting layer may be platinum. The current collecting layer may be aluminum. The current collecting layer may have a modified structure to increase the surface area. The current collecting layer may also act as an anode.
[0055] The deposition rate may be greater than 4 Å s. The deposition rate may be greater than 250 Å s. The deposition rate may be greater than 1000 Å s.
[0056] The method may include providing a first target and a second target, the target materials of the first target and the second target may optionally be different, and the orientations of the first target and the second target relative to the substrate may be different from one another.
[0057] The method may include exposing a first target to a plasma and exposing a second target to the plasma, thereby sputtering material from the first target and the second target. A substrate may be exposed to the sputtered material from the first target and the second target. The sputtering of material from the first target may generate a first plume corresponding to particle trajectories from the first target assembly to the substrate. The sputtering of material from the second target may generate a second plume corresponding to particle trajectories from the second target assembly to the substrate. The first plume and the second plume may focus at the substrate. One of the first target and the second target receives more plasma energy than the other of the first target and the second target. The first and second targets may be configured such that the energy required to sputter a material of the first target or the second target is greater than the energy required to sputter a material of the other of the first target or the second target. For example, if the first target includes elemental lithium and the second target includes cobalt, the first and second targets are configured such that the second target receives more plasma energy than the first target because cobalt requires more energy to sputter from the target than lithium.
[0058] The method includes containing and shaping the plasma using magnetic and / or electric fields such that the shape of the electron density distribution of the plasma is the same for every cross-sectional area across a majority of the width of the plasma, within a margin of error, which may optionally be up to 30%, optionally up to 20%, optionally up to 10%, and optionally up to 5%.
[0059] The shape of the electron density distribution of the plasma is identical, optionally within a margin of error. This can be tested using visual inspection, where the visible glow is substantially identical along the width of the plasma. The plasma may be blanket-like. In this regard, the width and length of the visible plasma cloud may each be at least five times greater than the thickness. The generation of the plasma may be performed by at least one antenna extending in a direction parallel to the width of the substrate. The generation of the plasma may be performed using a pair of antennas spaced a distance L apart on either side of the plasma, each antenna having a length W. The thickness of the plasma (defined either by the maximum extent of the glow in the visible spectrum or the maximum distance measured in a direction substantially perpendicular to both L and W that covers 90% of the free electrons in the plasma).
[0060] The first target or the second target may be closer to the plasma than the other of the first target and the second target, and such an arrangement may facilitate the first target or the second target receiving more plasma energy than the other of the first target and the second target.
[0061] The first target and the second target may be angled differently relative to the horizontal than the other of the first target and the second target for any given cross-section taken across most of the width of the plasma. Such an arrangement may encourage the first target or the second target to receive more plasma energy than the other of the first target and the second target.
[0062] One or both of the first target and the second target may be planar.
[0063] For any given cross-section taken across most of the width of the plasma, the targets of the second target assembly contribute substantially the same amount of material to the plasma as the targets of the first target assembly.
[0064] One or more targets are optionally facing the substrate, such an arrangement being advantageous when the plasma is generated remotely.
[0065] The surface on which the material is deposited is X S or less, where X S = 100 nm, and the deposited layer may have a thickness of 0.01 μm to 10 μm and a surface roughness of less than or equal to X1, where X1 is the sum of F and X S where F is a coefficient ranging from 1 to 2.
[0066] X S may be 10% or less of the thickness of the substrate. S The product of is 10 5 nm 2 It may be the following.
[0067] The substrate, optionally a polymeric substrate, may be provided with embedded particles and all of the embedded particles in and on the polymeric material, the majority of which contribute to the surface roughness of the substrate being less than X. S The median diameter is 10% to 125% of the mean diameter.
[0068] Alternatively, the substrate, optionally a polymeric substrate, may be provided with embedded particles and all of the embedded particles in and on the polymeric material, the majority of which contribute to the surface roughness of the substrate being less than X. S The median diameter is 150% or less of the above.
[0069] This method uses sputter deposition to deposit material on a surface, with thickness and x of 0.01 μm to 10 μm. S forming a further layer having a surface roughness of 150% or less, wherein the composition of the material of the crystalline layer is different from the composition of the material of the further layer.
[0070] The method may include plasma sputtering material onto a surface of the substrate or a surface supported by the substrate from a first target comprising an alkali metal or alkaline earth metal, wherein there is a first plume corresponding to particle trajectories from at least the first target to the surface, and plasma sputtering material onto the surface from a second target comprising a transition metal (such as cobalt), wherein there is a second plume corresponding to particle trajectories from at least the second target to the surface, wherein the first target is positioned non-parallel to the second target, and wherein the first plume and the second plume converge in a region proximate the surface of the substrate or a surface supported by the substrate, and optionally a crystalline layer is formed on the surface in said region.
[0071] More plasma energy may be received at the first target than at the second target.
[0072] The first target may face towards the substrate in a first direction and the second target may face towards the substrate in a second direction, the first direction and the second direction converging towards the substrate.
[0073] A notional line extending from a center of a surface of a first target and parallel to a first direction may intersect, in a cross-sectional view, a notional line extending from a center of a surface of a second target and parallel to a second direction at a location closer to the substrate than one of the targets, and the location of the intersection may be closer to the substrate than half of the shortest distance from one of the targets to the substrate.
[0074] At least one of the substrate, the first target and the second target may optionally be moved such that a crystalline layer is formed on the surface.
[0075] The substrate may have a radius of curvature in the region where the first and second plumes converge, with the targets disposed about a center of the radius of curvature.
[0076] According to a second aspect of the present invention, there is provided a method for determining an optimal operating distance of a remote plasma deposition system configured for deposition of a layered oxide material, the method comprising: Selecting a range of working distances, system selecting a range of working distances such that the theoretical mean free path of the carrying out a method according to the first aspect of the invention for a number of test samples at different working distances within a selected range for each sample; performing X-ray diffraction on each test sample after deposition has occurred; identifying a sample for which diffraction peaks characteristic of a layered oxide structure are present; From these samples, the sample with the highest (normalized) intensity of the characteristic peak was selected and then the intensity was calculated for the working distance used during the deposition of the test sample. system and selecting a working distance of
[0077] The test sample of the method may optionally be replaced by an average value of multiple test samples, including multiple test samples in which the method of the first aspect of the invention is performed multiple times at the same working distance and averaged, and the method may include any standard error analysis technique known to those skilled in the art.
[0078] This method may be optionally performed multiple times to find the optimum range of working distances for operating the system.
[0079] According to a third aspect of the present invention, there is provided a method for determining an optimum operating pressure range for a remote plasma deposition system configured for deposition of a layered oxide material, the method comprising: selecting an initial range of operating pressure from 0.00065mBar to 0.01mBar (optionally between 0.001mBar and 0.007mBar); carrying out a method according to the first aspect of the invention for a number of test samples at different operating pressures within a selected range, for each sample; performing X-ray diffraction on each test sample after deposition has occurred; selecting a test sample from the group of test samples exhibiting characteristic x-ray diffraction peaks of the layered oxide material that was deposited at the lowest operating pressure and defining this operating pressure as the lower limit of the range; From the group of test samples that show no observable signs of damage to the substrate, select the test sample deposited at the highest operating pressure and define this operating pressure as the upper limit of the range.
[0080] The initial range of operating pressures may be selected according to the selection of operating pressures described above with respect to the method of the present invention. The test sample of the method may optionally be replaced by an average value of multiple test samples, including multiple test samples in which the method of the first aspect of the invention is performed multiple times at the same operating pressure and averaged. The method may include any standard error analysis technique known to one skilled in the art.
