Method for producing rare earth transition metal alloy powder

By controlling temperature and pressure during hydrogen treatment, the method addresses decomposition issues in rare earth transition metal alloy powders, producing high-quality alloy powders with minimal foreign phases and enhanced magnetic properties.

JP7556327B2Active Publication Date: 2024-09-26SUMITOMO METAL MINING CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021084167
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-05-18
Publication Date
2024-09-26
Estimated Expiration
2041-05-18

AI Technical Summary

Technical Problem

Conventional methods for producing rare earth transition metal alloy powders using the reduction diffusion method face issues with decomposition during hydrogen treatment, leading to the precipitation of transition metal components as foreign phases, which deteriorate the alloy properties, particularly in materials for permanent magnets.

Method used

A method involving hydrogen treatment under specific temperature and pressure conditions is employed, maintaining the reaction product temperature at 300°C or less and ambient pressure at negative pressure to suppress decomposition while maintaining collapsibility, thereby producing rare earth transition metal alloy powders with few remaining foreign phases and good properties.

Benefits of technology

The method effectively suppresses decomposition during hydrogen treatment, resulting in rare earth transition metal alloy powders with improved properties and reduced foreign phases, enhancing the magnetic properties of materials like Sm2Fe17N3 alloy powder.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007556327000001
    Figure 0007556327000001
Patent Text Reader

Abstract

To provide a method for producing rare earth transition metal alloy powder using a reduction diffusion method which can suppress decomposition at the time of hydrogen treatment while maintaining collapsibility.SOLUTION: A method for producing rare earth transition metal alloy powder includes the following steps: mixing at least rare earth oxide powder, transition metal powder and a reduction agent and obtaining a mixture; heating the mixture under non-oxidation atmosphere, reducing rare earth transition powder, diffusing the reduced rare earth oxide powder into transition metal powder, and alloying the mixture, thereby obtaining a reaction product containing a rare earth transition metal alloy and a reduction agent-derived byproduct; exposing the reaction product to hydrogen atmosphere, thereby absorbing hydrogen and disintegrating the reaction product, and obtaining a disintegrated material; and cleaning the disintegrated material with cleaning liquid and obtaining alloy powder, and maintains a temperature of the reaction product at 300°C or lower when the reaction product is exposed to the hydrogen atmosphere, and holds an ambient pressure of the reaction product to be negative.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing rare earth transition metal alloy powder. [Background technology]

[0002] Rare earth transition metal alloy powder is an alloy powder mainly containing rare earth metals and transition metals. Rare earth transition metal alloy powder, especially intermetallic compound powder, is widely used in various applications such as permanent magnet materials, hydrogen storage materials, magneto-optical recording materials, and magnetic refrigeration materials. For example, Sm2Fe 17 Nitrided Sm2Fe alloy powder 17 N3 alloy powder, Nd2Fe 14 B alloy powder, SmCo5 alloy powder, Sm2Co 17 The LaNi5-based alloy powder and the PrCo5-based alloy powder have large magnetization and uniaxial magnetic anisotropy, and are useful as materials for permanent magnets. The LaNi5-based alloy powder is characterized by its ability to absorb and retain large amounts of hydrogen, and is used as a hydrogen storage material. The (Tb, Gd)-(Fe, Ni, Co)-based alloy powder can be used to form a thin film to form the recording layer of a magneto-optical recording medium. Furthermore, the La(Fe, Si) 13 La(Fe,Si) based alloy powder and its hydrogenated form 13 H x The alloy powders based on this system exhibit excellent magnetocaloric effects and are considered to be promising magnetic refrigeration materials.

[0003] Known methods for producing rare earth transition metal alloy powder include melting and casting, reduction and diffusion, etc. Among these, the melting and casting method is a method in which rare earth metals and transition metals are used as raw materials, these raw materials are mixed and melted in an inert gas atmosphere, the obtained alloy ingot is heat-treated to be homogenized, and then pulverized.

[0004] On the other hand, the reduction-diffusion method is a method in which rare earth oxides and transition metals are used as raw materials, mixed with a reducing agent, and then heated in an inert gas atmosphere to obtain a rare earth-transition metal alloy. During the heat treatment, the rare earth oxides are reduced to rare earth metals, and the rare earth metals diffuse into the transition metals to form an alloy. Components derived from the reducing agent remain in the reaction product obtained by the heat treatment. Therefore, the reaction product is put into water to dissolve and remove the components derived from the reducing agent. Also, by putting it into water, the alloy components in the reaction product are broken down and powdered. The reduction-diffusion method has the advantages of being able to use inexpensive rare earth oxides as raw materials, being simple in process, and being able to produce alloy powder at a lower cost than the melting casting method. Furthermore, by nitriding the alloy powder obtained by reduction-diffusion, it is possible to obtain rare earth-transition metal alloy powder as a nitride.

[0005] In the reduction-diffusion method, the raw material mixture is heated to cause a reduction-diffusion reaction, thereby obtaining a reaction product. In this case, the reaction product may shrink and form a strong mass. Even if such a strong mass is put into water, it has poor disintegrability and does not pulverize sufficiently. Such deterioration in disintegrability may be a factor in reducing the product yield. Therefore, it is required to improve the disintegrability. For this purpose, it has been proposed to improve the disintegrability by subjecting the reaction product obtained by the reduction-diffusion reaction to hydrogen treatment. When the reaction product is exposed to a hydrogen atmosphere, the rare earth metal in the reaction product absorbs hydrogen, which causes a volume expansion. This volume expansion makes the reaction product embrittled and increases its disintegrability.

[0006] Patent Documents 1 to 3 are examples of documents disclosing techniques for improving disintegrability by hydrogen treatment. Patent Document 1 describes a method for producing alloy powder containing rare earths and transition metals by a reduction diffusion method, in which the fired product is hydrogen-treated after firing, and the hydrogen-treated fired product undergoes natural disintegration simply by being cooled to room temperature and exposed to the air, and not only can it omit the previously required coarse crushing step of the fired product, but also can shorten the time required for the subsequent water washing and separation step, since the product disintegrates into fine particles (claim 1,

[0001] and

[0014] of Patent Document 1).

[0007] Patent Document 2 relates to a method for producing rare earth transition metal alloy powder using a reduction diffusion method, in which the alloy is placed in a sealed container, the atmospheric gas is discharged, and then hydrogen pressure treatment is performed at a pressure higher than atmospheric pressure to cause the alloy to self-heat, and it is described that the resulting reduction product has significantly improved disintegrability in water, making it possible to omit the crushing step used in conventional methods, reduce the amount of material left over when sieving before washing by decantation, and also reduce the number of decantation steps, thereby not only improving productivity but also reducing the amount of waste liquid to be treated (Claim 1 and

[0070] of Patent Document 2).

[0008] Patent Document 3 describes a method for producing rare earth transition metal alloy powder, which includes a reduction diffusion step of synthesizing a rare earth transition metal alloy by a reduction diffusion method, a hydrogen treatment step of loading the obtained reaction product into a sealed container and treating it with hydrogen, a water washing step, and an acid washing step, in which the hydrogen treatment step is performed by first reducing the pressure inside the sealed container to discharge the atmospheric gas, then filling it with hydrogen to a pressure 0.01 to 0.11 MPa higher than atmospheric pressure, causing the alloy to self-heat, and then continuing to pressurize the container with hydrogen to a pressure higher than atmospheric pressure until the alloy substantially no longer generates heat (claims 1 and 3 of Patent Document 3). [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Japanese Patent Application Publication No. 09-241708 [Patent Document 2] JP 2004-204285 A [Patent Document 3] JP 2005-008950 A Summary of the Invention [Problem to be solved by the invention]

[0010] In this way, when producing rare earth transition metal alloy powder by the reduction diffusion method, it has been proposed to improve the disintegrability of the reaction product by subjecting the reaction product after heat treatment to hydrogen treatment. Although such conventional methods have a certain effect in improving disintegrability, there is still room for improvement.

