Molding resin sheet and molded product using same
A resin sheet with a polycarbonate base and high hardness resin layer, combined with a hard coat or anti-glare layer, addresses color unevenness and molding issues, ensuring high hardness and visibility in polarized light, and facilitates touch sensor attachment on curved surfaces.
Patent Information
- Application Number
- JP2021539217
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-08-09
- Filing Date
- 2020-08-04
- Publication Date
- 2024-09-25
- Estimated Expiration
- 2040-08-04
AI Technical Summary
Existing resin sheets for molding in touch panel displays face challenges such as color unevenness and discoloration when viewed with polarized sunglasses, difficulty in attaching touch sensors to curved surfaces, and issues with abnormal appearances during molding, particularly due to differences in glass transition points and melt viscosities of layered resins.
A resin sheet with a polycarbonate resin base layer and a high hardness resin layer, combined with a hard coat or anti-glare layer, where the glass transition points of the resins satisfy a specific relationship, and a resin film touch sensor with controlled in-plane retardation is bonded to suppress color unevenness and enhance scratch resistance.
The resin sheet provides high hardness, reduces abnormal appearances during molding, and maintains visibility without color unevenness even when viewed with polarized sunglasses, while being suitable for thermoforming and easy attachment of touch sensors to curved surfaces.
Smart Images

Figure 0007555932000001 
Figure 0007555932000002 
Figure 0007555932000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a molding resin sheet and a molded article using the same. [Background technology]
[0002] Glass plates, transparent resin plates, etc. are used for components of display surfaces of automobile interior parts such as instrument covers, home appliances, OA equipment, personal computers, small portable devices, etc., and resin molded bodies are used for frame parts that hold them. On the other hand, components of touch panel type display surfaces used in mobile phone terminals, etc., are made of a transparent sheet, especially a glass plate, attached to a frame part made of injection molded resin with double-sided adhesive tape, etc. For touch panel type display surfaces, a thinner one is preferable from the viewpoint of response speed, but a certain thickness is necessary from the viewpoint of strength, so a material with a high elasticity is selected. In addition, scratch resistance and fingerprint wiping ability are also required.
[0003] The resin molded products used for the above-mentioned applications can be produced by molding a resin sheet, but various efforts have been made to impart properties according to the application, such as modifying the resin sheet with a hard coat layer, a decorative sheet, etc., constructing a resin sheet by laminating resin layers having different compositions, and improving the composition of the resin used.
[0004] The decorative sheet is made of, for example, an acrylic resin, and includes a sheet having a hard coat layer, a sheet having a design such as printing, and a sheet having a film laminated thereon. For example, Patent Document 1 discloses a decorative sheet in which, from the surface side, a transparent acrylic resin sheet layer, a picture-printed ink layer, an ABS resin sheet layer, and an ABS resin backer layer are laminated. Patent Document 2 discloses a multilayer film in which a layer made of methacrylic resin and acrylic rubber particles is laminated on the surface of a polycarbonate resin layer, and a decorative sheet in which one surface of the multilayer film is decorated and a thermoplastic resin sheet is laminated on the decorated surface. Furthermore, a decorated molded product manufactured by injection molding a thermoplastic resin on the decorated surface is also disclosed.
[0005] Patent Document 3 discloses a resin molded product that is molded using a sheet in which a thermosetting or ultraviolet curing hard coat layer is provided on a resin substrate. Patent Document 4 also discloses a decorative hard-coated film having a layer formed on one side of a base film using a hard-coat paint of a specific composition, and also describes that a printed layer may be provided on the base film. This decorative film is thermoformable. The decorative film described in Patent Document 4 is integrated with a molding resin to become a decorated molded product. Patent Document 5 discloses a laminate sheet having a coating layer mainly made of an acrylic resin on one side of a base layer mainly made of a polycarbonate resin composition.
[0006] In addition, components of the display surface may be provided with an anti-glare layer to scatter reflections of external light and make the display easier to see. Anti-glare treatment is performed by imparting fine structures or shapes to the surface. If the display surface is curved, when using a glass plate as a front panel component, it is necessary to bend the glass plate before applying anti-glare treatment. This is because the anti-glare layer cannot withstand the bending temperature of the glass and will disappear. However, it is difficult to apply anti-glare treatment uniformly to a curved surface. On the other hand, when using a resin plate, it is possible to bend a flat plate that has already been anti-glare treated. The bending temperature of a resin plate is significantly lower than that of glass, and the anti-glare layer will not disappear, so there is an advantage that there is no need to apply anti-glare treatment to the curved surface.
[0007] The display surfaces of car navigation systems, smartphones, etc. are often equipped with touch panel functions, but when the display surface is curved, it is very difficult to attach a touch sensor to the curved resin front panel. Therefore, a method in which a touch sensor is attached to the flat resin plate before it is shaped into a curved shape, and then the resin plate and the touch sensor are shaped at the same time, eliminates the need to attach a touch sensor to the curved front panel, making the manufacturing process extremely productive. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2001-334609 A [Patent Document 2] JP 2009-234184 A [Patent Document 3] Special Publication No. 4-40183 [Patent Document 4] JP 2010-284910 A [Patent Document 5] JP 2009-196153 A Summary of the Invention [Problem to be solved by the invention]
[0009] As a result of the inventors' investigation into the combination of a resin front panel and a touch sensor, it was found that a resin front panel with high retardation and a resin film touch sensor with low retardation were suitable. This is because with any other retardation combination, color unevenness or coloring occurs and visibility deteriorates when viewing a car navigation system or a smartphone while wearing polarized sunglasses.
[0010] In addition to the combination of a high-retardation resin front panel and a low-retardation resin film touch sensor, if the slow axis of the resin front panel and the slow axis of the resin film touch sensor are laminated in a parallel or perpendicular relationship, color unevenness or discoloration will not occur, but there is a high possibility that the axes will become misaligned during shaping.
[0011] Here, the inventors have found that the retardation of a high retardation resin front panel is preferably 3500 nm or more, and 4000 nm is even better, and that the retardation of a low retardation resin film touch sensor is preferably 100 nm or less, and 50 nm or less is even better.
[0012] When bending a resin plate, the plate is often hot-bent by pressing the heated resin plate using a metal mold, wooden mold, resin mold, etc.
[0013] The pursuit of resin sheets or films from which resin molded articles having properties suited to different applications can be produced is a never-ending challenge.
[0014] The present invention aims to provide a molding resin sheet that has high hardness, is less likely to cause appearance abnormalities during molding, and suppresses color unevenness and coloring even when wearing polarized sunglasses, and a resin molded product using the same. [Means for solving the problem]
[0015] The present inventors have intensively studied a molding resin sheet containing a polycarbonate resin as a substrate, the resin sheet having a hard coat layer on the surface, and a resin film touch sensor to be attached to the resin sheet. As a result, it has been found that a resin sheet having high hardness and hardly causing appearance abnormalities such as cracks and flow marks during molding can be provided by providing a high-hardness resin layer between the polycarbonate resin layer and the hard coat layer, and further selecting polycarbonate resin and high-hardness resin whose respective glass transition points satisfy a predetermined relationship. In addition, by selecting the retardation of the resin sheet and the retardation of the resin film touch sensor to be attached, it has become possible to suppress color unevenness and coloring when wearing polarized sunglasses, even after the molding resin sheet with the film sensor is thermally shaped. That is, the present invention is, for example, as follows.
[0016] <1> A resin sheet having a high-hardness resin layer containing a high-hardness resin on at least one surface of a substrate layer containing a polycarbonate resin (a1), and a hard coat layer or a hard coat anti-glare layer laminated on at least one surface of the high-hardness resin layer, The glass transition points of the polycarbonate resin (a1) and the high-hardness resin satisfy the following relationship: -10℃≦(glass transition point of high hardness resin)-(glass transition point of polycarbonate resin (a1))≦40℃ The in-plane retardation of the resin sheet when measured at a wavelength of 543 nm is 4000 nm or more; A molding resin sheet having a resin film (X) having an in-plane retardation of 50 nm or less when measured at a wavelength of 543 nm laminated to one surface of the resin sheet with an adhesive layer containing an adhesive. <2> The polycarbonate resin (a1) is an aromatic polycarbonate resin. <1> The molding resin sheet according to claim 1. <3> The aromatic polycarbonate resin contains a structural unit represented by the following general formula (4a): <2> The molding resin sheet according to claim 1. [ka] <4> The content of the polycarbonate resin (a1) is 75 to 100% by mass based on the total mass of the base layer. <1> ~ <3> 2. The molding resin sheet according to claim 1 . <5> The high-hardness resin is selected from the group consisting of the following resins (B1) to (B6). <1> ~ <4> The molding resin sheet according to any one of the preceding claims: Resin (B1): A copolymer containing a (meth)acrylic acid ester structural unit (a) represented by the following general formula (1) and an aliphatic vinyl structural unit (b) represented by the following general formula (2), or an alloy of the copolymer with resin (B2). [ka] (In the formula, R1 is a hydrogen atom or a methyl group; R2 is an alkyl group having 1 to 18 carbon atoms.) [ka] (In the formula, R3 is a hydrogen atom or a methyl group; R4 is a cyclohexyl group which may be substituted with a hydrocarbon group having 1 to 4 carbon atoms); Resin (B2): a copolymer (D) containing 6 to 77 mass% of (meth)acrylic acid ester structural units, 15 to 71 mass% of styrene structural units, and 8 to 23 mass% of unsaturated dicarboxylic acid structural units, an alloy of the copolymer (D) itself, an alloy of the copolymer (D) with another high-hardness resin, or an alloy of the copolymer (D) with an acrylic resin; Resin (B3): A copolymer containing a structural unit (c) represented by the following general formula (6) and, optionally, a structural unit (d) represented by the following general formula (7); [ka] [ka] Resin (B4): a copolymer (G) containing 5 to 20 mass% of styrene structural units, 60 to 90 mass% of (meth)acrylic acid ester structural units, and 5 to 20 mass% of N-substituted maleimide structural units, or an alloy of the copolymer (G) and the resin (B2); Resin (B5): A resin containing a structural unit (e) represented by the following general formula (8). [ka] Resin (B6): An alloy of a copolymer containing 50 to 95% by mass of styrene constituent units and 5 to 50% by mass of unsaturated dicarboxylic acid units and an acrylic resin. <6> The content of the high-hardness resin is 70 to 100% by mass based on the total mass of the high-hardness resin layer. <1> ~ <5> 2. The molding resin sheet according to claim 1 . <7> The total thickness of the base layer and the high-hardness resin layer is 0.5 mm to 3.5 mm. <1> ~ <6> 2. The molding resin sheet according to claim 1 . <8> The ratio of the thickness of the base material layer to the total thickness of the base material layer and the high-hardness resin layer is 75% to 99%. <1> ~ <7> 2. The molding resin sheet according to claim 1 . <9> The molding resin sheet has a haze of 2 to 30%. <1> ~ <8> 2. The molding resin sheet according to claim 1 . <10> The hard coat layer surface of the molding resin sheet has a pencil hardness of 2H or more. <1> ~ <9> 2. The molding resin sheet according to claim 1 . <11> The resin film (X) in the molding resin sheet is a polycarbonate film containing a polycarbonate resin (a1). <1> ~ <10> 2. The molding resin sheet according to claim 1 . <12> The resin film (X) in the molding resin sheet is a film touch sensor having a sensor electrode applied to a polycarbonate film. <1> ~ <10> 2. The molding resin sheet according to claim 1 . <13> The above-mentioned adhesive layer in the molding resin sheet is an optical adhesive sheet. <1> ~ <12> 2. The molding resin sheet according to claim 1 . <14> the above <1> ~ <13> 2. A resin molded product molded using the molding resin sheet according to claim 1. Effect of the Invention
[0017] According to the present invention, it is possible to provide a molding resin sheet that has high hardness, is unlikely to cause abnormal appearance during molding, and is suppressed from causing uneven coloring or coloring even when wearing polarized sunglasses, and a resin molded product using the same. In the present invention, a high-hardness resin layer is provided on a substrate layer containing a polycarbonate resin, and a hard coat layer or a hard coat anti-glare layer is further provided on the outside, so that it is possible to provide a resin plate that is resistant to scratches, has anti-glare properties, good visibility, and is easy to bend with heat. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Hereinafter, the present invention will be described in detail by way of examples and working examples. However, the present invention is not limited to the illustrated examples and working examples, and can be modified in any manner without departing from the scope of the present invention.
[0019] The molding resin sheet of the present invention (hereinafter, also simply referred to as "resin sheet") comprises a substrate layer containing a polycarbonate resin (a1), a high-hardness resin layer containing a high-hardness resin, and a hard coat layer or a hard coat anti-glare layer, and the high-hardness resin layer is located between the substrate layer and the hard coat layer or the hard coat anti-glare layer. An additional layer may be present between the substrate layer and the high-hardness resin layer, and between the high-hardness resin layer and the hard coat layer or the hard coat anti-glare layer, respectively. Examples of the additional layer include, but are not limited to, an adhesive layer, a primer layer, and the like. The additional layer may not be present, and as one embodiment, a resin sheet is provided that comprises a substrate layer containing a polycarbonate resin (a1), a high-hardness resin layer laminated on at least one surface of the substrate layer, and a hard coat layer or a hard coat anti-glare layer laminated on the high-hardness resin layer.
[0020] The high-hardness resin layer and the hard coat layer or the hard coat anti-glare layer may be provided on at least one side of the substrate layer, and there is no particular restriction on the configuration of the other side.The high-hardness resin layer may also be provided on both sides of the substrate layer, and in this case, the hard coat layer or the hard coat anti-glare layer can be provided on one or both of the high-hardness resin layers.When the high-hardness resin layer is provided on both sides of the substrate layer, it is desirable to use the same high-hardness resin for the two high-hardness resin layers in order to obtain a stable resin sheet with little warping.
[0021] As described above, the molding resin sheet of the present invention has a high hardness resin layer between the substrate layer and the hard coat layer or hard coat anti-glare layer, and further the glass transition points of the polycarbonate resin (a1) in the substrate layer and the high hardness resin in the high hardness resin layer satisfy a predetermined relationship, so that a resin sheet having high hardness and unlikely to cause abnormal appearance such as cracks and flow marks during molding can be obtained. In particular, since abnormal appearance is unlikely to occur during thermoforming, such a resin sheet can be said to be a resin sheet suitable for thermoforming because the conditions during thermoforming (temperature, heating time, etc.) can be set widely. In addition, by previously laminating a resin film touch sensor before molding a resin sheet suitable for thermoforming, the difficult process of laminating a touch sensor to a front panel having a curved surface after molding can be omitted. This makes it possible to improve the productivity of display front panels having curved surfaces.
[0022] The resin sheet having a hard coat layer or hard coat anti-glare layer with high hardness on the surface as in the present invention, particularly the resin sheet using polycarbonate resin as the substrate, has excellent impact resistance, high safety, and is lightweight compared to a normal glass plate.In addition, it is easier to bend than a normal glass plate, and does not break even with a small bend.This is thought to be because the hard coat layer or hard coat anti-glare layer in the resin sheet has a certain degree of flexibility. By providing a high-hardness resin layer between the substrate layer and the hard-coat anti-glare layer, the hardness of the resin sheet can be further increased. When the hard-coat anti-glare layer is provided directly on the polycarbonate resin layer, the elastic modulus is low and the layer is prone to buckling, but by providing a high-hardness resin layer, such a problem can be solved.
[0023] In the present invention, the glass transition points of the polycarbonate resin (a1) in the substrate layer and the high-hardness resin in the high-hardness resin layer satisfy the following relationship. -10℃≦(glass transition point of high hardness resin)-(glass transition point of polycarbonate resin (a1))≦40℃ Conventionally, when different types of resin layers are laminated and a hard coat layer is provided thereon, the resins contained in each layer have different glass transition points (Tg) and melt viscosities, which makes it difficult to perform thermoforming without causing defects such as cracks. However, according to the present invention, such problems can be solved by using a polycarbonate resin (a1) and a high hardness resin that satisfy the above-mentioned relationship.
