Binder composition for non-aqueous secondary battery, slurry composition for non-aqueous secondary battery electrode, electrode for non-aqueous secondary battery, and non-aqueous secondary battery

The introduction of an asymmetric block copolymer with defined molecular weight ranges in the binder composition for non-aqueous secondary batteries enhances electrode flexibility and cycle characteristics, overcoming the limitations of conventional compositions.

JP7556349B2Active Publication Date: 2024-09-26ZEON CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021511455
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-29
Filing Date
2020-03-19
Publication Date
2024-09-26
Estimated Expiration
2040-03-19

AI Technical Summary

Technical Problem

Conventional binder compositions for non-aqueous secondary battery electrodes lack sufficient flexibility and cycle characteristics, limiting the performance of non-aqueous secondary batteries.

Method used

A binder composition containing an asymmetric block copolymer with specific molecular weight ranges for aromatic vinyl and aliphatic conjugated diene monomer units, enhancing electrode flexibility and cycle characteristics.

Benefits of technology

The use of the asymmetric block copolymer in the binder composition results in electrodes with high flexibility and improved cycle characteristics, effectively addressing the limitations of conventional compositions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007556349000002
    Figure 0007556349000002
  • Figure 0007556349000001
    Figure 0007556349000001
Patent Text Reader

Abstract

This binder composition for a nonaqueous secondary battery includes a particulate polymer containing a block copolymer A represented by general formula (A): Arla-Da-Ar2a [Here, in general formula (A), Arla is a block region composed of aromatic vinyl monomer units having a weight average molecular weight of 5,500 to 20,000; Ar2a is a block region composed of aromatic vinyl monomer units having a weight average molecular weight of 40,000 to 400,000; and Da is a block region composed of aliphatic conjugate diene monomer units.]
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a binder composition for a non-aqueous secondary battery, a slurry composition for an electrode for a non-aqueous secondary battery, an electrode for a non-aqueous secondary battery, and a non-aqueous secondary battery. [Background technology]

[0002] Non-aqueous secondary batteries such as lithium ion secondary batteries (hereinafter sometimes simply referred to as "secondary batteries") are small, lightweight, have high energy density, and can be repeatedly charged and discharged, and are used in a wide range of applications. Therefore, in recent years, improvements to battery components such as electrodes have been studied in order to further improve the performance of non-aqueous secondary batteries.

[0003] Here, an electrode used in a secondary battery such as a lithium ion secondary battery usually includes a current collector and an electrode mixture layer (positive electrode mixture layer or negative electrode mixture layer) formed on the current collector. The electrode mixture layer is formed, for example, by applying a slurry composition containing an electrode active material and a binder composition containing a binding agent onto the current collector and drying the applied slurry composition.

[0004] Therefore, in recent years, attempts have been made to improve the binder composition used in forming the electrode mixture layer in order to achieve further improvements in the performance of secondary batteries. Specifically, for example, Patent Document 1 proposes a binder composition for non-aqueous secondary battery electrodes, which contains a particulate polymer A that is a copolymer having a block region composed of aromatic vinyl monomer units, and a particulate polymer B that is a random copolymer containing aliphatic conjugated diene monomer units and aromatic vinyl monomer units. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2018 / 168420 Summary of the Invention [Problem to be solved by the invention]

[0006] Here, from the viewpoint of improving battery characteristics such as cycle characteristics, the electrodes of secondary batteries are required to have excellent flexibility. Furthermore, in recent years, the electrodes are required to have even higher flexibility from the viewpoint of increasing capacity, etc.

[0007] However, the conventional binder composition for a non-aqueous secondary battery electrode leaves room for further improvement in the flexibility of the resulting electrode, and the non-aqueous secondary battery including an electrode formed using the conventional binder composition for a non-aqueous secondary battery electrode leaves room for further improvement in cycle characteristics.

[0008] Therefore, an object of the present invention is to provide a binder composition for a non-aqueous secondary battery, which is capable of forming an electrode having sufficiently high flexibility and capable of improving the cycle characteristics of the resulting secondary battery, and a slurry composition for a non-aqueous secondary battery electrode. Another object of the present invention is to provide an electrode for a non-aqueous secondary battery having sufficiently high flexibility, and a non-aqueous secondary battery including such an electrode and having excellent cycle characteristics. [Means for solving the problem]

[0009] The present inventors have conducted extensive research with the aim of solving the above problems, and have newly discovered that by blending a particulate polymer made of an asymmetric block copolymer satisfying certain conditions into a binder composition, the flexibility of the resulting electrode can be significantly improved and the cycle characteristics of the resulting secondary battery can be sufficiently improved, thereby completing the present invention.

[0010] That is, the present invention aims to advantageously solve the above-mentioned problems, and the binder composition for a nonaqueous secondary battery of the present invention is characterized in that it contains a particulate polymer containing a block copolymer A represented by the following general formula (A). Ar1 a -D a -Ar2a (A) [wherein, in the general formula (A), Ar1 a indicates a block region consisting of an aromatic vinyl monomer unit having a weight average molecular weight of 5,500 to 20,000, and Ar2 a indicates a block region consisting of an aromatic vinyl monomer unit having a weight average molecular weight of 40,000 to 400,000, D a indicates a block region composed of an aliphatic conjugated diene monomer unit. In this way, by using a binder composition containing at least a specific block copolymer A having a structure in which block regions made of aromatic vinyl monomer units having different weight-average molecular weights are separated by block regions made of aliphatic conjugated diene monomer units, i.e., an asymmetric structure, it is possible to form an electrode that has sufficiently high flexibility and can improve the cycle characteristics of the resulting secondary battery. In this specification, the term "monomer unit" of a polymer means "a repeating unit derived from the monomer contained in a polymer obtained using the monomer." In addition, in this specification, when a polymer "has a block region made of a monomer unit," it means that "the polymer has a portion in which only the monomer unit is linked together as a repeating unit." In this specification, the "weight average molecular weight" of each region contained in a certain block copolymer can be measured by the method described in the Examples.

[0011] Here, in the binder composition for a nonaqueous secondary battery of the present invention, it is preferable that the particulate polymer further contains a block copolymer B represented by the following general formula (B), and the ratio of the block copolymer A is 36 mass% or more and 85 mass% or less, relative to the total mass of the block copolymer A and the block copolymer B being 100 mass%. Ar1 b -D b -Ar2 b (B) [wherein, in the general formula (B), Ar1 b and Ar2 beach independently represents a block region composed of an aromatic vinyl monomer unit having a weight average molecular weight of 6,000 to 20,000; D b indicates a block region composed of an aliphatic conjugated diene monomer unit. If the binder composition further contains the above-mentioned predetermined block copolymer B, the cycle characteristics of the obtained secondary battery can be further improved.

[0012] In the binder composition for non-aqueous secondary batteries of the present invention, the surface acid amount of the particulate polymer is preferably 0.05 mmol / g or more and 0.90 mmol / g or less. If the surface acid amount of the particulate polymer is within the above range, the viscosity stability of a slurry composition prepared using the binder composition can be improved. In this specification, the "surface acid amount" of the particulate polymer can be measured by the method described in the Examples.

[0013] The present invention also aims to advantageously solve the above problems, and the slurry composition for a non-aqueous secondary battery electrode of the present invention is characterized by including an electrode active material and any one of the binder compositions for a non-aqueous secondary battery described above. In this way, by including any one of the binder compositions for a non-aqueous secondary battery described above, the flexibility of an electrode formed using the slurry composition for a non-aqueous secondary battery electrode can be sufficiently improved. In addition, the cycle characteristics of a secondary battery equipped with such an electrode can be sufficiently improved.

[0014] Furthermore, the present invention aims to advantageously solve the above problems, and the non-aqueous secondary battery electrode of the present invention is characterized in that it comprises an electrode mixture layer formed using the above-mentioned non-aqueous secondary battery electrode slurry composition. In this way, by forming the electrode mixture layer using the above-mentioned non-aqueous secondary battery electrode slurry composition, an electrode can be obtained that has sufficiently high flexibility and can improve the cycle characteristics of the resulting secondary battery.

[0015] The present invention has an object to advantageously solve the above problems, and the nonaqueous secondary battery of the present invention is characterized in that it has a positive electrode, a negative electrode, a separator, and an electrolyte, and at least one of the positive electrode and the negative electrode is the above-mentioned electrode for a nonaqueous secondary battery. By using the above-mentioned electrode for a nonaqueous secondary battery, a nonaqueous secondary battery having excellent cycle characteristics can be efficiently manufactured. Effect of the Invention

[0016] According to the binder composition for a non-aqueous secondary battery and the slurry composition for a non-aqueous secondary battery electrode of the present invention, it is possible to form an electrode that has sufficiently high flexibility and can improve the cycle characteristics of the resulting secondary battery. Furthermore, according to the present invention, it is possible to obtain an electrode for a non-aqueous secondary battery having sufficiently high flexibility, and a non-aqueous secondary battery having the electrode and excellent cycle characteristics. [Brief description of the drawings]

[0017] [Figure 1] FIG. 2 is a diagram showing an example of a plot used in measuring the surface acid amount of a particulate polymer in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, an embodiment of the present invention will be described in detail. Here, the binder composition for non-aqueous secondary batteries of the present invention can be used to prepare a slurry composition for non-aqueous secondary battery electrodes of the present invention. The slurry composition for non-aqueous secondary battery electrodes prepared using the binder composition for non-aqueous secondary batteries of the present invention can be used when manufacturing electrodes for non-aqueous secondary batteries such as lithium ion secondary batteries. Furthermore, the non-aqueous secondary battery of the present invention is characterized in that it uses an electrode for a non-aqueous secondary battery of the present invention formed using the slurry composition for non-aqueous secondary battery electrodes of the present invention. The binder composition for a non-aqueous secondary battery, the slurry composition for a non-aqueous secondary battery electrode, and the electrode for a non-aqueous secondary battery of the present invention are preferably for use in a negative electrode, and the non-aqueous secondary battery of the present invention preferably uses the electrode for a non-aqueous secondary battery of the present invention as a negative electrode.

[0019] (Binder composition for non-aqueous secondary batteries) The binder composition for a non-aqueous secondary battery of the present invention contains a predetermined particulate polymer, and may optionally further contain water as a dispersion medium and other components that can be blended in the binder composition. In addition, since the particulate polymer of the binder composition of the present invention contains the block copolymer A, which is an asymmetric block copolymer, it is possible to form an electrode that has sufficient flexibility and can improve the cycle characteristics of the obtained secondary battery. Here, in recent years, from the viewpoint of increasing the capacity of secondary batteries, silicon-based materials are sometimes adopted as electrode active materials. Since electrode active materials made of silicon-based materials (hereinafter also referred to as Si-based electrode active materials) have large expansion and contraction during charging and discharging, it is required that the flexibility of electrodes including electrode mixture layers containing Si-based electrode active materials be further improved. Therefore, since the binder composition of the present invention has excellent flexibility, even when used in combination with a Si-based electrode active material, it can well follow the expansion and contraction of the Si-based electrode active material in the electrode, and as a result, the cycle characteristics of the secondary battery can be improved.

