Compression coil spring for actuator for opening and closing a vehicle door or tailgate

By employing alloy steel with elongated layered pearlite microstructure and optimized manufacturing, the coil springs address the challenges of compact size, high compressive force, and fatigue resistance, ensuring durable and quiet operation of SUV tailgate actuators.

JP7555943B2Active Publication Date: 2024-09-25NV BEKAERT SA
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021549598
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-02-26
Filing Date
2020-01-29
Publication Date
2024-09-25
Estimated Expiration
2040-01-29

AI Technical Summary

Technical Problem

Existing coil springs for SUV tailgates face challenges in achieving compact size, high compressive force resistance, low spring stress relaxation, and sufficient fatigue life due to the large size and heavy weight of SUV tailgates, necessitating improvements in material composition and manufacturing processes.

Method used

The use of alloy steel with specific compositions and microstructures, such as elongated layered pearlite, combined with optimized manufacturing processes like patenting and stress relief, results in compression coil springs with enhanced strength, ductility, and reduced relaxation, suitable for high-cycle operations.

Benefits of technology

The solution provides coil springs with improved mechanical properties, enabling efficient and durable operation of electric tailgate actuators, reducing noise and maintaining consistent performance over numerous cycles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555943000002
    Figure 0007555943000002
  • Figure 0007555943000003
    Figure 0007555943000003
  • Figure 0007555943000004
    Figure 0007555943000004
Patent Text Reader

Abstract

The compression coil spring has an outer diameter of 15 to 50 mm. The compression coil spring comprises a spirally wound steel wire. The diameter d (mm) of the steel wire is 2 to 5 mm. The steel wire comprises an alloy steel consisting of 0.8 to 0.95 wt% C; 0.2 to 0.9 wt% Mn; 0.1 to 1.4 wt% Si; 0.15 to 0.4 wt% Cr; optionally 0.04 to 0.2 wt% V; optionally 0.0005 to 0.008 wt% B; optionally 0.02 to 0.06 wt% Al; unavoidable impurities; and the remainder iron. The alloy steel has a carbon equivalent greater than 1. The carbon equivalent is defined as C wt% + (Mn wt% / 6) + (Si wt% / 5) + (Cr wt% / 5) + (V wt% / 5). The microstructure of steel wire in compression springs is elongated lamellar pearlite.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a compression coil spring for an actuator for opening and closing a door or tailgate of a vehicle.The present invention further relates to an actuator for opening and closing a door or tailgate of a vehicle. [Background technology]

[0002] Sports utility vehicles (SUVs) are becoming increasingly popular. SUVs have large (and therefore heavy) tailgates. To open and close the tailgates of such SUVs, it is known to use a compressed coil steel spring in an actuator.

[0003] There is a growing trend to use power tailgate opening and closing actuators, US Patent Application Publication Nos. 2018 / 0216391 A1 and 2017 / 0114580 A1 disclose such actuators.

[0004] In such a typical actuator, the tailgate is opened by releasing the force of a coiled steel wire spring operating in a compression mode. The tailgate is closed by the operation of a motor; this causes the motor to compress the coiled steel wire spring. Coiled steel wire springs for such applications must meet very strict requirements. According to the first requirement, the diameter of the coiled spring must be small in order to make the tailgate opening and closing system as compact as possible. The spring must be able to withstand high compression forces in a consistent manner. Since the stress relaxation of the spring changes the spring force for a given compression, the stress relaxation of the spring must be low, which is a negative for the operation of the tailgate opening and closing actuator. Furthermore, the spring must have sufficient fatigue resistance in that it must withstand the required number of opening and closing cycles of the tailgate at high spring loads. Due to the size of the tailgate of an SUV, the length of the springs used is long.

[0005] It is known to use steel wire having a martensitic microstructure to manufacture coil springs for vehicle tailgate opening and closing actuators. Steel wire having a martensitic microstructure is typically manufactured by a hardening and tempering heat treatment process.

[0006] German Utility Model No. 202004015535U1 describes a tailgate opening and closing system for vehicles. The system comprises a coiled steel wire spring. The spring is made of a steel wire having a diameter of at least 1 mm. The alloy steel from which the steel wire is made contains 0.5-0.9% by weight carbon, 1-2.5% by weight silicon, 0.3-1.5% by weight manganese, 0.5-1.5% by weight chromium, iron and impurities. The alloy steel optionally contains 0.05-0.3% by weight vanadium and / or 0.5-0.3% by weight niobium and / or tantalum. The steel wire is produced by a patenting process followed by wire drawing. The steel wire is then hardened and tempered to give a martensitic microstructure, a strength of 2300 N / mm 2 Tensile strengths of greater than 0.2 mm and reduction in cross-sectional area at break of greater than 40% are obtained. The resulting steel wire is cold formed into coil springs and then stress relieved at temperatures between 200°C and 400°C. The springs can be shot peened to increase durability.