[0011] That is, the inventors have found that when hydrogen treatment is performed by the conventional method, the intermetallic compounds contained in the reaction product may decompose, and the transition metal components may precipitate as fine particles. When such decomposition occurs, the transition metal components that are not alloyed remain as heterophases in the finally obtained alloy powder, which may significantly deteriorate the alloy properties. For example, when the alloy powder is a material containing iron (Fe) as a transition metal, such as a material for permanent magnets, αFe with small magnetic anisotropy remains, resulting in a problem of a significant decrease in coercive force and residual magnetization. Therefore, it has been difficult to obtain a rare earth transition metal alloy powder with good properties and few heterophases by the conventional method.

[0012] The present inventors have conducted extensive research in light of these problems, and have found that, in a method for producing rare earth-transition metal alloy powder using a reduction-diffusion method, by carrying out hydrogen treatment under specific temperature and pressure conditions, it is possible to suppress decomposition during hydrogen treatment while maintaining disintegrability, and as a result, it is possible to obtain rare earth-transition metal alloy powder with excellent properties and with little residual heterogeneous phases.

[0013] The present invention was completed based on these findings, and an object of the present invention is to provide a method for producing rare earth transition metal alloy powder using a reduction diffusion method, which can suppress decomposition during hydrogen treatment while maintaining disintegrability. [Means for solving the problem]

[0014] The present invention includes the following aspects (1) to (7). In this specification, the expression "to" includes both ends of the expression. In other words, "X to Y" is synonymous with "X or more and Y or less."

[0015] (1) A method for producing a rare earth-transition metal alloy powder, comprising the steps of: Mixing at least a rare earth oxide powder, a transition metal powder, and a reducing agent to obtain a mixture; a step of subjecting the mixture to a heat treatment in a non-oxidizing atmosphere to reduce the rare earth oxide powder and to diffuse the rare earth oxide powder into the transition metal powder to form an alloy, thereby obtaining a reaction product containing a rare earth transition metal alloy and a by-product derived from the reducing agent; exposing the reaction product to a hydrogen atmosphere, thereby absorbing hydrogen and disintegrating the reaction product to obtain a disintegrated material; and washing the crushed product with a washing liquid to obtain an alloy powder. The method comprises exposing the reaction product to a hydrogen atmosphere while maintaining a temperature of the reaction product below 300° C. and maintaining a negative pressure around the reaction product.

[0016] (2) The method according to (1) above, wherein the temperature of the reaction product is maintained at 295° C. or less when the reaction product is exposed to a hydrogen atmosphere.

[0017] (3) The method according to (1) or (2) above, wherein the pressure around the reaction product is maintained at a negative pressure of -15 kPa or less when the reaction product is exposed to a hydrogen atmosphere.

[0018] (4) Any of the above methods (1) to (3), wherein the temperature of the reaction product is adjusted by controlling the amount of hydrogen supplied and / or the treatment temperature when the reaction product is exposed to a hydrogen atmosphere.

[0019] (5) Any of the above-mentioned methods (1) to (4), wherein the rare earth oxide powder is an oxide powder of one or more metals selected from the group consisting of yttrium (Y), lanthanum (La), cerium (Ce), praseodymium (Pr), neodymium (Nd), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), and ytterbium (Yb).

[0020] (6) The method according to any one of (1) to (5) above, wherein the transition metal powder is a powder of one or more metals selected from the group consisting of iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), chromium (Cr), manganese (Mn), zinc (Zn), molybdenum (Mo), and tungsten (W).

[0021] (7) Any of the above methods (1) to (6), further comprising a step of nitriding the crushed material and / or the alloy powder. Effect of the Invention

[0022] According to the present invention, there is provided a method for producing rare earth transition metal alloy powder using a reduction-diffusion method, which can suppress decomposition during hydrogen treatment while maintaining disintegrability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] A specific embodiment of the present invention (hereinafter, referred to as the present embodiment) will be described. Note that the present invention is not limited to the following embodiment, and various modifications are possible within the scope of the present invention.

[0024] <<Production method of rare earth transition metal alloy powder>> The method for producing the rare earth transition metal alloy powder (hereinafter, sometimes simply referred to as "alloy powder") of this embodiment includes the following steps: a step of mixing at least a rare earth oxide powder, a transition metal powder, and a reducing agent to obtain a mixture (raw material mixing step), a step of heat-treating the mixture in a non-oxidizing atmosphere to reduce the rare earth oxide powder and diffuse it into the transition metal powder to form an alloy, thereby obtaining a reaction product containing a rare earth transition metal alloy and a by-product derived from the reducing agent (reduction diffusion step), a step of exposing the reaction product to a hydrogen atmosphere, thereby absorbing hydrogen and crushing it to obtain a crushed product (hydrogen treatment step), and a step of washing the crushed product with a washing liquid to obtain an alloy powder (wet treatment step). When exposing the reaction product to the hydrogen atmosphere, the temperature of the reaction product is maintained at 300°C or less, and the ambient pressure of the reaction product is maintained at a negative pressure.

[0025] <Rare earth transition metal alloy powder> The rare earth transition metal alloy powder of this embodiment is a powder composed of an alloy containing a rare earth metal and a transition metal. Here, rare earth metal is a general term for metals (elements) constituting a group consisting of scandium (Sc) with atomic number 21, yttrium (Y) with atomic number 39, and lanthanum (La) with atomic number 57 to lutetium (Lu) with atomic number 71 in the periodic table. Transition metal is a general term for metals (elements) between group 3 elements and group 11 elements in the periodic table. Furthermore, the concept of alloy includes not only solid solutions but also eutectic bodies and intermetallic compounds. Examples of intermetallic compounds include CaCu5 type, Th2Zn 17 type, Th2Ni 17 type, TbCu7 type, ThMn 12 Type, NaZn 13 Type, Nd2Fe 14 Examples of the alloy powder include compounds having crystal structures such as B type, MgCu2 type, etc. Furthermore, the alloy powder of this embodiment may contain only rare earth metals and transition metals, or may contain other components. For example, it may contain components such as boron (B), carbon (C), nitrogen (N), magnesium (Mg), aluminum (Al), and silicon (Si).

[0026] The rare earth transition metal alloy powder is not limited in composition as long as it is an alloy mainly containing rare earth metals and transition metals. For example, SmFe 17 and its nitrided form, Sm2Fe 17 N3, Nd2Fe 14 B, SmCo5, Sm2Co 17 and PrCo5. Hydrogen storage materials and magneto-optical recording materials such as LaNi5 and (Tb, Gd)-(Fe, Ni, Co) are also suitable. La(Fe, Si) 13 and its hydrogenated form, La(Fe,Si) 13 H x The magnetic refrigeration material may be any of the above.

[0027] <Raw material mixing process> In the raw material mixing step, at least a rare earth oxide powder, a transition metal powder, and a reducing agent are mixed to obtain a mixture.

[0028] The rare earth oxide powder is a raw material of rare earth elements that constitute the target alloy powder. Although not limited thereto, one or more oxide powders selected from the group consisting of yttrium (Y), lanthanum (La), cerium (Ce), praseodymium (Pr), neodymium (Nd), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), and ytterbium (Yb) are preferred. As the rare earth oxide powder, one type of powder may be used alone, or two or more types of powders may be mixed and used.

