Highly processable multi-stage soft acrylic resins and methods for making same

A multi-stage flexible acrylic resin with a crosslinked core and branched outer layer addresses the limitations of existing resins by enhancing processability and mechanical properties, enabling applications like thin film extrusion and injection molding.

JP7556878B2Active Publication Date: 2024-09-26ROHM & HAAS CO
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021557593
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-28
Filing Date
2020-03-13
Publication Date
2024-09-26
Estimated Expiration
2040-03-13

AI Technical Summary

Technical Problem

Existing acrylic resins are either too expensive, too hard, or have low tear resistance, and their high viscosity makes processing difficult, especially in applications like thin film extrusion and injection molding.

Method used

A multi-stage flexible acrylic resin is developed, comprising a crosslinked core, interlayer compositions with a compositional gradient, and an outermost layer with branched polymers, reducing viscosity without causing whitening, and improving tensile properties.

Benefits of technology

The multi-stage resin achieves reduced viscosity and improved processing capabilities, allowing for applications such as very thin film extrusion and certain injection molding without undesirable whitening, while maintaining transparency and mechanical strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007556878000004
    Figure 0007556878000004
  • Figure 0007556878000003
    Figure 0007556878000003
  • Figure 0007556878000001
    Figure 0007556878000001
Patent Text Reader

Abstract

The multi-stage flexible acrylic resin comprises a branched polymer that is the reaction product of reactants including one or more monoethylenically unsaturated ester monomers, a chain transfer agent in an amount of 0.1-10 wt %, and a crosslinker in an amount of 0.1-10 wt %, where the weight percent is based on the total amount of reactants, with the proviso that the amount of crosslinker in moles is less than the amount of chain transfer agent in moles. A method for making the multi-stage flexible acrylic resin is also disclosed.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The field of this invention is multi-stage flexible acrylic resin compositions and methods for making multi-stage flexible acrylic resin compositions. Summary of the Invention [Problem to be solved by the invention]

[0002] A variety of indoor and outdoor products benefit from the use of flexible, transparent, weather-resistant plastic materials. Fluorine-containing polymers and thermoplastic polyurethanes offer these characteristics but are too expensive for many end uses. Low-cost resins such as polyvinyl chloride or polyethylene resins with plasticizers may not meet all performance requirements. Some of these polymers may have undesirable environmental impacts.

[0003] Various acrylic resins have also been proposed. However, many are too hard, have a high modulus, or have low tear resistance for certain end uses. One commercially available acrylic resin contains a block copolymer of poly(methyl methacrylate) and poly(butyl acrylate) produced by anionic polymerization. These resins are flexible and resistant to blushing, but are prohibitively expensive for certain applications. Multi-stage acrylic polymers have been taught as an alternative (see, for example, U.S. Pat. No. 10,040,915). These materials tend to be highly viscous (melt flow index or rate in the range of 15-20 g / 10 min at 220° C. and 10 kg) and difficult to process for certain applications.

[0004] Disclosed herein is a method for producing a medicament for the treatment of a cancer, comprising: a) a first stage comprising a crosslinked core having a Tg in the range of -85 to -10°C; b) a second stage comprising one or more layers comprising 88.5-100% by weight of units derived from one or more monomers selected from the group consisting of alkyl (meth)acrylate monomers, 0-5% by weight of units derived from a crosslinking monomer, a graft linking monomer, or a combination of two or more thereof, and optionally 0-2% by weight of one or more chain transfer agents, with a compositional gradient between the intermediate layers such that the Tg transitions between a lower Tg and a higher Tg, the lower Tg being at least 0° C. and the higher Tg being no greater than 70° C. across the width of the second stage; c) a third stage comprising one or more layers comprising 98.5-100 wt. % of units derived from one or more monomers selected from the group consisting of alkyl (meth)acrylates, styrenic monomers, and combinations of two or more thereof, and 0-1.5 wt. % of units derived from one or more chain transfer agents, the third stage having a Tg in the range of 40° C. to 110° C.; d) a fourth stage comprising one or more layers comprising a branched polymer that is the reaction product of reactants comprising one or more monoethylenically unsaturated ester monomers, a chain transfer agent in an amount of 0.1-10 wt %, and a crosslinker in an amount of 0.1-10 wt %, wherein the weight % is based on the total amount of reactants, with the proviso that the amount of crosslinker in molar is less than the amount of chain transfer agent in molar.

[0005] Another aspect of the present invention relates to a method for forming a multi-stage soft acrylic resin containing a branched polymer, the method comprising: 1) forming a first stage by emulsion polymerization of a first stage reaction mixture comprising 95-99.5% by weight of one or more monomers selected from the group consisting of alkyl (meth)acrylate monomers and 0.1-5% by weight of one or more monomers selected from the group consisting of crosslinking monomers, graft linking monomers, and mixtures thereof; 2) forming a second stage by emulsion polymerization of the polymerization product of the first stage with a reaction mixture comprising 93-100% by weight of monomers selected from the group consisting of alkyl (meth)acrylate monomers, 0-5% by weight of one or more monomers selected from the group consisting of crosslinking monomers, graft linking monomers, and mixtures thereof, and 0-2.0% by weight of a chain transfer agent; 3) forming a third stage by emulsion polymerization of the polymerization product of the second stage with a reaction mixture comprising 98.5-100% by weight of one or more monomers selected from the group consisting of alkyl (meth)acrylate monomers, styrenic monomers, and mixtures thereof, and 0-1.5% by weight of one or more chain transfer agents; 4) forming a fourth stage by emulsion polymerization of the polymerization product of the third stage with a reaction mixture comprising one or more monoethylenically unsaturated ester monomers, a chain transfer agent in an amount of 0.1-10% by weight, and a crosslinking agent in an amount of 0.1-10% by weight, wherein the amount of crosslinking agent in molar is less than the amount of chain transfer agent in molar. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0006] As used herein, the terms "a," "an," "the," "at least one," "one or more," and variations thereof are used interchangeably. The terms "comprise," "include," "contain," and variations thereof do not have a limiting meaning when these terms appear in the specification and claims. Thus, for example, a first mixed metal oxide catalyst that is included can be interpreted to mean that the mixture includes at least one polymerization inhibitor.

[0007] As used herein, the recitation of numerical ranges by endpoints includes all numbers subsumed within that range (e.g., 1 to 5 includes 1, 1.5, 2, 2.75, 3, 3.80, 4, 5, etc.). For purposes of the present invention, it should be understood that numerical ranges are intended to include and support all possible subranges subsumed within the range, consistent with what one of skill in the art would understand. For example, a range of 1 to 100 is intended to convey 1.1 to 100, 1 to 99.99, 1.01 to 99.99, 40 to 6, 1 to 55, etc.

[0008] As used herein, numerical ranges and / or recitations of values, including such recitations in the claims, may be read as including the term "about." In such cases, the term "about" refers to numerical ranges and / or values ​​that are substantially the same as those recited herein.

[0009] Unless stated to the contrary or implicit from the context, all parts and percentages are by weight and all test methods are as of the filing date of this application. Unless otherwise defined, weight percent references are to the total weight of the defined element, e.g., a first stage containing 95-99.9 wt. % of units derived from alkyl (meth)acrylate monomers means 95-99.9 wt. % based on the total weight of the first stage.

[0010] As used herein, "unit derived from" means the residue of a monomer following polymerization of the monomer.

