Sheet for forming protective film and method for processing sheet for forming protective film

The protective film-forming sheet with controlled release films addresses the issue of lifting and peeling during cutting, ensuring a high-quality protective film application on semiconductor wafers by minimizing adherence to the cutting blade and preventing float formation.

JP7555758B2Active Publication Date: 2024-09-25LINTEC CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020136431
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-08-12
Publication Date
2024-09-25
Estimated Expiration
2040-08-12

AI Technical Summary

Technical Problem

The issue of lifting and peeling during the cutting process of protective film-forming films, leading to marks and poor appearance, is prevalent due to the adherence of the film to the cutting blade, resulting in unintended peeling and deformation.

Method used

A protective film-forming sheet with a first release film and a second release film, where the first release film has a low surface elastic modulus and a specific probe tack value, ensuring minimal adherence to the cutting blade, and a controlled peeling force relationship between the films, preventing float formation and peeling.

Benefits of technology

The solution effectively suppresses float formation and peeling, maintaining the integrity of the film and preventing marks, ensuring a high-quality protective film application on semiconductor wafers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555758000005
    Figure 0007555758000005
  • Figure 0007555758000006
    Figure 0007555758000006
  • Figure 0007555758000007
    Figure 0007555758000007
Patent Text Reader

Abstract

To provide a protective film forming sheet in which the formation of float between a protective film forming film and a support film is suppressed even when the protective film forming film is cut out using a cutting blade, and a processing method for the protective film forming sheet.SOLUTION: A protective film forming sheet 1A includes a protective film forming film 10, and a first peeling film 20 peelably arranged on one main surface of the protective film forming film 10. A probe tack value of the protective film forming film 10 at 23°C is less than 6200 mN, the surface elastic modulus of the surface of the first peeling film 20 in contact with the protective film forming film 10 at 23°C is 17 MPa or less, and the product of the probe tack value and the surface elastic modulus is 66000 or less.SELECTED DRAWING: Figure 1A
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a sheet for forming a protective film and a method for processing the sheet for forming a protective film, and in particular to a sheet for forming a protective film that is less susceptible to lifting that may be the starting point for peeling or that may leave a mark on the protective film, and a method for processing the sheet for forming a protective film. [Background technology]

[0002] In recent years, semiconductor devices have been manufactured using a mounting method called flip chip bonding. In this mounting method, when mounting a semiconductor chip having a circuit surface on which convex electrodes such as bumps are formed, the circuit surface side of the semiconductor chip is inverted (face down) and bonded to the chip mounting part. This results in a structure in which the back side of the semiconductor chip on which no circuit is formed is exposed.

[0003] For this reason, a hard protective film made of an organic material is often formed on the back side of the semiconductor chip to protect the semiconductor chip from impact during transportation, etc. Such a protective film is formed, for example, in a cured or uncured state after a protective film-forming film is attached to the back side of the semiconductor wafer.

[0004] The protective film-forming film and the supporting film that supports the protective film-forming film constitute a long protective film-forming sheet. This long sheet is usually wound into a sheet roll before the protective film-forming film is used. When the protective film-forming film is used, the long protective film-forming sheet unwound from the sheet roll is cut into a shape substantially the same as that of the semiconductor wafer to be attached, and then attached to the semiconductor wafer.

[0005] Patent Document 1 discloses a long adhesive sheet in which a first sheet and a second sheet are provided on both sides of an adhesive layer. By subjecting this adhesive sheet to a punching process, the adhesive layer is separated into a punched portion and a continuous waste portion, and the adhesive layer in the punched portion is separated from the adhesive sheet together with a part of the first sheet in contact with the punched portion. The punched portion is attached as an adhesive film to, for example, the back surface of a semiconductor wafer. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] International Publication No. 2017 / 145735 Summary of the Invention [Problem to be solved by the invention]

[0007] When using the protective film-forming film, as described above, a protective film-forming film having a predetermined shape is cut out from the protective film-forming sheet. A punching blade is usually used to cut out the protective film-forming film. In the cutting process using the punching blade, the punching blade enters the protective film-forming film and cuts the protective film-forming film, reaching the middle of the support film and stopping. Next, by pulling out the punching blade, the protective film-forming film on the inside of the punching blade is completely separated from the protective film-forming film on the outside of the punching blade, and a protective film-forming film having a closed shape is obtained.

[0008] However, in the cutting process, the protective film-forming film and the punch blade come into contact with each other, so that the protective film-forming film is likely to adhere to the punch blade. Therefore, when the punch blade is pulled out, the protective film-forming film in the vicinity of the punch blade is pulled and deformed while still adhering to the punch blade, and is peeled off from the support film.

[0009] The portion where the protective film-forming film is peeled off from the support film becomes a floating portion. If such a floating portion occurs, in a process of removing the protective film-forming film on the outside of the punching blade to obtain the protective film-forming film on the inside of the punching blade, when the outer protective film-forming film is removed, the floating portion becomes a starting point for peeling, and the inner protective film-forming film that should remain is also unintentionally peeled off and removed.

[0010] In addition, the surface of the protective film-forming film at the portion peeled off from the support film is likely to have a mark due to peeling. The surface of the protective film-forming film that was in contact with the support film is exposed to the outside after the protective film-forming film is attached to the back surface of the wafer. Therefore, the portion peeled off from the support film and with the mark is also exposed to the outside. As a result, the mark causes a defective appearance of the protective film.

[0011] In addition, since such marks are formed when the protective film-forming film is peeled off from the support film, the marks tend to remain even if the protective film-forming film is re-adhered to the support film after peeling.

[0012] The present invention has been made in consideration of the above-mentioned circumstances, and aims to provide a sheet for forming a protective film, which suppresses the formation of a lift between a protective film-forming film and a support film, even when the protective film-forming film is cut out using a cutting blade, and a method for processing the sheet for forming a protective film. [Means for solving the problem]

[0013] The aspects of the present invention are as follows. [1] A protective film-forming film and a first release film releasably arranged on one main surface of the protective film-forming film, The probe tack value of the protective film-forming film at 23°C is less than 6200 mN; The surface elastic modulus of the surface of the first release film in contact with the protective film-forming film at 23°C is 17 MPa or less; The sheet for forming a protective film has a product of the probe tack value and the surface elastic modulus of 66,000 or less.

[0014] [2] The first release film is a sheet for forming a protective film described in [1], which has a substrate and a first release agent layer formed on one main surface of the substrate, and the first release agent layer is in contact with the protective film-forming film.

[0015] [3] A second release film is disposed releasably on the other main surface of the protective film-forming film, The sheet for forming a protective film according to [1] or [2], in which F1 and F2 satisfy the relationship F1>F2, where F1 is the peeling force of the first release film from the protective film-forming film and F2 is the peeling force of the second release film from the protective film-forming film.

[0016] [4] The sheet for forming a protective film according to any one of [1] to [3], wherein the thickness of the first release agent layer is within the range of 30 nm or more and 200 nm or less.

[0017] [5] When the protective film-forming sheet is viewed in plan, a cut is formed in the protective film-forming sheet so that a portion of the protective film-forming sheet has a predetermined closed shape, The sheet for forming a protective film according to any one of [1] to [4], wherein in the thickness direction of the sheet for forming a protective film, the incision penetrates the protective film-forming film and reaches a part of the first release film.

[0018] [6] A sheet for forming a protective film according to [5], wherein in a direction from the end face of the protective film-forming film having a closed shape toward the center of the protective film-forming film, the maximum distance between the end face and the portion where a lift formed between the protective film-forming film and the first release film is observed is less than 4 mm.

[0019] [7] A step of forming a cut so that a part of the sheet for forming a protective film according to any one of [1] to [4] has a predetermined closed shape, In the thickness direction of the sheet for forming a protective film, the cut penetrates the protective film-forming film and reaches a part of the first release film, which is a processing method for the sheet for forming a protective film. Effect of the Invention

[0020] According to the present invention, it is possible to provide a sheet for forming a protective film, in which the formation of a lift between the protective film-forming film and the support film is suppressed even when the protective film-forming film is cut out using a cutting blade, and a method for processing the sheet for forming a protective film. [Brief description of the drawings]

[0021] [Figure 1A] FIG. 1A is a schematic cross-sectional view of an example of a sheet for forming a protective film according to this embodiment. [Figure 1B] FIG. 1B is a schematic cross-sectional view of another example of the sheet for forming a protective film according to this embodiment. [Figure 2A] FIG. 2A is a perspective view for explaining a step of forming cuts in a long protective film forming sheet according to this embodiment. [Figure 2B] FIG. 2B is a schematic cross-sectional view of a long protective film forming sheet on which cuts are formed. [Figure 2C] FIG. 2C is a schematic cross-sectional view of a long protective film-forming sheet having cuts formed therein, from which the protective film-forming films other than the circular protective film-forming film and the second release film have been removed. [Figure 3A] FIG. 3A is a schematic cross-sectional view for explaining the formation of a float when the cutting blade is pulled out. [Figure 3B] FIG. 3B is a schematic cross-sectional view showing a laminate of a protective film-forming film in which a lift has been formed and a first release film. [Figure 3C] FIG. 3C is a schematic plan view showing a laminate of the protective film-forming film in which a lift has been formed and the first release film, as viewed from the direction of the arrow shown in FIG. 3B. [Figure 3D]FIG. 3D is a schematic cross-sectional view for explaining that in the sheet for forming a protective film according to this embodiment, the formation of lifting is suppressed when the cutting blade is pulled out. [Figure 4] FIG. 4 is a schematic cross-sectional view showing that the first release film and the second release film have a first release agent layer and a second release agent layer. [Diagram 5] FIG. 5 is a perspective view of a long sheet for forming a protective film according to the present embodiment, which is unwound from a sheet roll and has slits formed therein. [Figure 6A] FIG. 6A is a schematic cross-sectional view showing the protective film forming sheet shown in FIG. 2C being attached to a workpiece. [Figure 6B] FIG. 6B is a schematic cross-sectional view showing that the protective film-forming film attached to the workpiece has been turned into a protective film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] Hereinafter, the present invention will be described in detail based on specific embodiments with reference to the drawings.

