Ethylene-vinyl alcohol copolymer resin composition

The EVOH resin composition with a guanidine skeleton and optional additives addresses melt molding stability and coloring issues by maintaining high melt flow rate and stability during long-term operations.

JP7555790B2Active Publication Date: 2024-09-25KURARAY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020184068
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-04
Publication Date
2024-09-25
Estimated Expiration
2040-11-04

AI Technical Summary

Technical Problem

Existing ethylene-vinyl alcohol copolymer (EVOH) resin compositions experience decreased melt flow rate and molding stability during long-term melt molding, leading to handling difficulties and product coloring issues.

Method used

A resin composition containing 100 parts by mass of EVOH with an ethylene unit content of 20-60 mol% and 0.05 to 15 parts by mass of a compound with a guanidine skeleton, along with optional metal salts and other additives, to enhance melt flow rate stability and reduce coloring.

Benefits of technology

The composition maintains high melt flow rate and molding stability during continuous operations, ensuring good handling properties and reduced coloring of molded products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555790000001
    Figure 0007555790000001
Patent Text Reader

Abstract

To provide a resin composition that has high handleability when melted and molded continuously for a long time, and gives, after the long-term continuous treatment, a molding having high molding stability and coloration resistance.SOLUTION: A resin composition contains 100 pts.mass of an ethylene-vinyl alcohol copolymer (A) with an ethylene unit content of more than 20 mol% and 60 mol% or less, and 0.05-15 pts.mass of a compound (B) having guanidine skeleton.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition containing an ethylene-vinyl alcohol copolymer and a compound having a guanidine skeleton. [Background technology]

[0002] Ethylene-vinyl alcohol copolymer (hereinafter sometimes abbreviated as "EVOH") is a material with excellent oxygen barrier properties, oil resistance, antistatic properties, mechanical strength, etc., and is widely used as a variety of packaging materials such as films, sheets, and containers. It can be molded by a variety of methods, but is often melt molded such as extrusion molding or injection molding. In addition to oxygen barrier properties, it is required to have long-run properties during melt molding and good appearance of the molded product.

[0003] In light of such demands, Patent Document 1 describes that an EVOH resin composition containing an appropriate amount of an acid, such as a carboxylic acid or phosphoric acid, or a metal salt, such as an alkali metal salt or an alkaline earth metal salt, has excellent appearance and long-run properties during melt molding. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2001-164059 A Summary of the Invention [Problem to be solved by the invention]

[0005] Usually, melt molding of EVOH requires a temperature of 200°C or higher. When EVOH is exposed to conditions of 200°C or higher for a long period of time, its viscosity tends to gradually increase, or the viscosity may tend to gradually decrease due to the addition of metal salts, etc. The inventors of the present invention focused on viscosity behavior in order to improve melt moldability, and after heat treatment at 220°C for 24 hours under nitrogen, they measured the melt flow rate (MFR) at 230°C under a load of 10.9 kg. 24) is high (viscosity is low), and the ratio of MFR0 measured without heat treatment (MFR 24 It was found that the handleability during melt molding tends to be better when the MFR (MFR0) is lower than 1 and closer to 1.

[0006] However, when the above conventional resin compositions are subjected to melt molding at high temperatures for a long period of time, the MFR after 24 hours tends to be too low, and the molding stability of the molded article obtained by long-term continuous molding may deteriorate or coloring may be observed, leaving room for improvement in melt moldability.

[0007] An object of the present invention is to provide a resin composition which has good handleability when melt-molding is carried out continuously for a long period of time, and which produces molded articles with good molding stability and coloration resistance after long-term continuous operation. [Means for solving the problem]