[0029] The rare earth oxide powder may be selected according to the composition of the desired alloy powder. For example, samarium iron nitrogen (SmFe 17 N3) alloy powder and samarium cobalt (Sm2Co5, Sm2Co 17 When manufacturing alloy powders based on neodymium iron boron (NdFe 14 When producing B) type alloy powder, neodymium oxide (Nd2O3) should be selected.

[0030] The particle size of the rare earth oxide powder may be determined according to the composition and use of the alloy powder obtained. However, it is desirable to determine the particle size of the rare earth oxide powder so that it is uniformly distributed in the vicinity of the transition metal particles in the resulting mixture. The average particle size of the rare earth oxide powder is preferably 50 μm or less, more preferably 20 μm or less, and even more preferably 10 μm or less. The rare earth oxide powder may contain moisture or organic matter as impurities. These impurities may increase the oxygen content of the finally obtained alloy powder. Therefore, it is preferable that the amount of impurities contained in the rare earth oxide powder is small. For example, the heat loss after heating to 1000° C. is preferably 2 mass % or less, more preferably 1 mass % or less.

[0031] The amount of the rare earth oxide powder is preferably 1.0 to 1.5 times, and more preferably 1.05 to 1.2 times, the amount (equivalent) required to form an alloy powder of the target composition. For example, samarium iron nitrogen (SmFe 17 When manufacturing alloy powder based on samarium oxide (Sm2O3), the amount of samarium oxide (Sm2Fe 17 N3) is preferably 1.0 to 1.5 times the amount required. By making the amount of rare earth oxide 1.0 times or more the equivalent amount, the rare earth metal (rare earth element) can be sufficiently diffused into the transition metal powder, and the desired properties can be sufficiently imparted to the finally obtained alloy powder. On the other hand, by making the amount 1.5 times or less the equivalent amount, the formation of a rare earth-rich heterophase can be suppressed.

[0032] The transition metal powder is a raw material of the transition metal that constitutes the desired alloy powder. Although not limited thereto, one or more selected from the group consisting of iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), chromium (Cr), manganese (Mn), zinc (Zn), molybdenum (Mo), and tungsten (W) are preferred. As the transition metal powder, one type of powder may be used alone, or two or more types of powder may be mixed and used.

[0033] The transition metal powder may be selected according to the composition of the desired alloy powder. For example, samarium iron nitrogen (SmFe 17 N3) alloy powder and neodymium iron boron (Nd2Fe 14 When producing B)-based alloy powder, iron (Fe) powder should be selected. The iron powder may be reduced iron powder, gas atomized powder, water atomized powder, and / or electrolytic iron powder. Samarium cobalt (Sm2Co5, Sm2Co 17 When producing a Cr-based alloy powder, cobalt (Co) powder should be selected.

[0034] The particle size of the transition metal powder may be determined according to the composition and application of the alloy powder obtained. However, if the particle size of the transition metal powder is excessively large, the diffusion of the rare earth metal does not progress sufficiently to the inside in the subsequent reduction diffusion process, and an unalloyed phase may remain. The average particle size of the transition metal powder is preferably 100 μm or less, more preferably 80 μm or less, further preferably 60 μm or less, and particularly preferably 50 μm or less. In addition, it is preferable that the amount of impurities contained in the transition metal powder is small. For example, the heat loss after heating to 1000° C. is preferably 2 mass % or less, more preferably 1 mass % or less.

[0035] The reducing agent is added in the subsequent reduction diffusion step to reduce oxide components such as rare earth oxide powder and promote alloy formation. At least one selected from alkali metals, alkaline earth metals, and hydrides thereof is used as the reducing agent. Specifically, at least one selected from the group consisting of lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), and hydrides thereof is preferred. From the viewpoints of safety during handling and cost, lithium (Li) and / or calcium (Ca) are more preferred, and calcium (Ca) is particularly preferred.

[0036] The reducing agent is preferably used in the form of granules or powder. The average particle size of the reducing agent is preferably 10 mm or less, more preferably 0.1 mm to 7 mm, and even more preferably 0.2 mm to 5 mm. The amount of the reducing agent is preferably 1.0 to 10.0 times the amount (equivalent) required to reduce oxide components such as rare earth oxide powder, more preferably 1.0 to 3.0 times, and even more preferably 1.1 to 2.0 times. If the amount of the reducing agent is too small, the reduction and diffusion of the oxide components may not proceed sufficiently, and oxides may remain in the alloy powder. If the amount of the reducing agent is too large, it is difficult to remove the remaining components in the washing process.

[0037] If necessary, other components may be added in addition to the rare earth oxide powder, transition metal powder, and reducing agent. For example, rare earth metal powder and / or transition metal oxide powder may be added. Also, alloy powder of rare earth metal and transition metal or oxide powder thereof may be added. Furthermore, when producing alloy powder containing components other than rare earth metal and transition metal, raw materials of other components may be added. For example, Nd2Fe, which is a permanent magnet material, may be added. 14 To produce B alloy powder, a boron source such as boron (B) or boron oxide (BO) may be added. 13 H x In order to produce the alloy powder, a silicon source such as silicon (Si) or silicon oxide (SiO2) may be added. Furthermore, auxiliary additives may be added to facilitate the production of the alloy powder. Examples of auxiliary additives include disintegration promoters that promote disintegration of the reaction product in the subsequent wet processing step. As disintegration promoters, alkaline earth metal salts such as calcium chloride (CaCl2) and calcium oxide (CaO) or alkaline earth metal oxides can be used.

[0038] The raw materials are mixed uniformly by mixing the rare earth oxide powder, transition metal powder, reducing agent, and other components added as required, using a known mixer such as a ribbon blender, a tumbler, an S-shaped blender, a V-shaped blender, a Nauta mixer, a Henschel mixer, a super mixer, a high-speed mixer, a ball mill, a vibration mill, an attritor, or a jet mill.

[0039] <Reduction and diffusion process> In the reduction diffusion step, the mixture is subjected to a heat treatment in a non-oxidizing atmosphere to obtain a reaction product. Here, the non-oxidizing atmosphere is an atmosphere that does not substantially contain oxygen. As the atmospheric gas, an inert gas, for example, argon gas and / or helium gas, is preferable. The amount of oxygen in the atmosphere is preferably 5% or less, more preferably 1% or less.

[0040] When the mixture is heated in a non-oxidizing atmosphere, the rare earth oxide powder is reduced by the action of the reducing agent to produce rare earth metals. The produced rare earth metals diffuse into the transition metal powder and are alloyed to form a rare earth transition metal alloy. If the mixture contains oxides of components other than the rare earth oxide powder, the oxides of the other components are also reduced and diffused and incorporated into the alloy. Meanwhile, the reducing agent is oxidized to produce an oxide.

[0041] For example, samarium iron nitrogen (SmFe) can be produced by using samarium oxide (Sm2O3) as the rare earth oxide powder, iron (Fe) powder as the transition metal powder, and calcium metal (Ca) as the reducing agent. 17 When manufacturing samarium oxide (Sm2O3) based alloy powder, the reducing agent (Ca) reduces it to samarium (Sm). The reduced samarium (Sm) diffuses into the iron (Fe) powder and becomes Th2Zn 17 Samarium-iron alloys (SmFe 17 ) is produced. Meanwhile, metallic calcium (Ca), which is a reducing agent, is oxidized to calcium oxide (CaO). When metallic calcium is mixed in an amount greater than the equivalent amount, excess calcium (Ca) remains. This calcium oxide (CaO) and excess calcium (Ca) constitute by-products. In some cases, heterogeneous phases such as samarium iron compound (SmFe3) may also be produced. Therefore, the reaction product after heat treatment is a rare earth transition metal alloy component (Sm2Fe 17 The product of this heat treatment is usually a porous ingot.

