Secondary battery manufacturing method

The described method for manufacturing secondary batteries addresses the issue of battery case swelling by controlling thickness relationships and pressing conditions during the electrolyte injection and sealing process, ensuring the battery case maintains its shape and structural integrity.

JP7556925B2Active Publication Date: 2024-09-26PRIME PLANET ENERGY & SOLUTIONS INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2022173415
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-10-28
Publication Date
2024-09-26
Estimated Expiration
2042-10-28

AI Technical Summary

Technical Problem

Conventional methods for manufacturing secondary batteries do not adequately address the suppression of battery case swelling in the vertical direction due to gas generation during charging and discharging, which can lead to an increase in the height of the battery case.

Method used

A manufacturing method that involves injecting electrolyte through a sealing plate, charging the battery case, and sealing the liquid injection hole while pressing the first side walls with a jig, ensuring the thickness relationship of the sealing plate to the battery case components suppresses deformation and swelling.

Benefits of technology

This method effectively prevents the battery case from expanding into a convex shape by controlling the thickness relationships and pressing conditions, thereby reducing pressure and maintaining the battery case's structural integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007556925000007
    Figure 0007556925000007
  • Figure 0007556925000001
    Figure 0007556925000001
  • Figure 0007556925000002
    Figure 0007556925000002
Patent Text Reader

Abstract

To provide a method of manufacturing a secondary battery that can suppress an increase in thickness of a battery case caused by charge and discharge and also can suppress an increase in height of the battery case.SOLUTION: A method of manufacturing a secondary battery of the present disclosure includes a liquid injection step, a charging step and a sealing step. A secondary battery 100 includes a pair of first side walls 12a each having an area size larger than an area size of each of a pair of second side walls 12b, and a sealing plate 14 having a thickness larger than a thickness of a bottom part 12d. Here, at the sealing step, regarding a first area 51 pressed by a pressing jig 92 on a center in width directions of the pair of first side walls 12a, a second area 52 positioned at a sealing plate 14 side more than the first area 51, and a third area 53 positioned at a bottom part 12d side more than the first area 51, in the case where distances in a thickness direction of the battery case 1 directed from an outer surface of one of the first side walls 12a toward an outer surface of the other one of the first side walls 12a are respectively treated as T1, T2, and T3, the pair of first side walls 12a are pressed by the pressing jig 92 such that respective maximum values of the T1, the T2, and the T3 satisfy T2>T3>T1 to seal a liquid injection hole 15.SELECTED DRAWING: Figure 5
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for manufacturing a secondary battery. [Background technology]

[0002] Conventionally, a secondary battery is known that includes an electrode assembly including a positive electrode and a negative electrode, an electrolyte, and a battery case that contains the electrode assembly and the electrolyte. In this connection, for example, Patent Document 1 discloses a method for manufacturing a secondary battery, which is characterized in that a charging step, a degassing step, and an aging step are performed in a restrained state in which a pair of wide surfaces of the battery case are sandwiched from both sides and the battery case is pressed in the sandwiching direction. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent Publication No. 2010-21104 Summary of the Invention [Problem to be solved by the invention]

[0004] According to the inventors' study, there is room for further improvement in the above-mentioned technology. More specifically, the pressing method of the battery case according to the above-mentioned technology does not take into consideration the suppression of swelling in the height direction (vertical direction) of the battery case. That is, in the pressing method of the above-mentioned technology, there is a risk that the height of the battery case will increase due to the expansion of the bottom of the battery case.

[0005] The technology disclosed herein has been made in consideration of the above circumstances, and its purpose is to provide a method for manufacturing a secondary battery that suppresses convex expansion of the battery case due to gas generation associated with charging and discharging the secondary battery, and also suppresses an increase in the height of the battery case when the battery case is pressed. [Means for solving the problem]

[0006] The technology disclosed herein is a method for manufacturing a secondary battery including an electrode assembly including a positive electrode and a negative electrode, an electrolyte, and a battery case that accommodates the electrode assembly and the electrolyte. The battery case includes an exterior body including an opening, a bottom, a pair of first side walls, and a pair of second side walls each having an area smaller than that of the first side walls, and a sealing plate that seals the opening, and the thickness of the sealing plate is greater than the thickness of the bottom. The method for manufacturing such a secondary battery includes a liquid injection step of injecting the electrolyte into the battery case through an injection hole provided in the sealing plate, a charging step of charging, and a sealing step of sealing the injection hole while pressing the pair of first side walls from both sides with a pressing tool. Here, in the sealing process, when the region pressed by the pressing tool at the widthwise center of the pair of first side walls is defined as a first region, the region located closer to the sealing plate than the first region is defined as a second region, and the region located closer to the bottom than the first region is defined as a third region, and the distances in the thickness direction of the battery case from the outer surface of one of the first side walls to the outer surface of the other first side wall of the first region, the second region, and the third region are defined as T1, T2, and T3, respectively, the battery case is deformed by the pressing so that the maximum values ​​of T1, T2, and T3 satisfy the following relationship: T2>T3>T1.

