Nanomesh Sheet

The nanomesh sheet addresses the visibility and sunburn issues by setting specific haze and light transmittance values, ensuring the film is unnoticeable and uniform sun exposure.

JP7556273B2Active Publication Date: 2024-09-26MITSUBISHI CHEM CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2020196634
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-27
Publication Date
2024-09-26
Estimated Expiration
2040-11-27

AI Technical Summary

Technical Problem

When a nanomesh sheet with a water-soluble resin and conductive material layer is attached to the skin, the re-formed water-soluble resin film can become noticeable and cause uneven sunburn marks due to differences in sun exposure.

Method used

A nanomesh sheet with specific haze and light transmittance values for the water-soluble resin layer, ensuring the film is inconspicuous and uniform sun exposure by controlling the UV and visible light transmission.

Benefits of technology

The nanomesh sheet minimizes the visibility of the water-soluble resin film and reduces uneven sunburn marks by maintaining consistent light transmittance across the applied area.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007556273000003
    Figure 0007556273000003
  • Figure 0007556273000002
    Figure 0007556273000002
  • Figure 0007556273000001
    Figure 0007556273000001
Patent Text Reader

Abstract

To provide a nano mesh sheet in which a water soluble resin is inconspicuous after being adhered to an adherend, and which can relax a local sunburn trace after being adhered to a skin of a user.SOLUTION: A nano mesh sheet is formed by laminating: a nano mesh layer formed of a water soluble resin; a conductive substance layer. The conductive substance layer of the nano mesh sheet and an adherend are made face each other and the nano mesh sheet is installed on the adherend. A haze value of the nano mesh layer of the water soluble resin after dripping water from the nano mesh layer side for adhering the conductive substance layer to the adherend, is 12 or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a nanomesh sheet having a conductive material layer. [Background technology]

[0002] Flexible electronics, which involves forming electronic devices on flexible substrates, is currently being researched, and research into its application to living organisms is also progressing. For example, an electronic functional component has been proposed that has high surface conformability and can be used stably for a long period of time, and that has a substrate with an opening and a fiber network suspended around the opening as an outer frame (see Patent Document 1).

[0003] It has also been proposed to create a skin-attachable nanomesh sensor that is both breathable and stretchable using polyvinyl alcohol (PVA) resin, which is biocompatible and expected to be biodegradable (see non-patent document 1).

[0004] The nanomesh sensor disclosed in Non-Patent Document 1 is a PVA nanofiber mesh made by electrospinning, one side of which is coated with a conductive metal or the like. This nanomesh sensor is placed on the skin and water is sprayed onto it, causing the nanofiber mesh of the conductive metal or the like to adhere to the skin surface, and the adhered nanofiber mesh of the conductive metal or the like follows the deformation of the skin, making it applicable to joints and the like and usable for wiring to various sensors, etc. In particular, the use of gold as the conductive metal or the like and the mesh structure that does not interfere with skin respiration, etc., greatly reduces the occurrence of discomfort and inflammation caused by wearing the nanomesh. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2016-112246 A [Non-patent literature]

[0006] [Non-Patent Document 1] “Success in developing a skin-attachable nanomesh sensor that enables skin breathing”, [online], University of Tokyo, Japan Science and Technology Agency, Keio University, RIKEN, [Retrieved October 14, 2020], Internet<URL:http: / / www.jst.go.jp / pr / announce / 20170718 / > Summary of the Invention [Problem to be solved by the invention]

[0007] In the case of applying a conductive metal to the skin surface by dissolving a water-soluble resin such as PVA nanofiber by spraying water as in the method disclosed in Non-Patent Document 1, the water-soluble resin once dissolved in water will form a film on the skin surface again as the water evaporates. In this case, the film formed on the skin surface again may be very conspicuous depending on the type of water-soluble resin and the thickness of the film, and it was thought that the user may be put off by the film. The present invention solves the above-mentioned problem that arises only when a nanomesh sheet having a nanomesh layer of a water-soluble resin and a conductive material layer on a mesh-like base layer is attached to an adherend.

