Resin modifier and resin composition containing the modifier

A saponified ethylene-vinyl acetate copolymer addresses the moldability and contamination issues of resins with polar groups by enhancing extrusion efficiency and transparency.

JP7556196B2Active Publication Date: 2024-09-26TOSOH CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020005450
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-01-16
Publication Date
2024-09-26
Estimated Expiration
2040-01-16

AI Technical Summary

Technical Problem

Resins with polar groups, such as EVOH, suffer from poor extrusion molding efficiency due to thermal deterioration and contamination issues, leading to defects like fish eyes and gels, which hinder continuous production.

Method used

A saponified ethylene-vinyl acetate copolymer with specific ethylene and vinyl acetate content ranges and high melt mass flow rate is used to modify resins, preventing adhesion to metal surfaces and maintaining transparency.

Benefits of technology

The copolymer improves moldability by reducing resin retention in molding machines and minimizing defects, allowing continuous extrusion without impairing resin transparency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007556196000003
    Figure 0007556196000003
  • Figure 0007556196000001
    Figure 0007556196000001
  • Figure 0007556196000002
    Figure 0007556196000002
Patent Text Reader

Abstract

To provide a resin modifier which improves moldability of a resin having a polar group and prevents contamination of a foreign matter and thereby enables continuous mold-processability, and is compatible with a resin to be a base material without impairing transparency of the resin.SOLUTION: A resin modifier contains a saponified product of an ethylene-vinyl acetate copolymer obtained by saponifying an ethylene-vinyl acetate copolymer having a content of ethylene of 75 mol% or more and 95 mol% or less and a content of vinyl acetate of 5 mol% or more and 25 mol% or less, in which a degree of saponification of a vinyl acetate component is 20 wt.% or more, and a melt mass flow rate measured according to JIS K 6924-1 (under conditions of 190°C and load of 2,160 g) is 10 g / 10 min or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin modifier that improves the molding processability of a resin, and to a resin composition containing the modifier. [Background technology]

[0002] Resins containing many polar groups in the molecule, such as ethylene-vinyl alcohol copolymer (hereinafter referred to as "EVOH") and polyamide, are used as packaging materials for foods, beverages, and medicines. In particular, EVOH is used in various gas barrier films and the gas barrier layer of gas barrier containers because of its excellent mechanical properties such as impact strength and tensile strength, solvent resistance, chemical resistance, gas barrier properties, aroma retention, and oil resistance.

[0003] However, such resins containing many polar groups in the molecule have a problem that the production efficiency during extrusion molding is inferior to that of polyolefins having a low polarity, such as polyethylene and polypropylene, which have a low polarity. Specifically, when EVOH is extruded for a long period of time, if the EVOH adheres to and remains on the metal inner wall of the extruder, it is prone to thermal degradation. If the degraded products are contained in the molded body, the molded body will have poor appearance such as fish eyes, gels, and streaks, which makes it impossible to perform continuous extrusion molding. Such poor appearance is particularly noticeable in resins that exhibit transparency such as EVOH, among resins that have polar groups, and therefore a method for preventing this has been desired.

[0004] In response to this, it has been proposed to incorporate additives such as fatty acid metal salts into EVOH (for example, Patent Documents 1 and 2). According to Patent Document 1, adding a fatty acid metal salt to EVOH makes it possible to perform stable extrusion molding for a long period of time. However, since the fatty acid metal salt has a low molecular weight, it is prone to bleeding from the molded product. Therefore, the amount of fatty acid metal salt to be added is limited, and sufficient effects cannot be obtained. In light of this background, there has been a demand for a resin modifier that has excellent thermal stability, improves the moldability of resins having polar groups in their molecules, inhibits the long-term retention of such resins, and reduces foreign matter such as fish eyes and gel-like substances. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2002-60496 A [Patent Document 2] International Publication No. 2010 / 071241 Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention has been made in consideration of the above-mentioned circumstances, and has an object to provide a resin modifier that improves the moldability of a resin having a polar group and prevents contamination by foreign matter, thereby enabling continuous molding processing, and that is compatible with a base resin without impairing the transparency of the resin. [Means for solving the problem]

[0007] As a result of extensive investigations, the present inventors have found that a saponified ethylene-vinyl acetate copolymer having a specific structure can solve the above problems, and have thus completed the present invention.

