Polytetrafluoroethylene film and its manufacturing method
A PTFE film with controlled tensile strength and heat shrinkage rates, produced through specific molding and calendering processes, addresses the challenge of achieving high strength and low shrinkage, enhancing its performance in high-temperature environments.
Patent Information
- Application Number
- JP2021569209
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-06-21
- Filing Date
- 2020-04-09
- Publication Date
- 2024-09-25
- Estimated Expiration
- 2040-04-09
AI Technical Summary
Conventional polytetrafluoroethylene (PTFE) films face a challenge in achieving high strength and low shrinkage simultaneously, limiting their application and service life.
The PTFE film is produced with specific tensile strength and heat shrinkage rates within defined ranges, combined with controlled calendering processes to achieve high strength and low thermal shrinkage, using polytetrafluoroethylene powder molding, cutting, and calendering at controlled temperatures.
The resulting PTFE film exhibits high strength, low thermal shrinkage, and excellent abrasion resistance, suitable for high-temperature applications, with a simple and efficient production method.
Smart Images

Figure 0007555969000001 
Figure 0007555969000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a polytetrafluoroethylene film, a method for producing the polytetrafluoroethylene film, and a pressure-sensitive adhesive tape containing the polytetrafluoroethylene film. [Background technology]
[0002] It is known that various PTFE films can be obtained by using polytetrafluoroethylene (PTFE) and cutting after melt molding or calendering after extrusion molding. These known PTFE films are widely used in various fields, and can be used, for example, as a substrate for adhesive tape. However, the PTFE films obtained by conventional cutting after melt molding or calendering after extrusion molding have a problem that they cannot achieve both high strength and low shrinkage, and films with high strength and high shrinkage or low strength and low shrinkage are common, so the application and service life of PTFE films are significantly limited. Summary of the Invention [Problem to be solved by the invention]
[0003] In view of the above circumstances, the present invention aims to provide a PTFE film having high strength and low shrinkage, a method for producing the PTFE film, and an adhesive tape containing the PTFE film. The PTFE film of the present invention has high abrasion resistance and high strength, and can suppress shrinkage at high temperatures. In addition, the method for producing the PTFE film of the present invention is simple and easy to carry out, and has high production efficiency. [Means for solving the problem]
[0004] As a result of intensive research into the above problems, the inventors have found that the above problems can be solved by setting the tensile strength in the machine direction (MD) of the PTFE film and the thermal shrinkage rate in the machine direction (MD) after heating at 200°C for 30 minutes within specific ranges, and have thus completed the present invention.
[0005] That is, the present invention is as follows. [1] A polytetrafluoroethylene film having a tensile strength in the machine direction (MD) of 100 MPa or more and a heat shrinkage rate in the machine direction (MD) of 10% or less after heating at 200°C for 30 minutes. [2] The polytetrafluoroethylene film according to [1], having a thickness of 15 to 150 μm. [3] The polytetrafluoroethylene film according to [1] or [2], having a melting enthalpy of 25 kJ / kg or less. [4] Molding the polytetrafluoroethylene powder to obtain a molded product; The molded product is cut into a film to obtain a cut film. The method for producing a polytetrafluoroethylene film according to any one of [1] to [3], comprising: calendaring the cut film at a temperature lower than the melting point of polytetrafluoroethylene to obtain a polytetrafluoroethylene film. [5] The method according to [4], wherein the cutting film has a thickness of 30 to 300 μm. [6] The method according to [4] or [5], wherein the thickness ratio between the cut film and the polytetrafluoroethylene film, i.e., the thickness ratio between the cut film before calendar processing and the polytetrafluoroethylene film after calendar processing, is 5 / 1 to 1.5 / 1. [7] The method according to [6], wherein the calendaring is carried out in one or more stages. [8] The method according to [4] or [5], wherein the cut film is calendered at 230 to 310°C. [9] An adhesive tape comprising the polytetrafluoroethylene film according to any one of [1] to [3] as a substrate.