[0007] According to this manufacturing method, the pressing tool presses the first side wall of the battery case. Furthermore, the thickness of the sealing plate is greater than the thickness of the bottom of the exterior body. Therefore, even if the pressing tool presses the battery case so as to expand the second region, the sealing plate is unlikely to deform. That is, it is possible to suppress damage to the battery case and to suppress an increase in the height of the battery case (in other words, a downward protrusion of the bottom of the exterior body). Then, the liquid injection hole is sealed in a state in which the internal volume of the battery case is reduced by this pressing. This makes it possible to suppress the battery case from expanding in a convex shape due to gas generation accompanying charging and discharging of the secondary battery. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a perspective view showing a schematic diagram of a battery according to an embodiment. [Diagram 2] FIG. 2 is a schematic vertical cross-sectional view taken along line II-II in FIG. [Diagram 3] FIG. 3 is a schematic vertical cross-sectional view taken along line III-III in FIG. [Figure 4] FIG. 4 is a schematic diagram illustrating the configuration of an electrode body according to one embodiment. [Diagram 5] FIG. 5 is a vertical cross-sectional view illustrating a sealing step according to the first embodiment. [Figure 6] FIG. 6 is a vertical cross-sectional view illustrating a sealing step according to the second embodiment. [Figure 7] FIG. 7 is a vertical cross-sectional view illustrating a sealing step according to the third embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, the embodiments of the technology disclosed herein will be described with reference to the drawings. Matters not mentioned in this specification and necessary for implementing the technology disclosed herein can be understood as design matters for a person skilled in the art based on the prior art in the field. The technology disclosed herein can be implemented based on the contents disclosed in this specification and the technical common sense in the field. In addition, in the following drawings, the same reference numerals are used to describe members and parts that perform the same function. Furthermore, the dimensional relationships (length, width, thickness, etc.) in each drawing do not reflect the actual dimensional relationships. In addition, the numerical range expressed as "A to B" in this specification includes A and B, and also includes the meanings of "preferably larger than A" and "preferably smaller than B".

[0010] In this specification, the term "battery" refers to any power storage device capable of extracting electrical energy, and is a concept that includes primary batteries and secondary batteries. In addition, in this specification, the term "secondary battery" refers to any power storage device that can be repeatedly charged and discharged by the movement of charge carriers between a positive electrode and a negative electrode via an electrolyte. Secondary batteries include so-called storage batteries (chemical batteries) such as lithium ion secondary batteries and nickel metal hydride batteries. Below, an embodiment in which a lithium ion secondary battery is the subject will be described.

[0011] <Secondary battery 100> FIG. 1 is a perspective view showing a secondary battery 100 according to the first embodiment. FIG. 2 is a schematic longitudinal sectional view taken along line II-II in FIG. 1. FIG. 3 is a schematic longitudinal sectional view taken along line III-III in FIG. 1 (the center of the long side direction Y of the first side wall 12a). In the following description, the symbols L, R, F, Rr, U, and D in the drawings represent left, right, front, rear, top, and bottom. In addition, the symbol X in the drawings indicates the short side direction (also called the thickness direction) of the secondary battery 100, the symbol Y indicates the long side direction of the secondary battery 100, and the symbol Z indicates the up-down direction (also called the height direction) of the secondary battery 100. However, these are merely directions for convenience of description and do not limit the installation form of the secondary battery 100. Here, for convenience of description, the first region 51 is shown by a virtual line in FIG. 1.

[0012] 1 and 2, the secondary battery 100 includes a battery case 1, an electrode assembly 20, a positive electrode terminal 6, a negative electrode terminal 8, a positive electrode current collector 35, and a negative electrode current collector 45. Although not shown, the secondary battery 100 further includes an electrolyte. The secondary battery 100 is preferably a non-aqueous electrolyte secondary battery such as a lithium ion secondary battery.

[0013] The battery case 1 is a housing that houses the electrode assembly 20. As shown in FIG. 1, the battery case 1 here has a flat, bottomed rectangular parallelepiped (rectangular) outer shape. The material of the battery case 1 may be the same as that conventionally used, and is not particularly limited. The battery case 1 is preferably made of metal, and more preferably made of aluminum or an aluminum alloy. As shown in FIGS. 1 and 2, the battery case 1 includes an exterior body 12 having an opening 12u, and a sealing plate 14 that seals the opening 12u. The exterior body 12 and the sealing plate 14 have sizes according to the number of electrode bodies 20 housed (one or more; here, one), the size, etc.

[0014] As shown in Fig. 1 and Fig. 2, the exterior body 12 is a bottomed, rectangular container having an opening 12u on the upper surface. As shown in Fig. 1, the exterior body 12 includes a bottom 12d, a pair of first side walls (large area side walls) 12a extending upward from the long sides of the bottom 12d and facing each other, and a pair of second side walls (small area side walls) 12b extending upward from the short sides of the bottom 12d and facing each other. The bottom 12d is substantially rectangular. The area of ​​the first side wall 12a is larger than the area of ​​the second side wall 12b. The bottom 12d faces the opening 12u (see Fig. 2).

[0015] The sealing plate 14 is a planar, substantially rectangular, plate-like member attached to the exterior body 12 so as to close the opening 12u of the exterior body 12. As shown in FIG. 2, the sealing plate 14 has a base portion 14a, and is provided with a liquid inlet 15, a gas exhaust valve 17, and terminal outlet holes 18 and 19. The base portion 14a is an area where no irregularities are formed in the vertical direction Z, in other words, an area where the thickness of the sealing plate 14 is substantially uniform. The sealing plate 14 faces the bottom portion 12d of the exterior body 12. The battery case 1 is integrated by joining (for example, welding) the sealing plate 14 to the periphery of the opening 12u of the exterior body 12. As a result, the battery case 1 is hermetically sealed (sealed).

[0016] The liquid injection hole 15 is a through hole for injecting the electrolyte into the battery case 1 after the sealing plate 14 is attached to the exterior body 12. Here, the liquid injection hole 15 is sealed by a sealing member 16 after the electrolyte is injected. The gas release valve 17 is a thin-walled portion configured to break when the pressure inside the battery case 1 reaches or exceeds a predetermined value, thereby discharging the gas inside the battery case 1 to the outside. The material of the sealing member 16 can be any sealing member used in this type of secondary battery, without any particular limitation. The sealing member 16 is composed of, for example, only a metal member, or a metal member and a seal member (resin).