[0008] That is, the present invention relates to a resin modifier containing a saponified ethylene-vinyl acetate copolymer obtained by saponifying an ethylene-vinyl acetate copolymer having an ethylene content of 75 mol% or more and 95 mol% or less and a vinyl acetate content of 5 mol% or more and 25 mol% or less, wherein the saponification degree of the vinyl acetate component is 20% or more and the melt mass-flow rate measured in accordance with JIS K6924-1 (under conditions of 190°C and a load of 2160 g) is 10 g / 10 min or more. Another embodiment of the present invention is a composition containing the resin modifier and a resin having a polar group.

[0009] The present invention will be described in detail below.

[0010] The saponified ethylene-vinyl acetate copolymer used in the present invention is a saponified copolymer of ethylene and vinyl acetate having an ethylene content of 75 mol% to 95 mol% and a vinyl acetate content of 5 mol% to 25 mol%. By having a vinyl acetate content of 25 mol% or less, the resin to be blended is less likely to remain in the molding machine. By having a vinyl acetate content of 5 mol% or more, the difference in refractive index with the base resin is small, and the transparency of the resin is not impaired. Examples of methods for producing ethylene-vinyl acetate copolymers include well-known methods such as high-pressure radical polymerization, solution polymerization, and emulsion polymerization, and such resins can be conveniently selected from commercially available products. Ethylene-vinyl acetate copolymers are commercially available from Tosoh Corporation under the trade name Ultrathene, and from Lanxess KK under the trade names Levaprene and Levamelt.

[0011] The saponified ethylene-vinyl acetate copolymer of the present invention is obtained by hydrolyzing the vinyl acetate component of the ethylene-vinyl acetate copolymer, and has a degree of saponification of the vinyl acetate component of 20% by weight or more calculated in accordance with JIS K7192 (1999). This reduces the difference in refractive index with the base resin, and does not impair the transparency of the resin. The degree of saponification of the saponified ethylene-vinyl acetate copolymer is preferably 30% by weight or more and 100% by weight or less, and more preferably 61% by weight or more and 100% by weight or less. The hydrolysis method of ethylene-vinyl acetate copolymer can be, for example, a method of directly hydrolyzing pellets of ethylene-vinyl acetate copolymer in alkali, or it can be conveniently selected from commercial products, such as those sold by Tosoh Corporation under the trade name of Mersen H.

[0012] The saponified ethylene-vinyl acetate copolymer used in the present invention has a melt mass flow rate of 10 g / 10 min or more measured based on JIS K6924-1 (under conditions of 190°C and a load of 2160 g). The melt mass flow rate is preferably 40 g / 10 min or more. This makes it possible to further prevent the resin from being retained in the molding machine.

[0013] In the present invention, the saponified ethylene-vinyl acetate copolymer may be either a single type or a combination of two or more types. When a composition of two or more types of saponified ethylene-vinyl acetate copolymer is used, a combination of at least two types of saponified ethylene-vinyl acetate copolymers, namely, an ethylene-vinyl acetate copolymer having an ethylene content of 75 mol% or more and 90 mol% or less and a vinyl acetate content of 10 mol% or more and 25 mol% or less, and an ethylene-vinyl acetate copolymer having an ethylene content of more than 90 mol% and 95 mol% or less and a vinyl acetate content of 5 mol% or more and less than 10 mol%, is preferred because it enhances the resin retention suppression effect. When a composition of two or more kinds of saponified ethylene-vinyl acetate copolymers is used, the composition may be obtained by either a method in which two or more kinds of saponified ethylene-vinyl acetate copolymers are mixed in advance and the resulting mixture is subjected to a hydrolysis treatment to obtain a saponified product, or a method in which two or more kinds of saponified ethylene-vinyl acetate copolymers are mixed and used.