[10] An adhesive tape comprising, as a substrate, a polytetrafluoroethylene film obtained by the production method according to any one of [4] to [8]. Effect of the Invention
[0006] The PTFE film of the present invention can increase the strength of the film, effectively suppress heat shrinkage, and has the advantages of excellent flatness and high abrasion resistance, etc., and is particularly suitable for use in high temperature regions. In addition, the method for producing the PTFE film of the present invention is simple and easy to carry out, and has high production efficiency. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] The PTFE film of the present invention has a tensile strength in the machine direction (MD) of 100 MPa or more, preferably 100 to 200 MPa, and more preferably 130 to 200 MPa. By setting the tensile strength in the machine direction (MD) of the PTFE film within the above range, it is possible to increase the strength and impact resistance. If the tensile strength in the machine direction (MD) of the PTFE film is less than 100 MPa, the strength is insufficient, and the PTFE film is likely to deform or break, which limits the application of the PTFE film. The above "machine direction (MD)" usually means the longitudinal direction (longitudinal direction) of the PTFE film. The "tensile strength in the machine direction (MD)" is measured by the method described in the Examples of this specification.
[0008] The heat shrinkage at 200°C is an index showing the structural stability of the PTFE film at high temperatures, and the lower the value, the more stable the structure and the more suitable it is from the viewpoint of the application of the film. In the present invention, the heat shrinkage in the machine direction (MD) of the PTFE film after heating at 200°C for 30 minutes is 10% or less, preferably 7% or less, and more preferably 5% or less. By setting the heat shrinkage in the above range, the shrinkage of the PTFE film can be suppressed even at high temperatures, and a PTFE film having excellent structural stability can be obtained. If the heat shrinkage in the machine direction (MD) of the PTFE film after heating at 200°C for 30 minutes exceeds 10%, the effect of suppressing heat shrinkage becomes insufficient, and the effect of improving the dimensional stability of the PTFE film cannot be obtained. The heat shrinkage is measured by the method described in the examples of this specification.
[0009] In the present invention, the thickness of the PTFE film is 15 to 150 μm, and preferably 50 to 100 μm. By making the thickness of the PTFE film within the above range, a PTFE film with high strength and high abrasion resistance can be provided.
[0010] According to the present invention, the melting enthalpy of the PTFE film is 25 kJ / kg or less, preferably 22 kJ / kg or less. The melting enthalpy is an index of crystallinity, and research has revealed that the lower the crystallinity of the PTFE film, the higher the flexibility of the film. If the melting enthalpy of the PTFE film exceeds 25 kJ / kg, the flexibility of the PTFE film will be poor. In the present invention, the "melting enthalpy" means the melting enthalpy measured in the temperature range of 270 to 345°C.
[0011] According to another embodiment of the present invention, Molding the polytetrafluoroethylene powder to obtain a molded product; The molded product is cut into a film to obtain a cut film. calendering the cut film at a temperature lower than the melting point of polytetrafluoroethylene to obtain a polytetrafluoroethylene film; Further provided is a method for producing a polytetrafluoroethylene film comprising:
[0012] By molding the polytetrafluoroethylene powder, the gas between the polytetrafluoroethylene powder particles is removed, and the polytetrafluoroethylene powder particles are melted and integrated to obtain a molded body. The obtained molded body can be processed into molded bodies of various sizes, for example, into cylinders of various sizes, within a range that does not impair the effects of the present invention.
[0013] The polytetrafluoroethylene powder is not particularly limited, and commercially available products may be used. Depending on the manufacturing method of each manufacturer, the polytetrafluoroethylene powder may contain a small amount of at least one of perfluoroalkoxyalkane (PFA), perfluoroethylene-propylene copolymer (FEP), ethylene-tetrafluoroethylene copolymer (ETFE), and polyvinylidene fluoride (PVDF).
[0014] The molding temperature of the polytetrafluoroethylene powder is not particularly limited, but it is preferable to mold the polytetrafluoroethylene powder at a temperature of 360 to 390° C. If the sintering temperature is too high, the decomposition of PTFE is accelerated and toxic gas is generated.
[0015] The molding time for the polytetrafluoroethylene powder is not particularly limited, but is usually, for example, 10 to 20 hours. The molding time may be appropriately adjusted depending on the molding temperature.
[0016] The molding method is not particularly limited, but molding can be performed using, for example, a hydraulic press or a sintering furnace.
[0017] The method for cutting into a film is not particularly limited, but for example, a molded product can be cut by a precision CNC lathe to produce PTFE films of various thicknesses.