[0007] There are coil springs made of hard drawn steel wire. The European standard EN 10270-1:2011 is entitled “Steel wire for mechanical springs - Part 1: Patented cold drawn unalloyed spring steel wire”. Although the title refers to unalloyed spring steel wire, section 6.1.2 of the standard indicates that the addition of micro-alloy elements may be agreed between the manufacturer and the purchaser. This standard differentiates the steel spring wires in two ways. The first way is by static duty (S) or dynamic duty (D). The second way is by tensile strength, low (L), medium (M), or high (H). Combining the two ways, five grades of spring steel wire (SL, SM, DM, SH, and DH) are provided whose mechanical properties (especially tensile strength Rm) and quality requirements as a function of steel wire diameter are given in Table 3 of the standard EN 10270-1:2011. As an example, for a steel wire with a diameter of 3.8 to 4 mm, the tensile strength Rm of grade DH (the grade with the highest specified tensile strength) must be 1740 to 1930 MPa. Summary of the Invention [Means for solving the problem]

[0008] A first aspect of the present invention is a compression coil spring, preferably for use in an actuator for opening or closing a vehicle door or tailgate. The compression coil spring has an outer diameter of 15-50 mm. The compression coil spring comprises a spirally wound steel wire. The steel wire has a diameter d (mm) of 2-5 mm. The steel wire comprises an alloy steel consisting of 0.8-0.95 wt% C; 0.2-0.9 wt% Mn; 0.1-1.4 wt% Si; 0.15-0.4 wt% Cr; optionally 0.04-0.2 wt% V; optionally 0.0005-0.008 wt% B; optionally 0.02-0.06 wt% Al; unavoidable impurities; and the remainder iron. The alloy steel has a carbon equivalent greater than 1. Carbon equivalent is defined as: C wt% + (Mn wt% / 6) + (Si wt% / 5) + (Cr wt% / 5) + (V wt% / 5). The microstructure of steel wire for compression springs is elongated lamellar pearlite.

[0009] Surprisingly, the compression coil spring of the present invention is ideally suited for use in actuators for opening and closing vehicle doors or tailgates. Martensitic steel wire has been described in the prior art for use in compression coil springs for actuators for opening and closing tailgates. The steel wire required for coil springs for actuators for opening and closing tailgates should have a diameter of 2-5 mm and should have high strength and sufficient ductility. Hardened and tempered steel wire (with martensitic microstructure) of these diameters has the highest strength. Helically wound springs made of such hardened and tempered steel wire and subjected to standard post-treatments (e.g. stress relief and shot peening) offer a combination of excellent fatigue life and low relaxation of spring force. Due to the high demands on springs for actuators for opening and closing tailgates (high compression force, low relaxation tolerance and fatigue life requirements) which are perfectly in line with the known properties of martensitic steel wires, the skilled person has a technical prejudice against using martensitic steel wires and not hard drawn wires (hard drawn wires having an elongated pearlitic microstructure) for the manufacture of compression coil springs for actuators for opening and closing tailgates. The alloy steels selected in the present invention surprisingly provide steel wires with an elongated pearlitic microstructure having the combination of steel wire properties (strength, yield strength, ductility) required to obtain compression coil springs which meet the stringent requirements for use in actuators for opening and closing car doors or tailgates.

[0010] Preferably, the carbon content of the steel alloy is less than 0.93 wt%, more preferably less than 0.9 wt%.

[0011] Preferably, the alloy steel contains less than 0.35 wt% Cr, more preferably less than 0.3 wt% Cr.

[0012] If the steel alloy contains V, then preferably the steel alloy contains less than 0.15 wt% V.

[0013] Preferably, the alloy steel contains 0.02-0.06 wt% Al. It is an advantage of such an embodiment that a better compression coil spring can be obtained thanks to the higher ductility of the steel wire used to manufacture the compression coil spring.

[0014] Preferably, the compression coil spring has an outside diameter of less than 40 mm.

[0015] Preferably, the compression coil spring has a length in an unloaded state of more than 40 cm, more preferably more than 60 cm.

[0016] Preferably, the length of the spring in the unloaded state is less than 1000 mm.

[0017] Preferably, the compression coil spring has a spring index of 3 to 8. The spring index is the ratio of the diameter of the spring to the diameter of the spring steel wire (wherein the spring diameter for calculating the spring index is the average of the outer diameter and the inner diameter of the spring in an unloaded state).

[0018] Preferably, the alloy steel has a carbon equivalent greater than 1.05; more preferably greater than 1.1.