[0023] First, the main terms used in this specification will be explained.

[0024] The workpiece is a plate-like body to which a protective film-forming film is attached and processed. Examples of the workpiece include a wafer and a panel. Specifically, examples of the workpiece include a semiconductor wafer and a semiconductor panel. Examples of the processed product of the workpiece include a chip obtained by dividing a wafer. Specifically, an example of the processed product is a semiconductor chip obtained by dividing a semiconductor wafer. In this case, the protective film is formed on the back side of the wafer.

[0025] The "front surface" of a workpiece refers to the surface on which circuits, bumps, and other convex electrodes are formed, and the "back surface" refers to the surface on which circuits, etc. are not formed.

[0026] In this specification, for example, "(meth)acrylate" is used as a term indicating both "acrylate" and "methacrylate," and the same applies to other similar terms.

[0027] In this specification, the weight ratio of the components constituting each composition is shown as the solid content ratio.

[0028] (1. Protective film forming sheet) As shown in FIG. 1A, the protective film-forming sheet 1 in this embodiment has a configuration in which a first release film 20 supporting the protective film-forming film 10 is arranged on one main surface 10a of the protective film-forming film 10, and a second release film 30 is arranged on the other main surface 10b.

[0029] The protective film-forming sheet 1 according to the present embodiment is not limited to the configuration shown in Fig. 1A. For example, the protective film-forming sheet may be configured to have neither the first release film nor the second release film. Fig. 1B shows a protective film-forming sheet 1 having a configuration in which a first release film 20 is disposed on one main surface 10a of a protective film-forming film 10.

[0030] In the following, a description will be given using a sheet for forming a protective film having the configuration shown in FIG. 1A, but the following description naturally also applies to the configuration shown in FIG. 1B.

[0031] In this embodiment, the protective film forming sheet is used to attach the protective film forming film to the workpiece. After being attached to the workpiece, the protective film forming film becomes a protective film to form a protective film for protecting the workpiece or a processed product of the workpiece.

[0032] In this embodiment, in order to attach the protective film-forming film to a workpiece, a protective film-forming film having a predetermined closed shape is cut out from the protective film-forming sheet 1 shown in FIG. 1A. Specifically, a circular cut is formed from the second release film 30 side along the intended cutting position 40a on the protective film-forming sheet 1 shown in FIG. 2A by a cutting blade 50. As shown in FIG. 2B, the cut 40 penetrates the second release film 30 and the protective film-forming film 10, reaches a part of the first release film 20, and divides the protective film-forming film 11 into a circular protective film-forming film 11 and the remaining protective film-forming film 12.

[0033] 2C, the second release film 30 and the protective film-forming film 12 other than the circular protective film-forming film 11 are removed from the protective film-forming sheet 1 to obtain the circular protective film-forming film 11 and the long first release film 20. The protective film-forming film of this laminate is attached to the back surface of a workpiece, and the first release film is peeled off to make the protective film-forming film into a protective film.

[0034] As shown in Fig. 2A, the protective film forming sheet 1 is preferably a long sheet capable of forming a plurality of protective film forming films 11 to be attached to a work. The protective film forming sheet 1 is also preferably a sheet roll obtained by winding up the long sheet. The protective film forming sheet 1 may also be a single sheet capable of forming one protective film forming film 11 to be attached to a work by cutting the long protective film forming sheet.

[0035] When forming the incision, the protective film-forming film and the cutting blade come into contact with each other for a short time, and then the cutting blade separates from the protective film-forming film. At this time, tack occurs in the protective film-forming film, so that the protective film-forming film is likely to adhere to the cutting blade. Therefore, as shown in FIG. 3A, when the cutting blade 50 is pulled out after cutting the protective film-forming film 10, the protective film-forming film 10 near the cutting blade 50 tends to be pulled and deformed while still adhering to the cutting blade 50 as the cutting blade 50 is pulled out. Finally, the protective film-forming film 10 peels off from the first peeling film 20, and a float A is formed between the protective film-forming film 10 and the first peeling film 20. A laminate of the protective film-forming film 11 and the first peeling film 20 in which the float A is formed is shown in FIG. 3B. FIG. 3C shows the float A formed in the laminate of the protective film-forming film 10 and the first peeling film when viewed from the direction of the arrow shown in FIG. 3B.

[0036] Such a lift becomes the starting point for peeling of the protective film-forming film from the first release film. Therefore, if a lift is formed, when removing the protective film-forming film 12 other than the second release film 30 and the circular protective film-forming film 11 from the long first release film after cutting out the protective film-forming film, the circular protective film-forming film 11 may also be unintentionally peeled off from the first release film 20, even though it is not the original peeling process, and a part or all of the protective film-forming film 11 may be removed together with the second release film 30. If the protective film-forming film 11 is peeled off, the protective film-forming sheet 1 without the protective film-forming film 11 to be attached to the workpiece is transported to the next process, resulting in a defect.

[0037] In addition, in the protective film-forming film, the floating part peeled off from the first release film due to the pulling out of the cutting blade is likely to leave a mark. In the protective film-forming film, the surface in contact with the first release film is exposed to the outside after the opposite surface is attached to the back surface of the wafer and the first release film is peeled off. Therefore, the floating part is also exposed to the outside. In other words, since the mark is exposed to the outside, the protective film including the mark is judged to have a defective appearance.

[0038] Furthermore, since such marks are formed when the protective film-forming film is peeled off from the first release film, even if the protective film-forming film is re-adhered to the first release film after being peeled off, the marks tend not to disappear and to remain even after the protective film is formed.

[0039] In contrast, the protective film-forming sheet according to the present embodiment has the characteristics described below, so that when the cutting blade is pulled out, the protective film-forming film is less likely to adhere to the cutting blade, and the formation of the lift can be suppressed. As a result, unintended peeling of the protective film-forming film 11 from the first release film and poor appearance of the protective film can be suppressed.

[0040] In this embodiment, as shown in Fig. 3C, in a laminate of the protective film-forming film 11 and the first release film, when the maximum distance D from the end face of the protective film-forming film 11 to the part where the lift A is observed in the direction from the end face to the center O of the protective film-forming film 11 is less than 4 mm, it is determined that the formation of the lift is suppressed. Hereinafter, the components of the protective film-forming sheet 1 will be described in detail.

[0041] (2. Protective Film Forming Film) As described above, the protective film-forming film is attached to the workpiece and then becomes a protective film to form a protective film for protecting the workpiece or a processed product of the workpiece.

[0042] "Making a protective film" means making the protective film-forming film have sufficient properties to protect the workpiece or a processed product of the workpiece. Specifically, when the protective film-forming film is curable, "making a protective film" means making the uncured protective film-forming film into a cured product. In other words, the protective film-forming film that has been made into a protective film is a cured product of the protective film-forming film and is different from the protective film-forming film.

[0043] After the workpiece is superimposed on the curable protective film-forming film, the protective film-forming film is cured, whereby the protective film can be firmly adhered to the workpiece and a durable protective film can be formed.

[0044] On the other hand, when the protective film-forming film does not contain a curable component and is used in an uncured state, the protective film-forming film becomes a protective film when the protective film-forming film is attached to a workpiece. In other words, the protective film-forming film that has become a protective film is the same as the protective film-forming film.

[0045] When high protective performance is not required, the protective film-forming film does not need to be cured, and therefore the protective film-forming film is easy to use.

[0046] In this embodiment, the protective film-forming film is preferably curable. Therefore, the protective film is preferably a cured product. Examples of the cured product include a heat-cured product and an energy ray-cured product. In this embodiment, the protective film is more preferably a heat-cured product.

[0047] In addition, it is preferable that the protective film-forming film has adhesiveness at room temperature (23°C) or exhibits adhesiveness when heated. This allows the protective film-forming film and the workpiece to be laminated together when they are superimposed on each other. Therefore, positioning can be reliably performed before the protective film-forming film is cured.

[0048] The protective film-forming film may be composed of one layer (single layer) or may be composed of two or more layers. When the protective film-forming film has multiple layers, these multiple layers may be the same or different from each other, and the combination of layers constituting these multiple layers is not particularly limited.

