Nanotwin Cu-Ni alloy layer and method for producing same

The nano-twinned Cu-Ni alloy layer addresses the limitations of traditional copper film enhancements by maintaining conductivity and stability through a co-electrolytic plating process, achieving enhanced hardness and thermal stability for electronic applications.

JP7556592B2Active Publication Date: 2024-09-26NAT YANG MING CHIAO TUNG UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023000541
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-01-10
Filing Date
2023-01-05
Publication Date
2024-09-26
Estimated Expiration
2043-01-05

AI Technical Summary

Technical Problem

Traditional methods of enhancing copper films, such as rolling or doping with metals like Ti, Ni, or Zn, lead to increased resistance and decreased thermal conductivity, while twinned copper films with grain refinement suffer from poor thermal stability.

Method used

A nano-twinned Cu-Ni alloy layer is developed, comprising over 50% volume of twinned grains in a columnar shape with 0.05-20% Ni content, formed through a co-electrolytic plating process, maintaining high conductivity and low resistance.

Benefits of technology

The nano-twinned Cu-Ni alloy layer achieves improved hardness, thermal stability, and electrical conductivity, suitable for various electronic components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007556592000006
    Figure 0007556592000006
  • Figure 0007556592000012
    Figure 0007556592000012
  • Figure 0007556592000003
    Figure 0007556592000003
Patent Text Reader

Abstract

To provide a nano-twinned Cu-Ni alloy layer, having excellent hardness while retaining conductive properties (high conductivity and low resistance) of the twinned copper.SOLUTION: A nano-twinned Cu-Ni alloy layer is provided, wherein more than 50% in volume of the nano-twinned Cu-Ni alloy layer comprises plural twinned grains, the plural twinned grains comprise plural columnar twinned grains, and a Ni content in the nano-twinned Cu-Ni alloy layer is in a range from 0.05 at% to 20 at%. In addition, a method for manufacturing the nano-twinned Cu-Ni alloy layer is also provided.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of Taiwan Patent Application No. 111100892, filed on January 10, 2022, the subject matter of which is incorporated herein by reference.

[0002] The present disclosure relates to a nano-twinned Cu—Ni alloy layer and a method for manufacturing the same, more particularly, the present disclosure relates to a high hardness nano-twinned Cu—Ni alloy layer and a method for manufacturing the same. [Background technology]

[0003] Conventionally, the mechanical properties of copper can be enhanced by rolling or doping with other metals such as Ti, Ni or Zn, but the conventional methods still have their disadvantages.

[0004] When the copper film containing copper grains is strengthened by rolling, the pure copper grains may be deformed. Even if the mechanical properties of the copper film can be strengthened by rolling, its resistance may be increased and its thermal conductivity may be decreased. Furthermore, the copper film doped with other metals may increase the resistance of the copper film. Furthermore, the strength of the twinned copper film is high. When the strength of the twinned copper film is strengthened by grain refinement, the obtained twinned copper film may have the problem of poor thermal stability.

[0005] Therefore, it is desirable to provide a novel twinned copper film, the strength of which can be increased and the properties of which can be maintained, so that the twinned copper layer can be applied to various electronic components. Summary of the Invention

[0006] The objective of the present disclosure is to provide a nano-twinned Cu-Ni alloy layer with excellent hardness while retaining the conductive properties of twinned copper (high conductivity and low resistance).

[0007] In the nanotwinned Cu-Ni alloy layer of the present disclosure, more than 50% of the volume of the nanotwinned Cu-Ni alloy layer is composed of plural twinned grains, the plural twinned grains include plural columnar twinned grains, and the Ni content in the nanotwinned Cu-Ni alloy layer is in the range of 0.05 at% to 20 at%. Here, the volume percentage of the twinned grains can be observed or measured in any part of the nanotwinned Cu-Ni alloy layer. Furthermore, the element content can be obtained, for example, by chemical analysis or by field emission electron probe microanalyzer (EPMA).

[0008] Additionally, the present disclosure further provides a substrate comprising the aforementioned nanotwinned Cu—Ni alloy layer, comprising a substrate and the aforementioned nanotwinned Cu—Ni alloy layer disposed or embedded in the substrate.

[0009] Furthermore, the present disclosure further provides a method for manufacturing the aforementioned nanotwin Cu—Ni alloy layer, which includes the following steps: providing an electrodeposition apparatus including an anode, a cathode, a plating solution and a power source, the power source being connected to the cathode and the anode respectively, and the cathode and the anode being immersed in the plating solution; and performing an electrodeposition process by the electrodeposition apparatus to grow the aforementioned nanotwin Cu—Ni alloy layer on the surface of the cathode, the plating solution may include a Cu salt, an acid and a Ni salt.

[0010] In the method of the present disclosure, the nanotwin Cu-Ni alloy layer can be formed through a simple co-electrolytic plating process by adding an appropriate amount of Ni salt to the plating solution. Compared with the Ni-free nanotwin Cu layer, the nanotwin Cu-Ni alloy layer prepared by the present disclosure not only retains the twin structure of the Ni-free nanotwin Cu layer, but also has significantly improved hardness. Therefore, the nanotwin Cu-Ni alloy layer provided by the present disclosure not only retains the high electrical conductivity and high thermal conductivity of the Ni-free nanotwin Cu layer, but also has high strength. Therefore, the nanotwin Cu-Ni alloy layer of the present disclosure can be applied to various electronic devices.