[0081] This method is within the desired range system The method may further include selecting an optimal operating pressure of 100 to 200 MPa. The optimal operating pressure may be an operating pressure within the range that results in the fastest deposition rate. It should of course be understood that features described in connection with one aspect of the invention may be incorporated in other aspects of the invention. [Brief description of the drawings]
[0082] Embodiments of the invention will now be described, by way of example only, with reference to the accompanying schematic drawings, which are briefly summarised below. [Figure 1a] FIG. 2 is a schematic side view of a plasma deposition chamber used in accordance with a first example. [Figure 1b] 3 illustrates steps of a method for manufacturing a battery cathode according to a first example. [Figure 1c] 1A-1D are schematic diagrams of cross sections of various polymer substrate materials. [Figure 1d] 1A-1D are schematic diagrams of cross sections of various polymer substrate materials. [Figure 1e] 1A-1D are schematic diagrams of cross sections of various polymer substrate materials. [Figure 1f]1A-1D are schematic diagrams of cross sections of various polymer substrate materials. [Figure 1g] 1A-1D are schematic diagrams of cross sections of various polymer substrate materials. [Figure 1h] 1A-1D are schematic diagrams of cross sections of various polymer substrate materials. [Figure 2a] FIG. 13 is a schematic side view of a plasma deposition chamber used in accordance with the method of the second example. [Figure 2b] 1 is an X-ray diffraction (XRD) spectrum of a first sample of a battery cathode made according to the method of the second example. [Figure 2c] FIG. 2b is a Raman spectrum of the battery cathode from which the XRD data was obtained. [Figure 2d] 1 is an XRD spectrum of a second sample of a battery cathode made according to the method of the second example. [Figure 2e] FIG. 2d is a Raman spectrum of the battery cathode from which the XRD data was obtained. [Figure 3a] FIG. 13 is a schematic side view of a plasma deposition chamber used in a method according to a third example. [Figure 3b] FIG. 3b is a schematic plan view of the plasma deposition chamber shown in FIG. 3a. [Figure 3c] FIG. 4 is a further schematic side view of the plasma deposition chamber shown in FIGS. 3a and 3b. [Figure 3d] 1 is a graph comparing the sputtering yields of cobalt and lithium as a function of energy. [Figure 3e] FIG. 11 is a schematic side view of a plasma deposition chamber used in a method according to a fourth example. [Figure 4a] 1 is a cross-sectional scanning electron micrograph of a battery cathode relating to a first sample made according to the method of the second example. [Figure 4b] FIG. 13 is a perspective view of a scanning electron microscope photograph of a battery cathode relating to a second sample made according to the method of the second example. [Figure 5a] FIG. 11 is a schematic cross-sectional view of a battery cathode associated with a first sample fabricated using the method of the fifth example. [Figure 5b] FIG. 11 is a schematic cross-sectional view of a battery cathode associated with a second sample made using the method of the fifth example. [Figure 5c] 5 illustrates method steps for manufacturing a half-cell of a battery cathode according to a fifth example. [Figure 6] FIG. 13 is a schematic diagram of an example of a method for making a battery according to the sixth example. [Figure 7a] FIG. 13 is a schematic diagram of an example of a method for manufacturing a solid-state thin-film battery according to a seventh example. [Figure 7b] FIG. 13 is a schematic cross-sectional view of a solid-state thin-film battery according to a first sample of a seventh example. [Figure 7c] FIG. 13 is a schematic cross-sectional view of a solid-state thin-film battery sample fabricated according to the second sample of the seventh example. [Figure 8a] FIG. 13 is a schematic diagram of a method for determining an optimal working distance of a remote plasma deposition system configured to deposit a layered oxide material according to an eighth example. [Figure 8b] FIG. 8a shows a number of X-ray diffraction spectra collected as part of the method, where the characterization technique is X-ray diffraction and the distinctive features are characteristic X-ray diffraction peaks associated with a layered oxide structure. [Figure 9a] 1 is a micrograph of a membrane sample formed according to a first example of the invention. [Figure 9b] FIG. 9a is an X-ray diffraction spectrum obtained from the film shown in FIG. [Figure 10a] FIG. 13 is a schematic diagram of an example method for determining an optimal operating pressure for a remote plasma deposition system configured to deposit a layered oxide material according to a ninth example. [Figure 10b] FIG. 10a shows two X-ray diffraction spectra collected as part of the method described with respect to FIG. 10a, where the characterization technique is X-ray diffraction and the distinctive features are characteristic X-ray diffraction peaks associated with a layered oxide structure. [Figure 11a] 13 is an example of a method step for determining the crystallite size of a layered oxide material according to a tenth example. [Figure 11b]13 is a graph showing how to determine crystal size at different operating pressures according to the tenth example for a working distance of 16 cm, showing the crystal size of several films deposited according to the first example. [Figure 11c] 13 is a graph showing how to determine crystal size at different operating pressures according to the tenth example for a working distance of 8.5 cm, showing the crystal size of several films deposited according to the first example. [Figure 12] FIG. 15 is a schematic diagram of a method for depositing material on a substrate according to an eleventh embodiment of the invention. [Figure 13] FIG. 15 is a schematic diagram of an example method for manufacturing a component of an electronic device according to a twelfth example. [Figure 14] FIG. 23 is a schematic diagram of an example of a method for manufacturing a component of an electronic device according to a thirteenth embodiment of the invention. [Figure 15] 14 is a schematic diagram of an example of a method for manufacturing a light emitting diode (LED) according to a fourteenth embodiment of the invention. [Figure 16] FIG. 23 is a schematic diagram of an example of a method for manufacturing a permanent magnet according to a fifteenth example of the invention. [Figure 17] FIG. 2 is a schematic diagram of an example of a method for manufacturing an electronic device comprising a layer of indium tin oxide (ITO) according to a sixteenth embodiment of the invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0083] Figure 1a is a schematic side view of a plasma deposition process apparatus for use in a method of depositing (crystalline) material on a substrate according to a first method. The method is generally given by reference numeral 1001 and is shown diagrammatically in Figure 1b and comprises generating 1002 a plasma remote from one or more targets, exposing 1003 one or more targets to the plasma such that target material is sputtered from the one or more targets, and exposing 1004 a first portion of a substrate to the sputtered material such that the sputtered material is deposited on the first portion of the substrate, thereby forming a crystalline material on the first portion of the substrate. The method of depositing (crystalline) material on a substrate may be performed as part of a method of manufacturing a battery cathode.
[0084] The crystalline material in this example has the ABO2 structure. In this example, the ABO2 material has a layered oxide structure. In this example, the ABO2 material is LiCoO2. However, the method of this example has been shown to be effective with a wide range of ABO2 materials. In other examples, the ABO2 material structure includes at least one of the following compounds (described here with non-specific stoichiometry): LiCoO, LiCoAlO, LiNiCoAlO, LiMnO, LiNiMnO, LiNiMnCoO, LiNiO, and LiNiCoO. These materials are good candidates for making battery cathodes. One skilled in the art will recognize that the stoichiometry may vary.
[0085] In this example, the ABO2 material is LiCoO2 and is deposited as a layer about 1 micron thick. In another example, the ABO2 material is deposited as a layer about 5 microns thick. In yet another example, the ABO2 material is deposited as a layer about 10 microns thick.
[0086] Referring to FIG. 1a, a plasma deposition process apparatus is generally given the reference numeral 100 and includes a plasma target assembly 102 with a target 104, a remote plasma generator 106, a set of electromagnets 108 for confining the plasma generated by the remote plasma generator 106, a target power supply 110, a remote plasma source power supply 112, and a housing 114. The remote plasma generator 106 includes two sets of radio frequency (RF) antennas 116. The housing 114 includes a vacuum exhaust port 120 that is connected to a set of vacuum pumps located outside the chamber, so that the chamber 122 defined by the housing 114 can be evacuated. The housing 114 also includes a gas inlet 124 that can be connected to a gas supply (not shown) for introducing one or more gases into the chamber 122. In other examples, the gas inlet 124 may be located above the surface of the target assembly 102. As can be seen in FIG. 1a, the plasma is generated away from the target 104.
[0087] In this example, the target 104 comprises the material LiCoO2. Briefly, the chamber 122 is evacuated until a sufficiently low pressure is reached. Power provided by the power supply 112 is used to power the remote plasma generator 106, which generates a plasma. Power is applied to the target 104 such that the plasma interacts with the target 104, and LiCoO2 is sputtered from the target 104 and onto the substrate 128. In this example, the substrate 128 comprises a polymer sheet that is introduced into the housing 114 via an inlet 130 and exits the housing via an outlet 132. Motorized rollers 134 are used to aid in the movement of the substrate 128. The LiCoO2 deposits onto the substrate 128 as a crystalline (non-amorphous) material.
[0088] The apparatus 100 also includes a shutter 136 to limit deposition of the sputtered material on the substrate 128, and an input 138 for cooling the drum. The shutter 136 allows a portion of the substrate 128 to be exposed to the sputtered material.