[0017] The electrolyte may be any electrolyte used in conventional batteries without any particular limitations. As an example, a non-aqueous electrolyte in which a supporting salt (electrolyte salt) is dissolved in a non-aqueous solvent (organic solvent) is preferably used. As an example of the non-aqueous solvent, a carbonate-based solvent such as ethylene carbonate, dimethyl carbonate, ethyl methyl carbonate, etc. is mentioned. As an example of the supporting salt, a fluorine-containing lithium salt such as LiPF6 is mentioned. The electrolyte may contain an additive as necessary.

[0018] The positive electrode terminal 6 is attached to one end of the sealing plate 14 in the long side direction Y (the left end in FIG. 1 and FIG. 2). The negative electrode terminal 8 is attached to the other end of the sealing plate 14 in the long side direction Y (the right end in FIG. 1 and FIG. 2). As shown in FIG. 2, the positive electrode terminal 6 and the negative electrode terminal 8 are inserted through the terminal pull-out holes 18 and 19 and exposed on the outer surface of the sealing plate 14. As shown in FIG. 2, the lower end 6c of the positive electrode terminal 6 is electrically connected to the positive electrode 3 of the electrode body 20 through the positive electrode current collector 35 inside the exterior body 12. The lower end 8c of the negative electrode terminal 8 is electrically connected to the negative electrode 4 of the electrode body 20 through the negative electrode current collector 45 inside the exterior body 12. The positive electrode terminal 6 and the negative electrode terminal 8 are insulated from the sealing plate 14 by the gasket 72 and the insulating member 80. In addition, a current interrupter (CID) may be provided between the positive terminal 6 and the positive current collector 35 or between the negative terminal 8 and the negative current collector 45.

[0019] The positive electrode terminal 6 is electrically connected to a plate-shaped positive electrode external conductive member 70 on the outside of the battery case 1. The negative electrode terminal 8 is electrically connected to a plate-shaped negative electrode external conductive member 71 on the outside of the battery case 1. The positive electrode external conductive member 70 and the negative electrode external conductive member 71 are connected to other secondary batteries and external devices via external connection members such as bus bars. The positive electrode external conductive member 70 and the negative electrode external conductive member 71 are preferably made of a metal with excellent conductivity, such as aluminum, an aluminum alloy, copper, or a copper alloy. The positive electrode external conductive member 70 and the negative electrode external conductive member 71 are insulated from the sealing plate 14 by an external resin member 74. However, the positive electrode external conductive member 70 and the negative electrode external conductive member 71 are not essential and may be omitted in other embodiments.

[0020] The positive electrode terminal 6 is preferably made of a metal, more preferably made of aluminum or an aluminum alloy. The negative electrode terminal 8 is preferably made of a metal, more preferably made of copper or a copper alloy. The negative electrode terminal 8 may be formed by joining two conductive members together. For example, the portion connected to the negative electrode current collecting member 45 may be made of copper or a copper alloy, and the portion exposed on the outer surface of the sealing plate 14 may be made of aluminum or an aluminum alloy.

[0021] The number of electrode bodies 20 arranged inside one exterior body 12 is not particularly limited, and may be two or more (plural). As shown in Figs. 2 and 3, the electrode body 20 is arranged inside the exterior body 12 while being covered with an insulating sheet 9 (electrode body holder). For example, the insulating sheet 9 is folded into a box shape, and the electrode body 20 is arranged inside the insulating sheet 9. This makes it possible to prevent the electrode body 20 from coming into direct contact with the exterior body 12. The insulating sheet 9 is preferably made of resin.

[0022] Fig. 4 is a schematic diagram showing the configuration of the electrode body 20. As shown in Fig. 4, the electrode body 20 has a positive electrode 3 and a negative electrode 4. The electrode body 20 is preferably flat. As shown in Fig. 4, the electrode body 20 is preferably a flat wound electrode body in which a strip-shaped positive electrode 3 and a strip-shaped negative electrode 4 are stacked in a state insulated from each other via a strip-shaped separator 7, and wound around a winding axis WL.

[0023] 3, the electrode body 20 has a pair of curved portions 21 that face the bottom 12d and sealing plate 14 of the exterior body 12, and a flat portion 22 that connects the pair of curved portions 21 and faces the first side wall 12a of the exterior body 12. However, the electrode body 20 may be a laminated electrode body formed by stacking a plurality of square-shaped (typically rectangular) positive electrodes and a plurality of square-shaped (typically rectangular) negative electrodes in an insulated state.

[0024] As shown in FIG. 4, the positive electrode 3 has a positive electrode collector 30, a positive electrode active material layer 31 fixed on at least one surface of the positive electrode collector 30, and a positive electrode protective layer 32. However, the positive electrode protective layer 32 is not essential and can be omitted in other embodiments. The positive electrode collector 30 is made of a conductive metal such as aluminum, an aluminum alloy, nickel, or stainless steel, and is preferably made of aluminum or an aluminum alloy. The positive electrode active material layer 31 is a layer containing a positive electrode active material (e.g., a lithium transition metal composite oxide such as a lithium nickel cobalt manganese composite oxide) that can reversibly occlude and release charge carriers. The positive electrode protective layer 32 is a layer containing an inorganic filler such as alumina.

[0025] 4, the negative electrode 4 has a negative electrode current collector 40 and a negative electrode active material layer 41 fixed onto the negative electrode current collector 40. The negative electrode current collector 40 is made of a conductive metal such as copper, a copper alloy, nickel, or stainless steel, and is preferably made of copper or a copper alloy. The negative electrode active material layer 41 is a layer containing a negative electrode active material (e.g., a carbon material such as graphite) that can reversibly absorb and release charge carriers.