[0024] When a multi-layered resin sheet is thermoformed into a desired shape, it is usually formed according to the molding temperature of the resin contained in the largest amount in the layer. For example, in the case of a resin sheet using a polycarbonate resin as a substrate layer, since the polycarbonate resin having good impact resistance is usually contained in the largest amount, thermoforming is performed at a molding temperature suited to the polycarbonate resin. Since the resin sheet of the present invention uses the polycarbonate resin (a1) and the high hardness resin that satisfy the above relationship, the problem of abnormal appearance is unlikely to occur even when thermoforming is performed at a molding temperature suitable for the polycarbonate resin. Therefore, it can be said that the resin sheet of the present invention is a resin sheet that is more suitable for thermoforming than conventional ones.
[0025] The glass transition points of the polycarbonate resin (a1) and the high hardness resin are preferably -5°C < (glass transition point of the high hardness resin) - (glass transition point of the polycarbonate resin (a1)) < 30°C, and more preferably 0°C < (glass transition point of the high hardness resin) - (glass transition point of the polycarbonate resin (a1)) < 30°C. If the Tg of the high hardness resin is extremely lower than the Tg of the polycarbonate resin (a1), the high hardness resin becomes in a rubbery or molten state during thermoforming and becomes easily mobile. In such a case, the hard coat anti-glare layer, which has a highly crosslinked structure and remains hard even when heated, cannot follow the movement of the high hardness resin that has become easily mobile, and cracks are easily generated. On the other hand, if the Tg of the high-hardness resin is too high compared with the Tg of the polycarbonate resin (a1), the difference in viscosity between the high-hardness resin and the polycarbonate resin becomes large, causing the interface to become rough when they are laminated, which may result in flow marks.
[0026] The resin sheet of the present invention can be suitably used for manufacturing molded products having a curved shape that requires hardness. For example, it is possible to successfully manufacture components having a flat portion and a curved portion that is continuous with the flat portion, and therefore it is possible to provide products having novel designs and functions. When attempting to manufacture molded products having the above-mentioned shapes with conventional resin sheets, many problems occurred, such as cracks occurring during thermoforming, such as heat press molding, vacuum molding, pressure molding, and TOM molding. Therefore, in order to suppress the occurrence of cracks during thermoforming, it was necessary to devise measures such as reducing the hardness of the hard coat. However, when the hardness of the hard coat is reduced, although the thermoformability is improved, new problems occurred, such as the hard coat being easily scratched due to its softness and reduced chemical resistance.
[0027] In contrast, according to the present invention, since the occurrence of cracks is suppressed as described above, it is possible to provide a thermoformable resin sheet without reducing the hardness of the hard coat. The resin sheet of the present invention is resistant to scratches and has high chemical resistance because a hard hard coat anti-glare layer can be provided on the surface. By utilizing such characteristics, the resin sheet of the present invention can be used for components of display surfaces of personal computers, mobile phones, etc., exterior and interior parts of automobiles, and curved housings and front panels of mobile phone terminals, personal computers, tablet PCs, car navigation systems, etc.
[0028] Each of the components of the resin sheet according to the present invention will be described below. 1.Base material layer The substrate layer is a resin layer mainly containing a polycarbonate resin (a1). The polycarbonate resin (a1) contained in the substrate layer may be one type or two or more types. The content of the polycarbonate resin (a1) in the substrate layer is preferably 75 to 100 mass % relative to the total mass of the substrate layer, more preferably 90 to 100 mass %, and particularly preferably 100 mass %. By increasing the content of the polycarbonate resin, the impact resistance is improved.
[0029] The polycarbonate resin (a1) is not particularly limited as long as it contains a carbonate bond, i.e., -[OR-OCO]- unit (where R may contain an aliphatic group, an aromatic group, or both an aliphatic group and an aromatic group, and may have a straight-chain structure or a branched structure), in the molecular main chain, but is preferably an aromatic polycarbonate resin, and particularly preferably a polycarbonate resin containing a structural unit of the following formula (4a). By using such a polycarbonate resin, a resin sheet with excellent impact resistance can be obtained.
[0030] [ka] Specifically, as the polycarbonate resin (a1), aromatic polycarbonate resins (for example, Iupilon S-2000, Iupilon S-1000, Iupilon E-2000; manufactured by Mitsubishi Engineering Plastics Corporation) and the like can be used.
[0031] In recent years, polycarbonate resins to which a monohydric phenol represented by the following general formula (4) has been added as a terminal terminator have been used for the purpose of controlling the glass transition temperature of the polycarbonate resin. In the present invention, polycarbonate resins to which such a terminal terminator has been added can also be used. [ka] (In the formula, R1 represents an alkyl group having 8 to 36 carbon atoms or an alkenyl group having 8 to 36 carbon atoms; R2 to R5 each independently represent a hydrogen atom, a halogen, or an optionally substituted alkyl group having 1 to 20 carbon atoms or an optionally substituted aryl group having 6 to 12 carbon atoms; and the substituent is a halogen, an alkyl group having 1 to 20 carbon atoms, or an optionally substituted aryl group having 6 to 12 carbon atoms.) In this specification, the "alkyl group" and the "alkenyl group" may be straight-chain or branched, and may have a substituent.
[0032] More preferably, the monohydric phenol represented by the general formula (4) is represented by the following general formula (5). [ka] (In the formula, R1 represents an alkyl group having 8 to 36 carbon atoms or an alkenyl group having 8 to 36 carbon atoms.)
[0033] The number of carbon atoms in R1 in general formula (4) or general formula (5) is more preferably within a specific numerical range. Specifically, the upper limit of the number of carbon atoms in R1 is preferably 36, more preferably 22, and particularly preferably 18. The lower limit of the number of carbon atoms in R1 is preferably 8, and more preferably 12.
[0034] Among the monohydric phenols represented by the general formula (4) or the general formula (5), it is particularly preferable to use either or both of parahydroxybenzoic acid hexadecyl ester and parahydroxybenzoic acid 2-hexyldecyl ester as the end terminator.
[0035] For example, when a monohydric phenol in which R1 is an alkyl group having 16 carbon atoms in general formula (5) is used as an end terminator, a polycarbonate resin excellent in glass transition temperature, melt fluidity, moldability, drawdown resistance, etc. can be obtained, and further, the monohydric phenol has excellent solubility in a solvent during the production of the polycarbonate resin, which is particularly preferred.
[0036] On the other hand, if the number of carbon atoms in R1 in general formula (4) or general formula (5) is too large, the solubility of the monohydric phenol (end terminator) in organic solvents tends to decrease, which may result in a decrease in productivity during the production of polycarbonate resin. For example, if the carbon number of R1 is 36 or less, the productivity is high and the economic efficiency is good in producing the polycarbonate resin. If the carbon number of R1 is 22 or less, the monohydric phenol has particularly excellent solubility in organic solvents, and the productivity can be very high in producing the polycarbonate resin, and the economic efficiency is also improved. Examples of polycarbonate resins using such monohydric phenols include Iupizeta T-1380 (manufactured by Mitsubishi Gas Chemical Co., Ltd.). If the number of carbon atoms in R1 in general formula (4) or general formula (5) is too small, the glass transition point of the polycarbonate resin will not be a sufficiently low value, and thermoformability may decrease.
[0037] In the present invention, the weight average molecular weight of the polycarbonate resin (a1) may affect the impact resistance and molding conditions of the resin sheet. That is, if the weight average molecular weight is too small, the impact resistance of the resin sheet may decrease. If the weight average molecular weight is too high, an excessive heat source may be required when forming a base layer containing the polycarbonate resin (a1). In addition, depending on the molding method selected, a high temperature may be required, so that the polycarbonate resin (a1) is exposed to a high temperature, which may adversely affect its thermal stability. The weight average molecular weight of the polycarbonate resin (a1) is preferably 15,000 to 75,000, more preferably 20,000 to 70,000. It is further preferably 20,000 to 65,000. The weight average molecular weight in this specification is the weight average molecular weight measured by gel permeation chromatography (GPC) and converted into standard polystyrene.
[0038] Those skilled in the art can appropriately select and use a polycarbonate resin (a1) having a Tg that satisfies the above relationship from among known polycarbonate resins, taking into consideration the glass transition point (Tg) of the high hardness resin to be used. The Tg of the polycarbonate resin (a1) is preferably 90 to 190°C, more preferably 100 to 170°C, and particularly preferably 110 to 150°C. In this specification, the glass transition point is a temperature calculated by the midpoint method using a differential scanning calorimeter, measuring 10 mg of a sample at a heating rate of 10°C / min.
[0039] The substrate layer may contain other resins in addition to the polycarbonate resin (a1). Examples of such resins include polyester resins. The polyester resin preferably contains terephthalic acid as a dicarboxylic acid component, and may contain a dicarboxylic acid component other than terephthalic acid. For example, a polyester resin (so-called "PETG") obtained by polycondensation of glycol components containing 80 to 60 mol % of ethylene glycol as the main component and 20 to 40 mol % of 1,4-cyclohexanedimethanol (total 100 mol %) is preferred. The resin in the base layer is preferably only the polycarbonate resin (a1), but when other resins are contained, the amount thereof is preferably 0 to 25 mass % and more preferably 0 to 10 mass % based on the total mass of the base layer.
[0040] The substrate layer may further contain additives. As the additives, those usually used in resin sheets can be used, and examples of such additives include antioxidants, anti-coloring agents, anti-static agents, release agents, lubricants, dyes, pigments, plasticizers, flame retardants, resin modifiers, compatibilizers, and reinforcing materials such as organic fillers and inorganic fillers. The method of mixing the additives and the resin is not particularly limited, and a method of compounding the entire amount, a method of dry blending a master batch, a method of dry blending the entire amount, and the like can be used. The amount of the additive is preferably 0 to 10% by mass, more preferably 0 to 7% by mass, and particularly preferably 0 to 5% by mass, based on the total mass of the substrate layer.
[0041] The thickness of the substrate layer is preferably from 0.3 to 10 mm, more preferably from 0.3 to 5 mm, and particularly preferably from 0.3 to 3.5 mm.
[0042] 2.High hardness resin layer The high-hardness resin layer is a resin layer mainly containing a high-hardness resin. In this specification, the high-hardness resin means a resin having a higher hardness than the polycarbonate resin serving as the base material, and a pencil hardness of HB or more. The pencil hardness of the high-hardness resin is preferably HB to 3H, more preferably H to 3H, and particularly preferably 2H to 3H. The high-hardness resin layer may contain one type or two or more types of high-hardness resin. Those skilled in the art can appropriately select and use a high-hardness resin having a Tg that satisfies the relationship "-10°C ≦ (glass transition point of the high-hardness resin) - (glass transition point of the polycarbonate resin (a1)) ≦ 40°C" from among known high-hardness resins, taking into consideration the glass transition point (Tg) of the polycarbonate resin used. The high-hardness resin is preferably selected from at least one of the resins (B1) to (B6) shown below.
[0043] <Resin (B1)> Resin (B1) is a copolymer containing a (meth)acrylic acid ester structural unit (a) represented by the following general formula (1) and an aliphatic vinyl structural unit (b) represented by the following general formula (2), or an alloy of the copolymer with resin (B2) described below.
[0044] [ka] (In the formula, R1 is a hydrogen atom or a methyl group; R2 is an alkyl group having 1 to 18 carbon atoms.) [ka] (In the formula, R3 is a hydrogen atom or a methyl group; R4 is a cyclohexyl group which may be substituted with a hydrocarbon group having 1 to 4 carbon atoms.) In the present specification, the "hydrocarbon group" may be linear, branched, or cyclic, and may have a substituent.
[0045] In the (meth)acrylic acid ester structural unit (a) represented by general formula (1), R2 is an alkyl group having 1 to 18 carbon atoms, preferably an alkyl group having 1 to 10 carbon atoms, and more preferably an alkyl group having 1 to 6 carbon atoms. Specific examples include a methyl group, an ethyl group, a butyl group, a lauryl group, a stearyl group, a cyclohexyl group, and an isobornyl group. Of the (meth)acrylic acid ester structural units (a), preferred are (meth)acrylic acid ester structural units in which R2 is a methyl group or an ethyl group, and more preferred are methyl methacrylate structural units in which R1 is a methyl group and R2 is a methyl group.
[0046] In the aliphatic vinyl structural unit (b) represented by general formula (2), R3 is a hydrogen atom or a methyl group, and more preferably a hydrogen atom. R4 is a cyclohexyl group or a cyclohexyl group substituted with a hydrocarbon group having 1 to 4 carbon atoms, and preferably an unsubstituted cyclohexyl group. Therefore, among the aliphatic vinyl structural units (b), more preferred are those in which R3 is a hydrogen atom and R4 is a cyclohexyl group.
[0047] The resin (B1) may contain one or more types of (meth)acrylic acid ester structural units (a), and may contain one or more types of aliphatic vinyl structural units (b). The total content of the (meth)acrylic acid ester structural units (a) and the aliphatic vinyl structural units (b) is preferably 90 to 100 mol %, more preferably 95 to 100 mol %, and particularly preferably 98 to 100 mol %, based on all structural units of the resin (B1).
[0048] That is, the resin (B1) may contain structural units other than the (meth)acrylic acid ester structural unit (a) and the aliphatic vinyl structural unit (b). The amount of such units is preferably 10 mol % or less, more preferably 5 mol % or less, and particularly preferably 2 mol % or less, based on the total structural units of the resin (B1).
[0049] Examples of structural units other than the (meth)acrylic acid ester structural unit (a) and the aliphatic vinyl structural unit (b) include structural units derived from aromatic vinyl monomers containing an unhydrogenated aromatic double bond, which are generated in the process of producing resin (B1) by polymerizing a (meth)acrylic acid ester monomer and an aromatic vinyl monomer and then hydrogenating the aromatic double bond derived from the aromatic vinyl monomer.
[0050] The content of the (meth)acrylic acid ester structural unit (a) represented by the general formula (1) is preferably 65 to 80 mol %, more preferably 70 to 80 mol %, based on all structural units in the resin (B1). When the ratio of the (meth)acrylic acid ester structural unit (a) to all structural units in the resin (B1) is 65 mol % or more, a resin layer having excellent adhesion to the substrate layer and excellent surface hardness can be obtained. When the ratio is 80 mol % or less, warping due to water absorption of the resin sheet is unlikely to occur.
[0051] The content of the aliphatic vinyl structural unit (b) represented by general formula (2) is preferably 20 to 35 mol %, more preferably 20 to 30 mol %, based on the total structural units in the resin (B1). If the content of the aliphatic vinyl structural unit (b) is 20 mol % or more, warping under high temperature and high humidity conditions can be prevented, and if it is 35 mol % or less, peeling at the interface with the base layer can be prevented. In this specification, the "copolymer" may have any of a random, block and alternating copolymer structure.
[0052] The method for producing the resin (B1) is not particularly limited, but it is preferable to use a resin obtained by polymerizing at least one (meth)acrylic acid ester monomer and at least one aromatic vinyl monomer, and then hydrogenating the aromatic double bond derived from the aromatic vinyl monomer. Here, (meth)acrylic acid refers to methacrylic acid and / or acrylic acid. Specific examples of the aromatic vinyl monomer that can be used in this case include styrene, α-methylstyrene, p-hydroxystyrene, alkoxystyrene, chlorostyrene, and derivatives thereof, etc. Among these, styrene is preferred.
[0053] For the polymerization of the (meth)acrylic acid ester monomer and the aromatic vinyl monomer, a known method can be used, for example, a bulk polymerization method or a solution polymerization method can be used for production. The bulk polymerization method is carried out by continuously supplying a monomer composition containing the above-mentioned monomers and a polymerization initiator to a complete mixing tank and continuously polymerizing the monomers at 100 to 180° C. The above-mentioned monomer composition may contain a chain transfer agent as necessary.