[0089] As mentioned above, the motorized rollers 134 are used to assist in moving the substrate 128 into and out of the plasma deposition apparatus 100. The motorized rollers 134 may be part of a roll-to-roll substrate handling apparatus (not shown) that includes at least a first storage roller upstream of the plasma deposition apparatus 100 and a second storage roller downstream of the plasma deposition apparatus 100. The roll-to-roll substrate handling apparatus is a convenient means of handling, storing and moving thin, flexible substrates such as the polymer substrate used in this example. Such a roll-to-roll system has many other advantages. It allows for high material throughput through sequential depositions on a first portion of the substrate, followed by a second portion of the substrate, and allows for the deposition of large cathode areas on one substrate. Furthermore, such a roll-to-roll process allows many depositions to occur without breaking vacuum. This saves both time and energy compared to systems that require the chamber to be returned from vacuum to atmospheric pressure after deposition in order to load a new substrate. In another example, a sheet-to-sheet process is used instead of a roll-to-roll process, where the substrate is provided with supports. Alternatively, the substrate may be supplied in individual sheets that are handled and stored in relatively flat sheets. The substrate may be planar in order to deposit the material onto the substrate. This may be the case when the substrate is supplied in individual sheets and not transported to and from rolls. The sheets may each be mounted on a carrier with greater structural rigidity. This may allow thinner substrates to be used than with substrate films held on rollers. The substrate may be a sacrificial substrate. The substrate may be removed prior to the layer of material. Part or all of the substrate may be removed prior to incorporating the crystalline layer or a portion of the crystalline layer into an electronic product package, component, or other end product. For example, a layer of crystalline material may break away from the substrate. There may be another layer of intervening material between the base substrate and the crystalline material. This layer may break away with the crystalline material or may aid in the separation of the crystalline material from the base substrate. Laser-based lift-off techniques may be used.The substrate may be removed by a process that uses laser ablation.
[0090] Similar techniques are described in the prior art, for example in KR20130029488 which describes a method of making a battery that includes using a sacrificial substrate and a laser beam to collect the battery layers. In other examples, other suitable processing regimes are used, provided that a sufficiently high product throughput is possible.
[0091] The polymer substrate 128 is under tension as it moves through the system, for example, withstanding a tension of at least 0.001 N during at least a portion of the process. The polymer is robust enough not to deform under tensile stress when sent through the roll-to-roll equipment. In this example, the polymer is polyethylene terephthalate (PET) and the substrate 128 has a thickness of 1 micron or less, and in some examples, the thickness is 0.9 microns. The substrate 128 is precoated with a current collecting layer, which is made of an inert metal. In this example, the inert metal used as the current collecting layer is platinum. The yield strength of the PET film is strong enough that the substrate does not dent or plastically deform under the pressure of the roll-to-roll transport equipment. In other examples, the inert metal used may instead be gold, iridium, copper, aluminum or nickel. The use of such thin polymer substrates is beneficial because it facilitates the manufacture of batteries with higher energy density. In other examples, non-polymeric materials are used if they can be manufactured in a thin and flexible manner that allows for high battery density and ease of handling after deposition.
[0092] However, the plasma deposition process and subsequent manufacturing processes suffer from technical challenges posed by the regime of using such thin layers.
[0093] Before the substrate 128 is precoated, the substrate 128 has a surface roughness that is carefully designed to be (a) large enough to reduce undesirable effects due to electrostatic forces (e.g., increasing the force required to unwind a retained polymer film from a drum) and (b) small enough that the roughness does not cause problems when material is deposited on the substrate. In this example, the surface roughness is designed to be about 50 nm. In this example, the product of the substrate thickness (0.9 microns) and the surface roughness is 4.5×10 4 nm 2 and therefore, 10 5 nm 2 Less than or equal to 5 x 10 4 nm 2 Note that the roughness required to facilitate handling of thin films has been found to increase with decreasing thickness. In general, the roughness required to improve the handleability of thinner substrates (i.e., less than 10 microns, especially less than 1 micron) has been found to increase as the thickness of the substrate decreases.
[0094] Figure 1c shows (not to scale) a typical thin film polymer with a thickness of about 1 micron and embedded particles that provide roughness. The roughness, which is a surface feature provided by the particles, is at least 90 nm, and in some cases greater than 90 nm, which is too rough in certain anticipated cases (but may be tolerable in others).
[0095] FIG. 1d shows one way in which the desired roughness can be achieved (not to scale). Polystyrene spherical particles are embedded in the substrate material such that at least 90% of the spherical particles contributing to the substrate roughness protrude beyond the specific substrate surface with less than half the particle's volume. The particles have a diameter of about 90 nm. Therefore, the majority of the embedded particles contributing to the substrate surface roughness have a median diameter of about 180% of the substrate surface roughness. In another example, the spherical embedded particles are made of a different material, such as silicon oxide.
[0096] Figure 1e shows an alternative situation where the desired roughness can be achieved (not to scale). The polystyrene spherical embedded particles are present on the surface of the substrate material such that at least 90% of the spherical embedded particles contributing to the substrate roughness protrude beyond the particular substrate surface by more than half of the particle's volume. The particles used in the example of Figure 1e are smaller than those used in the example of Figure 1d.
[0097] Examples such as those in Figures 1d and 1e allow for the deposition of good quality films of crystalline material on thin substrates in a manufacturing environment. Only careful control of the location and size distribution of embedded particles can avoid or reduce the potential disadvantages while retaining the benefits of their presence. Figures 1f to 1h show schematic cross-sectional views corresponding to the substrates shown in Figures 1c to 1e after a layer of crystalline material has been formed on the substrate surface. The intermediate layer of metal current collector has been omitted from Figures 1f to 1h. The roughness of the substrates shown in Figures 1c and 1f can cause problems. Such is the case. The influencing extrusion caused by some embedded particles 152 causes shadowing and competing crystal growth, which is shown diagrammatically in FIG. 1f with contrasting shading 154. The competing crystal growths aligned in opposite directions increase the discontinuities of the layers, which affects the performance of the final product. It also has a surprisingly severe effect on the possibility of delamination of the layer of deposited material from the substrate. This can occur as a result of poor contact between the layer to be deposited and the underlying substrate in areas close to some embedded particles (schematically shown by spaces 156 in FIG. 1f) that protrude far from the central flat surface, where the extent of the local unevenness is small. On the other hand, no such problem is seen to occur in FIGS. 1g and 1h. The surface roughness of the material deposited on the substrate is approximately 50 nm.
[0098] The roughness of a substrate can be measured using a surface profilometer, an instrument that has a fixed stylus. The surface to be measured is moved under the stylus and the deflection of the stylus measures the surface profile from which various roughness parameters can be calculated.
[0099] Roughness can also be measured using "non-contact" methods. A suitable device for measuring roughness is the "Omniscan MicroXAM 5000B 3d", which uses optical phase-shifting interferometry to measure the surface profile.
[0100]
number
[0101]
number
[0102] In this example, the average surface roughness is measured by a non-contact method.
[0103] The remotely generated plasma is produced by power provided to the antenna 116 by the power supply 112. Therefore, there is a measurable power related to the power that generates the plasma. The plasma is accelerated towards the target 104 by electrically biasing the target, resulting in an associated current flow. Therefore, there is a power related to the bias at the target 104. In this example, the ratio of the power used to generate the plasma to the power related to the bias at the target is greater than 1:1, and optionally greater than 1.0:1.0. Note that in this example, the ratio is calculated assuming a 50% power efficiency of the plasma source. The power related to the bias at the target is at least 1 Wcm -2In a further example, the ratio of the power used to generate the plasma to the power related to the bias at the target is greater than 1:1 and less than or equal to 7:2, optionally less than or equal to 7.0:2.0. In another further example, the ratio of the power related to the bias at the target is greater than 1:1 and less than or equal to 3:2, optionally less than or equal to 3.0:2.0. In some examples, the power efficiency of the plasma source is 80%. In some examples, the power associated with the bias at the target is 10 Wcm. -2 In another further example, the power associated with the bias at the target is 100 Wcm -2 In another further example, the power associated with the bias at the target is 800 Wcm -2 In other examples, the efficiency of the plasma source may be different, and the power ratio may be different. When the LiCoO2 film is deposited on the substrate, a crystalline film of LiCoO2 is formed. The crystalline structure formed on the substrate is: JPEG0007555408000007.jpg1960. This structure is a layered oxide structure that offers many benefits, such as higher available capacity and faster charging and discharging, compared to the low-energy structure of LiCoO2, which has a structure in the Fd3m space group. JPEG0007555408000008.jpg1960Crystalline LiCoO2 is often preferred for solid-state battery applications.
[0104] Throughout the plasma deposition process, the temperature of the substrate 128 does not exceed the decomposition point of the polymer substrate 128. Additionally, the temperature of the substrate is low enough throughout the deposition process to keep the yield strength of the temperature conditioned polymer substrate sufficiently high so that the polymer substrate does not deform under the pressures applied by the roll-to-roll processing equipment.