[0020] The reason why the present invention provides a binder composition for a non-aqueous secondary battery capable of forming an electrode with sufficiently high flexibility is not clear, but is presumed to be as follows. First, the block copolymer A contained in the binder composition of the present invention is an asymmetric block copolymer. More specifically, the block copolymer A contains two block regions (hereinafter also referred to as "aromatic vinyl block regions") composed of aromatic vinyl monomer units having different weight average molecular weights, which are separated by a block region (hereinafter also referred to as "aliphatic conjugated diene block region") composed of an aliphatic conjugated diene monomer unit. In the block copolymer A, the aromatic vinyl block region having a smaller weight average molecular weight acts to soften the block copolymer A itself, while the aromatic vinyl block region having a larger weight average molecular weight prevents the block copolymer A from being excessively softened, and it is considered that the permanent elongation of the block copolymer A is effectively prevented from increasing. As a result, while the block copolymer A itself has appropriate flexibility, the electrode mixture layer containing such block copolymer A has a strength capable of adapting to deformation caused by repeated charging and discharging, thereby improving the cycle characteristics of the obtained secondary battery.

[0021] <Particulate polymer> The particulate polymer is a component that functions as a binder, and in an electrode mixture layer formed using a slurry composition containing the binder composition, it holds components such as an electrode active material from being detached from the electrode mixture layer, and enables adhesion between the electrode and the separator via the electrode mixture layer. The particulate polymer is required to contain a specific block copolymer A described later, and preferably further contains a specific block copolymer B described later as an option. The particulate polymer is a water-insoluble particle formed by a specific polymer. In the present invention, the particle is "water-insoluble" when 0.5 g of the polymer is dissolved in 100 g of water at 25° C., and the insoluble content is 90% by mass or more.

[0022] <<Block copolymer A>> The block copolymer A as a particulate polymer is a particle made of a copolymer having a structure represented by the following general formula (A). Ar1 a -D a -Ar2 a (A) [wherein, in general formula (A), Ar1 a indicates a block region consisting of an aromatic vinyl monomer unit having a weight average molecular weight of 5,500 to 20,000, and Ar2 a indicates a block region consisting of an aromatic vinyl monomer unit having a weight average molecular weight of 40,000 to 400,000, D a indicates a block region composed of an aliphatic conjugated diene monomer unit. In the following description, the components 1) to 3) of the block copolymer A are respectively defined as follows: 1) A block region consisting of aromatic vinyl monomer units having a weight average molecular weight of 5,500 to 20,000 is referred to as an "aromatic vinyl block region (Ar1 a )"and, 2) A block region consisting of aromatic vinyl monomer units having a weight average molecular weight of 40,000 to 400,000 is referred to as an "aromatic vinyl block region (Ar2 a )"and, 3) The block region consisting of aliphatic conjugated diene monomer units is referred to as the "aliphatic conjugated diene block region (D a )"and, It is sometimes referred to as. Aromatic vinyl block region (Ar1 a ) and aromatic vinyl block region (Ar2 a As is clear from the range of the weight average molecular weight for each of the aromatic vinyl block regions (Ar2) having a larger weight average molecular weight, the block copolymer A has a larger aromatic vinyl block region (Ar2) having a larger weight average molecular weight. a ) and the aromatic vinyl block region (Ar1 a As is apparent from the above general formula (A), the aromatic vinyl block regions (Ar1) have different weight average molecular weights. a ,Ar2 a ) is an aliphatic conjugated diene block region (Da In other words, the block copolymer A is separated by an aliphatic conjugated diene block region (D a ) is a block copolymer with an asymmetric structure.

[0023] In addition, the block copolymer A is in the above-mentioned region (Ar1 a ,D a ,Ar2 a ), other polymer chain portions not corresponding to these may be contained. However, from the viewpoint of effectively suppressing the permanent set from becoming large, it is preferable that the block copolymer A does not contain other polymer chain portions.

[0024] -Aromatic vinyl block region (Ar1 a ,Ar2 a )- Aromatic vinyl block region (Ar1 a ,Ar2 a ) is a region that contains a portion in which only aromatic vinyl monomer units are linked together. And the aromatic vinyl block region (Ar1 a ,Ar2 a ) is a region that mainly contains aromatic vinyl monomer units as repeating units. In this specification, the term "mainly contains" an aromatic vinyl monomer unit means that, with the total monomer units contained in a certain block region being 100% by mass, 80% by mass or more of the block region is occupied by aromatic vinyl monomer units. Here, one aromatic vinyl block region (Ar1 a ,Ar2 a ) may be composed of only one type of aromatic vinyl monomer unit or may be composed of multiple types of aromatic vinyl monomer units, but is preferably composed of only one type of aromatic vinyl monomer unit.

[0025] Aromatic vinyl block region (Ar1 a ,Ar2 aThe aromatic vinyl monomer that can be used to form the aromatic vinyl monomer unit constituting the aromatic vinyl block region (Ar1) is not particularly limited as long as it is an aromatic vinyl compound, but examples thereof include styrene, α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2-ethylstyrene, 3-ethylstyrene, 4-ethylstyrene, 2,4-diisopropylstyrene, 2,4-dimethylstyrene, 4-t-butylstyrene, 5-t-butyl-2-methylstyrene, 2-chlorostyrene, 3-chlorostyrene, 4-chlorostyrene, 4-bromostyrene, 2-methyl-4,6-dichlorostyrene, 2,4-dibromostyrene, vinylnaphthalene, and the like. Among these, styrene is preferred. These can be used alone or in combination of two or more, but it is preferred to use one alone. In addition, each aromatic vinyl block region (Ar1) can be used as a styrene monomer. a ,Ar2 a ) may be composed of polymerization units formed using the same aromatic vinyl monomer, or may be composed of polymerization units formed using different aromatic vinyl monomers.

[0026] The aromatic vinyl block region (Ar1) is an aromatic vinyl block region having a smaller weight average molecular weight. a ) is the weight average molecular weight MW(Ar1 a ) must be 5,500 or more and 20,000 or less. a ) is preferably 6,000 or more, and is preferably 15,000 or less, more preferably 13,000 or less, and even more preferably 11,000 or less. a If MW(Ar1) is equal to or greater than the lower limit, the cycle characteristics of the resulting secondary battery can be improved. a When MW(Ar1) is equal to or less than the upper limit, the block copolymer A is prevented from becoming excessively hard, and the flexibility of the resulting electrode can be improved. a ) is equal to or less than the upper limit, the electrode can easily follow the expansion and contraction that accompanies the charging and discharging of the secondary battery, and the cycle characteristics of the secondary battery can be improved.

[0027] In addition, the aromatic vinyl block region (Ar2 a ) is the weight average molecular weight MW(Ar2 a The weight average molecular weight MW(Ar2 a ) is preferably 42,000 or more and 370,000 or less. a ) is equal to or greater than the above lower limit, the cycle characteristics of the resulting secondary battery can be improved. a ) is equal to or less than the above upper limit, the flexibility of the obtained electrode can be further improved. a When the content is equal to or less than the above upper limit, the viscosity of the reaction solution during production of the block copolymer A can be prevented from becoming excessively high, and the ease of production of the block copolymer A can be improved. In addition, MW(Ar1 a ) and MW(Ar2 a The value of (a) can be adjusted by, for example, appropriately changing the amount of monomer units added when preparing the block copolymer A, the amount of polymerization initiator, the amounts of various additives added during polymerization, the amount of polymerization solvent, the polymerization time, and the like.

[0028] And the aromatic vinyl block region (Ar2 a ) weight average molecular weight MW(Ar2 a ) in the aromatic vinyl block region (Ar1 a ) weight average molecular weight MW(Ar1 a ), i.e., "MW(Ar2 a ) / MW(Ar1 a The value of MW(Ar2) is not particularly limited, but is preferably 2.6 or more, more preferably 4 or more, and is preferably 67 or less, more preferably 40 or less. a ) / MW(Ar1 a If the value of MW(Ar2) is within the above range, the cycle characteristics of the obtained secondary battery can be further improved. a ) / MW(Ar1 a) is within the above range, it is believed that block copolymer A can achieve a good balance between the attributes of "low permanent set" and "low spring back."

[0029] The aromatic vinyl block region (Ar1 a ,Ar2 a ) may each contain a monomer unit other than the aromatic vinyl monomer unit. Aromatic vinyl block region (Ar1 a ,Ar2 a Examples of monomers that can be used to form monomer units other than the aromatic vinyl monomer units that can be contained in the block region (D) include aliphatic conjugated diene monomers, nitrile group-containing monomers, acidic group-containing monomers and their anhydrides, (meth)acrylic acid ester monomers, and aliphatic non-conjugated diene monomers such as 1,2-butadiene and 1,4-pentadiene. Here, in the present invention, "(meth)acrylic acid" means acrylic acid and / or methacrylic acid. The above-mentioned monomers include those in the block region (D a ) can be used as described below. The content of monomer units other than aromatic vinyl monomer units in each aromatic vinyl block region is preferably 20% by mass or less, more preferably 10% by mass or less, and particularly preferably substantially 0% by mass.

[0030] -A block region consisting of aliphatic conjugated diene monomer units (D a )- The block region consisting of aliphatic conjugated diene monomer units (aliphatic conjugated diene block region (D a The aliphatic conjugated diene block region (D a) is a region that mainly contains aliphatic conjugated diene monomer units. In this specification, the term "mainly contains" aliphatic conjugated diene monomer units means that, with the total monomer units contained in a certain block region being 100% by mass, 80% by mass or more of the block region is occupied by aliphatic conjugated diene monomer units. Here, one aliphatic conjugated diene block region (D a ) may be composed of one type of repeating unit, or may be composed of multiple types of repeating units. In addition, one aliphatic conjugated diene block region (D a ) may contain a coupling site (i.e., one aliphatic conjugated diene block region (D a The repeating units constituting the formula (1) may be linked via a coupling site). Furthermore, the aliphatic conjugated diene block region (D a In particular, from the viewpoint of improving the viscosity stability of the resulting slurry composition, it is preferable that the aliphatic conjugated diene block region (D a ) preferably has a graft portion.

