Carbon nanotube structure and method for producing the same
The carbon nanotube structure with end-to-side wall joints, manufactured via oxidation and bonding, addresses the challenge of creating three-dimensional structures with improved properties and stability.
Patent Information
- Application Number
- JP2021062122
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-31
- Publication Date
- 2024-09-25
- Estimated Expiration
- 2041-03-31
AI Technical Summary
Existing methods for manufacturing carbon nanotube structures face difficulties in creating three-dimensional structures due to challenges in joining carbon nanotubes between side walls.
A carbon nanotube structure with joints between the ends and side walls of carbon nanotubes, achieved through an oxidation removal process to remove ends and sidewalls, followed by a joining process using linker molecules to form amide bonds.
Enables the easy fabrication of three-dimensional structures with enhanced electrical conductivity and tensile strength, while making the structure resistant to decomposition by acids or alkalis.
Smart Images

Figure 0007555544000001 
Figure 0007555544000002 
Figure 0007555544000003
Abstract
Description
[Technical field]
[0001] FIELD OF THE DISCLOSURE The present disclosure relates to carbon nanotube structures and methods for making carbon nanotube structures. [Background technology]
[0002] Carbon nanotubes are attracting attention as a substitute for metals used in power lines and signal lines because they are lightweight and have excellent properties such as electrical conductivity, current carrying capacity, elasticity, and mechanical strength. Carbon nanotubes are used, for example, as a material for structures such as wires, and are added to resins to improve their strength.
[0003] Patent Document 1 discloses a carbon nanotube aggregate having a plurality of carbon nanotubes and a bridge structure formed between the plurality of carbon nanotubes by organic molecules. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2018-115087 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, the technique described in Patent Document 1 has a problem in that it is difficult to manufacture a three-dimensional structure because the carbon nanotubes are joined between their side walls.
[0006] The present disclosure has been made to solve the above-mentioned problems, and aims to provide a carbon nanotube structure that enables easy production of three-dimensional structures, and a method for producing the carbon nanotube structure. [Means for solving the problem]
[0007] In order to solve the above problems, the carbon nanotube structure of the present disclosure is a carbon nanotube structure formed by assembling a plurality of carbon nanotubes, and has joints between the ends of the carbon nanotubes and between the ends of the carbon nanotubes, and joints between the ends of the carbon nanotubes and a side wall portion.
[0008] The method for manufacturing a carbon nanotube structure according to the present disclosure is a method for manufacturing a carbon nanotube structure comprising an assembly of multiple carbon nanotubes, and includes an oxidation removal process for oxidizing and removing the ends and side wall portions of the carbon nanotubes between the carbon nanotubes, and a joining process for obtaining a carbon nanotube structure by joining the ends of the carbon nanotubes, as well as the ends and side wall portions. Effect of the Invention
[0009] According to the carbon nanotube structure and the manufacturing method of the carbon nanotube structure of the present disclosure, it is possible to provide a carbon nanotube structure and a manufacturing method of the carbon nanotube structure that can easily manufacture a three-dimensional structure. [Brief description of the drawings]
[0010] [Figure 1] 1 is a schematic diagram of a carbon nanotube. [Diagram 2] FIG. 2 is a diagram showing a joint between the ends of a single-walled carbon nanotube and another single-walled carbon nanotube. [Diagram 3] FIG. 2 shows a junction between an end of a single-walled carbon nanotube and a sidewall of the single-walled carbon nanotube. [Figure 4] FIG. 2 is a diagram showing nitrogen adsorption isotherms obtained by performing a nitrogen gas adsorption method on various carbon nanotube aggregates and carbon nanotube structures. [Diagram 5] FIG. 2 is a diagram obtained by measuring the pores and their pore volumes for various carbon nanotube aggregates and carbon nanotube structures. [Figure 6] FIG. 4 is a diagram showing optical absorption spectra of a carbon nanotube structure before and after a bonding process. [Figure 7] FIG. 2 is a schematic diagram of single-walled carbon nanotubes after an oxidative removal process. [Figure 8] 1 is a TEM photograph of single-walled carbon nanotubes after an oxidation removal process. [Figure 9] 1 is a TEM photograph of single-walled carbon nanotubes after an oxidation removal process. [Figure 10] FIG. 1 is a graph showing the relationship between the heating temperature and the weight reduction rate, the surface area, and the pore volume in dry oxidation removal. [Figure 11] 1 is a diagram obtained by XPS measurement of carbon nanotubes after dry oxidation removal at 723K. [Figure 12] FIG. 2 is a graph showing the relationship between the reaction time with 30% hydrogen peroxide solution and the weight loss rate and surface area in wet oxidation removal. [Figure 13] FIG. 13 is a diagram for explaining a preferred amount of linker molecules to be added in the bonding step. [Figure 14] FIG. 13 is a diagram for explaining a preferred amount of linker molecules to be added in the bonding step. [Figure 15] FIG. 1 shows the electrical conductivity and tensile strength of various carbon nanotube aggregates and carbon nanotube structures. [Figure 16] FIG. 2 is a diagram showing nitrogen adsorption isotherms obtained in the examples. [Figure 17] FIG. 2 is a diagram showing the relationship between pores and pore volumes obtained in the examples. [Figure 18] FIG. 2 is a diagram showing infrared absorption spectra obtained in the examples. [Figure 19] 3 is a TEM photograph of a carbon nanotube structure obtained in an example. [Figure 20] 3 is a TEM photograph of a carbon nanotube structure obtained in an example. [Figure 21] 3 is a TEM photograph of a carbon nanotube structure obtained in an example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, a carbon nanotube structure and a method for manufacturing the carbon nanotube structure according to an embodiment of the present disclosure will be described with reference to FIGS.