[0105] The general shape of the confined plasma produced from the remote plasma generator 106 is shown by dashed line B in FIG. 1a. A series of electromagnets 108 are used to confine the plasma to the desired shape / volume. In this first example, the substrate 128 is fed into the chamber at an inlet 130 and exits the chamber at an outlet 132, although alternative arrangements are possible. For example, there may be other storage locations for the upstream rolls or shutters 136 inside the process chamber 122. There may be other storage locations for the downstream rolls or shutters 136 inside the process chamber 122 or they may be stored inside the process chamber 122.
[0106] In addition, the means 112 for supplying power to the plasma source may be of the RF type, (direct current) DC type or pulsed DC type.
[0107] In this first example, the target assembly 102 includes only one target 104. This target is made of LiCoO2. It is understood that alternative and / or multiple target assemblies may be used that include, for example, different regions of elemental lithium, different regions of elemental cobalt, different regions of lithium oxide, different regions of cobalt oxide, different regions of LiCo alloy, different regions of LiCoO2, or any combination thereof. In other examples, the ABO2 material need not be LiCoO2. In those examples, the target assembly or assemblies include different regions of A, different regions of B, different regions of a compound including A and / or B, and / or different regions including ABO2.
[0108] For the avoidance of doubt, the target 104 of the target assembly 103 acts solely as an element of material and does not function as a cathode when power is applied thereto from an RF power supply, a DC power supply or a pulsed DC power supply.
[0109] In this example: system The operating pressure is 0.0050 mBar. systemThe theoretical mean free path of the target 104 is approximately 10 cm. The theoretical mean free path is the average distance that an ion travels from collision to collision in the plasma. The working distance between the target 104 and the substrate 128 is approximately 8.5 cm. Therefore, the working distance is system This is approximately 85% of the theoretical mean free path.
[0110] In this example, the operating pressure is higher than the lower limit at which crystalline material of the layered oxide structure does not form, but is lower than the upper limit at which observable damage occurs to the substrate, and the operating distance is shorter than the upper limit at which crystalline material of the layered oxide structure does not form, but is longer than the lower limit at which the energy of deposition causes observable damage to the substrate or creates undesirable oxidation states.
[0111] The average crystal size of the crystals formed on the film in this example is about 20 nm. In another example, the average crystal size of the crystals formed on the film is about 50 nm.
[0112] In an alternative example, system The operating pressure is 0.0020mBar. system The theoretical mean free path of is approximately 12 cm. The working distance between the target 104 and the substrate 128 is approximately 9 cm. Therefore, this working distance is system This is approximately 75% of the theoretical mean free path.
[0113] In an alternative example, system The operating pressure is 0.0065 mBar. system The theoretical mean free path of the target 104 is approximately 15 cm. The working distance between the target 104 and the substrate 128 is approximately 7.5 cm. Therefore, this working distance is system This is approximately 50% of the theoretical mean free path.
[0114] The second method example uses the apparatus shown in FIG. 2a. The main differences between the apparatus of FIG. 1a and that of FIG. 2a are illustrated. FIG. 2a shows the use of a rigid planar glass substrate 228 instead of the flexible substrate 128 of the first example. Furthermore, there is no shutter in this example. The thickness of the glass substrate is on the order of millimeters. A single target 204 is used in this example. A temperature indicator sticker was attached to the side of the glass slide opposite the side on which the cathode material is deposited. The temperature indicator sticker is set to indicate whether the substrate 228 reaches a temperature of 270° C. or higher during the plasma deposition process. After deposition, the sticker indicated that the substrate did not reach a temperature of 270° C. or higher during the deposition process. The general shape of the plasma is indicated by the area enclosed by the dashed line B′ in FIG. 2a.
[0115] Table 1 shows the properties of example battery cathodes prepared according to the second example.
[0116] [Table 1] Table 1 - Properties of LiCoO2 cathode films as a function of deposition parameters
[0117] In Table 1 above, the elemental composition of the films was determined by X-ray photoelectron spectroscopy using a Themo Fisher K-alpha spectrometer with a MAGCIS ion gun. The quoted composition was obtained from depth profiling measured on the films at a level of about 10. Plasma source power is the power supplied to generate the plasma. Sputtering power is the power applied to the target 204. Process pressure is the pressure in the chamber. Film thickness and film roughness measurements were obtained after deposition using an Omniscan MicroXAM 5000b 3d optical profiler. Film thickness was measured after deposition, as were step height and roughness measurements at the masked edge obtained from a sample area of about 400 microns by 500 microns.
[0118] Figure 2b shows the X-ray diffraction (XRD) spectrum of the battery cathode of sample 1. The structure of the film was characterized by X-ray diffraction using a diffractometer (Rigaku-Smartlab) with nickel-filtered CuKα radiation (λ=1.5406 Å). Diffraction patterns were obtained at room temperature using a fixed incidence angle of <5° in the range of 10°<2θ<80°. Data were collected using a step scan with a resolution of 0.04° / step and a counting time of 0.5 s / step. The peak at approximately 37° is associated with the (101) plane of the crystals substantially oriented parallel to the substrate surface. The peak at approximately 66° is associated with the crystals substantially oriented such that the (110) plane is parallel to the substrate. The peak at approximately 55° is associated with the glass substrate and needs to be ignored to determine the crystal structure of LiCoO2.
[0119] The absence of extra reflected light related to the Fd3m space group indicates that the deposited LiCoO2 This is an initial indication that the image is JPEG0007555408000010.jpg1960.
[0120] There is also notable absence of peaks relating to the (003) plane. This suggests that very few crystals are oriented with the (003) plane parallel to the substrate surface. This orientation of very few crystals is beneficial. A detailed explanation is beyond the scope of this application, but in brief, a higher proportion of the crystals are oriented with the (101) and (110) planes parallel to the substrate, as opposed to oriented with the (003) plane parallel to the substrate, increases the usable capacity of the cathode due to a lower apparent resistance to ion movement. The crystals are formed such that their longitudinal axis is normal to the substrate. In other words, the crystals are formed by epitaxial growth. Applicant has found that crystalline material is deposited in most cases when the ratio of the power used to generate the plasma to the power related to the bias of the target is greater than 1:1. For sample 1, the ratio is 1800:500 (3.6:1), and for sample 2, it is 1800:800 (9:4). Note that in this example, the ratios are calculated assuming a 50% power efficiency of the plasma source.
[0121] In a comparative example, the experiment was repeated with a plasma source power of 1 kW and a power associated with the bias on the target of 1 kW. The deposited material was substantially amorphous. The performance of the comparative film as a cathode was investigated by depositing an electrolyte (in this case LiPON) and an anode metal onto the cathode layer, thereby fabricating a solid-state battery. The charge-discharge characteristics of the battery were investigated and it was found that the specific capacity of the cathode was insufficient, about 10 mAh / g. When a similar battery was fabricated using crystalline LiCoO2 as produced in samples 1 and 2, the charge-discharge characteristics were much better, with a typical cathode specific capacity of about 120 mAh / g.
[0122] Figure 2c shows the Raman spectrum of the battery cathode of Sample 1. The compounds have been characterized by Raman spectroscopy. Raman spectra were collected using a JY Horiba LabRAM ARAMIS imaging confocal Raman microscope using 532 nm excitation. 600cm -1 The strong and sharp peak at 487cm may be considered to be a unique peak due to the non-material nature of the peak sharpness. -1 The strong characteristic peak observed at is due to LiCoO2 It is well known in the art that this relates to the crystal structure of JPEG0007555408000011.jpg1960.
[0123] FIG. 2d shows the XRD spectrum (collected in the same manner as for sample 1) of the cathode of sample 2. The spectrum shown is similar to that shown in FIG. 2b. However, in FIG. 2d, the relative intensity of the peak at approximately 66° is much stronger than that of the peak at 37°. This indicates that for sample 2, the number of crystals with (110) faces parallel to the substrate is greater than the number of crystals with (101) faces parallel to the substrate. This is beneficial because it means that the ion channels in the thin film are oriented perpendicular to the substrate, facilitating the intercalation and deintercalation of ions from interstitial sites from within the crystal structure of the cathode. This improves the usable capacity and charging rate of the cathode. FIG. 2e shows the Raman spectrum of the cathode of sample 2, and the same comments that apply to FIG. 2c apply to FIG. 2e.