[0019] Preferably, the alloy steel has a carbon equivalent of less than 1.4, more preferably less than 1.3.

[0020] Preferably, the diameter of the steel wire is 2 to 4 mm, more preferably 2.5 to 3.8 mm.

[0021] Preferably, the compression coil spring has a pitch angle of 5 to 10 degrees. Such a compression coil spring can be beneficially used in a tailgate opening / closing actuator of a car equipped with a trunk closing system.

[0022] Preferably, the steel wire used for helically winding the compression spring has a tensile strength R greater than the value calculated by the formula 2680-390.71*ln(d). m (MPa). More preferably, the steel wire has a tensile strength Rm (MPa) is higher than the value calculated by the formula 2720-390.71*ln(d); more preferably, higher than the value calculated by the formula 2770-390.71*ln(d); even more preferably, higher than the value calculated by the formula 2800-390.71*ln(d). The function "ln(d)" refers to the natural logarithm of the diameter d (mm) of the steel wire. The tensile test for measuring the mechanical properties of the steel wire is carried out in accordance with ISO 6892-1:2009, entitled "Metallic materials--Tensile testing--Part 1: Method of test at room temperature".

[0023] Preferably, the reduction rate of the fracture area Z in the tensile test of the steel wire used in the manufacture of the compression coil spring is greater than 40%. The reduction rate of the area Z is Z=100*(S o -S u ) / S o It is calculated as S o is the original cross section of the steel wire, and S u is the minimum cross section of the steel wire after fracture in the tensile test.

[0024] Preferably, the alloy steel contains 0.3-0.6 wt% Mn; or the alloy steel contains 0.6-0.9 wt% Mn.

[0025] Preferably, the steel wire comprises at least 95% by volume, more preferably at least 97% by volume, of elongated lamellar pearlite in the spring.

[0026] In a preferred embodiment, the volume percentage of bainite in the microstructure of the steel wire is between 0.2% and 2%, more preferably less than 0.5%. Such an embodiment has surprisingly been shown to be particularly beneficial for the present invention. It has been shown that when the microstructure contains such an amount of bainite, the lamellar pearlite is very fine, without the bainite having a detrimental effect, which is advantageous for achieving optimal spring formation and excellent mechanical spring properties. Limiting the amount of bainite is important for the ductility of the steel wire. The amount of bainite can be reduced by a suitable patenting step in the manufacturing process of the steel wire. The volume percentage of bainite in the microstructure of the wire can be determined by optical microscopy or scanning electron microscopy using a suitable etchant.

[0027] Optionally, a phosphate coating can be applied to the steel wire before the wire drawing process. The step of spirally winding the steel wire into a compression coil spring can then be carried out using the steel wire with the phosphate coating on its surface. Such an embodiment provides a better compression coil spring, as the phosphate coating facilitates the wire drawing and spring winding process. Thus, in a preferred embodiment, the spirally wound steel wire includes a phosphate coating. In a more preferred embodiment, a thermosetting coating layer or a coating layer including zinc and / or aluminum flakes in a binder (preferably an inorganic binder is used) is applied on the phosphate coating layer. In an even more preferred embodiment, the spirally wound steel wire is provided with a layer of flock. By flock is meant a layer of short textile fibers, e.g. polyamide fibers, bonded to the compression coil spring with an adhesive.

[0028] In a preferred embodiment, the helically wound steel wire comprises a metal coating layer. The metal coating layer comprises, and preferably consists of, at least 84 wt. % zinc; optionally aluminum, optionally 0.2-1 wt. % magnesium, and optionally up to 0.6 wt. % silicon. Such an embodiment has the advantage that the spring is easier to manufacture. Moreover, there is no need to apply an additional (i.e. post) coating to the compression coil spring to give the spring corrosion resistance. Moreover, such a metal coating avoids the need to apply a flocking layer to the helically wound compression spring. Such a flocking layer has the function of avoiding the generation of noise in the actuator for opening and closing the tailgate or door of the car when driving the car. The metal coating of the helically wound steel wire also prevents the generation of such noise. Preferably, the metal coating layer has a thickness of 40 g / m 2 More preferably, 80 g / m 2 More preferably, it is 120 g / m 2 The mass of the metal coating layer is expressed per unit surface area of ​​the steel wire.

[0029] It is known to apply a polymer coating to an already wound compression spring to provide the spring with corrosion resistance. Such an approach is carried out with prior art compression springs made from steel wire having a martensitic microstructure. Such a coating can be, for example, a thermosetting polymer coating (e.g., with an epoxy backbone or an acrylic backbone or a combination of an epoxy / acrylic backbone) or a coating with zinc flakes in a binder. By applying a metal coating layer to the steel wire before or during the drawing process and winding a compression spring with such a steel wire according to the present invention, the step of coating the spring with a thermosetting polymer coating or a coating with zinc or aluminum flakes in a binder can be eliminated.