[0012] (Carbon nanotube structure) A carbon nanotube structure according to an embodiment of the present disclosure has joints between the ends of the carbon nanotubes and joints between the ends of the carbon nanotubes and sidewalls.
[0013] (Carbon Nanotubes) As shown in Figure 1, carbon nanotube 10 has a cap-shaped end 1 and a cylindrical side wall 2. Carbon nanotube 10 is mainly composed of six-membered rings in which carbon atoms are arranged in a hexagon. End 1 contains five-membered rings in which carbon atoms are arranged in a pentagon. A single-walled carbon nanotube has a single layer of tubes, while a multi-walled carbon nanotube has multiple tubes of different diameters stacked in layers. 1 is a single-walled carbon nanotube. In the following description, the numbers given in FIG. 1 will be omitted.
[0014] Here, the carbon nanotubes constituting the carbon nanotube structure according to the embodiment of the present disclosure may be single-walled carbon nanotubes or multi-walled carbon nanotubes.
[0015] (joint part) When the carbon nanotube structure according to the present disclosure is observed by a TEM (transmission electron microscope), the junctions between the ends of the carbon nanotubes and between the ends of the carbon nanotubes and the sidewalls can be observed, as shown in Figures 2 and 3. Figures 2 and 3 are observation photographs obtained by TEM observation using a method described below. Figure 2 is a diagram showing the junctions between the ends of single-walled carbon nanotubes. Figure 3 is a diagram showing the junctions between the ends of single-walled carbon nanotubes and the sidewalls of single-walled carbon nanotubes.
[0016] (Method of observing the joint) A method for observing the joints in the carbon nanotube structure will be described. As the TEM, for example, a double spherical aberration corrected transmission electron microscope JEOL2100F manufactured by JEOL Ltd. can be used. With an acceleration voltage of 80 kV, 15 to 20 fields of view are photographed at a magnification range of 500,000 to 1.5 million times. In the obtained observation photograph, the presence or absence of a joint between the ends of the carbon nanotubes and a joint between the end of the carbon nanotube and a side wall portion is confirmed. When at least one joint between the ends of the carbon nanotubes and a joint between the end of the carbon nanotube and a side wall portion are observed in the obtained observation photograph, it is determined that the carbon nanotube structure has a joint between the ends of the carbon nanotubes and a joint between the end of the carbon nanotube and a side wall portion.
[0017] The carbon nanotube structure according to the embodiment of the present disclosure may have a joint between the sidewalls of the carbon nanotube.
[0018] (Nitrogen adsorption amount) In the carbon nanotube structure according to the embodiment of the present disclosure, the nitrogen adsorption amount is 100 ml (STP) / g or less when the relative pressure P / P0 is 0 to 0.3 in the nitrogen adsorption isotherm. In other words, in the nitrogen adsorption isotherm, the nitrogen adsorption amount does not exceed 100 ml (STP) / g when the relative pressure P / P0 is in the range of 0 to 0.3. The nitrogen adsorption isotherm can be obtained by a nitrogen gas adsorption method.
[0019] Fig. 4 shows nitrogen adsorption isotherms obtained by performing nitrogen gas adsorption on various carbon nanotube aggregates and carbon nanotube structures. Fig. 4 shows that the carbon nanotube structure according to the embodiment of the present disclosure has a lower nitrogen adsorption amount than other examples, and when the relative pressure P / P0 is 0 to 0.3, the nitrogen adsorption amount is 100 ml (STP) / g or less. On the other hand, it can be seen that the nitrogen adsorption amount of the untreated carbon nanotube aggregate and the carbon nanotube aggregate after oxidative removal increases as the relative pressure P / P0 increases.