[0042] The heat treatment is performed at a temperature at which the reducing agent melts and at which the rare earth transition metal alloy components obtained do not melt. Specifically, the heat treatment temperature is preferably 900 to 1180°C. By setting the temperature at 900°C or higher, the rare earth metal diffuses uniformly into the transition metal powder, and the properties of the finally obtained alloy powder can be improved. On the other hand, by setting the temperature at 1180°C or lower, the rare earth transition metal alloy components are prevented from excessively growing into coarse grains. As a result, for example, when producing a nitride-based alloy powder, the rare earth transition metal alloy components are uniformly nitrided in the subsequent nitriding process, and the saturation magnetization and squareness of the magnet powder are improved. In addition, a low heat treatment temperature allows the amount of rare earth metal oxide to be reduced. This is because the evaporation of rare earth metals such as samarium (Sm) is suppressed.

[0043] The heat treatment holding time is preferably 3 to 10 hours. In this range, the primary particle size of the rare earth transition metal alloy component in the reaction product becomes small. Therefore, for example, when producing a nitride alloy powder, nitrogen can easily diffuse from the grain boundary of the rare earth transition alloy in the subsequent nitriding process, so that the nitriding distance can be shortened.

[0044] <Hydrogen treatment process> In the hydrogen treatment process, the reaction product is crushed by exposing it to a hydrogen atmosphere, thereby obtaining crushed material, while maintaining the temperature of the reaction product at 300°C or less and maintaining the pressure around the reaction product at a negative pressure.

[0045] Many rare earth transition metal alloys (intermetallic compounds) expand in volume when they absorb hydrogen. For example, SmFe3 expands in volume by 19% when it absorbs hydrogen. Similarly, Sm2Fe 17 is 3.4%, Nd2Fe 14B expands by 5.4%, LaNi5 by 27%, and SmCo5 by 7.4%. The temperature at which intermetallic compounds absorb hydrogen varies depending on the type of compound and its surface properties. However, all hydrogen absorption reactions are exothermic. Therefore, when a rare earth transition metal alloy contains multiple intermetallic compounds, a chain reaction may occur. In other words, absorption begins with a compound that absorbs hydrogen at a low temperature, which generates heat, which raises the temperature of the alloy, causing the next compound to absorb hydrogen.

[0046] By the way, hydrogen reversibly penetrates between the lattices of intermetallic compounds. If the temperature is too high, the intermetallic compounds may decompose. For example, when an SmFe alloy containing about 27 wt% Sm is produced by the reduction diffusion method, Sm2Fe 17 Intermetallic compound particles and Sm-rich particles such as SmFe3 and SmFe2 intermetallic compounds are formed. When this reaction product is exposed to hydrogen, hydrogen absorption begins in the Sm-rich particles, followed by the formation of Sm2Fe 17 The particles absorb hydrogen. If hydrogen absorption occurs rapidly in a short time, localized heat accumulation can cause a sudden rise in temperature, which can result in the decomposition of the intermetallic compound and the precipitation of αFe. Such decomposition of the intermetallic compound is undesirable because it reduces the properties of the desired alloy powder. For example, Sm2Fe 17 If decomposition of the intermetallic compound occurs during particle production and αFe precipitates, the resulting Sm2Fe 17 The particles are nitrided to form Sm2Fe 17 Even if N3 magnet powder is produced, the magnetic properties of this magnet powder, particularly the coercive force, are reduced.

[0047] Therefore, in the manufacturing method of this embodiment, the temperature of the reaction product is maintained at 300°C or less during hydrogen treatment. This is because if the reaction product temperature exceeds 300°C, the rare earth transition metal intermetallic compound decomposes and the transition metal components such as αFe are separated out, and the compound cannot fully exhibit the properties expected of it. The temperature of the reaction product is preferably maintained at 295°C or less, more preferably 260°C or less, and even more preferably 160°C or less.

[0048] There is no particular limitation on the means for controlling the temperature of the reaction product. However, it is preferable to adjust the amount of hydrogen supply and the treatment temperature. If the amount of hydrogen supply is appropriately adjusted relative to the amount of reaction product, hydrogen absorption can proceed gradually. Therefore, a sudden increase in temperature can be suppressed. Hydrogen treatment can be performed at room temperature. However, depending on the state of the intermetallic compounds contained in the reaction product, it is also effective to treat the reaction product by appropriately heating it under a hydrogen atmosphere. In this case, the rate of temperature rise and the holding temperature are appropriately adjusted to suppress hydrogen absorption, thereby suppressing the temperature rise.

[0049] In the manufacturing method of this embodiment, the ambient pressure of the reaction product is kept at a negative pressure. In order to maintain the reaction product at a low temperature of 300° C. or less, the hydrogen partial pressure for the reaction product may be lowered to gradually absorb hydrogen. In order to lower the hydrogen partial pressure, for example, the amount of hydrogen supplied may be suppressed, or a mixture of hydrogen gas and an inert gas may be used. If the amount of hydrogen supplied is suppressed by such a method, the hydrogen treatment is performed under a negative pressure less than atmospheric pressure. Therefore, it is possible to easily maintain the reaction product at a low temperature. Although the internal pressure of the treatment furnace becomes negative, there is no problem as long as the treatment is continued in an airtight state. The ambient pressure of the reaction product is preferably kept at −15 kPa or less, more preferably −30 kPa or less, and even more preferably −60 kPa or less. There is no particular limit to the lower limit of the ambient pressure. However, it is typically −90 kPa or more.

[0050] The hydrogen treatment is carried out in a hydrogen atmosphere using a hydrogen-containing gas. As the hydrogen-containing gas, hydrogen (H2) gas may be used alone, or a mixture of an inert gas such as argon (Ar) or helium (He) and hydrogen (H2) gas may be used. However, it is preferable to use hydrogen gas alone. In this case, in order to prevent oxygen (O2) from remaining, it is preferable to replace the atmosphere in the furnace with an inert gas such as argon before introducing hydrogen gas. In this case, it is preferable to evacuate the furnace once after replacing with the inert gas, and then introduce hydrogen gas. After the hydrogen treatment is completed, the gas is switched to an inert gas such as argon and the crushed material is recovered.

[0051] <Wet processing process> In the wet treatment process, the crushed material is washed with a washing liquid to obtain alloy powder. Specifically, the hydrogen-treated reaction product (crushed material) is put into the washing liquid and stirred. The product put into the washing liquid is broken down and becomes a slurry. At this time, the by-product derived from the reducing agent reacts with water and changes to a solid by-product-derived component consisting of hydroxide. Therefore, the solid by-product-derived component contains hydroxides of alkali metals and / or alkaline earth metals. For example, when metal calcium (Ca) is used as the reducing agent, the product after the reduction diffusion process contains rare earth transition metal alloy components and by-products (CaO, Ca). During water washing, this by-product (CaO, Ca) reacts with water and changes to calcium hydroxide (Ca(OH)2). Since calcium hydroxide has low solubility in water, most of it becomes a suspended solid and floats in the water. The slurry obtained by water washing is a suspension of rare earth transition metal alloy components and solid by-product-derived components (Ca(OH)2). By separating the solid by-product-derived components in the slurry from the rare earth-transition metal alloy components, a high-purity, high-performance alloy powder can be obtained.

[0052] The cleaning solution may be water, glycol, or a mixture of water and glycol. The water is preferably ion-exchanged water. The glycol is preferably one or more selected from the group consisting of ethylene glycol, propylene glycol, diethylene glycol, dipropylene glycol, triethylene glycol, and tripropylene glycol.