[0011] In the present disclosure, more than 50% of the volume of the nanotwin Cu-Ni alloy layer may be composed of multiple twin grains. In one embodiment of the present disclosure, for example, 50%-99%, 50%-95%, 50%-90%, 55%-90%, 60%-90%, or 65%-95% of the volume of the nanotwin Cu-Ni alloy layer may be composed of multiple twin grains, but the present disclosure is not limited thereto.

[0012] In the present disclosure, the plating solution contains not only Cu salt but also Ni salt. Therefore, a nanotwin Cu-Ni alloy layer can be formed by the co-electroplating process. By adjusting the concentration of Ni salt in the plating solution, a nanotwin Cu-Ni alloy layer with a specific Ni content can be formed by the co-electroplating process.

[0013] In the present disclosure, the Ni content in the nanotwin Cu-Ni alloy layer may be in the range of 0.05 at% to 20 at%, with the remainder being Cu. However, the present disclosure does not exclude the possibility that other trace impurity metal elements may be included. When the nanotwin Cu-Ni alloy layer contains a certain amount of Ni element, the resulting nanotwin Cu-Ni alloy layer has improved hardness. In one embodiment of the present disclosure, the Ni content may be in the range of, for example, 0.1 at% to 20 at%, 0.1 at% to 15 at%, 0.1 at% to 10 at%, 0.1 at% to 5 at%, 0.1 at% to 3 at%, or 0.1 at% to 1 at%, but the present disclosure is not limited thereto.

[0014] In the present disclosure, multiple twin grains in a nanotwinned Cu—Ni alloy layer may be formed by stacking multiple nanotwins along directions within ±15 degrees of the

[0111] crystal axis.

[0015] In one embodiment of the present disclosure, the twin grains may include a plurality of columnar twin grains, and the columnar twin grains are formed by stacking a plurality of nanotwins along a direction within ±15 degrees of the

[0111] crystal axis, and the included angle between the stacking direction of at least a part of the nanotwins and the thickness direction of the nanotwinned Cu-Ni alloy layer is in the range of 0 degrees to 20 degrees. When the columnar twin grains grow toward the surface of the nanotwinned Cu-Ni alloy layer, 50% or more of the surface area of ​​the nanotwinned Cu-Ni alloy layer may expose the (111) surface of the nanotwin. Therefore, the surface of the nanotwinned Cu-Ni alloy layer of the present disclosure may have a (111) preferred direction. In one embodiment of the present disclosure, the (111) surface of the nanotwin exposed on the surface of the nanotwin Cu-Ni alloy layer may be, for example, 50% to 99%, 55% to 99%, 60% to 99%, 65% to 99%, 70% to 99%, 75% to 99%, 75% to 95%, or 75% to 90% of the total surface area of ​​the nanotwin Cu-Ni alloy layer, but the present disclosure is not limited thereto. In one embodiment of the present disclosure, the (111) surface of the nanotwin exposed on the surface of the nanotwin Cu-Ni alloy layer may be about 95% to 99% of the total surface area of ​​the nanotwin Cu-Ni alloy layer, but the present disclosure is not limited thereto. Here, the preferred orientation of the surface of the nanotwin Cu-Ni alloy layer can be measured by electron backscatter diffraction (EBSD).

[0016] In one embodiment of the present disclosure, when a twin grain in a nanotwinned Cu—Ni alloy layer has a significant ratio of thickness to diameter, for example, the thickness is significantly greater than the diameter, the twin grain becomes a columnar twin grain.

[0017] In another embodiment of the present disclosure, the nanotwin Cu-Ni alloy layer may not only include the aforementioned columnar twin grain formed by stacking a plurality of nanotwins along a direction within ±15 degrees of the

[0111] crystal axis, but may also further include a plurality of fine grains stacked on the columnar twin grains, and the nanotwins of the fine grains are stacked without a preferred orientation. Here, the stacking direction (i.e., twin orientation) of the nanotwins of the fine grains is not particularly limited, and the nanotwins exposed on the surface of the nanotwin Cu-Ni alloy layer may not have a preferred orientation. In other words, the surface of the nanotwin Cu-Ni alloy layer has no preferred orientation. Here, the fine grains may not have a significant ratio of thickness to diameter, and the diameter and thickness of the fine grains are also smaller. For example, the thickness or diameter of the fine grains may be in the range of 100 nm to 500 nm.

[0018] In yet another embodiment of the present disclosure, the nanotwinned Cu-Ni alloy layer may not only include the aforementioned columnar twin grains formed by stacking a plurality of nanotwins along a direction within ±15 degrees of the

[0111] crystal axis, but may also further include a plurality of oblique twinned grains stacked on the plurality of columnar twin grains. Here, the oblique twinned grains may be formed by stacking a plurality of nanotwins along a direction within ±15 degrees of the

[0111] crystal axis, and the included angle between the stacking direction of at least a part of the nanotwins of the oblique twinned grains and the thickness direction of the nanotwinned Cu-Ni alloy layer may be in the range of 10 degrees to 60 degrees. Since the oblique twin grains become twin grains that intersect with the thickness direction of the nanotwinned Cu-Ni alloy layer at the aforementioned angle, the nanotwins exposed on the surface of the nanotwinned Cu-Ni alloy layer may not have a preferred orientation. In other words, the surface of the nanotwinned Cu-Ni alloy layer does not have a preferred orientation.