[0054] The polymerization initiator is not particularly limited, but includes organic peroxides such as t-amylperoxy-2-ethylhexanoate, t-butylperoxy-2-ethylhexanoate, benzoyl peroxide, 1,1-di(t-hexylperoxy)-3,3,5-trimethylcyclohexane, 1,1-di(t-hexylperoxy)cyclohexane, 1,1-di(t-butylperoxy)cyclohexane, t-hexylpropoxyisopropyl monocarbonate, t-amylperoxy normal octoate, t-butylperoxyisopropyl monocarbonate, and di-t-butyl peroxide, and azo compounds such as 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), and 2,2'-azobis(2,4-dimethylvaleronitrile). These can be used alone or in combination of two or more. A chain transfer agent is used as necessary, and an example of such an agent is α-methylstyrene dimer.
[0055] Examples of solvents used in the solution polymerization method include hydrocarbon solvents such as toluene, xylene, cyclohexane, and methylcyclohexane; ester solvents such as ethyl acetate and methyl isobutyrate; ketone solvents such as acetone and methyl ethyl ketone; ether solvents such as tetrahydrofuran and dioxane; and alcohol solvents such as methanol and isopropanol.
[0056] The solvent used in the hydrogenation reaction after polymerization of the (meth)acrylic acid ester monomer and the aromatic vinyl monomer may be the same as or different from the above-mentioned polymerization solvent, and examples thereof include hydrocarbon solvents such as cyclohexane and methylcyclohexane, ester solvents such as ethyl acetate and methyl isobutyrate, ketone solvents such as acetone and methyl ethyl ketone, ether solvents such as tetrahydrofuran and dioxane, and alcohol solvents such as methanol and isopropanol.
[0057] After the (meth)acrylic acid ester monomer and the aromatic vinyl monomer are polymerized as described above, the aromatic double bond derived from the aromatic vinyl monomer is hydrogenated to obtain the resin (B1) used in the present invention. The hydrogenation method is not particularly limited, and known methods can be used. For example, the hydrogenation can be carried out in a batch or continuous flow manner at a hydrogen pressure of 3 to 30 MPa and a reaction temperature of 60 to 250°C. By setting the temperature at 60°C or higher, the reaction time does not take too long, and by setting the temperature at 250°C or lower, cleavage of molecular chains and hydrogenation of ester moieties are unlikely to occur.
[0058] Examples of catalysts used in the hydrogenation reaction include solid catalysts in which metals such as nickel, palladium, platinum, cobalt, ruthenium, and rhodium, or oxides, salts, or complex compounds of these metals are supported on porous supports such as carbon, alumina, silica, silica-alumina, and diatomaceous earth.
[0059] In the resin (B1), 70% or more of the aromatic double bonds derived from the aromatic vinyl monomer are preferably hydrogenated. That is, the unhydrogenated ratio of the aromatic double bonds contained in the structural unit derived from the aromatic vinyl monomer is preferably less than 30%. When the unhydrogenated ratio is less than 30%, a resin having excellent transparency can be obtained. The unhydrogenated ratio is more preferably less than 10%, and further preferably less than 5%.
[0060] The weight average molecular weight of the resin (B1) is not particularly limited, but from the viewpoints of strength and moldability, it is preferably from 50,000 to 400,000, and more preferably from 70,000 to 300,000.
[0061] The glass transition point of the resin (B1) is preferably in the range of 110 to 140° C., more preferably 110 to 135° C., and particularly preferably 110 to 130° C. When the glass transition point is 110° C. or higher, the resin sheet provided by the present invention is less likely to deform or crack in a heat environment or a humid heat environment. On the other hand, when the glass transition point is 140° C. or lower, the resin sheet has excellent processability when molded by continuous thermal shaping using a mirror roll or a shaping roll, or batch-type thermal shaping using a mirror mold or a shaping mold.
[0062] Specific examples of the resin (B1) include Optimus 7500 and 6000 (manufactured by Mitsubishi Gas Chemical Company).
[0063] When resin (B1) is used as the high hardness resin, it is preferable to use Iupizeta T-1380 (manufactured by Mitsubishi Gas Chemical) as polycarbonate resin (a1). It is particularly preferable to use a copolymer containing 75 mol% of structural units represented by general formula (1) (R1 and R2 are both methyl groups; methyl methacrylate) and 25 mol% of structural units represented by general formula (2) (R3 is a hydrogen atom, R4 is a cyclohexyl group) as resin (B1), a polycarbonate resin containing structural units represented by general formula (4a) as polycarbonate resin (a1), and a monohydric phenol represented by general formula (5) (R1 has 8 to 22 carbon atoms) as a terminal terminator.
[0064] <Resin (B2)> Resin (B2) is a copolymer (D) containing 6 to 77% by mass of (meth)acrylic acid ester structural units, 15 to 71% by mass of styrene structural units, and 8 to 23% by mass of unsaturated dicarboxylic acid structural units, or a resin that is an alloy of copolymers (D) themselves, or a resin that is an alloy of copolymer (D) and a high-hardness resin other than resin (B2), or a resin that is an alloy of copolymer (D) and an acrylic resin. Examples of high-hardness resins other than resin (B2) include methyl methacrylate-styrene copolymers and acrylonitrile-butadiene-styrene copolymers. Examples of acrylic resins include polymethyl methacrylate, copolymers of methyl methacrylate and methyl acrylate or ethyl acrylate, and the like. Commercially available products can also be used, and specific examples include Acrypet from Mitsubishi Chemical Corporation, Sumipex from Sumitomo Chemical Co., Ltd., Parapet from Kuraray Co., Ltd., and Altoglass from Arkema. In the case of alloying, it is preferable to use alloys of resins with higher Tg in order to avoid a decrease in the Tg of the high hardness resin.
[0065] Examples of (meth)acrylic acid ester monomers constituting the (meth)acrylic acid ester structural unit include acrylic acid, methyl acrylate, ethyl acrylate, n-butyl acrylate, 2-ethylhexyl acrylate, methacrylic acid, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, 2-ethylhexyl methacrylate, etc., with methyl methacrylate being particularly preferred. Two or more of these (meth)acrylic acid ester monomers may be mixed and used. The content of the (meth)acrylic acid ester structural unit is from 6 to 77% by mass, and preferably from 20 to 70% by mass, based on the total mass of the resin (B2).
[0066] The styrene structural unit is not particularly limited, and any known styrene monomer can be used. From the viewpoint of easy availability, styrene, α-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, t-butylstyrene, etc. are preferred. Among these, styrene is particularly preferred from the viewpoint of compatibility. Two or more of these styrene monomers may be mixed and used. The content of the styrene structural unit is from 15 to 71 mass %, and preferably from 20 to 66 mass %, based on the total mass of the resin (B2).
[0067] Examples of the unsaturated dicarboxylic acid anhydride monomer constituting the unsaturated dicarboxylic acid structural unit include acid anhydrides such as maleic acid, itaconic acid, citraconic acid, aconitic acid, etc., and maleic anhydride is preferred from the viewpoint of compatibility with styrene-based monomers. Two or more of these unsaturated dicarboxylic acid anhydride monomers may be mixed and used. The content of the unsaturated dicarboxylic acid constituent units is from 8 to 23 mass %, and preferably from 10 to 23 mass %, based on the total mass of the resin (B2).
[0068] The total content of the (meth)acrylic acid ester structural units, styrene structural units and unsaturated dicarboxylic acid structural units is preferably 90 to 100 mol %, more preferably 95 to 100 mol %, and particularly preferably 98 to 100 mol %, based on all structural units of the resin (B2). That is, the resin (B2) may contain structural units other than the (meth)acrylic acid ester structural units, the styrene structural units and the unsaturated dicarboxylic acid structural units. The amount of such units is preferably 10 mol % or less, more preferably 5 mol % or less, and particularly preferably 2 mol % or less, based on the total structural units of the resin (B2).
[0069] Examples of other constituent units include N-phenylmaleimide. The method for producing the resin (B2) is not particularly limited, but examples thereof include bulk polymerization and solution polymerization.
[0070] Specific examples of the resin (B2) include Resisfy R100, R200, and R310 (manufactured by Denka), Delpet 980N (manufactured by Asahi Kasei Chemical), and hw55 (manufactured by Daicel Evonik).
[0071] The weight average molecular weight of the resin (B2) is not particularly limited, but is preferably from 50,000 to 300,000, and more preferably from 80,000 to 200,000.
[0072] The glass transition point of the resin (B2) is preferably from 90 to 150°C, more preferably from 100 to 150°C, and particularly preferably from 115 to 150°C.
[0073] When resin (B2) is used as the high hardness resin, a preferred embodiment is one in which a polycarbonate resin containing a structural unit of general formula (4a) is used as polycarbonate resin (a1). Furthermore, a particularly preferred embodiment is one in which a monohydric phenol represented by general formula (5) (R1 has 8 to 22 carbon atoms) is used as an end terminator. Examples of such polycarbonate resins include Iupizeta T-1380 (manufactured by Mitsubishi Gas Chemical Co., Ltd.) and Iupilon E-2000 (manufactured by Mitsubishi Engineering Plastics Co., Ltd.). A preferred embodiment is one in which a copolymer (R100, R200, or R310; manufactured by Denka Co., Ltd.) consisting of 6 to 26% by mass of methyl methacrylate structural units, 55 to 21% by mass of styrene structural units, and 15 to 23% by mass of maleic anhydride structural units is used as resin (B2), and Iupizeta T-1380 is used as polycarbonate resin (a1). In addition, a particularly preferred embodiment is one in which a copolymer (R310; manufactured by Denka) consisting of 6 mass% methyl methacrylate structural units, 71 mass% styrene structural units, and 23 mass% maleic anhydride structural units is used as the resin (B2), and Iupizeta T-1380 is used as the polycarbonate resin (a1).
[0074] <Resin (B3)> Resin (B3) is a copolymer containing a structural unit (c) represented by the following general formula (6) and, optionally, a structural unit (d) represented by the following general formula (7). Resin (B3) may or may not contain structural unit (d), but preferably contains it. [ka] [ka]
[0075] The proportion of the structural unit (c) in all structural units of the resin (B3) is preferably 50 to 100 mol%, more preferably 60 to 100 mol%, and particularly preferably 70 to 100 mol%. The proportion of the structural unit (d) in all structural units of the resin (B3) is preferably 0 to 50 mol%, more preferably 0 to 40 mol%, and particularly preferably 0 to 30 mol%.
[0076] The total content of the structural units (c) and (d) relative to the resin (B3) is preferably 90 to 100 mol %, more preferably 95 to 100 mol %, and particularly preferably 98 to 100 mol %.
[0077] Resin (B3) may contain structural units other than structural units (c) and (d). When other structural units are contained, the amount thereof is preferably 10 mol % or less, more preferably 5 mol % or less, and particularly preferably 2 mol % or less, based on the total structural units of resin (B3). Examples of other structural units include a structural unit represented by the following general formula (4a). [ka]
[0078] The method for producing resin (B3) is not particularly limited, but it can be produced by the same method as the method for producing polycarbonate resin (a1) described above, except that bisphenol C is used as the monomer.
[0079] Specific examples of the resin (B3) include Iupilon KH3410UR, KH3520UR, and KS3410UR (manufactured by Mitsubishi Engineering Plastics Corporation).
[0080] The weight average molecular weight of the resin (B3) is preferably from 15,000 to 75,000, more preferably from 20,000 to 70,000, and particularly preferably from 25,000 to 65,000.
[0081] The glass transition point of the resin (B3) is preferably from 105 to 150°C, more preferably from 110 to 140°C, and particularly preferably from 110 to 135°C.
[0082] When resin (B3) is used as the high hardness resin, a preferred embodiment is one in which a polycarbonate resin containing a structural unit of general formula (4a) is used as polycarbonate resin (a1). Furthermore, a particularly preferred embodiment is one in which a monohydric phenol (R1 has 8 to 22 carbon atoms) represented by general formula (5) is used as an end terminator. An example of such a polycarbonate resin is Iupizeta T-1380 (manufactured by Mitsubishi Gas Chemical). In particular, it is preferred to use Iupilon KS3410UR (manufactured by Mitsubishi Engineering Plastics) as resin (B3) and Iupizeta T-1380 (manufactured by Mitsubishi Gas Chemical) as polycarbonate resin (a1).
[0083] When resin (B3) is used as the high-hardness resin, the other resin contained in the high-hardness resin layer is preferably a resin that does not contain the structural unit (c) and contains the structural unit (d), and more preferably a resin that consists only of the structural unit (d). Specifically, aromatic polycarbonate resins (e.g., Iupilon S-2000, Iupilon S-1000, Iupilon E-2000; manufactured by Mitsubishi Engineering Plastics Corporation) and the like can be used. When other resins are contained, resin (B3) is preferably contained in a proportion of 45% by mass or more, more preferably 55% by mass or more, based on the total resins contained in the high-hardness resin layer.
[0084] <Resin (B4)> Resin (B4) is a copolymer (G) containing 5 to 20% by mass of styrene structural units, 60 to 90% by mass of (meth)acrylic acid ester structural units, and 5 to 20% by mass of N-substituted maleimide structural units, or an alloy of copolymer (G) and resin (B2). In the case of an alloy, an alloy of resins with higher Tg is preferable to avoid a decrease in the Tg of the high hardness resin layer.
[0085] The styrene structural unit is not particularly limited, and any known styrene-based monomer can be used, but from the viewpoint of easy availability, styrene, α-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, t-butylstyrene, etc. are preferred. Among these, styrene is particularly preferred from the viewpoint of compatibility. The copolymer (G) may contain two or more of these styrene structural units. The content of the styrene structural unit is 5 to 20 mass%, preferably 5 to 15 mass%, and more preferably 5 to 10 mass% based on the total mass of the resin (B4).
[0086] Examples of the (meth)acrylic acid ester structural unit include structural units derived from acrylic acid, methyl acrylate, ethyl acrylate, n-butyl acrylate, 2-ethylhexyl acrylate, methacrylic acid, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, 2-ethylhexyl methacrylate, etc., and structural units derived from methyl methacrylate are particularly preferred. The copolymer (G) may contain two or more of these (meth)acrylic acid ester structural units. The content of the (meth)acrylic acid ester structural unit is 60 to 90% by mass, preferably 70 to 90% by mass, and more preferably 80 to 90% by mass, based on the total mass of the resin (B4).
[0087] Examples of the N-substituted maleimide structural unit in the resin (B4) include structural units derived from N-arylmaleimides such as N-phenylmaleimide, N-chlorophenylmaleimide, N-methylphenylmaleimide, N-naphthylmaleimide, N-hydroxyphenylmaleimide, N-methoxyphenylmaleimide, N-carboxyphenylmaleimide, N-nitrophenylmaleimide, and N-tribromophenylmaleimide, and from the viewpoint of compatibility with acrylic resins, structural units derived from N-phenylmaleimide are preferred. The copolymer (G) may contain two or more of these N-substituted maleimide structural units. The content of the N-substituted maleimide structural unit is 5 to 20% by mass, preferably 5 to 15% by mass, and more preferably 5 to 10% by mass, based on the total mass of the resin (B4).
[0088] The total content of the styrene structural units, the (meth)acrylic acid ester structural units, and the N-substituted maleimide structural units is preferably 90 to 100 mol %, more preferably 95 to 100 mol %, and particularly preferably 98 to 100 mol %, based on the resin (B4). Resin (B4) may contain other structural units than the above structural units. When other structural units are contained, the amount thereof is preferably 10 mol % or less, more preferably 5 mol % or less, and particularly preferably 2 mol % or less, based on the total structural units of resin (B4).