[0020] The amount of nitrogen adsorption is approximately proportional to the surface area. In other words, the carbon nanotube structure according to the embodiment of the present disclosure, which has a small amount of nitrogen adsorption, has a smaller surface area than the other examples shown in Figure 4. This is believed to be because the carbon nanotubes, which have pores at the ends and sidewalls, are joined together to block the pores.
[0021] (Method for measuring nitrogen adsorption amount) A method for measuring the amount of nitrogen adsorption in a carbon nanotube structure will be described. The apparatus used is, for example, an autosorb iQ2 (Quantachrome) manufactured by Anton-Paar. Pretreatment is performed at 300 to 500 K for 2 to 4 hours, and the measurement temperature is set to 77 K, and the amount of nitrogen adsorption is measured by nitrogen gas adsorption method. The nitrogen adsorption isotherm is obtained from the measured relative pressure and the amount of nitrogen adsorption.
[0022] (Ratio of nitrogen adsorption before and after bonding) In the carbon nanotube structure according to the embodiment of the present disclosure, the nitrogen adsorption isotherm when the relative pressure P / P0 is 0 to 0.3 is divided by the nitrogen adsorption amount before bonding is 0.1 to 0.3. The reason why the nitrogen adsorption amount decreases after bonding (after the bonding step) is considered to be that the carbon nanotubes having pores in the ends and sidewalls are bonded to each other, blocking the pores and reducing the surface area.
[0023] The nitrogen adsorption amount ratio before and after bonding is obtained by obtaining nitrogen adsorption isotherms by the above-mentioned method before and after the bonding step, and determining the nitrogen adsorption amount ratio at each relative pressure P / P0.
[0024] (pore volume) In the carbon nanotube structure according to the embodiment of the present disclosure, the volume of a pore having a diameter of 2 nm is 0.15 cm 3 / nm·g or less.
[0025] 5 is a diagram obtained by measuring the pores and their pore volumes for various carbon nanotube aggregates and carbon nanotube structures. As shown in FIG. 5, the carbon nanotube structure according to the embodiment of the present disclosure has a small volume of pores with a diameter of 3 nm or more. Also, the volume of pores with a diameter of 2 nm is smaller than that of other examples. On the other hand, the untreated carbon nanotube aggregate and the carbon nanotube aggregate after oxidative removal have a large volume of pores with a diameter of 2 nm. Also, the untreated carbon nanotube aggregate has a large volume of pores with a diameter of 3 to 8 nm.
[0026] In the carbon nanotube structure according to the embodiment of the present disclosure, the volume of the pores with a diameter of 2 nm and the volume of the pores with a diameter of 3 nm or more are small because the pores are blocked by carbon nanotubes having pores in their ends and side walls being joined together.
[0027] (Method of measuring pore volume and pore distribution) The pore volume can be obtained by obtaining a nitrogen adsorption isotherm by the nitrogen gas adsorption method described above and calculating the pore distribution by the DFT method (density functional theory).
[0028] (Optical absorption spectrum) In the carbon nanotube structure according to the embodiment of the present disclosure, the difference between the first absorption peak and the first absorption peak before joining is 20 to 90 nm.
[0029] Fig. 6 is a diagram showing the optical absorption spectra of the carbon nanotube structure before and after the bonding process. As shown in Fig. 6, it can be seen that the difference between the first absorption peak after the bonding process (at a wavelength of 840 nm in Fig. 6) and the first absorption peak before the bonding process (at a wavelength of 788 nm in Fig. 6) is 52 nm.
[0030] The shift of the first absorption peak to the longer wavelength side through the bonding process is believed to be due to an increase in the number of amide bonds between the carbon nanotubes. The presence or absence of an amide bond can be determined by obtaining an infrared absorption spectrum of the carbon nanotube structure.
[0031] (Method of measuring optical absorption spectrum) The method for measuring the optical absorption spectrum will be described. The apparatus used is, for example, V-670 manufactured by JASCO Corp. The optical absorption spectrum is measured with a measurement range of 200 to 2500 nm, a scan speed of 200 nm / min, and a measurement interval of 0.1 nm.
[0032] (Method of manufacturing carbon nanotube structure) A method for manufacturing a carbon nanotube structure according to an embodiment of the present disclosure includes an oxidation removal process for oxidizing and removing the ends and side wall portions of a carbon nanotube, and a joining process for obtaining a carbon nanotube structure by joining the ends and the side wall portions of the carbon nanotubes.