[0018] The thickness of the cut film is 30 to 500 μm, preferably 30 to 300 μm, and more preferably 75 to 300 μm. The thickness of the cut film is in the above range, which is advantageous in forming the PTFE film of the present invention having high strength and suppressed shrinkage. If the thickness of the cut film is less than 30 μm, the processing performance is affected. If the thickness of the cut film is more than 500 μm, the practical performance of the PTFE film is limited.
[0019] In the present invention, the temperature is one of the important conditions in the calendering of the cut film at a temperature lower than the melting point of polytetrafluoroethylene. The calendering temperature is not particularly limited as long as it is lower than the melting point of polytetrafluoroethylene, but it is preferable to calender the cut film at 230 to 310°C, and more preferably to calender the cut film at 250 to 300°C. By setting the temperature within the above range, a PTFE film having high strength and low heat shrinkage can be obtained.
[0020] The calendering speed of the cut film is not particularly limited, but may be, for example, 0.5 to 5 m / min. The calendering speed may be appropriately adjusted according to the setting of the calendering temperature.
[0021] In the present invention, the thickness ratio of the cut film to the polytetrafluoroethylene film, i.e., the thickness ratio of the cut film before calendaring to the polytetrafluoroethylene film after calendaring, is 5 / 1 to 1.5 / 1, more preferably 5 / 1 to 2 / 1, and even more preferably 4 / 1 to 2 / 1. By setting the thickness ratio within the above range, a PTFE film having high strength can be obtained. If the thickness ratio is too high, the PTFE film is prone to burst defects, resulting in a problem of non-uniform structure. On the other hand, if the thickness ratio is too low, the strength of the PTFE film is reduced.
[0022] In the present invention, the calendering can be carried out in one or more stages so as to obtain a desired thickness ratio between the cut film and the polytetrafluoroethylene film.Within the scope of the present invention, the high thickness ratio step can be divided into a plurality of low thickness ratio steps.For example, the cut film can be subjected to a calendering process with a thickness ratio of 1.5 / 1, and then further subjected to a calendering process with a thickness ratio of 2 / 1, so that the thickness ratio between the cut film and the polytetrafluoroethylene film finally obtained is 3 / 1.
[0023] The device used for the calendering is not particularly limited as long as it can achieve the calendering temperature and thickness ratio required in the present invention. For example, calender rolls made of various materials and high-precision mirror rolls can be used.
[0024] The method for producing the PTFE film of the present invention may include steps other than the above steps, such as a step of preliminary press molding, as long as the effects of the present invention are not impaired.
[0025] According to another aspect of the present invention, there is provided an adhesive tape comprising, as a substrate, the PTFE film of the present invention, or a adhesive tape comprising, as a substrate, the PTFE film obtained by the method for producing a PTFE film of the present invention.
[0026] The PTFE film of the present invention can be used as a substrate and can be used to manufacture various adhesive tapes. For example, the adhesive tape of the present invention preferably includes a PTFE film as a substrate and an adhesive layer.
[0027] The pressure-sensitive adhesive tape of the present invention can be produced by any suitable method as long as the effect of the present invention is not impaired. For example, a method of forming a pressure-sensitive adhesive layer on a substrate by applying a composition that is a pressure-sensitive adhesive layer-forming material to the substrate can be used. Examples of such application methods include roll coating, gravure coating, reverse coating, roll brushing, spray coating, air knife coating, extrusion coating using a die coater, etc.
[0028] In addition, the PTFE film as the substrate may be subjected to any suitable surface treatment depending on the purpose. For example, the surface of the substrate may be subjected to a known or general suitable surface treatment such as a corona discharge treatment, a plasma treatment, or a primer treatment.
[0029] As the material of the adhesive layer, any appropriate adhesive can be used as long as the effects of the present invention are not impaired. For example, adhesives conventionally used for the adhesive layer of tapes can be mentioned, such as acrylic adhesives, rubber adhesives, polysiloxane adhesives, etc. From the viewpoint of the heat resistance of the tape, it is preferable to use an adhesive layer mainly composed of a polysiloxane adhesive.
[0030] When using a polysiloxane adhesive for the above adhesive layer, any appropriate polysiloxane adhesive can be used. As such a polysiloxane adhesive, it is preferable to use an adhesive obtained by blending or aggregating polysiloxane resins (polysiloxane-based polymers, polysiloxane components).