[0026] A plurality of positive electrode tabs 36 are provided at one end of the positive electrode current collector 30 in the long side direction Y (the left end in FIG. 4). The plurality of positive electrode tabs 36 each protrude toward one side of the long side direction Y (the left side in FIG. 4). The plurality of positive electrode tabs 36 protrude in the long side direction Y beyond the separator 7. Here, the plurality of positive electrode tabs 36 are each trapezoidal. However, the shape of the positive electrode tab 36 is not limited thereto. The size of the plurality of positive electrode tabs 36 is also not particularly limited. The shape and size of the positive electrode tab 36 can be appropriately adjusted depending on the formation position, etc., taking into consideration, for example, the state of being connected to the positive electrode current collector 35. The positive electrode tab 36 is preferably made of metal foil, and more preferably made of aluminum foil or aluminum alloy foil. Here, the positive electrode tab 36 is a portion of the positive electrode current collector 30 where the positive electrode active material layer 31 and the positive electrode protective layer 32 are not formed (so-called current collector exposed portion). However, the positive electrode tab 36 may be a separate member from the positive electrode current collector 30 .

[0027] A plurality of negative electrode tabs 46 are provided at one end of the negative electrode current collector 40 in the long side direction Y (the right end in FIG. 4). The plurality of negative electrode tabs 46 protrude toward one side of the long side direction Y (the right side in FIG. 4). The plurality of negative electrode tabs 46 protrude in the long side direction Y beyond the separator 7. Here, the plurality of negative electrode tabs 46 are each trapezoidal. However, the shape of the negative electrode tab 46 is not limited thereto. The size of the plurality of negative electrode tabs 46 is also not particularly limited. The shape and size of the negative electrode tab 46 can be appropriately adjusted depending on the formation position, etc., taking into consideration, for example, the state of being connected to the negative electrode current collector 45. The negative electrode tab 46 is preferably made of a metal foil, and more preferably made of a copper foil or a copper alloy foil. Here, the negative electrode tab 46 is a portion of the negative electrode current collector 40 where the negative electrode active material layer 41 is not formed (so-called current collector exposed portion). However, the negative electrode tab 46 may be a member separate from the negative electrode current collector 40.

[0028] The separator 7 is a member that insulates the positive electrode active material layer 31 of the positive electrode 3 from the negative electrode active material layer 41 of the negative electrode 4. The separator 7 is preferably a porous resin sheet made of a polyolefin resin such as polyethylene (PE) or polypropylene (PP). A heat resistance layer (HRL) containing an inorganic filler may be provided on the surface of the separator 7.

[0029] As shown in FIG. 2, the positive electrode tabs 36 are stacked at one end in the long side direction Y (the left end in FIG. 2) to form a positive electrode tab group 38. On the other hand, the negative electrode tabs 46 are stacked at one end in the long side direction Y (the right end in FIG. 2) to form a negative electrode tab group 48. Here, the secondary battery 100 has a so-called horizontal tab structure in which the positive electrode tab group 38 and the negative electrode tab group 48 are located on the left and right sides of the electrode body 20. However, the secondary battery 100 may have a so-called upper tab structure in which the positive electrode tab group 38 and the negative electrode tab group 48 are located above and below the electrode body 20. The positive electrode tab group 38 is curved in a state where it is joined to the positive electrode current collecting member 35. Similarly, the negative electrode tab group 48 is curved in a state where it is joined to the negative electrode current collecting member 45.

[0030] The positive electrode current collecting member 35 constitutes a conductive path that electrically connects the positive electrode tab group 38 of the electrode body 20 and the positive electrode terminal 6. The positive electrode current collecting member 35 is preferably made of a metal having excellent conductivity, for example, aluminum or an aluminum alloy. The negative electrode current collecting member 45 constitutes a conductive path that electrically connects the negative electrode tab group 48 of the electrode body 20 and the negative electrode terminal 8. The negative electrode current collecting member 45 is preferably made of a metal having excellent conductivity, for example, copper or a copper alloy.

[0031] <Manufacturing Method of Secondary Battery 100> The method for manufacturing the secondary battery 100 disclosed herein is characterized by including a liquid injection step, a charging step, and a sealing step. The method for manufacturing the secondary battery 100 disclosed herein may further include other steps at any stage in addition to the above steps. Although not particularly limited, for example, the secondary battery 100 can be manufactured by a manufacturing method that typically includes, in this order, (1) an assembly preparation step, (2) a drying step, (3) a liquid injection step, (4) a charging step, (5) a depressurization step, and (6) a sealing step. The method for manufacturing the secondary battery disclosed herein is characterized by the sealing step, and the other manufacturing processes may be the same as conventional ones.

[0032] (1) Assembly preparation process In the assembly preparation step, the electrode body 20 is placed in the battery case 1 (exterior body 12) to prepare a battery assembly. In this specification, the term "battery assembly" refers to a secondary battery that has been assembled to a state prior to the charging step described below.

[0033] For example, a battery case 1 (sealing plate 14 and exterior body 12), an electrode body 20, a positive electrode terminal 6, a negative electrode terminal 8, a positive electrode current collecting member 35, a negative electrode current collecting member 45, and an insulating sheet 9 are prepared. The electrode body 20 is preferably a flat wound electrode body in which a positive electrode and a negative electrode are wound with a separator interposed therebetween, as described above. The electrode body 20 can be produced by a conventionally known method. The secondary battery 100 disclosed herein is characterized by the battery case 1 (exterior body 12 and sealing plate 14), and other configurations may be similar to those of the conventional battery.