[0033] (Oxidation removal process) The oxidation removal process is a process for oxidizing and removing the ends and sidewalls of carbon nanotubes. FIG. 7 is a schematic diagram of a single-walled carbon nanotube after the oxidation removal process. As shown in FIG. 7, the end and part of the sidewall of the single-walled carbon nanotube are oxidized and removed by the oxidation removal process. FIG. 8 and FIG. 9 are TEM photographs of the single-walled carbon nanotube after the oxidation removal process. In particular, looking at the area indicated by the arrow in FIG. 8, it can be seen that the end of the single-walled carbon nanotube has been oxidized and removed. The oxidative removal referred to here means breaking the carbon bonds of the five- or six-membered rings of the carbon nanotubes and adding oxygen to the broken sites to make them functional. Oxidative removal applies to both dry and wet methods, and to both single-walled and multi-walled (two or more layers) carbon nanotubes.
[0034] As a method for oxidizing and removing the ends and sidewalls of carbon nanotubes, dry oxidation removal and wet oxidation removal can be used.
[0035] (Dry oxidation removal) The cap-shaped ends of carbon nanotubes contain five-membered rings that are more reactive than the sidewalls, and therefore the ends of carbon nanotubes are more easily oxidized by heating than the sidewalls. Therefore, in the case of dry oxidation removal, the sidewalls of carbon nanotubes are also oxidized and removed, but the ends of the carbon nanotubes are oxidized and removed preferentially.
[0036] An example of the method for dry oxidation removal is a method in which carbon nanotubes are placed in a reaction tube, and the reaction tube is heated in an electric furnace while introducing dry air into the reaction tube.
[0037] By adjusting the heating temperature, oxygen concentration and heating time during dry oxidation removal, the degree of oxidative removal of the ends and sidewalls of the carbon nanotubes can be controlled.
[0038] Fig. 10 shows the relationship between the heating temperature and the weight loss rate, surface area, and pore volume in dry oxidation removal. Fig. 10 shows that the surface area of a single-walled carbon nanotube with a diameter of 1.5 nm is maximized when the heating temperature is 773 K, and that of a single-walled carbon nanotube with a diameter of 2.0 nm is maximized when the heating temperature is 723 K. In other words, the amount of oxidized removal of the ends and sidewalls corresponds to a structure that can maximally effectively utilize the outer and inner surfaces of the carbon nanotube.
[0039] Fig. 11 is a diagram obtained by measuring the carbon nanotubes by XPS (X-ray Photoelectron Spectroscopy) after the dry oxidation removal at 723 K. Fig. 11 shows that functional groups are imparted to the carbon nanotubes by the dry oxidation removal.
[0040] (Wet oxidation removal) Wet oxidation removal is effective for removing both the ends and sidewalls of carbon nanotubes by oxidation. The wet oxidation removal method involves immersing carbon nanotubes in an acidic solution, such as a hydrogen peroxide solution or a nitric acid solution, heating and stirring or refluxing the solution to uniformly remove the desired areas by oxidation. The solution is then filtered and washed.
[0041] The degree of oxidation removal of the ends and sidewalls of the carbon nanotubes can be controlled by controlling the concentration of the acid solution, the reaction time, and the temperature. For example, when wet oxidation removal is performed using a 1 to 5 M aqueous nitric acid solution, the ends and sidewalls of the carbon nanotubes can be sufficiently oxidized and removed by setting the reaction time to 4 hours or more.
[0042] Fig. 12 is a diagram showing the relationship between the reaction time with 30% hydrogen peroxide and the weight loss rate and surface area in wet oxidation removal. Fig. 12 shows that when wet oxidation removal is performed using 30% hydrogen peroxide, the surface area increases by setting the reaction time to 4 to 8 hours, and the ends and sidewalls of carbon nanotubes with a diameter of 2 nm can be sufficiently oxidized and removed.
[0043] Furthermore, according to Figure 4 mentioned above, the carbon nanotube structure made of carbon nanotubes after oxidative removal has a large amount of nitrogen adsorption, which indicates that the ends and side walls of the carbon nanotubes have been oxidized and removed, resulting in a larger surface area than the carbon nanotube structure made of untreated carbon nanotubes.
[0044] Furthermore, according to FIG. 5 mentioned above, the carbon nanotube structure made of the carbon nanotubes after oxidative removal has a large volume of pores with diameters of 1 to 3 nm, which indicates that the ends and side walls of the carbon nanotubes have been oxidized and removed.
[0045] (Joining process) The bonding process is a process for obtaining a carbon nanotube structure by bonding the ends of the carbon nanotubes oxidized and removed in the oxidative removal process, as well as the ends and sidewalls of the carbon nanotubes. Bonding is performed by mixing the carbon nanotubes after the oxidative removal process or the dispersion process described below with linker molecules. By mixing these, the oxidatively removed (functionalized) parts of the carbon nanotubes are bonded together by amide bonds. It is not necessary for all of the functionalized parts to be bonded. In other words, the functionalized parts may remain after the bonding process.