[0031] In addition, examples of the above polysiloxane-based adhesives include addition reaction curable polysiloxane-based adhesives and peroxide curable polysiloxane-based adhesives. Among these polysiloxane-based adhesives, addition reaction curable polysiloxane-based adhesives are preferable from the viewpoint of not using peroxides (such as benzoyl peroxide) and not generating decomposition products.
[0032] As the curing reaction of the above addition reaction curable polysiloxane-based adhesive, for example, when trying to obtain a polyalkylpolysiloxane-based adhesive, a method of curing a polyalkylhydroxysiloxane composition with a platinum catalyst is generally mentioned.
[0033] The thickness of the adhesive layer is not particularly limited, but for example, it is preferably 5 to 100 μm, and more preferably 10 to 60 μm.
Examples
[0034] Hereinafter, the present invention will be described in detail by way of examples, but the present invention is not limited to the examples. The test and evaluation methods in the examples and the like are as follows.
[0035] <Tensile strength in the longitudinal direction (MD) of the PTFE film> In accordance with GB / T 1040.3-2006, the tensile strength in the MD direction (longitudinal direction) of the PTFE films obtained in each example and comparative example was measured using a tensile testing machine (AG-X plus, manufactured by Shimadzu Corporation) at a tensile speed of 200 mm / min. The measurement results are shown in Tables 1 and 2.
[0036] <Tensile strength in the longitudinal direction (MD) of the adhesive tape> In accordance with GB / T 30776-2014, the tensile strength in the MD direction (longitudinal direction) of the adhesive tape was measured using a tensile testing machine (AG-X plus, manufactured by Shimadzu Corporation) at a tensile speed of 300 mm / min. The measurement results are shown in Table 2.
[0037] <Thermal shrinkage rate> In accordance with GB / T 12027-2004, the PTFE film and the adhesive tape were cut into film samples (test pieces) of 120 mm × 120 mm, marked with a length of 100 mm × 100 mm, held under heating at 200 °C for 30 minutes, then held at room temperature for 30 minutes. The dimensions of the marked area in the MD direction of the test pieces before and after heating were measured with a vernier caliper, and the thermal shrinkage rate was determined by the following formula. Thermal shrinkage rate (%) = [[(Length before heating (mm) - Length after heating (mm)) / Length before heating (mm)]] × 100
[0038] <Melting enthalpy> The melting enthalpy was determined by differential scanning calorimetry (DSC measurement) in accordance with GB / T 19466.3-2004. Specifically, the melting enthalpy was determined using a differential scanning calorimeter (DSC 8000, manufactured by PerkinElmer). After heating from room temperature to 380 °C at 20 °C / min, it was cooled to room temperature at 20 °C / min, and the melting enthalpy of the PTFE film was measured based on the thermogram during heating in accordance with GB / T 19466.3-2004.
[0039] <Evaluation of the thermal shrinkage properties of the PTFE film and the adhesive tape> When the thermal shrinkage rate in the MD direction of the PTFE film and the adhesive tape exceeds 10%, the thermal shrinkage property evaluation is marked as "×". When the heat shrinkage rate in the MD direction of the PTFE film and the adhesive tape is more than 7% and less than or equal to 10%, the heat shrinkage property evaluation is "△". When the heat shrinkage rate in the MD direction of the PTFE film and the adhesive tape is more than 5% and less than or equal to 7%, the heat shrinkage property evaluation is "〇". When the heat shrinkage rate in the MD direction of the PTFE film and the adhesive tape is less than or equal to 5%, the heat shrinkage property evaluation is "◎".
[0040] <Evaluation of the breaking resistance of the PTFE film> When the tensile strength in the MD direction of the PTFE film is less than 100 MPa, the breaking resistance evaluation is "×". When the tensile strength in the MD direction of the PTFE film is 100 MPa or more and 130 MPa or less, the breaking resistance evaluation is "〇". When the tensile strength in the MD direction of the PTFE film is more than 130 MPa and less than or equal to 200 MPa, the breaking resistance evaluation is "◎".
[0041] <Evaluation of the breaking resistance of the adhesive tape> When the tensile strength in the MD direction of the adhesive tape is less than 60 N / cm, the breaking resistance evaluation is "×". When the tensile strength in the MD direction of the adhesive tape is 60 N / cm or more and 80 N / cm or less, the breaking resistance evaluation is "〇". When the tensile strength in the MD direction of the adhesive tape is more than 80 N / cm and less than or equal to 120 N / cm, the breaking resistance evaluation is "◎".