[0030] In embodiments in which the helically wound steel wire includes a metal coating layer, preferably the metal coating layer provides a surface for the compression spring.

[0031] Optionally, when the helically wound steel wire includes metal coating layers, the metal coating layers include other active elements, each in an individual amount of less than 1% by weight.

[0032] Preferably, when the helically wound steel wire comprises a metallic coating layer, the metallic coating comprises at least 88 wt.% zinc, more preferably at least 90 wt.% zinc. More preferably, the metallic coating layer comprises at least 93 wt.% zinc.

[0033] Preferably, if the helically wound steel wire comprises a metal coating layer, the metal coating comprises, preferably consists of, zinc, at least 4 wt.% aluminium, preferably less than 14 wt.% aluminium; optionally 0.2-2 wt.% magnesium (preferably less than 0.8 wt.% Mg); optionally up to 0.6 wt.% silicon; optionally up to 0.1 wt.% rare earth elements, and unavoidable impurities.

[0034] Preferably, when the helically wound steel wire comprises a metallic coating layer, the metallic coating layer comprises, preferably consists of, 86-92 wt. % Zn and 14-8 wt. % Al; and unavoidable impurities. Preferably, such a metallic coating layer has a thickness of 35-60 g / m 2 It has a mass of.

[0035] Preferably, when the helically wound steel wire comprises a metallic coating layer, the metallic coating layer consists of zinc, 3-8 wt. % aluminum; optionally 0.2-1 wt. % magnesium; optionally up to 0.1 wt. % rare earth elements; and unavoidable impurities. Preferably, such a metallic coating layer has a thickness of 60-120 g / m 2 It has a mass of.

[0036] Preferably, when the helically wound steel wire comprises a metal coating layer, the metal coating layer consists of zinc, 3-8 wt.% aluminum; 0.2-2 wt.% (preferably less than 0.8 wt.%) Mg; and unavoidable impurities. It is a particular advantage that such a metal coating layer can be thin while having good corrosion protection properties. A thinner coating layer also makes it easier to wind the compression coil spring. Such a metal coating layer can have a thickness of, for example, 60 g / m 2 Preferably, the thickness is 25 to 60 g / m 2 It could be.

[0037] Preferably, when the spirally wound steel wire comprises a metal coating layer, the mass of the metal coating layer is 120 g / m 2 More preferably, the mass of the metal coating layer is 20 to 80 g / m 2 and more preferably, 60 g / m 2 less than 40 g / m2 of the surface of the compression spring, and even more preferably 2 is less than.

[0038] Preferably, when the helically wound steel wire includes a metal coating layer, the metal coating layer includes a spheroidized aluminum-rich phase. Such a spheroidized aluminum-rich phase is created in the drawing when the steel wire is heated by the drawing energy; and to a large extent, when the compression coil spring is subjected to a stress relief heat treatment after it is wound. The spheroidized aluminum-rich phase is believed to improve the corrosion resistance of the metal coating layer; as a result, a thinner metal coating layer can be used.

[0039] Preferably, when the helically wound steel wire comprises a metallic coating layer, the coated steel wire comprises an intermetallic coating layer provided between the steel wire and the metallic coating layer. The intermetallic coating layer is Fe x Al yphase. More preferably, the intermetallic coating layer provides 30-65% of the total thickness of the intermetallic coating layer and the metallic coating layer. The intermetallic layer is beneficial because it creates the necessary adhesion of the metallic coating layer to allow the steel wire to be wound into a compression coil spring without damaging the metallic coating layer. A thinner intermetallic coating layer runs the risk of providing flaking when winding the spring; a thicker coating runs the risk of poor coil formability. Fe x Al y Intermetallic coating layers containing Fe phases are obtained when applying metallic coating layers using a double dipping process. The first dipping is performed in a zinc bath. x Zinc y A layer is formed on the surface of the steel. The second immersion is carried out in a bath containing Zn and Al. In the second bath, the Fe layer formed in the first bath is removed. x Zinc y The layer is Fe x Al y The intermetallic coating layer is converted to a layer containing the phase.

[0040] Preferably, when the spirally wound steel wire comprises a metallic coating layer, the coated steel wire comprises an inhibitor layer. The inhibitor layer is provided between the steel wire and the metallic coating layer. The inhibitor layer is made of Fe x Al y phase. Preferably, the inhibition layer is less than 1 μm thick. Coated steel wires with such an inhibition layer can be obtained by using a single dipping process for applying the metallic coating layer. The surface of the steel is activated, for example via the Sendzimir process, in which the steel wire is dipped into a bath containing molten Zn and Al. After dipping in the bath, the steel wire is wiped off and cooled.