[0034] The exterior body 12 prepared in the assembly preparation step is made of metal, and is preferably made of aluminum or an aluminum alloy. The thickness of the first side wall 12a is preferably smaller than the thickness of the second side wall 12b. The thickness of the first side wall 12a is preferably 0.2 mm or more, more preferably 0.4 mm or more, and even more preferably 0.6 mm or more. On the other hand, the thickness of the first side wall 12a is preferably 1.5 mm or less, more preferably 1.1 mm or less, and even more preferably 0.9 mm or less. The width of the first side wall 12a is preferably 15 cm or more, and more preferably 20 cm or more. The height of the first side wall 12a is preferably 5 cm or more, and more preferably 8 cm or more. The "width of the first side wall 12a" refers to the length of the first side wall 12a in the long side direction Y, and the "height of the first side wall 12a" refers to the length of the first side wall 12a in the up-down direction Z. The thickness of the bottom 12d is preferably 1.0 mm or more, more preferably 1.3 mm or more, and even more preferably 1.5 mm or more. Meanwhile, the thickness of the bottom 12d is preferably 2.5 mm or less, more preferably 2.1 mm or less, and even more preferably 1.9 mm or less. With the exterior body 12 having such a configuration, the first side wall 12a of the exterior body 12 is easily deformed in the sealing process described below. Therefore, an increase in the height H of the battery case 1 in the vertical direction can be more effectively suppressed.

[0035] The sealing plate 14 prepared in the assembly preparation step is made of metal, and is preferably made of aluminum or an aluminum alloy. As shown in FIGS. 3 and 5, the thickness of the base portion 14a of the sealing plate 14 is greater than the thickness of the bottom portion 12d of the exterior body 12. This allows the sealing plate 14 to have a certain degree of strength, and can suppress an increase in the vertical height H of the battery case 1. In addition, in order to improve the quality of the joint between the exterior body 12 and the sealing plate 14, it is preferable to increase the thickness of the sealing plate 14. The thickness of the base portion 14a of the sealing plate 14 is preferably 1.5 mm or more, more preferably 2.0 mm or more, and even more preferably 2.5 mm or more. On the other hand, the thickness of the base portion 14a of the sealing plate 14 is preferably 4.0 mm or less, preferably 3.0 mm or less, and even more preferably 2.9 mm or less. Note that the "thickness of the base portion 14a of the sealing plate 14" refers to the "thickness of the sealing plate 14" in this specification. The sealing plate 14 having the above configuration suppresses deformation of the sealing plate 14 during the sealing process described below, while more suitably facilitating deformation of the first side wall 12a of the exterior body 12. This makes it possible to more effectively suppress an increase in the vertical height H of the battery case 1.

[0036] The materials of the exterior body 12 and the sealing plate 14 are preferably the same, and are particularly preferably made of a metal mainly composed of aluminum (for example, an aluminum content of 85 mass % or more). However, the materials of the exterior body 12 and the sealing plate 14 may be different from each other.

[0037] In the assembly preparation step, the positive electrode current collecting member 35 is attached to the positive electrode tab group 38 of the electrode body 20, and further, the negative electrode current collecting member 45 is attached to the negative electrode tab group 48. Next, the positive electrode terminal 6 and the negative electrode terminal 8 are attached to the sealing plate 14. Electrode current collecting members of the same polarity are joined to these electrode terminals by a conventionally known method (e.g., ultrasonic bonding, resistance welding, laser welding, etc.). Next, the electrode body 20 is accommodated in the insulating sheet 9. Then, it is preferable to accommodate (insert) the electrode body 20 covered with the insulating sheet 9 into the internal space of the exterior body 12. Then, the exterior body 12 of the battery case 1 and the sealing plate 14 are joined to prepare a battery assembly. Such joining can be performed by welding, for example, laser welding.

[0038] In the assembly preparation step, the electrode body 20 is preferably placed inside the exterior body 12 such that the winding axis WL is parallel to the bottom 12d of the exterior body 12. Furthermore, the electrode body 20 is preferably placed inside the exterior body 12 such that the thickness (stacking) direction of the electrode body 20 is substantially perpendicular to the first side wall 12a (in a direction perpendicular to the first side wall 12a). In other words, the electrode body 20 is placed inside the battery case 1 in a direction (short side direction X) in which the thickness direction of the battery case 1 and the thickness direction of the electrode body 20 coincide. This makes it easier for a gap to be generated between the first side wall 12a and the curved surface portion 21 of the electrode body 20, and makes it easier for the battery case 1 (exterior body 12) to deform into an intended shape.

[0039] (2) Drying process In the drying step, the battery assembly is dried to remove moisture contained in the battery assembly (e.g., inside the electrode body 20, etc.). Such a drying method can be performed by a known method. For example, the drying step can be performed by transporting the battery assembly (battery case 1 containing the electrode body 20) to a drying furnace (not shown) and heating it.

[0040] The drying temperature and drying time in the drying step can be appropriately adjusted according to the amount of moisture contained in the electrode body 20. The drying temperature is not particularly limited as long as it is within a range in which moisture can be removed, but it is desirable to dry at a temperature at which the separator 7 of the electrode body 20 is not damaged. The drying step may be performed in an atmospheric pressure atmosphere or a reduced pressure atmosphere, but is preferably performed in a reduced pressure atmosphere. This makes it possible to shorten the drying time in the drying step. Note that the drying step is not an essential step in the technology disclosed herein. In some preferred embodiments, the drying step may be omitted.

[0041] (3) Liquid injection process In the liquid injection step, the electrolyte is injected into the battery case 1 containing the electrode body 20 through the liquid injection hole 15 provided in the sealing plate 14. The liquid injection step may be performed in an atmospheric pressure atmosphere or a reduced pressure atmosphere, but is preferably performed in a reduced pressure atmosphere. This improves the impregnation of the electrolyte into the electrode body 20, and the liquid injection step can be performed in a shorter time. In the liquid injection process, the electrolyte is injected so that the electrolyte is distributed throughout the electrode body 20. In the liquid injection step, a conventionally known electrolyte injection device can be appropriately used. In addition, as the pressure-transfer gas that can be used to pressure-transfer the electrolyte at this time, as in the conventional case, an inert gas such as nitrogen (N2), dry air, etc. can be used. After the liquid injection step is completed, it is preferable to appropriately pressurize or depressurize the inside of the battery case 1.

