Chemical vapor deposition raw material, atomic layer deposition raw material, and method for producing tin-containing thin film
Bis(alkylcyclopentadienyl)tin or bis(alkyltetramethylcyclopentadienyl)tin precursors address the inefficiencies of existing tin precursors by providing high vapor pressure and reactivity, enabling efficient formation of tin(II) oxide thin films for transparent conductive films.
Patent Information
- Application Number
- JP2023069076
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-04-20
- Publication Date
- 2024-09-25
- Estimated Expiration
- 2039-08-09
AI Technical Summary
Existing tin-containing precursors for chemical vapor deposition have low vapor pressure and strong Sn-O or Sn-N bonds, making it difficult to form large-area tin and tin oxide thin films efficiently, particularly tin(II) oxide films, which are desirable for transparent conductive films.
Employing bis(alkylcyclopentadienyl)tin or bis(alkyltetramethylcyclopentadienyl)tin as precursors for chemical vapor deposition, which have high vapor pressure and form divalent tin compounds, enabling efficient formation of tin(II) oxide thin films using ALD methods.
The use of these precursors allows for the efficient formation of n-type or p-type tin oxide thin films, particularly p-type transparent conductive films, by optimizing vapor pressure and reactivity for improved process efficiency.
Smart Images

Figure 0007555624000001 
Figure 0007555624000002 
Figure 0007555624000003
Abstract
Description
[Technical Field]
[0001] The present invention relates to a chemical compound containing a precursor of a tin thin film or a tin oxide thin film as a main component. gas phase The present invention relates to a deposition material and a method for producing a thin film containing tin. [Background technology]
[0002] Transparent conductive films have high electrical conductivity and high optical transparency in the visible light region, and are therefore used as electrodes for various photoelectric conversion elements, including light-receiving elements, such as solar cells, flat panel displays, and touch screens. Furthermore, because they have excellent reflection and absorption properties in the near-infrared region, they are also used as heat-reflecting films, transparent heaters, transparent electromagnetic wave shields, and antistatic films.
[0003] Materials commonly used for such transparent conductive films include tin(IV) oxide (SnO2), which contains dopants such as antimony and fluorine, zinc oxide (ZnO), which contains dopants such as aluminum, gallium, indium, and tin, and indium(III) oxide (In2O3), which contains dopants such as tin, tungsten, and titanium. In particular, indium oxide (ITO) films, which contain tin as a dopant, are widely used industrially because they can easily produce low-resistance transparent conductive films.
[0004] Such transparent conductive oxide films are manufactured using methods such as sputtering, chemical vapor deposition, and ion plating. Among these, thin films of metal oxides with precursors with relatively high vapor pressures, such as tin oxide and zinc oxide, can be easily formed by chemical vapor deposition (CVD) methods such as atomic layer deposition (ALD).
[0005] Tetraalkyltin, a tetravalent tin compound, is commonly used as a tin precursor. In addition to tetraalkyltin, for example, divalent tin complexes and tin aminoalkoxide complexes are disclosed in Patent Document 1 as precursors for tin and tin oxide thin films. In the tin aminoalkoxide complexes, a dialkylamino group is coordinated to tin as a new ligand, which not only improves thermal stability and volatility without causing carbon or halogen contamination, but also allows tin and tin oxide thin films to be easily formed at lower temperatures. In addition, Patent Document 2 discloses that bis(diisopropylamino)dimethyltin (Sn[N( i Furthermore, Non-Patent Document 1 uses a divalent tin complex, N,N'-tert-butyl-1,1-dimethylethyleneamine tin. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Laid-Open No. 2009-227674 [Patent Document 2] Japanese Patent Application Publication No. 2018-90586 [Non-patent literature]
[0007] [Non-Patent Document 1] Jung-Hoon Lee, Mi Yoo, DongHee Kang, Hyun-Mo Lee, Wan-ho Choi, Jung Woo Park, Yeonjin Yi, Hyun You Kim, and Jin-Seong Park, ACS Applied Materials & Interfaces 10 (39), 33335-33342(2018) Summary of the Invention [Problem to be solved by the invention]
[0008] However, in the tin aminoalkoxide complex of Patent Document 1, the bond between the tin atom and the ligand, Sn—O or Sn—N, is relatively strong. Also, the vapor pressure of the tin aminoalkoxide complex is 10 -2 Because of the high pressure of torr, in order to form large-area tin and tin oxide thin films using chemical vapor deposition, it is desirable to increase the vapor pressure and reactivity in order to improve the efficiency of the process. Furthermore, the tin complex of Patent Document 2 has a relatively high vapor pressure of 0.6 Torr at 80°C, but because tin is tetravalent, it is difficult to form a tin(II) oxide film. Widely used tetraalkyltins are also tetravalent, so it is similarly difficult to form a tin(II) oxide film. Furthermore, the vapor pressure of the tin complex of Non-Patent Document 1 is 0.2 Torr at 75°C, but like Patent Document 1, this complex also has a relatively strong bond between the tin atom and the Sn-N ligand.