[0008] That is, the present invention provides [1] A resin composition comprising 100 parts by mass of an ethylene-vinyl alcohol copolymer (A) having an ethylene unit content of more than 20 mol% and not more than 60 mol%, and 0.05 to 15 parts by mass of a compound (B) having a guanidine skeleton; [2] The resin composition according to [1], wherein the ethylene-vinyl alcohol copolymer (A) has a degree of saponification of 80 mol % or more; [3] The resin composition according to [1] or [2], containing a metal salt in an amount of 1 ppm to 10,000 ppm calculated as a metal atom; [4] The resin composition according to [3], wherein the metal salt comprises an alkaline earth metal salt; [5] A molded article comprising the resin composition according to any one of [1] to [4]; [6] A multilayer structure comprising at least one layer made of the resin composition according to any one of [1] to [4] and at least one layer containing a thermoplastic resin other than EVOH (A); This is achieved by providing: Effect of the Invention

[0009] According to the present invention, it is possible to provide a resin composition which has good handleability when melt molding is carried out continuously for a long period of time, and which produces molded articles with good molding stability and coloration resistance after long-term continuous operation. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The resin composition of the present invention is a resin composition containing 100 parts by mass of an ethylene-vinyl alcohol copolymer (A) (hereinafter may be abbreviated as "EVOH (A)") having an ethylene unit content of more than 20 mol% and not more than 60 mol%, and 0.05 to 15 parts by mass of a compound (B) having a guanidine skeleton (hereinafter may be abbreviated as "compound (B)").

[0011] (EVOH(A)) EVOH (A) can usually be obtained by saponifying an ethylene-vinyl ester copolymer. The production and saponification of the ethylene-vinyl ester copolymer can be carried out by a known method. A representative vinyl ester is vinyl acetate, but other fatty acid vinyl esters such as vinyl formate, vinyl propionate, vinyl valerate, vinyl caprate, vinyl laurate, vinyl stearate, vinyl pivalate, and vinyl versatate may also be used.

[0012] The ethylene unit content of EVOH (A) is more than 20 mol%, preferably 22 mol% or more, more preferably 23 mol% or more. The ethylene unit content of EVOH (A) is preferably 60 mol% or less, more preferably 55 mol% or less, even more preferably 50 mol% or less, even more preferably 40 mol% or less, particularly preferably 34 mol% or less, and in some cases 32 mol% or less, 30 mol% or less is preferable. If the ethylene unit content is 20 mol% or less, the handling property during melt molding decreases, and the molding stability and coloring resistance of the molded article of the present invention tend to deteriorate. If it is 60 mol% or more, the gas barrier property decreases, and the advantage as a barrier resin is impaired. If the ethylene unit content of EVOH (A) is a lower ethylene unit content such as 34 mol% or less, the effect of molding stability by compound (B) tends to be significantly manifested. The ethylene unit content of EVOH (A) can be determined by a nuclear magnetic resonance (NMR) method.

[0013] The saponification degree of the vinyl ester component of EVOH (A) is preferably 80 mol% or more, more preferably 90 mol% or more, and even more preferably 99 mol% or more. When the saponification degree is 80 mol% or more, the gas barrier property tends to be improved. The saponification degree of EVOH (A) may be 100 mol% or less, or 99.99 mol% or less. The saponification degree of EVOH (A) is 1 It can be calculated by measuring the peak area of ​​the hydrogen atoms contained in the vinyl ester structure and the peak area of ​​the hydrogen atoms contained in the vinyl alcohol structure through H-NMR measurement.