[0046] The linker molecule is preferably one in which two or more amino groups are bonded to a hydrocarbon or aromatic compound. An example of one in which two or more amino groups are bonded to a hydrocarbon is NH2-(CH2)n-NH2. n is preferably 2 to 18, more preferably 2 to 12. Examples of aromatic compounds with two or more amino groups bonded to them include 1,12-diaminododecane (DAD), 1,4-phenylenediamine (PDA), 3,3'-diaminobenzidine (DAB), 1,5-diaminonaphthalene (DAN), and 1,6-diaminopyrene (DAP).
[0047] In addition to the above-mentioned locations, the joining step may join the sidewalls of the carbon nanotubes. In addition to the carbon nanotubes and the linker molecules, a tertiary amine and a joining reagent may be added in multiple batches and mixed. The tertiary amine is added to deprotonate the carboxylic acid generated at the end or sidewall of the carbon nanotube. There is no particular limitation as long as the tertiary amine is used, but triethylamine is preferred. By adding the joining reagent, the carboxyl groups present at the end and sidewall of the carbon nanotube and the amino groups contained in the linker molecules are dehydrated and condensed to form amide bonds, thereby joining the carbon nanotubes. The reason for adding the joining reagent step by step is to efficiently proceed with the reaction involving the solid carbon nanotubes. There are no particular limitations on the conjugation reagent, and examples that can be used include 1H-benzotriazol-1-yloxytris(dimethylamino)phosphonium hexafluorophosphate (BOP), (benzotriazol-1-yloxy)tripyrrolidinophosphonium hexafluorophosphate (PyBOP), and 4-(4,6-dimethoxy-1,3,5-triazin-2-yl)-4-methylmorpholinium chloride (DMT-MM).
[0048] In addition, in the bonding step, it is preferable to add an appropriate amount of linker molecules. As shown in Fig. 13, if too much linker molecules are added, the number of bond chains will be greater than the functional groups imparted to the carbon nanotubes, and bonding by amide bonds may not be sufficient. As shown in Fig. 14, by adding an appropriate amount of linker molecules, bonding by amide bonds can be sufficient.
[0049] Fig. 15 is a diagram showing the electrical conductivity and tensile strength of a carbon nanotube aggregate before bonding (after oxidative removal), a carbon nanotube structure after bonding with an inappropriate amount of added linker molecules, and a carbon nanotube structure after bonding with an appropriate amount of added linker molecules. According to Fig. 15, the electrical conductivity of the carbon nanotube structure after bonding with an appropriate amount of added linker molecules is about 8 times higher and the tensile strength is about 5 times higher than that of the carbon nanotube aggregate before bonding, compared to before bonding. It is also found that the electrical conductivity and tensile strength of the carbon nanotube structure after bonding with an appropriate amount of added linker molecules are improved compared to the carbon nanotube structure after bonding with an inappropriate amount of added linker molecules.
[0050] (Dispersion process) The method for producing a carbon nanotube structure according to an embodiment of the present disclosure may include a dispersing step of dispersing aggregates (bundles) of carbon nanotubes before the oxidative removal step or between the oxidative removal step and the bonding step.
[0051] Carbon nanotubes tend to form aggregates due to the van der Waals forces between their sidewalls, and dispersing the aggregates of carbon nanotubes allows for more efficient bonding in the subsequent bonding step.
[0052] In the dispersion step, the aggregates of carbon nanotubes are mixed with a dispersant. As the dispersant, a dispersant containing a metal salt of a first metal and a second metal can be used. As the first metal, for example, one or more selected from the group consisting of Zn, Ni, Cu, Ag, Mg, and Pd can be used. As the second metal, a metal different from the first metal can be, for example, one or more selected from the group consisting of Al, Fe, Co, Ag, Gd, Cu, Ni, Mg, Li, K, and Ca. The dispersant that can be used in the embodiment according to the present disclosure can be an aqueous solvent or a non-aqueous solvent, or a mixture of an aqueous solvent and a non-aqueous solvent. As the non-aqueous solvent, chlorine-containing hydrocarbons (methylene chloride, chloroform, chlorobenzene, etc.), nitrogen-containing polar solvents (N,N-dimethylformamide, nitromethane, N-methylpyrrolidone, etc.), sulfur compounds (dimethyl sulfoxide, etc.), etc. can be used.