[0049] In this embodiment, the protective film-forming film is preferably one layer (single layer). A one-layer protective film-forming film can be easily produced because it can achieve high precision in terms of thickness. In addition, if the protective film-forming film is composed of multiple layers, it is necessary to consider the adhesion between the layers and the stretchability of each layer, which may result in a risk of peeling from the adherend. If the protective film-forming film is one layer, the above risks can be reduced and the design freedom is increased.

[0050] The thickness of the protective film-forming film is not particularly limited, but is preferably less than 100 μm, 70 μm or less, 45 μm or less, or 30 μm or less. By setting the upper limit of the thickness of the protective film-forming film to the above value, it is possible to suppress the protective film-forming film near the cutting blade from being pulled and deformed while remaining attached to the cutting blade when the cutting blade is pulled out.

[0051] The thickness of the protective film-forming film is preferably 5 μm or more, 10 μm or more, or 15 μm or more. By setting the lower limit of the thickness of the protective film-forming film to the above value, the protective film can easily obtain the performance of protecting the workpiece.

[0052] The thickness of the protective film-forming film means the thickness of the entire protective film-forming film. For example, the thickness of a protective film-forming film composed of multiple layers means the total thickness of all layers constituting the protective film-forming film.

[0053] (2.1 Probe tack value of protective film at 23°C) In this embodiment, the probe tack value of the protective film-forming film at 23° C. is less than 6200 mN. The probe tack value is an index of adhesive strength that appears in a short time after contact with an adherend. As shown in FIG. 3D, since the probe tack value of the protective film-forming film at 23° C. is within the above range, the protective film-forming film 10 and the cutting blade 50 come into contact and strongly adhere to each other, and when the cutting blade 50 is pulled out, the protective film-forming film 10 is prevented from being pulled while adhering to the cutting blade 50. As a result, the protective film-forming film 10 is prevented from being excessively pulled (deformed) and peeled off from the first release film 20 to form a lift.

[0054] The probe tack value of the protective film-forming film at 23° C. is preferably 5900 mN or less, 5400 mN or less, 4900 mN or less, 4400 mN or less, or 4000 mN or less. The lower limit of the probe tack value of the protective film-forming film at 23° C. is not particularly limited, but in this embodiment, it is preferably 50 mN, 200 mN, 500 mN, or 1000 mN. By setting the lower limit of the probe tack value at 23° C. to the above value, the temperature range applicable when attaching the protective film-forming film to the workpiece is expanded.

[0055] The probe tack value of the protective film-formed film at 23°C can be measured using a known probe tack tester in accordance with JIS Z0237:1991 Reference 5. That is, the probe tack value of the protective film-formed film at 23°C can be measured by a method similar to the method described in JIS Z0237:1991 Reference 5, but may be measured under test conditions different from those described in JIS Z0237:1991 Reference 5. The specific measurement method will be described in detail in the examples below.

[0056] (2.2 Composition for protective film-forming film) As long as the protective film-forming film has the above-mentioned physical properties, the composition of the protective film-forming film is not particularly limited. In this embodiment, the composition constituting the protective film-forming film (composition for protective film-forming film) is preferably a resin composition containing at least a polymer component (A), a curable component (B), and a filler (E). The polymer component is a component that can be considered to be formed by a polymerization reaction of a polymerizable compound. In addition, the curable component is a component that can undergo a curing (polymerization) reaction. In the present invention, the polymerization reaction also includes a polycondensation reaction.

[0057] In addition, the component contained in the polymer component may also be a curable component. In this embodiment, when the composition for forming a protective film contains a component that corresponds to both such a polymer component and a curable component, the composition for forming a protective film is considered to contain both a polymer component and a curable component.

[0058] 2.2.1 Polymer Components The polymer component (A) imparts film-forming properties (film-forming properties) to the protective film-forming film while imparting appropriate tack, thereby ensuring uniform attachment of the protective film-forming film to the workpiece. The weight-average molecular weight of the polymer component is usually in the range of 50,000 to 2,000,000, preferably 100,000 to 1,500,000, and particularly preferably 200,000 to 1,000,000. Examples of such polymer components include acrylic resins, urethane resins, phenoxy resins, silicone resins, and saturated polyester resins, and acrylic resins are particularly preferred.

[0059] In this specification, unless otherwise specified, the "weight average molecular weight" is a polystyrene equivalent value measured by gel permeation chromatography (GPC). Measurements by such a method can be performed, for example, using a high-speed GPC device "HLC-8120GPC" manufactured by Tosoh Corporation with a high-speed column "TSK guard column H XL -H", "TSK Gel GMH XL ", "TSK Gel G2000 H XL (All of the above are manufactured by Tosoh Corporation) connected in the above order, the column temperature was 40° C., the liquid flow rate was 1.0 mL / min, and the detector was a differential refractometer.

[0060] Examples of the acrylic resin include (meth)acrylic acid ester copolymers consisting of a (meth)acrylic acid ester monomer and a structural unit derived from a (meth)acrylic acid derivative. The (meth)acrylic acid ester monomer here preferably includes a (meth)acrylic acid alkyl ester having an alkyl group with 1 to 18 carbon atoms, specifically methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, etc. Examples of the (meth)acrylic acid derivative include (meth)acrylic acid, glycidyl (meth)acrylate, hydroxyethyl (meth)acrylate, etc.

[0061] In this embodiment, it is preferable to introduce a glycidyl group into the acrylic resin using glycidyl methacrylate or the like. The compatibility of the acrylic resin into which the glycidyl group has been introduced with the epoxy resin as a thermosetting component described later is improved, and a protective film-forming film with stable performance (including probe tack value) tends to be obtained. In addition, in this embodiment, it is preferable to introduce a hydroxyl group into the acrylic resin using hydroxyethyl acrylate or the like in order to control the adhesion to the workpiece and the adhesive properties.

[0062] The glass transition temperature of the acrylic resin is preferably −70 to 40° C., −35 to 35° C., −20 to 30° C., −10 to 25° C., or −5 to 20° C. By setting the lower limit of the glass transition temperature of the acrylic resin to the above value, it becomes easy to reduce the tack of the protective film-forming film. In addition, by setting the upper limit of the glass transition temperature of the acrylic resin to the above value, the tack of the protective film-forming film is appropriately increased, the adhesive strength of the protective film-forming film to the workpiece is improved, and the adhesive strength of the protective film to the workpiece is appropriately improved.

[0063] When an acrylic resin has m types of structural units (m is an integer of 2 or more), the glass transition temperature of the acrylic resin can be calculated as follows: That is, when m types of monomers that derive the structural units in the acrylic resin are each assigned a unique number from 1 to m in sequence and named "monomer m", the glass transition temperature (Tg) of the acrylic resin can be calculated using the Fox formula shown below.

number

number

[0064] For Tgk, values ​​listed in the Polymer Data Handbook, Adhesive Handbook, Polymer Handbook, etc. can be used. For example, the Tgk of the homopolymer of methyl acrylate is 10°C, the Tgk of the homopolymer of n-butyl acrylate is -54°C, the Tgk of the homopolymer of methyl methacrylate is 105°C, the Tgk of the homopolymer of 2-hydroxyethyl acrylate is -15°C, the Tgk of the homopolymer of glycidyl methacrylate is 41°C, and the Tgk of 2-ethylhexyl acrylate is -70°C.

[0065] The content of the polymer component when the total weight of the composition for the protective film-forming film is 100 parts by mass is preferably 5 to 80 parts by mass, 8 to 70 parts by mass, 10 to 60 parts by mass, 12 to 55 parts by mass, 14 to 50 parts by mass, or 15 to 45 parts by mass. By setting the content of the polymer component within the above range, it becomes easy to control the tack of the protective film-forming film, and therefore it is easy to control the above-mentioned probe tack value.

[0066] (2.2.2 Thermosetting components) The curable component (B) cures the protective film-forming film to form a hard protective film. As the curable component, a thermosetting component, an energy ray curable component, or a mixture thereof can be used. When curing by irradiation with energy rays, the protective film-forming film contains a filler and a colorant, which will be described later, and thus the light transmittance is reduced. Therefore, for example, when the thickness of the protective film-forming film is increased, the energy ray curing is likely to be insufficient.

[0067] On the other hand, a thermosetting protective film-forming film can be sufficiently cured by heating even if it is thick, so that a protective film with high protective performance can be formed. In addition, a large number of protective film-forming films can be heated and thermally cured at the same time by using a normal heating means such as a heating oven.

[0068] Therefore, in this embodiment, it is preferable that the curable component is thermosetting, that is, the protective film-forming film is preferably thermosetting.

[0069] Whether or not a protective film-forming film is thermosetting can be determined as follows. First, a protective film-forming film at room temperature (23°C) is heated to a temperature higher than room temperature, and then cooled to room temperature to obtain a protective film-forming film after heating and cooling. Next, when the hardness of the protective film-forming film after heating and cooling is compared with the hardness of the protective film-forming film before heating at the same temperature, if the protective film-forming film after heating and cooling is harder, this protective film-forming film is determined to be thermosetting.

[0070] As the thermosetting component, for example, an epoxy resin, a thermosetting polyimide resin, an unsaturated polyester resin, or a mixture thereof is preferably used. The thermosetting polyimide resin is a general term for a polyimide precursor and a thermosetting polyimide, which form a polyimide resin by thermal curing.