[0011] As used herein, "Tg" is the glass transition temperature of a copolymer calculated by the Fox equation [Bulletin of the American Physical Society 1,3 Page 123 (1956)] as follows:

number

[0012] For copolymers, w1 and w2 refer to the weight fractions of the two comonomers based on the weight of monomer charged to the reactor, and Tg (1) and Tg (2) refers to the glass transition temperature of the two corresponding homopolymers in degrees Kelvin. For polymers containing three or more monomers, additional terms are added (w n / Tg (n) For purposes of this invention, the glass transition temperatures of homopolymers are those reported in "Polymer Handbook," edited by J. Brandrup and EH Immergut, Interscience Publishers, 1966, but if that publication does not report the Tg of a particular homopolymer, the Tg of the homopolymer is measured by differential scanning calorimetry (DSC).

[0013] Unless stated to the contrary, all molecular weights disclosed herein are weight average molecular weights. Weight average molecular weight (Mw) is determined by size exclusion chromatography using EasiCal PS-2® polystyrene standards from Polymer Laboratories.

[0014] For purposes of United States patent practice, the contents of any referenced patent, patent application, or publication are hereby incorporated by reference in their entirety, particularly with respect to the disclosure of definitions (to the extent not inconsistent with any definitions specifically provided in this disclosure) and general knowledge in the art, or the equivalent United States version thereof is so incorporated by reference.

[0015] As used herein, the term "(meth)acrylate" means acrylate or methacrylate.

[0016] One aspect of the present invention relates to a multi-stage soft acrylic resin comprising the branched polymer described herein. The inventors have found that the viscosity of the multi-stage soft acrylic resin without the branched polymer is too high to use the resin in certain applications, such as when it is desired to extrude very thin films or in certain injection molding applications. Increasing the processing temperature can degrade the resin. Although the addition of low molecular weight linear additives can reduce the viscosity (increase the melt flow index), the inventors have found that the resulting product in some cases exhibits crease whitening, which may indicate phase separation of the mixture. Surprisingly, the inventors have found that by including an outermost layer comprising the disclosed branched polymer, the viscosity is reduced without exhibiting undesirable crease whitening. In addition, the multi-stage soft acrylic resin with a branched polymer in the outermost layer can exhibit improved tensile properties.

[0017] According to certain embodiments, the multi-stage soft acrylic resin is a multi-stage sequential polymer composition comprising a first stage crosslinked acrylic polymer composition forming a core, a second stage comprising one or more intermediate layer acrylic polymer compositions, a third stage comprising one or more outer layers comprising an acrylic polymer composition, and a fourth stage comprising a branched polymer.

[0018] The first, second, and third stages differ in one or more of the following: derived from different acrylate monomers, degree of crosslinking (second and third stage layers can be crosslinked or uncrosslinked), and glass transition temperature. The acrylic polymer composition is formed from a reaction mixture that includes one or more hydrocarbyl acrylates or hydrocarbyl methacrylates, an optional crosslinker (except some crosslinker is required in the core), and an optional chain transfer agent.

[0019] According to one particular embodiment, the multi-stage flexible acrylic resin comprises a first stage comprising a crosslinked core having a Tg in the range of -85 to -10°C.

[0020] The first stage may be a reaction product of one or more monomers selected from the group consisting of alkyl acrylates and alkyl methacrylates (i.e., alkyl (meth)acrylates) with one or more crosslinking monomers, graft-linking monomers, or combinations thereof. According to certain embodiments, the amount of units derived from alkyl (meth)acrylate monomers may range from 95 to 99.9% by weight of the first stage, and the amount of units derived from crosslinking monomers and / or graft-linking monomers may range from 0.1 to 5% by weight.

[0021] The multi-stage soft acrylic resin may include a second stage comprising one or more layers, each of which may include up to 100% by weight of units derived from one or more monomers selected from the group consisting of alkyl (meth)acrylate monomers, 0-5% by weight of units derived from crosslinking monomers, graft linking monomers, or combinations thereof, and may optionally include 0-2.0% by weight of units derived from one or more chain transfer agents.

[0022] The second stage may have a compositional gradient between one or more layers such that the Tg transitions between a lower Tg and a higher Tg across the width of the second stage. For example, the Tg of one or more layers in the second stage may transition from a low Tg of -30°C to a high Tg of 70°C across the width of the second stage.

[0023] The multi-stage flexible acrylic further comprises a third stage, the third stage comprising one or more layers that may comprise 98.5-100% by weight of units derived from one or more monomers selected from the group consisting of alkyl (meth)acrylates, styrenic monomers, and combinations thereof.

[0024] One or more layers of the third stage may contain 0 to 1.5 wt. % units derived from one or more chain transfer agents.

[0025] The third stage of the multi-stage soft acrylic resin may have a Tg of from 40°C to 110°C.

[0026] The multi-stage flexible acrylic also includes a fourth stage. The fourth stage of the multi-stage flexible acrylic includes one or more layers comprising a branched polymer that is the reaction product of reactants including one or more monoethylenically unsaturated ester monomers, a chain transfer agent in an amount of 0.1-10 wt %, and a crosslinker in an amount of 0.1-10 wt %, where the weight percent is based on the total amount of reactants, but with the proviso that the amount of crosslinker in moles is less than the amount of chain transfer agent in moles.

[0027] According to at least one embodiment, the crosslinkable core (i.e., the first stage) comprises greater than 95-99.9 weight percent units derived from one or more monomers selected from the group consisting of alkyl (meth)acrylate monomers. All individual values ​​and subranges from 95-99.9 weight percent are included herein and disclosed herein, for example, the amount of units derived from one or more alkyl (meth)acrylate monomers can be from a lower limit of 95, 95.5, 96, 96.5, 97, 975, 98, 98.5, 99, or 99.5 weight percent to an upper limit of 95.3, 95.8, 96.3, 96.9, 97.5, 98, 98.7, 99.4, or 99.9 weight percent. For example, the amount of units derived from one or more alkyl (meth)acrylate monomers may range from 95 to 99.9 wt%, or alternatively, the amount of units derived from one or more alkyl (meth)acrylate monomers may range from 95 to 97.5 wt%, or alternatively, the amount of units derived from one or more alkyl (meth)acrylate monomers may range from 97.8 to 99.9 wt%, or alternatively, the amount of units derived from one or more alkyl (meth)acrylate monomers may range from 96.5 to 97.9 wt%.

[0028] The crosslinkable core can include 0.1 to 5 weight percent units derived from crosslinking monomers, graftlinking monomers, or combinations thereof, all individual values ​​and subranges from 0.1 to 5 weight percent are included herein and disclosed herein, for example, the amount of units derived from crosslinking monomers, graftlinking monomers, or combinations thereof can be from a lower limit of 0.1, 0.7, 1.2, 1.9, 2.6, 3.1, 3.7, 4.4, or 4.9 weight percent to an upper limit of 0.2, 0.8, 1.4, 2.1, 2.7, 3.3, 3.8, 4.5, or 5 weight percent. For example, the amount of units derived from crosslinking monomers, graft-linking monomers, or a combination thereof may range from 0.1 to 5 weight percent, or alternatively, the amount of units derived from crosslinking monomers, graft-linking monomers, or a combination thereof may range from 0.5 to 2.5 weight percent, or alternatively, the amount of units derived from crosslinking monomers, graft-linking monomers, or a combination thereof may range from 1.0 to 4.0 weight percent, or alternatively, the amount of units derived from crosslinking monomers, graft-linking monomers, or a combination thereof may range from 0.3 to 3.5 weight percent.

[0029] The crosslinkable core has a Tg of -85 to -10° C. All individual values ​​and subranges of -70 to -10° C. are included herein and disclosed herein, for example, the Tg of the crosslinkable core can be from a lower limit of -85, -80, -70, -60, -50, -40, -30, -20, or -15° C. to an upper limit of -75, -65, -55, -45, -35, -25, -17, or -10° C. For example, the Tg of the crosslinkable core can be in the range of -85 to -10° C., or alternatively, the Tg of the crosslinkable core can be in the range of -60 to -40° C., or alternatively, the Tg of the crosslinkable core can be in the range of -70 to -50° C., or alternatively, the Tg of the crosslinkable core can be in the range of -50 to -30° C.