[0019] In the present disclosure, whether it is the aforementioned columnar twin grains, fine grains or orthorhombic twin grains, at least a portion of the twin grains may be interconnected, for example, more than 50%, 60%, 70%, 80%, 90% or 95% of the twin grains may be interconnected.

[0020] In the present disclosure, the thickness of the nanotwin Cu-Ni alloy layer can be adjusted as necessary. In one embodiment of the present disclosure, the thickness of the nanotwin Cu-Ni alloy layer can be in the range of, for example, 0.1 μm to 500 μm, 0.1 μm to 400 μm, 0.1 μm to 300 μm, 0.1 μm to 200 μm, 0.1 μm to 100 μm, 0.1 μm to 80 μm, 0.1 μm to 50 μm, 1 μm to 50 μm, 2 μm to 50 μm, 3 μm to 50 μm, 4 μm to 50 μm, 5 μm to 50 μm, 5 μm to 40 μm, 5 μm to 35 μm, 5 μm to 30 μm, or 5 μm to 25 μm, but the present disclosure is not limited thereto.

[0021] In the present disclosure, the diameter of the columnar twin grain or the oblique twin grain may be in the range of 0.1 μm to 50 μm, respectively. In one embodiment of the present disclosure, the diameter of the columnar twin grain or the oblique twin grain may be in the range of, for example, 0.1 μm to 45 μm, 0.1 μm to 40 μm, 0.1 μm to 35 μm, 0.5 μm to 35 μm, 0.5 μm to 30 μm, 1 μm to 30 μm, 1 μm to 25 μm, 1 μm to 20 μm, 1 μm to 15 μm, or 1 μm to 10 μm, respectively, but the present disclosure is not limited thereto. In the present disclosure, the diameter of the columnar twin grain or the oblique twin grain may be the length of the twin grain measured in a direction approximately perpendicular to the twin orientation of the twin grain. More specifically, the diameter of a columnar twin grain or an oblique twin grain can be the length (e.g., maximum length) of the twin grain measured in a direction approximately perpendicular to the stacking direction of the twins or twin grain boundary (i.e., the extension direction of the twin grain boundary).

[0022] In the present disclosure, the thickness of the columnar twin grains or the oblique twin grains may be in the range of 0.1 μm to 500 μm, respectively. In one embodiment of the present disclosure, the thickness of the columnar twin grains or the oblique twin grains may be in the range of, for example, 0.1 μm to 500 μm, 0.1 μm to 400 μm, 0.1 μm to 300 μm, 0.1 μm to 200 μm, 0.1 μm to 100 μm, 0.1 μm to 80 μm, 0.1 μm to 50 μm, 1 μm to 50 μm, 2 μm to 50 μm, 3 μm to 50 μm, 4 μm to 50 μm, 5 μm to 50 μm, 5 μm to 40 μm, 5 μm to 35 μm, 5 μm to 30 μm, or 5 μm to 25 μm, respectively. In the present disclosure, the thickness of a columnar twin grain or an oblique twin grain can be the thickness of the twin grain measured in the twin orientation of the twin grain. More specifically, the thickness of a columnar twin grain or an oblique twin grain can be the thickness of the twin grain measured in the stacking direction of the twin or twin grain boundary (e.g., maximum thickness).

[0023] In the present disclosure, the "twin orientation of a twin grain" refers to the stacking direction of a twin or a twin boundary in a twin grain, where the twin boundary of the twin grain can be approximately perpendicular to the stacking direction of the twin or the twin boundary.

[0024] In the present disclosure, the included angle between the twin orientation of the twin grain and the thickness direction of the nanotwin Cu-Ni alloy layer can be measured in the cross section of the nanotwin Cu-Ni alloy layer. Similarly, the thickness of the nanotwin Cu-Ni alloy layer and the characteristics such as the diameter or thickness of the twin grain can also be measured in the cross section of the twin copper layer. Alternatively, the diameter or thickness of the twin grain can also be measured by the surface of the twin copper layer. In the present disclosure, the measurement method is not particularly limited, and can be performed by a scanning electron microscope (SEM), a transmission electron microscope (TEM), a focused ion beam (FIB), or other suitable measurement forms.

[0025] In the present disclosure, the nanotwin Cu-Ni alloy layer of the present disclosure can be formed by a co-electrolytic plating process. Here, the cathode can be used as a substrate, and the formed nanotwin Cu-Ni alloy layer can be disposed or embedded in the substrate. The cathode can be a substrate having a metal layer formed thereon or a metal substrate. The substrate can be a silicon substrate, a glass substrate, a quartz substrate, a metal substrate, a plastic substrate, a printed circuit board, a III-IV substrate, or a laminated substrate thereof. Furthermore, the substrate can have a single layer or a multi-layer structure.

[0026] In the present disclosure, the plating solution may include a Cu salt, an acid, and a Ni salt. Examples of Cu salts included in the plating solution may include, but are not limited to, copper sulfate, copper methylsulfonate, or combinations thereof. Examples of acids included in the plating solution may include, but are not limited to, hydrochloric acid, sulfuric acid, methanesulfonic acid, or combinations thereof. Examples of Ni salts included in the plating solution may include, but are not limited to, nickel sulfate, nickel methylsulfonate, or combinations thereof. Furthermore, the plating solution may further include additives such as gelatin, surfactants, lattice modifiers, or combinations thereof.