[0071] The epoxy resin as a thermosetting component has the property of forming a three-dimensional network structure and a strong coating when heated. As such an epoxy resin, various known epoxy resins are used. In this embodiment, the molecular weight (formula weight) of the epoxy resin is preferably 300 or more and less than 50,000, 300 or more and less than 10,000, 300 or more and less than 5,000, or 300 or more and less than 3,000. The epoxy equivalent of the epoxy resin is preferably 50 to 5,000 g / eq, more preferably 100 to 2,000 g / eq, and even more preferably 150 to 1,000 g / eq.

[0072] Specific examples of such epoxy resins include glycidyl ethers of phenols such as bisphenol A, bisphenol F, resorcinol, phenyl novolac, and cresol novolac; glycidyl ethers of alcohols such as butanediol, polyethylene glycol, and polypropylene glycol; glycidyl ethers of carboxylic acids such as phthalic acid, isophthalic acid, and tetrahydrophthalic acid; glycidyl or alkyl glycidyl epoxy resins in which active hydrogen bonded to nitrogen atoms such as aniline isocyanurate is substituted with a glycidyl group; and so-called alicyclic epoxides in which epoxy is introduced by, for example, oxidizing carbon-carbon double bonds in the molecule, such as vinylcyclohexane diepoxide, 3,4-epoxycyclohexylmethyl-3,4-dicyclohexanecarboxylate, and 2-(3,4-epoxy)cyclohexyl-5,5-spiro(3,4-epoxy)cyclohexane-m-dioxane. Other epoxy resins having a biphenyl skeleton, a dicyclohexadiene skeleton, a naphthalene skeleton, and the like can also be used.

[0073] When a thermosetting component is used as the curing component (B), it is preferable to use a curing agent (C) as an auxiliary in combination. A heat-activated latent epoxy resin curing agent is preferable as a curing agent for epoxy resin. A "heat-activated latent epoxy resin curing agent" is a type of curing agent that does not react easily with epoxy resin at room temperature (23°C) and is activated by heating above a certain temperature and reacts with epoxy resin. Methods for activating a heat-activated latent epoxy resin curing agent include a method of generating active species (anions, cations) through a chemical reaction by heating; a method in which the agent is stably dispersed in epoxy resin near room temperature and becomes compatible and dissolved with epoxy resin at high temperatures to start a curing reaction; a method in which a molecular sieve-encapsulated type curing agent is dissolved at high temperatures to start a curing reaction; and a method using microcapsules.

[0074] Of the above-mentioned methods, a method in which the compound is stably dispersed in the epoxy resin at around room temperature, becomes compatible and dissolved in the epoxy resin at high temperatures, and initiates a curing reaction is preferred.

[0075] Specific examples of the heat-activated latent epoxy resin curing agent include various onium salts, dibasic acid dihydrazide compounds, dicyandiamide, amine adduct curing agents, high melting point active hydrogen compounds such as imidazole compounds, etc. These heat-activated latent epoxy resin curing agents can be used alone or in combination of two or more. In this embodiment, dicyandiamide is particularly preferred.

[0076] Phenol resins are also preferred as curing agents for epoxy resins. As phenol resins, condensates of phenols such as alkylphenols, polyhydric phenols, naphthol, and aldehydes, etc., can be used without any particular limitations. Specifically, phenol novolac resins, o-cresol novolac resins, p-cresol novolac resins, t-butylphenol novolac resins, dicyclopentadiene cresol resins, polyparavinylphenol resins, bisphenol A type novolac resins, or modified products thereof, etc. can be used.

[0077] The phenolic hydroxyl groups contained in these phenolic resins can easily undergo addition reaction with the epoxy groups of the above-mentioned epoxy resins upon heating to form a cured product with high impact resistance.

[0078] The content of the curing agent (C) is preferably 0.01 to 30 parts by mass, 0.1 to 20 parts by mass, 0.2 to 15 parts by mass, or 0.3 to 10 parts by mass, relative to 100 parts by mass of the epoxy resin. By setting the content of the curing agent (C) within the above range, it is easy to obtain the performance of protecting the workpiece as a protective film.

[0079] When dicyandiamide is used as the curing agent (C), it is preferable to use a curing accelerator (D) in combination. As the curing accelerator, for example, imidazoles (imidazoles in which one or more hydrogen atoms are substituted with groups other than hydrogen atoms) such as 2-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole, and 2-phenyl-4-methyl-5-hydroxymethylimidazole are preferable. Among these, 2-phenyl-4,5-dihydroxymethylimidazole is particularly preferable.

[0080] The content of the curing accelerator is preferably 0.01 to 30 parts by mass, 0.1 to 20 parts by mass, 0.2 to 15 parts by mass, or 0.3 to 10 parts by mass, relative to 100 parts by mass of the epoxy resin. By setting the content of the curing accelerator (D) within the above range, it is easy to obtain the performance of protecting the workpiece as a protective film.

[0081] When the total weight of the composition for protective film-forming film is 100 parts by mass, the total content of the thermosetting component and the curing agent is preferably 3 to 80 parts by mass, 5 to 60 parts by mass, 7 to 50 parts by mass, 9 to 40 parts by mass, or 10 to 30 parts by mass. When the thermosetting component and the curing agent are mixed in such a ratio, the performance of protecting the work as a protective film is easily obtained.

[0082] (2.2.3 Energy Ray-Curable Components) When the curable component (B) is an energy ray-curable component, the energy ray-curable component is preferably uncured and preferably has adhesive properties, and more preferably is uncured and has adhesive properties.

[0083] The energy ray curable component is a component that is cured by irradiation with energy rays, and is also a component that imparts film-forming properties, flexibility, and the like to the protective film-forming film.

[0084] As the energy ray-curable component, for example, a compound having an energy ray-curable group is preferable. Examples of such a compound include known compounds.

[0085] (2.2.4 Filler) By containing the filler (E) in the protective film-forming film, the protective film obtained by converting the protective film-forming film into a protective film can easily adjust the thermal expansion coefficient, and by bringing this thermal expansion coefficient closer to the thermal expansion coefficient of the workpiece, the adhesive reliability with the workpiece can be further improved. In addition, by containing the filler (E) in the protective film-forming film, a hard protective film can be obtained, making it easier to obtain the performance of protecting the workpiece, and further reducing the moisture absorption rate of the protective film.

[0086] The filler (E) may be either an organic filler or an inorganic filler, but is preferably an inorganic filler from the viewpoint of shape stability at high temperatures such as 260°C.

[0087] Examples of preferred inorganic fillers include powders of silica, alumina, talc, calcium carbonate, red iron oxide, silicon carbide, boron nitride, etc.; beads of these inorganic fillers that are spherical; surface-modified products of these inorganic fillers; single crystal fibers of these inorganic fillers; glass fibers, etc. Among these, silica and surface-modified silica are preferred. The surface-modified silica is preferably surface-modified with a coupling agent, and more preferably surface-modified with a silane coupling agent.

[0088] The average particle size of the filler is preferably 0.02 to 10 μm, 0.05 to 5 μm, or 0.10 to 3 μm.

[0089] By setting the average particle size of the filler within the above range, the composition for forming a protective film can be easily handled, and as a result, the quality of the composition for forming a protective film and the protective film can be easily stabilized.

[0090] In this specification, unless otherwise specified, the term "average particle size" refers to the particle size (D50) at an integrated value of 50% in a particle size distribution curve determined by a laser diffraction scattering method.

[0091] The content of the filler when the total weight of the composition for protective film-forming film is 100 parts by mass is preferably 15 to 80 parts by mass, 30 to 75 parts by mass, 40 to 70 parts by mass, or 45 to 65 parts by mass.

[0092] By setting the lower limit of the content of the filler to the above value, it is easy to reduce the tack of the protective film-forming film, so that the above-mentioned probe tack value is easy to control. Also, by setting the upper limit of the content of the filler to the above value, the adhesive strength of the protective film-forming film to the workpiece is improved, and the adhesive strength of the protective film to the workpiece is appropriately improved.

[0093] 2.2.5 Coupling Agents The protective film-forming film preferably contains a coupling agent (F). By containing the coupling agent, after the protective film-forming film is cured, the adhesion between the protective film and the workpiece can be improved without impairing the heat resistance of the protective film, and the water resistance (moisture and heat resistance) can be improved. As the coupling agent, a silane coupling agent is preferable from the viewpoint of its versatility and cost merit.

[0094] Examples of silane coupling agents include γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-(methacryloxypropyl)trimethoxysilane, γ-aminopropyltrimethoxysilane, N-6-(aminoethyl)-γ-aminopropyltrimethoxysilane, N-6-(aminoethyl)-γ-aminopropylmethyldiethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, γ-ureidopropyltriethoxysilane, γ-mercaptopropyltrimethoxysilane, γ-mercaptopropylmethyldimethoxysilane, bis(3-triethoxysilylpropyl)tetrasulfane, methyltrimethoxysilane, methyltriethoxysilane, vinyltrimethoxysilane, vinyltriacetoxysilane, imidazolesilane, etc. These can be used alone or in combination of two or more.