[0030] The second stage comprises one or more layers. All individual values ​​and subranges of the one or more layers of the second stage are disclosed and included herein. For example, the second stage may comprise one, two, three, four, or five layers.

[0031] Each of the one or more layers of the second stage comprises up to 100% by weight of units derived from one or more monomers selected from the group consisting of alkyl (meth)acrylate monomers. All individual values ​​and subranges up to 100% by weight are included herein and disclosed herein, for example, the amount of units derived from the one or more alkyl (meth)acrylate monomers can be a lower limit of 88.5, 89.4, 90.7, 91.8, 92.6, 93.7, 94, 94.9, 95.5, 96, 97.4, 98.1, 99.3, 99.9, or 100% by weight. For example, the amount of units derived from one or more alkyl (meth)acrylate monomers may range from 88.5 to 100% by weight, or alternatively, the amount of units derived from one or more alkyl (meth)acrylate monomers may range from 90.5 to 99.9% by weight, or alternatively, the amount of units derived from one or more alkyl (meth)acrylate monomers may range from 88.5 to 94.9% by weight, or alternatively, the amount of units derived from one or more alkyl (meth)acrylate monomers may range from 92.5 to 96% by weight.

[0032] Each of the one or more layers of the second stage comprises 0-5 wt. % units derived from a crosslinking monomer, a graftlinking monomer, or a combination of two or more thereof. All individual values ​​and subranges are included herein and disclosed herein, for example, the amount of units derived from a crosslinking monomer, a graftlinking monomer, or a combination thereof can be from a lower limit of 0, 0.5, 1, 1.5, 2, 2.5, 3, 3.5, 4, or 4.5 wt. %, to an upper limit of 0.2, 0.7, 1.2, 1.7, 2.5, 2.7, 3.2, 3.7, 4.2, 4.7, or 5 wt. %. For example, the amount of units derived from crosslinking monomers, graft-linking monomers, or a combination of two or more thereof may range from 0 to 5 weight percent, or alternatively, the amount of units derived from crosslinking monomers, graft-linking monomers, or a combination of two or more thereof may range from 0 to 2.5 weight percent, or alternatively, the amount of units derived from crosslinking monomers, graft-linking monomers, or a combination of two or more thereof may range from 2.5 to 5 weight percent, or alternatively, the amount of units derived from crosslinking monomers, graft-linking monomers, or a combination of two or more thereof may range from 2 to 4 weight percent.

[0033] Each of the one or more layers of the second stage optionally includes 0 to 2.0 wt. % units derived from one or more chain transfer agents, all individual values ​​and subranges between 0 and 2.0 wt. % are included herein and disclosed herein, for example, the amount of units derived from the one or more chain transfer agents can be from a lower limit of 0, 0.2, 0.4, 0.6, 0.8, 1.0, 1.2, 1.4, 1.6, 1.8, or 2.0 wt. % to an upper limit of 0.1, 0.3, 0.5, 0.7, 0.9, 1.1, 1.3, 1.7, or 1.9 wt. %. For example, the amount of units derived from the one or more chain transfer agents may be in the range of 0 to 2.0 wt%, or alternatively, the amount of units derived from the one or more chain transfer agents may be in the range of 0.75 to 2.0 wt%, or alternatively, the amount of units derived from the one or more chain transfer agents may be in the range of 0 to 0.75 wt%, or alternatively, the amount of units derived from the one or more chain transfer agents may be in the range of 0.5 to 1.0 wt%.

[0034] According to at least one embodiment, there is a compositional gradient between one or more layers of the second stage such that the Tg transitions from a lower Tg to a higher Tg across the width of the second stage, e.g., from a lower Tg of -30° C. to a higher Tg of 70° C. All individual values ​​and subranges from -30° C. to 70° C. are included herein and disclosed herein, e.g., the Tg transitions from a lower limit of -30, -20, -10, 0, 10, 20, 30, 40, 50, or 60° C. to an upper limit of -25, -15, -5, 5, 15, 45, or 70° C. For example, the Tg may transition over a range of -30 to 70°C, or alternatively, the Tg may transition over a range of -10 to 30°C, or alternatively, the Tg may transition over a range of -30 to -15°C, or alternatively, the Tg may transition over a range of -25 to 0°C, or alternatively, the Tg may transition over a range of 0 to 15°C, or alternatively, the Tg may transition over a range of -15 to 55°C, or alternatively, the Tg may transition over a range of 5 to 35°C.

[0035] In at least one embodiment, the third stage of the multi-stage flexible acrylic resin includes one or more layers each comprising 98.5-100% by weight of units derived from one or more monomers selected from the group consisting of alkyl (meth)acrylates, styrenic monomers, and combinations of two or more thereof. All individual values ​​and subranges from 98.5-100% by weight are included herein and disclosed herein, for example, the amount of units derived from one or more monomers selected from the group consisting of alkyl (meth)acrylates, styrenic monomers, and combinations of two or more thereof can be from lower limits of 98.5, 98.7, 98.9, 99.1, 99.3, 99.5, 99.7, or 99.9% by weight to upper limits of 98.6, 98.8, 99, 99.2, 99.4, 99.6, 99.8, or 100% by weight. For example, the amount of units derived from one or more monomers selected from the group consisting of alkyl (meth)acrylates, styrenic monomers, and combinations of two or more thereof may be in the range of 98.5 to 100% by weight, or alternatively, the amount of units derived from one or more monomers selected from the group consisting of alkyl (meth)acrylates, styrenic monomers, and combinations of two or more thereof may be in the range of 98.5 to 100% by weight, or alternatively, the amount of units derived from one or more monomers selected from the group consisting of alkyl (meth)acrylates, styrenic monomers, and combinations of two or more thereof may be in the range of 98.5 to 100% by weight, Or alternatively, the amount of units derived from one or more monomers selected from the group consisting of alkyl (meth)acrylates, styrenic monomers, and combinations of two or more thereof may be in the range of 98.5 to 100% by weight, or alternatively, the amount of units derived from one or more monomers selected from the group consisting of alkyl (meth)acrylates, styrenic monomers, and combinations of two or more thereof may be in the range of 98.5 to 99.6% by weight, or alternatively, the amount of units derived from one or more monomers selected from the group consisting of alkyl (meth)acrylates, styrenic monomers, and combinations of two or more thereof may be in the range of 96.5 to 100% by weight.

[0036] According to at least one embodiment, each of the one or more layers of the third stage comprises 0-1.5 wt.% units derived from one or more chain transfer agents. All individual values ​​and subranges from 0-1.5 wt.% are included herein and disclosed herein, for example, the amount of units derived from one or more chain transfer agents can be from a lower limit of 0, 0.2, 0.4, 0.6, 0.8, 1, 1.2, or 1.4 wt.% to an upper limit of 0.1, 0.3, 0.5, 0.7, 0.9, 1.1, 1.3, or 1.5 wt.%. For example, the amount of units derived from one or more chain transfer agents can be in the range of 0-1.5 wt.%, or alternatively, the amount of units derived from one or more chain transfer agents can be in the range of 0-0.75 wt.%, or alternatively, the amount of units derived from one or more chain transfer agents can be in the range of 0.75-1.5 wt.%, or alternatively, the amount of units derived from one or more chain transfer agents can be in the range of 0.3-1.2 wt.%.