[0009] The present invention relates to bis(alkylcyclopentadienyl)tin or bis(alkyltetramethylcyclopentadienyl)tin as precursors for tin thin films or tin oxide thin films, which have high vapor pressure even at low temperatures, and chemical compounds containing these precursors as their main components. gas phase Vapor deposition raw materials and related chemicals gas phase The object of the present invention is to provide a method for producing a tin-containing thin film by the ALD method using a deposition raw material. [Means for solving the problem]
[0010] The present invention comprises the following items. The chemistry of the present invention gas phase The deposition material is characterized by containing bis(alkylcyclopentadienyl)tin or bis(alkyltetramethylcyclopentadienyl)tin represented by the following formula (1) as a main component. [ka] In formula (1), R 1 and R 2each independently represents hydrogen or an alkyl group having 6 or less carbon atoms, and R 3 and R 4 each independently represents an alkyl group having 6 or less carbon atoms.
[0011] The present invention The atomic layer deposition raw material is a raw material for producing a tin-containing thin film using the atomic layer deposition method, and is characterized by containing bis(alkylcyclopentadienyl)tin or bis(alkyltetramethylcyclopentadienyl)tin represented by the following formula (1) as a main component. [ka] In formula (1), R 1 and R 2 each independently represents hydrogen or an alkyl group having 6 or less carbon atoms, and R 3 and R 4 each independently represents an alkyl group having 6 or less carbon atoms.
[0012] The method for producing a tin-containing thin film of the present invention comprises the steps of: In the chemical vapor deposition method, a chemical vapor deposition source containing bis(alkylcyclopentadienyl)tin or bis(alkyltetramethylcyclopentadienyl)tin represented by the following formula (1) is vaporized in a source container of a chemical vapor deposition apparatus, and the vaporized bis(alkylcyclopentadienyl)tin or bis(alkyltetramethylcyclopentadienyl)tin is supplied to a substrate in a reaction chamber. . [ka] In formula (1), R 1 and R 2 each independently represents an alkyl group having 6 or less carbon atoms, and R 3 and R 4 each independently represents an alkyl group having 6 or less carbon atoms. In the manufacturing method, the chemical vapor deposition is preferably an atomic layer deposition method, and the tin-containing thin film is specifically a tin(II) oxide thin film. Furthermore, in the manufacturing method, water is preferably used as an oxidizing agent. [Effects of the Invention]
[0013] According to the present invention, by using bis(alkylcyclopentadienyl)tin or bis(alkyltetramethylcyclopentadienyl)tin as a precursor with a high vapor pressure and appropriately selecting an oxidizing agent, it is possible to efficiently form n-type or p-type tin oxide thin films by chemical vapor deposition, specifically ALD. The present invention is particularly suitable for forming tin(II) oxide thin films, which are p-type transparent conductive films. DETAILED DESCRIPTION OF THE INVENTION
[0014] The chemistry of the present invention gas phaseThe deposition material contains, as a main component, bis(alkylcyclopentadienyl)tin represented by the following formula (1) or bis(alkyltetramethylcyclopentadienyl)tin represented by the following formula (1). In this specification and the like, chemical vapor deposition (method) refers to chemical vapor deposition (method). The same applies hereinafter. [ka]
[0015] Tin can usually be in divalent or tetravalent oxidation states. Divalent tin compounds have strong ionic bonding properties and are reducing, while tetravalent tin compounds have strong covalent bonding properties. Bis(alkylcyclopentadienyl)tin or bis(alkyltetramethylcyclopentadienyl)tin, represented by the above formula (1), is a divalent tin compound.