[0053] The dispersant can be produced by heating a solution containing an acetate of a first metal and a nitrate or chloride of a second metal. The acetate of the first metal can be, for example, one or more selected from the group consisting of zinc acetate (Zn(CH3COO)2·2H2O), nickel acetate (Ni(CH3COO)2·4H2O), copper acetate (Cu(CH3COO)2·H2O), silver acetate (Ag(CH3COO)2), magnesium acetate (Mg(CH3COO)2·4H2O) and palladium acetate (Pd(CH3COO)2). Nitrate or chloride salts of the second metal include, for example, aluminum nitrate (Al(NO3)3·9H2O), iron nitrate (Fe(NO3)3·9H2O), cobalt nitrate (Co(NO3)2·6H2O), silver nitrate (AgNO3), gadolinium nitrate (Gd(NO3)2·6H2O), copper nitrate (Cu(NO3)2·3H2O), nickel nitrate (Ni(NO3)2·6H2O), magnesium nitrate (Mg(NO3)2·6H2O), lithium nitrate (LiNO3), potassium nitrate (KNO3), calcium nitrate (CNO3), potassium nitrate (K ... a(NO3)2·4H2O), aluminum chloride (AlCl3·6H2O), iron chloride (FeCl3·6H2O), cobalt chloride (CoCl2·6H2O), silver chloride (AgCl), gadolinium chloride (GdCl2·6H2O), copper chloride (CuCl2·2H2O), magnesium chloride (MgCl2·6H2O), lithium chloride (LiCl), potassium chloride (KCl), calcium chloride (CaCl2·2H2O), and nickel chloride (NiCl2·6H2O).
[0054] In the dispersion process, in order to disperse the carbon nanotube aggregates, it is preferable to mix the carbon nanotube aggregates with a dispersant and then apply a predetermined amount of energy (vibration force, shear force, pressure, temperature, etc.) from the outside.
[0055] (Sintering process) The method for manufacturing a carbon nanotube structure according to an embodiment of the present disclosure may further include a sintering step of sintering the carbon nanotube structure after the bonding step, in which functional groups at the bonded portions bonded in the bonding step are removed to form carbon-carbon bonds. By sintering the carbon nanotube structure, the strength of the carbon nanotube structure can be further increased.
[0056] The sintering method is not particularly limited, but may be, for example, a method in which the carbon nanotube structure is preheated under reduced pressure conditions and then heated at 1200 to 2100 K for 2 to 15 hours. Preheating may be performed, for example, for 1 to 10 hours in a temperature range of 500 to 680 K. When heating to 1200 to 2100 K after preheating, the temperature increase rate is preferably 5 to 10 K / min.
[0057] (Action and effect) The carbon nanotube structure having the above configuration has joints between the ends of the carbon nanotubes and between the ends of the carbon nanotubes and the side walls, and therefore can be used to easily manufacture three-dimensional structures.
[0058] Furthermore, when carbon nanotubes are bonded to each other by ester bonds as in the above-mentioned Patent Document 1, the carbon nanotube structure is easily decomposed by acid or alkali. However, the carbon nanotube structure having the above configuration is not easily decomposed by acid or alkali because the carbon nanotubes are bonded to each other by amide bonds.
[0059] The manufacturing method of the carbon nanotube structure having the above-mentioned configuration includes an oxidation removal process for oxidizing and removing the ends and side wall portions of the carbon nanotubes, and a joining process for obtaining a carbon nanotube structure by joining the ends and the ends, and the ends and the side wall portions of the carbon nanotubes, and therefore it is possible to manufacture a carbon nanotube structure that is suitable for use in manufacturing three-dimensional structures.
[0060] Furthermore, in the manufacturing method of the carbon nanotube structure having the above-mentioned configuration, by providing a dispersion step for dispersing carbon nanotube aggregates before the oxidative removal step or between the oxidative removal step and the bonding step, bonding can be performed more efficiently in the subsequent bonding step.
[0061] Moreover, in the method for manufacturing a carbon nanotube structure having the above-mentioned configuration, by providing a sintering step of sintering the carbon nanotube structure after the joining step, the strength of the carbon nanotube structure can be further increased.
[0062] Although the embodiments of the present disclosure have been described in detail above with reference to the drawings, the specific configuration is not limited to this embodiment, and design changes and the like that do not depart from the gist of the present disclosure are also included.
[0063] The carbon nanotube structure according to the embodiment of the present disclosure can be suitably used as a winding for a small transformer, a small, high-power motor, a generator for electric vehicles, ships, electric aircraft, etc., a composite resin with improved heat resistance, and a heat dissipation material.
[0064] <Additional Notes> The carbon nanotube structure described in each embodiment can be understood, for example, as follows.