[0095] 2.2.6 Colorants The protective film-forming film preferably contains a colorant (G). This conceals the back surface of the workpiece such as a chip, thereby blocking various electromagnetic waves generated in electronic devices and reducing malfunction of the workpiece such as a chip. In addition, in the process of removing the protective film-forming film on the outside of the punching blade from the first release film to obtain the protective film-forming film on the inside of the punching blade on the first release film, it is possible to immediately determine by visual inspection whether the inner protective film-forming film that should remain has been unintentionally peeled off and removed.

[0096] As the colorant (G), for example, known colorants such as inorganic pigments, organic pigments, organic dyes, etc. In this embodiment, inorganic pigments are preferred.

[0097] Examples of inorganic pigments include carbon black, cobalt-based pigments, iron-based pigments, chromium-based pigments, titanium-based pigments, vanadium-based pigments, zirconium-based pigments, molybdenum-based pigments, ruthenium-based pigments, platinum-based pigments, ITO (indium tin oxide)-based pigments, and ATO (antimony tin oxide)-based pigments. Among these, it is particularly preferable to use carbon black. Carbon black can block electromagnetic waves in a wide wavelength range.

[0098] The amount of colorant (especially carbon black) in the protective film-forming film varies depending on the thickness of the protective film-forming film, but for example, when the thickness of the protective film-forming film is 20 μm, the amount is preferably 0.01 to 10 mass%, 0.04 to 7 mass%, or 0.07 to 4 mass% relative to the total mass of the protective film-forming film.

[0099] The average particle size of the colorant (particularly carbon black) is preferably 1 to 500 nm, more preferably 3 to 100 nm, and even more preferably 5 to 50 nm. When the average particle size of the colorant is within the above range, it is easy to control the light transmittance within a desired range.

[0100] 2.2.7 Other Additives The composition for the protective film-forming film may contain other additives, such as a photopolymerization initiator, a crosslinking agent, a plasticizer, an antistatic agent, an antioxidant, a gettering agent, a tackifier, a release agent, etc., within the range that does not impair the effects of the present invention.

[0101] However, the content of the release agent in the composition for the protective film-forming film is preferably less than a predetermined amount. In this embodiment, it is preferably less than 0.00099% by mass with respect to the total mass of the protective film-forming film. If the content of the release agent is too high, the adhesive reliability between the protective film and the workpiece tends to decrease. Examples of the release agent include alkyd-based release agents, silicone-based release agents, fluorine-based release agents, unsaturated polyester-based release agents, polyolefin-based release agents, and wax-based release agents.

[0102] (3. First release film) The first release film is a film that can support the protective film-forming film in a peelable manner. When a cut is formed in the sheet for forming a protective film, the cut does not penetrate the first release film, but reaches a part of the first release film. In other words, when a cut is formed in the sheet for forming a protective film, the first release film is half-cut.

[0103] The first release film may be composed of one layer (single layer) or two or more layers of substrate, and the surface of the substrate may be subjected to a release treatment in order to control the releasability. That is, the surface of the substrate may be modified, or a material not derived from the substrate may be formed on the surface of the substrate.

[0104] In this embodiment, the first release film preferably has a substrate and a first release agent layer. By having the first release agent layer, it is easy to control the physical properties of the surface of the first release film on which the first release agent layer is formed.

[0105] In the first release film, the first release agent layer is preferably formed directly on the surface of the substrate. By forming the first release agent layer directly on the surface of the substrate, the production of the first release film becomes easy, thereby realizing cost reduction.

[0106] In this embodiment, the first release agent layer is formed on the surface of the first release film on the protective film-forming film side. As shown in Fig. 4, in the sheet 1 for forming a protective film, the first release film 20 has a substrate 21 and a first release agent layer 22, and the main surface 20b of the first release agent layer 22 contacts the main surface 10a of the protective film-forming film.

[0107] The thickness of the first release film is not particularly limited, but is preferably 30 μm or more and 100 μm or less. The thickness of the first release film is more preferably 40 μm or more, and even more preferably 45 μm or more. The thickness of the first release film is more preferably 80 μm or less, and even more preferably 70 μm or less.

[0108] By setting the lower limit of the thickness of the first release film to the above value, when the protective film-forming film is cut out by the cutting blade, the cutting blade can be prevented from penetrating the first release film and cutting the first release film. Also, by setting the upper limit of the thickness of the first release film to the above value, the protective film-forming sheet passes through rollers such as guide rollers in the device before being fed out and the protective film-forming film is cut out and transported to the next process, and at that time, the protective film-forming film can be prevented from peeling off from the first release film.

[0109] The thickness of the first release film means the overall thickness of the first release film. For example, the thickness of a first release film composed of multiple layers means the total thickness of all layers constituting the first release film.

[0110] (3.1 Surface elastic modulus of the first release film at 23°C) In this embodiment, the surface elastic modulus of the surface of the first release film in contact with the protective film-forming film at 23° C. (hereinafter also referred to as the surface elastic modulus of the first release film at 23° C.) is 17 MPa or less. The surface elastic modulus is an index of the ease of deformation of the surface. As shown in FIG. 3D, since the surface elastic modulus of the first release film at 23° C. is within the above range, the surface 20b (for example, the first release agent layer) of the first release film 20 in contact with the protective film-forming film is more likely to follow the deformation of the protective film-forming film 10 when the cutting blade 50 is pulled out. As a result, it is possible to suppress the protective film-forming film 20 from peeling off from the first release film 10 and the formation of a lift.

[0111] The surface elastic modulus of the surface of the first release film in contact with the protective film-forming film at 23° C. is preferably 15 MPa or less, 14 MPa or less, 13 MPa or less, or 12 MPa or less. In addition, the lower limit of the surface elastic modulus of the surface of the first release film in contact with the protective film-forming film at 23° C. is not particularly limited, but in this embodiment, it is preferably 3 MPa or more, 4 MPa or more, or 5 MPa or more.

[0112] The surface elastic modulus of the surface of the first release film in contact with the protective film-forming film at 23°C can be measured using an atomic force microscope equipped with a cantilever. That is, the cantilever is pressed against and pulled away from the surface of the first release film in contact with the protective film-forming film to obtain a force curve. The obtained force curve is fitted by the JKR theoretical formula to obtain the elastic modulus, which is the surface elastic modulus of the present invention. A specific measurement method will be described in detail in the examples below.

[0113] In this embodiment, the product of the probe tack value (mN) of the protective film-forming film at 23° C. and the surface elastic modulus (MPa) of the surface of the first release film in contact with the protective film-forming film at 23° C. is 66000 or less. By making the product 66000 or less, it is possible to suppress the formation of lifting caused by peeling between the protective film-forming film and the first release film.

[0114] The product of the probe tack value (mN) of the protective film-forming film at 23°C and the surface elastic modulus (MPa) of the surface of the first release film in contact with the protective film-forming film at 23°C is preferably 60,000 or less, and more preferably 54,000 or less.

[0115] When the first release film has a substrate and a first release agent layer, as described above, the first release agent layer is the surface of the first release film that contacts the protective film-forming film. Therefore, it is sufficient that the surface elasticity of the first release agent layer is within the above range.

[0116] In the present embodiment, in the protective film-forming sheet, when the peeling force of the first release film from the protective film-forming film is F1 and the peeling force of the second release film from the protective film-forming film described later is F2, F1 and F2 satisfy the relationship F1>F2. By satisfying such a relationship, when removing the second release film from the protective film-forming sheet, the protective film-forming film 11 that should remain is not removed together with the second release film, and it becomes easy to leave the protective film-forming film 11 on the first release film.

[0117] Thus, the first release film is a heavy release film and the second release film is a light release film.

[0118] In addition, F1 is preferably 50 mN / 100 mm or more, 70 mN / 100 mm or more, 90 mN / 100 mm or more, 110 mN / 100 mm or more, and 130 mN / 100 mm or more. By having F1 within the above range, the formation of lifting caused by peeling between the protective film-forming film and the first release film can be further suppressed.

[0119] In this embodiment, F1 and F2 are load values ​​measured using a tensile tester. A specific measurement method will be described in detail in the examples below.

[0120] Hereinafter, the case where the first release film has a substrate and a first release agent layer will be described.

[0121] (3.2 Base material) The substrate of the first release film is not particularly limited as long as it is a material that can support the protective film-forming film until the protective film-forming film is attached to the workpiece, and is usually composed of a film primarily made of a resin-based material (hereinafter referred to as a "resin film").

[0122] Specific examples of the resin film include polyethylene film, polypropylene film, polybutene film, polybutadiene film, polymethylpentene film, polyvinyl chloride film, vinyl chloride copolymer film, polyethylene terephthalate film, polyethylene naphthalate film, polybutylene terephthalate film, polyurethane film, ethylene vinyl acetate copolymer film, ionomer resin film, ethylene-(meth)acrylic acid copolymer film, ethylene-(meth)acrylic acid ester copolymer film, polystyrene film, polycarbonate film, polyimide film, and fluororesin film. Crosslinked films of these films are also used. Furthermore, laminated films of these films may be used. In this embodiment, a polyethylene terephthalate film is preferred from the viewpoints of environmental safety, cost, and the like.