[0016] In formula (1), R 1 and R 2 each independently represents hydrogen or an alkyl group having 6 or less carbon atoms, and R 3 and R 4 Each independently represents an alkyl group having 6 or less carbon atoms. If the number of carbon atoms is too large, the precursor becomes bulky and the amount of adsorption during ALD decreases. 1 , R 2 , R 3 and R 4 has 6 or less carbon atoms, preferably 4 or less carbon atoms. Alkyl groups having four or fewer carbon atoms include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, and tert-butyl groups.
[0017] R 1 and R 2 are preferably all hydrogen or all the same number of carbon atoms, more preferably all 2 or 3 carbon atoms, and particularly preferably all 2-carbon ethyl groups.
[0018] R 3 and R 4Preferably, all of the groups have the same number of carbon atoms, more preferably all of the groups have 1 to 3 carbon atoms, and particularly preferably all of the groups are methyl groups having 1 carbon atom. Furthermore, from the viewpoint of the amount of adsorption in ALD, bis(alkylcyclopentadienyl)tin is more preferable than bis(alkyltetramethylcyclopentadienyl)tin.
[0019] The chemistry of the present invention gas phase The deposition material may be either solid or liquid as long as it has a high vapor pressure and is easily vaporized during chemical vapor deposition. However, from the viewpoint of process efficiency, it is preferable that the material be liquid at 23°C. gas phase The melting point of bis(alkylcyclopentadienyl)tin or bis(alkyltetramethylcyclopentadienyl)tin, which is the main component of the deposition material, is lower than room temperature, preferably lower than 35°C, and more preferably lower than 23°C.
[0020] In addition, R 1 and R 2 Biscyclopentadienyltin, where R is hydrogen, is a solid at 23°C, and its vapor pressure at 80°C is 0.1 torr. 1 and R 2 Bis(ethylcyclopentadienyl)tin, where is an ethyl group, is a liquid at 23°C, and has a vapor pressure of 1.2 torr at 80°C and 2.3 torr at 100°C.
[0021] In order to carry out chemical vapor deposition, it is necessary to use a compound with a high vapor pressure as a precursor. gas phase The deposition material is preferably liquid at 23° C. and has a high vapor pressure even at low temperatures. The vapor pressure of bis(alkylcyclopentadienyl)tin or bis(alkyltetramethylcyclopentadienyl)tin represented by formula (1) in the present invention is 0.05 to 10 torr at 80° C., and is therefore suitable for thin film formation by CVD, particularly ALD.
[0022] The chemistry gas phaseIn the deposition raw material, the content of bis(alkylcyclopentadienyl)tin or bis(alkyltetramethylcyclopentadienyl)tin represented by formula (1) should be close to 100 wt%. Specifically, the content of bis(alkylcyclopentadienyl)tin or bis(alkyltetramethylcyclopentadienyl)tin is preferably close to 100 wt%. gas phase The content of the bis(alkylcyclopentadienyl)tin or bis(alkyltetramethylcyclopentadienyl)tin in the vapor deposition raw material is preferably 95 to 100 wt %, more preferably 99 to 100 wt %. However, a substance that does not react with or vaporize bis(alkylcyclopentadienyl)tin or bis(alkyltetramethylcyclopentadienyl)tin at the temperature at which the raw material is vaporized during chemical vapor deposition may be contained within a range that does not impair the object of the present invention.
[0023] The chemistry of the present invention gas phase The deposition material can be produced by various methods. For example, 1 and R 2 Bis(ethylcyclopentadienyl)tin, in which ethyl is an ethyl group, can be obtained in high yield as a yellow liquid product by adding a THF solution of tin(II) chloride to a solution of ethylcyclopentadiene and metallic potassium in THF at -78°C, stirring the mixture, and then distilling it under reduced pressure.
[0024] The chemistry of the present invention gas phase Thin films are formed using deposition materials by the CVD method. In CVD, a source container filled with bis(alkylcyclopentadienyl)tin or bis(alkyltetramethylcyclopentadienyl)tin, as represented by formula (1), is heated to vaporize the tin and then supplied to a reaction chamber. Vaporization can be performed using a typical CVD method for vaporizing organometallic compounds, such as by heating or reducing pressure in the source container of a CVD apparatus. The vaporized bis(alkylcyclopentadienyl)tin or bis(alkyltetramethylcyclopentadienyl)tin is then supplied to the substrate in the reaction chamber. The piping from the source container to the reaction chamber and the reaction chamber are maintained at a temperature at which the source material, bis(alkylcyclopentadienyl)tin or bis(alkyltetramethylcyclopentadienyl)tin, remains in a gaseous state without thermal decomposition, i.e., higher than the temperature of the source container (the temperature at which the source material is vaporized) but lower than the thermal decomposition temperature of the source material. In the chemical vapor deposition method of the present invention, the heating temperature is approximately 23 to 200°C. To increase the degree of freedom in setting the film formation temperature (substrate temperature), it is better to keep the heating temperature as low as possible. gas phase It is preferable that the deposition material has a sufficient vapor pressure at low temperatures.