[0014] In addition, EVOH (A) may have units derived from other monomers other than ethylene, vinyl esters and their saponification products, within the scope of the present invention. When EVOH has the other monomer units, the content of the other monomer units relative to the total structural units of EVOH is preferably 30 mol% or less, more preferably 20 mol% or less, even more preferably 10 mol% or less, and particularly preferably 5 mol% or less. In addition, when EVOH (A) has units derived from the other monomers, the lower limit may be 0.05 mol% or 0.10 mol%. Examples of the other monomers include alkenes such as propylene, butylene, pentene, and hexene; 3-acyloxy-1-propene, 3-acyloxy-1-butene, 4-acyloxy-1-butene, 3,4-diacyloxy-1-butene, 3-acyloxy-4-methyl-1-butene, 4-acyloxy-2-methyl-1-butene, and 4-acyloxy-3-methyl. -1-butene, 3,4-diacyloxy-2-methyl-1-butene, 4-acyloxy-1-pentene, 5-acyloxy-1-pentene, 4,5-diacyloxy-1-pentene, 4-acyloxy-1-hexene, 5-acyloxy-1-hexene, 6-acyloxy-1-hexene, 5,6-diacyloxy-1-hexene, 1,3-diacetoxy-2-methyl alkenes having an ester group such as dimethylpropane or saponified products thereof; unsaturated acids such as acrylic acid, methacrylic acid, crotonic acid, itaconic acid, or the like, or their anhydrides, salts, or mono- or dialkyl esters; nitriles such as acrylonitrile and methacrylonitrile; amides such as acrylamide and methacrylamide; olefin sulfonic acids such as vinyl sulfonic acid, allyl sulfonic acid, methallylsulfonic acid, or the like, or their salts; vinyl silane compounds such as vinyltrimethoxysilane, vinyltriethoxysilane, vinyltri(β-methoxy-ethoxy)silane, γ-methacryloxypropylmethoxysilane; alkyl vinyl ethers, vinyl ketones, N-vinylpyrrolidone, vinyl chloride, vinylidene chloride, and the like.

[0015] The EVOH (A) may be an EVOH (A) that has been post-modified by a technique such as urethanization, acetalization, cyanoethylation, oxyalkylenation, etc. Such modified EVOH (A) tends to have good melt moldability.

[0016] As the EVOH (A), two or more kinds of EVOH (A) differing in ethylene unit content, degree of saponification, copolymer component, presence or absence of modification or type of modification, etc. may be mixed and used.

[0017] (Compound (B) having a guanidine skeleton) The resin composition of the present invention contains the compound (B), and after heat treatment at 220°C for 24 hours under nitrogen, the melt flow rate (MFR 24 ) is higher, and the ratio (MFR 24 / MFR0) approaches 1, which improves the handleability during melt molding and provides molding stability and coloring resistance for molded products after long-term continuous operation. Normally, when EVOH is heat-treated under nitrogen for 24 hours, the MFR tends to increase once and then gradually decrease, and the MFR of EVOH after 24 hours tends to be a very low value, but the addition of compound (B) tends to suppress the decrease in MFR. Although the reason why the addition of compound (B) has such an effect is unclear, it is presumed that the viscosity increase can be suppressed by capturing compounds generated by thermal degradation of EVOH (A). Here, the "compound having a guanidine skeleton" refers to a compound having a structure represented by C(=NR 1 )(-NR 2 R 3 is not particularly limited as long as it has the skeleton of R 1 , R 2 and R 3 Each may independently be any substituent, and a part of the guanidine skeleton may form an aromatic ring.

[0018] Examples of the compound (B) include triazoles such as 3-amino-1,2,4-triazole, salts of guanidine such as cyanoguanidine, guanidine hydrochloride, guanidine nitrate, guanidine carbonate, guanidine phosphate, and guanidine sulfamate, and acid aminoguanidines such as aminoguanidine bicarbonate, aminoguanidine hydrochloride, and aminoguanidine sulfate.

[0019] The content of the compound (B) in the resin composition of the present invention is 0.05 parts by mass or more, preferably 0.1 parts by mass or more, more preferably 0.25 parts by mass or more, even more preferably 0.4 parts by mass or more, and particularly preferably 0.5 parts by mass or more, relative to 100 parts by mass of EVOH (A). The content of the compound (B) is 15 parts by mass or less, preferably 10 parts by mass or less, more preferably 8 parts by mass or less, and particularly preferably 5 parts by mass or less, relative to 100 parts by mass of EVOH (A). When the amount of the compound (B) added is less than 0.05 parts by mass, the handling during melt molding becomes insufficient, and molding stability and coloring resistance tend to become insufficient. When the amount of the compound (B) added is more than 15 parts by mass, the melt moldability deteriorates, and gels and bumps tend to occur during continuous melt molding.