[0089] Examples of the other structural units include structural units derived from the following general formula (1) and structural units derived from the following general formula (2). [ka] (In the formula, R1 is a hydrogen atom or a methyl group; R2 is an alkyl group having 1 to 18 carbon atoms.) [ka] (In the formula, R3 is a hydrogen atom or a methyl group; R4 is a cyclohexyl group which may be substituted with a hydrocarbon group having 1 to 4 carbon atoms.)
[0090] The method for producing the resin (B4) is not particularly limited, but it can be produced by solution polymerization, bulk polymerization, or the like.
[0091] A specific example of the resin (B4) is Delpet PM120N (manufactured by Asahi Kasei Chemical Corporation).
[0092] The weight average molecular weight of the resin (B4) is preferably from 50,000 to 250,000, and more preferably from 100,000 to 200,000.
[0093] The glass transition point of the resin (B4) is preferably from 110 to 150°C, more preferably from 115 to 140°C, and particularly preferably from 115 to 135°C.
[0094] When resin (B4) is used as the high hardness resin, a preferred embodiment is one in which a polycarbonate resin containing a structural unit of general formula (4a) is used as polycarbonate resin (a1). Furthermore, a particularly preferred embodiment is one in which a monohydric phenol (R1 has 8 to 22 carbon atoms) represented by general formula (5) is used as an end terminator. An example of such a polycarbonate resin is Iupizeta T-1380 (manufactured by Mitsubishi Gas Chemical Co., Ltd.). In particular, it is preferred to use Delpet PM-120N, which is composed of 7% by mass of styrene structural units, 86% by mass of (meth)acrylic acid ester structural units, and 7% by mass of N-substituted maleimide structural units, as resin (B4), and Iupizeta T-1380 as polycarbonate resin (a1).
[0095] <Resin (B5)> The resin (B5) is a resin containing a structural unit (e) represented by the following general formula (8). [ka]
[0096] The proportion of the structural unit (e) in all structural units of the resin (B5) is preferably from 80 to 100 mol %, more preferably from 90 to 100 mol %, and particularly preferably from 95 to 100 mol %. Resin (B5) may contain a structural unit other than structural unit (e), but is preferably a polycarbonate resin consisting of structural unit (e). When other structural units are contained, the amount thereof is preferably 20 mol % or less, more preferably 10 mol % or less, and particularly preferably 5 mol % or less, based on the total structural units of resin (B5).
[0097] Examples of other structural units include a structural unit represented by the following general formula (6) and a structural unit represented by the following general formula (7). [ka] [ka]
[0098] The method for producing resin (B5) is not particularly limited, but it can be produced by the same method as the method for producing polycarbonate resin (a1) described above, except that bisphenol AP is used as the monomer. A specific example of the resin (B5) is Iupizeta FPC0220 (manufactured by Mitsubishi Gas Chemical Company, Inc.).
[0099] The weight average molecular weight of the resin (B5) is preferably from 10,000 to 1,000,000, and more preferably from 15,000 to 50,000.
[0100] The glass transition point of the resin (B5) is preferably from 120 to 200°C, more preferably from 130 to 190°C, and particularly preferably from 140 to 190°C.
[0101] When resin (B5) is used as the high hardness resin, it is preferable to use a polycarbonate resin containing a structural unit of general formula (4a) as polycarbonate resin (a1). An example of such a polycarbonate resin is Iupilon E-2000 (manufactured by Mitsubishi Engineering Plastics). In particular, it is preferable to use Iupizeta FPC0220 (manufactured by Mitsubishi Gas Chemical) as resin (B5) and Iupilon E-2000 (manufactured by Mitsubishi Engineering Plastics) as polycarbonate resin (a1).
[0102] When resin (B5) is used as the high-hardness resin, the other resin contained in the high-hardness resin layer is preferably a resin that does not contain the structural unit (e) and contains the structural unit (d) described in resin (B3), and more preferably a resin that consists only of the structural unit (d). Specifically, aromatic polycarbonate resins (e.g., Iupilon S-2000, Iupilon S-1000, Iupilon E-2000; manufactured by Mitsubishi Engineering Plastics Corporation) and the like can be used. When other resins are contained, resin (B5) is preferably contained in a proportion of 45% by mass or more, more preferably 55% by mass or more, based on the total resins contained in the high-hardness resin layer.
[0103] <Resin (B6)> Resin (B6) is a copolymer (H) containing 50 to 95% by mass of styrene structural units and 5 to 50% by mass of unsaturated dicarboxylic acid structural units, or an alloy of copolymer (H) and the above resin (B1), or an alloy of copolymer (H) and an acrylic resin. In the case of an alloy, an alloy of resins with higher Tg is preferable to avoid a decrease in the Tg of the high hardness resin layer.
[0104] As the styrene structural unit, the styrene monomer described in the resin (B4) can be used. The copolymer (H) may contain two or more of these styrene structural units. The content of the styrene structural unit is 50 to 95 mass % relative to the total mass of the copolymer (H), preferably 60 to 90 mass %, and more preferably 65 to 87 mass %.
[0105] Examples of the unsaturated dicarboxylic acid anhydride monomer constituting the unsaturated dicarboxylic acid structural unit include acid anhydrides such as maleic acid, itaconic acid, citraconic acid, aconitic acid, etc., and maleic anhydride is preferred from the viewpoint of compatibility with styrene-based monomers. Two or more of these unsaturated dicarboxylic acid anhydride monomers may be mixed and used. The content of the unsaturated dicarboxylic acid constituent units is from 5 to 50% by mass, preferably from 10 to 40% by mass, and more preferably from 13 to 35% by mass, based on the total mass of the copolymer (H).
[0106] The copolymer (H) may contain other structural units than the above structural units. When other structural units are contained, the amount of such units is preferably 10 mol % or less, more preferably 5 mol % or less, and particularly preferably 2 mol % or less, based on the total structural units of the resin (H).
[0107] Examples of the other structural units include structural units derived from the following general formula (1) and structural units derived from the following general formula (2). [ka] (In the formula, R1 is a hydrogen atom or a methyl group; R2 is an alkyl group having 1 to 18 carbon atoms.) [ka] (In the formula, R3 is a hydrogen atom or a methyl group; R4 is a cyclohexyl group which may be substituted with a hydrocarbon group having 1 to 4 carbon atoms.)
[0108] The method for producing the copolymer (H) is not particularly limited, but it can be produced by solution polymerization, bulk polymerization, or the like.
[0109] Specific examples of the copolymer (H) include XIBOND140 and XIBOND160 (manufactured by Polyscope Co., Ltd.).
[0110] The weight average molecular weight of the copolymer (H) is preferably from 50,000 to 250,000, and more preferably from 100,000 to 200,000.
[0111] The content of the copolymer (H) composed of styrene structural units and unsaturated dicarboxylic acid structural units in the resin (B6) is preferably 10 to 90 mass %, more preferably 20 to 85 mass %, and particularly preferably 30 to 80 mass %.
[0112] The glass transition point of the resin (B6) is preferably from 110 to 150°C, more preferably from 115 to 140°C, and particularly preferably from 115 to 137°C.
[0113] When resin (B6) is used as the high hardness resin, a preferred embodiment is one in which a polycarbonate resin containing a structural unit of general formula (4a) is used as polycarbonate resin (a1). Furthermore, a particularly preferred embodiment is one in which a monohydric phenol (R1 has 8 to 22 carbon atoms) represented by general formula (5) is used as an end terminator. An example of such a polycarbonate resin is Iupizeta T-1380 (manufactured by Mitsubishi Gas Chemical Co., Ltd.). In particular, it is preferred to use an alloy of XIBOND160, which is composed of 78% by mass of styrene structural units and 22% by mass of maleic anhydride structural units, and an acrylic resin as resin (B6), and to use Iupizeta T-1380 as polycarbonate resin (a1).
[0114] The high-hardness resin layer may contain one type or two or more types of high-hardness resins, and when two or more types are selected from the resins (B1) to (B6), they may be selected from the same or different categories, and may further contain a high-hardness resin other than the resins (B1) to (B6). The content of the high-hardness resin in the high-hardness resin layer is preferably 70 to 100% by mass, more preferably 80 to 100% by mass, and particularly preferably 100% by mass.
[0115] The high-hardness resin layer may contain other resins in addition to the high-hardness resins described above. Examples of such resins include methyl methacrylate-styrene copolymers, polymethyl methacrylate, polystyrene, polycarbonate, cycloolefin (co)polymer resins, acrylonitrile-styrene copolymers, acrylonitrile-butadiene-styrene copolymers, various elastomers, etc. The resin in the high-hardness resin layer is preferably only a high-hardness resin, but when other resins are contained, the amount of such resins is preferably 35% by mass or less, more preferably 25% by mass or less, and particularly preferably 10% by mass or less, relative to the high-hardness resin layer.
[0116] The high-hardness resin layer may further contain additives, etc. As the additives, the same additives as those described in "1. Base layer" above can be used, and the amounts thereof are also the same.
[0117] The thickness of the high-hardness resin layer affects the surface hardness and impact resistance of the molding resin sheet. That is, if the high-hardness resin layer is too thin, the surface hardness is low, and if it is too thick, the impact resistance is low. The thickness of the high-hardness resin layer is preferably 10 to 250 μm, more preferably 30 to 200 μm, and particularly preferably 60 to 150 μm.
[0118] 3.Lamination of the base material layer and the high-hardness resin layer As described above, there may be an additional layer between the substrate layer and the high-hardness resin layer, but here, the case where the high-hardness resin layer is laminated on the substrate layer will be described. The lamination method is not particularly limited, and the lamination can be performed in the same manner even when other layers are present. For example, there are various methods such as a method of overlapping a substrate layer and a high-hardness resin layer that are formed separately and heating and pressing them together; a method of overlapping a substrate layer and a high-hardness resin layer that are formed separately and bonding them together with an adhesive; a method of co-extrusion molding the substrate layer and the high-hardness resin layer; a method of in-mold molding the substrate layer into a high-hardness resin layer that has been formed in advance to integrate them. Among these, the co-extrusion molding method is preferable from the viewpoint of manufacturing cost and productivity.
[0119] The method of co-extrusion is not particularly limited. For example, in the feed block method, a high-hardness resin layer is arranged on one side of a base layer in a feed block, extruded into a sheet shape by a T-die, and then cooled while passing through a forming roll to form a desired laminate. In the multi-manifold method, a high-hardness resin layer is arranged on one side of a base layer in a multi-manifold die, extruded into a sheet shape, and then cooled while passing through a forming roll to form a desired laminate. At this time, the ratio of the rotation speed (m / min) of the forming roll and the sheet take-up roll is controlled, and the sheet is cooled while being stretched in a uniaxial direction. The stretching ratio is controlled to 1.0 to 1.5 times to control the in-plane retardation of the resin sheet. The in-plane retardation of the resin sheet of the present invention measured at a wavelength of 543 nm is 4000 nm or more, preferably 4500 to 10000 nm, and more preferably 5500 to 8000 nm. A resin sheet having an in-plane retardation of 4000 nm or more is preferable because, after the resin sheet is bonded to the front panel of a liquid crystal panel, coloring or color unevenness is unlikely to occur even when the liquid crystal display is viewed through polarized sunglasses.
[0120] The total thickness of the base layer and the high-hardness resin layer is preferably 0.5 to 3.5 mm, more preferably 0.5 to 3.0 mm, and particularly preferably 1.2 to 3.0 mm. By making the total thickness 0.5 mm or more, the rigidity of the sheet can be maintained. Furthermore, by making the total thickness 3.5 mm or less, it is possible to prevent the sensitivity of the touch sensor from being deteriorated when a touch panel is installed under the sheet. The ratio of the thickness of the base layer to the total thickness of the base layer and the high-hardness resin layer is preferably 75% to 99%, more preferably 80 to 99%, and particularly preferably 85 to 99%. By making it within the above range, both hardness and impact resistance can be achieved.
[0121] 4. Hard coat layer, hard coat anti-glare layer The resin sheet of the present invention has a hard coat layer or a hard coat anti-glare layer. An additional layer may be present between the hard coat layer or the hard coat anti-glare layer and the high hardness resin layer, but preferably, the hard coat layer or the hard coat anti-glare layer is laminated on the high hardness resin layer. The hard coat layer or the hard coat anti-glare layer is preferably made of an acrylic hard coat. In this specification, the term "acrylic hard coat" refers to a coating film formed by polymerizing a monomer, oligomer, or prepolymer containing a (meth)acryloyl group as a polymerization group to form a crosslinked structure. The composition of the acrylic hard coat preferably contains 2 to 98% by mass of a (meth)acrylic monomer, 2 to 98% by mass of a (meth)acrylic oligomer, and 0 to 15% by mass of a surface modifier, and further preferably contains 0.001 to 7 parts by mass of a photopolymerization initiator relative to 100 parts by mass of the total of the (meth)acrylic monomer, the (meth)acrylic oligomer, and the surface modifier.
[0122] The hard coat layer and the hard coat anti-glare layer more preferably contain 5 to 50 mass% of a (meth)acrylic monomer, 50 to 94 mass% of a (meth)acrylic oligomer, and 1 to 10 mass% of a surface modifier, and particularly preferably contain 20 to 40 mass% of a (meth)acrylic monomer, 60 to 78 mass% of a (meth)acrylic oligomer, and 2 to 5 mass% of a surface modifier. The amount of the photopolymerization initiator is more preferably 0.01 to 5 parts by mass, and particularly preferably 0.1 to 3 parts by mass, per 100 parts by mass of the total of the (meth)acrylic monomer, (meth)acrylic oligomer, and surface modifier.
[0123] (1) (Meth)acrylic monomers As the (meth)acrylic monomer, any monomer having a (meth)acryloyl group as a functional group in the molecule can be used, and it may be a monofunctional monomer, a difunctional monomer, or a trifunctional or higher functional monomer.
[0124] Examples of monofunctional monomers include (meth)acrylic acid and (meth)acrylic acid esters. Specific examples of difunctional and / or trifunctional or higher (meth)acrylic monomers include diethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, bisphenol A diglycidyl ether di(meth)acrylate, tetraethylene glycol di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,4-butanediol diacrylate, 1,3-butylene glycol di(meth)acrylate, dicyclopentaerythritol diacrylate, and the like. Examples of the alkyl acrylate include nyl di(meth)acrylate, polyethylene glycol diacrylate, 1,4-butanediol oligoacrylate, neopentyl glycol oligoacrylate, 1,6-hexanediol oligoacrylate, trimethylolpropane tri(meth)acrylate, trimethylolpropane ethoxy tri(meth)acrylate, trimethylolpropane propoxy tri(meth)acrylate, pentaerythritol tri(meth)acrylate, glyceryl propoxy tri(meth)acrylate, trimethylolpropane trimethacrylate, trimethylolpropane ethylene oxide adduct triacrylate, glycerin propylene oxide adduct triacrylate, and pentaerythritol tetraacrylate. The hard coat anti-glare layer may contain one or more types of (meth)acrylic monomers.
[0125] (2) (Meth)acrylic oligomer Examples of the (meth)acrylic oligomer include a bifunctional or higher polyfunctional urethane (meth)acrylate oligomer (hereinafter also referred to as a bifunctional urethane (meth)acrylate oligomer), a bifunctional or higher polyfunctional polyester (meth)acrylate oligomer (hereinafter also referred to as a bifunctional polyester (meth)acrylate oligomer), a bifunctional or higher polyfunctional epoxy (meth)acrylate oligomer (hereinafter also referred to as a bifunctional epoxy (meth)acrylate oligomer), etc. The hard coat anti-glare layer may contain one or more types of (meth)acrylic oligomers.
[0126] Examples of polyfunctional urethane (meth)acrylate oligomers include urethane reaction products between a (meth)acrylate monomer having at least one (meth)acryloyloxy group and a hydroxyl group in one molecule and a polyisocyanate; and urethane reaction products between an isocyanate compound obtained by reacting a polyol with a polyisocyanate and a (meth)acrylate monomer having at least one (meth)acryloyloxy group and a hydroxyl group in one molecule.