[0042] (4) Charging process In the charging step, the battery assembly is charged. By carrying out the charging step, a good quality coating can be formed on the surface of the negative electrode active material layer 41. Gas generated in the charging step is released to the outside of the battery case 1. The charging conditions in this step are not particularly limited and may be the same as those in conventional secondary battery manufacturing methods. In the charging step, the liquid injection hole 15 may be temporarily sealed. However, in the charging step, the liquid injection hole 15 is not completely sealed.

[0043] (5) Decompression process In the depressurization step, the pressure inside the battery case 1 is reduced, thereby further discharging gas present inside the battery case 1 (for example, air or gas generated in the charging step) to the outside of the battery case 1. This depressurization step may be similar to the depressurization step in this type of conventional battery manufacturing method, and is not a particular feature of the technology disclosed herein, so further detailed description will be omitted. Note that in the technology disclosed herein, the depressurization step is not an essential step. In some preferred embodiments, the depressurization step may be omitted.

[0044] (6) Sealing process In the sealing step, the first side wall 12a of the exterior body 12 is pressed from both sides by a pressing jig 92 to seal the liquid injection hole 15. The sealing step includes, in this order, (6-1) an exterior body pressing step and (6-2) a liquid injection hole sealing step. An aging step may be included before or after the sealing step (before the exterior body pressing step or after the liquid injection hole sealing step). The aging step may be the same as the aging step in a conventional battery manufacturing method of this type, and is not particularly characteristic of the technology disclosed herein, so further detailed description will be omitted.

[0045] (6-1) Exterior body pressing process Fig. 5 is a vertical cross-sectional view that typically illustrates the sealing step (exterior body pressing step) according to the first embodiment, and corresponds to Fig. 3. In the exterior body pressing step, first, pressing jigs 92 are disposed so as to sandwich a pair of first side walls 12a of the exterior body 12 from both sides. Then, as shown in Fig. 5, the pair of pressing jigs 92 are used to press the pair of first side walls 12a of the exterior body 12 in the sandwiching direction of the pressing jigs 92 (X direction in Fig. 5), thereby deforming the battery case 1 (exterior body 12).

[0046] In the exterior body pressing step, the secondary battery 100 has a first region 51, which is a region pressed by a pressing tool 92, at the center of the width direction (long side direction Y) of the first side wall 12a, as shown in Fig. 5. Meanwhile, in the up-down direction Z, the secondary battery 100 has a second region 52, which is a region located closer to the sealing plate 14 side (upper side) than the first region 51, and a third region 53, which is a region located closer to the bottom 12d side (lower side) of the exterior body 12 than the first region 51. Then, when the distances of the first region 51, the second region 52, and the third region 53 in the thickness direction X of the battery case 1 from the outer surface of one first side wall 12a toward the other first side wall 12a are T1, T2, and T3, respectively, the battery case 1 (exterior body 12) is deformed so that the maximum values ​​of the respective distances satisfy the following formula (i): T2>T3>T1. This makes it possible to suppress damage to the battery case 1 and to suppress an increase in the height H of the battery case 1 (in other words, protrusion of the bottom 12d of the exterior body 12 in the D direction).

[0047] More specifically, as shown in FIG. 5, in the first region 51, the portion of the first side wall 12a that abuts against the pressing jig 92 is pressed (pressed) toward the inside (electrode body 20 side) of the exterior body 12. As a result, T1 becomes smaller than the thickness T0 (see FIG. 3) of the battery case 1 before pressing. Then, in the second region 52, an expansion portion 52a that protrudes outward from the end of the sealing plate 14 in the thickness direction (short side direction X) of the battery case 1 is formed. On the other hand, in the third region 53, no expansion portion is formed. That is, T2 becomes larger than T3 of the third region 53 where no expansion portion is formed by the amount that the expansion portion 52a is formed in the second region. Therefore, the above-mentioned formula (i): T2>T3>T1 holds true.

[0048] Here, in the conventional manufacturing method, when the first side wall 12a is pressed by the pressing jig 92 so that the third region 53 expands, there is a risk that the bottom 12d of the exterior body 12 will be curved downwardly convexly. In other words, there is a risk that the height H of the battery case 1 will increase. In contrast, in the secondary battery 100 according to this embodiment, the thickness of the sealing plate 14 is thicker than the bottom 12d of the exterior body 12. Therefore, even if the second region 52 is pressed so that it has the expanding portion 52a, the sealing plate 14 is unlikely to deform. Therefore, when pressed by the pressing jig 92, an increase in the height H of the battery case 1 can be suppressed.

[0049] In the exterior body pressing step, the deformation of the battery case 1 can be controlled to satisfy the above formula (i) by using the battery case 1 (sealing plate 14 and exterior body 12) having the above shape and controlling the pressing conditions. Such pressing conditions can be appropriately adjusted depending on the shape, thickness, material, etc. of the battery case 1. Preferred pressing conditions in the exterior body pressing step are described in detail below.

[0050] 5, the pressing jig 92 is preferably made of metal. However, the present invention is not limited to this, and for example, a member made of resin, rubber, or the like may be disposed on the surface of the pressing jig 92 (in other words, the area where the pressing jig 92 and the battery case 1 come into contact).