[0008] Furthermore, the inventors have also realized the problem that when the adherend is skin, when going outside, there will be a difference in the degree of sunburn between the area where the above-mentioned water-soluble resin film is formed and other areas, resulting in noticeable sunburn marks. Another object of the present invention is to alleviate such localized unevenness in tan marks. [Means for solving the problem]

[0009] The inventors conducted extensive research to solve the above problems and discovered that the above problems can be solved by setting the haze value of the water-soluble resin nanomesh layer after the conductive material layer is attached to an adherend to a specific value or less.

[0010] That is, the present invention includes the following. [1] A nanomesh sheet having a water-soluble resin nanomesh layer and a conductive material layer laminated thereon, a nanomesh sheet, wherein the nanomesh sheet is placed on an adherend with the conductive material layer of the nanomesh sheet facing the adherend, and the conductive material layer is attached to the adherend by dripping water from the nanomesh layer side, and the haze value of the nanomesh layer made of a water-soluble resin after the nanomesh sheet is adhered to the adherend is 12 or less. [2] The nanomesh sheet according to [1], wherein the nanomesh sheet is placed on an adherend with the conductive material layer of the nanomesh sheet facing the adherend, and the conductive material layer is attached to the adherend by dripping water from the nanomesh layer side, and the visible light transmittance of the nanomesh layer made of a water-soluble resin is 95.0% or more and 99.9% or less. [3] The nanomesh sheet according to [1] or [2], wherein the conductive material layer of the nanomesh sheet is placed on an adherend with the conductive material layer facing the adherend, and the conductive material layer is attached to the adherend by dripping water from the nanomesh layer side, and the UV light transmittance of the nanomesh layer made of a water-soluble resin is 95.0% or more and 99.9% or less. [4] The nanomesh sheet according to any one of [1] to [3], wherein the conductive material layer of the nanomesh sheet is placed on an adherend with the conductive material layer facing the adherend, and the conductive material layer is attached to the adherend by dripping water from the nanomesh layer side, and the UV light transmittance / visible light transmittance of the nanomesh layer made of a water-soluble resin after that is 0.95 or more and 1.0 or less.

[0011] Furthermore, the inventors conducted extensive research to solve the other problem described above, and discovered that the other problem described above can be solved by setting the UV light transmittance / visible light transmittance value of the water-soluble resin nanomesh layer after the conductive material layer is attached to an adherend to a specific range.

[0012] That is, the present invention also includes the following. [5] A nanomesh sheet having a water-soluble resin nanomesh layer and a conductive material layer laminated thereon, The nanomesh sheet is placed on an adherend with the conductive material layer of the nanomesh sheet facing the adherend, and water is dropped from the nanomesh layer side to attach the conductive material layer to the adherend, and the UV light transmittance / visible light transmittance value of the nanomesh layer made of a water-soluble resin after the nanomesh sheet is adhered to the adherend is 0.95 or more and 1.00 or less. Effect of the Invention

[0013] According to the present invention, it is possible to provide a nanomesh sheet in which the water-soluble resin is not noticeable after application to an adherend, and a nanomesh sheet capable of reducing localized unevenness in tan marks after application to skin. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is a schematic cross-sectional view showing a nanomesh sheet according to one embodiment. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing measurement points for the haze value and light transmittance of a nanomesh layer in an example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The present invention will be described in detail below. However, the description of the constituent elements described below is one example (representative example) of an embodiment of the present invention, and the present invention is not limited to these contents, and can be implemented in various modifications within the scope of the gist of the present invention.

[0016] One embodiment of the present invention is a nanomesh sheet having a nanomesh layer of a water-soluble resin and a conductive material layer laminated thereon, the nanomesh sheet being placed on an adherend with the conductive material layer of the nanomesh sheet facing the adherend, and water being dropped from the nanomesh layer side to attach the conductive material layer to the adherend, after which the haze value of the nanomesh layer of the water-soluble resin is no more than 12. The nanomesh sheet according to this embodiment will be described with reference to the drawings.