[0065] The carbon nanotube structure of the first embodiment is a carbon nanotube structure formed by assembling a plurality of carbon nanotubes 10, and has joints between the ends 1 of the carbon nanotubes 10 and between the ends 1 of the carbon nanotubes 10, and joints between the ends 1 of the carbon nanotubes 10 and a side wall portion 2.
[0066] The carbon nanotube structure having the above-mentioned configuration has a joint between the ends 1 of the carbon nanotubes 10, and a joint between the ends 1 of the carbon nanotubes 10 and the side wall portions 2, and therefore can be suitably used for manufacturing three-dimensional structures. In addition, since the carbon nanotubes 10 are bonded to each other by amide bonds, the carbon nanotubes 10 are not easily decomposed by acids or alkalis.
[0067] In the carbon nanotube structure according to the second embodiment, the nitrogen adsorption isotherm shows a nitrogen adsorption amount of 100 ml(STP) / g or less when the relative pressure P / P0 is 0 to 0.3. This is because the carbon nanotubes 10 having pores at the end 1 and the side wall 2 are joined to each other, thereby blocking the pores.
[0068] In the carbon nanotube structure according to the third embodiment, the difference between the first absorption peak and the first absorption peak before bonding is 20 to 90 nm, because the carbon nanotubes 10 are bonded to each other via amide bonds.
[0069] In the carbon nanotube structure according to the fourth embodiment, the nitrogen adsorption isotherm has a value of 0.1 to 0.3 obtained by dividing the nitrogen adsorption amount when the relative pressure P / P0 is 0 to 0.3 by the nitrogen adsorption amount before bonding. This is because the pores are blocked by bonding the carbon nanotubes 10 having pores at the ends 1 and sidewalls 2 to each other.
[0070] The method for manufacturing the carbon nanotube structure described in each embodiment can be understood, for example, as follows.
[0071] The manufacturing method of the carbon nanotube structure of the first embodiment is a manufacturing method of a carbon nanotube structure comprising a plurality of carbon nanotubes 10, and includes an oxidation removal process of oxidizing and removing the ends 1 and side wall portions 2 of the carbon nanotubes 10 between the carbon nanotubes 10, and a joining process of joining the ends 1 and 1 of the carbon nanotubes 10, as well as the ends 1 and the side wall portions 2, to obtain a carbon nanotube structure.
[0072] The manufacturing method of the carbon nanotube structure having the above-mentioned configuration can manufacture a carbon nanotube structure having a joint between the ends 1 of the carbon nanotubes 10 and a joint between the ends 1 of the carbon nanotubes 10 and the sidewalls 2. Therefore, it is possible to manufacture a carbon nanotube structure that can be suitably used for manufacturing a three-dimensional structure. Furthermore, since a carbon nanotube structure in which the carbon nanotubes 10 are bonded together by amide bonds can be manufactured, a carbon nanotube structure that is not easily decomposed by acids or alkalis can be manufactured.
[0073] The method for producing a carbon nanotube structure according to the second aspect includes a dispersing step of dispersing aggregates of the carbon nanotubes 10 before the oxidative removal step or between the oxidative removal step and the joining step.
[0074] In the method for producing the carbon nanotube structure having the above-mentioned configuration, by dispersing the aggregates of the carbon nanotubes 10, bonding can be performed more efficiently in the subsequent bonding step.
[0075] A method for producing a carbon nanotube structure according to a third aspect includes a sintering step of sintering the carbon nanotube structure after the joining step.
[0076] In the method for producing a carbon nanotube structure having the above-mentioned configuration, the strength of the carbon nanotube structure can be further increased by sintering the carbon nanotube structure. EXAMPLES
[0077] An example will be described below. The conditions in the example are an example of conditions adopted to confirm the feasibility and effects of an embodiment of the present disclosure, and the embodiment of the present disclosure is not limited to this example of conditions.
[0078] The ends and side walls of the single-walled carbon nanotube aggregates were oxidized and removed by heating them in dry air to 450-750K at a temperature increase rate of 2-10K / min (dry oxidation removal). Next, the mixture of the dichloromethane and dimethylformamide dispersion and the carbon nanotube aggregates was stirred for 30 minutes using a magnetic stirrer. After stirring, it was visually confirmed that the carbon nanotube aggregates had been dispersed.
[0079] Next, the dispersed carbon nanotubes were mixed with linker molecules, triethylamine, and a conjugation reagent to conjugate the carbon nanotubes. 1,4-phenylenediamine (PDA) and 3,3'-diaminobenzidine (DAB) were used as linker molecules. 1H-benzotriazol-1-yloxytris(dimethylamino)phosphonium hexafluorophosphate (BOP) was used as a conjugation reagent. The linker molecules, triethylamine, and conjugation reagent were added in multiple portions at 0.5 M each. By the above method, a carbon nanotube structure was obtained.