[0037] Each of the one or more layers of the third stage has a Tg of 40° C. to 110° C. All individual values ​​and subranges between 50° C. and 110° C. are included herein and disclosed herein, for example, the Tg of the outermost layer can be from a lower limit of 40, 43, 45, 50, 60, 70, 80, 90, or 100° C. to an upper limit of 55, 65, 75, 85, 95, 105, or 110° C. For example, the Tg of the outermost layer can be in the range of 40° C. to 110° C., or alternatively, the Tg of the outermost layer can be in the range of 45° C. to 80° C., or alternatively, the Tg of the outermost layer can be in the range of 75° C. to 110° C., or alternatively, the Tg of the outermost layer can be in the range of 65° C. to 95° C.

[0038] The alkyl of the alkyl (meth)acrylate used in any one of the first, second, and third steps can be a linear or branched alkyl group having 1 to 12 carbon atoms. Exemplary monomers include, and exemplary useful alkyl groups include, butyl acrylate, ethylhexyl acrylate, ethyl acrylate, methyl methacrylate, butyl methacrylate, and iso-octyl acrylate.

[0039] Examples of crosslinking and / or graft linking monomers useful in any of the first, second, and third stages may include, for example, butanediol diacrylate, butanediol dimethacrylate, ethylene glycol diacrylate, ethylene glycol dimethacrylate, divinylbenzene, diethylene glycol diacrylate, diethylene glycol dimethacrylate, diallyl maleate, allyl methacrylate, diallyl phthalate, triallyl phthalate, trimethylolpropane triacrylate, trimethylolpropane trimethacrylate blends thereof, and combinations of two or more thereof.

[0040] According to at least one embodiment, the fourth stage of the multi-stage flexible acrylic resin includes a branched polymer that is the reaction product of reactants including one or more monoethylenically unsaturated ester monomers, a chain transfer agent in an amount of 0.1-10% by weight, and a crosslinker in an amount of 0.1-10% by weight of the crosslinker, the weight percentages being based on the total amount of reactants. The branched polymer is not crosslinked. To avoid crosslinking, the amount of crosslinker does not exceed the amount of chain transfer agent. Thus, according to certain embodiments, the moles of crosslinker are equal to or less than the moles of chain transfer agent. According to certain embodiments, the weight percentage of crosslinker is less than the weight percentage of chain transfer agent.

[0041] Suitable monoethylenically unsaturated ester monomers useful for making the fourth stage branched polymer according to certain embodiments can have the structure R'-C(O)OR, where R is a hydrocarbyl group (e.g., an alkyl group or an aryl group) and R' is a monoethylenically unsaturated aliphatic group having at least 2 or 3 carbon atoms. According to certain embodiments, R is an alkyl group of at least 1 or 2 or 3 carbon atoms. According to certain embodiments, R is an alkyl group having 12 or 10 or 8 or 6 or 5 or less carbon atoms. According to certain embodiments, R is an aryl group of 6 to 12 carbon atoms. According to certain embodiments, R' has 6 or less carbon atoms. Examples of suitable monomers useful for making the fourth stage branched polymer include butyl acrylate, ethylhexyl acrylate, ethyl acrylate, methyl methacrylate, butyl methacrylate, cyclohexyl (meth)acrylate, cyclopentyl methacrylate, tetrahydrofurfyl methacrylate, and benzyl (meth)acrylate. A combination of two or more such monoethylenically unsaturated ester monomers can be used. For example, a combination of methyl methacrylate and butyl methacrylate can be used. For example, the amount of methyl methacrylate can be at least 20, 30, 40, 50, 60, 70, or 80% by weight of the reactants, and can be, for example, less than 99.8, 99, 98, 97, 96, 95, 90, 85% by weight of the reactants. The second monoethylenically unsaturated ester monomer (e.g., butyl acrylate) can be 0 or more than 0, 1, 2, 3, 4, 5% by weight of the reactants and less than 60, 50, 40, 30, 20, or 10% by weight of the reactants. In certain embodiments, an additional monoethylenically unsaturated ester monomer can be used. In such embodiments, the combination of the second and additional monoethylenically unsaturated monomers taken together is more than 0, 1, 2, 3, 4, 5% by weight of the reactants and less than 60, 50, 40, 30, 20, or 10% by weight of the reactants.

[0042] According to certain embodiments, one or more additional monounsaturated addition polymerizable (e.g., monoethylenically unsaturated) monomers may be included in the fourth stage branched polymer. For example, styrene or acrylonitrile may be added. The amount of such additives is preferably less than 10 or 5% by weight based on the weight of the reactants.

[0043] The reactants for forming the branched polymer further include a chain transfer agent (CTA). The chain transfer agent can be any compound known or found to be useful as a chain transfer agent in the polymerization of acrylate or methacrylate monomers. For example, a thiol chain transfer agent can be used. Examples of such thiol CTAs include monofunctional and multifunctional thiols. Monofunctional thiols include, but are not limited to, propyl mercaptan, butyl mercaptan, hexyl mercaptan, octyl mercaptan, dodecyl mercaptan, thioglycolic acid, mercaptopropionic acid, alkyl thioglycolates, such as 2-ethylhexyl thioglycolate or octyl thioglycolate, mercaptoethanol, mercaptoundecanoic acid, thiolactic acid, thiobutyric acid. Multifunctional thiols include trifunctional compounds such as trimethylolpropane tris(3-mercaptopropionate), tetrafunctional compounds such as pentaerythritol tetra(3-mercaptopropionate), pentaerythritol tetrathioglycolate, pentaerythritol tetrathiolactate, pentaerythritol tetrathiobutyrate, hexafunctional compounds such as dipentaerythritol hexa(3-mercaptopropionate), dipentaerythritol hexathioglycolate, and octafunctional thiols such as tripentaerythritol octa(3-mercaptopropionate), tripentaerythritol octathioglycolate. The use of multifunctional thiols is a useful method for increasing the branching degree of the polymer. Optionally, the chain transfer agent may include a mixture of two or more compounds. According to one embodiment, the CTA is: [ka] It is.

[0044] The alternative chain transfer agent can be any species known to reduce molecular weight in conventional free radical polymerization of vinyl monomers. Examples include sulfides, disulfides, halogen-containing species. Catalytic chain transfer agents such as cobalt complexes, e.g., cobalt(II) chelates such as cobalt porphyrin compounds, are also useful chain transfer agents for the present invention. Suitable cobalt chelates are known in the art and described in WO98 / 04603. A particularly suitable compound is bis(borondifluorodimethylglyoximate)cobaltate(II), also known as CoBF. Catalytic chain transfer agents are generally very effective at low concentrations, and therefore can be used at relatively low concentrations, e.g., <0.5 wt%, preferably <0.1 wt% (based on monofunctional monomer), compared to conventional thiol chain transfer agents. Surprisingly, we have found that catalytic chain transfer compounds based on cobalt complexes can be used very effectively in the polymerization process of the invention to obtain soluble branched polymers at concentrations of less than 0.05% by weight (500 ppmw), for example 0.0001-0.01% by weight (1-100 ppmw), based on the monofunctional monomer.

[0045] The amount of chain transfer agent used to form the fourth stage branched polymer is at least 0.1 or 0.5 or 1 weight percent based on the total weight of the reactants. According to some embodiments, the amount of chain transfer agent is no more than 10 or 8 or 6 or 5 weight percent based on the total weight of the reactants.