[0127] Examples of the (meth)acrylate monomer having at least one (meth)acryloyloxy group and one hydroxyl group in one molecule used in the urethanization reaction include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, glycerin di(meth)acrylate, trimethylolpropane di(meth)acrylate, pentaerythritol tri(meth)acrylate, and dipentaerythritol penta(meth)acrylate.
[0128] Examples of polyisocyanates used in the urethanization reaction include hexamethylene diisocyanate, lysine diisocyanate, isophorone diisocyanate, dicyclohexylmethane diisocyanate, tolylene diisocyanate, xylylene diisocyanate, diisocyanates obtained by hydrogenating aromatic isocyanates among these diisocyanates (e.g., diisocyanates such as hydrogenated tolylene diisocyanate and hydrogenated xylylene diisocyanate), di- or tri-polyisocyanates such as triphenylmethane triisocyanate and dimethylene triphenyl triisocyanate, and polyisocyanates obtained by polymerizing diisocyanates.
[0129] Polyols used in the urethanization reaction generally include aromatic, aliphatic and alicyclic polyols, as well as polyester polyols, polyether polyols, etc. Typical aliphatic and alicyclic polyols include 1,4-butanediol, 1,6-hexanediol, neopentyl glycol, ethylene glycol, propylene glycol, trimethylolethane, trimethylolpropane, dimethylolheptane, dimethylolpropionic acid, dimethylolbutyric acid, glycerin, hydrogenated bisphenol A, etc.
[0130] The polyester polyol may be one obtained by the dehydration condensation reaction of the above-mentioned polyols and polycarboxylic acid. Specific examples of the polycarboxylic acid include succinic acid, adipic acid, maleic acid, trimellitic acid, hexahydrophthalic acid, phthalic acid, isophthalic acid, and terephthalic acid. These polycarboxylic acids may be anhydrides. In addition to polyalkylene glycol, the polyether polyol may be one obtained by the reaction of the above-mentioned polyols or phenols with alkylene oxide.
[0131] Also, the multifunctional polyester (meth)acrylate oligomer is obtained by a dehydration condensation reaction using (meth)acrylic acid, a polycarboxylic acid, and a polyol. Examples of the polycarboxylic acid used in the dehydration condensation reaction include succinic acid, adipic acid, maleic acid, itaconic acid, trimellitic acid, pyromellitic acid, hexahydrophthalic acid, phthalic acid, isophthalic acid, and terephthalic acid. These polycarboxylic acids may be anhydrides. Examples of the polyol used in the dehydration condensation reaction include 1,4-butanediol, 1,6-hexanediol, diethylene glycol, triethylene glycol, propylene glycol, neopentyl glycol, dimethylolheptane, dimethylolpropionic acid, dimethylolbutyric acid, trimethylolpropane, ditrimethylolpropane, pentaerythritol, and dipentaerythritol.
[0132] Multifunctional epoxy (meth)acrylate oligomers are obtained by addition reaction of polyglycidyl ethers with (meth)acrylic acid. Examples of polyglycidyl ethers include ethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, tripropylene glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, and bisphenol A diglycidyl ether.
[0133] (3) Surface modifier The surface modifier used in the present invention is an agent that changes the surface performance of the hard coat anti-glare layer, such as a leveling agent, an antistatic agent, a surfactant, a water- and oil-repellent agent, inorganic particles, or organic particles. Examples of the leveling agent include polyether-modified polyalkylsiloxane, polyether-modified siloxane, polyester-modified hydroxyl-containing polyalkylsiloxane, polyether-modified polydimethylsiloxane having an alkyl group, modified polyether, and silicon-modified acrylic.
[0134] Examples of the antistatic agent include glycerin fatty acid ester monoglycerides, glycerin fatty acid ester organic acid monoglycerides, polyglycerin fatty acid esters, sorbitan fatty acid esters, cationic surfactants, and anionic surfactants. Examples of inorganic particles include silica particles, alumina particles, zirconia particles, silicon particles, silver particles, and glass particles. Examples of the organic particles include acrylic particles and silicon particles. Examples of surfactants and water- and oil-repellents include fluorine-containing surfactants and water- and oil-repellents such as oligomers containing a fluorine-containing group and a lipophilic group, and oligomers containing a fluorine-containing group, a hydrophilic group, a lipophilic group, and a UV-reactive group.
[0135] (4) Photopolymerization initiator The hard coat layer and the hard coat anti-glare layer may contain a photopolymerization initiator. In this specification, the photopolymerization initiator refers to a photoradical generator.
[0136] Examples of monofunctional photopolymerization initiators that can be used in the present invention include 4-(2-hydroxyethoxy)phenyl(2-hydroxy-2-propyl)ketone [Darocure 2959: manufactured by Merck]; α-hydroxy-α,α'-dimethylacetophenone [Darocure 1173: manufactured by Merck]; acetophenone-based initiators such as methoxyacetophenone, 2,2'-dimethoxy-2-phenylacetophenone [Irgacure 651], and 1-hydroxy-cyclohexyl phenyl ketone; benzoin ether-based initiators such as benzoin ethyl ether and benzoin isopropyl ether; and other halogenated ketones, acylphosphinoxides, and acylphosphonates.
[0137] (5) Method for forming hard coat layer and hard coat anti-glare layer The method for forming the hard coat layer and the hard coat anti-glare layer is not particularly limited. For example, the hard coat layer and the hard coat anti-glare layer can be formed by applying a hard coat liquid onto a layer (e.g., a high-hardness resin layer) located below the hard coat anti-glare layer, and then photopolymerizing the hard coat liquid.
[0138] The method of applying the hard coat liquid (polymerizable composition) is not particularly limited, and any known method can be used, such as spin coating, dipping, spraying, slide coating, bar coating, roll coating, gravure coating, meniscus coating, flexographic printing, screen printing, beat coating, and brushing.
[0139] Lamps used for light irradiation in photopolymerization are those having an emission distribution at a light wavelength of 420 nm or less, examples of which include low-pressure mercury lamps, medium-pressure mercury lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, chemical lamps, black light lamps, microwave-excited mercury lamps, metal halide lamps, etc. Among these, high-pressure mercury lamps and metal halide lamps are preferred because they efficiently emit light in the active wavelength region of the initiator and do not emit much short-wavelength light that reduces the viscoelastic properties of the resulting polymer due to crosslinking, or long-wavelength light that heats and evaporates the reaction composition.
[0140] The irradiation intensity of the lamp is a factor that determines the degree of polymerization of the resulting polymer, and is appropriately controlled for each performance of the target product. When a typical cleavage-type initiator having an acetophenone group is blended, the illuminance is 0.1 to 300 mW / cm 2 In particular, a metal halide lamp is used, and the illuminance is set to 10 to 40 mW / cm. 2 It is preferable to set the above.
[0141] Photopolymerization reaction is inhibited by oxygen in air or oxygen dissolved in the reactive composition. Therefore, it is desirable to carry out light irradiation using a method that can eliminate reaction inhibition by oxygen. One such method is a method in which the reactive composition is covered with a film made of polyethylene terephthalate or Teflon to prevent contact with oxygen, and light is irradiated to the reactive composition through the film. In addition, light may be irradiated to the composition through a light-transmitting window in an inert atmosphere in which oxygen is replaced with an inert gas such as nitrogen gas or carbon dioxide gas.
[0142] When light irradiation is performed under an inert atmosphere, a certain amount of inert gas is always introduced to keep the oxygen concentration of the atmosphere at a low level. The introduction of this inert gas generates an airflow on the surface of the reactive composition, causing monomer evaporation. In order to suppress the level of monomer evaporation, the airflow speed of the inert gas is preferably 1 m / sec or less, more preferably 0.1 m / sec or less, as a relative speed to the laminate coated with the hard coat liquid moving under the inert gas atmosphere. By setting the airflow speed within the above range, monomer evaporation due to airflow is substantially suppressed.
[0143] In order to improve the adhesion of the hard coat layer and the hard coat anti-glare layer, the coated surface may be pretreated. Examples of the pretreatment include known methods such as sandblasting, solvent treatment, corona discharge treatment, chromic acid treatment, flame treatment, hot air treatment, ozone treatment, ultraviolet treatment, and primer treatment using a resin composition.
[0144] The hard coat layer and hard coat anti-glare layer have an irradiation output of 20 mW / cm of UV light (254 nm). 2 When irradiated with ultraviolet light using a metal halide lamp, it is preferable that the pencil hardness is 2H or more.
[0145] The thickness of the hard coat layer and the hard coat anti-glare layer is preferably 1 μm or more and 40 μm or less, more preferably 2 μm or more and 10 μm or less. A thickness of 1 μm or more can provide sufficient hardness. A thickness of 40 μm or less can suppress the occurrence of cracks during bending. The thickness of the hard coat anti-glare layer can be measured by observing the cross section with a microscope or the like and measuring from the coating interface to the surface.
[0146] The hard coat layer and hard coat anti-glare layer can be produced by applying an acrylic hard coat between the mirror type or anti-glare type and the high hardness resin, curing it with UV light, and then removing it from the mirror type or anti-glare type. When the mirror type is used, the resin sheet will have a mirror hard coat layer, and when the anti-glare type is used, the resin sheet will have a hard coat anti-glare layer. The material for the mirror type and anti-glare type can be anything that transmits UV light, and examples of materials include glass and transparent resin.
[0147] The hard coat layer and the hard coat anti-glare layer may be further modified. For example, one or more of anti-reflection treatment, antifouling treatment, antistatic treatment, weather resistance treatment, and anti-glare treatment may be applied. The method of these treatments is not particularly limited, and known methods can be used. For example, a method of applying a reflection reducing paint, a method of depositing a dielectric thin film, a method of applying an antistatic paint, etc. may be mentioned.
[0148] The pencil hardness of the resin sheet of the present invention is preferably 2H or more, for example, 2H to 4H, and particularly preferably 3H to 4H. The pencil hardness of the resin sheet referred to here means the hardness of the hardest pencil that does not leave a scratch when a pencil of gradually increasing hardness is pressed against the surface of the hard coat anti-glare layer at an angle of 45 degrees and a load of 750 g (pencil scratch hardness test according to JIS K 5600-5-4).
[0149] 5. Resin film (X) The present invention is a molding resin sheet in which a resin film (X) having an in-plane retardation of 50 nm or less when measured at a wavelength of 543 nm is laminated to one surface of the resin sheet by an adhesive layer containing an adhesive. The resin film (X) having an in-plane retardation of 45 nm or less, more preferably an in-plane retardation of 3 to 45 nm is laminated. By laminating a resin film (X) having an in-plane retardation of 50 nm or less, even if the combination of the slow axes of the resin film (X) and the resin sheet or the combination of the slow axis and the fast axis of the resin film (X) are misaligned during molding during thermoforming after lamination with the resin sheet, coloring or color unevenness is unlikely to occur even when the liquid crystal display is viewed through polarized sunglasses after the molding resin sheet is laminated as a front panel of a liquid crystal panel, which is preferable. A preferred embodiment of the present invention is that the resin film (X) is laminated on the substrate layer side containing the polycarbonate resin (a1). In another preferred embodiment of the present invention, the resin film (X) is made of a polycarbonate film containing the polycarbonate resin (a1). In yet another preferred embodiment of the present invention, the resin film (X) is made of a film touch sensor in which a sensor electrode is applied to a substrate film. As the substrate film, COP (cycloolefin polymer), COC (cycloolefin copolymer), acrylic resin, polycarbonate resin, PET resin, etc. can be used, and polycarbonate resin can be preferably used. As the sensor electrode, a resistive film type sensor and a capacitive type sensor in which a transparent electrode made of ITO or the like is arranged can be mentioned.
[0150] 6. Glue The adhesive may be any transparent optical adhesive, and it is preferable to use, as the adhesive layer, optically clear adhesive sheets (OCA: Optically Clear Adhesive) (Opteria series) from Lintec Corporation, optically clear adhesive sheets LUCIACS series from Nitto Denko Corporation, highly transparent double-sided tape from Sekisui Chemical Co., Ltd., and display optical adhesive silicone from Asahi Kasei Corporation.
[0151] The haze of the resin sheet of the present invention is preferably 2 to 30%, and more preferably 4 to 25%. The haze is a value measured in accordance with JIS K 7136 using HR-100 model manufactured by Murakami Color Research Laboratory.
[0152] According to one embodiment of the present invention, a resin molded product is provided by using the above-mentioned molding resin sheet. The molding method is not particularly limited, but thermoforming is suitable due to the characteristics of the resin sheet of the present invention. Thermoforming can be performed by a method commonly used in the field, such as heat press molding, pressure molding, vacuum molding, and TOM molding. The molding temperature is preferably 100°C to 200°C. EXAMPLES
[0153] Examples of the present invention will be described below, but the present invention is not limited to the embodiments of the examples. <Measurement of glass transition point (Tg) and melting point> Using a Hitachi High-Tech Science DSC7020 differential scanning calorimeter, the glass transition points of the polycarbonate resin and high hardness resin used in the examples and comparative examples and the melting points of the protective films were measured at a heating rate of 10°C / min under a nitrogen atmosphere. The weight of the resin used in the measurement was 10 to 20 mg.
[0154] <Measurement of pencil hardness of resin sheet> The resin sheets produced in the examples and comparative examples were evaluated by a pencil scratch hardness test according to JIS K 5600-5-4. Pencils of gradually increasing hardness were pressed against the surface of the hard coat anti-glare layer at an angle of 45 degrees and a load of 750 g, and the hardness of the hardest pencil that did not leave a scratch was evaluated as the pencil hardness. A hardness of 2H or more was considered to be acceptable.
[0155] <Production of molded products with bent shapes and evaluation of hard coat cracks after molding> The resin sheets produced in the examples and comparative examples were thermoformed. For examples 1 to 3, 5 to 15 and comparative examples 1 to 6, 8 to 11, a heat press mold with a clearance (the gap between the upper and lower parts of the mold to sandwich the molded sheet) of 2 mm and a molding R of 50 mm was used, and for example 4 and comparative example 7, a heat press mold with a clearance of 3.5 mm and a molding R of 100 mm was used. The pressure applied to the heat press mold was 0.6 MPa. The mold material was aluminum. The mold temperature during thermoforming was 124°C for examples 1 to 5, 7 to 11, 13 to 15 and comparative examples 1 to 4, 9, and 10, and 143°C for examples 6, 12, and comparative examples 5 to 8 and 11.
[0156] The obtained molded products were checked for the presence or absence of cracks in the 50 mmR or 100 mmR parts. When using a heat press mold with a clearance of 2 mm to mold resin sheets with a base layer and high hardness resin layer having a total thickness of 0.5 mm, 1.2 mm, or 1.5 mm, single-layer polycarbonate sheets of 1.5 mm, 0.8 mm, and 0.5 mm, respectively, were placed underneath to achieve a total thickness of 2 mm, and heat press molding was performed.
[0157] <Flow mark> The laminates of the high-hardness resin layer and the polycarbonate resin layer before hard coating produced in the examples and comparative examples were visually inspected under a three-wavelength fluorescent lamp to check for the presence or absence of scaly patterns and cloudiness. When neither scaly patterns nor cloudiness were observed, it was evaluated as "no flow marks", and when either scaly patterns or cloudiness were observed, it was evaluated as "present flow marks".
[0158] <Measurement of in-plane retardation> The retardation of the resin sheet or film was measured using a Photonic Lattice birefringence evaluation device WPA-200-L. The measurement wavelength was 543 nm. Since the retardation range over 3500 nm cannot be measured using the standard lens provided, the high phase difference measurement lens K4 FUJINON1:1.4 / 16mm HF16HA-1B was used.
[0159] <Measurement of haze of resin sheet> The evaluation was carried out in accordance with JIS K 7136 using the HR-100 model manufactured by Murakami Color Research Laboratory.