[0053] The solid by-product-derived components can be separated by decantation. Decantation may be performed once or multiple times. For example, the crushed material is put into a washing liquid, stirred, and allowed to stand, and then the supernatant liquid is removed. The washing liquid is further added to the obtained residue, and the mixture is stirred and allowed to stand, after which the supernatant liquid is removed. The rare earth transition metal alloy components have a relatively large specific gravity, whereas the solid by-product-derived components have a small specific gravity. Therefore, the solid by-product-derived components having a small specific gravity can be separated and removed together with the supernatant liquid by decantation. Alternatively, instead of performing decantation, the solid by-product-derived components may be separated and removed using a gravity separator such as a liquid cyclone or a centrifuge.

[0054] During the wet treatment, the crushed material may be subjected to an acid pickling treatment. This makes it possible to more effectively remove solid by-product-derived components and foreign phases. For example, it is possible to remove solid by-product-derived components (Ca(OH)2, etc.) that could not be completely removed during treatment with the cleaning solution together with foreign phases (SmFe3, etc.) in the product. The acid pickling treatment can be performed, for example, by putting the product into water and adding an acid while stirring. As the type of acid, inorganic acids such as hydrochloric acid, acetic acid, nitric acid, and sulfuric acid, or organic acids can be used.

[0055] The manufacturing method of this embodiment may further include a step of nitriding the product (nitriding treatment step) as necessary. By including this step, samarium iron nitrogen (SmFe 17 Nitriding can be performed at any time after the hydrogen treatment step. The crushed material obtained in the hydrogen treatment step may be nitrided, or the alloy powder obtained in the wet treatment step may be nitrided.

[0056] In the nitriding treatment, the product (crushed material, alloy powder) is heated to preferably 350 to 500°C, more preferably 400 to 480°C, while a mixed gas flow containing ammonia is passed through it. This causes the rare earth transition metal alloy components to be nitrided. If the heating temperature is 350°C or higher, the nitriding reaction takes place in a short time, improving efficiency. On the other hand, if the heating temperature is too high, the main phase may decompose. For example, samarium iron (Sm2Fe 17 The rare earth-transition metal alloy components are nitrided to form samarium iron nitrogen (SmFe 17 When producing samarium iron (SmFeN3)-based alloy powder, if the nitriding temperature is too high, the main phase 17 ) may decompose to form αFe. Since αFe reduces the squareness of the demagnetization curve of the magnet powder, its formation is undesirable. By setting the nitriding temperature to 500°C or less, it is possible to suppress the decomposition of the main phase. The holding time depends on the amount of material to be treated, but is preferably 5 to 10 hours.

[0057] The nitriding gas circulated during the nitriding process should contain at least nitrogen atoms, and nitrogen gas or ammonia gas is suitable. In addition, hydrogen, argon, etc. may be further contained to control the reaction. When a mixed gas flow of ammonia and hydrogen is used, the mixture ratio (gas flow ratio) is preferably ammonia:hydrogen=10-70:30-90, more preferably 30-60:40-70. Within this range, the flow rate of ammonia becomes sufficient, and the nitriding efficiency is further improved.

[0058] <Heat treatment process> If necessary, the product (nitride alloy powder) obtained by the nitriding treatment may be further subjected to a heat treatment in an inert gas atmosphere. Examples of the inert gas include hydrogen gas, nitrogen gas, argon gas, and helium gas. By performing such a heat treatment, the nitrogen distribution in each crystal cell constituting the obtained alloy powder becomes uniform, and the properties of the alloy powder can be further improved. The heat treatment temperature is preferably 350 to 500°C, and more preferably 400 to 480°C. The holding time is preferably 20 to 200 minutes, and more preferably 30 to 150 minutes.

[0059] <Fine grinding process> If necessary, the product (alloy powder) obtained in the wet treatment, nitriding treatment, or heat treatment process may be finely pulverized. In the fine pulverization process, the pulverized material is placed in a pulverizer together with media and pulverized until the average particle size is 1 to 3 μm. As the media, isopropyl alcohol, ethanol, toluene, methanol, hexane, etc. can be used. In addition, by adding a surface treatment agent to the media, it is possible to perform surface treatment of the alloy powder simultaneously with pulverization. As the surface treatment agent, phosphate compounds such as orthophosphoric acid, disodium hydrogen phosphate, pyrophosphoric acid, metaphosphoric acid, manganese phosphate, zinc phosphate, and aluminum phosphate can be mentioned.

[0060] In this manner, the rare earth transition metal alloy powder of the present embodiment can be manufactured. The average particle size (x50) of the alloy powder is not particularly limited and may be appropriately set according to the application. The average particle size may be, for example, 1.0 μm or more and 10.0 μm or less, 1.5 μm or more and 5.0 μm or less, or 1.7 μm or more and 3.0 μm or less. The alloy powder of the present embodiment preferably does not contain a transition metal component such as αFe as a heterogeneous phase. The presence of the heterogeneous phase can be confirmed by analyzing the alloy powder by X-ray diffraction (XRD).

[0061] According to the manufacturing method of this embodiment, by providing hydrogen treatment, it is possible to increase the disintegrability of the reaction product obtained by the reduction-diffusion reaction, and to obtain fine alloy powder. In addition, by maintaining the temperature of the reaction product during hydrogen treatment at 300°C or less and keeping the ambient pressure at a negative pressure, it is possible to suppress decomposition during hydrogen treatment and the resulting formation of heterogeneous phases while maintaining the disintegrability. Therefore, it is possible to obtain rare earth transition metal alloy powder with good properties and little residual heterogeneous phases.

[0062] In contrast, in the manufacturing methods proposed in Patent Documents 1 to 3, hydrogen treatment is performed under atmospheric pressure or under pressure. If hydrogen treatment is performed under an atmosphere above atmospheric pressure, hydrogen absorption proceeds excessively quickly. In addition, in the manufacturing methods proposed in Patent Documents 1 to 3, although the ambient temperature during the reduction diffusion treatment is adjusted, the temperature of the reaction product itself is not controlled. Therefore, the temperature of the reaction product becomes high and exceeds 300°C, and as a result, the reaction product may decompose and produce heterogeneous phases such as αFe, which causes deterioration of characteristics. EXAMPLES

[0063] [Example 1] In Example 1, SmFe 17 The N3 alloy powder was prepared and evaluated. The manufacturing conditions and evaluation results of the alloy powder are summarized in Table 1.

[0064] (1) Preparation of alloy powder <Mixing process> A mixture was obtained by mixing 53 g of samarium oxide (Sm2O3) powder, 130 g of iron (Fe) powder, and 21 g of metallic calcium (Ca).

[0065] <Reduction and diffusion process> The mixture was placed in an iron reaction vessel, argon gas was sealed inside, and the vessel was then loaded into a heating furnace. The reaction vessel containing the mixture was heated to 1100°C over 4 hours and held at this temperature for 6 hours to allow the mixture to undergo a reduction-diffusion reaction. The reaction vessel was then cooled to room temperature while still in the heating furnace, and the reaction product was removed from the reaction vessel. 203 g of reaction product was obtained. This reaction product was in a hard sintered state.