[0046] The reactants for forming the branched polymer further include a crosslinking agent. The inclusion of the crosslinking agent results in branching. However, the amount of crosslinking agent must be controlled so that the polymer does not crosslink. According to an embodiment, the amount of crosslinking agent is equal to or less than the amount of chain transfer agent. According to an embodiment, the amount of crosslinking agent is less than the amount of chain transfer agent. According to an embodiment, the weight percentage of the crosslinking agent is lower than the weight percentage of the chain transfer agent. According to an embodiment, the weight ratio of the chain transfer agent to the crosslinking agent is in the range of 1:1 or 1.5:1 to 10:1. According to an embodiment, the molar percentage of the crosslinking agent is lower than the molar percentage of the chain transfer agent. According to an embodiment, the molar ratio of the chain transfer agent to the crosslinking agent is at least 1.2:1 or 1.4:1 or 1.5:1 or 1.7:1 or 2:1 or 4:1. According to an embodiment, the molar ratio of the chain transfer agent to the crosslinking agent is less than 20:1 or 15:1 or 10:1.

[0047] The crosslinking agent used to form the branched polymer can be any polyfunctional unsaturated monomer, i.e., any monomer with two or more unsaturated groups available for addition polymerization. Examples of suitable difunctional monomers include ethylene glycol di(meth)acrylate, hexanediol di(meth)acrylate, tripropylene glycol di(meth)acrylate, butanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, allyl (meth)acrylate, divinylbenzene, and derivatives thereof. Examples of trifunctional include tripropylene glycol tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate. Tetrafunctional monomers such as pentaerythritol tetra(meth)acrylate and hexafunctional monomers such as dipentaerythritol hexa(meth)acrylate can also be used. Optionally, the multifunctional monomer may comprise a mixture of two or more multifunctional compounds. According to one embodiment, the crosslinking agent is [ka] It is.

[0048] The amount of crosslinker according to some embodiments is at least 0.1 or 0.5 or 1 weight percent based on the total weight of the reactants used to form the branched polymer. According to some embodiments, the amount of crosslinker is no more than 10 or 8 or 6 or 5 weight percent based on the total weight of the reactants.

[0049] According to certain embodiments, the crosslinker is BGDMA and the chain transfer agent is BMA. According to certain embodiments, the acrylate monomer (e.g., methyl methacrylate) is present in an amount of 90-99% by weight, the amount of BGDMA ranges from 1 or 2 to 4 or 3% by weight, and the amount of BMA ranges from 1 or 2 or 3 to 7 or 6% by weight, based on the total weight of the acrylate monomer, BGDMA, and BMA.

[0050] According to certain embodiments, the total amount of the first, second, and third stages of the multi-stage soft acrylic resin comprises at least 10, 20, 30, 40, 50, 60, 70, 75, 80, 85, or 90% by weight based on the total weight of the multi-stage soft acrylic resin. The total amount of the first, second, and third stages of the multi-stage soft acrylic resin may comprise less than 90, 85, 80, 75, 70, 60, 50, or 40% by weight based on the total weight of the multi-stage soft acrylic resin. The fourth stage may comprise at least 10, 15, 20, 25, 30, 40, 50, 60, 70, 80, or 90% by weight based on the total weight of the multi-stage soft acrylic resin. The fourth stage may comprise less than 90, 80, 70, 60, 50, 40, 30, 25, 20, 15, or 10% by weight based on the total weight of the multi-stage soft acrylic resin.

[0051] According to at least one embodiment, the ratio of the amount of the fourth stage in the multi-stage soft acrylic resin to the total amount of the first, second, and third stages can be varied to control the melt flow index (viscosity) of the resin. The inventors have found that multi-stage acrylic resins without a fourth stage have viscosities that may be too high for use in certain applications, such as very thin film extrusion or certain injection molding applications. The inventors have found that the presence of a branched polymer in the fourth stage can increase the melt flow index (reduce the viscosity) of the multi-stage soft acrylic resin.

[0052] According to at least one embodiment, the weight ratio of the fourth stage to the combined weight of the first, second and third stages ranges from 5:95 to 50:50. Preferably, the weight ratio of the fourth stage to the combined weight of the first, second and third stages ranges from 10:90 to 40:60, more preferably from 15:85 to 30:70.

[0053] The multi-stage soft acrylic resin preferably has a melt flow index according to ASTM D1238 of at least 30, 40, 50, or 60 g / 10 min, 220° C., 10 kg. According to certain embodiments, the melt flow index is less than 100 or 90 g / 10 min, 220° C., 10 kg.

[0054] According to certain embodiments, the multi-stage soft acrylic resin is non-hazy, e.g., the turbidity as measured by light transmission is less than 1% when measured according to ASTM D1003 using a suitable device, e.g., BYK HazeGuard Plus.

[0055] Another aspect of the invention relates to a method for forming a multi-stage flexible acrylic resin. According to at least one embodiment, the multi-stage flexible acrylic resin is formed by emulsion polymerization, with each stage of the multi-stage flexible acrylic resin being formed sequentially. In at least one embodiment, the multi-stage flexible acrylic resin is formed in a single reactor.

[0056] In certain embodiments, the first stage is formed by emulsion polymerization of a reaction mixture comprising 95-99.9% by weight of one or more monomers selected from the group consisting of alkyl (meth)acrylate monomers, and 0.1-5% by weight of one or more monomers selected from crosslinking monomers, graft linking monomers, and mixtures thereof.

[0057] The second stage is formed by emulsion polymerization in the presence of the first stage and a reaction mixture comprising up to 100% by weight of a monomer selected from the group consisting of alkyl (meth)acrylate monomers. The reaction mixture of the second stage may comprise 0-5% by weight of one or more monomers selected from crosslinking monomers, graft linking monomers, and mixtures thereof, and 0-2% by weight of a chain transfer agent. The emulsion polymerization can be repeated to form two or more layers for the second stage. The reaction mixture used to form the additional layers can be the same or different, for example, by adding additional monomers to the reaction mixture to modify the composition of the reaction mixture. In this way, the layers of the second stage can be different from each other. Thus, the product includes a layer(s) of the second stage forming a shell around the crosslinkable core of the first stage.

[0058] The third stage is formed by emulsion polymerization in the presence of a reaction mixture comprising the product of the second stage polymerization reaction, i.e., the first stage and the second stage, and the monomer to be incorporated into the third stage. The reaction mixture for forming the third stage may comprise 98.5 to 100 weight percent of one or more monomers selected from the group consisting of alkyl (meth)acrylate monomers, styrenic monomers, and mixtures thereof. The reaction mixture for the third stage polymerization reaction may also comprise 0 to 1.5 weight percent of one or more chain transfer agents. The product of the third stage polymerization comprises the first stage, the second stage, and the third stage.

[0059] The fourth stage is formed by emulsion polymerization in the presence of the product from the third stage polymerization, i.e., a reaction mixture comprising the first stage, the second stage, and the third stage, and the fourth stage monomers. The reaction mixture for the fourth stage polymerization reaction may comprise one or more monoethylenically unsaturated ester monomers, a chain transfer agent in an amount of 0.1-10% by weight, and a crosslinker in an amount of 0.1-10% by weight, the weight percentages being based on the total amount of monoethylenically unsaturated ester monomers, chain transfer agent, and crosslinker in the fourth stage polymerization reaction mixture, provided that the amount of crosslinker in moles is less than the amount of chain transfer agent in moles. The product of the fourth stage polymerization reaction is a multi-stage flexible acrylic resin comprising the first stage, the second stage, the third stage, and the fourth stage.

[0060] Surfactants or emulsifiers can be used in any of the process steps. Examples of emulsifiers include nonionic, anionic, and cationic emulsifiers.