[0042] [Example 1] PTFE powder (62X, manufactured by DuPont) was sintered in a sintering furnace at 380 °C for 15 hours to obtain a molded body. Then, the obtained molded body was machined by a precision CNC lathe to obtain a cut film with a thickness of 180 μm. Next, the obtained cut film was calendered at 240 °C at a calendering speed of 1.5 m / min to obtain a PTFE film with a thickness of 60 μm. The thickness ratio of the cut film to the PTFE film, that is, the thickness ratio of the cut film before calendering to the calendered PTFE film, was 3 / 1.
[0043] [Example 2] PTFE powder (62X, DuPont) was molded in a sintering furnace at 380°C for 15 hours to obtain a molded body. The molded body was then cut using a precision CNC lathe to obtain a cut film having a thickness of 240 μm. The cut film was then calendered at 240°C at a calendering speed of 1.5 m / min to obtain a PTFE film having a thickness of 60 μm. The thickness ratio of the cut film to the PTFE film, i.e., the thickness ratio of the cut film before calendering to the calendered PTFE film, was 4 / 1.
[0044] [Example 3] PTFE powder (62X, DuPont) was molded in a sintering furnace at 380°C for 15 hours to obtain a molded body. The molded body obtained was then cut using a precision CNC lathe to obtain a cut film having a thickness of 240 μm. The cut film obtained was then calendered at 260°C at a calendering speed of 1.5 m / min to obtain a PTFE film having a thickness of 60 μm. The thickness ratio of the cut film to the PTFE film, i.e., the thickness ratio of the cut film before calendering to the calendered PTFE film, was 4 / 1.
[0045] [Example 4] PTFE powder (62X, DuPont) was molded in a sintering furnace at 380°C for 15 hours to obtain a molded body. The molded body was then cut using a precision CNC lathe to obtain a cut film having a thickness of 300 μm. The cut film was then calendered at 300°C at a calendering speed of 1.5 m / min to obtain a PTFE film having a thickness of 60 μm. The thickness ratio of the cut film to the PTFE film, i.e., the thickness ratio of the cut film before calendering to the calendered PTFE film, was 5 / 1.
[0046] [Comparative Example 1] PTFE powder (62X, DuPont) was molded in a sintering furnace at 380°C for 15 hours to obtain a molded body. The molded body was then cut using a precision CNC lathe to obtain a cut film having a thickness of 240 μm. The cut film was then calendered at 150°C at a calendering speed of 1.5 m / min to obtain a PTFE film having a thickness of 60 μm. The thickness ratio of the cut film to the PTFE film, i.e., the thickness ratio of the cut film before calendering to the calendered PTFE film, was 4 / 1.
[0047] [Comparative Example 2] PTFE powder (62X, DuPont) was molded in a sintering furnace at 380°C for 15 hours to obtain a molded body. The molded body was then cut using a precision CNC lathe to obtain a cut film with a thickness of 90 μm. The cut film was then calendered at 150°C at a calendering speed of 1.5 m / min to obtain a PTFE film with a thickness of 60 μm. The thickness ratio of the cut film to the PTFE film, i.e., the thickness ratio of the cut film before calendering to the calendered PTFE film, was 1.5 / 1.
[0048] [Example 5] PTFE powder (62X, DuPont) was molded in a sintering furnace at 380°C for 15 hours to obtain a molded body. The molded body obtained was then cut using a precision CNC lathe to obtain a cut film having a thickness of 180 μm. The cut film obtained was then calendered at a calendering speed of 1.5 m / min at 240°C to obtain a PTFE film having a thickness of 60 μm. The thickness ratio of the cut film to the PTFE film, i.e., the thickness ratio of the cut film before calendering to the calendered PTFE film, was 3 / 1. The above obtained PTFE film was used as a substrate, and silica gel (DOWSIL 7657 Adhesive, manufactured by Dow) was applied onto the substrate to form an adhesive layer with a thickness of 30 μm, thereby obtaining an adhesive tape.