[0066] <Hydrogen treatment> The resulting reaction product was treated with hydrogen to obtain a crushed material. Specifically, the reaction product was put into a tubular furnace, and the inside of the furnace was evacuated until the pressure reached -100 kPa. Hydrogen was then introduced until the pressure inside the furnace reached atmospheric pressure, and hydrogen was then allowed to flow at a flow rate of 1 L / min at room temperature. After a while, hydrogen absorption began. The exhaust valve of the tubular furnace was then closed, and hydrogen was continued to be supplied at a flow rate of 1 L / min while maintaining the pressure inside the furnace at negative pressure. Hydrogen supply was continued until hydrogen absorption was completed and the pressure inside the furnace returned to atmospheric pressure. During hydrogen absorption, the internal pressure of the furnace reached a negative pressure of -40 kPa. The maximum temperature of the reaction product reached 148°C due to the heat generated by hydrogen absorption. The temperature of the reaction product was measured by directly contacting a thermocouple with the reaction product.

[0067] <Nitriding treatment> Next, the hydrogen-treated reaction product (crushed material) was nitrided. Specifically, a mixture of ammonia and hydrogen gas was flowed while the hydrogen-treated reaction product was placed in a tubular furnace, and the temperature was raised and the heat treatment was performed at 440°C for 10 hours. At this time, the flow rate of ammonia was 29 mL / min and the flow rate of hydrogen was 9 mL / min.

[0068] <Wet processing> After cooling, the collected reaction product (nitride) was added to 300 mL of water to form a slurry, and decantation was repeated 10 times using ion-exchanged water. Then, 29 g of acetic acid was added while stirring the slurry, and decantation was repeated 10 times using ion-exchanged water again. The ion-exchanged water was replaced with ethanol, and the mixture was filtered. The collected cake was dried under reduced pressure at 200°C. This resulted in a rare earth transition metal alloy powder.

[0069] (2) Evaluation The alloy powder thus obtained was evaluated for various properties as follows.

[0070] <Composition analysis> The samarium (Sm) and calcium (Ca) contents of the alloy powder were measured by IPC emission spectrometry, the nitrogen (N) content was measured by inert gas fusion thermal conductivity method, and the oxygen (O2) and hydrogen (H2) contents were measured by inert gas fusion infrared absorption method.

[0071] <xrd> The crystal phase in the alloy powder was identified by powder X-ray diffraction. X-ray diffraction was performed under the following conditions: radiation source: Cu-Kα1 monochromatic radiation source, acceleration voltage: 40 kV, acceleration current: 40 mA, 2θ: 20 to 60°, and scan speed: 0.5° / min.

[0072] <Average particle size> The particle size of the powder was measured using a laser diffraction particle size distribution measuring device (HELOS&RODOS, Japan Laser Co., Ltd.), and the cumulative 50% diameter (x50) in the volumetric particle size distribution was calculated as the average particle size.

[0073] <Magnetic properties> The magnetic properties of the alloy powder (magnetic powder) were measured using a vibrating sample magnetometer (VSM) in accordance with the Bonded Magnet Testing Method Guidebook BMG-2005 of the Japan Bonded Magnetic Materials Association.

[0074] (3) Evaluation results The recovered powder was Th2Zn 17 SmFe with type crystal structure 17 The powder was confirmed to be N3 by XRD diffraction. The powder had a composition of Sm: 23.3 wt%, N: 3.5 wt%, O: 0.20 wt%, and Ca: less than 0.01 wt%. The average particle size (x50) was 18.0 μm. The collected powder was pulverized in a vibration ball mill using ethanol as a solvent until the x50 was 2.3 μm, and then dried under reduced pressure at room temperature to produce magnetic powder. The magnetic properties of the magnetic powder were Br: 1.42 T, HcJ: 1.06 MA / m.

[0075] [Example 2] (1) Preparation of alloy powder The hydrogen flow rate in the hydrogen treatment was changed to 0.5 L / min. Otherwise, the same procedure as in Example 1 was used to prepare SmFe 17 N3 powder was produced. By controlling the hydrogen flow rate to 0.5 L / min, the internal pressure of the tube furnace became negative at -53 kPa during the treatment. The maximum temperature of the reaction product reached 71°C due to the heat generated by hydrogen absorption.

[0076] (2) Evaluation The alloy powder thus obtained was subjected to evaluation of various properties in the same manner as in Example 1.

[0077] (3) Evaluation results The recovered powder had a composition of Sm: 23.4 wt%, N: 3.5 wt%, O: 0.18 wt%, and Ca: less than 0.01 wt%, and was found to be Th2Zn 17 SmFe with type crystal structure 17 It was confirmed that the powder was N3. The x50 was 18.7 μm. This powder was pulverized in a vibration ball mill until the x50 was 2.3 μm to produce magnetic powder. The magnetic properties of the magnetic powder were Br: 1.41 T, HcJ: 1.12 MA / m.

[0078] [Example 3] (1) Preparation of alloy powder The hydrogen flow rate in the hydrogen treatment was changed to 2 L / min. Otherwise, the same procedure as in Example 1 was used to prepare SmFe 17 N3 powder was produced. By increasing the hydrogen flow rate to 2 L / min, the internal pressure of the tube furnace became negative at -28 kPa during the treatment. The maximum temperature of the reaction product reached 251°C due to the heat generated by hydrogen absorption.

[0079] (2) Evaluation The alloy powder thus obtained was subjected to evaluation of various properties in the same manner as in Example 1.

[0080] (3) Evaluation results The recovered powder had a composition of Sm: 23.3 wt%, N: 3.4 wt%, O: 0.23 wt%, and Ca: less than 0.01 wt%, and was found to be Th2Zn 17 SmFe with type crystal structure 17 It was confirmed that the powder was N3. The x50 was 17.3 μm. This powder was pulverized in a vibration ball mill until the x50 was 2.3 μm to produce magnetic powder. The magnetic properties of the magnetic powder were Br: 1.44 T, HcJ: 1.23 MA / m.

[0081] [Example 4] (1) Preparation of alloy powder The hydrogen flow rate in the hydrogen treatment was changed to 3 L / min. Otherwise, the same procedure as in Example 1 was used to prepare SmFe 17 N3 powder was produced. By increasing the flow rate to 3 L / min, the internal pressure of the tube furnace became negative at -18 kPa during the treatment. The maximum temperature of the reaction product reached 295°C due to the heat generated by hydrogen absorption. (2) Evaluation The alloy powder thus obtained was subjected to evaluation of various properties in the same manner as in Example 1.

[0082] (3) Evaluation results The recovered powder had a composition of Sm: 23.2 wt%, N: 3.4 wt%, O: 0.25 wt%, and Ca: less than 0.01 wt%, and was found to be Th2Zn 17 SmFe with type crystal structure 17 It was confirmed that the powder was N3. The x50 was 17.2 μm. This powder was pulverized in a vibration ball mill until the x50 was 2.3 μm to produce magnetic powder. The magnetic properties of the magnetic powder were Br: 1.43 T, HcJ: 1.21 MA / m.

[0083] [Comparative Example 1] (1) Preparation of alloy powder The hydrogen flow rate in the hydrogen treatment was changed to 5 L / min. Otherwise, the same procedure as in Example 1 was used to prepare SmFe 17 N3 powder was produced. By increasing the flow rate to 5 L / min, the internal pressure of the tube furnace became negative at -2 kPa during the treatment. The maximum temperature of the reaction product due to the heat generated by hydrogen absorption was 311°C.

[0084] (2) Evaluation The alloy powder thus obtained was subjected to evaluation of various properties in the same manner as in Example 1.

[0085] (3) Evaluation results The recovered powder had a composition of Sm: 23.8 wt%, N: 3.6 wt%, O: 0.32 wt%, and Ca: less than 0.01 wt%, and was found to be Th2Zn 17 SmFe with a crystal structure of 17 It was confirmed that the powder was N3. In addition, the (110) diffraction line of αFe was observed in the XRD diffraction. The x50 was 18.3 μm. This powder was ground in a vibrating ball mill until the x50 was 2.3 μm to produce magnetic powder. The magnetic properties of the magnetic powder were Br: 1.32 T, HcJ: 0.91 MA / m.