[0017] FIG. 1 shows a schematic cross-sectional view of a nanomesh sheet according to this embodiment. The nanomesh sheet 100 has a configuration in which a nanomesh layer 11 made of a water-soluble resin and a conductive material layer 12 are laminated on a mesh-like base layer 10. The mesh-like base layer 10 supports a laminate in which a water-soluble resin nanomesh layer 11 and a conductive material layer 12 are laminated. Since the laminate in which a water-soluble resin nanomesh layer 11 and a conductive material layer 12 are laminated is very thin, it is preferable from the viewpoint of ease of attachment to laminate it on the mesh-like base layer 10. There are no particular limitations on the mesh-like base layer 10, so long as it is sparingly soluble and allows liquid to permeate through the mesh. The thickness of the mesh-like base layer 10 is not particularly limited as long as it can support the water-soluble resin nanomesh layer 11 and the conductive material layer 12, but is usually 10 μm or more, preferably 50 μm or more, and usually 5000 μm or less, preferably 1000 μm or less.

[0018] The mesh size of the mesh-like substrate layer 10 is not particularly limited as long as it is permeable to liquid, but is usually 50 nm or more, preferably 100 nm or more, and usually 20 mm or less, preferably 10 mm or less. The material of the mesh-like base layer 10 is not particularly limited, but from the viewpoint of ease of handling when attaching it to an adherend, examples of the material include thermoplastic resins having a moderate elastic modulus, and general-purpose plastics such as polyethylene, polypropylene, polyethylene terephthalate, and polybutylene terephthalate can be used. The mesh-like substrate layer 10 may be a commercially available product such as a porous film, or may be produced by a known method.

[0019] The water-soluble resin nanomesh layer 11 is made of water-soluble resin fibers, and examples of the water-soluble resin include polyvinyl alcohol (PVA), polyacrylamide, carboxymethyl cellulose, polyvinylpyrrolidone (PVP), polyglycolic acid (PGA), polylactic acid (PLA), etc., with PVA being preferred. The PVA may be modified PVA with hydroxyl groups, acetate groups, acetoacetyl groups, etc. introduced therein. The water-soluble resin is not particularly limited as long as it is soluble, but the solubility is usually 10% or more, preferably 20% or more, and more preferably 30% or more. The solubility here refers to the reduction ratio of the soluble polymer weight when immersed in pure water at 22±1° C. for 1 hour to the soluble polymer weight before immersion.

[0020] The nanomesh layer 11 of the water-soluble resin is typically produced by electrospinning. In the electrospinning method, the mesh-like base layer 10 is prepared, and a nanomesh layer of the water-soluble resin is formed thereon. The electrospinning method is also used in Patent Document 1, and reference can be made to this document. The fiber diameter of the water-soluble resin fiber that constitutes the nanomesh layer in this case is usually 50 nm or more and 1000 μm or less, and preferably 100 nm or more and 900 μm or less in terms of solubility in water. The fiber diameter of the water-soluble resin fiber that constitutes the nanomesh layer is usually 50 nm or more and 1000 μm or less, and preferably 100 nm or more and 900 μm or less in terms of solubility in water. The fiber diameter can be controlled by, for example, the aqueous solution concentration, the liquid supply rate, etc., in the case of the electrospinning method. To make the fiber diameter thinner, the aqueous solution concentration can be diluted and / or the liquid supply rate can be decreased. On the other hand, to make the fiber diameter thicker, the aqueous solution concentration can be increased and / or the liquid supply rate can be increased.