[0031] Here, the aliphatic conjugated diene monomer that can be used to form the aliphatic conjugated diene monomer unit is not particularly limited as long as it is an aliphatic conjugated diene compound, and examples thereof include 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 2-chloro-1,3-butadiene, 1,3-pentadiene, and 1,3-hexadiene. Among these, it is preferable to use 1,3-butadiene and / or isoprene, and it is particularly preferable to use isoprene. By using isoprene in forming the aliphatic conjugated diene block region, the adhesive strength of the block copolymer A can be effectively increased.

[0032] In addition, by crosslinking the block region made of an aliphatic conjugated diene, a crosslinked structure can be introduced into the block region made of an aliphatic conjugated diene. In other words, by crosslinking a polymer containing a block region made of an aliphatic conjugated diene, an aliphatic conjugated diene block region (D a ) can be formed.

[0033] The structural unit formed by crosslinking an aliphatic conjugated diene monomer unit can be introduced into the block copolymer A by crosslinking a polymer containing a block region made of an aliphatic conjugated diene. Here, the crosslinking can be carried out using a radical initiator such as a redox initiator formed by combining an oxidizing agent and a reducing agent, without being particularly limited. As the oxidizing agent, for example, organic peroxides such as diisopropylbenzene hydroperoxide, cumene hydroperoxide, t-butyl hydroperoxide, 1,1,3,3-tetramethylbutyl hydroperoxide, di-t-butyl peroxide, isobutyryl peroxide, and benzoyl peroxide can be used. As the reducing agent, compounds containing metal ions in a reduced state such as ferrous sulfate and cuprous naphthenate; sulfonic acid compounds such as sodium methanesulfonate; amine compounds such as dimethylaniline; and the like can be used. These organic peroxides and reducing agents may be used alone or in combination of two or more. The crosslinking may be carried out in the presence of a crosslinking agent such as a polyvinyl compound such as divinylbenzene, a polyallyl compound such as diallyl phthalate, triallyl trimellitate, diethylene glycol bisallyl carbonate, or various glycols such as ethylene glycol diacrylate. The crosslinking may also be carried out by irradiation with active energy rays such as gamma rays.

[0034] Furthermore, the aliphatic conjugated diene block region (D a ) may contain repeating units other than those mentioned above. Specifically, the aliphatic conjugated diene block region (D a) is a monomer unit containing an acid group, such as a carboxyl group-containing monomer unit, a sulfonic acid group-containing monomer unit, and a phosphoric acid group-containing monomer unit; a monomer unit containing a nitrile group, such as an acrylonitrile unit and a methacrylonitrile unit; a monomer unit containing a (meth)acrylic acid ester, such as an acrylic acid alkyl ester unit and a methacrylic acid alkyl ester unit; and a block region (Ar1 a ,Ar2 a In particular, from the viewpoint of improving the viscosity stability of a slurry composition prepared using the binder composition by making the surface acid amount of the particulate polymer to an appropriate value, the aliphatic conjugated diene block region (D a ) preferably contains an acidic group-containing monomer unit. The acidic group contained in the acidic group-containing monomer unit may form a salt with an alkali metal, ammonia, or the like.

[0035] Examples of the carboxyl group-containing monomer capable of forming the carboxyl group-containing monomer unit include monocarboxylic acids and derivatives thereof, dicarboxylic acids and acid anhydrides thereof, and derivatives thereof. Examples of the monocarboxylic acid include acrylic acid, methacrylic acid, and crotonic acid. Examples of the monocarboxylic acid derivatives include 2-ethylacrylic acid, isocrotonic acid, α-acetoxyacrylic acid, β-trans-aryloxyacrylic acid, and α-chloro-β-E-methoxyacrylic acid. The dicarboxylic acids include maleic acid, fumaric acid, and itaconic acid. Examples of dicarboxylic acid derivatives include methylmaleic acid, dimethylmaleic acid, phenylmaleic acid, chloromaleic acid, dichloromaleic acid, fluoromaleic acid, and maleic acid monoesters such as butyl maleate, nonyl maleate, decyl maleate, dodecyl maleate, octadecyl maleate, and fluoroalkyl maleates. Examples of the acid anhydrides of dicarboxylic acids include maleic anhydride, acrylic anhydride, methylmaleic anhydride, dimethylmaleic anhydride, and citraconic anhydride. Furthermore, as the carboxyl group-containing monomer, an acid anhydride which generates a carboxyl group upon hydrolysis can also be used. Furthermore, as the carboxyl group-containing monomer, ethylenically unsaturated polycarboxylic acids such as butene tricarboxylic acid, and partial esters of ethylenically unsaturated polycarboxylic acids such as monobutyl fumarate and mono-2-hydroxypropyl maleate can also be used.

[0036] Examples of sulfonic acid group-containing monomers capable of forming sulfonic acid group-containing monomer units include styrene sulfonic acid, vinyl sulfonic acid (ethylene sulfonic acid), methyl vinyl sulfonic acid, (meth)allyl sulfonic acid, and 3-allyloxy-2-hydroxypropane sulfonic acid. In the present invention, "(meth)allyl" means allyl and / or methallyl.

[0037] Furthermore, examples of phosphate group-containing monomers capable of forming phosphate group-containing monomer units include 2-(meth)acryloyloxyethyl phosphate, methyl-2-(meth)acryloyloxyethyl phosphate, and ethyl-(meth)acryloyloxyethyl phosphate. In the present invention, "(meth)acryloyl" means acryloyl and / or methacryloyl.

[0038] Here, the above-mentioned monomers may be used alone or in combination of two or more. As the acidic group-containing monomer capable of forming the acidic group-containing monomer unit, methacrylic acid, itaconic acid, and acrylic acid are preferable, and methacrylic acid is more preferable.

[0039] The above-mentioned other monomer units such as the acidic group-containing monomer unit, the nitrile group-containing monomer unit and the (meth)acrylic acid ester monomer unit can be introduced into the polymer by any polymerization method such as graft polymerization without any particular limitation. When the other monomer unit is introduced by graft polymerization, the polymer contains a graft portion, and has a structure in which the polymer that becomes the trunk portion is bonded to the polymer that becomes the graft portion.

[0040] Here, the graft polymerization can be carried out using a known graft polymerization method without any particular limitation. Specifically, the graft polymerization can be carried out using a radical initiator such as a redox initiator that is a combination of an oxidizing agent and a reducing agent. The oxidizing agent and the reducing agent can be the same as the oxidizing agent and the reducing agent described above that can be used for crosslinking the block copolymer A. When graft polymerization is performed on the block copolymer A using a redox initiator, the introduction of other monomer units by graft polymerization and crosslinking of the aliphatic conjugated diene monomer units can proceed simultaneously. Note that graft polymerization and crosslinking do not have to proceed simultaneously, and only graft polymerization may proceed by adjusting the type of radical initiator and reaction conditions.

[0041] And the aliphatic conjugated diene block region (D a ) is the weight average molecular weight MW(D a ) is preferably 20,000 or more, more preferably 30,000 or more, and even more preferably 35,000 or more. a By making the weight average molecular weight MW(D) equal to or greater than the lower limit, the block copolymer A is prevented from becoming excessively hard, and the flexibility of the resulting electrode can be increased. a From the viewpoint of improving the cycle characteristics of the obtained secondary battery, the weight average molecular weight MW(D aFrom the viewpoint of effectively suppressing the springback of the resulting electrode mixture layer from becoming large, MW(D a The value of (a) can be adjusted by, for example, appropriately changing the amount of the monomer unit added when preparing the block copolymer A, the amount of the polymerization initiator, the amounts of various additives added during polymerization, the amount of the polymerization solvent, the amount of the coupling agent, the polymerization time, etc.

[0042] --Weight average molecular weight of block copolymer A-- The weight average molecular weight MW(A) of the block copolymer A is preferably 66,000 or more, more preferably 79,000 or more, even more preferably 100,000 or more, and preferably 300,000 or less, more preferably 200,000 or less. If the value of MW(A) is within the above range, the cycle characteristics of the obtained secondary battery can be further improved. In particular, if the value of MW(A) is equal to or less than the above upper limit, it is considered that the block copolymer A, which is a particulate polymer, can be prevented from irreversibly changing due to stress generated in the electrode mixture layer due to expansion and contraction of the electrode active material.

[0043] <<Block copolymer B>> The block copolymer B as a particulate polymer is a particle made of a copolymer having a structure represented by the following general formula (B). Ar1 b -D b -Ar2 b (B) [wherein, in the general formula (B), Ar1 b and Ar2 b each independently represents a block region composed of an aromatic vinyl monomer unit having a weight average molecular weight of 6,000 to 20,000; D b indicates a block region composed of an aliphatic conjugated diene monomer unit. In the following description, the components 4) to 6) of the block copolymer B are respectively defined as follows: 4) The first block region consisting of an aromatic vinyl monomer unit having a weight average molecular weight of 6,000 to 20,000 is referred to as an "aromatic vinyl block region (Ar1 b )"and, 5) The second block region consisting of aromatic vinyl monomer units having a weight average molecular weight of 6,000 to 20,000 is called the "aromatic vinyl block region (Ar2 b )"and, 6) The block region consisting of aliphatic conjugated diene monomer units is referred to as the "aliphatic conjugated diene block region (D b )"and, It is sometimes referred to as.

[0044] In addition, the block copolymer B is in the above-mentioned region (Ar1 b ,D b ,Ar2 b ), other polymer chain portions not corresponding to these may be included. However, from the viewpoint of effectively suppressing the permanent set from becoming large, it is preferable that block copolymer B does not contain other polymer chain portions.

[0045] -Aromatic vinyl block region (Ar1 b ,Ar2 b )- Aromatic vinyl block region (Ar1 b ,Ar2 b ) is a region mainly containing an aromatic vinyl monomer unit as a repeating unit. As in the case of the block copolymer A described above, one aromatic vinyl block region (Ar1 b ,D b ,Ar2 b Although the aromatic vinyl block region (Ar1) may be composed of only one or more types of aromatic vinyl monomer units, it is preferable that the aromatic vinyl block region (Ar1) is composed of only one type of aromatic vinyl monomer unit. b ,D b ,Ar2 b ) may include a coupling site.

[0046] Aromatic vinyl block region (Ar1 b ,Ar2 bExamples of aromatic vinyl monomers that can be used to form the aromatic vinyl monomer units constituting the block copolymer A include the various compounds described above in the section on block copolymer A. Among these, styrene is preferred. As with block copolymer A, each aromatic vinyl block region (Ar1 b ,Ar2 b ) may be composed of polymerization units formed using the same aromatic vinyl monomer, or may be composed of polymerization units formed using different aromatic vinyl monomers. Furthermore, as in the case of block copolymer A, the aromatic vinyl block region (Ar1 b ,Ar2 b Each of the aromatic vinyl block regions (Ar1) may contain a monomer unit other than the aromatic vinyl monomer unit. b ,Ar2 b As a monomer that can be used when forming a monomer unit other than the aromatic vinyl monomer unit that can be contained in the block copolymer A, the same monomers as those listed for the block copolymer A can be used.