[0020] In addition to EVOH (A) and compound (B), the resin composition of the present invention may contain other components such as a thermoplastic resin other than EVOH (A), a metal salt, an acid, a boron compound, a plasticizer, a filler, an antiblocking agent, a lubricant, a stabilizer, a surfactant, a colorant, an ultraviolet absorber, an antistatic agent, a drying agent, a crosslinking agent, a filler, a reinforcing material such as various fibers, etc. Among these, it is preferable to contain a metal salt and an acid from the viewpoint of thermal stability and adhesion between a layer containing the resin composition of the present invention and other layers.

[0021] As the metal salt, an alkali metal salt is preferred from the viewpoint of further increasing the interlayer adhesion between the layer containing the resin composition of the present invention and another layer, and an alkaline earth metal salt is preferred from the viewpoint of thermal stability. Examples of metals constituting the alkali metal salt include lithium, sodium, potassium, etc., and sodium or potassium is preferred. Examples of the alkali metal salt include aliphatic carboxylates, aromatic carboxylates, carbonates, hydrochlorides, nitrates, sulfates, phosphates, and metal complexes. Among them, aliphatic carboxylates and phosphates are preferred from the viewpoint of easy availability, and specifically, sodium acetate, potassium acetate, sodium phosphate, and potassium phosphate are preferred. Examples of metals constituting the alkaline earth metal salt include magnesium, calcium, strontium, etc., and magnesium or calcium is preferred. Examples of the alkaline earth metal salt include aliphatic carboxylates, aromatic carboxylates, carbonates, hydrochlorides, nitrates, sulfates, phosphates, and metal complexes. Among them, aliphatic carboxylates are preferred, and specifically, when the resin composition of the present invention contains a metal salt, the content is preferably 1 ppm or more in terms of metal atoms of the metal salt, more preferably 5 ppm or more, even more preferably 10 ppm or more, and particularly preferably 20 ppm or more. The content of the metal salt is preferably 10000 ppm or less in terms of metal atoms, more preferably 5000 ppm or less, even more preferably 1000 ppm or less, and particularly preferably 500 ppm or less. When the content of the metal salt is within the above range, the interlayer adhesion between the layer containing the resin composition of the present invention and other layers is maintained well, and the thermal stability during recycling tends to be good. In addition, when a certain amount or more of alkaline earth metal salt is contained, the viscosity tends to decrease (MFR increases) due to heat treatment.

[0022] As the acid, a carboxylic acid compound or a phosphoric acid compound is preferred from the viewpoint of increasing the thermal stability during melt molding of the resin composition of the present invention. The carboxylic acid compound is not particularly limited, and examples thereof include formic acid, acetic acid, propionic acid, butyric acid, caproic acid, capric acid, acrylic acid, methacrylic acid, benzoic acid, 2-naphthoic acid, succinic acid, malic acid, tartaric acid, and citric acid, and an aliphatic carboxylic acid such as acetic acid is preferably used. When the resin composition of the present invention contains a carboxylic acid compound, the content of the carboxylic acid is preferably 1 ppm or more, more preferably 10 ppm or more, and even more preferably 50 ppm or more, based on EVOH (A). In addition, the content of the carboxylic acid is preferably 10,000 ppm or less, more preferably 1,000 ppm or less, and even more preferably 500 ppm or less. The phosphoric acid compound is not particularly limited, and various acids such as phosphoric acid and phosphorous acid and their salts can be used, and sodium dihydrogen phosphate, potassium dihydrogen phosphate, disodium hydrogen phosphate, dipotassium hydrogen phosphate, etc. are preferably used. When the resin composition of the present invention contains a phosphoric acid compound, the content of the phosphoric acid compound is preferably 1 ppm or more, more preferably 10 ppm or more, and even more preferably 30 ppm or more, based on EVOH (A). On the other hand, the content of the phosphoric acid compound is preferably 10,000 ppm or less, more preferably 1,000 ppm or less, and even more preferably 300 ppm or less. When the resin composition of the present invention contains a carboxylic acid compound or a phosphoric acid compound within the above range, the thermal stability during melt molding tends to be improved.