[0123] The substrate may contain various additives such as a colorant, a flame retardant, a plasticizer, an antistatic agent, a lubricant, and a filler in the resin film.

[0124] The thickness of the substrate is not particularly limited within the range of the thickness of the first release film, so long as the protective film-forming sheet can function properly in each process in which it is used. The thickness of the substrate is preferably 30 μm or more and 100 μm or less. The thickness of the substrate is more preferably 40 μm or more, and even more preferably 45 μm or more. The thickness of the substrate is more preferably 80 μm or less, and even more preferably 70 μm or less.

[0125] (3.3 First Release Agent Layer) The first release agent layer imparts releasability from the protective film-forming film to the first release film. The first release agent layer is not particularly limited as long as it is made of a material that can impart releasability. In this embodiment, the first release agent layer is obtained by curing a composition for the first release agent layer that contains silicone.

[0126] The thickness of the first release agent layer is not particularly limited, but is preferably 30 nm or more and 200 nm or less. The thickness of the first release agent layer is more preferably 50 nm or more, and even more preferably 80 nm or more. The thickness of the first release agent layer is more preferably 180 nm or less.

[0127] When the thickness of the first release agent layer is within the above range, stable release performance can be exhibited when the protective film-forming film is attached to a workpiece.

[0128] (3.4 Composition for first release agent layer) In this embodiment, the composition for the first release agent layer may be, for example, an alkyd-based release agent, a silicone-based release agent, a fluorine-based release agent, an unsaturated polyester-based release agent, a polyolefin-based release agent, or a wax-based release agent, and among these, a silicone-based release agent is preferred. When the composition for the first release agent layer contains a silicone-based release agent, it is preferred that the composition contains a silicone-based release agent and a heavy release additive.

[0129] (3.4.1 Silicone-based release agents) As the silicone-based release agent, a silicone release agent containing silicone having dimethylpolysiloxane as a basic skeleton can be used.

[0130] The silicone may be any of addition reaction type, condensation reaction type, and energy ray curing type such as ultraviolet ray curing type and electron beam curing type, but addition reaction type silicone is preferable. Addition reaction type silicone has high reactivity and excellent productivity, and has advantages such as small change in release force after production and no cure shrinkage compared to condensation reaction type.

[0131] Specific examples of the addition reaction type silicone include organopolysiloxanes having two or more alkenyl groups having 2 to 10 carbon atoms, such as vinyl groups, allyl groups, propenyl groups, and hexenyl groups, at the ends and / or side chains of the molecule. From the viewpoint of reducing the surface elastic modulus, it is preferable that the number of alkenyl groups in the addition reaction type silicone is small.

[0132] When the total weight of the composition for the first release agent layer (excluding the catalyst described below) is 100 parts by mass, the content of silicone consisting of dimethylpolysiloxane is preferably less than 100 parts by mass, less than 90 parts by mass, less than 80 parts by mass, or less than 70 parts by mass.

[0133] When using such an addition reaction type silicone, it is preferable to use a crosslinking agent and a catalyst in combination.

[0134] An example of the crosslinking agent is an organopolysiloxane having at least two hydrogen atoms bonded to silicon atoms in one molecule.

[0135] Specific examples of the crosslinking agent include dimethylhydrogensiloxy group-endblocked dimethylsiloxane-methylhydrogensiloxane copolymer, trimethylsiloxy group-endblocked dimethylsiloxane-methylhydrogensiloxane copolymer, trimethylsiloxy group-endblocked methylhydrogenpolysiloxane, poly(hydrogensilsesquioxane), and the like.

[0136] From the viewpoint of reducing the surface elastic modulus, the content of the crosslinking agent in the composition for the first release agent layer is preferably small.

[0137] Examples of the catalyst include fine particle platinum, fine particle platinum adsorbed on a carbon powder support, chloroplatinic acid, alcohol-modified chloroplatinic acid, olefin complexes of chloroplatinic acid, and platinum group metal compounds such as palladium and rhodium.

[0138] By using such a catalyst, the curing reaction of the composition for the first release agent layer can be made to proceed more efficiently.

[0139] The content of the silicone-based release agent when the total weight of the composition for the first release agent layer (excluding the catalyst) is 100 parts by mass, is preferably 30 to 100 parts by mass, or 50 to 100 parts by mass, from the viewpoint of setting the surface elastic modulus within the above-mentioned range and from the viewpoint of setting the peel force F1 within the above-mentioned range.

[0140] (3.4.2 Heavy Release Additives) The strong release additive is used to increase the peeling force F1 of the first release film from the protective film-forming film. Examples of the strong release additive include silicone resins and organosilanes such as silane coupling agents, among which silicone resins are preferably used.

[0141] Silicone resins include, for example, monofunctional siloxane units [RSiO 1 / 2 ] and tetrafunctional siloxane units [SiO 4 / 2 It is preferable to use an MQ resin containing a Q unit that is a group represented by the formula: [Q unit]. The three R in the M unit each independently represents a hydrogen atom, a hydroxyl group, or an organic group. From the viewpoint of easily suppressing silicone migration, it is preferable that one or more of the three R in the M unit is a hydroxyl group or a vinyl group, and more preferably a vinyl group.

[0142] The content of the heavy release additive when the total weight of the first release agent layer composition (excluding the catalyst) is 100 parts by mass is preferably 0 to 50 parts by mass, 5 to 45 parts by mass, or 10 to 40 parts by mass.

[0143] However, from the viewpoint of reducing the surface elastic modulus, it is preferable that the content of the silicone resin (particularly the MQ resin) in the composition for the first release agent layer is small.

[0144] The composition for the first release agent layer may contain additives that are generally used in release agent layers, such as dyes and dispersants, within the scope of not impairing the effects of the present invention.

[0145] (4. Second release film) The second release film is a film capable of supporting the protective film-forming film in a peelable manner. When a cut is formed in the sheet for forming a protective film, the cut penetrates the second release film, and the second release film is removed together with the protective film-forming film other than the protective film-forming film having a closed shape when forming a laminate of the protective film-forming film having a closed shape and the first release film.

[0146] The second release film may be composed of one layer (single layer) or two or more layers of substrate, and the surface of the substrate may be subjected to a release treatment in order to control the releasability. That is, the surface of the substrate may be modified, or a material not derived from the substrate may be formed on the surface of the substrate.

[0147] In addition, when the second release agent layer is formed, the second release agent layer is formed on the surface of the second release film on the protective film-forming film side. As shown in Fig. 4, in the sheet 1 for forming a protective film, the second release film 30 has a substrate 31 and a second release agent layer 32, and the main surface 30b of the second release agent layer 32 contacts the main surface 10b of the protective film-forming film.

[0148] The thickness of the second release film is not particularly limited, but is preferably 10 μm or more and 75 μm or less. The thickness of the second release film is more preferably 18 μm or more, and even more preferably 24 μm or more. The thickness of the second release film is more preferably 60 μm or less, and even more preferably 45 μm or less. From the viewpoint of making the peeling force F2 and the peeling force 1 satisfy the above-mentioned F1>F2, the thickness of the second release film is preferably equal to or less than the thickness of the first release film, and more preferably less than the thickness of the first release film.

[0149] The thickness of the second release film means the thickness of the entire second release film. For example, the thickness of a second release film composed of multiple layers means the total thickness of all layers constituting the second release film.

[0150] (4.1 Base material) The substrate of the second release film can be appropriately selected from the materials exemplified as the substrate of the first release film.

[0151] (4.2 Second Release Agent Layer) When the second release film has a second release agent layer, the second release agent layer is not particularly limited as long as it is made of a material that can impart release properties. For example, the second release agent layer is obtained by curing a composition for the second release agent layer that contains silicone, similar to the first release agent layer.

[0152] The composition for the second release agent layer can be selected from the materials exemplified for the composition for the first release agent layer as long as the relationship between F1 and F2 above is satisfied. However, it is preferable that the material exemplified as the heavy release additive is contained in a smaller amount than in the composition for the first release agent layer, or is not contained at all.

[0153] (5. Method for producing sheet for forming protective film) The method for producing the sheet for forming a protective film according to this embodiment is not particularly limited, and a known method can be adopted. For example, first, a composition for a release agent layer (a composition for a first release agent layer and a composition for a second release agent layer) for forming a first release film and a second release film is prepared. In this embodiment, from the viewpoint of adjusting the viscosity to improve the applicability to a substrate, it is preferable to apply a coating agent obtained by diluting the composition for a release agent layer containing each of the above-mentioned components with a diluting solvent to a substrate.

[0154] Examples of the dilution solvent include organic solvents such as aromatic hydrocarbons such as toluene, fatty acid esters such as ethyl acetate, ketones such as methyl ethyl ketone, aliphatic hydrocarbons such as hexane, heptane, etc. These dilution solvents may be used alone or in combination of two or more.

[0155] The solid content concentration of the coating agent containing the composition for the first release agent layer is preferably 0.3 to 10 mass%, more preferably 0.5 to 5 mass%, and even more preferably 0.5 to 3 mass%. The solid content concentration of the coating agent containing the composition for the second release agent layer is also similar to the solid content concentration of the coating agent containing the composition for the first release agent layer.