[0047] Aromatic vinyl block region (Ar1 b ,Ar2 b ) is the weight average molecular weight MW(Ar1 b ) and MW(Ar2 b ) are each independently preferably 6,000 or more, more preferably 7,000 or more, and preferably 20,000 or less, more preferably 15,000 or less, and even more preferably 13,000 or less. b ) and MW(Ar2 b ) may be the same or different, but from the viewpoint of effectively suppressing an increase in permanent set, it is preferable that they are substantially the same.

[0048] MW(Ar1 b ) and MW(Ar2 b If MW(Ar1) is equal to or greater than the lower limit, the cycle characteristics of the resulting secondary battery can be improved. b ) and MW(Ar2b If MW(Ar1) is equal to or less than the upper limit, the flexibility of the obtained electrode can be improved. b ) and MW(Ar2 b ) is equal to or less than the upper limit, the electrode can easily follow the expansion and contraction that accompanies the charging and discharging of the secondary battery, and the cycle characteristics of the secondary battery can be improved.

[0049] Furthermore, MW(Ar1 b ) and MW(Ar2 b ) is the aromatic vinyl block region (Ar1) contained in the block copolymer A described above. a ) weight average molecular weight MW(Ar1 a ) is preferably substantially the same as the above, since this can effectively prevent the permanent set from becoming large and can also improve the ease of production of the binder composition.

[0050] -A block region consisting of aliphatic conjugated diene monomer units (D b )- The block region consisting of aliphatic conjugated diene monomer units (aliphatic conjugated diene block region (D b The aliphatic conjugated diene block region (D b ) is a region mainly containing aliphatic conjugated diene monomer units. As in the case of the block copolymer A described above, one aliphatic conjugated diene block region (D b The aliphatic conjugated diene block region (D) can be composed of one or more types of repeating units. b In particular, from the viewpoint of improving the viscosity stability of the resulting slurry composition, the aliphatic conjugated diene block region (D b ) preferably has a graft portion.

[0051] Aliphatic conjugated diene block region (D bExamples of the aliphatic conjugated diene monomer that can be used to form the aliphatic conjugated diene monomer unit of (Block Copolymer A) include the various compounds described above. Among them, it is preferable to use 1,3-butadiene and / or isoprene, and it is particularly preferable to use isoprene. Aliphatic conjugated diene block region (D b By using isoprene in forming the block copolymer B, the adhesive strength of the block copolymer B can be effectively increased.

[0052] In addition, the aliphatic conjugated diene block region (D b Other repeating units that can be contained in the block copolymer (B) include various monomer units similar to those in the case of the block copolymer A described above.

[0053] And the aliphatic conjugated diene block region (D b ) is the weight average molecular weight MW(D a ) is preferably 60,000 or more, more preferably 90,000 or more, and is preferably 400,000 or less, more preferably 300,000 or less, and even more preferably 200,000 or less. a ) is equal to or greater than the above lower limit, the block copolymer B is prevented from becoming excessively hard, and the flexibility of the resulting electrode can be increased. a ) is equal to or less than the above upper limit, the cycle characteristics of the obtained secondary battery can be improved.

[0054] <<Ratio of block copolymer A>> The ratio of block copolymer A is preferably 36% by mass or more, more preferably 38% by mass or more, even more preferably 40% by mass or more, preferably 85% by mass or less, more preferably 80% by mass or less, and even more preferably 75% by mass or less, based on the total mass of block copolymer A and block copolymer B contained in the binder composition for non-aqueous secondary batteries of the present invention taken as 100% by mass. If the ratio of block copolymer A is equal to or greater than the above lower limit, the flexibility of the resulting electrode can be effectively improved. If the ratio of block copolymer A is equal to or less than the above upper limit, the springback of the resulting electrode mixture layer can be effectively suppressed from increasing, and the cycle characteristics of the resulting secondary battery can be further improved. The reason why these advantageous effects are achieved is unclear, but it is believed that if the ratio of block copolymer A is within the above range, the resulting electrode can have a well-balanced combination of the attributes of "low permanent elongation" and "low springback".

[0055] <<Surface acidity of particulate polymer>> The particulate polymer preferably has a surface acid amount of 0.05 mmol / g or more, more preferably 0.06 mmol / g or more, even more preferably 0.08 mmol / g or more, even more preferably 0.10 mmol / g or more, particularly preferably 0.20 mmol / g or more, preferably 0.90 mmol / g or less, more preferably 0.50 mmol / g or less, and even more preferably 0.45 mmol / g or less. If the surface acid amount of the particulate polymer is equal to or more than the above lower limit, the viscosity stability of the slurry composition prepared using the binder composition can be increased, and the cycle characteristics of the obtained secondary battery can be further improved. On the other hand, if the surface acid amount of the particulate polymer is equal to or less than the above upper limit, the electrode formed using the binder composition is less likely to cause springback, and therefore has excellent pressability. Furthermore, if the surface acid amount of the particulate polymer is within the above range, the coating property of the slurry composition can also be improved.

[0056] The surface acid amount of the particulate polymer can be adjusted by changing the type and amount of monomers used in the production of the particulate polymers, block copolymer A and block copolymer B. Specifically, for example, the surface acid amount can be increased by increasing the amount of an acidic group-containing monomer, such as a monomer containing a carboxylic acid group, used.

[0057] <<Vinyl bond content of particulate polymer>> As described above, the block copolymer A and the block copolymer B as particulate polymers are regions containing aliphatic conjugated diene monomer units. Therefore, the "vinyl bond content ratio" of the aliphatic conjugated diene block region contained in these block copolymers A and B is defined as the ratio of 1,2-vinyl bonds and 3,4-vinyl bonds based on all the aliphatic conjugated diene monomer units contained in the aliphatic conjugated diene block region. The vinyl bond content ratio of the aliphatic conjugated diene block region is preferably 1 mol% or more, preferably 20 mol% or less, and more preferably 10 mol% or less. If the vinyl bond content ratio of the aliphatic conjugated diene block region is the above upper limit value or less, the cycle characteristics of the obtained secondary battery can be further improved. The "vinyl bond content ratio" of the aliphatic conjugated diene block region can be measured by the method described in the Examples. In addition, when the particulate polymer is a polymer obtained through graft polymerization, the "vinyl bond content ratio" measured for the particulate polymer before grafting is larger than the "vinyl bond content ratio" measured for the particulate polymer after grafting.

[0058] <<Volume average particle size of particulate polymer>> The particulate polymer preferably has a volume average particle diameter of 50 nm or more, more preferably 200 nm or more, even more preferably 300 nm or more, preferably 1500 nm or less, more preferably 800 nm or less, and even more preferably 500 nm or less. If the volume average particle diameter of the particulate polymer is equal to or greater than the lower limit, the ease of production of the particulate polymer can be improved. If the volume average particle diameter of the particulate polymer is equal to or less than the upper limit, the performance of the particulate polymer as a binder can be improved, and as a result, the cycle characteristics of the obtained secondary battery can be improved. The volume average particle diameter of the particulate polymer can be measured by the method described in the examples.

[0059] <<Proportion of aromatic vinyl monomer units in particulate polymer>> The proportion of aromatic vinyl monomer units in the particulate polymer is preferably 27% by mass or more, more preferably 30% by mass or more, more preferably 70% by mass or less, and more preferably 60% by mass or less, when the total mass of the particulate polymer is taken as 100% by mass. If the proportion of aromatic vinyl monomer units in the particulate polymer is equal to or more than the above lower limit, the particulate polymer can be effectively prevented from exhibiting excessively high tackiness, and when electrodes having the obtained electrode mixture layer are stacked and stored, the electrodes can be effectively prevented from easily blocking each other. On the other hand, if the proportion of aromatic vinyl monomer units in the particulate polymer is equal to or less than the above upper limit, the flexibility of the particulate polymer can be effectively increased, and the flexibility of the obtained electrode can be further increased. In addition, in the block copolymer A and the block copolymer B as the particulate polymer, the proportion of the aromatic vinyl block region in each block copolymer usually coincides with the proportion of the aromatic vinyl monomer units in each block copolymer.

[0060] As described above, the particulate polymer as a component of the binder composition of the present invention may contain the above-mentioned predetermined block copolymer A, and may preferably contain the above-mentioned predetermined block copolymer B. Therefore, the above-mentioned "surface acid amount of the particulate polymer", "volume average particle size of the particulate polymer", and "proportion of aromatic vinyl monomer units in the particulate polymer" correspond to the attribute values ​​of the block copolymer A when the particulate polymer is composed of only the block copolymer A, and correspond to the attribute values ​​of a mixture of these when the particulate polymer contains the block copolymer A and the block copolymer B.

[0061] <<Method for preparing particulate polymer>> The particulate polymer can be prepared, for example, through a process of block polymerizing monomers such as the above-mentioned aromatic vinyl monomers and aliphatic conjugated diene monomers in an organic solvent to obtain a solution of a predetermined block copolymer (block copolymer solution preparation process), a process of adding water to the obtained block copolymer solution to emulsify the block copolymer to form particles (emulsification process), and a process of graft polymerization of the particulate block copolymer to obtain an aqueous dispersion of a particulate polymer consisting of the predetermined copolymer (grafting process). In the preparation of the particulate polymer, the grafting step may be carried out before the emulsification step. That is, the particulate polymer may be prepared by carrying out a step (grafting step) of obtaining a solution of a predetermined polymer by graft polymerization of the block polymer contained in the obtained block polymer solution after the block polymer solution preparation step, and then carrying out a step (emulsification step) of forming particles of the predetermined polymer by adding water to the obtained solution of the predetermined polymer to emulsify it.

[0062] - Block copolymer solution preparation process - The block copolymer solution preparation step can be carried out, for example, using the organic solvent, polymerization initiator, and various additives disclosed in International Publication No. 2009 / 123089 under the conditions disclosed in the same document. More specifically, in the block copolymer solution preparation step, (1) Polymerizing an aromatic vinyl monomer in an organic solvent using a polymerization initiator to obtain an aromatic vinyl polymer having an active terminal; (2) adding an aliphatic conjugated diene monomer to the solution containing the aromatic vinyl polymer having active terminals to obtain an aromatic vinyl-aliphatic conjugated diene block copolymer having active terminals; (3) adding a bifunctional coupling agent to the solution containing the aromatic vinyl-aliphatic conjugated diene block copolymer having the obtained active terminal in an amount such that the functional group is less than 1 molar equivalent relative to the active terminal to form a block copolymer B; (4) An aromatic vinyl monomer is added thereto and further polymerized to form a block copolymer A, thereby obtaining a block copolymer solution. The block copolymer solution obtained through the above operations (1) to (4) contains a mixture of block copolymer A and block copolymer B. For example, when only block copolymer A is to be synthesized, the above operation (3) can be omitted.