[0023] The proportion of EVOH (A) and compound (B) in the resin composition of the present invention is preferably 70 mass% or more, more preferably 80 mass% or more, even more preferably 90 mass% or more, particularly preferably 95 mass% or more, and in some cases 98 mass% or more or 99 mass% or more is preferred. The resin composition of the present invention may essentially consist of only EVOH (A) and compound (B).

[0024] The resin composition of the present invention was heat-treated at 220°C for 24 hours under nitrogen, and then the MFR was measured at 230°C under a load of 10.9 kg. 24The MFR is preferably 3 g / 10 min or more, more preferably 3.5 g / 10 min or more, and in some cases 5 g / 10 min or more, or 10 g / 10 min or more. 24 The MFR may be 55 g / 10 min or less, 40 g / 10 min or less, or 30 g / 10 min or less. 24 When it is within the above range, molding stability tends to be good.

[0025] The MFR of the resin composition of the present invention is 24 and MFR0 under the conditions of 230℃ and 10.9kg load (MFR 24 / MFR0) is preferably 0.05 or more, more preferably 0.07 or more, and in some cases 0.15 or more, or 0.25 or more. 24 / MFR0 is preferably 1 or less, and may be 0.9 or less, 0.8 or less, 0.7 or less, 0.6 or less, or m0.5 or less.

[0026] (Method of producing resin composition) The method for producing the resin composition of the present invention is not particularly limited, and for example, a method of adding compound (B) to EVOH (A) to adjust the composition is preferably adopted. Examples of the method for adding compound (B) to EVOH (A) include a method of dry blending EVOH (A) and compound (B), a method of adding a solution containing compound (B) to EVOH (A) in a molten state, a method of adding a solution containing compound (B) to EVOH (A) in a paste state impregnated with a solvent, a method of adding compound (B) in a suspended state in a liquid, and a method of adding EVOH (A) by contacting (or immersing) the solution containing compound (B). Among them, from the viewpoint of uniformly dispersing compound (B) in EVOH (A), a method of adding a solution containing compound (B) to EVOH (A) in a molten state, or a method of adding EVOH (A) by contacting (or immersing) the solution containing compound (B) is preferred. The solvent for dissolving compound (B) is not particularly limited, but water is preferably used from the viewpoints of solubility of additives, cost, ease of handling, safety of the working environment, and the like. A similar approach can be used when adding metal salts and acids.

[0027] (Molded body) The resin composition of the present invention can be molded into a molded article such as a film, sheet, tube, bag, or container by melt molding or the like. The resin composition of the present invention has good molding stability and coloring resistance even when melt molding is performed continuously for a long period of time, so that the molded article of the present invention has high productivity. The molded article of the present invention may be a molded article consisting of only the resin composition of the present invention, or may be a molded article consisting of a part consisting of only the resin composition of the present invention and other parts. Examples of methods for melt molding the resin composition of the present invention include extrusion molding, cast molding, inflation extrusion molding, blow molding, melt spinning, injection molding, injection blow molding, etc. The melt molding temperature varies depending on the melting point of EVOH (A), etc., but is preferably about 150 to 270°C. These molded articles can be crushed and molded again for the purpose of reuse. In addition, the film, sheet, etc. can be uniaxially or biaxially stretched.

[0028] (Multilayer structure) The multilayer structure of the present invention comprises at least one layer made of the resin composition of the present invention (hereinafter sometimes referred to as "barrier layer") and at least one layer containing a thermoplastic resin other than EVOH (A) (hereinafter sometimes abbreviated as "thermoplastic resin layer"). The proportion of the thermoplastic resin in the thermoplastic resin layer is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more, and the thermoplastic resin layer may be a layer made of a thermoplastic resin. The number of layers constituting the multilayer structure of the present invention is 2 layers or more, preferably 3 layers or more. The number of layers of the multilayer structure may be 1000 layers or less, 100 layers or less, or 10 layers or less. The multilayer structure of the present invention may further have a layer formed from a material other than a resin, such as a paper layer, a metal layer, etc. The resin composition of the present invention has good molding stability even after long-term continuous operation, so the multilayer structure of the present invention has high production stability.