[0027] In the present disclosure, the electrodeposition process may be interchangeably performed by direct current electrodeposition, pulse electrodeposition, or direct current electrodeposition and pulse electrodeposition to form the nanotwinned Cu—Ni alloy layer.

[0028] In one embodiment of the present disclosure, the nanotwinned Cu-Ni alloy layer is formed by direct current electrodeposition. The current density used in direct current electrodeposition can be in the range of, for example, 0.5ASD to 30ASD, 1ASD to 30ASD, 2ASD to 30ASD, 2ASD to 25ASD, 2ASD to 20ASD, 2ASD to 15ASD, or 2ASD to 10ASD, but the present disclosure is not limited thereto.

[0029] In another embodiment of the present disclosure, the nanotwin Cu-Ni alloy layer is formed by pulse electrodeposition. The forward current density of the pulse electrodeposition may be, for example, in the range of 0.5ASD to 30ASD, 1ASD to 30ASD, 2ASD to 30ASD, 2ASD to 25ASD, 2ASD to 20ASD, 2ASD to 15ASD, or 2ASD to 10ASD, and the reverse current density of the pulse electrodeposition may be, for example, in the range of 0.1ASD to 10ASD, 0.1ASD to 8ASD, 0.1ASD to 5ASD, 0.1ASD to 3ASD, 0.3ASD to 3ASD, or 0.3ASD to 1ASD, but the present disclosure is not limited thereto. When the nanotwin Cu-Ni alloy layer is formed by pulse electrodeposition, in one embodiment of the present disclosure, the twin grains of the nanotwin Cu-Ni alloy layer may further include columnar twin grains. In another embodiment of the present disclosure, when the thickness of the formed nanotwinned Cu—Ni alloy layer is increased, the twin grains of the nanotwinned Cu—Ni alloy layer may not only include columnar twin grains, but also selectively include fine grains stacked in a plurality of columnar twin grains, oblique twin grains, or a combination thereof.

[0030] In one embodiment of the present disclosure, after forming the nanotwin Cu-Ni alloy layer on the surface of the cathode, the nanotwin Cu-Ni alloy layer may be optionally annealed. Thus, the hardness of the nanotwin Cu-Ni alloy layer may be further improved. Here, the annealing temperature may be in the range of 50°C to 250°C. If the annealing temperature exceeds this range, the twin structure in the nanotwin Cu-Ni alloy layer may be lost or disappear. In one embodiment of the present disclosure, the annealing temperature may be in the range of 50°C to 250°C, 75°C to 250°C, 75°C to 200°C, 100°C to 200°C, 100°C to 175°C, or 100°C to 150°C, but the present disclosure is not limited thereto. Furthermore, in the present disclosure, the annealing time is not particularly limited, and may be, for example, in the range of 30 minutes to 10 hours, 30 minutes to 8 hours, 30 minutes to 5 hours, or 1 hour to 5 hours, but the present disclosure is not limited thereto.

[0031] The shape of the nanotwin Cu-Ni alloy layer provided by the present disclosure is not particularly limited, and can be a foil, a film, a wire, or a bulk, but the present disclosure is not limited thereto. Furthermore, the nanotwin Cu-Ni alloy layer provided by the present disclosure can have a single-layer or multi-layer structure. Furthermore, the nanotwin Cu-Ni alloy layer provided by the present disclosure can be combined with other materials to form a multi-layer composite structure.

[0032] The nanotwinned Cu-Ni alloy layer provided by the present disclosure can be applied in various electronic products, such as through-holes or vias in three-dimensional integrated circuits (3D-ICs), pin-through-holes in packaging substrates, metal interconnects, substrate circuits, or connectors, but the present disclosure is not limited thereto.

[0033] Other novel features of the present disclosure will become more apparent from the following detailed description when taken in conjunction with the accompanying drawings. [Brief description of the drawings]

[0034] [Figure 1] FIG. 1 is an EBSD photograph of a nanotwinned Cu specimen according to Comparative Example 1 of the present disclosure. [Diagram 2] FIG. 2 is an EBSD photograph of a nanotwinned Cu—Ni alloy specimen according to Example 1 of the present disclosure. [Diagram 3] FIG. 3 is an FIB photograph of a nanotwinned Cu—Ni alloy specimen according to Example 1 of the present disclosure. [Figure 4] FIG. 4 is a comparison diagram of the hardness of test pieces according to Example 1 and Comparative Example 1 of the present disclosure before and after annealing at various temperatures for 1 hour. [Diagram 5] FIG. 5 is a comparative diagram of the hardness of test pieces according to Example 1 of the present disclosure and Comparative Example 1 after annealing at 100° C. for 1 hour and 5 hours. [Figure 6] FIG. 6 is a comparative diagram of the hardness of test pieces according to Example 1 of the present disclosure and Comparative Example 1 after annealing at 200° C. for 1 hour and 5 hours. [Figure 7] FIG. 7 is an EBSD photograph of a nanotwinned Cu specimen according to Comparative Example 2 of the present disclosure. [Figure 8] FIG. 8 is an EBSD photograph of a nanotwinned Cu—Ni alloy specimen according to Example 2 of the present disclosure. [Figure 9] FIG. 9 is an FIB photograph of a nanotwinned Cu—Ni alloy specimen according to Example 2 of the present disclosure. [Figure 10] FIG. 10 is a comparison diagram of the hardness of test pieces according to Example 2 and Comparative Example 2 of the present disclosure before and after annealing at various temperatures for 1 hour. [Figure 11] FIG. 11 is a comparative diagram of the hardness of test pieces according to Example 2 of the present disclosure and Comparative Example 2 after annealing at 100° C. for 1 hour and 5 hours. [Figure 12] FIG. 12 is a comparative diagram of the hardness of test pieces according to Example 2 of the present disclosure and Comparative Example 2 after annealing at 200° C. for 1 hour and 5 hours. [Figure 13] FIG. 13 is a phase diagram of a Cu—Ni alloy. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0035] Various embodiments of the present disclosure are provided in the following description. These embodiments are intended to describe the technical content of the present disclosure, and do not limit the scope of the present disclosure. The features described in the embodiments can be applied to other embodiments by appropriate modification, substitution, combination, or separation.