[0160] Example 1: R100 (Tg 124°C) / Low Tg PC (Tg 125°C) / 1.2 mmt A laminate consisting of a base material layer and a high-hardness resin layer was formed using a multi-layer extrusion device having a single-screw extruder with a shaft diameter of 35 mm, a single-screw extruder with a shaft diameter of 65 mm, a feed block connected to each extruder, and a T-die connected to the feed block. Specifically, a high-hardness resin (B2) (a copolymer of 21% by mass of methyl methacrylate structural units, 64% by mass of styrene structural units, and 15% by mass of maleic anhydride structural units; Resify R100 (manufactured by Denka)) was continuously introduced into a single-screw extruder with a shaft diameter of 35 mm, and extruded under conditions of a cylinder temperature of 230°C and an extrusion rate of 2.6 kg / h. In addition, a polycarbonate resin (Iupizeta T-1380; manufactured by Mitsubishi Gas Chemical) was continuously introduced into a single-screw extruder with a shaft diameter of 65 mm, and extruded under conditions of a cylinder temperature of 240°C and an extrusion rate of 50.0 kg / h.
[0161] The extruded high-hardness resin and polycarbonate resin were introduced into a feed block equipped with two-type, two-layer distribution pins, and the high-hardness resin and polycarbonate resin were laminated at a temperature of 240 ° C. The sheet was then introduced into a T-die at a temperature of 240 ° C. and extruded into a sheet, and cooled and stretched while transferring a mirror surface with three mirror-finished rolls at temperatures of 120 ° C., 130 ° C., and 190 ° C. from the upstream side, to obtain a laminate of a high-hardness resin layer and a polycarbonate resin layer (base layer). The stretching ratio was 1.3 times. The thickness of the obtained laminate was 1.2 mm, and the thickness of the high-hardness resin layer was 60 μm near the center.
[0162] A hard coat antiglare layer was formed on the high hardness resin layer side of the laminate obtained above. The materials for the hard coat antiglare layer are as follows. U6HA: 60% by mass of hexafunctional urethane acrylate oligomer (manufactured by Shin-Nakamura Chemical Co., Ltd.), 4EG-A: PEG200# diacrylate (Kyoeisha Chemical Co., Ltd.) 35% by mass, and ·RS-90: For 100 parts by mass of a 5% by mass mixture of fluorine-containing group, hydrophilic group, lipophilic group, and UV-reactive group-containing oligomer (manufactured by DIC Corporation), Photopolymerization initiator: I-184 (manufactured by BASF Ltd. [compound name: 1-hydroxy-cyclohexyl phenyl ketone]) 1 part by mass.
[0163] The above material was applied to the laminate using a bar coater, and the uneven surface of a 2 mm thick frosted glass plate with a haze of 10% was placed on top of it. A metal halide lamp (20 mW / cm 2 ) for 5 seconds to cure the hard coat, and after the hard coat anti-glare layer was attached, the frosted glass plate was peeled off to produce a resin sheet. The hard coat anti-glare layer had a thickness of 6 μm. The haze of the resin sheet was 9%, and the in-plane retardation was 6200 to 6500 nm.
[0164] A polycarbonate film (FS-2000, 100 μmt, manufactured by Mitsubishi Gas Chemical Co., Ltd.) was attached to the substrate layer side of the above resin sheet with an adhesive (acrylic OCA) to form a resin sheet for molding. The polycarbonate film had a thickness of 0.1 mm and an in-plane retardation of 20 nm or less.
[0165] Example 2: R100 (Tg 124°C) / Low Tg PC (Tg 125°C) / 2mmt The extrusion speed of the polycarbonate resin in the single screw extruder was 83.0 kg / h, and the thickness of the laminate of the high hardness resin layer and the polycarbonate resin layer (substrate layer) was 2 mm (the thickness of the high hardness resin layer was 60 μm near the center). The stretching ratio was 1.17 times. A hard coat anti-glare layer was formed in the same manner as in Example 1 to obtain a resin sheet. The in-plane retardation of the resin sheet was 6200 to 6500 nm. The method of laminating the polycarbonate film to the resin sheet was the same as in Example 1 to produce a molding resin sheet.
[0166] Example 3: R100 (Tg 124°C) / low Tg PC (Tg 125°C) / 0.5mmt The extrusion speeds of the high-hardness resin (B2) and the polycarbonate resin in the single-screw extruder were 4.8 kg / h and 35.0 kg / h, respectively, and the thickness of the laminate of the high-hardness resin layer and the polycarbonate resin layer (substrate layer) was 0.5 mm (the thickness of the high-hardness resin layer was 60 μm near the center). The stretching ratio was 1.5 times. A hard coat anti-glare layer was formed in the same manner as in Example 1 to obtain a resin sheet. The in-plane retardation was 4100 to 4500 nm. The method of laminating the polycarbonate film to the resin sheet was the same as in Example 1, and a molding resin sheet was produced.
[0167] Example 4: R100 (Tg 124°C) / low Tg PC (Tg 125°C) / 3.5mmt The extrusion speeds of the high-hardness resin (B2) and the polycarbonate resin in the single-screw extruder were 1.3 kg / h and 72.0 kg / h, respectively, and the thickness of the laminate of the high-hardness resin layer and the polycarbonate resin layer (substrate layer) was 3.5 mm (the thickness of the high-hardness resin layer was 60 μm near the center). The stretching ratio was 1.1 times. A hard coat anti-glare layer was formed in the same manner as in Example 1 to obtain a resin sheet. The in-plane retardation was 6800 to 7000 nm. The method of laminating the polycarbonate film to the resin sheet was the same as in Example 1, and a molding resin sheet was produced.
[0168] Example 5: R310 (Tg 141°C) / low Tg PC (Tg 125°C) / 2mmt A laminate consisting of a base layer and a high-hardness resin layer was formed using the same multi-layer extrusion device as in Example 1. Specifically, a high-hardness resin (B2) (a copolymer of 6% by mass of methyl methacrylate structural units, 71% by mass of styrene structural units, and 23% by mass of maleic anhydride structural units; Resiphi R310 (manufactured by Denka)) was continuously introduced into a single-screw extruder having a shaft diameter of 35 mm, and extruded under conditions of a cylinder temperature of 240°C and a discharge rate of 2.6 kg / h. In addition, a polycarbonate resin (Iupizeta T-1380; manufactured by Mitsubishi Gas Chemical) was continuously introduced into a single-screw extruder having a shaft diameter of 65 mm, and extruded under conditions of a cylinder temperature of 240°C and a discharge rate of 83.0 kg / h.
[0169] Thereafter, a laminate of a high-hardness resin layer and a polycarbonate resin layer (substrate layer) was obtained by extrusion using a T-die in the same manner as in Example 1. The thickness of the obtained laminate was 2 mm, and the thickness of the high-hardness resin layer was 60 μm near the center. The stretching ratio was 1.17 times. The hard coat anti-glare layer was formed in the same manner as in Example 1. The in-plane retardation of the resin sheet was 6200 to 6500 nm. The method of bonding the polycarbonate film to the resin sheet was the same as in Example 1, to produce a molding resin sheet.
[0170] Example 6: R310 (Tg 141° C.) / S-1000 (Tg 147° C.) / 2 mmt A laminate consisting of a base layer and a high-hardness resin layer was formed using the same multi-layer extrusion device as in Example 1. Specifically, a high-hardness resin (B2) (a copolymer of 6% by mass of methyl methacrylate structural units, 71% by mass of styrene structural units, and 23% by mass of maleic anhydride structural units; Resiphi R310 (manufactured by Denka)) was continuously introduced into a single-screw extruder having a shaft diameter of 35 mm, and extruded under conditions of a cylinder temperature of 240°C and an extrusion rate of 2.6 kg / h. In addition, a polycarbonate resin (Iupilon S-1000; manufactured by Mitsubishi Engineering Plastics Corporation) was continuously introduced into a single-screw extruder having a shaft diameter of 65 mm, and extruded under conditions of a cylinder temperature of 280°C and an extrusion rate of 83.0 kg / h.
[0171] The extruded high-hardness resin and polycarbonate resin were introduced into a feed block equipped with two-type, two-layer distribution pins, and the high-hardness resin and polycarbonate resin were laminated at a temperature of 280 ° C. The sheet was then introduced into a T-die at a temperature of 280 ° C. and extruded into a sheet, and cooled and stretched while transferring a mirror surface with three mirror-finished rolls at temperatures of 120 ° C., 130 ° C., and 190 ° C. from the upstream side, to obtain a laminate of a high-hardness resin layer and a polycarbonate resin layer (substrate layer). The thickness of the obtained laminate was 2 mm, and the thickness of the high-hardness resin layer was 60 μm near the center. The stretching ratio was 1.17 times. The hard coat anti-glare layer was formed in the same manner as in Example 1. The in-plane retardation of the resin sheet was 6200 to 6500 nm. The method of bonding the polycarbonate film to the resin sheet was the same as in Example 1, to produce a molding resin sheet.
[0172] Example 7: PM120N (Tg 120°C) / low Tg PC (Tg 125°C) / 1.5 mmt A laminate consisting of a base layer and a high-hardness resin layer was formed using the same multi-layer extrusion device as in Example 1. Specifically, a high-hardness resin (B4) (a copolymer of 7% by mass of styrene structural units, 86% by mass of methyl methacrylate structural units, and 7% by mass of N-phenylmaleimide structural units; Delpet PM120N (manufactured by Asahi Kasei Chemical Co., Ltd.)) was continuously introduced into a single-screw extruder having a shaft diameter of 35 mm, and extruded under conditions of a cylinder temperature of 230°C and an extrusion rate of 2.6 kg / h. In addition, a polycarbonate resin (Iupizeta T-1380; manufactured by Mitsubishi Gas Chemical Co., Ltd.) was continuously introduced into a single-screw extruder having a shaft diameter of 65 mm, and extruded under conditions of a cylinder temperature of 240°C and an extrusion rate of 62.0 kg / h.
[0173] Thereafter, a laminate of a high-hardness resin layer and a polycarbonate resin layer (substrate layer) was obtained by extrusion using a T-die in the same manner as in Example 1. The thickness of the obtained laminate was 1.5 mm, and the thickness of the high-hardness resin layer was 60 μm near the center. The stretching ratio was 1.23 times. The hard coat anti-glare layer was formed in the same manner as in Example 1. The in-plane retardation of the resin sheet was 6200 to 6500 nm. The method of bonding the polycarbonate film to the resin sheet was the same as in Example 1, to produce a molding resin sheet.
[0174] Example 8: R200 (Tg 126°C) / low Tg PC (Tg 125°C) / 2mmt A laminate consisting of a base layer and a high-hardness resin layer was formed using the same multi-layer extrusion device as in Example 1. Specifically, a high-hardness resin (B2) (a copolymer of 26% by mass of methyl methacrylate structural units, 55% by mass of styrene structural units, and 19% by mass of maleic anhydride structural units; Resify R200 (manufactured by Denka)) was continuously introduced into a single-screw extruder having a shaft diameter of 35 mm, and extruded under conditions of a cylinder temperature of 230°C and an extrusion rate of 2.6 kg / h. In addition, a polycarbonate resin (Iupizeta T-1380; manufactured by Mitsubishi Gas Chemical) was continuously introduced into a single-screw extruder having a shaft diameter of 65 mm, and extruded under conditions of a cylinder temperature of 240°C and an extrusion rate of 83.0 kg / h.
[0175] Thereafter, a laminate of a high-hardness resin layer and a polycarbonate resin layer (substrate layer) was obtained by extrusion using a T-die in the same manner as in Example 1. The thickness of the obtained laminate was 2 mm, and the thickness of the high-hardness resin layer was 60 μm near the center. The stretching ratio was 1.17 times. The material of the hard coat anti-glare layer was the same as that in Example 1. It was applied to the laminate using a bar coater, and then a 2 mm thick frosted glass with a haze of 30% was placed on top of it, and a metal halide lamp (20 mW / cm 2 ) for 5 seconds to cure the hard coat, and after adhering the hard coat anti-glare layer, the frosted glass plate was peeled off to prepare a resin sheet. The hard coat anti-glare layer had a film thickness of 6 μm. The haze of the resin sheet was 29%, and the in-plane retardation of the resin sheet was 6200 to 6500 nm. The method of laminating the polycarbonate film to the resin sheet was the same as in Example 1, and a molding resin sheet was prepared.
[0176] Example 9: C-PC (KH3410UR) (Tg 118°C) / low Tg PC (Tg 125°C) / 2mmt A laminate consisting of a substrate layer and a high-hardness resin layer was formed using the same multi-layer extrusion device as in Example 1. Specifically, a high-hardness resin (B3) (polycarbonate resin; Iupilon KH3410UR (manufactured by Mitsubishi Engineering Plastics Co., Ltd.)) was continuously introduced and extruded under the conditions of a cylinder temperature of 270°C and a discharge rate of 2.6 kg / h. In addition, a polycarbonate resin (Iupizeta T-1380; manufactured by Mitsubishi Gas Chemical Co., Ltd.) was continuously introduced into a single-screw extruder having a shaft diameter of 65 mm and extruded under the conditions of a cylinder temperature of 240°C and a discharge rate of 83.0 kg / h.
[0177] Thereafter, a laminate of a high-hardness resin layer and a polycarbonate resin layer (substrate layer) was obtained by extrusion using a T-die in the same manner as in Example 1. The thickness of the obtained laminate was 2 mm, and the thickness of the high-hardness resin layer was 60 μm near the center. The stretching ratio was 1.17 times. The hard coat anti-glare layer was formed in the same manner as in Example 8. The in-plane retardation of the resin sheet was 6200 to 6500 nm. The method of laminating the polycarbonate film to the resin sheet was the same as in Example 1, to prepare a molding resin sheet.
[0178] Example 10: Alloy of R100 and PM120N (Tg 123°C) / Low Tg PC (Tg 125°C) / 1.2 mmt 75% by mass of a copolymer having 21% by mass of methyl methacrylate structural units, 64% by mass of styrene structural units, and 15% by mass of maleic anhydride structural units (Resify R100 (manufactured by Denka)) and 25% by mass of a copolymer having 7% by mass of styrene structural units, 86% by mass of methyl methacrylate structural units, and 7% by mass of N-phenylmaleimide structural units (Delpet PM120N; manufactured by Asahi Kasei Chemical) were introduced into an extruder having a screw diameter of 26 mm (TEM-26SS, L / D ≒ 40; manufactured by Toshiba Machine) and melt-kneaded at 240 ° C. to obtain a high-hardness resin (B4).
[0179] A laminate consisting of a base layer and a high-hardness resin layer was formed using the same multi-layer extrusion device as in Example 1. Specifically, the above-mentioned high-hardness resin (B4) was continuously introduced into a single-screw extruder having a shaft diameter of 35 mm, and extruded under the conditions of a cylinder temperature of 230° C. and a discharge rate of 2.6 kg / h. In addition, a polycarbonate resin (Iupizeta T-1380; manufactured by Mitsubishi Gas Chemical Co., Ltd.) was continuously introduced into a single-screw extruder having a shaft diameter of 65 mm, and extruded under the conditions of a cylinder temperature of 240° C. and a discharge rate of 50.0 kg / h.
[0180] Thereafter, a laminate of a high-hardness resin layer and a polycarbonate resin layer (substrate layer) was obtained by extrusion using a T-die in the same manner as in Example 1. The thickness of the obtained laminate was 1.2 mm, and the thickness of the high-hardness resin layer was 60 μm near the center. The stretching ratio was 1.3 times. The hard coat anti-glare layer was formed in the same manner as in Example 8. The in-plane retardation of the resin sheet was 6200 to 6500 nm. A polycarbonate film (FS-2000, 200 μmt, manufactured by Mitsubishi Gas Chemical Co., Ltd.) was attached to the substrate layer side of the above resin sheet with an adhesive (acrylic OCA) to form a resin sheet for molding. The polycarbonate film had a thickness of 0.2 mm and an in-plane retardation of 45 nm or less.