[0086] [Comparative Example 2] (1) Preparation of alloy powder The hydrogen flow rate in the hydrogen treatment was changed to 10 L / min. Otherwise, the same procedure as in Example 1 was used to prepare SmFe 17 N3 powder was produced. By increasing the flow rate to 10 L / min, the internal pressure of the tube furnace did not become negative during the treatment. In addition, the maximum temperature of the reaction product reached 373°C due to the heat generated by hydrogen absorption.

[0087] (2) Evaluation The alloy powder thus obtained was subjected to evaluation of various properties in the same manner as in Example 1.

[0088] (3) Evaluation results The recovered powder had a composition of Sm: 24.2 wt%, N: 3.7 wt%, O: 0.41 wt%, and Ca: less than 0.01 wt%, and was found to be Th2Zn 17 SmFe with type crystal structure 17 It was confirmed that the powder was N3. In addition, the (110) diffraction line of αFe was observed by XRD diffraction. x50 was 20.1 μm. This powder was ground in a vibration ball mill until x50 was 2.3 μm to produce magnetic powder. The magnetic properties of the magnetic powder were Br: 1.27 T, HcJ: 0.78 MA / m.

[0089] [Example 5] (1) Preparation of alloy powder In Example 5, SmFe 17 The N3 alloy powder was prepared and evaluated according to the following procedure.

[0090] <Mixing process> A mixture was obtained by mixing 27 g of samarium oxide (Sm2O3) powder, 67 g of carbonyl iron (Fe) powder, and 16 g of metallic calcium (Ca).

[0091] <Reduction and diffusion process> The mixture obtained was placed in an iron reaction vessel, argon gas was sealed inside, and the vessel was then loaded into a heating furnace. The reaction vessel containing the mixture was heated to 970°C over 4 hours, and held at this temperature for 5 hours to allow the mixture to undergo a reduction-diffusion reaction. The reaction vessel was then cooled to room temperature while still in the heating furnace, and the reaction product was removed from the reaction vessel. 101 g of reaction product was obtained. This reaction product was in a sintered state.

[0092] <Hydrogen treatment> The reaction product was treated with hydrogen to obtain a crushed material. Specifically, the reaction product was put into a tubular furnace, and the inside of the furnace was evacuated until the pressure reached -100 kPa. Hydrogen was then introduced until the pressure inside the furnace reached atmospheric pressure, and the temperature was raised to 150°C over 40 minutes while hydrogen was flowing at a flow rate of 1 L / min. When the reaction product temperature reached approximately 110°C, hydrogen absorption began. The exhaust valve of the tubular furnace was then closed, and the temperature was continued to rise while maintaining the pressure inside the furnace at negative pressure. Hydrogen supply was continued at a flow rate of 1 L / min until hydrogen absorption was completed and the pressure inside the furnace returned to atmospheric pressure. During this time, the internal pressure of the furnace reached a negative pressure of -50 kPa. The maximum temperature of the reaction product reached 237°C due to the heat generated by hydrogen absorption. After hydrogen absorption was completed and the temperature of the reaction product was confirmed to have settled at 150°C, the same as the furnace temperature, the reaction product was cooled.

[0093] <Nitriding treatment> Next, the hydrogen-treated reaction product (crushed material) was nitrided. Specifically, while the hydrogen-treated reaction product was placed in a tubular furnace, a mixed gas of ammonia and hydrogen was flowed, and the temperature was raised in that state and the heat treatment was performed under the conditions of 445°C x 2.5 hours. At this time, the ammonia flow rate was 40 mL / min and the hydrogen flow rate was 160 mL / min.

[0094] <Wet processing> After cooling, the reaction product was collected and poured into 200 mL of water to form a slurry, and decantation was repeated 10 times using ion-exchanged water. After that, 6 g of acetic acid was poured into the slurry while stirring, and decantation was repeated 10 times again using ion-exchanged water. The ion-exchanged water was then replaced with ethanol, and the mixture was filtered. The collected cake was dried under reduced pressure at 200°C. This resulted in a rare earth transition metal alloy powder.

[0095] (2) Evaluation The alloy powder thus obtained was subjected to evaluation of various properties in the same manner as in Example 1.

[0096] (3) Evaluation results <Evaluation Results> The recovered powder was Th2Zn 17 SmFe with type crystal structure 17 The powder was confirmed to be N3 by XRD diffraction. The powder had a composition of Sm: 23.2 wt%, N: 3.2 wt%, O: 0.57 wt%, and Ca: less than 0.01 wt%. The average particle size (x50) was 9.1 μm. The magnetic properties of the powder were Br: 0.80 T and HcJ: 1.11 MA / m.

[0097] [Example 6] (1) Preparation of alloy powder During the hydrogen treatment, the temperature was raised to 280° C. over 60 minutes while hydrogen was flowed at a flow rate of 1 L / min. Otherwise, the same procedure as in Example 5 was used to prepare SmFe 17 N 3粉 During the hydrogen treatment, the pressure in the furnace reached a negative pressure of -70 kPa. The maximum temperature of the reaction product reached 293°C due to the heat generated by hydrogen absorption.

[0098] (2) Evaluation The alloy powder thus obtained was subjected to evaluation of various properties in the same manner as in Example 1.

[0099] (3) Evaluation results The recovered powder was Th2Zn 17 SmFe with type crystal structure 17 The powder was confirmed to be N3 by XRD diffraction. The powder had a composition of Sm: 23.3 wt%, N: 3.3 wt%, O: 0.60 wt%, and Ca: less than 0.01 wt%. The x50 was 8.8 μm. The magnetic properties of the powder were Br: 0.77 T, HcJ: 1.16 MA / m.

[0100] [Comparative Example 3] (1) Preparation of alloy powder During the hydrogen treatment, hydrogen was flowed at a flow rate of 3 L / min. Otherwise, the same procedure as in Example 6 was used to prepare SmFe 17 During the hydrogen treatment, the pressure in the furnace reached -38kPa, and the maximum temperature of the reaction product reached 324℃ due to the heat generated by hydrogen absorption.

[0101] (2) Evaluation The alloy powder thus obtained was subjected to evaluation of various properties in the same manner as in Example 1.

[0102] (3) Evaluation results The recovered powder was Th2Zn 17 SmFe with type crystal structure 17 The powder was confirmed to be N3 by XRD diffraction. The diffraction lines of αFe were also observed. The powder had a composition of Sm: 23.5 wt%, N: 3.3 wt%, O: 0.52 wt%, and Ca: less than 0.01 wt%. The x50 was 10.2 μm. The magnetic properties of the powder were Br: 0.71 T, HcJ: 0.74 MA / m.

[0103] [Example 7] In Example 7, NdFe 14 The alloy powder B was produced and evaluated according to the following procedure.

[0104] (1) Preparation of alloy powder <Mixing process> A mixture was obtained by mixing 41 g of neodymium oxide (Nd2O3) powder, 61 g of iron (Fe) powder, 7 g of ferroboron powder with a boron content of 19.0%, 22 g of metallic calcium (Ca), and 4.6 g of anhydrous calcium oxide (CaO).

[0105] <Reduction and diffusion process> The resulting mixture was placed in an iron reaction vessel, argon gas was sealed inside, and the vessel was then loaded into a heating furnace. The reaction vessel containing the mixture was heated to 1000°C over one hour, and held at this temperature for two hours to allow the reduction-diffusion reaction to occur. The reaction vessel was then cooled to room temperature while still in the heating furnace, and the reaction product was removed from the reaction vessel. 133 g of reaction product was obtained. This reaction product was in a sintered state.