[0051] In the exterior body pressing step, when viewed along the thickness direction of the electrode body 20 (front view), in the pair of first side walls 12a of the exterior body 12, when the entire area where one of the first side walls 12a and the flat portion 22 of the electrode body 20 overlap is taken as 100%, the first region 51 preferably includes at least 80% or more of the area, more preferably includes 90% or more, and even more preferably includes 100% or more (see FIG. 1). Furthermore, the first region 51 may be larger than the area overlapping with the flat portion 22 of the electrode body 20 and may include this area. Furthermore, the first region 51 preferably includes the first side walls and the area of ​​the flat portion 22 of the electrode body 20 that includes the positive electrode active material layer 31 when viewed from the front.

[0052] In the exterior body pressing step, regarding the ratio of the above-mentioned distances T1, T2, and T3, T2 / T1 is preferably 1.03 or more, while T3 / T1 is preferably 1.02 or less.

[0053] The amount of pressing by pressing jig 92 on pair of first side walls 12a of exterior body 12 is preferably about 0.5 to 5 mm, and more preferably about 0.5 to 2 mm. This makes it possible to suitably prevent the battery case 1 from expanding in a convex shape during charging and discharging of the secondary battery 100. In this specification, the "pressing amount" refers to the difference (i.e., T0-T1) between the distance (thickness) T0 (see FIG. 3) of the battery case 1 before pressing and the distance T1 (see FIG. 5) of the first region during pressing in the short side direction X.

[0054] In the exterior body pressing step, the pressing strength (pressing force) when the pressing jig 92 presses the first side wall 12a of the exterior body 12 is preferably 5 kN or more, more preferably 10 kN or more, and even more preferably 20 kN or more. On the other hand, the pressing strength (pressing force) is preferably 40 kN or less, more preferably 35 kN or less, and even more preferably 30 kN or less.

[0055] The following embodiments are some suitable examples of a method for pressing the exterior body 12 (a method for deforming the battery case 1) in the exterior body pressing step. However, the present invention is not limited to these embodiments and can be implemented by other methods.

[0056] Second embodiment FIG. 6 is a vertical cross-sectional view that typically illustrates a sealing step (exterior body pressing step) according to the second embodiment. As shown in FIG. 6, in the second embodiment, a first guide member 94 is disposed at the upper end of a pressing jig 92. Other than that, the second embodiment may be the same as the first embodiment described above. The first guide member 94 serves to guide the first side wall 12a. The first guide member 94 is tapered in the vertical direction Z so that the thickness gradually decreases upward. The first guide member 94 and the pressing jig 92 are integrally molded here. However, this is not limited thereto. For example, the first guide member 94 and the pressing jig 92 may be molded separately and then joined by welding or the like, or may be separate members. As a result, when pressing is performed by the pressing jig 92, the exterior body 12 is deformed along the tapered portion of the first guide member 94. Therefore, the expansion portion 52a is easily formed in the second region 52.

[0057] (Third embodiment) FIG. 7 is a vertical cross-sectional view that shows a sealing step (exterior pressing step) according to the third embodiment. As shown in FIG. 7, in the third embodiment, a first guide member 294 is arranged at the upper end of the pressing jig 92 instead of the first guide member 94. A second guide member 296 is provided at the lower end of the pressing jig 92. The rest may be the same as the second embodiment. The second guide member 296 has a role of guiding the first side wall 12a. As shown in FIG. 7, the first guide member 294 and the second guide member 296 are made of resin here. Here, the first guide member 294 is configured to cover the entire second region 52. On the other hand, the second guide member 296 is configured to cover the entire third region 53. As a result, when the pressing jig 92 presses the first side wall 12a of the outer casing 12, the second guide member 296 suppresses the formation of an expansion portion in the third region 53, and the first guide member 294 makes it easier to form the expansion portion 52a in the second region 52.

[0058] (6-2) Liquid injection hole sealing process In the liquid injection hole sealing step, the liquid injection hole 15 of the battery case 1 is sealed while the exterior body 12 is pressed in the exterior body pressing step. As a result, the liquid injection hole 15 is sealed while the internal volume of the battery case 1 is reduced. This makes it possible to prevent the battery case 1 from expanding in a convex shape due to gas generated when the secondary battery 100 is charged and discharged. Here, the liquid injection hole 15 is sealed with a metallic sealing member 16, and the metallic portion of the sealing member 16 is sealed by welding to the battery case 1. However, the method of sealing the liquid injection hole 15 is not limited to this. Although not shown in the drawings, the liquid injection hole 15 may be sealed with a rivet such as a blind rivet.

[0059] As described above, the manufacturing method of a secondary battery disclosed herein can suppress damage to the battery case 1, seal the liquid injection hole 15 while suppressing an increase in the height H of the battery case 1, and suppress the battery case 1 from expanding in a convex shape due to gas generation accompanying charging and discharging of the secondary battery 100.

[0060] The secondary battery 100 can be used for various purposes, but typically can be suitably used as a power source (driving power source) for motors mounted on various vehicles, such as passenger cars and trucks. The type of vehicle is not particularly limited, but examples include plug-in hybrid vehicles (PHEVs), hybrid electric vehicles (HEVs), and battery electric vehicles (BEVs). The secondary battery 100 can also be suitably used to construct a battery pack.

[0061] Although several embodiments of the technology disclosed herein have been described above, the above embodiments are merely examples. The technology disclosed herein can be implemented in various other forms. The technology disclosed herein can be implemented based on the contents disclosed in this specification and the technical common sense in the field. The technology described in the claims includes various modifications and changes to the above-exemplified embodiments. For example, it is possible to replace a part of the above-mentioned embodiment with another modified form, and it is also possible to add another modified form to the above-mentioned embodiment. Furthermore, if the technical feature is not described as essential, it is also possible to delete it as appropriate.