[0181] Example 11: R310 (Tg 141° C.) / low Tg PC (Tg 125° C.) / 0.5 mmt A laminate consisting of a base layer and a high-hardness resin layer was formed using the same multi-layer extrusion device as in Example 1. Specifically, a high-hardness resin (B2) (a copolymer of 6% by mass of methyl methacrylate structural units, 71% by mass of styrene structural units, and 23% by mass of maleic anhydride structural units; Resiphi R310 (manufactured by Denka)) was continuously introduced into a single-screw extruder having a shaft diameter of 35 mm, and extruded under conditions of a cylinder temperature of 230°C and an extrusion rate of 8 kg / h. In addition, a polycarbonate resin (Iupizeta T-1380; manufactured by Mitsubishi Gas Chemical) was continuously introduced into a single-screw extruder having a shaft diameter of 65 mm, and extruded under conditions of a cylinder temperature of 240°C and an extrusion rate of 35.0 kg / h.
[0182] Thereafter, a laminate of a high-hardness resin layer and a polycarbonate resin layer (substrate layer) was obtained by extrusion using a T-die in the same manner as in Example 1. The thickness of the obtained laminate was 0.5 mm, and the thickness of the high-hardness resin layer was 100 μm near the center. The stretching ratio was 1.5 times. The material of the hard coat anti-glare layer was the same as that in Example 1. It was applied to the laminate using a bar coater, and then a 2 mm thick frosted glass with a haze of 4% was placed on top of it, and a metal halide lamp (20 mW / cm 2 ) for 5 seconds to cure the hard coat, and after the hard coat anti-glare layer was attached, the frosted glass plate was peeled off to prepare a resin sheet. The hard coat anti-glare layer had a thickness of 6 μm. The haze of the resin sheet was 2%, and the in-plane retardation was 4100 to 4500 nm. The method of laminating the polycarbonate film to the resin sheet was the same as in Example 10 to prepare a molding resin sheet.
[0183] Example 12: FPC0220 (Tg 184° C.) / E2000 (147° C.) / 1.2 mmt A laminate consisting of a base layer and a high-hardness resin layer was molded using the same multi-layer extrusion device as in Example 1. Specifically, a high-hardness resin (B5) (a polycarbonate resin containing a structural unit represented by general formula (8); Iupizeta FPC0220 (manufactured by Mitsubishi Gas Chemical)) was continuously introduced into a single-screw extruder having a shaft diameter of 35 mm, and extruded under conditions of a cylinder temperature of 300° C. and a discharge rate of 2.6 kg / h. In addition, a polycarbonate resin (Iupilon E2000; manufactured by Mitsubishi Gas Chemical) was continuously introduced into a single-screw extruder having a shaft diameter of 65 mm, and extruded under conditions of a cylinder temperature of 280° C. and a discharge rate of 50.0 kg / h.
[0184] The extruded high-hardness resin and polycarbonate resin were introduced into a feed block equipped with two-type, two-layer distribution pins, and the high-hardness resin and polycarbonate resin were laminated at a temperature of 280°C. The sheet was then extruded into a sheet shape using a T-die at a temperature of 280°C, and cooled and stretched while transferring a mirror surface using three mirror-finished rolls at temperatures of 120°C, 130°C, and 190°C from the upstream side, to obtain a laminate of a high-hardness resin layer and a polycarbonate resin layer (substrate layer). The thickness of the obtained laminate was 1.2 mm, and the thickness of the high-hardness resin layer was 60 μm near the center. The stretching ratio was 1.3 times. The hard coat anti-glare layer was formed in the same manner as in Example 11. The in-plane retardation of the resin sheet was 6200 to 6500 nm. The method of laminating the polycarbonate film to the resin sheet was the same as in Example 10 to prepare a molding resin sheet. The first protective film and the second protective film were attached in the same manner as in Example 1.
[0185] Example 13: MS-H (Tg115℃) / Low TgPC (Tg125℃) / 1.2mmt A laminate consisting of a base layer and a high-hardness resin layer was formed using the same multi-layer extrusion device as in Example 1. A high-hardness resin (B1) (a resin in which R1 and R2 in general formula (1) are both methyl groups, R3 in general formula (2) is a hydrogen atom, and R4 is a cyclohexyl group; consisting of 75 mol% (meth)acrylic acid ester structural units and 25 mol% aliphatic vinyl structural units, with a weight-average molecular weight of 120,000) was continuously introduced into a single-screw extruder with a shaft diameter of 35 mm, and extruded under conditions of a cylinder temperature of 240°C and an extrusion rate of 2.6 kg / h. A polycarbonate resin (Iupizeta T-1380; manufactured by Mitsubishi Gas Chemical) was continuously introduced into a single-screw extruder with a shaft diameter of 65 mm, and extruded under conditions of a cylinder temperature of 240°C and an extrusion rate of 50.0 kg / h.
[0186] Thereafter, a laminate of a high-hardness resin layer and a polycarbonate resin layer (substrate layer) was obtained by extrusion using a T-die in the same manner as in Example 1. The thickness of the obtained laminate was 1.2 mm, and the thickness of the high-hardness resin layer was 60 μm near the center. The stretching ratio was 1.3 times. The hard coat anti-glare layer was formed in the same manner as in Example 11. The in-plane retardation of the resin sheet was 6200 to 6500 nm. The method of laminating the polycarbonate film to the resin sheet was the same as in Example 10 to prepare a molding resin sheet.
[0187] Example 14: Alloy of V040 and St-MAH resin (Tg 136°C) / Low Tg PC (Tg 125°C) / 1.2 mmt 75% by mass of a copolymer (XIBOND160 (manufactured by Polyscope)) containing 78% by mass of styrene constituent units and 22% by mass of maleic anhydride constituent units, and 25% by mass of an acrylic resin (Altoglass V040 (manufactured by Arkema)) were introduced into an extruder (TEM-26SS, L / D ≒ 40; manufactured by Toshiba Machine) with a screw diameter of 26 mm, and melt-kneaded at 240°C to obtain a high-hardness resin (B6).
[0188] A laminate consisting of a base layer and a high-hardness resin layer was molded using the same multi-layer extrusion device as in Example 1. Specifically, the high-hardness resin (B6) was continuously introduced into a single-screw extruder having a shaft diameter of 35 mm, and extruded under the conditions of a cylinder temperature of 230° C. and a discharge rate of 2.6 kg / h. In addition, a polycarbonate resin (Iupizeta T-1380; manufactured by Mitsubishi Gas Chemical Co., Ltd.) was continuously introduced into a single-screw extruder having a shaft diameter of 65 mm, and extruded under the conditions of a cylinder temperature of 240° C. and a discharge rate of 50.0 kg / h.
[0189] Thereafter, a laminate of a high-hardness resin layer and a polycarbonate resin layer (substrate layer) was obtained by extrusion using a T-die in the same manner as in Example 1. The thickness of the obtained laminate was 1.2 mm, and the thickness of the high-hardness resin layer was 60 μm near the center. The stretching ratio was 1.3 times. The hard coat anti-glare layer was formed in the same manner as in Example 8. The in-plane retardation of the resin sheet was 6200 to 6500 nm. A polycarbonate film (FS-2000, 200 μmt, manufactured by Mitsubishi Gas Chemical Co., Ltd.) was attached to the substrate layer side of the above resin sheet with an adhesive (acrylic OCA) to form a resin sheet for molding. The polycarbonate film had a thickness of 0.2 mm and an in-plane retardation of 45 nm or less.
[0190] Example 15: Alloy of V020 and St-MAH resin (Tg 132°C) / Low Tg PC (Tg 125°C) / 1.2 mmt A copolymer (XIBOND160 (manufactured by Polyscope)) of 78% by mass of styrene constituent units and 22% by mass of maleic anhydride constituent units, 75% by mass, and an acrylic resin (Altoglass V020 (manufactured by Arkema) 25% by mass) were introduced into an extruder (TEM-26SS, L / D ≒ 40; manufactured by Toshiba Machine) with a screw diameter of 26 mm and melt-kneaded at 240°C to obtain a high-hardness resin (B6).
[0191] A laminate consisting of a base layer and a high-hardness resin layer was molded using the same multi-layer extrusion device as in Example 1. Specifically, the high-hardness resin (B6) was continuously introduced into a single-screw extruder having a shaft diameter of 35 mm, and extruded under the conditions of a cylinder temperature of 230° C. and a discharge rate of 2.6 kg / h. In addition, a polycarbonate resin (Iupizeta T-1380; manufactured by Mitsubishi Gas Chemical Co., Ltd.) was continuously introduced into a single-screw extruder having a shaft diameter of 65 mm, and extruded under the conditions of a cylinder temperature of 240° C. and a discharge rate of 50.0 kg / h.
[0192] Thereafter, a laminate of a high-hardness resin layer and a polycarbonate resin layer (substrate layer) was obtained by extrusion using a T-die in the same manner as in Example 1. The thickness of the obtained laminate was 1.2 mm, and the thickness of the high-hardness resin layer was 60 μm near the center. The stretching ratio was 1.3 times. The hard coat anti-glare layer was formed in the same manner as in Example 8. The in-plane retardation of the resin sheet was 6200 to 6500 nm. A polycarbonate film (FS-2000, 200 μmt, manufactured by Mitsubishi Gas Chemical Co., Ltd.) was attached to the substrate layer side of the above resin sheet with an adhesive (acrylic OCA) to form a resin sheet for molding. The polycarbonate film had a thickness of 0.2 mm and an in-plane retardation of 45 nm or less.
[0193] Comparative example 1: MS-H (Tg115℃) / Low TgPC (125℃) / 0.5mmt The conditions for extruding the high-hardness resin (B1) with a single-screw extruder were a cylinder temperature of 230°C and a discharge rate of 8.0 kg / h, and the discharge rate for extruding the polycarbonate resin with a single-screw extruder was 35.0 kg / h, and the thickness of the laminate of the high-hardness resin layer and the polycarbonate resin layer (base layer) was 0.5 mm (the thickness of the high-hardness resin layer was 60 μm near the center). The stretching ratio was 1.5 times. The hard coat anti-glare layer was formed in the same manner as in Example 1. The in-plane retardation of the resin sheet was 4100 to 4500 nm. A polycarbonate film (Mitsubishi Gas Chemical's NF-2000NS, 500 μmt) was attached as a resin film (X) to the substrate layer side of the above resin sheet with an adhesive (acrylic OCA) to prepare a molding resin sheet. The polycarbonate film had a thickness of 0.5 mm and an in-plane retardation of 300 to 400 nm.
[0194] Comparative Example 2: Alloy of R100 and PMMA (Tg 115°C) / Low Tg PC (Tg 125°C) / 1.2 mmt 75% by mass of a copolymer consisting of 21% by mass of methyl methacrylate structural units, 64% by mass of styrene structural units, and 15% by mass of maleic anhydride structural units (Resify R100; manufactured by Denka) and 25% by mass of an acrylic resin (Parapet HR-1000L (PMMA); manufactured by Kuraray Co., Ltd.) were introduced into an extruder with a screw diameter of 26 mm (TEM-26SS, L / D ≒ 40; manufactured by Toshiba Machine Co., Ltd.) and melt-kneaded at 240°C to obtain a high-hardness resin (B2).
[0195] A laminate consisting of a base layer and a high-hardness resin layer was formed using the same multi-layer extrusion device as in Example 1. Specifically, the high-hardness resin was continuously introduced into a single-screw extruder having a shaft diameter of 35 mm, and extruded under conditions of a cylinder temperature of 230° C. and a discharge rate of 2.6 kg / h. In addition, a polycarbonate resin (Iupizeta T-1380; manufactured by Mitsubishi Gas Chemical Co., Ltd.) was continuously introduced into a single-screw extruder having a shaft diameter of 65 mm, and extruded under conditions of a cylinder temperature of 240° C. and a discharge rate of 50.0 kg / h.
[0196] Thereafter, a laminate of a high-hardness resin layer and a polycarbonate resin layer (substrate layer) was obtained by extrusion using a T-die in the same manner as in Example 1. The thickness of the obtained laminate was 1.2 mm, and the thickness of the high-hardness resin layer was 60 μm near the center. The stretching ratio was 1.3 times. The hard coat anti-glare layer was formed in the same manner as in Example 1. The in-plane retardation of the above resin sheet was 6200 to 6500 nm. A polycarbonate film (Mitsubishi Gas Chemical's NF-2000NS, 500 μmt) was attached as a resin film (X) to the substrate layer side of the above resin sheet with an adhesive (acrylic OCA) to prepare a molding resin sheet. The polycarbonate film had a thickness of 0.5 mm and an in-plane retardation of 300 to 400 nm.
[0197] Comparative example 3: R100 (Tg124℃) / Low TgPC (Tg125℃) / 1.2mmt A laminate consisting of a base material layer and a high-hardness resin layer was formed using a multi-layer extrusion device having a single-screw extruder with a shaft diameter of 35 mm, a single-screw extruder with a shaft diameter of 65 mm, a feed block connected to each extruder, and a T-die connected to the feed block. Specifically, a high-hardness resin (B2) (a copolymer of 21% by mass of methyl methacrylate structural units, 64% by mass of styrene structural units, and 15% by mass of maleic anhydride structural units; Resify R100 (manufactured by Denka)) was continuously introduced into a single-screw extruder with a shaft diameter of 35 mm, and extruded under conditions of a cylinder temperature of 230°C and an extrusion rate of 2.6 kg / h. In addition, a polycarbonate resin (Iupizeta T-1380; manufactured by Mitsubishi Gas Chemical) was continuously introduced into a single-screw extruder with a shaft diameter of 65 mm, and extruded under conditions of a cylinder temperature of 240°C and an extrusion rate of 50.0 kg / h.
[0198] The extruded high-hardness resin and polycarbonate resin were introduced into a feed block equipped with two-kind two-layer distribution pins, and the high-hardness resin and polycarbonate resin were laminated at a temperature of 240 ° C. The sheet was then introduced into a T-die at a temperature of 240 ° C. and extruded into a sheet, and cooled and stretched while transferring a mirror surface with three mirror-finished rolls at temperatures of 120 ° C., 130 ° C., and 190 ° C. from the upstream side, to obtain a laminate of a high-hardness resin layer and a polycarbonate resin layer (substrate layer). The stretching ratio was 1.3 times. The thickness of the obtained laminate was 1.2 mm, and the thickness of the high-hardness resin layer was 60 μm near the center. The hard coat anti-glare layer was formed in the same manner as in Example 1. The in-plane retardation of the above resin sheet was 3000 to 3500 nm. A polycarbonate film (FS-2000, 100 μmt, manufactured by Mitsubishi Gas Chemical Co., Ltd.) was attached as a resin film (X) to the substrate layer side of the above resin sheet with an adhesive (acrylic OCA) to prepare a molding resin sheet. The polycarbonate film had a thickness of 0.1 mm and an in-plane retardation of 20 nm or less.
[0199] Comparative Example 4 Similarly to Example 1, a laminate of a high-hardness resin layer and a polycarbonate resin layer (substrate layer) was obtained. The hard coat anti-glare layer was formed in the same manner as in Example 1. The in-plane retardation of the above resin sheet was 6200 to 6500 nm. A polycarbonate film (Mitsubishi Gas Chemical's NF-2000 (H11), 500 μmt) was attached as a resin film (X) to the substrate layer side of the above resin sheet with an adhesive (acrylic OCA) to prepare a molding resin sheet. The polycarbonate film had a thickness of 0.5 mm and an in-plane retardation of 5000 to 6000 nm.