[0124] 3a to 3c show an alternative apparatus example using another example of a method for producing a layer of crystalline material on a surface using plasma sputtering according to the third example. The apparatus used and the method of production are similar to the apparatus described with respect to the first example. Here, only the major differences are described. Identical parts are indicated by the same last two digits of the reference numeral. For example, the rotating drum 334 in FIG. 3a is identical to the rotating drum 134 in FIG. 1a. The apparatus in FIG. 3a comprises a rotating drum 334 on which a polymer substrate 328 is supported within an area defined by a process chamber 322 (the walls of the chamber are omitted for clarity). The target assembly 302 comprises a plurality of targets. There is a first target 304 composed of elemental lithium and a plurality of targets 303 (herein referred to as second targets) composed of elemental cobalt. The targets are all positioned at a working distance of about 10 cm from the substrate 328 (the working distance is the shortest distance between them). The surface of each target 303, 304 facing the drum 334 is flat (planar). The radius of the drum 334 is much larger than the working distance (for illustration purposes, the size of the drum 334 shown in the figure is relatively smaller than in reality). The targets 303, 304 are circumferentially arranged around the circumference of the drum 334. The apparatus also includes a shutter 336 to limit deposition of sputtered material onto the substrate 328.
[0125] A plasma consisting of argon ions and electrons is generated using two spaced apart electrically powered antennas 316. The plasma is confined and concentrated by a magnetic field controlled by two sets of electromagnets 308, each set positioned in close proximity to one of the antennas 316 and the electric field generated by the system. The overall shape of the plasma (90% full density shown in a very schematic manner by plasma cloud B in FIG. 3c) is blanket-like in that the length and width of the plasma cloud are much greater than its thickness. The width of the plasma is controlled in part by the length of the antennas 316. The two sets of antennas 316 are separated by a distance corresponding to the length of the plasma. The length and width of the plasma are in the same general direction as the length and width of the substrate, respectively.
[0126] The plasma source is located remotely from the target and may therefore be considered a remotely generated plasma. system The theoretical mean free path (i.e., the average distance an ion in the plasma travels from collision to collision) is about 12 cm, meaning that the majority of particles will travel from the target to the substrate without colliding with any argon ions in the plasma.
[0127] FIG. 3a is a partial schematic cross-sectional view showing a portion of the substrate moving on the drum 334 and shows diagrammatically the trajectories of particles moving from the targets 303, 304 to the substrate. Thus, there is a first plume corresponding to the trajectories of particles from the first target 304 to the surface of the substrate 328 and a second plume corresponding to the trajectories of particles from the second target 303 to the surface of the substrate 328. The first plumes are shown as speckled areas and each second plume is shown as a dark grey area. It can be seen from FIG. 3a that the first and second plumes are concentrated in an area close to the substrate. The first target 304 faces towards the substrate in a first direction (defined in this example by a notional line extending from the center of the surface of the target 304) and the left adjacent second target 303 faces towards the substrate in a second direction (defined in this example by a notional line extending from the center of the surface of the target 303) as shown in FIG. 3a. The first and second directions converge toward the substrate and intersect a short distance past the substrate (the location is approximately 3 cm past the substrate). Oxygen gas is supplied at a controlled rate through inlet 325 into the process chamber 322. The substrate moves with the rotation of the drum, while the target is fixed. In another example, an inert sputtering gas is introduced through a gas inlet (not shown here, but of substantially the same shape as shown in FIG. 1a).
[0128] The amount of oxygen introduced into the chamber may be reduced in some other instances when distinct regions of lithium oxide and cobalt oxide are present in the targets 304, 303, and the oxygen content of such targets may be so high in some instances that no additional oxygen gas needs to be introduced into the chamber 322 at all.
[0129] Figure 3b is a view looking down from the drum towards the target, and Figure 3c is a cross-sectional view including a cutaway of the first target 304, the second target 303 and the substrate 328 on the drum 334.
[0130] In FIG. 3 c (cross-sectional view), it can be seen that the first targets 304 are curved relative to the respective second targets 303 .
[0131] In carrying out this method, the plasma that is generated is used to sputter material from a first target and a second target onto a substrate.
[0132] As shown in FIG. 3d, elemental lithium material has a lower sputter yield (less than half at 10 keV) than cobalt, measured as the yield of atoms per ion that reaches the surface at a given energy. Accordingly, the (negative) potential applied to the first target has a larger magnitude than the potential applied to the second target. Also, the surface area of the first target exposed to the plasma is slightly larger than the sum of the areas of the second targets. Thereby, the number of ionized Li atoms reaching each unit of the substrate is substantially the same as the number of ionized Co atoms reaching each unit of the substrate. There are also ionized oxygen atoms, as well as electrons from the plasma. The high energy particles made possible by the remote plasma allow the formation of a crystalline LiCoO2 material with a hexagonal crystal structure in situ on the surface of the substrate. A greater number of high energy particles from the plasma reach the first target 304 (over the entire surface area of the target) than the second target 303 (over the entire surface area of both targets in total).
[0133] Figure 3e shows a schematic cross-sectional view of a further example of an apparatus according to the fourth example, similar to the cross-sectional views shown in Figures 3a to 3c, but in which the targets are moving and arranged in sets around a drum 334. The targets in each set (i.e. each assembly 302) are positioned at an angle so that they face towards a position very close to the substrate on the drum. Each set 302 comprises a first target 304 of elemental lithium and a second target 303 of elemental cobalt. The targets are all positioned at a working distance of about 15 cm from the substrate, which is the minimum separation between them. systemThe theoretical mean free path (i.e. the average distance between collisions of ions in the plasma) of the target (302) is about 20 cm. For each set of targets (302), during use, there is a first plume of particles from the first target (304) and a second plume of particles from the second target (303), which are concentrated in the area adjacent to the substrate. The center of rotation of the main drum 334 is also the center of rotation of the targets. The targets move around the center of rotation at a slower angular velocity than the drum. The principle of rotation allows targets to be replaced when they move out of the plasma, thus allowing continuous deposition of material on a moving substrate.
[0134] An example of a battery cathode made according to the second example is described with reference to Figures 4a, 4b and 5a. A substrate 428, 528 includes a current collecting layer 429, 529, in this case a layer of platinum, on which a layer 442, 542 of LiCoO2 is deposited. In other examples, another inert metal is used as the current collecting layer, for example gold, iridium, copper, aluminum or nickel. In other further examples, the current collecting layer may be carbon-based. In some examples, the current collecting layer is surface modified, and in some examples, the current collecting layer includes a rod-like structure.
[0135] As shown in the scanning electron microscope (SEM) images of Figure 4a (cross-sectional view of the first film-deposited sample) and Figure 4b (bird's-eye view of the second film-deposited sample), the LiCoO2 film layers 442, 542 of both samples are polycrystalline in nature. The battery cathodes of Figures 4a, 4b and 5a can also be fabricated according to the method of the third example or the method of the fourth example.
[0136] A method of making a cathode half-cell according to the fifth example is described with reference to Fig. 5a (first sample), Fig. 5b (second sample) and Fig. 5c. The method, generally described with reference numeral 3001, includes depositing 3002 a battery cathode material 542 on a substrate (including a current collecting layer 529 in this example) and depositing 3003 a battery electrolyte material 544 on the battery cathode material 542. In this example, the material deposited as electrolyte 544 is lithium oxynitride phosphate (LiPON). In other examples, the material deposited is another suitable electrolyte material. In some samples (such as the second sample) of the fifth example of the invention, the half-cell may include electrode material 544, and in other samples of the fifth example, the half-cell may not include electrode material 544 (such as the first sample).
[0137] In this example, a remotely generated plasma is used to deposit LiPON in substantially the same manner as the ABO2 material in the first, second, third or fourth examples. However, in this example, the target material used is Li3PO4 and deposition occurs in a reactive nitrogen atmosphere. In other examples, the target assembly may include multiple targets having different regions of lithium and / or different regions of phosphorus-containing compounds, elemental lithium, or lithium oxide. In other examples, deposition also occurs in a reactive oxygen atmosphere.
[0138] An example of a method of making a solid-state battery according to the sixth example will be described with reference to Figure 6. The method is generally designated by reference numeral 5001 and includes the steps of making 5002 a cathode half-cell according to the sixth example (e.g., as described above with respect to Figures 5b and 5c); Contacting the cathode half-cell with an anode 5003. In this example, the anode is deposited by any convenient method such as remote plasma sputtering, magnetron sputtering, CVD, etc. In other examples, the anode is deposited by thermal evaporation, e-beam evaporation, pulsed laser deposition, or simple DC sputtering.