[0014] When a composition of two or more saponified ethylene-vinyl acetate copolymers is used, a crosslinking agent may be added to the composition to crosslink and modify the composition in order to further increase the dispersibility of each component. The crosslinking agent may be any agent capable of crosslinking each component, and it is preferable to use an organic peroxide in consideration of reactivity, etc. The crosslinking modification method generally involves the addition of a crosslinking agent, and the method of hydrolyzing a crosslinked ethylene-vinyl acetate copolymer or crosslinking a saponified ethylene-vinyl acetate copolymer is selected. Examples of organic peroxides for the crosslinking agent include dicumyl peroxide, di-t-butyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, 1,1-di(t-butylperoxy)cyclohexane, 2,5-dimethyl-2,5-di(t-butylperoxy)hexyne-3, 1,3-bis(t-butylperoxyisopropyl)benzene, 1,1-bis(t-butylperoxy)-3,3,5-trimethylcyclohexane, 1,3-di(t-butylperoxy)-diisopropylbenzene, n-butyl-4,4-bis(t-butylperoxy)valerate, benzoyl peroxide, p-chlorobenzoyl peroxide, 2,4-dichlorobenzoyl peroxide, t-butylperoxybenzoate, t-butylperoxyisopropylcarbonate, diacetyl peroxide, lauroyl peroxide, and t-butylcumyl peroxide. These can be used alone or in combination of two or more kinds. Among them, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane and 1,1-di(t-butylperoxy)cyclohexane are preferably used from the viewpoint of reactivity. In addition, crosslinking assistants such as triallyl isocyanurate and divinylbenzene may be used together with the above crosslinking agents, if necessary.

[0015] The saponified ethylene-vinyl acetate copolymer of the present invention may contain, as necessary, one or more of commonly used additives such as an antioxidant, a lubricant, a neutralizing agent, an antiblocking agent, a surfactant, a slip agent, silicone oil, an ultraviolet absorber, a flame retardant, a release agent, a foaming agent, and a fragrance.

[0016] The saponified ethylene-vinyl acetate copolymer of the present invention can be blended with a base resin to improve the moldability of the resin and prevent adhesion to metals, and therefore can be suitably used as a resin modifier. The saponified ethylene-vinyl acetate copolymer of the present invention can be used as a resin modifier in any form such as pellets or powder. Furthermore, since the resin modifier of the present invention has thermoplastic properties, it can be molded using ordinary molding equipment.

[0017] The modifier of the present invention is added to a resin having a polar group, particularly a transparent resin, to prevent the resin from staying in a molding machine. Examples of the resin to which the modifier can be added include resins containing many polar groups in the molecule, such as polyvinyl alcohol, ethylene-vinyl alcohol copolymers (EVOH) with an ethylene content of less than 75 mol%, polyamide, polyester, and polycarbonate.

[0018] The amount of the modifier of the present invention to be added is preferably 0.1 to 10 parts by weight, more preferably 0.5 to 6 parts by weight, and even more preferably 0.5 to 3 parts by weight, based on 100 parts by weight of the transparent resin.

[0019] EVOH is a copolymer consisting of ethylene units and vinyl alcohol units, and is distinguished from the saponified ethylene-vinyl acetate copolymer, which is the modifier of the present application, and therefore has an ethylene content of less than 75 mol%. The ethylene content of EVOH can be 60 mol% or less, or even 20 mol% or more and 50 mol% or less. Usually, EVOH refers to one with an ethylene content in this range. The EVOH used in the present invention may be, for example, a known one used for molding purposes. The method for producing EVOH is not particularly limited, and for example, EVOH can be produced by producing an ethylene and vinyl ester copolymer according to a known method, and then saponifying the copolymer. However, the content of ethylene units in EVOH is preferably 55 mol% or less, more preferably 10 mol% or more and 55 mol% or less, from the viewpoint of high barrier properties against gases, organic liquids, etc., and good molding processability. Such a resin can be conveniently selected from commercially available products, and is commercially available, for example, under the trade name EVAL from Kuraray Co., Ltd. and under the trade name Soarnol from Nippon Synthetic Chemical Industry Co., Ltd.

[0020] Examples of resins having polar groups that can be blended with the modifier of the present invention include polyvinyl alcohol, polyamides such as nylon-6, nylon-6,6, and metaxylene adipamide, polyesters such as polyethylene terephthalate, polybutylene terephthalate, polylactic acid, and polybutylene succinate, and polycarbonates, which are resins that contain many polar groups in their molecules.

[0021] The method for kneading the saponified ethylene-vinyl acetate copolymer and the resin having a polar group of the present invention can be, for example, a method in which a dry blend of the saponified ethylene-vinyl acetate copolymer and the resin having a polar group is fed into a hopper of an extruder, etc. At least one of the saponified ethylene-vinyl acetate copolymer and the resin may be added from a side feeder, etc. For dry blending of the saponified ethylene-vinyl acetate copolymer and the resin, a Henschel mixer, V blender, ribbon blender, tumbler, etc. may be used, and if such equipment is not available, the saponified ethylene-vinyl acetate copolymer may be fed separately.