[0061] Suitable nonionic emulsifiers are araliphatic or aliphatic nonionic emulsifiers, examples of which include ethoxylated mono-, di-, and trialkylphenols (degree of ethoxylation: 3 to 50, alkyl radical: C4-C 10 ), ethoxylates of long-chain alcohols (ethoxylation degree: 3-100, alkyl radical: C8-C 36 ), as well as polyethylene oxide / polypropylene oxide homopolymers and copolymers. These may contain alkylene oxide units in random distribution or copolymerized in the form of blocks. For example, ethylene oxide / propylene oxide block copolymers are very suitable. Ethoxylates of long-chain alkanols (alkyl radicals C1-C 30 It is preferable to use linear C 12 -C 20 Those having alkyl radicals and an average degree of ethoxylation of 10 to 50, also ethoxylated monoalkylphenols, are particularly preferred.

[0062] Suitable anionic emulsifiers are, for example, alkyl sulfates (alkyl radical: C8-C 22 ), ethoxylated alkanol (ethoxylation degree: 2-50, alkyl radical: C 12 -C 18 ) and ethoxylated alkylphenols (ethoxylation degree: 3-50, alkyl radical: C4-C9) with sulfuric acid monoesters, alkylsulfonic acids (alkyl radical: C 12 -C 18 ), and alkylarylsulfonic acids (alkyl radical: C9-C 18 Further suitable emulsifiers are described in Houben-Weyl, Methoden der organischen Chemie, volume XIV / 1, Makromolekulare Stoffe, Georg-Thieme-Verlag, Stuttgart, 1961, pp. 192-208. Also suitable as anionic emulsifiers are bis(phenylsulfonic acid) ethers and phenylsulfonic acid ethers having C4-C in one or both aromatic rings. 24 These compounds include the alkali metal or ammonium salts thereof bearing alkyl groups. These compounds, for example from US Patent No. 4,269,749, are well known and are commercially available, for example in the form of Dowfax™ 2A1 (Dow Chemical Company).

[0063] Suitable cationic emulsifiers are preferably quaternary ammonium halides, such as trimethylcetylammonium chloride, methyltrioctylammonium chloride, benzyltriethylammonium chloride, or N-C6-C 20 -alkylpyridine, -morpholine or -imidazole quaternary compounds, for example N-laurylpyridinium chloride.

[0064] The amount of emulsifier (or surfactant) can be at least 0.01 or 0.1% to 10 or 5% by weight based on the amount of monomer polymerized in each of the emulsion polymerization steps.

[0065] An initiator can be used. Examples of initiators include and can be initiated by any suitable method of generating free radicals, such as by thermally induced decomposition of a thermal initiator such as an azo compound, a peroxide, or a peroxyester. Thus, the polymerization mixture also preferably contains a polymerization initiator, which can be any of those known and conventionally used in free radical polymerization reactions. Examples of azo initiators include azobis(isobutyronitrile) (AIBN), azobis(2-methylbutyronitrile), azobis(2,4-dimethylvaleronitrile), azobis(4-cyanovaleric acid). Examples of peroxide and peroxy initiators include hydrogen peroxide, sodium peroxide, potassium peroxide, t-butyl hydroperoxide, cumene hydroperoxide, dilauroyl peroxide, tert-butyl peroxyneodecanoate, dibenzoyl peroxide, cumyl peroxide, tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxydiethyl acetate, and tert-butyl peroxybenzoate. Examples of additional initiators include ammonium and / or alkali metal persulfates, sodium perborate, perphosphoric acid and its salts, potassium permanganate, and ammonium or alkali metal salts of peroxydisulfate, such as alkali metal or ammonium peroxydisulfates, diacetyl peroxide, dibenzoyl peroxide, succinyl peroxide, di-tert-butyl peroxide, tert-butyl perbenzoate, tert-butyl perpivalate, tort-butyl peroxy-2-ethylhexanoate, te rt-butyl permaleinate, cumene hydroperoxide, diisopropyl peroxydicarbamate, bis(o-toluoyl) peroxide, didecanoyl peroxide, dioctanoyl peroxide, dilauroyl peroxide, tert-butyl perisobutyrate, tert-butyl peracetate, di-tert-amyl peroxide, tert-butyl hydroperoxide, azobisisobutyronitrile, 2,2'-azobis(2-amidino-propane) dihydrochloride, or 2,2'-azobis(2-methylbutyronitrile).Mixtures of these initiators are also suitable. It is also possible to use reduction / oxidation (i.e. redox) initiator systems as initiators. Redox initiator systems consist of at least one, usually inorganic, reducing agent and one organic or inorganic oxidizing agent. The oxidizing component includes, for example, the emulsion polymerization initiators already specified above. The reducing component includes, for example, alkali metal salts of sulfite, such as sodium sulfite, sodium hydrogen sulfite, alkali metal salts of disulfite, such as sodium disulfite, hydrogen sulfite adducts of aliphatic aldehydes and ketones, such as acetone sulfite, or reducing agents, such as hydroxymethanesulfinic acid and its salts, or ascorbic acid. Redox initiator systems can be used with soluble metal compounds whose metal components can exist in multiple valence states. Typical redox initiator systems are, for example, ascorbic acid / iron(II) sulfate / sodium peroxodisulfate, tert-butyl hydroperoxide / sodium disulfite, tert-butyl hydroperoxide / Na hydroxymethanesulfinate. Individual components, such as the reducing component, can also be mixtures, an example being a mixture of the sodium salt of hydroxymethanesulfinic acid and sodium disulfite.

[0066] The amount of initiator is generally at least 0.01 or 0.05 or 0.01% to 10 or 5 or 3% by weight based on all monomers being polymerized.

[0067] The fourth stage branched polymer is not crosslinked. For example, this can be demonstrated by evaluating the solubility of the polymer in a solvent such as tetrahydrofuran. The crosslinked polymer is not soluble.

[0068] Branched polymers according to certain embodiments may be characterized by a polymer branching ratio g' of less than 1, 0.95, 0.9, or 0.8. According to some embodiments, g' is at least 0.5 or 0.6 or 0.7. The polymer branching ratio (g') is the ratio of the branched polymer ([η]) measured at each elution volume increment in gel permeation chromatography (GPC) analysis.branched ) of a linear polymer with the same molecular weight (M) ([η] linear ) (Equation 1). For linear polymers, the g' value is equal to 1, for branched polymers, g' is less than 1.

number

[0069] Molecular weight analysis: absolute molecular weight of polymer (M w , M n ), PMMA relative molecular weight (M w_PMMA , M n_PMMA ), intrinsic viscosity ([η] w , [η] n ), and branching ratio (g') can be measured by gel permeation chromatography with an online multi-angle light scattering (MALS) detector, a viscometer (VS), and a differential refractive index (dRI) detector. For example, a GPC instrument setup can include an Agilent 1200 series HPLC system (degasser, pump, autosampler, column oven), a Wyatt HELEOS II MALS detector, a Wyatt ViscoStar II viscometer, and a Wyatt T-rEX dRI detector. Polymer separation can be performed on a column set with two PLgel 10 μm PLgel mixed B LS columns (7.5x300mm) using tetrahydrofuran (THF) as the mobile phase at a flow rate of 1 mL / min. The column oven temperature is set at 30 °C. A set of 10-point PMMA standards (Agilent EasiCal PM-1) is used to calibrate the GPC column to obtain PMMA relative molecular weights. Absolute molecular weights are obtained from MALS detection using the Zimm format, and intrinsic viscosity data are obtained from the viscometer. The high molecular weight fraction data (PMMA relative molecular weight above 6500 Da) are used to calculate the average g' value. To keep the g' calculations consistent, a linear PMMA model from the Mark-Houwink equation (Eq. 2, where K = 0.03044 mL / g and α = 0.615) is used to calculate the ([η] linear) is obtained using the M data from MALS detection. [η] = KM α (Formula 2)

[0070] The weight average molecular weight M of the fourth stage branched polymer measured by GPC w According to certain embodiments, the weight average molecular weight is at least in the range of 8000 or 10,000 or 15,000 or 20,000 g / mol. According to certain embodiments, the weight average molecular weight is not more than 100,000 or 80,000 g / mol. According to certain embodiments, the number average molecular weight M of the branched polymer, as measured by GPC, is at least in the range of 8000 or 10,000 or 15,000 or 2 ... is at least in the range of 8000 or 10,000 or 15,000 g n is at least 3000 or 4000 or 5000 g / mol. According to certain embodiments, the number average molecular weight is not more than 50,000 or 40,000 or 30,000 or 20,000 g / mol.