[0156] In this embodiment, a coating agent containing a composition for a first release agent layer is applied to one side of a substrate, and the coating film is then dried and cured to form a first release agent layer. This results in a first release film. A second release film can also be produced in the same manner.

[0157] Next, prepare a composition for forming a protective film-forming film. In the same manner as the composition for release agent layer, in this embodiment, it is preferable to apply a coating agent obtained by diluting the composition for protective film-forming film with a diluting solvent to the release film. The type of diluting solvent may be the same as that of the composition for release agent layer.

[0158] On the other hand, the solid content concentration of the coating agent containing the composition for the protective film-forming film is preferably 20 to 80 mass %, more preferably 30 to 70 mass %.

[0159] In this embodiment, a coating agent containing a composition for a protective film-forming film is applied by a known method onto the first release agent layer of the first release film or onto the second release agent layer of the second release film, and then heated and dried to form a coating film. Next, the second release agent layer of the second release film or the first release agent layer of the first release film is bonded onto the coating film to produce a sheet for forming a protective film. In this embodiment, from the viewpoint of setting the peel force F1 within the above-mentioned range and from the viewpoint of setting F1>F2, it is preferable to apply a coating agent containing a composition for a protective film-forming film onto the first release agent layer of the first release film, rather than onto the second release agent layer.

[0160] Examples of methods for applying the coating agent containing each composition include spin coating, spray coating, bar coating, knife coating, roll coating, roll knife coating, blade coating, die coating, and gravure coating.

[0161] (6. Device Manufacturing Method) As an example of a method for manufacturing a device using the protective film-forming sheet according to this embodiment, a method for manufacturing a chip with a protective film obtained by processing a wafer to which a protective film-forming film is attached will be described.

[0162] First, as shown in Fig. 5, a long protective film-forming sheet 1 is prepared by unwinding the protective film-forming sheet 1 from a sheet roll of the protective film-forming sheet 1. Next, as shown in Fig. 5 and Fig. 2B, a cutting blade 50 is used to form a cut 40 in the long protective film-forming sheet, penetrating the second release film 30 and the protective film-forming film 10 and reaching a part of the first release film 20.

[0163] By forming the incision 40, a circular protective film-forming film 11 is obtained. In the protective film-forming sheet 1, the probe tack value of the protective film-forming film at 23° C. is less than 6200 mN, the surface elastic modulus of the surface of the first release film in contact with the protective film-forming film at 23° C. is 17 MPa or less, and the product of the probe tack value and the surface elastic modulus is 66000 or less. Therefore, as shown in FIG. 3C, when the cutting blade 30 is pulled out, the formation of a lift caused by the peeling of the protective film-forming film 10 and the first release film 20 is suppressed. That is, in the circular protective film-forming film 11, the maximum distance D from the end face of the protective film-forming film 11 to the part where the lifting is observed is less than 4 mm. In addition, the mark of the protective film-forming film 10 caused by the peeling of the protective film-forming film 10 and the first release film 20 is also suppressed.

[0164] Therefore, when removing the protective film-forming film 12 other than the second release film 30 and the protective film-forming film 11 after the incisions are formed, the protective film-forming film 11 is not unintentionally peeled off and removed from the long first release film 20 due to floating. That is, as shown in FIG. 2C, a protective film-forming sheet in which the protective film-forming film 11 remains on the long first release film can be easily obtained.

[0165] Next, as shown in Fig. 6A, the protective film-forming film 11 is attached to the back surface 60b of the wafer 60 as a workpiece, and as shown in Fig. 6B, the first release film 20 is peeled off from the laminate to convert the protective film-forming film 11 into a protective film, thereby forming the protective film 15. Then, the wafer having the protective film is diced into individual pieces to obtain chips with the protective film. The protective film may be converted into a protective film after the wafer is diced into individual pieces.

[0166] Since the formation of floating portions is suppressed in the protective film-forming film, the formation of marks on the surface of the protective film is also suppressed, and therefore a chip with a protective film in which defects in the appearance of the protective film are also suppressed can be obtained.

[0167] (7. Modifications) The above describes a protective film-forming sheet (Figure 1A) having a configuration in which a first release film is arranged on one side of a protective film-forming film and a second release film is arranged on the other side. However, as mentioned above, the protective film-forming sheet may also have a configuration that does not have a second release film (Figure 1B).

[0168] The protective film forming sheet according to the present embodiment also includes a long protective film forming sheet (FIG. 2B) having cuts and on which a plurality of protective film forming films 11 to be attached to a workpiece are formed, as shown in FIG. 2B. It also includes a sheet roll in which the long protective film forming sheet is wound up. The protective film forming sheet according to the present embodiment also includes a sheet obtained by cutting the long protective film forming sheet into a single protective film forming film 11 to be attached to a workpiece.

[0169] Furthermore, the protective film forming sheet according to this embodiment also includes a long protective film forming sheet having cuts and on which multiple protective film forming films 11 to be attached to a workpiece are formed, a sheet roll of the long protective film forming sheet, and a single sheet from which a single protective film forming film 11 can be formed by cutting the long protective film forming sheet.

[0170] 5, the protective film-forming film 11 to be attached to the workpiece is circular, but may be any other shape as long as it is a closed shape. Examples of other shapes include polygons such as triangles, and ellipses. It is preferable that the closed shape corresponds to the shape of the workpiece.

[0171] Although the embodiment of the present invention has been described above, the present invention is not limited to the above embodiment, and may be modified in various aspects within the scope of the present invention. EXAMPLES

[0172] The present invention will be described in more detail below using examples, but the present invention is not limited to these examples.

[0173] (Preparation of First Release Film) The following components were mixed in the ratio (solid content equivalent) shown in Table 1, and a coating agent containing a composition for the first release agent layer was prepared using a mixed solvent of toluene and methyl ethyl ketone (toluene / methyl ethyl ketone = 1 / 1 (mass ratio)) so that the solid content concentration was 2 mass%. (α) Silicone-based release agent (α-1) Silicone-based release agent containing an organopolysiloxane having a vinyl group and an organopolysiloxane having a hydrosilyl group (manufactured by Dow Corning Toray Co., Ltd., BY24-561, solid content 30% by mass) (α-2) Dimethylpolysiloxane (Shin-Etsu Chemical Co., Ltd., product name: X-62-1387, weight average molecular weight: 2000) (β) Silicone resin MQ resin with vinyl groups (Toray Dow Corning Co., Ltd., SD-7292, solid content 71% by mass) (γ)Catalyst Platinum (Pt) catalyst (Toray Dow Corning Co., Ltd., SRX-212, solid content 100% by mass)

[0174] A coating agent containing the prepared composition for forming a first release agent layer was applied to a PET film (manufactured by Mitsubishi Chemical, product name: Diafoil (registered trademark) T-100, thickness: 50 μm) as a substrate so that the film thickness after heating and drying would be 0.15 μm, forming a first release agent layer on the PET film and producing a first release film.

[0175] [Table 1]

[0176] (Preparation of the second release film) As the second release film, a release-treated PET film ("SP-PET381130" manufactured by Lintec, thickness 38 μm) was used.

[0177] (Preparation of protective film) The following components were mixed in the compounding ratio (solid content equivalent) shown in Table 2, and diluted with methyl ethyl ketone to a solid content concentration of 50 mass % to prepare a coating agent containing a composition for a protective film-forming film. (A) Polymer Component (A-1) (meth)acrylic acid ester copolymer obtained by copolymerizing 10 parts by mass of n-butyl acrylate, 70 parts by mass of methyl acrylate, 5 parts by mass of glycidyl methacrylate, and 15 parts by mass of 2-hydroxyethyl acrylate (weight average molecular weight: 400,000, glass transition temperature: -1°C) (A-2) (meth)acrylic acid ester copolymer obtained by copolymerizing 10 parts by mass of n-butyl acrylate, 65 parts by mass of methyl acrylate, 12 parts by mass of glycidyl methacrylate, and 13 parts by mass of 2-hydroxyethyl acrylate (weight average molecular weight: 450,000, glass transition temperature: 2°C) (B) Curing component (thermosetting component) (B-1) Bisphenol A type epoxy resin (Mitsubishi Chemical Corporation, jER828, epoxy equivalent 184-194g / eq) (B-2) Acrylic rubber microparticle dispersed bisphenol A type liquid epoxy resin (Nippon Shokubai Co., Ltd., BPA328, epoxy equivalent 230g / eq, acrylic rubber content 20phr) (B-3) Dicyclopentadiene type epoxy resin (manufactured by Dainippon Ink and Chemicals, Epicron HP-7200HH, softening point 88-98°C, epoxy equivalent 255-260g / eq) (C) Hardener: Dicyandiamide (DICY7, manufactured by Mitsubishi Chemical Corporation) (D) Curing accelerator: 2-phenyl-4,5-dihydroxymethylimidazole (Curesol 2PHZ, manufactured by Shikoku Chemical Industry Co., Ltd.) (E) Filler (E-1) Epoxy group-modified spherical silica filler (manufactured by Admatechs Co., Ltd., SC2050MA, average particle size 0.5 μm) (E-2) Silica filler (Admatechs, YC100C-MLA, average particle size 0.1 μm) (F) Silane coupling agent: γ-glycidoxypropyltrimethoxysilane (Shin-Etsu Chemical Co., Ltd., KBM403, methoxy equivalent 12.7 mmol / g, molecular weight 236.3) (G) Colorant: Carbon black (manufactured by Mitsubishi Chemical Corporation, MA600B, average particle size 28 nm)

[0178] The coating agent containing the prepared composition for protective film-forming film was applied to the surface of the prepared first release film on which the first release agent layer was formed, and dried at 100°C for 2 minutes to form a protective film-forming film with a thickness of 20 μm. Next, the release-treated surface of the prepared second release film was attached to the protective film-forming film to obtain a sheet for protective film-forming in which release films were formed on both sides of the protective film-forming film. The attachment conditions were a temperature of 60°C, a pressure of 0.4 MPa, and a speed of 1 m / min.