[0021] A conductive material layer 12 is formed on the nanomesh layer 11 of the water-soluble resin. The conductive material is not particularly limited as long as it has conductivity, and specifically, gold, silver, copper, titanium, carbon, etc. can be used. When it is desired to make the conductive material transparent, ITO (indium tin oxide) may be used. Other conductive metal oxides such as nickel oxide, tin oxide, indium oxide, indium-zirconium oxide (IZO), titanium oxide, indium oxide, or zinc oxide may be used. PEDOT:PSS in which polystyrene sulfonic acid is doped into a polythiophene derivative, PEDOT:PTS in which paratoluene sulfonic acid is doped into a polythiophene derivative, or a conductive polymer material in which iodine or the like is doped into polypyrrole or polyaniline may be used. Among these, considering application to living bodies, gold, carbon, titanium, PEDOT:PSS, and PEDOT:PTS are preferred, and gold is particularly preferred. The method of forming the conductive material layer is not particularly limited, and the conductive material layer is formed by a dry process or a coating method. As the dry process, deposition, sputtering, CVD, etc. are used. Among these, forming the conductive material layer by deposition is the simplest. There is no particular limit to the coating method, but specific examples include wire bar coating, blade coating, die coating, slit die coating, reverse roll coating, gravure coating, kiss coating, roll brushing, spray coating, air knife coating, pipe doctor, impregnation coating, curtain coating, flexographic printing, screen printing, inkjet, etc.

[0022] The thickness of the water-soluble resin nanomesh layer 11 may be appropriately set depending on the purpose, and is not particularly limited, but is usually 0.1 μm or more, and may be 1 μm or more, and is usually 100 μm or less, and may be 80 μm or less. The thickness of the conductive material layer 12 is not particularly limited, but is usually 5 nm or more, and may be 10 nm or more, and is usually 2 μm or less, and may be 1 μm or less, and may be 500 nm or less.

[0023] The weight of the nanomesh layer 11 made of water-soluble resin is 0.3 g / m 2 It is preferable that the content is 0.5 g / m or more. 2 More preferably, it is 3 g / m or more. 2 It is preferable that the content is 2.5 g / m or less. 2 It is more preferable that: When the basis weight is within the above range, the solubility of the nanomesh layer 11 tends to be within an appropriate range, and the breathability can be sufficient when the laminate is attached to an adherend. The basis weight of the nanomesh layer can be controlled by, for example, the applied voltage, the spinning time, etc., in the case of the electrospinning method. When it is desired to reduce the basis weight, it can be controlled by lowering the applied voltage and / or shortening the spinning time. On the other hand, when it is desired to increase the basis weight, it can be controlled by increasing the applied voltage and / or lengthening the spinning time.

[0024] The water-soluble resin nanomesh layer 11 is formed by placing the conductive material layer 12 of the nanomesh sheet 100 on the adherend (not shown) with the conductive material layer 12 facing the adherend, and attaching the conductive material layer 12 to the adherend by dripping water from the mesh-like base layer 10 side, and after removing the mesh-like base layer 10, the water-soluble resin nanomesh layer 11 has a haze value of 12 or less.

[0025] In this embodiment, the water-soluble resin nanomesh layer 11 satisfies the above haze value, so that the nanomesh sheet 100 is not noticeable when attached to an adherend. The water-soluble resin once dissolved in water will form a film again on the adherend as the water evaporates. Depending on the type of water-soluble resin and the thickness of the coating, this may be very noticeable, but the nanomesh sheet of the present embodiment makes this less noticeable even after it is attached to the adherend. The haze value is preferably 10 or less, more preferably 5 or less, and even more preferably 2 or less. The smaller the value, the better, but it is usually 0.1 or more.

[0026] Furthermore, the water-soluble resin nanomesh layer 11 is formed by placing the conductive material layer 12 of the nanomesh sheet 100 on an adherend (not shown) with the conductive material layer 12 of the nanomesh sheet 100 facing the adherend, dripping water from the mesh-like base layer 10 side to adhere the conductive material layer 12 onto the adherend, and removing the mesh-like base layer 10. The visible light transmittance of the water-soluble resin nanomesh layer 11 may be 90.0% or more and 99.9% or less, or may be 95.0% or more and 99.9% or less. By having the visible light transmittance in the above range, the water-soluble resin nanomesh layer 11 can be made less noticeable after the nanomesh sheet is adhered to the adherend. The above haze value and visible light transmittance can be set to desired values ​​by appropriately adjusting the resin material, fiber diameter, basis weight, porosity, etc. constituting the nanomesh layer of the water-soluble resin. The haze value is closely related to the film thickness and fiber remaining rate of the water-soluble resin film, and the haze value can be reduced by decreasing the film thickness and / or decreasing the fiber remaining rate in the film. On the other hand, the haze value can be increased by increasing the film thickness and / or increasing the fiber remaining rate in the film.