[0041] In a preferred embodiment, the helically wound steel wire comprises a metallic coating layer, which consists of zinc and unavoidable impurities. More preferably, the mass of such a metallic coating layer is less than 80 g / m 2 More preferably, 100 g / m 2 Exceeds.

[0042] In a preferred embodiment, the alloy steel contains 0.15 to 0.35 wt% Si, or the alloy steel contains 0.6 to 0.8 wt% Si, or the alloy steel contains 0.8 to 1.4 wt% Si.

[0043] In a more preferred embodiment where the spirally wound steel wire comprises a metal coating, the alloy steel comprises 0.6-1.4 wt% Si; more preferably 0.8-1.4 wt% Si. Such an embodiment is particularly beneficial when applying the metal coating in an intermediate step of the wire drawing process, since a high amount of Si prevents loss of strength of the steel wire in the hot dip galvanizing process, thus allowing a high strength coated steel wire to be obtained.

[0044] In a preferred compression coil spring, the alloy steel consists of 0.83-0.89 wt% C, 0.55-0.7 wt% Mn, 0.1-0.4 wt% Si, 0.15-0.3 wt% Cr, 0.04-0.08 wt% V, optionally 0.02-0.06 wt% Al; and unavoidable impurities and the balance iron.

[0045] In a preferred compression coil spring, the alloy steel consists of 0.83-0.89 wt% C, 0.55-0.7 wt% Mn, 0.55-0.85 wt% Si, 0.15-0.3 wt% Cr, 0.04-0.08 wt% V, optionally 0.2-0.06 wt% Al; and unavoidable impurities and the balance iron.

[0046] In a preferred compression coil spring, the alloy steel comprises 0.9-0.95 wt% C, 0.2-0.5 wt% Mn, 1.1-1.3 wt% Si, 0.15-0.3 wt% Cr; and unavoidable impurities and the balance iron.

[0047] In a preferred embodiment, the helically wound steel wire has a non-circular cross-section, preferably a rectangular or square cross-section. In the embodiment where the cross-section of the helically wound steel wire is non-circular, the diameter of this steel wire is an equivalent diameter. The equivalent diameter is the diameter of a wire with a circular cross-section having the same cross-sectional area as the wire with a non-circular cross-section.

[0048] Preferably, the steel wire of the compression spring has a stretch reduction of more than 75%. The wire from which the steel wire is stretched, or the steel wire itself, is subjected to a patenting process to create a pearlitic microstructure; and subsequently to a steel wire stretching process. The stretch reduction (%) is defined as 100*(A0-A1) / A0, where A0 is equal to the cross-sectional area of ​​the wire or steel wire after patenting and before stretching; A1 is equal to the cross-sectional area of ​​the stretched steel wire used to manufacture the spring. During the stretching deformation, the pearlite grains are oriented in the longitudinal direction of the steel wire. The orientation level of the pearlite grains is determined by the stretch reduction of the steel wire. The stretch reduction can be determined from the evaluation of the stretched lamellar pearlitic microstructure of the steel wire in the compression spring, for example, by optical microscopy in the longitudinal sections (i.e., along the longitudinal direction of the steel wire of the compression spring).

[0049] In a preferred compression coil spring, after 20,000 compression load cycles of a coil spring between 63% and 37% of its unloaded length, the load loss at 63% of the length is less than 5% (preferably less than 3%) compared to the load at 63% of the length on the first cycle.

[0050] A second aspect of the present invention is a method for making a compression coil spring as any of the embodiments of the first aspect of the present invention, the method comprising the steps of: - providing a steel wire rod, preferably having a diameter of 7 to 14 mm; - patenting the steel wire or a steel wire drawn from the steel wire in order to obtain a pearlitic microstructure; - drawing the patented steel wire rod having a pearlitic microstructure or the patented steel wire having a pearlitic microstructure with a drawing reduction of more than 75% to obtain a drawn steel wire having a pearlitic microstructure with a diameter d (mm) of 2 to 5 mm; - Winding the steel wire into a coil spring; Optionally, performing thermal stress relief on the coil spring.

[0051] The steel wire rod comprises an alloy steel consisting of 0.8-0.95 wt% C (preferably less than 0.93 wt% C, more preferably less than 0.9 wt% C); 0.2-0.9 wt% Mn; 0.1-1.4 wt% Si; 0.15-0.4 wt% Cr (preferably less than 0.35 wt% Cr, more preferably less than 0.3 wt% Cr); optionally, 0.04-0.2 wt% V (preferably less than 0.15 wt% V); optionally, 0.0005-0.008 wt% B; optionally, 0.02-0.06 wt% Al; unavoidable impurities; and the remainder iron. The alloy steel has a carbon equivalent greater than 1. The carbon equivalent is defined as follows: C wt%+(Mn wt% / 6)+(Si wt% / 5)+(Cr wt% / 5)+(V wt% / 5).