[0062] As described above, specific aspects of the technology disclosed herein include those described in the following sections. Item 1: A method for manufacturing a secondary battery including an electrode assembly including a positive electrode and a negative electrode, an electrolyte, and a battery case that accommodates the electrode assembly and the electrolyte, the battery case including an exterior body including an opening, a bottom, a pair of first side walls, and a pair of second side walls each having an area smaller than that of the first side walls, and a sealing plate that seals the opening, the thickness of the sealing plate being greater than the thickness of the bottom, the method including: an injection step of injecting the electrolyte into the battery case through an injection hole provided in the sealing plate; a charging step of charging; and a sealing step of sealing the injection hole while pressing the pair of first side walls from both sides with a pressing tool, wherein the sealing plate a pressing step in which a region pressed by the pressing jig at the width direction center of the pair of first side walls is defined as a first region, a region closer to the sealing plate than the first region is defined as a second region, and a region closer to the bottom than the first region is defined as a third region, and distances in a thickness direction of the battery case from an outer surface of one of the first side walls to an outer surface of the other first side wall of the first region, the second region, and the third region are defined as T1, T2, and T3, respectively, and the battery case is deformed by pressing such that the maximum values ​​of T1, T2, and T3 satisfy the following relationship: T2>T3>T1. Item 2: The method for producing a secondary battery according to item 1, wherein the bottom of the exterior body has a thickness of 1.0 to 2.5 mm, the first side wall of the exterior body has a thickness of 0.2 to 1.5 mm, and the sealing plate has a thickness of 1.5 to 4.0 mm. Item 3: The method for producing a secondary battery according to item 1 or 2, wherein the first side wall has a thickness smaller than a thickness of the second side wall. Item 4: The method for producing a secondary battery according to any one of Items 1 to 3, wherein the exterior body is made of aluminum or an aluminum alloy, and the sealing plate is made of aluminum or an aluminum alloy. Item 5: The method for producing a secondary battery according to any one of Items 1 to 4, wherein the first side wall has a width of 20 cm or more and a height of 8 cm or more. Item 6: The method for manufacturing a secondary battery according to any one of items 1 to 5, wherein the electrode body is a flat wound electrode body, the winding axis of the wound electrode body is arranged parallel to the bottom of the outer casing, and the thickness direction of the wound electrode body is arranged perpendicular to the first side wall. [Explanation of symbols]

[0063] 1 Battery case 3 Positive electrode 4 Negative electrode 6 Positive terminal 7 Separator 8 Negative terminal 9. Insulation sheet 12 Exterior body 12d bottom 12a 1st side wall 12b 2nd side wall 14 Sealing plate 14a Base 15 Liquid injection hole 20 Electrode body 21 Curved part 22 Flat area 30 Positive electrode current collector 35 Positive electrode current collector 36 Positive tab 38 Positive electrode tab group 40 Negative electrode current collector 46 Negative tab 48 Negative electrode tab group 51 First area 52 Second area 53 Third area 72 Gasket 80 Insulating materials 92 Pressing tool 94, 294 First guide member 296 Second guide member 100 Secondary battery

Claims

1. An electrode assembly including a positive electrode and a negative electrode; An electrolyte; a battery case that accommodates the electrode assembly and the electrolyte; A method for manufacturing a secondary battery comprising: the battery case includes an exterior body including an opening, a bottom, a pair of first side walls, and a pair of second side walls each having an area smaller than that of the first side walls, and a sealing plate that seals the opening, The thickness of the sealing plate is greater than the thickness of the bottom portion, a liquid injection step of injecting the electrolyte into the battery case through an injection hole provided in the sealing plate; a charging step for charging the battery; a sealing step of sealing the liquid injection hole in a state in which the pair of first side walls are pressed from both sides by a pressing tool, Here, in the sealing step, A region pressed by the pressing tool at the widthwise center of the pair of first side walls is referred to as a first region, a region located closer to the sealing plate than the first region is referred to as a second region; a third region is a region located closer to the bottom than the first region; When distances in the thickness direction of the battery case from an outer surface of one of the first side walls to an outer surface of the other of the first side walls of the first region, the second region, and the third region are T1, T2, and T3, respectively, The maximum values ​​of T1, T2, and T3 are in the following relationship: T2>T3>T1; The battery case is deformed by the pressing so that A method for manufacturing a secondary battery.

2. The thickness of the bottom of the exterior body is 1.0 to 2.5 mm, The thickness of the first side wall of the exterior body is 0.2 to 1.5 mm, The thickness of the sealing plate is 1.5 to 4.0 mm. The method for producing the secondary battery according to claim 1 .

3. The thickness of the first side wall is smaller than the thickness of the second side wall. The method for producing the secondary battery according to claim 1 or 2.

4. The exterior body is made of aluminum or an aluminum alloy, The sealing plate is made of aluminum or an aluminum alloy. The method for producing the secondary battery according to claim 1 or 2.

5. The first side wall has a width of 20 cm or more and a height of 8 cm or more. The method for producing the secondary battery according to claim 1 or 2.

6. The electrode body is a flat wound electrode body, A winding axis of the wound electrode body is arranged parallel to the bottom of the exterior body, The wound electrode body is disposed so that a thickness direction of the wound electrode body is perpendicular to the first side wall. The method for producing the secondary battery according to claim 1 or 2.

Citation Information

Patent Citations

  • Can body for secondary battery, and secondary battery

    JP2003208877A

  • Rectangular nonaqueous electrolyte secondary battery

    JP2005149763A

  • Manufacturing method of nonaqueous electrolyte secondary battery

    JP2008027741A

  • Method of manufacturing secondary battery

    JP2010021104A

  • Method of manufacturing battery, and battery

    JP2010176989A