[0139] An example of a method for fabricating a solid-state battery according to the seventh embodiment is described with reference to Fig. 7a. The method is generally given by reference numeral 6001 and includes fabricating a plurality of cathode half-cells of a solid-state thin-film battery 6002, fabricating a plurality of anode half-cells of a solid-state thin-film battery 6003, and contacting the cathode and anode half-cells with each other 6004, thereby forming at least one battery. A battery thus fabricated according to a first sample of the seventh embodiment of the present invention is shown diagrammatically in Fig. 7b. With reference to Fig. 7b, 628 and 628' are substrate materials, 629 and 629' are current collecting layers, 642 is a cathode material, in this case LiCoO2, and 644 is LiPON, which acts as both electrolyte and anode.
[0140] Alternatively, in other examples, the current collector material serves as the anode material. Alternatively, in the second sample of the seventh example of the invention, further anode material may be deposited. This is shown diagrammatically in FIG. 7c. Referring to FIG. 7c, 628 and 628' are substrate materials, 629 and 629' are current collector layers, 642 is a cathode material, in this case LiCoO2, 644 is LiPON, which serves as an electrolyte, and 646 is a suitable anode material.
[0141] An example of a method for determining an optimal working distance for a remote plasma deposition system configured to deposit a layered oxide material according to an eighth example will now be described with reference to Figure 8a. This method is generally illustrated by the numeral 7001, selecting 7002 a range of working distances, wherein the working distances within the range system + / - 50% of the theoretical mean free path of performing 7003 a method of depositing material according to the first example for a number of test samples at different working distances within a selected range for each sample; performing 7004 a characterization technique on each test sample after deposition has occurred that can determine unique features of the layered oxide structure; identifying a sample in which the unique property is present 7005; and Selecting from those samples the sample with the highest (normalized) intensity of said characteristic peak 7006, and subsequently, system and selecting 7007 a working distance for the
[0142] In this eighth example, the characterization technique used is X-ray diffraction, and the characteristic feature is a diffraction peak or a series of diffraction peaks. In FIG. 8b, a number of X-ray diffraction patterns recorded for films deposited at different working distances are shown. From the top to bottom, the diffraction patterns are for working distances of 5 cm (731), 8 cm (733), 12 cm (735), and 15 cm (737), respectively. As can be seen, the 8 cm working distance shows the highest intensity peak 733 at 19 degrees 2θ (one of the peak positions 739 required for hexagonal LiCoO2, this particular peak does not exist for cubic or spinel structured LiCoO2). Therefore, in this example, 8 cm is selected as the working distance. In other examples, other characterization techniques different from X-ray diffraction may be used. The intensity of the diffraction pattern 731 measured for a working distance of 5 cm is lower at 19 degrees 2θ than the diffraction pattern 733 for a working distance of 8 cm. Diffraction pattern 735 collected for a working distance of 12 cm and diffraction pattern 737 collected for a working distance of 15 cm do not show any characteristic hexagonal peak at 19 degrees 2θ.
[0143] In some examples, the test sample of the method is replaced with an average value for multiple test samples, the test sample including multiple test samples, where the method of the first example is run multiple times at the same working distance and the average value is taken. In some examples, the method may be run multiple times to find an optimal working distance for operating the system.
[0144] FIG. 9a shows a sample formed according to the first example while carrying out the method of the eighth example, and FIG. 9a shows a damaged substrate surface (with undesired oxide) resulting from deposition when the working distance is too short. In this example, the working distance was 5 cm and the deposited material was LiCoO2. As can be seen, crystals do not form over the entire substrate surface and the substrate is deformed. In addition, regions of Co(II)O, an undesired cobalt oxide phase, form on the substrate at this working distance. This can be confirmed by the spectrum shown in FIG. 9b, which shows peaks related to the Co(II)O phase (identified at two values of 2θ 843) detected in the diffraction pattern 831 obtained for the sample with a working distance of 5 cm, in addition to the peaks of hexagonal LCO (identified at five values of 2θ 839). A structure refinement model 831' including both hexagonal LiCoO2 and CO(II)O phases was obtained from the collected diffraction pattern of 831. The difference between the diffraction pattern 831 and the improved model 831' is shown by difference line 841. Therefore, during the eighth example method, an excessively short working distance is not selected as the optimal working distance.
[0145] An example of a method for determining an optimal range of operating pressures for a remote plasma deposition system configured for depositing a layered oxide material according to a ninth example is described with reference to Figure 10a. This method is generally illustrated by numeral 8001 and includes: Selecting an initial range of operating pressure from 0.00065 mBar to 0.01 mBar (optionally, from 0.001 mBar to 0.007 mBar) 8002; performing, for each of a number of test samples, the method of depositing material according to the first example at different operating pressures within a selected range 8003; performing 8004 a characterization technique on each test sample after deposition has occurred that can determine specific properties of the layered oxide structure; selecting a test sample from the group of test samples that exhibits the distinctive characteristics of the layered oxide material 8005, the test sample deposited at the lowest operating pressure, and setting this operating pressure as the lower limit of the range 8006; selecting 8007 a test sample deposited at the highest operating pressure from the group of test samples that show no observable signs of damage to the substrate, and setting 8008 this operating pressure as the upper limit of the range.
[0146] In a ninth example, the characterization technique used is X-ray diffraction and the characteristic features are those including characteristic X-ray diffraction peaks of layered oxide materials. Figure 10b shows an example X-ray spectrum showing the absence of this characteristic feature below a certain operating pressure. In this example, the presence of a peak at 19 degrees 2θ in pattern 947 of the sample deposited at 0.0046 mBar leads to the formation of a hexagonal crystalline phase, while pattern 945 of the sample deposited at 0.0012 mBar does not lead to the formation of a hexagonal crystalline phase, as shown by the absence of the peak. In other examples, characterization techniques other than X-ray diffraction may be used.
[0147] In a further example, the test sample of this method is replaced with an average value for multiple test samples, which includes multiple test samples in which the method of the first example is run multiple times at the same operating pressure and the average is taken.
[0148] In some instances, the method provides for system In this example, the optimal operating pressure is the operating pressure within the range that results in the fastest deposition.
[0149] An example of a method for determining crystal size for depositing a layered oxide material according to a tenth example is described with reference to FIG. 11a. This method is generally illustrated by numeral 9001, and the method comprises: Selecting an initial range of operating pressure from 0.00065mBar and 0.01mBar 9002; performing 9003 a method for depositing material according to the first example at different operating pressures within a selected range for a number of test samples; After deposition has occurred, performing 9004 a characterization technique capable of determining the crystallite size of each film of each test sample.
[0150] The selected range of operating pressure may be, for example, 0.001 mBar to 0.007 mBar.
[0151] FIG. 11b is a graph showing that after carrying out the method of the tenth example at a given range of operating pressures, the range of crystal sizes resulting in a number of films deposited according to the first example at different operating pressures between 0.001 mBar and 0.0065 mBar for an operating distance of 16 cm is relatively wide compared to FIG. 11c.
[0152] FIG. 11c is a graph showing that after carrying out the method of the tenth example at a given range of operating pressures, the range of crystallite sizes produced in a number of films deposited according to the first example at different operating pressures between 0.001 mBar and 0.0065 mBar for an operating distance of 8.5 cm is relatively narrow compared to FIG. 11b.
[0153] Having a narrow distribution of crystallite sizes is beneficial because it allows the crystallite sizes of films deposited on an industrial scale to be predictable and repeatable.
[0154] An example method of depositing material on a substrate according to an eleventh example will now be described with reference to Figure 12. This method is generally illustrated by numeral 1101 and includes the following steps: generating 1102 a plasma separate from one or more plasma targets suitable for plasma sputtering; exposing 1103 one or more plasma targets to a plasma, thereby generating sputtered material from the one or more targets; Depositing 1104 a sputtered material onto a first portion of the substrate.
[0155] As illustrated by an eleventh example, the method of depositing a material on a substrate includes all the features of deposition of the first example, although in this example the target material may be any material. In this example, the target material is crystalline, but in other examples the deposited material may be semi-crystalline or amorphous.