[0036] It should be noted that in this specification, when a part / component is described as having an element / element, this means that the part / component may have one or more of the element / element, and does not mean that the part / component has only one of the element / element, unless otherwise specified.

[0037] In this specification, unless otherwise specified, feature A "or" or "and / or" feature B means the presence of feature A, the presence of feature B, or the presence of both features A and B. Feature A "and" feature B means the presence of both features A and B. The terms "comprise", "comprising", "including", "including", "have", "has" and "having" mean "comprising / comprising, but not limited to".

[0038] Furthermore, when an element / element is described herein as being disposed "on" another element / element, unless otherwise specified, it does not inherently mean that the element / element is in contact with the other element / element. Such an interpretation also applies to other cases similar to the case of "on."

[0039] Furthermore, in this specification, a value may be interpreted as encompassing a range within ±10% of that value, particularly a range within ±5% of that value, unless otherwise specified, and a range may be interpreted as consisting of multiple subranges defined by a lower endpoint, lower quartile, median, upper quartile and upper endpoint, unless otherwise specified.

[0040] Example 1 - Nanotwinned Cu-Ni alloy specimen In this example, a 12-inch silicon wafer coated with 100 nm Ti / 200 nm Cu was divided into 2 cm x 3 cm test pieces as the cathode. The test pieces were washed with citric acid to remove oxides, and the electrodeposition area was defined with acid-alkali resistant tape. The area of ​​the total electrodeposition area was 2 cm x 2 cm.

[0041] The plating solution used in this example was formulated with CuSO4·5H2O. The amount of CuSO4·5H2O powder added was 196.54 g (50 g / L Cu ion). Then, 4.5 ml of additives were added to the plating solution, 100 g of H2SO4 (96%) was added, and 0.1 ml of HCl (12N) was added. The plating solution was stirred with a stirrer until the CuSO4·5H2O was well mixed in the plating solution (1 L). The resulting plating solution was divided into two tanks, one of which was added with 10 ml of NiSO4 (0.1 M) as the plating solution of this example, and the other without NiSO4 was used as the plating solution of the comparative example. The stirrer at the bottom of the electroplating tank was rotated at 1200 rpm per minute to maintain a uniform ion concentration. Electrodeposition was carried out at room temperature and 1 atm. HCl added to the plating solution can usually dissolve the copper target (as the anode) in the electroplating bath to balance the copper ion concentration in the plating solution. Here, the power supply (Keithley 2400) was controlled by a computer, and the electrodeposition was performed by direct current electrodeposition. After the electrodeposition was performed at a current density of 6 ASD (A / dm2) for 20 minutes, a nanotwinned Cu-Ni alloy layer with a thickness of 20 μm was obtained. In another embodiment of the present disclosure, a nanotwinned Cu-Ni alloy layer with a desired thickness can be obtained by controlling the current density during electrodeposition.

[0042] Then, the obtained specimen was polished by electrolytic polishing, and the solution for electrolytic polishing included 100ml H3PO4, 1ml acetic acid and 1ml glycerol. The specimen to be polished was placed on the anode, and electrolytic polishing was performed at 1.75V for 10 minutes. The specimen after electrolytic polishing has a thickness of about 19μm. The electrolytic polishing process can not only flatten the surface of the nanotwinned Cu-Ni alloy specimen, but also make the subsequent hardness test results more accurate.

[0043] Comparative Example 1 - Nanotwinned Cu specimen The method for preparing the nanotwinned Cu specimens of this comparative example is similar to that for preparing the nanotwinned Cu-Ni alloy specimens of Example 1, except that a plating solution without NiSO4 as described in Example 1 was used for electrodeposition in this comparative example.

[0044] The surface preferred orientation and microstructure of the electropolished specimens of Example 1 and Comparative Example 1 were analyzed by electron backscatter diffraction (EBSD) and focused ion beam (FIB).

[0045] 1 and 2 are EBSD photographs of a nanotwinned Cu specimen according to Comparative Example 1 and a nanotwinned Cu—Ni alloy specimen according to Example 1 of the present disclosure, respectively. Fig. 3 is an FIB photograph of the nanotwinned Cu—Ni alloy specimen according to Example 1 of the present disclosure.