[0049] [Example 6] PTFE powder (62X, DuPont) was molded in a sintering furnace at 380°C for 15 hours to obtain a molded body. The molded body obtained was then cut using a precision CNC lathe to obtain a cut film having a thickness of 240 μm. The cut film obtained was then calendered at 260°C at a calendering speed of 1.5 m / min to obtain a PTFE film having a thickness of 60 μm. The thickness ratio of the cut film to the PTFE film, i.e., the thickness ratio of the cut film before calendering to the calendered PTFE film, was 4 / 1. The above obtained PTFE film was used as a substrate, and silica gel (DOWSIL 7657 Adhesive, manufactured by Dow) was applied onto the substrate to form an adhesive layer with a thickness of 30 μm, thereby obtaining an adhesive tape.
[0050] [Example 7] PTFE powder (62X, DuPont) was molded in a sintering furnace at 380°C for 15 hours to obtain a molded body. The molded body was then cut using a precision CNC lathe to obtain a cut film having a thickness of 300 μm. The cut film was then calendered at 300°C at a calendering speed of 1.5 m / min to obtain a PTFE film having a thickness of 60 μm. The thickness ratio of the cut film to the PTFE film, i.e., the thickness ratio of the cut film before calendering to the calendered PTFE film, was 5 / 1. The above obtained PTFE film was used as a substrate, and silica gel (DOWSIL 7657 Adhesive, manufactured by Dow) was applied onto the substrate to form an adhesive layer with a thickness of 30 μm, thereby obtaining an adhesive tape.
[0051] [Table 1]
[0052] [Table 2]
[0053] From the above results, it was found that by controlling the tensile strength in the machine direction (MD) of the PTFE film and the thermal shrinkage rate in the machine direction (MD) after heating at 200°C for 30 minutes within a specific range, the strength of the PTFE film can be increased and the thermal shrinkage can be effectively suppressed, resulting in a PTFE film that has both high strength and low thermal shrinkage. Therefore, the PTFE film of the present invention is particularly suitable for use in high temperature regions.
[0054] On the other hand, in Comparative Examples 1 and 2, either the tensile strength in the machine direction (MD) of the PTFE film or the heat shrinkage rate in the machine direction (MD) after heating at 200°C for 30 minutes was outside the range of the present invention, so the obtained PTFE film had poor strength or heat shrinkability, and a PTFE film having both high strength and low shrinkage rate was not obtained.
Claims
1. The tensile strength in the machine direction (MD) is 100 MPa or more, and the heat shrinkage rate in the machine direction (MD) after heating at 200° C. for 30 minutes is 10% or less, A polytetrafluoroethylene film having a melting enthalpy of 25 kJ / kg or less.
2. 2. The polytetrafluoroethylene film according to claim 1, which has a thickness of 15 to 150 μm.
3. Molding the polytetrafluoroethylene powder to obtain a molded product; The molded product is cut into a film to obtain a cut film. and calendering the cut film at a temperature lower than the melting point of polytetrafluoroethylene to obtain a polytetrafluoroethylene film. The method for producing a polytetrafluoroethylene film according to claim 1 or 2, characterized in that the cut film has a thickness of 75 to 300 μm.
4. The manufacturing method described in claim 3, characterized in that the thickness of the polytetrafluoroethylene film is greater than 50 μm and less than 100 μm.
5. The manufacturing method according to claim 3, characterized in that the thickness ratio of the cutting film to the polytetrafluoroethylene film, i.e., the thickness ratio of the cutting film before calendaring to the polytetrafluoroethylene film after calendaring, is 5 / 1 to 1.5 / 1.
6. 6. The method according to claim 5, wherein the calendering is carried out in one or more stages.
7. The method according to claim 3, wherein the calendered film is calendered at 230-310°C.
8. 3. An adhesive tape comprising the polytetrafluoroethylene film according to claim 1 or 2 as a substrate.
Citation Information
Patent Citations
Preparation method of teflon oriented film of ultra-thin breadth
CN101491945A
Pressure-sensitive adhesive tape-rolled material and method of producing the pressure-sensitive adhesive tape
JP2001164202A
High density polytetrafluoroethylene tape and method of manufacturing the same
JP2012036266A
Fluoropolymer Tape, Article Comprising a Fluoropolymer Tape and Process for Manufacturing a Fluoropolymer Tape
US20080014423A1
Method for molding polytetrafluoroethylene, polytetrafluoroethylene molded body, crosslinkable polytetrafluoroethylene, crosslinked polytetrafluoroethylene powder, resin blend composition, and molded body of resin blend
WO2007052664A1