[0052] In a preferred method, the drawing step produces a wire having a diameter d (mm) of 2 to 5 mm and a tensile strength R m More preferably, the drawing results in a steel wire having a tensile strength R MPa higher than the value calculated by the formula 2680-390.71*ln(d). More preferably, the drawing results in a steel wire having a tensile strength R MPa higher than the value calculated by the formula 2720-390.71*ln(d); more preferably, the drawing results in a steel wire having a tensile strength R MPa higher than the value calculated by the formula 2770-390.71*ln(d); even more preferably, the drawing results in a steel wire having a tensile strength R MPa higher than the value calculated by the formula 2800-390.71*ln(d). m(MPa). The function "ln(d)" means the natural logarithm of the wire diameter d (mm). The tensile tests for determining the mechanical properties of the steel wire are carried out according to ISO 6892-1:2009 entitled "Metallic materials--Tensile testing--Part 1: Method of test at room temperature".

[0053] The patenting step to obtain a pearlitic microstructure can be performed on the wire rod or on the steel wire drawn from the wire rod. The patenting step can be performed as an in-line step in the wire rod manufacturing process, for example via direct in-line patenting. The patenting step can also be performed on the wire rod or on the steel wire drawn from the wire rod via known patenting techniques, using either a suitable molten metal bath (such as Pb) or alternatives such as fluidized beds, molten salts, and water-based polymers. Prior to the drawing of the wire, pickling and wire coating steps can be performed.

[0054] Optionally, a phosphate coating can be applied to the steel wire prior to the wire drawing process. The step of helically winding the steel wire into a coil spring can then be carried out with the steel wire including the phosphate coating on its surface. Such an embodiment provides a better compression coil spring since the phosphate coating facilitates the wire drawing and spring winding process.

[0055] Preferably, after the patenting process and before or during the drawing step, a metal coating is applied to the steel wire by a hot dip galvanizing process. The metal coating comprises at least 84% by weight of zinc; and optionally aluminium.

[0056] Preferably, the method of making the helical compression spring includes a step of thermally relieving the helical compression spring after it has been wound. More preferably, the thermal stress relieving heat treatment step is carried out on the helical compression spring after its formation at a temperature of less than 450° C. More preferably, the stress relieving heat treatment step is carried out at a temperature of less than 300° C., more preferably less than 250° C.

[0057] Optionally, after stress relaxation, other process steps, such as hot hardening or multiple low temperature cures, can be applied to the compression coil spring. Hot hardening means that the spring is kept in compression at high temperature for some time. Low temperature cure means that the spring is compressed for several cycles at room temperature. Such hardening steps allow the spring to achieve more strictly limited spring relaxation requirements.

[0058] A third aspect of the present invention is an actuator for opening or closing a vehicle door or tailgate. The actuator comprises a compression coil spring according to any of the embodiments of the first aspect of the present invention for opening a vehicle door or tailgate when the compression force of the compression coil spring is released; and a motor. The motor is provided for compressing the compression coil spring to close the vehicle door or tailgate. Preferably, the actuator comprises two connectors, one for connecting the actuator to the door or tailgate; and another for connecting the actuator to a vehicle body.

[0059] In a preferred actuator, the spirally wound steel wire comprises a metal coating layer containing at least 84% by weight of zinc. More preferably, the metal coating layer provides the surface of the compression coil spring. Such an embodiment has the advantage that noise in the actuator is prevented when driving the car. In prior art actuators for opening and closing car doors or tailgates, it is common practice to apply a flock layer to the compression coil spring: after winding the spring, a layer of short textile fibers (e.g. polyamide fibers) is glued to the compression coil spring by an adhesive; in this way a velvet layer is formed that acts as a noise damping for the tightly compressed spring in the actuator. The use of a metal coating layer has been shown to eliminate the need to apply a flock layer to the compression coil spring. [Brief description of the drawings]

[0060] [Figure 1] An SUV is shown equipped with an actuator for opening and closing the tailgate. [Diagram 2] 1 shows an actuator for opening and closing a vehicle tailgate. [Diagram 3] 1 shows a compression coil spring according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0061] [Table 1]

[0062] FIG. 1 shows an SUV 12 with a tailgate 14 and an actuator 16 for opening and closing the tailgate. The actuator 16 (FIG. 2 shows the actuator 16 for opening and closing the tailgate of the vehicle) comprises a compression coil spring 18 and a motor 20. The actuator comprises two connectors 22, 23, one for connecting the actuator to the door or tailgate; the other for connecting the actuator to the vehicle body. A compression coil spring is provided for opening the tailgate when the compression force of the compression coil spring is released. A motor is provided for compressing the compression coil spring for closing the tailgate. An example of a compression coil spring that can be used is shown in FIG. 3, such a spring has a length L and a pitch p.