[0071] According to one particular embodiment, the branched structure is a dendritic structure.

[0072] Another aspect of the present invention relates to compositions incorporating multi-stage soft acrylic resins.

[0073] According to at least one embodiment, the multi-stage soft acrylic resin may be blended with another polymer to form a composition, examples of which include acrylate polymers such as poly(methyl methacrylate), or other polymers such as polyvinyl chloride.

[0074] In other embodiments, the multi-stage soft acrylic resin can be blended with another multi-stage resin. For example, the multi-stage soft acrylic resin according to the embodiments disclosed herein can be blended with a multi-stage acrylic resin that does not contain a branched polymer, such as a multi-stage acrylic resin that includes three stages corresponding to the first stage, second stage, and third stage of the multi-component soft acrylic resin disclosed herein. The ratio of the multi-stage acrylic resin in such a blend can be adjusted, for example, to control the amount of branched polymer contained in the blend and adjust the properties of the polymer blend, such as, for example, the melt flow index.

[0075] The composition may further include additional additives desired in the final product. Examples of such additives include UV light stabilizers and antioxidants. According to certain embodiments, the additives are selected so that the composition remains transparent. Examples of UV light stabilizers include benzophenones, benzotriazoles, triazines, benzoxazinones, hindered amine light stabilizers (HALS), and hindered benzoates. Commercially available UV and light stabilizers include Cyasorb light absorbers and light stabilizers from Solvay, Cyasorb Cynergy Solutions, TINUVIN FROM BASF, LowLite from Chemtura, OnCap from PolyOne, and Light Stabilizer from EI du Pont de Nemours and Company of Delaware, USA.210, examples of which include phenolic antioxidants and combinations of phenolic antioxidants with phosphites, thioethers or organic sulfides. Phenolic antioxidants include fully hindered and partially hindered phenols; sterically hindered amines such as tetramethyl-piperidine derivatives. Suitable phenolic antioxidants include vitamin E, and IRGANOX™ 1010 from BASF. IRGANOX™ 1010 includes pentaerythritol tetrakis(3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate). Additional examples of antioxidants include acetylcysteine, arbutin, ascorbic acid, ascorbic acid polypeptide, ascorbyl dipalmitate, methylsilanol ascorbyl pectate, ascorbyl palmitate, ascorbyl stearate, BHA, p-hydroxyanisole, BHT, t-butylhydroquinone, caffeic acid, camellia oil, chitosan ascorbate, chitosan glycolate, chitosan salicylate, chlorogenic acid, cysteine, cysteine ​​HCI, decylmercaptomethylimidazole, erythorbic acid, diamylhydroquinone, di-t-butylhydroquinone, dicetyl thiodipropionate, dicyclopentadiene / t-butylcresol copolymer. Polymer, digalloyl trioleate, dilauryl thiodipropionate, dimyristyl thiodipropionate, dioleyl tocopheryl methylsilanol, isoquercitrin, diosmin, disodium ascorbyl sulfate, disodium rutinyl disulfate, distearyl thiodipropionate, ditridecyl thiodipropionate, dodecyl gallate, ethyl ferulate, ferulic acid, hydroquinone, hydroxylamine HCI, hydroxylamine sulfate, isooctyl thioglycolate, kojic acid, madecassoside, magnesium ascorbate, magnesium ascorbyl phosphate, melatonin, methoxy-PEG-7 rutinyl succinatesuccinate), methylenedi-t-butylcresol, methylsilanol ascorbate, nordihydroguaiaretic acid, octyl gallate, phenylthioglycolic acid, phloroglucinol, potassium ascorbyl tocopheryl phosphate, thiodiglycolamide, potassium sulfite, propyl gallate, rosmarinic acid, rutin, sodium ascorbate, sodium ascorbyl / cholesteryl phosphate, sodium bisulfite, sodium erythorbate, sodium metadisulfide, sodium sulfite, sodium thioglycolate, sorbityl furfural, tea tree (melaleuca alternifolia) oil, Tocopheryl acetate, tetrahexyldecyl ascorbate, tetrahydrodiferuloylmethane, tocopheryl linoleate / oleate, thiodiglycol, tocopheryl succinate, thiodiglycolic acid, thioglycolic acid, thiolactic acid, thiosalicylic acid, thiotaurine, retinol, tocopheryl acetate, tocopheryl acetate 10, tocopheryl acetate 12, tocopheryl acetate 18, tocopheryl acetate 50, tocopherol, tocophersolan, tocopheryl linoleate, tocopheryl acetate nicotinate, tocoquinone, o-tolylbiguanide, tris(nonylphenyl)phosphite, ubiquinone, zinc dibutyldithiocarbamate, and mixtures thereof. According to certain embodiments, the total amount of additives (if any) used is less than 10 or 5 or 3% by weight based on the total weight of the composition.

[0076] The composition preferably has a melt flow index of at least 30, 40, 50, or 60 g / 10 min, 220° C., 10 kg according to ASTM D 1238. According to certain embodiments, the melt flow index is less than 100 or 90 g / 10 min, 220° C., 10 kg.

[0077] According to certain embodiments, the composition is not turbid, e.g., the turbidity, as measured by light transmission, is less than 1% when measured according to ASTM D1003 using a suitable device, e.g., BYK HazeGuard Plus.

[0078] Multi-stage soft acrylic resins, either alone or incorporated within compositions, are useful for extrusion and injection molding applications due to their favorable melt flow index.

[0079] According to certain embodiments, the multi-stage soft acrylic resin or composition thereof can be extruded as a thin film. The film can have a thickness of 150 or 125 or 100 microns or less. According to certain embodiments, the thickness is at least 50 microns. According to certain embodiments, the multi-stage soft acrylic resin or composition thereof can be coextruded as a layer of a multi-layer film. The layer can have a thickness of 150 or 125 or 100 microns or less. According to certain embodiments, the layer has a thickness of at least 10, 20, 30, or 50 microns. The film is transparent. The film does not exhibit flute whitening. EXAMPLES

[0080] The multi-stage flexible acrylic resin was formed by conventional emulsion polymerization. For comparison purposes and for use in compositions according to embodiments of the present invention, a three-stage flexible acrylic resin was prepared. A four-stage flexible acrylic resin according to embodiments of the present invention was prepared by carrying out a fourth stage emulsion polymerization reaction using the products of the three-stage polymerization reaction in the same reactor.

[0081] Three-stage soft acrylic resin A three stage flexible acrylic resin (3-FAR) was prepared by conventional emulsion polymerization as disclosed in US Pat. No. 10,040,915.

[0082] 4-stage soft acrylic resin A four-stage flexible acrylic resin according to an embodiment of the present invention was made by conventional emulsion polymerization using the three-stage flexible acrylic resin (3-FAR) prepared above with a fourth stage reaction mixture containing MMA and BA monomers, a chain transfer agent (CTA) containing butyl 3-mercaptopropionate (BMP), and a crosslinker (XL) containing 1,4-butanediol dimethacrylate (BGDMA). The fourth stage contains 87.5 wt% MMA, 5 wt% BA, 5 wt% BMP, and 2.5 wt% BGDMA. The composition of the fourth stage is the same in each of the following examples.