[0063] -Emulsification process- The emulsification method in the emulsification step is not particularly limited, but for example, a method of phase inversion emulsification of a preliminary mixture of the block copolymer solution obtained in the above-mentioned block copolymer solution preparation step and an aqueous solution of an emulsifier is preferred. Here, for example, a known emulsifier and emulsification disperser can be used for phase inversion emulsification. Specifically, the emulsification disperser is not particularly limited, and examples thereof include batch-type emulsification dispersers such as the product name "Homogenizer" (manufactured by IKA), the product name "Polytron" (manufactured by Kinematica), and the product name "TK Auto Homo Mixer" (manufactured by Tokushu Kika Kogyo); the product name "TK Pipeline Homo Mixer" (manufactured by Tokushu Kika Kogyo), the product name "Colloid Mill" (manufactured by Kobe Steel Pantech), the product name "Thrasher" (manufactured by Nippon Coke & Engineering Co., Ltd.), the product name "Trigonal Wet Fine Grinding Mill" (manufactured by Mitsui Miike Chemical Engineering Co., Ltd.), and the product name "Cavitron" (manufactured by Eurotech), Continuous emulsifying and dispersing machines such as "Milder" (manufactured by Pacific Machinery Co., Ltd.) and "Fine Flow Mill" (manufactured by Pacific Machinery Co., Ltd.); high-pressure emulsifying and dispersing machines such as "Microfluidizer" (manufactured by Mizuho Kogyo Co., Ltd.), "Nanomizer" (manufactured by Nanomizer Co., Ltd.), and "APV Gaulin" (manufactured by Gaulin Co., Ltd.); membrane emulsifying and dispersing machines such as "Membrane Emulsifier" (manufactured by Reika Kogyo Co., Ltd.); vibration emulsifying and dispersing machines such as "Vibro Mixer" (manufactured by Reika Kogyo Co., Ltd.); ultrasonic emulsifying and dispersing machines such as "Ultrasonic Homogenizer" (manufactured by Branson Co., Ltd.); and the like can be used. The conditions for the emulsifying operation using the emulsifying and dispersing machine (e.g., processing temperature, processing time, etc.) are not particularly limited and may be appropriately selected so as to obtain the desired dispersion state. Then, from the emulsion obtained after the phase inversion emulsification, the organic solvent may be removed, if necessary, by a known method, to obtain an aqueous dispersion of the particulate block copolymer.

[0064] - Grafting process - The method of graft polymerization in the grafting step is not particularly limited. For example, a method in which graft polymerization and crosslinking of a block polymer are simultaneously carried out using a radical initiator such as a redox initiator in the presence of a monomer to be graft polymerized is preferred. Here, the reaction conditions can be adjusted depending on the composition of the block copolymer, the desired amount of surface acid, and the like. In the grafting step, an aqueous dispersion of the particulate polymer can be obtained. When the grafting step is performed after the emulsification step, that is, when graft polymerization is performed on the particulate block copolymer, the monomer units introduced by graft polymerization, such as the acidic group-containing monomer units, are present more on the surface side than in the center of the particulate polymer, and are unevenly distributed in the surface layer portion.

[0065] <Dispersion medium> The dispersion medium contained in the binder composition is not particularly limited, and may be water. The dispersion medium may be an aqueous solution or a mixed solution of water and a small amount of an organic solvent.

[0066] <Other ingredients> Other components that can be contained in the binder composition are not particularly limited, and can include, for example, reinforcing materials, leveling agents, viscosity modifiers, electrolyte additives, etc. These components can be used alone or in combination of two or more at any ratio.

[0067] <Method of preparing binder composition> The binder composition of the present invention is not particularly limited, and can be prepared by mixing the particulate polymer and other components that are optionally used in a dispersion medium. When the binder composition is prepared using a dispersion liquid of the particulate polymer, the liquid contained in the dispersion liquid may be used as it is as a dispersion medium of the binder composition.

[0068] (Slurry composition for non-aqueous secondary battery electrodes) The slurry composition of the present invention is a composition used for forming an electrode mixture layer of an electrode, and contains the above-mentioned binder composition and further contains an electrode active material. That is, the slurry composition of the present invention contains the above-mentioned particulate polymer and electrode active material, and optionally further contains other components. And, since the slurry composition of the present invention contains the above-mentioned binder composition, an electrode having an electrode mixture layer formed from the slurry composition has sufficiently high flexibility, and can improve the cycle characteristics of the obtained secondary battery.

[0069] <Binder composition> As the binder composition, the above-mentioned binder composition of the present invention containing a predetermined particulate polymer is used. The amount of the binder composition in the slurry composition is not particularly limited. For example, the amount of the binder composition may be such that the amount of the particulate polymer is 0.5 parts by mass or more and 15 parts by mass or less in terms of solid content per 100 parts by mass of the electrode active material.

[0070] <Electrode active material> The electrode active material is not particularly limited, and any known electrode active material used in secondary batteries can be used. Specifically, for example, the electrode active material that can be used in the electrode mixture layer of a lithium ion secondary battery, which is an example of a secondary battery, is not particularly limited, and the following electrode active materials can be used.

[0071] <<Cathode active material>> The positive electrode active material to be blended in the positive electrode composite layer of the positive electrode of the lithium ion secondary battery may be, for example, a compound containing a transition metal, such as a transition metal oxide, a transition metal sulfide, a composite metal oxide of lithium and a transition metal, etc. Examples of the transition metal include Ti, V, Cr, Mn, Fe, Co, Ni, Cu, and Mo. Specifically, the positive electrode active material is not particularly limited, and may be lithium-containing cobalt oxide (LiCoO 2 ), lithium manganate (LiMn 2 O 4) Lithium-containing nickel oxide (LiNiO 2 ) Lithium-containing composite oxides of Co-Ni-Mn, lithium-containing composite oxides of Ni-Mn-Al, lithium-containing composite oxides of Ni-Co-Al, olivine-type lithium iron phosphate (LiFePO 4 ) Olivine-type lithium manganese phosphate (LiMnPO 4 ) Li 1+x Mn 2-x O 4 (0 < X < 2) Spinel compounds with excess lithium, Li[Ni 0.17 Li 0.2 Co 0.07 Mn 0.56 O 2 LiNi 0.5 Mn 1.5 O 4 etc. can be mentioned. Note that the above-mentioned positive electrode active materials may be used alone or in combination of two or more.

[0072] <<Negative electrode active material>> As the negative electrode active material incorporated in the negative electrode mixture layer of the negative electrode of the lithium ion secondary battery, for example, carbon-based negative electrode active materials, metal-based negative electrode active materials, and negative electrode active materials combining these can be mentioned. Here, the carbon-based negative electrode active material refers to an active material having carbon as the main skeleton into which lithium can be inserted (also referred to as "doped"). Specifically, as the carbon-based negative electrode active material, there are, for example, coke, mesocarbon microbeads (MCMB), mesophase pitch-based carbon fibers, pyrolytic vapor-grown carbon fibers, phenolic resin fired bodies, polyacrylonitrile-based carbon fibers, isotropic carbon, furfuryl alcohol resin fired bodies (PFA), and hard carbon and other carbonaceous materials, as well as graphite materials such as natural graphite and artificial graphite. The metal-based negative electrode active material is an active material containing a metal, and usually refers to an active material that contains an element capable of inserting lithium in its structure and has a theoretical electric capacity of 500mAh / g or more per unit mass when lithium is inserted. Examples of the metal-based active material include lithium metal, elemental metals capable of forming lithium alloys (e.g., Ag, Al, Ba, Bi, Cu, Ga, Ge, In, Ni, P, Pb, Sb, Si, Sn, Sr, Zn, Ti, etc.), and oxides, sulfides, nitrides, silicides, carbides, phosphides, etc. thereof. Furthermore, oxides such as lithium titanate can be mentioned. The negative electrode active materials described above may be used alone or in combination of two or more.

[0073] <Other ingredients> Other components that can be added to the slurry composition are not particularly limited, and include conductive materials and other components that can be added to the binder composition of the present invention. The other components may be used alone or in combination of two or more in any ratio.

[0074] <Preparation of Slurry Composition> The method for preparing the slurry composition is not particularly limited. For example, a binder composition, an electrode active material, and other components used as necessary can be mixed in the presence of an aqueous medium to prepare a slurry composition. The aqueous medium used in preparing the slurry composition includes the aqueous medium contained in the binder composition. The mixing method is not particularly limited, but mixing can be performed using a commonly used stirrer or disperser.

[0075] (Electrode for non-aqueous secondary batteries) The electrode for a non-aqueous secondary battery of the present invention comprises an electrode mixture layer formed using the above-mentioned slurry composition for a non-aqueous secondary battery electrode. Therefore, the electrode mixture layer is made of a dried product of the above-mentioned slurry composition, and usually contains an electrode active material and a component derived from a particulate polymer, and optionally contains other components. Note that each component contained in the electrode mixture layer is contained in the above-mentioned slurry composition for a non-aqueous secondary battery electrode, and the preferred abundance ratio of each component is the same as the preferred abundance ratio of each component in the slurry composition. In addition, the particulate polymer exists in a particulate form in the slurry composition, but in the electrode mixture layer formed using the slurry composition, it may be in a particulate form or any other form. Furthermore, since the non-aqueous secondary battery electrode of the present invention has an electrode mixture layer formed using the above-mentioned slurry composition for a non-aqueous secondary battery electrode, it has sufficiently high flexibility and can improve the cycle characteristics of the resulting secondary battery.

[0076] <Production of electrodes for non-aqueous secondary batteries> Here, the electrode mixture layer of the electrode for a non-aqueous secondary battery of the present invention can be formed, for example, by the following method. 1) A method in which the slurry composition of the present invention is applied to the surface of a current collector, and then dried; 2) a method of immersing a current collector in the slurry composition of the present invention and then drying the same; and 3) A method in which the slurry composition of the present invention is applied onto a release substrate, followed by drying to produce an electrode mixture layer, and the resulting electrode mixture layer is transferred onto the surface of a current collector. Among these, the method 1) is particularly preferred because it is easy to control the thickness of the electrode mixture layer. Specifically, the method 1) includes a step of applying a slurry composition onto a current collector (application step) and a step of drying the slurry composition applied onto the current collector to form an electrode mixture layer on the current collector (drying step).

[0077] [Coating process] The method of applying the above-mentioned slurry composition onto the current collector is not particularly limited, and any known method can be used. Specifically, the application method can be a doctor blade method, a dip method, a reverse roll method, a direct roll method, a gravure method, an extrusion method, a brush coating method, or the like. In this case, the slurry composition may be applied to only one side of the current collector, or may be applied to both sides. The thickness of the slurry film on the current collector after application and before drying can be appropriately set according to the thickness of the electrode mixture layer obtained by drying.