[0027] Another embodiment of the present invention is a nanomesh sheet having a mesh-like base layer on which a nanomesh layer of a water-soluble resin and a conductive material layer are laminated in this order, the nanomesh sheet being placed on an adherend with the conductive material layer of the nanomesh sheet facing the adherend, and water being dropped from the mesh-like base layer side to attach the conductive material layer to the adherend, and the water-soluble resin nanomesh layer after removing the mesh-like base layer has a UV light transmittance / visible light transmittance value of 0.95 or more and 1.0 or less.

[0028] The present inventors have newly discovered a problem that when the adherend to which a nanomesh sheet is applied is the skin, the degree of tanning differs between the area where the water-soluble resin film is formed and the other areas, resulting in noticeable tan marks. In response to this problem, the present inventors have set the UV light transmittance / visible light transmittance values ​​of the nanomesh layer of the water-soluble resin within the above-mentioned ranges, thereby making it possible to suppress unevenness in tan marks depending on the application location after the nanomesh sheet is applied to the skin. The value of the UV light transmittance / visible light transmittance is more preferably 0.98 to 1.0, which can reduce the difference in light transmittance for each wavelength in a wide wavelength range, and is particularly effective for a light source having a relatively high incident energy in the UV wavelength range, such as when used outdoors.

[0029] Furthermore, the water-soluble resin nanomesh layer 11 is formed by placing the conductive material layer 12 of the nanomesh sheet 100 on an adherend (not shown) with the conductive material layer 12 of the nanomesh sheet 100 facing the adherend, and attaching the conductive material layer 12 to the adherend by dripping water from the mesh-like base layer 10 side, and the UV light transmittance of the water-soluble resin nanomesh layer 11 after removing the mesh-like base layer 10 is generally preferably 80% or more. The UV transmittance of the nanomesh layer 11 is preferably 90% or more, and the smaller the value, the better, but is usually 99.9% or less.

[0030] The UV light transmittance of the water-soluble resin nanomesh layer 11 can be adjusted to a desired value by appropriately adjusting the resin material, film thickness, fiber diameter, and basis weight constituting the water-soluble resin nanomesh layer 11, as well as by adding (kneading) metal particles such as titanium oxide or an ultraviolet absorbing agent into the resin material constituting the nanomesh layer 11. When metal particles or an ultraviolet absorbing agent are added to 11, the haze value of the nanomesh layer 11 tends to increase as the amount added increases, so the amount added needs to be adjusted appropriately. UV light transmittance is closely related to the fiber diameter and fiber residual rate in the water-soluble resin coating, and because the fibers are denser than normal fiber aggregates of mm to μm order, it is possible for nm-order light to be diffused and scattered without being transmitted. Therefore, if you want to lower the UV light transmittance, you can control it by increasing the fiber residual rate in the coating. On the other hand, if you want to increase the UV light transmittance, you can control it by decreasing the fiber residual rate in the coating.

[0031] The nanomesh sheet of the present embodiment is attached to an adherend such as the skin with the mesh-like base layer side facing up, and when the nanomesh layer of water-soluble resin is brought into contact with water, the nanomesh of the water-soluble resin dissolves, and as the water dries, the water-soluble resin acts as an adhesive, forming a conductive material layer on the adherend, i.e., wiring or conductive circuits. In this case, water may be used, but an alcoholic solution may be used instead of water. The use of an alcoholic solution is preferable because it improves the drying speed of the liquid, makes it difficult for the water-soluble resin nanomesh to curl up, and suppresses positional deviation.