[0029] The multilayer structure of the present invention may have an adhesive layer because the adhesive layer may enhance the interlayer adhesion between the barrier layer and the thermoplastic resin layer. The layer structure of the multilayer structure of the present invention is not particularly limited, and when the barrier layer is represented by E, the adhesive layer is represented by Ad, and the thermoplastic resin layer is represented by T, examples of the layer structure include T / E / T, E / Ad / T, and T / Ad / E / Ad / T, and the like. The multilayer structure having these layer structures is preferable. Each of these layers may be a single layer or a multilayer.

[0030] Examples of the thermoplastic resin include linear low-density polyethylene, low-density polyethylene, medium-density polyethylene, high-density polyethylene, ethylene-vinyl acetate copolymer, ethylene-propylene copolymer, polypropylene, propylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymer, polybutene, polypentene, and other olefin homopolymers or copolymers; polyethylene terephthalate, and other polyesters; polyester elastomers; polyamides such as nylon-6 and nylon-66; polystyrene; polyvinyl chloride, polyvinylidene chloride, acrylic resins, vinyl ester resins, polyurethane elastomers, polycarbonate, chlorinated polyethylene, chlorinated polypropylene, etc. Among these, polypropylene, polyethylene, ethylene-propylene copolymer, ethylene-vinyl acetate copolymer, polyamide, polystyrene, and polyester are preferably used.

[0031] The adhesive layer may be a layer made of an adhesive used for lamination or the like, or may be a layer made of an adhesive resin. The adhesive resin is not particularly limited as long as it has adhesiveness with the barrier layer and layers made of other components (for example, a thermoplastic resin layer), but an adhesive resin containing a carboxylic acid-modified polyolefin is preferred. The carboxylic acid-modified polyolefin is preferably a modified olefin polymer containing a carboxyl group in which an ethylenically unsaturated carboxylic acid, its ester, or its anhydride is chemically bonded to an olefin polymer. Here, the olefin polymer means a polyolefin such as polyethylene, linear low-density polyethylene, polypropylene, polybutene, or a copolymer of an olefin and another monomer, and the olefin polymer serving as the base of the adhesive resin is preferably a linear low-density polyethylene, an ethylene-vinyl acetate copolymer, or an ethylene-ethyl acrylate copolymer, and particularly preferably a linear low-density polyethylene or an ethylene-vinyl acetate copolymer.

[0032] The method for producing the multilayer structure of the present invention is not particularly limited, and examples thereof include a method of melt-extruding a thermoplastic resin into a molded article made of the resin composition of the present invention, a method of co-extruding the resin composition of the present invention and a thermoplastic resin, a method of coinjection molding the resin composition of the present invention and a thermoplastic resin, and a method of laminating a barrier layer and a resin composition layer using a known adhesive such as an organic titanium compound, an isocyanate compound, or a polyester-based compound.

[0033] The method for co-extrusion of the resin composition of the present invention and a thermoplastic resin is not particularly limited, and examples thereof include a multi-manifold merging type T-die method, a feed block merging type T-die method, and an inflation method.

[0034] The multilayer structure of the present invention may be in the form of a film or sheet, and may be molded into various shapes. The multilayer structure of the present invention can be used for packaging materials, containers, tubes, etc., and can also be suitably used as a material for thermoforming, such as for thermoformed containers. EXAMPLES

[0035] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to the examples shown below.

[0036] <Materials used> EVOH(A) A-1: "Eval (trademark) L101B"; manufactured by Kuraray Co., Ltd., EVOH, ethylene unit content 27 mol% A-2: "EVAL (trademark) M100B"; manufactured by Kuraray Co., Ltd., EVOH, ethylene unit content 24 mol% ·Compound (B) B-1: "3-amino-1H-1,2,4-triazole"; manufactured by Wako Pure Chemical Industries, Ltd. B-2: "Guanidino carbonate"; manufactured by Wako Pure Chemical Industries, Ltd. Additives other than compound (B) B-C1: "Pyrogallol"; Fujifilm Wako Pure Chemical Industries, Ltd. B-C2: "Benzotriazole"; manufactured by Wako Pure Chemical Industries, Ltd.