[0022] In addition to the saponified ethylene-vinyl acetate copolymer and resin, additives such as antioxidants, lubricants, neutralizing agents, antiblocking agents, surfactants, slip agents, etc., which are normally used in polyolefins such as polyethylene and polypropylene, can also be added as necessary.

[0023] The composition of saponified ethylene-vinyl acetate copolymer and resin can be molded by any method such as injection molding, compression molding, extrusion molding, etc. Among these, the extrusion molding methods include T-die method, hollow molding, pipe extrusion, irregular die extrusion, inflation method, etc. The shape of the molded product is arbitrary, and it can be applied not only to pellets, but also to films, sheets, tapes, bottles, pipes, filaments, and irregular cross-section extrusions, as well as laminates with other resins. The composition of the saponified ethylene-vinyl acetate copolymer and the resin having a polar group can be molded by the above-mentioned molding method and used as a molded article, for example in the form of a film.

[0024] The film has gas barrier properties and can therefore be suitably used as a laminate having at least one layer of the film.

[0025] The modifier of the present invention can be used as a molding aid for resins containing polar groups in the molecule, and can suppress long-term retention of the resin by adding a small amount of the modifier without impairing the inherent performance of the resin, so that the modifier can be used in a wide range of applications. Effect of the Invention

[0026] The resin modifier of the present invention can suppress adhesion of resin to the metal inner wall of an extruder, and reduce foreign matter such as fish eyes and gel-like substances. EXAMPLES

[0027] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0028] [Vinyl acetate content and degree of saponification] The vinyl acetate content of the ethylene-vinyl acetate copolymer or saponified ethylene-vinyl acetate copolymer used in the examples was measured in accordance with JIS K7192 (1999), and the degree of saponification (wt%) was calculated according to the following formula. Degree of saponification (wt%) = 100 × {(acetic acid of ethylene-vinyl acetate copolymer before hydrolysis)} Vinyl content (wt%) - (vinyl acetate of ethylene-vinyl acetate copolymer after hydrolysis (Vinyl acetate content (wt%)) / (Vinyl acetate content of ethylene-vinyl acetate copolymer before hydrolysis (weight%)) [Melt Mass Flow Rate] The melt mass flow rate (hereinafter referred to as "MFR") of the saponified ethylene-vinyl acetate copolymer used in the examples was measured using a melt indexer (manufactured by Takara Kogyo Co., Ltd.) in accordance with JIS K6924-1 (under conditions of 190°C and a load of 2160 g).

[0029] [Evaluation of fading time] A blend of 2 parts by weight of a blue pigment master batch prepared under the conditions described in (1) below and the resulting blend was placed in the hopper of an extruder and extruded for 30 minutes under the conditions described in (2) below. After 30 minutes, the blend was replaced with the dry blend described in the examples that did not contain the blue pigment master batch, and extrusion was continued for another 30 minutes, and the color change over time (fading time) was observed. If the color of the extrudate changed from blue to colorless or white within 5 minutes, it was marked as "Good", if it changed within 5 to 10 minutes, it was marked as "Good", and if it changed in more than 10 minutes, it was marked as "Poor". (1) A blue content masterbatch was prepared by adding 0.5 parts by weight of phthalocyanine blue manufactured by Dainichiseika Color & Chemicals Mfg. Co., Ltd. to 100 parts by weight of ethylene-vinyl alcohol copolymer (manufactured by Kuraray Co., Ltd., product name C109B, ethylene content 35 mol%, MFR 8.5 g / 10 min) and melt-kneading the mixture at 200°C. (2) The extruder used was a single-screw extruder D2025N (non-vent, inner diameter 20 mm) manufactured by Toyo Seiki Co., Ltd. The set temperatures were C1 / C2 / C3 / D = 180 / 200 / 230 / 230°C, and the screw rotation speed was 30 rpm.