[0083] Melt Flow Index According to an embodiment of the present invention, the melt flow index (MFI) of a three stage soft acrylic resin (3-FAR) was compared to the melt flow index of a four stage soft acrylic resin. The MFI was measured according to ASTM D1238. As shown in Table 1 below, the presence of the fourth stage significantly increases the MFI of the multi-stage soft acrylic resin. [Table 1]

[0084] Blend Composition A composition containing a multi-stage soft acrylic resin according to an embodiment of the present invention was prepared by blending a four-stage soft acrylic resin with the three-stage soft acrylic resin (3-FAR) described above. The components that make up the composition can be mixed together by any known mixing method and conventional equipment such as a polymer compounding device or powder mixer.

[0085] The fourth stage of each of the four-stage soft acrylics had the same composition as above, i.e., 87.5 wt% MMA, 5 wt% BA, 5 wt% BMP, and 2.5 wt% BGDMA, and the first, second, and third stages of the four-stage soft acrylics had the same composition as the three stages of 3-FAR. The weight ratio of the fourth stage to the total weight of the first, second, and third stages was varied. The four-stage soft acrylics were isolated and blended with 3-FAR. The samples were then milled at 185°C for 5 minutes using a laboratory two-roll mill to form clear films and tested for MFI. [Table 2]

Claims

1. A multi-stage soft acrylic resin, a) a first stage comprising a crosslinked core having a Tg in the range of -85 to -10°C, said first stage comprising 95 to 99.9 wt% units derived from one or more monomers selected from the group consisting of alkyl (meth)acrylate monomers and 0.1 to 5 wt% units derived from one or more crosslinking monomers; b) a second stage consisting of one or more layers comprising 88.5-100% by weight of units derived from one or more monomers selected from the group consisting of alkyl (meth)acrylate monomers, 0-5% by weight of units derived from a crosslinking monomer, and optionally 0-2% by weight of one or more chain transfer agents, wherein there is a compositional gradient between said one or more layers such that the Tg transitions between a lower Tg and a higher Tg, said lower Tg being at least 0° C. and said higher Tg being no greater than 70° C. across the width of said second stage; c) a third stage comprising one or more layers comprising 98.5-100% by weight of units derived from one or more monomers selected from the group consisting of alkyl (meth)acrylates and 0-1.5% by weight of units derived from one or more chain transfer agents, the third stage having a Tg in the range of 40° C. to 110° C.; d) a fourth stage comprising one or more layers comprising a branched polymer that is the reaction product of reactants comprising one or more monoethylenically unsaturated ester monomers, a chain transfer agent in an amount of 0.1-10% by weight, and a crosslinker in an amount of 0.1-10% by weight, wherein the weight percentages are based on the total amount of reactants, with the proviso that the amount of crosslinker in molar is less than the amount of chain transfer agent in molar.

2. 10. The multi-stage soft acrylic resin of claim 1, wherein the branched polymer of the fourth stage is not crosslinked.

3. 3. The multi-stage flexible acrylic resin of claim 1 or 2, wherein the one or more monoethylenically unsaturated ester monomers have the structure R'-C(O)O-R, where R is a hydrocarbyl group of 1 to 12 carbon atoms and R' is a monoethylenically unsaturated aliphatic group having at least 2 or 3 carbon atoms.

4. The chain transfer agent of the fourth stage is selected from the group consisting of propyl mercaptan, butyl mercaptan, hexyl mercaptan, octyl mercaptan, dodecyl mercaptan, thioglycolic acid, mercaptopropionic acid, alkyl thioglycolate, mercaptoethanol, mercaptoundecanoic acid, thiolactic acid, thiobutyric acid, trimethylolpropane tris(3-mercaptopropionate), pentaerythritol tetra(3-mercaptopropionate), pentaerythritol tetrathioglycolate, ...

4. The multi-stage soft acrylic resin of any of claims 1 to 3, wherein the mercury-containing acrylic resin is selected from the group consisting of erythritol tetrathiolactate, pentaerythritol tetrathiobutyrate, dipentaerythritol hexa(3-mercaptopropionate), dipentaerythritol hexathioglycolate, tripentaerythritol octa(3-mercaptopropionate), tripentaerythritol octathioglycolate, butyl 3-mercaptopropioante, and combinations of two or more thereof.

5. 5. The multi-stage flexible acrylic resin of any of claims 1 to 4, wherein the crosslinker of the fourth stage is selected from the group consisting of ethylene glycol di(meth)acrylate, hexanediol di(meth)acrylate, tripropylene glycol di(meth)acrylate, butanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, allyl (meth)acrylate, divinylbenzene and its derivatives, tripropylene glycol tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,4 butanediol dimethacrylate, and combinations of two or more thereof.

6. The multi-stage soft acrylic resin according to any of claims 1 to 5, wherein the amount of said crosslinker in said fourth stage is 0.5 to 4 wt%.

7. 7. The multi-stage flexible acrylic resin according to any one of claims 1 to 6, wherein the amount of said chain transfer agent in said fourth stage is 1 to 5 weight percent.

8. 8. The multi-stage soft acrylic resin of any of claims 1 to 7, wherein the branched polymer of the fourth stage is characterized by a g' of 0.9 or less.

9. The multi-stage flexible acrylic resin of any of claims 1 to 8, wherein the fourth stage comprises 1 to 75 weight percent based on the total weight of the multi-stage flexible acrylic resin.

10. 10. The multi-stage flexible acrylic resin of claim 9, wherein said fourth stage comprises 5 to 50 weight percent based on the total weight of said multi-stage flexible acrylic resin.

11. The multi-stage soft acrylic resin of any one of claims 1 to 10 having a melt flow index of at least less than 40 g / 10 min, 220°C, 10 kg.

12. 10. A method for producing the multi-stage flexible acrylic resin of claim 1, comprising: 1) forming a first stage by emulsion polymerization of a first stage reaction mixture comprising 95-99.5% by weight of one or more monomers selected from the group consisting of alkyl (meth)acrylate monomers and 0.1-5% by weight of one or more monomers selected from crosslinking monomers; 2) forming said second stage by emulsion polymerization of the polymerization product of said first stage with a reaction mixture comprising 93-100% by weight of a monomer selected from the group consisting of alkyl (meth)acrylate monomers, 0-5% by weight of one or more monomers selected from crosslinking monomers, and 0-2.0% by weight of a chain transfer agent; 3) forming the third stage by emulsion polymerization of the polymerization product of the second stage with a reaction mixture comprising 98.5 to 100 weight percent of one or more monomers selected from the group consisting of alkyl (meth)acrylate monomers, and 0 to 1.5 weight percent of one or more chain transfer agents; 4) forming said fourth stage by emulsion polymerization of the polymerization product of said third stage with a reaction mixture comprising one or more monoethylenically unsaturated ester monomers, a chain transfer agent in an amount of 0.1-10% by weight, and a crosslinking agent in an amount of 0.1-10% by weight, wherein the amount of crosslinking agent in molar is less than the amount of chain transfer agent in molar.

13. 13. The process of claim 12, wherein the emulsion polymerizations are carried out sequentially in the same reactor.

Citation Information

Patent Citations

  • Multilayered structural polymer and resin composition containing the same, acrylic resin film-like article, acrylic resin lamination film, optically thermosetting resin film or sheet, lamination film or sheet, and laminated formed product by laminating them

    JP2005163003A

  • Multi-stage polymer compositions and films and polarizers produced therefrom

    JP2014524511A

  • Multi-step polymer composition and film made from this composition

    JP2015532674A

  • Multi-stage polymer composition, and films and polarizer plates made thereof

    JP2017179375A

  • Multistage polymer compositions and films made therefrom

    JP2019516848A