[0025] Chemical vapor deposition methods include thermal CVD, which deposits materials by continuous thermal decomposition on a substrate, and ALD, which deposits materials one atomic layer at a time. gas phase The deposition material is suitable for the thermal CVD method, but is particularly suitable for the ALD method. In ALD, chemistry gas phase By alternately supplying deposition precursors and an oxidizing agent, a thin film of tin(II) oxide or tin(IV) oxide is formed on the substrate by the reaction of bis(alkylcyclopentadienyl)tin or bis(alkyltetramethylcyclopentadienyl)tin with the oxidizing agent, controlled at the atomic layer level. Examples of oxidizing agents include water, ozone, and plasma-activated oxygen. When water is used as the oxidizing agent, a thin film of tin(II) oxide, which is a p-type transparent conductive film, is formed. When ozone or plasma-activated oxygen is used, a thin film of tin(IV) oxide, which is an n-type transparent conductive film, is formed.
[0026] In ALD, (i) a gas-phase chemical reaction takes place in a chamber with a substrate placed on a heater. gas phase (ii) introducing a vapor source material and adsorbing the vapor source material onto the substrate; and (iii) removing excess chemicals from the chamber. gas phase The film is formed by repeating a film formation cycle consisting of (iii) a step of purging the deposition source material with an inert gas, (iv) a step of introducing a gaseous oxidizing agent and reacting it with bis(alkylcyclopentadienyl)tin or bis(alkyltetramethylcyclopentadienyl)tin on the substrate to form tin oxide, and (v) a step of purging excess oxidizing agent from the chamber with an inert gas. The number of film formation cycles varies depending on the area of the substrate and the thickness of the tin-containing thin film, but is usually 100 to 10,000 times.
[0027] The film formation temperature is set so that the substrate temperature is the same as the reaction temperature, and the substrate temperature is set lower than the temperature at which the adsorbed bis(alkylcyclopentadienyl)tin or bis(alkyltetramethylcyclopentadienyl)tin thermally decomposes, but high enough to sufficiently react with the oxidizing agent. In addition, chemistry gas phase The deposition raw materials and oxidizing agent are supplied in the gas phase from the outside to the reaction chamber where the substrate is placed, but they must be sublimated or evaporated at a temperature lower than the substrate temperature to prevent condensation on the substrate. gas phase When the deposition source material is solid at room temperature, it is difficult to control the gas phase supply rate using a flow rate control device. gas phase When the deposition source material is liquid at room temperature, the gas supply rate can be precisely and easily controlled using a flow rate controller, making it suitable for ALD. [Example]
[0028] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples. Example 1: Bis(ethylcyclopentadienyl)tin (Sn[C5H4(C2H5)]2) 400 ml of THF, 21.7 g (0.55 mol) of metallic potassium, and 70.8 g (0.75 mol) of ethylcyclopentadiene (C5H5(C2H5)) were placed in a 1 L four-neck flask and reacted for 26 hours. After that, the solvent was distilled off under reduced pressure at 40°C to obtain C5H4(C2H5)K. To the obtained C5H4(C2H5)K, 600 ml of THF and 50.7 g (0.27 mol) of SnCl2 were added at -78°C, and the mixture was stirred at room temperature for 23 hours. After that, the mixture was distilled under reduced pressure at 50°C to obtain a solid. The solid obtained was placed in a simple distillation apparatus and subjected to vacuum distillation twice at 110°C and 0.1 torr, yielding a yellow liquid in an amount of 61.3 g (0.20 mol), a yield of 76.2% (based on SnCl2).