[0030] [Haze] The dry blend obtained in the example was melt-kneaded in an internal mixer (manufactured by Toyo Seiki Seisakusho, trade name: Labo Blast Mill R-100) under conditions of a resin temperature of 200° C., a roller rotation speed of 60 rpm, and a kneading time of 3 minutes. The obtained kneaded product was press molded using a press molding machine (AWFA-50 model manufactured by Shinto Metal Industries Co., Ltd.) under the conditions of a heating temperature of 200°C (primary pressurization x 3 minutes, secondary pressurization x 3 minutes) and a cooling temperature of 25°C (4 minutes), and the obtained press sheet with a thickness of 0.1 mm was measured for haze using a haze meter (NDH7000 model manufactured by Nippon Denshoku Industries Co., Ltd.). Five points were selected and evaluated for the same sample, and the average value was taken as the haze value. When the haze was 50% or less, the transparency was good and it was marked as "◯", when the haze was 51 to 70%, it was marked as "△", and when the haze was more than 71%, it was marked as "X" because the transparency was poor.

[0031] Example 1 As a resin having a polar group, 100 parts by weight of ethylene-vinyl alcohol copolymer (Kuraray Co., Ltd., trade name F171B, ethylene content 32 mol%, MFR 1.7g / 10min) was used, and 5 parts by weight of ethylene-vinyl acetate copolymer saponification product (Tosoh Corporation, trade name Mersen H H6822X) with ethylene content 89 mol%, vinyl acetate content 11 mol%, saponification degree of vinyl acetate component 80 wt%, MFR 220g / 10min was added and mixed at room temperature to obtain a dry blend. The obtained dry blend was processed according to the above-mentioned method, and the residence time and haze were evaluated. The results are shown in Table 1.

[0032] Example 2 A dry blend was obtained in the same manner as in Example 1, except that the amount of the saponified ethylene-vinyl acetate copolymer was 1 part by weight. The evaluation results are shown in Table 1.

[0033] Example 3 A dry blend was obtained in the same manner as in Example 1, except that the amount of the saponified ethylene-vinyl acetate copolymer was changed to 0.5 parts by weight. The evaluation results are shown in Table 1.

[0034] Example 4 A dry blend was obtained in the same manner as in Example 1, except that the amount of the saponified ethylene-vinyl acetate copolymer was 0.25 parts by weight. The evaluation results are shown in Table 1.

[0035] Example 5 A dry blend was obtained in the same manner as in Example 1, except that the saponified ethylene-vinyl acetate copolymer used had an ethylene content of 81 mol%, a vinyl acetate content of 19 mol%, a degree of saponification of the vinyl acetate component of 90% by weight, and an MFR of 40 g / 10 min (manufactured by Tosoh Corporation, product name: Mersen H H6960) and was blended in an amount of 5 parts by weight. The evaluation results are shown in Table 1.

[0036] Example 6 A dry blend was obtained in the same manner as in Example 1, except that the saponified ethylene-vinyl acetate copolymer used had an ethylene content of 89 mol%, a vinyl acetate content of 11 mol%, a degree of saponification of the vinyl acetate component of 40% by weight, and an MFR of 16 g / 10 min (manufactured by Tosoh Corporation, product name: Mersen H H6410M) and was blended in an amount of 5 parts by weight. The evaluation results are shown in Table 1.

[0037] [Table 1]

[0038] Example 7 As a resin having a polar group, ethylene-vinyl alcohol copolymer (manufactured by Kuraray Co., Ltd., product name F171B, ethylene content 32 mol%, MFR 1.7 g / 10 min) was used, with respect to 100 parts by weight. 2.5 parts by weight of ethylene-vinyl acetate copolymer saponified product A (manufactured by Tosoh Corporation, trade name Mersen H H6960) having an ethylene content of 81 mol%, a vinyl acetate content of 19 mol%, a degree of saponification of the vinyl acetate component of 90% by weight, and an MFR of 40 g / 10 min; 2.5 parts of 50% by weight saponification product B of an ethylene-vinyl acetate copolymer (manufactured by Tosoh Corporation, trade name Ultrathene 680) having an ethylene content of 93 mol%, a vinyl acetate content of 7 mol%, and an MFR of 180 g / 10 min; Except for the above, a dry blend was obtained in the same manner as in Example 1. The evaluation results are shown in Table 2. However, saponification of Ultrathene 680 was carried out in the following manner. Ultrathene 680 was added to a methanol solution with a caustic soda concentration of 4% by weight, and the mixture was stirred at 60°C under a nitrogen atmosphere for 8 hours to carry out the saponification reaction (solid-liquid ratio 2.5). After solid-liquid separation, a methanol solution with a hydrochloric acid concentration of 1% by weight was added, and the saponification reaction product was neutralized at a temperature of 45°C. Finally, the neutralized reaction product was washed with water and dried to obtain the desired saponified ethylene-vinyl acetate copolymer.