[0032] The alcohol is preferably one that can accelerate the evaporation of liquids containing water, and preferably contains ethyl alcohol, methyl alcohol, or isopropyl alcohol, or these may be mixed. The mixing ratio with water can be selected in the range of 5:95-98:2. Among these, the ratio of ethanol is preferably 90% to 50%, and alcohol used for disinfection (about 80% ethyl alcohol) is particularly preferable. It can also contain a surfactant, etc.

[0033] In addition, water or the like can be supplied to the nanomesh laminate according to this embodiment using a spray bottle or a carrier such as absorbent cotton soaked in water. By using the nanomesh laminate and the carrier integrally, a conductive circuit can be easily formed on the human body, which makes it very easy to attach a sensor for measuring various parameters of a sick patient, for example. In addition, the same circuit can be stably provided for many patients. In addition, there is little variation in the circuits formed for each patient, which can reduce errors in circuit formation. EXAMPLES

[0034] The present invention will be described in more detail below using examples, but it goes without saying that the scope of the present invention is not limited to the description of the examples. First, the measurement and evaluation tests carried out in the examples will be described.

[0035] <Method of measuring haze value and total light transmittance of water-soluble resin film> The haze value and total light transmittance of the water-soluble resin film were measured by placing the nanomesh sheet on a glass plate 20, dripping water from the mesh substrate layer (not shown) side to attach the conductive material layer 22 to the glass plate 20 via the water-soluble resin film 21, and drying the mesh substrate layer to remove it. The haze value and total light transmittance were measured in the normal direction (from above in the figure) to the glass plate 20 at a location on the glass plate 20 where only the water-soluble resin film 21 was present, using a haze meter NDH7000 manufactured by Nippon Denshoku Industries Co., Ltd. The calculation method for the haze value and total light transmittance was based on JIS K 7136. The haze value and total light transmittance of only the water-soluble resin film were calculated by dividing the measured values ​​by the haze value and total light transmittance of only the glass plate, respectively.

[0036] <Method for measuring the transmittance of water-soluble resin film in the visible and UV regions> The visible light transmittance and UV light transmittance of the water-soluble resin film were measured by placing the nanomesh sheet on a glass plate 20 as shown in FIG. 2 and dripping water onto the mesh substrate layer (not shown). By this, the conductive material layer 22 was attached to the glass plate 20 via the water-soluble resin film 21, and after drying, the mesh-like substrate layer was removed, and measurements were made in the normal direction (from above in the figure) to the glass plate 20 at the locations on the glass plate 20 where only the water-soluble resin film 21 was present, using a spectrophotometer U4100 manufactured by Hitachi High-Technologies Corporation. The light transmittance for each wavelength region was calculated in accordance with JIS R 3106. The light transmittance of only the water-soluble resin film was calculated by dividing the obtained measured value by the light transmittance of only the glass plate.

[0037] <Evaluation of visibility of water-soluble resin film> The nanomesh sheet was placed on the skin of the forearm, and water or an alcohol solution was dropped onto the mesh substrate layer side to attach the water-soluble resin to the skin, and after drying, the mesh substrate layer was removed. After the water-soluble resin film was formed, the area where the water-soluble resin film was attached was observed from a distance of 30 cm in a bright room to confirm whether the film was visible. The following were the evaluation criteria. ○: The boundary between the applied area and other areas is almost indistinguishable. △: The attached portion is partially visible. ×: The entire applied portion is visible.

[0038] <Evaluation of sunburn marks on water-soluble resin films> The nanomesh sheet was placed on the skin of the forearm, and water or an alcohol solution was dropped onto the mesh substrate layer side to attach the water-soluble resin to the skin. After drying, the mesh substrate layer was removed. After the water-soluble resin film was formed, the sheet was exposed to 1000 W / cm under AM1.5G conditions. 2 The water-soluble resin film was completely removed immediately after the exposure, and the area where the water-soluble resin film was applied was observed from a distance of 30 cm in a bright room to observe the condition of the sunburn marks. The following are the evaluation criteria. ○: The boundary between the applied area and other areas cannot be distinguished at all. △: The boundary between the applied area and other areas is vaguely visible. ×: The boundary between the applied area and other areas is clearly visible.