[0046] As shown in Figures 1 and 2, the results obtained by EBSD measurements show that almost the entire volume (more than 95% of the volume) of the nanotwinned Cu specimen of Comparative Example 1 and the nanotwinned Cu-Ni alloy specimen of Example 1 is composed of interconnected columnar twin grains, and the diameter of the columnar twin grains is in the range of about 0.5 μm to about 3 μm. Furthermore, the twin grains are formed by stacking nanotwins along the

[0111] crystal axis, and the grain boundaries of the nanotwins are approximately parallel to the surface of the cathode (i.e., the stacking direction of the nanotwins is approximately parallel to the thickness direction of the specimen). Therefore, almost the entire surface of the specimen (more than 95% of the area) exposes the (111) surface of the nanotwins, which indicates that the nanotwinned Cu specimen of Comparative Example 1 and the nanotwinned Cu-Ni alloy specimen of Example 1 have a (111) preferred orientation.

[0047] As shown in FIG. 3, the results obtained by FIB measurement show that most of the particles in the nanotwinned Cu-Ni alloy specimen of Example 1 have high density twin grains. More than 95% of the volume of the nanotwinned Cu-Ni alloy specimen consists of twin grains. The included angle between the twin orientation of more than 95% of the twin grains and the thickness direction of the nanotwinned Cu-Ni alloy specimen is about 0 degrees, and the included angle between the twin orientation of more than 95% of the twin grains and the surface of the substrate is about 90 degrees, which means that the twin grain boundaries of the twin grains are approximately parallel to the surface of the substrate. Furthermore, more than 95% of the twin grains in the nanotwinned Cu-Ni alloy specimen have a thickness in the range of about 1 μm to about 20 μm.

[0048] Hardness Testing The test pieces of Example 1 and Comparative Example 1 obtained after electrolytic polishing were washed with a citric acid solution, and water droplets on the surfaces of the test pieces were removed with a nitrogen spray gun. Then, the nanotwin Cu test piece of Comparative Example 1 and the nanotwin Cu-Ni alloy test piece of Example 1 were annealed in a furnace tube. The pressure of the vacuum environment was 10 -3 Torr, the annealing temperatures were 100°C, 150°C and 200°C, and the annealing times were 1 hour and 5 hours, respectively. The test pieces of Example 1 and Comparative Example 1 before and after annealing were tested by a Vickers hardness tester. The Vickers hardness tester drilled a diamond-shaped hole in the test piece, and the hardness of the test piece before and after annealing was obtained after computer calculation.

[0049] 4 is a comparison diagram of the hardness of the test pieces according to Example 1 of the present disclosure and Comparative Example 1 before and after annealing at various temperatures for 1 hour. Table 1 below shows the comparison results of the overall reinforcement of the test pieces according to Example 1 of the present disclosure and Comparative Example 1, and the comparison subject of the overall reinforcement is the hardness of the test piece according to Comparative Example 1 before annealing, as shown by the rectangle in FIG. 4. [Table 1]

[0050] As shown in FIG. 4 and Table 1, before annealing, the hardness of the nanotwinned Cu-Ni alloy specimen of Example 1 is greater than that of the nanotwinned Cu specimen of Comparative Example 1, which indicates that the hardness of the nanotwinned Cu specimen can be increased by adding an appropriate amount of nickel. Furthermore, the nanotwinned Cu-Ni alloy specimen of Example 1 after annealing at 100°C for 1 hour has a hardness of 191HV. Compared with the nanotwinned Cu specimen of Comparative Example 1 before annealing, the hardness of the nanotwinned Cu-Ni alloy specimen of Example 1 can be increased by 30.28%. This result indicates that the hardness of the nanotwinned Cu-Ni alloy specimen of Example 1 can be further improved by annealing at low temperature.

[0051] 5 and 6 are comparative diagrams of the hardness of the specimens according to Example 1 and Comparative Example 1 of the present disclosure after annealing at 100° C. and 200° C. for 1 hour and 5 hours, respectively. The results show that the hardness of the nanotwinned Cu—Ni alloy specimen of Example 1 does not decrease significantly even after long-term annealing, indicating that the nanotwinned Cu—Ni alloy specimen of Example 1 has good thermal stability.

[0052] Example 2 - Nanotwinned Cu-Ni alloy specimen The method for preparing the nanotwinned Cu-Ni alloy specimen in this example is similar to that for preparing the nanotwinned Cu-Ni alloy specimen in Example 1, except that the electrodeposition process used in this example is pulse electrodeposition. The forward current density is 8 ASD, the reverse current density is 0.7 ASD, the plating time is about 24 minutes, and the thickness of the obtained specimen is about 23 μm. After the specimen is polished by electrolytic polishing as described in Example 1, the specimen after electrolytic polishing has a thickness of about 22 μm.

[0053] Comparative Example 2 - Nanotwinned Cu specimen The method for preparing the nanotwinned Cu specimens in this comparative example is similar to that for preparing the nanotwinned Cu-Ni alloy specimens in Example 2, except that a plating solution not containing NiSO4 was used in the electrodeposition in this comparative example.

[0054] The surface preferred orientation and microstructure of the electropolished specimens of Example 2 and Comparative Example 2 were analyzed by EBSD and FIB.

[0055] 7 and 8 are EBSD photographs of the nanotwinned Cu specimen according to Comparative Example 2 and the nanotwinned Cu—Ni alloy specimen according to Example 2 of the present disclosure, respectively. Fig. 9 is an FIB photograph of the nanotwinned Cu—Ni alloy specimen according to Example 2 of the present disclosure.