[0039] [Table 2]

[0040] Comparative Example 1 A dry blend was obtained in the same manner as in Example 1, except that 5 parts by weight of an ethylene-vinyl acetate copolymer (manufactured by Tosoh Corporation, product name Ultrathene 720) having an ethylene content of 89 mol%, vinyl acetate content of 11 mol%, and MFR of 150 g / 10 min was blended with 100 parts by weight of an ethylene-vinyl alcohol copolymer (manufactured by Kuraray Co., Ltd., product name F171B, ethylene content 32 mol%, MFR 1.7 g / 10 min) as a resin having a polar group. The evaluation results are shown in Table 3.

[0041] Comparative Example 2 A dry blend was obtained in the same manner as in Example 1, except that 5 parts by weight of a saponified ethylene-vinyl acetate copolymer (product name: Mersen H H6051K, manufactured by Tosoh Corporation) having an ethylene content of 89 mol%, a vinyl acetate content of 11 mol%, a saponification degree of the vinyl acetate component of 100 wt%, and an MFR of 5.5 g / 10 min was blended with 100 parts by weight of an ethylene-vinyl alcohol copolymer (product name: F171B, manufactured by Kuraray Co., Ltd., ethylene content 32 mol%, MFR 1.7 g / 10 min) as a resin having a polar group. The evaluation results are shown in Table 3. It took a long time for the color to fade, and it was found that the resin was retained in the molding machine.

[0042] Comparative Example 3 A dry blend was obtained in the same manner as in Example 1, except that a high-pressure low-density polyethylene (manufactured by Tosoh Corporation, product name Petrothene 208) having an ethylene content of 100 mol%, vinyl acetate content of 0 mol%, and MFR of 23 g / 10 min was used in place of the saponified ethylene-vinyl acetate copolymer, and the blending amount was changed to 5 parts. The evaluation results are shown in Table 3. It can be seen that the haze was high and the transparency was impaired.

[0043] Comparative Example 4 The evaluation was carried out in the same manner as in Example 1, except that saponified ethylene-vinyl acetate copolymer was not added and only EVOH was used. The results are shown in Table 3. It took a long time for the color to fade, which indicates that the resin was retained in the molding machine. But it was late.

[0044] [Table 3]

Claims

1. A resin composition comprising 100 parts by weight of an ethylene-vinyl alcohol copolymer having an ethylene content of less than 75 mol%, and 0.1 parts by weight or more and 5 parts by weight or less of a molding aid for ethylene-vinyl alcohol copolymer (EVOH) having an ethylene content of less than 75 mol%, the molding aid being an ethylene-vinyl acetate copolymer saponified product obtained by saponifying an ethylene-vinyl acetate copolymer having an ethylene content of 75 mol% or more and 95 mol% or less and a vinyl acetate content of 5 mol% or more and 25 mol% or less, the degree of saponification of the vinyl acetate component being 20% ​​by weight or more and a melt mass-flow rate measured in accordance with JIS K6924-1 (under conditions of 190°C and a load of 2160 g) being 10 g / 10 min or more.

2. The melt mass flow rate of saponified ethylene-vinyl acetate copolymer is 40g / 10min or more. The resin composition according to claim 1,

3. The ethylene-vinyl acetate copolymer saponification product has an ethylene content of 75 mol % or more and 90 mol % or less. The vinyl acetate content of the ethylene-vinyl acetate copolymer is 10 mol % or more and 25 mol % or less. and saponified polyolefins having an ethylene content of more than 90 mol% and not more than 95 mol% and a vinyl acetate content of 5 mol% or less.

3. The resin composition according to claim 1, which is a composition of a saponified ethylene-vinyl acetate copolymer in which the saponification product is from 1 mol % to less than 10 mol %.

4. A molded article comprising the resin composition according to any one of claims 1 to 3.

5. A film comprising the resin composition according to any one of claims 1 to 3.

6. A laminate comprising at least one layer of the film according to claim 5.

Citation Information

Patent Citations

  • Resin composition and molded product therefrom

    JP1991026736A

  • Resin composition and laminate

    JP2001049069A

  • Resin composition pellets and molded product

    JP2002060496A

  • Resin molded product for painting

    JP2007284647A

  • Poly-3-hydroxy butyrate polymer composition

    JP2009173803A