[0106] <Hydrogen treatment> The resulting reaction product was treated with hydrogen to obtain a crushed material. Specifically, the reaction product was put into a tubular furnace, and the inside of the furnace was evacuated until the pressure reached -100 kPa. Hydrogen was then introduced until the pressure inside the furnace reached atmospheric pressure, and the temperature was raised to 200°C over 40 minutes while hydrogen was flowing at a flow rate of 1 L / min. When the reaction product temperature reached approximately 180°C, hydrogen absorption began. The exhaust valve of the tubular furnace was then closed, and the temperature was continued to be raised while maintaining the pressure inside the furnace at negative pressure. Hydrogen was supplied at a flow rate of 1 L / min until hydrogen absorption was completed and the pressure inside the furnace returned to atmospheric pressure. During hydrogen absorption, the internal pressure of the furnace reached a negative pressure of -37 kPa. The maximum temperature of the reaction product reached 285°C due to the heat generated by hydrogen absorption. After hydrogen absorption was completed, the reaction product was cooled down after confirming that the temperature of the reaction product had settled at 200°C, the same as the furnace temperature. The reaction product was then removed from the container and collected.

[0107] <Wet processing> The collected reaction product was poured into 500 mL of water to form a slurry, and decantation was repeated 20 times using ion-exchanged water. The ion-exchanged water was then replaced with ethanol, followed by filtration, and the collected cake was dried under reduced pressure at 50°C. This produced a rare earth transition metal alloy powder.

[0108] (2) Evaluation The alloy powder thus obtained was subjected to evaluation of various properties in the same manner as in Example 1.

[0109] (3) Evaluation results The recovered powder is tetragonal Nd2Fe 14 XRD diffraction confirmed that the powder had a B structure. The powder had a composition of Nd: 33.1 wt%, B: 1.3 wt%, O: 0.70 wt%, and Ca: 0.17 wt%. The x50 was 27 μm. This powder was pulverized in a vibration ball mill using ethanol as a solvent until the x50 was 2.8 μm, and then dried under reduced pressure to produce magnetic powder. The magnetic properties of the magnetic powder were Br: 1.42 T and HcJ: 0.38 MA / m.

[0110] [Comparative Example 4] (1) Preparation of alloy powder The hydrogen treatment was carried out while heating the material to 280° C. over a period of 60 minutes under a flow of hydrogen at a flow rate of 5 L / min. 14 Powder with B structure was produced. During hydrogen treatment, the internal pressure of the furnace became negative at -10 kPa. The maximum temperature of the reaction product due to the heat generated by hydrogen absorption reached 307°C.

[0111] (2) Evaluation The alloy powder thus obtained was subjected to evaluation of various properties in the same manner as in Example 1.

[0112] (3) Evaluation results The recovered powder is tetragonal Nd2Fe 14 XRD diffraction confirmed that it had a B structure. The diffraction lines of αFe were also observed. The powder had a composition of Nd: 32.6 wt%, B: 1.2 wt%, O: 0.91 wt%, and Ca: 0.22 wt%. The x50 was 31 μm. This powder was pulverized in a vibration ball mill using ethanol as the solvent until the x50 was 2.9 μm, and then dried under reduced pressure to produce magnetic powder. The magnetic properties of the magnetic powder were Br: 1.20 T, HcJ: 0.19 MA / m.

[0113] (4) Summary of evaluation results Table 1 shows the hydrogen treatment conditions and the properties of the obtained alloy powders for Examples 1 to 7 and Comparative Examples 1 to 4.

[0114] In Examples 1 to 4, the maximum temperature of the reaction product due to the heat generated by hydrogen absorption was 300°C or less. 17 The coercive force HcJ of the N3 magnetic powder was as high as 1.06 to 1.23 MA / m. In contrast, in Comparative Examples 1 and 2, the maximum temperature of the reaction product exceeded 300°C, and the coercive force was 0.91 MA / m or less. In Comparative Examples 1 and 2, the generation of αFe was confirmed by XRD diffraction, and it is presumed that the coercive force was reduced by this αFe.

[0115] Similarly, in Examples 5 and 6, the maximum temperature of the reaction product due to hydrogen absorption was below 300°C, and the obtained SmFe 17 The coercive force of the N3 magnetic powder was as high as 1.11 to 1.16 MA / m. In contrast, in Comparative Example 3, in which the maximum temperature of the reaction product exceeded 300° C., the coercive force was as low as 0.74 MA / m. In addition, as in Comparative Examples 1 and 2, the formation of αFe was confirmed by XRD diffraction.

[0116] NdFe 17 For the magnetic powder having the B structure, Example 7, in which the maximum temperature of the reaction product due to hydrogen absorption was 300°C or less, had a high coercive force of 0.38 MA / m. In contrast, Comparative Example 4, in which the maximum temperature exceeded 300°C, had a low coercive force of 0.19 MA / m. Furthermore, in Comparative Example 4, the generation of αFe was observed.

[0117] [Table 1] < / xrd>

Claims

1. A method for producing a rare earth transition metal alloy powder, comprising the steps of: Mixing at least a rare earth oxide powder, a transition metal powder, and a reducing agent to obtain a mixture; a step of subjecting the mixture to a heat treatment in a non-oxidizing atmosphere to reduce the rare earth oxide powder and to diffuse the rare earth oxide powder into the transition metal powder to form an alloy, thereby obtaining a reaction product containing a rare earth transition metal alloy and a by-product derived from the reducing agent; exposing the reaction product to a hydrogen atmosphere, thereby absorbing hydrogen and disintegrating the reaction product to obtain a disintegrated material; and washing the crushed product with a washing liquid to obtain an alloy powder. The method comprises exposing the reaction product to a hydrogen atmosphere while maintaining a temperature of the reaction product below 300° C. and maintaining a negative pressure around the reaction product.

2. 10. The method of claim 1, wherein the temperature of the reaction product is maintained at or below 295°C when exposing the reaction product to the hydrogen atmosphere.

3. 3. The method according to claim 1, wherein the pressure around the reaction product is maintained at a negative pressure of -15 kPa or less when the reaction product is exposed to a hydrogen atmosphere.

4. The method according to any one of claims 1 to 3, wherein the temperature of the reaction product is adjusted by controlling the amount of hydrogen supplied and / or the treatment temperature when the reaction product is exposed to a hydrogen atmosphere.

5. The rare earth oxide powder is an oxide powder of one or more metals selected from the group consisting of yttrium (Y), lanthanum (La), cerium (Ce), praseodymium (Pr), neodymium (Nd), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), and ytterbium (Yb). The method according to any one of claims 1 to 4.

6. The method according to any one of claims 1 to 5, wherein the transition metal powder is a powder of one or more metals selected from the group consisting of iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), chromium (Cr), manganese (Mn), zinc (Zn), molybdenum (Mo), and tungsten (W).

7. The method according to any one of claims 1 to 6, further comprising a step of nitriding the crushed material and / or the alloy powder.

Citation Information

Patent Citations

  • Production by reduction diffusion method of alloy powder containing rare earth and transition metal

    JP1997241708A

  • Method of producing rare earth-transition metal-based alloy powder, rare earth-transition metal-nitrogen-based alloy powder, and production method therefor

    JP2004204285A

  • Rare earth-transition metal based alloy powder, rare earth-transition metal-nitrogen based alloy powder, and production method therefor

    JP2005008950A

  • Rare-earth-iron-nitrogen-base magnet powder and method for manufacturing the same

    JP2007119909A

  • Short-process method for preparing sintered ndfeb magnets with high magnetic properties recycling from ndfeb sludge