[0200] Comparative example 5: MS-H (Tg115℃) / S1000 (Tg147℃) / 1.2mmt A laminate consisting of a base layer and a high-hardness resin layer was formed using the same multi-layer extrusion device as in Example 1. Specifically, a high-hardness resin (B1) (a resin in which R1 and R2 in general formula (1) are both methyl groups, R3 in general formula (2) is a hydrogen atom, and R4 is a cyclohexyl group; consisting of 75 mol% (meth)acrylic acid ester structural units and 25 mol% aliphatic vinyl structural units, with a weight average molecular weight of 120,000) was continuously introduced into a single-screw extruder with a shaft diameter of 35 mm, and extruded under conditions of a cylinder temperature of 240°C and an extrusion rate of 2.6 kg / h. In addition, a polycarbonate resin (Iupilon S-1000; manufactured by Mitsubishi Engineering Plastics Corporation) was continuously introduced into a single-screw extruder with a shaft diameter of 65 mm, and extruded under conditions of a cylinder temperature of 280°C and an extrusion rate of 50.0 kg / h.
[0201] The extruded high-hardness resin and polycarbonate resin were introduced into a feed block equipped with two-type, two-layer distribution pins, and the high-hardness resin and polycarbonate resin were laminated at a temperature of 270°C. The sheet was then extruded into a sheet shape using a T-die at a temperature of 270°C, and cooled while transferring a mirror surface using three mirror-finished rolls at temperatures of 120°C, 130°C, and 190°C from the upstream side, to obtain a laminate of a high-hardness resin layer and a polycarbonate resin layer (substrate layer). The stretching ratio was 1.3 times. The thickness of the obtained laminate was 1.2 mm, and the thickness of the high-hardness resin layer was 60 μm near the center. The hard coat anti-glare layer was formed in the same manner as in Example 1. The in-plane retardation of the above resin sheet was 6200 to 6500 nm. A polycarbonate film (FS-2000, 200 μmt, manufactured by Mitsubishi Gas Chemical Co., Ltd.) was attached to the substrate layer side of the above resin sheet with an adhesive (acrylic OCA) to form a resin sheet for molding. The polycarbonate film had a thickness of 0.2 mm and an in-plane retardation of 45 nm or less.
[0202] Comparative example 6: MS-H (Tg115℃) / S1000 (Tg147℃) / 2mmt In Comparative Example 5, the extrusion speed of the polycarbonate resin in the single screw extruder was 83.0 kg / h, and the thickness of the laminate of the high hardness resin layer and the polycarbonate resin layer (substrate layer) was 2 mm (the thickness of the high hardness resin layer was 60 μm near the center). The stretching ratio was 1.17 times. The hard coat anti-glare layer was formed in the same manner as in Example 1. The in-plane retardation of the above resin sheet was 6200 to 6500 nm. A polycarbonate film (FS-2000, 200 μmt, manufactured by Mitsubishi Gas Chemical Co., Ltd.) was attached to the substrate layer side of the above resin sheet with an adhesive (acrylic OCA) to form a resin sheet for molding. The polycarbonate film had a thickness of 0.2 mm and an in-plane retardation of 45 nm or less.
[0203] Comparative example 7: MS-H (Tg115℃) / S1000 (Tg147℃) / 3.5mmt In Comparative Example 5, the extrusion speeds of the high-hardness resin (B1) and the polycarbonate resin in the single-screw extruder were 1.3 kg / h and 72.0 kg / h, respectively, and the thickness of the laminate of the high-hardness resin layer and the polycarbonate resin layer (base layer) was 3.5 mm (the thickness of the high-hardness resin layer was 60 μm near the center). The stretching ratio was 1.1 times. The hard coat anti-glare layer was formed in the same manner as in Example 1. The in-plane retardation of the above resin sheet was 6800 to 7000 nm. A polycarbonate film (FS-2000, 200 μmt, manufactured by Mitsubishi Gas Chemical Co., Ltd.) was attached to the substrate layer side of the above resin sheet with an adhesive (acrylic OCA) to form a resin sheet for molding. The polycarbonate film had a thickness of 0.2 mm and an in-plane retardation of 45 nm or less.
[0204] Comparative example 8: MS-H (Tg115℃) / S1000 (Tg147℃) / 0.5mmt In Comparative Example 5, the extrusion speeds of the high-hardness resin (B1) and the polycarbonate resin in the single-screw extruder were 4.8 kg / h and 35.0 kg / h, respectively, and the thickness of the laminate of the high-hardness resin layer and the polycarbonate resin layer (base layer) was 0.5 mm (the thickness of the high-hardness resin layer was 60 μm near the center). The stretching ratio was 1.5 times. The hard coat anti-glare layer was formed in the same manner as in Example 1. The in-plane retardation of the above resin sheet was 4100 to 4500 nm. A polycarbonate film (FS-2000, 200 μmt, manufactured by Mitsubishi Gas Chemical Co., Ltd.) was attached to the substrate layer side of the above resin sheet with an adhesive (acrylic OCA) to form a resin sheet for molding. The polycarbonate film had a thickness of 0.2 mm and an in-plane retardation of 45 nm or less.
[0205] Comparative example 9: PMMA (Tg105℃) / Low TgPC (Tg125℃) / 0.8mmt A laminate consisting of a base material layer and a high-hardness resin layer was formed using a multi-layer extrusion device having a single-screw extruder with a shaft diameter of 32 mm, a single-screw extruder with a shaft diameter of 65 mm, a feed block connected to each extruder, and a T-die connected to the feed block. Specifically, a high-hardness resin (acrylic resin; Parapet HR-1000L (PMMA); manufactured by Kuraray Co., Ltd.) was continuously introduced into the single-screw extruder with a shaft diameter of 32 mm, and extruded under conditions of a cylinder temperature of 250°C and an extrusion rate of 2.6 kg / h. In addition, a polycarbonate resin (Iupizeta T-1380; manufactured by Mitsubishi Gas Chemical Co., Ltd.) was continuously introduced into the single-screw extruder with a shaft diameter of 65 mm, and extruded under conditions of a cylinder temperature of 240°C and an extrusion rate of 32.0 kg / h.
[0206] The extruded high-hardness resin and polycarbonate resin were introduced into a feed block equipped with two-type, two-layer distribution pins, and the high-hardness resin and polycarbonate resin were laminated at a temperature of 240 ° C. The sheet was then extruded into a T-die at a temperature of 240 ° C., and cooled while transferring a mirror surface with three mirror-finished rolls at temperatures of 110 ° C., 140 ° C., and 185 ° C. from the upstream side, to obtain a laminate of a high-hardness resin layer and a polycarbonate resin layer (substrate layer). The thickness of the obtained laminate was 0.8 mm, and the thickness of the high-hardness resin layer was 60 μm near the center. The stretching ratio was 1.43 times. The hard coat anti-glare layer was formed in the same manner as in Example 1. The in-plane retardation of the above resin sheet was 5800 to 6300 nm. A polycarbonate film (FS-2000, 200 μmt, manufactured by Mitsubishi Gas Chemical Co., Ltd.) was attached to the substrate layer side of the above resin sheet with an adhesive (acrylic OCA) to form a resin sheet for molding. The polycarbonate film had a thickness of 0.2 mm and an in-plane retardation of 45 nm or less.
[0207] Comparative example 10: FPC0220(Tg184℃) / T1380(125℃) / 1.2mmt A laminate consisting of a base layer and a high-hardness resin layer was molded using the same multi-layer extrusion device as in Example 1. Specifically, a high-hardness resin (B5) (a polycarbonate resin containing a structural unit represented by general formula (8); Iupizeta FPC0220 (manufactured by Mitsubishi Gas Chemical)) was continuously introduced into a single-screw extruder having a shaft diameter of 35 mm, and extruded under conditions of a cylinder temperature of 300° C. and a discharge rate of 2.6 kg / h. In addition, a polycarbonate resin (Iupizeta T1380; manufactured by Mitsubishi Gas Chemical) was continuously introduced into a single-screw extruder having a shaft diameter of 65 mm, and extruded under conditions of a cylinder temperature of 240° C. and a discharge rate of 50.0 kg / h.
[0208] The extruded high-hardness resin and polycarbonate resin were introduced into a feed block equipped with two-type, two-layer distribution pins, and the high-hardness resin and polycarbonate resin were laminated at a temperature of 280°C. The sheet was then extruded into a sheet shape using a T-die at a temperature of 280°C, and cooled and stretched while transferring a mirror surface using three mirror-finished rolls at temperatures of 120°C, 130°C, and 190°C from the upstream side, to obtain a laminate of a high-hardness resin layer and a polycarbonate resin layer (substrate layer). The stretching ratio was 1.3 times. The thickness of the obtained laminate was 1.2 mm, and the thickness of the high-hardness resin layer was 60 μm near the center. The hard coat anti-glare layer was formed in the same manner as in Example 1. The in-plane retardation of the above resin sheet was 6200 to 6500 nm. A polycarbonate film (FS-2000, 200 μmt, manufactured by Mitsubishi Gas Chemical Co., Ltd.) was attached to the substrate layer side of the above resin sheet with an adhesive (acrylic OCA) to form a resin sheet for molding. The polycarbonate film had a thickness of 0.2 mm and an in-plane retardation of 45 nm or less.
[0209] Comparative Example 11: S-1000 (Tg 147°C) alone / 2mmt Instead of the high hardness resin, the same polycarbonate resin as that contained in the base layer was used to form a laminate. The same multi-layer extrusion device as in Example 1 was used as the extrusion device. Specifically, polycarbonate resin (Iupilon S-1000 (manufactured by Mitsubishi Engineering Plastics Corporation); pencil hardness 3B) was continuously introduced into a single-screw extruder with a shaft diameter of 35 mm, and extruded under the conditions of a cylinder temperature of 280° C. and an extrusion speed of 2.6 kg / h. In addition, polycarbonate resin (Iupilon S-1000; manufactured by Mitsubishi Engineering Plastics Corporation) was continuously introduced into a single-screw extruder with a shaft diameter of 65 mm, and extruded under the conditions of a cylinder temperature of 280° C. and an extrusion speed of 83.0 kg / h.
[0210] The extruded polycarbonate resin was introduced into a feed block equipped with two-type, two-layer distribution pins and laminated at a temperature of 280°C. It was further introduced into a T-die at a temperature of 280°C and extruded into a sheet, and cooled and stretched while transferring a mirror surface with three mirror-finished rolls at temperatures of 120°C, 130°C, and 190°C from the upstream side, to obtain a polycarbonate resin laminate. The stretching ratio was 1.17 times. The thickness of the obtained laminate was 2 mm. The hard coat anti-glare layer was formed in the same manner as in Example 1. The in-plane retardation of the above resin sheet was 6200 to 6500 nm. A polycarbonate film (FS-2000, 200 μmt, manufactured by Mitsubishi Gas Chemical Co., Ltd.) was attached to the substrate layer side of the above resin sheet with an adhesive (acrylic OCA) to form a resin sheet for molding. The polycarbonate film had a thickness of 0.2 mm and an in-plane retardation of 45 nm or less.
[0211] The resin sheets produced in the examples and comparative examples were evaluated for hardness, the presence or absence of cracks after molding, flow marks, mold scratch transfer, and the presence or absence of protective film fusion. The results are shown in Table 1 below.
[0212] [Table 1] TIFF0007555932000023.tif250170
[0213] It can be seen that the resin sheet of the present invention has excellent hardness, is free of flow marks, and does not suffer from abnormal appearance such as cracks after thermoforming.
[0214] Although some embodiments of the present invention have been described, these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their modifications are included in the scope and spirit of the invention, and are included in the scope of the invention and its equivalents described in the claims.
Claims
1. A resin sheet having a high-hardness resin layer containing a high-hardness resin on at least one surface of a substrate layer containing a polycarbonate resin (a1), and a hard coat layer or a hard coat anti-glare layer laminated on at least one surface of the high-hardness resin layer, The glass transition points of the polycarbonate resin (a1) and the high-hardness resin satisfy the following relationship: −10° C.≦(glass transition point of high hardness resin)−(glass transition point of polycarbonate resin (a1))≦40° C. The in-plane retardation of the resin sheet measured at a wavelength of 543 nm is 4000 nm or more; A molding resin sheet having a resin film (X) having an in-plane retardation of 50 nm or less when measured at a wavelength of 543 nm laminated to one surface of the resin sheet with an adhesive layer containing an adhesive.
2. 2. The molding resin sheet according to claim 1, wherein the polycarbonate resin (a1) is an aromatic polycarbonate resin.
3. The molding resin sheet according to claim 2 , wherein the aromatic polycarbonate resin contains a structural unit represented by the following general formula (4a): [Formula 1]
4. The molding resin sheet according to any one of claims 1 to 3, wherein the content of the polycarbonate resin (a1) is 75 to 100 mass% with respect to the total mass of the base layer.
5. The molding resin sheet according to any one of claims 1 to 4, wherein the high-hardness resin is selected from the group consisting of the following resins (B1) to (B6): Resin (B1): A copolymer containing a (meth)acrylic acid ester structural unit (a) represented by the following general formula (1) and an aliphatic vinyl structural unit (b) represented by the following general formula (2), or an alloy of the copolymer with resin (B2). [chemical 2] (In the formula, R1 is a hydrogen atom or a methyl group; R2 is an alkyl group having 1 to 18 carbon atoms.) [C3] (wherein R3 is a hydrogen atom or a methyl group; R4 is a cyclohexyl group which may be substituted with a hydrocarbon group having 1 to 4 carbon atoms); Resin (B2): a copolymer (D) containing 6 to 77% by mass of (meth)acrylic acid ester structural units, 15 to 71% by mass of styrene structural units, and 8 to 23% by mass of unsaturated dicarboxylic acid structural units, an alloy of the copolymer (D) itself, an alloy of the copolymer (D) with another high-hardness resin, or an alloy of the copolymer (D) with an acrylic resin; Resin (B3): A copolymer containing a structural unit (c) represented by the following general formula (6) and, optionally, a structural unit (d) represented by the following general formula (7): [C4] [C5] Resin (B4): a copolymer (G) containing 5 to 20 mass% of styrene structural units, 60 to 90 mass% of (meth)acrylic acid ester structural units, and 5 to 20 mass% of N-substituted maleimide structural units, or an alloy of the copolymer (G) and the resin (B2); Resin (B5): A resin containing a structural unit (e) represented by the following general formula (8). [C6] Resin (B6): An alloy of a copolymer containing 50 to 95% by mass of styrene constituent units and 5 to 50% by mass of unsaturated dicarboxylic acid units and an acrylic resin.
6. The molding resin sheet according to any one of claims 1 to 5, wherein the content of the high hardness resin is 70 to 100 mass % based on the total mass of the high hardness resin layer.
7. The molding resin sheet according to any one of claims 1 to 6, wherein a total thickness of the base material layer and the high-hardness resin layer is 0.5 mm to 3.5 mm.
8. The molding resin sheet according to any one of claims 1 to 7, wherein a ratio of a thickness of the base material layer to a total thickness of the base material layer and the high-hardness resin layer is 75% to 99%.
9. The molding resin sheet according to any one of claims 1 to 8, wherein the molding resin sheet has a haze of 2 to 30%.
10. 10. The molding resin sheet according to claim 1, wherein the hard coat layer surface in the molding resin sheet has a pencil hardness of 2H or more.
11. The molding resin sheet according to any one of claims 1 to 10, wherein the resin film (X) in the molding resin sheet is a polycarbonate film containing a polycarbonate resin (a1).
12. The molding resin sheet according to any one of claims 1 to 10, wherein the resin film (X) in the molding resin sheet is made of a film touch sensor in which a sensor electrode is applied to a polycarbonate film.
13. The molding resin sheet according to any one of claims 1 to 12, wherein the adhesive layer in the molding resin sheet is an optically adhesive sheet.
14. A resin molded product molded using the molding resin sheet according to any one of claims 1 to 13.
Citation Information
Patent Citations
Signal reproducing device
JP1992040183A
Decorative sheet and foil decorating resin molded article
JP2001334609A
Resin sheet for molding and molded body
JP2009196153A
Multilayer film for sticking simultaneously with injection molding
JP2009234184A
Hard coat film for decoration, decorative film, and decorative molded product
JP2010284910A