[0056] As shown in FIG. 9, within a range of about 5 μm from the surface of the substrate, the twin grains of the nanotwinned Cu-Ni alloy specimen of Example 2 include columnar twin grains. Outside a range of about 5 μm from the surface of the substrate, the twin grains of the nanotwinned Cu-Ni alloy specimen of Example 2 further include oblique twin grains and fine grains stacked in a plurality of columnar twin grains. The included angle between the stacking direction of the nanotwin of the oblique twin grains and the thickness direction of the specimen is in the range of 10 degrees to 60 degrees. The stacking direction of the nanotwin of the fine grains does not have a preferred orientation. This result demonstrates the reason why the specimen shown in the EBSD photographs of FIG. 7 and FIG. 8 does not have a preferred orientation.

[0057] The hardness of the test pieces of Example 2 and Comparative Example 2 obtained after electrolytic polishing was tested by the same method as above. Figure 10 is a comparison diagram of the hardness of the test pieces of Example 2 and Comparative Example 2 of the present disclosure before and after annealing at various temperatures for 1 hour. Table 2 below shows the comparison results of the overall strengthening degree of the test pieces of Example 2 and Comparative Example 2 of the present disclosure, and the comparison object of the overall strengthening degree is the hardness of the test piece of Comparative Example 2 before annealing, as shown by the rectangle in Figure 10. [Table 2]

[0058] As shown in FIG. 10 and Table 2, before annealing, the hardness of the nanotwinned Cu-Ni alloy specimen of Example 2 is greater than that of the nanotwinned Cu specimen of Comparative Example 2, which indicates that the hardness of the nanotwinned Cu specimen can be increased by adding an appropriate amount of nickel. Furthermore, the nanotwinned Cu-Ni alloy specimen of Example 2 after annealing at 100°C for 1 hour has a hardness of 234.2HV. Compared with the nanotwinned Cu specimen of Comparative Example 2 before annealing, the hardness of the nanotwinned Cu-Ni alloy specimen of Example 2 can be increased by 39.57%. This result indicates that the hardness of the nanotwinned Cu-Ni alloy specimen of Example 2 can be further improved by annealing at low temperature.

[0059] 11 and 12 are comparative diagrams of the hardness of the specimens according to Example 2 of the present disclosure and Comparative Example 2 after annealing at 100° C. and 200° C. for 1 hour and 5 hours, respectively. The results show that the hardness of the nanotwinned Cu—Ni alloy specimen of Example 2 does not decrease significantly even after long-term annealing, indicating that the nanotwinned Cu—Ni alloy specimen of Example 2 has good thermal stability.

[0060] Resistivity Test The resistivity of the test pieces of Example 2 and Comparative Example 2 obtained after electrolytic polishing was tested. Here, after measuring at four points, the resistivity of the test piece was converted by the following formula (I). ρ=Rs×T=[CF×(V / I)]×T...(I) where ρ is the resistivity of the specimen (μΩ-cm), Rs is the sheet resistance (Ω), T is the thickness of the specimen (cm), CF is a correction factor, V is the DC voltage passed through the voltage probe, and I is a fixed DC current passed through the current probe.

[0061] The results show that the resistivity of the nickel-free nanotwinned Cu specimen of Comparative Example 2 is about 2.18 μΩ-cm, and the resistivity of the nanotwinned Cu-Ni alloy specimen of Example 2 is about 2.07 μΩ-cm to 3.44 μΩ-cm. This result indicates that by adding an appropriate amount of nickel, not only can the hardness of nanotwinned Cu be increased, but also the high conductivity and low resistance characteristics of nanotwinned Cu can be maintained.

[0062] As a result, nanotwinned Cu-Ni alloys with preferred orientation of lattice orientation (as shown in Example 1) and random orientation of lattice orientation (as shown in Example 2) can be easily obtained by co-electrolytic plating, optionally followed by an annealing treatment. <111> The hardness of the nanotwinned Cu-Ni alloy specimen with preferred orientation is <111> The hardness is significantly higher than that of the nanotwinned Cu layer without nickel having preferred orientation. In the present disclosure, nanotwinned Cu-Ni alloy specimens with high hardness can also be obtained by pulse electrodeposition (as shown in Example 2), and the hardness of the specimens can be increased without further hardening treatment.

[0063] Nanotwinned Cu with preferred orientation has good lattice orientation, and the strength itself is better than Cu bulk. Since nanotwinned Cu already has high strength, it is not easy to increase its strength. Therefore, in the present disclosure, the hardness of nanotwinned Cu-Ni alloy specimens can be further improved by short-time, low-temperature, and rapid annealing. In addition, nickel is a high-strength metal among metals. According to the phase diagram (as shown in FIG. 13), the Cu-Ni alloy of the present disclosure is soluble and no eutectoids are formed. In addition, the amount of nickel added to the nanotwinned Cu-Ni alloy specimens is not large, which can also reduce the possibility of electromigration effect, and the electrical properties of the parts are not affected, and the reliability of the parts can be effectively improved. In particular, in the nanotwinned Cu-Ni alloy specimens of the present disclosure, the resistivity of the specimens is not significantly improved after adding nickel, and the specimens still have high conductivity. Therefore, the nanotwinned Cu—Ni alloy specimen of the present disclosure has high strength, high electrical conductivity and high thermal conductivity, and can be applied to various electronic components.