[0078] Here, the current collector to which the slurry composition is applied is made of a material that is electrically conductive and electrochemically durable. Specifically, the current collector may be made of, for example, iron, copper, aluminum, nickel, stainless steel, titanium, tantalum, gold, platinum, etc. The above-mentioned materials may be used alone or in combination of two or more kinds in any ratio.

[0079] [Drying process] The method for drying the slurry composition on the current collector is not particularly limited and may be a known method, for example, a drying method using warm air, hot air, or low-humidity air, a vacuum drying method, or a drying method using irradiation with infrared rays or electron beams, etc. By drying the slurry composition on the current collector in this manner, an electrode mixture layer can be formed on the current collector, and a nonaqueous secondary battery electrode including the current collector and the electrode mixture layer can be obtained.

[0080] After the drying step, the electrode mixture layer may be subjected to a pressure treatment using a mold press or a roll press. The pressure treatment can improve the adhesion between the electrode mixture layer and the current collector and further increase the density of the resulting electrode mixture layer. In addition, when the electrode mixture layer contains a curable polymer, it is preferable to cure the polymer after the electrode mixture layer is formed.

[0081] (Non-aqueous secondary battery) The nonaqueous secondary battery of the present invention includes a positive electrode, a negative electrode, an electrolyte, and a separator, and uses the above-mentioned nonaqueous secondary battery electrode as at least one of the positive electrode and the negative electrode. Since the nonaqueous secondary battery of the present invention uses the above-mentioned nonaqueous secondary battery electrode as at least one of the positive electrode and the negative electrode, the nonaqueous secondary battery of the present invention has excellent cycle characteristics. In the following, a case where the secondary battery is a lithium ion secondary battery will be described as an example, but the present invention is not limited to the following example.

[0082] <Electrode> Here, the electrode other than the above-mentioned electrode for a nonaqueous secondary battery of the present invention that can be used in the nonaqueous secondary battery of the present invention is not particularly limited, and a known electrode used in the manufacture of a secondary battery can be used. Specifically, the electrode other than the above-mentioned electrode for a nonaqueous secondary battery of the present invention can be an electrode formed by forming an electrode mixture layer on a current collector using a known manufacturing method.

[0083] <Electrolyte> The electrolyte is usually an organic electrolyte in which a supporting electrolyte is dissolved in an organic solvent. For example, a lithium salt is used as the supporting electrolyte of the lithium ion secondary battery. For example, LiPF 6 , LiAsF 6 , LiBF 4 , LiSbF 6 , LiAlCl 4 , LiClO 4 , C.F. 3 SO 3 Li, C. 4 F 9 SO 3 Li, C.F. 3 COOLi, (CF 3 CO) 2 NLi, (CF 3 SO 2 ) 2 NLi, (C 2 F 5 SO 2 Among them, LiPF is the most popular because it is easily soluble in solvents and has a high degree of dissociation. 6 , LiClO4 , C.F. 3 SO 3 Li is preferred. The electrolyte may be used alone or in any combination of two or more kinds in any ratio. Usually, the lithium ion conductivity tends to be higher when a supporting electrolyte with a higher degree of dissociation is used, so the lithium ion conductivity can be adjusted by the type of supporting electrolyte.

[0084] The organic solvent used in the electrolyte is not particularly limited as long as it can dissolve the supporting electrolyte, but for example, carbonates such as dimethyl carbonate (DMC), ethylene carbonate (EC), diethyl carbonate (DEC), propylene carbonate (PC), butylene carbonate (BC), ethyl methyl carbonate (EMC), vinylene carbonate (VC), etc.; esters such as γ-butyrolactone and methyl formate; ethers such as 1,2-dimethoxyethane and tetrahydrofuran; sulfur-containing compounds such as sulfolane and dimethyl sulfoxide; and the like are preferably used. A mixture of these solvents may also be used. Among them, it is preferable to use carbonates because they have a high dielectric constant and a wide stable potential range. Usually, the lower the viscosity of the solvent used, the higher the lithium ion conductivity tends to be, so the lithium ion conductivity can be adjusted by the type of solvent. The concentration of the electrolyte in the electrolytic solution can be appropriately adjusted. Known additives can be added to the electrolytic solution.

[0085] <separator> The separator is not particularly limited, and may be one described in, for example, JP 2012-204303 A. Among these, a microporous film made of a polyolefin resin (polyethylene, polypropylene, polybutene, polyvinyl chloride) is preferred, since it can reduce the thickness of the entire separator, thereby increasing the ratio of the electrode active material in the secondary battery and increasing the capacity per volume.

[0086] The secondary battery of the present invention can be manufactured, for example, by stacking a positive electrode and a negative electrode with a separator interposed therebetween, wrapping or folding the stack according to the shape of the battery as necessary, placing the stack in a battery container, injecting an electrolyte into the battery container, and sealing the container. Here, in the nonaqueous secondary battery of the present invention, the above-mentioned electrode for a nonaqueous secondary battery is used as at least one of the positive electrode and the negative electrode, preferably the negative electrode. In addition, in the nonaqueous secondary battery of the present invention, a fuse, an overcurrent prevention element such as a PTC element, an expanded metal, a lead plate, etc. may be provided as necessary to prevent the occurrence of an internal pressure rise of the secondary battery, overcharging and discharging, etc. The shape of the secondary battery may be, for example, any of a coin type, a button type, a sheet type, a cylindrical type, a square type, a flat type, etc. EXAMPLES

[0087] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the following description, the units "%" and "parts" expressing amounts are by mass unless otherwise specified. In addition, in a polymer produced by polymerizing multiple types of monomers, the ratio of monomer units formed by polymerizing a certain monomer in the polymer usually coincides with the ratio (feed ratio) of that certain monomer to all monomers used in the polymerization of the polymer, unless otherwise specified. In the examples and comparative examples, various attributes were measured by the following methods. In the examples and comparative examples, various evaluations were performed by the following methods.

[0088] <Weight average molecular weight of block copolymers A and B> The weight average molecular weight of the aqueous dispersion of the particulate polymer prepared in the Examples and Comparative Examples was determined as a polystyrene-equivalent molecular weight by high performance liquid chromatography at a flow rate of 0.35 ml / min using tetrahydrofuran as a carrier. The apparatus used was HLC8220 manufactured by Tosoh Corporation, the column used was three Shodex KF-404HQs manufactured by Showa Denko K.K. connected together (column temperature 40°C), and the detectors used were a differential refractometer and an ultraviolet detector. The molecular weight was calibrated at 12 points using standard polystyrene (5 to 3 million) manufactured by Polymer Laboratory Co., Ltd.

[0089] <Mass Ratio of Block Copolymer A and Block Copolymer B> The mass ratio of block copolymer A to block copolymer B was calculated from the areas of the peaks corresponding to block copolymer A and block copolymer B in the chart obtained when measuring the above-mentioned <Weight average molecular weights of block copolymers A and B>.

[0090] Each aromatic vinyl block region (Ar1) contained in block copolymers A and B a ,Ar2 a ,Ar1 b ,Ar2 b ) Weight average molecular weight> According to the method described in Rubber Chemistry and Technology, Vol. 45, pp. 1295 (1972), the block copolymers A and B obtained in the examples and comparative examples were reacted with ozone and reduced with lithium aluminum hydride to decompose the isoprene polymer blocks, which are the aliphatic conjugated diene block regions of the block copolymers A and B. Specifically, the following procedure was performed. The aqueous dispersion (binder composition) of the particulate polymer obtained in the examples and comparative examples was dried under an environment of 50% absolute humidity and 23°C to 25°C temperature to prepare a polymer film having a thickness of 3±0.3 mm as a sample. 300 mg of the sample was dissolved in a reaction vessel containing 100 ml of dichloromethane treated with molecular sieves. The reaction vessel was placed in a cooling tank and cooled to -25°C, and ozone generated by an ozone generator was introduced into the reaction vessel while oxygen was flowing at a flow rate of 170 ml / min. After 30 minutes had passed since the start of the reaction, the gas flowing out of the reaction vessel was introduced into an aqueous potassium iodide solution to confirm that the reaction was complete. Next, 50 ml of diethyl ether and 470 mg of lithium aluminum hydride were charged into another reaction vessel substituted with nitrogen, and the solution reacted with ozone was slowly dropped into the reaction vessel while cooling the reaction vessel with ice water. Then, the reaction vessel was placed in a water bath, gradually heated, and refluxed at 40°C for 30 minutes. After that, dilute hydrochloric acid was dropped into the reaction vessel little by little while stirring the solution, and the dropwise addition was continued until the generation of hydrogen was hardly observed. After this reaction, the solid product generated in the solution was filtered, and the solid product was extracted with 100 ml of diethyl ether for 10 minutes. This extract and the filtrate from the filtration were combined, and the solvent was distilled off to obtain a solid sample. The weight average molecular weight of the sample thus obtained was measured according to the above-mentioned method for measuring weight average molecular weight, and the value was taken as the weight average molecular weight of the styrene block as the aromatic vinyl block region.

[0091] <Each aliphatic conjugated diene block region (D a ,D b ) Weight average molecular weight> The weight average molecular weight of the corresponding aromatic vinyl block region was subtracted from the weight average molecular weight of each of block copolymer A and block copolymer B determined as described above, and the weight average molecular weight of the aliphatic conjugated diene block region was determined based on the calculated value.

[0092] <Proportion of aromatic vinyl monomer units in each of block copolymers A and B> Based on the detection intensity ratio between the differential refractometer and the ultraviolet detector in the above-mentioned high performance liquid chromatography measurement, the proportion (mass%) of the aromatic vinyl monomer unit was determined for each of the block copolymers A and B. Note that, a plurality of copolymers having different contents of styrene units as aromatic vinyl monomer units were prepared in advance, and a calibration curve was created using them. Based on the proportions of aromatic vinyl monomer units in each of the block copolymers A and B obtained by this measurement, the aromatic vinyl block regions (Ar1) contained in the block copolymers A and B were calculated. a ,Ar2 a ,Ar1 b ,Ar2 b The weight average molecular weight of each aromatic vinyl block region (Ar1 a ,Ar2 a ,Ar1 b ,Ar2 b It was determined which block copolymer the weight average molecular weight value of the block region of the block copolymer belonged to.

[0093] <Vinyl bond content of particulate polymer> The block copolymer solution obtained by the block copolymer solution preparation step was subjected to proton NMR measurement to determine the aliphatic conjugated diene block region (D a ,D b The vinyl bond content (mol%) of the aliphatic conjugated diene block region (D a ,D b ) indicates the proportion (mol %) of vinyl bonds contained in the copolymer.