[0080] Using the above-mentioned method, nitrogen adsorption isotherms and graphs showing the relationship between pores and pore volume were obtained for the carbon nanotube structure after bonding, the carbon nanotubes before bonding (after oxidative removal and dispersion), and the carbon nanotube aggregates before oxidative removal (untreated).
[0081] Further, infrared absorption spectra were obtained by performing measurements under the following conditions for the carbon nanotube structure after bonding and the carbon nanotubes before bonding (after oxidation removal and dispersion). Measurement method: KBr pellet method (φ7mm) Sample concentration: 0.2wt% CNT Measurement range: 4000cm -1 ~500cm -1 Resolution: 1cm -1 Number of times accumulated: 1024 Measurement atmosphere: Nitrogen
[0082] Nitrogen adsorption isotherms are shown in Fig. 16. Fig. 16 shows that the carbon nanotube structure (bonded CNT) obtained in this example has a lower nitrogen adsorption amount, i.e., a smaller surface area, than the other examples. This shows that the pores formed at the ends and sidewalls of the carbon nanotubes are blocked by bonding these portions.
[0083] Fig. 17 shows the relationship between pores and pore volume. Fig. 17 shows that the carbon nanotube structure obtained in this example has a small volume of pores with a diameter of 3 nm or more, and a small volume of pores with a diameter of 2 nm compared to other examples. On the other hand, it can be seen that the untreated carbon nanotubes and the carbon nanotubes before bonding have a large volume of pores with a diameter of 2 nm. It can also be seen that the untreated carbon nanotubes have a large volume of pores with a diameter of 3 to 8 nm.
[0084] The infrared absorption spectrum is shown in Fig. 18. From Fig. 18, it is found that the carbon nanotube structure after bonding has an amide bond.
[0085] Next, the obtained carbon nanotube structure was sintered. Sintering was performed by preheating at 500-680K for 10 hours under reduced pressure conditions, followed by heating at a temperature of 1273-2073K for 1-5 minutes at a temperature increase rate of 5-10K / min. For sintering, an electric furnace, a NEWTONIAN Pascal-40 VP04-A45 ultra-high temperature vacuum / atmosphere furnace manufactured by Nagano Corporation, was used.
[0086] After sintering, the bonded portions were confirmed by TEM observation. Photographs taken by TEM observation are shown in Figures 19 to 21. From Figures 18 to 21, it can be confirmed that the carbon nanotubes are bonded to each other. [Explanation of symbols]
[0087] 1...End 2…Side wall 10…Carbon nanotube
Claims
1. A carbon nanotube structure in which a plurality of carbon nanotubes are assembled, A carbon nanotube structure having carbon nanotube end-to-end junctions between the carbon nanotubes and junctions between the carbon nanotube ends and sidewalls.
2. In the nitrogen adsorption isotherm, the relative pressure P / P 0 2. The carbon nanotube structure according to claim 1, wherein the nitrogen adsorption amount is 100 ml (STP) / g or less when the ratio is 0 to 0.
3.
3. 3. The carbon nanotube structure according to claim 1, wherein a difference between the first absorption peak and the first absorption peak before joining is 20 to 90 nm.
4. In the nitrogen adsorption isotherm, the relative pressure P / P 0 4. The carbon nanotube structure according to claim 1, wherein a value obtained by dividing the nitrogen adsorption amount when is 0 to 0.3 by the nitrogen adsorption amount before joining is 0.1 to 0.
3.
5. A method for manufacturing a carbon nanotube structure comprising an assembly of multiple carbon nanotubes, comprising: an oxidation removal process for oxidizing and removing the ends and side wall portions of the carbon nanotubes between the carbon nanotubes; and a joining process for obtaining a carbon nanotube structure by joining the ends of the carbon nanotubes, as well as the ends and side wall portions.
6. The method for producing a carbon nanotube structure according to claim 5 , further comprising a dispersing step of dispersing aggregates of the carbon nanotubes before the oxidative removal step or between the oxidative removal step and the joining step.
7. The method for producing a carbon nanotube structure according to claim 5 or 6, further comprising a sintering step of sintering the carbon nanotube structure after the joining step.
Citation Information
Patent Citations
Macroscopically arranged assemblies of carbon nanotubes
JP2003512286A
Polymer-modified nanoscale carbon tube and its manufacturing method
JP2006028421A
T type structure nanotube, field effect transistor, and manufacturing method thereof
JP2006228864A
Single wall carbon nanotube heterojunction, its manufacturing method, semiconductor device, and its manufacturing method
JP2008105906A
Electrode body, manufacturing method thereof and electric double-layer capacitor
JP2008192695A