[0029] The obtained sample was analyzed as follows (1)-(3), and was confirmed to be Sn[C5H4(C2H5)]2. (1) Composition analysis ICP emission spectroscopy of the liquid obtained by wet decomposition revealed that the Sn content was 38.2% (theoretical value: 38.9%). (2) 1 H-NMR Measurement conditions (apparatus: AVANCE NEO 500 (500 MHz), Bruker BioSpin, solvent: THF-d8, method: 1D) CH2C H 3, 1.15(6H,triplet)ppm:C H 2CH3, 2.48(4H,quartet)ppm:C5 H 4. 5.71 (4H, multiple) ppm: C5 H 4, 5.79 (4H, multiple) ppm (3) 13 C-NMR Measurement conditions (apparatus: AVANCE NEO 500 (125 MHz), Bruker BioSpin, solvent: THF-d8, method: 1D) 133.61, 110.31, 108.37ppm:C5, 22.53, 16.88 ppm: C2H5
[0030] Next, the vapor pressure was directly measured at 70-130°C using a pressure gauge (model: 121A, manufacturer: mks), and the following equation was obtained. log P(torr)=-1930 / T(K)+5.54 From this formula, the vapor pressure at 80°C was calculated to be 1.2 torr and the vapor pressure at 100°C to be 2.3 torr. Sn[C5H4(C2H5)]2 has a high vapor pressure and is said to have the volatility required for chemical vapor deposition. Furthermore, the synthesized Sn[C5H4(C2H5)]2 reacted with water at room temperature to produce a white solid. This indicates that water can be used as an oxidizing agent, and that ALD can be used to successfully form thin films of tin(II) oxide, which are p-type transparent conductive films.
[0031] [ Example 2 ]Dicyclopentadienyltin (Sn(C5H5)2) Dicyclopentadienyltin is not a new substance, as shown in Christoph Janiak, Z. Anorg. Allg. Chem. 2010, 636, 2387-2390, but it is a chemical compound. gas phase There are no reports of its use as a vapor deposition raw material. According to the above-mentioned literature, Sn(C5H5)2 is a solid at room temperature, but can be purified by sublimation at 80°C and 0.1 torr, and has the properties required for chemical vapor deposition.
[0032] [Comparative Example 1] Bis(dimethylamino-2-methyl-2-propoxy)tin (Sn(dmamp)2) In the synthesis method described in Example 1 of Patent Document 1, fractional distillation is performed at 100°C and 0.01 torr. Even at 100°C, the vapor pressure is only about 0.01 torr, making it difficult to use the vapor pressure alone for chemical vapor deposition, and requiring some ingenuity, such as the use of a bubbler.
Claims
1. The composition contains, as a main component, bis(alkylcyclopentadienyl)tin or bis(alkyltetramethylcyclopentadienyl)tin represented by the following formula (1): A source of atomic layer deposition material for producing tin-containing thin films by atomic layer deposition. 【Chemistry 1】 (In formula (1), R 1 and R 2 each independently represents hydrogen or an alkyl group having 6 or less carbon atoms; R 3 and R 4 each independently represents an alkyl group having 6 or less carbon atoms.
2. A method for producing a tin-containing thin film by atomic layer deposition, comprising vaporizing an atomic layer deposition source containing bis(alkylcyclopentadienyl)tin or bis(alkyltetramethylcyclopentadienyl)tin represented by the following formula (1) in a source container of a chemical vapor deposition apparatus, and supplying the vaporized bis(alkylcyclopentadienyl)tin or bis(alkyltetramethylcyclopentadienyl)tin to a substrate in a reaction chamber: 【Chemistry 2】 (In formula (1), R 1 and R 2 each independently represents hydrogen or an alkyl group having 6 or less carbon atoms; R 3 and R 4 each independently represents an alkyl group having 6 or less carbon atoms.
3. 3. The method for producing a tin-containing thin film according to claim 2, wherein the tin-containing thin film is a tin (II) oxide thin film.
4. 4. The method for producing a tin-containing thin film according to claim 3, wherein water is used as the oxidizing agent.
Citation Information
Patent Citations
Formation of inorganic film and solution therefor
JP1987182279A
Method for forming strontium-containing thin film
JP2009030162A
Novel tin aminoalkoxide complex and method for producing the same
JP2009227674A
Method for forming metal thin film, metal thin film, and device for forming metal thin film
JP2012184449A
Tin compound, method of synthesizing the same, tin precursor compound for ALD, and method of forming tin-containing material film
JP2018090586A