[0037] <Evaluation method> (1) Quantitative determination of carboxylic acid compounds The resin compositions obtained in the examples and comparative examples were pulverized by freeze pulverization. The pulverized material obtained was sieved with a sieve with a nominal size of 1 mm (based on the standard sieve standard JIS-Z8801). 10 g of the pulverized material that passed through the sieve and 50 mL of ion-exchanged water were placed in a 100 mL Erlenmeyer flask with a stopper, and a cooling condenser was attached, followed by stirring and extraction at 95°C for 10 hours. 2 mL of the obtained extract was diluted with 8 mL of ion-exchanged water. The diluted extract was quantitatively analyzed using an ion chromatography "IC7000" manufactured by Yokogawa Electric Corporation, and the amount of carboxylate ions was quantified to calculate the amount of carboxylate radicals of the carboxylate compound. In addition, a calibration curve prepared using an aqueous acetic acid solution was used for quantification. Ion chromatography measurement conditions: Column: Dionex IonPac "ICE-AS-1" Eluent: 1.0mmol / L octanesulfonic acid solution Measurement temperature: 35℃ Eluent flow rate: 1mL / min. Sample injection volume: 50 μL

[0038] (2) Quantitative determination of metal salts The resin compositions obtained in the examples and comparative examples were pulverized by freeze pulverization. 10 g of the pulverized material obtained and 50 mL of ion-exchanged water were placed in a 100 mL Erlenmeyer flask with a stopper, and a cooling condenser was attached, and the mixture was stirred at 95°C for 10 hours and heated for extraction. 2 mL of the obtained extract was diluted with 8 mL of ion-exchanged water. The diluted extract was quantitatively analyzed at each observation wavelength shown below using an ICP emission spectrometer "Optima 4300 DV" manufactured by PerkinElmer Japan, to calculate the metal atom equivalent amount of the metal salt. Na: 589.592 nm K: 766.490 nm Mg: 285.213 nm Ca: 317.933 nm

[0039] (3) Quantitative determination of phosphate compounds The resin compositions obtained in the examples and comparative examples were pulverized by freeze pulverization. 1.0 g of the pulverized material obtained, 15 mL of concentrated nitric acid, and 4 mL of concentrated sulfuric acid were placed in a 100 mL Erlenmeyer flask with a stopper, and a cooling condenser was attached, followed by thermal decomposition at 200 to 230°C. The resulting solution was made up to 50 mL of a measuring flask with ion-exchanged water. The above solution was quantitatively analyzed at an observation wavelength of 214.914 nm using an ICP emission spectrometer "Optima 4300 DV" manufactured by PerkinElmer Japan, to quantify the amount of phosphorus element, and the amount of phosphate radical of the phosphate compound was calculated.

[0040] (4) Melt viscosity behavior evaluation For the resin compositions obtained in the examples and comparative examples, the MFR0 was measured under a load of 10.9 kg at 230°C, and the MFR under a load of 10.9 kg at 230°C after a sealed tube heat treatment under nitrogen at 220°C for 24 hours was measured. 24 The MFR was high after 24 hours, and the MFR ratio (MFR 24The lower the MFR0 is and the closer it is to 1, the more stable the melt viscosity is, and the greater the long-term thermal stability is.

[0041] (5) Evaluation of molding stability of single-layer film using resin composition The resin compositions obtained in the examples and comparative examples were extruded into a monolayer film under the following conditions using a 20 mm extruder "D2020" (D (mm) = 20, L / D = 20, compression ratio = 2.0, screw: full flight) manufactured by Toyo Seiki Seisakusho Co., Ltd. The film was sampled after 24 hours of continuous operation. Extrusion temperature: feeding section / compression section / metering section / die = 180 / 260 / 260 / 260℃ Screw rotation speed: 40 rpm Discharge amount: 1.3kg / hr Take-up roll temperature: 80℃ Take-off roll speed: 3.1m / min. Film thickness: 20μm