[0156] A twelfth example is also shown, which relates to a method of manufacturing a part of an electronic device comprising a substrate and is described with reference to FIG. 13. The method is generally illustrated by numeral 1201 and includes depositing 1202 a material on a substrate using a method as described in the eleventh example. In this example, the method of the eleventh example is performed multiple times 1203 to deposit multiple layers. In this example, at least some of the multiple layers may be semiconductor layers. In this example, the method is therefore a method of manufacturing a semiconductor device and part thereof. In this example, adjacent layers are deposited with different parameters and / or different target materials used for the deposition of each layer to manufacture the electronic device. In another example, multiple layers of materials are deposited using substantially the same target material and substantially the same parameters.
[0157] In this example, the substrate includes one intermediate layer, which may optionally act as a current collecting layer. In other examples, more intermediate layers are present and aid in adhesion during the deposition step. In some other examples, no intermediate layers are present. Deposition of the intermediate layer on the substrate may be performed according to the method described in the eleventh example. In other examples, deposition of the intermediate layer on the substrate is performed by other suitable deposition techniques, such as sputtering, thermal evaporation, electron beam evaporation, pulsed laser deposition, or other thin film deposition techniques.
[0158] In this example, the method includes depositing a first semiconductor layer of material. In this example, the first semiconductor layer is deposited on an intermediate layer of material. In another example, the first semiconductor layer is deposited directly on a substrate. In this example, the first semiconductor layer includes silicon. In another example, the first semiconductor layer includes aluminum, and in some further examples, gallium nitride. In examples where the semiconductor layer of material is gallium nitride, deposition occurs under a reactive nitrogen atmosphere. In this example, the first semiconductor layer of material is doped n-type. This is achieved in this example by sputtering a target that includes a phosphorus-containing compound. In other examples, this is achieved by using a different dopant, such as arsenic, antimony, bismuth, or lithium. In some further examples, the semiconductor layer of material is doped p-type with a dopant, such as boron, aluminum, gallium, or indium. In further examples, the semiconductor layer of material is undoped and is an intrinsic semiconductor. In some of these examples, the dopant material is not introduced as a material that can be sputtered, but instead is introduced as a gas after deposition such that the dopant diffuses to the surface of the semiconductor layer.
[0159] In this example, the method includes depositing a second semiconductor layer of material on the first semiconductor layer of material. In other examples, the second semiconductor layer of material is deposited directly on the substrate or on the intermediate layer (if any). In this example, the second semiconductor layer of material is an intrinsic semiconductor. In this example, the second conductive layer of material is gallium nitride. In a further example, the second semiconductor layer of material is doped n-type with a dopant such as phosphorus, arsenic, antimony, bismuth, or lithium. In some further examples, the second semiconductor layer of material is doped p-type with a dopant such as boron, aluminum, gallium, or indium. In some of these examples, the dopant material is not introduced as a target that can be sputtered, but instead is introduced as a gas after deposition such that the dopant diffuses at the surface of the semiconductor layer.
[0160] In this example, the method includes depositing a third semiconductor layer of material. In this example, the third semiconductor layer is deposited on the second semiconductor layer of material. In other examples, the third semiconductor layer is deposited directly on the first semiconductor layer, the second semiconductor layer, the intermediate layer, or the substrate. In this example, the third semiconductor layer includes silicon. In other examples, the third semiconductor layer includes aluminum, and in some further examples, includes gallium nitride. In some examples where the material of the semiconductor layer is gallium nitride, deposition occurs under a reactive nitrogen atmosphere. In this example, the third semiconductor layer of material is doped p-type. In this example, this is achieved by sputtering a target that includes a boron-containing compound. In other examples, this is achieved by using a different dopant, such as aluminum, gallium, or indium. In some further examples, the third semiconductor layer of material is doped n-type with a dopant, such as phosphorus, arsenic, antimony, bismuth, or lithium. In further examples, the third semiconductor layer of material is undoped and is an intrinsic semiconductor. In some of these examples, the dopant material is not introduced as a target that can be sputtered, but instead is introduced as a gas after deposition such that the dopant diffuses at the surface of the semiconductor layer.
[0161] This example method may be used to form pn junctions or pin junctions.
[0162] In this example, no additional dopants are introduced into some of the semiconductor layers described thus far. In some examples, germanium is introduced as a dopant into the first layer, the second layer, and / or the third layer. Germanium changes the band gap of the electronic device and improves the mechanical properties of each semiconductor layer of material. In some examples, nitrogen is introduced as a dopant into the first layer, the second layer, and / or the third layer of material. Nitrogen is used to improve the mechanical properties of the semiconductor layers being formed.
[0163] A thirteenth example is also provided and relates to a method of producing a crystalline layer of yttrium aluminum garnet (YAG) and is described with reference to Figure 14. The method is generally represented by numeral 1301 and includes using the method described in the eleventh example 1302, where the YAG is doped 1303 with at least one f-block transition metal.
[0164] In this example, the dopant material is a lanthanide.
[0165] In this example, the dopant material includes neodymium. In other examples, the dopant material includes chromium and cerium in addition to neodymium. In this example, the crystalline layer of material includes 1.0 mole percent neodymium. Also, in some examples, the material includes 0.5 mole percent cerium.
[0166] In another further example, the dopant material includes erbium. In this example, the dopant material is provided as a target and sputtered as described in the eleventh example. The crystalline layer of material in this further example includes 40 mole percent erbium. In one example, the crystalline layer of material includes 55 mole percent erbium.
[0167] In yet another further example, the dopant material includes ytterbium. In one of these examples, the crystalline layer of material includes 15 mole percent ytterbium.
[0168] In yet another example, the dopant material includes thulium. In a further example, the dopant material includes dysprosium. In a further example, the dopant material includes samarium. In a further example, the dopant material includes terbium.
[0169] In other further examples, the dopant material includes cerium. In some examples where the dopant material includes cerium, the dopant material also includes gadolinium.
[0170] In some instances, instead of the dopant material being supplied as distinct regions of one or more targets, the dopant material is introduced at least in part by supplying the dopant material as a gas after deposition of the layer of crystalline material so that it diffuses into the layer of crystalline material.
[0171] According to a fourteenth example, a method of manufacturing a light emitting diode is shown, which method will be described with reference to Figure 15. The method is generally illustrated by numerals 1401 and includes performing 1402 a method according to the twelfth example and thereafter or at the same time performing 1403 a method according to the thirteenth example, where the dopant used during the method of the thirteenth example includes cerium 1404. In this example, a layer of cerium doped YAG is used as a scintillator in the LED.
[0172] The methods according to the twelfth and thirteenth examples may be carried out in the same process chamber.
[0173] According to a fifteenth example, a method of manufacturing a permanent magnet is shown and will be described with reference to Figure 16. The method is generally illustrated by numeral 1501 and includes carrying out 1502 a method according to the eleventh example, where different regions of one or more targets are provided comprising neodymium, iron, boron and dysprosium 1503, the method including treating the film 1504 such that the layer of material becomes a permanent magnet.
[0174] In this example, the final layer of material includes 6.0 mole percent dysprosium. In a further example, the mole percent of dysprosium is less than 6.0 mole percent.
[0175] The high target utilization that the method provides is beneficial when making electronic devices from rare elements such as dysprosium, which is available in limited terrestrial abundance, and a deposition system with high target utilization results in less material loss.
[0176] According to a sixteenth example, a method of manufacturing a layer of indium tin oxide (ITO) is shown and will be described with reference to FIG. 17. The method is generally illustrated by numeral 1601 and includes carrying out 1602 a method according to the eleventh example, where different areas of a target are provided that contain indium and tin 1603. Depositing 1604 deposits the layer of ITO in such a way that a transparent crystalline layer of material is formed directly on the substrate. In other examples, a composite target is used, the composite target containing both indium and tin. In other further examples, the composite target contains oxides of indium and tin. Thus, the number of targets used may be different in further examples, or a single target may be used.
[0177] In another further example, the target may include indium oxide or tin oxide. In a further example, the deposition process includes providing oxygen such that material sputtered from the target reacts with the oxygen to form indium tin oxide on the substrate.
[0178] According to the seventeenth example, although not shown separately, a method of manufacturing a photovoltaic cell is shown. In this example, the method further comprises the deposition of ITO as described in the fifteenth example. In a further example, no layer of ITO is deposited. In this example, it also comprises depositing a layer of perovskite material between an n-type doped layer of semiconductor material and a p-type doped layer of semiconductor material. In this case, the perovskite layer of material is deposited by the method described in the eleventh example. In a further example, it is deposited by other suitable methods such as physical vapor deposition or wet chemical techniques. In a further example, no perovskite layer of material is deposited.