[0179] The obtained sheet for forming a protective film was cut to a width of 320 mm, and wound up to a length of 10 m around a hollow plastic core having a diameter of 3 inches to form a sheet roll.

[0180] Subsequently, the following measurements and evaluations were carried out.

[0181] (Probe tack value of protective film at 23℃) From the prepared protective film-forming sheet, a plurality of individual sheets on which one protective film-forming film 11 was formed were obtained. From two individual sheets, the second release film was peeled off, and the protective film-forming films were bonded together to obtain a laminate in which the first release film, two protective film-forming films, and the first release film were laminated in this order. From the obtained laminate, the first release film was peeled off, and the second release film was peeled off from another individual sheet, and the protective film-forming films were bonded together to obtain a laminate in which the first release film, three protective film-forming films, and the first release film were laminated in this order. This was repeated a predetermined number of times to obtain a measurement sample in which the first release film, a laminate of a protective film-forming film having a thickness of 800 μm±20 μm, and the first release film were laminated in this order.

[0182] One of the first release films was peeled off from the obtained measurement sample, and the probe tack value of the protective film-formed film surface was measured at 23° C. using a probe tack tester (stainless steel probe) manufactured by Tester Sangyo Co., Ltd. The probe was wiped and cleaned with methyl ethyl ketone before the measurement. The measurement conditions are: Contact load: 200gf, Contact speed: 10mm / sec, Probe Area: 5mmΦ, Contact time: 1 minute, Peeling speed: 10 mm / sec. The measurement was performed seven times by changing the contact position of the probe on the protective film-coated film surface. Of the seven test values, the first and second smallest values ​​were omitted. The average of the remaining five test values ​​was taken as the "probe tack value of the protective film-coated film at 23°C" (mN). The measured values ​​were rounded off to the nearest integer. The results are shown in Table 2.

[0183] (Surface elasticity of the first release film at 23°C) A cantilever made of silicon nitride (manufactured by Bruker Corporation, product name: MLCT, tip radius: 20 nm, resonance frequency: 125 kHz, spring constant: 0.6 N / m) was installed on an atomic force microscope (manufactured by Bruker Corporation, MultiMode8). The first release film prepared was placed on the atomic force microscope, and the surface of the first release agent layer of the first release film prepared was pressed and pulled away with the installed cantilever at a pressing amount of 2 nm and a scan speed of 10 Hz. The force curve obtained by this operation was fitted by the JKR theoretical formula to calculate the surface elastic modulus. The surface elastic modulus was measured at 4096 points within a 1 μm × 1 μm surface of the first release agent layer of the first release film, and the values ​​were averaged and rounded off to the nearest tenth to obtain the surface elastic modulus (MPa). The results are shown in Table 2.

[0184] (Peeling force F1 of the first release film from the protective film-forming film) The second release film was peeled off from the obtained protective film-forming sheet. A good adhesive surface of a good adhesive PET (PET25A-4100, manufactured by Toyobo Co., Ltd.) having a thickness of 25 μm was attached to the surface of the protective film-forming film exposed by peeling by thermal lamination (70° C., 1 m / min) to prepare a laminate sample. The laminate sample was cut into a width of 100 mm to prepare a measurement sample. The back surface of the first release film of the measurement sample was fixed to a hard support plate with double-sided tape.

[0185] Using a universal tensile tester (manufactured by Shimadzu Corporation, product name "Autograph (registered trademark) AG-IS"), the protective film-forming film / good adhesion PET composite (integrated) was peeled from the first release film at a measurement distance of 100 mm, a peel angle of 180°, and a peel speed of 1 m / min, and the load at that time was measured. Of the measured loads, the average value of the load over 80 mm, excluding the load at the first 10 mm and the load at the last 10 mm of the measurement distance, was taken as the peel force F1. The results are shown in Table 2.

[0186] (Peeling force F2 of second release film from protective film-forming film) The obtained sheet for forming a protective film was cut into a width of 100 mm to prepare a measurement sample. The back surface of the first release film of the measurement sample was fixed to a hard support plate with double-sided tape.

[0187] Using a universal tensile tester (Shimadzu Corporation, product name "Autograph (registered trademark) AG-IS"), the second release film was peeled off from the measurement sample at a measurement distance of 100 mm, a peel angle of 180°, and a peel speed of 1 m / min, and the load at that time was measured. Of the measured loads, the average value of the loads over 80 mm, excluding the loads at the first 10 mm and the last 10 mm of the measurement distance, was taken as the peel force F2.

[0188] The resulting peel forces F1 and F2 were compared and it was confirmed that F1 was greater than F2 for all samples.

[0189] (Punching evaluation) The obtained sheet for forming a protective film was subjected to punching processing (a circular shape with an inner diameter of 298 mm) of the protective film-forming film using a Lintec RAD-3600F / 12, and a laminate of the protective film-forming film and the first release film shown in Figure 2B was obtained. In the direction from the end face of the protective film-forming film toward the center of the protective film-forming film, the distance between the end face and the part where the lifting occurring between the protective film-forming film and the first release film was observed was measured, and the maximum value was judged according to the following criteria. The results are shown in Table 2. A: Less than 1 mm B: 1 or more and less than 2 mm C 2 or more and less than 4 mm D...4mm or more

[0190] [Table 2]

[0191] From Table 2, it was confirmed that when the probe tack value of the protective film-forming film at 23°C, the surface elastic modulus of the surface of the first peel film in contact with the protective film-forming film at 23°C, and the product of these are within the above-mentioned ranges, the formation of lifting is suppressed. [Explanation of symbols]

[0192] 1...Protective film forming sheet 10...Protective film forming film 11...Circular protective film forming film 12...Protective film-forming film other than circular protective film-forming film 20…First release film 21...Base material 22...First release agent layer 30…Second release film 31...Base material 32...Second release agent layer 40…Notch 50...cutting blade

Claims

1. A protective film-forming film and a first release film releasably disposed on one main surface of the protective film-forming film, The probe tack value of the protective film-forming film at 23 ° C. is less than 6200 mN, The surface elastic modulus of the surface of the first release film in contact with the protective film-forming film at 23° C. is 17 MPa or less, The product of the probe tack value and the surface elastic modulus is 66000 mN·MPa or less.

2. The protective film forming sheet according to claim 1, wherein the first release film has a substrate and a first release agent layer formed on one main surface of the substrate, and the first release agent layer is in contact with the protective film forming film.

3. A second release film is disposed releasably on the other main surface of the protective film-forming film, A sheet for forming a protective film as described in claim 1 or 2, wherein when the peeling force of the first release film from the protective film-forming film is F1 and the peeling force of the second release film from the protective film-forming film is F2, F1 and F2 satisfy the relationship F1 > F2.

4. The sheet for forming a protective film according to claim 2 or claim 3 which cites claim 2, wherein the thickness of the first release agent layer is within a range of 30 nm to 200 nm.

5. A sheet for forming a protective film described in any one of claims 1 to 4, wherein the surface elasticity modulus of the surface of the first peelable film in contact with the protective film forming film at 23°C is 15 MPa or less.

6. When the protective film-forming sheet is viewed in plan, a cut is formed in the protective film-forming sheet so that a part of the protective film-forming sheet has a predetermined closed shape, The sheet for forming a protective film according to claim 1 , wherein the cut penetrates the protective film-forming film in a thickness direction of the sheet for forming a protective film and reaches a part of the first release film.

7. A protective film-forming sheet as described in claim 6, wherein in a direction from an end face of a protective film-forming film having a closed shape toward the center of the protective film-forming film, the maximum distance between the end face and a portion where a lift formed between the protective film-forming film and the first release film is observed is less than 4 mm.

8. The method includes a step of forming a cut so that a part of the sheet for forming a protective film according to any one of claims 1 to 5 has a predetermined closed shape, The method for processing a sheet for forming a protective film, wherein the incision penetrates the protective film-forming film in a thickness direction of the sheet for forming a protective film and reaches a part of the first release film.

Citation Information

Patent Citations

  • Sheet sticking device and sticking method

    JP2009026904A

  • Dicing tape for semiconductor processing

    JP2013098224A

  • Sheet manufacturing device

    JP2016141568A

  • Release sheet and method for producing release sheet

    JP2017149048A

  • Release film, and resin composition and coating composition used in the same

    JP2017170672A