[0094] <Surface acid amount of particulate polymer> The aqueous dispersion of the particulate polymer (binder composition) obtained in the examples and comparative examples was diluted with a 0.3% aqueous dodecylbenzenesulfonic acid solution to adjust the solid content to 10%. Then, the mixture was centrifuged at 7000G for 30 minutes to separate the light liquid. The obtained light liquid was diluted with a 0.3% aqueous dodecylbenzenesulfonic acid solution to adjust the solid content to 10%. Then, the mixture was centrifuged at 7000G for 30 minutes to separate the light liquid. The obtained light liquid was diluted with a 0.3% aqueous dodecylbenzenesulfonic acid solution to adjust the solid content to 10%. Then, the adjusted sample was centrifuged at 7000G for 30 minutes to separate the light liquid. The obtained light liquid was adjusted to pH 12.0 with a 5% aqueous sodium hydroxide solution. 3.0 g of the pH-adjusted sample was placed in a 100 mL beaker in terms of solid content, and 3 g of an aqueous solution of Kao's Emulgen 120 diluted to 0.2% and 1 g of an aqueous solution of Toray Dow Corning's SM5512 diluted to 1% were added. While stirring uniformly with a stirrer, 0.1 N hydrochloric acid was added at a rate of 0.5 mL / 30 seconds, and the electrical conductivity was measured every 30 seconds. The obtained electrical conductivity data was plotted on a graph with electrical conductivity on the vertical axis (Y-axis) and the cumulative amount of hydrochloric acid added on the horizontal axis (X-axis). As a result, a hydrochloric acid amount-electrical conductivity curve with three inflection points is obtained as shown in Figure 1. The X-coordinates of the three inflection points are designated P1, P2, and P3, in ascending order of value. Approximation lines L1, L2, and L3 are obtained by the least squares method for data in the three sections of X-coordinates from zero to coordinate P1, from coordinate P1 to coordinate P2, and from coordinate P2 to coordinate P3. The X-coordinate of the intersection of the approximation lines L1 and L2 is designated A1, and the X-coordinate of the intersection of the approximation lines L2 and L3 is designated A2. Then, the amount of surface acid per 1 g of the particulate polymer is calculated as a hydrochloric acid equivalent value (mmol / g) from the following formula (a). (a) Amount of surface acid per 1 g of particulate polymer = (A2-A1) / 3.0 g

[0095] <Volume average particle size of particulate polymer> The solid content of the aqueous dispersion of the particulate polymer (binder composition) obtained in the examples and comparative examples was adjusted to 0.1% by mass, and the particle size distribution (volume basis) of the aqueous dispersion of the polymer after the solid content adjustment was measured using a laser diffraction particle size distribution measuring device (manufactured by Beckman Coulter, Inc., product name "LS-230"). Then, the particle size at which the cumulative volume calculated from the small diameter side in the obtained particle size distribution becomes 50% was obtained, and this was taken as the volume average particle size (D50) of the particulate polymer.

[0096] <Viscosity stability of slurry composition> When preparing the slurry composition, an aliquot of the solution before the addition of the binder composition was taken, and the viscosity M0 (mPa s) was measured using a B-type viscometer (manufactured by Toki Sangyo Co., Ltd., product name "TV-25") under the conditions of a measurement temperature of 25°C, measurement rotor No. 4, and a rotor rotation speed of 60 rpm. Furthermore, the slurry composition obtained by adding the binder composition was dispensed and placed in a container with a diameter of 5.5 cm and a height of 8.0 cm, and stirred at 3000 rpm for 10 minutes using a TK Homodisper (manufactured by Primix Corporation, disper diameter: 40 mm). The viscosity M1 (mPa s) of the slurry composition after stirring was measured in the same manner as the viscosity M0 of the solution before the addition of the binder composition. Then, the viscosity change rate ΔM (={(M1-M0) / M0}×100%) was calculated and evaluated according to the following criteria. A smaller viscosity change rate ΔM indicates higher viscosity stability of the slurry composition. A: Viscosity change rate ΔM is less than 10% B: Viscosity change rate ΔM is 10% or more

[0097] <Electrode flexibility> Rods of different diameters were placed on the negative electrode composite layer side of the negative electrodes for lithium ion secondary batteries obtained in the Examples and Comparative Examples, and the negative electrodes were wrapped around the rods to evaluate whether the negative electrode composite layer cracked. The smaller the diameter of the rod that did not crack when wrapped, the more flexible the negative electrode was and the more excellent the winding properties were. Excellent winding properties can suppress peeling of the negative electrode composite layer, resulting in excellent cycle characteristics of the secondary battery. A: The smallest rod diameter that can be wrapped around without breaking is 1.2 mm. B: The smallest rod diameter that can be wrapped around without breaking is 1.5 mm. C: The smallest rod diameter that can be wrapped around without breaking is 2 mm. D: The smallest rod diameter that can be wrapped around without breaking is 3 mm.

[0098] <Springback of electrode mixture layer> The springback of the electrode mixture layer was evaluated based on the electrode density. Specifically, the negative electrode mixture layer side of the negative electrode raw material prepared in the examples and comparative examples was first roll-pressed under conditions of a temperature of 25±3°C and a linear pressure of 11 t (tons) to obtain an electrode mixture layer density of 1.70 g / cm. 3 The negative electrode was then left for one week in an environment with a temperature of 25±3°C and a relative humidity of 50±5%. The electrode mixture layer density (g / cm 3 ) was measured and evaluated according to the following criteria. A higher density of the electrode mixture layer after standing indicates that the electrode mixture layer does not spring back and has excellent pressability, and the electrode has been effectively densified. A: The density of the electrode mixture layer after standing is 1.65 g / cm 3 End B: The density of the electrode mixture layer after standing is 1.65 g / cm 3 less than

[0099] <Cycle characteristics> The lithium ion secondary batteries obtained in the examples and comparative examples were subjected to a charge-discharge cycle test in which the batteries were charged at a constant current of 0.5C at 60°C until the battery reached 4.2V, then charged at a constant voltage, and then discharged at a constant current of 0.5C until the battery reached 3.0V. The charge-discharge cycle test was performed up to 100 cycles, and the ratio of the discharge capacity at the 100th cycle to the initial discharge capacity was taken as the capacity retention rate. The capacity retention rate was evaluated according to the following criteria. A larger capacity retention rate indicates a smaller decrease in capacity due to repeated charging and discharging. A: Capacity retention rate is 90% or more B: Capacity retention rate is 80% or more and less than 90% C: Capacity retention rate is 75% or more and less than 80% D: Capacity retention rate is less than 75%

[0100] Example 1 <Preparation of particulate polymer> <<Block copolymer solution preparation process>> ·Operation(1) In a pressure reactor, 20.0 kg of cyclohexane as a polymerization solvent, 2.2 mmol of N,N,N',N'-tetramethylethylenediamine (hereinafter referred to as "TMEDA") as a Lewis base compound added for the purpose of preparing a block structure, and 1.50 kg of styrene as an aromatic vinyl monomer were added and stirred at 40°C. 149.6 mmol of n-butyllithium as a polymerization initiator was added, and polymerization was carried out for 1 hour while raising the temperature to 50°C, to obtain a styrene polymer as an aromatic vinyl polymer having an active terminal. The polymerization conversion rate of styrene was 100%. ·Operation(2) Subsequently, 6.50 kg of isoprene as an aliphatic conjugated diene monomer was continuously added to the reactor over 1 hour while controlling the temperature to maintain 50-60°C. After the addition of isoprene was completed, polymerization was continued for another 1 hour to obtain a styrene-isoprene block copolymer as an aromatic vinyl-aliphatic conjugated diene block copolymer having active terminals. The polymerization conversion rate of isoprene was 100%. ·Operation(3) Next, 47.1 mmol of dimethyldichlorosilane was added as a coupling agent, and a coupling reaction was carried out for 2 hours to form a styrene-isoprene-styrene block copolymer which became block copolymer B. ·Operation(4) Thereafter, 2.10 kg of styrene as an aromatic vinyl monomer was continuously added over 1 hour while controlling the temperature to maintain it at 50 to 60° C. After the addition of styrene was completed, polymerization was continued for another 1 hour to form a styrene-isoprene-styrene block copolymer that would become block copolymer A. The polymerization conversion rate of styrene was 100%. ·Operation(5) Thereafter, 299.1 mmol of methanol was added as a polymerization terminator and mixed thoroughly to terminate the reaction. A portion of the reaction solution (block copolymer solution) obtained as described above was taken out, and various attributes were measured according to the methods described above. The results are shown in Table 1.

[0101] <<Emulsification process (phase inversion emulsification process)>> A mixture of sodium alkylbenzenesulfonate, sodium polyoxyethylene alkylsulfosuccinate, and sodium polyoxyethylene alkyl ether sulfate in a ratio of 1:1:1 (by mass) was dissolved in ion-exchanged water to prepare a 5% aqueous solution. Then, 500 g of the obtained block polymer solution and 500 g of the obtained aqueous solution were charged into a tank and premixed by stirring. The premix was then transferred from the tank to a continuous high-efficiency emulsifying and dispersing machine (manufactured by Pacific Machinery Works, product name "Milder MDN303V") at a speed of 100 g / min using a metering pump, and stirred at a rotation speed of 15,000 rpm to obtain an emulsion in which the premix was subjected to phase inversion emulsification. Next, the cyclohexane in the obtained emulsion was distilled off under reduced pressure using a rotary evaporator.Then, the distilled emulsion was left to stand for one day in a chromatographic column equipped with a cock for separation, and the lower layer after separation was removed to concentrate the emulsion. Finally, the upper layer was filtered through a 100 mesh wire screen to obtain an aqueous dispersion containing particulate block polymer (block polymer latex).

[0102] <<Grafting process>> In the grafting process, crosslinking was carried out simultaneously with graft polymerization. The block polymer latex obtained in the above emulsification process was diluted by adding 850 parts of distilled water per 100 parts of solid content. The diluted block polymer latex was then placed in a nitrogen-substituted polymerization reaction vessel equipped with a stirrer and heated to 30°C while stirring. In addition, 10 parts of methacrylic acid as an acidic group-containing monomer and 16 parts of distilled water were mixed in another vessel to prepare a diluted methacrylic acid solution. This diluted methacrylic acid solution was added to a polymerization reaction vessel heated to 30° C. over a period of 30 minutes. Furthermore, a solution containing 7 parts of distilled water and 0.01 parts of ferrous sulfate (manufactured by Chubu Chelesto Co., Ltd., product name "Frost Fe") as a reducing agent was prepared in a separate container. The obtained solution was added to a polymerization reaction vessel, and then 0.5 parts of 1,1,3,3-tetramethylbutyl hydroperoxide (manufactured by Nippon Oil & Fats Co., Ltd., product name "Perocta H") as an oxidizing agent was added, and the reaction was carried out at 30°C for 1 hour, and then at 70°C for another 2 hours. The polymerization conversion rate was 99%. Then, an aqueous dispersion of a particulate polymer (binder composition) consisting of a polymer obtained by graft polymerization and crosslinking of the block polymer was obtained. Using the obtained aqueous dispersion of the particulate polymer, various attributes of the particulate polymer were measured. The results are shown in Table 1.