[0179] In an alternative example, the method includes depositing a layer of copper indium gallium selenide according to the eleventh example. Copper, indium, gallium and selenide are provided as different regions of one or more targets. In this example, copper is provided as an elemental target and indium, gallium and selenide are provided as oxide targets. In further examples, other combinations of oxide, elemental, compound or composite targets are used. Thus, the number of targets used may vary in further examples, or a single target may be used.
[0180] In some examples, the method includes depositing a layer of cadmium sulfide according to the eleventh example. In this example, the cadmium and sulfide are provided as different regions of an oxide-producing target. Other combinations of oxide, element, compound or composite targets are used in further examples. Thus, the number of targets used may vary in further examples. The targets may be different or a single target may be used.
[0181] In some examples, the method includes depositing a layer of cadmium telluride according to the eleventh example. The cadmium and telluride are provided as different regions of an elemental target in this example. In other examples, the cadmium and telluride are provided as different regions of one or more targets of element, oxide, composite, or any combination thereof. Thus, the number of targets used may vary in further examples, or a single target may be used.
[0182] Although the foregoing description has been described and illustrated with respect to specific examples, those skilled in the art will appreciate that the invention is susceptible to many different variations not specifically set forth herein. Merely by way of example, examples of certain possible variations are described.
[0183] Where integers or elements having known, obvious or foreseeable equivalents are mentioned in the above description, such equivalents are incorporated herein as if set forth separately. Reference should be made to the claims to determine the exact scope of the examples, which should be interpreted to include any such equivalents. The reader should also understand that any integers or features of the invention described as preferred, advantageous, convenient or similar are optional and do not limit the scope of the independent claims. Furthermore, it should be understood that any such integers or features may not be desirable in some embodiments of the invention due to possible benefits, and therefore may not be present in other embodiments.
Claims
1. 1. A method for depositing material on a substrate, comprising: generating a plasma remote from two or more sputter targets suitable for plasma sputtering, wherein a distinct region of at least one of the two or more targets comprises an alkali metal, an alkaline earth metal, an alkali metal-containing compound, an alkaline earth metal-containing compound, or a combination thereof; Confining the plasma to two or more targets; using a confined plasma to generate sputtered material from two or more targets; depositing sputtered material on a substrate, the working distance between the target and the substrate being within + / - 50% of the theoretical mean free path of the system; moving the substrate over a drum, the drum having a center of rotation; moving two or more targets about a center of rotation at an angular velocity that is slower than the angular velocity of the drum; Including, 11. A method of depositing material on a substrate, wherein the two or more targets comprise a first target and a second target, the first target being angled relative to each of the second targets.
2. The method of claim 1 , wherein the working distance is less than the mean free path of the system.
3. 3. The method of claim 1 or 2, wherein the alkali metal-containing compound or alkaline earth metal-containing compound occurs as a crystalline material when the material is deposited.
4. The method of claim 3 , wherein the alkali metal-containing compound or alkaline earth metal-containing compound is in the form of a layered oxide material.
5. 5. The method of claim 1 , wherein the working distance is greater than a lower limit defined by the working distance at which the energy of deposition damages the substrate or causes the formation of undesirable oxide states of the constituent elements of the alkali metal-containing compound or alkaline earth metal-containing compound.
6. The method according to claim 1 , wherein the working distance is greater than 5 cm.
7. 7. The method according to claim 4, wherein the working distance is greater than a lower limit defined by the working distance at which no layered oxide structure occurs.
8. 8. The method according to claim 1, wherein the working distance is between 8 cm and 9 cm.
9. The process occurs in a deposition chamber, the operating pressure being defined as the chamber pressure prior to ignition of the remote plasma, the operating pressure being a substantially constant value throughout the deposition process, and the value being within the range of 0.00065 mBar and 1 e -2 9. The method according to claim 1 , wherein the pressure is between 100 and 2000 bar.
10. 10. The method of claim 9, wherein sputtering is caused by bombardment of ions of a sputter gas, and wherein a flow rate of said sputter gas into the chamber is substantially constant throughout the deposition process, said value being between 5 sccm and 100 sccm.
11. 11. The method according to claim 9 or 10, wherein the operating pressure is below an upper limit defined by the operating pressure at which damage to the substrate or softening of the substrate occurs.
12. 12. The method according to any one of claims 9 to 11, wherein the operating pressure may be between 0.0010 mBar and 0.0065 mBar.
13. 13. The method according to any one of claims 9 to 12, wherein the operating pressure is higher than the lower limit defined by the operating pressure at which no layered oxide structure occurs.
14. Operating pressure: 4.5e -3 14. The method according to any one of claims 9 to 13, wherein the pressure is higher than mBar.
15. 15. The method of any one of claims 1 to 14, wherein the crystal size of the film formed is between 8 nm and 65 nm.
16. 16. The method of any one of claims 1 to 15, wherein the range of crystal sizes does not exceed two standard deviations of the average crystal size across the membrane.
17. The step of using a sputter deposition technique to deposit material on a substrate includes measuring a surface area of 1 cm2, averaged over 1 second, measured on a surface opposite to the surface on which the material is deposited. 2 17. A method according to any one of claims 1 to 16, wherein the method is carried out at a temperature such that the maximum temperature reached on any given square of substrate material at any one time is less than 200°C.
18. The deposition rate is 4 Ås -1 The method of any one of claims 1 to 17, wherein the
19. 1. A method for determining an optimal working distance of a remote plasma deposition system configured for deposition of a layered oxide material, comprising: selecting a range of working distances, the working distances within said range being + / - 50% of the theoretical mean free path of the system; carrying out a method according to any one of claims 4 to 18 for a number of test samples at different working distances within a selected range for each sample; performing characterization techniques capable of determining specific properties of the layered oxide structure on each test sample after deposition has occurred; identifying a sample having said unique property; and selecting from the samples that most strongly exhibits said characteristic property, and then selecting a system working distance relative to the working distance used during deposition of said test sample.
20. 1. A method for determining an optimal working distance of a remote plasma deposition system configured for deposition of a layered oxide material, comprising: selecting a range of working distances, the working distances within said range being + / - 50% of the theoretical mean free path of the system; carrying out for each sample a method according to any one of claims 4 to 18 for a number of test samples at different working distances within a selected range; performing X-ray diffraction on each test sample after deposition has occurred; identifying a sample for which diffraction peaks characteristic of a layered oxide structure are present; A method for determining an optimal working distance of a remote plasma deposition system configured for deposition of a layered oxide material, comprising: selecting from the samples the sample having the highest (normalized) intensity of the characteristic peak; and then selecting a system working distance relative to the working distance used during deposition of the test sample.
21. 21. The method according to claim 19 or 20, wherein the method may optionally be performed multiple times to find an optimal range of working distances for operating the system.
22. 1. A method for determining an optimal range of operating pressure for a remote plasma deposition system configured for deposition of a layered oxide material, comprising: 0.00065mBar and 1.0e -2 selecting an initial range of operating pressure between 100 and 2000 mBar; carrying out for each of a number of test samples a method according to any one of claims 4 to 18 at different operating pressures within a selected range; performing a characterization technique on each test sample after deposition has occurred; selecting a test sample from the group of test samples that exhibits the characteristic characteristics of the layered oxide material, the test sample deposited at the lowest operating pressure, and setting this operating pressure as the lower limit of the range; A method for determining an optimal range of operating pressures for a remote plasma deposition system configured for depositing a layered oxide material, comprising: selecting a test sample deposited at the highest operating pressure from a group of test samples that exhibits no observable signs of damage to the substrate and setting this operating pressure as the upper limit of the range.
23. 23. The method of claim 22, wherein the characterization technique used comprises X-ray diffraction and the distinctive features comprise characteristic X-ray diffraction peaks of the layered oxide material.
24. 24. The method of any one of claims 19 to 23, wherein the test sample of the method comprises an average value for a number of test samples, the method according to any one of claims 4 to 18 being carried out a number of times at the same working pressure or working distance and the average value being taken.
25. 25. The method of any one of claims 22 to 24, further comprising selecting an optimal operating pressure for the system within a range of optimal operating pressures, the optimal operating pressure being the operating pressure within the range of optimal operating pressures that results in the highest deposition rate.
26. 26. A method of manufacturing a battery, the method comprising any of claims 1 to 25.
Citation Information
Patent Citations
JP1974101273A
Forming device and forming method of electrode for lithium secondary battery
JP2003007291A
Oxide sintered body sputtering target for forming positive electrode film and method for manufacturing the same
JP2017186581A
Lithium vanadium oxide thin-film battery
US20040048157A1
High density plasma source
WO2011131921A1