[0063] Compression springs consist of a spirally wound steel wire with a diameter d (mm) of 2 to 5 mm.

[0064] Table I provides specific examples of steel alloys that can be used in the steel core of the present invention (along with the minimum and maximum wt% of the elements in the steel alloys). The microstructure of the steel wire in the spirally wound steel wire is elongated lamellar pearlite.

[0065] A particular example of such a coiled compression spring is wound with a steel wire having a drawn pearlitic microstructure and a diameter of 3.4 mm. The coiled compression spring has a length L of 0.8 m in the unloaded state. The spring index of the exemplary coiled spring is 6.5. The spring pitch p is 15.2 mm. The outer diameter of the coiled compression spring is 26.8 mm. However, although not essential to the invention, the steel wire was provided with a metal coating layer including zinc and aluminum.

[0066] A steel wire rod with a diameter of 10 mm was used to manufacture the steel wire used to wind the compression coil springs.

[0067] The steel wire rod was made from an alloy steel consisting of 0.86 wt% C, 0.63 wt% Mn, 0.2 wt% Si, 0.22 wt% Cr, 0.06 wt% V; 0.04 wt% Al; unavoidable impurities and the balance Fe. This is alloy "A" of Table I. The carbon equivalent is 0.86 + (0.63 / 6) + (0.2 / 5) + (0.22 / 5) + (0.06 / 5) = 1.169.

[0068] A steel wire rod of 10 mm diameter was patented to provide it with a pearlitic microstructure; and, although not essential to the invention, was then provided with a metallic coating via a hot-dip galvanizing process. The hot-dip galvanizing process used was a double dipping process in which the steel wire was first immersed in a bath of molten zinc; and then the steel wire was immersed in a bath containing 10 wt. % aluminum and the remainder zinc. The metallic coating layer of the hot-dip galvanized steel wire consisted of 10 wt. % aluminum and the remainder zinc.

[0069] The patented hot-dip galvanized wire with a diameter of 10 mm was drawn to a steel wire with a diameter of 3.4 mm. This means that a reduction in drawing of 88.4% was applied. The resulting steel wire has a drawn pearlitic microstructure. The tensile strength Rm of the steel wire is 2354 MPa; the Rp0.2 value is 1990 MPa, which is 84.5% of the Rm value. The reduction in the fracture area Z in the tensile test of the steel wire is 44.1%.

[0070] Metal coating on 3.4mm drawn wire is 45g / m 2 It was.

[0071] After the coated steel wire was wound into a compression spring, a thermal stress relaxation step was carried out, for example, by keeping the compression spring in an unloaded state at 250° C. for 30 minutes.

[0072] The coated steel wire included an intermetallic coating layer between the steel core and the metallic coating layer. The intermetallic coating layer provided 45% of the total thickness of the intermetallic coating layer and the metallic coating layer. The intermetallic coating layer was made of Fe x Al y The metal coating layer was observed to contain a spheroidized aluminum-rich phase.

[0073] The steel wire samples used to make the coil springs were heat treated in an oven for 30 minutes at an oven temperature of 250°C. After this heat treatment, the steel wire samples were tensile tested. The tensile strength Rm was 2426 MPa; the Rp0.2 value was 2366 MPa, which was 97.5% of the tensile strength Rm; and the reduction rate of the fracture area Z was 42%.

[0074] Analysis of the steel wire for the compression springs showed that the steel had an elongated pearlitic microstructure with over 97% by volume elongated pearlite and approximately 1% by volume bainite.

[0075] Compression springs were used in actuators for vehicle tailgate opening and closing actuators. The metallic coating of coated steel wire provided the surface of the compression spring.

Claims

1. A compression coil spring for use in an actuator for opening and closing a door or tailgate of a vehicle, comprising: The compression coil spring has an outer diameter of 15 to 50 mm; the compression spring includes a helically wound steel wire; The diameter d (mm) of the steel wire is 2 to 5 mm, The steel wire comprises an alloy steel, the alloy steel comprising: 0.8-0.95 wt.% C; 0.2-0.9 wt.% Mn; 0.1-1.4 wt.% Si; 0.15-0.4 wt.% Cr; Optionally, 0.04 to 0.2 wt % V; optionally 0.0005 to 0.008 wt % B; Optionally, 0.02-0.06 wt % Al; unavoidable impurities; and Remaining iron; It consists of: The alloy steel has a carbon equivalent greater than 1; The carbon equivalent is defined as C wt% + (Mn wt% / 6) + (Si wt% / 5) + (Cr wt% / 5) + (V wt% / 5); The microstructure of the steel wire of the compression spring is greater than 97% by volume of elongated lamellar pearlite. Compression coil spring.