[0039] Example 1 [Preparation of network substrate] A mesh substrate (opening ratio 26%, square hole parallel type mesh, made of polypropylene, thickness 240 μm) was attached to the nanomesh forming section (on the drum) of a drum-type electrospinning device manufactured by Kato Tech.

[0040] [Production of nanomesh sheet] PVA (unmodified, saponification degree 88 mol%, 20 wt% aqueous solution viscosity 1052 mPa·s) was dissolved in pure water to prepare a 20 wt% aqueous PVA solution with a viscosity of 5 mPa·s, which was used as the spinning solution. The spinning solution (4 ml) was placed in a syringe in the electrospinning apparatus equipped with the mesh substrate prepared above, and an electrode was attached to the non-bevel needle 18G (Terumo Corporation) at the tip of the syringe. A nanomesh layer was produced by electrospinning, with a fiber diameter of 300 nm and a basis weight of 1.2 g / m. 2 The electrospinning apparatus settings were as follows: In this example, a nanomesh sheet without circuit formation was used instead of a sensor layer with a circuit formed of a conductive material. <Setting conditions> Target speed: 5m / min Traverse speed: 10cm / min Syringe speed: 0.050~0.080mm / min Voltage: 15~20kV Film formation time: 15 min

[0041] The nanomesh sheet obtained in Example 1 was evaluated. The nanomesh sheet was cut into a size of 3 cm square, and placed on a 4 cm square, 0.7 mm thick glass plate so that the nanomesh layer was in contact with it. Then, in an indoor environment of about 23 ° C, absorbent cotton soaked in water was pressed against the glass plate from the mesh-like base layer side for 3 minutes, and the water-soluble resin film was attached to the glass plate. After drying, the mesh-like base layer was removed, and the water-soluble resin film side was left standing near the spray nozzle of a humidifier for 3 minutes. The water-soluble resin film obtained on the glass plate was measured with a haze meter and a spectrophotometer. In addition, the water-soluble resin film was attached to the forearm skin of a subject with a body temperature of about 36 ° C in the same attachment process as described above, and visibility evaluation and sunburn mark evaluation were performed. The results obtained are shown in Table 1.

[0042] Example 2 Except for not spraying with a humidifier, the water-soluble resin film was applied and evaluated in the same manner as in Example 1. The results are shown in Table 1.

[0043] Example 3 The water-soluble resin film was applied and evaluated in the same manner as in Example 2, except that the liquid soaked in the absorbent cotton was changed to an alcohol aqueous solution (80% ethyl alcohol, 20% water) and the pressing time was changed to 3 minutes. The results are shown in Table 1.

[0044] Comparative Example 1 Except for changing the pressing time to 1 minute, the water-soluble resin film was applied and evaluated in the same manner as in Example 3. The obtained results are shown in Table 1.

[0045] [Table 1] [Explanation of symbols]

[0046] 100 Nanomesh Sheet 10 Mesh-like substrate layer 11 Nanomesh sheet made of water-soluble resin 12 Conductive material layer 20 Glass Plate 21 Water-soluble resin coating 22 Conductive material layer

Claims

[Claim 1] A nanomesh sheet on an adherend, comprising a nanomesh layer of a water-soluble resin attached to the adherend by dropping water or an alcohol aqueous solution thereon and a conductive material layer, the nanomesh sheet being laminated on the adherend, the haze value of the nanomesh layer of the water-soluble resin is 12 or less; The visible light transmittance is 95.0% or more and 99.9% or less, The UV light transmittance is 95.0% or more and 99.9% or less, And the value of the UV light transmittance / the visible light transmittance is 0.95 or more and 1.0 or less.

Citation Information

Patent Citations

  • Electronic functional member, electronic component, and wearable device

    JP2016112246A

  • Electronic functional member, method for manufacturing same, and biological measurement sensor

    WO2020179907A1