[0103] <Preparation of Slurry Composition for Non-Aqueous Secondary Battery Negative Electrode> A mixture was obtained by adding 100 parts of artificial graphite (capacity: 360 mAh / g) as a negative electrode active material, 1 part of carbon black (manufactured by TIMCAL, product name "Super C65") as a conductive material, and 1.2 parts of a 2% aqueous solution of carboxymethylcellulose (manufactured by Nippon Paper Chemicals, product name "MAC-350HC") as a thickener in terms of solid content to a planetary mixer with a disperser. The obtained mixture was adjusted to a solid content concentration of 60% with ion-exchanged water, and then mixed at 25°C for 60 minutes. Next, the solid content concentration was adjusted to 52% with ion-exchanged water, and then mixed for another 15 minutes at 25°C to obtain a mixed liquid. 2.0 parts of the binder composition consisting of the aqueous dispersion prepared above in terms of solid content and ion-exchanged water were added to the obtained mixed liquid, and the final solid content concentration was adjusted to 48%. After further mixing for 10 minutes, the mixture was defoamed under reduced pressure to obtain a slurry composition for a negative electrode with good fluidity. The viscosity stability of the slurry composition for the negative electrode was evaluated during the preparation of the slurry composition, and the results are shown in Table 1. <Formation of the negative electrode> The obtained slurry composition for negative electrodes was coated on a copper foil having a thickness of 15 μm, which was used as a current collector, with a comma coater so that the coating weight after drying was 11 mg / cm 2The copper foil was coated so that the thickness of the coating was 100 μm and dried. The drying was performed by conveying the copper foil at a speed of 0.5 m / min through an oven at 60° C. for 2 minutes. The copper foil was then heat-treated at 120° C. for 2 minutes to obtain a negative electrode blank. The obtained negative electrode blank was evaluated according to the above-mentioned method to obtain the evaluation result of the springback of the electrode (negative electrode) composite layer. The results are shown in Table 1. The negative electrode raw material is then rolled with a roll press to make the density of the negative electrode mixture layer 1.75 g / cm 3 A negative electrode of 1000 nm was obtained. The obtained negative electrode was evaluated according to the above-mentioned method to obtain the evaluation results of the electrode flexibility. The results are shown in Table 1. <Formation of the positive electrode> LiCoO with a volume average particle size of 12 μm as a positive electrode active material 2 100 parts of the above, 2 parts of acetylene black (manufactured by Denki Kagaku Kogyo Co., Ltd., product name "HS-100") as a conductive material, 2 parts of polyvinylidene fluoride (manufactured by Kureha Corporation, product name "#7208") as a binder in terms of solid content, and N-methylpyrrolidone as a solvent were mixed to a total solid content concentration of 70%. These were mixed using a planetary mixer to obtain a slurry composition for a positive electrode. The obtained slurry composition for positive electrodes was coated on an aluminum foil having a thickness of 20 μm, which was used as a current collector, with a comma coater so that the basis weight after drying was 23 mg / cm 2 The aluminum foil was then dried by conveying it through an oven at 60° C. for 2 minutes at a speed of 0.5 m / min. Thereafter, the aluminum foil was heated at 120° C. for 2 minutes to obtain a positive electrode sheet. The positive electrode raw material is then rolled with a roll press to make the density of the positive electrode mixture layer 4.0 g / cm 3 A positive electrode of 1000 nm was obtained. <Preparing the separator> As a separator made of a separator substrate, a single-layer polypropylene separator (manufactured by Celgard, product name "Celgard 2500") was prepared. <Production of lithium-ion secondary battery> The obtained positive electrode was cut into a rectangle of 49 cm x 5 cm and placed with the surface on the positive electrode composite layer side facing up, and a separator cut to 120 cm x 5.5 cm was placed on the positive electrode composite layer so that the positive electrode was located on the left side of the separator in the longitudinal direction. Furthermore, the obtained negative electrode was cut into a rectangle of 50 x 5.2 cm and placed on the separator so that the surface on the negative electrode composite layer side faced the separator and the negative electrode was located on the right side of the separator in the longitudinal direction. Then, the obtained laminate was wound by a winding machine to obtain a wound body. The obtained wound body was pressed. This wound body was wrapped in an aluminum packaging exterior as the exterior of the battery, and an electrolyte (solvent: ethylene carbonate / diethyl carbonate / vinylene carbonate = 68.5 / 30 / 1.5 (volume ratio), electrolyte: LiPF with a concentration of 1M) was added. 6 ) was injected so that no air remained, and the opening of the aluminum packaging exterior was closed by heat sealing at 150°C to produce a wound type lithium ion secondary battery with a capacity of 800 mAh. It was confirmed that this lithium ion secondary battery operated well. The cycle characteristics of the obtained secondary battery were evaluated as described above. The results are shown in Table 1.

[0104] (Examples 2 to 4, Comparative Example 2) In the block copolymer solution preparation step, the amounts of styrene, isoprene, n-butyllithium, TMEDA, dimethyldichlorosilane, methanol, and the like to be added were appropriately changed as necessary so that block copolymer A contained in the obtained block copolymer solution satisfied the constitutional conditions shown in Table 1. Except for this, various operations, measurements, and evaluations were carried out in the same manner as in Example 1. The results are shown in Table 1.

[0105] Example 5 In the block copolymer solution preparation step, the amount of coupling agent added in "operation (3)" was changed so that the mass ratio of block copolymers A and B contained in the resulting block copolymer solution would be as shown in Table 1. Except for this, various operations, measurements, and evaluations were carried out in the same manner as in Example 1. The results are shown in Table 1.

[0106] Example 6 In the grafting step, the amount of methacrylic acid added was changed so that the amount of surface acid of the particulate polymer was as shown in Table 1. Except for this, various operations, measurements, and evaluations were carried out in the same manner as in Example 1. The results are shown in Table 1.

[0107] Example 7 In the block copolymer solution preparation step, the "operation (3)" of adding a predetermined amount of coupling agent to the solution containing the aromatic vinyl-aliphatic conjugated diene block copolymer having an active terminal was not performed. Except for this, various operations, measurements, and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0108] Comparative Example 1 In the block copolymer solution preparation step, the "operation (3)" of adding a predetermined amount of coupling agent to a solution containing an aromatic vinyl-aliphatic conjugated diene block copolymer having an active terminal was not performed. In addition, the amounts of styrene, isoprene, n-butyllithium, TMEDA, methanol, and the like added in other operations were appropriately changed as necessary so that block copolymer B contained in the block copolymer solution satisfied the composition shown in Table 1. Except for this, various operations, measurements, and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0109] [Table 1]

[0110] From Table 1, it can be seen that the negative electrodes of Examples 1 to 7 formed using a binder composition containing a particulate polymer containing at least an asymmetric block copolymer A satisfying a predetermined configuration have sufficiently high flexibility and can improve the cycle characteristics of the obtained secondary battery. Also, from Table 1, it can be seen that in Comparative Example 1 using a binder composition containing a particulate polymer that does not contain an asymmetric block copolymer, and Comparative Example 2 using a binder composition containing a particulate polymer containing a block copolymer having an asymmetric structure but containing an aromatic vinyl block region whose molecular weight is outside the predetermined range instead of the predetermined block copolymer, the flexibility of the obtained negative electrode and the cycle characteristics of the secondary battery were significantly inferior to Examples 1 to 7. [Industrial Applicability]

[0111] According to the present invention, it is possible to provide a binder composition for a non-aqueous secondary battery, which is capable of forming an electrode having sufficiently high flexibility and capable of improving the cycle characteristics of the resulting secondary battery, and a slurry composition for a non-aqueous secondary battery electrode. Furthermore, according to the present invention, it is possible to provide an electrode for a non-aqueous secondary battery having sufficiently high flexibility, and a non-aqueous secondary battery having the electrode and excellent cycle characteristics.

Claims

1. A binder composition for a non-aqueous secondary battery, comprising a particulate polymer containing a block copolymer A represented by the following general formula (A): Ar1 a -D a -Ar2 a ・・・(A) [wherein, in the general formula (A), Ar1 a represents a block region consisting of only aromatic vinyl monomer units having a weight average molecular weight of 5,500 to 20,000, and Ar2 a indicates a block region consisting of only aromatic vinyl monomer units having a weight average molecular weight of 40,000 to 400,000, D a indicates a block region composed of an aliphatic conjugated diene monomer unit.

2. The particulate polymer further contains a block copolymer B represented by the following general formula (B):

2. The binder composition for a nonaqueous secondary battery according to claim 1, wherein a ratio of the block copolymer A is 36% by mass or more and 85% by mass or less, relative to a total mass of the block copolymer A and the block copolymer B being 100% by mass. Ar1 b -D b -Ar2 b ・・・(B) [wherein, in the general formula (B), Ar1 b and Ar2 b each independently represents a block region composed of an aromatic vinyl monomer unit having a weight average molecular weight of 6,000 to 20,000; D b indicates a block region composed of an aliphatic conjugated diene monomer unit.

3. 3. The binder composition for a nonaqueous secondary battery according to claim 1, wherein the particulate polymer has a surface acid amount of 0.05 mmol / g or more and 0.90 mmol / g or less.

4. A slurry composition for a non-aqueous secondary battery electrode, comprising an electrode active material and the binder composition for a non-aqueous secondary battery electrode according to any one of claims 1 to 3.

5. A non-aqueous secondary battery electrode comprising an electrode mixture layer formed using the slurry composition for a non-aqueous secondary battery electrode according to claim 4.

6. The battery has a positive electrode, a negative electrode, a separator, and an electrolyte solution, A non-aqueous secondary battery, wherein at least one of the positive electrode and the negative electrode is the electrode for a non-aqueous secondary battery according to claim 5 .

Citation Information

Patent Citations

  • Asymmetrical butadiene-styrene block copolymer, manufacture and use

    JP1988286413A

  • Method for producing polymer composition

    JP2012077158A

  • Elastic single layer film and manufacturing method of laminate for disposable hygiene products

    JP2016166283A

  • Block copolymer composition, film, and process for producing block copolymer composition

    WO2010074270A1

  • All-solid-state secondary battery

    WO2013065738A2