2. 2. The compression coil spring according to claim 1, wherein the steel wire used for helically winding the compression coil spring has a tensile strength Rm (MPa) higher than a value calculated by the formula 2680-390.71*ln(d).

3. 3. The compression coil spring according to claim 1, wherein the alloy steel contains 0.2 to 0.6 wt % Mn, or the alloy steel contains 0.6 to 0.9 wt % Mn.

4. The compression coil spring according to any one of claims 1 to 3, wherein the microstructure of the steel wire of the compression coil spring comprises 0.2 to 2 volume % bainite.

5. 5. The compression spring of claim 1, wherein the helically wound steel wire comprises a phosphate coating.

6. the helically wound steel wire includes a metal coating layer; The compression coil spring according to any one of claims 1 to 4, wherein the metal coating layer comprises at least 84% by mass of zinc and aluminum.

7. 7. The compression coil spring according to claim 6, wherein the metal coating layer comprises at least 86% by weight of zinc; and 4-14% by weight of aluminum; and optionally magnesium and / or silicon.

8. 7. The compression coil spring according to claim 6, wherein the metal coating layer consists of zinc, 3-8 wt. % aluminum, optionally 0.2-1 wt. % Mg, optionally up to 0.1 wt. % rare earth elements, and unavoidable impurities.

9. The alloy steel contains 0.15 to 0.35 wt % Si, or the alloy steel contains 0.6 to 0. The compression coil spring according to any one of claims 1 to 8, wherein the alloy steel contains 0.8 to 1.4 wt% Si, or the alloy steel contains 8 wt% Si.

10. The alloy steel contains 0.83 to 0.89 wt % C, 0.55 to 0.7 wt % Mn, 0.

10. The compression coil spring according to any one of claims 1 to 9, consisting of 1 to 0.4 wt% Si, 0.15 to 0.3 wt% Cr, 0.04 to 0.08 wt% V, optionally 0.02 to 0.06 wt% Al; unavoidable impurities and the remainder iron.

11. A method for producing a compression coil spring according to any one of claims 1 to 10, comprising the steps of: - providing a steel wire; - patenting the steel wire or a steel wire drawn from the steel wire to obtain a pearlitic microstructure; - drawing the patented steel wire rod having a pearlitic microstructure or the patented steel wire having a pearlitic microstructure with a drawing reduction of more than 75%; thereby obtaining a drawn steel wire having a pearlitic microstructure with a diameter d (mm) of 2-5 mm; - spirally winding the steel wire into a coil spring; - optionally comprising the step of subjecting said coil spring to thermal stress relief; The steel wire comprises an alloy steel, 0.8-0.95 wt.% C; 0.2-0.9 wt.% Mn; 0.1-1.4 wt.% Si; 0.15-0.4 wt.% Cr; Optionally, 0.04 to 0.2 wt % V; optionally 0.0005 to 0.008 wt % B; Optionally, 0.02-0.06 wt % Al; Inevitable impurities; and the remainder iron, the alloy steel having a carbon equivalent greater than 1; The carbon equivalent is defined as C wt% + (Mn wt% / 6) + (Si wt% / 5) + (Cr wt% / 5) + (V wt% / 5); method.

12. 12. The method according to claim 11, wherein said drawing step results in a steel wire having a diameter d (mm) between 2 and 5 mm and a tensile strength Rm (MPa) higher than the value calculated by the formula 2680-390.71*ln(d).

13. 13. The method according to claim 11 or 12, wherein after the patenting step and before or during the drawing step, a metal coating is applied to the steel wire by a hot dip galvanizing method, said metal coating comprising at least 84% by weight of zinc and optionally aluminium.

14. An actuator for opening and closing a door or tailgate of a vehicle, comprising: - a compression coil spring according to any one of claims 1 to 10 for opening a door or a tailgate of a vehicle when the compression force of said compression coil spring is released; a motor for compressing said compression coil spring to close the door or tailgate of said vehicle; An actuator including:

Citation Information

Patent Citations

  • Production of steel wire having excellent spring workability

    JP1983138513A

  • High fatigue strength steel wire and spring, and their production

    JP1999140589A

  • Coil spring and method of manufacturing the same

    JP2012077367A

  • Coil spring and production method thereof

    JP2015017288A

  • Wire for diagonal winding spring, diagonal winding spring and method for producing the same

    JP2017218659A