[0064] Although the present disclosure has been described with reference to embodiments thereof, it should be understood that many other possible modifications and variations can be made without departing from the spirit and scope of the present disclosure as claimed below.

Claims

1. A nanotwinned Cu—Ni alloy layer, wherein more than 50% of the volume of the nanotwinned Cu—Ni alloy layer is composed of a plurality of twin grains, the plurality of twin grains including a plurality of columnar twin grains, and the Ni content in the nanotwinned Cu—Ni alloy layer is in the range of 0.05 at% to 20 at%.

2. 2. The nanotwin Cu—Ni alloy layer of claim 1, wherein the plurality of twin grains are formed by stacking a plurality of nanotwins along a direction within ±15 degrees of the [111] crystal axis.

3. 2. The nanotwin Cu—Ni alloy layer according to claim 1, wherein the plurality of columnar twin grains are formed by stacking a plurality of nanotwins along a direction within ±15 degrees of a [111] crystal axis, and an included angle between the stacking direction of at least a part of the plurality of nanotwins and a thickness direction of the nanotwin Cu—Ni alloy layer is in the range of 0 degrees to 20 degrees.

4. The nanotwinned Cu—Ni alloy layer according to claim 3, wherein 50% or more of the surface area of ​​the nanotwinned Cu—Ni alloy layer exposes the (111) surface of the nanotwin.

5. 2. The nanotwin Cu—Ni alloy layer of claim 1, wherein the plurality of twin grains further comprises a plurality of fine grains stacked on the plurality of columnar twin grains, and the nanotwins of the plurality of fine grains are stacked without preferred orientation.

6. The nanotwinned Cu—Ni alloy layer of claim 5, wherein a surface of the nanotwinned Cu—Ni alloy layer is not a preferential surface.

7. 2. The nanotwinned Cu—Ni alloy layer as claimed in claim 1, wherein the plurality of twin grains further comprises a plurality of oblique twin grains stacked on the plurality of columnar twin grains.

8. The nanotwin Cu—Ni alloy layer according to claim 7, wherein the plurality of oblique twin grains are formed by stacking a plurality of nanotwins along a direction within ±15 degrees of a [111] crystal axis, and an included angle between a stacking direction of at least a part of the plurality of nanotwins and a thickness direction of the nanotwin Cu—Ni alloy layer is in a range of 10 degrees to 60 degrees.

9. The nanotwinned Cu—Ni alloy layer of claim 8, wherein a surface of the nanotwinned Cu—Ni alloy layer is not a preferential surface.

10. 2. The nanotwinned Cu—Ni alloy layer according to claim 1, wherein the diameters of the plurality of columnar twin grains are each in the range of 0.1 μm to 50 μm.

11. The nanotwinned Cu—Ni alloy layer according to claim 1 , wherein the thickness of each of the plurality of columnar twin grains is in the range of 0.1 μm to 500 μm.

12. The nanotwinned Cu—Ni alloy layer of claim 1 , wherein at least a portion of the plurality of columnar twin grains are connected to each other.

13. A method for producing a nanotwinned Cu—Ni alloy layer, comprising the steps of: providing an electrodeposition apparatus comprising an anode, a cathode, a plating solution, and a power source, the power source being connected to the cathode and the anode, respectively, and the cathode and the anode being immersed in the plating solution; and growing a nano-twinned Cu—Ni alloy layer on the surface of the cathode by performing an electrodeposition process using the electrodeposition device; More than 50% of the volume of the nanotwin Cu—Ni alloy layer is composed of a plurality of twin grains, the plurality of twin grains including a plurality of columnar twin grains, and the Ni content in the nanotwin Cu—Ni alloy layer is in the range of 0.05 at% to 20 at%, The plating solution comprises a Cu salt, an acid and a Ni salt.

14. The method of claim 13, further comprising the step of annealing the nano-twinned Cu—Ni alloy layer after growing the nano-twinned Cu—Ni alloy layer on a surface of the cathode.

15. The method of claim 14, wherein the temperature for annealing the nanotwinned Cu—Ni alloy layer is in the range of 50° C. to 250° C.

16. The method of claim 13, wherein the electrodeposition process is direct current electrodeposition.

17. The method of claim 13, wherein the electrodeposition process is pulse electrodeposition.

18. 20. The method of claim 17, wherein the plurality of twin grains further comprises a plurality of fine grains stacked on the plurality of columnar twin grains, and nanotwins of the plurality of fine grains are stacked without preferred orientation.

19. 20. The method of claim 17, wherein the plurality of twin grains further comprises a plurality of oblique twin grains stacked on the plurality of columnar twin grains.

20. 20. The method of claim 19, wherein the plurality of oblique twin grains are formed by stacking a plurality of nanotwins along a direction within ±15 degrees of a [111] crystal axis, and an included angle between the stacking direction of at least a part of the plurality of nanotwins and a thickness direction of the nanotwin Cu—Ni alloy layer is in the range of 10 degrees to 60 degrees.

Citation Information

Patent Citations

  • Method and apparatus for alloy plating

    JP1985021398A

  • Copper-nickel alloy electroplating bath

    JP2016037649A

  • Nano-twin copper metal layer, method of producing the same, and substrate comprising the same