[0042] The monolayer film sampled 24 hours later was wound up on a paper tube, and the roughness of the film surface was judged with the naked eye as follows, and molding stability was evaluated. Judgment criteria A: No roughness on the film surface B: Film surface is rough C: Significant film surface roughness

[0043] (6) Color resistance evaluation The coloring degree of the end surface of the roll of the monolayer film wound around the paper tube produced by the above evaluation method (5) was judged by the naked eye as follows. Judgment criteria A: No coloring B: Slightly yellowed C: Yellowing

[0044] <Example 1> "EVAL (registered trademark) L101B" was dried at 60°C for 48 hours using a dryer. 20 kg was taken out of the dried EVOH, and dissolved in 43 L of a water / methanol mixed solution (weight ratio: water / methanol = 4 / 6) at 80°C for 12 hours while stirring, and the solution temperature was lowered to 65°C and then left for 5 hours. Then, the solution was extruded from a gold plate having a circular opening with a diameter of 3.5 mm into a water / methanol mixed solution (weight ratio: water / methanol = 9 / 1) to precipitate in the form of strands, and cut into pellets with a diameter of about 4 mm and a length of about 5 mm. 2.4 kg was taken out of the obtained pellets, 24 L of pure water was added, and the operation of stirring at 25°C for 2 hours and dehydrating was repeated twice to obtain hydrous EVOH pellets.

[0045] The obtained hydrous EVOH pellets (2 kg) were placed in 40 L of the immersion liquid described below, and immersed at 25°C for 4 hours while being intermittently stirred. The hydrous EVOH pellets after immersion were centrifuged and dried in a hot air dryer at 80°C for 3 hours, and then dried at 105°C for 15 hours to obtain a resin composition 1. The obtained resin composition 1 was evaluated according to the above evaluation methods (1) to (6). The evaluation results are shown in Table 1. As the immersion liquid, an aqueous solution containing sodium acetate, potassium dihydrogen phosphate, magnesium acetate, acetic acid, and 3-amino-1H-1,2,4-triazole was used, and the concentration of each component was appropriately adjusted so that the content of each component in the obtained resin composition 1 was the content shown in Table 1.

[0046] <Examples 2 to 4, Comparative Examples 1 to 4> Resin compositions 2 to 4 and C1 to C4 were produced and evaluated in the same manner as in Example 1, except that the types of resins and the types and amounts of additives used were changed as shown in Table 1. The evaluation results are shown in Table 1.

[0047] [Table 1]

Claims

1. A resin composition comprising: 100 parts by mass of an ethylene-vinyl alcohol copolymer (A) having an ethylene unit content of more than 20 mol% and not more than 60 mol%; and 0.5 to 15 parts by mass of a compound (B) having a guanidine skeleton, wherein the compound (B) having a guanidine skeleton is a triazole.

2. 2. The resin composition according to claim 1, wherein the ethylene-vinyl alcohol copolymer (A) has a degree of saponification of 80 mol % or more.

3. 3. The resin composition according to claim 1, comprising a metal salt in an amount of 1 ppm to 10,000 ppm in terms of metal atom.

4. The resin composition according to claim 3 , wherein the metal salt comprises an alkaline earth metal salt.

5. A molded article comprising the resin composition according to any one of claims 1 to 4.

6. A multilayer structure comprising at least one layer made of the resin composition according to any one of claims 1 to 4 and at least one layer containing a thermoplastic resin other than EVOH (A).

Citation Information

Patent Citations

  • Resin composition comprising ethylene-vinyl alcohol copolymer having excellent long run property and multilayer structure using the composition

    JP2001164059A

  • Ethylene-vinyl ester copolymer saponification product composition and multilayer structure using the composition

    JP2012107197A

  • Thermoplastic elastomer composition for non-pneumatic tire and non-pneumatic tire

    JP2016003265A

  • Thermoplastic resin composition

    WO2010110077A1

  • Saponified ethylene / vinyl ester copolymer composition and multilayer structure using the composition

    WO2012005288A1